Method for enriching indium from zinc oxide smoke dust leachate through ultrasonic-enhanced calcium carbonate precipitation

The ultrasonic enhanced calcium carbonate precipitation technology enriches indium from zinc oxide soot leaching solution, solving the problems of environmental pollution and low efficiency in the existing indium enrichment methods, and achieving efficient and low-cost indium enrichment and separation effects.

CN118957313AInactive Publication Date: 2024-11-15BEIJING MINING & METALLURGICAL TECH GRP CO LTD +1

Patent Information

Application Number
CN202410849787.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-27
Publication Date
2024-11-15
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing indium enrichment methods have problems such as environmental pollution caused by solvent extraction, long mechanical stirring time, large reagent consumption and low efficiency, and lack of efficient precipitation and separation technology.

Method used

Ultrasonic enhanced calcium carbonate precipitation is used to enrich indium from zinc oxide soot leaching solution, and the precipitation time is shortened by ultrasonic cavitation, mechanical and thermal effects. The pH of the precipitation solution is controlled by hydrolysis of calcium carbonate to achieve separation of indium and zinc.

Benefits of technology

It significantly shortens the precipitation time of indium, reduces production costs, reduces environmental pollution, improves the enrichment efficiency of indium, and saves energy consumption and calcium carbonate consumption.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118957313A_ABST
    Figure CN118957313A_ABST
Patent Text Reader

Abstract

The invention discloses a method for enriching indium from zinc oxide smoke dust leach liquor through ultrasonic-enhanced calcium carbonate precipitation, which comprises the following steps: 1) mixing zinc oxide smoke dust and acid liquor, carrying out ultrasonic-microwave synergistic leaching, and filtering to obtain the zinc oxide smoke dust leach liquor; 2) carrying out ultrasonic iron powder reduction on the zinc oxide smoke dust leaching solution obtained in the step 1) to obtain a precipitation mother solution; and (3) carrying out ultrasonic enhanced calcium carbonate precipitation on the precipitation mother liquor obtained in the step (2), and filtering after carrying out ultrasonic precipitation reaction on the leachate. According to the method, the indium precipitation time can be shortened, the production cost of enterprises is reduced, the environmental pollution is effectively reduced, and a new idea is provided for indium enrichment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of indium precipitation, and in particular to a method for enriching indium from zinc oxide fume leaching solution by ultrasonically strengthening calcium carbonate precipitation. Background Art

[0002] Indium has been listed as a key strategic metal by many countries. It is an important raw material for the electronics industry and is widely used in display screens, solar photovoltaic cells, solders and other fields. Indium does not have an independent deposit. It is usually associated with lead-zinc ores. It is a by-product of lead-zinc smelting and is enriched in the smoke produced by rotary furnace roasting. The indium content is about 0.4%, which has recycling value. Due to the low content of indium in minerals, it is generally necessary to enrich it after leaching before the subsequent process can be carried out. At present, the main methods for enriching indium are solvent extraction, precipitation, adsorption and other methods; however, solvent extraction will discharge a large amount of organic wastewater, causing environmental pollution, conventional mechanical stirring precipitation of indium has a long existence time, large reagent consumption, and low efficiency of adsorption method. Therefore, it is of great significance to develop a new type of indium precipitation technology. However, research on ultrasonic enhanced precipitation separation of metal ions has not been reported, so ultrasonic enhanced precipitation technology has broad prospects. Summary of the invention

[0003] In view of the above-mentioned existing problems, the present invention provides a method for efficiently enriching indium from zinc oxide smoke leachate by ultrasonic enhanced precipitation. The present invention can shorten the time of indium precipitation, reduce the production cost of enterprises, effectively reduce environmental pollution, and precipitate indium in zinc oxide smoke leachate by ultrasonic enhanced calcium carbonate, providing a new idea for the enrichment of indium. The present invention adopts ultrasonic enhanced calcium carbonate precipitation to enrich indium in zinc oxide smoke leachate, and utilizes the cavitation, mechanical and thermal effects of ultrasound to shorten the time of indium precipitation. Utilizing the principle that calcium carbonate belongs to the strong base and weak acid salt, carbonate hydrolysis produces hydroxide, making the solution weakly alkaline, which is convenient for controlling the pH of the precipitate, and indium ions combine with hydroxide to generate indium hydroxide precipitation, while achieving the separation of indium and zinc.

