Coating solution for forming pressure measurement layer, method for producing pressure measurement layer, and article including non-flat portion with pressure measurement layer

A coating liquid with microcapsules and a color developer forms a pressure measurement layer that achieves excellent color development and gradation on non-planar surfaces at low pressures, addressing the limitations of existing resin materials.

JP7578700B2Active Publication Date: 2024-11-06FUJIFILM CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2022544464
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-08-31
Filing Date
2021-08-16
Publication Date
2024-11-06
Estimated Expiration
2041-08-16

AI Technical Summary

Technical Problem

Existing pressure-sensitive coloring resin materials fail to provide good color distribution (gradation) at low pressures and are inadequate for measuring pressure distribution on non-planar surfaces.

Method used

A coating liquid comprising microcapsules containing a color former and an aromatic solvent, a color developer not encapsulated in microcapsules, a resin, and a solvent, with specific resin content and viscosity, is used to form a pressure measurement layer that can be applied to non-planar surfaces.

Benefits of technology

The coating liquid enables excellent color development and gradation on non-planar surfaces even at low pressures, allowing accurate pressure measurement.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007578700000010
    Figure 0007578700000010
  • Figure 0007578700000011
    Figure 0007578700000011
  • Figure 0007578700000012
    Figure 0007578700000012
Patent Text Reader

Abstract

A first problem addressed by the present invention is to provide a coating liquid for pressure measurement layer formation with which it is possible to form a pressure measurement layer that can be used in measurement of the pressure or pressure distribution at a non-planar portion of an article having said non-planar portion, and that exhibits a color forming portion having excellent gradation properties even when subjected to low pressures (for example, 300 MPa or lower). A second problem addressed by the present invention is to provide a method for producing a pressure measurement layer that can be used in measurement of the pressure or pressure distribution at a non-planar portion of an article having said non-planar portion, and that provides a color forming portion having excellent gradation properties even when subjected to low pressures (for example, 300 MPa or lower). A third problem addressed by the present invention is to provide a non-planar-portion-including article with a pressure measurement layer formed using the above coating liquid for pressure measurement layer formation, and a non-planar-portion-including article with a pressure measurement layer formed with the above method for producing a pressure measurement layer. A coating liquid for pressure measurement layer formation according to the present invention includes: microcapsules that encapsulate a color forming agent an aromatic solvent; a developer that is not encapsulated in the microcapsules; a resin; and a solvent, wherein the resin content is not more than 17 mass% with respect to all solid content.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a coating liquid for forming a pressure measurement layer, a method for producing a pressure measurement layer, and an article containing a non-flat portion and having a pressure measurement layer. [Background technology]

[0002] In recent years, with the increasing sophistication and precision of products, there is an increasing need to measure pressure distribution. For example, Patent Document 1 proposes a pressure-sensitive color-changing resin material characterized in that at least one of a color former and a color developer that change color upon contact is encapsulated in a microcapsule and both are blended into a resin composition that serves as a matrix. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2007-132756 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have studied the pressure-sensitive color-developing resin material described in Patent Document 1 and have found that unless a relatively high pressure is applied, it is insufficient to obtain a good color distribution (gradation) according to the pressure difference in the color-developing portion generated by the reaction between the color former and the color developer in the pressurized area. In other words, it has been found that there is room for further improvement of the pressure-sensitive color-developing resin material so that a color-developing portion with excellent gradation can be obtained even when pressurized at a low pressure range (for example, 300 MPa or less). In addition, the surface shape of the object to be measured is not only flat but also diverse, such as curved and uneven surfaces, and when the object has a surface shape other than flat, the pressure measurement member having the form of a film or sheet cannot follow the surface of the object, making it difficult to measure the pressure or pressure distribution. For this reason, there is a demand for a pressure measurement member that can be used on the non-flat portion of an object having a non-flat portion.

[0005] Therefore, an object of the present invention is to provide a coating liquid for forming a pressure measurement layer that can be applied to measure pressure or pressure distribution in a non-flat portion of an article having a non-flat portion, and that can form a pressure measurement layer that exhibits a color development portion with excellent gradation even when pressurized in a low pressure range (e.g., 300 MPa or less). Another object of the present invention is to provide a method for manufacturing a pressure measurement layer that can be applied to measure pressure or pressure distribution in a non-flat portion of an article having a non-flat portion, and that can provide a color-developing portion with excellent gradation even when pressurized at a low pressure range (e.g., 300 MPa or less). Another object of the present invention is to provide an article including a non-flat portion with a pressure measurement layer formed using the above-mentioned coating liquid for forming a pressure measurement layer, and an article including a non-flat portion with a pressure measurement layer formed by the above-mentioned method for manufacturing a pressure measurement layer. [Means for solving the problem]

[0006] As a result of intensive research into solving the above problems, the present inventors have found that the above problems can be solved by the following configuration.

[0007] [1] A microcapsule containing a color former and an aromatic solvent; A color developer that is not encapsulated in a microcapsule; Resin and A coating liquid for forming a pressure measuring layer, comprising: The coating liquid for forming a pressure measuring layer has a resin content of 17% by mass or less based on the total solid content of the coating liquid for forming a pressure measuring layer. [2] The coating liquid for forming a pressure measuring layer according to [1], wherein the content of the resin is 13 mass % or less based on the total solid content of the coating liquid for forming a pressure measuring layer. [3] The coating liquid for forming a pressure-measuring layer according to [1] or [2], having a viscosity at 25°C of less than 5000 mPa·s. [4] The coating liquid for forming a pressure-measuring layer according to any one of [1] to [3], wherein the microcapsules encapsulating the color former and the aromatic solvent are substantially free of a color developer. [5] The coating liquid for forming a pressure measuring layer according to any one of [1] to [4], wherein the average particle size of microcapsules contained in the coating liquid for forming a pressure measuring layer is 5 μm or more. [6] The coating liquid for forming a pressure-measuring layer according to any one of [1] to [5], wherein the developer contains a material selected from the group consisting of activated clay, acid clay, and zinc salicylate derivatives. [7] The coating liquid for forming a pressure-measuring layer according to [6], wherein the developer is zinc 3,5-bis(α-methylbenzyl)salicylate. [8] The coating liquid for forming a pressure measuring layer according to any one of [1] to [7], wherein the particle size distribution of the microcapsules contained in the coating liquid for forming a pressure measuring layer is 15% or more. [9] The coating liquid for forming a pressure measurement layer according to any one of [1] to [8], wherein a total content of the microcapsules encapsulating the color former and the aromatic solvent, and the color developer is 50 mass % or more based on a total solid content of the coating liquid for forming a pressure measurement layer.

[10] The coating solution for forming a pressure-measuring layer according to any one of [1] to [9], wherein the color former is selected from the group consisting of a compound represented by general formula (1) described later and a compound having an indole structure.

[11] A method for producing a pressure measurement layer, comprising a step of applying a coating liquid for forming a pressure measurement layer to a non-flat surface of an article including a non-flat surface to form a pressure measurement layer, the pressure measurement layer-forming coating liquid contains microcapsules encapsulating a color former and an aromatic solvent, a color developer not encapsulated in the microcapsules, a resin, and a solvent; The average particle size of the microcapsules encapsulating the color former and the aromatic solvent is X μm, and the coating amount of the solid content of the coating liquid for forming the pressure measurement layer is Y g / m 2 When the average particle size is expressed as Y / X, the solid coating amount is Yg / m 2 The method for manufacturing a pressure measurement layer, wherein the ratio is less than 1.

[12] The method for producing a pressure measurement layer according to

[11] , wherein the content of the resin is 17 mass % or less based on the total solid content of the coating liquid for forming the pressure measurement layer.

[13] The method for producing a pressure measurement layer according to

[11] or

[12] , wherein the content of the resin is 13 mass % or less based on the total solid content of the coating liquid for forming the pressure measurement layer.

[14] The method for producing a pressure measurement layer according to any one of

[11] to

[13] , wherein the coating liquid for forming the pressure measurement layer has a viscosity of less than 5000 mPa·s at 25° C.

[15] The method for producing a pressure measuring layer according to any one of

[11] to

[14] , wherein the microcapsules encapsulating the color former and the aromatic solvent are substantially free of a color developer.

[16] The method for producing a pressure measurement layer according to any one of

[11] to

[15] , wherein the average particle size of microcapsules contained in the coating liquid for forming the pressure measurement layer is 5 μm or more.

[17] The method for producing a pressure measurement layer according to any one of

[11] to

[16] , wherein the developer contains a material selected from the group consisting of activated clay, acid clay, and zinc salicylate derivatives.

[18] The method for producing a pressure measuring layer according to any one of

[11] to

[17] , wherein the color developer is zinc 3,5-bis(α-methylbenzyl)salicylate.

[19] The method for producing a pressure measurement layer according to any one of

[11] to

[18] , wherein the particle size distribution of the microcapsules contained in the coating liquid for forming the pressure measurement layer is 15% or more.

[20] The method for producing a pressure measurement layer according to any one of

[11] to

[19] , wherein the total content of the microcapsules encapsulating the color former and the aromatic solvent, and the color developer is 50 mass % or more based on the total solid content of the coating liquid for forming the pressure measurement layer.

[21] The method for producing a pressure measurement layer according to any one of

[11] to

[20] , wherein the color former is selected from the group consisting of a compound represented by general formula (1) described later and a compound having an indole structure.

[22] A non-flat portion-containing article with a pressure measurement layer, comprising: an article including a non-flat portion; and a pressure measurement layer formed on the non-flat portion using the coating liquid for forming a pressure measurement layer according to any one of [1] to

[10] .

[23] A non-flat portion-containing article having a pressure measurement layer, obtained by the method for producing a coating liquid for forming a pressure measurement layer according to any one of

[11] to

[21] . Effect of the Invention

[0008] According to the present invention, a coating liquid for forming a pressure measurement layer can be provided which can be applied to measure pressure or pressure distribution in a non-flat portion of an article having a non-flat portion, and which can form a pressure measurement layer that exhibits a color development portion with excellent gradation even when pressurized in a low pressure range (e.g., 300 MPa or less). Furthermore, the present invention can provide a manufacturing method for a pressure measurement layer that can be applied to measure pressure or pressure distribution in a non-flat portion of an article having a non-flat portion, and that can obtain a color-developing portion with excellent gradation even when pressurized in a low pressure range (e.g., 300 MPa or less). Furthermore, according to the present invention, it is possible to provide an article including a non-flat portion with a pressure measurement layer formed using the above-mentioned coating liquid for forming a pressure measurement layer, and an article including a non-flat portion with a pressure measurement layer formed by the above-mentioned method for manufacturing a pressure measurement layer. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a schematic cross-sectional view showing an example of a pressure measurement layer formed by the coating liquid of the present invention, and is a schematic view for illustrating the relationship between specific microcapsules and a binder. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing an example of a pressure measurement layer formed by the coating liquid of the present invention, and is a schematic view for illustrating the relationship between specific microcapsules and a binder. [Diagram 3]1 is a schematic cross-sectional view showing an example of an article including a non-flat portion with a pressure measurement layer according to the present invention. [Figure 4] 1 is a schematic cross-sectional view showing an example of an article including a non-flat portion with a pressure measurement layer according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In addition, in the numerical ranges described in this specification, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in a certain numerical range. In addition, in the numerical ranges described in this specification, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples. The various components described below may be used alone or in combination of two or more. For example, the polyisocyanates described below may be used alone or in combination of two or more.

