Photocurable material and image display device
A photocurable material with controlled refractive index differences addresses the visibility of knit lines in image display devices by using (meth)acrylic acid ester components and plasticizers, improving the visual appearance of image display devices.
Patent Information
- Application Number
- JP2021137824
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-26
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2041-08-26
AI Technical Summary
The visibility of knit lines between the dam and fill parts in the transparent resin layer of image display devices is a concern due to differences in refractive index and migration of low-molecular substances, which are not adequately addressed by existing technologies.
A photocurable material composed of (meth)acrylic acid ester components, plasticizers, and photopolymerization initiators is developed, with a refractive index difference of 0.02 or less between the photocured products, minimizing the visibility of knit lines.
The developed photocurable material effectively reduces the visibility of knit lines by ensuring a minimal refractive index difference, enhancing the aesthetic quality of image display devices.
Smart Images

Figure 0007578878000005 
Figure 0007578878000001 
Figure 0007578878000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocurable material and an image display device. [Background technology]
[0002] A general image display device has a structure in which a front panel and an image display panel are laminated via a transparent resin layer which is a cured product of a photocurable resin composition. This structure is usually produced by a method (so-called dam-fill method) in which a photocurable dam part is formed by applying a photocurable resin composition which functions as a dam agent to the outer edge of the image display panel, and then a photocurable fill part is formed by applying the same or a different photocurable resin composition which functions as a fill agent to the area surrounded by the photocurable dam part, and then the image display panel and the front panel are bonded together, and the photocurable dam part and the photocurable fill part are irradiated with ultraviolet light to photocur them, thereby forming a transparent resin layer (Patent Document 1).
[0003] In the dam and fill portions of the transparent resin layer of an image display device created using such a dam-fill method, there is a concern that a difference in refractive index will arise between the dam and fill portions due to differences in the types and mixing ratios of the components of the photocurable resin composition used, or due to migration of low molecular weight substances occurring between the dam and fill portions, causing the boundary between them to be visible as a so-called knit line.
[0004] For this reason, Patent Document 1 recommends that when adjusting the curable resin composition that functions as a dam agent and the curable resin composition that functions as a fill agent, in order to prevent knit lines from being visible between the dam portion and the fill portion, the difference in 400 nm transmittance between the two should be adjusted to 5% or less, the difference in refractive index should be adjusted to 0.01% or less, and the difference in haze should be adjusted to 0.2% or less. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] WO2014 / 168173 publication Summary of the Invention [Problem to be solved by the invention]
[0006] Incidentally, regarding the knit line between the dam portion and the fill portion in the transparent resin layer of the image display device, the visibility of the transparent resin layer after curing becomes an issue.
[0007] However, in Patent Document 1, the visibility of the boundary line when the curable resin composition used as a dam agent before curing and the curable resin composition used as a fill agent before curing come into contact is the problem, and it cannot be said that the knit line in the transparent resin layer after curing is considered. Moreover, Patent Document 1 only recommends that the "400 nm transmittance difference", "refractive index difference", and "haze difference" between the curable resin composition used as a dam agent before curing and the curable resin composition used as a fill agent before curing should not exceed a predetermined value, and does not provide any specific indicators on how to select the constituent components.
[0008] The object of the present invention is to solve the above-mentioned conventional problems, and to make it difficult to visually detect knit lines between the dam portion and the fill portion of the cured transparent resin layer when a photocurable material for forming the transparent resin layer is used as a dam agent or fill agent in the manufacture of an image display device in which an image display panel and a front panel are laminated via a transparent resin layer. [Means for solving the problem]
[0009] The inventors have discovered that the above-mentioned object can be achieved by forming a photocurable material for forming a dam portion and / or a fill portion of a transparent resin layer of an image display device in which an image display panel and a front panel are laminated together via a transparent resin layer, comprising a specific photocurable component, a plasticizer and a photopolymerization initiator, and setting the difference between the refractive index of the photocured product of the photocurable component and the refractive index of the plasticizer to a predetermined numerical value or less, thereby completing the present invention.
[0010] That is, the present invention relates to a photocurable material for forming a transparent resin layer of an image display device in which an image display panel and a front panel are laminated with the transparent resin layer interposed therebetween, the photocurable material comprising the following components (a) to (c): Component (a) a (meth)acrylic acid ester component; Component (b) a plasticizer component; and Component (c) Photopolymerization initiator component Contains The present invention provides a photocurable material in which the difference in refractive index between the photocured product of the (meth)acrylic acid ester component of component (a) and the plasticizer component of component (b) is 0.02 or less.
[0011] The present invention also provides an image display device in which an image display panel and a front panel are laminated via a transparent resin layer, the transparent resin layer being a photocured product of the photocurable material of the present invention described above. Effect of the Invention
[0012] The photocurable material of the present invention contains a component (a) (meth)acrylic ester component, a component (b) plasticizer component, and a component (c) photopolymerization initiator component, and the difference between the refractive index of the photocured product of the component (a) (meth)acrylic ester component and the refractive index of the component (b) plasticizer component is 0.02 or less. In general, when a component that is prone to migration in the component (a) (meth)acrylic ester component migrates from one of the dam part and the fill part of the transparent resin layer to the other, there is a concern that the boundary between the dam part and the fill part will be visually recognized as a knit line. As described above, in the photocurable material of the present invention, the difference between the refractive index of the photocured product of the component (a) (meth)acrylic ester component and the component (b) plasticizer component is very small, 0.02 or less. Therefore, it is expected that the boundary between the dam part and the fill part of the transparent resin layer will be less likely to be visually recognized as a knit line. [Brief description of the drawings]
[0013] [Figure 1]FIG. 1 is a schematic cross-sectional view of one embodiment of an image display device. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0014] The photocurable material of the present invention will be described in detail below.
