Method for operating electrolysis device and electrolysis system

By employing a capacitance ratio of 1.1:1 between cathode and anode and discharging to 0.1 V within 60 minutes, the electrolyzer mitigates electrode deterioration and gas purity issues in alkaline water electrolysis systems under fluctuating power, ensuring stable operation.

JP7579086B2Active Publication Date: 2024-11-07ASAHI KASEI KOGYO KABUSHIKI KAISHA
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2020141204
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-08-24
Publication Date
2024-11-07
Estimated Expiration
2040-08-24

AI Technical Summary

Technical Problem

Conventional electrolyzers experience electrode deterioration and gas purity issues due to reverse currents and potential convergence when power supply fluctuates, particularly in alkaline water electrolysis systems.

Method used

The method involves operating an electrolyzer with a capacitance ratio of cathode to anode of 1.1:1, discharging the electrolytic cell to 0.1 V or less within 60 minutes using an external load during the stop step, and employing a bipolar electrolytic cell design with specific electrode materials and configurations to minimize reverse current effects.

Benefits of technology

This approach effectively suppresses electrode deterioration and maintains gas purity by quickly dissipating potential differences across electrodes, reducing corrosion and gas mixing under fluctuating power conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579086000002
    Figure 0007579086000002
  • Figure 0007579086000003
    Figure 0007579086000003
  • Figure 0007579086000004
    Figure 0007579086000004
Patent Text Reader

Abstract

To provide an operational method of an electrolytic apparatus that can suppress the deterioration of an electrode under a fluctuating power supply.SOLUTION: An electrolytic apparatus of the present invention comprises an anode chamber having an anode and a cathode chamber having a cathode, both chambers being separated from each other by a diaphragm. The capacitance of the cathode is 1.1 times as large as or larger than that of the anode. The operational method of the electrolytic apparatus includes: an electrification step in which electrolysis of an electrolyte is performed in the anode and cathode chambers; and a stop step in which the electrolysis of the electrolyte is stopped in the anode and cathode chambers. The stop step includes a discharge step in which an electrolytic tank of the electrolytic apparatus is electrically connected to an external load.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for operating an electrolysis device and an electrolysis system. [Background technology]

[0002] 2. Description of the Related Art In recent years, in order to solve problems such as global warming caused by greenhouse gases such as carbon dioxide and dwindling reserves of fossil fuels, technologies that utilize renewable energy, such as wind power generation and solar power generation, have been attracting attention.

[0003] Renewable energy output is highly variable because it depends on weather conditions. As a result, it is not always possible to transport the electricity generated by renewable energy sources to the general power grid, and there are concerns about the social impacts of this, such as an imbalance in power supply and demand and instability in the power grid.

[0004] Therefore, research is being conducted into converting electricity generated from renewable energy sources into a form that can be stored and transported, and using this electricity.Specifically, research is being conducted into the generation of storable and transportable hydrogen through the electrolysis of water using electricity generated from renewable energy, and the use of hydrogen as an energy source or raw material.

[0005] Hydrogen is widely used industrially in oil refining, chemical synthesis, metal refining, etc., and in recent years, the possibility of its use is expanding in hydrogen stations for fuel cell vehicles (FCVs), smart communities, hydrogen power plants, etc. For this reason, there are high expectations for the development of technology to obtain hydrogen, especially from renewable energy sources.

[0006] Methods for electrolyzing water include solid polymer water electrolysis, high-temperature steam electrolysis, and alkaline water electrolysis. Alkaline water electrolysis is considered to be one of the most promising methods because it has been industrialized for several decades, can be carried out on a large scale, and is inexpensive compared to other water electrolysis systems.

[0007] However, in order to adapt alkaline water electrolysis as a means for storing and transporting energy in the future, it is necessary to enable water electrolysis by efficiently and stably utilizing electric power, the output of which varies greatly as described above, and there is a demand for resolving various issues related to electrolytic cells and devices for alkaline water electrolysis.

[0008] For example, in order to solve the problem of reducing the electrolysis voltage in alkaline water electrolysis and improving the power consumption rate of hydrogen production, it is well known that it is effective to employ, as the structure of the electrolysis cell, a structure called a zero-gap structure, which is a structure in which the gap between the diaphragm and the electrodes is substantially eliminated (see, for example, Patent Documents 1 and 2). In the zero-gap structure, the generated gas is quickly released to the side opposite the diaphragm of the electrode through the pores of the electrode, thereby reducing the distance between the electrodes and minimizing the occurrence of gas accumulation near the electrodes, thereby reducing the electrolysis voltage. The zero-gap structure is extremely effective in reducing the electrolysis voltage, and is adopted in various electrolysis devices. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 5553605 [Patent Document 2] International Publication No. 2015 / 098058 Summary of the Invention [Problem to be solved by the invention]

[0010] However, in conventional electrolysis devices, when exposed to fluctuating power sources such as solar power and wind power, charges accumulated in the anode and cathode during electrolysis operation may flow in the opposite direction to the anode and cathode when electrolysis is stopped, causing a reverse current. As a result, when the electrolysis is stopped, a reverse current occurs, and in the process of the potential converging, the potential of the anode and cathode passes through a certain potential range over a certain period of time, where the electrode itself corrodes due to the oxidation-reduction reaction of the anode and cathode during normal electrolysis operation, raising concerns that each electrode may deteriorate due to the stopping and operation of electrolysis [Concern 1]. In addition, in the process of the reverse current flowing and the potential converging, hydrogen gas is generated in the anode chamber and oxygen gas is generated in the cathode chamber, which may deteriorate the gas purity [Concern 2]. In particular, in conventional alkaline water electrolysis cells, a large current flows near the center due to the potential gradient of the electrolytic cell, making them more susceptible to the effects of the reverse current, and resolving [Concern 1] and [Concern 2] near the center of the electrolytic cell was a challenge.

[0011] Therefore, the present invention aims to suppress the deterioration of electrodes [Concern 1] and the deterioration of gas purity [Concern 2] under variable power supply conditions. [Means for solving the problem]

[0012] The gist of the present invention is as follows. (1) A method for operating an electrolytic device comprising an anode chamber having an anode and a cathode chamber having a cathode separated from each other by a diaphragm, the cathode having an electric capacity being 1.1 times or more the electric capacity of the anode, the method comprising: a current application step in which electrolysis of an electrolyte in the anode chamber and the cathode chamber is performed; and a stop step in which electrolysis of the electrolyte in the anode chamber and the cathode chamber is stopped, the method comprising: a discharge step in which an electrolytic cell of the electrolytic device is electrically connected to an external load during the stop step. (2) The capacitance of the anode is 10,000 C / m 2 The capacitance of the cathode is 1000 C / m or less. 2 The method for operating an electrolytic device according to (1) above, (3) The method for operating an electrolytic device according to (1) or (2), wherein the discharge step reduces the discharge voltage to 0.1 V or less within 60 minutes. (4) The method for operating an electrolytic device according to any one of (1) to (3), wherein the discharging step is carried out when a voltage of the electrolytic cell falls below a predetermined threshold in the stopping step. (5) The method for operating the electrolytic apparatus according to any one of (1) to (4), characterized in that the electrolytic cell of the electrolytic apparatus is of a bipolar type, has a plurality of electrolytic cells each of which is composed of one of the anode chambers and one of the cathode chambers, and the discharging step is carried out in some of the plurality of electrolytic cells. (6) The method for operating the electrolytic device according to any one of (1) to (5), comprising 30 or more electrolytic cells each including one anode chamber and one cathode chamber. (7) The method for operating the electrolysis apparatus according to any one of (1) to (6), wherein the anode contains at least one nickel compound selected from the group consisting of nickel oxide, metallic nickel, nickel hydroxide, and a nickel alloy. (8) The method for operating the electrolysis apparatus according to any one of (1) to (7), wherein the anode does not contain any distinct catalytic layer other than a nickel compound derived from a base material containing nickel as a main component. (9) The method for operating the electrolytic apparatus according to any one of (1) to (8), wherein the anode has a thickness in the range of 0.1 mm to 3.0 mm. (10) The method for operating the electrolytic device according to any one of (1) to (7), characterized in that the cathode contains at least one Pt group compound selected from the group consisting of Ru-La-Pt based, Ru-Ce based, Pt-Ce based, Pt-Ir based, Ir-Pt-Pd based, Pt-Pd based, and Pt-Ni based compounds. (11) The method for operating the electrolytic device according to any one of (1) to (10), wherein the power supply is a variable power supply. (12) The method for operating the electrolysis apparatus according to any one of (1) to (11), wherein the power source is a variable power source, and the method includes a step of stopping power supply. (13) An electrolytic device having an anode chamber having an anode and a cathode chamber having a cathode, which are separated from each other by a diaphragm, the electric capacity of the cathode being 1.1 times or more the electric capacity of the anode, and the electric capacity of the anode being 10,000 C / m or more.2 The capacitance of the cathode is 1000 C / m or less. 2 The electrolysis system according to the above, characterized in that the electrolytic cell of the electrolysis device is electrically connected to an external load. (14) The resistance of the external load is 0.02 to 2 Ωm 2 The electrolysis system according to (13), characterized in that it is a 1 / Cell. Effect of the Invention

[0013] According to the present invention, it is possible to provide a method for operating an electrolysis device that can suppress the deterioration of electrodes [concern 1] and the deterioration of gas purity [concern 2] under a variable power supply. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a diagram showing an outline of an electrolysis apparatus that can be used in the method for operating the electrolysis apparatus of the present embodiment. [Diagram 2] FIG. 2 is a side view showing an example of an entire electrolytic cell of the electrolytic apparatus shown in FIG. [Diagram 3] FIG. 2 is a perspective view showing an electrolysis chamber, a header, and a conduit of an external header type electrolysis cell, which is an example of the electrolysis cell of the electrolysis apparatus shown in FIG. 1. [Figure 4] FIG. 2 is a plan view showing an external header type electrolytic cell, which is an example of the electrolytic cell of the electrolysis apparatus shown in FIG. [Figure 5A] FIG. 2 is a schematic cross-sectional view of the cathode chamber of an example of an electrolytic cell of the electrolysis device of FIG. 1, showing the cathode chamber in a cross section along a plane along the vertical direction and a direction perpendicular to the cathode. [Figure 5B] FIG. 2 is a diagram showing a cathode chamber of an example of an electrolytic cell of the electrolysis device of FIG. 1, and is a schematic plan view showing the cathode chamber. [Figure 6] FIG. 5C is a schematic cross-sectional view showing an example in which the cathode chamber shown in FIGS. 5A and 5B is modified, the cross-section being taken along a plane along a vertical direction and a direction perpendicular to the cathode. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Hereinafter, an embodiment of the present invention (hereinafter, referred to as "the present embodiment") will be described in detail. Note that the present invention is not limited to the following embodiment, and can be modified in various ways within the scope of the gist of the present invention.

[0016] FIG. 1 shows an electrolysis apparatus that can be used in the method for operating the electrolysis apparatus according to this embodiment, and an overview of the electrolysis apparatus according to this embodiment.

[0017] (electrolyzer) 1, the electrolysis device 70 includes an electrolytic cell 50, a liquid feed pump 71 for circulating the electrolytic solution, a gas-liquid separation tank 72 for separating the electrolytic solution from hydrogen and / or oxygen, and a water supply device 73 for replenishing water consumed by electrolysis. More specifically, the electrolysis device 70 according to this embodiment includes an anode chamber 5a having an anode 2a and a cathode chamber 5c having a cathode 2c, which are separated from each other by a diaphragm 4 (see FIGS. 2 and 3).

[0018] First, among the components of the electrolysis device 70, the electrolytic cell 50 will be mainly described.

[0019] (electrolytic cell) The electrolytic cell 50 in the electrolysis device 70 is not particularly limited and may be either a monopolar type or a bipolar type, but as shown in FIG. 1 etc., a bipolar type electrolytic cell is industrially preferred.

[0020] The bipolar type is one of the methods for connecting multiple cells to a power source, in which multiple bipolar elements 60, one side of which is an anode 2a and the other side of which is a cathode 2c, are arranged in the same direction and connected in series, and only both ends are connected to the power source. The bipolar electrolytic cell 50 has the characteristic of being able to reduce the current of the power source, and can produce large amounts of compounds and specified substances by electrolysis in a short period of time. If the power output is the same, a constant current, high voltage power supply is cheaper and more compact, so from an industrial perspective, the bipolar type is preferable to the monopolar type.

[0021] As shown in FIG. 2 , the bipolar electrolytic cell 50 of the electrolysis device 70 is a bipolar electrolytic cell 50 in which a plurality of bipolar elements 60, each of which includes an anode 2a, a cathode 2c, a partition wall 1 separating the anode 2a and the cathode 2c, and an outer frame 3 bordering the partition wall 1, are stacked with a diaphragm 4 sandwiched therebetween.

[0022] ((Duplex element)) 2, a bipolar element 60 used in a bipolar electrolytic cell 50 of an example of the electrolysis device 70 includes a partition wall 1 that separates an anode 2a and a cathode 2c, and an outer frame 3 that borders the partition wall 1. More specifically, the partition wall 1 is conductive, and the outer frame 3 is provided so as to surround the partition wall 1 along the outer edge of the partition wall 1.

[0023] In the electrolysis device 70, the bipolar element 60 may usually be used so that a given direction D1 along the partition wall 1 is the vertical direction. Specifically, when the partition wall 1 has a rectangular shape in a plan view as shown in Figs. 3 and 4, the bipolar element 60 may be used so that the given direction D1 along the partition wall 1 is the same direction as the direction of one of two pairs of opposing sides (see Figs. 2 and 3).

[0024] As shown in FIG. 2, the bipolar electrolytic cell 50 is constructed by stacking a required number of bipolar elements 60 . In the example shown in Fig. 2, the bipolar electrolytic cell 50 has a fast head 51g, an insulating plate 51i, and an anode terminal element 51a arranged in this order from one end, and further has an anode side gasket portion 7, a diaphragm 4, a cathode side gasket portion 7, and a bipolar element 60 arranged in this order. At this time, the bipolar element 60 is arranged so that the cathode 2c faces the anode terminal element 51a side. The anode side gasket portion 7 to the bipolar element 60 are arranged repeatedly as many times as necessary for the designed production volume. After the anode side gasket portion 7 to the bipolar element 60 are arranged repeatedly as many times as necessary, the anode side gasket portion 7, the diaphragm 4, and the cathode side gasket portion 7 are arranged again, and finally the cathode terminal element 51c, the insulating plate 51i, and the loose head 51g are arranged in this order. The bipolar electrolytic cell 50 is integrated by clamping the entire cell using a clamping mechanism such as a tie rod type 51r (see FIG. 2) or a hydraulic cylinder type. The arrangement of the bipolar electrolytic cell 50 can be arbitrarily selected from either the anode 2a side or the cathode 2c side, and is not limited to the above order.

