Method and device for treating electrodeposited nickel anolyte
By treating the electrowinning nickel anolyte through multiple continuous neutralization, sorting, and impurity removal processes, and using calcium hydroxide or calcium oxide as a neutralizing agent, the problems of nickel loss and impurity treatment in the electrowinning nickel anolyte are solved, achieving efficient nickel recovery and purity improvement, while reducing treatment costs and wastewater generation.
Patent Information
- Application Number
- CN202411213125.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-12
AI Technical Summary
The electrolytic nickel anolyte treatment process suffers from a large amount of impurities and acid consumption, leading to increased nickel loss.
A combination of continuous neutralization process and multi-stage sorting, solid-liquid separation and impurity removal process is adopted. Calcium hydroxide or calcium oxide is used as a neutralizing agent. Through multi-stage continuous neutralization, sorting, solid-liquid separation and impurity removal, the pH value is controlled, nickel hydroxide precipitation is reduced and impurities are recovered.
It effectively reduces nickel loss, lowers neutralization costs, reduces wastewater generation, improves nickel purity, and controls and stabilizes the endpoint pH value, thereby reducing wastewater treatment costs.
Smart Images

Figure CN118929977A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of nickel electrolytic anode liquid treatment, and in particular to a method and device for treating nickel electrolytic anode liquid. Background Art
[0002] Electrolytic nickel production produces a large amount of anolyte. The anolyte contains a large amount of nickel sulfate, which needs to be circulated to the electrolytic nickel production line for continued use. However, in addition to nickel sulfate, the anolyte also contains a large amount of acid and impurities enriched in the electrolytic process, such as iron, copper, zinc, manganese, calcium, cobalt, magnesium, etc.
[0003] In the related art, the treatment of the electrolytic nickel anode liquid consumes a large amount of alkali and also leads to increased nickel loss. Summary of the invention
[0004] The purpose of the present application is to provide a method and device for treating electrolytic nickel anode liquid to solve the above-mentioned problems.
[0005] To achieve the above objectives, the present application provides a method for treating an electrolytic nickel anolyte in a first aspect, comprising:
[0006] A continuous neutralization process, mixing a neutralizer and an electrodeposited nickel anolyte to perform a multi-stage continuous neutralization treatment, so as to precipitate impurities in the electrodeposited nickel anolyte to obtain a neutralized slurry, wherein the neutralized slurry comprises a nickel-containing solution, a first precipitated particle having a first particle size, and a second precipitated particle having a second particle size, wherein the first particle size is smaller than the second particle size;
[0007] A sorting process, performing a sorting treatment on the neutralized slurry to sort out the second precipitated particles from the neutralized slurry to obtain a sorted slurry and the second precipitated particles, wherein the sorted slurry includes the nickel-containing solution and the first precipitated particles;
[0008] A solid-liquid separation step, performing solid-liquid separation on the sorted slurry to obtain the nickel-containing solution;
[0009] The impurity removal step is to remove impurities from the nickel-containing solution to obtain a nickel-rich impurity-removed solution.
[0010] Optionally, the multi-stage continuous neutralization treatment includes a continuous first-stage neutralization treatment, a second-stage neutralization treatment and a third-stage neutralization treatment, and the endpoint pH of the first-stage neutralization treatment is less than or equal to the endpoint pH of the second-stage neutralization treatment, and the endpoint pH of the second-stage neutralization treatment is less than or equal to the endpoint pH of the third-stage neutralization treatment.
[0011] Optionally, the endpoint pH of the neutralization treatment in the first stage is 1-2;
[0012] The endpoint pH of the second stage neutralization treatment is 2-5;
[0013] The endpoint pH of the neutralization treatment in the third stage is 5-6.
[0014] Optionally, the neutralizing agent includes at least one of calcium hydroxide, calcium oxide, and a slurry containing calcium hydroxide and / or calcium oxide.
[0015] Optionally, the impurity removal process includes:
[0016] The first impurity removal step is to filter and remove impurities from the nickel-containing solution to obtain a first impurity-removed liquid after removing suspended matter, wherein the first impurity-removed liquid satisfies Si≤100mg / L and Ca≤650mg / L;
[0017] A second impurity removal step, performing an extraction and impurity removal treatment on the first impurity-removed liquid to obtain a nickel-containing raffinate, wherein the nickel-containing raffinate satisfies Ca≤50mg / L and Mg≤2000mg / L;
[0018] The deoiling step is to deoil the nickel-containing raffinate to obtain a nickel-rich impurity-free liquid.
[0019] Optionally, the second impurity removal step includes:
[0020] The first impurity-removed liquid is mixed with a saponified extractant to perform extraction and impurity-removal treatment to obtain a nickel-containing raffinate, wherein the saponification rate of the extractant is 20%-30%.
[0021] Optionally, also include:
[0022] The pH adjustment step is to adjust the pH of the nickel-rich impurity-removed liquid to obtain a pH-adjusted liquid with a pH of 3-4, and the pH-adjusted liquid is used as a cathode liquid for nickel electrolysis.
[0023] Optionally, the pH adjustment step includes:
[0024] The nickel-rich impurity-removed liquid is mixed with a pH buffer and the electrolytic nickel anode liquid to perform pH adjustment treatment to obtain a pH-adjusted liquid with a pH of 3-4.
[0025] Optionally, also include:
[0026] In the dissolution process, the second precipitated particles are mixed with the electrolytic nickel anode liquid to dissolve the nickel hydroxide contained in the second precipitated particles to obtain a dissolving solution, and the dissolving solution is used to return to the continuous neutralization process.