[0015] The photocurable material of the present invention is preferably used to form the transparent resin layer 5 of the image display device 10 of FIG. 1. Here, the image display device 10 has a structure in which an image display panel 1 and a front panel 2 are laminated via a transparent resin layer 5 consisting of a dam portion 3 and a fill portion 4 surrounded by the dam portion 3, and a polarizing plate 6 is usually arranged on the surface of the image display panel 1 on the transparent resin layer 5 side. The photocurable material of the present invention may be applied to the formation of both the dam portion 3 and the fill portion 4 of the transparent resin layer 5 in the image display device 10, or may be applied to the formation of either the dam portion 3 or the fill portion 4. Note that the image display device to which the photocurable material of the present invention can be applied is not limited to the embodiment of FIG. 1.
[0016] <Refractive index of photocurable material> The photocurable material of the present invention contains a (meth)acrylic acid ester component (a) which is a photopolymerizable component, a plasticizer component (b) and a photopolymerization initiator component (c). The photocurable material of the present invention is a material in which the difference in refractive index between the photocured product of the (meth)acrylic acid ester component (a) and the plasticizer component (b) is adjusted to 0.02 or less, preferably 0.015 or less.
[0017] If the viscosity of the photocurable material of the present invention is too low, the material tends to spread beyond the intended area when applied, making it difficult to control the application area, whereas if the viscosity is too high, the material tends to have poor wettability and difficult to apply, so the viscosity is preferably 1000 to 8000 mPa·s, more preferably 2000 to 7000 mPa·s at 25° C. The viscosity can be measured using a general rotational viscometer (cone and plate rheometer, 25° C., cone C35 / 2, rotation speed 10 rpm).
[0018] As mentioned above, even if a component that is prone to migration in the (meth)acrylic acid ester component (a) before curing migrates from one of the dam section and the fill section to the other, the difference in refractive index between the photocured product of the (meth)acrylic acid ester component (a) and the plasticizer component of component (b) is very small, at 0.02 or less, so that the boundary between the dam section and the fill section of the transparent resin layer after photocuring is difficult to visually recognize as a knit line.
[0019] (Measurement of refractive index of photocured product of component (a)) The photocured product of the component (a) (meth)acrylic acid ester component, which is the object of refractive index measurement, is prepared by mixing 100 parts by mass of the component (a) (meth)acrylic acid ester component with 0.5 to 1.0 parts by mass of the component (c) photopolymerization initiator component, and photocuring the mixture by irradiation with light such as ultraviolet light. The other object of refractive index measurement, the component (b) plasticizer component, can be measured for its refractive index as is without any special pretreatment such as curing treatment. When the photocured product to be measured for refractive index is a solid, its refractive index can be measured using a commercially available Abbe type refractive index measuring device. When the photocured product to be measured for refractive index is a high viscosity liquid, it can be measured using a digital refractometer that detects the critical angle of light refraction.
[0020] The photocuring conditions for the component (a) (meth)acrylic acid ester component can be appropriately selected so that the degree of cure calculated by the FT-IR method is 90% or more, preferably 95% or more. For example, a metal halide lamp is used at 5000 mJ / cm 2 The above curing conditions can be mentioned.
[0021] The refractive index of the photocured product of component (a) (meth)acrylic acid ester component can be specifically measured as follows. When component (a) (meth)acrylic acid ester component contains multiple components, the photocured product of a mixture of the multiple components is measured. The refractive index of the photocured product of component (a) (meth)acrylic acid ester component can be adjusted by changing the type and number of (meth)acrylic acid esters used as the (meth)acrylic acid ester component and the mixing ratio of each.
[0022] Photocuring of the component (a) (meth)acrylic acid ester component can be carried out appropriately according to a known method depending on the type of the component and the polymerization form depending on the type of polymerization initiator. Photocuring is usually carried out by exposing a 0.3 mm thick component (a) (meth)acrylic acid ester component to ultraviolet light emitted by a metal halide lamp at an integrated light amount of 3000 to 5000 mJ / cm. 2 In this case, the photocured product is one that has been cured so that the overall average reaction rate (curing rate) is 90% or more (preferably 95% or more). The reaction rate of the entire photocured product means the reaction rate measured for a cured product formed into a film having a thickness of, for example, 0.3 mm.
[0023] Here, the reaction rate is a value defined as the ratio (consumption rate) of the amount of (meth)acryloyl groups present after photocuring to the amount of (meth)acryloyl groups present in the (meth)acrylic acid ester component (a) before photocuring. The higher the reaction rate value, the more the reaction has progressed. Specifically, the reaction rate is the ratio of the amount of (meth)acryloyl groups present after photocuring at 1640 to 1620 cm from the baseline in the FT-IR measurement chart of the photocurable material before photocuring. -1 The absorption peak height (X) of the photocurable material (photocured layer) after photocuring is measured from the baseline at 1640 to 1620 cm -1 and the absorption peak height (Y) of the sample in the above formula.
