Polyvinyl alcohol polymer composition and binder for glass paper

By adding citric acid to polyvinyl alcohol polymers, the yellowing resistance is improved, ensuring effective adhesive performance and appearance of glass paper binders under high heat conditions.

JP7579973B2Active Publication Date: 2024-11-08DENKA CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023525712
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-31
Filing Date
2022-05-17
Publication Date
2024-11-08
Estimated Expiration
2042-05-17

AI Technical Summary

Technical Problem

Existing polyvinyl alcohol polymers used as binders for glass paper suffer from insufficient yellowing resistance during heating, which affects their performance and appearance.

Method used

Incorporating citric acid into the polyvinyl alcohol polymer composition to enhance yellowing resistance, with optimal citric acid content ranging from 0.01 to 10 parts by mass, improves the polymer's resistance to yellowing during heating.

Benefits of technology

The addition of citric acid significantly enhances the yellowing resistance of polyvinyl alcohol polymers, maintaining their adhesive properties and appearance under high temperatures, making them suitable for glass paper applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007579973000001
    Figure 0007579973000001
Patent Text Reader

Abstract

Provided is a polyvinyl alcohol-based polymer composition having improved yellowing resistance. The polyvinyl alcohol-based polymer composition contains a polyvinyl alcohol-based polymer and citric acid.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polyvinyl alcohol-based polymer composition and a binder for glass paper comprising the composition. [Background technology]

[0002] Due to its excellent adhesive performance, polyvinyl alcohol-based polymers are suitably used as adhesives, binders, etc. One such example is a binder for glass paper, in which polyvinyl alcohol-based polymers are used.

[0003] The polyvinyl alcohol-based polymer used as a binder for glass paper is used in the form of a slurry in which it is dispersed in water, or in the form of an aqueous solution in which it is dissolved in water. Therefore, glass paper is manufactured by heating and drying. In this process, the polyvinyl alcohol-based polymer can turn yellow when heated, which is a problem.

[0004] Patent Documents 1 and 2 disclose polyvinyl alcohol-based polymers used as binders for glass paper. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] US Patent Application Publication No. 2017 / 0044407 [Patent Document 2] International Publication No. 2019 / 012581 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the polyvinyl alcohol-based polymers described in Patent Documents 1 and 2 did not have sufficient yellowing resistance. Therefore, one object of the present invention is to provide a polyvinyl alcohol-based polymer composition having improved yellowing resistance. Another object of the present invention is to provide a binder for glass paper containing such a polyvinyl alcohol-based polymer composition. [Means for solving the problem]

[0007] According to one embodiment of the present invention, a polyvinyl alcohol-based polymer composition having improved yellowing resistance is provided by adding citric acid to a polyvinyl alcohol-based polymer. Effect of the Invention

[0008] According to one embodiment of the present invention, it is possible to provide a polyvinyl alcohol-based polymer composition having improved yellowing resistance. In addition, by using the polyvinyl alcohol-based polymer composition, an excellent binder for glass paper is provided. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, the embodiments of the present invention will be described in detail. However, the present invention is not limited to the following embodiments.

[0010] In one embodiment, the polyvinyl alcohol-based polymer composition according to the present invention must contain a polyvinyl alcohol-based polymer and citric acid. The higher the content of citric acid, the easier it is to improve the yellowing resistance. Therefore, the lower limit of the content of citric acid in the polyvinyl alcohol-based polymer composition is preferably 0.01 parts by mass or more, more preferably 0.1 parts by mass or more, and even more preferably 0.5 parts by mass or more, relative to 100 parts by mass of the polyvinyl alcohol-based polymer. However, from the viewpoint of ensuring the adhesive performance when used as a binder for glass paper, it is desirable that the content of citric acid is low. Therefore, the upper limit of the content of citric acid in the polyvinyl alcohol-based polymer composition is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 3.0 parts by mass or less, relative to 100 parts by mass of the polyvinyl alcohol-based polymer. Therefore, the content of citric acid in the polyvinyl alcohol-based polymer composition is, for example, preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5.0 parts by mass, and even more preferably 0.5 to 3.0 parts by mass, per 100 parts by mass of the polyvinyl alcohol-based polymer.

[0011] The polyvinyl alcohol polymer in the present invention is prepared by saponifying all or a part of polyvinyl esters obtained by polymerizing vinyl esters, and may be a commercially available polyvinyl alcohol.

