Thermal insulation, waterproof, high strength packaging bag and its manufacturing process

The composite paper structure with laminated layers and symmetric buffer structures addresses the issues of heat retention, waterproofing, and durability in packaging bags, ensuring effective protection and resistance to deformation.

JP7579031B1Active Publication Date: 2024-11-07DONGGUAN TAIHONG PACKAGING CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024032508
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2024-01-23
Filing Date
2024-03-04
Publication Date
2024-11-07
Estimated Expiration
2044-03-04

AI Technical Summary

Technical Problem

Current environmentally friendly packaging bags suffer from low heat retention, waterproof performance, and are prone to wrinkles and breakage during transportation, reducing their protective capabilities.

Method used

A heat-retaining waterproof high-strength packaging bag composed of composite paper with multiple laminated layers, including an outer and inner waterproof layer, a heat insulation buffer layer, and adhesive layers, which are bonded with elastic adhesives to enhance strength and insulation, and features symmetric buffer structures to distribute pressure evenly.

Benefits of technology

The packaging bag provides excellent heat retention, waterproofing, and resistance to wrinkles and damage, offering improved protection for packaged goods by enhancing pressure resistance and maintaining a three-dimensional shape.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579031000001_ABST
    Figure 0007579031000001_ABST
Patent Text Reader

Abstract

To provide a packaging bag having good heat retention and waterproof properties, high strength, resistance to wrinkling, deformation and breakage, good protection for articles, and wide range of applications. [Solution] The thermal insulation, waterproof, high-strength packaging bag is made from composite paper, which includes an outer waterproof layer, an outer paper layer, a first adhesive layer, a heat insulating buffer layer, a second adhesive layer, an inner paper layer and an inner waterproof layer arranged in that order, where the first adhesive layer and the second adhesive layer are elastic adhesive layers, and the manufacturing process includes bonding the first adhesive layer to the heat insulating buffer layer, then bonding the outer paper layer, keeping warm, drying, bonding the second adhesive layer to the heat insulating buffer layer, then bonding the outer paper layer, keeping warm, drying, applying a waterproofing agent to the outer paper layer and the inner paper layer respectively, forming an outer waterproof layer and an inner waterproof layer, drying, producing the composite paper, cutting and combining the composite paper to produce the thermal insulation, waterproof, high-strength packaging bag.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the field of packaging materials, more specifically, it relates to a thermally-insulated, waterproof, high-strength packaging bag and its manufacturing process. [Background technology]

[0002] Packaging bags are used for packaging goods, and different kinds of goods need to use packaging bags with different demand functions.

[0003] In order to improve the environmental protection and recyclability of packaging bags, packaging bags are generally made of recyclable paper such as kraft paper and cardboard. At present, ordinary environmentally friendly packaging bags are divided into several types as follows: the first type is a packaging bag made of single-layer kraft paper, which has the advantage of being lightweight, but its heat retention performance, waterproof performance and pressure resistance are all low; the second type is a packaging bag made of composite cardboard, which has good pressure resistance but average heat retention and waterproof performance; the third type is a packaging bag made by combining kraft paper and thermal insulation foam, which has good heat retention performance but is not environmentally friendly, and during transportation, the packaging bag is prone to wrinkles and breakage, and has low waterproof performance, which reduces the protective performance for goods. Therefore, the current environmentally friendly packaging bags need to be further improved. Summary of the Invention [Problem to be solved by the invention]

[0004] In order to solve the problem that the thermal insulation and waterproof performance of current environmentally friendly packaging bags is poor, and they are prone to wrinkles and breakage during transportation, resulting in reduced protective performance for items, the present application provides a thermal insulation, waterproof, high-strength packaging bag and a manufacturing process thereof. [Means for solving the problem]

[0005] In a first aspect, the present application provides a thermal insulation, waterproof, high-strength packaging bag, which adopts the following technical solutions:

[0006] A thermal insulation, waterproof, high-strength packaging bag is made from composite paper, the composite paper including an outer waterproof layer, an outer paper layer, a heat insulating buffer layer, an inner paper layer and an inner waterproof layer, which are bonded together in that order, the outer paper layer and the heat insulating buffer layer are bonded together with a first adhesive layer, and the inner paper layer and the heat insulating buffer layer are bonded together with a second adhesive layer, and both the first adhesive layer and the second adhesive layer are elastic adhesive layers.