[0027] A second aspect of the present application provides a device for treating an electrolytic nickel anode liquid, the device being used to perform the method described, comprising:
[0028] A neutralization unit, comprising a plurality of neutralization tanks connected in series, wherein the plurality of neutralization tanks connected in series are used to mix a neutralizer and an electrodeposited nickel anolyte to perform a continuous multi-stage neutralization treatment, so as to precipitate impurities in the electrodeposited nickel anolyte to obtain a neutralized slurry, wherein the neutralized slurry comprises a nickel-containing solution, a first precipitated particle having a first particle size, and a second precipitated particle having a second particle size, wherein the first particle size is smaller than the second particle size;
[0029] A sorting unit is used to sort the neutralized slurry obtained by the neutralization unit to sort the second precipitated particles from the neutralized slurry to obtain sorted slurry and the second precipitated particles, wherein the sorted slurry includes the nickel-containing solution and the first precipitated particles;
[0030] A filtering unit, used for performing solid-liquid separation on the sorted slurry obtained by the sorting unit to obtain the nickel-containing solution;
[0031] The impurity removal unit is used to remove impurities from the nickel-containing solution obtained by the filtering unit to obtain a nickel-rich impurity-removed solution.
[0032] Optionally, the sorting unit includes a cyclone.
[0033] Optionally, the filtration unit includes a thickener and a filter.
[0034] Optionally, the impurity removal unit includes an extraction device.
[0035] Optionally, the device further comprises:
[0036] A dissolving unit is used to mix the second precipitated particles obtained by the sorting unit with the electrolytic nickel anode liquid to dissolve the nickel hydroxide contained in the second precipitated particles to obtain a dissolving solution, and the dissolving solution is used to return to the continuous neutralization process.
[0037] Optionally, the device further comprises:
[0038] The pH adjusting unit is used to perform pH adjustment on the nickel-rich impurity-removed liquid obtained by the impurity removal unit to obtain a pH-adjusted liquid with a pH of 3-4, and the pH-adjusted liquid is used as a cathode liquid for nickel electrolysis.
[0039] Compared with the prior art, the beneficial effects of this application include:
[0040] The method for treating electrolytic nickel anolyte provided in the present application continuously neutralizes the neutralizer and the electrolytic nickel anolyte, which can not only reduce the nickel hydroxide precipitation caused by local over-alkali, but also facilitate the control of stable endpoint pH. In addition, almost no wastewater is generated during the neutralization process, the amount of chlorinated wastewater produced during the impurity removal process is small, and the wastewater treatment cost is low.
[0041] The device for treating electrolytic nickel anode liquid provided in the present application includes a neutralization unit, a sorting unit, a filtration unit and an impurity removal unit, wherein the neutralization unit includes a plurality of neutralization tanks connected in series, and the pH value can be adjusted by slowly adding alkali, which can reduce the amount of nickel hydroxide precipitation caused by local over-alkalinity and is also convenient for controlling the stable endpoint pH. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] In order to more clearly illustrate the technical solutions of the embodiments of the present application, the drawings required for use in the embodiments will be briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present application and therefore should not be regarded as limiting the scope of the present application.
[0043] Figure 1 A flow chart of a method for treating an electrolytic nickel anolyte provided in some embodiments of the present application;
[0044] Figure 2 A flow chart of a method for treating an electrolytic nickel anolyte provided in some embodiments of the present application;
[0045] Figure 3 A flow chart of a method for treating an electrolytic nickel anolyte provided in some embodiments of the present application;
[0046] Figure 4 A flow chart of a method for treating an electrolytic nickel anolyte provided in some embodiments of the present application;
[0047] Figure 5 A flow chart of an apparatus for treating an electrolytic nickel anolyte provided in some embodiments of the present application;
[0048] Figure 6 A flow chart of an apparatus for treating electrolytic nickel anode liquid provided in some other embodiments of the present application.
[0049] Digital ID Description:
[0050] 100-neutralization unit, 200-sorting unit, 300-filtration unit, 400-impurity removal unit, 500-dissolution unit, 600-pH adjustment unit. DETAILED DESCRIPTION
[0051] As used herein:
[0052] "Prepared from" is synonymous with "comprising." As used herein, the terms "comprising," "including," "having," "containing," or any other variation thereof, are intended to cover a non-exclusive inclusion. For example, a composition, process, method, article, or apparatus that comprises the listed elements is not necessarily limited to only those elements but may include other elements not expressly listed or inherent to such composition, process, method, article, or apparatus.
[0053] The conjunction "consisting of excludes any unspecified element, step, or component. If used in a claim, this phrase renders the claim closed-ended so that it does not include materials other than those described, except for conventional impurities associated therewith. When the phrase "consisting of" appears in a clause of the body of a claim rather than immediately following the subject matter, it limits only the elements described in that clause; other elements are not excluded from the claim as a whole.
[0054] When an amount, concentration, or other value or parameter is expressed as a range, a preferred range, or a range defined by a series of upper preferred values and lower preferred values, this should be understood as specifically disclosing all ranges formed by any pairing of any range upper limit or preferred value with any range lower limit or preferred value, regardless of whether the range is disclosed separately. For example, when a range of "1 to 5" is disclosed, the described range should be interpreted as including ranges "1 to 4", "1 to 3", "1 to 2", "1 to 2 and 4 to 5", "1 to 3 and 5", etc. When a numerical range is described in this article, unless otherwise stated, the range is intended to include its end values and all integers and fractions within the range.
[0055] In these examples, parts and percentages are by mass unless otherwise indicated.
[0056] "Parts by mass" refers to the basic unit of measurement for expressing the mass ratio of multiple components. 1 part can represent any unit mass, such as 1g or 2.689g. If we say that the mass of component A is a parts and the mass of component B is b parts, it means the ratio of the mass of component A to the mass of component B is a:b. Alternatively, it means that the mass of component A is aK and the mass of component B is bK (K is an arbitrary number, indicating a multiple factor). It should not be misunderstood that, unlike the mass parts, the sum of the mass of all components is not limited to 100 parts.
