Bio-based reactive plasticizers, and adhesives and sealants containing the same

Biobased reactive plasticizers derived from vegetable oils address migration and hardening issues in adhesives and sealants, offering improved mechanical properties and sustainability without compromising performance.

JP7579707B2Active Publication Date: 2024-11-08HENKEL KGAA
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2020568026
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-02-27
Filing Date
2019-02-13
Publication Date
2024-11-08
Estimated Expiration
2039-02-13

AI Technical Summary

Technical Problem

Existing adhesives and sealants face challenges with plasticizer migration, undesirable hardening during storage, and the need for sustainable, renewable materials that maintain performance comparable to non-sustainable products.

Method used

Development of biobased reactive plasticizers derived from vegetable oils functionalized with mercaptoalkoxysilane, which reduce migration, allow for selective adjustment of mechanical properties, and act as antioxidants, while being compatible with silyl-terminated polymers.

Benefits of technology

The new plasticizers provide adhesives and sealants with reduced migration, improved mechanical properties, and extended storage stability, while utilizing renewable resources and potentially reducing the need for conventional plasticizers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579707000001
    Figure 0007579707000001
  • Figure 0007579707000002
    Figure 0007579707000002
  • Figure 0007579707000003
    Figure 0007579707000003
Patent Text Reader

Abstract

The present invention relates to novel reactive (moisture-curable) plasticizers of formula (I) as described herein, and adhesives and sealants containing them for bonding and sealing substrates.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel reactive (moisture-curable) plasticizer, and an adhesive and a sealant containing the same for bonding and sealing substrates. The reactive plasticizer of the present invention is a bio-based plasticizer derived from vegetable oil functionalized with mercaptoalkoxysilane. By using the novel reactive plasticizer according to the present invention, adhesives and sealants can be obtained in which the migration of the plasticizer is reduced or is not present. Furthermore, the mechanical properties can be selectively adjusted depending on the amount of alkoxysilane groups contained in the plasticizer, leading to improvements in the adhesives and sealants. [Background technology]

[0002] Generally, there are two types of plasticizers for adhesives and sealants: reactive and non-reactive. Generally, plasticizers are petrochemical-based, without moisture-reactive functional groups. The technical advantage of reactive plasticizers is that the migration of classical plasticizers to the surface, which leads to adhesion difficulties, is avoided. This is achieved by chemical reaction of the reactive (functionalized) plasticizer with the other components of the adhesive.

[0003] Recently, there is a demand in the market for sustainable products based on renewable raw materials. In particular, there is a need for adhesives and sealants that contain a high amount of renewable raw materials. The use of such materials can essentially contribute to sustainability goals such as carbon footprint. Furthermore, the performance of these products must be at least comparable to non-sustainable products. Summary of the Invention [Problem to be solved by the invention]

[0004] It is an object of the present invention to provide a renewable (bio)material-based reactive plasticizer that can be used in adhesives or sealants that contain a silyl-terminated polymer as the base polymer.

[0005] To date, reactive plasticizers based on mercaptoalkoxysilane-modified vegetable oils are not known. It was common knowledge among those skilled in the art that functionalization of vegetable oils with mercaptoalkoxysilanes was difficult. In this regard, it was assumed that sulfur-containing compounds interact with the catalyst during the reaction, inhibiting its activity. Furthermore, it was assumed that storage of the final adhesive or sealant at higher temperatures would lead to undesirable side reactions between the components used (e.g., transesterification between alkoxysilanes and triglycerides), resulting in undesirable hardening in the cartridge. [Means for solving the problem]

[0006] The above problems are solved by the novel compounds of formula (I) of the present invention. It has been found by the inventors of the present invention that certain compounds of formula (I) of the present invention are suitable as reactive and therefore non-migratory plasticizers. An advantageous property compared to conventional plasticizers is the significantly reduced migration of the newly identified compounds. Furthermore, the amount of conventional plasticizers used can be reduced when they are partially or completely replaced by the plasticizers according to the present invention. Furthermore, it has been found that the compounds of the present invention are suitable for certain adhesive and sealant compositions of the present invention. Surprisingly, it has been found that certain adhesives and sealants of the present invention are capable of long-term storage without hardening. Surprisingly, it is possible to selectively increase or modify the tensile strength and tensile elongation. Furthermore, it has been found that the compounds of the present invention simultaneously function as antioxidants when used in adhesive and sealant compositions. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] A "composition" is understood in the context of the present invention as a mixture of at least two components / compounds.

[0008] The term "hardenable" is understood to mean that the composition can change from a relatively soft, possibly plastically ductile, state to a harder state under the influence of external conditions, in particular under the influence of moisture present in the environment and / or provided for this purpose. In general, crosslinking can be carried out by chemical and / or physical influences, i.e. in addition to the already mentioned moisture, for example by the provision of energy in the form of heat, light or other electromagnetic radiation, but also simply by contacting the composition with air or reactive components.

[0009] In the Markush formula of the present invention, only the trans configuration of the double bond is depicted for ease of representation, but all double bonds in the molecule may have cis or trans configuration, independently of each other. Furthermore, all numerical values ​​given in the formula are integers, e.g., when r is 1-3, r is 1, 2 or 3.

[0010] The number average molecular weight Mn and the weight average molecular weight Mw are determined according to the invention by gel permeation chromatography (GPC, also known as SEC) at 23° C. using styrene standards. This method is known to those skilled in the art. The polydispersity is derived from the average molecular weights Mw and Mn. It is calculated as PD=Mw / Mn.

[0011] The BET value is determined in accordance with DIN ISO 9277:2014-01.

[0012] As used herein, the terms "a" and "an" and "at least one" are the same as the term "one or more" and may be used interchangeably. "At least one" means one or more, i.e., 1, 2, 3, 4, 5, 6, 7, 8, 9, or more. "At least one" as used herein with respect to any component refers to the number of chemically distinct molecules, i.e., the number of different kinds of the referenced species, and not the total number of molecules. For example, "at least one polyol" means that at least one type of molecule that fits the definition of a polyol is used, and that there may be two or more different types of molecules that fit this definition, and does not mean that there is only one molecule of said polyol.

[0013] All percentages stated herein in relation to compositions or formulations relate to weight % based on the total weight of the respective composition or formulation, unless otherwise stated.

[0014] In the present invention, when a group is described as being substituted, preferred substituents are selected from: -OH, -OCH3, -F, -Cl, -Br, -I, ═O, -NO2 and -NH2.

[0015] The present invention relates in particular to the following:

[0016] [1] Formula (I): [ka] [In the formula, m=0~25; n = 0–25; q=0~50; p = 0 to 5; r=1~3; Within each unit p or r, each m, n, and q is independently selected; X is independently H or -SR 1 Selected from; R 1 =-(CH2) 1-10 Si(O(CH2)0-8 CH3)3, preferably -(CH2) 1-5 Si(O(CH2) 0-3 More preferably, it is -(CH2)3Si(OCH3)3 or -(CH2)3Si(O(CH2)2CH3)3, provided that there are two or more -SR 1 When present, they are not attached to adjacent carbon atoms, and said -SR 1 the group is not attached to a carbon atom that is bonded to an adjacent carbon atom by a double bond, and preferably is not attached to a carbon atom alpha to a double bond; and R 2 = Substituted or unsubstituted aliphatic C 1-12 Hydrocarbon group, preferably a saturated unsubstituted aliphatic C 1-12 Hydrocarbon group; more preferably saturated unsubstituted aliphatic C 1-6 A hydrocarbon group, most preferably a saturated unsubstituted aliphatic C 1-3 is a hydrocarbon group. Compound. [2] p=1 to 3, preferably 1 or 2, more preferably 1; m=1 to 25, preferably 2 to 15, more preferably 3 to 10; n=1 to 25, preferably 2 to 15, more preferably 3 to 10; and q=0 The compound according to [1], [3] p=0; q=2 to 50, preferably 5 to 40, more preferably 10 to 20 The compound according to [1], [4] The compound according to any one of [1] to [3], wherein r=1. [5] The compound according to any one of [1] to [3], wherein r=3. [6] 1 to 10 -SR 1 , preferably 1 to 5 -SR 1 , more preferably one or two -SR 1 , most preferably one -SR 1The compound according to any one of [1] to [5], wherein [7] The compound of formula (I) is derived from an oil selected from the group consisting of rapeseed oil, soybean oil, castor oil, linseed oil, palm oil, palm kernel oil, tall oil, jatropha oil, candlenut oil, grapeseed oil, sunflower oil, medium oleic sunflower oil, high oleic sunflower oil, canola oil, corn oil, cashew nut oil, or algae oil or chemically / biologically produced triglycerides such as trioleates. [8] Formula (II): [ka] [In the formula, s=0~101; t=0~101; u=1~20; v=1~3; and R 2 is defined as in [1]. The compound of R 1 Compound HSR is defined as in [1] 1 and reacting in the presence of a catalyst. A method for producing a compound of formula (I) according to any one of [1] to [7], comprising: [9] The method according to [8], wherein the reaction is carried out at a temperature of 30 to 100°C, preferably 50 to 90°C, and more preferably 70 to 85°C.

[10] Use of the compound according to any one of [1] to [7] as a reactive plasticizer, preferably as a reactive plasticizer in an adhesive composition.

[11] A) at least one silyl-terminated polymer; B) at least one compound according to any one of [1] to [7]; C) optionally, at least one filler; and D) Optionally, one or more auxiliary substances 1. An adhesive or sealant composition comprising:

[12] The adhesive or sealant composition according to

[11] , wherein the amount of the at least one compound B is 0.1 to 30% by weight based on the total weight of the composition.

[13] 10 to 80% by weight, preferably 10 to 50% by weight, more preferably 15 to 35% by weight of A; 0.1 to 30% by weight, preferably 0.1 to 20% by weight, more preferably 1 to 10% by weight of B; 0 to 70% by weight, preferably 20 to 60% by weight, more preferably 30 to 50% by weight of C; and 0 to 60% by weight, preferably 1 to 30% by weight, more preferably 1 to 10% by weight of D The adhesive composition or sealant composition according to

[11] or

[12] , which comprises or consists of:

[0017] It was found that the tensile strength can vary depending on the number of silyl groups added and the nature (base structure) of the reactive plasticizer, such as triglyceride or methyl ester. In particular, a low number of alkoxysilyl groups resulted in a softer adhesive, while a high number increased brittleness. Without wishing to be bound by any theory, it is assumed that the reactive plasticizer underwent partial transesterification with the other components of the composition. Said transesterification occurred without a significant increase in the viscosity of the composition, and no undesirable hardening during storage was observed. It appears that chemical modification of the compounds of the invention results in better incorporation and bonding with the other components of the composition during storage. Thus, depending on the amount of alkoxysilyl groups and the nature of the reactive plasticizer, it is possible to selectively adjust the mechanical properties from soft and elastic to hard and brittle. Another option for adjusting the mechanical properties is to use compounds of the invention that are not fully saturated, i.e. still have double bonds remaining in the structure. They have the additional advantage of being more sustainable by reducing the amount of raw materials required. A further technical advantage of the compounds of the invention is that, via their thioether groups, they can also act as antioxidants. In particular, thioether groups can be oxidized to sulfones when in contact with radicals, and therefore the loadings of antioxidants commonly used in adhesives or sealants can be lowered or avoided altogether.

[0018] To obtain the compounds of the invention, a compound containing at least one double bond is reacted with a compound of formula HSR as defined above. 1This is carried out in the presence of a catalyst. Suitable commonly known catalysts include, for example, azo compounds such as azobisisobutyronitrile, 1,1'-azobis(cyclohexanecarbonitrile), azobenzene, and peroxides such as dibenzoyl peroxide, di-tert-butyl peroxide, methyl ethyl ketone peroxide, acetone peroxide, hydrogen peroxide, peroxodisulfate, and also benzophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-benzoylcyclohexanol, methyl ethyl ketone, etc. However, ultraviolet light and common photopolymerization initiators may also be used. Thermally induced radical reactions are preferred.

[0019] For reference, "-SR 1 The -SR group is characterized in that it is not attached to a carbon atom that is connected to an adjacent carbon atom by a double bond. This is the case in a double-bonded structural element of the formula -H2C=CH2-, 1 means that a hydrogen atom attached to a carbon atom forming a double bond cannot be replaced. 1 The characteristic that the group is "not attached to a carbon atom alpha to a double bond" is represented by the formula -C * H2-CR2=CR2-C * In the structural element H2- (where R is H or alkyl), this means that it is not bonded to the carbon atom marked with an asterisk.

[0020] The present invention also relates to an adhesive composition or sealant composition (hereinafter simply referred to as "composition") containing a specific compound of the present invention. The adhesive composition or sealant composition is preferably a curable composition.

[0021] The composition may further comprise reactive or non-reactive plasticizers generally known to those skilled in the art, different from the compounds according to the present invention, but in a preferred embodiment, the presence of additional plasticizers is 10% by weight or less, preferably 5% by weight or less, more preferably 0.5% by weight or less, most preferably 0.001% by weight or less. In a further preferred embodiment, the composition does not comprise any additional plasticizers.

[0022] The composition comprises at least one basic polymer. Suitable polymers include, for example, those represented by the general formula (III): -A n -R-SiXYZ (III) [In the formula, A is a divalent or trivalent linking group containing at least one heteroatom; R is selected from divalent hydrocarbon groups having 1 to 12 carbon atoms; X, Y, Z are independently selected from the group consisting of hydroxyl, C1-C8 alkyl, C1-C8 alkoxy, and C1-C8 acyloxy, where X, Y, Z are substituents directly bonded to a Si atom, or two of the substituents X, Y, Z form a ring together with the Si atom to which they are bonded, and at least one of the substituents X, Y, Z is selected from the group consisting of hydroxyl, C1-C8 alkoxy, and C1-C8 acyloxy; and n is 0 or 1. is a polymer having at least one end group of

[0023] In a preferred embodiment, the polymer has at least two end groups of general formula (III).

[0024] The polymer having at least one end group of general formula (III) is preferably a polyether, a poly(meth)acrylate, or a polyurethane.

[0025] "Polyether" is understood to be a polymer whose organic repeating units contain ether functional groups COC in the main chain. Polymers with lateral ether groups, such as cellulose ethers, starch ethers and vinyl ether polymers, as well as polyacetals, such as polyoxymethylene (POM), are not included in polyethers.

[0026] "Poly(meth)acrylate" is understood to be a polymer based on (meth)acrylate. It therefore has the structural motif -CH2-CR as a repeating unit. a (COOR b )-, where R a represents a hydrogen atom (acrylate ester) or a methyl group (methacrylate ester), and R b represents a straight chain alkyl group, a branched alkyl group, a cycloalkyl group and / or an alkyl group containing functional substituents, such as a methyl, ethyl, isopropyl, cyclohexyl, 2-ethylhexyl or 2-hydroxyethyl group.

[0027] "Polyurethane" is understood to be a polymer having at least two urethane groups --NH--CO--O-- in the main chain.

[0028] The polymer containing at least one end group of general formula (III) is preferably a polyether. Polyether has a flexible and elastic structure, and can produce a composition with excellent elastic properties. Polyether has a flexible backbone, but also has strength at the same time. Therefore, polyether is not attacked or decomposed by, for example, water and bacteria, in contrast to, for example, polyester.