[0007] By adopting the above technical solutions, the packaging bag of the present application is manufactured by combining composite paper, among which the inner paper layer and the outer paper layer play the role of improving the support of the packaging bag, improving the pressure resistance of the packaging bag, and making the packaging bag less likely to break; the heat insulating buffer layer can prevent the air flow between the inside and outside, and has good heat insulation and heat retention effects, and also has good buffering effect, so that the packaging bag is less likely to wrinkle and break when it is subjected to external pressure, and improves the protective effect for the packaged goods; the outer waterproof layer and the inner waterproof layer have a waterproof effect, and can further prevent moisture and air flow. The first adhesive layer functions to bond the outer paper layer to the insulating buffer layer, and the second adhesive layer functions to bond the inner paper layer to the insulating buffer layer. The first adhesive layer and the second adhesive layer are installed as elastic adhesive layers that can cooperate with the insulating buffer layer. When the packaging bag is subjected to external pressure, the outer paper layer, the insulating buffer layer and the inner paper layer act to evenly disperse and repel the external pressure, reducing the problem that the inner paper layer and the outer paper layer are prone to wrinkling, improving the pressure resistance of the packaging bag, and making the packaging bag less likely to be damaged.

[0008] Preferably, the outer waterproof layer has a first buffer structure on one side close to the insulating buffer layer, and the inner waterproof layer has a second buffer structure on one side close to the insulating buffer layer, the first buffer structure and the second buffer structure being the same, and the first buffer structure and the second buffer structure being installed symmetrically.

[0009] By adopting the above technical solution, the first buffer structure and the second buffer structure are installed symmetrically, and the structures of the first buffer structure and the second buffer structure are identical. When the packaging bag is subjected to external pressure, the first buffer structure of the outer paper layer and the second buffer structure of the inner paper layer cooperate with the insulating buffer layer, so that the surface of the packaging bag uniformly buffers and rebounds against the external pressure, and further improves the pressure resistance of the packaging bag and reduces the situation in which the packaging bag is wrinkled and damaged.

[0010] Preferably, the first buffer structure is composed of several raised portions, the horizontal height of which increases gradually from the central region along the peripheral edge region of the outer paper layer.

[0011] By adopting the above technical solution, the horizontal height of the convex portion near the central region of the outer paper layer is low, and the horizontal height of the convex portion near the peripheral edge region of the outer paper layer is high, the thickness of the first adhesive layer between the central region of the outer paper layer and the insulating cushioning layer is thickened, and the thickness of the first adhesive layer between the peripheral edge region of the outer paper layer and the insulating cushioning layer is thinned. The central region of a typical packaging bag is easily compressed and wrinkled. Therefore, the first adhesive layer and the insulating cushioning layer corresponding to the central region of the outer paper layer work well together to generate a cushioning effect for the central region of the outer paper layer, dispersing the compression force that the outer paper layer is about to receive to the surrounding area, improving the pressure resistance of the packaging bag, and making the packaging bag less likely to wrinkle or break.

[0012] Furthermore, the horizontal height of the convex portion in the central region of the outer paper layer in the present application is 1 / 3 to 3 / 4 of the height of the outer paper layer, so that the outer paper layer has good isolation performance and at the same time has good cushioning elasticity, reducing the occurrence of wrinkles and damage to the packaging bag.

[0013] Preferably, the distribution density of the protrusions gradually decreases from the central region of the outer paper layer along the peripheral edge region.

[0014] By adopting the above technical solution, the central region of the packaging bag is easily wrinkled when pressed from the outside, so by increasing the distribution density of the convex parts in the central region of the outer paper layer, the pressure can be evenly distributed and the occurrence of wrinkles and breakage can be reduced; the first buffer structure cooperates with the first adhesive layer and the insulating buffer layer to evenly distribute and release the pressure; the edge region of the packaging bag needs to be wrinkled during the assembly process, so the thickness of the peripheral edge region of the outer paper layer is controlled to be thick, making it easy to shape, and allowing the packaging bag to maintain a three-dimensional shape, with buffering performance and not easily deformed.

[0015] Preferably, the heat insulating buffer layer is made of any one of aerogel cotton, silicone cotton, and urethane.

[0016] By adopting the above technical solution, the above heat insulating buffer layer has excellent heat insulating and buffer elasticity, and can improve the heat retention and buffer performance of the manufactured packaging bag.

