Polarizing film with pressure-sensitive adhesive layer and image display device
The polarizing film with an adhesive layer addresses thickness issues and UV protection in image display devices, ensuring effective UV-cutting and preventing curling, thereby improving production yield and device durability.
Patent Information
- Application Number
- JP2021134046
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2015-12-25
- Filing Date
- 2021-08-19
- Publication Date
- 2024-11-07
- Estimated Expiration
- 2036-05-11
AI Technical Summary
Existing polarizing films in image display devices face issues with thickness unevenness, production yield deterioration, workability, and curling due to thinning, while requiring enhanced ultraviolet absorption and maintaining optical properties under prolonged UV exposure.
A polarizing film with an adhesive layer on both sides, featuring a transparent protective film with low UV transmission and an ultraviolet-absorbing adhesive layer, ensuring a higher UV-cutting function and preventing curling, using materials like triacetyl cellulose, acrylic, or polyolefin films with a cyclo or norbornene structure.
The solution provides improved UV protection, reduces production defects, and maintains optical integrity by suppressing curling and deterioration of display components, enhancing the durability and performance of image display devices.
Smart Images

Figure 0007579219000004 
Figure 0007579219000005 
Figure 0007579219000006
Abstract
Description
[Technical field]
[0001] The present invention relates to a polarizing film with an adhesive layer for use in an image display device. The present invention also relates to an image display device using the polarizing film with an adhesive layer. Examples of image display devices include liquid crystal display devices, organic EL (electroluminescence) display devices, PDPs (plasma display panels), and electronic paper. [Background technology]
[0002] Due to the image formation method of liquid crystal display devices and organic EL display devices, for example, in liquid crystal display devices, it is essential to place polarizing elements on both sides of the liquid crystal cell, and polarizing films are generally attached to the liquid crystal display devices. In addition to polarizing films, various optical elements have come to be used in display panels such as liquid crystal panels and organic EL panels in order to improve the display quality of the displays.
[0003] The polarizing films used in these image display devices generally have a structure in which a polarizer is sandwiched between two protective films, and triacetyl cellulose (TAC) is widely used as the protective films.
[0004] In recent years, with the trend toward lighter and thinner image display devices, thinner components are being required for the image display devices, and thinner protective films for polarizing films are also being required. When the thickness of the protective film is thin, it becomes difficult to sufficiently block ultraviolet rays incident on the image display device, and this causes problems such as accelerating the deterioration of not only polarizers but also various optical components such as liquid crystal panels and organic EL elements used in image display devices due to ultraviolet rays.
[0005] To solve such problems, for example, a double-sided pressure-sensitive adhesive sheet for an image display device is known, which is disposed between a surface protection panel and a viewing side of a liquid crystal module in the image display device to integrate the two members, and has at least one ultraviolet absorbing layer, a light transmittance of 30% or less at a wavelength of 380 nm, and a visible light transmittance of 80% or more at wavelengths longer than 430 nm (see, for example, Patent Document 1), and a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer containing an acrylic polymer and a triazine-based ultraviolet absorber (see, for example, Patent Document 2). It is also known that in a pressure-sensitive adhesive optical film in which a pressure-sensitive adhesive layer is provided on one or both sides of the optical film, the pressure-sensitive adhesive layer can be given ultraviolet absorbing ability (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2012-211305 A [Patent Document 2] JP 2013-75978 A [Patent Document 3] Patent No. 4208187 Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, as described in Patent Documents 1 to 3, it has become known to use a transparent adhesive having an ultraviolet absorbing function to bond various components used in an image display device. However, this method has problems such as uneven thickness, poor yield, and workability.
[0008] Depending on the application of the polarizing film, there are cases where the polarizing film is required to have a higher ultraviolet absorbing function. Specifically, it is required that the optical properties do not change even when exposed to ultraviolet light for a long period of time (specifically, about 300 hours) or when exposed to ultraviolet light having a wide wavelength range, and a polarizing film that satisfies such a higher ultraviolet absorbing function has been desired.
[0009] Furthermore, there has been a problem that the resulting polarizing film tends to curl due to the thinning of the polarizer and protective film of the polarizing film.
[0010] Therefore, the present invention aims to provide a polarizing film with a pressure-sensitive adhesive layer that can solve the problem of reduced yield, and can impart a higher ultraviolet ray blocking function and suppress curling even when the polarizing film is thin. Another object of the present invention is to provide an image display device using the polarizing film with a pressure-sensitive adhesive layer. [Means for solving the problem]
[0011] Means of the Invention The present inventors have conducted extensive research to solve the above problems, and as a result have found the following polarizing film with a pressure-sensitive adhesive layer, thereby completing the present invention.
[0012] That is, the present invention provides a polarizing film with a pressure-sensitive adhesive layer, which is used on the viewing side of an image display unit in an image display device, The polarizing film with a pressure-sensitive adhesive layer has a polarizing film and pressure-sensitive adhesive layers on both sides of the polarizing film, The polarizing film has a polarizer and transparent protective films on both sides of the polarizer, The transparent protective film on the viewing side of the polarizer has a transmittance of less than 6% at a wavelength of 380 nm; and The present invention relates to a polarizing film with a pressure-sensitive adhesive layer, wherein the pressure-sensitive adhesive layer on the viewing side of the polarizing film has an ultraviolet absorbing function.
[0013] It is preferable that the transparent protective film on the viewing side of the polarizer is at least one film selected from the group consisting of triacetyl cellulose film, acrylic film, polyethylene terephthalate film, and polyolefin film having a cyclo- or norbornene structure, and has a thickness of 40 μm or less.
[0014] The thickness of the pressure-sensitive adhesive layer on the viewing side of the polarizing film is preferably at least twice as thick as the thickness of the pressure-sensitive adhesive layer on the image display portion side of the polarizing film.
[0015] It is preferable that the pressure-sensitive adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm and a transmittance of 60% or more at a wavelength of 400 nm.
[0016] The pressure-sensitive adhesive layer on the viewing side of the polarizing film preferably has a b* value of 3.0 or less.
[0017] It is preferable that the pressure-sensitive adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm and a transmittance of 75% or less at a wavelength of 420 nm.
[0018] The pressure-sensitive adhesive layer on the viewing side of the polarizing film preferably contains an acrylic polymer as a base polymer.
[0019] The pressure-sensitive adhesive layer-attached polarizing film of the present invention is preferably used in a liquid crystal display device or an organic EL display device.
[0020] The present invention also relates to an image display device, characterized in that the pressure-sensitive adhesive layer-attached polarizing film of the present invention is used on the viewing side of an image display section. Effect of the Invention
[0021] The polarizing film with a pressure-sensitive adhesive layer of the present invention has a structure in which a pressure-sensitive adhesive layer having an ultraviolet absorbing function is laminated in advance on the viewing side of the polarizing film, and therefore the problems of process elimination and yield reduction can be solved, and even if the polarizing film is thin, a higher ultraviolet blocking function can be imparted and curling can be suppressed. In addition, the image display device of the present invention uses the polarizing film with a pressure-sensitive adhesive layer, and therefore deterioration of various optical members including liquid crystal panels and organic EL elements used in the image display device due to ultraviolet rays can be suppressed. [Brief description of the drawings]
[0022] [Figure 1] 1 is a cross-sectional view that illustrates a schematic diagram of one embodiment of a pressure-sensitive adhesive layer-attached polarizing film of the present invention. [Diagram 2] 1 is a cross-sectional view that illustrates a schematic diagram of an embodiment of an image display device of the present invention. [Diagram 3] 1 is a cross-sectional view that illustrates a schematic diagram of an embodiment of an image display device of the present invention. [Figure 4] 1 is a cross-sectional view that illustrates a schematic diagram of an embodiment of an image display device of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0023] 1. Polarizing film with adhesive layer The pressure-sensitive adhesive layer-attached polarizing film of the present invention is used on the viewing side of an image display unit in an image display device, The polarizing film with a pressure-sensitive adhesive layer has a polarizing film and pressure-sensitive adhesive layers on both sides of the polarizing film, The polarizing film has a polarizer and transparent protective films on both sides of the polarizer, The transparent protective film on the viewing side of the polarizer has a transmittance of less than 6% at a wavelength of 380 nm; and The pressure-sensitive adhesive layer on the viewing side of the polarizing film has an ultraviolet absorbing function.
[0024] As shown in FIG. 1, the polarizing film 1 with the adhesive layer of the present invention may be configured to include a visible-side adhesive layer 2a / a visible-side transparent protective film 3a / a polarizer 4 / a transparent protective film 3b on the image display unit side / a pressure-sensitive adhesive layer 2b, and may further include a retardation film or the like. Specifically, the polarizing film 5 may be configured to include a visible-side adhesive layer 2a / a visible-side transparent protective film 3a / a polarizer 4 / a transparent protective film 3b on the image display unit side / a pressure-sensitive adhesive layer 2b on the image display unit side / a retardation film (not shown) / a pressure-sensitive adhesive layer (not shown) or the like. The polarizing film 5 is configured to include a visible-side transparent protective film 3a / a polarizer 4 / a transparent protective film 3b on the image display unit side. Each layer will be described in detail below.
[0025] (1) Visible side adhesive layer In the present invention, the pressure-sensitive adhesive layer on the viewing side of the polarizing film (viewing-side pressure-sensitive adhesive layer) has an ultraviolet ray absorbing function. The pressure-sensitive adhesive layer on the viewing side may have an ultraviolet ray absorbing function, and the composition thereof is not particularly limited.
[0026] The visible-side adhesive layer can be formed using an appropriate adhesive, and the type is not particularly limited. Examples of the adhesive include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinylpyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives. Among these adhesives, acrylic-based adhesives are preferably used because they have excellent optical transparency, appropriate adhesion, cohesion, and adhesive properties, and are excellent in weather resistance and heat resistance. The acrylic adhesive (composition) contains an acrylic polymer as a base polymer.
[0027] The acrylic pressure-sensitive adhesive composition preferably contains, for example, a partial polymer of a monomer component containing an alkyl (meth)acrylate and / or a (meth)acrylic polymer obtained from the monomer component, and an ultraviolet absorber.
[0028] (1-1) Partially polymerized product of monomer component, and (meth)acrylic polymer The acrylic pressure-sensitive adhesive composition contains a partial polymer of a monomer component containing an alkyl (meth)acrylate and / or a (meth)acrylic polymer obtained from the monomer component.
[0029] The alkyl (meth)acrylate may be, for example, one having a linear or branched alkyl group having 1 to 24 carbon atoms at the ester end. The alkyl (meth)acrylate may be used alone or in combination of two or more. The alkyl (meth)acrylate refers to alkyl acrylate and / or alkyl methacrylate, and (meth) in the present invention has the same meaning.
[0030] The alkyl (meth)acrylate may preferably be, for example, the alkyl (meth)acrylate having a branch having 1 to 9 carbon atoms. The alkyl (meth)acrylate is preferable in that it is easy to balance the adhesive properties. Specifically, n-butyl (meth)acrylate, s-butyl (meth)acrylate, t-butyl (meth)acrylate, isobutyl (meth)acrylate, n-pentyl (meth)acrylate, isopentyl (meth)acrylate, isohexyl (meth)acrylate, isoheptyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, etc. may be mentioned, and these may be used alone or in combination of two or more.
[0031] In the present invention, the alkyl (meth)acrylate having an alkyl group having 1 to 24 carbon atoms at the ester terminal is preferably 40% by weight or more, more preferably 50% by weight or more, and even more preferably 60% by weight or more, of the total amount of monofunctional monomer components forming the (meth)acrylic polymer.
