Adhesive sheet
A pressure-sensitive adhesive sheet with tailored properties addresses peeling and light leakage issues in repeatedly bent displays by enhancing adhesion and optical properties, ensuring durability and clarity in flexible displays.
Patent Information
- Application Number
- JP2020173617
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-14
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2040-10-14
AI Technical Summary
Conventional adhesive sheets used in repeatedly bent displays suffer from peeling at the interface between the adhesive layer and the adherend, leading to light leakage over time.
A pressure-sensitive adhesive sheet with specific properties, including a refractive index of 1.55 or more, a gel fraction of 30% to 100%, a haze value of 10% or less, and a storage modulus of 0.05 MPa to 20 MPa, is developed to suppress light leakage in long-term bending.
The adhesive sheet effectively prevents light leakage and maintains appearance in displays subjected to repeated bending by ensuring strong adhesion and optical clarity.
Smart Images

Figure 0007579669000003 
Figure 0007579669000004 
Figure 0007579669000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a pressure-sensitive adhesive sheet suitable for use in displays and the like. [Background technology]
[0002] In recent years, bendable displays have been proposed as displays for electronic devices, which are a type of device. In addition to displays that are curved only once, repeatedly bent displays that are repeatedly bent (folded) have also been proposed.
[0003] In the above-mentioned repeatedly bent display, it is considered that one bendable member (flexible member) constituting the said bent display and another bendable member are bonded with an adhesive layer of an adhesive sheet. However, when a conventional adhesive sheet is used in a repeatedly bent display, a problem occurs in that peeling occurs at the interface between the adhesive layer and the adherend at the bent portion.
[0004] Patent Document 1 discloses a pressure-sensitive adhesive intended to suppress the occurrence of peeling during repeated bending. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2016-108555 A Summary of the Invention [Problem to be solved by the invention]
[0006] On the other hand, in the above-mentioned repeatedly bent display, light leakage may occur around the bent portion after a long period of bending. The adhesive described in Patent Document 1 cannot sufficiently solve the problem of light leakage.
[0007] The present invention has been made in consideration of the above-mentioned circumstances, and has an object to provide a pressure-sensitive adhesive sheet that can suppress light leakage caused by being bent for a long period of time. [Means for solving the problem]
[0008] In order to achieve the above-mentioned object, firstly, the present invention provides an adhesive sheet having at least an adhesive layer, characterized in that the refractive index of the adhesive constituting the adhesive layer is 1.55 or more, and the gel fraction of the adhesive is 30% or more and 100% or less (Invention 1).
[0009] According to the above invention (Invention 1), when a laminate formed by bonding one member (particularly a flexible member) to another member (particularly a flexible member) with the pressure-sensitive adhesive layer is placed in a bent state for a long period of time, light leakage at the bent portion is suppressed.
[0010] In the above invention (Invention 1), the haze value of the pressure-sensitive adhesive layer is preferably 10% or less (Invention 2).
[0011] In the above inventions (Inventions 1 and 2), the pressure-sensitive adhesive layer preferably has a total light transmittance of 70% or more (Invention 3).
[0012] In the above inventions (Inventions 1 to 3), the pressure-sensitive adhesive preferably has a storage modulus G' at 23° C. of 0.05 MPa or more and 20 MPa or less (Invention 4).
[0013] In the above inventions (Inventions 1 to 4), the pressure-sensitive adhesive preferably has a storage modulus G' at 80° C. of 0.01 MPa or more and 15 MPa or less (Invention 5).
[0014] In the above inventions (Inventions 1 to 5), it is preferable that the weight average molecular weight of the sol component of the pressure-sensitive adhesive is 10,000 or more and 2,000,000 or less (Invention 6).
[0015] In the above inventions (Inventions 1 to 6), it is preferable that the pressure-sensitive adhesive contains high refractive index fine particles (Invention 7).
[0016] In the above inventions (Inventions 1 to 7), the pressure-sensitive adhesive is preferably an acrylic pressure-sensitive adhesive (Invention 8).
[0017] In the above invention (Invention 8), it is preferable that the acrylic pressure-sensitive adhesive contains a (meth)acrylic acid ester polymer, and the (meth)acrylic acid ester polymer contains an aromatic ring-containing monomer as a monomer unit constituting the polymer (Invention 9).
[0018] In the above inventions (Inventions 1 to 9), it is preferable that the adhesive layer comprises two release sheets and is sandwiched between the release sheets so as to be in contact with the release surfaces of the two release sheets (Invention 10).
[0019] The pressure-sensitive adhesive sheets according to the above inventions (Inventions 1 to 10) are preferably used for displays (Invention 11). Effect of the Invention
[0020] The pressure-sensitive adhesive sheet according to the present invention can suppress light leakage caused by a long period of bending. [Brief description of the drawings]
[0021] [Figure 1] 1 is a cross-sectional view of a pressure-sensitive adhesive sheet according to one embodiment of the present invention. [Diagram 2] 1 is a cross-sectional view of a display according to an embodiment of the present invention. [Diagram 3] FIG. 1 is an explanatory diagram (side view) for explaining a static bending test. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, an embodiment of the present invention will be described. [Adhesive sheet] The pressure-sensitive adhesive sheet according to one embodiment of the present invention has at least a pressure-sensitive adhesive layer, and preferably has a release sheet laminated on one or both sides of the pressure-sensitive adhesive layer.
[0023] The refractive index of the adhesive constituting the adhesive layer is preferably 1.55 or more, and the gel fraction of the adhesive is preferably 30% or more and 100% or less, which suppresses light leakage at the bent portion when a laminate obtained by bonding one member (particularly a flexible member) to another member (particularly a flexible member) with the adhesive layer is placed in a bent state for a long period of time.
[0024] In this specification, the refractive index of the adhesive is a value measured according to JIS K0062-1992. The method for measuring the gel fraction is as shown in the test examples described later. In this specification, the haze value is a value measured according to JIS K7136:2000.
[0025] From the viewpoint of suppressing light leakage, the refractive index of the pressure-sensitive adhesive is preferably 1.55 or more, more preferably 1.57 or more, particularly preferably 1.59 or more, and even more preferably 1.60 or more. The upper limit of the refractive index of the pressure-sensitive adhesive is not particularly limited, but is usually preferably 3.00 or less, more preferably 2.00 or less, particularly preferably 1.80 or less, and even more preferably 1.70 or less.
[0026] From the viewpoint of achieving excellent appearance after long-term bending, the gel fraction of the pressure-sensitive adhesive is preferably 30% or more, more preferably 50% or more, particularly preferably 70% or more, and even more preferably 75% or more. From the same viewpoint, the gel fraction of the pressure-sensitive adhesive is preferably 100% or less, more preferably 95% or less, particularly preferably 90% or less, and even more preferably 85% or less.
[0027] The haze value of the pressure-sensitive adhesive layer is preferably 10% or less, more preferably 7% or less, particularly preferably 3% or less, and even more preferably 1% or less. If the haze value is as low as above, the pressure-sensitive adhesive layer can suppress appearance changes due to long-term bending, even though the pressure-sensitive adhesive layer has a very high refractive index. The lower limit of the haze value of the pressure-sensitive adhesive layer is not particularly limited, but from the viewpoint of easily satisfying the refractive index of the pressure-sensitive adhesive, it is preferably 0.01% or more, more preferably 0.1% or more, particularly preferably 0.3% or more, and even more preferably 0.5% or more.
[0028] From the viewpoint of visibility of the display, the total light transmittance of the pressure-sensitive adhesive layer is preferably 70% or more, more preferably 80% or more, particularly preferably 90% or more, and even more preferably 97% or more. The upper limit of the total light transmittance of the pressure-sensitive adhesive layer is not particularly limited, and may be 100%, or may be a value slightly exceeding 100% due to measurement. The total light transmittance in this specification is a value measured in accordance with JIS K7361-1:1997.
[0029] On the other hand, the storage modulus G' of the pressure-sensitive adhesive at 23°C is preferably 0.05 MPa or more, more preferably 0.10 MPa or more, particularly preferably 0.30 MPa or more, more preferably 1.0 MPa or more, and most preferably 2.0 MPa or more. The storage modulus G' of the pressure-sensitive adhesive at 23°C is preferably 20 MPa or less, more preferably 10 MPa or less, particularly preferably 5 MPa or less, and even more preferably 3.5 MPa or less. When the storage modulus G' of the pressure-sensitive adhesive at 23°C is in the above range, the light leakage resistance and the appearance after long-term bending become more excellent. The storage modulus G' in this specification is a value measured by a torsional shear method at a measurement frequency of 1 Hz in accordance with JIS K7244-6. Specifically, it is as shown in the test example described later.