[0057] "And / or" is used to indicate that one or both of the stated situations may occur, for example, A and / or B includes (A and B) and (A or B).
[0058] See also Figure 1 As shown, the first aspect of the present application provides a method for treating an electrolytic nickel anode liquid, comprising:
[0059] S100, a continuous neutralization step, mixing a neutralizer and an electrodeposited nickel anolyte to perform a multi-stage continuous neutralization treatment, so as to precipitate impurities in the electrodeposited nickel anolyte to obtain a neutralized slurry, wherein the neutralized slurry includes a nickel-containing solution, a first precipitated particle having a first particle size, and a second precipitated particle having a second particle size, wherein the first particle size is smaller than the second particle size;
[0060] In some embodiments, the neutralizer is slurried before use, and the slurrying includes: mixing the neutralizer and water to obtain a neutralizer slurry;
[0061] S200, a sorting process, performing a sorting treatment on the neutralized slurry to sort out the second precipitated particles from the neutralized slurry to obtain a sorted slurry and a second precipitated particle, wherein the sorted slurry includes a nickel-containing solution and the first precipitated particle;
[0062] S300, a solid-liquid separation step, performing solid-liquid separation on the sorted slurry to obtain a nickel-containing solution;
[0063] It should be noted that the solid-liquid separation process also produces filter residues, in which Ni is ≤ 0.1%; the filter residues can be recycled as gypsum waste and used as building materials;
[0064] In some embodiments, the filter residue is washed to obtain filter residue washing water, and the filter residue washing water is returned to the neutralizer slurry;
[0065] S400, an impurity removal step, removing impurities from the nickel-containing solution to obtain a nickel-rich impurity-removed solution.
[0066] In some embodiments, the multi-stage continuous neutralization treatment includes a first-stage neutralization treatment, a second-stage neutralization treatment, and a third-stage neutralization treatment, and the endpoint pH of the first-stage neutralization treatment is less than or equal to the endpoint pH of the second-stage neutralization treatment, and the endpoint pH of the second-stage neutralization treatment is less than or equal to the endpoint pH of the third-stage neutralization treatment. The above-mentioned multi-stage continuous neutralization treatment can further reduce the loss of nickel.
[0067] In some embodiments, the endpoint pH of the first stage neutralization treatment is 1-2;
[0068] Optionally, the endpoint pH of the first stage neutralization treatment may be 1, 1.1, 1.2, 1.3, 1.4, 1.5, 1.6, 1.7, 1.8, 1.9, 2 or any value between 1 and 2;
[0069] The endpoint pH of the second stage neutralization treatment is 2-5;
[0070] Optionally, the endpoint pH of the second stage neutralization treatment may be 2, 2.5, 3, 3.5, 4, 4.5, 5 or any value between 2 and 5;
[0071] The endpoint pH of the third stage neutralization treatment is 5-6.
[0072] Optionally, the endpoint pH of the third stage neutralization treatment can be 5, 5.1, 5.2, 5.3, 5.4, 5.5, 5.6, 5.7, 5.8, 5.9, 6 or any value between 5 and 6.
[0073] In the above embodiment, the temperature of the neutralization process can be room temperature, which can help reduce the processing cost of the electrolytic nickel anolyte. The end point of the third stage neutralization treatment is greater than 5, which can effectively remove impurity silicon and further improve the purity of nickel.
[0074] The time of the continuous neutralization reaction can be adjusted according to the amount of the electrolytic nickel anode liquid to be treated. In some embodiments, the time of the continuous neutralization reaction is 2h-4h.
[0075] In some embodiments, the neutralizer includes at least one of calcium hydroxide, calcium oxide, and a solution containing calcium hydroxide and / or calcium oxide. When the above-mentioned neutralizer includes at least one of calcium hydroxide, calcium oxide, and a slurry containing calcium hydroxide and / or calcium oxide, it can replace liquid alkali or soda ash to reduce the neutralization cost; in addition, the unit price of the above-mentioned neutralizer is relatively low, and the pH value can be adjusted to above 5 during neutralization, while the pH value needs to be adjusted to above 7 when using liquid alkali to precipitate nickel, and the alkali demand is large.
[0076] See also Figure 2 As shown, in some embodiments, the impurity removal process includes:
[0077] S410, a first impurity removal step, filtering and removing impurities from the nickel-containing solution, removing suspended matter to obtain a first impurity-removed liquid, wherein the first impurity-removed liquid satisfies Si≤100mg / L and Ca≤650mg / L;
[0078] Optionally, the Si content of the first impurity-removed liquid can be 0.1 mg / L, 1 mg / L, 10 mg / L, 20 mg / L, 40 mg / L, 60 mg / L, 80 mg / L, 100 mg / L or any value less than or equal to 100 mg / L, and the Ca content can be 450 mg / L, 500 mg / L, 550 mg / L, 600 mg / L, 650 mg / L or any value between 450 mg / L and 650 mg / L;
[0079] S420, a second impurity removal step, performing an extraction and impurity removal treatment on the first impurity-removed liquid to obtain a nickel-containing raffinate, wherein the nickel-containing raffinate satisfies Ca≤50mg / L and Mg≤2000mg / L;
[0080] Optionally, the Ca content in the nickel-containing raffinate may be 0.1 mg / L, 1 mg / L, 10 mg / L, 20 mg / L, 30 mg / L, 40 mg / L, 50 mg / L or any value less than or equal to 50 mg / L, and the Mg content may be 1 mg / L, 10 mg / L, 100 mg / L, 500 mg / L, 1000 mg / L, 1500 mg / L, 2000 mg / L or any value less than or equal to 2000 mg / L;
[0081] It should be noted that the Ca content in the nickel-containing raffinate is high, while the Mg content is relatively low. The standard electrode potentials of Ca and Mg are relatively high. 2+ Negative, will not take precedence over nickel ion reduction and precipitation, but the high calcium ion concentration in the nickel-containing raffinate is prone to produce calcium sulfate, affecting the electrolytic process, so the extraction and impurity removal treatment is used to control Ca≤50mg / L, and Mg is removed at the same time;
[0082] S430, deoiling step, deoiling the nickel-containing raffinate to obtain a nickel-rich impurity-free liquid.
