Energy storage devices, components and materials for energy storage devices, and energy storage methods

By using resealable containers and low-cost materials, supercapacitors are made serviceable, extending their lifespan and reducing costs, addressing the inefficiencies of current designs for grid-scale energy storage.

JP7580089B2Active Publication Date: 2024-11-11ATLAS POWER TECHNOLOGIES INC
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2022574335
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-06-30
Filing Date
2020-12-17
Publication Date
2024-11-11
Estimated Expiration
2040-12-17

AI Technical Summary

Technical Problem

Current supercapacitors are expensive, have low energy density, and are designed as sealed, non-serviceable units, leading to premature failure and high disposal rates, which is economically inefficient and environmentally wasteful, especially for grid-scale energy storage applications.

Method used

Designing supercapacitors with resealable containers that allow maintenance, using low-cost materials like activated carbon from coal and petroleum coke, and employing a hybrid electrolyte system to extend the lifespan by replenishing electrolytes and maintaining internal components.

Benefits of technology

The solution extends the operational life of supercapacitors to 50-100 years, reduces manufacturing costs, and enables the transition to renewable energy grids with less infrastructure investment by making supercapacitors serviceable and cost-effective.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580089000003
    Figure 0007580089000003
  • Figure 0007580089000004
    Figure 0007580089000004
  • Figure 0007580089000005
    Figure 0007580089000005
Patent Text Reader

Abstract

[Solution] Practical energy storage devices, such as capacitors, ultracapacitors, and supercapacitors, include electrodes made from activated carbon produced from low-cost sources, such as fuel coal or other low-cost raw materials. The practical energy storage devices include a replaceable electrolyte, which includes a low-cost co-solvent and salt solution. The activated carbon is manufactured with pore widths selected to match the electrolyte, so that the pore structure of the electrode material matches the ionic bond size of the electrolyte. The improved manufacturing process for the energy storage device is effective in normal atmospheric environments and allows for subsequent replacement of the electrolyte under normal atmospheric conditions.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims priority to Canadian Patent Application No. 3085109, filed in Canada on June 30, 2020.

[0002] This disclosure relates generally to energy storage devices, and more particularly to systems and methods for the construction, material composition, utility, and maintenance of practical "electrostatic storage devices" such as capacitors, including "supercapacitors." This application also discloses processes, systems, and methods for the production of activated carbon for tailoring its properties and composition for various applications, including supercapacitors. Additionally, process improvements for energy storage technologies, particularly those related to supercapacitor manufacturing processes, can occur in normal atmospheric environments, including electrolyte processing steps. [Background technology]

[0003] The concept of utilizing energy storage devices and their structures and various elemental compositions is well known and continues to attract large capital investments due to its societal benefits and necessity. Battery life is shortened due to the chemical reactions that occur to store energy, as elements degrade during charging and discharging. Some batteries have the ability to be recharged after discharging, while other types of batteries have a life cycle that allows them to be used only once. Capacitors store energy in the form of an electrostatic field rather than an electrochemical reaction. Capacitors therefore charge and discharge more rapidly than batteries and are expected to have a lifespan that is orders of magnitude longer than current battery technology.

[0004] Demand for energy storage has grown significantly over the past decade as solar power has become established as a low-cost form of electricity generation, leading to exponential growth in solar PV installation projects. With the rise of solar power generation, the need for energy storage is growing at a critical rate. As we continue our transition to a renewable power grid, energy-dense, low-cost, and abundant materials for energy storage are desirable and key to achieving renewable power generation. Furthermore, extending the life of energy storage devices is always desirable, and this also addresses commercial competitiveness.

[0005] Supercapacitors are electrochemical energy storage devices that can store energy for later use. Therefore, supercapacitors play an important role among clean energy technologies in overcoming global pollution and enabling the sustainable and renewable use of energy resources. Supercapacitors are being considered as an alternative to batteries for grid-scale applications due to their fast charge / discharge rates, high power density, low maintenance, and long cycle life. While the supercapacitor market has found applications in consumer electronics and transportation technology, supercapacitors are said to still be lagging behind the fast-growing market for grid-scale energy storage due to their low energy density and high cost.