[0011] In this specification, when the term "substituent" is used simply, examples of the substituent include the following substituent T.

[0012] (substituent T) Examples of the substituent T include a halogen atom (such as a fluorine atom, a chlorine atom, a bromine atom, or an iodine atom), an alkyl group, a cycloalkyl group, an alkenyl group, a cycloalkenyl group, an alkynyl group, an aryl group, a heterocyclic group, a cyano group, a hydroxyl group, a nitro group, a carboxyl group, an alkoxy group, an aryloxy group, a silyloxy group, a heterocyclic oxy group, an acyloxy group, a carbamoyloxy group, an amino group (including an alkylamino group and an anilino group), an acylamino group, an aminocarbonylamino group, an alkoxycarbonylamino group, an aryl ... Examples of such groups include a phenylamino group, a sulfamoylamino group, an alkyl or arylsulfonylamino group, a mercapto group, an alkylthio group, an arylthio group, a heterocyclic thio group, a sulfamoyl group, a sulfo group, an alkyl or arylsulfinyl group, an alkyl or arylsulfonyl group, an acyl group, an aryloxycarbonyl group, an alkoxycarbonyl group, a carbamoyl group, an aryl or heterocyclic azo group, an imido group, a phosphino group, a phosphinyl group, a phosphinyloxy group, a phosphinylamino group, a silyl group, and a group containing a polymerizable group.

[0013] Among the above-mentioned substituents, those having a hydrogen atom may further have the hydrogen atom portion substituted with any one of the above-mentioned substituents.

[0014] In this specification, unless otherwise specified, the weight average molecular weight (Mw) and the number average molecular weight (Mn) are values ​​calculated in terms of polystyrene by gel permeation chromatography (GPC). In this specification, unless otherwise specified, the molecular weight of a compound having a molecular weight distribution is the weight average molecular weight (Mw).

[0015] In this specification, the "solid content" of the coating liquid for forming a pressure measurement layer means the components forming the pressure measurement layer formed using the coating liquid for forming a pressure measurement layer, and when the coating liquid for forming a pressure measurement layer contains a solvent (organic solvent, water, etc.), it means all components excluding the solvent. In addition, liquid components are also considered to be solid contents as long as they are components forming the coating liquid for forming a pressure measurement layer.

[0016] [Coating solution for forming pressure measurement layer] The coating liquid for forming a pressure measurement layer of the present invention (hereinafter also referred to simply as the "coating liquid" or "coating liquid A") contains microcapsules (hereinafter also referred to simply as the "specific microcapsules") containing a color former and an aromatic solvent, a color developer not contained in the microcapsules (hereinafter also referred to simply as the "color developer"), a resin, and a solvent, The content of the resin is 17% by mass or less based on the total solid content of the coating liquid for forming the pressure measurement layer.

[0017] The coating liquid of the present invention having the above-mentioned configuration can be applied to measure pressure or pressure distribution in a non-flat portion of an article having a non-flat portion, and can form a pressure measurement layer that exhibits a color-developing portion with excellent gradation even when pressurized in a low pressure range (e.g., 300 MPa or less).

[0018] Although the mechanism of action of the above-mentioned configuration and effect is not clear, the present inventors speculate as follows. The main feature of the coating liquid of the present invention is that the resin content in the coating liquid is 17% by mass or less based on the total solid content. It is considered that the resin functions as a resin binder that supports the specific microcapsules and the color developer in the pressure measurement layer formed from the coating liquid of the present invention. Since the pressure measurement layer formed from the coating liquid of the present invention has a resin binder content of a predetermined amount or less, when the coating liquid is applied to the measurement object at a coating amount per unit area that is usually used for pressure measurement, the specific microcapsules are unlikely to be buried in the resin binder. In other words, it is considered that the pressure measurement layer formed from the coating liquid of the present invention is likely to have the form shown in FIG. 1 or FIG. 2. Specifically, as shown in FIG. 1, it is likely to have a form in which one area of ​​the specific microcapsules 14 completely protrudes from the film 12 of the resin binder that holds and supports the specific microcapsules 14 on the coating surface of the measurement object 10. 2, a region of the specific microcapsule 14 protrudes from a film 12 of the resin binder that holds and supports the specific microcapsule 14 on the surface to be coated of the measurement object 10, and the surface of the region protruding from the film 12 of the specific microcapsule 14 (a region of the surface or the entire surface) has a coating 15, which is a thin film of the resin binder. That is, as shown in FIG. 1 and FIG. 2, the pressure measurement layer formed from the coating liquid of the present invention has a particle diameter D1 of the specific microcapsule 14 larger than the thickness D2 of the film 12, so that it is presumed that the specific microcapsule is easily broken when pressurized. As a result, good color development (color development density) and gradation are easily obtained even when pressurized at a low pressure range (for example, 300 MPa or less). As described above, the coating liquid of the present invention can be applied to the measurement of pressure or pressure distribution in a non-flat portion of an article having a non-flat portion. That is, even for a measurement object that is difficult to measure with a conventional film, sheet, etc., a pressure measurement layer can be formed with a coating amount per unit area that is usually used for pressure measurement, regardless of the surface shape.

[0019] Hereinafter, the term "the effect of the present invention is superior" means that one or more selected from the group consisting of the color density, gradation, and image quality of the pressure measurement layer formed from the coating liquid of the present invention, and the coatability of the coating liquid of the present invention, are superior.

[0020] First, various components contained in the coating liquid of the present invention will be described below.

[0021] [Microcapsules Encapsulating a Color Forming Agent and an Aromatic Solvent (Specific Microcapsules)] The coating liquid of the present invention contains microcapsules (specific microcapsules) encapsulating a color former and an aromatic solvent. First, the materials constituting the specific microcapsules will be described in detail below.

[0022] A microcapsule generally has a core portion and a capsule wall for encapsulating a core material (an entity to be encapsulated (also referred to as an encapsulated component)) that constitutes the core portion. In the present invention, the specific microcapsule contains a color former and an aromatic solvent as a core material (encapsulated component). Since the color former is encapsulated in the microcapsule, the color former can exist stably until the microcapsule is broken by pressure application. The capsule wall and the core material will now be described.

[0023] <Capsule wall> Examples of wall materials contained in the capsule walls of the specific microcapsules include polyethylene, polystyrene, polyvinyl, polyurethane, polyurea, and polyurethane polyurea. From the viewpoint of storage stability, the wall material contained in the capsule wall preferably contains a polymer obtained using an isocyanate compound and an organic solvent, more preferably contains a polymer having at least one of a urethane bond and a urea bond, and further preferably contains a polyurethane polyurea.

[0024] <Core material> The specific microcapsules contain a color former as a core material. (Color former) The "color former" is a compound that develops color from a colorless state by contacting with a color developer described later. The color former is preferably an electron-donating dye precursor (a precursor of a dye that develops color). In other words, the color former is preferably an electron-donating colorless dye. Examples of electron donating dye precursors include triphenylmethanephthalide compounds, fluoran compounds, phenothiazine compounds, indolylphthalide compounds, leucoauramine compounds, rhodamine lactam compounds, triphenylmethane compounds, diphenylmethane compounds, triazene compounds, spiropyran compounds, fluorene compounds, pyridine compounds, pyrazine compounds, etc. For details of these compounds, refer to the description in JP-A-5-257272. The color formers include 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-ethyl-2-methylindol-3-yl)-4-azaphthalide, 3-(4-diethylamino-2-ethoxyphenyl)-3-(1-n-octyl-2-methylindol-3-yl)phthalide, 3-[2,2-bis(1-ethyl-2-methylindol-3-yl)vinyl]-3-(4-diethylaminophenyl)-phthalide, 2-anilino-6-dibutylamino-3-methylfluoran, 6-diethylamino-3-methyl-2-(2,6-xylidino)-fluoran, 2-(2-chloroanilino)-6-dibutylaminofluoran, 3,3-bis(4 -dimethylaminophenyl)-6-dimethylaminophthalide, 2-anilino-6-diethylamino-3-methylfluoran, 9-[ethyl(3-methylbutyl)amino]spiro[12H-benzo[a]xanthene-12,1'(3'H)isobenzofuran]-3'-one, and 2'-methyl-6'-(Np-tolyl-N-ethylamino)spiro[isobenzofuran-1(3H),9'-[9H]xanthene]-3-one, 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindole-1,9'-xanthene]-3-one, and 6'-(diethylamino)-1',3'-dimethylfluoran. In addition, Pink-DCF and Orange-DCF (both manufactured by Hodogaya Chemical Co., Ltd.) can also be used as color formers.

[0025] The electron donating dye precursor is preferably a compound represented by the following formula (1) or a compound having an indole structure. The compound represented by the formula (1) and the compound having an indole structure are described in detail below.

[0026] <Compound represented by general formula (1)>

[0027] [ka]

[0028] In general formula (1), R 1 and R 3each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 1 and R 3 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5, in terms of providing better effects for the present invention. The type of the substituent that the alkyl group or the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among them, R 1 and R 3 Each of them is independently preferably an alkyl group which may have a substituent or an aryl group which may have a substituent, more preferably an alkyl group which may have a substituent, and further preferably an unsubstituted alkyl group.

[0029] R 2 and R 4 each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent. R 2 and R 4 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5, in terms of providing better effects for the present invention. R 2 and R 4 The aryl group represented by the following formula (I) may have a monocyclic structure or a polycyclic structure. The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among them, R 2 and R 4 Each of the alkyl groups is preferably an alkyl group which may have a substituent, and more preferably an unsubstituted alkyl group.

[0030] Among them, R 1 ~R 4It is preferable that all of the groups are unsubstituted alkyl groups, and it is more preferable that they are the same unsubstituted alkyl groups.

[0031] X 1 is -O- or -NR 5 Among them, -NR 5 - is preferred. R 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 5 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5, in terms of providing better effects for the present invention. R 5 The aryl group represented by the following formula (I) may have a monocyclic structure or a polycyclic structure. The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among them, R 5 As the alkyl group, an aryl group which may have a substituent is preferable, and an aryl group substituted with a group selected from the group consisting of a halogen atom, a cyano group, a nitro group, and a carboxyl group is more preferable. The aryl group is preferably a phenyl group. Examples of the compound represented by the general formula (1) include 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindole-1,9'-xanthen]-3-one.

[0032] The molecular weight of the compound represented by formula (1) is not particularly limited, but is preferably at least 300, more preferably at least 500. The upper limit is not particularly limited, but is preferably at most 2000, more preferably at most 1000.

[0033] <Compound having an indole structure> A compound having an indole structure is a compound having an indole structure as a partial structure.

[0034] The number of indole structures in the compound having an indole structure is not particularly limited and may be one or more. Among them, in terms of better effects of the present invention, two or more indole structures are preferred, and two is more preferred.