[0025] 2, in the bipolar electrolytic cell 50, the bipolar element 60 is disposed between the anode terminal element 51a and the cathode terminal element 51c. The diaphragms 4 are disposed between the anode terminal element 51a and the bipolar element 60, between adjacent bipolar elements 60, and between the bipolar element 60 and the cathode terminal element 51c.

[0026] In the bipolar electrolytic cell 50, as shown in Figs. 3 and 4, the partition wall 1, the outer frame 3 and the diaphragm 4 define an electrode chamber 5 through which the electrolyte passes.

[0027] In this embodiment, in particular, the portion between the partition walls 1 between two adjacent bipolar elements 60 and the portion between the partition walls 1 between the adjacent bipolar elements 60 and the terminal element in the bipolar electrolytic cell 50 are referred to as the electrolytic cell 65. The electrolytic cell 65 includes the partition wall 1, anode chamber 5a, anode 2a, and diaphragm 4 of one element, and the cathode 2c, cathode chamber 5c, and partition wall 1 of the other element.

[0028] Specifically, the electrode chamber 5 has, at the boundary with the outer frame 3, an electrolyte inlet 5i for introducing the electrolyte into the electrode chamber 5 and an electrolyte outlet 5o for discharging the electrolyte from the electrode chamber 5. More specifically, the anode chamber 5a is provided with an anolyte inlet 5ai for introducing the electrolyte into the anode chamber 5a and an anolyte outlet 5ao for discharging the electrolyte from the anode chamber 5a. Similarly, the cathode chamber 5c is provided with a cathode electrolyte inlet 5ci for introducing the electrolyte into the cathode chamber 5c and a cathode electrolyte outlet 5co for discharging the electrolyte from the cathode chamber 5c.

[0029] The anode chamber 5a and the cathode chamber 5c may each be provided with an internal distributor for uniformly distributing the electrolyte solution on the electrode surface inside the electrolytic cell 50. The electrode chamber 5 may also be provided with a baffle plate having a function of restricting the flow of the electrolyte solution inside the electrolytic cell 50. Furthermore, the anode chamber 5a and the cathode chamber 5c may each be provided with a protrusion for creating a Karman vortex in order to uniformize the concentration and temperature of the electrolyte solution inside the electrolytic cell 50 and to promote degassing of gas adhering to the electrode 2 and the diaphragm 4.

[0030] The bipolar electrolytic cell 50 is provided with a header 10 on the outside of the outer frame 3, the header 10 communicating with the electrode chamber 5 (see Figs. 3 and 4).

[0031] 3 and 4 , a header 10, which is a pipe for distributing or collecting gas and electrolyte, is attached to a bipolar electrolytic cell 50. In detail, the header 10 comprises an inlet header for introducing electrolyte into the electrode chamber 5 and an outlet header for discharging gas and electrolyte from the electrode chamber 5. In one example, an anode inlet header 10Oai for introducing electrolyte into the anode chamber 5a and a cathode inlet header 10Oci for introducing electrolyte into the cathode chamber 5c are provided below the outer frame 3 at the edge of the partition 1, and similarly, an anode outlet header 10Oao for discharging electrode electrolyte from the anode chamber 5a and a cathode outlet header 10Oco for discharging electrolyte from the cathode chamber 5c are provided on the side of the outer frame 3 at the edge of the partition 1. In addition, in one example, in the anode chamber 5a and the cathode chamber 5c, an inlet header and an outlet header are provided to face each other with the center of the electrode chamber 5 in between.

[0032] In particular, the bipolar electrolytic cell 50 in this example employs an external header 10O type in which the bipolar electrolytic cell 50 and the header 10 are independent of each other. FIG. 4 is a plan view showing an example of an electrolytic cell of an external header type electrolytic device.

[0033] Representative examples of the arrangement of the header 10 attached to the bipolar electrolytic cell shown in Figs. 2 to 4 include an internal header type and an external header 10O type, but either type may be adopted in the present invention, and there is no particular limitation.

[0034] 3 and 4, a conduit 20 is attached to the header 10, which is a pipe for collecting the gas and electrolyte distributed or collected in the header 10. In detail, the conduit 20 is composed of a distribution pipe communicating with the inlet header and a collection pipe communicating with the outlet header. In one example, an anode liquid distribution pipe 20Oai communicating with the anode inlet header 10Oai, and a cathode liquid distribution pipe 20Oci communicating with the cathode inlet header 10Oci are provided at the lower part of the outer frame 3, and similarly, an anode liquid collection pipe 20Oao communicating with the anode outlet header 10Oao, and a cathode liquid collection pipe 20Oco communicating with the cathode outlet header 10Oco are provided at the side of the outer frame 3.

[0035] In the anode chamber 5a and the cathode chamber 5c, the inlet header and the outlet header are preferably provided at positions separated from each other from the viewpoint of water electrolysis efficiency and are preferably provided opposite each other across the center of the electrode chamber 5. When the partition wall 1 has a rectangular shape in a plan view as shown in Figs. 3 and 4, the inlet header and the outlet header are preferably provided symmetrically about the center of the rectangle.

[0036] Typically, as shown in Figures 3 and 4, one anode inlet header 10Oai, one cathode inlet header 10Oci, one anode outlet header 10Oao, and one cathode outlet header 10Oco are provided in each electrode chamber 5, but this is not limited to this and multiple headers may be provided in each electrode chamber 5. In addition, typically, one anode distribution pipe 20Oai, one cathode distribution pipe 20Oci, one anode collection pipe 20Oao, and one cathode collection pipe 20Oco are provided for each electrode chamber 5, but this is not limited to this and they may be shared by multiple electrode chambers 5.

[0037] In the illustrated example, the partition 1 having a rectangular shape in a plan view and the diaphragm 4 having a rectangular shape in a plan view are arranged in parallel, and the inner surface of the partition 1 side of the rectangular parallelepiped outer frame provided on the end edge of the partition 1 is perpendicular to the partition 1, so that the shape of the electrode chamber 5 is rectangular. However, in the present invention, the shape of the electrode chamber 5 is not limited to the rectangular parallelepiped in the illustrated example, and may be appropriately modified depending on the planar shapes of the partition 1 and the diaphragm 4, the angle between the partition 1 and the inner surface of the outer frame 3 on the partition 1 side, etc., and may be any shape as long as the effects of the present invention can be obtained.

[0038] The positional relationship between the electrode chamber 5 and the header 10 is not particularly limited, and as shown in Figures 3 and 4, when the bipolar element 60 is used so that a given direction D1 along the partition 1 is vertical, the inlet header may be located below or to the side of the electrode chamber 5 (below in the illustration), the outlet header may be located above or to the side of the electrode chamber 5 (side in the illustration), and the distribution pipe communicating with the inlet header may be located below or to the side of the electrode chamber 5 (below in the illustration), and the collection pipe communicating with the outlet header may be located above or to the side of the electrode chamber 5 (side in the illustration).

[0039] The extending direction of the header 10 is not particularly limited.

[0040] The extension direction of the conduits 20 is not particularly limited, but as shown in an example in Figures 3 and 4, from the viewpoint of easily obtaining the effects of the present invention, it is preferable that the distribution pipes (anode distribution pipe 20Oai, cathode distribution pipe 20Oci) and collection pipes (anode collection pipe 20Oao, cathode collection pipe 20Oco) each extend in a direction perpendicular to the partition wall 1, and it is even more preferable that all of the conduits 20 extend in a direction perpendicular to the partition wall 1.

[0041] The bipolar electrolytic cell 50 of the electrolysis device 70 may be provided with a plurality of baffles 6 arranged parallel to a given direction D1 along the partition wall 1 in order to reduce convection occurring in the electrolysis chamber 5 due to turbulence in the gas-liquid flow in the electrolysis chamber 5 and suppress a local increase in the temperature of the electrolyte.

[0042] The bipolar electrolytic cell 50 of the electrolysis device 70 preferably has 29 to 500 bipolar elements 60, more preferably has 50 to 500 bipolar elements 60, further preferably has 70 to 300 bipolar elements 60, and particularly preferably has 100 to 200 bipolar elements 60. A decrease in the logarithm reduces the effect of leakage current on gas purity, while an increase in the logarithm makes it difficult to uniformly distribute the electrolyte to each electrolytic cell 65. If the logarithm is below the lower limit or above the upper limit, it becomes difficult to simultaneously achieve the effect of reducing self-discharge that occurs when power supply is stopped, thereby enabling stabilization of the electrical control system, and the effect of enabling highly efficient storage of electricity, specifically, the effect of enabling reduction in pump power and reduction in leakage current. Furthermore, if the number (number of pairs) of bipolar elements 60 is too large, it may become difficult to manufacture the electrolytic cell 50, and if a large number of bipolar elements 60 with poor manufacturing precision are stacked, the sealing surface pressure is likely to become uneven, making it easy for electrolyte leakage or gas leakage to occur.

[0043] In the electrolysis device 70, the multiple elements 60 are preferably stacked with the diaphragm 4 sandwiched between them while being insulated from each other. In this manner, the elements 60 are insulated from each other, and therefore it is possible to prevent the charge accumulated in each element 60 in the current application step (a step in which electrolysis of the electrolyte is performed) from affecting the other elements 60 in the stop step (a step in which electrolysis of the electrolyte is stopped). Specifically, the elements 60 are preferably insulated from one another between the outer frames 3 of the elements 60, and this can be achieved, for example, by improving the insulation of the gaskets 7 disposed between the elements 60. Moreover, the insulation here preferably means that the insulation resistance between the elements 60 is 1 MΩ or more.

[0044] The bipolar electrolytic cell 50 of the electrolysis device 70 preferably has 30 or more electrolytic cells 65, more preferably has 100 or more electrolytic cells 65, and even more preferably has 150 to 200 electrolytic cells 65. In an electrolysis device 70 having a plurality of electrolytic cells 65, the reverse current flowing through each electrolytic cell 65 is relatively large in the electrolytic cell 65 at the center and relatively small in the electrolytic cell 65 at the end. Therefore, when the number of electrolytic cells 65 is 30 or more, the operation method of the electrolysis device 70 according to this embodiment described below can be suitably applied.

[0045] The components of the bipolar electrolytic cell 50 of the electrolysis device 70 will be mainly described in detail below. In addition, preferred embodiments for enhancing the effects of the present invention will be described in detail below.

[0046] -Bulkhead- The shape of the partition wall 1 may be a plate shape having a predetermined thickness, but is not particularly limited.

[0047] In addition, the partition 1 may usually be used so that a given direction D1 along the partition 1 is the vertical direction. Specifically, when the partition 1 has a rectangular shape in a plan view as shown in Figures 3 and 4, the partition 1 may be used so that a given direction D1 along the partition 1 is the same direction as the direction of one of two pairs of opposing sides.

[0048] The material of the partition 1 is preferably a conductive material from the viewpoint of realizing a uniform supply of power, and is preferably nickel, a nickel alloy, mild steel, or a nickel alloy plated with nickel from the viewpoint of alkali resistance and heat resistance.

[0049] -electrode- In hydrogen production by alkaline water electrolysis, reducing energy consumption, specifically, reducing the electrolysis voltage, is a major issue. Since this electrolysis voltage is highly dependent on the electrodes 2, the performance of both electrodes 2 is important.

[0050] The electrolysis voltage for alkaline water electrolysis is divided into the theoretically required voltage for water electrolysis, the overvoltage for the anode reaction (oxygen generation), the overvoltage for the cathode reaction (hydrogen generation), and the voltage due to the distance between the electrodes 2, the anode 2a and the cathode 2c. Here, overvoltage refers to the voltage that must be applied in excess of the theoretical decomposition potential when passing a certain current, and its value depends on the current value. When passing the same current, power consumption can be reduced by using an electrode 2 with a lower overvoltage.

[0051] In order to achieve a low overvoltage, the electrode 2 must have high electrical conductivity, high oxygen generating capacity (or hydrogen generating capacity), and high wettability of the surface of the electrode 2 with the electrolyte.

[0052] As the electrode 2 for alkaline water electrolysis, in addition to having a low overvoltage, corrosion of the base material and catalytic layer of the electrode 2, loss of the catalytic layer, dissolution in the electrolyte, adhesion of inclusions to the diaphragm 4, etc. are unlikely to occur, even when an unstable current such as that from renewable energy is used.

[0053] The electrode 2 is preferably a porous body in order to increase the surface area used for electrolysis and to efficiently remove gas generated by electrolysis from the surface of the electrode 2. In particular, in the case of a zero gap electrolytic cell, it is necessary to degas the gas generated from the back side of the surface in contact with the diaphragm 4, so that the surface of the electrode 2 opposite to the surface in contact with the membrane is preferably perforated.

[0054] Examples of the porous body include plain woven mesh, punched metal, expanded metal, and metal foam.

[0055] The electrode 2 may be the substrate itself, or may have a highly reactive catalyst layer on the surface of the substrate, but is preferably one having a highly reactive catalyst layer on the surface of the substrate.

[0056] The material of the substrate is not particularly limited, but mild steel, stainless steel, nickel, and nickel-based alloys are preferred in terms of resistance to the usage environment.

[0057] The catalytic layer of the anode 2a is preferably one having high oxygen generating ability, and nickel, cobalt, iron, platinum group elements, etc. can be used. In order to achieve the desired activity and durability, the catalytic layer can be formed as a simple metal, a compound such as an oxide, a composite oxide or alloy consisting of multiple metal elements, or a mixture thereof. An organic substance such as a polymer may be included in order to improve durability and adhesion to the substrate.

[0058] The catalytic layer of the cathode 2c is preferably one having high hydrogen generating ability, and nickel, cobalt, iron, platinum group elements, etc. can be used. In order to achieve the desired activity and durability, the catalytic layer can be formed as a simple metal, a compound such as an oxide, a composite oxide or alloy made of multiple metal elements, or a mixture of these. An organic substance such as a polymer material may be included in order to improve durability and adhesion to the substrate.

