Piezoelectric thin film, piezoelectric thin film element, and piezoelectric transducer
A lead-free piezoelectric thin film with a tetragonal crystal structure and specific c/a ratio addresses the challenge of high piezoelectricity in thin films, offering improved performance and environmental safety for piezoelectric devices.
Patent Information
- Application Number
- JP2020180666
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-28
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2040-10-28
AI Technical Summary
Existing piezoelectric thin films face challenges in achieving high piezoelectricity due to their thinness, and lead-based materials pose environmental and health hazards, necessitating the development of lead-free piezoelectric materials with improved piezoelectric figures of merit.
A piezoelectric thin film composed of a tetragonal crystal oxide with specific c/a ratio and orientation, containing elements like Bi, Fe, and optionally Na, K, Mg, Al, Zr, Ti, Ni, or Zn, which is epitaxially grown to enhance piezoelectricity and avoid lead.
The proposed thin film exhibits a large piezoelectric figure of merit, suitable for applications in piezoelectric transducers and sensors, with enhanced piezoelectric properties and environmental safety.
Smart Images

Figure 0007579109000007 
Figure 0007579109000008 
Figure 0007579109000009
Abstract
Description
[Technical field]
[0001] The present invention relates to a piezoelectric thin film, a piezoelectric thin film element, and a piezoelectric transducer. [Background technology]
[0002] Piezoelectric bodies are processed into various piezoelectric elements for various purposes. For example, a piezoelectric actuator converts voltage into force by applying a voltage to a piezoelectric body, deforming the piezoelectric body through the inverse piezoelectric effect. A piezoelectric sensor also converts force into voltage by applying pressure to a piezoelectric body, deforming the piezoelectric body through the piezoelectric effect. These piezoelectric elements are installed in various electronic devices.
[0003] In recent years, in response to market demands for miniaturization and improved performance of electronic devices, there has been active research into piezoelectric elements (piezoelectric thin film elements) that use piezoelectric thin films. However, the thinner the piezoelectric body is, the more difficult it is to obtain the piezoelectric effect and inverse piezoelectric effect, so there is a demand for the development of piezoelectric bodies that have excellent piezoelectric properties in a thin film state.
[0004] Conventionally, lead zirconate titanate (PZT), a perovskite-type ferroelectric, has been widely used as a piezoelectric material. However, since PZT contains lead (Pb), which is harmful to the human body and the environment, the development of lead-free piezoelectric materials as an alternative to PZT is expected. For example, Non-Patent Document 1 describes BiFeO3 as an example of a lead-free piezoelectric material. Among lead-free piezoelectric materials, BiFeO3 has relatively excellent piezoelectric properties, and is particularly expected to be applied to piezoelectric thin film elements. [Prior art documents] [Non-patent literature]
[0005] [Non-Patent Document 1] K.Ujimoto et al, Direct piezoelectric properties of (100) and (111) BiFeO3 epitaxial thin films, APPLIED PHYSICS LETTERS. 100, 102901 (2012) Summary of the Invention [Problem to be solved by the invention]
[0006] (-e 31,f ) 2 / ε0ε r is the piezoelectric performance index that indicates the piezoelectricity of the piezoelectric thin film. -e 31,f is a type of piezoelectric constant, -e 31,f The unit is C / m 2 ε0 is the dielectric constant of a vacuum, and the unit of ε0 is F / m. ε r is the relative dielectric constant of the piezoelectric thin film, and ε r There is no unit. (-e 31,f ) 2 / ε0ε r The unit of is Pa. A piezoelectric thin film having a large piezoelectric figure of merit is suitable for use in piezoelectric thin film elements such as piezoelectric transducers (sensors).
[0007] An object of the present invention is to provide a piezoelectric thin film having a large piezoelectric figure of merit, and a piezoelectric thin film element and a piezoelectric transducer including the piezoelectric thin film. [Means for solving the problem]
[0008] A piezoelectric thin film according to one aspect of the present invention is a piezoelectric thin film including an oxide having a perovskite structure, the piezoelectric thin film including a tetragonal crystal of an oxide, a (001) plane of the tetragonal crystal being oriented in a normal direction to a surface of the piezoelectric thin film, a spacing between the (001) planes of the tetragonal crystal being c, a spacing between the (100) planes of the tetragonal crystal being a, c / a being 1.050 or more and 1.250 or less, and the oxide being Fe 2+ Includes.
[0009] The oxide is Bi 3+and Fe 3+ It may further include.
[0010] The oxide may be represented by the following formula 1, where E in the following formula 1 A may be at least one element selected from the group consisting of Na, K and Ag, and E in the following chemical formula 1 B may be at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni, and Zn, x in the following chemical formula 1 may be 0.10 or more and 0.80 or less, y in the following chemical formula 1 may be 0.10 or more and 0.85 or less, z in the following chemical formula 1 may be 0.05 or more and 0.80 or less, x+y+z may be 1.00, and α in the following chemical formula 1 may be 0.00 or more and less than 1.00. x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0011] The thickness of the piezoelectric thin film may be 500 nm or more and 5000 nm or less.
[0012] The piezoelectric thin film may be an epitaxial film.
[0013] A piezoelectric thin film element according to one aspect of the present invention includes the above-described piezoelectric thin film.
[0014] The piezoelectric thin film element may include a single crystal substrate and a piezoelectric thin film overlying the single crystal substrate.
[0015] The piezoelectric thin film element may include a single crystal substrate, an electrode layer overlying the single crystal substrate, and a piezoelectric thin film overlying the electrode layer.
[0016] The piezoelectric thin film element may include an electrode layer and a piezoelectric thin film overlying the electrode layer.
[0017] The piezoelectric thin film element may further include a first intermediate layer, and the first intermediate layer may be disposed between the single crystal substrate and the electrode layer.
[0018] The first intermediate layer may include ZrO2 and Y2O3.
[0019] The piezoelectric thin film element may further include a second intermediate layer, and the second intermediate layer may be disposed between the electrode layer and the piezoelectric thin film.
[0020] The second intermediate layer may contain at least one of SrRuO3 and LaNiO3.
[0021] The electrode layer may include platinum crystals, the (002) plane of the platinum crystals may be oriented in a normal direction to the surface of the electrode layer, and the (200) plane of the platinum crystals may be oriented in an in-plane direction to the surface of the electrode layer.
[0022] A piezoelectric transducer according to one aspect of the present invention includes the above-described piezoelectric thin film element. Effect of the Invention
[0023] According to the present invention, there are provided a piezoelectric thin film having a large piezoelectric figure of merit, a piezoelectric thin film element including the piezoelectric thin film, and a piezoelectric transducer. [Brief description of the drawings]
[0024] [Figure 1] FIG. 1(a) is a schematic cross-sectional view of a piezoelectric thin film element according to one embodiment of the present invention, and FIG. 1(b) is an exploded perspective view of the piezoelectric thin film element shown in FIG. 1(a). [Diagram 2] FIG. 2 is a perspective view of a unit cell of an oxide (tetragonal crystal) having a perovskite structure, and shows the arrangement of each element in the perovskite structure. [Diagram 3] FIG. 3 is a perspective view of a unit cell of an oxide (tetragonal) having a perovskite structure, showing the crystal planes and crystal orientation of the tetragonal crystal. [Figure 4] FIG. 4 is a schematic cross-sectional view of a piezoelectric thin film element (ultrasonic transducer) according to another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] A preferred embodiment of the present invention will be described in detail below with reference to the drawings. However, the present invention is not limited to the following embodiment. In the drawings, the same or equivalent elements are given the same reference numerals. The X-axis, Y-axis, and Z-axis shown in Fig. 1(a), Fig. 1(b), and Fig. 4 are three coordinate axes that are perpendicular to each other. The directions of the three coordinate axes are common to Fig. 1(a), Fig. 1(b), and Fig. 4.
[0026] (Piezoelectric thin film and piezoelectric thin film element) The piezoelectric thin film element according to this embodiment includes a piezoelectric thin film. (a) in FIG. 1 shows a cross section of a piezoelectric thin film element 10 according to this embodiment. The cross section of the piezoelectric thin film element 10 is perpendicular to the surface of the piezoelectric thin film 3. The piezoelectric thin film element 10 may include a single crystal substrate 1, a first electrode layer 2 (lower electrode layer) overlapping the single crystal substrate 1, a piezoelectric thin film 3 overlapping the first electrode layer 2, and a second electrode layer 4 (upper electrode layer) overlapping the piezoelectric thin film 3. The piezoelectric thin film element 10 may further include a first intermediate layer 5. The first intermediate layer 5 may be disposed between the single crystal substrate 1 and the first electrode layer 2, and the first electrode layer 2 may directly overlap the surface of the first intermediate layer 5. The piezoelectric thin film element 10 may include a second intermediate layer 6. The second intermediate layer 6 may be disposed between the first electrode layer 2 and the piezoelectric thin film 3, and the piezoelectric thin film 3 may directly overlap the surface of the second intermediate layer 6. The thickness of each of the single crystal substrate 1, the first intermediate layer 5, the first electrode layer 2, the second intermediate layer 6, the piezoelectric thin film 3, and the second electrode layer 4 may be uniform. As shown in FIG. 1(b), the normal direction dn of the surface of the piezoelectric thin film 3 is perpendicular to the normal direction D N The first electrode layer, the first intermediate layer, the second intermediate layer, and the second electrode layer are omitted in (b) of Fig. 1.
[0027] The modified piezoelectric thin film element 10 may not include the single crystal substrate 1. For example, the single crystal substrate 1 may be removed after the first electrode layer 2 and the piezoelectric thin film 3 are formed. The modified piezoelectric thin film element 10 may not include the second electrode layer 4. For example, the piezoelectric thin film element without the second electrode layer may be supplied to an electronic device manufacturer as a product, and then the second electrode layer may be added to the piezoelectric thin film element during the manufacturing process of the electronic device. When the single crystal substrate 1 functions as an electrode, the modified piezoelectric thin film element 10 may not include the first electrode layer 2. That is, the modified piezoelectric thin film element 10 may include the single crystal substrate 1 and the piezoelectric thin film 3 overlapping the single crystal substrate 1. When the first electrode layer 2 is not present, the piezoelectric thin film 3 may directly overlap the single crystal substrate 1. When the first electrode layer 2 is not present, the piezoelectric thin film 3 may overlap the single crystal substrate 1 via at least one intermediate layer selected from the first intermediate layer 5 and the second intermediate layer 6.