[0035] As the compound having an indole structure, a compound represented by general formula (2) or a compound represented by general formula (3) is preferable, and a compound represented by general formula (3) is more preferable.

[0036] [ka]

[0037] In general formula (2), R 6 and R 7 each independently represents a hydrogen atom or an alkyl group which may have a substituent. R 6 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 30, more preferably 1 to 20, further preferably 1 to 12, and particularly preferably 5 to 10, in terms of superior effects of the present invention. R 7 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3, in terms of superior effects of the present invention. The type of the substituent that the alkyl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among them, R 6 and R 7 preferably represents an alkyl group which may have a substituent, and more preferably an unsubstituted alkyl group.

[0038] R 8 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 8The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5, in terms of providing better effects for the present invention. R 8 The aryl group represented by the following formula (I) may have a monocyclic structure or a polycyclic structure. The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among them, R 8 As the aryl group, an aryl group which may have a substituent is preferable, and an aryl group which has a substituent is more preferable.

[0039] X 2 is -O- or -NR 9 - represents. Among them, the effect of the present invention is more excellent, 2 As the group, -O- is preferable. R 9 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 9 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5, in terms of providing better effects for the present invention. R 9 The aryl group represented by the following formula (I) may have a monocyclic structure or a polycyclic structure. The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above.

[0040] The molecular weight of the compound represented by formula (2) is not particularly limited, but is preferably at least 300, more preferably at least 500. The upper limit is not particularly limited, but is preferably at most 2000, more preferably at most 1000.

[0041] [ka]

[0042] In general formula (3), R 10 ~R 13 each independently represents a hydrogen atom or an alkyl group which may have a substituent. R 10 and R 12 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 30, more preferably 1 to 20, further preferably 1 to 12, and particularly preferably 5 to 10, in terms of superior effects of the present invention. R 11 and R 13 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, more preferably 1 to 5, and even more preferably 1 to 3, in terms of superior effects of the present invention. The type of the substituent that the alkyl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among them, R 10 ~R 13 As the alkyl group, an alkyl group which may have a substituent is preferable, and an unsubstituted alkyl group is more preferable.

[0043] X 3 is -O- or -NR 14 - represents. Among them, the effect of the present invention is more excellent, 3 As the substituent, -O- is preferable. R 14 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 14 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 10, and more preferably 1 to 5, in terms of providing better effects for the present invention. R 14 The aryl group represented by the following formula (I) may have a monocyclic structure or a polycyclic structure. The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Specific examples of the compound represented by the general formula (3) include 3,3-bis(2-methyl-1-octyl-3-indolyl)phthalide.

[0044] The molecular weight of the compound represented by formula (3) is not particularly limited, but is preferably at least 300, more preferably at least 500. The upper limit is not particularly limited, but is preferably at most 2000, more preferably at most 1000.

[0045] As the color former, it is preferable to select from the group consisting of the compound represented by the general formula (1) and the compound having an indole structure, in that the effect of the present invention is more excellent.

[0046] The color former may be used alone or in combination of two or more kinds. The content of the color former (the total content when multiple types are included) is not particularly limited, but is preferably 1 to 50 mass % relative to the total mass of the core material, more preferably 3 to 35 mass %, and even more preferably 5 to 25 mass %. The content of the color former selected from the group consisting of the compound represented by the general formula (1) and the compound having an indole structure (the total content when multiple types are included) is preferably 20 to 100 mass %, more preferably 40 to 100 mass %, based on the total mass of the color former.

[0047] (Aromatic Solvents) The specific microcapsules contain an aromatic solvent as a core material. The aromatic solvent means a solvent having an aromatic ring. The aromatic solvent is preferably in a liquid state at 25°C.

[0048] The aromatic solvent is not particularly limited, but preferably includes a compound having at least one aromatic ring and no condensed aromatic ring (specific aromatic solvent). The number of aromatic rings contained in the specific aromatic solvent is not particularly limited, but is preferably 1 or more in terms of better effects of the present invention. The upper limit is not particularly limited, but is preferably 5 or less, more preferably 3 or less, and even more preferably 1 or 2. The aromatic ring may have a substituent. Examples of the substituent that the aromatic ring may have include the groups exemplified as the substituent T above. The specific aromatic solvent does not have a fused aromatic ring. A fused aromatic ring is a ring formed by condensing two or more aromatic rings.

[0049] The aromatic solvent preferably contains a compound represented by general formula (5).

[0050] [ka]

[0051] In general formula (5), R 20 ~R 24 each independently represents a hydrogen atom, an alkyl group which may have a substituent, or a monocyclic aromatic group which may have a substituent. R 20 ~R 24 The number of carbon atoms in the alkyl group represented by the following formula (1) is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5, in terms of providing better effects for the present invention. R 20 ~R 24 The monocyclic aromatic group represented by the following formula means a monocyclic aromatic group, and examples of the monocyclic aromatic group include a benzene ring group and a monocyclic aromatic heterocyclic group. Among these, the effect of the present invention is excellent in R 20 ~R 24 is preferably a hydrogen atom or an alkyl group which may have a substituent. The type of the substituent that the alkyl group and the monocyclic aromatic group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above.

[0052] L represents a single bond or an alkylene group which may have a substituent. The number of carbon atoms in the alkylene group represented by L is not particularly limited, but is preferably 1 to 20, more preferably 1 to 10, and even more preferably 1 to 5, in terms of better effects of the present invention. Among these, an optionally substituted alkylene group is preferred as L in that the effects of the present invention are more excellent. The type of the substituent that the alkylene group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above.

[0053] R 25 represents a hydrogen atom or a monocyclic aromatic group which may have a substituent. R 25 The monocyclic aromatic group represented by the following formula means a monocyclic aromatic group, and examples of the monocyclic aromatic group include a benzene ring group and a monocyclic aromatic heterocyclic group. The type of the substituent that the monocyclic aromatic group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among these, the effect of the present invention is excellent in R 25 As the group, a monocyclic aromatic group which may have a substituent is preferable.

[0054] The specific aromatic solvent is not particularly limited, and examples thereof include aromatic hydrocarbons such as alkylbenzene compounds such as linear alkylbenzene, diarylalkane compounds such as 1,1-diphenylethane and 1-phenyl-1-(2,3-xylyl)ethane, alkylbiphenyl compounds such as isopropylbiphenyl, triarylmethane compounds, diarylalkylene compounds, and arylindane compounds.

[0055] Among these, the aromatic solvents are preferably alkylbenzene compounds or diarylalkane compounds because they have excellent solubility for compounds having a benzotriazole structure.

[0056] The aromatic solvents may be used alone or in combination of two or more. Among them, in terms of obtaining a more excellent effect of the present invention, it is preferable to use two or more aromatic solvents, and it is more preferable to use a mixture of 2 to 5 aromatic solvents. The aromatic solvent may be used in combination with an aromatic solvent other than the specific aromatic solvent. The content of aromatic solvents (the total content when multiple types are included) is not particularly limited, but is preferably 30 to 95 mass % relative to the total mass of the core material, more preferably 40 to 90 mass %, and even more preferably 50 to 80 mass %. The content of the specific aromatic solvent is preferably from 50 to 100 mass %, more preferably from 75 to 100 mass %, based on the total mass of the aromatic solvents.

[0057] The content of the aromatic solvent in the specific microcapsules is not particularly limited, but in terms of achieving the desired effects of the present invention, it is preferably 20 to 80 mass%, and more preferably 30 to 70 mass%, relative to the total mass of the specific microcapsules.

[0058] (Other Ingredients) The specific microcapsules may contain other components in addition to the above-mentioned color former and aromatic solvent, such as additives such as aliphatic solvents, ultraviolet absorbers, light stabilizers, antioxidants, waxes, and odor suppressants.

[0059] It is also preferable that the specific microcapsules contain an aliphatic solvent. An aliphatic solvent refers to a solvent containing a compound having an aliphatic group, that is, a solvent containing a compound having no aromatic ring.

[0060] Examples of aliphatic solvents include, but are not limited to, aliphatic hydrocarbons such as isoparaffin and dibutyl phthalate; natural animal and vegetable oils such as soybean oil, corn oil, cottonseed oil, rapeseed oil, olive oil, palm oil, castor oil, and fish oil; and high-boiling fractions of natural products such as mineral oils.

[0061] Among these, as the aliphatic solvent, aliphatic hydrocarbons are preferred, and isoparaffin is more preferred, in terms of superior effects of the present invention.

[0062] The aliphatic solvents may be used alone or in combination of two or more.

[0063] The content of the aliphatic solvent in the specific microcapsules is not particularly limited, but in terms of achieving the desired effects of the present invention, it is preferably 5 to 40 mass % relative to the total mass of the aromatic solvent, and more preferably 10 to 30 mass %.

[0064] The specific microcapsules preferably contain an ultraviolet absorbing agent, which is an organic compound that has the function of absorbing ultraviolet light irradiated from outside. The ultraviolet absorbing agent is preferably a compound having a benzotriazole structure.

[0065] The number of benzotriazole structures in the compound having a benzotriazole structure is not particularly limited, and may be one or more.

[0066] The compound having a benzotriazole structure is preferably a compound represented by the general formula (4).

[0067] [ka]

[0068] In general formula (4), R 15 ~R 18 each independently represents a hydrogen atom or a substituent. R 15 ~R 18 The substituent represented by the following formula (I) is not particularly limited, and examples thereof include the groups exemplified for the substituent T described above. Among them, R 15 ~R 18 is a substituent, the effect of the present invention is excellent, 15 ~R 18At least one of these is preferably a halogen atom.

[0069] R 19 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 19 The aryl group represented by the following formula (I) may have a monocyclic structure or a polycyclic structure. The type of the substituent that the alkyl group and the aryl group may have is not particularly limited, and examples thereof include the groups exemplified for the substituent T above. Among these, the effect of the present invention is excellent in R 19 As the alkyl group, an aryl group which may have a substituent is preferable, and an aryl group substituted with at least one hydroxyl group is more preferable. The aryl group is preferably a phenyl group.

[0070] The molecular weight of the compound having a benzotriazole structure is not particularly limited, but is preferably 500 or less, more preferably 400 or less, and even more preferably 350 or less, in terms of better effects of the present invention. The lower limit is not particularly limited, but is often 100 or more. When the molecular weight of the compound having a benzotriazole structure is small, it is easily dissolved in the above-mentioned aromatic solvent, and as a result, the storage stability is better.