[0059] Methods for forming a catalyst layer on a substrate include plating, thermal spraying such as plasma spraying, pyrolysis in which a precursor layer solution is applied to a substrate and then heated, a method in which a catalyst substance is mixed with a binder component and fixed to the substrate, and vacuum film formation such as sputtering.

[0060] The capacitance of the cathode 2c is preferably larger than that of the anode 2a. In this case, the capacitance of the cathode 2c is preferably 1.1 times or more the capacitance of the anode 2a. The capacitance of the anode 2a is, for example, 10000 C / m 2 The capacitance of the cathode 2c is preferably 1000 C / m or less, for example. 2 More preferably, it is equal to or greater than this.

[0061] When a catalyst layer is not formed, the increase in electrode overvoltage caused by the reverse current accompanying the termination of electrolysis is small. Therefore, if a high initial overvoltage due to the absence of a catalyst layer is acceptable, not forming a catalyst layer can be taken as one of the measures to maintain the performance of the electrolytic cell over the long term.

[0062] In alkaline water electrolysis, the effect of reducing overvoltage by forming a catalyst layer on a substrate is generally easier to obtain in hydrogen generation than in oxygen generation, and therefore forming a highly active catalyst on the cathode side is highly effective not only in reducing power consumption but also in terms of economy.

[0063] If the electric capacity of the cathode 2c is less than 1000 C / m2, the effective area of ​​the reaction field for hydrogen generation is small, and the initial overvoltage tends to be high. Therefore, it is not possible to reduce the energy consumption, specifically the electrolysis voltage, which is a proposition in hydrogen production by alkaline water electrolysis. Therefore, it is preferable that the electric capacity of the cathode 2c is 1000 C / m2 or more.

[0064] If the capacitance of the anode 2a exceeds 10,000 C / m, the effect of reducing the overvoltage for oxygen evolution is small relative to the amount of modification by the catalyst, but in order to obtain the effects of the present invention, the capacitance of the cathode 2c must be made larger than necessary, which is not preferable.

[0065] Even in the case where the anode side does not contain a distinct catalytic layer other than a nickel compound derived from a base material whose main component is nickel, the effects of the present invention can be easily obtained by forming a highly active catalytic layer on the cathode side and making the electrical capacity of the cathode 2c 1.1 times or more the electrical capacity of the anode 2a.

[0066] In this case, the substrate on the anode side is corroded and worn slightly due to the flow of reverse current accompanying the termination of electrolysis. Therefore, in order to be able to withstand repeated terminations of electrolysis, the thickness is preferably 0.1 mm or more, and more preferably 0.4 mm or more.

[0067] From the viewpoint of protecting the zero gap joint surface, it is preferable that the rigidity of the electrodes is not too high, and the thickness is preferably 3.0 mm or less, and more preferably 2.0 mm or less.

[0068] -Outer frame- The shape of the outer frame 3 is not particularly limited as long as it can frame the partition wall 1 , but it may be a shape that has an inner surface along a direction perpendicular to the plane of the partition wall 1 over the entire extent of the partition wall 1 . The shape of the outer frame 3 is not particularly limited and may be determined appropriately in accordance with the shape of the partition wall 1 in a plan view.

[0069] The material of the outer frame 3 is preferably a conductive material, and from the standpoint of alkali resistance and heat resistance, nickel, nickel alloy, mild steel, or nickel alloy plated with nickel is preferable.

[0070] -diaphragm- As the diaphragm 4 used in the bipolar electrolytic cell 50 of the electrolysis device 70, an ion-permeable diaphragm 4 is used to separate the generated hydrogen gas and oxygen gas while conducting ions. For this ion-permeable diaphragm 4, an ion exchange membrane having ion exchange ability and a porous membrane capable of permeating the electrolytic solution can be used. For this ion-permeable diaphragm 4, one having low gas permeability, high ion conductivity, low electronic conductivity, and high strength is preferred.

[0071] --Porous membrane-- The porous membrane has a structure with multiple fine through-holes that allows the electrolyte to pass through the diaphragm 4. Since the electrolyte permeates the porous membrane to exhibit ionic conduction, it is extremely important to control the pore structure, such as the pore size, porosity, and hydrophilicity. On the other hand, it is required that not only the electrolyte but also the generated gas does not pass through, that is, the membrane has gas barrier properties. From this viewpoint, control of the pore structure is also important.

[0072] The porous membrane has a plurality of fine through-holes, and examples of the porous membrane include a polymer porous membrane, an inorganic porous membrane, a woven fabric, a nonwoven fabric, etc. These can be produced by known techniques. Examples of methods for producing a porous polymer membrane include a phase inversion method (microphase separation method), an extraction method, a stretching method, and a wet gel stretching method.

[0073] The porous membrane preferably contains a polymeric material and hydrophilic inorganic particles, and the presence of the hydrophilic inorganic particles can impart hydrophilicity to the porous membrane.

[0074] ---Polymer materials--- Examples of polymeric materials include polysulfone, polyethersulfone, polyphenylsulfone, polyvinylidene fluoride, polycarbonate, tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer, tetrafluoroethylene-ethylene copolymer, polyvinylidene fluoride, polytetrafluoroethylene, perfluorosulfonic acid, perfluorocarboxylic acid, polyethylene, polypropylene, polyphenylene sulfide, polyparaphenylene benzobisoxazole, polyketone, polyimide, polyetherimide, etc. Among these, polysulfone, polyethersulfone, polyphenylsulfone, polyphenylene sulfide, and polytetrafluoroethylene are preferred, and polysulfone is more preferred. These may be used alone or in combination of two or more.

[0075] It is preferable to control the pore size of the porous membrane in order to obtain appropriate membrane properties such as separation ability, strength, etc. When used for alkaline water electrolysis, it is preferable to control the pore size of the porous membrane from the viewpoints of preventing mixing of oxygen gas generated from the anode 2a and hydrogen gas generated from the cathode 2c and reducing voltage loss in electrolysis. The larger the average pore size of the porous membrane, the larger the amount of ion passing through the porous membrane per unit area, and in particular, in electrolysis, the porous membrane has good ion permeability and tends to reduce voltage loss. Also, the larger the average pore size of the porous membrane, the smaller the contact surface area with alkaline water, and therefore the more likely it is that degradation of the polymer is suppressed. On the other hand, the smaller the average pore size of the porous membrane, the higher the separation accuracy of the porous membrane, and the better the gas barrier property of the porous membrane in electrolysis. Furthermore, when hydrophilic inorganic particles having a small particle size, which will be described later, are supported on the porous membrane, they can be firmly held without falling off. This allows the high holding ability of the hydrophilic inorganic particles to be imparted, and the effect can be maintained for a long period of time.

[0076] From this viewpoint, the average pore size of the porous membrane is preferably in the range of 0.1 μm or more and 1.0 μm or less. If the pore size is in this range, the porous membrane can achieve both excellent gas barrier properties and high ion permeability. In addition, the pore size of the porous membrane is preferably controlled in the temperature range in which it is actually used. Therefore, for example, when the porous membrane is used as the diaphragm 4 for electrolysis in an environment of 90°C, it is preferable that the above-mentioned pore size range is satisfied at 90°C. In addition, the porous membrane more preferably has an average pore size of 0.1 μm or more and 0.5 μm or less, which is a range in which the porous membrane can exhibit better gas barrier properties and high ion permeability as the diaphragm 4 for alkaline water electrolysis.

[0077] The average pore size of the porous membrane can be measured by the following method. The average pore size of the porous membrane refers to the average water permeation pore size measured by the following method using an integrity tester (Sartorius Stedim Japan, "Sartocheck Junior BP-Plus"). First, the porous membrane, including the core material, is cut to a specified size and used as a sample. This sample is placed in a pressure-resistant container and filled with pure water. Next, the pressure-resistant container is kept in a thermostatic chamber set to a specified temperature, and measurement begins when the inside of the pressure-resistant container reaches the specified temperature. When measurement begins, the upper side of the sample is pressurized with nitrogen, and the pressure and permeation flow rate when pure water permeates from the lower side of the sample are recorded. The average water permeation pore size can be calculated from the following Hagen-Poiseuille equation using the gradient between pressure and water permeation flow rate when the pressure is between 10 kPa and 30 kPa. Average permeable pore diameter (m)={32ηLμ0 / (εP)} 0.5 Here, η is the viscosity of water (Pa s), L is the thickness of the porous membrane (m), and μ0 is the apparent flow velocity, μ0 (m / s) = flow rate (m 3 / s) / flow area (m 2 ) where ε is the porosity and P is the pressure (Pa).

[0078] It is preferable to control the porosity of the porous membrane of the diaphragm 4 for alkaline water electrolysis from the viewpoints of gas barrier properties, maintaining hydrophilicity, preventing a decrease in ion permeability due to adhesion of air bubbles, and obtaining stable electrolysis performance (low voltage loss, etc.) for a long period of time. From the viewpoint of achieving high levels of gas barrier properties and low voltage loss, the lower limit of the porosity of the porous membrane is preferably 30% or more, more preferably 35% or more, and even more preferably 40% or more. The upper limit of the porosity is preferably 70% or less, more preferably 65% ​​or less, and even more preferably 55% or less. If the porosity of the porous membrane is the above upper limit or less, ions can easily permeate the membrane, and the voltage loss of the membrane can be suppressed.

[0079] The porosity of the porous membrane refers to the open porosity determined by Archimedes' method, and can be calculated by the following formula. Porosity P(%)=ρ / (1+ρ)×100 Here, ρ=(W3-W1) / (W3-W2), W1 is the dry mass of the porous membrane (g), W2 is the mass of the porous membrane in water (g), and W3 is the mass of the porous membrane saturated with water (g).

[0080] The porosity is measured by cutting the porous membrane washed with pure water into three pieces measuring 3 cm x 3 cm. First, W2 and W3 of the sample are measured. Then, the porous membrane is left to stand in a dryer set at 50°C for 12 hours or more to dry, and W1 is measured. Then, the porosity is calculated from the values ​​of W1, W2, and W3. The porosity of the three samples is calculated, and the arithmetic average value of these values ​​is taken as the porosity P.

[0081] The thickness of the porous membrane is not particularly limited, but is preferably from 100 μm to 700 μm, more preferably from 100 μm to 600 μm, and further preferably from 200 μm to 600 μm. When the thickness of the porous membrane is equal to or greater than the lower limit, it is difficult to break by piercing or the like, and the electrodes are unlikely to short-circuit. In addition, the gas barrier property is good. When the thickness is equal to or less than the upper limit, the voltage loss is unlikely to increase. In addition, the influence of the variation in the thickness of the porous membrane is reduced. In addition, when the thickness of the membrane is 100 μm or more, it is difficult to break by piercing, etc., and the electrodes are unlikely to short-circuit. In addition, the gas barrier property is good. When the thickness is 600 μm or less, the voltage loss is unlikely to increase. In addition, the influence of the variation in the thickness of the porous membrane is reduced. If the thickness of the porous membrane is 250 μm or more, better gas barrier properties are obtained, and the strength of the porous membrane against impact is further improved. From this viewpoint, the lower limit of the thickness of the porous membrane is more preferably 300 μm or more, more preferably 350 μm or more, and even more preferably 400 μm or more. On the other hand, if the thickness of the porous membrane is 700 μm or less, the ion permeability is less likely to be hindered by the resistance of the electrolyte contained in the pores during operation, and better ion permeability can be maintained. From this viewpoint, the upper limit of the thickness of the porous membrane is more preferably 600 μm or less, more preferably 550 μm or less, and even more preferably 500 μm or less.

[0082] ---Hydrophilic inorganic particles--- The porous membrane preferably contains hydrophilic inorganic particles in order to exhibit high ion permeability and high gas barrier property. The hydrophilic inorganic particles may be attached to the surface of the porous membrane, or may be partially embedded in the polymer material constituting the porous membrane. When the hydrophilic inorganic particles are contained in the voids of the porous membrane, they are difficult to be detached from the porous membrane, and the performance of the porous membrane can be maintained for a long time.

[0083] Examples of hydrophilic inorganic particles include at least one inorganic material selected from the group consisting of oxides or hydroxides of zirconium, bismuth, and cerium, oxides of Group IV elements of the periodic table, nitrides of Group IV elements of the periodic table, and carbides of Group IV elements of the periodic table. Among these, from the viewpoint of chemical stability, oxides of zirconium, bismuth, and cerium, and oxides of Group IV elements of the periodic table are more preferred, oxides of zirconium, bismuth, and cerium are even more preferred, and zirconium oxide is even more preferred.

[0084] The hydrophilic inorganic particles are preferably in the form of fine particles.

[0085] --Porous support-- When a porous membrane is used as the membrane 4, the porous membrane may be used together with a porous support. Preferably, the porous membrane has a structure in which the porous support is disposed therein, and more preferably, the porous membrane is laminated on both sides of the porous support. Alternatively, the porous membrane may be laminated symmetrically on both sides of the porous support.

[0086] Examples of the porous support include mesh, porous membrane, nonwoven fabric, woven fabric, and composite fabric containing nonwoven fabric and woven fabric contained in the nonwoven fabric. These may be used alone or in combination of two or more. More preferred embodiments of the porous support include mesh substrates made of polyphenylene sulfide monofilaments, and composite fabrics containing nonwoven fabric and woven fabric contained in the nonwoven fabric.

[0087] --Ion exchange membrane-- Ion exchange membranes include cation exchange membranes that selectively allow cations to pass therethrough and anion exchange membranes that selectively allow anions to pass therethrough, and either type of exchange membrane can be used. The material of the ion exchange membrane is not particularly limited, and known materials can be used. For example, modified resins such as fluorine-containing resins and polystyrene-divinylbenzene copolymers can be suitably used. In particular, fluorine-containing ion exchange membranes are preferred because of their excellent heat resistance and chemical resistance.

[0088] Examples of the fluorine-containing ion exchange membrane include those that have a function of selectively permeating ions generated during electrolysis and contain a fluorine-containing polymer having an ion exchange group. The fluorine-containing polymer having an ion exchange group here refers to a fluorine-containing polymer having an ion exchange group or an ion exchange group precursor that can become an ion exchange group by hydrolysis. For example, there can be mentioned a polymer that has a fluorinated hydrocarbon main chain, has a functional group that can be converted into an ion exchange group by hydrolysis or the like as a pendant side chain, and is melt-processable.