[0028] The piezoelectric thin film 3 contains an oxide having a perovskite structure. That is, at least a part of the oxide contained in the piezoelectric thin film 3 is a crystal having a perovskite structure. All of the oxides contained in the piezoelectric thin film 3 may be crystals having a perovskite structure. In some cases, an oxide having a perovskite structure is referred to as a "perovskite oxide." The perovskite oxide is the main component of the piezoelectric thin film 3. The ratio of the perovskite oxide to the entire piezoelectric thin film 3 may be 99 mol% or more and 100 mol% or less. The piezoelectric thin film 3 may be composed of only the perovskite oxide.
[0029] Perovskite oxides contain at least divalent iron (Fe 2+ ) and oxygen (O). Perovskite oxides contain bismuth (Bi), divalent iron (Fe 2+ ), trivalent iron (Fe 3+ ) and oxygen (O). Perovskite oxides may contain bismuth (Bi), divalent iron (Fe 2+ ), trivalent iron (Fe 3+ ), titanium (Ti) and oxygen (O). The perovskite oxide may contain bismuth (Bi), divalent iron (Fe 2+ ), trivalent iron (Fe3+ ), titanium (Ti), element E B and oxygen (O), E B may be at least one element selected from the group consisting of magnesium (Mg), aluminum (Al), zirconium (Zr), titanium (Ti), nickel (Ni) and zinc (Zn). The perovskite oxide is B The perovskite oxide may contain multiple elements as bismuth (Bi), element E A , divalent iron (Fe 2+ ), trivalent iron (Fe 3+ ), titanium (Ti), element E B and oxygen (O), E A may be at least one element selected from the group consisting of sodium (Na), potassium (K) and silver (Ag). The perovskite oxide is A It may contain multiple elements.
[0030] FIG. 2 shows a unit cell uc of a perovskite oxide. At least a part of the elements located at the A site of the unit cell uc of the perovskite oxide may be Bi. The element located at the A site may be only Bi. The part of the elements located at the A site may be E A At least a part of the elements located at the B site of the unit cell uc of the perovskite oxide is Fe. At least a part of the Fe located at the B site is Fe 2+ Some of the Fe atoms at the B site are 3+ Some elements located at the B site may be E such as Ti. B may be also possible.
[0031] The piezoelectric thin film 3 includes a tetragonal crystal of a perovskite oxide. FIG. 3 shows a unit cell uc of the tetragonal crystal. The unit cell uc of the tetragonal crystal in FIG. 3 is the same as the unit cell uc in FIG. 2, but for convenience of illustration, E B and O has been omitted.
[0032] In FIG. 2 and FIG. 3, a, b, and c are fundamental vectors of a tetragonal crystal (perovskite oxide). a, b, and c are perpendicular to each other. The orientation of vector a (a-axis) is
[0100] . The orientation of vector b (b-axis) is
[0010] . The orientation of vector c (c-axis) is
[0001] . The length a of vector a is the spacing between the (100) planes of a tetragonal crystal. In other words, the length a of vector a is the lattice constant in the
[0100] direction of a tetragonal crystal. The length b of vector b is the spacing between the (010) planes of a tetragonal crystal. In other words, the length b of vector b is the lattice constant in the
[0010] direction of a tetragonal crystal. The length c of vector c is the spacing between the (001) planes of a tetragonal crystal. In other words, the length c of vector c is the lattice constant in the
[0001] direction of a tetragonal crystal. a is equal to b. c is greater than a.
[0033] 1(b) and 3, the (001) plane of the tetragonal crystal (uc) is oriented in the normal direction dn of the surface of the piezoelectric thin film 3. For example, the (001) plane of the tetragonal crystal may be approximately parallel to the surface of the piezoelectric thin film 3, and the
[0001] direction of the tetragonal crystal may be approximately parallel to the normal direction dn of the surface of the piezoelectric thin film 3. The normal direction dn of the surface of the piezoelectric thin film 3 is approximately parallel to the normal direction D N Therefore, the (001) plane of the tetragonal crystal is approximately parallel to the normal direction D N In other words, the (001) plane of the tetragonal crystal may be approximately parallel to the surface of the single crystal substrate 1, and the
[0001] direction of the tetragonal crystal may be oriented in the normal direction D of the surface of the single crystal substrate 1. N It may be approximately parallel to.
[0034] Perovskite oxides are easily polarized in the
[0001] direction. In other words,
[0001] is an orientation in which perovskite oxides are more easily polarized than other crystal orientations. Therefore, the (001) plane of the tetragonal crystal is oriented in the normal direction dn of the surface of the piezoelectric thin film 3, so that the piezoelectric thin film 3 can have excellent piezoelectric properties. For the same reason, the piezoelectric thin film 3 may be ferroelectric. The crystal orientation described below means that the (001) plane of the tetragonal crystal is oriented in the normal direction dn of the surface of the piezoelectric thin film 3.
[0035] Since the piezoelectric thin film 3 has the above-mentioned crystal orientation, the piezoelectric thin film 3 has a large (-e 31,f ) 2 / ε0ε r (piezoelectric performance index). The above crystal orientation is a characteristic inherent to the thin film. A thin film is a crystalline film formed by a vapor phase growth method or a solution method. On the other hand, it is difficult for a bulk of a piezoelectric body having the same composition as the piezoelectric thin film 3 to have the above crystal orientation. The bulk of a piezoelectric body is a sintered body (ceramic) of powder containing essential elements of the piezoelectric body, and it is difficult to control the structure and orientation of the many crystals that make up the sintered body. Due to the difficulty of the bulk of a piezoelectric body having the above crystal orientation, when the bulk of a piezoelectric body contains Fe, the resistivity of the bulk of the piezoelectric body is likely to be lower than that of the piezoelectric thin film 3. As a result, leakage current is likely to occur in the bulk of the piezoelectric body. Therefore, it is difficult to polarize the bulk of a piezoelectric body by applying a high electric field, and it is difficult for the bulk of a piezoelectric body to have a large piezoelectric performance index.
[0036] c / a is 1.050 or more and 1.250 or less. By having c / a 1.050 or more and 1.250 or less, the piezoelectric thin film 3 can have a large piezoelectric performance index. If c / a is less than 1.050, it is difficult for the piezoelectric thin film 3 to have a large piezoelectric performance index. If c / a is greater than 1.250, it is also difficult for the piezoelectric thin film 3 to have a large piezoelectric performance index. Since the piezoelectric thin film 3 is likely to have a large piezoelectric performance index, c / a may be 1.050 or more and 1.248 or less. a may be, for example, 3.762 Å or more and 3.950 Å or less. c may be, for example, 4.148 Å or more and 4.692 Å or less.
[0037] According to the inventor's consideration, Fe 2+ The reason why the piezoelectric thin film 3 containing Fe has a large piezoelectric performance index is as follows. 2+ The reason why the piezoelectric thin film 3 including the piezoelectric layer 3 has a large piezoelectric figure of merit is not limited to the following. When the piezoelectric thin film of BiFeO3-(Bi,K)TiO3 system has a composition near the morphotropic phase boundary (MPB) between tetragonal crystal and rhombohedral crystal, the piezoelectric properties derived from the tetragonal crystal (-e 31,f ) is improved, but the dielectric constant (ε0ε r) also increases, so that the piezoelectric figure of merit is difficult to improve. In order to suppress the increase in the dielectric constant, it is desirable to improve the piezoelectricity (ferroelectricity) of the piezoelectric thin film by constructing the piezoelectric thin film only from tetragonal crystals. The tetragonality of the piezoelectric thin film is realized by epitaxial stress (compressive stress due to lattice mismatch). This is because the epitaxial stress parallel to the surface of the piezoelectric thin film compresses the piezoelectric thin film in a direction parallel to the surface of the piezoelectric thin film (i.e., the a-axis direction and the b-axis direction), distorting the piezoelectric thin film. However, the thicker the piezoelectric thin film is, the more difficult it is to improve the tetragonality of the piezoelectric thin film only by epitaxial stress. This is because the thicker the piezoelectric thin film is, the more difficult it is to distort the entire piezoelectric thin film 3 by epitaxial stress. Therefore, even if the piezoelectric thin film is so thick that the epitaxial stress generated in the piezoelectric thin film is weakened, it is desirable to stabilize the tetragonal structure of the piezoelectric thin film. Therefore, in the piezoelectric thin film 3 according to this embodiment, the electron configuration of the element (ion) located at the B site of the perovskite oxide is Co which constitutes BiCoO3. 3+ The B site ion is Fe, so that the d6 electron configuration is similar to that of 2+ As a result, the tetragonality of the piezoelectric thin film 3 is improved even when the piezoelectric thin film 3 is so thick that the epitaxial stress generated in the piezoelectric thin film 3 is weakened. In other words, even when the piezoelectric thin film 3 is so thick that the epitaxial stress generated in the piezoelectric thin film 3 is weakened, the piezoelectric thin film 3 contains tetragonal crystals with c / a of 1.050 or more. Even in the case of compositions near the MPB where rhombohedral crystals are expected to form in the bulk of the piezoelectric material, some of the ions in the B site are Fe 2+ In the piezoelectric thin film 3 substituted with Fe, the rotation (rotation around the c-axis) of the BO6 octahedron (or BO5 pyramid) in the tetragonal crystal can occur, but the polarization rotation due to the formation of a pseudo cubic crystal is suppressed. In other words, when a part of the B site is replaced by Fe 2+ The piezoelectric thin film 3 substituted with is unlikely to have an MPB, and polarization rotation in which the direction of the c-axis of the tetragonal crystal changes is unlikely to occur. Due to the above mechanism, in the piezoelectric thin film 3 according to this embodiment, the piezoelectric characteristic (-e 31,f) and dielectric constant (ε0ε r ) and the piezoelectric figure of merit increases.
[0038] In contrast to the piezoelectric thin film 3, stress-induced distortion of the crystal structure is unlikely to occur in the bulk of the piezoelectric body. Therefore, most perovskite oxides constituting the bulk of the piezoelectric body are cubic crystals, and it is difficult for the bulk of the piezoelectric body to have piezoelectricity resulting from the tetragonal crystal structure of the perovskite oxide.