[0004] Specifically, the method provided by the present invention for enriching indium from zinc oxide fume leaching solution by ultrasonically enhancing calcium carbonate precipitation comprises the following steps: 1) mixing zinc oxide fume and acid solution and performing ultrasonic-microwave synergistic leaching, and obtaining zinc oxide fume leaching solution after filtering; 2) subjecting the zinc oxide smoke leaching solution obtained in step 1) to ultrasonic iron powder reduction to obtain a precipitation mother solution; 3) The precipitation mother solution obtained in step 2) is subjected to ultrasonic enhanced calcium carbonate precipitation, and the leaching solution is filtered after the ultrasonic precipitation reaction.

[0005] In the present invention, the preparation of the leachate is prepared by using ultrasound-microwave synergistic leaching, which has the advantages of short leaching time and high leaching rate. Ultrasonic waves have cavitation and mechanical effects, and no additional mechanical stirring is required. The cavitation effect of ultrasound can make calcium carbonate powder evenly dispersed, and the collapse of bubbles produced by cavitation can release a large amount of energy, accelerate the occurrence of precipitation reaction, and shorten the time for indium precipitation to reach equilibrium. Ultrasound has a thermal effect, and no external heating is required. The thermal effect of ultrasound is not constant, and a temperature gradient effect is generated. This temperature gradient effect can promote the occurrence of indium precipitation reaction, reduce the activation energy of precipitation reaction, and save energy consumption. Calcium carbonate is a strong base weak acid salt. The hydrolysis of carbonate produces hydroxide, making the solution weakly alkaline, which is convenient for controlling the pH of the precipitate. Indium ions combine with hydroxide to generate indium hydroxide precipitation, and the separation of indium and zinc is achieved at the same time. And calcium carbonate is cheap and low in cost.

[0006] Preferably, in step 1), the ultrasonic power is 180-230 W, and the microwave power is 150-220 W; preferably, the ultrasonic power is 200 W, and the microwave power is 200 W.

[0007] Preferably, in step 1), the ultrasound-microwave synergistic leaching time is 25 to 70 minutes, preferably 30 to 60 minutes.

[0008] Preferably, in step 1), the acid solution is sulfuric acid, the concentration of sulfuric acid is 150-200 g / L, and the liquid-solid ratio is (6-10):1; preferably, the concentration of sulfuric acid is 180 g / L, and the liquid-solid ratio is 8:1.

[0009] More preferably, in step 1), the pH of the filtrate obtained after leaching the zinc oxide fume is between 0 and -0.5.

[0010] Preferably, in step 2), the reduction treatment includes adding iron powder for reduction and performing ultrasonic enhanced reduction.

[0011] In the present invention, before precipitation begins, iron powder is used to reduce the precipitation mother liquid to make Fe 3+ Reduction to Fe 2+ , which can prevent the co-precipitation of trivalent iron and indium. The iron powder can also consume the remaining sulfuric acid in the zinc oxide fume leaching solution and reduce the subsequent amount of calcium carbonate.

[0012] More preferably, in step 2), the time of the ultrasonic enhanced reduction is 15 to 25 minutes, preferably 20 minutes.

[0013] More preferably, in step 2), the power of ultrasonic enhanced iron powder reduction is 200±50W.

[0014] In the present invention, the Fe in the leaching solution is reduced by optimized ultrasonic enhanced reduction.3+ Better reduction to Fe 2+ , which facilitates the subsequent precipitation of indium.

[0015] Further preferably, in step 2), the amount of iron powder added is determined according to the content of trivalent iron in the leaching solution combined with the chemical reaction measurement, following the principle of appropriate excess. For example, the amount of iron powder used in the embodiment of the present invention is 5-10g.