[0024]
number
[0025] (Measurement of refractive index of plasticizer component (b)) The case where the plasticizer component is a single component and the case where a plurality of plasticizers are contained (total refractive index) will be described separately.
[0026] (Specific example of refractive index measurement when component (b) contains only a single plasticizer component) Since plasticizer components are usually high-viscosity liquids, the refractive index of the plasticizer component to be measured can be measured by placing the plasticizer component to be measured in the prism part of a commercially available digital refractometer (e.g., ATAGO's RX-5000α) that detects the critical angle of optical refraction.
[0027] (Specific example of refractive index measurement when component (b) contains multiple plasticizers) As described above, the refractive index R of each of the multiple plasticizers is measured. The refractive index R of each plasticizer is multiplied by its amount (parts by mass) M to obtain a value A, and the values A obtained for each plasticizer are all added together to obtain a value B, which is then divided by the total amount C of the multiple plasticizers present to obtain the refractive index. As a specific example, when the plasticizer component of component (b) contains two types of plasticizers (a first plasticizer and a second plasticizer), the refractive index is calculated as follows:
[0028] That is, when the plasticizer component of component (b) contains a first plasticizer having a refractive index RIa and a second plasticizer having a refractive index RIb, the amount of the first plasticizer present is W1 parts by mass, and the amount of the second plasticizer present is W2 parts by mass, the refractive index of the plasticizer component of component (b) is calculated according to the following formula:
[0029]
number
[0030] The components of the photocurable material of the present invention will be described below one by one.
[0031] <Component (a)> The photocurable material of the present invention contains a (meth)acrylic acid ester component as component (a), where the term "(meth)acrylic acid ester" as used herein includes acrylic acid ester and methacrylic acid ester.
[0032] The (meth)acrylic acid ester component (a) preferably contains one or more polyfunctional (meth)acrylate oligomers and one or more monofunctional (meth)acrylate monomers. The reason for containing the polyfunctional (meth)acrylate oligomer is to maintain the film-forming properties of the photocurable material when a transparent resin layer is formed from the photocurable material, and the reason for containing the monofunctional (meth)acrylate monomer is to adjust the application properties and viscosity of the photocurable material and to impart good adhesion to the transparent resin layer containing the oligomer.
[0033] The polyfunctional (meth)acrylate oligomer preferably has a dielectric constant of 4.0 or more at 100 kHz. If the dielectric constant is less than 4.0, the moisture permeability of the cured product of the photocurable material tends to be too low. The dielectric constant can be measured by a general LCR meter.
[0034] Preferred examples of the polyfunctional (meth)acrylate oligomer having a relative dielectric constant of 4.0 or more at 100 kHz include polyfunctional polyether-based urethane (meth)acrylate oligomers, polyfunctional polyester-based urethane oligomers, polyfunctional hydroxyl group-containing oligomers, etc. Among these, bifunctional polyether-based urethane (meth)acrylate oligomers are preferred because they can impart good moisture permeability to the cured product of the photocurable material.
[0035] If the weight-average molecular weight of the polyfunctional (meth)acrylate oligomer is too small, the cured product of the photocurable material becomes too hard and display unevenness occurs when applied to a display device, while if it is too large, there is a concern that the photocurable material cannot be given an appropriate viscosity when handled, so the weight-average molecular weight is preferably 20,000 to 50,000, more preferably 30,000 to 40,000. This weight-average molecular weight can be measured using a general gel permeation chromatography device (GPC device).
[0036] Furthermore, if the viscosity of the polyfunctional (meth)acrylate oligomer is too low, the cured product of the photocurable material becomes too hard and display unevenness occurs when applied to a display device, while if it is too high, the photocurable material tends to be unable to be given an appropriate viscosity when handled, so the viscosity is preferably 20,000 to 60,000 mPa·s, and more preferably 30,000 to 50,000 mPa·s at 60° C. The viscosity can be measured using a general B-type viscometer.
[0037] If the glass transition temperature of the polyfunctional (meth)acrylate oligomer is too low, good adhesion cannot be imparted to the photocurable material, and if it is too high, the cured product of the photocurable material becomes too hard and tends to cause display unevenness when applied to a display device, so it is preferably −30 to 10° C., more preferably −20 to 0° C. The glass transition temperature can be measured using a general differential scanning calorimeter.
[0038] The content of the polyfunctional (meth)acrylate oligomer having a relative dielectric constant of 4.0 or more at 100 kHz in the component (a) (meth)acrylic acid ester component is preferably 20% by mass to 40% by mass, and more preferably 20% by mass to 30% by mass, from the viewpoints of the adhesiveness and reactivity of the photocurable material.
[0039] The component (a), the (meth)acrylic acid ester component, may contain a polyfunctional (meth)acrylate oligomer other than the polyfunctional (meth)acrylate oligomer having a relative dielectric constant of 4.0 or more at 100 kHz, such as a polyether-modified polyfunctional (meth)acrylate oligomer, as long as the effects of the present invention are not impaired.
[0040] As the monofunctional (meth)acrylate monomer contained in the component (a) (meth)acrylic acid ester component, a hydroxyl group-containing (meth)acrylate monomer is preferably used in order to impart high polarity to the photocurable material, improve the moisture permeability of the cured product of the photocurable material, and allow moisture generated from the polarizing plate to escape to the outside of the image display device. The hydroxyl group-containing (meth)acrylate monomer may contain two or more hydroxyl groups, but preferably contains one hydroxyl group in order to avoid a decrease in the water resistance and adhesive strength of the photocured product.