[0039] The thickness Tp of the piezoelectric thin film 3 may be 500 nm or more and 5000 nm or less. Even if the thickness Tp of the piezoelectric thin film 3 is 500 nm or more and the piezoelectric thin film 3 is thick, the ions located at the B site of the perovskite oxide may be Fe 2+ By being replaced with, the piezoelectric thin film 3 can have a large piezoelectric figure of merit. By adjusting the thickness Tp of the piezoelectric thin film 3 to 5000 nm or less, the entire piezoelectric thin film 3 is likely to contain tetragonal crystals regardless of epitaxial stress, and the piezoelectric thin film 3 is likely to have a large piezoelectric figure of merit. However, the thickness Tp of the piezoelectric thin film 3 is not limited to the above range. The method for measuring the thickness Tp of the piezoelectric thin film 3 is not limited. For example, the thickness Tp of the piezoelectric thin film 3 may be measured by a scanning electron microscope (SEM) in a cross section of the piezoelectric thin film 3 perpendicular to the surface of the piezoelectric thin film 3.
[0040] The degree of orientation of the (001) plane of the tetragonal crystal may be quantified by the degree of orientation. The greater the degree of orientation of the (001) plane of the tetragonal crystal, the greater the piezoelectric performance index of the piezoelectric thin film 3. The degree of orientation of the (001) plane of the tetragonal crystal may be calculated based on the peak of the diffracted X-rays originating from each crystal plane. The peak of the diffracted X-rays originating from each crystal plane may be measured by out-of-plane measurement on the surface of the piezoelectric thin film 3. The degree of orientation of the (001) plane of the tetragonal crystal in the normal direction dn to the surface of the piezoelectric thin film 3 is 100×I (001) / ΣI (hkl) It can be expressed as ΣI (hkl) is the sum of the peak intensities of the diffracted X-rays of each crystal plane of the tetragonal crystal measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. (hkl) For example, I(001) +I (110) +I (111) It may be. (001) is the peak intensity (maximum value) of the diffracted X-rays of the (001) plane of the tetragonal crystal measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. (110) is the peak intensity (maximum value) of the diffracted X-rays of the (110) plane of the tetragonal crystal measured in the out-of-plane direction on the surface of the piezoelectric thin film 3. (111) is the peak intensity (maximum value) of the diffracted X-rays of the (111) plane of the tetragonal crystal measured in the out-of-plane direction of the surface of the piezoelectric thin film 3. The degree of orientation of the (001) plane of the tetragonal crystal may be quantified by the orientation degree F based on the Lotgering method. Regardless of which of the above methods is used to calculate the orientation degree, the orientation degree of the (001) plane of the tetragonal crystal may be 70% or more and 100% or less, preferably 80% or more and 100% or less, and more preferably 90% or more and 100% or less. In other words, the (001) plane of the tetragonal crystal may be oriented in the normal direction dn of the surface of the piezoelectric thin film 3 in preference to other crystal planes of the tetragonal crystal.
[0041] The piezoelectric thin film 3 may be composed of only tetragonal crystals. As long as the piezoelectric thin film 3 has a large piezoelectric figure of merit, the piezoelectric thin film 3 may further contain, in addition to the tetragonal crystals, at least one type of perovskite oxide crystal selected from the group consisting of cubic crystals and rhombohedral crystals.
[0042] As described above, the perovskite oxide contained in the piezoelectric thin film 3 contains at least Fe 2+ and O(O 2- ). Perovskite oxides include Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), Fe 2+ , Fe 3+ and O(O 2- The perovskite oxide may contain Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), Fe 2+ , Fe 3+ , Ti(Ti4+ ) and O(O 2- The perovskite oxide may contain Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), E B , Fe 2+ , Fe 3+ , Ti(Ti 4+ ), and O(O 2- ). E B may be at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni and Zn. The perovskite oxide may be Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), E A , E B , Fe 2+ , Fe 3+ , Ti(Ti 4+ ) and O(O 2- ). E A may be at least one element selected from the group consisting of Na, K and Ag. When the perovskite oxide is composed of the above elements, the tetragonal crystals in the piezoelectric thin film 3 tend to have the above crystal orientation, and c / a tends to fall within the above range. The piezoelectric thin film 3 is preferably made of Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), E B , Fe 2+ , Fe 3+ , Ti(Ti 4+ ) and O(O 2- The piezoelectric thin film 3 may be made of only Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), E A , E B , Fe 2+ , Fe 3+ , Ti(Ti 4+ ) and O(O 2- As long as the piezoelectric thin film 3 has a large piezoelectric figure of merit, the piezoelectric thin film 3 may be made of only Bi (Bi 3+ , or Bi 3+ and Bi 5+ ), E A , EB , Fe 2+ , Fe 3+ , Ti(Ti 4+ ) and O(O 2- ) may further contain other elements. The piezoelectric thin film 3 does not have to contain Pb. The piezoelectric thin film 3 may contain Pb.
[0043] The perovskite oxide contained in the piezoelectric thin film 3 may be represented by the following Chemical Formula 1. The following Chemical Formula 1 is substantially the same as the following Chemical Formula 1a. x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1) (Bi x(1-α)+y+z E A xα )(E B x Fe y+0.5z Ti 0.5z )O 3±δ (1a)
[0044] In the above chemical formulas 1 and 1a, x+y+z may be 1.00.
[0045] E in the above chemical formula 1 and 1a A may be at least one element selected from the group consisting of Na, K and Ag. B may be at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni and Zn.
[0046] In the above formula 1, (Bi 1-α E A α )E B E that constitutes O3 A The sum of the valences (ionic valences) of is V A (Bi 1-α E A α )E B E that constitutes O3 B The sum of the valences (ionic valences) of is VB In chemical formula 1, (Bi 1-α E A α )E B Bi and E that compose O3 A and E B The sum of the valences is 3(1-α)+V A α+V B , or 5(1-α)+V A α+V B It is expressed as 3(1-α)+V A α+V B , or 5(1-α)+V A α+V B may be +6 to balance the sum of the valences (ionic valences) of O (-6). 3(1-α)+V A α or 5(1-α)+V A α may be +3. B The perovskite oxide may have an E B Two elements (E B1 and E B2 In the case where the above formula 1 includes the group E, the above formula 1 is substantially the same as the following formula 1'. In the following formula 1', β may be greater than 0.00 and less than 1.00. B1 The valence (ionic valence) of is V B1 It is expressed as E B2 The valence (ionic valence) of is V B2 It is expressed as E B The sum of the valences (ionic valences) of V B is (1-β)V B1 +βV B2 It is expressed as (1-β)V B1 +βV B2 may be +3. x(Bi 1-α E A α )(E B1 1-β E B2 β )O3‐yBiFeO3‐zBi(Fe 0.5 Ti 0.5 )O3(1')
[0047] Bi in the above formula 1a x(1-α)+y+z E Axα is an element located at the A site of the perovskite structure. B x Fe y+0.5z Ti 0.5z is an element located at the B site of the perovskite structure.
[0048] The valence of Fe constituting yBiFeO3 in the above chemical formulas 1 and 1' is 3, but the valence of Fe in zBi(Fe 0.5 Ti 0.5 The valence of Fe constituting )O3 is 2. Therefore, the Bi, E A , E B The molar ratios of Bi, E, Fe and Ti are the same as those in the above chemical formula 1, 1' or 1a. A , E B The composition of the raw material of the piezoelectric thin film 3 is adjusted so that the molar ratio of Fe, Ti and Ti is equal to that of Fe. 2+ may include.
[0049] In the above chemical formulas 1, 1' and 1a, x may be 0.10 or more and 0.80 or less. When x is 0.10 or more and 0.80 or less, the tetragonal crystals in the piezoelectric thin film 3 tend to have the above crystal orientation, and c / a tends to fall within the above range.
[0050] In the above chemical formulas 1, 1' and 1a, y may be 0.10 or more and 0.85 or less. When y is 0.10 or more and 0.85 or less, the tetragonal crystals in the piezoelectric thin film 3 tend to have the above crystal orientation, and c / a tends to fall within the above range.
[0051] In the above chemical formulas 1, 1', and 1a, z may be 0.05 or more and 0.80 or less. When z is 0.05 or more and 0.80 or less, the tetragonal crystals in the piezoelectric thin film 3 tend to have the above crystal orientation, and c / a tends to fall within the above range.
[0052] In the above chemical formulas 1, 1', and 1a, α may be 0.00 or more and less than 1.00. Since the tetragonal crystals in the piezoelectric thin film 3 tend to have the above crystal orientation and c / a tends to fall within the above range, α may be 0.50. As described above, β in the above chemical formula 1' may be greater than 0.00 and less than 1.00. Since the tetragonal crystals in the piezoelectric thin film 3 tend to have the above crystal orientation and c / a tends to fall within the above range, β may be 0.50.
[0053] In the above chemical formula 1a, δ may be 0 or more. As long as the crystal structure of the perovskite oxide (perovskite structure) is maintained, δ may be a value other than 0. For example, δ may be greater than 0 and less than or equal to 1.0. δ may be calculated, for example, from the valence of each ion located at the A site and the B site in the perovskite structure. The valence of each ion may be measured by X-ray photoelectron spectroscopy (XPS).
[0054] Bi and E in perovskite oxides A The total number of moles of Fe contained in the perovskite oxide may be expressed as [A]. 2+ , Fe 3+ , Ti and E B The total number of moles may be represented as [B], and [A] / [B] may be 1.0. As long as the crystal structure of the perovskite oxide (perovskite structure) is maintained, [A] / [B] may be a value other than 1.0. In other words, [A] / [B] may be less than 1.0, and [A] / [B] may be greater than 1.0.
[0055] The area of the piezoelectric thin film 3 is, for example, 1 μm 2 More than 500mm 2 The area of each of the single crystal substrate 1, the first intermediate layer 5, the first electrode layer 2, the second intermediate layer 6, and the second electrode layer 4 may be the same as the area of the piezoelectric thin film 3.
[0056] The composition of the piezoelectric thin film may be analyzed by, for example, X-ray fluorescence analysis (XRF), inductively coupled plasma (ICP) emission spectroscopy, and photoelectron spectroscopy (XPS). The crystal structure and crystal orientation of the piezoelectric thin film may be identified by X-ray diffraction (XRD). The above-mentioned crystal structure and crystal orientation of the piezoelectric thin film may be the crystal structure and crystal orientation of the piezoelectric thin film at room temperature.
[0057] The piezoelectric thin film 3 may be formed, for example, by the following method.