[0017] Preferably, the first adhesive layer and the second adhesive layer are both formed by curing an adhesive, and the adhesive is Polyurethane emulsion 40-60 parts Thickener 12-22 parts Wetting agent 4-8 parts Long-chain alkyl silane coupling agent 0.5 to 2 parts It is prepared with 20 to 30 parts by weight of the raw materials and 20 to 30 parts by weight of water.

[0018] By adopting the above technical solution, the pressure resistance and wrinkle resistance of the produced thermal insulation waterproof high strength packaging bag can be further improved, and the adhesive of the present application can be used to achieve adhesion stability between multiple layers. The adhesive of the present application uses a polyurethane emulsion as the resin body, and the polyurethane emulsion has good adhesion and has good elasticity and toughness after curing. The thickener plays the role of improving adhesion and can support the polyurethane emulsion, further improving the adhesion of the prepared adhesive. The wetting agent can generate a good synergistic effect with the thickener, improve the uniform dispersion performance of the prepared adhesive on the surface of the thermal insulation buffer layer, and can uniformly infiltrate and disperse in the gap between the first buffer structure and the second buffer structure, and can stably adhere the outer paper layer, the thermal insulation buffer layer and the inner paper layer. The long-chain alkyl silane coupling agent has a long carbon chain, and can further improve the dispersion stability between the polyurethane emulsion, the thickener and the wetting agent, and the adhesive prepared thereby has good adhesion stability and elasticity after curing.

[0019] Preferably, the thickening agent is Step A1 of adding 10 to 18 parts of starch, calculated in parts by weight, to 80 to 120 parts of water, adding 0.3 to 0.8 parts of a 1 to 2 mol / L aqueous hydrochloric acid solution dropwise, heating the mixture to 65 to 85° C., and stirring for 30 to 60 minutes to prepare a starch hydrolysate; and The thickener is prepared in step A2 by adding 0.2 to 0.5 parts of diethylene glycol, 0.1 to 0.3 parts of an acrylic acid ester copolymer, and 1 to 3 parts of magnesium aluminum silicate to the starch hydrolysate and stirring uniformly.

[0020] By adopting the above technical solution, starch is first hydrolyzed under acidic conditions to loosen and stabilize the molecular structure of starch, improve the water absorption and swelling effect of starch, and improve the supporting effect for polyurethane emulsion; then diethylene glycol, acrylic ester copolymer and magnesium aluminum silicate are added to mix with the starch hydrolyzate; diethylene glycol has a flexible long-chain ether chain segment, which can improve the dispersibility of acrylic ester copolymer and magnesium aluminum silicate in the starch hydrolyzate; the addition of acrylic ester copolymer and magnesium aluminum silicate can further improve the fluidity and adsorption performance of the starch hydrolyzate; the prepared thickener can be stably adsorbed to the polyurethane emulsion and has good adhesion stability.

[0021] Preferably, the wetting agent is composed of oleylamine polyoxyethylene ether and polyvinyl alcohol, and the weight ratio of the oleylamine polyoxyethylene ether to the polyvinyl alcohol is 1:(0.2 to 0.6).

[0022] By adopting the above technical solution, the suitable ratio of oleylamine polyoxyethylene ether and polyvinyl alcohol has a good synergistic effect, which can improve the wettability and adhesive performance of the prepared adhesive, and further improve the adhesive stability between the outer paper layer, the heat insulating buffer layer and the inner paper layer of the packaging bag.

[0023] Preferably, the adhesive comprises: Step B1 of adding a wetting agent to water and stirring uniformly to prepare a mixed solution; The polyurethane emulsion, the thickener and the long-chain alkyl silane coupling agent are added to the mixed liquid, and the mixture is stirred uniformly to prepare an adhesive, which is prepared in step B2.

[0024] By adopting the above technical solution, the wetting agent is first dissolved in water to form a homogeneously dispersed mixed liquid, and the polyurethane emulsion, thickener and long-chain alkyl silane coupling agent are homogeneously dispersed by the action of the wetting agent, so that an adhesive with a stable system and excellent adhesive performance is prepared.