[0032] The monomer component may contain a copolymerizable monomer other than the alkyl (meth)acrylate as a monofunctional monomer component. The copolymerizable monomer may be used as the remainder of the alkyl (meth)acrylate in the monomer component.
[0033] The copolymerization monomer may include, for example, a cyclic nitrogen-containing monomer. As the cyclic nitrogen-containing monomer, a monomer having a polymerizable functional group with an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and having a cyclic nitrogen structure may be used without any particular limitation. The cyclic nitrogen structure is preferably one having a nitrogen atom in the cyclic structure. Examples of the cyclic nitrogen-containing monomer include lactam vinyl monomers such as N-vinylpyrrolidone, N-vinyl-ε-caprolactam, and methylvinylpyrrolidone; vinyl monomers having a nitrogen-containing heterocycle such as vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, and vinylmorpholine. In addition, examples of the cyclic nitrogen-containing monomer include (meth)acrylic monomers containing a heterocycle such as a morpholine ring, a piperidine ring, a pyrrolidine ring, and a piperazine ring. Specific examples include N-acryloylmorpholine, N-acryloylpiperidine, N-methacryloylpiperidine, and N-acryloylpyrrolidine. Among the above cyclic nitrogen-containing monomers, lactam vinyl monomers are preferred.
[0034] In the present invention, the amount of the cyclic nitrogen-containing monomer is preferably 0.5 to 50% by weight, more preferably 0.5 to 40% by weight, and even more preferably 0.5 to 30% by weight, based on the total amount of monofunctional monomer components forming the (meth)acrylic polymer.
[0035] The monomer component used in the present invention may contain a hydroxyl group-containing monomer as a monofunctional monomer component. As the hydroxyl group-containing monomer, a monomer having a polymerizable functional group with an unsaturated double bond such as a (meth)acryloyl group or a vinyl group and having a hydroxyl group may be used without any particular limitation. As the hydroxyl group-containing monomer, for example, hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, 10-hydroxydecyl (meth)acrylate, and 12-hydroxylauryl (meth)acrylate; and hydroxyalkyl cycloalkane (meth)acrylates such as (4-hydroxymethylcyclohexyl)methyl (meth)acrylate may be mentioned. Other examples include hydroxyethyl (meth)acrylamide, allyl alcohol, 2-hydroxyethyl vinyl ether, 4-hydroxybutyl vinyl ether, diethylene glycol monovinyl ether, etc. These can be used alone or in combination. Among these, hydroxyalkyl (meth)acrylates are preferred.
[0036] In the present invention, the hydroxyl group-containing monomer is preferably 1% by weight or more, more preferably 2% by weight or more, and even more preferably 3% by weight or more, based on the total amount of the monofunctional monomer components forming the (meth)acrylic polymer, from the viewpoint of increasing adhesive strength and cohesive strength. On the other hand, if the amount of the hydroxyl group-containing monomer is too much, the adhesive layer may become hard and adhesive strength may decrease, and the adhesive may become too viscous or gel, so the hydroxyl group-containing monomer is preferably 30% by weight or less, more preferably 27% by weight or less, and even more preferably 25% by weight or less, based on the total amount of the monofunctional monomer components forming the (meth)acrylic polymer.
[0037] Furthermore, the monomer component forming the (meth)acrylic polymer may contain other functional group-containing monomers as monofunctional monomers, such as carboxyl group-containing monomers and monomers having a cyclic ether group.
[0038] The carboxyl group-containing monomer may be any monomer having a polymerizable functional group with an unsaturated double bond, such as a (meth)acryloyl group or a vinyl group, and having a carboxyl group, without any particular limitations. Examples of the carboxyl group-containing monomer include (meth)acrylic acid, carboxyethyl (meth)acrylate, carboxypentyl (meth)acrylate, itaconic acid, maleic acid, fumaric acid, crotonic acid, isocrotonic acid, etc., which may be used alone or in combination. Anhydrides of itaconic acid and maleic acid may be used. Among these, acrylic acid and methacrylic acid are preferred, and acrylic acid is particularly preferred. In addition, a carboxyl group-containing monomer may be used as the monomer component used in the production of the (meth)acrylic polymer of the present invention, and on the other hand, a carboxyl group-containing monomer may not be used.
[0039] As the monomer having a cyclic ether group, those having a polymerizable functional group having an unsaturated double bond such as a (meth)acryloyl group or a vinyl group, and having a cyclic ether group such as an epoxy group or an oxetane group, can be used without any particular limitation. As the epoxy group-containing monomer, for example, glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate glycidyl ether, etc. can be mentioned. As the oxetane group-containing monomer, for example, 3-oxetanylmethyl (meth)acrylate, 3-methyl-oxetanylmethyl (meth)acrylate, 3-ethyl-oxetanylmethyl (meth)acrylate, 3-butyl-oxetanylmethyl (meth)acrylate, 3-hexyl-oxetanylmethyl (meth)acrylate, etc. can be mentioned. These can be used alone or in combination.
[0040] In the present invention, the amount of the carboxyl group-containing monomer and the monomer having a cyclic ether group is preferably 30% by weight or less, more preferably 27% by weight or less, and even more preferably 25% by weight or less, of the total amount of monofunctional monomer components forming the (meth)acrylic polymer.
[0041] The monomer components forming the (meth)acrylic polymer of the present invention include, for example, copolymerizable monomers such as CH2=C(R 1 )COOR 2 (The above R 1 is hydrogen or a methyl group, R 2 represents a substituted alkyl group having 1 to 3 carbon atoms, or a cyclic cycloalkyl group.
[0042] Here, R 2 As the substituent of the substituted alkyl group having 1 to 3 carbon atoms as mentioned above, an aryl group having 3 to 8 carbon atoms or an aryloxy group having 3 to 8 carbon atoms is preferable. The aryl group is not limited, but a phenyl group is preferable.
[0043] Such CH2=C(R 1 )COOR 2 Examples of the monomer represented by the formula (I) include phenoxyethyl (meth)acrylate, benzyl (meth)acrylate, cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, etc. These can be used alone or in combination.
[0044] In the present invention, the CH2=C(R 1 )COOR 2 The (meth)acrylate represented by the formula (I) can be used in an amount of 50% by weight or less, preferably 45% by weight or less, more preferably 40% by weight or less, and even more preferably 35% by weight or less, based on the total amount of monofunctional monomer components forming the (meth)acrylic polymer.
[0045] Other copolymerizable monomers include vinyl acetate, vinyl propionate, styrene, α-methylstyrene; glycol-based acrylic ester monomers such as polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, methoxyethylene glycol (meth)acrylate, and methoxypolypropylene glycol (meth)acrylate; acrylic ester monomers such as tetrahydrofurfuryl (meth)acrylate, fluorine (meth)acrylate, silicone (meth)acrylate, and 2-methoxyethyl acrylate; amide group-containing monomers, amino group-containing monomers, imide group-containing monomers, N-acryloylmorpholine, and vinyl ether monomers. Also, monomers having a cyclic structure such as terpene (meth)acrylate and dicyclopentanyl (meth)acrylate can be used as copolymerizable monomers.
[0046] Further, examples of the silane monomers include those containing silicon atoms. Examples of the silane monomers include 3-acryloxypropyltriethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 4-vinylbutyltrimethoxysilane, 4-vinylbutyltriethoxysilane, 8-vinyloctyltrimethoxysilane, 8-vinyloctyltriethoxysilane, 10-methacryloyloxydecyltrimethoxysilane, 10-acryloyloxydecyltrimethoxysilane, 10-methacryloyloxydecyltriethoxysilane, and 10-acryloyloxydecyltriethoxysilane.
[0047] The monomer components forming the (meth)acrylic polymer of the present invention may contain, in addition to the monofunctional monomers exemplified above, a polyfunctional monomer, if necessary, in order to adjust the cohesive strength of the pressure-sensitive adhesive.
[0048] The polyfunctional monomer is a monomer having at least two polymerizable functional groups having an unsaturated double bond, such as a (meth)acryloyl group or a vinyl group, and examples thereof include (poly)ethylene glycol di(meth)acrylate, (poly)propylene glycol di(meth)acrylate, neopentyl glycol di(meth)acrylate, pentaerythritol di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol hexa(meth)acrylate, and 1,2-ethylene glycol di(meth)acrylate. Examples of the polyhydric alcohols include ester compounds of polyhydric alcohols and (meth)acrylic acid, such as 1,6-hexanediol di(meth)acrylate, 1,12-dodecanediol di(meth)acrylate, trimethylolpropane tri(meth)acrylate, and tetramethylolmethane tri(meth)acrylate; allyl (meth)acrylate, vinyl (meth)acrylate, divinylbenzene, epoxy acrylate, polyester acrylate, urethane acrylate, butyl di(meth)acrylate, and hexyl di(meth)acrylate. Among these, trimethylolpropane tri(meth)acrylate, hexanediol di(meth)acrylate, and dipentaerythritol hexa(meth)acrylate can be preferably used. The polyfunctional monomers can be used alone or in combination of two or more.
[0049] The amount of polyfunctional monomer used varies depending on its molecular weight, the number of functional groups, etc., but is preferably 3 parts by weight or less, more preferably 2 parts by weight or less, and even more preferably 1 part by weight or less, based on 100 parts by weight of the total of monofunctional monomers. The lower limit is not particularly limited, but is preferably 0 parts by weight or more, and more preferably 0.001 parts by weight or more. By keeping the amount of polyfunctional monomer used within the above range, the adhesive strength can be improved.
[0050] The (meth)acrylic polymer can be produced by appropriately selecting a known production method such as solution polymerization, radiation polymerization such as ultraviolet (UV) polymerization, various radical polymerizations such as bulk polymerization, emulsion polymerization, etc. The obtained (meth)acrylic polymer may be any of a random copolymer, a block copolymer, a graft copolymer, etc.
[0051] In the present invention, a partial polymer of the above monomer component can also be suitably used.
[0052] When the (meth)acrylic polymer is produced by radical polymerization, a polymerization initiator, a chain transfer agent, an emulsifier, etc. used in radical polymerization can be appropriately added to the monomer component to perform polymerization. The polymerization initiator, the chain transfer agent, the emulsifier, etc. used in the radical polymerization are not particularly limited and can be appropriately selected and used. The weight average molecular weight of the (meth)acrylic polymer can be controlled by the amount of the polymerization initiator and the chain transfer agent used and the reaction conditions, and the amount used is appropriately adjusted depending on the type of these.
[0053] For example, in solution polymerization, for example, ethyl acetate, toluene, etc. are used as a polymerization solvent. In a specific example of solution polymerization, the reaction is carried out under a stream of an inert gas such as nitrogen, with the addition of a polymerization initiator, usually at about 50 to 70° C., for about 5 to 30 hours.