[0089] The molecular weight of the fluorine-containing copolymer is not particularly limited, but the melt flow index (MFI) value of the precursor measured in accordance with ASTM:D1238 (measurement conditions: temperature 270°C, load 2160 g) is preferably 0.05 to 50 (g / 10 min), more preferably 0.1 to 30 (g / 10 min).

[0090] Examples of the ion exchange group of the ion exchange membrane include cation exchange groups such as a sulfonic acid group, a carboxylic acid group, and a phosphate group, and anion exchange groups such as a quaternary ammonium group.

[0091] By adjusting the equivalent mass EW of the ion exchange group, the ion exchange membrane can be endowed with excellent ion exchange capacity and hydrophilicity. In addition, it can be controlled to have many smaller clusters (microscopic parts where the ion exchange group coordinates and / or adsorbs water molecules), which tends to improve alkali resistance and ion selective permeability. This equivalent weight EW can be measured by salt-substitution of the ion exchange membrane and back titration of the resulting solution with an alkali or acid solution. The equivalent weight EW can be adjusted by the copolymerization ratio of the raw monomers, the selection of the monomer species, etc. The equivalent mass EW of the ion exchange membrane is preferably 300 or more from the viewpoints of hydrophilicity and water resistance of the membrane, and is preferably 1300 or less from the viewpoints of hydrophilicity and ion exchange capacity.

[0092] The thickness of the ion exchange membrane is not particularly limited, but from the viewpoints of ion permeability and strength, it is preferably in the range of 5 μm to 300 μm.

[0093] In order to improve the hydrophilicity of the surface of the ion exchange membrane, the surface may be subjected to a surface treatment, specifically, a method of coating the surface with hydrophilic inorganic particles such as zirconium oxide, or a method of providing the surface with fine irregularities.

[0094] From the viewpoint of membrane strength, it is preferable to use the ion exchange membrane together with a reinforcing material. The reinforcing material is not particularly limited, and examples thereof include general nonwoven fabrics, woven fabrics, and porous membranes made of various materials. In this case, the porous membrane is not particularly limited, but is preferably a PTFE-based membrane that has been stretched and made porous.

[0095] ((Zero Gap Structure)) In the bipolar element 60 in the zero gap type cell, it is preferable to adopt a configuration in which a spring, which is an elastic body, is disposed between the electrode 2 and the partition wall 1 as a means for reducing the inter-electrode distance, and the electrode 2 is supported by this spring. For example, in a first example, a spring made of a conductive material may be attached to the partition wall 1, and the electrode 2 may be attached to this spring. In a second example, a spring may be attached to an electrode rib attached to the partition wall 1, and the electrode 2 may be attached to this spring. When adopting a configuration using such an elastic body, it is necessary to appropriately adjust the strength, number, shape, etc. of the spring as necessary so that the pressure at which the electrode 2 contacts the diaphragm 4 is not uneven.

[0096] -Electrode chamber- As shown in FIG. 3, in a bipolar electrolytic cell 50, a partition wall 1, an outer frame 3, and a diaphragm 4 define an electrode chamber 5 through which the electrolyte passes.

[0097] In this embodiment, the arrangement of the header 10 of the bipolar electrolytic cell can be an internal header type or an external header 10O type, and for example, in the illustrated example, the space occupied by the anode 2a and the cathode 2c themselves may also be considered to be the space inside the electrode chamber 5. Furthermore, particularly when a gas-liquid separation box is provided, the space occupied by the gas-liquid separation box may also be considered to be the space inside the electrode chamber 5.

[0098] -Rectifier plate- In the bipolar electrolytic cell 50 of the electrolysis device 70, it is preferable that the current plates 6 (anode current plate 6a, cathode current plate 6c) are attached to the partition wall 1, and the current plates 6 are physically connected to the electrodes 2. According to such a configuration, the current plates 6 serve as supports for the electrodes 2, making it easy to maintain the zero gap structure Z. Here, the electrode 2 may be provided on the rectifying plate 6, or the current collector 2r, the conductive elastic body 2e, and the electrode 2 may be provided on the rectifying plate 6 in this order. In the bipolar electrolytic cell 50 of the above-mentioned example of the electrolytic device 70, a structure in which a current rectifier plate 6-a current collector 2r-a conductive elastic body 2e-an electrode 2 are stacked in this order is adopted in the cathode chamber 5c, and a structure in which a current rectifier plate 6-an electrode 2 are stacked in this order is adopted in the anode chamber 5a.

[0099] In the bipolar electrolytic cell 50 of the above-mentioned example of the electrolytic device 70, the above-mentioned structure of "rectifier plate 6-current collector 2r-conductive elastomer 2e-electrode 2" is adopted in the cathode chamber 5c, and the above-mentioned structure of "rectifier plate 6-electrode 2" is adopted in the anode chamber 5a, but the present invention is not limited to this, and the "rectifier plate 6-current collector 2r-conductive elastomer 2e-electrode 2" structure may also be adopted in the anode chamber 5a.

[0100] It is preferable that the current rectifying plates 6 (anode current rectifying plate 6a, cathode current rectifying plate 6c) not only have the role of supporting the anode 2a or cathode 2c but also have the role of transmitting a current from the partition wall 1 to the anode 2a or cathode 2c.

[0101] In the bipolar electrolytic cell 50 of the electrolysis device 70, it is preferable that at least a part of the current plate 6 is conductive, and it is more preferable that the entire current plate 6 is conductive. With this configuration, it is possible to suppress an increase in cell voltage due to electrode deflection.

[0102] A conductive metal is generally used as the material for the current plate 6. For example, nickel-plated mild steel, stainless steel, nickel, etc. can be used.

[0103] The distance between adjacent anode current plates 6a or the distance between adjacent cathode current plates 6c is determined taking into consideration the electrolysis pressure and the pressure difference between the anode chamber 5a and the cathode chamber 5c.

[0104] The length of the current plates 6 (anode current plate 6a, cathode current plate 6c) may be determined appropriately depending on the size of the partition wall 1. The height of the straightening plate 6 may be determined appropriately depending on the distance from the partition wall 1 to each flange portion, the thickness of the gasket 7, the thickness of the electrodes 2 (anode 2a, cathode 2c), the distance between the anode 2a and the cathode 2c, etc. The thickness of the rectifying plate 6 may be 0.5 mm to 5 mm, taking into consideration costs, ease of manufacture, strength, and the like, and is not particularly limited, although a thickness of 1 mm to 2 mm is easily used.

[0105] -gasket- In the bipolar electrolytic cell 50 of the electrolysis device 70, a gasket 7 having a diaphragm 4 is preferably sandwiched between the outer frames 3 that border the partition walls 1. The gasket 7 is used to seal between the bipolar element 60 and the diaphragm 4 and between the bipolar elements 60 against the electrolyte and the generated gas, and can prevent leakage of the electrolyte and the generated gas to the outside of the electrolytic cell and mixing of gases between the two electrode chambers.

[0106] The gasket 7 generally has a rectangular or annular structure with the electrode surface hollowed out to match the surface that contacts the frame of the element. The diaphragm 4 can be stacked between the elements by sandwiching it between two such gaskets. Furthermore, the gasket 7 preferably has a slit that can accommodate the diaphragm 4 so that the diaphragm 4 can be held, and also has openings that allow the accommodated diaphragm 4 to be exposed on both surfaces of the gasket 7. This allows the gasket 7 to accommodate the edge of the diaphragm 4 in the slit and cover the end faces of the edge of the diaphragm 4. This makes it possible to more reliably prevent the electrolyte or gas from leaking from the end faces of the diaphragm 4.

[0107] The material of the gasket 7 is not particularly limited, and any known rubber material or resin material having insulating properties can be selected. Examples of rubber and resin materials that can be used include natural rubber (NR), styrene butadiene rubber (SBR), chloroprene rubber (CR), butadiene rubber (BR), acrylonitrile-butadiene rubber (NBR), silicone rubber (SR), ethylene-propylene rubber (EPT), ethylene-propylene-diene rubber (EPDM), fluororubber (FR), isobutylene-isoprene rubber (IIR), urethane rubber (UR), and chlorosulfonated polyethylene rubber (CSM). Fluororesin materials include polytetrafluoroethylene (PTFE), tetrafluoroethylene-perfluoroalkylvinylether copolymer (PFA), tetrafluoroethylene-ethylene copolymer (ETFE), and chlorotrifluoroethylene-ethylene copolymer (ECTFE). Resin materials include polyphenylene sulfide (PPS), polyethylene, polyimide, and polyacetal. Among these, ethylene-propylene-diene rubber (EPDM) and fluororubber (FR) are particularly suitable in terms of elastic modulus and alkali resistance.

[0108] A reinforcing material may be embedded in the gasket 7. This can prevent the gasket 7 from being crushed when it is sandwiched and pressed between frames during stacking, making it easier to prevent damage. Such reinforcing materials can be made of known metal materials, resin materials, carbon materials, etc., and specific examples include metals such as nickel and stainless steel, resins such as nylon, polypropylene, PVDF, PTFE, PPS, etc., and carbon materials such as carbon particles and carbon fibers.

[0109] The size of the gasket 7 is not particularly limited and may be designed according to the dimensions of the electrode chamber 5 and the membrane, but the width is preferably 10 mm to 40 mm. In this case, when the gasket 7 has a slit portion, the size of the slit portion is preferably set so that the inner dimensions of the slit are 0.5 mm to 5 mm larger in length and width than the size of the membrane.

[0110] The thickness of the gasket 7 is not particularly limited, and is designed depending on the material, elastic modulus, and cell area of ​​the gasket 7. A preferable range of the thickness is 1.0 mm to 10 mm, and more preferably 3.0 mm to 10 mm. Furthermore, when the gasket 7 has a slit portion, the opening width of the slit portion may be 0.5 to 1.0 times the thickness of the film.

[0111] The elastic modulus of the gasket 7 is not particularly limited, and is designed depending on the material and cell area of ​​the electrode 2. A preferable range of the elastic modulus is 0.20 MPa to 20 MPa in tensile stress at 100% deformation, and from the viewpoint of sealing characteristics and cell strength when stacked, a range of 1.0 MPa to 10 MPa is more preferable. The tensile stress can be measured in accordance with JIS K6251. For example, an Autograph AG manufactured by Shimadzu Corporation may be used.

[0112] In particular, it is preferable that the gasket 7 has a thickness of 3.0 mm to 10 mm and a tensile stress of 1.0 MPa to 10 MPa at 100% deformation from the viewpoint of suppressing an increase in cell voltage due to electrode deflection, and from the viewpoint of sealing characteristics and cell strength when stacked.

[0113] In the electrolysis device 70, it is preferable to cover the surface of the gasket 7 with an insulating resin sheet (e.g., a fluororesin such as polytetrafluoroethylene). By doing so, the elements 60 are insulated from each other, so that the charge accumulated in each element 60 in the current application step (the step in which electrolysis of the electrolyte is performed) can be prevented from affecting the other elements 60 in the stop step (the step in which electrolysis of the electrolyte is stopped).

[0114] -Header- The bipolar electrolytic cell 50 of the electrolysis device 70 has a cathode chamber 5c and an anode chamber 5a for each electrolytic cell 65. In order to continuously perform the electrolytic reaction in the electrolytic cell 50, it is necessary to continuously supply an electrolyte containing a sufficient amount of the raw materials to be consumed by electrolysis to the cathode chamber 5c and the anode chamber 5a of each electrolytic cell 65.

[0115] The electrolytic cell 65 is connected to an electrolyte supply / discharge pipe called a header 10, which is common to the multiple electrolytic cells 65. In general, the anode distribution pipe is called the anode inlet header 10ai, the cathode distribution pipe is called the cathode inlet header 10ci, the anode collection pipe is called the anode outlet header 10ao, and the cathode collection pipe is called the cathode outlet header 10co. The electrolytic cell 65 is connected to the electrode distribution pipes and electrode collection pipes via hoses or the like.

[0116] The material of the header 10 is not particularly limited, but it is necessary to adopt a material that can sufficiently withstand the corrosiveness of the electrolyte used and the operating conditions such as pressure and temperature. The material of the header 10 may be iron, nickel, cobalt, PTFE, ETFE, PFA, polyvinyl chloride, polyethylene, etc.

[0117] The range of the electrode chambers 5 varies depending on the detailed structure of the outer frame 3 provided at the outer end of the partition wall 1, and the detailed structure of the outer frame 3 may differ depending on the arrangement of the headers 10 (pipes for distributing or collecting the electrolyte) attached to the outer frame 3. Representative arrangements of the headers 10 in the bipolar electrolytic cell 50 include an internal header 10I type and an external header 10O type.

[0118] -Internal Header- The internal header type refers to a type in which the bipolar electrolytic cell 50 and the header 10 (a tube for distributing or collecting the electrolyte) are integrated together.

[0119] More specifically, in the internal header type bipolar electrolytic cell 50, an anode inlet header and a cathode inlet header are provided in the partition 1 and / or at a lower part in the outer frame 3 and are provided so as to extend in a direction perpendicular to the partition 1, and an anode outlet header and a cathode outlet header are provided in the partition 1 and / or at an upper part in the outer frame 3 and are provided so as to extend in a direction perpendicular to the partition 1.

[0120] The anode inlet header, cathode inlet header, anode outlet header, and cathode outlet header inherently included in the internal header type bipolar electrolytic cell 50 are collectively referred to as the internal headers.

[0121] In an example of the internal header type, an anode inlet header and a cathode inlet header are provided in a part of a lower portion of the outer frame 3 at the end edge of the partition 1, and similarly, an anode outlet header and a cathode outlet header are provided in a part of an upper portion of the outer frame 3 at the end edge of the partition 1.

[0122] -External headers- The external header 10O type refers to a type in which the bipolar electrolytic cell 50 and the header 10 (a tube for distributing or collecting the electrolyte) are independent.

[0123] The external header 10O type bipolar electrolytic cell 50 has an anode inlet header 10Oai and a cathode inlet header 10Oci that are provided independently, running parallel to the electrolytic cell 50 in a direction perpendicular to the current-carrying surface of the electrolytic cell 65. The anode inlet header 10Oai and the cathode inlet header 10Oci are connected to each electrolytic cell 65 by hoses.