[0025] In a second aspect, the present application provides a manufacturing process for a thermal insulation, waterproof, high strength packaging bag, and adopts the following technical solutions:

[0026] A manufacturing process for a thermally insulating, waterproof, high-strength packaging bag, comprising: Step S1: applying adhesive to one side of the heat insulating buffer layer to form a first adhesive layer, then attaching an outer paper layer, keeping warm, and drying; Step S2: applying adhesive to one side of the heat insulating buffer layer away from the outer paper layer to form a second adhesive layer, and then bonding the outer paper layer, keeping it warm, and drying it; Step S3 of applying a waterproofing agent to the inner paper layer to form an inner waterproof layer, applying a waterproofing agent to the outer paper layer to form an outer waterproof layer, and drying to produce a composite paper; and S4, cutting and combining the composite paper to manufacture a thermal insulation, waterproof, high strength packaging bag.

[0027] By adopting the above technical solution, a packaging bag having excellent heat retention performance, excellent waterproof performance, and resistance to wrinkles, deformation and breakage is manufactured. Effect of the Invention

[0028] As described above, the present application has the following beneficial effects.

[0029] 1. The thermal insulation, waterproof, high-strength packaging bag of the present application is composed of an outer waterproof layer, an outer paper layer, a first adhesive layer, a heat insulating buffer layer, a second adhesive layer, an inner paper layer and an inner waterproof layer, and has good thermal insulation and waterproof performance, is not easily wrinkled or damaged, has good protective effect on packaged goods, and has a wide range of applications.

[0030] 2. A first buffer structure is installed on one side of the outer waterproof layer close to the thermal insulation buffer layer, and a second buffer structure is installed on one side of the inner waterproof layer close to the thermal insulation buffer layer, so that the structures of the first buffer structure and the second buffer structure are the same, and the first buffer structure is composed of a plurality of convex parts, the horizontal height of the convex parts gradually increases from the central region of the outer paper layer along the peripheral edge region, and the distribution density of the convex parts gradually decreases from the central region of the outer paper layer along the peripheral edge region, thereby making the thickness of the first adhesive layer between the central region of the outer paper layer and the thermal insulation buffer layer thicker, but the thickness of the outer paper layer The thickness of the first adhesive layer between the peripheral edge region and the insulating buffer layer is thin, so that when the packaging bag is subjected to external pressure, the outer paper layer, the first adhesive layer, the insulating buffer layer, the second adhesive layer and the inner paper layer form a cooperative structure, which can evenly distribute the pressure and reduce the occurrence of wrinkles and breakage. The edge region of the packaging bag needs to wrinkle by itself during the assembly process, so the thickness of the peripheral edge region of the outer paper layer is controlled to be thick, which makes it easy to shape, and allows the packaging bag to maintain a three-dimensional shape, has cushioning performance, and is not easily deformed.

[0031] 3. The adhesive is prepared by using polyurethane emulsion, thickener, wetting agent, long-chain alkyl silane coupling agent and water, among which the thickener is composed of starch, diethylene glycol, acrylic ester copolymer and magnesium aluminum silicate, and the wetting agent is composed of oleylamine polyoxyethylene ether and polyvinyl alcohol, the thickener and the wetting agent generate a good synergistic effect and stably adsorb the polyurethane emulsion, the adhesive prepared thereby has good adhesion stability, and the first adhesive layer and the second adhesive layer formed after curing have good elasticity, which can further improve the strength and buffer performance of the packaging bag. [Brief description of the drawings]

[0032] [Figure 1] 1 is a schematic diagram of the interlayer structure of the composite paper of the thermal insulation, waterproof, high-strength packaging bag of Example 1 of the present application. [Diagram 2] 1 is a schematic diagram of the interlayer structure of the composite paper of the thermal insulation, waterproof, high-strength packaging bag of Example 4 of the present application. [Diagram 3]1 is a schematic diagram of the interlayer structure of the composite paper of the thermal insulation, waterproof, high-strength packaging bag of Example 5 of the present application. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] The present invention will be described in further detail below with reference to Figures 1 to 3 and examples.