[0016] Preferably, step 3) further comprises adding calcium carbonate powder, and when the pH value of the solution reaches 3.5 to 4.5, preferably 4, turning off the ultrasound, stopping adding calcium carbonate, and rapidly filtering the precipitate. The ultrasonic treatment power is 150 to 300W.

[0017] In the present invention, the pH values ​​of the hydrolysis precipitation of indium ions, zinc ions, divalent iron ions and aluminum ions in the precipitation mother liquor are different. Calcium carbonate can be used to hydrolyze to be alkaline, and the end point pH of the precipitation liquid is controlled to be 4, which can better achieve the purpose of separating indium from other metal ions in the mother liquor.

[0018] Further preferably, step 3) further comprises charging the precipitation mother liquor of step 2) (the leaching liquor after the iron powder is reduced) into a reaction container, placing the reaction container into an ultrasonic-microwave chemical reactor, monitoring the pH value and temperature of the leaching liquor, performing ultrasonic treatment, optionally opening the microwave reactor but not running the microwave reactor to record the solution temperature; adding calcium carbonate powder, and when the pH value of the solution reaches 4, turning off the ultrasonic generator and filtering the precipitate; and optionally, taking the supernatant and analyzing the ion concentration by ICP to calculate the precipitation rate of indium.

[0019] As a preferred embodiment of the present invention, the zinc oxide smoke leaching solution was prepared by using an ultrasonic-microwave synergistic leaching method, and the process conditions were 180 g / L sulfuric acid, 200 W ultrasonic power, 200 W microwave power, 8:1 liquid-solid ratio, and 30 minutes of leaching time. The zinc oxide smoke leaching solution obtained after filtration was subjected to ultrasonic enhanced iron powder reduction for 20 minutes to reduce the Fe in the leaching solution. 3+ Reduction to Fe 2+ , which is convenient for the subsequent precipitation of indium. After filtration, the concentration of the main metal ions in the mother liquor is: In 3 + :0.564g / L,Zn 2+ :68.15g / L,Fe 2+ :1.49g / L,Al 3+:0.4g / L. The leaching solution after iron powder reduction is placed in a 500ml four-necked flask, and the four-necked flask is placed in an ultrasonic-microwave chemical reactor. A pH agent and a temperature thermocouple are inserted into the four-necked flask to monitor the pH value and temperature of the solution. Turn on the ultrasonic generator, set the appropriate ultrasonic power, and turn on the microwave reactor at the same time, but do not run the microwave reactor in order to record the solution temperature; at the same time, slowly add calcium carbonate powder, and when the solution pH reaches 4, immediately turn off the ultrasonic generator, and quickly filter the precipitate, take the supernatant, analyze the ion concentration by ICP, and calculate the precipitation rate of indium.

[0020] The beneficial effects of the present invention are at least that: the present invention adopts ultrasound to strengthen the precipitation of indium, utilizes the thermal effect of ultrasound, does not need external heating, can save energy consumption, and the thermal effect of ultrasound will produce a temperature gradient. This instantaneous temperature gradient can promote the precipitation of indium, and inhibit the precipitation of impurity ions such as zinc, iron, and aluminum. At the same time, the mechanical effect of ultrasound is utilized, and no additional mechanical stirring is required, which can save energy consumption. At the same time, the cavitation effect of ultrasound can be utilized to accelerate the precipitation reaction speed, shorten the precipitation time, and save the production cost of the enterprise. At the same time, the cavitation effect of ultrasound is utilized, and the precipitant calcium carbonate is evenly dispersed, and the hydrolysis of carbonate ions is more thorough, which can shorten the time required for the pH of the precipitate to reach 4.0, can reduce the consumption of calcium carbonate, and reduce the production cost of the enterprise. The method of the present invention is simple and safe to operate, has a short process flow, and is suitable for industrial process production. The present invention selects calcium carbonate as a precipitant, which is lower in cost than precipitants such as sodium hydroxide, oxalic acid, ammonia water, and sodium carbonate, and is easy to control the pH of the precipitate, and has a better enrichment effect of indium; calcium carbonate is a strong base and weak acid salt, and the alkalinity of the precipitate after precipitation is weak, which is easy to discharge. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the technical solutions in the present invention or the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 This is a process flow chart for enriching indium in zinc oxide fume leaching solution by ultrasonic enhanced calcium carbonate precipitation.