[0006] A supercapacitor device typically consists of two "electrodes" separated by an ion-permeable separator, an "electrolyte" that ionically connects the electrodes, and two "current collectors" that are directly connected to the electrodes. The design of a supercapacitor requires the proper selection of electrode materials, electrolytes, separators, and sealants. Electrode materials play a crucial role in the performance of supercapacitors, so designing the right electrodes is key to producing high-energy-density, low-cost devices. Activated carbon, derived from a variety of materials, is widely used as the active material for electrodes in commercial supercapacitors due to its high double-layer capacitance, low cost, large surface area, chemical stability, and excellent electrical conductivity.

[0007] Traditionally, common electrostatic and electrochemical energy storage technologies (mainly batteries and capacitors) have relied primarily on two types of electrolytes: aqueous electrolytes and organic electrolytes. Companies have benefited from the ability to select an appropriate liquid electrolyte based on typical applications.

[0008] Although the safety and ease of use of aqueous electrolytes are attractive, many manufacturers have chosen to use primarily "organic electrolytes" rather than aqueous ones due to their voltage stability, which allows for significantly improved energy density (reduced device size). The use of organic electrolytes generally suffers from, but is not limited to, critical and difficult properties in their use and handling. Organic electrolytes are highly volatile and undergo thermochemical reactions when mixed with water, including when exposed to minute droplets in the atmosphere. This makes the use of organic electrolytes difficult and expensive, including during manufacturing.

[0009] Additionally, manufacturers are currently opting to purchase off-the-shelf products (e.g., activated carbon and electrolyte) in their designs, as development is focused on increasing the surface area of ​​activated carbon to increase energy density.

[0010] Therefore, industry and researchers have not yet developed or attempted to specifically tailor the pore width and pore distribution of activated carbons through specific mineral processing, carbon source selection, or manufacturing process control to produce activated carbons with specifically engineered pore hierarchies for specific electrolytes. Also, pre-engineered activated carbons and "ion-permeable separators" with pre-selected pore widths and pore distribution hierarchies for improved wettability, intercalation, saturation, and permeability of desired electrolytes, and for activated carbon pores that synergistically couple with electrolytes based on ion-solvated ion-solvated shell size. Below, a complete end-to-end manufacturing process is developed to achieve the above-mentioned material processing control and resulting material properties, resulting in a safe and low-cost manufacturing process. Summary of the Invention

[0011] Below, we present embodiments of the present invention that, when implemented in practice, are expected to significantly improve the operational life of electrostatic storage devices such as capacitors. Furthermore, embodiments disclosed herein enable the fabrication of superior performance supercapacitors using very inexpensive and widely available building blocks (e.g., activated carbons produced from coal, petroleum coke, bituminous coke, biomass, and low-cost salt electrolytes). [Problem to be solved by the invention]

[0012] Currently, commercially available supercapacitors, ranging from millifarads to thousands of farads, are generally designed to operate in electrical devices in a variety of processes, including charging and discharging. These supercapacitors have many applications ranging from sub-circuit level integration to large scale installations for grid-scale energy storage and load shifting.

[0013] The design and operation methodology of commercial supercapacitor systems has resulted in products designed to achieve the highest energy density possible, making them competitive in size with batteries. Supercapacitors are self-contained, sealed units with relatively long life expectancies and, like battery systems, are typically discarded and replaced with new capacitors upon reaching their life expectancy or physical failure. This method of operation is generally dependent on the life cycle of these devices, with many supercapacitors having a lifespan of 20 years or more and an average lifespan of 1 to 2 million charge-discharge cycles. Because the majority of commercially available supercapacitors are for electronic devices, the costs of ensuring a relatively small storage capacity and making these units commercially viable are non-existent or have not proven economical.

[0014] Generally, supercapacitors are not very expensive, and the cost of using these tiny electronic components does not make it commercially viable, other than for environmental considerations. In fact, it is cheaper to replace a supercapacitor than it is to use it. The transition to energy generation from clean renewable sources is underway, and as energy storage systems are needed to compensate for the intermittent nature of most forms of renewable power generation, supercapacitors are being researched and implemented as a commercially viable solution to energy storage needs. As larger units continue to be constructed for energy storage, there is a continuing need to fabricate supercapacitors from inexpensive and abundant materials, and to extend the lifetime of supercapacitors. This will enable our society to enjoy the long-term benefits of long-life, low-cost energy storage devices, helping us meet our needs as we transition to a clean energy future.