[0029] The number-average molecular weight Mn of the polyether on which the polymer is based is preferably 2000 to 100,000 g / mol (Dalton), particularly preferably at least 6000 g / mol, particularly preferably at least 8000 g / mol. The polyethers used in the present invention advantageously have a number-average molecular weight of at least 2000 g / mol, since compositions according to the invention based on polyethers with such a minimum molecular weight have significant film-forming properties. For example, the number-average molecular weight Mn of the polyether is 4000 to 100,000, preferably 8000 to 50,000, particularly preferably 10,000 to 30,000, in particular 10,000 to 25,000 g / mol. These molecular weights are particularly advantageous, since the corresponding compositions have a balanced ratio of viscosity (ease of processing), strength and elasticity.

[0030] Particularly advantageous viscoelastic properties can be achieved when polyethers with narrow molecular weight distributions and therefore low polydispersity are used. These can be obtained, for example, by so-called double metal cyanide catalysts (DMC catalysts). Polyethers produced in this way are distinguished by a particularly narrow molecular weight distribution, a high average molecular weight, and a very low number of double bonds at the ends of the polymer chains.

[0031] Thus, in a preferred embodiment of the invention, the maximum polydispersity Mw / Mn of the polyether on which the polymer is based is 3, more preferably 1.7, and most preferably 1.5.

[0032] The ratio Mw / Mn (polydispersity) indicates the width of the molecular weight distribution and therefore the difference in the degree of polymerization of the individual chains in a polydisperse polymer. For many polymers and polycondensates, a polydispersity of about 2 applies. Strict monodispersity exists at a value of 1. A low polydispersity, for example less than 1.5, indicates a relatively narrow molecular weight distribution and therefore a specific expression of the properties related to molecular weight, such as, for example, viscosity. Thus, in particular, in the context of the present invention, the polyether on which polymer A is based has a polydispersity (Mw / Mn) of less than 1.3.

[0033] In a preferred embodiment, the polymer having at least one end group of general formula (III) may be a polyurethane obtained by reaction of at least i) one polyol or a mixture of two or more polyols with ii) one polyisocyanate or a mixture of two or more polyisocyanates.

[0034] A "polyol" is understood to be a compound containing at least two OH groups, regardless of whether the compound contains other functional groups. However, it is preferred that the polyols used according to the invention contain only OH groups as functional groups, or, if other functional groups are present, none of these other functional groups reacts with isocyanates, at least under the conditions prevailing during the reaction of the polyol and the polyisocyanate.

[0035] The polyol suitable for preparing the polyurethane according to the invention is preferably a polyether polyol.The above explanations regarding the molecular weight and polydispersity of polyethers apply to polyether polyols.The polyether polyol is preferably a polyalkylene oxide, particularly preferably a polyethylene oxide and / or a polypropylene oxide.In a preferred embodiment, a polyether or a mixture of two polyethers is used.

[0036] The polyols used according to the invention preferably have an OH number of about 5 to about 15, more preferably about 10. The content of primary OH groups is preferably less than about 20%, more preferably less than about 15%, based on all OH groups. In a particularly advantageous embodiment, the acid number of the polyethers used is less than about 0.1, preferably less than about 0.05, more preferably less than about 0.02.

[0037] In addition to the polyether, the polyol mixture may contain other polyols, for example polyester polyols having a molecular weight of about 200 to about 30,000 g / mol.

[0038] A "polyisocyanate" is understood to be a compound having at least two isocyanate groups -NCO. The compound does not necessarily have to be a polymer, but is instead often a low molecular weight compound.

[0039] Polyisocyanates suitable for the preparation of the polyurethanes according to the invention include ethylene diisocyanate, 1,4-tetramethylene diisocyanate, 1,4-tetramethoxybutane diisocyanate, 1,6-hexamethylene diisocyanate (HDI), cyclobutane-1,3-diisocyanate, cyclohexane-1,3- and -1,4-diisocyanate, bis(2-isocyanatoethyl) fumarate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), 2,4- and 2,6-hexahydrotoluylene diisocyanate, hexahydro-1,3- or -1,4-diisocyanate, bis(2-isocyanatoethyl) fumarate, 1-isocyanato-3,3,5-trimethyl-5-isocyanatomethylcyclohexane (isophorone diisocyanate, IPDI), bis(2-isocyanatoethyl) fumarate, ... Examples of isocyanates include 4-phenylene diisocyanate, benzidine diisocyanate, naphthalene-1,5-diisocyanate, 1,6-diisocyanato-2,2,4-trimethylhexane, 1,6-diisocyanato-2,4,4-trimethylhexane, xylylene diisocyanate (XDI), tetramethylxylylene diisocyanate (TMXDI), 1,3- and 1,4-phenylene diisocyanate, 2,4- or 2,6-toluylene diisocyanate (TDI), 2,4'-diphenylmethane diisocyanate, 2,2'-diphenylmethane diisocyanate, or 4,4'-diphenylmethane diisocyanate and isomeric mixtures thereof. Also suitable are partially or fully hydrogenated cycloalkyl derivatives of MDI, such as fully hydrogenated MDI (H 12-MDI), alkyl-substituted diphenylmethane diisocyanates such as mono-, di-, tri-, or tetraalkyldiphenylmethane diisocyanates and their partially or fully hydrogenated cycloalkyl derivatives, 4,4'-diisocyanatophenylperfluoroethane, phthalic acid bis-isocyanatoethyl ester, 1-chloromethylphenyl-2,4- or -2,6-diisocyanate, 1-bromomethylphenyl-2,4- or -2,6-diisocyanate, 3,3'-bis-chloromethylether-4,4'-diphenyl diisocyanate, sulfur-containing diisocyanates such as those obtained by reacting two moles of a diisocyanate with one mole of thiodiglycol or dihydroxydihexyl sulfide, diisocyanates of dimer fatty acids, or mixtures of two or more diisocyanates. The polyisocyanate is preferably IPDI, TDI or MDI.

[0040] Other polyisocyanates suitable for use according to the invention are isocyanates with a functionality of three or more which can be obtained, for example, by oligomerization of diisocyanates, more particularly by oligomerization of the isocyanates mentioned above. Examples of such tri- and higher isocyanates are the triisocyanurates of HDI or IPDI, or mixtures thereof, or mixed triisocyanurates thereof, and the polyphenylmethylene polyisocyanates obtained by phosgenation of aniline / formaldehyde condensates.

[0041] It is preferred that there is a stoichiometric excess of NCO groups of the polyisocyanate present relative to the hydroxyl groups of the polyol. "Polyol" and "polyisocyanate" in each case include the presence of only one polyol and / or only one polyisocyanate. This stoichiometric excess must be present under the process conditions, i.e., it is insufficient if the excess is nominally present. Since some of the NCO groups of the polyisocyanate react with reactants other than the OH groups of the polyol, for example monofunctional alcohols, a virtual deficiency of NCO groups of the polyisocyanate relative to the OH groups of the polyol occurs. The ratio of the number of OH groups of the polyol to the number of NCO groups of the polyisocyanate is particularly preferably 1:3 to 1:1.1, in particular 1:2.5 to 1:1.5.

[0042] Formula (III): -A n -R-SiXYZ (III) Further suitable polymers having end groups of the formula: wherein A is a divalent or trivalent linking group containing at least one heteroatom, R is selected from divalent hydrocarbon groups having 1 to 12 carbon atoms, and X, Y, Z are each independently selected from the group consisting of hydroxyl groups, C1-C8 alkyl, C1-C8 alkoxy, and C1-C8 acyloxy groups, where X, Y, Z are substituents directly bonded to the Si atom or two of the substituents X, Y, Z form a ring together with the Si atom to which they are bonded, and at least one of the substituents X, Y, Z is selected from the group consisting of hydroxyl groups, C1-C8 alkoxy groups, and C1-C8 acyloxy groups, and n is 0 or 1.