[0023] Figure 2 This is the experimental diagram of ultrasonic enhanced calcium carbonate precipitation of indium. DETAILED DESCRIPTION

[0024] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be clearly and completely described below in conjunction with the drawings of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0025] In the embodiments of the present invention, the raw material zinc oxide dust used is dust generated during the zinc smelting process of Qinghai Western Mining Company, and its composition is shown in the following table.

[0026] Table 1 In Zn Fe Al Cu Pb Ag Si As s Cl F 0.39 50.64 1.82 0.39 0.07 20.00 574.8g / t 0.92 0.08 1.09 0.13 0.04

[0027] Example 1

[0028] First, the zinc oxide smoke leaching solution was prepared by ultrasonic-microwave synergistic enhancement. The preparation process conditions were sulfuric acid concentration of 180g / L, liquid-solid ratio of 8:1, ultrasonic power of 200W, microwave power of 200W, and leaching time of 30 minutes. The zinc oxide smoke leaching solution was obtained after vacuum filtration, and the pH of the leaching solution was -0.3. Then, iron powder was used for reduction, and ultrasonic treatment was performed for 20 minutes to reduce trivalent iron to divalent iron. After vacuum filtration, the precipitation mother liquor was obtained, and the pH of the precipitation mother liquor was 0.4. After that, the precipitation mother liquor was loaded into a 500ml four-necked flask to start the precipitation experiment. The ultrasonic power was set to 200W, and calcium carbonate powder was slowly added. When the precipitation termination pH reached 4.0, the ultrasonic generator was immediately turned off, and the precipitation liquid was quickly vacuum filtered to obtain the precipitation supernatant. 20ml of the precipitation supernatant was taken for ICP analysis, and the precipitation rate of indium was 99.78%. The required time was 23 minutes, and the calcium carbonate consumption was 6.34g. Figure 1 The process of enriching indium in zinc oxide dust leachate by ultrasonic enhanced calcium carbonate precipitation is proposed. Figure 2 This is an experiment on ultrasonic enhanced calcium carbonate precipitation of indium.

[0029] Example 2

[0030] First, the zinc oxide smoke leaching solution was prepared by ultrasonic-microwave synergistic enhancement. The preparation process conditions were sulfuric acid concentration of 180g / L, liquid-solid ratio of 8:1, ultrasonic power of 200W, microwave power of 200W, leaching time of 30 minutes, and zinc oxide smoke leaching solution was obtained after vacuum filtration, and the pH of the leaching solution was -0.3. Then, iron powder was used for reduction, and ultrasonic treatment was performed for 20 minutes to reduce trivalent iron to divalent iron. After vacuum filtration, the precipitation mother liquor was obtained, and the pH of the precipitation mother liquor was 0.4. After that, the precipitation mother liquor was loaded into a 500ml four-necked flask to start the precipitation experiment, the ultrasonic power was set to 200W, and calcium carbonate powder was slowly added. When the precipitation termination pH reached 4.5, the ultrasonic generator was immediately turned off, and the precipitation liquid was quickly vacuum filtered to obtain the precipitation supernatant. 20ml of the precipitation supernatant was taken for ICP analysis, and the precipitation rate of indium was 99.64%. The required time was 24 minutes, and the calcium carbonate consumption was 6.81g.