[0041] Examples of hydroxyl group-containing (meth)acrylate monomers include hydroxyalkyl (meth)acrylate monomers, and the number of carbon atoms in the alkyl is not limited, but is usually C1-12, preferably C1-6. Specific examples include methyl, ethyl, propyl, isopropyl, butyl, isobutyl, sec-butyl, tert-butyl, pentyl, hexyl, and 2-ethylbutyl. Specific examples include 2-hydroxyethyl (meth)acrylate, 1-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and phenyl glycidyl ether (meth)acrylate. Among these, 2-hydroxyethyl (meth)acrylate and especially 4-hydroxybutyl (meth)acrylate are preferred because they can efficiently increase the moisture permeability of the photocured product of the photocurable material.
[0042] In addition, the component (a) (meth)acrylic acid ester component may contain a (meth)acrylate monomer that does not contain a hydroxyl group, so long as the effect of the invention is not impaired. Examples of the (meth)acrylate monomer that does not contain a hydroxyl group include a chain-shaped hydrocarbon group-containing type and a cyclic hydrocarbon group-containing type. For example, alkyl (meth)acrylate monomers, cycloalkyl or bicycloalkyl (meth)acrylate monomers, or heterocycloalkyl or heterobicycloalkyl (meth)acrylate monomers can be mentioned. Preferred examples of the alkyl (meth)acrylate monomers include isostearyl acrylate and lauryl acrylate. Preferred examples of the cycloalkyl or bicycloalkyl (meth)acrylate monomers include isobornyl acrylate. Preferred examples of the heterocycloalkyl or heterobicycloalkyl (meth)acrylate monomers include morpholyl acrylate.
[0043] The content of the monofunctional (meth)acrylate monomer such as a hydroxyl group-containing (meth)acrylate monomer in the component (a) (meth)acrylic acid ester component is preferably 25 mass % or more, more preferably 50 mass % or more, in order to improve the moisture permeability of the cured product of the photocurable material, as described above.
[0044] The content of the component (a) (meth)acrylic acid ester component in the photocurable material is preferably 20% by mass to 40% by mass, and more preferably 25% by mass to 35% by mass, since if the content is too low it will be difficult to impart an appropriate viscosity to the photocurable material when it is handled, and if the content is too high there is concern that the shrinkage rate of the photocurable material when cured will become too large.
[0045] The difference in refractive index between the photocured products of one or more polyfunctional (meth)acrylate oligomers and one or more monofunctional (meth)acrylate monomers contained in the component (a) (meth)acrylic acid ester component [i.e., the refractive index difference within component (a)] is preferably 0.02 or less, and more preferably 0.015 or less, from the viewpoint of migration from one of the dam portion and the fill portion to the other.
[0046] The photocured products of each polyfunctional (meth)acrylate oligomer and each monofunctional (meth)acrylate monomer are prepared by mixing 100 parts by mass of each oligomer or monomer with 0.5 to 1.0 parts by mass of the photopolymerization initiator component (c) and photocuring the mixture. The photocuring conditions can be appropriately selected so that the curing rate calculated by the FT-IR method is 90% or more, preferably 95% or more. As an example, a metal halide lamp is used to illuminate the mixture at 5000 mJ / cm. 2 The curing conditions are as described above. In the present invention, the refractive index can be measured using a commercially available Abbe type refractive index measuring device.
[0047] <Component (b)> The photocurable material of the present invention contains a plasticizer component as component (b). The plasticizer does not photocure by itself upon irradiation with light, but imparts flexibility to the photocured product after photocuring. From the viewpoint of compatibility with other components, such a plasticizer preferably contains one of polyether-based polyol and polyester-based polyol. It is more preferable to contain a polyether-based polyol. In addition, general polymers that are miscible with these plasticizer components can also be used as plasticizers. As a polymer that can be used as such a plasticizer, a polymer that has a small refractive index difference from the plasticizer component of component (b) used in combination can be preferably used. For example, a polymer containing a hydroxyl group can be exemplified.
[0048] As the polyether polyol, for example, a general polyether polyol obtained by addition polymerization of an alkylene oxide to a polyol such as ethylene glycol, propylene glycol, glycerin, trimethylolpropane, etc. The alkylene oxide is not particularly limited, and examples thereof include ethylene oxide, propylene oxide, butylene oxide, etc.
[0049] Commercially available polyether polyols include, for example, "ADEKA Polyether" manufactured by ADEKA Corp. More specifically, the polypropylene glycol "P Series", the polypropylene glycol adduct of bisphenol A "BPX Series", the polypropylene glycol adduct of glycerin "G Series", the polypropylene glycol adduct of trimethylolpropane "T Series", the polypropylene glycol adduct of ethylenediamine "EDP Series", the polypropylene glycol adduct of sorbitol "SP Series", the polypropylene glycol adduct of sorbitol "PR Series", the random copolymer of ethylene oxide and propylene oxide, the propylene oxide-ethylene oxide block copolymer "CM Series", and the like are included.