[0030] The storage modulus G' of the pressure-sensitive adhesive at 80°C is preferably 0.01 MPa or more, more preferably 0.03 MPa or more, particularly preferably 0.08 MPa or more, and even more preferably 0.14 MPa or more. The storage modulus G' of the pressure-sensitive adhesive at 80°C is preferably 15 MPa or less, more preferably 10 MPa or less, particularly preferably 5 MPa or less, and even more preferably 2 MPa or less. When the storage modulus G' of the pressure-sensitive adhesive at 80°C is within the above range, the light leakage resistance and the appearance after long-term bending are more excellent.
[0031] The weight average molecular weight of the sol content of the pressure-sensitive adhesive is preferably 10,000 or more, more preferably 40,000 or more, particularly preferably 80,000 or more, and even more preferably 100,000 or more. The weight average molecular weight of the sol content of the pressure-sensitive adhesive is preferably 2,000,000 or less, more preferably 1,000,000 or less, particularly preferably 500,000 or less, and even more preferably 300,000 or less. Since the weight average molecular weight of the sol content of the pressure-sensitive adhesive is within the above range and the gel fraction is within the above range, the pressure-sensitive adhesive has a more excellent appearance after long-term bending and is easy to reduce the haze value.
[0032] The weight average molecular weight of the sol component in this specification is a value calculated in terms of standard polystyrene as measured by gel permeation chromatography (GPC). The specific measurement method is as shown in the test examples described later.
[0033] FIG. 1 shows a specific configuration of one example of the pressure-sensitive adhesive sheet according to this embodiment. 1, an adhesive sheet 1 according to one embodiment is composed of two release sheets 12a, 12b and an adhesive layer 11 sandwiched between the two release sheets 12a, 12b so as to be in contact with the release surfaces of the two release sheets 12a, 12b. In this specification, the release surface of a release sheet refers to a surface of the release sheet that has releasability, and includes both a surface that has been subjected to a release treatment and a surface that exhibits releasability even without being subjected to a release treatment.
[0034] 1. Components 1-1. Adhesive layer The adhesive layer 11 is preferably made of an adhesive having the above-mentioned physical properties. The type of adhesive constituting the adhesive layer 11 is not particularly limited, and may be, for example, any of an acrylic adhesive, a polyester adhesive, a polyurethane adhesive, a rubber adhesive, a silicone adhesive, etc. The adhesive may be any of an emulsion type, a solvent type, or a solventless type, and may be any of a cross-linked type or a non-cross-linked type. Among them, an acrylic adhesive is preferred because it is easy to satisfy the above-mentioned physical properties and has excellent adhesive properties and optical properties, etc., and in particular, a solvent-type acrylic adhesive is preferred, and a cross-linked acrylic adhesive is more preferred.
[0035] The adhesive in this embodiment may be either non-curable or curable by active energy rays. Furthermore, the adhesive in this embodiment preferably contains high refractive index fine particles in order to satisfy the refractive index described above. In this specification, the high refractive index fine particles refer to fine particles that can impart a higher refractive index than the matrix to the adhesive obtained.
[0036] Specifically, the adhesive in this embodiment is preferably a crosslinked adhesive composition (hereinafter sometimes referred to as "adhesive composition P") containing a (meth)acrylic acid ester polymer (A), a crosslinking agent (B), high refractive index fine particles (C), and, if desired, an active energy ray curable component (D). In addition, when the active energy ray curable component (D) is contained, it is preferable that the composition is cured by irradiation with active energy rays. The adhesive obtained by crosslinking (and curing) the adhesive composition P is likely to satisfy the above-mentioned physical properties. In this specification, (meth)acrylic acid means both acrylic acid and methacrylic acid. The same applies to other similar terms. In addition, the concept of "copolymer" is also included in "polymer".
[0037] (1) Components of adhesive composition P (1-1) (Meth)acrylic acid ester polymer (A) The (meth)acrylic acid ester polymer (A) preferably contains, as a monomer unit constituting the polymer, a (meth)acrylic acid alkyl ester for exhibiting good adhesion and a monomer having a reactive functional group (reactive functional group-containing monomer) that serves as a crosslinking point. In addition, the (meth)acrylic acid ester polymer (A) preferably further contains, as a monomer unit constituting the polymer, a monomer (high refractive index monomer) that can increase the refractive index of the matrix of the obtained adhesive. By containing a high refractive index monomer, the difference between the refractive index of the matrix of the adhesive and the refractive index of the high refractive index fine particles (C) can be reduced, and the above-mentioned haze value is easily satisfied. Therefore, it is more preferable that the (meth)acrylic acid ester polymer (A) contains, as a monomer unit constituting the polymer, a (meth)acrylic acid alkyl ester, a high refractive index monomer, and a reactive functional group-containing monomer.
[0038] The (meth)acrylic acid alkyl ester preferably includes a (meth)acrylic acid alkyl ester in which the carbon number of the alkyl group is 1 to 20. The alkyl group is preferably linear or branched.
[0039] Examples of (meth)acrylic acid alkyl esters having 1 to 20 carbon atoms in the alkyl group include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, n-decyl (meth)acrylate, n-dodecyl (meth)acrylate, myristyl (meth)acrylate, palmityl (meth)acrylate, and stearyl (meth)acrylate. Among them, from the viewpoint of the above-mentioned storage modulus G' and adhesive strength, (meth)acrylic acid esters having 1 to 10 carbon atoms in the alkyl group are preferred, and (meth)acrylic acid esters having 4 to 8 carbon atoms in the alkyl group are particularly preferred. Specifically, n-butyl acrylate, isooctyl acrylate, or 2-ethylhexyl acrylate are preferred. These may be used alone or in combination of two or more.
[0040] From the viewpoint of obtaining a desired adhesive strength or from the viewpoint of lowering the storage modulus G', the (meth)acrylic acid ester polymer (A) preferably contains 5% by mass or more, more preferably 10% by mass or more, particularly preferably 15% by mass or more, and even more preferably 20% by mass or more of a (meth)acrylic acid alkyl ester having an alkyl group carbon number of 1 to 20 as a monomer unit constituting the polymer. Also, from the viewpoint of ensuring the blending amount of other monomer components, the (meth)acrylic acid alkyl ester is preferably contained in an amount of 60% by mass or less, more preferably 50% by mass or less, particularly preferably 40% by mass or less, and even more preferably 30% by mass or less.
[0041] As the high refractive index monomer, a monomer having a cyclic structure is preferably used, and a monomer having an aromatic ring (aromatic ring-containing monomer) is particularly preferably used. As the aromatic ring-containing monomer, a monomer having one or more aromatic rings, a monomer having a polycyclic aromatic skeleton, etc. are exemplified. Among them, from the viewpoint of lowering the storage modulus G' and increasing the adhesive strength, an aromatic ring-containing monomer having one aromatic ring is preferred.
[0042] Examples of aromatic ring-containing monomers containing one aromatic ring include phenyl (meth)acrylate, 2-phenylethyl (meth)acrylate, benzyl (meth)acrylate, 2-phenoxyethyl (meth)acrylate, phenoxybutyl (meth)acrylate, styryl (meth)acrylate, phenoxydiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, etc. These may be used alone or in combination of two or more.
[0043] The (meth)acrylic acid ester polymer (A) preferably contains 20% by mass or more of aromatic ring-containing monomer as a monomer unit constituting the polymer, more preferably 30% by mass or more, particularly preferably 40% by mass or more, and even more preferably 50% by mass or more. Also, the aromatic ring-containing monomer is preferably contained at 90% by mass or less, more preferably 85% by mass or less, particularly preferably 80% by mass or less, and even more preferably 70% by mass or less. By containing the aromatic ring-containing monomer within the above range, it is estimated that the refractive index difference between the obtained (meth)acrylic acid ester polymer (A) and the high refractive index fine particles (C) is in a suitable range, and it becomes easy to obtain a pressure-sensitive adhesive having a low haze value and a high refractive index.
[0044] The (meth)acrylic acid ester polymer (A) contains a reactive functional group-containing monomer as a monomer unit constituting the polymer, and reacts with the crosslinking agent (B) described below via the reactive functional group derived from the reactive functional group-containing monomer, thereby forming a crosslinked structure (three-dimensional network structure), and a pressure-sensitive adhesive having the desired cohesive strength is obtained. The pressure-sensitive adhesive is likely to satisfy the gel fraction and storage modulus G' described above.