[0031] Example 3

[0032] First, the zinc oxide smoke leaching solution was prepared by ultrasonic-microwave synergistic enhancement. The preparation process conditions were sulfuric acid concentration of 180g / L, liquid-solid ratio of 8:1, ultrasonic power of 200W, microwave power of 200W, leaching time of 30 minutes, and zinc oxide smoke leaching solution was obtained after vacuum filtration, and the pH of the leaching solution was -0.3. Then, iron powder was used for reduction, and ultrasonic treatment was performed for 20 minutes to reduce trivalent iron to divalent iron. After vacuum filtration, the precipitation mother liquor was obtained, and the pH of the precipitation mother liquor was 0.4. After that, the precipitation mother liquor was loaded into a 500ml four-necked flask to start the precipitation experiment, the ultrasonic power was set to 200W, and calcium carbonate powder was slowly added. When the precipitation termination pH reached 5.0, the ultrasonic generator was immediately turned off, and the precipitation liquid was quickly vacuum filtered to obtain the precipitation supernatant. 20ml of the precipitation supernatant was taken for ICP analysis, and the precipitation rate of indium was 99.98%. The required time was 25 minutes, and the calcium carbonate consumption was 7.36g.

[0033] Example 4

[0034] First, the zinc oxide smoke leaching solution was prepared by ultrasonic-microwave synergistic enhancement. The preparation process conditions were sulfuric acid concentration of 180g / L, liquid-solid ratio of 8:1, ultrasonic power of 200W, microwave power of 200W, leaching time of 30 minutes, and zinc oxide smoke leaching solution was obtained after vacuum filtration, and the pH of the leaching solution was -0.3. Then, iron powder was used for reduction, and ultrasonic treatment was performed for 20 minutes to reduce trivalent iron to divalent iron. After vacuum filtration, the precipitation mother liquor was obtained, and the pH of the precipitation mother liquor was 0.4. After that, the precipitation mother liquor was loaded into a 500ml four-necked flask to start the precipitation experiment, the ultrasonic power was set to 150W, and calcium carbonate powder was slowly added. When the precipitation termination pH reached 4.0, the ultrasonic generator was immediately turned off, and the precipitation liquid was quickly vacuum filtered to obtain the precipitation supernatant. 20ml of the precipitation supernatant was taken for ICP analysis, and the precipitation rate of indium was 94.51%. The required time was 27 minutes, and the calcium carbonate consumption was 7.18g.

[0035] Example 5

[0036] First, the zinc oxide smoke leaching solution was prepared by ultrasonic-microwave synergistic enhancement. The preparation process conditions were sulfuric acid concentration of 180g / L, liquid-solid ratio of 8:1, ultrasonic power of 200W, microwave power of 200W, leaching time of 30 minutes, and zinc oxide smoke leaching solution was obtained after vacuum filtration, and the pH of the leaching solution was -0.3. Then, iron powder was used for reduction, and ultrasonic treatment was performed for 20 minutes to reduce trivalent iron to divalent iron. After vacuum filtration, the precipitation mother liquor was obtained, and the pH of the precipitation mother liquor was 0.4. After that, the precipitation mother liquor was loaded into a 500ml four-necked flask to start the precipitation experiment, the ultrasonic power was set to 250W, and calcium carbonate powder was slowly added. When the precipitation termination pH reached 4.0, the ultrasonic generator was immediately turned off, and the precipitation liquid was quickly vacuum filtered to obtain the precipitation supernatant. 20ml of the precipitation supernatant was taken for ICP analysis, and the precipitation rate of indium was 99.79%. The required time was 20 minutes, and the calcium carbonate consumption was 5.98g.

[0037] Comparative Example 1

[0038] First, the zinc oxide smoke leaching solution was prepared by ultrasonic-microwave synergistic enhancement. The preparation process conditions were sulfuric acid concentration of 180g / L, liquid-solid ratio of 8:1, ultrasonic power of 200W, microwave power of 200W, leaching time of 30 minutes, and zinc oxide smoke leaching solution was obtained after vacuum filtration, and the pH of the leaching solution was -0.3. Then, iron powder was used for reduction, ultrasonic for 20 minutes, and trivalent iron was reduced to divalent iron. After vacuum filtration, the precipitation mother liquor was obtained, and the pH of the precipitation mother liquor was 0.4. After that, the precipitation mother liquor was loaded into a 500ml four-necked flask to start the precipitation experiment. The constant temperature water bath temperature was 90℃, mechanical stirring, stirring rate of 500rpm, and calcium carbonate powder was slowly added. When the precipitation termination pH reached 4.0, the agitator was immediately turned off, and the precipitation liquid was quickly vacuum filtered to obtain the precipitation supernatant. 20ml of the precipitation supernatant was taken for ICP analysis, and the precipitation rate of indium was 99.61%. The required time was 45 minutes, and the calcium carbonate consumption was 9.4g.