[0054] Examples of the thermal polymerization initiator used in solution polymerization and the like include 2,2'-azobisisobutyronitrile, 2,2'-azobis-2-methylbutyronitrile, 2,2'-azobis(2-methylpropionic acid) dimethyl, 4,4'-azobis-4-cyanovaleric acid, azobisisovaleronitrile, 2,2'-azobis(2-amidinopropane) dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazoline-2- azo initiators such as 2,2'-azobis(2-methylpropionamidine) dihydrochloride, 2,2'-azobis(N,N'-dimethyleneisobutylamidine), and 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine]hydrate (VA-057, manufactured by Wako Pure Chemical Industries, Ltd.); persulfates such as potassium persulfate and ammonium persulfate; and di(2-ethylhexyl)peroxy Examples of initiators include, but are not limited to, peroxide initiators such as dicarbonate, di(4-t-butylcyclohexyl)peroxydicarbonate, di-sec-butylperoxydicarbonate, t-butylperoxyneodecanoate, t-hexylperoxypivalate, t-butylperoxypivalate, dilauroyl peroxide, di-n-octanoyl peroxide, 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate, di(4-methylbenzoyl)peroxide, dibenzoyl peroxide, t-butylperoxyisobutyrate, 1,1-di(t-hexylperoxy)cyclohexane, t-butyl hydroperoxide, and hydrogen peroxide; and redox initiators combining a peroxide and a reducing agent, such as a combination of a persulfate and sodium hydrogen sulfite, or a combination of a peroxide and sodium ascorbate.
[0055] The polymerization initiator may be used alone or in a mixture of two or more kinds. The amount of the polymerization initiator is preferably about 1 part by weight or less, more preferably about 0.005 to 1 part by weight, and even more preferably about 0.02 to 0.5 parts by weight, relative to 100 parts by weight of the total amount of the monomer components.
[0056] When 2,2'-azobisisobutyronitrile is used as the polymerization initiator, the amount of the polymerization initiator used is preferably about 0.2 part by weight or less, and more preferably about 0.06 to 0.2 part by weight, per 100 parts by weight of the total amount of the monomer components.
[0057] Examples of the chain transfer agent include lauryl mercaptan, glycidyl mercaptan, mercaptoacetic acid, 2-mercaptoethanol, thioglycolic acid, 2-ethylhexyl thioglycolate, 2,3-dimercapto-1-propanol, etc. The chain transfer agent may be used alone or in combination of two or more kinds, but the total content is about 0.3 parts by weight or less relative to 100 parts by weight of the total amount of the monomer components.
[0058] Examples of emulsifiers used in emulsion polymerization include anionic emulsifiers such as sodium lauryl sulfate, ammonium lauryl sulfate, sodium dodecylbenzenesulfonate, polyoxyethylene alkyl ether ammonium sulfate, and sodium polyoxyethylene alkyl phenyl ether sulfate, and nonionic emulsifiers such as polyoxyethylene alkyl ether, polyoxyethylene alkyl phenyl ether, polyoxyethylene fatty acid ester, and polyoxyethylene-polyoxypropylene block polymer. These emulsifiers may be used alone or in combination of two or more.
[0059] Furthermore, as reactive emulsifiers, emulsifiers into which a radically polymerizable functional group such as a propenyl group or an allyl ether group has been introduced include, for example, Aqualon HS-10, HS-20, KH-10, BC-05, BC-10, BC-20 (all manufactured by Daiichi Kogyo Seiyaku Co., Ltd.), Adeka Reasoap SE10N (manufactured by ADEKA Corporation), etc. The amount of the emulsifier used is preferably 5 parts by weight or less based on 100 parts by weight of the total amount of the monomer components.
[0060] In addition, when the (meth)acrylic polymer is produced by radiation polymerization, the monomer component can be polymerized by irradiating it with radiation such as an electron beam or ultraviolet (UV) rays. Among these, ultraviolet polymerization is preferred. Hereinafter, ultraviolet polymerization, which is a preferred embodiment of radiation polymerization, will be described.
[0061] When carrying out ultraviolet polymerization, it is preferable to include a photopolymerization initiator in the monomer component, because of the advantage of being able to shorten the polymerization time. Therefore, when carrying out ultraviolet polymerization, it is preferable to form, for example, by ultraviolet polymerization of an ultraviolet-curable acrylic adhesive composition containing a monomer component containing the alkyl (meth)acrylate and / or a partial polymer of the monomer component, an ultraviolet absorber, and a photopolymerization initiator. The adhesive layer formed by ultraviolet polymerization of the ultraviolet-curable acrylic adhesive composition can be formed to a thickness of 150 μm or more, which is preferable because an adhesive layer of a wide range of thicknesses can be formed.
[0062] The photopolymerization initiator preferably contains a photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more. When the pressure-sensitive adhesive composition contains an ultraviolet absorber, ultraviolet light is absorbed by the ultraviolet absorber when ultraviolet polymerization is performed, and the polymerization cannot be performed sufficiently. However, if the photopolymerization initiator (A) has an absorption band at a wavelength of 400 nm or more, it is preferable because the composition can be sufficiently polymerized despite the inclusion of an ultraviolet absorber.
[0063] Examples of the photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more include bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (Irgacure 819, manufactured by BASF) and 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide (LUCIRIN TPO, manufactured by BASF).
[0064] The photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more may be used alone or in combination of two or more kinds.
[0065] The amount of the photopolymerization initiator (A) having an absorption band of 400 nm or more is not particularly limited, but is preferably less than the amount of the ultraviolet absorber described below, and is preferably about 0.005 to 1 part by weight, more preferably about 0.02 to 0.5 parts by weight, relative to 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer. By setting the amount of the photopolymerization initiator (A) to be added within the above range, ultraviolet polymerization can be sufficiently promoted, which is preferable.
[0066] The photopolymerization initiator may contain a photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm. The photopolymerization initiator (B) preferably does not have an absorption band at a wavelength of 400 nm or more. The photopolymerization initiator (B) is not particularly limited as long as it generates radicals by ultraviolet light and initiates photopolymerization and has an absorption band at a wavelength of less than 400 nm, and any photopolymerization initiator that is commonly used may be suitably used. For example, benzoin ether-based photopolymerization initiators, acetophenone-based photopolymerization initiators, α-ketol-based photopolymerization initiators, photoactive oxime-based photopolymerization initiators, benzoin-based photopolymerization initiators, benzyl-based photopolymerization initiators, benzophenone-based photopolymerization initiators, ketal-based photopolymerization initiators, thioxanthone-based photopolymerization initiators, acylphosphine oxide-based photopolymerization initiators, etc. may be used.
[0067] Specifically, examples of the benzoin ether-based photopolymerization initiator include benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin isopropyl ether, benzoin isobutyl ether, 2,2-dimethoxy-1,2-diphenylethan-1-one, and anisole methyl ether.
[0068] Examples of the acetophenone-based photopolymerization initiator include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 4-phenoxydichloroacetophenone, and 4-t-butyldichloroacetophenone.
[0069] Examples of the α-ketol photopolymerization initiator include 2-methyl-2-hydroxypropiophenone, 1-[4-(2-hydroxyethyl)phenyl]-2-hydroxy-2-methylpropan-1-one, and the like.
[0070] An example of the photoactive oxime-based photopolymerization initiator is 1-phenyl-1,2-propanedione-2-(O-ethoxycarbonyl)-oxime.
[0071] An example of the benzoin-based photopolymerization initiator is benzoin.
[0072] The benzyl-based photopolymerization initiator includes, for example, benzyl.
[0073] Benzophenone-based photopolymerization initiators include, for example, benzophenone, benzoylbenzoic acid, 3,3'-dimethyl-4-methoxybenzophenone, polyvinylbenzophenone, α-hydroxycyclohexyl phenyl ketone, and the like.
[0074] Ketal-based photopolymerization initiators include benzyl dimethyl ketal and the like.
[0075] Examples of thioxanthone-based photopolymerization initiators include thioxanthone, 2-chlorothioxanthone, 2-methylthioxanthone, 2,4-dimethylthioxanthone, isopropylthioxanthone, 2,4-dichlorothioxanthone, 2,4-diethylthioxanthone, 2,4-diisopropylthioxanthone, and dodecylthioxanthone.
[0076] Examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, and the like.
[0077] The photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm can be used alone or in combination of two or more kinds. The photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm can be added within a range that does not impair the effects of the present invention, and the amount added is preferably about 0.005 to 0.5 parts by weight, more preferably about 0.02 to 0.1 parts by weight, relative to 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer.
[0078] In the present invention, when the monomer components are polymerized by ultraviolet light, it is preferable to first add a photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm to the monomer components, and then add a photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more and an ultraviolet absorber to a partial polymer (prepolymer composition) of the monomer components partially polymerized by ultraviolet light irradiation, and then polymerize the monomer components by ultraviolet light. When adding the photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more to a partial polymer (prepolymer composition) of the monomer components partially polymerized by ultraviolet light irradiation, it is preferable to add the photopolymerization initiator after dissolving it in the monomer.
[0079] (1-2) Ultraviolet absorbers The ultraviolet absorber contained in the acrylic adhesive composition is not particularly limited, but examples thereof include triazine-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, oxybenzophenone-based ultraviolet absorbers, salicylic acid ester-based ultraviolet absorbers, and cyanoacrylate-based ultraviolet absorbers, and these can be used alone or in combination of two or more. Among these, triazine-based ultraviolet absorbers and benzotriazole-based ultraviolet absorbers are preferred, and at least one ultraviolet absorber selected from the group consisting of triazine-based ultraviolet absorbers having two or less hydroxyl groups in one molecule and benzotriazole-based ultraviolet absorbers having one benzotriazole skeleton in one molecule is preferred because it has good solubility in the monomer used to form the acrylic adhesive composition and has high ultraviolet absorption ability at a wavelength of around 380 nm.
[0080] Specific examples of triazine-based ultraviolet absorbers having two or less hydroxyl groups in one molecule include 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (Tinosorb S, manufactured by BASF), 2,4-bis[2-hydroxy-4-butoxyphenyl]-6-(2,4-dibutoxyphenyl)-1,3,5-triazine (TINUVIN 460, manufactured by BASF), 2-(4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl)-5-hydroxyphenyl and [(C10-C16 (mainly C12-C13) alkyloxy)methyl]oxirane reaction products (TINUVIN400, manufactured by BASF), 2-[4,6-bis(2,4-dimethylphenyl)-1,3,5-triazin-2-yl]-5-[3-(dodecyloxy)-2-hydroxypropoxy]phenol), 2-(2,4-dihydroxyf Examples of such phenols include the reaction product of 2-(4,6-diphenyl-1,3,5-triazine and (2-ethylhexyl)-glycidic acid ester (TINUVIN 405, manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[(hexyl)oxy]-phenol (TINUVIN 1577, manufactured by BASF), 2-(4,6-diphenyl-1,3,5-triazin-2-yl)-5-[2-(2-ethylhexanoyloxy)ethoxy]-phenol (ADK STAB LA46, manufactured by ADEKA), and 2-(2-hydroxy-4-[1-octyloxycarbonylethoxy]phenyl)-4,6-bis(4-phenylphenyl)-1,3,5-triazine (TINUVIN 479, manufactured by BASF).