[0124] External Header 10O The anode inlet header 10Oai, the cathode inlet header 10Oci, the anode outlet header 10Oao, and the cathode outlet header 10Oco, which are externally connected to the external header 10O type bipolar electrolyzer 50, are collectively referred to as the external header 10O. In the example of the external header 10O type, a tubular member is installed in a through hole for the header 10 provided in a lower portion of the outer frame 3 at the edge of the partition 1, and the tubular member is connected to an anode inlet header 10Oai and a cathode inlet header 10Oci, and similarly, a tubular member (e.g., a hose, tube, etc.) is installed in a through hole for the header 10 provided in an upper portion of the outer frame 3 at the edge of the partition 1, and the tubular member is connected to an anode outlet header 10Oao and a cathode outlet header 10Oco.

[0125] In addition, the bipolar electrolytic cell 50 having the internal header 10I type and the external header 10O type may have a gas-liquid separation box therein for separating the gas generated by electrolysis from the electrolytic solution. The installation position of the gas-liquid separation box is not particularly limited, and it may be installed between the anode chamber 5a and the anode outlet header 10ao, or between the cathode chamber 5c and the cathode outlet header 10co.

[0126] The surface of the gas-liquid separation box may be coated with a coating material that is sufficiently resistant to the corrosiveness of the electrolyte and to operating conditions such as pressure and temperature. The coating material may be insulating in order to increase the electrical resistance of the leakage current circuit inside the electrolytic cell. The coating material may be EPDM, PTFE, ETFE, PFA, polyvinyl chloride, polyethylene, etc.

[0127] -Liquid level gauge- The electrolytic cell 50 of the electrolysis device 70 may have a level gauge capable of measuring the liquid level in each of the electrode chambers 5a, 5c of the electrolytic cell 50. In particular, in this embodiment (II), it is preferable to have the above-mentioned level gauge. The level gauge monitors the liquid level in each of the electrode chambers 5a, 5c (monitors the height of the liquid level in the electrode chambers 5a, 5c), and makes it possible to know whether the surface of the diaphragm 4 in each of the electrode chambers 5a, 5c is immersed in the electrolyte or not immersed in the electrolyte. The liquid level gauge is not particularly limited, but for example, a direct vision type, a contact type, or a differential pressure type liquid level gauge can be used.

[0128] (First cathode protection unit) The electrolysis device 70 may have a first cathode protection unit capable of insulating the supply path and / or the discharge path from the cathode chamber 5c. In particular, in this embodiment (II), it is preferable to have a first cathode protection unit. In the stopping step, the supply path and / or the discharge path are insulated from the cathode chamber 5c by the first cathode protection unit, so that the total amount of reverse current generated in the cathode 2c in the stopping step can be reduced. As a result, deterioration of the cathode 2c under a variable power supply can be suppressed. Note that an example of the first cathode protection unit is providing a resin valve in the supply path and / or discharge path (specifically, cathode distribution pipe 20Oci, cathode inlet header (cathode inlet side hose) 10Oci, cathode collection pipe 20Oco, cathode outlet header (cathode outlet side hose) 10Oco, etc.). Another example of the first cathode protection unit is that the supply path is located vertically above the cathode chamber 5c and that the discharge path is located vertically above the cathode chamber 5c. By doing so, for example, when the liquid feed pump 71 is stopped in the stopping step, the electrolyte flows down by its own weight, and an insulating gas layer can be formed in the supply path and / or discharge path.

[0129] (Second cathode protection unit) In the electrolysis device 70, an electric circuit including the electrolytic cell and the electrolysis power supply (rectifier) ​​74 is formed, and the electrolysis device 70 may have a second cathode protection unit capable of interrupting the electric circuit. In particular, in this embodiment (II), it is preferable to have a second cathode protection unit. By interrupting the electric circuit by the second cathode protection unit in the stopping step, it is possible to reduce the reverse current generated in the cathode 2c. The second cathode protection unit may be a circuit breaker, a disconnector, a switch, or a diode that blocks reverse current in an electric circuit.

[0130] (Regarding the positional relationship of the upper ends of the cathode and the diaphragm in the vertical direction D1) In the electrolysis device 70, it is preferable that at least a part of the cathode 2c is located in the vertical direction D1 above the uncoated upper end 4t of the diaphragm 4. This makes it possible, in the stopping step, to expose at least a part of the cathode 2c to a hydrogen gas layer that may be present in the cathode chamber 5c, while positioning the waterline L (position of the liquid level) of the electrolytic solution in the anode chamber 5a and / or the cathode chamber 5c vertically above the uncoated upper end 4t of the diaphragm 4, as shown in Figs. 5A, 5B, and 6. As a result, deterioration of the cathode 2c when electrolysis is stopped can be suppressed, and diffusion and mixing of gas between the electrode chambers 5a, 5c via the diaphragm can be suppressed. Specifically, in the operation of the conventional electrolysis device, a reverse current is generated in the cathode 2c during the stop step due to the charge accumulated in the cathode (and the anode 2a) during the current-passing step, and when the reverse current is generated, the cathode itself may be oxidized (a reduction reaction occurs in the cathode chamber during the current-passing step). Then, there is a concern that the cathode 2c may be deteriorated by repeating the current-passing step and the stop step. In contrast, in the electrolysis device according to the present embodiment (particularly, the present embodiment (II)), as shown in Figs. 5A, 5B, and 6, a part of the cathode 2c is above the waterline L and exposed to hydrogen gas during the stop step. Therefore, even if a reverse current is generated in the cathode 2c, the hydrogen in contact with the cathode 2c is oxidized, and the oxidation of the cathode 2c itself is reduced, and deterioration of the cathode 2c can be suppressed. Regarding the suppression of diffusion and mixing of gas through the diaphragm 4, in the operation of a conventional electrolysis device, when both surfaces of the diaphragm 4 are exposed to gas, a small amount of gas in each of the electrode chambers 5a, 5c may permeate the diaphragm 4 and diffuse into each of the electrode chambers 5a, 5c. However, in the electrolysis device according to the present embodiment, while part of the cathode 2c is exposed to hydrogen gas, the waterline L (position of the liquid level) of the electrolyte in the anode chamber 5a and / or the cathode chamber 5c can be positioned vertically above the uncovered upper end 4t of the diaphragm 4 in the shutdown step, so that at least one surface of the diaphragm 4 is immersed in the liquid. Therefore, diffusion and mixing of gas between the electrode chambers 5a, 5c can be suppressed. Note that the above-mentioned "uncovered upper end of the diaphragm" refers to the upper end of the diaphragm 4 in the vertical direction D1, or in a case where the upper end portion of the diaphragm itself in the vertical direction D1 is partly covered with a gasket or the like used to fix the diaphragm 4 between the outer frames 3 of the electrolytic cell 50 as shown in FIG. 5A , or partly covered with a covering material 41 as will be described later together with a gasket 7 as shown in FIG. 6 , the "uncovered upper end of the diaphragm" refers to the upper end in the vertical direction D1 of the portion of the diaphragm 4 that is not covered with the gasket 7, the covering material 41, or the like.

[0131] Specifically, as shown in Figures 5A and 5B which are schematic diagrams of a cathode chamber 5c, such an electrolysis device 70 uses a cathode 2c formed of a cathode main body portion 2c1 and a cathode auxiliary portion 2c2 connected to the cathode main body portion 2c1 via a conductor portion 2c3, and at least a part of the cathode auxiliary portion 2c2 above in the vertical direction D1 is present above the uncoated upper end 4t of the diaphragm 4 in the vertical direction D1, as shown in Figure 5A. Since the cathode 2c has the cathode auxiliary portion 2c2 in this manner, the waterline L of the electrolytic solution is positioned as shown in the figure in the stopping step, so that even if a reverse current occurs, the cathode auxiliary portion 2c2 oxidizes hydrogen gas to prevent deterioration of the cathode 2c, and oxygen can be prevented from being mixed into hydrogen present in the cathode chamber 5c, which may be caused by the surface of the diaphragm 4 being exposed to gas in the stopping step. As the electrolysis device 70, a cathode 2c consisting of only the cathode main body 2c1, rather than the cathode auxiliary part 2c2 spaced apart from the cathode main body 2c1, may be used, in which the upper end of the cathode main body 2c1 in the vertical direction D1 is extended to the position of the upper end of the cathode auxiliary part 2c2 in the vertical direction D1 in FIG. 5A. However, by having the cathode 2c having the cathode auxiliary part 2c2 as shown in FIG. 5A, it is possible to more easily replace the cathode 2c during maintenance, compared to a case where the cathode 2c does not have the cathode auxiliary part 2c2. In addition, by using the cathode auxiliary part 2c2, the size of the cathode 2c as a whole can be reduced, or, for example, the electrolysis performance of the cathode auxiliary part 2c2 during the current application step can be made lower than that of the cathode main body 2c1 (for example, the amount of catalyst can be reduced, etc.), so that the cost of the cathode 2c can be reduced.

[0132] Here, the cathode main body portion 2c1 is an electrode for electrolyzing the electrolyte in the current passage step, like the cathode 2c that does not have the cathode auxiliary portion 2c2, and can have the same configuration and material as the cathode 2c that does not have the cathode auxiliary portion 2c2. The cathode auxiliary part 2c2 can be made of a material that can be used for the cathode main body part 2c1, and can be made of the same material as the cathode main body part 2c1, but is not particularly limited as long as it can be oxidized by contacting with hydrogen when a reverse current occurs. As shown in the schematic plan view of the cathode chamber 5c in FIG. 5B, the length of the cathode auxiliary part 2c2 in the vertical direction D1 and the length in the direction perpendicular to the vertical direction D1 are smaller than the horizontal length of the cathode main body part 2c1 and the length in the direction perpendicular to the vertical direction D1. The specific dimensions are not particularly limited as long as the cathode auxiliary part 2c2 is smaller than the size that can be accommodated in the cathode chamber 5c together with the cathode main body part 2c1, and the length of the cathode auxiliary part 2c2 in the vertical direction D1 is preferably 90 mm or less. Conductive wire portion 2c3 connecting cathode main portion 2c1 and cathode auxiliary portion 2c2 can be made of a material that can be used for the base material of cathode 2c, and can also be made of the same material as cathode main portion 2c1. In the example of FIG. 5A, the covering material 41 for covering the surface of the diaphragm 4 as used in the example of FIG. 6 is not used, but the covering material 41 can also be used.

[0133] As an electrolysis device 70 in which at least a part of the cathode 2c is located above the uncoated upper end 4t of the diaphragm 4, it is also preferable to use the electrolysis device 70 shown in FIG. 6 instead of the example shown in FIGS. 5A and 5B. Specifically, in the electrolysis device 70 shown in FIG. 6, the surface of the diaphragm 4 is covered with a covering material 41 such that the lower end in the vertical direction of the covering material 41 is the uncoated upper end 4t of the diaphragm 4. More specifically, a part of the surface of the diaphragm 4 is covered with the covering material 41 together with the gasket 7 as described later, so that at least a part of the cathode 2c is located above the uncoated upper end 4t of the diaphragm 4. In this way, the same effects as those of the electrolysis device 70 shown in FIGS. 5A and 5B can be obtained, and the structure of the cathode itself can be simplified as compared with the case in which the cathode 2c has a cathode auxiliary part 2c2 as shown in FIGS. 5A and 5B.

[0134] Here, the covering material 41 is not particularly limited as long as it is capable of covering the surface of the diaphragm 4 and, when the portion of the diaphragm 4 covered with the covering material 41 is present in gas, can prevent the gas from passing through each of the electrode chambers 5 a, 5 c partitioned by the diaphragm 4. For example, polytetrafluoroethylene or the like can be used. 6, the covering material 41 is provided on both surfaces of the diaphragm 4, but it may be provided on only one surface of the diaphragm 4 as long as the gas in each of the electrode chambers 5a, 5c partitioned by the diaphragm 4 can be prevented from passing therethrough when the portion of the diaphragm 4 covered with the covering material 41 is present in gas. Note that in this way, when the vertical positions of the uncovered upper ends of the surfaces on one and the other sides of the diaphragm 4 differ and therefore the areas covered by the surfaces on one and the other sides differ, the uncovered upper end of the surface on the lower vertical side is regarded as the "uncovered upper end of the diaphragm."

[0135] Furthermore, when the covering material 41 is provided on the surface of the diaphragm 4, it is preferable that the covering material 41 is used to cover the surface from the upper end of the diaphragm 4 (when the surface on the upper end side of the diaphragm 4 is covered by a gasket or the like, the covering material 41 is used to cover from a position adjacent to the lower end of the gasket or the like) and that the lower end of the covering material 41 in the vertical direction D1 is located in the vertical direction D1 lower than the position of the upper end of the cathode 2c in the vertical direction D1. More preferably, the lower end of the covering material 41 in the vertical direction D1 is located in the vertical direction D1 lower than the position of the upper end of the cathode 2c in the vertical direction D1 and higher in the vertical direction D1 than a position spaced 20 mm below the position of the upper end of the cathode 2c in the vertical direction D1, and even more preferably, the lower end is located in the vertical direction D1 higher than a position spaced 10 mm below the position of the upper end of the cathode 2c in the vertical direction D1.

[0136] Next, the components of the electrolysis device 70 other than the electrolytic cell 50 will be mainly described.

[0137] - Liquid delivery pump - The liquid delivery pump 71 is not particularly limited and may be determined appropriately. The electrolysis device 70 that can be used in this embodiment can have, as its liquid delivery pump 71, a cathode-side liquid delivery pump for delivering liquid to the cathode chamber 5c and an anode-side liquid delivery pump for delivering liquid to the anode chamber 5a, and these pumps can be operated separately.

[0138] -Gas-liquid separation tank- The gas-liquid separation tank 72 includes a hydrogen separation tank 72h that separates the electrolytic solution from hydrogen gas, and an oxygen separation tank 72o that separates the electrolytic solution from oxygen gas. The hydrogen separation tank 72h is connected to the cathode chamber 5c, and the oxygen separation tank 72o is connected to the anode chamber 5a.

[0139] The gas-liquid separation tank 72 of the electrolysis device 70 includes an oxygen separation tank 72o used for the anode chamber 5a, and a hydrogen separation tank 72h used for the cathode chamber 5c.

[0140] The gas-liquid separation tank 72 for the anode chamber 5a separates the oxygen gas and the electrolyte generated in the anode chamber 5a, and the gas-liquid separation tank 72 for the cathode chamber 5c separates the hydrogen gas and the electrolyte generated in the cathode chamber 5c.

[0141] The mixture of the electrolyte and the generated gas discharged from the electrolytic cell 65 is allowed to flow into the gas-liquid separation tank 72. If gas-liquid separation is not performed properly, oxygen gas and hydrogen gas will be mixed when the electrolytes in the cathode chamber 5c and the anode chamber 5a are mixed, and the purity of the gas will decrease. In the worst case, there is a risk of explosive gas being formed.