[0045] The reactive functional group-containing monomer contained in the (meth)acrylic acid ester polymer (A) as a monomer unit constituting the polymer is preferably a monomer having a hydroxyl group in the molecule (hydroxyl group-containing monomer), a monomer having a carboxyl group in the molecule (carboxyl group-containing monomer), a monomer having an amino group in the molecule (amino group-containing monomer), etc. These reactive functional group-containing monomers may be used alone or in combination of two or more kinds.
[0046] Among the above reactive functional group-containing monomers, from the viewpoint of improving the dispersibility of the high refractive index fine particles (C) and giving the resulting adhesive a low haze value, hydroxyl group-containing monomers or carboxyl group-containing monomers are preferred, and hydroxyl group-containing monomers are particularly preferred.
[0047] Examples of the hydroxyl group-containing monomer include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-hydroxybutyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate. Among the above, from the viewpoint of ease of satisfying the physical property related to the storage elastic modulus G' described above, a (meth)acrylic acid hydroxyalkyl ester having a hydroxyalkyl group having 1 to 4 carbon atoms is preferred. Specifically, for example, 2-hydroxyethyl acrylate or 4-hydroxybutyl acrylate is preferred. These may be used alone or in combination of two or more.
[0048] Examples of the carboxyl group-containing monomer include ethylenically unsaturated carboxylic acids such as acrylic acid, methacrylic acid, crotonic acid, maleic acid, itaconic acid, and citraconic acid. Among them, acrylic acid is preferred from the viewpoint of the adhesive strength of the (meth)acrylic acid ester polymer (A) obtained. These may be used alone or in combination of two or more kinds.
[0049] The (meth)acrylic acid ester polymer (A) preferably contains 2% by mass or more of reactive functional group-containing monomer as a monomer unit constituting the polymer, more preferably 4% by mass or more, particularly preferably 8% by mass or more, and even more preferably 12% by mass or more. The (meth)acrylic acid ester polymer (A) preferably contains 34% by mass or less of reactive functional group-containing monomer as a monomer unit constituting the polymer, more preferably 28% by mass or less, particularly preferably 24% by mass or less, and even more preferably 18% by mass or less. When the (meth)acrylic acid ester polymer (A) contains the reactive functional group-containing monomer as a monomer unit in the above amount, the cohesive force of the obtained adhesive becomes appropriate due to the crosslinking reaction with the crosslinking agent (B), and the above-mentioned gel fraction and storage modulus G' are more easily satisfied. In addition, although the reason is unclear, it is presumed that the dispersibility of the high refractive index fine particles (C) is improved, and the above-mentioned haze value is more easily satisfied.
[0050] It is also preferable that the (meth)acrylic acid ester polymer (A) does not contain a carboxyl group-containing monomer as a monomer unit constituting the polymer. If the (meth)acrylic acid ester polymer (A) contains a carboxyl group-containing monomer, the coating solution of the pressure-sensitive adhesive composition may gel in relation to the high refractive index fine particles (C), resulting in poor coating.
[0051] Here, "not containing a carboxyl group-containing monomer" means that the carboxyl group-containing monomer is not substantially contained, and in addition to not containing any carboxyl group-containing monomer at all, the carboxyl group-containing monomer may be contained to the extent that gelation does not occur. Specifically, the (meth)acrylic acid ester polymer (A) may contain the carboxyl group-containing monomer as a monomer unit in an amount of 0.1% by mass or less, preferably 0.01% by mass or less, and more preferably 0.001% by mass or less.
[0052] The (meth)acrylic acid ester polymer (A) may contain other monomers as monomer units constituting the polymer, if desired. As the other monomers, monomers not containing reactive functional groups are preferred so as not to inhibit the above-mentioned action of the reactive functional group-containing monomer. Examples of such monomers include non-reactive nitrogen atom-containing monomers such as N-acryloylmorpholine and N-vinyl-2-pyrrolidone, (meth)acrylic acid alkoxyalkyl esters such as methoxyethyl (meth)acrylate and ethoxyethyl (meth)acrylate, vinyl acetate, and styrene. These may be used alone or in combination of two or more.
[0053] The polymerization mode of the (meth)acrylic acid ester polymer (A) may be a random copolymer or a block copolymer.
[0054] The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 200,000 or more, more preferably 400,000 or more, particularly preferably 600,000 or more, and even more preferably 750,000 or more. The weight average molecular weight of the (meth)acrylic acid ester polymer (A) is preferably 2,000,000 or less, more preferably 1,500,000 or less, particularly preferably 1,000,000 or less, and even more preferably 900,000 or less. When the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is within the above range, the above-mentioned gel fraction, weight average molecular weight of the sol content, storage elastic modulus G', and adhesive force described below are easily satisfied. In addition, since the upper limit of the weight average molecular weight of the (meth)acrylic acid ester polymer (A) is as described above, the above-mentioned haze value is easily satisfied. The weight average molecular weight of the polymer in this specification is a value measured by gel permeation chromatography (GPC) in terms of standard polystyrene.
[0055] The refractive index of the (meth)acrylic acid ester polymer (A) is preferably 1.40 or more, more preferably 1.46 or more, particularly preferably 1.48 or more, and even more preferably 1.50 or more. This makes it easier to meet the above-mentioned haze value. The upper limit of the (meth)acrylic acid ester polymer (A) is not particularly limited, but is usually preferably 2.00 or less, more preferably 1.80 or less, particularly preferably 1.60 or less, and even more preferably 1.55 or less. When the refractive index of the (meth)acrylic acid ester polymer (A) is within the above range, it is estimated that the refractive index difference with the high refractive index fine particles (C) is optimized, and it is easy to obtain a pressure-sensitive adhesive with low haze and high refractive index. The refractive index of the (meth)acrylic acid ester polymer (A) in this specification is a value measured in accordance with JIS K0062-1992.
[0056] In the pressure-sensitive adhesive composition P, the (meth)acrylic acid ester polymer (A) may be used alone or in combination of two or more kinds.
[0057] (1-2) Crosslinking agent (B) The crosslinking agent (B) crosslinks the (meth)acrylic acid ester polymer (A) and forms a three-dimensional network structure when the pressure-sensitive adhesive composition P containing the crosslinking agent (B) is heated or the like, which is a trigger. This improves the cohesive strength of the resulting pressure-sensitive adhesive, and makes it easier to satisfy the above-mentioned gel fraction, storage modulus G', and molecular weight of the sol fraction.
[0058] The crosslinking agent (B) may be any one that reacts with the reactive group of the (meth)acrylic acid ester polymer (A), and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, amine-based crosslinking agents, melamine-based crosslinking agents, aziridine-based crosslinking agents, hydrazine-based crosslinking agents, aldehyde-based crosslinking agents, oxazoline-based crosslinking agents, metal alkoxide-based crosslinking agents, metal chelate-based crosslinking agents, metal salt-based crosslinking agents, and ammonium salt-based crosslinking agents. Among the above, it is preferable to use an isocyanate-based crosslinking agent that has excellent reactivity with a reactive functional group-containing monomer. The crosslinking agent (B) may be used alone or in combination of two or more.
[0059] The isocyanate-based crosslinking agent contains at least a polyisocyanate compound. Examples of the polyisocyanate compound include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and their biuret and isocyanurate forms, as well as adducts which are reactants with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, trimethylolpropane-modified aromatic polyisocyanates, particularly trimethylolpropane-modified tolylene diisocyanate or trimethylolpropane-modified xylylene diisocyanate, are preferred from the viewpoint of reactivity with hydroxyl groups.
[0060] The content of the crosslinking agent (B) in the adhesive composition P is preferably 0.001 parts by mass or more, more preferably 0.01 parts by mass or more, and even more preferably 0.1 parts by mass or more, based on 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, and even more preferably 1 part by mass or less. When the content of the crosslinking agent (B) is within the above range, the gel fraction, storage modulus G', and molecular weight of the sol fraction described above are more easily satisfied.
[0061] (1-3) High refractive index particles (C) The high refractive index fine particles (C) are not particularly limited as long as they can impart a higher refractive index than the (meth)acrylic acid ester polymer (A) to the obtained adhesive and can satisfy the above-mentioned refractive index. Examples of such high refractive index fine particles (C) include metal oxide fine particles, as well as fine particles using high refractive index resins such as styrene resins and sulfur-containing resins. Among these, metal oxide fine particles are preferred from the viewpoint of ease of satisfying the above-mentioned refractive index, and metal oxide fine particles containing transition metals are particularly preferred.