[0058] A target containing all elements common to the piezoelectric thin film 3 may be used as the raw material of the piezoelectric thin film 3. The target is prepared as follows.
[0059] Starting materials include, for example, Bi, E A , E B The oxides of Bi, E, and Ti may be used. As the starting materials, instead of oxides, substances that become oxides upon firing, such as carbonates or oxalates, may be used. After these starting materials are sufficiently dried at 100° C. or higher, Bi, E, and Ti are added to the mixture. A , E B Each starting material is weighed out so that the molar ratio of each of the elements, Fe and Ti, coincides with the molar ratio of each element in the above chemical formula 1, 1' or 1a. In the vapor phase epitaxy described below, Bi in the target is more likely to volatilize than other elements. Therefore, the molar ratio of Bi in the target may be adjusted to a value higher than the molar ratio of Bi in the piezoelectric thin film 3. A When a raw material containing K is used as the target, K in the target is more likely to volatilize than other elements. Therefore, the molar ratio of K in the target may be adjusted to a value higher than the molar ratio of K in the piezoelectric thin film 3.
[0060] The weighed starting materials are thoroughly mixed in an organic solvent or water. The mixing time may be 5 hours or more and 20 hours or less. The mixing means may be, for example, a ball mill. After the mixed starting materials are thoroughly dried, the starting materials are molded in a press. The molded starting materials are calcinated to obtain a calcine. The calcine temperature may be 750°C or more and 900°C or less. The calcine time may be 1 hour or more and 3 hours or less. The calcine is pulverized in an organic solvent or water. The pulverization time may be 5 hours or more and 30 hours or less. The pulverization means may be a ball mill. After drying the pulverized calcine, the calcine to which a binder solution has been added is granulated to obtain a calcine powder. The calcine powder is press molded to obtain a block-shaped molded body.
[0061] The block-shaped compact is heated to volatilize the binder in the compact. The heating temperature may be 400° C. or higher and 800° C. or lower. The heating time may be 2 hours or higher and 4 hours or lower.
[0062] After the binder is evaporated, the molded body is sintered. The sintering temperature may be 800° C. or more and 1100° C. or less. The sintering time may be 2 hours or more and 4 hours or less. The temperature increase rate and the temperature decrease rate of the molded body during the sintering process may be, for example, 50° C. / hour or more and 300° C. / hour or less.
[0063] The target is obtained by the above steps. The average grain size of the crystal grains of the oxide (perovskite oxide) contained in the target may be, for example, 1 μm or more and 20 μm or less. The target is Fe 3+ However, the target does not necessarily contain Fe 2+ In the process of forming the piezoelectric thin film 3 by the vapor phase growth method described later, Fe derived from the target may be included. 3+ By reducing a part of Fe 2+ A piezoelectric thin film 3 including the above structure can be obtained.
[0064] The piezoelectric thin film 3 may be formed by a vapor phase growth method using the above target. In the vapor phase growth method, elements constituting the target are evaporated in a vacuum atmosphere. The evaporated elements are attached and deposited on the surface of any one of the second intermediate layer 6, the first electrode layer 2, or the single crystal substrate 1, thereby growing the piezoelectric thin film 3. The vapor phase growth method may be, for example, a sputtering method, an electron beam evaporation method, a chemical vapor deposition method, or a pulsed-laser deposition method. In the following, the pulsed-laser deposition method is referred to as a PLD method. The excitation source differs depending on the type of vapor phase growth method. The excitation source of the sputtering method is Ar plasma. The excitation source of the electron beam evaporation method is an electron beam. The excitation source of the PLD method is a laser beam (for example, an excimer laser). When these excitation sources are irradiated onto the target, the elements constituting the target are evaporated. By using the above vapor phase growth method, the piezoelectric thin film 3 is easily grown epitaxially. By using the above-mentioned vapor phase growth method, it is possible to form a piezoelectric thin film 3 that is dense at the atomic level, and segregation of elements in the piezoelectric thin film 3 is suppressed.
[0065] Among the above vapor phase growth methods, the PLD method is relatively superior in the following respects. In the PLD method, the elements constituting the target can be instantaneously and uniformly converted into plasma by a pulsed laser. Therefore, it is easy to form a piezoelectric thin film 3 in which the molar ratio of each element is approximately the same as the molar ratio of each element in the target. Furthermore, in the PLD method, the thickness of the piezoelectric thin film 3 can be easily controlled by changing the number of laser pulses (repetition frequency).
[0066] The piezoelectric thin film 3 may be an epitaxial film. That is, the piezoelectric thin film 3 may be formed by epitaxial growth. By epitaxial growth, the c / a of the tetragonal crystal is likely to fall within the above range, and a piezoelectric thin film 3 having excellent anisotropy and crystal orientation is likely to be formed. When the piezoelectric thin film 3 is formed by the PLD method, the piezoelectric thin film 3 is likely to be formed by epitaxial growth.
[0067] In the PLD method, the piezoelectric thin film 3 may be formed while heating the single crystal substrate 1 and the first electrode layer 2 in a vacuum chamber. The temperature (film formation temperature) of the single crystal substrate 1 and the first electrode layer 2 may be, for example, 450° C. or higher and 600° C. or lower. By setting the film formation temperature to 450° C. or higher, the Fe 3+ Part of the Fe is easily reduced. 2+ When the film formation temperature is less than 450° C., the piezoelectric thin film 3 containing Fe derived from the target is easily formed. 3+ is difficult to reduce, and Fe 2+ It is difficult to obtain a piezoelectric thin film 3 containing the above. The higher the film formation temperature, the more improved the cleanliness of the surface of the single crystal substrate 1 or the first electrode layer 2, the higher the crystallinity of the piezoelectric thin film 3, and the more likely it is that the degree of orientation of the tetragonal crystal planes will increase. If the film formation temperature is too high, the elements constituting the piezoelectric thin film 3 will be excessively reduced, making it difficult to obtain a piezoelectric thin film 3 having a desired composition. Furthermore, if the film formation temperature is too high, Bi or K will be easily desorbed from the piezoelectric thin film 3, making it difficult to control the composition of the piezoelectric thin film 3.
[0068] In the PLD method, the oxygen partial pressure in the vacuum chamber may be, for example, 0.1 Pa or more and 3.0 Pa or less, preferably 0.1 Pa or more and 1.0 Pa or less, and more preferably 0.1 Pa or more and 0.5 Pa or less. By maintaining the oxygen partial pressure within the above range, Fe derived from the target can be easily obtained. 3+ Part of the Fe is easily reduced. 2+ If the oxygen partial pressure is too low, the elements derived from the target are not sufficiently oxidized, making it difficult to form a perovskite-type oxide, and the orientation of the crystal plane of the piezoelectric thin film 3 is likely to decrease. If the oxygen partial pressure is too high, the Fe 3+ is difficult to reduce, and Fe 2+ In addition, if the oxygen partial pressure is too high, the growth rate of the piezoelectric thin film 3 tends to decrease, and the degree of orientation of the crystal plane of the piezoelectric thin film 3 tends to decrease.
[0069] Other parameters controlled by the PLD method include, for example, the laser oscillation frequency and the distance between the substrate and the target. By controlling these parameters, the crystal structure, crystal orientation, and thickness Tp of the piezoelectric thin film 3 can be easily controlled. For example, when the laser oscillation frequency is 10 Hz or less, the degree of orientation of the crystal plane of the piezoelectric thin film 3 is easily increased.
[0070] After the piezoelectric thin film 3 is grown, the piezoelectric thin film 3 may be annealed (heated). The temperature (annealing temperature) of the piezoelectric thin film 3 in the annealing may be, for example, 300°C to 1000°C, 600°C to 1000°C, or 850°C to 1000°C. Annealing the piezoelectric thin film 3 tends to further improve the piezoelectricity of the piezoelectric thin film 3. In particular, annealing at 850°C to 1000°C tends to improve the piezoelectricity of the piezoelectric thin film 3. However, annealing is not essential. The annealing may be performed in a reducing atmosphere such as nitrogen gas (N2). Annealing in a reducing atmosphere reduces the Fe in the piezoelectric thin film 3 due to the annealing. 2+ Oxidation of (Fe 3+ The formation of Fe in the piezoelectric thin film 3 is suppressed. 2+ is easily maintained.
[0071] In the above-mentioned growth process of the piezoelectric thin film 3 and the subsequent temperature drop process, compressive stress is generated in the piezoelectric thin film 3. The compressive stress compresses the piezoelectric thin film 3 in directions (a-axis direction and b-axis direction) substantially parallel to the surface of the piezoelectric thin film 3. As a result, a tetragonal crystal of a perovskite oxide is formed. The compressive stress is caused by, for example, lattice mismatch between the single crystal substrate 1 and the piezoelectric thin film 3, or a difference in thermal expansion coefficient between the single crystal substrate 1 and the piezoelectric thin film 3.
[0072] The single crystal substrate 1 may be, for example, a substrate made of a single crystal of Si, or a substrate made of a single crystal of a compound semiconductor such as GaAs. The single crystal substrate 1 may be a substrate made of a single crystal of an oxide. The single crystal of the oxide may be, for example, MgO or a perovskite-type oxide (for example, SrTiO3). The thickness of the single crystal substrate 1 may be, for example, 10 μm or more and 1000 μm or less. When the single crystal substrate 1 has conductivity, the single crystal substrate 1 functions as an electrode, so that the first electrode layer 2 may not be required. In other words, the conductive single crystal substrate 1 may be, for example, a single crystal of SrTiO3 doped with niobium (Nb).
[0073] The crystal orientation of the single crystal substrate 1 is the normal direction D of the surface of the single crystal substrate 1. N That is, the surface of the single crystal substrate 1 may be parallel to the crystal plane of the single crystal substrate 1. The single crystal substrate 1 may be a uniaxially oriented substrate. For example, the (100) plane of the single crystal substrate 1 (e.g., Si) may be parallel to the surface of the single crystal substrate 1. That is, the
[0100] direction of the single crystal substrate 1 (e.g., Si) may be equal to the normal direction D of the surface of the single crystal substrate 1. N may be parallel to
[0074] When the (100) plane of the single crystal substrate 1 (eg, Si) is parallel to the surface of the single crystal substrate 1, the (001) plane of the perovskite oxide (tetragonal crystal) in the piezoelectric thin film 3 tends to be oriented in the normal direction dn to the surface of the piezoelectric thin film 3.