[0083] In some embodiments, activated carbon is used for oil removal.
[0084] In some embodiments, the second impurity removal step comprises:
[0085] The first impurity-removed liquid is mixed with the saponified extractant to perform extraction and impurity-removal treatment to obtain a nickel-containing raffinate, wherein the saponification rate of the extractant is 20%-30%.
[0086] Optionally, the saponification rate of the extractant can be 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30% or any value between 20% and 30%.
[0087] It should be noted that the extractant includes P204 and / or P507. The above extractants can effectively separate nickel from impurities and further improve the purity of nickel.
[0088] In some embodiments, the pH value of the nickel-containing raffinate is 2.5-4. The pH value of the nickel-containing raffinate within the above range can be helpful for preparing a cathode liquid for nickel electrowinning.
[0089] See also Figure 3 As shown, in some embodiments, it also includes:
[0090] S500, pH adjustment process, pH adjustment treatment is performed on the nickel-rich impurity-removed liquid to obtain a pH-adjusted liquid with a pH of 3-4, and the pH-adjusted liquid is used as a cathode liquid for nickel electrowinning.
[0091] Optionally, the pH value of the pH-adjusted liquid can be 3, 3.1, 3.2, 3.3, 3.4, 3.5, 3.6, 3.7, 3.8, 3.9, 4 or any value between 3 and 4.
[0092] In some embodiments, the pH adjustment step comprises:
[0093] The nickel-rich impurity-removed liquid is mixed with a pH buffer and an electrodeposited nickel anode liquid for pH adjustment treatment to obtain a pH-adjusted liquid with a pH of 3-4.
[0094] It should be noted that when the pH of the solution after pH adjustment is 3-4, it is used as the cathode liquid for nickel electrolysis in the electrolysis process.
[0095] See also Figure 4 As shown, in some embodiments, it also includes:
[0096] S600, a dissolution process, mixing the second precipitated particles with the electrolytic nickel anode liquid to dissolve the nickel hydroxide contained in the second precipitated particles to obtain a dissolving solution, which is used to return to the continuous neutralization process.
[0097] It should be noted that the second precipitated particles are calcium sulfate particles mixed with large nickel hydroxide precipitates. By mixing with the electrolytic nickel anode liquid, the large nickel hydroxide precipitates can be dissolved in the dissolving solution. The dissolving solution is then returned to the continuous neutralization process to recover the nickel hydroxide in the large particle precipitates, thereby reducing nickel losses.
[0098] See also Figure 5 As shown, the second aspect of the present application provides a device for treating an electrolytic nickel anode liquid, the device being used to perform the above method, comprising:
[0099] The neutralization unit 100 includes a plurality of neutralization tanks connected in series, and the plurality of neutralization tanks connected in series are used to mix a neutralizer and an electrodeposited nickel anolyte to perform a continuous multi-stage neutralization treatment, so as to precipitate impurities in the electrodeposited nickel anolyte to obtain a neutralized slurry, wherein the neutralized slurry includes a nickel-containing solution, a first precipitated particle having a first particle size, and a second precipitated particle having a second particle size, wherein the first particle size is smaller than the second particle size;
[0100] The sorting unit 200 is used to sort the neutralized slurry obtained by the neutralization unit 100 to sort out the second precipitated particles from the neutralized slurry to obtain sorted slurry and second precipitated particles, wherein the sorted slurry includes the nickel-containing solution and the first precipitated particles;
[0101] The filtering unit 300 is used to perform solid-liquid separation on the sorted slurry obtained by the sorting unit 200 to obtain a nickel-containing solution;
[0102] The impurity removal unit 400 is used to remove impurities from the nickel-containing solution obtained by the filtering unit 300 to obtain a nickel-rich impurity-removed solution.
[0103] In some embodiments, the inlet of the neutralization unit 100 is connected to the slurrying unit, which includes a slaked / quicklime silo, a screw feeder, a slurrying tank, and a neutralizer slurry storage tank connected in sequence; the neutralizer slurry storage tank provides neutralizer slurry and is connected to the inlet of the neutralization unit 100.
[0104] In some embodiments, the separation unit 200 includes a cyclone that is connected to the outlet of the neutralization unit 100 through a pipeline.
[0105] In some embodiments, the filtration unit 300 includes a thickener and a filter, wherein the inlet of the thickener is in communication with the overflow port of the cyclone.
[0106] In some embodiments, the filtration unit 300 further includes a slag washing water storage tank, a thickener supernatant storage tank, and a filtration filtrate tank.
[0107] Exemplarily, the outlet of the thickener in the filtration unit 300 includes a supernatant outlet and an underflow outlet, the supernatant outlet is connected to the thickener supernatant storage tank, the underflow outlet is connected to the inlet of the filter, the filtrate outlet of the filter is connected to the inlet of the filter filtrate tank, and the filter residue outlet in the filter is connected to the inlet of the residue washing water storage tank.
[0108] In some embodiments, the impurity removal unit 400 includes an extraction device, which is connected to the outlet of the filtrate tank.
[0109] See also Figure 6 As shown, in some embodiments, the device further includes:
[0110] The dissolution unit 500 is used to mix the second precipitated particles obtained by the sorting unit 200 with the electrolytic nickel anode liquid to dissolve the nickel hydroxide contained in the second precipitated particles to obtain a dissolving solution, which is used to return to the continuous neutralization process.