[0062] As the metal oxide fine particles containing a transition metal, for example, fine particles of zirconium oxide, titanium oxide, barium titanate, tantalum oxide, zinc oxide, hafnium oxide, cerium oxide, niobium oxide, etc. are preferable. These are used alone or in combination of two or more. Among the above, zirconium oxide fine particles, which easily satisfy the above-mentioned refractive index, are particularly preferable.
[0063] The surface of the metal oxide fine particles may be chemically modified with an organic compound, etc. The shape of the metal oxide fine particles may be spherical or non-spherical, but is preferably spherical from the viewpoint of easily satisfying the above-mentioned refractive index.
[0064] The average particle size of the high refractive index fine particles (C) is preferably 1000 nm or less, more preferably 700 nm or less. This makes it easier to satisfy the refractive index and haze values described above. The average particle size of the high refractive index fine particles (C) is preferably 2 nm or more, more preferably 10 nm or more. This improves dispersibility and makes it easier to satisfy the storage modulus G' described above. The average particle size of the high refractive index fine particles (C) is determined by measuring the primary particle size using a zeta potential measurement method.
[0065] The high refractive index fine particles (C) are preferably used as a dispersion solution in consideration of dispersibility in the adhesive composition P. The dispersion solvent used in this case is preferably a hydrophobic solvent, and preferably does not contain a hydrophilic solvent or contains only a small amount of a hydrophilic solvent. This makes it easier to reduce the haze value of the resulting adhesive.
[0066] Hydrophobic solvents have a solubility parameter (SP) of 12 (cal / cm 3 ) 1 / 2 The use of such a solvent improves the dispersibility of the high refractive index fine particles (C), particularly the metal oxide fine particles, in the adhesive composition P. The SP value of the hydrophobic solvent is preferably 10 (cal / cm 3 ) 1 / 2 More preferably, it is equal to or less than 9.5 (cal / cm 3 ) 1 / 2 The lower limit of the SP value of the hydrophobic solvent is not particularly limited, but from the viewpoint of availability, it is preferable that the SP value is 6.5 (cal / cm 3 ) 1 / 2 More preferably, it is equal to or greater than this.
[0067] SP value is 12 (cal / cm 3 ) 1 / 2Examples of the following solvents include amides such as dimethylformamide (12.0); nitriles such as acetonitrile (11.8); ketones such as acetone (10.0), methyl ethyl ketone (9.3), methyl propyl ketone (8.7), and methyl isopropyl ketone (8.5); esters (e.g., carboxylate esters) such as di-n-butyl phthalate (9.4), ethyl acetate (9.1), n-butyl acetate (8.5), isopropyl acetate (8.4), and isobutyl acetate (8.3); dioxane (9.9), tetrahydrofuran (9.1), and diethyl ether ( Examples of solvents include linear and cyclic ethers such as benzene (9.2), toluene (8.9), xylene (8.8), ethylbenzene (8.8), cyclohexane (8.2), n-octane (7.6), n-hexane (7.3), n-pentane (7.0), and other aromatic and aliphatic hydrocarbons; halogenated hydrocarbons (e.g., halogenated aliphatic hydrocarbons) such as methylene chloride (9.7), chloroform (9.3), trichloroethylene (9.2), and carbon tetrachloride (8.6); and carbon sulfides such as carbon disulfide (10.0). The numbers in parentheses next to the solvent names are SP values (cal / cm 3 ) 1 / 2 )
[0068] The dispersion solvent of the high refractive index particles (C) is a hydrophilic solvent (SP value is 12 (cal / cm 3 ) 1 / 2 When the component (above 10%) is contained, its content is preferably 15% by mass or less, particularly preferably 10% by mass or less, and further preferably 8% by mass or less.
[0069] A dispersant may be used to further improve the dispersibility of the high refractive index fine particles (C). The dispersant preferably contains an acrylic component from the viewpoint of compatibility with the (meth)acrylic acid ester polymer (A). As an example, it is also preferable to use the active energy ray curable component (D) (and a photopolymerization initiator) described below as the dispersant. When the high refractive index fine particles (C) are used as a dispersion solution containing such a dispersant, the dispersion solution is called a high refractive index component.
[0070] The refractive index of the high refractive index particles (C) is preferably 1.5 or more, more preferably 1.6 or more, particularly preferably 1.7 or more, and even more preferably 1.8 or more, from the viewpoint that the obtained adhesive easily meets the refractive index described above. The upper limit of the refractive index of the high refractive index particles (C) is not particularly limited, but is usually preferably 5.0 or less, particularly preferably 3.0 or less, and even more preferably 2.0 or less. The refractive index of the high refractive index particles (C) is a value measured in accordance with JIS K7142:2014 B method.
[0071] In addition, the refractive index of the coating film of the high refractive index component is preferably 1.4 or more, more preferably 1.5 or more, particularly preferably 1.6 or more, and even more preferably 1.7 or more, from the viewpoint that the obtained adhesive easily meets the refractive index described above. The upper limit of the refractive index of the high refractive index component is not particularly limited, but is usually preferably 3.0 or less, particularly preferably 2.0 or less, and even more preferably 1.8 or less. The refractive index of the coating film of the high refractive index component is a value measured in accordance with JIS K0062-1992.
[0072] The content of the high refractive index fine particles (C) in the adhesive composition P is preferably 5% by mass or more, more preferably 20% by mass or more, particularly preferably 35% by mass or more, and even more preferably 45% by mass or more. The content is preferably 90% by mass or less, more preferably 80% by mass or less, particularly preferably 70% by mass or less, and even more preferably 65% by mass or less. When the content of the high refractive index fine particles (C) is within the above range, the refractive index, storage modulus G', and haze value described above are easily satisfied, and good adhesiveness is maintained. In addition, when the high refractive index fine particles (C) are blended in the adhesive composition P as a high refractive index component, the above "content of the high refractive index fine particles (C) in the adhesive composition P" is defined as "the content of the solid content of the high refractive index component in the adhesive composition P (the matrix such as the high refractive index fine particles (C) and the dispersant)".
[0073] (1-4) Active energy ray-curable component (D) In the present embodiment, when the adhesive composition P contains an active energy ray curable component (D), in the adhesive obtained by thermally crosslinking and curing the adhesive composition P with active energy rays, the active energy ray curable components (D) are presumed to polymerize with each other, and the polymerized active energy ray curable components (D) are presumed to be entangled with the crosslinked structure (three-dimensional network structure) of the (meth)acrylic acid ester polymer (A). An adhesive having such a high-order structure is likely to satisfy the gel fraction and storage modulus G' described above.
[0074] The active energy ray curable component (D) is not particularly limited as long as it is a component that is cured by irradiation with active energy rays and can obtain the above-mentioned effects, and may be any of a monomer, oligomer, or polymer, or a mixture thereof. Among them, a polyfunctional acrylate monomer, oligomer, or polymer is preferable, and a mixture thereof may be used. In addition, since the active energy ray curable component (D) contains at least a polyfunctional acrylate monomer, the active energy ray curable component (D) can be used as a dispersant for the high refractive index fine particles (C).
[0075] (1-5) Various additives If desired, various additives commonly used in acrylic adhesives, such as silane coupling agents, photopolymerization initiators, tackifiers, UV absorbers, antistatic agents, antioxidants, light stabilizers, softeners, and fillers, can be added to the adhesive composition P. The active energy ray curable component (D) not included in the refractive index increasing component may be included in the additives referred to here. The polymerization solvent and dilution solvent described below are not included in the additives constituting the adhesive composition P.
[0076] The pressure-sensitive adhesive composition P preferably contains the above-mentioned silane coupling agent, which improves the adhesion of the resulting pressure-sensitive adhesive layer to the flexible member that is the adherend, and provides more preferable adhesive strength.
[0077] The silane coupling agent is preferably an organosilicon compound having at least one alkoxysilyl group in the molecule, which has good compatibility with the (meth)acrylic acid ester polymer (A) and has optical transparency.