[0050] If the number average molecular weight of the polyether polyol is too small, it may bleed out from the cured product of the photocurable material, and if it is too large, it may be difficult to impart an appropriate viscosity to the photocurable material when it is handled, so the number average molecular weight is preferably 500 to 8000, and more preferably 1000 to 5000. The number average molecular weight can be measured using a general gel permeation chromatography apparatus (GPC apparatus).
[0051] As the polyester polyol, for example, a general polyester polyol obtained by condensation polymerization of a dicarboxylic acid and a diol can be used. As the dicarboxylic acid, for example, aliphatic carboxylic acids such as adipic acid, azelaic acid, sebacic acid, dodecanedioic acid, etc.; aromatic carboxylic acids such as terephthalic acid, isophthalic acid, etc. can be mentioned. As the diol, for example, linear diols such as ethylene glycol, 1,4-butanediol, 1,6-hexanediol, 1,9-nonanediol, diethylene glycol, etc.; 1,2-propylene glycol, 1,3-butylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,2-dimethyl-1,3-propanediol, 2-methyl-1,8-octanediol, etc. can be mentioned.
[0052] Commercially available polyester polyols include "P-1010", "P-2010", "P-3010", and "P-2050" (all manufactured by Kuraray Co., Ltd.), "OD-X-102", "OD-X-668", and "OD-X-2068" (all manufactured by DIC Corporation), "NS-2400", "YT-101", "F7-67", "#50", "F1212-29", "YG-108", "V14-90", and "Y65-55" (all manufactured by ADEKA Corporation), and the like.
[0053] If the number average molecular weight of the polyester polyol is too small, it may bleed out from the cured product of the photocurable material, whereas if it is too large, it may be difficult to impart an appropriate viscosity to the photocurable material when it is handled. Therefore, the number average molecular weight is preferably 500 to 8,000, and more preferably 1,000 to 5,000.
[0054] The content of the plasticizer component (b) in the photocurable material is preferably 30% by mass to 60% by mass, more preferably 40% by mass to 50% by mass, since if the content is too low, the sufficient flexibility required for applying the cured product of the photocurable material as an adhesive for an image display device will not be obtained, whereas if the content is too high, there is a concern that the photocurable material will not be given sufficient adhesive strength.
[0055] When the plasticizer component of component (b) contains two or more plasticizers, the difference in refractive index between them [i.e., the refractive index difference within component (b)] is preferably 0.03 or less, more preferably 0.02 or less, in order to suppress migration from one of the dam section and the fill section to the other. Here, the reason why the preferred upper limit of the refractive index difference within component (b) (0.03 or less) is set higher than the preferred upper limit of the refractive index difference within component (a) (preferably 0.02 or less) is that the plasticizer component of component (b) has a higher viscosity than component (a) and is difficult to flow in the first place.
[0056] <Ingredient (c)> The photocurable material of the present invention contains a photopolymerization initiator according to the polymerization type as component (c). Among them, it is preferable to contain a photoradical polymerization initiator in order to impart high reactivity to the photocurable material. As the photoradical polymerization initiator, it is more preferable to contain at least one of an alkylphenone-based photopolymerization initiator and an acylphosphine oxide-based photopolymerization initiator. As the alkylphenone-based photopolymerization initiator, 1-hydroxycyclohexyl phenyl ketone (Irgacure 184, manufactured by BASF), 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propylonyl)benzyl]phenyl}-2-methyl-1-propan-1-one (Irgacure 127, manufactured by BASF), etc. can be used. As the acylphosphine oxide-based photopolymerization initiator, 2,4,6-trimethylbenzoyldiphenylphosphine oxide (Irgacure TPO, manufactured by BASF), etc. can be used. Other examples of the photopolymerization initiator that can be used include benzophenone and acetophenone.
[0057] The content of the photopolymerization initiator of component (c) in the photocurable material of the present invention, when it is a photoradical polymerization initiator, is preferably 0.2 parts by mass to 2 parts by mass, more preferably 0.5 parts by mass to 1 part by mass, relative to 100 parts by mass of the above-mentioned component (a) (meth)acrylic acid ester component. By setting it in such a range, it is possible to more effectively prevent insufficient curing during light irradiation and to more effectively prevent an increase in outgassing due to the polymerization reaction. The photopolymerization initiator may be used alone or in combination of two or more types. When two or more types of photopolymerization initiators are used in combination, it is preferable that the total amount thereof satisfies the above range.
[0058] <Ingredient (d)> The photocurable material of the present invention may contain a known filler as component (d) depending on the application of the photocurable material. In particular, it is preferable to contain silica as a filler. By containing silica, the photocurable material can be given a thixotropic ratio of preferably 2 to 5, more preferably 2.5 to 3.5, which is useful as a damming agent. Specifically, if the thixotropic ratio is too small, it becomes difficult for the photocurable material to maintain its shape, and if it is too large, the dischargeability of the photocurable material from a dispenser or the like decreases. Here, the thixotropic ratio is calculated from the viscosity measured using a general rotational viscometer (cone plate rheometer, 25°C, cone C35 / 2, rotation speed 10 rpm), and is specifically defined as a value obtained by dividing the viscosity at 25°C and a rotation speed of 1 rpm by the viscosity at a rotation speed of 10 rpm.
[0059] If the average particle size of such silica is too small, there is a high risk of secondary aggregation in the photocurable material, and if it is too large, there is a possibility that sufficient thixotropy cannot be imparted to the photocurable material, so it is preferably 7 nm or more and 40 nm or less, more preferably 10 nm or more and 20 nm or less. The average particle size can be measured using a general laser diffraction particle size distribution meter.