[0111] It can be seen from the above that the dissolving unit 500 is connected to the underflow outlet of the cyclone.
[0112] See also Figure 6 As shown, in some embodiments, the device further includes:
[0113] The pH adjustment unit 600 is used to perform pH adjustment on the nickel-rich impurity-removed liquid obtained by the impurity removal unit 400 to obtain a pH-adjusted liquid with a pH of 3-4. The pH-adjusted liquid is used as a cathode liquid for nickel electrolysis.
[0114] It can be seen from the above that the pH adjustment unit 600 is communicated with the outlet of the dissolution unit 500 .
[0115] The embodiments of the present application will be described in detail below in conjunction with specific examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present application and should not be considered as limiting the scope of the present application. If specific conditions are not specified in the examples, they are carried out according to normal conditions or the conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0116] The components of the electrolytic nickel anolyte, calcium hydroxide, and calcium oxide used in the examples and comparative examples of the present application are shown in Table 1, Table 2, and Table 3, respectively.
[0117] Table 1 Composition of nickel electrodeposition anolyte
[0118]
[0119] Table 2 Calcium hydroxide composition
[0120]
[0121] Table 3 Calcium oxide composition
[0122]
[0123] Example 1
[0124] This embodiment provides a method for treating an electrolytic nickel anolyte, comprising:
[0125] S1. Slurrying: Calcium oxide is slurried with pure water, and the liquid-to-solid ratio of the slurry is 4m 3 : 1t, stir evenly to prepare neutralizer slurry;
[0126] S2. Neutralization: The neutralizer slurry and the electrolytic nickel anode liquid are continuously added into a continuous neutralization tank composed of 6 stirring neutralization reaction tanks in series. The process reaction temperature is room temperature. The pH of the first two reaction tanks is controlled to be 1-2, the pH of the third and fourth reaction tanks is controlled to be 2-4, and the pH of the last two reaction tanks is controlled to be 5-6. Calcium oxide is added at 1.0 times the theoretical amount for neutralization reaction with sulfuric acid. 70% of the total amount of calcium oxide is added to the first tank. The pH of the second tank is measured. H; 20% of the total amount of calcium oxide added in the third tank, and the pH value is measured in the fourth tank; 10% of the total amount of calcium oxide added in the fifth tank, and the pH value is measured in the sixth tank. The amount of calcium hydroxide added in the rear tank is adjusted in time according to the pH value measured in the front tank. After continuous reaction for 3 hours, the neutralized slurry is pumped from the sixth neutralization reaction tank into the cyclone, wherein the neutralized slurry includes a nickel-containing solution, calcium sulfate particles less than 150 mesh, and calcium sulfate particles greater than 150 mesh;
[0127] S3, sorting: nickel-containing solution and calcium sulfate particles smaller than 150 mesh in the neutralized slurry are discharged from the overflow pipe under the action of the inner spiral flow in the cyclone, and calcium sulfate particles larger than 150 mesh are discharged from the bottom flow port into the pickling tank as the outer spiral descends. Electrolytic nickel anode liquid is added to adjust the pH of calcium sulfate particles larger than 150 mesh in the pickling tank to about 2, and the reaction is returned to the neutralization tank after 0.5h;
[0128] S4, solid-liquid separation: the nickel-containing solution and calcium sulfate particles less than 150 mesh enter the thickener to obtain the thickener underflow and the thickener supernatant. The thickener underflow is filtered and separated to obtain filter residue and filtrate. The filter residue is washed simultaneously during the filtration and separation. The Ni content in the filter residue is 0.09%. The slag washing water is returned to step S1 as slurry bottom water. The filtrate and the thickener supernatant are mixed to obtain the nickel-containing solution;
[0129] S5, impurity removal: the nickel-containing solution is filtered through a precision filter to obtain a first impurity-removed liquid, the first impurity-removed liquid enters a neutralization liquid storage tank for standby use, the Si content of the first impurity-removed liquid is 89 mg / L, and the Ca content is 645 mg / L; the first impurity-removed liquid is subjected to extraction and impurity removal to obtain a nickel-containing raffinate, the extractant used is P204, the saponification rate of the extractant is 20%, and the pH of the nickel-containing raffinate is controlled to be 2.6; the nickel-containing raffinate is deoiled by activated carbon to obtain a nickel-rich impurity-removed liquid, and the oil content of the nickel-rich impurity-removed liquid is 0.33 mg / L;
[0130] S6. pH adjustment: Mix the nickel-rich impurity-removed liquid, boric acid, and nickel electrodeposition anode liquid for pH adjustment treatment, control the pH to be stable at 3, and reuse it as cathode liquid in the electrodeposition process.
[0131] The method for treating the electrolytic nickel anode liquid is as follows: Figure 1 shown.
[0132] A second aspect of the present embodiment provides a device for treating an electrolytic nickel anode liquid, which is used to perform the above method, including:
[0133] Slurrying unit, neutralization unit, sorting unit, filtration unit, impurity removal unit, dissolution unit and pH adjustment unit;
[0134] The slurry unit includes a slaked / quicklime silo, a screw feeder, a slurry tank, and a neutralizer slurry storage tank;
[0135] The neutralization unit includes 6 neutralization tanks connected in series;
[0136] The sorting unit includes a cyclone;
[0137] The filtration unit includes a thickener and a security filter;
[0138] The impurity removal unit includes a box-type extraction system;
[0139] The dissolution unit includes a pickling tank;
[0140] The pH adjustment unit includes a pH adjustment reaction tank;
[0141] The neutralizer in the slaked / quicklime silo is transported to the slurry tank by the screw feeder in the slurrying unit, water is added to obtain the neutralizer slurry, and the neutralizer slurry is transported to the neutralizer slurry storage tank; the neutralizer slurry in the neutralizer slurry storage tank is respectively transported to the 1st tank, the 3rd tank and the 5th tank in the neutralization unit, the outlet of the 6th tank is connected to the inlet of the cyclone, the outlet of the bottom flow port at the lower end of the cyclone is connected to the inlet of the pickling tank, the outlet of the pickling tank is connected to the neutralization unit, the outlet of the overflow pipe at the upper end of the cyclone is connected to the inlet of the thickener, the bottom flow outlet of the thickener is connected to the inlet of the filter separator, the filtrate outlet of the filter separator and the supernatant outlet of the thickener are connected to the inlet of the security filter, the outlet of the security filter is connected to the inlet of the box-type extraction system, and the outlet of the box-type extraction system is connected to the inlet of the value adjustment reaction tank.