[0071] The compound having a benzotriazole structure is not particularly limited, and examples thereof include 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-5'-t-butylphenyl)benzotriazole, 2-(2'-hydroxy-3',5'-di-t-butylphenyl)-5-chlorobenzotriazole, 2-(2'-hydroxy-3'-dodecyl-5'-methylphenyl)-5-chlorobenzotriazole, '-Hydroxy-3',5'-di-t-amylphenyl)benzotriazole, 2-(2'-hydroxy-5'-(1,1,3,3-tetramethylbutyl)phenyl)benzotriazole, 2-(2'-hydroxy-4'-octyloxyphenyl)benzotriazole, 2-(2'-hydroxy-3'-(3,4,5,6-tetrahydrophthalimidylmethyl)-5'-methylbenzylphenyl)benzotriazole, 2-(3'-sec-butyl-5'-t-butyl-2'-hydroxyphenyl)benzotriazole, 2-(3',5'-bis-(α,α-Dimethylbenzyl)-2'-hydroxyphenyl)benzotriazole, 2-(3'-t-butyl-2'-hydroxy-5'-(2-octyloxycarbonylethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-t-butyl-5'-[2-(2-ethylhexyloxy)-carbonylethyl]-2'-hydroxyphenyl)-5-chloro-benzotriazole, 2-(3'-t-butyl-2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)-5-chloro-benzotriazole, 2-(3'-t-butyl-2'-hydroxy-5'-(2-methoxycarbonylethyl)phenyl)benzotriazole, Examples of the benzotriazole include 2-(3'-t-butyl-2'-hydroxy-5'-(2-octyloxycarbonylethyl)phenyl)benzotriazole, 2-(3'-t-butyl-5'-[2-(2-ethylhexyloxy)carbonylethyl]-2'-hydroxyphenyl)benzotriazole, 2-(3'-dodecyl-2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(3'-t-butyl-2'-hydroxy-5'-(2-isooctyloxycarbonylethyl)phenyl)benzotriazole, and 2,2'-methylene-bis[4-(1,1,3,3-tetramethylbutyl)-6-benzotriazol-2-ylphenol].

[0072] Among these, 2-(2'-hydroxy-5'-methylphenyl)benzotriazole or 2-(2'-hydroxy-3'-t-butyl-5'-methylphenyl)-5-chlorobenzotriazole is preferred as a compound having a benzotriazole structure in terms of better effects of the present invention.

[0073] The compound having a benzotriazole structure may be used alone or in combination of two or more kinds.

[0074] The content of the compound having a benzotriazole structure in the specific microcapsules is not particularly limited, but in terms of providing better effects of the present invention, it is preferably 10% by mass or more, more preferably 20% by mass or more, and even more preferably 30% by mass or more, relative to the content of the color former. The upper limit is not particularly limited, but from the viewpoint of the solubility of the compound having a benzotriazole structure, it is preferably 500% by mass or less, more preferably 300% by mass or less, and even more preferably 100% by mass or less.

[0075] As the ultraviolet absorbing agent, an ultraviolet absorbing agent other than a compound having a benzotriazole structure may be used. The content of the ultraviolet absorber other than the compound having a benzotriazole structure is preferably from 0 to 50 mass %, more preferably from 0 to 25 mass %, based on the total mass of the compound having a benzotriazole structure.

[0076] The specific microcapsules preferably contain substantially no color developer. By "substantially no color developer" is meant that the content of the color developer is 1% by mass or less relative to the total mass of the core material of the specific microcapsules.

[0077] (Method of manufacturing specific microcapsules) The method for producing the specific microcapsule is not particularly limited, and includes a method having a step of forming the specific microcapsule using the color former, the aromatic solvent, and the capsule wall material.Specific examples of the method include known methods such as interfacial polymerization, internal polymerization, phase separation, external polymerization, and coacervation.Among them, the interfacial polymerization is preferred. Hereinafter, the interfacial polymerization method will be described as an example of a method for producing specific microcapsules whose capsule walls are polyurea or polyurethane urea. The interfacial polymerization method preferably includes a step of dispersing an oil phase containing a color former, an aromatic solvent, and a capsule wall material (e.g., a raw material containing at least one selected from the group consisting of a polyisocyanate, a polyol, and a polyamine. Note that, when a polyamine is produced in the system by reacting a polyisocyanate with water, the polyol and the polyamine do not have to be used.) into an aqueous phase containing an emulsifier to prepare an emulsion (emulsification step), and a step of polymerizing the capsule wall material at the interface between the oil phase and the aqueous phase to form a capsule wall and form a specific microcapsule containing a color former (encapsulation step). The mass ratio of the total amount of polyol and polyamine to the amount of polyisocyanate in the above raw materials (total amount of polyol and polyamine / amount of polyisocyanate) is not particularly limited, but is preferably 0.1 / 99.9 to 30 / 70, and more preferably 1 / 99 to 25 / 75.

[0078] The type of emulsifier used in the emulsification step is not particularly limited, and examples thereof include dispersants and surfactants. The dispersant may be, for example, a resin such as polyvinyl alcohol.

[0079] The number average wall thickness of the specific microcapsules is not particularly limited, and is preferably, for example, 10 to 1000 nm. The wall thickness of a specific microcapsule refers to the thickness (μm) of the capsule wall that forms the capsule particle of the specific microcapsule, and the number average wall thickness refers to the average value obtained by averaging the individual capsule wall thicknesses (μm) of five specific microcapsules measured using a scanning electron microscope (SEM).

[0080] Specifically, the number average wall thickness of a specific microcapsule is measured by the following method. First, the coating solution is applied onto an arbitrary support to form a coating film. A cross-sectional slice of the obtained coating film is formed, and the formed cross-section is observed using an SEM to arbitrarily select five specific microcapsules. The cross-sections of the selected individual specific microcapsules are observed, and the thickness of the capsule wall is measured to calculate the average value.

[0081] The wall thickness (capsule wall thickness) of the specific microcapsule is governed by the relationship between the capsule wall and inclusions and the particle size of the specific microcapsule, as represented by the formula below, and can be adjusted by the particle size of the specific microcapsule (average primary particle size), the density of the capsule wall (wall density), the amount of solute, solvent and auxiliary solvent encapsulated in the specific microcapsule, the density of the solute, solvent and auxiliary solvent encapsulated in the specific microcapsule, and the amount of wall material (wall material amount), etc. Specifically, for example, the capsule wall can be adjusted to be thin by increasing the amount of solute, solvent, and co-solvent (i.e., the encapsulated substances) encapsulated in a particular microcapsule.

[0082]

number

[0083] The specific microcapsules may be used alone or in combination of two or more types. The content of the specific microcapsules in the coating liquid of the present invention is preferably from 10 to 70% by mass, more preferably from 20 to 50% by mass, and even more preferably from 20 to 45% by mass, based on the total solid content of the coating liquid.

[0084] The contents of the specific macrocapsules, the color developer, and the resin in the coating liquid can be identified, for example, by subjecting the coating liquid to a centrifugation process to separate the components, and then using various measuring devices.

[0085] [Other microcapsules] The coating liquid of the present invention may contain other microcapsules (hereinafter also referred to as "other microcapsules") other than the specific microcapsules, within the scope that does not impair the effects of the present invention. The other microcapsules are not particularly limited, but include macrocapsules that do not encapsulate an aromatic solvent, and microcapsules that do not encapsulate a color former. Of the macrocapsules contained in the coating liquid of the present invention (meaning the specific microcapsules and all other microcapsules that may be optionally contained), the content of the specific microcapsules is preferably 85 to 100 mass% relative to the total mass of the microcapsules, more preferably 95 to 100 mass%, even more preferably 98 to 100 mass%, particularly preferably 99 to 100 mass%, and most preferably 100 mass%.

[0086] [Average particle size and particle size distribution of microcapsules contained in the coating solution of the present invention] Next, preferred embodiments of the average particle size and particle size distribution of the microcapsules contained in the coating solution of the present invention (note that the term "microcapsules" used here refers to specific microcapsules and all other microcapsules that may be optionally contained) will be described. The average particle size of the microcapsules contained in the coating solution of the present invention is not particularly limited, but the volume-based median diameter (D50) is preferably 1 μm or more, more preferably 5 μm or more, and from the viewpoint of the superior effect of the present invention, it is even more preferably 10 μm or more, and particularly preferably 15 μm or more. The upper limit is preferably 200 μm or less, more preferably less than 100 μm, even more preferably 80 μm or less, and particularly preferably 50 μm or less. The volume-based median diameter (D50) of a microcapsule refers to the diameter at which the total volume of particles on the larger and smaller diameter sides is equal when the entire microcapsule is divided into two parts with a threshold particle diameter at which the cumulative volume is 50%.

[0087] The particle size distribution of the microcapsules contained in the coating solution of the present invention is preferably, for example, 10% or more, more preferably 15% or more, and even more preferably 20% or more, in terms of better effects of the present invention. The upper limit is not particularly limited, and is preferably 40% or less.

[0088] The volume-based median diameter and particle size distribution of the microcapsules can be controlled by adjusting the production conditions of the microcapsules.

[0089] The volume-based particle size distribution and median diameter (D50) of the microcapsules contained in the coating solution of the present invention can be measured by using a laser diffraction / scattering type particle size distribution measuring device (device: for example, Microtrac MT3300EXII (manufactured by Nikkiso Co., Ltd.)) for the microcapsules dispersed in the solution.

[0090] When measuring the volume-based median diameter (D50) of the microcapsules contained in the coating solution of the present invention in a coated state, the surface of the coating film is photographed at 150x magnification using an optical microscope, and the sizes of all microcapsules within a randomly set area of ​​2 cm x 2 cm are measured, whereby the size can be calculated.

[0091] [Developer] The coating liquid of the present invention contains a color developer. The "color developer" referred to here is a color developer that exists outside the microcapsules (in other words, that is not encapsulated in the microcapsules). That is, the coating liquid of the present invention contains the specific microcapsules, and may further contain microcapsules other than the specific microcapsules, but the "color developer" referred to here is a color developer that exists outside the microcapsules without being encapsulated in any of the microcapsules. A color developer is a compound that does not have a color-developing function by itself, but has the property of causing a color former to develop color when it comes into contact with the color former. As the color developer, an electron-accepting compound is preferable. Examples of the electron-accepting compound include clay substances such as activated clay, acid clay, attapulgite, zeolite, bentonite, and kaolin, phenolic compounds, zinc salicylate derivatives, and hydroxybenzoic acid esters. Specific examples of electron-accepting compounds include 2,2-bis(4-hydroxyphenyl)propane (also known as bisphenol A), 2,2-bis(4-hydroxyphenyl)hexafluoropropane (also known as bisphenol AF), 2,2-bis(p-hydroxyphenyl)pentane, 2,2-bis(p-hydroxyphenyl)ethane, 2,2-bis(p-hydroxyphenyl)butane, 2,2-bis(4'-hydroxy-3',5'-dichlorophenyl)propane, 1,1-(p-hydroxyphenyl)cyclohexane ... Examples of suitable electron-accepting compounds include 1,1-(p-hydroxyphenyl)propane, 1,1-(p-hydroxyphenyl)pentane, 1,1-(p-hydroxyphenyl)-2-ethylhexane, 3,5-bis(α-methylbenzyl)salicylic acid and its polyvalent metal salts, 3,5-di(tert-butyl)salicylic acid and its polyvalent metal salts, 3-α,α-dimethylbenzylsalicylic acid and its polyvalent metal salts, butyl p-hydroxybenzoate, benzyl p-hydroxybenzoate, 2-ethylhexyl p-hydroxybenzoate, p-phenylphenol, and p-cumylphenol. In addition, compounds represented by the general formula (1) described in paragraphs 0051 to 0060 of International Publication No. 2018 / 199044A1 can also be used as electron-accepting compounds.