[0142] The gas and electrolyte that flow into the gas-liquid separation tank 72 are separated into the gas phase in the upper layer of the tank and the liquid phase in the lower layer of the tank. The degree of gas-liquid separation is determined by the flux of the electrolyte in the gas-liquid separation tank 72, the floating speed of the generated gas bubbles, and the residence time in the gas-liquid separation tank 72.

[0143] The electrolyte after gas separation flows out from an outlet at the bottom of the tank and flows back into the electrolytic cell 65, thereby forming a circulation path. Since the oxygen and hydrogen gas discharged from the outlet at the top of the tank both contain alkaline mist, it is preferable to install a device, such as a mist separator or a cooler, downstream of the outlet that can liquefy the excess mist and return it to the gas-liquid separation tank 72.

[0144] The gas-liquid separation tank 72 may be provided with a level gauge in order to grasp the height of the liquid level L of the electrolyte stored therein.

[0145] In addition, the gas-liquid separation tank 72 is preferably provided with a pressure relief valve, so that even if pressure rises due to gas generated during electrolysis and exceeds the design pressure, it is possible to safely reduce the pressure.

[0146] In order to improve gas-liquid separation performance, the inlet to the gas-liquid separation tank 72 is preferably located above the electrolyte surface, but is not limited to this. In order to prevent a drop in the liquid level L in the electrolytic cell when circulation is stopped, it is preferable that the electrolyte level in the gas-liquid separation tank 72 is higher than the upper surface of the electrolytic cell, but this is not limiting. It is preferable to provide a shutoff valve between the electrolytic cell 65 and the gas-liquid separation tank 72, but this is not a limitation.

[0147] An alkali-resistant metal such as nickel is used as the material for the gas-liquid separation tank 72. On the other hand, when a general-purpose metal such as iron is used as the tank housing material, the electrolyte contact surface inside the tank may be coated with a fluorine-based resin or the like, but the material for the gas-liquid separation tank 72 in this embodiment is not limited thereto.

[0148] Considering the installation volume, it is preferable that the capacity of the gas-liquid separation tank 72 is small. However, if the volume is too small, when the pressure difference between the cathode 2c and the anode 2a increases or when there is a fluctuation in the electrolytic current value, the liquid level in the tank will fluctuate, and it is necessary to take this fluctuation into consideration. Similarly, when the tank height is low, it is easily affected by the above fluctuations, so it is preferable to make the tank height high.

[0149] -Water supply device- The water supply device 73 used in the electrolysis device 70 is not particularly limited and may be determined appropriately. As the water, ordinary tap water may be used, but in consideration of long-term operation, it is preferable to use ion-exchanged water, RO water, ultrapure water, etc.

[0150] -Electric circuit- The electrolysis device 70 is equipped with an electrolysis power supply (rectifier) ​​74. Furthermore, an electric circuit C including the electrolysis cell 50 and the electrolysis power supply (rectifier) ​​74 may be formed. Furthermore, the electrolysis device 70 may be equipped with an external load 8 connected to the electrolysis cell 50. In particular, in this embodiment (I), it is preferable that the electrolysis device 70 is equipped with the electric circuit C and the external load 8. Furthermore, the resistance value of the external load 8 is 0.02 to 2 Ωm 2 / Cell is preferred. Specifically, in the example of FIG. 1, the anode 2a of the electrolytic cell 65 at the end of the electrolytic bath 50 is connected to the positive electrode of the electrolytic power source 74 by a cable, and the cathode 2c of the electrolytic cell 65 at the end of the electrolytic bath 50 is connected to the negative electrode of the electrolytic power source 74 by a cable, and the cables are connected by an external load 8 and a switch 9. As a result, for example, in the stopping step, by closing the switch 9 in a state in which the electrolytic power source 74 is stopped, a circuit between the electrolytic bath 50 (all the electrolytic cells 65) and the external load 8 can be formed. Also, in the example of FIG. 1, the external load 8 is connected to all of the electrolytic cells 65 of the electrolytic bath 50, but although not shown, the external load 8 may be connected to some of the electrolytic cells 65 of the electrolytic bath 50. As a result, for example, in the stopping step, a circuit between some of the electrolytic cells 65 of the electrolytic bath 50 and the external load 8 can be formed.

[0151] -Storage tank- The electrolysis device 70 may have a storage tank for storing the electrolytic solution. The storage tank is preferably located vertically above the electrolytic cell 50 of the electrolytic device 70. By connecting the storage tank to the electrolytic cell 50 via piping or the like, the electrolytic solution in the storage tank can be injected into the electrolytic cell by utilizing gravity. The flow rate can also be appropriately adjusted by providing a valve or the like on the piping or the like.

[0152] -others- The electrolysis device 70 may include, in addition to the electrolytic cell 50, the gas-liquid separation tank 72, and the water supply device 73, a rectifier 74, an oxygen concentration meter 75, a hydrogen concentration meter 76, a flow meter 77, a pressure gauge 78, a heat exchanger, a pressure control valve 80, etc.

[0153] In addition, the electrolysis device 70 preferably further includes a detector for detecting the interruption of the power supply and a controller for automatically stopping the liquid delivery pump. By including the detector and the controller, it becomes possible to efficiently reduce the effect of self-discharge without manual operation, even under a power source with large fluctuations such as renewable energy.

[0154] (Method of operating electrolysis device) The method for operating the electrolysis device according to this embodiment can be carried out using the electrolysis device 70 according to this embodiment described above. Specifically, an example of the method for operating the electrolytic device according to this embodiment is a method for operating the electrolytic device 70 using an electrolytic device 70 including an anode chamber 5a having an anode 2a and a cathode chamber 5c having a cathode 2c, which are separated from each other by a diaphragm 4, the method including a current application step in which electrolysis of the electrolyte in the anode chamber 5a and the cathode chamber 5c is performed, and a stop step in which the electrolysis of the electrolyte in the anode chamber 5a and the cathode chamber 5c is stopped, and a discharge step in the stop step in which the electrolytic cell 50 of the electrolytic device 70 is electrically connected to an external load 8 and the voltage versus the electrolyte is reduced to 0.1 V or less within 5 hours. The method for operating the electrolytic device 70 according to this embodiment makes it possible to suppress deterioration of the electrode 2 under a variable power supply.

[0155] First, the current application step, which is one of the components of the method for operating the electrolysis device 70, will be described. The current application step is a step in which the electrolyte in the anode chamber 5a and the cathode chamber 5c is electrolyzed. Specifically, in an electrolysis device 70 as shown in FIG. 1, the electrolyte is sent to the anode chamber 5a and the cathode chamber 5c of the electrolytic cell 50 using a liquid delivery pump 71, while a positive current is applied from a rectifier 74 to electrolyze the electrolyte in the anode chamber 5a and the cathode chamber 5c. In addition, the electrolyte containing oxygen and the electrolyte containing hydrogen generated by the electrolysis are sent from the anode chamber 5a and the cathode chamber 5c, respectively, to a gas-liquid separation tank 72, where they are separated into gas and liquid. Furthermore, the electrolyte separated into gas and liquid in the gas-liquid separation tank 72 is returned to the liquid delivery pump 71 while water is replenished by a water replenisher 73. In this way, the electrolyte is electrolyzed while circulating in the current application step, so that the electrolysis can be performed efficiently.

[0156] Here, positive current flow refers to current flow in a direction that enables oxygen to be obtained at the anode 2a and hydrogen to be obtained at the cathode 2c by electrolysis of the electrolyte using the electrolysis device .

[0157] The electrolyte may be an alkaline aqueous solution in which an alkaline salt is dissolved, such as an aqueous NaOH solution or an aqueous KOH solution. The concentration of the alkali salt is preferably from 20% by mass to 50% by mass, and more preferably from 25% by mass to 40% by mass. In the above-mentioned operating method, from the viewpoints of ionic conductivity, kinetic viscosity, and freezing at low temperatures, a 25% by mass to 40% by mass KOH aqueous solution is particularly preferable.

[0158] In the current application step, the temperature of the electrolytic solution in the electrolytic cell 65 is preferably 80°C to 130°C. Within the above temperature range, it is possible to effectively prevent the components of the electrolysis device 70, such as the gasket 7 and the diaphragm 4, from being deteriorated due to heat while maintaining high electrolysis efficiency. The temperature of the electrolytic solution is more preferably 85°C to 125°C, and particularly preferably 90°C to 115°C.

[0159] In the current application step, the current density applied to the electrolytic cell 65 is 4 kA / m 2 ~20kA / m 2 Preferably, 6 kA / m 2 ~15kA / m 2 It is even more preferable that: In particular, when a variable power supply is used, it is preferable to set the upper limit of the current density within the above range. In addition, in terms of production, it is preferable to carry out electrolysis at the above-mentioned preferred current density in the current passing step, but the current passing step also includes a case where a current below the preferred current density flows.

[0160] In the current passing step, the pressure (gauge pressure) inside the electrolytic cell 65 is preferably 3 kPa to 3000 kPa, more preferably 3 kPa to 1000 kPa, even more preferably 3 kPa to 500 kPa, and even more preferably 3 kPa to 100 kPa.

[0161] Next, the stopping step, which is one of the components of the above-mentioned operation method of the electrolysis device 70, will be described. The stop step is a step in which electrolysis of the electrolyte in the anode chamber 5a and the cathode chamber 5c is stopped. Specifically, in the above-mentioned current passing step, oxygen is generated by electrolysis of the electrolyte in the anode chamber 5a, and hydrogen is generated by electrolysis of the electrolyte in the cathode chamber 5c. In the stop step, such electrolysis is stopped. However, in the stop step, the amount of current passing is the maximum positive current (kA / m 2 The maximum positive current flow rate means the maximum positive current flow rate that is allowed as an operating condition of the electrolysis device 70 used. In the stopping step, the liquid sending pump 71 may be stopped or may be kept running, but it is preferable to stop the liquid sending pump 71.

[0162] Next, the discharging step, which is one of the components of the method for operating the electrolysis device 70 according to this embodiment, will be described. In the discharging step, in the stopping step, the electrolytic cell 50 of the electrolysis device 70 is electrically connected to the external load 8, and the voltage across the electrolytic cell 50 is reduced to 0.1 V or less within 5 hours. When the operating method of the electrolysis device 70 includes a discharging step, it becomes possible to further suppress the deterioration of the electrode 2 under a variable power supply. Specifically, in the conventional operating method of the electrolysis device 70, the charges accumulated in the anode 2a and the cathode 2c during the current-carrying step flow inversely to the anode 2a and the cathode 2c during the stop step, generating a reverse current, and the potential of each electrode 2 gradually changes accordingly, so that the potential converges. However, in the process of the potential convergence, the potential of the anode 2a and the cathode 2c passes through a predetermined potential range in which the electrode 2 itself corrodes over a certain period of time, and therefore there is a concern that each electrode 2 may deteriorate due to repeated electrolysis stoppage and electrolysis operation under a variable power supply. In response to this, the deterioration of the electrode 2 can be suppressed by making the capacitance of the cathode 2c 1.1 times or more the capacitance of the anode 2a. The capacitance of the anode 2a is, for example, 10000 C / m 2 The capacitance of the cathode 2c is preferably 1000 C / m or less, for example. 2However, since the amount of reverse current is in principle large near the center of the electrolytic cell 50, the center is subject to the effect of the reverse current for a longer period of time than other electrolytic cells, and so there was a concern that even if the cathodes 2c of the cells other than the center were stable at or below the corrosion potential, the anodes 2a and cathodes 2c near the center would characteristically deteriorate [Concern 1]. In addition, for the same reason as Concern 1, the cells were subject to the effects of reverse current for a longer period of time than other electrolytic cells. This caused safety concerns due to the cathode 2c of the cells other than those near the center entering the oxygen generating potential, generating oxygen, and the anode 2a entering the hydrogen generating potential, generating hydrogen, which could result in the generation of explosive gases [Concern 2]. In the above-described operation method of the electrolysis device 70, when the electrolytic cell 50 of the electrolysis device 70 is electrically connected to an external load 8 and set to 0.1 V or less, the potential of the anode 2 a and the cathode 2 c, common to all cells, quickly passes through a predetermined corrosion potential range, and concerns 1 and 2 can be sufficiently suppressed. As described above, when electrolysis is stopped, a reverse current occurs, the potential of each electrode 2 converges, and the relative voltage approaches 0 V. However, if the relative voltage is 0.1 V or less, it can be kept outside the specified potential range where the electrode 2 itself corrodes. In addition, the shorter the time for which the voltage is kept below 0.1 V, the better from the standpoint of suppressing deterioration of electrode 2; however, if the time is within 5 hours, deterioration of electrode 2 can be suppressed while preventing the current flowing through external load 8 in a short period of time from becoming too large, allowing for appropriate design of heat generation and heat dissipation in external load 8.

[0163] Moreover, the time for achieving a voltage of 0.1 V or less in the discharge step is preferably within 60 minutes, more preferably within 30 minutes. The voltage is preferably 0.1 V or less, and more preferably 0.0 V or less. The counter voltage means the voltage of one electrolytic cell 65. When discharging is performed for all electrolytic cells 65 using an external load 8 as shown in FIG. 1, the counter voltage can be obtained by measuring the potential difference between the anode 2a of the electrolytic cell 65 at the end of the electrolytic cell 50 and the cathode 2c of the electrolytic cell 65 at the end of the electrolytic cell 50 (measured at both ends of the external load 8, etc.) and dividing by the number of electrolytic cells 65. Alternatively, the counter voltage can be obtained by measuring the counter voltage for each electrolytic cell 65 and dividing the integrated value of each counter voltage by the number of electrolytic cells. Alternatively, the counter voltage of a specific electrolytic cell 65 can be used as the reference counter voltage in the discharging step.

[0164] Incidentally, the discharge step may be performed when the voltage of the electrolytic cell 50 falls below a predetermined threshold in the stop step. In this way, the predetermined threshold is set, for example, before the potential of each electrode 2 is reached, so that corrosion of each electrode 2 can be suppressed and the amount of heat generated by the external load 8 can be suppressed. The threshold value can be set arbitrarily depending on the amount of heat generated by the external load 8 and its heat dissipation design, but is preferably 0.5 V or more in terms of voltage, more preferably 1.0 V or more, and even more preferably 1.2 V or more.