[0043] In this context, a divalent or trivalent linking group A containing at least one heteroatom is understood to be a divalent or trivalent chemical group that connects the polymer backbone of the silane-terminated polymer with the group R of formula (III). For example, the divalent or trivalent linking group A can be formed as an amide or urethane group, for example by reaction of a hydroxyl-functionalized polyether with isocyanatosilane, for example during the preparation of the alkoxysilane- and / or acyloxysilane-terminated polymer. The linking group can be either distinguishable or not from the structural features occurring in the underlying polymer backbone. The latter is, for example, when it is identical to the connection point of the repeating units of the polymer backbone.

[0044] The index "n" corresponds to 0 (zero) or 1, i.e., the divalent linking group A connects the polymer backbone to the group R (n=1), or the polymer backbone is directly bonded or connected to the group R (n=0).

[0045] In some embodiments, the divalent or trivalent linking group A of general formula (III) is preferably an oxygen atom, or a group [ka] where R″ is selected from the group consisting of a hydrogen atom and an alkyl or aryl group having 1 to 12 carbon atoms, or a substituted or unsubstituted amide, carbamate, urethane, urea, imino, carboxylate, carbamoyl, amidino, carbonate, sulfonate or sulfinate group. Particularly preferred as linking group A are urethane and urea groups which can be obtained by reacting certain functional groups of the prepolymer with organosilanes carrying further functional groups. Urethane groups can be formed, for example, either when the polymer backbone contains terminal hydroxy groups and isocyanatosilanes are used as further components, or, conversely, when a polymer carrying terminal isocyanate groups reacts with an alkoxysilane containing terminal hydroxy groups. Similarly, urea groups can be obtained by the use of terminal primary or secondary amino groups, either in the silane or in the polymer, which react with terminal isocyanate groups present in the respective reactants. This means that either an aminosilane is reacted with a polymer having terminal isocyanate groups, or a polymer which is terminally substituted with amino groups is reacted with an isocyanatosilane.

[0046] The urethane and urea groups advantageously increase the strength of the polymer chain and the overall strength of the crosslinked polymer.

[0047] The radical R is a divalent hydrocarbon radical having 1 to 12 carbon atoms. The hydrocarbon radical may be a linear, branched or cyclic alkylene radical. The hydrocarbon radical may be saturated or unsaturated. R is preferably a divalent hydrocarbon radical having 1 to 6 carbon atoms. The curing speed of the composition may be influenced by the length of the hydrocarbon radical forming one of the binding links or the binding link between the polymer backbone and the silyl group. Particularly preferably, R is a methylene, ethylene or n-propylene radical, in particular a methylene or n-propylene radical.

[0048] Alkoxysilane-terminated compounds having a methylene group as the connecting link to the polymer backbone (so-called "alpha silanes") have a particularly high reactivity of the terminal silyl groups, which shortens the cure time and therefore leads to very rapid cure of formulations based on these polymers.

[0049] In general, the longer the connecting hydrocarbon chain, the lower the reactivity of the polymer. In particular, "gamma silanes" containing branched propylene groups as connecting links provide a good balance between the required reactivity (acceptable cure time) and delayed cure (open time, possibility of post-connection modification). Thus, by carefully combining alpha and gamma alkoxysilane terminal building blocks, the cure rate of the system can be influenced as desired.

[0050] Within the context of the present invention, R is most particularly preferably an n-propylene radical.

[0051] X, Y, Z are independently selected from the group consisting of hydroxyl, C1-C8 alkyl, C1-C8 alkoxy and C1-C8 acyloxy groups, where at least one of the substituents X, Y, Z must be a hydrolyzable group, preferably a C1-C8 alkoxy or a C1-C8 acyloxy group, where the substituents X, Y, Z are directly bonded to the Si atom or two of the substituents X, Y, Z form a ring together with the Si atom to which they are bonded. In a preferred embodiment, X, Y and Z are substituents directly bonded to the Si atom. As hydrolyzable groups, preferably alkoxy groups are selected, in particular methoxy, ethoxy, i-propyloxy and i-butyloxy groups. This is advantageous, since during the hardening of compositions containing alkoxy groups, no substances irritating to mucous membranes are released. The alcohol formed by hydrolysis of the groups is harmless in the amounts released and evaporates. These compositions are therefore particularly suitable for the DIY field. However, acyloxy groups, such as the acetoxy group -O-CO-CH3, may also be used as hydrolyzable groups.

[0052] In a preferred embodiment, the alkoxy- and / or acyloxysilane-terminated polymers have at least two end groups of general formula (III). Thus, each polymer chain contains at least two linking points that can complete the condensation of the polymer and separate the hydrolyzed residues in the presence of atmospheric moisture. In this way, regular and rapid crosslinking is achieved, resulting in bonds with good strength. Furthermore, the amount and structure of the hydrolyzable groups can thus affect in particular the elasticity, flexibility and heat resistance of the finished crosslinked composition, since it is possible to control the configuration of the network, which can be achieved as a long-chain system (thermoplastics), a relatively wide-mesh three-dimensional network (elastomers) or a highly crosslinked system (thermosets), for example by using di- or trialkoxysilyl groups, methoxy groups or longer groups.

[0053] In a preferred embodiment, X in the general formula (III) is preferably an alkyl group, and Y and Z, independently of one another, are alkoxy groups, or X, Y and Z, independently of one another, are alkoxy groups. In general, polymers containing di- or trialkoxysilyl groups have highly reactive linking points, which allows for rapid curing, a high degree of crosslinking, and therefore good final strength. A particular advantage of dialkoxysilyl groups lies in the fact that, after curing, the corresponding compositions are more elastic, softer and more flexible than systems containing trialkoxysilyl groups. They are therefore particularly suitable for use as sealants. Moreover, they separate even less alcohol during curing, which is particularly important when reducing the amount of alcohol released.

[0054] On the other hand, a higher degree of crosslinking can be achieved by using trialkoxysilyl groups. This is particularly advantageous when a harder and stronger material is required after curing. Furthermore, trialkoxysilyl groups are more reactive and therefore crosslink more quickly, which reduces the amount of catalyst required and provides benefits to the "cold flow", i.e. the dimensional stability of the corresponding adhesive under the influence of force and temperature.

[0055] Particularly preferably, the substituents X, Y and Z in general formula (III) are each independently selected from hydroxyl, methyl, ethyl, methoxy or ethoxy, and at least one of the substituents is hydroxyl, methoxy or ethoxy, preferably methoxy. The relatively small hydrolyzable groups methoxy and ethoxy have low steric bulk and high reactivity, allowing rapid curing even with low catalyst usage. Therefore, they are particularly important for systems where rapid curing is desired, such as adhesives that require high initial adhesion.

[0056] The combination of the two groups also opens up interesting configuration possibilities: if, for example, X is selected as methoxy and Y as ethoxy within the same alkoxysilyl group, the desired reactivity of the terminal silyl group can be particularly finely adjusted if it is determined that the reactivity of the silyl group carrying only methoxy groups is too high and that of the silyl group carrying ethoxy groups is not sufficient.

[0057] In addition to methoxy and ethoxy groups, it is of course possible to use larger groups as hydrolyzable groups, which inherently show lower reactivity, which is particularly important when delayed cure is also achieved by the placement of alkoxy groups.