[0092] As the electron accepting compound, in terms of the superior effect of the present invention, at least one selected from the group consisting of activated clay, acid clay, kaolin, a phenolic compound (e.g., a bisphenolic compound), a zinc salicylate derivative, and a hydroxybenzoic acid ester is preferable, at least one selected from the group consisting of activated clay, acid clay, and a zinc salicylate derivative is more preferable, and zinc 3,5-bis(α-methylbenzyl)salicylate is even more preferable.

[0093] When the electron-accepting compound is a particulate material, its shape is not particularly limited and may be, for example, any shape such as a sphere, an ellipse, a cube, a needle, an irregular shape, etc. The same applies when the electron-accepting compound particle is an aggregate of a plurality of particles.

[0094] The color developer may be used alone or in combination of two or more kinds. The developer may be surface-modified with a dispersing agent such as sodium hexametaphosphate. The content of the developer in the coating liquid of the present invention (when the developer is surface-modified with a dispersant, this means the content of the developer after surface modification; in other words, the content of the developer surface-modified with a dispersant) is not particularly limited, but is preferably 20 to 90 mass %, and more preferably 50 to 80 mass %, based on the total solid content of the coating liquid.

[0095] In the coating solution of the present invention, the mass content ratio (specific microcapsules / developer) of the specific microcapsules to the color developer (in the case where the color developer has been surface-modified with a dispersant, the color developer after surface modification) is preferably 1 / 9 to 9 / 1, more preferably 2 / 8 to 8 / 2, even more preferably 3 / 7 to 7 / 3, and particularly preferably 3 / 7 to 5 / 5, in terms of superior effects of the present invention.

[0096] In the coating of the present invention, the total content of the specific microcapsules and the color developer is preferably 50% by mass or more based on the total solid content of the coating solution. The upper limit is not particularly limited, but is preferably 99.5% by mass or less.

[0097] 〔resin〕 The coating liquid of the present invention contains a resin, which functions as a resin binder that supports the specific microcapsules and the color developer. The above-mentioned resins include not only resins that can be added during preparation of the coating liquid of the present invention, but also resins that are brought into the coating liquid from raw material components, such as emulsifiers such as polyvinyl alcohol used during the production of a specific microcapsule dispersion liquid and dispersants such as polyvinyl alcohol used during the production of a developer dispersion liquid. The type of resin is not particularly limited, and examples thereof include synthetic polymers and natural polymers such as styrene-butadiene copolymers, polyvinyl acetate, polyacrylic acid esters, polyvinyl alcohol, polyacrylic acid, maleic anhydride-styrene copolymers, olefin resins, modified acrylic acid ester copolymers, starch, casein, gum arabic, gelatin, carboxymethylcellulose or a salt thereof, and methylcellulose.

[0098] The resin content in the coating solution of the present invention is 17% by mass or less, and from the viewpoint of obtaining a better effect of the present invention, it is preferably 13% by mass or less. The lower limit of the resin content is not particularly limited, but is preferably 0.5% by mass or more, and more preferably 1% by mass or more, based on the total solid content of the coating solution.

[0099] The weight average molecular weight of the resin is not particularly limited, but is preferably 1,000 to 1,000,000.

[0100] 〔solvent〕 The coating liquid of the present invention contains a solvent. The "solvent" referred to here is a solvent that exists outside the microcapsules (in other words, that is not encapsulated in the microcapsules). That is, the coating liquid of the present invention contains the specific microcapsules, and may further contain other microcapsules other than the specific microcapsules, but the "solvent" referred to here is a solvent that exists outside the microcapsules without being encapsulated in any of the microcapsules. The solvent is not particularly limited as long as it can disperse the microcapsules and dissolve or disperse the color developer. Among these, solvents that do not swell the capsule walls of the specific microcapsules and do not cause the capsule contents (core material) to ooze or be released from within the capsules are preferred, and solvents that do not have an aromatic group are more preferred. Specific examples of the solvent include water (pure water, distilled water, ion-exchanged water, etc. can be used, and distilled water is preferred from the viewpoint of stability over time), ketone-based solvents such as methyl ethyl ketone, and ester-based solvents such as ethyl acetate.

[0101] The content of the solvent in the coating liquid of the present invention is preferably 10 to 90% by mass, more preferably 20 to 80% by mass, and even more preferably 20 to 70% by mass, based on the total mass of the coating liquid. When the coating solution of the present invention contains water, the content of water is preferably 50% by mass or more, more preferably 70% by mass or more, based on the total mass of the solvent. The upper limit is not particularly limited, but is preferably 100% by mass or less, more preferably 99.5% by mass or less, and even more preferably 98% by mass or less.

[0102] [Other ingredients] The coating liquid of the present invention may contain other components in addition to the above-mentioned components. Other components are not particularly limited, but include thickeners, dyes, surfactants, fluorescent brighteners, defoamers, penetrating agents, UV absorbers, pH adjusters, and preservatives.

[0103] In addition, when the coating liquid of the present invention contains a surfactant, the content of the surfactant is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less, based on the total solid content of the coating liquid. The lower limit is not particularly limited, but is, for example, 0.5% by mass or more. The surfactant is preferably a low molecular weight surfactant.

[0104] In addition, the coating liquid of the present invention preferably contains substantially no inorganic particles other than the color developer (e.g., pigments such as talc and titanium dioxide, silica particles, heavy calcium carbonate, and light calcium carbonate) in order to provide superior coating properties on non-flat surfaces and / or superior suitability for spray coating. "Substantially does not contain inorganic particles other than the color developer" means that the content of inorganic particles other than the color developer is 3% by mass or less, preferably 1% by mass or less, more preferably 0.5% by mass or less, and even more preferably 0% by mass, based on the total solid content of the coating liquid.

[0105] [Method of producing coating liquid] The method for producing the coating liquid of the present invention is not particularly limited, but it is preferable to produce the coating liquid by mixing a microcapsule dispersion liquid containing specific microcapsules, a dispersion liquid containing a color developer, and optional components added as necessary. The coating liquid of the present invention essentially contains a resin. The resin may be contained in the microcapsule dispersion and / or the dispersion containing a developer, or may be further added when the microcapsule dispersion and the dispersion containing a developer are mixed. In addition, the coating liquid of the present invention essentially contains a solvent, and the solvent may be a solvent contained in the microcapsule dispersion and the dispersion containing a developer, or may be further added when the microcapsule dispersion and the dispersion containing a developer are mixed.

[0106] The upper limit of the viscosity of the coating solution of the present invention at 25°C is not particularly limited, but is preferably 100,000 mPa·s or less in terms of ensuring coatability, and more preferably less than 5,000 mPa·s, even more preferably 3,000 mPa·s or less, particularly preferably 2,000 mPa·s or less, and most preferably 1,000 mPa·s or less in terms of achieving superior effects of the present invention. The lower limit is preferably 0.1 mPa·s or more, more preferably 0.5 mPa·s or more, and even more preferably 1 mPa·s or more. In this specification, the term "viscosity" refers to a value measured by an E-type viscometer at 25° C. As the E-type viscometer, for example, a VISCOSITY METER TVB-10H (manufactured by Toki Sangyo Co., Ltd.) can be used. The viscosity of the coating liquid of the present invention can be adjusted, for example, by changing the type and content of each component contained in the coating liquid of the present invention.

[0107] The coating liquid of the present invention is preferably substantially free of coarse particles, in terms of excellent coatability on non-flat surfaces and / or excellent suitability for spray coating. An embodiment of such a coating liquid may be one in which the volume-based median diameter (D50) of the microcapsules contained in the coating liquid is 1 to 50 μm, and the developer is an organic compound (the organic compound is preferably a metal salt of an aromatic carboxylic acid, more preferably a metal salicylate derivative, and even more preferably a zinc salicylate derivative).

[0108] [Uses of the coating solution of the present invention] By using the coating liquid of the present invention, it is possible to measure the pressure or pressure distribution on the non-flat surface of an article having a non-flat surface. A pressure measuring method using the coating liquid of the present invention will be described below. A pressure measurement method using the coating liquid of the present invention preferably includes a step of applying the coating liquid of the present invention to a measurement surface of an object to be measured for pressure or pressure distribution to form a coating film (pressure measurement layer), and a step of applying pressure to the obtained pressure measurement layer (pressure measurement step). When pressure is applied to the pressure measurement layer, the specific microcapsules are broken, and the color former contained in the specific microcapsules comes out of the specific microcapsules and a color reaction proceeds between the color former and the color developer. As a result, color development proceeds in the pressurized area.

[0109] As described above, the coating liquid of the present invention can be applied to measurement objects having surface shapes other than flat surfaces. The shape of the measurement surface of the measurement object is not particularly limited, and examples thereof include a flat surface, a curved surface, and an uneven surface. The measurement surface for pressure measurement may be a part or the entire surface of the measurement object. The object to be measured preferably includes a non-flat portion such as a curved surface or an uneven surface, and more preferably, a part or the whole of the measurement surface includes a non-flat portion.

[0110] The method for applying the coating liquid of the present invention is not particularly limited, and examples thereof include roller coating, spray coating, brush coating, and dip coating. When applying the coating liquid of the present invention, the coating liquid of the present invention may be applied directly to the measurement surface of the object to be measured, or an intermediate object (e.g., a film, paper, etc.) may be placed on the measurement surface of the object to be measured, and the coating liquid of the present invention may be applied onto the intermediate object. The coating amount of the coating solution of the present invention can be set depending on the purpose of measurement. However, in terms of obtaining good color development and color distribution, it is preferably, for example, 2 to 40 g / m in terms of solid content. 2 It is preferable that the thickness is 2 to 30 g / m 2 More preferably, the thickness is 2 to 20 g / m 2 More preferably, the thickness is 2 to 15 g / m 2 It is particularly preferable that:

[0111] In addition, the coating liquid of the present invention may be dried by heat treatment after being applied to the measurement surface of the measurement object. The drying temperature is not particularly limited, but is preferably, for example, 40 to 120° C. In addition, the drying time is not particularly limited, but is preferably, for example, 5 to 600 seconds.

[0112] When pressure is applied to the pressure measurement layer, the pressure may be any of a point pressure, a line pressure, and a surface pressure. The pressure range measurable by the pressure measurement layer is not particularly limited, but is preferably, for example, 300 MPa or less, and more preferably 0.1 to 300 MPa. When a pressure of 300 MPa or less is applied to the pressure measurement layer, the pressure measurement layer exhibits a property in which the color density increases with increasing pressure (in other words, color gradation). The color gradation of the pressure measurement layer is preferably a property in which the color density increases with increasing pressure. The pressure range measurable by the pressure measurement layer can be appropriately set depending on the measurement application. The measurable pressure range can be adjusted, for example, by controlling the particle size, wall thickness, and constituent material of the specific microcapsule, as well as the coating amount of the coating liquid of the present invention. The color development (color development density) and gradation of the color development portion generated in the pressurized area of ​​the pressure measurement layer can be measured using a reflection densitometer (for example, RD-19I manufactured by Gregg Macbeth) or the like.