[0015] Given this, creating energy storage solutions that are cheap and can continue to operate for long periods of time is essential for the transition to a renewable electricity grid and the long-term success and health of our planet and humanity.

[0016] Existing construction and operation of electrostatic storage devices, such as supercapacitors, are designed as sealed or non-serviceable units that are operated for a desired and expected "life expectancy" and then discarded. This is the same challenge faced by commercial battery systems, which are manufactured, then used, disposed of, and remanufactured. Additionally, supercapacitors have a wide variety of applications, many of which are high-end demand. This is because manufacturers are primarily focused on increasing energy density, which means that materials such as coconut shell-derived activated carbon and organic and ionic liquid electrolytes are generally expensive in terms of actual material costs, and the cost required for equipment in the manufacturing process is high.

[0017] More specifically for grid-scale applications, the amount of energy storage required during the future clean energy transition will be staggering. For us to transition fully to a renewable electricity grid, we would need to accommodate around 40% of our current daytime energy use and use renewable energy to load-shift into the night. The expansion of consumption is explained by the fact that, with the current battery and supercapacitor technologies in commercial use and installation, a huge amount of manufacturing capacity would need to be configured just to keep up with current demand. This is due to the fact that the energy storage assets we produce, typically batteries with a lifespan of 3,000-8,000 cycles or 10 years, must be disposed of and replaced before reaching the end of their useful life.

[0018] Supercapacitors are more advantageous as they typically have a lifespan of 1-2 million cycles or 20 years. Although supercapacitors have a long lifespan, as mentioned above, they are still considered a disposable solution made from expensive precursor components. This means that the manufacturing capacity of supercapacitors needed to enable the future clean energy transition will be half that of batteries. Batteries are needed in large quantities and there are still a huge number of orders.

[0019] This disclosure provides systems and methods for making "supercapacitors" (electrostatic storage devices) serviceable products that are manufactured from low-cost, abundant materials, extending their expected lifespan and reducing their costs. This is extremely beneficial in that the solution reduces levelized operational costs and provides a clear path for our society to achieve the goal of reaching a fully renewable electricity grid with less production volume than human civilization will require to reach that milestone.

[0020] One way to achieve such a system / method is to design the electrostatic storage device (capacitor) to be "serviceable." Further embodiments are constructed from low-cost, widely available materials such as waste materials, including but not limited to low-cost mined minerals such as biomass, petroleum coke, bituminous coke, coal, and thermal coal, and use low-cost electrolyte materials such as water, salts, solvents, co-solvents, or combinations thereof.

[0021] "Serviceable" is defined as "a device that can be maintained, a device that can be changed, a device that can be opened or closed, a device that can be reused, or a device that can be supplied with electrolytes or other solutions after the device's original manufacture is complete." This means that maintaining the supercapacitor itself can extend its lifespan and improve its operation. This can be accomplished by accessing the "contents" of the supercapacitor container, accessing the component requiring maintenance, performing the maintenance on the accessed component, and then reclosing the container to return the device to an operational state.

[0022] One novel and differentiating component of the present systems and methods is the ability to maintain, for example, the supercapacitor, thereby increasing the potential for a longer life expectancy and improved product. For example, recharging the liquid electrolyte to remove old, suboptimal or used liquid electrolytes or adding improved liquid electrolytes provides the ability to increase energy density and further extend the operating life of the device. For example, maintenance of failed components in the device, such as liquid electrolytes or conductors.

[0023] Supercapacitors in some embodiments of the present invention include activated carbon or other materials that provide high surface area, conductive additives, binders, current collectors, separator(s), electrolytes, and a number of different elemental compositions and methods of manufacture. Typically, activated carbon products contain a conductive additive and a binder, and are bound to a conductive current collector such as aluminum, copper, stainless steel, or titanium. Furthermore, this combination is mixed with an "electrolyte" and a "separator" that acts as an intermediary to prevent direct contact between the anode and cathode, and is then placed in a sealed container together with a "lead case separator" that is generally made of rubber or plastic. The type of liquid electrolyte used affects various properties of the capacitor, including voltage tolerance, stability, volatility, manufacturing process, lifetime, temperature range, and energy density.