[0034] The following are the origins and specifications of some of the raw materials in the present application. The raw materials in the preparation examples and examples of the present application can all be obtained commercially. The raw materials used in the present application include, but are not limited to, the specific model numbers and manufacturers disclosed below. Any raw materials having the same specification parameters and performance can be used. 1. Regarding starch, corn starch, industrial grade, content is 99%; 2. Regarding acrylic ester copolymers, the brand is Carbomer U21 and Lu Borun. 3. Magnesium aluminum silicate: 325 mesh, content 99%, pH=6.3, whiteness 90%; 4. Kaolin: Calcined kaolin, 325 mesh, density 2.54-2.60g / cm 3 and 5. The polyurethane emulsion is Bayer brand, the content is 40-50%, the viscosity at 25 degrees Celsius is 700-1500mPa s, the pH is 7-9, and the density is 1.04-1.09g / cm 3 and 6. Regarding oleylamine polyoxyethylene ether, it is oleylamine polyoxyethylene (2) ether, 7. Regarding polyvinyl alcohol, the molecular weight is 25,000 to 35,000 Daltons, the content is 99%, and the pH is 4.5 to 6.5.

[0035] Preparation examples of thickeners Preparation Example 1 Preparation Example 1 discloses a thickener, which is prepared by the following steps: In A1, 1 kg of starch is added to 8 kg of water, 0.03 kg of 1 mol / L hydrochloric acid solution is added dropwise, the temperature is raised to 65°C, and the mixture is stirred for 30 minutes to prepare a starch hydrolysate; In A2, 0.02 kg of diethylene glycol, 0.01 kg of carbomer U21 and 0.1 kg of magnesium aluminum silicate were added to the starch hydrolysate, and the mixture was stirred at a stirring speed of 300 r / min for 20 minutes to prepare a thickener.

[0036] Preparation Examples 2-3 Preparation Examples 2 and 3 differ from Preparation Example 1 in that the amounts of raw materials used and preparation conditions are different. See Table 1 below for details.

[0037] JPEG0007579031000002.jpg125162

[0038] Comparative Preparation Example 1 Comparative Preparation 1 differs from Preparation Example 1 in that diethylene glycol is replaced with the same amount of polyethylene glycol 400, and the rest is the same as Preparation Example 1.

[0039] Comparative Preparation Example 2 Comparative Preparation 2 is different from Preparation 1 in that magnesium aluminum silicate is replaced with an equal amount of kaolin, and the rest is the same as Preparation 1.

[0040] Comparative Preparation Example 3 The difference between Comparative Preparation 3 and Preparation Example 1 is that Carbomer U21 is replaced with the same amount of hydroxyethyl methylcellulose, and the rest is the same as Preparation Example 1.

[0041] Comparative Preparation Example 4 The difference between Comparative Preparation 4 and Preparation Example 1 is that magnesium aluminum silicate is replaced with the same amount of Carbomer U21, and the rest is the same as Preparation Example 1.

[0042] Adhesive preparation example Preparation Example 4 Preparation Example 4 discloses an adhesive, which is prepared by the following steps: In B1, 0.4 kg of polyvinyl alcohol is added to 2 kg of water as a wetting agent, and the mixture is stirred for 20 minutes at a temperature of 60°C and a stirring speed of 300 r / min to prepare a homogeneous mixture. In B2, 4 kg of polyurethane emulsion, 1.2 kg of hydroxyethylmethylcellulose as a thickener, and 0.05 kg of dodecyltrimethoxysilane as a silane coupling agent were added to the mixed liquid, and the mixture was stirred at a stirring speed of 500 r / min for 30 minutes to prepare an adhesive.

[0043] Preparation Examples 5-6 Preparation Examples 5 and 6 differ from Preparation Example 1 in that the amounts of raw materials used and preparation conditions are different. See Table 2 below for details.

[0044] JPEG0007579031000003.jpg171157

[0045] Preparation Examples 7 to 13 Preparation Examples 7 to 13 differ from Preparation Example 4 in that the origin of the thickener is different. See Table 3 below for details.

[0046] JPEG0007579031000004.jpg86145

[0047] Preparation Example 14 Preparation Example 14 differs from Preparation Example 7 in that the wetting agent is different; the wetting agent in Preparation Example 14 is composed of oleylamine polyoxyethylene ether and polyvinyl alcohol, the amount of oleylamine polyoxyethylene ether used is 0.33 kg, and the amount of polyvinyl alcohol used is 0.07 kg; otherwise, it is the same as Preparation Example 7.

[0048] Preparation Example 15 The difference between Preparation Example 15 and Preparation Example 7 is that the wetting agent in Preparation Example 15 is composed of oleylamine polyoxyethylene ether and polyvinyl alcohol, the amount of oleylamine polyoxyethylene ether used is 0.25 kg, and the amount of polyvinyl alcohol used is 0.15 kg; otherwise, it is the same as Preparation Example 7.