[0113] The measurement object is not particularly limited as long as it has a shape that allows measurement of pressure or pressure distribution. Specific examples include various molding dies including press dies, vacuum molding dies, and injection molding dies.

[0114] Applications to which the coating liquid of the present invention can be applied are not particularly limited, and examples thereof include confirmation of pressure distribution in the molding of various components, bodies, etc., and assembly of components in the manufacture of vehicles such as automobiles and aircraft; confirmation of pressure distribution in the assembly of building materials; confirmation of pressure distribution in the curved surface processing of electronic products (such as lamination of curved displays); confirmation of impact force applied to cargo during transportation; confirmation of die contact in the manufacture of metal products; confirmation of die contact during molding of resin products; confirmation of pressure distribution in tableting of pharmaceuticals; confirmation of pressure distribution on furniture surfaces such as chairs and sofa seats; confirmation of stationery pressure, such as confirmation of grip force applied to writing instruments, etc.; confirmation of impact force applied to sporting goods such as balls made of elastic material; confirmation of gaps (clearance) between upper and lower teeth in dental products, etc.

[0115] Furthermore, pressure measurement using the coating liquid of the present invention is also suitable for applications such as checking the contact with a die in metal processing and checking the pressure distribution when laminating a curved display.

[0116] [Items containing non-flat surfaces with pressure measurement layers] The present invention further relates to an article including a non-flat portion with a pressure measurement layer. The article including a non-flat portion with a pressure measurement layer of the present invention comprises an article including a non-flat portion, and a pressure measurement layer formed using Coating Liquid A and disposed on the non-flat portion.

[0117] The article containing a non-flat portion with a pressure measurement layer of the present invention can be formed by the pressure measurement method using the above-mentioned coating liquid of the present invention (Coating Liquid A). That is, the article containing a non-flat portion with a pressure measurement layer of the present invention corresponds to a laminate obtained by forming a pressure measurement layer on the non-flat portion of an article that is a measurement target having non-flat portions such as curved and uneven surfaces on a part or all of its measurement surface in the pressure measurement method using the above-mentioned coating liquid of the present invention (Coating Liquid A). The measurement object may be an article having a shape that allows measurement of pressure or pressure distribution, and specific examples of the article are as described above.

[0118] 3 and 4 show a specific example of an article including a non-flat portion with a pressure measurement layer.

[0119] The non-flat portion-containing article 31 with a pressure measurement layer shown in Fig. 3 includes an article 30 including a non-flat portion, and a pressure measurement layer 33 disposed on the non-flat portion of the article 30 including a non-flat portion. The pressure measurement layer 33 includes specific microcapsules 34, a color developer 35, and a film 32 formed of a resin binder that holds and supports the specific microcapsules 34 and the color developer 35 on the article 30 including a non-flat portion. In the pressure measurement layer 33, one region of the specific microcapsules 34 completely protrudes from the film 32. In the pressure measurement layer 33, the particle diameter D31 of the specific microcapsules 34 is larger than the thickness D32 of the film 32.

[0120] The non-flat portion-containing article 41 with a pressure measurement layer shown in FIG. 4 has an article 40 including a non-flat portion and a pressure measurement layer 43 arranged on the non-flat portion of the article 40 including a non-flat portion. The pressure measurement layer 43 includes a specific microcapsule 44, a color developer 45, a film 42 formed of a resin binder that holds and supports the specific microcapsule 44 and the color developer 45 on the article 40 including a non-flat portion, and a coating 46 formed of the same resin binder as the film 42. In the pressure measurement layer 43, a region of the specific microcapsule 44 protrudes from the film 42, and the surface of the region of the specific microcapsule 44 protruding from the film 42 (a region of the surface or the entire surface) is covered with a coating 46 that is a thin film of the resin binder. In the pressure measurement layer 43, the particle diameter D41 of the specific microcapsule 44 is larger than the thickness D42 of the film 42.

[0121] [Manufacturing method of pressure measurement layer] The invention also relates to a method for manufacturing the pressure measuring layer. The method for producing a pressure measurement layer of the present invention includes a step of applying a coating liquid for forming a pressure measurement layer (hereinafter, also simply referred to as a "coating liquid" or "coating liquid B") to a non-flat portion of an article including a non-flat portion to form a pressure measurement layer, the pressure-measuring layer-forming coating liquid contains microcapsules containing a color former and an aromatic solvent (hereinafter also referred to as "specific microcapsules"), a color developer not contained in the microcapsules (hereinafter also simply referred to as "color developer"), a resin, and a solvent; The average particle size of the specific microcapsules is X μm, and the coating amount of the solid content of the coating solution for forming the pressure measurement layer is Y g / m 2 When the average particle size is expressed as Y / X, the solid coating amount is Yg / m 2 The ratio is less than 1.

[0122] When pressure is applied to the pressure measurement layer formed by the method of manufacturing the pressure measurement layer of the present invention, the specific microcapsules are broken, and the color former contained in the specific microcapsules comes out of the specific microcapsules and a color development reaction proceeds between the color former and the color developer. As a result, color development proceeds in the pressurized area.

[0123] The method for producing a pressure measurement layer of the present invention having the above-mentioned configuration can be applied to measuring pressure or pressure distribution in a non-flat portion of an article having a non-flat portion. Furthermore, the pressure measurement layer obtained by the method for producing a pressure measurement layer of the present invention has excellent gradation in the color-developing portion even when pressurized in a low pressure range (for example, 300 MPa or less).

[0124] Although the mechanism of action of the above-mentioned configuration and effect is not clear, the present inventors speculate as follows. The main feature of the method for producing a pressure measurement layer of the present invention is to use the above-mentioned pressure measurement layer forming coating liquid (coating liquid B) to set the average particle size of the specific microcapsules to X μm and the solid coating amount of coating liquid B to Y g / m 2 When the average particle size is expressed as Y / X, the solid coating amount is Yg / m 2 The pressure measurement layer is formed on the non-flat portion of the article including the non-flat portion so that the ratio of the specific microcapsules to the color developer is less than 1. Coating liquid B further contains a resin in addition to the specific microcapsules and the color developer. It is considered that the resin functions as a resin binder that supports the specific microcapsules and the color developer in the pressure measurement layer formed from coating liquid B. In this study, the inventors have determined that the average particle size of the specific microcapsules is X μm and the coating amount of the solid content of the coating solution B is Y g / m 2 It has been clarified that by forming the pressure measurement layer so that Y / X is less than 1, the resulting pressure measurement layer has a configuration in which the specific microcapsules are not embedded in the resin binder (specifically, the configuration is as shown in the above-mentioned Figs. 1 and 2). It is presumed that the specific microcapsules in such a pressure measurement layer are easily destroyed when pressurized, and as a result, good color development (color development density) and gradation are easily obtained even when pressurized at a low pressure range (for example, 300 MPa or less). Furthermore, as described above, the method for producing a pressure measurement layer of the present invention can be applied to the measurement of pressure or pressure distribution in a non-flat portion of an article having a non-flat portion. That is, even for a measurement object that is difficult to measure in the form of a conventional film, sheet, etc., a pressure measurement layer can be formed with a coating amount per unit area that is normally used for pressure measurement, regardless of the surface shape of the object.

[0125] In the following description, when one or more of color density, gradation, and image quality of the pressure measurement layer formed by the method for producing a pressure measurement layer of the present invention are superior, this is also referred to as "the effect of the present invention being superior."

[0126] [Coating liquid for forming pressure measurement layer (Coating liquid B)] The coating liquid for forming a pressure measurement layer (coating liquid B) used in the manufacturing method of a pressure measurement layer of the present invention contains microcapsules (specific microcapsules) encapsulating a color former and an aromatic solvent, a color developer (color developer) that is not encapsulated in the microcapsules, a resin, and a solvent. Coating liquid B used in the method for producing a pressure measurement layer of the present invention is the same as the above-mentioned coating liquid for forming a pressure measurement layer of the present invention (coating liquid A) except for the resin content, and the preferred embodiments are also the same.

[0127] In the coating solution used in the method for producing the pressure measurement layer of the present invention, the resin content is preferably 30% by mass or less based on the total solid content, and is preferably 17% by mass or less, more preferably 13% by mass or less, in that the specific microcapsules protrude more from the membrane in the pressure measurement layer formed, thereby making the effect of the present invention more excellent. The lower limit of the resin content is not particularly limited, but is preferably 1% by mass or more, more preferably 3% by mass or more.

[0128] In the manufacturing method of the pressure measurement layer of the present invention, the measurement object is a measurement object having a surface shape other than a flat surface. Specifically, the measurement object may have a measurement surface such as a curved surface or an uneven surface. The measurement surface for pressure measurement may be a part or the entire surface of the measurement object.

[0129] In the method for producing a pressure measurement layer of the present invention, the method for applying the coating liquid B is not particularly limited, and examples thereof include roller application, spray application, brush application, and dip coating. When applying the coating liquid B, the coating liquid B may be applied directly to the measurement surface of the object to be measured, or an intermediate object (e.g., a film, a paper, etc.) may be placed on the measurement surface of the object to be measured, and the coating liquid B may be applied onto the intermediate object.

[0130] The coating amount of coating solution B is expressed as follows: the average particle size of the specific microcapsules is X μm, and the coating amount of the solid content of coating solution B is Y g / m 2 When the average particle size is expressed as Y / X, the solid coating amount is Yg / m 2 (hereinafter abbreviated as "Y / X") is less than 1. In other words, when the average particle size of the specific microcapsules is 3 μm, the coating amount of solids is 3 g / m 2 When the coating amount of the coating liquid B and the average particle size of the specific microcapsules satisfy the above relationship, a pressure measurement layer having a configuration as shown in Figs. In order to obtain a more excellent effect of the present invention, it is preferable that the average particle size (X) of the specific microcapsules is 1 to 100 μm and Y / X is 0.8 or less, and it is more preferable that the average particle size (X) of the specific microcapsules is 3 to 50 μm and Y / X is 0.6 or less. In order to obtain a more excellent color density of the colored portion generated in the pressurized region of the pressure measurement layer, it is preferable that Y / X is 0.1 or more.

[0131] In addition, after being applied to the measurement surface of the measurement object, the coating liquid B may be dried by a heat treatment. The drying temperature is not particularly limited, but is preferably, for example, 40 to 120° C. In addition, the drying time is not particularly limited, but is preferably, for example, 5 to 600 seconds.

[0132] When pressure is applied to the pressure measurement layer, the pressure may be any of a point pressure, a line pressure, and a surface pressure. The pressure range measurable by the pressure measurement layer is not particularly limited, but is preferably, for example, 300 MPa or less, more preferably 100 MPa or less, and even more preferably 1 to 100 MPa. When a pressure of 300 MPa or less is applied to the pressure measurement layer, the pressure measurement layer exhibits a property in which the color density increases with increasing pressure (in other words, color gradation). The color gradation of the pressure measurement layer is preferably a property in which the color density increases with increasing pressure. The pressure range measurable by the pressure measurement layer can be appropriately set depending on the measurement application. The measurable pressure range can be adjusted, for example, by controlling the particle size, wall thickness, and constituent material of the specific microcapsules, as well as the amount of coating liquid B applied. The color development (color development density) and gradation of the color development portion generated in the pressurized area of ​​the pressure measurement layer can be measured using a reflection densitometer (for example, RD-19I manufactured by Gregg Macbeth) or the like.