[0039] By comparison, it can be found that the ultrasonic enhanced precipitation in the embodiment of the present invention can significantly shorten the precipitation time and reduce the consumption of calcium carbonate. Under the same conditions, the precipitation time can be reduced by 22 minutes and 3.06g of calcium carbonate can be saved. Therefore, the ultrasonic enhanced precipitation has significant economic value, can reduce the production cost of enterprises, and has broad application prospects.

[0040] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation, It is characterized in that The following steps are involved: 1) mixing zinc oxide fume and acid solution and performing ultrasonic-microwave synergistic leaching, and obtaining zinc oxide fume leaching solution after filtering; 2) subjecting the zinc oxide smoke leaching solution obtained in step 1) to ultrasonic iron powder reduction to obtain a precipitation mother solution; 3) The precipitation mother solution obtained in step 2) is subjected to ultrasonic enhanced calcium carbonate precipitation, and the leaching solution is filtered after the ultrasonic precipitation reaction.

2. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 1, It is characterized in that In step 1), the ultrasonic power is 180-230W, and the microwave power is 150-220W.

3. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 2, It is characterized in that In step 1), the ultrasonic-microwave synergistic leaching time is 25 to 70 minutes.

4. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 3, It is characterized in that In step 1), the acid solution is sulfuric acid, the concentration of sulfuric acid is 150-200 g / L, and the liquid-to-solid ratio is (6-10):

1.

5. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 4, It is characterized in that In step 1), the pH of the zinc oxide fume leaching solution is 0 to -0.

5.

6. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to any one of claims 1 to 5, It is characterized in that In step 2), the reduction treatment includes adding iron powder for reduction and performing ultrasonic enhanced reduction.

7. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 6, It is characterized in that In step 2), the time of the ultrasonic enhanced reduction is 15 to 25 minutes.

8. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 7, It is characterized in that In step 2), the power of ultrasonic enhanced iron powder reduction is 200±50W.

9. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to any one of claims 1 to 8, It is characterized in that Step 3) further includes adding calcium carbonate powder, and stopping the ultrasonic treatment when the pH value of the solution reaches 3.5 to 4.

5.

10. The method for enriching indium from zinc oxide fume leaching solution by ultrasonically enhanced calcium carbonate precipitation according to claim 9, It is characterized in that Step 3) further comprises charging the precipitation mother solution of step 2) into a reaction container, placing the reaction container into an ultrasonic-microwave chemical reactor, monitoring the pH value and temperature of the leaching solution, performing ultrasonic treatment, and optionally opening the microwave reactor but not operating the microwave reactor to record the solution temperature; adding calcium carbonate powder, and when the solution pH reaches 4, turning off the ultrasonic generator and filtering the precipitated solution; and optionally, taking the supernatant and analyzing the ion concentration by ICP to calculate the precipitation rate of indium.

Citation Information

Patent Citations

  • Method for removing arsenic and antimony from zinc smelting leach liquor

    CN103911512A

  • Method for recovering indium from indium-contained materials in zinc smelting

    CN107828970A

  • Method for efficiently enriching indium from low-grade smelting slag containing indium

    CN108411128A

  • Method for enriching indium from low-indium zinc smelting material

    CN108486365A

  • Zinc hydrometallurgy starting method

    CN114438318A

Cited By

  • Method for preparing zinc oxide by directly utilizing zinc oxide smoke dust

    CN120793998A