[0060] In addition, the silica as component (d) is preferably surface-treated for hydrophobization. A photocurable material containing hydrophobized silica can exhibit good thixotropy without impairing the moisture permeability and transparency of the cured product. A preferred example of such a hydrophobization treatment is a known alkylsilylation treatment of silica. Among them, a higher alkylsilylation treatment having 12 to 18 carbon atoms, particularly a hexadecylsilylation treatment as described below, is preferred.
[0061] The hexadecylsilylation treatment of silica can be carried out by a conventional method, for example, by subjecting silanol having a hexadecyl group to a polycondensation reaction with hydroxyl groups present on the surface of a silica filler having an untreated surface.
[0062] In addition, if the BET specific surface area of the filler (especially silica) of component (d) is too small, it may not be possible to impart sufficient thixotropy to the photocurable material, and if it is too large, there is a tendency for the risk of secondary aggregation in the photocurable material to increase. Therefore, it is preferable that the BET specific surface area is 100 m 2 / g or more 300m 2 / g or less, more preferably 130m 2 / g or more 200m 2 The BET specific surface area can be measured by the so-called BET method.
[0063] The content of the filler (particularly silica) of component (d) in the photocurable material is preferably 5% by mass or more and 15% by mass or less, more preferably 5% by mass or more and 10% by mass or less, since if the content is too low, sufficient thixotropy will not be obtained, and if the content is too high, there is a concern that the transparency of the cured product will not be maintained.
[0064] <Other components of the photocurable material> In addition to the above-mentioned components (a) to (d), the photocurable material of the present invention may contain known resin additives such as antioxidants, solvents, UV absorbers, colorants, organic or inorganic fillers, etc., within the scope of the invention.
[0065] <Method of manufacturing photocurable material> The photocurable material of the present invention can be prepared by uniformly mixing the above-mentioned components according to a known mixing method.
[0066] <Image display device> The photocurable material of the present invention can be preferably used as a material for forming the dam section 3 or the fill section 4, or both the dam section 3 and the fill section 4, of an image display device 10 in which an image display panel 1 and a front panel 2 are laminated via a transparent resin layer 5 composed of a fill section 4 and a dam section 3 surrounding the outer periphery of the fill section 4, as shown in FIG. 1. In this way, by applying the photocurable material of the present invention to the transparent resin layer, it is possible to make the knit line less visible at the boundary between the dam section 3 and the fill section 4. A polarizing plate 6 may be disposed on the surface of the image display panel in contact with the transparent resin layer 5. Although such an image display device is also one embodiment of the present invention, the image display device of the present invention is not limited to the embodiment of FIG. 1.
[0067] When the transparent resin layer 5 is composed of a fill portion 4 located at a position corresponding to the display portion of the image display panel 1 and a dam portion 3 surrounding the periphery of the fill portion 4, not only is the difference between the refractive index of the photocured product of the (meth)acrylic ester component of component (a) and the refractive index of the plasticizer component of component (b) in the dam portion 3 made 0.02 or less, preferably 0.015 or less, but also the difference between the refractive index of the photocured product of the (meth)acrylic ester component of component (a) and the refractive index of the plasticizer component of component (b) in the fill portion 4 made 0.02 or less, preferably 0.015 or less. This makes it possible to make the knit line less visible at the boundary between the dam portion 3 and the fill portion 4. Furthermore, in order to make the knit lines less visible, the difference between the refractive index of the photocured product of the (meth)acrylic acid ester component of component (a) in the dam portion 3 and the refractive index of the photocured product of the (meth)acrylic acid ester component of component (a) in the fill portion 4 is preferably 0.02 or less, more preferably 0.015 or less, and the difference between the refractive index of the plasticizer component of component (b) in the dam portion 3 and the refractive index of the plasticizer component of component (b) in the fill portion 4 is also preferably 0.02 or less, more preferably 0.015 or less.
[0068] (Image display panel 1) Examples of the image display panel 1 constituting the image display device 10 of the present invention include a liquid crystal display panel, an organic EL display panel, a touch panel, etc. Here, the touch panel means an image display / input panel that combines a display element such as a liquid crystal display panel with a position input device such as a touch pad.
[0069] (Front Panel 2) The front panel 2 constituting the image display device 10 of the present invention functions as a protective panel for the image display panel 1. Examples of the front panel 2 include plate-shaped materials and sheet-shaped materials such as glass, acrylic resin, polyethylene terephthalate, polyethylene naphthalate, and polycarbonate. These materials may be subjected to hard coat treatment, anti-reflection treatment, etc. on one or both sides. The physical properties such as the thickness and elastic modulus of the front panel 2 can be appropriately determined depending on the purpose of use. The front panel 2 includes not only the above-mentioned members with a relatively simple structure, but also those in which various sheets or film materials are laminated, such as a touch panel module.
[0070] A light-shielding layer (not shown) may be provided on the periphery of the front panel 2 to improve the contrast of the image. The light-shielding layer can be formed, for example, by applying a paint colored black or the like by screen printing or the like, and then drying and curing the paint. The thickness of the light-shielding layer is usually 5 to 100 μm.