[0133] The article to be measured is not particularly limited as long as it has a non-flat portion in at least one region of the measurement surface, and specific examples include various molding dies including press dies, vacuum molding dies, and injection molding dies.

[0134] There are no particular limitations on the applications to which the method for producing a pressure measurement layer of the present invention can be applied, and examples of the applications include the various applications exemplified above as applications to which the coating liquid A can be applied.

[0135] The method for producing a pressure measurement layer of the present invention is also suitable for applications such as checking the contact of a die in metal processing and checking the pressure distribution when bonding a curved display.

[0136] [Items containing non-flat surfaces with pressure measurement layers] The present invention further relates to an article including a non-flat portion with a pressure measurement layer. The article having a non-flat portion with a pressure measurement layer of the present invention is a laminate formed by the above-mentioned method for producing a pressure measurement layer of the present invention. That is, it corresponds to a laminate in which a pressure measurement layer is formed on the non-flat portion of an article that is a measurement target having a non-flat portion such as a curved surface and an uneven surface on a part or all of the measurement surface. Specific examples of the article having a non-flat portion with a pressure measurement layer include the article having a non-flat portion with a pressure measurement layer 31 shown in FIG. 3 and the article having a non-flat portion with a pressure measurement layer 41 shown in FIG. 4. EXAMPLES

[0137] The present invention will be described in more detail below based on examples. The materials, amounts used, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples. In the following, "parts" and "%" are based on mass unless otherwise specified.

[0138] [Example 1] [Preparation of color former-encapsulating microcapsule dispersion 1] 50 parts of a mixture of 1,2-dimethyl-4-(1-phenylethyl)benzene, 1,3-dimethyl-4-(1-phenylethyl)benzene, 1,4-dimethyl-2-(1-phenylethyl)benzene, and 1-(ethylphenyl)-1-phenylethane (manufactured by Yantai Jinzheng Precision Chemical Co., Ltd., SRS-101) were dissolved with 3 parts of 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindole-1,9'-xanthene]-3-one (manufactured by Hodogaya Chemical Co., Ltd., Pink-DCF) as a color developer, 4 parts of 6'-(diethylamino)-1',3'-dimethylfluoran (manufactured by Hodogaya Chemical Co., Ltd., Orange-DCF), and 3 parts of 2-(2'-hydroxy-5'-methylphenyl)benzotriazole (manufactured by Johoku Chemical Co., Ltd., JF-77-P) as an ultraviolet absorber to obtain solution A. Next, 13 parts of synthetic isoparaffin (IP Solvent 1620, manufactured by Idemitsu Kosan Co., Ltd.) and 0.3 parts of N,N,N',N'-tetrakis(2-hydroxypropyl)ethylenediamine (ADEKA Polyether EDP-300, manufactured by ADEKA Co., Ltd.) dissolved in 2.5 parts of methyl ethyl ketone were added to the stirred solution A to obtain solution B. Furthermore, 2.5 parts of a trimethylolpropane adduct of tolylene diisocyanate (Burnoc D-750, manufactured by DIC Co., Ltd., solid content 75% by mass, ethyl acetate solution) dissolved in 6 parts of ethyl acetate were added to the stirred solution B to obtain solution C. Then, the above solution C was added to a solution obtained by dissolving 7 parts of polyvinyl alcohol (PVA-217E, manufactured by Kuraray Co., Ltd.) in 140 parts of water, and emulsified and dispersed. 200 parts of water was added to the emulsion after emulsification and dispersion, and the mixture was heated to 70°C while stirring, stirred for 1 hour, and then cooled. Water was further added to adjust the concentration, to obtain a color former-encapsulating microcapsule dispersion with a solid content concentration of 20%. The average particle size of the obtained color former-encapsulating microcapsules was 20 μm. The average particle size and particle size distribution were measured by a laser light scattering method using a Microtrac MT3300EXII (manufactured by Nikkiso Co., Ltd.), with the average particle size being measured as the D50 value and the particle size distribution being measured as the CV value (both the average particle size and the particle size distribution are based on volume). With respect to the total solid content of the microcapsule dispersion, the content of the resin binder was 8.5% by mass, and the content of the microcapsules was 91.5% by mass. The contents of the resin binder and the microcapsules were determined by separating them by centrifugation until they were separated.

[0139] [Preparation of Color Developer Dispersion 1] 100 parts of activated clay (Mizusawa Chemicals, Silton F-242) as a developer, 0.5 parts of sodium hexametaphosphate (Nippon Chemical Industry, sodium hexametaphosphate), 15 parts of a 10% aqueous sodium hydroxide solution, and 240 parts of water were added to obtain a developer-containing dispersion.

[0140] A pressure measurement layer forming coating liquid 1 was prepared by mixing the color former-containing microcapsule dispersion liquid 1 and the color developer dispersion liquid 1. In the pressure measurement layer forming coating liquid 1 after mixing, the color former-containing microcapsule dispersion liquid 1 and the color developer dispersion liquid 1 were mixed at a mixing ratio of 50 mass % each.

[0141] 〔evaluation〕 <Preparation of pressure measurement layer> Coating solution 1 for forming a pressure measurement layer was sprayed onto a metal plate (concave mirror / convex mirror (R=100 mm) made of stainless steel (SUS304)) as the coating target, in the amount shown in Table 1. A similar metal plate was placed on top of the coated surface so as to cover the coated area, and pressure was applied at three points of 1 MPa, 5 MPa, and 10 MPa for 120 seconds using a press (product name: H1F35-1, manufactured by Komatsu Ltd.). After the pressing was completed, the metal plate placed on the coated surface was removed, and the color and color distribution of the coated area were visually confirmed and subjected to a sensory evaluation according to the following evaluation criteria.

[0142] <Color evaluation (density)> The color development state of the sample was visually inspected after applying a pressure of 5 MPa and evaluated according to the following criteria. "A": The color is developed at a sufficient intensity to be visible. "B": The color density is slightly low, but the color is developed to an extent that does not cause any problems in practical use. "C": No color development.

[0143] <Gradation> "AA": The difference of 3 points is clearly visible. "A": The difference of 3 points is visible. "B": The difference between 1 MPa and 5 MPa, or the difference between 5 MPa and 10 MPa, is visible. "C": The difference between 1 MPa and 5 MPa and the difference between 5 MPa and 10 MPa are not visible, but the difference between 1 MPa and 10 MPa is visible. "D": No visible difference.

[0144] <Color granularity (image quality)> After pressing, the colored surface state of the metal plate was visually observed and evaluated according to the following criteria. "A": The graininess in the colored areas is very small. "B": There is some graininess in the colored areas, but this does not cause any problems in practical use. "C": The graininess in the colored areas is clearly significant.

[0145] <Applyability evaluation> After coating, the metal plate was visually observed and evaluated according to the following criteria. "A": No visible unevenness in application (thickness). "B": Uneven application (thickness) is visible.

[0146] [Example 2] A pressure-measuring layer-forming coating solution 2 was prepared in the same manner as in Example 1, except that the developer dispersion solution 1 was changed to the developer dispersion solution 2, and the same evaluation as in Example 1 was carried out.

[0147] <Developer dispersion 2> 35 parts of 3,5-di-α-methylbenzyl zinc salicylate (substituted salicylic acid metal salt, developer), 7 parts of sodium hexametaphosphate, and 50 parts of water were dispersed using a sand grinder mill to prepare a dispersion liquid so that the average particle size was 2 μm. 10 parts of a 10% aqueous solution of polyvinyl alcohol (PVA-203, manufactured by Kuraray Co., Ltd.) were added to the dispersion liquid to prepare a developer dispersion liquid. The content of the developer was 98 mass% based on the total solid content of the developer dispersion liquid. The contents of the binder and developer were determined by separating them by centrifugation. Centrifugation was performed multiple times as necessary.

[0148] [Examples 3 to 14, 16 to 22 (Developer type: zinc salicylate)] As shown in Table 1, the coating liquids for forming the pressure measurement layer of Examples 3 to 14 and 16 to 22 (type of developer: zinc salicylate) were prepared according to the same procedure as in Example 2, except that various conditions such as each material and the content of each material were changed. In Examples 19 to 21, a resin binder dispersion was also used in addition to the microcapsule dispersion and the developer dispersion. In Example 22, a high viscosity solution was obtained by removing part of the water in the coating liquid for forming the pressure measurement layer by heating. The same evaluation as in Example 1 was carried out using the obtained pressure measurement layer forming coating liquid.

[0149] [Example 15 and Comparative Example 1 (Developer type: activated clay)] As shown in Table 1, the coating solutions for forming pressure measurement layers of Example 15 and Comparative Example 1 (type of developer: activated clay) were prepared according to the same procedure as in Example 1, except that various conditions such as each material and the content of each material were changed. The same evaluation as in Example 1 was carried out using the obtained pressure measurement layer forming coating liquid.

[0150] [Reference Example 1 (Developer type: activated clay)] A coating solution for forming a pressure measurement layer for Reference Example 1 (type of developer: activated clay) was prepared according to the same procedure as in Example 1, except that various conditions such as each material and the content of each material were changed as shown in Table 1. The same evaluation as in Example 1 was carried out using the obtained pressure measurement layer forming coating liquid.

[0151] [Example 23] A pressure-measuring layer-forming coating liquid was prepared in the same manner as in Example 1, except that the developer dispersion liquid 1 was changed to LR-220 (solid content concentration: 43%) manufactured by Sanko Co., Ltd. In the coating liquid for forming a pressure measurement layer prepared in Example 23, the resin content was 17 mass % or less based on the total solid content of the coating liquid for forming a pressure measurement layer. The obtained coating liquid for forming a pressure measurement layer was used to carry out the same evaluation as in Example 1. The results showed that the color development (density), gradation, color development granularity (image quality), and application properties were all rated A.

[0152] [Comparative Example 2] When a two-sheet type pressure measurement sheet set consisting of an electron-donating colorless dye sheet and a color developer sheet disclosed in Example 1 of JP 2009-019949 A was used to measure pressure against the uneven surface of the metal plate used in the above-mentioned [Example 1], the sheet did not conform to the uneven surface and measurement was not possible.

[0153] Table 1 is shown below. The various components shown in Table 1 are as follows: <Microcapsule composition> (Color former) Orange-DCF: 6'-(diethylamino)-1',3'-dimethylfluoran, manufactured by Hodogaya Chemical Co., Ltd. Pink-DCF: 3',6'-bis(diethylamino)-2-(4-nitrophenyl)spiro[isoindol-1,9'-xanthen]-3-one, manufactured by Hodogaya Chemical Co., Ltd. Color former A: 3,3-bis(2-methyl-1-octyl-3-indolyl)phthalide Coloring agent B: RED40, manufactured by Yamamoto Kasei Co., Ltd.