[0012] The polyvinyl esters may be homopolymers of one or more vinyl esters, or copolymers of vinyl esters and monomers other than vinyl esters that are copolymerizable with the vinyl esters. From the viewpoint of the adhesive performance of the polyvinyl alcohol polymer, the polyvinyl esters are preferably homopolymers of vinyl esters.

[0013] Examples of vinyl esters include vinyl acetate, vinyl propionate, vinyl valerate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, and vinyl pivalate, and vinyl acetate is preferred from the viewpoint of ease of polymerization. The vinyl esters may be used alone or in combination of two or more.

[0014] Examples of monomers other than vinyl esters that can be copolymerized with vinyl esters include α-olefin monomers such as ethylene and propylene, (meth)acrylic acid alkyl ester monomers such as methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate, unsaturated amide monomers such as (meth)acrylamide and N-methylolacrylamide, unsaturated carboxylic acid monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, and fumaric acid, and alkyl (methyl, ethyl, propyl) groups of unsaturated carboxylic acids. Examples of the monomers include, but are not limited to, ester monomers such as glycidyl ester monomers, anhydrides of unsaturated carboxylic acids such as maleic anhydride, salts of unsaturated carboxylic acids with sodium, potassium, ammonium, etc., glycidyl group-containing monomers such as allyl glycidyl ether and glycidyl (meth)acrylate, sulfonic acid group-containing monomers such as 2-acrylamido-2-methylpropanesulfonic acid or salts thereof, phosphoric acid group-containing monomers such as acid phosphooxyethyl methacrylate and acid phosphooxypropyl methacrylate, alkyl vinyl ether monomers, etc. The monomers other than vinyl esters that are copolymerizable with vinyl esters may be used alone or in combination of two or more.

[0015] When polymerizing vinyl esters, a polymerization initiator may be used. The polymerization initiator may be, for example, a radical polymerization initiator. The radical polymerization initiator may be an azo-based compound such as azobisisobutyronitrile or azobisdimethylvaleronitrile, an organic peroxide such as benzoyl peroxide or dicumyl peroxide, an inorganic peroxide such as potassium persulfate, or a redox polymerization initiator such as a cerium (IV) salt-alcohol system.

[0016] The polymerization method of vinyl esters may be a known polymerization method such as solution polymerization, suspension polymerization, bulk polymerization, etc., and is preferably solution polymerization because of ease of operation. In addition, the polymerization method of vinyl esters is preferably solution polymerization in alcohol because it is possible to use a solvent that is the same as the solvent for the subsequent saponification reaction. In the case of solution polymerization, the polymerization reaction temperature may be preferably 30°C or higher and 90°C or lower.

[0017] The saponification reaction is carried out by dissolving the polyvinyl esters obtained by polymerization in alcohol to prepare an alcohol solution, and then causing an ester exchange reaction (alcohololysis) between the ester in the molecule and the alcohol solvent in the presence of an alkali or acid catalyst.

[0018] Examples of the alcohol as a solvent for the saponification reaction include methanol, ethanol, propanol, and butanol. From the viewpoint of ease of reaction, it is preferable to use methanol. The concentration of the polyvinyl ester in the alcohol solution may be, for example, 10 parts by mass or more and 80 parts by mass or less. The reaction temperature during the saponification reaction is preferably 10 to 70°C, more preferably 30 to 50°C. The reaction time for the saponification is preferably 10 minutes to 10 hours, more preferably 30 minutes to 3 hours.

[0019] Examples of the alkali catalyst that can be used include alkali metal hydroxides such as sodium hydroxide and potassium hydroxide, and alcoholates such as sodium methylate, sodium ethylate and potassium methylate. Examples of the acid catalyst that can be used include aqueous solutions of inorganic acids such as hydrochloric acid and sulfuric acid, and organic acids such as p-toluenesulfonic acid. From the viewpoints of ease of reaction control and production costs, it is preferable to use sodium hydroxide. The amount of these catalysts used is preferably, for example, 0.1 to 100 mmol equivalents relative to the vinyl ester monomer unit of the polyvinyl ester.

[0020] The degree of saponification of the polyvinyl alcohol-based polymer is not particularly limited, but from the viewpoint of water resistance and adhesive performance, it is preferably 95.0 mol% or more, more preferably 97.0 mol% or more, and even more preferably 99.0 mol% or more. The upper limit of the degree of saponification of the polyvinyl alcohol-based polymer is not particularly limited, and may be 100 mol%.