[0024] The electrostatic storage property of a "supercapacitor" is in the form of an electrostatic field. This is because the charge is transferred through the electrolyte and subsequently stored on the surface and within the "porous structure" of the activated carbon element. When a supercapacitor undergoes a "charging process," charge is collected in the form of an electrostatic field. This electric field causes charges on the other side of the conductor to be released, completing a circuit and allowing current to flow. In these devices, the conductive components are generally the anode and cathode as well as the casing. This is to prevent the formation of a galvanic cell, i.e., to prevent electrochemical reactions between the metals from occurring during charging and discharging.

[0025] The storage profile and characteristics of a "battery" differ from those of a supercapacitor; a galvanic cell is formed within the battery to generate an electric current, storing the charge generated by the electrochemical reaction. This electrochemical process allows for the collection of charge at higher densities than currently available supercapacitors, resulting in batteries that exhibit relatively high energy densities. The adverse effect of electrochemical reactions is the degradation of metals and other components that make up the battery during the discharge process and, in the case of rechargeable batteries, the recharge process.

[0026] The nature of supercapacitors, which store energy in the form of electrostatic fields, causes limited chemical reactions to occur within the supercapacitor during charging and discharging. This means that supercapacitors do not undergo the same elemental decomposition that batteries undergo as they are charged and discharged over their lifespan.

[0027] This raises the question: why do supercapacitors fail? What accounts for the longevity of supercapacitors, even though they are not subjected to the same types of reactions that severely degrade battery materials during the charge and discharge process?

[0028] The answers to these questions are complex, and there are many factors that affect a supercapacitor's long-term operational capability as a factor in its expected lifespan. Some factors that affect the lifespan of a supercapacitor include the type of electrolyte and the effect of corrosion on the supercapacitor's components, such as the current collector (typically the container and foil), which generally includes the casing and foil. The operating temperature of the device, the environment in which the supercapacitor is placed, and the properties of the electrolyte, including its voltage range and temperature stability, also affect the lifetime of the supercapacitor.

[0029] The present system and method improves upon conventional electrostatic storage devices by identifying the cause of the failure and providing a solution to that failure in a practical, implementable, and commercially applicable manner. Furthermore, the present invention identifies low-cost, widely available materials for constructing supercapacitors, lowering their cost and enabling access to existing infrastructure for feedstock minerals. Specifically, the present invention uses "activated carbon combinations" derived from low-cost materials such as coal, thermal coal, petroleum coke, bituminous coke, lignin, biomass, garbage, plastics, and other waste materials. The "electrolyte" is selected from aqueous electrolytes, "cosolvents in salt electrolytes", salts, water, and solvents. The current collectors are selected from stainless steel, titanium, copper, and aluminum. Examples of "ion permeable separators" include paper, glass fiber, and "plastic fiber." One representative embodiment is "Activated carbon" derived from low-cost fuel coal, "Electrolytes" are co-solvents for salts, A stainless steel "current collector" and "Ion-permeable separator" made of paper, cellulose, and plastic fibers, fabrics, and mesh, PVDF·PTFE "binder" and Carbon black, acetylene black, and Super P's conductive additives. It consists of:

[0030] To improve the operation and life expectancy of supercapacitors, the inventors have identified the reasons for failure. One of these is, among other things, the properties and performance of the electrolyte of the device during the life of the device.

[0031] The "electrolyte" is the component that is most subject to the most severe physical action in an electrostatic storage device and is most susceptible to environmental influences. Carbon (especially activated carbon) is a very stable element and can theoretically persist indefinitely. The conductors used in the electrodes can last for an indefinite period of time unless the elements they contact corrode or the conductor decays. Marine grade stainless steel (e.g., 316 stainless steel) can have an expected lifespan of 50 to 100 years in seawater.