[0049] Comparative Preparation Example 5 Comparative Preparation 5 is different from Preparation 7 in that the long-chain alkylsilane coupling agent is replaced with the same amount of methyltriethoxysilane coupling agent.

[0050] Example 1 Example 1 discloses a thermal insulation waterproof high strength packaging bag, which is manufactured by cutting and assembling composite paper. See FIG. 1. The composite paper includes an outer waterproof layer, an outer paper layer, a heat insulating buffer layer, an inner paper layer and an inner waterproof layer, which are sequentially pasted together. The outer paper layer and the heat insulating buffer layer are pasted together via a first adhesive layer, and the inner paper layer and the heat insulating buffer layer are pasted together via a second adhesive layer. The outer waterproof layer and the inner waterproof layer are PE waterproof layers. The outer paper layer and the inner paper layer are both kraft paper. The thickness of the kraft paper is 0.1-1 mm. The thickness of the kraft paper in this embodiment is 0.5 mm. The heat insulating buffer layer is aerogel cotton, silicone cotton, urethane, etc. The heat insulating buffer layer in this embodiment is silicone cotton. The thickness of the heat insulating buffer layer is 0.1-2 mm. The thickness of the heat insulating buffer layer in this embodiment is 1 mm. The first adhesive layer and the second adhesive layer are both elastic adhesive layers, which are prepared by curing the adhesive.

[0051] The thermal insulation, waterproof, high-strength packaging bag is manufactured by the following steps: In S1, a commercially available adhesive was applied to one side of the thermal insulation buffer layer with a coating amount of 30 g / m 2 The temperature is controlled to 40°C to form a first adhesive layer, and then the outer paper layer is laminated. The temperature is kept at 40°C for 20 minutes, and then the sheet is dried at 100°C. In S2, a commercially available adhesive was applied to the side of the thermal insulation cushioning layer away from the outer paper layer, with the amount of adhesive applied being 30 g / m2 The temperature is controlled to 40°C, a second adhesive layer is formed, and then the outer paper layer is laminated. The temperature is kept at 40°C for 20 minutes, and then the sheet is dried at 100°C. In S3, the PE material is melted to form a PE waterproofing agent, which is cast onto the inner paper layer to form an inner waterproof layer, and the PE waterproofing agent is applied onto the outer paper layer to form an outer waterproof layer. The amount of the PE waterproofing agent applied is 10 g / m 2 The temperature is controlled to 20°C, and the drying time is 30 minutes to produce composite paper. In S4, the composite paper is cut and combined to produce a thermal insulation, waterproof, high strength packaging bag; The commercially available adhesive is a water-based polyurethane adhesive, the brand is Jimbo Namie Technology, the viscosity is 100-450cps at 25 degrees Celsius, the solid content is 40%, and the pH is 7.0-8.5. The PE material is low density polyethylene, the brand is Tao Chemical, the model number is 4203, Aerogel cotton has a thermal conductivity of 0.02W / (m K), a compressive strength of 18MPa, and a density of 180-220kg / m 3 and Silicone cotton has a thermal conductivity of 0.02W / (m K) and a density of 120-160kg / m 3 and The urethane is EPE foam cotton, with a thermal conductivity of 0.02W / (m K) and a density of 28-35kg / m 3 It is.

[0052] (Examples 2 to 3) Examples 2 and 3 differ from Example 1 in that the manufacturing process parameters are different and the origin of the adhesive is different; specifically, see Table 4 below.

[0053] JPEG0007579031000005.jpg165159

[0054] Example 4 The difference between Example 4 and Example 1 is that, as shown in Figure 2, the structure of the composite paper is different, one side of the outer waterproof layer close to the insulating buffer layer has a first buffer structure, and one side of the inner waterproof layer close to the insulating buffer layer has a second buffer structure, the first buffer structure and the second buffer structure are installed symmetrically, among which the first buffer structure is composed of several convex parts, the horizontal height of the convex parts gradually increases from the central region of the outer paper layer along the peripheral edge region, the first buffer structure and the second buffer structure are the same, and the distribution density of the convex parts is the same, and the rest is the same as Example 1.

[0055] Example 5 The difference between Example 5 and Example 4 is that, as shown in Figure 3, in Example 4, the distribution density of the convex portions gradually decreases from the central region of the outer paper layer along the peripheral edge region, and the distribution density of the convex portions of the inner paper layer is the same as that of the outer paper layer; otherwise, it is the same as Example 4.