[0075] As described above, the first intermediate layer 5 may be disposed between the single crystal substrate 1 and the first electrode layer 2. The first intermediate layer 5 may contain, for example, at least one selected from the group consisting of titanium (Ti), chromium (Cr), titanium oxide (TiO2), silicon oxide (SiO2), and zirconium oxide (ZrO2). The first intermediate layer 5 facilitates adhesion of the first electrode layer 2 to the single crystal substrate 1. The first intermediate layer 5 may be crystalline. The crystal plane of the first intermediate layer 5 may be aligned in the normal direction D of the surface of the single crystal substrate 1. N Both the crystal plane of the single crystal substrate 1 and the crystal plane of the first intermediate layer 5 may be oriented in the normal direction D NThe method for forming the first intermediate layer 5 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method.
[0076] The first intermediate layer 5 may contain ZrO2 and an oxide of a rare earth element. When the first intermediate layer 5 contains ZrO2 and an oxide of a rare earth element, the first electrode layer 2 made of platinum crystals is easily formed on the surface of the first intermediate layer 5, the (002) plane of the platinum crystals is easily oriented in the normal direction to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals is easily oriented in the in-plane direction of the surface of the first electrode layer 2. The rare earth element may be at least one selected from the group consisting of scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), promethium (Pm), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb), and lutetium (Lu).
[0077] The first intermediate layer 5 may contain ZrO2 and Y2O3. For example, the first intermediate layer 5 may be made of yttria-stabilized zirconia (ZrO2 with added Y2O3). The first intermediate layer 5 may have a first layer made of ZrO2 and a second layer made of Y2O3. The first layer made of ZrO2 may be directly laminated on the surface of the single crystal substrate 1. The second layer made of Y2O3 may be directly laminated on the surface of the first layer. The first electrode layer 2 may be directly laminated on the surface of the second layer made of Y2O3. When the first intermediate layer 5 contains ZrO2 and Y2O3, the piezoelectric thin film 3 is likely to grow epitaxially, and the tetragonal (001) plane in the piezoelectric thin film 3 is likely to be preferentially oriented in the normal direction dn of the surface of the piezoelectric thin film 3. Furthermore, when the first intermediate layer 5 contains ZrO2 and Y2O3, a first electrode layer 2 made of platinum crystals is likely to be formed on the surface of the first intermediate layer 5, the (002) plane of the platinum crystals is likely to be oriented in the normal direction to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals is likely to be oriented in the in-plane direction of the surface of the first electrode layer 2.
[0078] The first electrode layer 2 may be made of at least one metal selected from the group consisting of platinum (Pt), palladium (Pd), rhodium (Rh), gold (Au), ruthenium (Ru), iridium (Ir), molybdenum (Mo), titanium (Ti), tantalum (Ta), and nickel (Ni). The first electrode layer 2 may be made of a conductive metal oxide such as strontium ruthenate (SrRuO3), lanthanum nickelate (LaNiO3), or lanthanum strontium cobaltate ((La,Sr)CoO3). The first electrode layer 2 may be crystalline. The crystal plane of the first electrode layer 2 is aligned in the normal direction D of the single crystal substrate 1. N The crystal plane of the first electrode layer 2 may be substantially parallel to the surface of the single crystal substrate 1. Both the crystal plane of the single crystal substrate 1 and the crystal plane of the first electrode layer 2 may be oriented in the normal direction D N The single crystal substrate 1 may be oriented in the normal direction D N The crystal plane of the first electrode layer 2 oriented in the plane may be approximately parallel to the (001) plane of the tetragonal crystal in the piezoelectric thin film 3. The thickness of the first electrode layer 2 may be, for example, 1 nm or more and 1.0 μm or less. The method for forming the first electrode layer 2 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method. In the case of the printing method, the spin coating method, or the sol-gel method, the first electrode layer 2 may be subjected to a heat treatment (annealing) in order to enhance the crystallinity of the first electrode layer 2.
[0079] The first electrode layer 2 may include platinum crystals. The first electrode layer 2 may consist only of platinum crystals. The platinum crystals are cubic crystals having a face-centered cubic lattice structure (fcc structure). The (002) plane of the platinum crystals may be oriented in the normal direction to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals may be oriented in the in-plane direction of the surface of the first electrode layer 2. In other words, the (002) plane of the platinum crystals may be approximately parallel to the surface of the first electrode layer 2, and the (200) plane of the platinum crystals may be approximately perpendicular to the surface of the first electrode layer 2. When the (002) and (200) planes of the platinum crystals constituting the first electrode layer 2 have the above-mentioned orientation, the piezoelectric thin film 3 is likely to grow epitaxially on the surface of the first electrode layer 2, and the (001) plane of the tetragonal crystals in the piezoelectric thin film 3 is likely to be preferentially oriented in the normal direction dn to the surface of the piezoelectric thin film 3. The surface of the first electrode layer 2 may be approximately parallel to the surface of the piezoelectric thin film 3. In other words, the normal direction to the surface of the first electrode layer 2 may be approximately parallel to the normal direction dn to the surface of the piezoelectric thin film 3.
[0080] As described above, the second intermediate layer 6 may be disposed between the first electrode layer 2 and the piezoelectric thin film 3. The second intermediate layer 6 may contain, for example, at least one selected from the group consisting of SrRuO3, LaNiO3, and (La,Sr)CoO3. (La,Sr)CoO3 may be, for example, La 0.5 Sr 0.5 CoO3. The second intermediate layer 6 may be crystalline. For example, the second intermediate layer 6 may be a laminate composed of at least two types of buffer layers selected from the group consisting of a layer containing SrRuO3 crystals, a layer containing LaNiO3 crystals, and a layer containing (La,Sr)CoO3 crystals. All of SrRuO3, LaNiO3, and (La,Sr)CoO3 have a perovskite structure. Therefore, when the second intermediate layer 6 contains at least one selected from the group consisting of SrRuO3, LaNiO3, and (La,Sr)CoO3, the piezoelectric thin film 3 is likely to grow epitaxially, and the (001) plane of the tetragonal crystal in the piezoelectric thin film 3 is likely to be preferentially oriented in the normal direction dn of the surface of the piezoelectric thin film 3. In addition, by interposing the second intermediate layer 6, the piezoelectric thin film 3 is likely to adhere to the first electrode layer 2. The crystal plane of the second intermediate layer 6 is likely to be oriented in the normal direction D of the surface of the single crystal substrate 1.N Both the crystal plane of the single crystal substrate 1 and the crystal plane of the second intermediate layer 6 may be oriented in the normal direction D N The second intermediate layer 6 may be formed by a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method.
[0081] The second electrode layer 4 may be made of at least one metal selected from the group consisting of Pt, Pd, Rh, Au, Ru, Ir, Mo, Ti, Ta, and Ni. The second electrode layer 4 may be made of at least one conductive metal oxide selected from the group consisting of LaNiO3, SrRuO3, and (La,Sr)CoO3. The second electrode layer 4 may be crystalline. The crystal plane of the second electrode layer 4 is aligned in the normal direction D of the single crystal substrate 1. N The crystal plane of the second electrode layer 4 may be approximately parallel to the surface of the single crystal substrate 1. N The crystal plane of the second electrode layer 4 oriented in the plane may be approximately parallel to the (001) plane of the tetragonal crystal in the piezoelectric thin film 3. The thickness of the second electrode layer 4 may be, for example, 1 nm or more and 1.0 μm or less. The method for forming the second electrode layer 4 may be a sputtering method, a vacuum deposition method, a printing method, a spin coating method, or a sol-gel method. In the case of the printing method, the spin coating method, or the sol-gel method, the second electrode layer 4 may be subjected to a heat treatment (annealing) in order to enhance the crystallinity of the second electrode layer 4.
[0082] A third intermediate layer may be disposed between the piezoelectric thin film 3 and the second electrode layer 4. The third intermediate layer facilitates adhesion of the second electrode layer 4 to the piezoelectric thin film 3. The composition, crystal structure, and formation method of the third intermediate layer may be the same as those of the second intermediate layer.
[0083] At least a part or the entire surface of the piezoelectric thin film element 10 may be covered with a protective film. Covering with a protective film improves, for example, the moisture resistance of the piezoelectric thin film element 10.
[0084] The piezoelectric thin film element according to this embodiment has a variety of applications. For example, the piezoelectric thin film element may be used in a piezoelectric transducer. That is, the piezoelectric transducer according to this embodiment may include the above-described piezoelectric thin film or piezoelectric thin film element. The piezoelectric transducer may be, for example, an ultrasonic transducer such as an ultrasonic sensor. The piezoelectric thin film element may be, for example, a harvester (vibration power generation element). The piezoelectric thin film element according to this embodiment has a large (-e 31f ) 2 / ε0ε r Since the piezoelectric thin film has a piezoelectric thin film having a piezoelectric ... Specific examples of products that use piezoelectric micromechanical ultrasonic transducers include biometric sensors or medical / healthcare sensors (fingerprint sensors, ultrasonic blood vessel authentication sensors, etc.), as well as ToF (Time of Flight) sensors.
[0085] FIG. 4 shows a schematic cross section of an ultrasonic transducer 10a including the above-mentioned piezoelectric thin film 3. The cross section of the ultrasonic transducer 10a is perpendicular to the surface of the piezoelectric thin film 3. The ultrasonic transducer 10a may include substrates 1a and 1b, a first electrode layer 2 disposed on the substrates 1a and 1b, a piezoelectric thin film 3 overlapping the first electrode layer 2, and a second electrode layer 4 overlapping the piezoelectric thin film 3. An acoustic cavity 1c may be provided below the piezoelectric thin film 3. An ultrasonic signal is transmitted or received by the deflection or vibration of the piezoelectric thin film 3. A first intermediate layer may be interposed between the substrates 1a and 1b and the first electrode layer 2. A second intermediate layer may be interposed between the first electrode layer 2 and the piezoelectric thin film 3. EXAMPLES
[0086] The present invention will be described in detail with reference to the following examples and comparative examples, but the present invention is not limited to the following examples.
[0087] Example 1 A single crystal substrate made of Si was used to fabricate the piezoelectric thin film element of Example 1. The (100) plane of Si was parallel to the surface of the single crystal substrate. The single crystal substrate was a square of 20 mm x 20 mm. The thickness of the single crystal substrate was 500 μm.
[0088] In a vacuum chamber, a crystalline first intermediate layer made of ZrO2 and Y2O3 was formed on the entire surface of the single crystal substrate. The first intermediate layer was formed by a sputtering method. The thickness of the first intermediate layer was 30 nm.