[0032] On the other hand, the electrolyte degrades over time and acts as an ion carrier and charge transport medium within the device. The degradation described above is exacerbated by the actual device operation (voltage charging range) and the environmental and temperature changes to which the device is exposed. Degradation of the electrolyte can reduce the performance of supercapacitors and electrostatic storage devices, ultimately leading to complete failure of the device and can also lead to the application of voltages that exceed the stability threshold of the electrolyte.

[0033] Such liquid electrolyte degradation and device failure can be reduced or eliminated by configuring the device to be serviceable, allowing for maintenance and re-application of the liquid electrolyte, and achieving numerous improvements in the device. One improvement to the devices of the present system and method is to make the actual "container" that houses the supercapacitor or electrostatic storage device resealable, allowing occasional access to the contents. While this functionality can be achieved in several ways, it is essential to maintain and recover the contents of the supercapacitor, as opening the sealed container may damage the container and cause it to be discarded. However, making the container resealable allows the device to be opened, serviced, and resealed.

[0034] The next step in improving the proposed device is to provide a method for efficiently recharging the electrolyte into the supercapacitor's internal contents. Assembling a supercapacitor presents a challenge in that it is difficult to ensure that the liquid electrolyte reaches the interior or central region of the supercapacitor without damaging the supercapacitor or its layers when it is introduced. If tampered with, it can flake off or separate from the current collector.

[0035] There are several methods for maintaining a supercapacitor and dosing it with liquid electrolyte. One approach is to inject a liquid electrolyte into the supercapacitor, ensuring that the electrolyte is saturated throughout the desired conductive parts of the device. This method of injecting and saturating the device can be difficult and time-consuming, especially for large and small supercapacitors. For very large supercapacitors, it may not be possible to physically inject the liquid electrolyte into the center of the device without proper "separation" or "perforation."

[0036] These challenges arise from several factors. One of these is the case of cylindrical supercapacitors, which are wound very tightly to reduce size and improve performance, and stacked supercapacitors, which are pressed to reduce size and improve performance.

[0037] A further refinement of the present system and method to improve the ability to "load / saturate" the supercapacitor with the "electrolyte" applied to the desired conductive elements of the device or activated carbon to saturate the entire desired area is to "perforate" the electrodes and separator or "separate / expose" the interior of the electrodes and separator. By "perforating" or separating the material, the electrolyte can diffuse (percolate) around the perforated or separated area, allowing the electrolyte to reach the inner regions of the device, even in large supercapacitors. This can be achieved in several ways, depending on the viscosity of the electrolyte, including perforating a layer of the supercapacitor far from other perforations to fully saturate it. This complete saturation can also be achieved by configuring the layers within the supercapacitor in sections or slices, which allows the electrolyte to be saturated when maintenance is performed after the device's operational life.

[0038] The maintenance process may include flushing the supercapacitor with the existing electrolyte. Such a cleaning process is beneficial because many electrolytes contain salts and other dissolved minerals that can become deposited and trapped within the activated carbon. These dissolved minerals can adversely affect device performance, and a cleaning process during maintenance is desirable to extract these dissolved minerals.

[0039] Such maintenance techniques are advantageous because the resulting operational life of the device is extended while the structure of the device is not damaged. To further illustrate this point, when assembling a supercapacitor, in this example a double layer electrolytic capacitor (DLEC), the layers are stacked or wound together. The layer is configured to be tightly compressed so that the bonded carbon does not pull away from the conductor. If the layers become separated during maintenance, the carbon will flake or peel off from the surface of the conductor, reducing device performance. Furthermore, the process of separating the layers is very difficult and time consuming, reducing the viability of maintaining such devices. By providing a "resealable container" as well as "perforations or separations," the internal region of the supercapacitor can be more efficiently accessed and saturated, providing an end product with both better performance and lifespan.