[0021] In this specification, the "saponification degree" refers to a value calculated by measurement according to JIS K 6726-1994 "3.5 Saponification degree".

[0022] The method for saponifying the polyvinyl ester may be a conventional method such as the belt saponification method or the kneader saponification method, and from the viewpoint of ease of production, the belt saponification method is preferred.

[0023] When the saponification reaction is carried out using sodium hydroxide, sodium acetate is produced as a by-product of the reaction. Since sodium acetate deteriorates the yellowing resistance of the polyvinyl alcohol-based polymer composition, it is preferable to reduce the amount of sodium acetate as much as possible.

[0024] As a method for reducing sodium acetate in a polyvinyl alcohol-based polymer composition, it can be achieved by reducing the amount of sodium hydroxide added in the saponification reaction to extend the reaction time or by reducing the water content in the reaction system. However, a method in which the polyvinyl alcohol-based polymer obtained after the saponification reaction is washed with an alcohol such as methanol to wash away sodium acetate is simple and preferable.

[0025] In this case, the content of sodium acetate in the polyvinyl alcohol-based polymer composition is preferably 1.0 parts by mass or less, more preferably 0.7 parts by mass or less, and even more preferably 0.5 parts by mass or less, based on 100 parts by mass of the polyvinyl alcohol-based polymer, from the viewpoint of maintaining the effect of improving the yellowing resistance when citric acid is added. The lower limit of the content of sodium acetate in the polyvinyl alcohol-based polymer composition is not particularly set. However, in consideration of the cost for complete removal and the effect thereof, the content of sodium acetate in the polyvinyl alcohol-based polymer composition is typically 0.01 parts by mass or more, more typically 0.1 parts by mass or more, and even more typically 0.5 parts by mass or more, based on 100 parts by mass of the polyvinyl alcohol-based polymer. The content of sodium acetate in the polyvinyl alcohol-based polymer composition is measured by the dissolution conductivity method described in JIS K 6726-1994.

[0026] From the viewpoint of suppressing blocking, the methanol content in the polyvinyl alcohol-based polymer composition is, for example, preferably 0.1 to 3.0 parts by mass, more preferably 0.1 to 1.0 parts by mass, based on 100 parts by mass of the polyvinyl alcohol-based polymer. The methanol content can be adjusted by the drying time of the polyvinyl alcohol-based polymer. The methanol content is determined by an absolute calibration curve method using gas chromatography. First, a calibration curve is created using a mixture of methanol and water with a known methanol content. Next, 1 g of the polyvinyl alcohol-based polymer composition is added to 49 mL of water, and the mixture is heated in an incubator at 80°C to dissolve. After visually confirming the dissolution of the polyvinyl alcohol-based polymer composition, a measurement is performed using gas chromatography (GC-9A, manufactured by Shimadzu Corporation, is used in the embodiment), and the methanol content in the polyvinyl alcohol-based polymer composition is determined based on the created calibration curve.

[0027] The larger the ratio (Y / X) of the mass fraction (Y) of the polyvinyl alcohol polymer having a particle diameter of 1000 μm or more to the mass fraction (X) of the polyvinyl alcohol polymer having a particle diameter of 500 μm or less, the higher the blocking suppression effect tends to be. From this viewpoint, the lower limit of Y / X is preferably 0.3 or more, more preferably 0.5 or more, and even more preferably 1.0 or more. Also, the smaller Y / X is, the easier it is to improve the adhesive performance. From this viewpoint, the upper limit of Y / X is 5.0 or less, more preferably 4.0 or less, and even more preferably 3.0 or less. Therefore, from the viewpoint of achieving both the blocking suppression effect and the adhesive performance, the range of Y / X is preferably 0.3 to 5.0, more preferably 0.5 to 4.0, and even more preferably 1.0 to 3.0. The particle diameter of the polyvinyl alcohol polymer can be adjusted by the grinding time in the grinding step or by sieving. Blocking can be suppressed by adjusting the particle diameter of the polyvinyl alcohol polymer to be within the above range.