[0089] In the vacuum chamber, a first electrode layer made of Pt crystals was formed on the entire surface of the first intermediate layer. The first electrode layer was formed by a sputtering method. The thickness of the first electrode layer was 200 nm. The temperature of the single crystal substrate during the formation of the first electrode layer was maintained at 500°C.
[0090] The XRD pattern of the first electrode layer was measured by out-of-plane measurement on the surface of the first electrode layer. The XRD pattern of the first electrode layer was measured by in-plane measurement on the surface of the first electrode layer. An X-ray diffractometer (SmartLab) manufactured by Rigaku Corporation was used to measure these XRD patterns. The measurement conditions were set so that each peak intensity in the XRD pattern was at least three orders of magnitude higher than the background intensity. The out-of-plane measurement detected a diffracted X-ray peak of the (002) plane of the Pt crystal. In other words, the (002) plane of the Pt crystal was oriented in the normal direction of the surface of the first electrode layer. The in-plane measurement detected a diffracted X-ray peak of the (200) plane of the Pt crystal. In other words, the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.
[0091] In the vacuum chamber, a piezoelectric thin film was formed on the entire surface of the first electrode layer. The piezoelectric thin film was formed by the PLD method. The thickness Tp of the piezoelectric thin film was 3000 nm. The temperature of the single crystal substrate (film formation temperature) during the process of forming the piezoelectric thin film was maintained at 500°C. The oxygen partial pressure in the vacuum chamber during the process of forming the piezoelectric thin film was maintained at 1 Pa. A target (sintered body of raw material powder) was used as the raw material for the piezoelectric thin film. Bismuth oxide, potassium carbonate, titanium oxide, and iron oxide were used as the raw material powder for the target. The Bi, E in the entire raw material powder was 100 nm. A , E B The molar ratios of Bi, E, Fe and Ti in the desired piezoelectric thin film are A , E B The starting materials were weighed and mixed so that the molar ratios of E, Fe, and Ti were consistent with each other. The composition of the target piezoelectric thin film was represented by the following chemical formula 1A. That is, in the case of Example 1, E in the following chemical formula 1 A is K, and E in the following chemical formula 1 B is Ti, and α in the following Chemical Formula 1 was 0.5. In the case of Example 1, x, y, and z in the following Chemical Formulas 1 and 1A had the values shown in Table 1 below. x(Bi 0.5 K 0.5)TiO3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1A) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0092] The composition of the piezoelectric thin film was analyzed by XRF using a PW2404 analyzer manufactured by Philips Japan Ltd. As a result of the analysis, the composition of the piezoelectric thin film of Example 1 was approximately the same as that of Chemical Formula 1A above.
[0093] The XRD pattern of the piezoelectric thin film was measured by out-of-plane measurement of the surface of the piezoelectric thin film using the above-mentioned X-ray diffractometer. Furthermore, the XRD pattern of the piezoelectric thin film was measured by in-plane measurement of the surface of the piezoelectric thin film. The measurement conditions were set so that each peak intensity in the XRD pattern was at least three orders of magnitude higher than the background intensity. The measurement device and measurement conditions for the XRD pattern were the same as those described above.
[0094] The analysis results of the piezoelectric thin film based on the above-mentioned XRD method showed that the piezoelectric thin film had the following characteristics.
[0095] The piezoelectric thin film was made of tetragonal crystals of perovskite-type oxide. The (001) plane of the tetragonal crystal was preferentially oriented in the normal direction to the surface of the piezoelectric thin film. In other words, the degree of orientation of the (001) plane of the tetragonal crystal in the normal direction to the surface of the piezoelectric thin film was 90% or more. As mentioned above, the degree of orientation of the (001) plane of the tetragonal crystal was 100×I (001) / ( I (001) + I (110) + I (111) ) The c / a ratio of the tetragonal crystal was the value shown in Table 1 below.
[0096] In the above manner, a laminate was produced that included a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, and a piezoelectric thin film overlapping the first electrode layer. The following steps were then carried out using this laminate.
[0097] In a vacuum chamber, a second electrode layer made of Pt was formed on the entire surface of the piezoelectric thin film. The second electrode layer was formed by a sputtering method. The temperature of the single crystal substrate during the process of forming the second electrode layer was maintained at 500°C. The thickness of the second electrode layer was 200 nm.
[0098] Through the above steps, a laminate was produced that included a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a piezoelectric thin film overlapping the first electrode layer, and a second electrode layer overlapping the piezoelectric thin film. The laminate structure on the single crystal substrate was then patterned by photolithography. After patterning, the laminate was cut by dicing.
[0099] Through the above steps, a rectangular piezoelectric thin film element of Example 1 was obtained. The piezoelectric thin film element included a single crystal substrate, a first intermediate layer overlapping the single crystal substrate, a first electrode layer overlapping the first intermediate layer, a piezoelectric thin film overlapping the first electrode layer, and a second electrode layer overlapping the piezoelectric thin film. The area of the movable part of the piezoelectric thin film was 20 mm x 1.0 mm.
[0100] <Evaluation of piezoelectricity> The piezoelectric properties of the piezoelectric thin film were evaluated by the following method.
[0101] [Measurement of residual polarization] The polarization hysteresis of the piezoelectric thin film was measured. For the measurement, an apparatus combining an atomic microscope (AFM) and a ferroelectric evaluation system was used. The atomic microscope was an SPA-400 manufactured by Seiko Instruments Inc. The ferroelectric evaluation system was an FCE manufactured by Toyo Corporation. The frequency of the AC voltage used in the hysteresis measurement was 5 Hz. The maximum voltage applied to the piezoelectric thin film during the measurement was 20 V. The remnant polarization Pr of the piezoelectric thin film is shown in Table 1 below. The unit of the remnant polarization Pr is μC / cm. 2 It is.
[0102] [Calculation of relative dielectric constant] The capacitance C of the piezoelectric thin film element was measured. The details of the measurement of the capacitance C were as follows. Measurement equipment: Impedance Gain-Phase Analyzer 4194A manufactured by Hewlett Packard Co. Frequency: 10kHz Electric field: 0.1V / μm
[0103] Based on the following formula A, the relative dielectric constant ε r was calculated. r is shown in Table 1 below. C = ε0 × ε r ×(S / d) (A) ε0 in formula A is the dielectric constant of a vacuum (8.854×10 -12 Fm -1 ) In formula A, S is the surface area of the piezoelectric thin film. In other words, S is the area of the first electrode layer that overlaps the piezoelectric thin film. In formula A, d is the thickness of the piezoelectric thin film.
[0104] [Piezoelectric constant - e 31,f Measurement of Piezoelectric constant of piezoelectric thin film -e 31,fIn order to measure, a rectangular sample (cantilever) was prepared as the piezoelectric thin film element. The dimensions of the sample were 3 mm wide x 15 mm long. Except for the dimensions, the sample was the same as the piezoelectric thin film element in Example 1 above. A homemade evaluation system was used for the measurement. One end of the sample was fixed, and the other end of the sample was a free end. While applying a voltage to the piezoelectric thin film in the sample, the displacement of the free end of the sample was measured with a laser. Then, the piezoelectric constant -e was calculated from the following formula B. 31,f was calculated. Note that E in formula B s is the Young's modulus of the single crystal substrate. h s is the thickness of the single crystal substrate. L is the length of the sample (cantilever). ν s is the Poisson's ratio of the single crystal substrate. δ out is the output displacement based on the measured displacement. V in is the voltage applied to the piezoelectric thin film. Piezoelectric constant -e 31,f The frequency of the AC electric field (AC voltage) in the measurement was 100 Hz. The maximum voltage applied to the piezoelectric thin film was 50 V. 31,f The unit is C / m 2 Example 1-e 31,f is shown in Table 1 below. 31,f ) 2 / ε0ε r (Piezoelectric figure of merit) is shown in Table 1 below.
number
[0105] (Examples 2 to 8, Comparative Examples 1, 2 and 7) The composition of the targets used in forming the piezoelectric thin films of Examples 2 to 8 and Comparative Examples 1, 2 and 7 was different from the composition of the target of Example 1.
[0106] In the case of Example 2, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E BThe starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. A is K, and E in the following chemical formula 1 B are Zn and Ti, and α in the following Chemical Formula 1 was 0.5. In the case of Example 2, x, y and z in the following Chemical Formulas 1 and 1B were the values shown in Table 1 below. x(Bi 0.5 K 0.5 )(Zn 0.5 Ti 0.5 )O3‐yBiFeO3‐zBi(Fe 0.5 Ti 0.5 )O3(1B) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0107] In the case of Example 3, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to match the molar ratios of E, Fe, and Ti. In the case of Example 3, however, the target was E A In the case of Example 3, E in the following chemical formula 1 was not included, and α in the following chemical formula 1 was 0.0. B are Mg and Ti, and x, y and z in the following chemical formulas 1 and 1C have the values shown in Table 1 below. xBi(Mg 0.5 Ti 0.5 )O3‐yBiFeO3‐zBi(Fe 0.5 Ti 0.5 )O3(1C) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0108] In the case of Example 4, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to match the molar ratios of E, Fe, and Ti. However, in the case of Example 4, the target was E A In the case of Example 4, E in the following chemical formula 1 was not included, and α in the following chemical formula 1 was 0.0. B are Zn and Zr, and x, y and z in the following chemical formulas 1 and 1D have the values shown in Table 1 below. xBi(Zn 0.5 Zr 0.5 )O3‐yBiFeO3‐zBi(Fe 0.5 Ti 0.5 )O3(1D) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0109] In the case of Example 5, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to match the molar ratios of E, Fe, and Ti. However, the target of Example 5 was A In the case of Example 5, E in the following chemical formula 1 was not included, and α in the following chemical formula 1 was 0.0. B is Al, and x, y and z in the following chemical formulas 1 and 1E have the values shown in Table 1 below. xBiAlO3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1E) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti0.5 )O3(1)
[0110] In the case of Example 6, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. In the case of Example 6, E in the following chemical formula 1 was A is Ag, and E in the following chemical formula 1 B is Ti, α in the following chemical formula 1 is 0.5, and x, y and z in the following chemical formulas 1 and 1F have the values shown in Table 1 below. xBi 0.5 Ag 0.5 Ti O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1F) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0111] In the case of Example 7, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. A is Ag, and E in the following chemical formula 1 B are Ni and Ti, α in the following chemical formula 1 is 0.5, and x, y and z in the following chemical formulas 1 and 1G are the values shown in Table 1 below. xBi 0.5 Ag 0.5 Ni 0.5 Ti 0.5 O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1G) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0112] In the case of Example 8, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. A is Na, and E in the following chemical formula 1 B is Zr, α in the following chemical formula 1 is 0.5, and x, y and z in the following chemical formulas 1 and 1H have the values shown in Table 1 below. xBi 0.5 Na 0.5 ZrO3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1H) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0113] In the case of Comparative Example 1, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. A is K, and E in the following chemical formula 1 B are Zn and Ti, α in the following chemical formula 1 is 0.5, and x, y and z in the following chemical formulas 1 and 1I have the values shown in Table 1 below. x(Bi 0.5 K 0.5)(Zn 0.5 Ti 0.5 )O3‐yBiFeO3‐zBi(Fe 0.5 Ti 0.5 )O3(1I) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0114] In the case of Comparative Example 2, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. A is Na, and E in the following chemical formula 1 B is Ti, α in the following chemical formula 1 is 0.5, and x, y and z in the following chemical formulas 1 and 1J have the values shown in Table 1 below. x(Bi 0.5 Na 0.5 )TiO3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1J) x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0115] The composition of the target of Comparative Example 7 was BiFeO3. That is, in the case of Comparative Example 7, α, x, and z in the following chemical formula 1 were 0.0. x(Bi 1-α E A α )E B O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0116] The piezoelectric thin film elements of Examples 2 to 8 and Comparative Examples 1, 2 and 7 were each produced in the same manner as in Example 1, except that the compositions of the targets used to form the piezoelectric thin film were different.