[0078] Examples of such silane coupling agents include polymerizable unsaturated group-containing silicon compounds such as vinyltrimethoxysilane, vinyltriethoxysilane, and methacryloxypropyltrimethoxysilane; epoxy structure-containing silicon compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, and 3-mercaptopropyldimethoxymethylsilane; Examples of the silane include capryl group-containing silicon compounds, amino group-containing silicon compounds such as 3-aminopropyltrimethoxysilane, N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and N-(2-aminoethyl)-3-aminopropylmethyldimethoxysilane, 3-chloropropyltrimethoxysilane, and 3-isocyanatepropyltriethoxysilane, or condensates of at least one of these with alkyl group-containing silicon compounds such as methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, and ethyltrimethoxysilane. These may be used alone or in combination of two or more.
[0079] The content of the silane coupling agent in the pressure-sensitive adhesive composition P is preferably 0.01 parts by mass or more, more preferably 0.05 parts by mass or more, and even more preferably 0.1 parts by mass or more, based on 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 10 parts by mass or less, more preferably 1 part by mass or less, and even more preferably 0.5 parts by mass or less. When the content of the silane coupling agent is within the above range, the obtained pressure-sensitive adhesive layer has improved adhesion to the flexible member that is the adherend, and has greater adhesive strength.
[0080] In the case where the adhesive composition P contains an active energy ray curable component (D) and ultraviolet rays are used as the active energy rays for curing the adhesive composition P, it is preferable that the adhesive composition P further contains a photopolymerization initiator. As the photopolymerization initiator, a conventionally known one can be used. The content of the photopolymerization initiator in the adhesive composition P is about 0.1 to 30 parts by mass with respect to 100 parts by mass of the active energy ray curable component (D).
[0081] It is also preferable that the adhesive composition P contains a tackifier, because by containing a tackifier, a predetermined adhesive strength can be easily obtained even in a thin adhesive layer.
[0082] Examples of tackifiers include natural resins such as rosin-based resins and polyterpene-based resins, petroleum resins such as C5-based, C9-based, and dicyclopentadiene-based resins, and synthetic resins such as coumarone-indene resins and xylene resins. These may be used alone or in combination of two or more.
[0083] When the adhesive composition P contains a tackifier, the content of the tackifier in the adhesive composition P is preferably 1 part by mass or more, particularly preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, per 100 parts by mass of the (meth)acrylic acid ester polymer (A). The content is preferably 90 parts by mass or less, particularly preferably 50 parts by mass or less, and even more preferably 30 parts by mass or less.
[0084] (2) Preparation of adhesive composition P The adhesive composition P can be produced by producing a (meth)acrylic acid ester polymer (A), mixing the obtained (meth)acrylic acid ester polymer (A) with a crosslinking agent (B) and high refractive index fine particles (C) (or a component for increasing refractive index), and adding additives as desired.
[0085] The (meth)acrylic acid ester polymer (A) can be produced by polymerizing a mixture of monomers constituting the polymer by a normal radical polymerization method. The polymerization of the (meth)acrylic acid ester polymer (A) is preferably carried out by a solution polymerization method using a polymerization initiator as desired. By polymerizing the (meth)acrylic acid ester polymer (A) by a solution polymerization method, it becomes easy to increase the molecular weight of the obtained polymer and adjust the molecular weight distribution, and further it becomes possible to reduce the generation of low molecular weight substances. Therefore, even if the gel fraction is relatively small and the degree of crosslinking is relaxed, the pressure-sensitive adhesive is unlikely to become biased due to bending, and a pressure-sensitive adhesive with excellent peel resistance is easily obtained.
[0086] Examples of the polymerization solvent used in the solution polymerization method include ethyl acetate, n-butyl acetate, isobutyl acetate, toluene, acetone, hexane, and methyl ethyl ketone, and two or more of these may be used in combination.
[0087] Examples of the polymerization initiator include azo compounds and organic peroxides, and two or more of them may be used in combination. Examples of the azo compounds include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2-methylbutyronitrile), 1,1'-azobis(cyclohexane 1-carbonitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethyl-4-methoxyvaleronitrile), dimethyl 2,2'-azobis(2-methylpropionate), 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-hydroxymethylpropionitrile), and 2,2'-azobis[2-(2-imidazolin-2-yl)propane].
[0088] Examples of organic peroxides include benzoyl peroxide, t-butyl perbenzoate, cumene hydroperoxide, diisopropyl peroxydicarbonate, di-n-propyl peroxydicarbonate, di(2-ethoxyethyl)peroxydicarbonate, t-butyl peroxyneodecanoate, t-butyl peroxypivalate, (3,5,5-trimethylhexanoyl)peroxide, dipropionyl peroxide, and diacetyl peroxide.
[0089] In the above polymerization step, the weight average molecular weight of the resulting polymer can be adjusted by adding a chain transfer agent such as 2-mercaptoethanol.
[0090] Once the (meth)acrylic acid ester polymer (A) is obtained, the crosslinking agent (B), high refractive index fine particles (C) (or a component for increasing refractive index), and optionally additives and a dilution solvent are added to the solution of the (meth)acrylic acid ester polymer (A) and thoroughly mixed to obtain a pressure-sensitive adhesive composition P (coating solution) diluted with the solvent.
[0091] In addition, when any of the above components is used in a solid state, or when precipitation occurs when the component is mixed with other components in an undiluted state, the component may be dissolved or diluted in a dilution solvent before being mixed with the other components.
[0092] Examples of the dilution solvent include aliphatic hydrocarbons such as hexane, heptane, and cyclohexane; aromatic hydrocarbons such as toluene and xylene; halogenated hydrocarbons such as methylene chloride and ethylene chloride; alcohols such as methanol, ethanol, propanol, butanol, and 1-methoxy-2-propanol; ketones such as acetone, methyl ethyl ketone, 2-pentanone, isophorone, and cyclohexanone; esters such as ethyl acetate and butyl acetate; and cellosolve-based solvents such as ethyl cellosolve.
[0093] The concentration and viscosity of the coating solution thus prepared are not particularly limited as long as they are within the range that allows coating, and can be appropriately selected according to the situation. For example, the adhesive composition P is diluted so that the concentration becomes 10 to 60 mass %. In addition, when obtaining the coating solution, the addition of a dilution solvent or the like is not a necessary condition, and if the adhesive composition P has a viscosity that allows coating, it is not necessary to add a dilution solvent. In this case, the adhesive composition P becomes a coating solution in which the polymerization solvent of the (meth)acrylic acid ester polymer (A) itself serves as the dilution solvent.
[0094] (3) Manufacture of adhesives The adhesive constituting the adhesive layer 11 in this embodiment is preferably obtained by crosslinking the adhesive composition P. The crosslinking of the adhesive composition P can usually be carried out by a heat treatment. This heat treatment can also serve as a drying treatment for volatilizing a diluting solvent and the like from a coating film of the adhesive composition P applied to a desired object.
[0095] The heating temperature in the heat treatment is preferably 50 to 150° C., and more preferably 70 to 120° C. The heating time is preferably 10 seconds to 10 minutes, and more preferably 50 seconds to 2 minutes.
[0096] After the heat treatment, a curing period of about 1 to 2 weeks may be provided at room temperature (e.g., 23°C, 50% RH) as necessary. If this curing period is required, the adhesive is formed after the curing period has elapsed, and if no curing period is required, the adhesive is formed after the heat treatment is completed.
[0097] By the above heat treatment (and curing), the (meth)acrylic acid ester polymer (A) is sufficiently crosslinked via the crosslinking agent (B) to form a crosslinked structure, thereby obtaining a pressure-sensitive adhesive.
[0098] When the adhesive composition P contains the active energy ray-curable component (D), the adhesive constituting the adhesive layer 11 is preferably obtained by thermally crosslinking and active energy ray-curing the adhesive composition P. In this case, it is preferable to cure the adhesive composition P by irradiating it with active energy rays after carrying out the heat treatment as described above.
[0099] Here, the active energy ray refers to an electromagnetic wave or a charged particle beam having an energy quantum, and specific examples thereof include ultraviolet rays, electron beams, etc. Among active energy rays, ultraviolet rays are particularly preferred because they are easy to handle.
[0100] The ultraviolet irradiation can be performed by a high pressure mercury lamp, a fusion H lamp, a xenon lamp, etc., and the amount of ultraviolet irradiation is 50 to 1000 mW / cm 2 . 2 The light intensity is preferably about 50 to 10,000 mJ / cm. 2 is preferably 80 to 5000 mJ / cm 2 More preferably, it is 200 to 2000 mJ / cm 2 On the other hand, the irradiation with the electron beam can be carried out by an electron beam accelerator or the like, and the irradiation dose of the electron beam is preferably about 10 to 1000 krad.