[0081] Benzotriazole-based UV absorbers having one benzotriazole skeleton per molecule include 2-(2H-benzotriazole-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol (TINUVIN 928, manufactured by BASF), 2-(2-hydroxy-5-tert-butylphenyl)-2H-benzotriazole (TINUVIN PS, manufactured by BASF), ester compound of benzenepropanoic acid and 3-(2H-benzotriazole-2-yl)-5-(1,1-dimethylethyl)-4-hydroxy (C7-9 side chain and linear alkyl) (TINUVIN 384-2, manufactured by BASF), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (TINUVIN 900, manufactured by BASF), 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (TINUVIN 900, manufactured by BASF), and 2-(2H-benzotriazole-2-yl)-4,6-bis(1-methyl-1-phenylethyl)phenol (TINUVIN 900, manufactured by BASF). methyl-3-(3-(2H-benzotriazol-2-yl)-5-t-butyl-4-hydroxyphenyl)propionate / polyethylene glycol 300 reaction product (TINUVIN 1130, BASF), 2-(2H-benzotriazol-2-yl)-p-cresol (TINUVIN P, manufactured by BASF), 2(2H-benzotriazol-2-yl)-4-6-bis(1-methyl-1-phenylethyl)phenol (TINUVIN234, manufactured by BASF), 2-[5-chloro(2H)-benzotriazol-2-yl]-4-methyl-6-(tert-butyl)phenol (TINUVIN326, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4,6-di-tert-pentylphenol (TINUVIN328, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-4-(1,1,3,Examples of the 2-hydroxy-3-(3,4,5,6-tetrahydrophthalimido-methyl)-4-hydroxyphenyl)phenol include 3-(tetramethylbutyl)phenol (TINUVIN 329, manufactured by BASF), a reaction product of methyl 3-(3-(2H-benzotriazol-2-yl)-5-tert-butyl-4-hydroxyphenyl)propionate and polyethylene glycol 300 (TINUVIN 213, manufactured by BASF), 2-(2H-benzotriazol-2-yl)-6-dodecyl-4-methylphenol (TINUVIN 571, manufactured by BASF), and 2-[2-hydroxy-3-(3,4,5,6-tetrahydrophthalimido-methyl)-5-methylphenyl]benzotriazole (Sumisorb 250, manufactured by Sumitomo Chemical Co., Ltd.).
[0082] Furthermore, examples of the benzophenone-based ultraviolet absorbers (benzophenone-based compounds) and oxybenzophenone-based ultraviolet absorbers (oxybenzophenone-based compounds) include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxybenzophenone, 2-hydroxy-4-methoxybenzophenone-5-sulfonic acid (anhydrous and trihydrate), 2-hydroxy-4-octyloxybenzophenone, 4-dodecyloxy-2-hydroxybenzophenone, 4-benzyloxy-2-hydroxybenzophenone, 2,2',4,4'-tetrahydroxybenzophenone, and 2,2'-dihydroxy-4,4-dimethoxybenzophenone.
[0083] Examples of the salicylic acid ester-based ultraviolet absorbers (salicylic acid ester-based compounds) include phenyl-2-acryloyloxybenzoate, phenyl-2-acryloyloxy-3-methylbenzoate, phenyl-2-acryloyloxy-4-methylbenzoate, phenyl-2-acryloyloxy-5-methylbenzoate, phenyl-2-acryloyloxy-3-methoxybenzoate, phenyl-2-hydroxybenzoate, phenyl-2-hydroxy-3-methylbenzoate, phenyl-2-hydroxy-4-methylbenzoate, phenyl-2-hydroxy-5-methylbenzoate, phenyl-2-hydroxy-3-methoxybenzoate, and 2,4-di-tert-butylphenyl-3,5-di-tert-butyl-4-hydroxybenzoate (TINUVIN120, manufactured by BASF).
[0084] Examples of the cyanoacrylate-based ultraviolet absorber (cyanoacrylate-based compound) include alkyl-2-cyanoacrylate, cycloalkyl-2-cyanoacrylate, alkoxyalkyl-2-cyanoacrylate, alkenyl-2-cyanoacrylate, and alkynyl-2-cyanoacrylate.
[0085] In addition, as the ultraviolet absorber, for example, dyes such as the trade name "FDB-001" (manufactured by Yamada Chemical Industry Co., Ltd.), the trade name "SMP-122" (manufactured by Hayashibara Co., Ltd.), an azomethine compound (trade name: BONASORB UA-3911, manufactured by Orient Chemical Industry Co., Ltd.), an indole chemical (trade name: BONASORB UA-3701, manufactured by Orient Chemical Industry Co., Ltd.), Disperse Yellow 54 (trade name: KAYASET YELLOW AG, manufactured by Nippon Kayaku Co., Ltd.), a quinophthalone compound (trade name: MS YELLOW HD-137, manufactured by Yamada Chemical Industry Co., Ltd.), Solvent Yellow 93 (PLASTYELLOW 8000, manufactured by Arimoto Chemical Industry Co., Ltd.), and Solvent Yellow 163 (KP Plast Yellow MK, manufactured by Kiwa Chemical Industry Co., Ltd.) can also be used.
[0086] The ultraviolet absorbent may be used alone or in combination of two or more kinds, but the total content is preferably about 0.1 to 5 parts by weight, more preferably about 0.5 to 3 parts by weight, based on 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer. By setting the amount of ultraviolet absorbent added within the above range, the ultraviolet absorbing function of the pressure-sensitive adhesive layer can be fully exhibited, and when ultraviolet polymerization is performed, it is preferable because the polymerization is not hindered.
[0087] (1-3) Silane coupling agents Furthermore, the acrylic pressure-sensitive adhesive composition used in the present invention may contain a silane coupling agent. The amount of the silane coupling agent is preferably 1 part by weight or less, more preferably 0.01 to 1 part by weight, and even more preferably 0.02 to 0.6 parts by weight, based on 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer.
[0088] Examples of the silane coupling agent include epoxy group-containing silane coupling agents such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; amino group-containing silane coupling agents such as 3-aminopropyltrimethoxysilane, N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-triethoxysilyl-N-(1,3-dimethylbutylidene)propylamine, and N-phenyl-γ-aminopropyltrimethoxysilane; (meth)acrylic group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane and 3-methacryloxypropyltriethoxysilane; and isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane.
[0089] (1-4) Crosslinking agent The acrylic adhesive composition used in the present invention may contain a crosslinking agent. Examples of the crosslinking agent include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, silicone-based crosslinking agents, oxazoline-based crosslinking agents, aziridine-based crosslinking agents, silane-based crosslinking agents, alkyl etherified melamine-based crosslinking agents, metal chelate-based crosslinking agents, and peroxide-based crosslinking agents. The crosslinking agents may be used alone or in combination of two or more. Among these, isocyanate-based crosslinking agents are preferably used.
[0090] The above crosslinking agents may be used alone or in combination of two or more. The total content is preferably 5 parts by weight or less, more preferably 0.01 to 5 parts by weight, even more preferably 0.01 to 4 parts by weight, and particularly preferably 0.02 to 3 parts by weight, relative to 100 parts by weight of the monofunctional monomer component forming the (meth)acrylic polymer.
[0091] An isocyanate crosslinking agent refers to a compound having two or more isocyanate groups (including isocyanate regenerating functional groups in which the isocyanate groups are temporarily protected by a blocking agent or oligomerization, etc.) in one molecule. Examples of the isocyanate crosslinking agent include aromatic isocyanates such as tolylene diisocyanate and xylylene diisocyanate, alicyclic isocyanates such as isophorone diisocyanate, and aliphatic isocyanates such as hexamethylene diisocyanate.
[0092] More specifically, for example, lower aliphatic polyisocyanates such as butylene diisocyanate and hexamethylene diisocyanate, alicyclic isocyanates such as cyclopentylene diisocyanate, cyclohexylene diisocyanate and isophorone diisocyanate, aromatic diisocyanates such as 2,4-tolylene diisocyanate, 4,4'-diphenylmethane diisocyanate, xylylene diisocyanate and polymethylene polyphenyl isocyanate, trimethylolpropane / tolylene diisocyanate trimer adduct (product name: Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.), trimethylolpropane / hexamethylene diisocyanate trimer adduct (product name: Examples of such polyisocyanates include isocyanate adducts such as Coronate HL, manufactured by Nippon Polyurethane Industry Co., Ltd., and an isocyanurate of hexamethylene diisocyanate (trade name: Coronate HX, manufactured by Nippon Polyurethane Industry Co., Ltd.), a trimethylolpropane adduct of xylylene diisocyanate (trade name: D110N, manufactured by Mitsui Chemicals, Inc.), and a trimethylolpropane adduct of hexamethylene diisocyanate (trade name: D160N, manufactured by Mitsui Chemicals, Inc.); polyether polyisocyanates, polyester polyisocyanates, and adducts of these with various polyols, and polyisocyanates that have been multifunctionalized with an isocyanurate bond, a biuret bond, an allophanate bond, or the like.
[0093] (1-5) Other additives In addition to the above components, the acrylic adhesive composition used in the present invention may contain appropriate additives depending on the application, such as tackifiers (e.g., rosin derivative resins, polyterpene resins, petroleum resins, oil-soluble phenolic resins, etc., which are solid, semi-solid, or liquid at room temperature); fillers such as hollow glass balloons; plasticizers; antioxidants; antioxidants; and the like.
[0094] (1-6) Method for forming visible side adhesive layer In the present invention, the acrylic pressure-sensitive adhesive composition is preferably adjusted to a viscosity suitable for application on a substrate. The viscosity of the acrylic pressure-sensitive adhesive composition is adjusted, for example, by adding various polymers such as thickening additives, polyfunctional monomers, etc., or by partially polymerizing the monomer components in the acrylic pressure-sensitive adhesive composition. The partial polymerization may be performed before or after adding various polymers such as thickening additives, polyfunctional monomers, etc. The viscosity of the acrylic pressure-sensitive adhesive composition varies depending on the amount of additives, etc., so the polymerization rate when the monomer components in the acrylic pressure-sensitive adhesive composition are partially polymerized cannot be uniquely determined, but as a guideline, it is preferably about 20% or less, more preferably about 3 to 20%, and even more preferably about 5 to 15%. If it exceeds 20%, the viscosity becomes too high, making it difficult to apply to a substrate.
[0095] The viewing-side pressure-sensitive adhesive layer can be formed by applying the acrylic pressure-sensitive adhesive composition to at least one surface of a substrate and drying a coating film formed from the acrylic pressure-sensitive adhesive composition, or by irradiating the coating film with active energy rays such as ultraviolet rays.
[0096] The substrate is not particularly limited, and for example, various substrates such as a release film, a transparent resin film substrate, and a polarizing film described later can be suitably used as the substrate. When the visible-side pressure-sensitive adhesive layer is formed on a substrate other than a polarizing film, the visible-side pressure-sensitive adhesive layer can be transferred by being attached to the polarizing film.
[0097] Examples of the material constituting the release film include resin films such as polyethylene, polypropylene, polyethylene terephthalate, and polyester films; porous materials such as paper, cloth, and nonwoven fabrics; nets, foam sheets, metal foils, and appropriate thin sheets such as laminates thereof. Among these, resin films are preferably used because of their excellent surface smoothness.
[0098] Examples of the resin film include polyethylene film, polypropylene film, polybutene film, polybutadiene film, polymethylpentene film, polyvinyl chloride film, vinyl chloride copolymer film, polyethylene terephthalate film, polybutylene terephthalate film, polyurethane film, and ethylene-vinyl acetate copolymer film.
[0099] The thickness of the release film is usually 5 to 200 μm, and preferably about 5 to 100 μm. The release film may be subjected to a release and antifouling treatment using a silicone-based, fluorine-based, long-chain alkyl-based or fatty acid amide-based release agent, silica powder, or the like, or an antistatic treatment such as a coating type, kneading type, or deposition type. In particular, by appropriately performing a release treatment such as a silicone treatment, a long-chain alkyl treatment, or a fluorine treatment on the surface of the release film, the releasability from the pressure-sensitive adhesive layer can be further improved.