[0117] The XRD patterns of the first electrode layers of Examples 2 to 8 and Comparative Examples 1, 2, and 7 were measured by the same method as in Example 1. In all of Examples 2 to 8 and Comparative Examples 1, 2, and 7, the (002) plane of the Pt crystals constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystals was oriented in the in-plane direction of the surface of the first electrode layer.
[0118] The compositions of the piezoelectric thin films of Examples 2 to 8 and Comparative Examples 1, 2, and 7 were analyzed by the same method as in Example 1. In all of Examples 2 to 8 and Comparative Examples 1, 2, and 7, the compositions of the piezoelectric thin films were approximately the same as the compositions of the targets.
[0119] In the same manner as in Example 1, the piezoelectric thin films of Examples 2 to 8 and Comparative Examples 1, 2 and 7 were analyzed based on the XRD method.
[0120] In all of the cases of Examples 2 to 8 and Comparative Examples 1 and 2, the piezoelectric thin films had the following characteristics. The piezoelectric thin film was made of tetragonal crystals of perovskite-type oxide. The (001) plane of the tetragonal crystal was preferentially oriented in the normal direction to the surface of the piezoelectric thin film, i.e., the degree of orientation of the (001) plane of the tetragonal crystal in the normal direction to the surface of the piezoelectric thin film was 90% or more.
[0121] The piezoelectric thin film of Comparative Example 7 contained cubic crystals of a perovskite-type oxide, but did not contain tetragonal crystals of a perovskite-type oxide.
[0122] The c / a ratios for each of Examples 2 to 8 and Comparative Examples 1, 2 and 7 are shown in Table 1 below.
[0123] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin films of Examples 2 to 8 and Comparative Examples 1, 2 and 7 were evaluated. The Pr of each of Examples 2 to 8 and Comparative Examples 1, 2 and 7 is shown in Table 1 below. ε of Examples 2 to 8 and Comparative Examples 1, 2 and 7 r is shown in Table 1 below. -e of Examples 2 to 8 and Comparative Examples 1, 2 and 7 31,f is shown in Table 1 below. (-e 31,f ) 2 / ε0ε r is shown in Table 1 below.
[0124] [Table 1]
[0125] Comparative Example 3 The oxygen partial pressure in the vacuum chamber during the formation of the piezoelectric thin film of Comparative Example 3 was maintained at 0.01 Pa.
[0126] A piezoelectric thin film element of Comparative Example 3 was produced in the same manner as in Example 2, except for the oxygen partial pressure in the process of forming the piezoelectric thin film.
[0127] The XRD pattern of the first electrode layer of Comparative Example 3 was measured by the same method as in Example 1. In the case of Comparative Example 3, the (002) plane of the Pt crystal constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.
[0128] The composition of the piezoelectric thin film of Comparative Example 3 was analyzed by the same method as in Example 1. In the case of Comparative Example 3, the composition of the piezoelectric thin film did not match the composition of the target in terms of the oxygen content.
[0129] The piezoelectric thin film of Comparative Example 3 was analyzed based on the XRD method in the same manner as in Example 1. Since the piezoelectric thin film of Comparative Example 3 did not have crystallinity or crystal orientation, it was not possible to specify c / a of Comparative Example 3.
[0130] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin film of Comparative Example 3 were evaluated. Pr of Comparative Example 3 is shown in Table 2 below. ε of Comparative Example 3 r is shown in Table 2 below. Comparative Example 3-e 31,f is shown in Table 2 below. Comparative Example 3 (-e 31,f ) 2 / ε0ε r is shown in Table 2 below.
[0131] [Table 2]
[0132] (Examples 9 and 10, Comparative Examples 4 and 5) In the case of Examples 9 and 10, the thickness Tp of the piezoelectric thin film 3 was controlled to the value shown in the following Table 3 by changing the number of laser pulses (repetition frequency) in the PLD method. The piezoelectric thin film elements of Examples 9 and 10 were each produced in the same manner as in Example 2, except for the thickness Tp of the piezoelectric thin film 3.
[0133] In the cases of Comparative Examples 4 and 5, Bi, E in the entire raw material powder of the target A , E B The molar ratios of Bi, E, Fe and Ti are as follows: A , E B The starting materials were weighed and mixed so as to correspond to the molar ratios of E, Fe, and Ti. A is K, and E in the following chemical formula 1 B are Zn and Ti, α in the following chemical formula 1 is 0.5, x and y in the following chemical formulas 1 and 1K are the values shown in Table 3 below, and z in the following chemical formula 1 is zero. x(Bi 0.5 K 0.5 )(Zn 0.5 Ti 0.5 )O3-yBiFeO3(1K) x(Bi 1-α E A α )EB O3-yBiFeO3-zBi(Fe 0.5 Ti 0.5 )O3(1)
[0134] In the case of Comparative Examples 4 and 5, the thickness Tp of the piezoelectric thin film 3 was controlled to the value shown in Table 3 below by changing the number of laser pulses (repetition frequency) in the PLD method.
[0135] The piezoelectric thin film elements of Comparative Examples 4 and 5 were fabricated in the same manner as in Example 2, except for the composition of the target and the thickness Tp of the piezoelectric thin film.
[0136] The XRD patterns of the first electrode layers of Examples 9, 10, and Comparative Examples 4 and 5 were measured by the same method as in Example 1. In each of Examples 9, 10, and Comparative Examples 4 and 5, the (002) plane of the Pt crystal constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.
[0137] The compositions of the piezoelectric thin films of Examples 9, 10, and Comparative Examples 4 and 5 were analyzed by the same method as in Example 1. In all of Examples 9, 10, and Comparative Examples 4 and 5, the compositions of the piezoelectric thin films were approximately the same as the compositions of the targets.
[0138] In the same manner as in Example 1, the piezoelectric thin films of Examples 9, 10, and Comparative Examples 4 and 5 were analyzed based on the XRD method.
[0139] In all of Examples 9 and 10 and Comparative Example 5, the piezoelectric thin films had the following characteristics. The piezoelectric thin film was made of tetragonal crystals of perovskite-type oxide. The (001) plane of the tetragonal crystal was preferentially oriented in the normal direction to the surface of the piezoelectric thin film, i.e., the degree of orientation of the (001) plane of the tetragonal crystal in the normal direction to the surface of the piezoelectric thin film was 90% or more.
[0140] The piezoelectric thin film of Comparative Example 4 contained cubic crystals of a perovskite-type oxide, but did not contain tetragonal crystals of a perovskite-type oxide.
[0141] The c / a for each of Examples 9, 10 and Comparative Examples 4 and 5 is shown in Table 3 below.
[0142] The photoelectron spectrum of the piezoelectric thin film of Example 2 was measured by the XPS method. The horizontal axis of the photoelectron spectrum is the binding energy of the photoelectron (unit: eV), and the vertical axis of the photoelectron spectrum is the intensity of the photoelectron (unit: arbitrary unit). The photoelectron spectrum of the piezoelectric thin film of Example 2 included a photoelectron peak derived from Fe.
[0143] Fe 2+ The binding energy of the photoelectron originating from Fe 3+ The binding energy of the photoelectrons is close to that of the Fe 2+ and Fe 3+ When both are included, the photoelectron peak of iron in the photoelectron spectrum is Fe 2+ Photoelectron peak (Fe 2+ Peak) and Fe 3+ Photoelectron peak (Fe 3+ The peaks are superimposed on the Fe 2+ Peak and Fe 3+ It is difficult to measure the peaks individually. 2+ The peaks were fitted with a Gaussian function g1. 3+ The peak was fitted with another Gaussian function g2. The measured Fe photoelectron peak was fitted with g1 + g2. Curve fitting of the measured Fe photoelectron peak with g1 + g2 was performed. The integral of g1 after the curve fitting gave the Fe 2+ The peak area S1 was calculated. From the integral of g2 after curve fitting, Fe 3+ The peak area S2 was calculated based on the following formula C: <Fe 2+ > was calculated from S1 and S2. S1 is the Fe 2+S2 is approximately proportional to the content (unit: atomic %) of Fe in the piezoelectric thin film. 3+ The content (unit: atomic %) of <Fe 2+ > is the Fe in the piezoelectric thin film 2+ and Fe 3+ Fe content relative to the total 2 may be regarded as the percentage of the content (unit: atomic %) of <Fe 2+ >=100×S1 / (S1+S2) (C)
[0144] In the same manner as in Example 2, Examples 9, 10, Comparative Examples 4 and 5 were <Fe 2+ > was calculated. <Fe 2+ > is shown in Table 3 below.