[0101] It is presumed that, when the adhesive composition P is irradiated with active energy rays, the multiple active energy ray-curable components (D) polymerize with each other, and the polymerized active energy ray-curable components (D) become entangled with the cross-linked structure of the (meth)acrylic acid ester polymer (A).
[0102] The high refractive index fine particles (C) are preferably uniformly dispersed in the pressure-sensitive adhesive layer 11. When the high refractive index fine particles (C) are uniformly dispersed in the pressure-sensitive adhesive layer 11, the haze value can be suppressed to a low value with good reproducibility.
[0103] (4) Thickness of the adhesive layer The thickness of the adhesive layer 11 in the adhesive sheet 1 according to this embodiment (measured according to JIS K7130) is preferably 1 μm or more as a lower limit, more preferably 5 μm or more, particularly preferably 10 μm or more, and even more preferably 20 μm or more. When the lower limit of the thickness of the adhesive layer 11 is within the above range, the desired adhesive strength is easily achieved.
[0104] The thickness of the adhesive layer 11 is preferably 1000 μm or less as an upper limit, more preferably 300 μm or less, particularly preferably 80 μm or less, and even more preferably 35 μm or less. When the upper limit of the thickness of the adhesive layer 11 is as above, the stress generated in the adhesive layer due to bending can be suppressed from becoming too large, and light leakage resistance can be improved. The adhesive layer 11 may be formed as a single layer, or may be formed by laminating multiple layers.
[0105] 1-2.Release sheet Release sheets 12a and 12b protect adhesive layer 11 until adhesive sheet 1 is used, and are peeled off when adhesive sheet 1 (adhesive layer 11) is to be used. In adhesive sheet 1 according to this embodiment, one or both of release sheets 12a and 12b are not necessarily required.
[0106] Examples of the release sheets 12a and 12b include polyethylene films, polypropylene films, polybutene films, polybutadiene films, polymethylpentene films, polyvinyl chloride films, vinyl chloride copolymer films, polyethylene terephthalate films, polyethylene naphthalate films, polybutylene terephthalate films, polyurethane films, ethylene vinyl acetate films, ionomer resin films, ethylene-(meth)acrylic acid copolymer films, ethylene-(meth)acrylic acid ester copolymer films, polystyrene films, polycarbonate films, polyimide films, and fluororesin films. Crosslinked films of these films are also used. Furthermore, laminated films of these films may be used.
[0107] The release surfaces of the release sheets 12a and 12b (particularly the surfaces in contact with the adhesive layer 11) are preferably subjected to a release treatment. Examples of release agents used in the release treatment include alkyd-based, silicone-based, fluorine-based, unsaturated polyester-based, polyolefin-based, and wax-based release agents. It is preferable that one of the release sheets 12a and 12b is a heavy release type release sheet having a large release strength, and the other is a light release type release sheet having a small release strength.
[0108] There is no particular limitation on the thickness of the release sheets 12a and 12b, but it is usually about 20 to 150 μm.
[0109] 2.Physical properties (adhesion) The adhesive strength of the adhesive sheet 1 according to the present embodiment to soda lime glass is preferably 0.01 N / 25 mm or more as a lower limit, more preferably 0.05 N / 25 mm or more, particularly preferably 0.1 N / 25 mm or more, and even more preferably 1.0 N / 25 mm or more. When the adhesive sheet 1 has the above lower limit of the adhesive strength to soda lime glass, the appearance after long-term bending is more excellent. On the other hand, the upper limit of the adhesive strength is not particularly limited, but reworkability may be required. From this viewpoint, the adhesive strength is preferably 50 N / 25 mm or less, more preferably 40 N / 25 mm or less, and particularly preferably 20 N / 25 mm or less. In addition, the adhesive strength in this specification basically refers to the adhesive strength measured by a 180-degree peeling method in accordance with JIS Z0237:2009, and a specific test method is as shown in the test example described later.
[0110] 3. Manufacturing of adhesive sheets As an example of manufacturing the adhesive sheet 1, a case where the adhesive composition P is used will be described. A coating solution of the adhesive composition P is applied to the release surface of one of the release sheets 12a (or 12b), and a heat treatment is performed to thermally crosslink the adhesive composition P to form a coating layer. The coating layer is then overlaid with the release surface of the other release sheet 12b (or 12a), and active energy rays are irradiated as desired. If a curing period is required, a curing period is left, and if no curing period is required, the coating layer becomes the adhesive layer 11 as is. In this way, the adhesive sheet 1 is obtained. The conditions for the heat treatment and curing are as described above.
[0111] In another manufacturing example of the adhesive sheet 1, a coating solution of the adhesive composition P is applied to the release surface of one release sheet 12a, and a heat treatment is performed to thermally crosslink the adhesive composition P to form a coating layer, thereby obtaining a release sheet 12a with a coating layer. In addition, a coating solution of the adhesive composition P is applied to the release surface of the other release sheet 12b, and a heat treatment is performed to thermally crosslink the adhesive composition P to form a coating layer, thereby obtaining a release sheet 12b with a coating layer. Then, the release sheet 12a with the coating layer and the release sheet 12b with the coating layer are bonded together so that both coating layers are in contact with each other, and active energy rays are irradiated as desired. If a curing period is required, a curing period is provided, and if no curing period is required, the laminated coating layer becomes the adhesive layer 11 as it is. This results in the above-mentioned adhesive sheet 1. According to this manufacturing example, even if the adhesive layer 11 is relatively thick, it is possible to stably manufacture it.
[0112] The coating solution of the pressure-sensitive adhesive composition P can be applied by, for example, bar coating, knife coating, roll coating, blade coating, die coating, gravure coating, or the like.
[0113] The pressure-sensitive adhesive layer 11 in this embodiment is formed as described above, so that the high refractive index fine particles (C) are uniformly dispersed throughout the layer.
[0114] [Display body] By using the pressure-sensitive adhesive sheet 1, various optical members and optical products can be manufactured, and in particular, displays can be manufactured. Examples of the types of displays include organic electroluminescence (organic EL) displays, electrophoretic displays (electronic paper), liquid crystal displays using a plastic substrate (film) as a substrate, and touch panels are also possible. Among the above displays, organic EL displays are particularly preferred. Light extraction efficiency is often required for organic EL displays, and the pressure-sensitive adhesive layer 11 of the pressure-sensitive adhesive sheet 1 has a high refractive index and therefore has excellent light extraction efficiency, making the pressure-sensitive adhesive sheet 1 particularly useful for organic EL displays.
[0115] The display body may be a bendable display, or may be a display that can be repeatedly bent (foldable display).
[0116] An example of a display, specifically an organic EL display, is shown in Fig. 2. The display 3 shown in Fig. 2 is formed by laminating, from the top, a cover film 31, a first adhesive layer 32, a polarizing film 33, a second adhesive layer 34, a touch sensor film 35, a third adhesive layer 36, an organic EL element 37, a fourth adhesive layer 38, and a TFT substrate 39. The cover film 31, the polarizing film 33, the touch sensor film 35, the organic EL element 37, and the TFT substrate 39 may be flexible members that can be bent.
[0117] At least one of the first adhesive layer 32, the second adhesive layer 34, the third adhesive layer 36, and the fourth adhesive layer 38 is the adhesive layer 11 of the adhesive sheet 1 described above. It is preferable that two or more of the first adhesive layer 32, the second adhesive layer 34, the third adhesive layer 36, and the fourth adhesive layer 38 are the adhesive layer 11 of the adhesive sheet 1 described above, and it is most preferable that all of the adhesive layers 32, 34, 36, and 38 are the adhesive layer 11 of the adhesive sheet 1.
[0118] The display 3 described above suppresses light leakage due to bending even when it is left in a bent state for a long period of time.
[0119] The above-described embodiments are described for the purpose of facilitating understanding of the present invention, and are not described for the purpose of limiting the present invention. Therefore, each element disclosed in the above embodiment is intended to include all design modifications and equivalents that fall within the technical scope of the present invention.
[0120] For example, either one or both of release sheets 12a, 12b in pressure-sensitive adhesive sheet 1 may be omitted, and a desired member (eg, a flexible member) may be laminated in place of release sheets 12a and / or 12b. EXAMPLES
[0121] The present invention will be described in more detail below with reference to examples, but the scope of the present invention is not limited to these examples.