[0058] The total proportion of polymers having at least one silicone-containing group, preferably at least one terminal group, of general formula (III) in the composition according to the invention is preferably from 10 to 80% by weight, more preferably from 10 to 60% by weight and most preferably from 20 to 60% by weight, in each case based on the total weight of the composition.

[0059] Further suitable polymers are those of general formula (IV): R-[AR 3 -SiR 1 x (OR 2 ) 3-x ] n (IV) where R is an organic base structure, A is an oxygen atom, an alkylene group, such as a methylene group, or a carboxy group, a carbamate group, a carbonate group, a ureido group, a urethane group, or a sulfonate group, and R 1 is an alkyl group having 1 to 4 carbon atoms, and R 2 is an alkyl group having 1 to 4 carbon atoms or an acyl group having 1 to 4 carbon atoms, and R 3 is a linear or branched, substituted or unsubstituted alkylene group having 1 to 8 carbon atoms; R 3 is a linear or branched, substituted or unsubstituted alkylene group having 1 to 8 carbon atoms, x=0 to 2, and n=1 to 10,000, where the silyl groups are the same or different, and multiple R 1 and / or R 2 If groups are present, the latter are each identical or different.Preference is given to the silyl-terminated polymers described in WO 2005 / 047394 A1 and EP 1 093 482 A1.

[0060] Filler The composition according to the invention may further comprise at least one filler, for example selected from chalk, powdered limestone, precipitated and / or pyrogenic silica, zeolite, bentonite, magnesium carbonate, diatomaceous earth (diatomaceous earth), alumina, clay, tallow, titanium oxide, iron oxide, zinc oxide, sand, quartz, flint, mica, powdered glass and other minerals. Further suitable fillers are in particular silicates, such as natural layered magnesium silicate hydrate, natural aluminum silicate hydrate and natural potassium aluminum hydrate; carbonates, such as natural calcium carbonate in crystalline form or from shell residues, precipitated calcium carbonate and natural calcium magnesium carbonate; sulfates, such as natural or synthetic barium salts; and several further substances, such as graphite or micaceous hematite. In a preferred embodiment, the filler is precipitated and / or pyrogenic silica. In addition, organic fillers may also be used, in particular carbon black, graphite, wood fibers, wood flour, sawdust, cellulose, cotton, pulp, wood chips, chopped straw, rice husks, walnut shells, and other short fibers. In addition, short fibers such as glass fibers, glass filaments, polyacrylonitrile, carbon fibers, Kevlar fibers, polyethylene fibers, etc. Aluminum powder is also suitable as a filler. In addition, hollow spheres with a mineral or plastic shell are suitable as fillers. These may be, for example, hollow glass spheres, which are commercially available under the trade name GlassBubbles®. Plastic-based hollow spheres are commercially available under the names Expancel® or Dualite®. They are preferably composed of inorganic or organic substances, each with a diameter of 1 mm or less, preferably 500 μm or less. Depending on the application, fillers that make the formulation thixotropic are preferred. These fillers are also described as rheological auxiliaries, for example hydrogenated castor oil, fatty acid amides, or swellable plastics, such as PVC.So that they can be easily squeezed out of a suitable metering device (eg tube), these preparations preferably have a viscosity of 3000 to 15,000 mPas, preferably 4000 to 8,000 mPas or 5000 to 6000 mPas.

[0061] The fillers are preferably used in an amount of 10 to 70% by weight, more preferably 20 to 60% by weight, for example 25 to 55% by weight, in particular 35 to 50% by weight, based on the total weight of the composition of the present invention. Individual fillers or combinations of several fillers may be used.

[0062] In one embodiment, 10 to 500 m 2 Highly dispersible silicas having a BET surface area of ​​100 m / g may be used as fillers. The use of such silicas does not result in a substantial increase in the viscosity of the compositions according to the invention, but contributes to the reinforcement of the cured preparations. This reinforcement improves, for example, the early strength, tensile shear strength and adhesion of the compositions according to the invention used. Preferably, the fillers have a BET surface area of ​​100 m / g. 2 / g, more preferably less than 65m 2 Uncoated silica with a BET surface area of ​​less than 100-400 m 2 / g, more preferably 100 to 300m 2 / g, especially 150-300m 2 / g, most particularly preferably 200 to 300m 2 A coated silica having a BET surface area of ​​1000 nm / g is used.

[0063] In another embodiment, a zeolite is used. As the zeolite, preferably an alkali aluminosilicate, such as, for example, an alkali aluminosilicate having the general empirical formula aK2O * bNa2O * Al2O3 * 2SiO *Sodium-potassium aluminosilicate of nH2O (0 < a, b < 1 and a + b = 1, n = 0 to 10) is used. The pore openings of the zeolite used are large enough to accept water molecules. Therefore, zeolites with effective pore openings less than 0.4 nm are preferred. Particularly preferably, the effective pore opening is 0.3 nm ± 0.02 nm. The zeolite is preferably used in powder form.

[0064] Chalk is preferably used as a filler. Cubic, non-cubic, amorphous and other modifications of calcium carbonate can be used as chalk. Preferably, the chalk used is surface-treated or coated. As coating agents, fatty acids, fatty acid soaps and fatty acid esters, such as lauric acid, palmitic acid or stearic acid, sodium or potassium salts of such acids or their alkyl esters are preferably used. However, in addition, other surfactants, such as sulfates of long-chain alcohols or alkylbenzene sulfonic acids or their sodium or potassium salts or coupling reagents based on silanes or titanates are also suitable. The surface treatment of chalk is often related to the improvement of the processability, adhesion strength and weather resistance of the composition. Preferably, it is in an amount of 0.1 to 20% by weight, preferably 1 to 5% by weight, based on the total weight of the composition.

[0065] Depending on the desired property profile, precipitated or ground chalk or mixtures thereof can be used. Ground chalk can be produced, for example, from natural lime, limestone or marble by mechanical grinding using either a dry method or a wet method. Depending on the grinding method, fractions with different average particle sizes can be obtained. Advantageous specific surface area values (BET) are between 1.5 m 2 / g and 50 m 2 / g.

[0066] Further suitable examples of fillers are, for example, Omyacarb chalk grades from the company Omya, or filler particles made of andalusite, sillimanite, kyanite, mullite, pyrophyllite, imogolite, or allophane. Compounds based on sodium aluminate or calcium silicate are also suitable. Minerals such as siliceous earth, calcium sulfate (gypsum), not originating from flue gas desulfurization plants and in the form of anhydrite, hemihydrate, or dihydrate, notably quartz flour, silica gel, barium sulfate, titanium dioxide, zeolites, muscovite, feldspar potash, biotite, the group of soro-, cyclo-, ino-, phyllo-, and tectosilicates, the group of sparingly soluble sulfates such as gypsum, anhydrite, or barium sulfate, as well as calcium minerals such as calcite and chalk (CaCO3). The aforementioned inorganic materials may be used individually. However, it is likewise possible to use mixtures of two or more of the aforementioned compounds.

[0067] Auxiliary substances The composition according to the invention may further comprise one or more auxiliary substances. Suitable auxiliary substances are disclosed below.

[0068] The composition according to the invention may further comprise, as an additional component, a compound of general formula (V): [ka] In the formula (V), R' may be the same or different and are independently selected from the group consisting of hydrogen atoms and hydrocarbon groups having 1 to 12 carbon atoms, and Ar is selected from aryl groups. In a preferred embodiment, the aryl group is a phenyl group, and / or R' in the general formula (V) is selected from methyl or ethyl groups, more preferably methyl groups. Most preferred is diphenyltetramethoxydisiloxane. When using at least one compound of the above general formula (V), the composition according to the present invention has improved tensile strength and elongation.