[0100] The transparent resin film substrate is not particularly limited, and various resin films having transparency are used. The resin film is formed of a single layer film. For example, the material thereof may be polyester-based resins such as polyethylene terephthalate and polyethylene naphthalate, acetate-based resins, polyethersulfone-based resins, polycarbonate-based resins, polyamide-based resins, polyimide-based resins, polyolefin-based resins, (meth)acrylic-based resins, polyvinyl chloride-based resins, polyvinylidene chloride-based resins, polystyrene-based resins, polyvinyl alcohol-based resins, polyarylate-based resins, polyphenylene sulfide-based resins, etc. Among these, polyester-based resins, polyimide-based resins, and polyethersulfone-based resins are particularly preferred.
[0101] The thickness of the film substrate is preferably from 15 to 200 μm, and more preferably from 25 to 188 μm.
[0102] The method for applying the acrylic pressure-sensitive adhesive composition onto the substrate is not particularly limited, and any suitable known method can be used, such as roll coating, kiss roll coating, gravure coating, reverse coating, roll brush, spray coating, dip roll coating, bar coating, knife coating, air knife coating, curtain coating, lip coating, or die coating.
[0103] When the visible-side pressure-sensitive adhesive layer is formed by drying a coating film formed from the acrylic pressure-sensitive adhesive composition, the drying conditions (temperature, time) are not particularly limited and can be appropriately set depending on the composition, concentration, etc. of the pressure-sensitive adhesive composition. For example, the drying conditions are about 60 to 170° C., preferably 60 to 150° C., for 1 to 60 minutes, preferably 2 to 30 minutes.
[0104] When the acrylic pressure-sensitive adhesive composition is an ultraviolet-curable acrylic pressure-sensitive adhesive composition and a coating film formed from the ultraviolet-curable acrylic pressure-sensitive adhesive composition is irradiated with ultraviolet light, the illuminance of the irradiated ultraviolet light is 5 mW / cm 2 The illuminance of the ultraviolet light is preferably 5 mW / cm or more. 2 If the ultraviolet ray is less than 200 mW / cm2, the polymerization reaction time will be long, and the productivity may be poor. 2 The illuminance of the ultraviolet light is preferably 200 mW / cm or less. 2 If the dose exceeds 100 mJ / cm, the photopolymerization initiator is consumed rapidly, causing the polymer to have a low molecular weight and reducing its holding power, especially at high temperatures. 2 ~5000mJ / cm 2 It is preferable that:
[0105] The ultraviolet lamp used in the present invention is not particularly limited, but an LED lamp is preferable. Since an LED lamp emits less heat than other ultraviolet lamps, the temperature during polymerization of the adhesive layer can be suppressed. Therefore, it is possible to prevent the polymer from being depolymerized, prevent the cohesive strength of the adhesive layer from decreasing, and increase the holding power at high temperatures when the adhesive layer is made into an adhesive sheet. It is also possible to combine multiple ultraviolet lamps. It is also possible to irradiate ultraviolet rays intermittently, and provide a light period in which ultraviolet rays are irradiated and a dark period in which ultraviolet rays are not irradiated.
[0106] In the present invention, the final polymerization rate of the monomer components in the ultraviolet-curable acrylic pressure-sensitive adhesive composition is preferably 90% or more, more preferably 95% or more, and even more preferably 98% or more.
[0107] In the present invention, the peak wavelength of the ultraviolet light irradiated to the ultraviolet-curable acrylic pressure-sensitive adhesive composition is preferably within the range of 200 to 500 nm, more preferably within the range of 300 to 450 nm. If the peak wavelength of the ultraviolet light exceeds 500 nm, the photopolymerization initiator may not be decomposed, and the polymerization reaction may not start. If the peak wavelength of the ultraviolet light is less than 200 nm, the polymer chain may be cut, and the adhesive properties may be reduced.
[0108] Since the reaction is inhibited by oxygen in the air, it is preferable to form a release film or the like on the coating film formed from the ultraviolet-curable acrylic pressure-sensitive adhesive composition, or to carry out the photopolymerization reaction under a nitrogen atmosphere, in order to block oxygen. Examples of the release film include those mentioned above. When a release film is used, the release film can be used as it is as a separator for the polarizing film with the pressure-sensitive adhesive layer.
[0109] In addition, when the ultraviolet-curable acrylic pressure-sensitive adhesive composition used in the present invention contains a photopolymerization initiator (B), it is preferable to irradiate a composition containing a monomer component containing an alkyl (meth)acrylate and the photopolymerization initiator (B) (sometimes referred to as a "pre-added polymerization initiator") with ultraviolet light to form a partial polymer of the monomer component, and to add an ultraviolet absorber and a photopolymerization initiator (A) (sometimes referred to as a "post-added polymerization initiator") having an absorption band at a wavelength of 400 nm or more to the partial polymer of the monomer component to prepare an ultraviolet-curable acrylic pressure-sensitive adhesive composition. The polymerization rate of the partial polymer is preferably about 20% or less, more preferably about 3 to 20%, and even more preferably about 5 to 15%. The ultraviolet irradiation conditions are as described above.
[0110] As described above, when a pressure-sensitive adhesive layer is formed from an ultraviolet-curable acrylic pressure-sensitive adhesive composition containing a photopolymerization initiator (B), the polymerization rate of the monomer components can be increased by carrying out the polymerization in two steps as described above, and the ultraviolet absorbing function of the finally produced pressure-sensitive adhesive layer can be improved.
[0111] From the viewpoint of ensuring ultraviolet absorbing function, the thickness of the viewer-side adhesive layer is preferably at least twice, more preferably at least five times, and even more preferably at least ten times, the thickness of the adhesive layer on the image display section side of the polarizing film described later (image display section side adhesive layer). Specifically, the thickness of the viewer-side adhesive layer is preferably at least 50 μm, more preferably at least 100 μm, and even more preferably at least 150 μm. The upper limit of the thickness of the viewer-side adhesive layer is not particularly limited, but is preferably 10 mm or less. If the thickness of the adhesive layer exceeds 10 mm, ultraviolet light transmission becomes difficult, polymerization of the monomer component takes a long time, and productivity may be poor, which is not preferable.
[0112] The gel fraction of the pressure-sensitive adhesive layer on the viewing side of the present invention is not particularly limited, but is preferably 35% or more, more preferably 50% or more, even more preferably 75% or more, and particularly preferably 85% or more. If the gel fraction of the pressure-sensitive adhesive layer on the viewing side is small, the cohesive strength may be poor, and if it is too large, the adhesive strength may be poor.
[0113] The transmission b* value of the viewing-side pressure-sensitive adhesive layer is not particularly limited, but is preferably 3.0 or less, more preferably 1.5 or less, and even more preferably 0.5 or less. The b* value refers to the b* value (chromaticity) in the L*a*b* color system in accordance with JIS Z8729, and can be measured, for example, using a spectrophotometer (product name: U4100, manufactured by Hitachi High-Technologies Corporation).
[0114] The transmittance of the viewing-side pressure-sensitive adhesive layer at a wavelength of 380 nm is preferably 9% or less, more preferably 7% or less, even more preferably 5% or less, and particularly preferably 3% or less. When the transmittance at a wavelength of 380 nm is in the above range, incident ultraviolet light can be blocked to a higher degree, and deterioration of optical members such as liquid crystal panels, organic EL elements, polarizers, etc. can be significantly suppressed.
[0115] The transmittance of the viewing-side pressure-sensitive adhesive layer at a wavelength of 400 nm is preferably 60% or more, more preferably 70% or more, and more preferably 75% or more. When the transmittance at a wavelength of 400 nm is in the above range, incident visible light can be sufficiently transmitted, and sufficient visibility can be ensured in an image display device, which is preferable.
[0116] In addition, when the pressure-sensitive adhesive layer-attached polarizing film of the present invention is used in an organic electroluminescence display device (OLED), the transmittance of the viewing-side pressure-sensitive adhesive layer at a wavelength of 420 nm is preferably 75% or less, more preferably 50% or less, and even more preferably 40% or less. The transmittance at a wavelength of 420 nm being in the above range is preferable from the viewpoint of protecting the light-emitting element of the OLED.
[0117] When the viewing side pressure-sensitive adhesive layer is exposed, the pressure-sensitive adhesive layer may be protected with a release film until it is put to practical use. The release film can be used as a separator for the pressure-sensitive adhesive layer-attached polarizing film as it is, which can simplify the process.
[0118] (2) Adhesive layer on the image display side The adhesive layer on the image display section side surface of the polarizing film (image display section side adhesive layer) is not particularly limited, and may be the same as the acrylic adhesive composition described in detail for the viewing side adhesive layer, or any of various commonly used adhesive layers.
[0119] The adhesive layer on the image display unit side surface can be formed using an appropriate adhesive, and there is no particular restriction on the type. Examples of the adhesive include rubber-based adhesives, acrylic-based adhesives, silicone-based adhesives, urethane-based adhesives, vinyl alkyl ether-based adhesives, polyvinyl alcohol-based adhesives, polyvinyl pyrrolidone-based adhesives, polyacrylamide-based adhesives, and cellulose-based adhesives. Among these adhesives, acrylic-based adhesives are preferably used because they have excellent optical transparency, exhibit appropriate adhesive properties such as adhesion, cohesion, and adhesion, and are excellent in weather resistance and heat resistance.
[0120] The acrylic adhesive has an acrylic polymer having a monomer unit of (meth)acrylic acid alkyl ester as a main skeleton as a base polymer. The (meth)acrylic acid alkyl ester constituting the main skeleton of the acrylic polymer may be the same as that used in the acrylic adhesive composition forming the visible side adhesive layer. The copolymerization monomer and its ratio may be the same as that used in the acrylic adhesive composition.
[0121] The acrylic polymer can be produced by various known methods, and for example, radical polymerization methods such as bulk polymerization, solution polymerization, and suspension polymerization can be appropriately selected. As the radical polymerization initiator, various known azo-based and peroxide-based initiators can be used. The reaction temperature is usually about 50 to 80°C, and the reaction time is 1 to 8 hours. Among the above production methods, the solution polymerization method is preferable, and ethyl acetate, toluene, etc. are generally used as the solvent for the acrylic polymer. The solution concentration is usually about 20 to 80% by weight.
[0122] The pressure-sensitive adhesive may be a pressure-sensitive adhesive composition containing a crosslinking agent. Examples of the crosslinking agent include those mentioned above, but isocyanate-based crosslinking agents are particularly preferred. The blending ratio of the acrylic polymer and the crosslinking agent is not particularly limited, but in general, the crosslinking agent (solid content) is preferably about 0.001 to 20 parts by weight, more preferably about 0.01 to 15 parts by weight, per 100 parts by weight of the acrylic polymer (solid content).
[0123] Furthermore, the adhesive may contain, as necessary, tackifiers, plasticizers, fillers made of glass fibers, glass beads, metal powders, other inorganic powders, pigments, colorants, fillers, antioxidants, ultraviolet absorbers, silane coupling agents, etc., and may also contain various additives within the scope of the present invention.Also, the adhesive layer may contain fine particles and exhibit light diffusion properties.As the silane coupling agent, the above-mentioned ones may be mentioned.
[0124] The image display unit side pressure-sensitive adhesive layer is formed by applying the pressure-sensitive adhesive composition to various substrates such as a polarizing film or a release film, and drying the composition. When the pressure-sensitive adhesive layer is formed on various substrates such as a release film, the pressure-sensitive adhesive layer can be transferred by being attached to a polarizing film. The pressure-sensitive adhesive application method and the various substrates can be the same as those of the acrylic pressure-sensitive adhesive composition application method and the various substrates.