[0071] (Transparent resin layer 5) The transparent resin layer 5 of the image display device 10 of the present invention is composed of a dam portion 3 and a fill portion 4. The dam portion 3 is provided on the outer periphery of the image display panel, and the fill portion 4 is filled inside the dam portion 3. The dam portion 3 is a continuous structure usually having a width of 0.3 mm to 3 mm and a height of 0.1 mm to 2 mm. In addition, when a metal bezel (not shown) is provided on the outer edge of the image display panel 1, another continuous dam portion usually having a width of 0.3 mm to 3 mm and a height of 0.1 mm to 2 mm may be provided at the boundary between the metal bezel and the image display panel.
[0072] (Polarizing plate 6) The polarizing plate 6 has a polarizer (not shown) sandwiched between a pair of protective layers (not shown). An adhesive may be used when sandwiching the polarizer and the protective layers. The polarizing plate 6 may further include an optical layer (e.g., a retardation plate) other than the polarizer and the protective layers. The thickness of the polarizing plate 6 is usually 0.1 mm to 0.3 mm.
[0073] As the polarizer, for example, a polarizer having a known structure obtained by subjecting a polyvinyl alcohol resin to a dyeing treatment using a dichroic substance (for example, an iodine compound) and a stretching treatment can be used.
[0074] The protective layers sandwiching the polarizer may be, for example, films made of thermoplastic resins excellent in transparency, mechanical strength, thermal stability, moisture blocking properties, isotropy, etc. Examples of such thermoplastic resins include cellulose resins such as triacetyl cellulose (TAC), polyester resins such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyethersulfone resins, polysulfone resins, polycarbonate resins, polyamide resins, polyimide resins, polyolefin resins, (meth)acrylic resins, cyclic polyolefin resins, polyarylate resins, polystyrene resins, polyvinyl alcohol resins, and mixtures thereof.
[0075] <Manufacturing method for image display device> The image display device of the present invention shown in FIG. 1 can be manufactured as described below, but is not limited thereto.
[0076] First, a polarizing plate is placed on one side of an image display panel in a conventional manner, and the photocurable material of the present invention is applied around the polarizing plate in a dam shape using a dispenser or the like, and a photocurable dam portion is formed by irradiating with ultraviolet light.
[0077] Next, a photocurable resin composition for forming a fill portion is applied to the area surrounded by the photocurable dam portion using a dispenser or the like and dried to form the photocurable fill portion, thereby forming a photocurable resin layer consisting of the photocurable dam portion and the photocurable fill portion.
[0078] Next, the front panel is laminated on the photocurable resin layer.
[0079] Subsequently, the photocurable resin layer is photocured by irradiating it with ultraviolet light through the front panel, thereby forming a photocured transparent resin layer, and the image display device of FIG. 1 is obtained. EXAMPLES
[0080] The present invention will be described in more detail below with reference to examples and comparative examples. The compounds used in the following examples and comparative examples are as follows.
[0081] <Component (a) (meth)acrylic acid ester component> (Oligomer) Polyether oligomer: UV-3700B (urethane acrylate oligomer, manufactured by Mitsubishi Chemical Corporation). (monomer) Hydroxyl-containing monomer: 4-HBA (4-hydroxybutyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.); Cyclic group-containing monomer: Viscoat 200 (cyclic trimethylolpropane formal acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.); Ether group-containing monomer: Viscoat 190 (ethoxyethoxyethyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.); Alkyl group-containing monomer: IDAA (isodecyl acrylate, manufactured by Osaka Organic Chemical Industry Co., Ltd.).
[0082] <Component (b) Plasticizer Component> Polyether plasticizer: Adeka Polyether P-3000 (a reaction product of propionic glycol, manufactured by ADEKA Corporation); Hydroxyl-containing polymer: Elfort 3122L (polymer of 2-ethylhexyl acrylate and hydroxyethyl acrylate, manufactured by Showa Denko Materials Co., Ltd.).
[0083] <Component (c) Photopolymerization initiator component> Phosphine oxide photopolymerization initiator: SPEEDCURE TPO (diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide, manufactured by Ransom).
[0084] <Component (d) Silica> Surface-untreated silica: Aerosil 200 (fumed silica, manufactured by Nippon Aerosil Co., Ltd.); Hydrophobized surface-treated silica: VP NKC130 (fumed silica surface-treated with hexadecyl group-containing silane (a silane compound containing an alkyl group having 16 carbon atoms), manufactured by Nippon Aerosil Co., Ltd.).
[0085] Examples 1 to 3, Comparative Examples 1 to 2 Components (a) to (d) and other components shown in Table 1 were mixed uniformly in a conventional manner to prepare photocurable materials for the dam portion and the fill portion.
[0086] (Evaluation of knit line visibility) Table 1 shows the results of visually evaluating the visibility of the knit line at the boundary between the dam portion and the fill portion of the transparent resin layer of the image display device having the structure of FIG.
[0087] [Table 1]
[0088] (Discussion of evaluation results) As can be seen from Table 1, the difference in refractive index between the entire component (a) and the component (b) was less than 0.02 in the photocurable materials of Examples 1 to 3, and therefore knit lines were not visible. In particular, the photocurable materials of Examples 1 and 2 were significantly below 0.02, and therefore knit lines are expected to be less visible than in the photocurable material of Example 3.