[0142] Example 2
[0143] This embodiment provides a method for treating an electrolytic nickel anolyte, and the device used is consistent with that in embodiment 1, including:
[0144] S1. Slurrying: Calcium hydroxide is slurried with pure water, and the slurry liquid-to-solid ratio is 4m 3 : 1t, stir evenly to prepare neutralizer slurry;
[0145] S2, neutralization: the neutralizer slurry and the electrolytic nickel anolyte are continuously added to a continuous neutralization tank composed of 6 stirring neutralization reaction tanks connected in series at the same time. The process reaction temperature is room temperature. The pH of the first two reaction tanks is controlled to be 1-2, the pH of the third and fourth reaction tanks is controlled to be 2-4, and the pH of the last two reaction tanks is controlled to be 5-6. Calcium hydroxide is added at 1.05 times the theoretical amount for neutralization reaction with sulfuric acid. The first tank is added at 55% of the total amount of calcium hydroxide added, and the pH of the second tank is measured; the third tank is added at 35% of the total amount of calcium hydroxide added, and the pH of the fourth tank is measured; the fifth tank is added at 10% of the total amount, and the pH of the sixth tank is measured. The amount of calcium hydroxide added in the rear tank is adjusted in time according to the pH value measured in the front tank. After continuous reaction for 3 hours, the neutralized slurry is pumped from the sixth neutralization reaction tank into the cyclone;
[0146] S3, sorting: nickel-containing solution and calcium sulfate particles smaller than 150 mesh in the neutralized slurry are discharged from the overflow pipe under the action of the inner spiral flow in the cyclone, and calcium sulfate particles larger than 150 mesh are discharged from the bottom flow port into the pickling tank along with the outer spiral flow. Electrolytic nickel anode liquid is added to adjust the pH of calcium sulfate particles larger than 150 mesh in the pickling tank to about 2.1, and the reaction is returned to the neutralization tank after 0.5h.
[0147] S4, solid-liquid separation: the nickel-containing solution and calcium sulfate particles less than 150 mesh enter the thickener to obtain the thickener underflow and the thickener supernatant. The thickener underflow is filtered and separated to obtain filter residue and filtrate. The filter residue is washed simultaneously during the filtration and separation. The Ni content in the filter residue is 0.06%. The slag washing water is returned to step S1 as slurry bottom water. The filtrate and the thickener supernatant are mixed to obtain the nickel-containing solution;
[0148] S5, impurity removal: the nickel-containing solution is filtered through a precision filter to obtain a first impurity-removed liquid, the first impurity-removed liquid enters a neutralization liquid storage tank for standby use, the Si content of the first impurity-removed liquid is 58 mg / L, and the Ca content is 530 mg / L; the first impurity-removed liquid is subjected to extraction and impurity removal to obtain a nickel-containing raffinate, the extractant used is P507, the saponification rate of the extractant is 30%, and the pH of the raffinate is controlled to be 3.9; the nickel-containing raffinate is deoiled by activated carbon to obtain a nickel-rich impurity-removed liquid, and the oil content of the nickel-rich impurity-removed liquid is 0.96 mg / L;
[0149] S6. pH adjustment: Mix the nickel-rich impurity-removed liquid, boric acid, and nickel electrodeposition anode liquid for pH adjustment treatment to control the pH to be stable at 3.6, and reuse it as cathode liquid in the electrodeposition process.