[0125] In the coating step, the coating amount is controlled so that the formed adhesive layer has a predetermined thickness (thickness after drying). The thickness of the image display section side adhesive layer is not particularly limited, but is preferably 1 / 2 or less, more preferably 1 / 5 or less, and more preferably 1 / 10 or less of the thickness of the viewing side adhesive layer. Specifically, the thickness of the image display section side adhesive layer is preferably about 1 to 100 μm, more preferably about 3 to 50 μm, and even more preferably about 5 to 30 μm.
[0126] When forming the image display unit side pressure-sensitive adhesive layer, the applied pressure-sensitive adhesive is dried. The drying temperature and drying time are not particularly limited and may be appropriately set, but are preferably, for example, about 80 to 200° C. and 0.5 to 10 minutes.
[0127] When the pressure-sensitive adhesive layer on the image display section side is exposed, the pressure-sensitive adhesive layer may be protected with a release film until it is put to practical use. The release film can be used as it is as a separator for the pressure-sensitive adhesive layer-attached polarizing film, which can simplify the process.
[0128] (3) Polarizing film The polarizing film used in the present invention has a polarizer and transparent protective films on both sides of the polarizer, and is characterized in that the transparent protective film on the viewing side of the polarizer (viewing-side transparent protective film) has a transmittance of less than 6% at a wavelength of 380 nm.
[0129] (3-1) Transparent protective film on the viewing side The transmittance of the visible-side transparent protective film used in the present invention at a wavelength of 380 nm is less than 6%, preferably 3% or less, more preferably 2% or less, and even more preferably 1% or less. In the present invention, by combining the visible-side transparent protective film having a transmittance of less than 6% at a wavelength of 380 nm with the visible-side pressure-sensitive adhesive layer (containing an ultraviolet absorber), a higher level of ultraviolet absorption ability can be achieved. In addition, the lower limit of the transmittance of the visible-side transparent protective film at a wavelength of 380 nm is not particularly limited, and the smaller the transmittance, the more preferable it is from the viewpoint of ultraviolet absorption function.
[0130] The material for forming the visible-side transparent protective film is preferably one having excellent transparency, mechanical strength, thermal stability, moisture barrier properties, isotropy, etc. Examples of the material include polyester-based polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose-based polymers such as diacetyl cellulose and triacetyl cellulose, acrylic polymers such as polymethyl methacrylate, styrene-based polymers such as polystyrene and acrylonitrile-styrene copolymers (AS resins), polycarbonate-based polymers, etc. In addition, examples of the polymer for forming the transparent protective film include polyethylene, polypropylene, polyolefins having a cyclo- or norbornene structure, polyolefin-based polymers such as ethylene-propylene copolymers, vinyl chloride-based polymers, amide-based polymers such as nylon and aromatic polyamide, imide-based polymers, sulfone-based polymers, polyethersulfone-based polymers, polyetheretherketone-based polymers, polyphenylene sulfide-based polymers, vinyl alcohol-based polymers, vinylidene chloride-based polymers, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, epoxy-based polymers, and blends of the above polymers. The transparent protective film can also be formed as a cured layer of a thermosetting or ultraviolet curing resin such as an acrylic, urethane, acrylic urethane, epoxy, silicone, etc. Among these, the viewing-side transparent protective film is preferably at least one film selected from the group consisting of a triacetyl cellulose film, an acrylic film (a film using an acrylic polymer), a polyethylene terephthalate film, and a polyolefin film having a cyclo- or norbornene structure, and more preferably a triacetyl cellulose film.
[0131] The thickness of the viewer-side transparent protective film is not particularly limited, but is preferably 40 μm or less, more preferably 35 μm or less, and even more preferably 30 μm or less. The lower limit of the thickness of the viewer-side transparent protective film is not particularly limited, but is preferably 1 μm or more. When the thickness of the viewer-side transparent protective film is in the above range, it is preferable because the polarizing film can be sufficiently thinned and the protective function of the polarizer is not impaired.
[0132] The polarizer and the viewing-side protective film described below are preferably adhered to each other via a water-based adhesive or the like. Examples of the water-based adhesive include isocyanate-based adhesives, polyvinyl alcohol-based adhesives, gelatin-based adhesives, vinyl-based latex-based adhesives, water-based polyurethanes, water-based polyesters, and the like. In addition to the above, examples of the adhesive between the polarizer and the viewing-side transparent protective film include ultraviolet-curing adhesives and electron beam-curing adhesives. The electron beam-curing polarizing film adhesive shows suitable adhesion to the above-mentioned various viewing-side transparent protective films. The adhesive used in the present invention may contain a metal compound filler.
[0133] The surface of the viewer-side transparent protective film to which the polarizer is not attached may be provided with a hard coat layer, anti-reflection treatment, anti-sticking treatment, or treatment for diffusing or anti-glare.
[0134] (3-2) Polarizer The polarizer is not particularly limited, and various polarizers can be used. Examples of polarizers include hydrophilic polymer films such as polyvinyl alcohol films, partially formalized polyvinyl alcohol films, and partially saponified ethylene-vinyl acetate copolymer films, which are uniaxially stretched after adsorbing a dichroic substance such as iodine or a dichroic dye, and polyene-based oriented films such as dehydrated polyvinyl alcohol and dehydrochlorinated polyvinyl chloride. Among these, polarizers made of a polyvinyl alcohol film and a dichroic substance such as iodine are suitable. The thickness of these polarizers is not particularly limited, but is generally about 5 to 80 μm.
[0135] A polarizer obtained by dyeing a polyvinyl alcohol-based film with iodine and stretching it uniaxially can be produced, for example, by immersing polyvinyl alcohol in an aqueous solution of iodine to dye it and stretching it to 3 to 7 times its original length. If necessary, it can also be immersed in an aqueous solution of potassium iodide or the like which may contain boric acid, zinc sulfate, zinc chloride, or the like. Furthermore, if necessary, the polyvinyl alcohol-based film can be immersed in water and washed before dyeing. Washing the polyvinyl alcohol-based film with water can wash off dirt and blocking inhibitors on the surface of the polyvinyl alcohol-based film, and also has the effect of preventing unevenness such as uneven dyeing by swelling the polyvinyl alcohol-based film. Stretching may be performed after dyeing with iodine, or may be stretched while dyeing, or may be dyed with iodine after stretching. Stretching can be performed in an aqueous solution of boric acid, potassium iodide, or the like, or in a water bath.
[0136] In the present invention, a thin polarizer having a thickness of 10 μm or less can also be used. From the viewpoint of thinning, the thickness is preferably 1 to 7 μm. Such a thin polarizer has less thickness unevenness, excellent visibility, and excellent durability due to less dimensional change, and is also preferable in that the thickness of the polarizing film can be reduced.
[0137] Representative examples of the thin polarizer include the thin polarizing films described in JP-A-51-069644, JP-A-2000-338329, WO-A-2010 / 100917, WO-A-2010 / 100917, or Japanese Patent No. 4751481 and JP-A-2012-073563. These thin polarizing films can be obtained by a manufacturing method including a step of stretching a polyvinyl alcohol-based resin (hereinafter also referred to as PVA-based resin) layer and a resin substrate for stretching in a laminated state, and a step of dyeing. With this manufacturing method, even if the PVA-based resin layer is thin, it can be stretched without problems such as breakage due to stretching because it is supported by the resin substrate for stretching.
[0138] As the thin polarizing film, among the production methods including a step of stretching and a step of dyeing a laminate, those obtained by a production method including a step of stretching in an aqueous boric acid solution as described in WO 2010 / 100917, WO 2010 / 100917, Japanese Patent No. 4751481, and JP-A 2012-073563 are preferred, in that they can be stretched at a high ratio and have improved polarization performance, and in particular those obtained by a production method including a step of auxiliary in-air stretching before stretching in an aqueous boric acid solution as described in Japanese Patent No. 4751481 and JP-A 2012-073563 are preferred.
[0139] (3-3) Transparent protective film on the image display side The image display side transparent protective film may be any of those conventionally used. Specifically, a transparent protective film formed from a material having excellent transparency, mechanical strength, thermal stability, moisture blocking properties, isotropy, etc. is preferred, and examples thereof include polyester polymers such as polyethylene terephthalate and polyethylene naphthalate, cellulose polymers such as diacetyl cellulose and triacetyl cellulose, acrylic polymers such as polymethyl methacrylate, styrene polymers such as polystyrene and acrylonitrile-styrene copolymer (AS resin), polycarbonate polymers, etc. Examples of the polymer forming the transparent protective film include polyethylene, polypropylene, polyolefins having a cyclo- or norbornene structure, polyolefin-based polymers such as ethylene-propylene copolymers, vinyl chloride-based polymers, amide-based polymers such as nylon and aromatic polyamides, imide-based polymers, sulfone-based polymers, polyethersulfone-based polymers, polyetheretherketone-based polymers, polyphenylene sulfide-based polymers, vinyl alcohol-based polymers, vinylidene chloride-based polymers, vinyl butyral-based polymers, arylate-based polymers, polyoxymethylene-based polymers, epoxy-based polymers, and blends of the above polymers. The transparent protective film can also be formed as a cured layer of a thermosetting or ultraviolet-curing resin such as an acrylic, urethane, acrylic urethane, epoxy, or silicone.
[0140] The thickness of the image display unit side protective film can be appropriately determined, but is generally about 1 to 500 μm in terms of strength, workability such as handleability, thinness, and the like.
[0141] The polarizer and the transparent protective film on the image display section side are also usually adhered to each other via a water-based adhesive, etc. Examples of the water-based adhesive include those mentioned above.
[0142] The surface of the transparent protective film on the image display portion side to which the polarizer is not attached may be provided with a hard coat layer, anti-reflection treatment, anti-sticking treatment, or treatment for diffusion or anti-glare purposes.
[0143] 2. Image display device The image display device of the present invention is characterized by using the pressure-sensitive adhesive layer-attached polarizing film of the present invention.
[0144] As an example of a specific configuration of the image display device, for example, as shown in FIG. 2 to FIG. 4, a cover glass or cover plastic 6 / visual side adhesive layer 2a / visual side transparent protective film 3a / polarizer 4 / image display unit side transparent protective film 3b / image display unit side adhesive layer 2b / liquid crystal display device (LCD) or organic EL display device (OLED) 7 (FIG. 2); cover glass or cover plastic 6 / adhesive layer 8a / sensor layer 9 / visual side adhesive layer 2a / visual side transparent protective film 3a / polarizer 4 / image display unit side transparent protective film Examples of image displays in which the layers are laminated in this order include: cover glass or cover plastic 6 / adhesive layer 8a / sensor layer 9 / adhesive layer 8b / sensor layer 9 / visible-side adhesive layer 2a / visible-side transparent protective film 3a / polarizer 4 / image-display-part-side transparent protective film 3b / image-display-part-side adhesive layer 2b / liquid crystal display device (LCD) or organic electroluminescence display device (OLED) 7 (FIG. 3); cover glass or cover plastic 6 / adhesive layer 8a / sensor layer 9 / adhesive layer 8b / sensor layer 9 / visible-side adhesive layer 2a / visible-side transparent protective film 3a / polarizer 4 / image-display-part-side transparent protective film 3b / image-display-part-side adhesive layer 2b / liquid crystal display device (LCD) or organic electroluminescence display device (OLED) 7 (FIG. 4). The adhesive layer-attached polarizing film 1 of the present invention refers to the portion of "visible-side adhesive layer 2a / visible-side transparent protective film 3a / polarizer 4 / image-display-part-side transparent protective film 3b / image-display-part-side adhesive layer 2b" in the above-mentioned configuration, and may also include a retardation film and the like in addition to these. In addition, when a retardation film is included, specifically, a pressure-sensitive adhesive layer can be laminated between the image display unit side pressure-sensitive adhesive layer 2b and a liquid crystal display device (LCD) or an organic electroluminescence display device (OLED) 7. In addition, a pressure-sensitive adhesive layer and / or an adhesive layer can be appropriately used in laminating each layer.