[0089] On the other hand, in the photocurable materials of Comparative Examples 1 and 2, the difference between the overall refractive index of component (a) and the refractive index of component (b) exceeded 0.02, so that knit lines were visible. [Industrial Applicability]
[0090] The photocurable material of the present invention contains component (a) a (meth)acrylic acid ester component, component (b) a plasticizer component, and component (c) a photopolymerization initiator component, and the difference between the refractive index of the photocured product of component (a) the (meth)acrylic acid ester component and the refractive index of component (b) the plasticizer component is 0.02 or less. Therefore, when the photocurable material of the present invention is applied to the formation of a transparent resin layer of an image display device in which an image display panel and a front panel are laminated with the transparent resin layer interposed therebetween, it is expected that the boundary line between the dam part and the fill part of the transparent resin layer will be difficult to visually recognize as a knit line. Therefore, the photocurable material of the present invention is useful for the manufacture of various types of image display devices. [Explanation of symbols]
[0091] 1 Image display panel 2 Front Panel 3. Dam Section 4 Phil Section 5 Transparent resin layer 6 Polarizing Plate 10 Image display device
Claims
1. A photocurable material for forming a transparent resin layer of an image display device in which an image display panel and a front panel are laminated with the transparent resin layer interposed therebetween, the photocurable material comprising the following components (a) to (c): Component (a) a (meth)acrylic acid ester component; Component (b) a plasticizer component; and Component (c) Photopolymerization initiator component Contains A photocurable material in which the difference between the refractive index of a photocured product of the (meth)acrylic acid ester component of component (a) and the refractive index of the plasticizer component of component (b) is 0.02 or less.
2. The photocurable material according to claim 1, wherein the photocured product of the (meth)acrylic acid ester component of component (a) is obtained by mixing 100 parts by mass of the (meth)acrylic acid ester component with 0.5 parts by mass to 1.0 parts by mass of the photopolymerization initiator component of component (c), and photocuring the mixture.
3. 3. The photocurable material according to claim 1, wherein the (meth)acrylic acid ester component of component (a) contains one or more polyfunctional (meth)acrylate oligomers and one or more monofunctional (meth)acrylate monomers.
4. 4. The photocurable material according to claim 3, wherein the polyfunctional (meth)acrylate oligomer is a difunctional polyether-based urethane (meth)acrylate oligomer, and the monofunctional (meth)acrylate monomer is a hydroxyl group-containing (meth)acrylate monomer.
5. 5. The photocurable material according to claim 1, wherein the difference in refractive index between photocured products of each of the oligomers and monomers contained in the (meth)acrylic acid ester component of component (a) is 0.02 or less.
6. The photocurable material according to any one of claims 1 to 5, wherein when the plasticizer component of component (b) contains a plurality of plasticizers, the refractive index of the plasticizer component of component (b) is a numerical value obtained by multiplying the refractive index of each of the plurality of plasticizers by the amount (parts by mass) present therein, adding up the numerical values obtained for each plasticizer, and dividing the sum by the total amount of the plurality of plasticizers present.
7. When the plasticizer component of component (b) contains a first plasticizer having a refractive index RIa and a second plasticizer having a refractive index RIb, the amount of the first plasticizer present is W1 parts by mass, and the amount of the second plasticizer present is W2 parts by mass, the refractive index of the plasticizer component of component (b) is expressed by the following formula: [0010] The photocurable material according to any one of claims 1 to 6, calculated according to the following:
8. 8. The photocurable material according to claim 1, wherein, when the plasticizer component of component (b) contains a plurality of plasticizers, the mutual refractive index difference between the plurality of plasticizers is 0.03 or less.
9. When the transparent resin layer is composed of a fill portion present at a position corresponding to the display portion of the image display panel and a dam portion surrounding the outer periphery of the fill portion, the photocurable material described in any one of claims 1 to 8 for forming the dam portion further contains a filler as component (d).
10. An image display device in which an image display panel and a front panel are laminated via a transparent resin layer, the transparent resin layer being a photocured product of the photocurable material according to any one of claims 1 to 9.
11. When the transparent resin layer is composed of a fill portion present at a position corresponding to the display portion of the image display panel and a dam portion surrounding the outer periphery of the fill portion, the difference in refractive index between the photocured product of the (meth)acrylic acid ester component of component (a) in the photocurable material according to any one of claims 1 to 9 for forming the dam portion and the refractive index between the plasticizer component of component (b) is 0.02 or less, and the difference in refractive index between the photocured product of the (meth)acrylic acid ester component of component (a) in the photocurable material according to any one of claims 1 to 9 for forming the fill portion and the plasticizer component of component (b) is 0.02 or less.
12. The image display device according to claim 11, wherein the difference between the refractive index of the photocured product of the (meth)acrylic acid ester component of component (a) in the dam portion and the refractive index of the photocured product of the (meth)acrylic acid ester component of component (a) in the fill portion, and the difference between the refractive index of the plasticizer component of component (b) in the dam portion and the refractive index of the plasticizer component of component (b) in the fill portion are each 0.02 or less.
Citation Information
Patent Citations
Curable resin composition
JP2014148606A
Active energy ray-curable adhesive composition and adhesion method using the same
JP2014162853A
Manufacturing method for laminate, and light curable resin composition
JP2018140601A
Optical Diffusers, Photomasks and Their Methods of Fabrication
US20100302641A1
Urea-based and urethane-based pressure sensitive adhesive blends
WO2013148506A1