[0069] The proportion of the compound of general formula (V) in the composition according to the present invention is preferably 1-60% by weight, more preferably 2-50% by weight, based on the total weight of the composition. In a preferred embodiment, the composition according to the present invention contains at least one compound of general formula (V) in an amount of 20-60% by weight, more preferably 20-50% by weight, most preferably 30-50% by weight, based on the total weight of the composition. In another preferred embodiment, the composition according to the present invention contains at least one compound of general formula (V) in an amount of 1-50% by weight, more preferably 2-40% by weight, most preferably 4-30% by weight, based on the total weight of the composition.

[0070] The composition according to the present invention comprises a compound represented by the general formula (VI): [ka] The silicone oligomer may further comprise at least one silicone oligomer. In the formula, R' are the same or different and are independently selected from the group consisting of a hydrogen atom and a hydrocarbon group having 1 to 12 carbon atoms, preferably a methyl group or an ethyl group, more preferably a methyl group; Ar is selected from an aryl group, preferably a phenyl group; and n is an integer selected from 2 to 10, preferably 2 to 4, more preferably 2 to 3, and most preferably 3.

[0071] Solvents may be used to reduce the viscosity of the compositions according to the invention. Suitable solvents are aliphatic or aromatic hydrocarbons, halogenated hydrocarbons, alcohols, ketones, ethers, esters, ester alcohols, keto alcohols, keto ethers, keto esters and ether esters. However, alcohols are preferably used, since they increase the storage stability. C1-C 10 Alcohols are particularly preferred, in particular methanol, ethanol, i-propanol, isoamyl alcohol and hexanol.

[0072] The composition according to the invention may further comprise an adhesion promoter. An adhesion promoter is understood to be a substance that improves the adhesive properties of the adhesive layer on the surface. It is possible to use conventional adhesion promoters (tackifiers) known to the skilled artisan individually or as a combination of several compounds. Suitable examples are resins, terpene oligomers, coumarone / indene resins, aliphatic, petrochemical resins and modified phenolic resins. Suitable within the scope of the present invention are, for example, hydrocarbon resins such as those obtained by polymerization of terpenes, mainly α- or β-pinene, dipentene or limonene. The polymerization of these monomers is generally carried out cationically with initiation by Friedel-Crafts catalysts. Terpene resins also include copolymers of terpenes with other monomers, such as styrene, α-methylstyrene, isoprene, etc. The above resins are used, for example, as adhesion promoters for pressure-sensitive adhesives and coating materials. Also suitable are terpene-phenolic resins, which are produced by acid-catalyzed addition of phenols to terpenes or rosins. Terpene-phenolic resins are soluble in most organic solvents and oils and are miscible with other resins, waxes and rubbers. Likewise, within the scope of the present invention, rosin and its derivatives, such as their esters or alcohols, are suitable as adhesion promoters in the above sense. Silane adhesion promoters, especially aminosilanes, are particularly suitable.

[0073] In a particular embodiment of the composition according to the invention, the composition contains as adhesion promoter a compound of the general formula (VII): R 1 'R 2 'NR 3 '-SiXYZ (VII) where R 1 ' and R 2 ' are each independently hydrogen or a C1-C8 alkyl group, R 3' is a divalent hydrocarbon radical having 1 to 12 carbon atoms, optionally containing heteroatoms, and X, Y, Z are selected independently from hydroxyl groups or C1-C8 alkyl, C1-C8 alkoxy or C1-C8 acyloxy groups, with at least one of the substituents X, Y, Z being a C1-C8 alkoxy or C1-C8 acyloxy group. Compounds of this type inherently exhibit high affinity not only for the binding polymeric components of the composition according to the invention, but also for a wide range of polar and non-polar surfaces, thus contributing to the formation of a particularly stable bond between the adhesive composition and the particular substrate to be adhered. The linking group R 3 ' may be, for example, a linear, branched or cyclic, substituted or unsubstituted alkylene group. They may contain nitrogen (N) or oxygen (O) as heteroatoms. When X, Y and / or Z is an acyloxy group, it may be, for example, an acetoxy group -OCO-CH3.

[0074] The one or more adhesion promoters are preferably contained in the composition according to the invention in an amount of 0.1 to 10% by weight, more preferably 0.2 to 5% by weight, especially 0.3 to 3% by weight, based on the total weight of the composition.

[0075] The composition according to the invention may further comprise a UV stabilizer. Preferably, the proportion of UV stabilizer in the composition according to the invention is up to about 2% by weight, in particular up to 1% by weight. So-called hindered amine light stabilizers (HALS) are particularly suitable as UV stabilizers. For example, UV stabilizers having silyl groups and which are incorporated into the final product during crosslinking or curing may be used. In addition, benzotriazoles, benzophenones, benzoates, cyanoacrylates, acrylates, sterically hindered phenols, phosphorus, and / or sulfur may be added. The composition according to the invention preferably comprises at least one bis(piperidyl)dicarboxylic acid diester, for example bis(2,2,6,6-tetramethyl-4-piperidyl)sebacate.

[0076] In order to further increase the shelf life, it is often useful to further stabilize the composition according to the present invention against moisture penetration.This improvement in shelf life can be achieved, for example, by using a drying agent.Suitable as drying agent are all compounds that can react with water to form groups that are inert to the reactive groups present in the composition, while causing the change in molecular weight as little as possible.Furthermore, the reactivity of the drying agent to the moisture that penetrates into the composition must be higher than the reactivity of the end groups of the silyl group-containing polymer according to the present invention present in the composition.For example, isocyanates are suitable as drying agents.

[0077] Advantageously, silanes may also be used as drying agents, for example vinyl silanes such as 3-vinylpropyltriethoxysilane, oximesilanes such as methyl-O,O',O''-butan-2-one trioximosilanes or O,O',O'',O''''-butan-2-one tetraoximosilanes (CAS numbers: 022984-54-9 and 034206-40-1), or benzamidosilanes such as bis(N-methylbenzamido)methylethoxysilane (CAS number: 16230-35-6), or carbamatosilanes such as carbamatomethyltrimethoxysilane. However, the use of methyl-, ethyl- or vinyltrimethoxysilane, tetramethyl- or tetraethylethoxysilane is also possible. Particular preference here is given to vinyltrimethoxysilane and tetraethoxysilane, from the standpoint of efficiency and cost. Also suitable as desiccants are the reactive diluents mentioned above, provided that they have a molecular weight (Mn) of less than about 5000 g / mol and an end group that is at least as reactive with penetrating moisture as, and preferably more reactive than, the reactive group of the silyl-containing polymer according to the invention. Finally, alkyl orthoformates or orthoacetates can also be used as desiccants, such as methyl or ethyl orthoformate or methyl or ethyl orthoacetate. In general, the compositions according to the invention preferably contain 0.01 to 10% by weight of desiccants, based on the total weight of the composition.

[0078] The term "auxiliary substances" covers minor ingredients such as curing catalysts, adhesion promoters, water scavengers, UV stabilizers, anti-aging agents, rheology aids, pigments or pigment pastes, fungicides, flame retardants, solvents, etc.

[0079] The thickeners used in the structural adhesives according to the invention are preferably high molecular weight, usually organic substances that absorb liquids, such as water and / or organic solvents, and thereby swell or form intermolecular lattice structures. Fillers that absorb liquids and thereby swell or form intermolecular lattice structures, i.e. act as thickening agents or thickeners, are considered thickeners in the context of the present invention.

[0080] The thickening agents mentioned are in particular organic natural compounds such as agar-agar, carrageenan, tragacanth, gum arabic, alginates, pectins, polyoses, guar flour, locust bean flour, starch, dextrin, gelatin and casein; modified organic natural substances such as carboxymethylcellulose and other cellulose ethers, hydroxyethylcellulose, hydroxypropylcellulose, as well as seed flour ethers, hydrogenated castor oil, stearic acid, etc.; fully synthetic organic compounds such as polyacrylates and polymethacrylates, vinyl polymers, polycarboxylic acids, polyethers, polyimines, polyamides, etc.; and inorganic compounds such as polysilicic acid, silicic acid, etc.