[0154] (Aromatic Solvents) SAS-296: 1,1-diphenylethane, manufactured by JXTG Nippon Oil & Energy Corporation SRS-101: A mixture of 1,2-dimethyl-4-(1-phenylethyl)benzene, 1,3-dimethyl-4-(1-phenylethyl)benzene, 1,4-dimethyl-2-(1-phenylethyl)benzene, and 1-(ethylphenyl)-1-phenylethane (manufactured by Yantai Jinzheng Fine Chemical Co., Ltd.) Alkene L: Linear alkylbenzene, manufactured by JXTG Nippon Oil & Energy Corporation

[0155] (Emulsifier (resin binder)) PVA (Polyvinyl alcohol): PVA-217E, manufactured by Kuraray Co., Ltd.

[0156] <Developer dispersion liquid> (Developer) Activated clay: Shilton F-242, manufactured by Mizusawa Industrial Chemicals Zinc salicylate: 3,5-bis(α-methylbenzyl) zinc salicylate, 43% solids aqueous dispersion, manufactured by Sanko Co., Ltd. (Dispersant (resin binder)) PVA (Polyvinyl alcohol): PVA-203, manufactured by Kuraray Co., Ltd.

[0157] <Resin binder (dispersion liquid)> (Resin binder) NPL: Modified acrylic ester copolymer (product name: Nipol LX814, manufactured by Zeon Corporation, aqueous dispersion with solid content of 47% by mass)

[0158] In the table, the values ​​in the "average particle size and particle size distribution of microcapsules" column are values ​​obtained by measuring the average particle size and particle size distribution of microcapsules in a microcapsule dispersion by a laser light scattering method using a Microtrac MT3300EXII (manufactured by Nikkiso Co., Ltd.) The average particle size was measured using the D50 value, and the particle size distribution was measured using the CV value (both the average particle size and particle size distribution are based on volume). The "viscosity" is a value measured at a temperature of 25°C using an E-type viscometer (VISCOSITY METER TVB-10H, manufactured by Toki Sangyo Co., Ltd.). In addition, in the table, the PVA (polyvinyl alcohol) resin listed in the "emulsifier (resin binder)" column, the PVA (polyvinyl alcohol) resin listed in the "dispersant (resin binder)" column, and the NPL (modified acrylic acid ester copolymer) resin listed in the "resin binder (dispersion liquid)" column correspond to the "resin" in the coating liquid of the present invention. In the table, "Pink-DCF" corresponds to the compound represented by general formula (1), and color former A corresponds to the compound having an indole structure. In the table, in the columns "microcapsule dispersion", "color developer dispersion", and "resin binder (dispersion)", "mixing ratio (liquid)" refers to the mixing ratio of each of the above dispersions. In the table, in the column "Total content of microcapsules and color developer relative to the total solids content of the coating liquid for forming the pressure measurement layer [mass %]", "P" indicates that the total content of microcapsules and color developer relative to the total solids content of the coating liquid for forming the pressure measurement layer is 50 mass % or more, and "N" indicates that the total content of microcapsules and color developer relative to the total solids content of the coating liquid for forming the pressure measurement layer is less than 50 mass %. In the table, the "Y / X" column indicates the solid coating amount Yg / m of the coating solution relative to the average microcapsule particle size Xμm. 2 "P" represents the case where the value of Y / X is less than 1, and "N" represents the case where the value of Y / X is 1 or more.

[0159] [Table 1]

[0160] As shown in Table 1, it was confirmed that the desired effects were obtained when the pressure measurement layer forming coating liquid of the present invention was used. It was also confirmed that the desired effects were obtained when the pressure measurement layer forming coating liquid of the present invention was used. Furthermore, by comparing Examples 1 to 7 with Example 8, it was confirmed that when the particle size distribution of the microcapsules is 15% or more (preferably 30% or more), the gradation of the color-developed portion is more excellent. In addition, by comparing Example 2 with Examples 9 to 14, it was confirmed that when the average particle size of the microcapsules is 10 μm or more, the color development and gradation of the color-developing portion are more excellent, and further, when the average particle size of the microcapsules is less than 100 μm, the image quality of the color-developing portion is more excellent. Furthermore, by comparing Example 2 with Example 18, it was confirmed that when the color former encapsulated in the microcapsules contains a compound represented by the above-mentioned general formula (1), the color development and gradation of the color-developing portion are superior. Furthermore, in comparison with Examples 19 to 21, it was confirmed that when the resin binder content relative to the total solid content of the coating liquid for forming the pressure measurement layer was 13 mass % or less, the color development and gradation of the color-developed portion were superior. Moreover, by comparing Example 2 with Example 22, it was confirmed that when the viscosity (25° C.) of the coating liquid for forming the pressure measurement layer is less than 5000 mPa·s, the application property is superior.

[0161] The coating liquid for forming a pressure measurement layer of the comparative example did not provide the desired effect. Also, the method of using the coating liquid for forming a pressure measurement layer of the comparative example did not provide the desired effect. [Explanation of symbols]

[0162] 10 Measurement object (object to be coated) 12, 32, 42 membrane 14, 34, 44 Specific microcapsules 15, 46 coating 35, 45 Developer 30, 40 Articles containing non-flat surfaces 31, 41 Articles containing non-flat surfaces with pressure measuring layers 33, 43 Pressure measurement layer D1 Particle size of specific microcapsules D2 Thickness of film 12 D31 Particle size of specific microcapsule 34 D32 Thickness of film 32 D41 Particle size of specific microcapsule 44 D42 Thickness of membrane 42

Claims

1. A coating liquid for forming a pressure measurement layer for forming a pressure measurement layer used for pressure measurement at a pressure of 10 MPa or less, A microcapsule containing a color former and an aromatic solvent; A developer that is not encapsulated in a microcapsule; Resin and a solvent; the content of the resin is 7.2% by mass or less with respect to the total solid content of the coating liquid for forming the pressure measurement layer, The coating liquid for forming a pressure measurement layer, wherein the average particle size of microcapsules contained in the coating liquid for forming a pressure measurement layer is 10 μm or more.

2. 2. The coating liquid for forming a pressure-measuring layer according to claim 1, which has a viscosity at 25°C of less than 5000 mPa·s.

3. 3. The coating liquid for forming a pressure-measuring layer according to claim 1, wherein the microcapsules encapsulating the color former and the aromatic solvent are substantially free of a color developer.

4. 4. The pressure-measuring layer-forming coating liquid according to claim 1, wherein the developer comprises a material selected from the group consisting of activated clay, acid clay, and zinc salicylate derivatives.

5. 5. The coating liquid for forming a pressure-measuring layer according to claim 4, wherein the developer is zinc 3,5-bis(α-methylbenzyl)salicylate.

6. 6. The coating liquid for forming a pressure measuring layer according to claim 1, wherein the particle size distribution of the microcapsules contained in the coating liquid for forming a pressure measuring layer is 15% or more.

7. The coating liquid for forming a pressure measurement layer according to any one of claims 1 to 6, wherein a total content of the microcapsules encapsulating the color former and the aromatic solvent, and the color developer is 50 mass% or more with respect to a total solid content of the coating liquid for forming a pressure measurement layer.

8. The coating liquid for forming a pressure measurement layer according to any one of claims 1 to 7, wherein the color former is selected from the group consisting of a compound represented by general formula (1) and a compound having an indole structure: 【Chemistry 1】 In the formula, R 1 and R 3 each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 2 and R 4 each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent. X 1 is -O- or -NR 5 - represents. 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

9. A method for producing a pressure measurement layer, comprising a step of applying a coating liquid for forming a pressure measurement layer to a non-flat surface of an article including the non-flat surface to form a pressure measurement layer, the pressure measurement layer forming coating liquid contains microcapsules encapsulating a color former and an aromatic solvent, a color developer not encapsulated in the microcapsules, a resin, and a solvent; the content of the resin is 17% by mass or less with respect to the total solid content of the coating liquid for forming the pressure measurement layer, The average particle size of the microcapsules encapsulating the color former and the aromatic solvent is X μm, and the coating amount of the solid content of the coating liquid for forming the pressure measurement layer is Y g / m 2 When the average particle diameter is expressed as Y / X, the solid coating amount is Yg / m 2 The method for manufacturing a pressure measurement layer, wherein the ratio is less than 1.

10. The method for producing a pressure measurement layer according to claim 9 , wherein the content of the resin is 13% by mass or less with respect to a total solid content of the coating liquid for forming the pressure measurement layer.

11. The method for producing a pressure measurement layer according to claim 9 or 10, wherein the pressure measurement layer forming coating liquid has a viscosity of less than 5000 mPa·s at 25°C.

12. The method for manufacturing a pressure measurement layer according to any one of claims 9 to 11, wherein the microcapsules encapsulating the color former and the aromatic solvent are substantially free of a color developer.

13. The method for producing a pressure measurement layer according to any one of claims 9 to 12, wherein the average particle size of the microcapsules contained in the coating liquid for forming the pressure measurement layer is 5 µm or more.

14. The method for manufacturing a pressure measurement layer according to any one of claims 9 to 13, wherein the color developer contains a material selected from the group consisting of activated clay, acid clay, and zinc salicylate derivatives.

15. The method for producing a pressure measurement layer according to any one of claims 9 to 14, wherein the developer is zinc 3,5-bis(α-methylbenzyl)salicylate.

16. The method for producing a pressure measurement layer according to any one of claims 9 to 15, wherein the particle size distribution of the microcapsules contained in the coating liquid for forming the pressure measurement layer is 15% or more.

17. The method for manufacturing a pressure measurement layer according to any one of claims 9 to 16, wherein the total content of the microcapsules encapsulating the color former and the aromatic solvent and the color developer is 50 mass% or more relative to the total solid content of the coating liquid for forming the pressure measurement layer.

18. The method for producing a pressure measurement layer according to any one of claims 9 to 17, wherein the color former is selected from the group consisting of a compound represented by general formula (1) and a compound having an indole structure: 【Chemistry 2】 In the formula, R 1 and R 3 each independently represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent. R 2 and R 4 each independently represents an alkyl group which may have a substituent or an aryl group which may have a substituent. X 1 is -O- or -NR 5 - represents. 5 represents a hydrogen atom, an alkyl group which may have a substituent, or an aryl group which may have a substituent.

19. A non-flat portion-containing article with a pressure measurement layer, comprising: an article including a non-flat portion; and a pressure measurement layer formed using the coating liquid for forming a pressure measurement layer according to any one of claims 1 to 8, the pressure measurement layer being disposed on the non-flat portion.

Citation Information

Patent Citations

  • Pressure-sensitive coloring resin material, pressure-sensitive member, and buffer material

    JP2007132756A

  • Impact indicator coatings and methods

    US20170029625A1

  • Pressure measuring material and pressure measuring material production method

    WO2020149410A1

  • Paste-like composition for pressure determination and pressure determination method

    WO2020195131A1