[0165] Here, the above-mentioned operating method of the electrolysis device 70 can be more suitably applied when the electrolytic cell 50 of the electrolysis device 70 is of a bipolar type and has a plurality of electrolytic cells 65, particularly when the electrolytic cell 50 has 30 or more electrolytic cells 65. That is, the conventional method of operating the electrolysis device 70 has the following problems. In an electrolytic cell 50 in which multiple electrolytic cells 65 are stacked in series, the reverse current flowing during the shutdown process was relatively large in the electrolytic cells 65 in the center of the electrolytic cell 50 and relatively small in the electrolytic cells 65 at the ends. For this reason, the change in electrode potential during the shutdown process was significantly faster at the center and slower at the ends. Therefore, in the conventional operating method of the electrolytic device 70, the electrode 2 of the central electrolytic cell 65 and the electrode 2 of the end electrolytic cell 65 were exposed to the corrosion potential for different periods of time during the shutdown process, resulting in a distribution of deterioration of the electrode 2 depending on the position in the electrolytic cell 65, and in addition, deterioration of the electrode 2 of the end electrolytic cell 65 was prominent. In addition to the distribution of deterioration of the electrodes 2, there was also the following problem. That is, when a reverse current occurs as described above, the potential of each electrode 2 gradually changes, and when the potential of the anode 2a reaches a predetermined hydrogen generation potential and the potential of the cathode 2c reaches a predetermined oxygen generation potential, hydrogen is generated in the anode chamber 5a and oxygen is generated in the cathode chamber 5c. In an electrolytic cell 50 in which a plurality of electrolytic cells 65 are stacked in series, the potential of the central electrolytic cell 65 reaches a predetermined potential early. Even after that, a reverse current continues to flow in the central electrolytic cell 65 due to the voltage of the electrolytic cell 65 on the end side, so that in the central electrolytic cell 65, the hydrogen concentration in oxygen in the anode chamber 5a and the oxygen concentration in hydrogen in the cathode chamber 5c may be locally increased. In contrast, the above-described operating method having the above-described discharge step of the electrolysis device 70 makes the discharge by the external load 8 uniform, thereby suppressing the distribution of electrode deterioration and shortening the time of exposure to the corrosion potential by promoting discharge. Regarding the above-mentioned increase in the hydrogen concentration in oxygen in the anode chamber 5a and the oxygen concentration in hydrogen in the cathode chamber 5c, the amount of hydrogen generated in the anode chamber 5a and the amount of oxygen generated in the cathode chamber 5c are suppressed by making the discharge uniform by the external load 8, and thereby reducing the reverse current in the central electrolytic cell 65 after the potential of the electrode 2 reaches the hydrogen generation potential or the oxygen generation potential. By using the external load 8 to quickly reduce the voltage of the electrolytic cell 50, the risk of electric shock when performing maintenance work etc. can be reduced, and the time from stopping electrolysis to starting maintenance work can be shortened.

[0166] In the above-mentioned operating method of the electrolysis device 70, when the electrolytic cell 50 of the electrolysis device 70 is of a bipolar type and has a plurality of electrolytic cells 65, the discharging step can be performed for all of the electrolytic cells 65 using an external load 8 as shown in Fig. 1. However, the discharging step can be performed for a portion of the plurality of electrolytic cells 65 (one electrolytic cell 65 or a plurality of electrolytic cells 65). By performing the discharging step for a portion of the electrolytic cells 65, the electrodes 2 in the portion of the electrolytic cells 65 can be more sufficiently protected from deterioration. When implementing this for some of the electrolytic cells 65, it is sufficient to form an electric circuit including some of the electrolytic cells 65 and the external load 8. Specifically, this can be implemented for some of the electrolytic cells 65 by connecting the anode 2a of the electrolytic cell 65 at the upstream end in the positive current direction and the cathode 2c of the electrolytic cell 65 at the downstream end in the positive current direction with a cable or the like, with the external load 8 interposed therebetween. Furthermore, when discharging is performed for some of the electrolytic cells 65, the counter voltage can be obtained by measuring the potential difference between the anode 2a of the electrolytic cell 65 at the end of the electrolytic cell 65 to be subjected to the discharging step and the cathode 2c of the electrolytic cell 65 at the end of the electrolytic cell 65 in the electrolytic bath 50 (measured at both ends of the external load 8, etc.), and dividing by the number of the electrolytic cells 65, in the same manner as when measuring for all of the electrolytic cells 65. Alternatively, the counter voltage can be obtained by measuring the counter voltage for each electrolytic cell 65 and dividing the integrated value of each counter voltage by the number of the electrolytic cells.

[0167] In the above-mentioned operating method, the amount of charge held by the cathode 2c is preferably 1.1 times or more the amount of charge held by the anode 2a. When the electrolysis device 70 is operated using such electrodes, the operating method of the electrolysis device 70 can be suitably applied. The charge held by the cathode 2c is the charge held by the cathode 2c in the cathode chamber 5c that controls the amount of hydrogen gas based on the charge held (C) when electrolysis of the electrolyte in the current application step is stopped (at the end of the current application step). Specifically, the charge held by the cathode 2c (C) is determined by passing a positive current through the cathode 2c to sufficiently reduce it, stopping the positive current, and measuring the potential of the cathode 2c while passing a reverse current, and the time integrated value of the reverse current until the potential of the cathode 2c becomes equal to the potential of the anode 2a. The charge held by the anode 2a (c) can be measured in the same manner as the charge held by the cathode 2c. In the above-mentioned operating method, the amount of charge held by the cathode 2c can be made 1.1 times or more the amount of charge held by the anode 2a by appropriately selecting the materials of the anode 2a and the cathode 2c.

[0168] In this embodiment, the components of the electrolysis device 70 described above can be used to fabricate an electrolysis device 70 having a configuration as shown in FIG. 1, for example, but is not limited to this.

[0169] In the method for operating the electrolysis apparatus according to the present embodiment, the above-mentioned effects become more pronounced by using a variable power source such as solar power or wind power.

[0170] The electrolytic apparatus and the method of operating the electrolytic apparatus according to the embodiments of the present invention have been illustrated above with reference to the drawings. However, the electrolytic apparatus and the method of operating the electrolytic apparatus according to the present invention are not limited to the above examples, and the above embodiments can be modified as appropriate.

[0171] The present invention will be specifically described below with reference to Examples and Comparative Examples in Table 1, but the present invention is not limited thereto.

[0172] [Table 1]

[0173] (Electrodes and diaphragms used in the examples and comparative examples) (Creation of the cathode) First, a plain weave mesh obtained by weaving nickel fine wires with a diameter of 0.15 mm with an opening size of 20 meshes was blasted with alumina powder having a weight average particle size of 100 μm or less, and then the mesh was acid-treated in 6 N hydrochloric acid at room temperature for 5 minutes, washed with water, dried, and cut to a size of 50 cm square to obtain cathode substrate A.

[0174] A plain weave mesh in which nickel fine wires with a diameter of 0.15 mm were woven with an opening of 40 mesh was blasted with alumina powder having a weight average particle size of 100 μm or less, and then subjected to an acid treatment in 6 N hydrochloric acid at room temperature for 5 minutes. Thereafter, the mesh was washed with water, dried, and cut to a size of 50 cm square to obtain cathode substrate B.

[0175] A plain weave mesh made by weaving nickel fine wires with a diameter of 0.1 mm with an opening of 60 mesh was blasted with alumina powder having a weight average particle size of 100 μm or less, and then subjected to an acid treatment in 6 N hydrochloric acid at room temperature for 5 minutes. Thereafter, the mesh was washed with water, dried, and cut to a size of 50 cm square to obtain cathode substrate C.

[0176] A plain weave mesh in which nickel fine wires with a diameter of 0.1 mm were woven with 100 mesh openings was blasted with alumina powder having a weight average particle size of 100 μm or less, and then subjected to an acid treatment in 6 N hydrochloric acid at room temperature for 5 minutes. Thereafter, the mesh was washed with water, dried, and cut to a size of 50 cm square to obtain cathode substrate D.

[0177] A plain weave mesh in which nickel fine wires with a diameter of 0.05 mm were woven with 200 mesh openings was blasted with alumina powder having a weight average particle size of 100 μm or less, and then subjected to an acid treatment in 6 N hydrochloric acid at room temperature for 5 minutes. Thereafter, the mesh was washed with water, dried, and cut to a size of 50 cm square to obtain cathode substrate E.

[0178] Next, a palladium nitrate solution (Tanaka Precious Metals, palladium concentration: 100 g / L) and a dinitrodiammine platinum nitrate solution (Tanaka Precious Metals, platinum concentration: 100 g / L) were mixed so that the molar ratio of palladium to platinum was 1:1 to prepare a coating solution.

[0179] A vat containing the first coating liquid was placed at the bottom of the coating roll, the coating liquid was soaked into an EPDM coating roll, a roll was placed on top of it so that the roll and the coating liquid were always in contact with each other, and a PVC roller was placed on top of it to apply the coating liquid to the cathode substrate A (roll method). Before the coating liquid dried, the substrate sample A was quickly passed between two EPDM sponge rolls to suck up and remove the coating liquid that had accumulated at the intersections of the mesh of the cathode substrate A. Thereafter, the substrate sample A was dried at 50°C for 10 minutes to form a coating film, and then the coating film was thermally decomposed by heating and baking at 500°C for 10 minutes using a muffle furnace. This cycle of roll coating, drying and thermal decomposition was repeated a predetermined number of times, and further, post-heating was performed in an air atmosphere at 500°C for 1 hour to prepare a cathode A.

[0180] Cathode B was produced in the same manner as cathode A, except that cathode substrate B was used as the substrate.

[0181] Cathode C was produced in the same manner as cathode A, except that cathode substrate C was used as the substrate.

[0182] Cathode D was produced in the same manner as cathode A, except that cathode substrate D was used as the substrate.

[0183] Cathode E was produced in the same manner as cathode A, except that cathode substrate E was used as the substrate.

[0184] Cathode F was prepared in a manner similar to that of Cathode B, except that the substrate was subjected to fewer roll coating, drying and pyrolysis cycles.

[0185] (Measurement of the oxidation curve of the cathode sample) Each of the cathodes A to F was prepared and immersed in a fluororesin beaker filled with an electrolytic solution of 30 wt % KOH. The temperature of the KOH aqueous solution was maintained at 90° C. A current of 0.4 A / cm was applied to the cathode in an apparatus equipped with a cathode, a platinum wire mesh (counter electrode), and a fluororesin cylinder surrounding the counter electrode, which ensured electrical conductivity. 2 A reduction current with a current density of 0.05 A / cm was applied for 30 minutes to generate hydrogen. 2The change in the potential of the cathode was measured by passing an oxidation current of 100 kcal / g, and the change in the potential was plotted against the total charge of the current passed to obtain an oxidation curve of the cathode.

[0186] The measurements were carried out at 90°C using a meshed platinum electrode as the counter electrode. The fluororesin cylinder used had many 1mm diameter holes drilled around it. The hydrogen electrode potential of the cathode was measured by the three-electrode method using a Luggin capillary to eliminate the effects of ohmic loss due to liquid resistance. The distance between the tip of the Luggin capillary and the cathode was always fixed at 0.05 mm. Silver-silver chloride (Ag / AgCl) was used as the reference electrode for the three-electrode method.

[0187] (Measurement of the amount of negative charge stored in the cathode chamber during hydrogen generation) For cathodes A to F, the total charge of the current passed until the hydrogen electrode potential reached -0.8 Vv.s. Ag / AgCl in the measured cathode oxidation curve was taken as the negative charge stored in the cathode chamber during hydrogen generation.

[0188] (Preparation of anode) The anodes used in the examples and comparative examples will be described.

[0189] Anode A was prepared by cutting an expanded nickel sheet having a thickness of 0.5 mm and an aperture ratio of 40% into a 50 cm square.

[0190] Anode B was prepared by treating an expanded nickel plate having a thickness of 0.5 mm and an aperture ratio of 40% with 6N hydrochloric acid at room temperature for 5 minutes, rinsing with water, drying, and cutting into a 50 cm square.

[0191] Anode C was prepared by cutting a nickel expand sheet having a thickness of 1 mm and an aperture ratio of 54%, which had been subjected to a blasting treatment in advance, into a 50 cm square.

[0192] A suspension was prepared by mixing and stirring 100 parts by weight of nickel oxide powder having a particle size of 0.2 to 2 μm, 2.25 parts by weight of gum arabic, 0.7 parts by weight of carboxymethylcellulose, 0.001 parts by weight of sodium lauryl sulfate, and 100 parts by weight of water. Granules having a particle size of 5 to 50 μm were prepared from the suspension using a spray dryer granulator.

[0193] The granulated material was sprayed onto both sides of anode C by plasma spraying. In the plasma spraying, a mixture of argon and nitrogen in a ratio of 1:0.8 was used as the plasma gas. The thickness of the catalyst layer precursor that covers the surface of the conductive substrate was appropriately adjusted so that the final capacity of the anode chamber would be an arbitrary value, and these were used as anode precursors D and E.

[0194] This was placed in a quartz tube. The quartz tube was inserted into a tubular furnace, the inside of the quartz tube was heated to 200°C, and a hydrogen gas flow was continuously supplied into the quartz tube for 2 hours to reduce the precursor of the catalyst layer. Through the above steps, an electrode was obtained that had a conductive base material and a catalyst layer that covered the conductive base material. This electrode was cut to a 50 cm square. Anodes C and E were cut to a size of 50 cm long x 50 cm wide.

[0195] (Measurement of oxygen electrode potential of anode sample) Each of the anodes A to E was prepared and immersed in a fluororesin beaker filled with an electrolyte solution of 30 wt % KOH. The temperature of the KOH aqueous solution was maintained at 90° C. In a device equipped with an anode, a platinum wire mesh (counter electrode), and a fluororesin cylinder surrounding the counter electrode, and with these elements ensuring electrical conductivity, a current of 0.4 A / cm was applied to the anode. 2 A current density of 0.05 A / cm was applied to generate hydrogen for 30 minutes. 2 A reduction current of 1000 kcal / kg was applied to the anode sample, and the change in potential was measured. This change in potential was plotted against the total charge retained by the applied current to obtain the oxidation curve of the anode.