[0056] (Examples 6 to 18) Examples 6 to 18 differ from Example 5 in that the origin of the adhesive is different. See Table 5 below for details.

[0057] JPEG0007579031000006.jpg164138

[0058] Performance Detection Test The performance tests were carried out on the heat-insulating, waterproof, high-strength packaging bags produced in Examples 1 to 18 as follows: (1) Folding endurance test According to the test method in GB / T 13024-2003, the folding endurance (unit: times) of the thermal insulation waterproof high strength packaging bag is tested, and the detection results are recorded. (2) Destruction resistance test Based on the test method in GB / T 13024-2003, the fracture resistance index of the thermal insulation, waterproof, high strength packaging bag (unit: kPa m 2 / g), detect and record the detection results, (3) Peel strength test Refer to the test method in GB / T 34444-2017 to test the peel strength (unit: N / cm) of the thermal insulation waterproof high strength packaging bag, and detect and record the detection results. The following is performance test data of the thermal insulation, waterproof, high-strength packaging bags produced in Examples 1 to 18. For details, see Table 6 below.

[0059] JPEG0007579031000007.jpg145165

[0060] As can be seen with reference to Examples 1 to 5 and Table 6, the first cushioning structure of the outer paper layer and the second cushioning structure of the inner paper layer of the present application cooperate with the insulating cushioning layer to improve the strength of the packaging bag produced, the interlayer adhesion is more stable, and wrinkles and deformation are less likely to occur. The convex parts in Example 2 are uniformly distributed, while the distribution density of the convex parts in Example 3 decreases in order from the central region to the peripheral edge region. As can be seen from the data, the peel strength in Example 2 is slightly higher than that in Example 3, and it may be more advantageous to use the uniformly distributed convex parts for bonding, but the folding resistance and fracture resistance index in Example 2 are both obviously higher than those in Example 3. The difference in the distribution density of the convex parts can improve the strength of the packaging bag produced. Overall, the performance of the packaging bag in Example 3 is better.

[0061] As can be seen from Table 6 with reference to Examples 1 to 5 and Examples 6 to 15, the adhesive stability of the adhesive prepared using the thickener of the present application can be further improved, and the strength of the produced packaging bags can be improved. However, in Examples 12 to 15, when starch, diethylene glycol, carbomer U21, and magnesium aluminum silicate are not used, the strength of the produced packaging bags decreases and the folding resistance also decreases. However, it is explained that starch, diethylene glycol, carbomer U21, and magnesium aluminum silicate produce a good synergistic effect, and the strength of the produced packaging bags is good.

[0062] As can be seen from Examples 9 to 11 and Examples 16 to 17 and Table 6, the use of a suitable ratio of oleylamine polyoxyethylene ether and polyvinyl alcohol in the present application can produce a good synergistic effect with the thickener, which further improves the adhesive stability between the layers of the packaging bag and improves the strength of the manufactured packaging bag.

[0063] As can be seen from Examples 16 to 17 and Example 18 and Table 6, the strength of the packaging bag manufactured using the long-chain alkyl silane coupling agent can be improved.

[0064] To summarize the above, in the present application, a composite paper is formed by bonding together an outer waterproof layer, an outer paper layer, a first adhesive layer, an insulating cushioning layer, a second adhesive layer, an inner paper layer and an inner waterproof layer, and a packaging bag made from this composite paper has good heat retention performance, waterproof performance and strength, and is hardened using the adhesive of the present application to form a first adhesive layer and a second adhesive layer, which has good elasticity and adhesion and is less likely to wrinkle or deform when subjected to external pressure, and further improves the cushioning performance and strength of the packaging bag manufactured.

[0065] The specific examples are merely illustrative of the present application and are not intended to limit the present application. After reading this specification, a person skilled in the art may make modifications to the present examples as necessary without making any creative contribution thereto, but all such modifications are protected by the Patent Law as long as they fall within the scope of the claims of the present application. [Explanation of symbols]

[0066] 1...outer waterproof layer, 2...outer paper layer, 21...first cushioning structure, 3...first adhesive layer, 4...insulating cushioning layer, 5...second adhesive layer, 6...inner paper layer, 61...second cushioning structure, 7...inner waterproof layer.