[0145] Examples of image display devices include liquid crystal display devices, organic EL (electroluminescence) display devices, PDPs (plasma display panels), electronic paper, and the like. Among these, liquid crystal display devices and organic EL (electroluminescence) display devices having the above-mentioned configurations are preferred. EXAMPLES
[0146] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In each example, parts and percentages are all by weight.
[0147] Production Example 1 (Production of Acrylic Pressure Sensitive Adhesive Composition (a-1)) A monomer mixture consisting of 78 parts by weight of 2-ethylhexyl acrylate (2EHA), 18 parts by weight of N-vinyl-2-pyrrolidone (NVP), and 4 parts by weight of 2-hydroxyethyl acrylate (HEA) was mixed with 0.035 parts by weight of 1-hydroxycyclohexyl phenyl ketone (product name: Irgacure 184, having an absorption band at wavelengths of 200 to 370 nm, manufactured by BASF) and 0.035 parts by weight of 2,2-dimethoxy-1,2-diphenylethan-1-one (product name: Irgacure 651, having an absorption band at wavelengths of 200 to 380 nm, manufactured by BASF) as photopolymerization initiators, and then irradiated with ultraviolet light until the viscosity (measurement conditions: BH viscometer No. 5 rotor, 10 rpm, measurement temperature 30°C) reached approximately 20 Pa·s, to obtain a prepolymer composition (polymerization rate: 8%) in which a portion of the monomer components was polymerized. Next, 0.15 parts by weight of hexanediol diacrylate (HDDA) and 0.3 parts by weight of a silane coupling agent (product name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) were added to the prepolymer composition and mixed to obtain an acrylic pressure-sensitive adhesive composition (a-1).
[0148] Production Example 2 (Production of acrylic pressure-sensitive adhesive composition (a-2)) A monomer mixture consisting of 72 parts by weight of 2-ethylhexyl acrylate (2EHA), 1 part by weight of methacrylic acid acrylate (MMA), 12 parts by weight of N-vinylpyrrolidone (NVP), and 15 parts by weight of hydroxyethyl acrylate (HEA) was charged with 0.2 parts by weight of azobisbutylnitrile (AIBN) and 233 parts by weight of ethyl acetate as a polymerization initiator, and then reacted for 7 hours at 60°C under a nitrogen atmosphere to obtain a partial polymer in which a part of the monomer components was polymerized. Next, 0.3 parts by weight of a silane coupling agent (trade name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) and 0.21 parts by weight of an isocyanate-based crosslinking agent (trade name: Takenate D110N, manufactured by Mitsui Chemicals, Inc.) were added to the partial polymer to obtain an acrylic pressure-sensitive adhesive composition (a-2).
[0149] Production Example 3 (Production of Pressure-Sensitive Adhesive Layer (B-1) on Image Display Side) In a separable flask equipped with a thermometer, a stirrer, a reflux condenser, and a nitrogen gas inlet tube, 95 parts by weight of butyl acrylate, 5 parts by weight of acrylic acid, 0.2 parts by weight of azobisisobutyronitrile as a polymerization initiator, and 233 parts by weight of ethyl acetate were added, and then nitrogen gas was introduced and the mixture was substituted with nitrogen for about 1 hour while stirring.Then, the flask was heated to 60°C and reacted for 7 hours to obtain an acrylic polymer with a weight average molecular weight (Mw) of 1.1 million. To the above acrylic polymer solution (solid content: 100 parts by weight), 0.8 parts by weight of trimethylolpropane tolylene diisocyanate (product name: Coronate L, manufactured by Nippon Polyurethane Industry Co., Ltd.) as an isocyanate crosslinking agent and 0.1 parts by weight of a silane coupling agent (product name: KBM-403, manufactured by Shin-Etsu Chemical Co., Ltd.) were added to prepare a pressure-sensitive adhesive composition (solution). The obtained adhesive composition solution was applied onto a 38 μm thick separator (a polyethylene terephthalate film with a release-treated surface) so that the thickness after drying would be 12 μm, and the layer was dried at 100° C. for 3 minutes to remove the solvent, obtaining an adhesive layer. Then, the layer was heated at 50° C. for 48 hours to carry out a crosslinking treatment. Hereinafter, this adhesive layer will be referred to as the "image display section side adhesive layer (B-1)".
[0150] Production Example 4 (Production of Pressure-Sensitive Adhesive Layer (B-2) on Image Display Side) The adhesive composition solution obtained in Production Example 3 was applied onto a 38 μm thick separator (a polyethylene terephthalate film with a release-treated surface) so that the thickness after drying would be 15 μm, and the layer was dried at 100° C. for 3 minutes to remove the solvent, obtaining an adhesive layer. Thereafter, the layer was heated at 50° C. for 48 hours to carry out a crosslinking treatment. Hereinafter, this adhesive layer will be referred to as the "image display section side adhesive layer (B-2)".
[0151] Example 1 (Production of adhesive composition with ultraviolet absorbing function) To the obtained acrylic adhesive composition (a-1), 1.4 parts by weight of 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (trade name: Tinosorb S, "UV absorber 1" in Tables 1 and 2, manufactured by BASF Japan) dissolved in butyl acrylate to a solid content of 15% and 0.2 parts by weight of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (trade name: Irgacure 819, having absorption resistance in the wavelength range of 200 to 450 nm, manufactured by BASF Japan) were added and stirred to obtain an adhesive composition with UV absorption function.
[0152] The pressure-sensitive adhesive composition with ultraviolet absorbing function was applied onto a release-treated film of a release film so that the thickness of the pressure-sensitive adhesive layer after formation was 150 μm, and then a release film was attached to the surface of the pressure-sensitive adhesive composition layer. Thereafter, illuminance: 6.5 mW / cm 2 , Light amount: 1500mJ / cm 2 The pressure-sensitive adhesive composition layer was photocured by irradiation with ultraviolet light at a peak wavelength of 350 nm to form a viewing-side pressure-sensitive adhesive layer (A-1).
[0153] (Production of polarizing film (P-1)) A 25 μm thick cycloolefin polymer (COP) film was attached to the viewing side of a polarizer made of a 5 μm thick stretched polyvinyl alcohol film impregnated with iodine using a polyvinyl alcohol adhesive, and a 20 μm thick acrylic film was laminated to the image display side surface of the polarizer using a polyvinyl alcohol adhesive to obtain a polarizing film (P-1). The polarization degree of the polarizing film was 99.995.
[0154] (Manufacture of polarizing film with adhesive layer) A viewing-side adhesive layer (A-1) was laminated on the viewing side of the polarizing film (P-1) (i.e., the surface of a cycloolefin polymer (COP) film having a thickness of 25 μm). An image display section side adhesive layer (B-1) was laminated on the image display section side surface of the polarizing film (P-1) (i.e., the surface of an acrylic film having a thickness of 20 μm), and a retardation film (thickness: 56 μm, material: polycarbonate) and an image display section side adhesive layer (B-2) were further laminated to form a polarizing film with an adhesive layer. The obtained polarizing film with an adhesive layer had a configuration of a viewing-side adhesive layer (A-1) / polarizing film (P-1) / image display section side adhesive layer (B-1) / retardation film / image display section side adhesive layer (B-2).
[0155] Examples 2 to 3 A polarizing film with a pressure-sensitive adhesive layer was formed in the same manner as in Example 1, except that the type of acrylic pressure-sensitive adhesive composition, the amount of ultraviolet absorber 1 added, and the thickness after formation of the visible-side pressure-sensitive adhesive layer were as shown in Table 1.
[0156] Example 4 A polarized film with adhesive was formed in the same manner as in Example 1, except that the adhesive layer on the viewing side was changed from the adhesive layer on the viewing side (A-1) to the adhesive layer on the viewing side (A-2) obtained below.
[0157] (Production of Visible Side Adhesive Layer (A-2)) To the acrylic adhesive composition (a-2) obtained in Production Example 2, 1.4 parts by weight of 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (trade name: Tinosorb S, manufactured by BASF Japan Ltd.) dissolved in ethyl acetate to a solid content of 15% was added and stirred to obtain an adhesive composition with ultraviolet absorbing function.
[0158] The adhesive composition with ultraviolet absorbing function was applied onto a release film that had been treated with a release agent so that the thickness of the adhesive layer after formation would be 150 μm, and the adhesive layer was dried at 60° C. for 2 minutes and at 120° C. for 2 minutes. The release-treated film was then bonded to the adhesive layer to form a viewing-side adhesive layer (A-2).
[0159] Examples 5 to 6 A polarizing film with a pressure-sensitive adhesive layer was formed in the same manner as in Example 4, except that the thickness of the pressure-sensitive adhesive layer on the viewing side after formation and the pressure-sensitive adhesive layer on the image display portion side were as shown in Table 1.
[0160] Example 7 (Production of Visible Side Adhesive Layer (A-3)) The acrylic adhesive composition (a-1) obtained in Production Example 1 was mixed with 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine dissolved in butyl acrylate to a solid content of 15%. An adhesive composition with ultraviolet absorbing function was obtained by adding and stirring 0.7 parts by weight of (trade name: Tinosorb S, manufactured by BASF Japan Ltd.), 0.2 parts by weight of Solvent Yellow 163 (KP Plast Yellow MK, "UV absorber 2" in Table 2, manufactured by Kiwa Chemical Industry Co., Ltd.), and 0.2 parts by weight of bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide (trade name: Irgacure 819, has absorption resistance in the wavelength range of 200 to 450 nm, manufactured by BASF Japan Ltd.).
[0161] The pressure-sensitive adhesive composition with ultraviolet absorbing function was applied onto a release-treated film of a release film so that the thickness of the pressure-sensitive adhesive layer after formation was 150 μm, and then a release film was attached to the surface of the pressure-sensitive adhesive composition layer. Thereafter, illuminance: 6.5 mW / cm 2 , Light amount: 3000mJ / cm 2 The pressure-sensitive adhesive composition layer was photocured by irradiation with ultraviolet light at a peak wavelength of 350 nm to form a viewing-side pressure-sensitive adhesive layer (A-3).
[0162] A polarized film with adhesive was formed in the same manner as in Example 1, except that the adhesive layer on the viewing side was changed from the adhesive layer on the viewing side (A-1) to the adhesive layer on the viewing side (A-3) obtained above.
[0163] Comparative Example 1 A polarizing film with a pressure-sensitive adhesive layer was formed in the same manner as in Example 1, except that the viewing-side pressure-sensitive adhesive layer (A-1), the retardation film, and the image display portion-side pressure-sensitive adhesive layer (B-2) were not formed.
[0164] Comparative Example 2 A polarizing film with a pressure-sensitive adhesive layer was formed in the same manner as in Example 1, except that the viewing-side pressure-sensitive adhesive layer (A-1) was not formed.
[0165] Comparative Examples 3 and 4 A polarizing film with a pressure-sensitive adhesive was formed in the same manner as in Examples 1 and 4, except that no ultraviolet absorbing agent was added to the viewing-side pressure-sensitive adhesive layers (A-1) and (A-2).