[0028] The mass fraction of polyvinyl alcohol-based polymers having a particle size of 1000 μm or more means the mass ratio of polyvinyl alcohol-based polymers (sieved product) remaining on the sieve when the polyvinyl alcohol-based polymer to be measured is sieved using a test sieve (nominal mesh size 1000 μm) described in JIS Z 8801-1: 2006 (mass of sieved product / total mass of polyvinyl alcohol-based polymer to be measured). The mass fraction of polyvinyl alcohol-based polymers having a particle size of 500 μm or less means the mass ratio of polyvinyl alcohol-based polymers (undersieved product) that pass through the sieve when the polyvinyl alcohol-based polymer to be measured is sieved using a test sieve (nominal mesh size 500 μm) described in JIS Z 8801-1: 2006 (mass of undersieved product / total mass of polyvinyl alcohol-based polymer to be measured).

[0029] The viscosity average degree of polymerization of the polyvinyl alcohol-based polymer may be, for example, 100 or more, for example, 700 or more, for example, 1000 or more, and is, for example, 10000 or less, 6000 or less, 4000 or less.

[0030] The "viscosity average degree of polymerization" in this specification is calculated from the intrinsic viscosity [η] (g / dL) measured at 30° C. using an Ostwald viscometer with ion-exchanged water as a solvent, according to the following formula (1). log(P) = 1.613 × log([η] × 10 4 / 8.29)...Equation (1)

[0031] In one embodiment of the polyvinyl alcohol-based polymer composition according to the present invention, the total content of the polyvinyl alcohol-based polymer and citric acid is 90% by mass or more, preferably 95% by mass or more, and can be, for example, 90 to 99% by mass.

[0032] According to one embodiment of the present invention, a binder for glass paper containing the polyvinyl alcohol-based polymer composition of the present invention is provided. The binder for glass paper may be composed of the polyvinyl alcohol-based polymer composition of the present invention itself, or may contain known additives as appropriate. Glass paper is a type of nonwoven fabric made from short glass fibers (glass wool), and is produced by bonding short glass fibers with a binder. A polyvinyl alcohol-based polymer is one of the representative binders. The polyvinyl alcohol-based polymer composition of the present invention can be used as a primary binder in which the polyvinyl alcohol-based polymer is used in the form of a slurry in which the polyvinyl alcohol-based polymer is swollen and dispersed in water, and as a secondary binder in which the polyvinyl alcohol-based polymer is used as an aqueous solution. The primary binder is formed into a sheet on a wire net together with the short glass fibers, and then heated in a dryer to bond the short glass fibers. The secondary binder is applied to a sheet of short glass fibers bonded with the primary binder, and then heated and dried to improve the adhesive strength. The polyvinyl alcohol-based polymer composition of the present invention can be used as both a primary binder and a secondary binder, but is particularly suitable for use as a secondary binder. EXAMPLES

[0033] The present invention will be specifically described below with reference to examples, but the present invention is not limited to these examples.

[0034] [Example 1] In a reactor equipped with a reflux condenser, a dropping funnel, and a stirrer, 100 parts by mass of vinyl acetate, 28.2 parts by mass of methanol, and 0.03 parts by mass of azobisisobutyronitrile were charged, and polymerization was carried out for 6.7 hours at boiling point while stirring under nitrogen gas flow. Next, unreacted vinyl acetate was removed from the polymerization system to obtain a methanol solution of polyvinyl acetate with a degree of polymerization of 2150 (solid content concentration 54% by mass). The solid content concentration was measured from the mass change after weighing about 3 g of the obtained methanol solution of polyvinyl acetate into an aluminum cup and drying at 150 ° C for 30 minutes.

[0035] A sodium hydroxide solution (prepared so that the sodium hydroxide is 20 mmol per vinyl acetate unit of polyvinyl acetate) was added to 100 parts by mass of the methanol solution of polyvinyl acetate obtained above, and a saponification reaction was carried out at 40°C for 40 minutes. After the reaction was completed, the obtained wet cake was roughly pulverized, and acetic acid was added to stop the saponification reaction. After removing the reaction mother liquor by centrifugation, the mixture was washed with 50 parts by mass of methanol, and then centrifuged again to remove the methanol. Powdered polyvinyl alcohol (PVA) was obtained by drying at 120°C for 50 minutes in a gear oven. The mixture was then pulverized for 10 minutes in a grinder.