[0196] The measurements were carried out at 90°C using a meshed platinum electrode as the counter electrode. The fluororesin cylinder used had many 1mmφ holes drilled around it. The oxygen electrode potential of the anode was measured by the three-electrode method using a Luggin capillary to eliminate the effects of ohmic loss due to solution resistance. The distance between the tip of the Luggin capillary and the anode was always fixed at 0.05 mm. Silver-silver chloride (Ag / AgCl) was used as the reference electrode for the three-electrode method.

[0197] (Measurement of the amount of positive charge stored in the oxygen electrode chamber during oxygen generation) In the anode reduction curves measured for anodes A to E, the total charge of the current passed until the oxygen electrode potential became 0 V vs. Ag / AgCl was defined as the positive charge stored in the anode chamber during oxygen evolution.

[0198] The diaphragms used in the examples and comparative examples were prepared as follows. 135 g of zirconium oxide ("EP Zirconium Oxide", manufactured by Daiichi Kigenso Kagaku Kogyo Co., Ltd.) and 210 g of N-methyl-2-pyrrolidone (manufactured by Wako Pure Chemical Industries, Ltd.) were placed in a 1000 mL ball mill pot containing 1 kg of SUS balls with a particle size of 0.5 mm. These were stirred at a rotation speed of 70 rpm in an atmosphere of 25°C for 3 hours to obtain a mixture through which they were dispersed. The obtained mixture was filtered through a stainless steel sieve (mesh size 30) to separate the balls from the mixture. 45 g of polysulfone ("Udel" (trademark), manufactured by Solvay Advanced Polymers, Inc.) and 18 g of polyvinylpyrrolidone (weight average molecular weight (Mw) 900000, manufactured by Wako Pure Chemical Industries, Ltd.) were added to the mixture from which the balls were separated, and the mixture was stirred and dissolved at 60°C for 12 hours using a three-one motor to obtain a coating liquid having the following composition. Polysulfone: 15 parts by weight Polyvinylpyrrolidone: 6 parts by weight N-methyl-2-pyrrolidone: 70 parts by weight Zirconium oxide: 45 parts by weight

[0199] This coating liquid was applied to both surfaces of a substrate, a polyphenylene sulfide mesh (manufactured by Kureha Co., Ltd., film thickness 280 μm, mesh size 358 μm, thread diameter 150 μm), using a comma coater so that the coating thickness was 150 μm on each side. Immediately after coating, the substrate coated with the coating liquid was exposed to steam from a coagulation bath containing a 30°C pure water / isopropanol mixture (manufactured by Wako Pure Chemical Industries, Ltd., pure water / isopropanol = 50 / 50 (v / v)) for 2 minutes. Immediately thereafter, the substrate coated with the coating liquid was immersed in the coagulation bath for 4 minutes. Then, a coating film was formed on the substrate surface by coagulating the polysulfone. The coating film was then thoroughly washed with pure water to obtain a porous membrane.

[0200] The average pore size on the surface of this porous membrane was 1.9 μm. The thickness was 580 μm. The porosity was 43%. The mode diameter of ZrO2 was 5.0 μm. The ratio of the mode diameter of the inorganic particles to the average pore size of the porous membrane (mode diameter / average pore size) was 2.6. This porous membrane was named diaphragm A.

[0201] (Gaskets and conductive elastic mats used in the examples and comparative examples) The gaskets used in this example and comparative example were rectangular with a thickness of 4.0 mm, a width of 18 mm, and inner dimensions of 504 mm square, with a slit structure for inserting and holding the diaphragm inside. The slit structure had a 0.4 mm gap 14 mm in the width direction on the inside of the gasket to accommodate the edge of the diaphragm. This gasket was made of EPDM rubber, and had an elastic modulus of 4.0 MPa at 100% deformation.

[0202] The conductive elastic mat used was made by weaving nickel wire with a wire diameter of 0.15 mm and corrugating it to a wave height of 5 mm. It was 5 mm thick, had a resilience of 150 g / cm2 at 50% compression deformation, and had an opening of about 5 mesh.

[0203] Example 1 The bipolar electrolytic cell of Example 1 was prepared in the following manner.

[0204] A bipolar element was made by attaching cathode A to the cathode surface of a bipolar frame and an anode to the anode surface of a bipolar element frame. A cathode terminal element was made by attaching cathode A to the frame of a cathode terminal element. Anode terminal element was made by attaching anode A to the frame of an anode terminal element.

[0205] 99 pieces of the bipolar elements were prepared. In addition, one each of the cathode terminal element and the anode terminal element was prepared.

[0206] Gaskets were attached to the metal frame portions of all bipolar elements, cathode terminal elements, and anode terminal electrolytic cell elements.

[0207] One diaphragm A was sandwiched between the anode terminal element and the cathode side of the bipolar element. 99 bipolar elements were arranged in series such that the anode side of one of the adjacent bipolar elements faced the cathode side of the other, and 98 diaphragms A were sandwiched between each of the adjacent bipolar elements. Furthermore, one diaphragm A was sandwiched between the anode side of the 99th bipolar element and the cathode terminal element. A total of 100 cells were then clamped using a press machine using a fast head, an insulating plate, and a loose head to form the bipolar electrolytic cell of Example 1.

[0208] Example 2 A bipolar electrolytic cell of Example 2 was prepared in the same manner as in Example 1.

[0209] Example 3 A bipolar electrolytic cell of Example 3 was prepared in the same manner as in Example 1, except that the total number of cells was 200.

[0210] Example 4 A bipolar electrolytic cell of Example 4 was prepared in the same manner as in Example 1, except that the cathode B and the anode D were used to make the total number of cells 200.

[0211] Example 5 A bipolar electrolytic cell of Example 5 was prepared in the same manner as in Example 1, except that cathode C and anode C were used.

[0212] Example 6 A bipolar electrolytic cell of Example 6 was prepared in the same manner as in Example 1, except that the cathode D and the anode C were used.

[0213] Example 7 A bipolar electrolytic cell of Example 7 was prepared in the same manner as in Example 1, except that the cathode E and the anode C were used.

[0214] Comparative Example 1 A bipolar electrolytic cell of Comparative Example 1 was prepared in the same manner as in Example 1, except that the cathode A and the anode B were adjusted.

[0215] Comparative Example 2 A bipolar electrolytic cell of Comparative Example 2 was prepared in the same manner as in Example 1, except that the cathode F and the anode E were adjusted to a total of 200 cells.

[0216] Comparative Example 3 In the same manner as in Example 1, a bipolar electrolytic cell of Comparative Example 3 was prepared.

[0217] Comparative Example 4 A bipolar electrolytic cell of Example 4 was prepared in the same manner as in Example 1, except that the total number of cells was 200.

[0218] The electrolyte used was a 30% KOH aqueous solution. A liquid pump was used to circulate the electrolyte between the anode chamber, oxygen separation tank (gas-liquid separation tank for the anode), and anode chamber, and between the cathode chamber, hydrogen separation tank (gas-liquid separation tank for the cathode), and cathode chamber. The temperature of the electrolyte was adjusted to 90°C.

[0219] As the circulation flow path, a 20A pipe was used, in which the part of the pipe that came into contact with the electrolyte was made of SGP (carbon steel pipe for piping) and the inside surface was treated with Teflon lining.

[0220] The gas-liquid separation tank is 1400mm high and has a volume of 1m 3 The liquid volume in the gas-liquid separation tank was set to about 50% of the design volume.

[0221] From the rectifier to the bipolar electrolytic cell, 6 kA / m for each cathode and anode area S1 2 In Example 1, since the area S1 of the electrode was 500 mm×500 mm, a current of 1.5 kA was applied from the rectifier to the bipolar electrolytic cell.

[0222] The pressure in the electrolytic cell was measured with a pressure gauge and electrolysis was performed while adjusting the cathode side pressure to 50 kPa and the oxygen side pressure to 49 kPa. The pressure was adjusted with a pressure control valve installed downstream of the pressure gauge.

[0223] The alkaline water electrolysis in the examples and comparative examples was evaluated as follows.

[0224] (Electrolytic Test) Current density 6kA / m 2 The cell voltage V of the electrolytic cell was measured, and the arithmetic mean value (V) of the electrolytic cell was calculated.

[0225] (stop electrolysis) Current density 6kA / m 2 After applying current continuously for 1 hour, the rectifier was turned off and the cell voltage V was continued to be measured. The time until the arithmetic mean of the cell voltage V became 0.1 V or less was defined as the discharge time, based on the time immediately after the electrolysis was stopped.

[0226] In Examples 1, 4, 5, 6, and 7 and Comparative Examples 1 and 2, the voltage of the electrolytic cell was rapidly reduced during discharge using an external load of 0.02 Ωm2 / cell.

[0227] For Examples 2 and 3, an external load of 2 Ωm2 / cell was used to rapidly reduce the voltage of the electrolytic cell during discharge.

[0228] In Comparative Examples 3 and 4, no external load was used and the batteries were allowed to discharge naturally.

[0229] (SD test) The electrolysis test and the stop of electrolysis were repeated 5000 times. At 500, 1000, and 5000 times, the current density was 6 kA / m 2 The current was passed continuously for 1 hour, the cell voltage of the electrolytic cell was measured, and the arithmetic mean value V was calculated.

[0230] (Gas concentration measurement) Regarding the impurity gas concentration in the electrolytic cell when restarting after electrolysis was stopped, the oxygen concentration in hydrogen (H2 / O2) was measured using a hydrogen concentration meter on the cathode chamber side, and the hydrogen concentration in oxygen (O2 / H2) was constantly measured using a hydrogen concentration meter on the anode chamber side. [Industrial Applicability]

[0231] According to the present invention, it is possible to provide a method for operating an electrolysis device that can suppress the deterioration of electrodes [concern 1] and the deterioration of gas purity [concern 2] under a variable power supply. [Explanation of symbols]

[0232] 1 Bulkhead 2 electrodes 2a anode 2c cathode 2c1 Cathode main body 2c2 Cathode auxiliary part 2c3 Conductor section 3 Outer frame 4 Diaphragm 41 Covering material 4t Uncoated top of membrane 5 Electrode chamber 5a Anode chamber 5c cathode chamber 5i Electrolyte inlet 5o Electrolyte outlet 5ai anolyte inlet 5ao anolyte outlet 5ci catholyte inlet 5co catholyte outlet 6 Rectifier plate 7 Gasket 8 External Load 9 Switchgear 10. Header 10O External Header 10Oai Anode inlet header (anode inlet hose) 10Oao Anode outlet header (anode outlet hose) 10Oci Cathode Inlet Header (Cathode Inlet Hose) 10Oco Cathode Outlet Header (Cathode Outlet Hose) 20 Conduit 20Oai anode liquid pipe 20Oao liquid collection tube for anode 20Oci cathode liquid pipe 20Oco Cathode collection tube 50 bipolar electrolyzer 51g fast head, loose head 51a Anode terminal element 51c Cathode Terminal Element 51r tie rod 51i Insulating plate 60 Multi-pole element 65 Electrolysis Cell 70 Electrolyzer 71 Liquid delivery pump 72 Gas-liquid separation tank 72h Hydrogen Separation Tank 72o Oxygen Separation Tank 73 Water supply device 74 Rectifier 75 Oxygen concentration meter 76 Hydrogen concentration meter 77 Flow meter 78 Pressure Gauge 80 Pressure Control Valve 102a anode 102c cathode 104 Diaphragm 104t Uncoated upper end of membrane 105a Anode chamber 105c Cathode chamber 107 Gasket 165 Electrolysis Cell D1 given direction along the bulkhead (vertical direction) Z Zero gap structure L Waterline C Electrical Circuit

Claims

1. A method for operating an electrolysis apparatus having an anode chamber having an anode and a cathode chamber having a cathode, the anode chamber and the cathode chamber being separated from each other by a diaphragm, comprising the steps of: The power source is variable, The capacitance of the cathode is 1.1 times or more the capacitance of the anode; a current application step in which electrolysis of the electrolyte in the anode chamber and the cathode chamber is performed; a stopping step in which electrolysis of the electrolyte in the anode chamber and the cathode chamber is stopped, In the stopping step, a discharging step of electrically connecting the electrolytic cell of the electrolysis device to an external load; A method for operating an electrolysis apparatus comprising the steps of:

2. The capacitance of the anode is 10000 C / m 2 is as follows: The capacitance of the cathode is 1000 C / m 2 That's all.

2. The method for operating an electrolysis apparatus according to claim 1.

3. The discharge step reduces the discharge voltage to 0.1 V or less within 60 minutes.

3. A method for operating an electrolysis apparatus according to claim 1 or 2.

4. The discharging step is carried out when the voltage of the electrolytic cell falls below a value set before the voltage of the electrolytic cell reaches a potential range in which each electrode corrodes in the stopping step. A method for operating the electrolysis apparatus according to any one of claims 1 to 3.

5. The electrolytic cell of the electrolysis device is a bipolar type, The electrolytic cell includes a plurality of electrolytic cells each including one anode chamber and one cathode chamber, and the discharging step is performed in a part of the plurality of electrolytic cells. A method for operating the electrolysis apparatus according to any one of claims 1 to 4.

6. The electrolytic cell has 30 or more electrolytic cells each including one anode chamber and one cathode chamber. A method for operating the electrolysis apparatus according to any one of claims 1 to 5.

7. The anode comprises at least one nickel compound selected from the group consisting of nickel oxide, metallic nickel, nickel hydroxide, and a nickel alloy; A method for operating the electrolysis apparatus according to any one of claims 1 to 6.

8. The anode has a thickness in the range of 0.1 mm to 3.0 mm; A method for operating the electrolysis apparatus according to any one of claims 1 to 7.

9. The cathode contains at least one Pt group compound selected from the group consisting of Ru-La-Pt, Ru-Ce, Pt-Ce, Pt-Ir, Ir-Pt-Pd, Pt-Pd, and Pt-Ni compounds; A method for operating the electrolysis apparatus according to any one of claims 1 to 8.

10. Including a step of stopping the passage of current. A method for operating the electrolysis apparatus according to any one of claims 1 to 9.

11. The resistance value of the external load is 0.02 to 2 Ωm 2 / cell. A method for operating the electrolysis apparatus according to any one of claims 1 to 10.

Citation Information

Patent Citations

  • Burner for liquid fuel combustion equipment

    JP1980053605A

  • Electrolyzer

    JP2000054177A

  • Alkaline water electrolysis system

    JP2017206731A

  • Electrolysis tank, and method of using the same

    JP2020012146A

  • Electrode for hydrogen generation, process for producing same, and method of electrolysis therewith