[0150] Example 3
[0151] This embodiment provides a method for treating an electrolytic nickel anolyte, and the device used is consistent with that in embodiment 1, including:
[0152] S1. Slurrying: Calcium hydroxide is slurried with pure water, and the slurry liquid-to-solid ratio is 4m 3 : 1t, stir evenly to prepare neutralizer slurry;
[0153] S2, neutralization: the neutralizer slurry and the electrolytic nickel anolyte are continuously added to a continuous neutralization tank composed of 6 stirring neutralization reaction tanks connected in series at the same time. The process reaction temperature is room temperature. The pH of the first two reaction tanks is controlled to be 1-2, the pH of the third and fourth reaction tanks is controlled to be 2-4, and the pH of the last two reaction tanks is controlled to be 5-6. Calcium hydroxide is added at 1.1 times the theoretical amount for neutralization reaction with sulfuric acid. The first tank is added at 65% of the total amount of calcium hydroxide added, and the pH of the second tank is measured; the third tank is added at 25% of the total amount of calcium hydroxide added, and the pH of the fourth tank is measured; the fifth tank is added at 10% of the total amount, and the pH of the sixth tank is measured. The amount of calcium hydroxide added in the rear tank is adjusted in time according to the pH value measured in the front tank. After continuous reaction for 3 hours, the neutralized slurry is pumped from the sixth neutralization reaction tank into the cyclone;
[0154] S3, sorting: nickel-containing solution and calcium sulfate particles smaller than 150 mesh in the neutralized slurry are discharged from the overflow pipe under the action of the inner spiral flow in the cyclone, and calcium sulfate particles larger than 150 mesh are discharged from the bottom flow port into the pickling tank as the outer spiral descends. Electrolytic nickel anode liquid is added to adjust the pH of calcium sulfate particles larger than 150 mesh in the pickling tank to 1.8, and the reaction is returned to the neutralization tank after 0.5h;
[0155] S4, solid-liquid separation: the nickel-containing solution and calcium sulfate particles less than 150 mesh enter the thickener to obtain the thickener underflow and the thickener supernatant. The thickener underflow is filtered and separated to obtain filter residue and filtrate. The filter residue is washed simultaneously during the filtration and separation. The Ni content in the filter residue is 0.04%. The slag washing water is returned to step S1 as slurry bottom water. The filtrate and the thickener supernatant are mixed to obtain the nickel-containing solution;
[0156] S5, impurity removal: the nickel-containing solution is filtered through a precision filter to obtain a first impurity-removed liquid, the first impurity-removed liquid enters a neutralization liquid storage tank for standby use, the Si content of the first impurity-removed liquid is 35 mg / L, and the Ca content is 576 mg / L; the first impurity-removed liquid is subjected to extraction and impurity removal to obtain a nickel-containing raffinate, the extractant used is P507, the saponification rate of the extractant is 30%, and the pH of the raffinate is controlled to be 3.4; the nickel-containing raffinate is deoiled by activated carbon to obtain a nickel-rich impurity-removed liquid, and the oil content of the nickel-rich impurity-removed liquid is 0.62 mg / L;
[0157] S6. pH adjustment: Mix the nickel-rich impurity-removed liquid, boric acid, and nickel electrodeposition anode liquid for pH adjustment treatment, control the pH to be stable at 3.3, and reuse it as cathode liquid in the electrodeposition process.
[0158] Comparative Example 1
[0159] This comparative example provides a method for treating an electrolytic nickel anolyte, and the device used is consistent with that in Example 1, comprising:
[0160] S1. Add soda ash solution (soda ash consumption is about 2.5t / tNi) to the electrolytic nickel anode liquid, control the pH value to 7-8 during the reaction, react at 60°C for 3h, filter and wash, backwash to remove sodium in the filter cake during filtration, obtain nickel hydroxide / nickel carbonate filter cake and nickel precipitation liquid (filtrate), and the nickel precipitation liquid is successively deweighted by resin (recovering nickel and cobalt), magnesium precipitation (adding calcium carbonate), and decarbonization (decarbonization tower) to obtain sodium sulfate wastewater, with a wastewater volume of about 20m 3 / t Ni needs to be processed separately;
[0161] S2. Add the nickel hydroxide / nickel carbonate filter cake into another part of the electrolytic nickel anode liquid for slurry dissolution, control the Ni concentration to about 90 g / L, and add a pH buffer to stabilize the end point pH at 3.6 (after nickel precipitation, some impurities in the original electrolytic nickel anode liquid are opened out and go with the filtrate, and then the nickel hydroxide / nickel carbonate is used as a base to neutralize the other part of the anode liquid, reducing the amount of liquid alkali / soda ash, and returning nickel to the system). After the reaction is completed, filter to obtain the electrolytic nickel cathode liquid for nickel electrolysis.
[0162] This process requires all nickel to be precipitated, so the neutralization cost is very high, the amount of wastewater is large, the wastewater treatment cost is high, and water resources are wasted.
[0163] Comparative Example 2
[0164] This comparative example provides a method and device for treating electrolytic nickel anolyte, which is different from Example 1 in that in S2, the neutralization step of this comparative example, the neutralizer slurry and the electrolytic nickel anolyte are simultaneously and continuously added to a neutralization unit consisting of a neutralization tank, and the other conditions are consistent with the example. After neutralization, obvious large-particle green crystals appear in the slurry, and the nickel content of the liquid after neutralization drops to about 85g / L, and the endpoint pH value drops to 4.5.
[0165] The components of the nickel electrodeposition cathode liquid prepared in the above examples and comparative examples are shown in Table 4.
[0166] Table 4 Composition of cathode solution for nickel electrowinning
[0167] Ingredients (mg / L) Ni Ca Mg Si Co Cu Zn Fe Pb Oil content pH Example 1 91360 14 115 79 0.73 0.15 0.01 1.37 0.01 0.39 3 Example 2 93870 3 131 59 0.66 0.14 0.01 0.51 0.01 0.96 3.6 Example 3 93150 9 142 35 0.54 0.09 0.01 0.63 0.01 0.62 3.3 Comparative Example 1 92640 0.15 1.19 97 9.42 0.12 0.01 0.14 0.10 0.53 3.6 Comparative Example 2 85140 12 123 85 2.59 0.62 0.05 2.58 0.06 0.65 3.5
[0168] It can be seen from the above embodiments and comparative examples that the continuous neutralization reaction between the neutralizer and the electrolytic nickel anode liquid can not only reduce the nickel hydroxide precipitation caused by local over-alkali, but also facilitate the control of the stable endpoint pH, and almost no wastewater is generated during the neutralization process, the amount of chlorinated wastewater produced during the impurity removal process is small, and the wastewater treatment cost is low.
[0169] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present application.
[0170] In addition, those skilled in the art will appreciate that, although some embodiments herein include certain features included in other embodiments but not other features, the combination of features of different embodiments is meant to be within the scope of the present application and form different embodiments. For example, in the above claims, any one of the claimed embodiments may be used in any combination. The information disclosed in this background technology section is intended only to deepen the understanding of the overall background technology of the present application and should not be regarded as an admission or in any form of implication that the information constitutes prior art known to those skilled in the art.