[0122] Example 1 1. Preparation of (meth)acrylic acid ester polymer (A) 25 parts by mass of n-butyl acrylate, 60 parts by mass of 2-phenoxyethyl acrylate, and 15 parts by mass of 2-hydroxyethyl acrylate were copolymerized by solution polymerization to prepare a (meth)acrylic acid ester polymer (A). The molecular weight of this (meth)acrylic acid ester polymer (A) was measured by the method described below, and the weight average molecular weight (Mw) was 800,000.
[0123] 2. Preparation of adhesive composition 100 parts by mass (solid content equivalent; same below) of the (meth)acrylic acid ester polymer (A) obtained in step 1 above, 0.3 parts by mass of trimethylolpropane-modified tolylene diisocyanate (manufactured by Soken Chemical Industries, Ltd., product name "L-45") as a crosslinking agent (B), 100 parts by mass of a high refractive index component containing zirconium oxide microparticles (C1; manufactured by Sakata Inx Corporation, product name "Ecostage TM RT-HRU-1") as high refractive index microparticles (C), and 0.3 parts by mass of 3-glycidoxypropyltrimethoxysilane (Si1) as a silane coupling agent were mixed, thoroughly stirred, and diluted with methyl ethyl ketone to obtain a coating solution of an adhesive composition.
[0124] 3. Manufacturing of adhesive sheets The obtained adhesive composition coating solution was applied by a knife coater to the release-treated surface of a heavy-release type release sheet (manufactured by Lintec Corporation, product name "SP-PET382150"), one side of which was a polyethylene terephthalate film treated with a silicone-based release agent. The coating layer was then heat-treated at 90°C for 1 minute to form a coating layer.
[0125] Next, a light release type release sheet was laminated on the coating layer so that its release-treated surface was in contact with the coating layer, and ultraviolet light was irradiated through the light release type release sheet under the following conditions to harden the coating layer and form a 25 μm thick adhesive layer. This produced an adhesive sheet consisting of heavy release type release sheet / adhesive layer (thickness: 25 μm) / light release type release sheet. The thickness of the adhesive layer was measured using a constant pressure thickness gauge (manufactured by Techclock, product name "PG-02") in accordance with JIS K7130.
[0126] <Ultraviolet irradiation conditions> -Uses high pressure mercury lamp ·Illuminance 200mW / cm 2 ,Light intensity 200mJ / cm 2 The UV illuminance and light intensity meter used is the "UVPF-A1" manufactured by Eye Graphics.
[0127] Here, the formulations (solid content equivalent) of the pressure-sensitive adhesive composition when the (meth)acrylic acid ester polymer (A) is taken as 100 parts by mass (solid content equivalent) are shown in Table 1. The details of the abbreviations and the like shown in Table 1 are as follows. [(Meth)acrylic acid ester polymer (A)] BA: n-butyl acrylate 2EHA: 2-ethylhexyl acrylate PhEA: 2-phenoxyethyl acrylate HEA: 2-hydroxyethyl acrylate AA: Acrylic acid [High refractive index particles (C)] C1: High refractive index component containing nano-order zirconium oxide particles (manufactured by Sakata Inx Corporation, product name "Eco Stage TM RT-HRU-1", dispersion solution containing zirconium oxide particles, active energy ray curable components, photopolymerization initiators and dispersion solvents, refractive index of single coating film: 1.73 (measured according to JIS K0062-1992)) C2: Zirconium oxide microparticles (manufactured by Daiken Chemical Co., Ltd., product name "DLZ-007", average particle size: 10 nm, dispersion solvent: methyl ethyl ketone, dispersion solution concentration: 40% by mass, refractive index of microparticles: 1.9 (measured according to JIS K7142:2014 B method)) C3: Zirconium oxide microparticles (manufactured by Sakai Chemical Industry Co., Ltd., product name "SZR-K", average particle size: 6 nm, dispersion solvent: methyl ethyl ketone (63% by mass) and methanol (7% by mass), dispersion solution concentration: 30% by mass, refractive index of microparticles: 1.9 (measured according to JIS K7142:2014 B method)) [Silane coupling agents] Si1: 3-glycidoxypropyltrimethoxysilane Si2: 3-glycidoxypropylmethyldimethoxysilane [Tackifier] T1: Rosin-based tackifier (Arakawa Chemical Co., Ltd., product name "Pine Crystal ME-GH") T2: Rosin-based tackifier (Arakawa Chemical Co., Ltd., product name "Pine Crystal ME-G")
[0128] [Examples 2 to 8, Comparative Examples 1 to 5] An adhesive sheet was produced in the same manner as in Example 1, except that the types and ratios of the monomers constituting the (meth)acrylic acid ester polymer (A), the type and amount of the high refractive index fine particles (C), the type of silane coupling agent, and the type and amount of the tackifier were changed as shown in Table 1.
[0129] The weight average molecular weight (Mw) mentioned above is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC) under the following conditions (GPC measurement). <Measurement conditions> GPC measuring device: Tosoh HLC-8020 GPC columns (passed in the following order): Tosoh Corporation TSK guard column HXL-H TSK gel GMHXL (×2) TSK gel G2000HXL Measurement solvent: Tetrahydrofuran ·Measurement temperature: 40℃
[0130] [Test Example 1] (Evaluation of compatibility) The adhesive composition coating solution prepared in the examples and comparative examples was dispensed into a vial, and the degree of turbidity of the coating solution was visually judged. In addition, the state of the coating layer formed on the release-treated surface of the heavy release type release sheet in the examples and comparative examples was visually judged. Based on the judgment results, the compatibility of the adhesive composition was evaluated according to the following criteria. The results are shown in Table 2. ◯: The coating solution was transparent, and the coating layer was also transparent. Δ: The coating solution was cloudy, but the coating layer was transparent. ×: The coating solution was cloudy, and the transparency was not improved even after forming a coating layer.
[0131] The adhesive composition coating solutions of Comparative Examples 3 and 4 gelled and could not be coated, and an adhesive layer could not be formed, so other test examples were not carried out.
[0132] [Test Example 2] (Measurement of gel fraction) The adhesive sheets produced in the examples and comparative examples were cut to a size of 80 mm x 80 mm, the adhesive layer was wrapped in a polyester mesh (product name: Tetoron mesh #200), and the mass was measured using a precision balance. The mass of the mesh alone was subtracted to calculate the mass of the adhesive alone. This mass was designated M1.
[0133] Next, the adhesive wrapped in the polyester mesh was immersed in ethyl acetate at room temperature (23°C) for 24 hours. The adhesive was then removed and air-dried for 24 hours in an environment with a temperature of 23°C and a relative humidity of 50%, and then dried in an oven at 80°C for 12 hours. After drying, the mass was weighed using a precision balance, and the mass of the adhesive alone was calculated by subtracting the mass of the mesh alone. The mass at this time was designated M2. The gel fraction (%) was expressed as (M2 / M1) x 100. The results are shown in Table 2.
[0134] [Test Example 3] (Measurement of weight average molecular weight of sol content) The ethyl acetate used in the measurement of the gel fraction in Test Example 2 was concentrated with an evaporator to obtain a sol fraction. The sol fraction was then diluted with tetrahydrofuran to a 0.3% by mass solution, filtered through a 0.45 μm filter, and the weight average molecular weight (Mw) of the sol fraction was measured by GPC measurement. The measurement conditions for the GPC measurement were as described above. The results are shown in Table 2.
[0135] [Test Example 4] (Measurement of storage modulus G') The pressure-sensitive adhesive layers of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples were laminated together to form a laminate having a thickness of 800 μm. A cylindrical body having a diameter of 8 mm (height of 800 μm) was punched out from the resulting laminate of pressure-sensitive adhesive layers to form a sample.
[0136] The storage modulus G' of the above samples was measured under the following conditions by a torsional shear method using a viscoelasticity measuring device (manufactured by Anton Paar, product name "MCR302") in accordance with JIS K7244-1, and the storage modulus G' (MPa) at 23°C and the storage modulus G' (MPa) at 80°C were obtained. The results are shown in Table 2. Measurement frequency: 1Hz Measurement temperature: -20℃~150℃ Heating rate: 2℃ / min
[0137] [Test Example 5] (Measurement of refractive index) The (meth)acrylic acid ester polymer (A) prepared in the examples and comparative examples was diluted with a solvent and applied in the form of a layer on the release surface of a release film (manufactured by Lintec Corporation, product name "SP-PET382150"). Then, it was heated at 90°C for 1 minute to form a coating layer with a thickness of 25 μm. The refractive index of the formed coating layer was measured in accordance with JIS K0062-1992 using an Abbe refractometer (manufactured by Atago Corporation, product name "Abbe refractometer DR-M2", Na light source, wavelength: 589 nm). The results are shown in Table 1.