[0036] The viscosity average polymerization degree, saponification degree, content of sodium acetate per 100 parts by mass of polyvinyl alcohol, content of methanol per 100 parts by mass of polyvinyl alcohol, and mass ratio of large particle size to small particle size (ratio of mass fraction of polyvinyl alcohol polymer with particle size of 1000 μm or more to mass fraction of polyvinyl alcohol polymer with particle size of 500 μm or less) of the obtained polyvinyl alcohol were measured by the above-mentioned method, and the viscosity average polymerization degree was 1700, the saponification degree was 99.3 mol%, the content of sodium acetate was 0.5 parts by mass, the content of methanol was 1.0 parts by mass, and the mass ratio of large particle size to small particle size was 2.0. The results are shown in Table 1.

[0037] <Yellowing resistance test> To 100 parts by mass of the powdered polyvinyl alcohol obtained above, 3.0 parts by mass of powdered citric acid was added and mixed uniformly to obtain a polyvinyl alcohol-based polymer composition. Then, using this polyvinyl alcohol-based polymer composition, a polyvinyl alcohol film with a thickness of about 100 μm was produced by a solution casting method. The film was cut into a 50 mm square and heat-treated at 150° C. for 30 minutes. In addition, a film produced in the same manner was heat-treated at 200° C. for 30 minutes.

[0038] The yellowness of the film before and after the heat treatment was measured by the following method. A film with a thickness of approximately 100 μm was conditioned for 24 hours at 20° C. and 60% RH, and the XYZ in the XYZ color system was measured using a transmission color difference meter (ZE 2000, manufactured by Nippon Denshoku Industries Co., Ltd.) to calculate the yellowness index (YI). (Formula: YI=100*(1.28X-1.06Z) / Y) The yellowness index was 0.5 (before heat treatment), 3.0 (after heat treatment at 150° C.), and 25.4 (after heat treatment at 200° C.), respectively. The results are shown in Table 1.

[0039] <Adhesion test> The polyvinyl alcohol-based polymer composition prepared above was subjected to an adhesion test according to the following procedure. 50 mL of pure water was measured into a 100 mL disco cup, and 0.438 g of the polyvinyl alcohol-based polymer composition was gradually added thereto while stirring with a stirrer, and allowed to swell. 450 mL of pure water was weighed out and placed in a mixer, and 1.750 g of short glass fibers with a length of 6 mm was gradually added thereto, followed by gentle stirring with a Teflon rod. The swollen polyvinyl alcohol-based polymer-containing slurry was placed in a mixer and stirred with the mixer for 2 minutes. The stirred slurry was poured into a Nutsche fitted with an 80-mesh Teflon mesh (Shimadzu Corporation), and after lightly stirring with a Teflon rod to make it uniform, the rubber stopper was removed without tilting the Nutsche. When the slurry liquid stopped passing through the Teflon net, the Teflon net and the filtered material on it were pulled up together with tweezers and placed on a recording board, and a 10-mesh Teflon net (manufactured by Shimadzu Corporation) and industrial filter paper were placed on top of the filtered material in that order. The 80-mesh Teflon net was removed by turning it upside down, and the 10-mesh Teflon net and industrial filter paper were placed on top of the filtered material in that order. A pressure roller was moved back and forth five times on the laminate thus produced, and the upper and lower industrial filter papers were replaced with different industrial filter papers. Further, a pressure of 0.49 MPa was applied for 5 minutes using a press, and after removal, the industrial filter paper was replaced with another industrial filter paper. The sample was placed in a 110°C electric heat press for 2 minutes, removed, the pressure released, and left in the air for 10 minutes to remove moisture. After that, the sample was placed in a 110°C electric heat press for 1 minute and removed. The Teflon mesh and industrial filter paper were then peeled off. The glass paper thus prepared was cut into a size of 20 mm x 80 mm, and a tensile test was carried out at a tensile speed of 1 mm / min at 20°C using a tensile tester (manufactured by Shimadzu Corporation, model AG-X 5kN) to evaluate the adhesive strength. The adhesive strength was found to be 13 N. The results are shown in Table 1.