[0081] Examples of organic thickeners are, inter alia, also (aqueous solutions of) copolymers based on acrylic acid and / or acrylamide, emulsified in the oil fraction, especially in the mineral oil fraction. Specific examples of w / o emulsifiers are Collacral HP from BASF and the Texipol grades from Scott-Bader. Further commercially available thickeners are, for example, Disparlon® grades, e.g. Disparlon® 6500. Other organic thickeners are, for example, the water-soluble polyurethane thickener Nopco DSX 3290 from Cognis, associative thickeners, such as, for example, Indunal T 112 from Indulor Chemie, which is an aqueous solution of a terpolymer of acrylates and methacrylates and carboxyl-containing comonomers (which is an anionic associative thickener), alkali-swellable thickeners, such as, for example, the acrylate polymer dispersion Acrysol TT 615 from Rohm&Haas, which is an alkali-swellable anionic dispersion with a solids content of about 30% by weight, and polymer dispersions based on acrylic acid and acrylamide.

[0082] Non-reactive thickeners such as amide waxes, for example Crayvallac SLX from Cray Valley, are particularly suitable as organic thickeners.

[0083] Examples of inorganic thickeners are especially pyrogenic silicic acids, preferably highly dispersed in either hydrophilic or hydrophobic form. Preferred hydrophilic silicic acids are water-wettable and are produced by flame hydrolysis. Hydrophobic silicic acids are then obtained, for example, by reaction with organosilanes. The surface area, measured by the BET method according to DIN ISO 9277:2014-01, is between 125 and 400 m 2 / g range is preferred. Highly dispersed silicic acids can be used both as powders and as aqueous dispersions. Examples are HDK from Wacker and Aerosil from Degussa-Huls.

[0084] Preferred concentrations of the thickeners are 5 to 50% by weight, particularly preferably 5 to 40, very particularly preferably 8 to 40% by weight or 10 to 35% by weight, based on the total weight of the composition.

[0085] The flow limit of the composition is preferably adjusted to at least a value of at least 1500 Pa. However, as mentioned above, this value may preferably be higher, for example at least 1800 Pa, particularly preferably at least 2000 Pa, 2500 Pa, 3000 Pa, 4000 Pa, 6000 Pa, 8000 Pa or even more than 10,000 Pa, for example 12,000 Pa.

[0086] Preferably, the composition is thickened with a thickener until its consistency is dimensionally stable and the structural adhesive compound can be kneaded. The addition of thickeners and / or fillers is recommended for economic reasons, since thickeners and fillers are usually cheaper than the binders contained in structural adhesives. The upper limit is reached only as a result of the wettability of the substrates to be adhesively bonded. Too high a concentration of thickener and / or filler reduces the wettability of the substrates to be bonded, leading to poor adhesive bonding results. The upper limit can be easily ascertained for each substrate in a few experiments.

[0087] As further additives, the compositions according to the invention may contain, for example, curing catalysts, such as dibutyltin dilaurate (DBTL), dyes and pigments. Pigments that absorb liquids and thereby swell or form intermolecular lattice structures, i.e. thickeners or thickeners, are considered thickeners in the context of the present invention.

[0088] The preparation of the compositions according to the invention is carried out in known manner by intimate mixing of the components in a suitable dispersing device, for example a high speed mixer.

[0089] All of the compositions disclosed herein can be used as described herein, for example, in the methods disclosed herein. EXAMPLES

[0090] Reagents and solvents were obtained from commercial sources and used as received unless otherwise noted. 29 Si NMR spectra were recorded on a Bruker AV400. 29 Si-NMR spectra were referenced to tetramethylsilane (TMS). Chemical shifts are in ppm. HR-MS measurements were recorded on an Agilent 6210 time-of-flight LC / MS (ESI) and the peaks listed correspond to the most abundant peaks and are the expected isotopic patterns. A microanalyzer TruSpec CHNS manufactured by Leco was used for the quantification of C / H / N / S. The tensile properties (elongation to break) were determined according to DIN EN ISO 8339:2005-09. The materials were measured after 7 days of curing on a Zwick machine, e.g. Zwick Z010. The Shore A hardness was measured according to DIN EN ISO 868:2003-10. The probe was applied with a coating knife (2 cm width / 1 cm height). The hardness was measured with a durometer 1 and 7 days after curing and the through hardening was measured with a vernier caliper. Skin over time (SOT): The build-up of the skin (touch-free time) was measured as follows: A film of the composition was applied with a spatula (length 5 cm / width 3 cm / height 2 mm) on a flat surface (sheet) and every 2-3 minutes it was tested whether a skin had formed. This can be done by applying a 20 g weight for 5 seconds through a finger, or a polyethylene film carefully placed on the film. When no film remains on the finger or on the polyethylene film, the skin formation time has been reached. The entire procedure is carried out at 23 ° C and 50% humidity. The unit used is minutes.

[0091] Example 1 (Compound A) Methyl ((3-(trimethoxysilyl)propyl)thio)octadecanoate-oleic acid methyl ester adduct [ka]

[0092] Methyl oleate (MO, 100 g, 337 mmol), (3-mercaptopropyl)trimethoxysilane (MPTSM, 125.4 mL, 132.5 g, 675 mmol, 2 equiv. relative to MO), and (2,2'-azobis(2-methylpropionitrile)) (AIBN, 1.46 g, 0.9 mmol, 2.4 mol % relative to MO) were added to an oven-dried 250 mL Schlenk round-bottom flask under argon and stirred for 18 h in an oil bath preheated to 85 °C. The reaction mixture was cooled to room temperature and excess MPTSM was removed under reduced pressure. The product was obtained in 84% yield (155 g, 314.5 mmol) as a yellowish oil without further purification. 29 Si NMR (79.5MHz, CDCl3):δ=-42.29ppm. HRMS (ESI+): m / z calculated for C25H52O5SSi: 492.3305; found: 515.3195 [M+Na]+. Calculated EA for C25H52O5SSi: C, 60.93; H, 10.64; S, 6.50 found: C, 61.01; H, 10.36; S, 6.37.

[0093] Example 2 (Compound B) Glyceryl trioleate-MPTSM adduct [ka]

[0094] Glyceryl trioleate (GTO, 14 mL, 12.74 g, 14.39 mmol), (3-mercaptopropyl)trimethoxysilane (MPTSM, 16.0 mL, 16.9 g, 86.34 mmol, 6 eq. relative to GTO), and (2,2'-azobis(2-methylpropionitrile)) (AIBN, 72 mg, 0.43 mmol, 3 mol % relative to MO) were added to an oven-dried 50 mL Schlenk flask under argon and stirred for 25 h in an oil bath preheated to 85 °C. The reaction mixture was cooled to room temperature and excess MPTSM was removed under reduced pressure. The product was obtained in 94% yield (20 g, 13.6 mmol) as a yellowish oil without further purification. 29 Si NMR (79.5MHz, CDCl3): δ=-42.24ppm. HRMS (ESI+): m / z calculated for C75H152O15S3Si3: 1472.9601; found: 1495.9484 [M+Na]+. Calculated EA for C75H152O15S3Si3: C, 61.10; H, 10.39; S, 6.52; found: C, 61.01; H, 10.68; S, 6.45.