[0166] Comparative Example 5 (Production of polarizing film (P-2)) A 25 μm-thick triacetyl cellulose film was attached to the viewing side of a polarizer made of a 12 μm-thick stretched polyvinyl alcohol film impregnated with iodine using a polyvinyl alcohol-based adhesive, and a 20 μm-thick acrylic film was laminated to the image display surface of the polarizer using a polyvinyl alcohol-based adhesive to obtain a polarizing film (P-2). The polarization degree of the polarizing film was 99.995.
[0167] A polarizing film with adhesive was formed in the same manner as in Example 2, except that the polarizing film (P-1) in Example 2 was changed to the polarizing film (P-2) described above.
[0168] The obtained pressure-sensitive adhesive layer and the polarizing film with the pressure-sensitive adhesive layer were evaluated as follows.
[0169] <Polymerization rate> The release film of the visible-side adhesive layer obtained in the Examples and Comparative Examples was peeled off, and only the visible-side adhesive layer was placed on the weighed aluminum petri dish. The weight of (aluminum petri dish + visible-side adhesive layer) was measured to determine the weight of the adhesive layer before drying. After drying at 130°C for 2 hours and cooling at room temperature for about 20 minutes, the weight of (aluminum petri dish + adhesive) was measured again to determine the weight of the visible-side adhesive layer after drying. The polymerization rate was calculated using the following formula.
number
[0170] <Gel fraction> About 0.1 g of the visible-side adhesive layer obtained in each of the examples and comparative examples was taken, wrapped in a porous tetrafluoroethylene sheet (trade name: NTF1122, manufactured by Nitto Denko Corporation) having an average pore size of 0.2 μm, and then tied with a kite string. The weight at that time was measured (Zg), and this weight was taken as the weight before immersion. The weight before immersion was the total weight of the visible-side adhesive layer (the adhesive layer taken above), the tetrafluoroethylene sheet, and the kite string. The total weight of the tetrafluoroethylene sheet and the kite string was also measured (Yg). Next, the visible-side adhesive layer wrapped in the tetrafluoroethylene sheet and tied with the kite string (referred to as "sample") was placed in a 50 mL container filled with ethyl acetate and left to stand at 23° C. for 7 days. The sample (after ethyl acetate treatment) was then removed from the container, transferred to an aluminum cup, and dried in a dryer at 130°C for 2 hours to remove the ethyl acetate, after which the weight was measured (Xg), and this weight was taken as the weight after immersion. The gel fraction was calculated from the following formula. Gel fraction (wt%)=(XY) / (ZY)×100
[0171] <Measurement of transmittance and b* value of visible side adhesive layer> The release film of the visible-side pressure-sensitive adhesive layer obtained in each of the Examples and Comparative Examples was peeled off, and the visible-side pressure-sensitive adhesive layer was attached to a measuring jig and measured with a spectrophotometer (product name: U4100, manufactured by Hitachi High-Technologies Corp.) The transmittance was measured at wavelengths of 380 nm, 400 nm, and 420 nm (however, the wavelength of 420 nm was measured only in Examples 2 and 7).
[0172] <Residual stress> A test piece was prepared by cutting out a piece of 30 mm wide and 50 mm long from the visible side pressure-sensitive adhesive layer obtained in the Examples and Comparative Examples, and forming it into a cylindrical shape. This was placed with a chuck gap of 20 mm, and the test piece was pulled 60 mm (300%) at a pulling speed of 200 mm / min (the chuck gap after pulling was 80 mm). The test piece was fixed (held) at the position where it was pulled 60 mm for 300 seconds, and the stress value (N) after 300 seconds was measured. The residual stress was calculated using the following formula. Residual stress after 300 seconds = stress value after 300 seconds (N) / (4 x thickness of test piece / 10)
[0173] <Optical reliability> The visible-side adhesive layer obtained in Examples 1 to 7 and Comparative Examples 3 to 5 was attached to the COP film of the polarizing film (P-1) used in Example 1. Furthermore, a 56 μm retardation film with a 15 μm adhesive (manufactured by Nitto Denko Corporation) was attached to the opposite side (acrylic film side) of the polarizing film to which the visible-side adhesive layer was attached. Both sides of the sample were attached with glass (product name: S200200, thickness: 1.3 mm, size: 45 mm x 50 mm, manufactured by Matsunami Glass Industry Co., Ltd.), and autoclaved (atmospheric pressure: 0.5 MPa, temperature: 50°C) for 15 minutes. Thereafter, the sample was placed under the following various reliability conditions, and the transmittance was measured with a spectral transmittance measuring device (product name: DOT-3, manufactured by Murakami Color Research Laboratory Co., Ltd.). The amount of change in transmittance from the initial state was determined. Evaluation was performed according to the following evaluation criteria. (Various reliability conditions) (Condition 1) 85℃×500h (Condition 2) 60℃, 95% x 500h (Condition 3) Heat shock (HS) (-40℃ to 85℃) x 300 cycles (Condition 4) Under UV irradiation × 100h, illuminance: 500W / cm 2 (300~700nm), Environmental temperature: 60~65℃, Environmental humidity: 50% (Condition 5) Under Xenon irradiation × 300h, illuminance: 2.40W / cm 2 (420nm), environmental temperature: 50℃, environmental humidity: 30% (Evaluation Criteria) ◯: The change in transmittance is 2.0% or less. △: The amount of change in transmittance exceeds 2.0% and is 3.0% or less. ×: The change in transmittance exceeds 3.0%.
[0174] <Glue stains, dimensional accuracy, edge appearance> The polarizing film with the adhesive layer obtained in the examples and comparative examples was cut into a size of 25 mm x 30 mm using a super cutter. Then, the four sides of the cut pieces were cut off by 0.05 mm using an edge processing machine (Megalo Technica Co., Ltd.) to obtain samples. The sides of the samples were visually inspected for glue stains to confirm the presence or absence of glue stains. The dimensional accuracy and edge appearance were observed using an optical microscope and evaluated according to the following evaluation criteria. (Dimensional accuracy) ○:Within ±0.3mm ×: Exceeds ±0.3mm (Exterior view of end) ○: When the edge is not sticky when touched with the hand ×: If the edge is sticky when touched with your hand
[0175] <Curl measurement> A sample cut to 50 mm x 40 mm was placed on a flat desk, and curl was measured using a gap gauge. (curl) ○: Within ±1.0mm △: More than ±1.0mm, within ±2.0mm ×: Greater than ±2.0mm
[0176] [Table 1]
[0177] [Table 2]
[0178] In Table 1, P-1 indicates the polarizing film (P-1), P-2 indicates the polarizing film (P-2), a-1 indicates the acrylic adhesive composition (a-1) obtained in Production Example 1, a-2 indicates the acrylic adhesive composition (a-2) obtained in Production Example 2, UV absorber 1 indicates 2,4-bis-[{4-(4-ethylhexyloxy)-4-hydroxy}-phenyl]-6-(4-methoxyphenyl)-1,3,5-triazine (product name: Tinosorb S, manufactured by BASF Japan Ltd.), UV absorber 2 indicates Solvent Yellow 163 (KP Plast Yellow MK, manufactured by Kiwa Chemical Industry Co., Ltd.), B-1 indicates the adhesive layer (B-1) on the image display portion side obtained in Production Example 3, and B-2 indicates the adhesive layer (B-2) on the image display portion side obtained in Production Example 4. [Explanation of symbols]
[0179] 1 Polarizing film with adhesive layer 2a Visible side adhesive layer 2b Adhesive layer on image display side 3a Transparent protective film on the viewing side 3b Transparent protective film on image display side 4 Polarizer 5. Polarizing Film 6 Cover glass or cover plastic 7 Liquid crystal display (LCD) or organic light emitting diode (OLED) 8a, 8b Adhesive layer 9 Sensor Layer
Claims
1. A polarizing film with a pressure-sensitive adhesive layer for use on a viewing side of an image display unit in an image display device, The polarizing film with a pressure-sensitive adhesive layer has a polarizing film and pressure-sensitive adhesive layers on both sides of the polarizing film, The polarizing film has a polarizer and transparent protective films on both sides of the polarizer, the polarizer is made of a polyvinyl alcohol film and a dichroic material, The transparent protective film on the viewing side of the polarizer has a transmittance at a wavelength of 380 nm of less than 6%, the transparent protective film on the viewing side of the polarizer is at least one film selected from the group consisting of a triacetyl cellulose film, a polyethylene terephthalate film, and a polyolefin film having a cyclo- or norbornene structure, The transparent protective film on the viewing side of the polarizer and the transparent protective film on the image display portion side of the polarizer are not both triacetyl cellulose films, the pressure-sensitive adhesive layer on the viewing side of the polarizing film is formed from an ultraviolet-curable acrylic pressure-sensitive adhesive composition, and the ultraviolet-curable acrylic pressure-sensitive adhesive composition is prepared by irradiating with ultraviolet light a composition containing a monomer component containing an alkyl(meth)acrylate and a photopolymerization initiator (B) having an absorption band at a wavelength of less than 400 nm to form a partial polymer of the monomer component, and adding an ultraviolet absorber and a photopolymerization initiator (A) having an absorption band at a wavelength of 400 nm or more to the partial polymer of the monomer component; The thickness of the pressure-sensitive adhesive layer on the viewing side of the polarizing film is 50 μm or more, the pressure-sensitive adhesive layer on the viewing side of the polarizing film contains, as the ultraviolet absorbing agent, one or more of a triazine-based ultraviolet absorbing agent, a benzotriazole-based ultraviolet absorbing agent, an oxybenzophenone-based ultraviolet absorbing agent, a salicylic acid ester-based ultraviolet absorbing agent, and a cyanoacrylate-based ultraviolet absorbing agent, and a dye; A polarizing film with an adhesive layer, wherein the adhesive layer on the viewing side of the polarizing film has an ultraviolet absorbing function.
2. 2. The polarizing film with a pressure-sensitive adhesive layer according to claim 1, wherein the transparent protective film on the viewing side of the polarizer has a thickness of 40 μm or less.
3. 3. The polarizing film with an adhesive layer according to claim 1, wherein the thickness of the adhesive layer on the viewing side of the polarizing film is at least twice the thickness of the adhesive layer on the image display side of the polarizing film.
4. The polarizing film with a pressure-sensitive adhesive layer according to any one of claims 1 to 3, characterized in that the pressure-sensitive adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm and a transmittance of 60% or more at a wavelength of 400 nm.
5. The polarizing film with a pressure-sensitive adhesive layer according to any one of claims 1 to 3, characterized in that the pressure-sensitive adhesive layer on the viewing side of the polarizing film has a transmittance of 9% or less at a wavelength of 380 nm and a transmittance of 75% or less at a wavelength of 420 nm.
6. 5. The polarizing film with a pressure-sensitive adhesive layer according to claim 1, wherein the b* value of the pressure-sensitive adhesive layer on the viewing side of the polarizing film is 3.0 or less.
7. 7. The polarizing film with a pressure-sensitive adhesive layer according to claim 1, wherein the pressure-sensitive adhesive layer on the viewing side of the polarizing film contains an acrylic polymer as a base polymer.
8. 8. The pressure-sensitive adhesive layer-attached polarizing film according to claim 1, which is used in a liquid crystal display device or an organic EL display device.
9. 9. An image display device, comprising the pressure-sensitive adhesive layer-attached polarizing film according to claim 1 on a viewing side of an image display section.
Citation Information
Patent Citations
A polarizing plate laminated with adhesive
JP1985133402U
Polarizing plate protection film, and polarizing plate and liquid crystal display using same
JP2006184883A
Polarizing plate
JP2008040277A
Polarizing plate and liquid crystal display device using the same
JP2011232493A
Polarizer protective film, polarizing plate, and image display device
JP2012003269A