[0138] The refractive index of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheets produced in the Examples and Comparative Examples was measured in the same manner as above. The results are shown in Table 2.
[0139] In addition, the pressure-sensitive adhesive layers of Comparative Examples 1 and 2 were whitened, and therefore the refractive index could not be measured.
[0140] [Test Example 6] (Haze value measurement) The adhesive layer of the adhesive sheet produced in the examples and comparative examples was attached to glass to prepare a measurement sample. After background measurement was performed on the glass, the haze value (%) of the measurement sample was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH5000") in accordance with JIS K7136:2000. The results are shown in Table 2.
[0141] [Test Example 7] (Measurement of total light transmittance) The adhesive layer of the adhesive sheet produced in the examples and comparative examples was attached to glass to prepare a measurement sample. After background measurement was performed on the glass, the total light transmittance (%) of the measurement sample was measured using a haze meter (manufactured by Nippon Denshoku Industries Co., Ltd., product name "NDH5000") in accordance with JIS K7361-1:1997. The results are shown in Table 2.
[0142] [Test Example 8] (Measurement of adhesive strength) The light release type release sheet was peeled off from the adhesive sheet produced in the Examples and Comparative Examples, and the exposed adhesive layer was attached to an easy-adhesion layer of a polyethylene terephthalate (PET) film (manufactured by Toyobo Co., Ltd., product name "PET A4300", thickness: 100 μm) having an easy-adhesion layer to obtain a heavy release type release sheet / adhesive layer / PET film laminate. The obtained laminate was cut to a width of 25 mm and a length of 110 mm.
[0143] The heavy release type release sheet was peeled off from the laminate under an environment of 23°C and 50% RH, and the exposed adhesive layer was attached to one side of a soda lime glass plate (manufactured by Nippon Sheet Glass Co., Ltd., product name "Soda Lime Glass", thickness: 1.1 mm), and pressurized for 20 minutes at 0.5 MPa and 50°C in an autoclave manufactured by Kurihara Seisakusho Co., Ltd. After that, the laminate was left for 24 hours under conditions of 23°C and 50% RH, and the adhesive strength (N / 25mm) was measured when the laminate of the PET film and the adhesive layer was peeled off from the adherend using a tensile tester (manufactured by Orientec Co., Ltd., Tensilon) under conditions of a peel speed of 300 mm / min and a peel angle of 180 degrees. The measurement was performed under conditions other than those described here in accordance with JIS Z0237:2009. The results are shown in Table 2.
[0144] [Test Example 9] (Evaluation of light leakage resistance) A number of COP polarizing plates (60 μm thick) were prepared, each of which was made by laminating a triacetyl cellulose (TAC) film (25 μm thick), a polyvinyl alcohol (PVA) film polarizer (12 μm thick), and a cycloolefin polymer (COP) film (23 μm thick) in that order. The surfaces of the COP polarizing plates that were to be bonded to the adhesive layer were corona-treated.
[0145] The light release type release sheet was peeled off from the adhesive sheet produced in the examples and comparative examples, and the exposed adhesive layer was attached to the TAC film side of one COP polarizer. Next, the heavy release type release sheet was peeled off, and the exposed adhesive layer was attached to the COP film side of another COP polarizer in a cross-nicol state. Then, it was pressurized at 0.5 MPa and 50°C for 20 minutes in an autoclave manufactured by Chiyoda Electric Industry Co., Ltd., and then left for 24 hours under conditions of 23°C and 50% RH. The laminate consisting of the COP polarizer / adhesive layer / COP polarizer obtained in this way was cut into a width of 50 mm and a length of 200 mm, which was used as a sample.
[0146] The obtained sample was held in a bent state between two holding plates (distance between each other: 3 mm) consisting of two standing glass plates as shown in FIG. 3 for 1000 hours using a durability tester (manufactured by Yuasa System Co., Ltd., product name "Planar body unloaded U-shaped expansion and contraction tester, model: CL09-typeD01-FSC90") (test conditions are as follows). After that, the bent state was released and the sample was left for 24 hours in an environment of 23°C and 50% RH. Then, light leakage was visually confirmed using transmitted light from a backlight (manufactured by Dentsu Sangyo Co., Ltd., product name "HF-SL-A312LC"), and light leakage resistance was evaluated according to the following criteria. The results are shown in Table 2.
[0147] <Test conditions> Bending direction: Bending so that the TAC film of one COP polarizer is on the outside and the COP film of the other COP polarizer is on the inside. Minimum bending diameter: 3mmφ Bending time: 1000 hours Test environment: 60℃, 50% RH <Evaluation criteria for light leakage resistance> No light leakage occurred at the bent portion. ◯: A slight amount of light leakage occurred at the bent portion, but was at a level that did not cause any practical problems. △: Light leakage occurred at the bent portion. ×: Light leakage occurred at the bent portion, and the light leakage spread to the periphery of the bent portion.
[0148] [Test Example 10] (Evaluation of appearance after long-term bending) The test was carried out in the same manner as in Test Example 9, except that the test temperature was changed to 80° C., and then the appearance after long-term bending was evaluated according to the following criteria. ◎: No changes were observed in the bent portion or its surroundings. ◯: A few air bubbles were found either at the bent portion or in the vicinity thereof, but no peeling was found. Δ: A series of air bubbles were observed either at the bent portion or in its vicinity, but no peeling was observed. ×: Large bubbles or peeling was observed either at the bent portion or in the vicinity thereof.
[0149] [Table 1]
[0150] [Table 2]
[0151] As can be seen from Table 2, the adhesive layer of the adhesive sheet of the example had excellent light leakage resistance when two flexible members were attached and left in a bent state for a long time. In addition, the adhesive layer of the adhesive sheet of the example also had excellent appearance after being bent for a long time. [Industrial Applicability]
[0152] The present invention is suitable for bonding one flexible member and another flexible member that constitute a display body. [Explanation of symbols]
[0153] 1...Adhesive sheet 11...Adhesive layer 12a, 12b...Release sheet 3...Display body 31…Cover film 32...First adhesive layer 33...Polarizing film 34...Second adhesive layer 35...Touch sensor film 36...Third adhesive layer 37...Organic EL element 38...Fourth adhesive layer 39...TFT substrate S: Test piece P…Retaining plate
Claims
1. A pressure-sensitive adhesive sheet having at least a pressure-sensitive adhesive layer, The refractive index of the adhesive constituting the adhesive layer is 1.55 or more, The pressure-sensitive adhesive has a gel fraction of 30% or more and 100% or less, The haze value of the pressure-sensitive adhesive layer is 10% or less, the pressure-sensitive adhesive is an acrylic pressure-sensitive adhesive containing high refractive index fine particles, the acrylic pressure-sensitive adhesive contains a (meth)acrylic acid ester polymer, The (meth)acrylic acid ester polymer contains an aromatic ring-containing monomer as a monomer unit constituting the polymer. A pressure-sensitive adhesive sheet characterized by:
2. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive layer has a total light transmittance of 70% or more.
3. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive has a storage modulus G' at 23° C. of 0.05 MPa or more and 20 MPa or less.
4. 4. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive has a storage modulus G' at 80° C. of 0.01 MPa or more and 15 MPa or less.
5. 5. The pressure-sensitive adhesive sheet according to claim 1, wherein the weight-average molecular weight of the sol component of the pressure-sensitive adhesive is 10,000 or more and 2,000,000 or less.
6. Two release sheets; the pressure-sensitive adhesive layer sandwiched between the two release sheets so as to be in contact with the release surfaces of the two release sheets; The pressure-sensitive adhesive sheet according to any one of claims 1 to 5, characterized in that it comprises:
7. 7. The pressure-sensitive adhesive sheet according to claim 1, which is for use as a display material.
Citation Information
Patent Citations
Optical adhesive composition, optical adhesive, and optical film
JP2011093957A
Pressure-sensitive adhesive composition which is excellent in heat resistance, pressure-sensitive adhesive layer, and pressure-sensitive adhesive sheet
JP2012001695A
Adhesive composition, adhesive and adhesive sheet
JP2015010192A
Composition for transparent adhesive sheet, and transparent adhesive sheet
JP2016020442A
Adhesive for optical film, adhesive layer for optical film, optical member and image display device
JP2016108555A