[0040] <Water resistance test> The initial mass of the polyvinyl alcohol-based polymer composition prepared above was measured. Next, after immersion in water at 20°C for 5 minutes, the composition was filtered using a Buchner funnel equipped with No. 5A filter paper, and the mass of the polyvinyl alcohol-based polymer composition in a swollen state was measured. The swelling degree was calculated using the following formula to evaluate water resistance. As a result, the swelling degree was 3%. The results are shown in Table 1. Swelling degree (%)=[mass of filtered polyvinyl alcohol-based polymer composition in a swollen state] / [initial mass of polyvinyl alcohol-based polymer composition]×100

[0041] <Blocking test> 30 g of the polyvinyl alcohol-based polymer composition was heat-sealed with polyethylene film to a size of 95 mm x 50 mm, and the resulting sample was sealed with 210 g / cm 2 After applying a load of 0.01 kg / cm2, the sample was left at 40°C for 12 hours, and then further left at -20°C for 12 hours, and the blocking state was evaluated. If the blocked mass was less than 5% relative to 30 g of the polyvinyl alcohol-based polymer composition, it was evaluated as ⊚, if it was 5 to 30%, it was evaluated as ◯, and if it was more than 30%, it was evaluated as △. As a result, the blocking test was evaluated as ⊚. The results are shown in Table 1. Here, the blocked mass was calculated by taking out the polyvinyl alcohol-based polymer composition (30 g) from the sample prepared above, sieving it using a test sieve (nominal mesh size 2 mm) described in JIS Z 8801-1:2006, weighing the mass A (g) of the polyvinyl alcohol-based polymer composition (sieve-remaining product) remaining on the sieve, and calculating it according to the following formula. Blocked mass (%) = (A / 30) x 100

[0042] [Example 2] A polyvinyl alcohol-based polymer composition was obtained in the same manner as in Example 1, except that the citric acid content was changed to 1.0 part by mass, and various tests were carried out. The yellowness index was 0.5 (before heat treatment), 5.2 (after heat treatment at 150°C), and 76.4 (after heat treatment at 200°C), respectively. The adhesive strength was 12N, the swelling degree was 4%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0043] [Example 3] A polyvinyl alcohol-based polymer composition was obtained in the same manner as in Example 1, except that the citric acid content was changed to 0.5 parts by mass, and various tests were carried out. The yellowness index was 0.5 (before heat treatment), 6.5 (after heat treatment at 150°C), and 112 (after heat treatment at 200°C), respectively. The adhesive strength was 13N, the swelling degree was 5%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0044] [Example 4] A polyvinyl alcohol-based polymer composition was obtained in the same manner as in Example 1, except that the citric acid content was changed to 0.1 parts by mass, and various tests were carried out. The yellowness index was 0.5 (before heat treatment), 7.1 (after heat treatment at 150°C), and 140 (after heat treatment at 200°C), respectively. The adhesive strength was 14N, the swelling degree was 4%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0045] [Example 5] A polyvinyl alcohol-based polymer composition was obtained in the same manner as in Example 1, except that the citric acid content was changed to 11 parts by mass, and various tests were carried out. The yellowness index was 0.5 (before heat treatment), 3.1 (after heat treatment at 150°C), and 26.3 (after heat treatment at 200°C), respectively. The adhesive strength was 7N, the swelling degree was 3%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0046] [Example 6] A polyvinyl alcohol-based polymer composition was obtained and various tests were carried out in the same manner as in Example 1, except that the amount of methanol for washing was changed to 20 parts by mass and the content of sodium acetate was changed to 0.7 parts by mass. The yellowness index was 0.7 (before heat treatment), 3.5 (after heat treatment at 150°C), and 28.9 (after heat treatment at 200°C), respectively. The adhesive strength was 13N, the swelling degree was 3%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0047] [Example 7] A polyvinyl alcohol-based polymer composition was obtained and various tests were carried out in the same manner as in Example 1, except that the amount of methanol for washing was 0 parts by mass and the content of sodium acetate was 1.0 parts by mass. The yellowness index was 0.7 (before heat treatment), 4.6 (after heat treatment at 150°C), and 30.5 (after heat treatment at 200°C), respectively. The adhesive strength was 13N, the swelling degree was 5%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0048] [Example 8] A polyvinyl alcohol polymer composition was obtained in the same manner as in Example 1, except that the amount of sodium hydroxide added was changed to 19 mmol and the degree of saponification was changed to 95.0 mol%, and various tests were carried out. The yellowness index was 0.5 (before heat treatment), 3.5 (after heat treatment at 150°C), and 27.8 (after heat treatment at 200°C), respectively. The adhesive strength was 10 N, the swelling degree was 8%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0049] [Example 9] A polyvinyl alcohol polymer composition was obtained and various tests were carried out in the same manner as in Example 1, except that the amount of sodium hydroxide added was changed to 18.5 mmol and the degree of saponification was changed to 93.0 mol%. The yellowness index was 0.5 (before heat treatment), 3.2 (after heat treatment at 150°C), and 26.1 (after heat treatment at 200°C), respectively. The adhesive strength was 8N, the swelling degree was 12%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0050] [Example 10] A polyvinyl alcohol-based polymer composition was obtained and various tests were carried out in the same manner as in Example 1, except that the drying time was changed to 40 minutes and the methanol content was changed to 3.0 parts by mass. The yellowness index was 0.5 (before heat treatment), 3.1 (after heat treatment at 150°C), and 26.2 (after heat treatment at 200°C), respectively. The adhesive strength was 13N, the swelling degree was 4%, and the blocking test was evaluated as ◯. The results are shown in Table 1.