Claims
1. A method for treating an electrolytic nickel anolyte, characterized in that: include: A continuous neutralization process, mixing a neutralizer and an electrodeposited nickel anolyte to perform a multi-stage continuous neutralization treatment, so as to precipitate impurities in the electrodeposited nickel anolyte to obtain a neutralized slurry, wherein the neutralized slurry comprises a nickel-containing solution, a first precipitated particle having a first particle size, and a second precipitated particle having a second particle size, wherein the first particle size is smaller than the second particle size; A sorting process, performing a sorting treatment on the neutralized slurry to sort out the second precipitated particles from the neutralized slurry to obtain a sorted slurry and the second precipitated particles, wherein the sorted slurry includes the nickel-containing solution and the first precipitated particles; A solid-liquid separation step, performing solid-liquid separation on the sorted slurry to obtain the nickel-containing solution; The impurity removal step is to remove impurities from the nickel-containing solution to obtain a nickel-rich impurity-removed solution.
2. The method according to claim 1, characterized in that: The multi-stage continuous neutralization treatment includes a first-stage neutralization treatment, a second-stage neutralization treatment and a third-stage neutralization treatment, and the endpoint pH of the first-stage neutralization treatment is less than or equal to the endpoint pH of the second-stage neutralization treatment, and the endpoint pH of the second-stage neutralization treatment is less than or equal to the endpoint pH of the third-stage neutralization treatment.
3. The method according to claim 2, characterized in that The endpoint pH of the neutralization treatment in the first stage is 1-2; The endpoint pH of the second stage neutralization treatment is 2-5; The endpoint pH of the neutralization treatment in the third stage is 5-6.
4. The method according to claim 1, characterized in that: The neutralizing agent includes at least one of calcium hydroxide, calcium oxide, and a slurry containing calcium hydroxide and / or calcium oxide.
5. The method according to claim 4, characterized in that The impurity removal process comprises: The first impurity removal step is to filter and remove impurities from the nickel-containing solution to obtain a first impurity-removed liquid after removing suspended matter, wherein the first impurity-removed liquid satisfies Si≤100mg / L and Ca≤650mg / L; A second impurity removal step, performing an extraction and impurity removal treatment on the first impurity-removed liquid to obtain a nickel-containing raffinate, wherein the nickel-containing raffinate satisfies Ca≤50mg / L and Mg≤2000mg / L; The deoiling step is to deoil the nickel-containing raffinate to obtain a nickel-rich impurity-free liquid.
6. The method according to claim 5, characterized in that The second impurity removal step comprises: The first impurity-removed liquid is mixed with a saponified extractant to perform extraction and impurity-removal treatment to obtain a nickel-containing raffinate, wherein the saponification rate of the extractant is 20%-30%.
7. The method according to claim 1, characterized in that Also includes: The pH adjustment step is to adjust the pH of the nickel-rich impurity-removed liquid to obtain a pH-adjusted liquid with a pH of 3-4, and the pH-adjusted liquid is used as a cathode liquid for nickel electrolysis.
8. The method according to claim 7, characterized in that The pH adjustment process comprises: The nickel-rich impurity-removed liquid is mixed with a pH buffer and the electrolytic nickel anode liquid to perform pH adjustment treatment to obtain a pH-adjusted liquid with a pH of 3-4.
9. The method according to claim 1, characterized in that: Also includes: In the dissolution process, the second precipitated particles are mixed with the electrolytic nickel anode liquid to dissolve the nickel hydroxide contained in the second precipitated particles to obtain a dissolving solution, and the dissolving solution is used to return to the continuous neutralization process.
10. A device for treating nickel electrodeposition anolyte, characterized in that: The device is used to perform the method according to any one of claims 1 to 9, comprising: A neutralization unit, comprising a plurality of neutralization tanks connected in series, wherein the plurality of neutralization tanks connected in series are used to mix a neutralizer and an electrodeposited nickel anolyte to perform a continuous multi-stage neutralization treatment, so as to precipitate impurities in the electrodeposited nickel anolyte to obtain a neutralized slurry, wherein the neutralized slurry comprises a nickel-containing solution, a first precipitated particle having a first particle size, and a second precipitated particle having a second particle size, wherein the first particle size is smaller than the second particle size; A sorting unit is used to sort the neutralized slurry obtained by the neutralization unit to sort the second precipitated particles from the neutralized slurry to obtain sorted slurry and the second precipitated particles, wherein the sorted slurry includes the nickel-containing solution and the first precipitated particles; A filtering unit, used for performing solid-liquid separation on the sorted slurry obtained by the sorting unit to obtain the nickel-containing solution; The impurity removal unit is used to remove impurities from the nickel-containing solution obtained by the filtering unit to obtain a nickel-rich impurity-removed solution.
11. The device according to claim 10, characterized in that The separation unit comprises a cyclone; and / or, the filtration unit comprises a thickener and a filter; And / or, the impurity removal unit includes an extraction device.
12. The device according to claim 10, characterized in that The device also includes: A dissolving unit is used to mix the second precipitated particles obtained by the sorting unit with the electrolytic nickel anode liquid to dissolve the nickel hydroxide contained in the second precipitated particles to obtain a dissolving solution, and the dissolving solution is used to return to the continuous neutralization process.
13. The device according to claim 10, characterized in that The device also includes: The pH adjusting unit is used to perform pH adjustment on the nickel-rich impurity-removed liquid obtained by the impurity removal unit to obtain a pH-adjusted liquid with a pH of 3-4, and the pH-adjusted liquid is used as a cathode liquid for nickel electrolysis.
Citation Information
Cited By
Method and device for treating electrodeposited nickel anolyte
CN119932653A
Method and apparatus for treating nickel electrowinning anolyte
CN119932653B
Impurity removal and recovery method for electrodeposited nickel anolyte
CN120099591A
Method and device for treating electro-deposition nickel anolyte
WO2026152895A1
Impurity removal and recovery for electrowon nickel anolyte
WO2026199732A1