[0095] Example 3 (Compound C) Linseed oil-MPTSM adduct [ka]

[0096] Under argon, linseed oil (LSO, 35 mL, 32.6 g), (3-mercaptopropyl)trimethoxysilane (MPTSM, 350 mL, 370 g, 1.88 mol), and (2,2'-azobis(2-methylpropionitrile)) (AIBN, 6.2 g, 37.8 mmol, 20 wt % with respect to LSO) were added to an oven-dried 500 mL Schlenk flask and stirred in an oil bath preheated to 85 °C. The progress of the reaction was monitored. 1The reaction mixture was monitored by H NMR. After 16 hours, additional AIBN (3.1 g) was added to the reaction mixture. After 41 hours at 85° C., the reaction mixture was cooled to room temperature and the excess MPTSM was removed under reduced pressure. 106 g of a yellow oil was obtained as product. Calculated EA for C93H194O24S6Si6: C, 54.29; H, 9.50; O, 18.66; S, 9.35; found: C, 54.07; H, 10.45; S, 9.86.

[0097] [Preparation Example 1] Polymer 1 (gamma-silane terminated polymer): 282 g (15 mmol) of polypropylene glycol 18000 (hydroxyl number = 6.0) was dried under vacuum at 80-90 °C in a 500 ml three-neck flask. 0.1 g of dibutyltin laurate was added at 80 °C under nitrogen atmosphere, followed by 7.2 g (32 mmol) of 3-isocyanatopropyltrimethoxysilane (% NCO = 18.4). After stirring at 80 °C for 1 hour, the resulting polymer was cooled. 3 g of light stabilizer (Tinuvin 770 DF) and 6 g of Geniosil XL 10 were added to the reactor, and after stirring and homogenization at 80 °C for 10-30 minutes, the resulting polymer was stored in a moisture-proof glass container under nitrogen atmosphere before further processing into a composition.

[0098] Example 4 (Adhesive) compound (composition) was prepared in a speed mixer such as the SpeedMixer DAC 400 FVZ from Hauschild Engineering. P Rimer 1 (22.5 g), and the respective plasticizer (Comparative DIUP (diisodecyl phthalate), 19.8 g) (A); or the reactive plasticizers of Examples 1-3 (Compound AC)One of the above (19.8 g) was homogenized in a 600 ml speed mixer can with a spatula. Then, calcium carbonate (Eskal 30, 92.5 g), rheology modifier (Rilanit Micro Spezial (hydrogenated castor oil; (12R)-12-hydroxyoctadecanoic acid, 9.8 g), and stabilizer (Tinuvin 328, 0.3 g) were added and the composition was mixed for 60 seconds at 2300 rpm. It was tested whether the can could reach about 37°C (body temperature), and if not, the mixing process was repeated. The composition was then cooled to room temperature for 15 minutes. Then, vinyltrimethoxysilane (Geniosil XL10, 2.6 g) and aminosilane (Geniosil GF96, 1.4 g) were added to the composition and mixed for 60 seconds at 2300 rpm each. Finally, a catalyst (DOTL; octyltin laurate catalyst, 1.1 g) was added to the composition and the composition was filled into a 150 ml PE cartridge.

[0099] All compounds of Examples 1-3 were compatible with the other compounds of the composition. The compositions were mixed and cured at room temperature for 7 days without any prior storage period. After curing, the specific properties and adhesion to various substrates were evaluated (Table 1).

[0100] In a further example, the same compositions were stored at 40°C for 4 weeks to simulate at least one year of aging. The samples were then cured at room temperature for 7 days. After curing, the specific properties and adhesion to various substrates were evaluated (Table 2).

[0101] Visual observations showed no difference between the stored and unstored specimens. However, it was surprisingly found that the mechanical properties (tensile strength and elongation) of the cured specimens after 4 weeks of storage at 40°C showed different mechanical properties compared to those that were not stored before curing. The novel reactive plasticizers resulted in either higher elasticity when compound A was used or higher tensile strength when compounds B and C were used.

[0102] [Table 1]

[0103]

Table 2

change

change

[10] Use of the compound according to any one of [1] to [7] as a reactive plasticizer, preferably as a reactive plasticizer in an adhesive composition.

[11] A) at least one silyl-terminated polymer; B) at least one compound according to any one of [1] to [7]; C) optionally, at least one filler; and D) Optionally, one or more auxiliary substances 1. An adhesive or sealant composition comprising:

[12] The adhesive or sealant composition according to

[11] , wherein the amount of the at least one compound B is 0.1 to 30% by weight based on the total weight of the composition.

[13] 10 to 80% by weight, preferably 10 to 50% by weight, more preferably 15 to 35% by weight of A; 0.1 to 30% by weight, preferably 0.1 to 20% by weight, more preferably 1 to 10% by weight of B; 0 to 70% by weight, preferably 20 to 60% by weight, more preferably 30 to 50% by weight of C; and 0 to 60% by weight, preferably 1 to 30% by weight, more preferably 1 to 10% by weight of D The adhesive composition or sealant composition according to

[11] or

[12] , which comprises or consists of:

Claims

1. Formula (I): 【Chemistry 1】 [In the formula, m=0 to 25; n=0-25; q=0 to 50; p=0-5; r = 1 to 3; Within each unit p or r, each m, n and q is independently selected; X is independently H or -SR 1 Selected from: R 1 =-(CH 2 ) 1-10 Si(O(CH 2 ) 0-8 CH 3 ) 3 However, there are two or more -SR 1 When present, they are not bonded to adjacent carbon atoms, and the -SR 1 the group is not bonded to a carbon atom which is bonded to an adjacent carbon atom by a double bond; Here, 1 to 10 -SR 1 is present; and R 2 = Substituted or unsubstituted aliphatic C 1-12 A hydrocarbon group, where the substituents are -OH, -OCH 3 , -F, -Cl, -Br, -I, =O, -NO 2 and -NH 2 selected from the group consisting of Compound.

2. p=1 to 3; m = 1 to 25; n=1 to 25; and q=0 2. The compound of claim 1,

3. p=0; q=2 to 50 2. The compound of claim 1,

4. The compound according to any one of claims 1 to 3, wherein r=1.

5. The compound according to any one of claims 1 to 3, wherein r=3.

6. 1 to 5 of -SR 1 The compound according to any one of claims 1 to 5, wherein

7. Formula (II): 【Chemistry 2】 [In the formula, s=0 to 25; t = 0 to 25; u = 1 to 5; v=1 to 3; and R 2 are defined as in claim 1. The compound of R 1 The compound HSR is defined as in claim 1. 1 and reacting in the presence of a catalyst. A process for preparing a compound of formula (I) according to any one of claims 1 to 6, comprising:

8. The process of claim 7, wherein the reaction is carried out at a temperature of from 30 to 100° C.

9. Use of the compound according to any one of claims 1 to 6 as a reactive plasticizer.

10. A) at least one silyl-terminated polymer; B) at least one compound according to any one of claims 1 to 6; C) optionally, at least one filler; and D) Optionally, one or more auxiliary substances 1. An adhesive or sealant composition comprising:

11. The adhesive or sealant composition according to claim 10, wherein the amount of said at least one compound B is from 0.1 to 30% by weight, based on the total weight of the composition.

12. 10 to 80% by weight of A; 0.1 to 30% by weight of B; 0-70% by weight of C; and 0 to 60% by weight of D 12. The adhesive or sealant composition according to claim 10 or 11, comprising or consisting of:

Citation Information

Patent Citations

  • Coupling agent between filler and elastomer

    JP2007514033A

  • Silane-crosslinked adhesives or encapsulating compounds, methods for their production and uses

    JP2008546879A

  • Filled rubber compound with improved processability

    JP2009509015A

  • Method for producing alkoxyhydrosilane compound

    JP2012158617A

  • Curable composition containing a silyl group and its use

    JP2012528204A