Claims

1. The composite paper is made of composite paper, and the composite paper includes an outer waterproof layer, an outer paper layer, a heat insulating buffer layer, an inner paper layer, and an inner waterproof layer, which are laminated together in this order, the outer paper layer and the heat insulating buffer layer are laminated together with a first adhesive layer, the inner paper layer and the heat insulating buffer layer are laminated together with a second adhesive layer, and both the first adhesive layer and the second adhesive layer are elastic adhesive layers; A heat-retaining, waterproof, high-strength packaging bag characterized in that it has a first cushioning structure on one side of the outer waterproof layer near the insulating cushioning layer, the first cushioning structure being composed of several convex portions, and the horizontal height of the convex portions gradually increases from the central region of the outer paper layer along the peripheral edge region.

2. The thermal insulation, waterproof, high-strength packaging bag as described in claim 1, characterized in that the inner waterproof layer has a second buffer structure on one side close to the thermal insulation buffer layer, the first buffer structure and the second buffer structure are the same, and the first buffer structure and the second buffer structure are installed symmetrically.

3. 2. The heat-retaining, waterproof, high-strength packaging bag according to claim 1, wherein the distribution density of the protruding portions gradually decreases from the central region of the outer paper layer along the peripheral edge region.

4. 2. The heat-retaining, waterproof, high-strength packaging bag according to claim 1, wherein the heat-insulating buffer layer is any one of aerogel cotton, silicone cotton, and urethane.

5. The first adhesive layer and the second adhesive layer are both formed by curing an adhesive, and the adhesive comprises: Polyurethane emulsion 40-60 parts Thickener 12-22 parts Wetting agent: 4 to 8 parts Long-chain alkyl silane coupling agent 0.5 to 2 parts 2. The heat-retaining, waterproof, high-strength packaging bag according to claim 1, characterized in that it is prepared using raw materials of 20 to 30 parts by weight of water.

6. The thickener is Step A1, in which 10-18 parts of starch is added to 80-120 parts of water (by weight), 0.3-0.8 parts of 1-2 mol / L aqueous hydrochloric acid is added dropwise, the temperature is raised to 65-85° C., and the mixture is stirred for 30-60 minutes to prepare a starch hydrolysate; and 6. The heat-retaining, waterproof, high-strength packaging bag according to claim 5, which is prepared by step A2 of adding 0.2 to 0.5 parts of diethylene glycol, 0.1 to 0.3 parts of an acrylic acid ester-based copolymer, and 1 to 3 parts of magnesium aluminum silicate to a starch hydrolysate, and uniformly stirring the mixture to prepare a thickener.

7. The heat-retaining, waterproof, high-strength packaging bag according to claim 5, characterized in that the wetting agent is composed of oleylamine polyoxyethylene ether and polyvinyl alcohol, and the weight ratio of the oleylamine polyoxyethylene ether to the polyvinyl alcohol is 1:(0.2 to 0.6).

8. The adhesive is Step B1 of adding a wetting agent to water and stirring uniformly to prepare a mixed solution; The heat-retaining, waterproof, high-strength packaging bag according to any one of claims 5 to 7, characterized in that it is prepared by step B2, which includes adding a polyurethane emulsion, a thickener, and a long-chain alkyl silane coupling agent to the mixed liquid, stirring the mixture uniformly, and preparing an adhesive.

9. Step S1: applying adhesive to one side of the heat insulating buffer layer to form a first adhesive layer, attaching an outer paper layer, and keeping the layer warm and drying; Step S2: applying adhesive to one side of the heat insulating buffer layer away from the outer paper layer to form a second adhesive layer, and then bonding the inner paper layer, keeping it warm, and drying it; Step S3 of applying a waterproofing agent to the inner paper layer to form an inner waterproof layer, applying a waterproofing agent to the outer paper layer to form an outer waterproof layer, and drying to manufacture a composite paper; S4: cutting and combining the composite paper to manufacture a thermal insulation, waterproof, high strength packaging bag; A process for producing the heat-retaining, waterproof, high-strength packaging bag according to any one of claims 5 to 7.

Citation Information

Patent Citations

  • JP1974128688U

  • Insulating packaging material

    JP1984129770U

  • Paper container

    JP1993294341A

  • Resin composition for forming sealant layer and sealant film, laminate film and packaging medium using the same

    JP2020200392A