[0051] [ reference example 1 ] A polyvinyl alcohol polymer composition was obtained and various tests were carried out in the same manner as in Example 1, except that the grinding time was changed to 15 minutes and the mass ratio of large particle diameter to small particle diameter was changed to 0.2. The yellowness index was 0.5 (before heat treatment), 3.4 (after heat treatment at 150°C), and 26.6 (after heat treatment at 200°C), respectively. The adhesive strength was 12N, the swelling degree was 4%, and the blocking test was evaluated as ◯. The results are shown in Table 1.

[0052] [Example 11 ] A polyvinyl alcohol polymer composition was obtained and various tests were carried out in the same manner as in Example 1, except that the grinding time was changed to 5 minutes and the mass ratio of large particle diameter to small particle diameter was changed to 4.0. The yellowness index was 0.5 (before heat treatment), 3.2 (after heat treatment at 150°C), and 24.1 (after heat treatment at 200°C), respectively. The adhesive strength was 8N, the swelling degree was 3%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0053] [Comparative Example 1] A polyvinyl alcohol-based polymer composition was obtained in the same manner as in Example 1, except that citric acid was not added, and various tests were carried out. The yellowness index was 0.5 (before heat treatment), 7.6 (after heat treatment at 150°C), and 171 (after heat treatment at 200°C), respectively. The adhesive strength was 13N, the swelling degree was 4%, and the blocking test was evaluated as ⊚. The results are shown in Table 1.

[0054] [Table 1]

[0055] In Comparative Example 1, citric acid was not added to the polyvinyl alcohol, and therefore the resistance to yellowing during heating was low. 1 In Examples 1 to 1, the addition of an appropriate amount of citric acid to polyvinyl alcohol significantly improved the yellowing resistance when heated, especially when heated at 200° C., compared with Comparative Example 1. 1 The polyvinyl alcohol-based polymer composition according to the present invention is extremely advantageous from an industrial viewpoint.

Claims

1. A polyvinyl alcohol-based polymer composition comprising a polyvinyl alcohol-based polymer and citric acid, wherein the ratio of the mass fraction of the polyvinyl alcohol-based polymer having a particle size of 1000 μm or more to the mass fraction of the polyvinyl alcohol-based polymer having a particle size of 500 μm or less is 0.3 to 5.

0.

2. 2. The polyvinyl alcohol-based polymer composition according to claim 1, wherein the content of citric acid is 0.01 to 10 parts by mass based on 100 parts by mass of the polyvinyl alcohol-based polymer.

3. 3. The polyvinyl alcohol-based polymer composition according to claim 1, wherein the content of sodium acetate is 1.0 part by mass or less based on 100 parts by mass of the polyvinyl alcohol-based polymer.

4. 3. The polyvinyl alcohol-based polymer composition according to claim 1, wherein the polyvinyl alcohol-based polymer has a degree of saponification of 95.0 mol % or more.

5. 3. The polyvinyl alcohol-based polymer composition according to claim 1, wherein the content of methanol is 0.1 to 3.0 parts by mass based on 100 parts by mass of the polyvinyl alcohol-based polymer.

6. The polyvinyl alcohol-based polymer composition according to claim 1 or 2, wherein the ratio of the mass fraction of the polyvinyl alcohol-based polymer having a particle size of 1000 μm or more to the mass fraction of the polyvinyl alcohol-based polymer having a particle size of 500 μm or less is 0.3 to 3.

0.

7. A binder for glass paper, comprising the polyvinyl alcohol-based polymer composition according to claim 1 or 2.

Citation Information

Patent Citations

  • Polyvinyl alcohol based composition and its use

    JP1999093075A

  • Amino-modified polyvinyl alcohol composition

    JP1999199740A

  • Water-soluble film

    JP1999222546A

  • Binder for Glass Paper