[0145] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin films of Examples 9, 10, and Comparative Examples 4 and 5 were evaluated. The Pr of each of Examples 9, 10 and Comparative Examples 4 and 5 is shown in Table 3 below. ε of Examples 9 and 10 and Comparative Examples 4 and 5 r is shown in Table 3 below. -e of Examples 9, 10, Comparative Examples 4 and 5 31,f is shown in Table 3 below. (-e 31,f ) 2 / ε0ε r is shown in Table 3 below.
[0146] [Table 3]
[0147] (Examples 11 and 12 and Comparative Example 6) In the cases of Examples 11 and 12 and Comparative Example 6, the second intermediate layer was formed on the entire surface of the first electrode layer, and the piezoelectric thin film was formed on the entire surface of the second intermediate layer. The second intermediate layer of Example 11 was made of crystalline SrRuO3. The thickness of the second intermediate layer of Example 11 was 50 nm. "SRO" in Table 4 below means SrRuO3. The second intermediate layer of Example 12 was made of crystalline LaNiO3. The thickness of the second intermediate layer of Example 12 was 50 nm. "LNO" in Table 4 below means LaNiO3. The second intermediate layer of Comparative Example 6 was made of crystalline Fe3O4. The thickness of the second intermediate layer of Comparative Example 6 was 50 nm. "FO" in Table 4 below means Fe3O4.
[0148] The piezoelectric thin film elements of Examples 11 and 12 and Comparative Example 6 were each produced in the same manner as in Example 2, except that a second intermediate layer was formed.
[0149] The XRD patterns of the first electrode layers of Examples 11 and 12 and Comparative Example 6 were measured by the same method as in Example 1. In each of Examples 11 and 12 and Comparative Example 6, the (002) plane of the Pt crystal constituting the first electrode layer was oriented in the normal direction to the surface of the first electrode layer, and the (200) plane of the Pt crystal was oriented in the in-plane direction of the surface of the first electrode layer.
[0150] The compositions of the piezoelectric thin films of Examples 11 and 12 and Comparative Example 6 were analyzed by the same method as in Example 1. In all of Examples 11 and 12 and Comparative Example 6, the compositions of the piezoelectric thin films were almost identical to the compositions of the targets.
[0151] The piezoelectric thin films of Examples 11 and 12 and Comparative Example 6 were analyzed by the XRD method in the same manner as in Example 1. In all of Examples 11 and 12 and Comparative Example 6, the piezoelectric thin films had the following characteristics.
[0152] The piezoelectric thin film was made of tetragonal crystals of perovskite-type oxide. The (001) plane of the tetragonal crystal was preferentially oriented in the normal direction to the surface of the piezoelectric thin film, i.e., the degree of orientation of the (001) plane of the tetragonal crystal in the normal direction to the surface of the piezoelectric thin film was 90% or more. The c / a for each of Examples 11 and 12 and Comparative Example 6 is shown in Table 4 below.
[0153] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin films of Examples 11 and 12 and Comparative Example 6 were evaluated. The Pr of each of Examples 11 and 12 and Comparative Example 6 is shown in Table 4 below. ε of Examples 11 and 12 and Comparative Example 6 r is shown in Table 4 below. -e of Examples 11 and 12 and Comparative Example 6 31,f is shown in Table 4 below. (-e 31,f ) 2 / ε0ε r is shown in Table 4 below.
[0154] [Table 4]
[0155] (Example 13) In the process of producing the piezoelectric thin film element of Example 13, a first intermediate layer was not formed. In the process of producing the piezoelectric thin film element of Example 13, a first electrode layer made of crystalline SrRuO3 was formed directly on the entire surface of the single crystal substrate. The thickness of the first electrode layer of Example 13 was 200 nm. Except for these details, the piezoelectric thin film element of Example 13 was produced in the same manner as in Example 2.
[0156] The XRD pattern of the first electrode layer of Example 13 was measured by the same method as in Example 1. The in-plane orientation of the crystals of the first electrode layer of Example 13 was evaluated by the in-plane measurement similar to that of Example 1. In the case of Example 13, the crystal plane of the first electrode layer was not oriented in the in-plane direction of the surface of the first electrode layer. In other words, in the case of Example 13, the crystals of the first electrode layer did not have in-plane orientation.
[0157] The composition of the piezoelectric thin film of Example 13 was analyzed by the same method as in Example 1. In the case of Example 13, the composition of the piezoelectric thin film was approximately the same as the composition of the target.
[0158] The piezoelectric thin film of Example 13 was analyzed by XRD in the same manner as in Example 1. The piezoelectric thin film of Example 13 had the following characteristics.
[0159] The piezoelectric thin film was made of tetragonal crystals of perovskite-type oxide. The (001) plane of the tetragonal crystal was preferentially oriented in the normal direction to the surface of the piezoelectric thin film, i.e., the degree of orientation of the (001) plane of the tetragonal crystal in the normal direction to the surface of the piezoelectric thin film was 90% or more. The c / a for Example 13 is shown in Table 5 below.
[0160] In the same manner as in Example 1, the piezoelectric properties of the piezoelectric thin film of Example 13 were evaluated. Pr for Example 13 is shown in Table 5 below. ε in Example 13 r is shown in Table 5 below. Example 13-e 31,f is shown in Table 5 below. (-e 31,f ) 2 / ε0ε r is shown in Table 5 below.
[0161] [Table 5] [Industrial Applicability]
[0162] The piezoelectric thin film according to the present invention is applied to, for example, a piezoelectric transducer, a piezoelectric actuator, and a piezoelectric sensor. [Explanation of symbols]
[0163] 10...piezoelectric thin film element, 10a...ultrasonic transducer, 1...single crystal substrate, 2...first electrode layer, 3...piezoelectric thin film, 4...second electrode layer, 5...first intermediate layer, 6...second intermediate layer, D N...Normal direction to the surface of the single crystal substrate, dn...Normal direction to the surface of the piezoelectric thin film, uc...Unit cell of oxide (tetragonal crystal) having a perovskite structure.
Claims
1. A piezoelectric thin film including an oxide having a perovskite structure, the piezoelectric thin film contains a tetragonal crystal of the oxide, the (001) plane of the tetragonal crystal is oriented in a normal direction to the surface of the piezoelectric thin film, The spacing between the (001) planes of the tetragonal crystal is c; The spacing between the (100) planes of the tetragonal crystal is a, c / a is equal to or greater than 1.050 and equal to or less than 1.250, The oxide is Fe 2+ Including, The oxide is represented by the following chemical formula 1: E in the following chemical formula 1 A is at least one element selected from the group consisting of Na, K and Ag, E in the following chemical formula 1 B is at least one element selected from the group consisting of Mg, Al, Zr, Ti, Ni and Zn, In the following chemical formula 1, x is 0.10 or more and 0.80 or less, In the following chemical formula 1, y is 0.10 or more and 0.85 or less, In the following chemical formula 1, z is 0.05 or more and 0.80 or less, x+y+z is 1.00, In the following chemical formula 1, α is 0.00 or more and less than 1.00, I(001) is the peak intensity of the diffracted X-rays of the (001) plane of the tetragonal crystal measured in the out-of-plane direction of the surface of the piezoelectric thin film, I(110) is the peak intensity of the diffracted X-rays of the (110) plane of the tetragonal crystal measured in the out-of-plane direction of the surface of the piezoelectric thin film, I(111) is the peak intensity of the diffracted X-rays from the (111) plane of the tetragonal crystal measured in the out-of-plane direction of the surface of the piezoelectric thin film, ΣI (hkl) is I (001) + I (110) + I (111), The degree of orientation of the (001) plane of the tetragonal crystal in the normal direction to the surface of the piezoelectric thin film is expressed as 100×I (001) / ΣI (hkl), The degree of orientation is 70% or more and 100% or less. Piezoelectric thin film. x(Bi 1-α E A α )E B O 3 -yBiFeO 3 -zBi(Fe 0.5 Ti 0.5 ) 3 (1)
2. The oxide is Bi. 3+ and Fe 3+ Further comprising: The piezoelectric thin film according to claim 1 .
3. The thickness of the piezoelectric thin film is 500 nm or more and 5000 nm or less. The piezoelectric thin film according to claim 1 or 2.
4. It is an epitaxial film. The piezoelectric thin film according to any one of claims 1 to 3.
5. A piezoelectric thin film according to any one of claims 1 to 4, Piezoelectric thin film element.
6. A single crystal substrate; the piezoelectric thin film overlying the single crystal substrate; Equipped with 6. The piezoelectric thin film element according to claim 5.
7. A single crystal substrate; an electrode layer overlying the single crystal substrate; the piezoelectric thin film overlying the electrode layer; Equipped with 6. The piezoelectric thin film element according to claim 5.
8. An electrode layer; the piezoelectric thin film overlying the electrode layer; Equipped with 6. The piezoelectric thin film element according to claim 5.
9. Further comprising a first intermediate layer, the first intermediate layer is disposed between the single crystal substrate and the electrode layer; 8. The piezoelectric thin film element according to claim 7.
10. The first intermediate layer is made of ZrO 2 and Y 2 O 3 Including, 10. The piezoelectric thin film element according to claim 9.
11. Further comprising a second intermediate layer, the second intermediate layer is disposed between the electrode layer and the piezoelectric thin film; The piezoelectric thin film element according to any one of claims 7 to 10.
12. The second intermediate layer is made of SrRuO 3 and LaNiO 3 At least one of the following is included: The piezoelectric thin film element according to claim 11.
13. The electrode layer includes platinum crystals, the (002) plane of the platinum crystal is oriented in a direction normal to the surface of the electrode layer; The (200) plane of the platinum crystal is oriented in the in-plane direction of the surface of the electrode layer. The piezoelectric thin film element according to any one of claims 7 to 12.
14. A piezoelectric thin film element according to any one of claims 5 to 13, Piezoelectric transducer.
Citation Information
Patent Citations
Piezoelectric element, ink jet head, angular rate sensor, and ink jet type recording device
JP2005333108A
Oxide body, method for producing the same, and piezoelectric element
JP2010053422A
Piezoelectric thin film, piezoelectric element, method of manufacturing the piezoelectric element, liquid discharge head, and ultrasonic motor
JP2011181776A
Perovskite oxide, oxide composition, oxide material, piezoelectric element, and liquid discharge device
JP2011249588A
Piezoelectric thin film, piezoelectric thin film element, piezoelectric actuator, piezoelectric sensor, head assembly, head stack assembly, hard disk drive, printer head, and inkjet printer device
JP2020113649A