[0040] Another improvement of this device is that "it allows for the selection of high-quality conductive materials for the electrodes." By choosing maintainable "electrostatic storage devices" (supercapacitors), manufacturers and designers can choose conductive materials that last significantly longer than traditional conductive materials such as aluminum and copper. Examples of "long-lasting materials" are stainless steel or titanium, which are "necessary when used with certain electrolytes," such as the exemplary "co-solvent in a salt electrolyte." Stainless steel has proven to be more robust and long-lasting when used in environments exposed to salt and brine. The advantage of the proposed system and method is that the expected lifespan and economic efficiency of using supercapacitors that are maintainable and last significantly longer than conventional supercapacitors offsets the initial cost of using more expensive current collectors. However, this is not a requirement and less convenient metals such as copper or aluminum may be used. For example, instead of using aluminum or copper, which degrade at a constant rate when exposed to salt, marine-grade stainless steel (e.g., 316 stainless steel or resistant 306 stainless steel) can be used, which with regular maintenance can extend the expected lifespan from 20 to over 100 years. With careful consideration of the electrolyte and conductive electrode materials, it is reasonable to believe that capacitors have a projected lifetime that could reach a typical operating life of 50 to 100 years, far exceeding current technology.

[0041] The systems and methods disclosed herein provide an effective approach to significantly reduce the cost and improve the lifespan of these devices, ensuring a path to a sustainable, renewable power grid. The stable properties of the contents inside the supercapacitor, combined with its non-reactive operation, make it an extremely long-life energy storage solution.

[0042] By using low-cost raw material minerals such as thermal coal and a "salt electrolyte-based co-solvent," production can be rapidly scaled up even in normal atmospheric conditions, providing low-cost production capacity. Another major advantage of the present invention is the ability of the electrolyte to be added to a supercapacitor in a normal atmospheric terrestrial environment, as opposed to organic electrolytes, which require a moisture-free environment due to their reactivity when mixed with water (including the natural moisture found in the Earth's atmosphere). By utilizing the present systems and methods, it is possible to create energy storage solutions with useful operating lives reaching over 100 years and costs below $50.00 per kWh. This long expected lifespan and low cost will bring about a paradigm shift in humanity's ability to produce energy storage to meet human needs, maintaining and operating sufficient energy storage to enable the transition to and maintenance of a fully renewable electricity grid. [Means for solving the problem]

[0043] Additionally, embodiments of the present disclosure provide novel ways to manage and control the maintenance and serviceability of electrostatic storage devices, and provide improved methods and systems and methods for operating supercapacitor configurations. This is briefly described and implemented in the configuration of one embodiment. 1. An improved "system for maintainable electrical supercapacitors," comprising: "Casing" and an "electrostatic operable section" within said casing; It is composed of a combination of the following. The "electrostatically operable section" is a pair of spaced apart electrodes in contact with activated carbon obtained from a low-cost carbon source, such as aluminum, costing less than $250 per ton (including less than $100 per ton, if possible); and a conductive additive; An "ion permeable separator" between the electrodes, (a) a "casing" with means for connecting said electrodes to a power source; (b) a liquid electrolyte fluid within the casing in contact with the electrodes and an ion permeable material; (c) "electrostatic storage devices" consisting of resealable and non-resealable containers that provide access to the contents within the electrostatic storage devices; (d) the electrostatic storage device having an interior content including perforated, separated, or isolated sections of electrodes, separators, and layers; (e) an electrostatic storage device having means for maintenance, removal, and replacement, means for recharging and removing the liquid electrolyte, and means for adding new liquid electrolyte; (f) a means for resealing the "resealable container" of said electrostatic storage device, or a means for sealing the contents of said electrostatic storage device into a non-resealable container, or a means for resealing an existing container; It is composed of a combination of the following.

[0044] In this system, activated carbon is derived from low-cost carbon sources, including coal, bituminous coke, and petroleum coke, or from waste or biomass. In this system, the liquid electrolyte is a "co-solvent in a salt electrolyte" consisting of sodium perchlorate, which has the general formula NACLO4, and a cation exchanger, which has the general formula CH3CN. A system containing acetonitrile (TIFF0007580089000001.tif5977) and water as components.

[0045] In this system, the molar ratio of the electrolyte, which is 1 part sodium perchlorate, 1.5 parts water, and 2.4 parts acetonitrile, is about 7-8.

[0046] In this system, the molar ratio range of the electrolyte is "4 to 10", and the electrolyte is composed of 0.25 to 2 parts sodium perchlorate, 0.25 to 3 parts water, and 0.25 to 4 parts acetonitrile.

[0047] In this system, part of the electrolyte consists of sodium chloride, lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), sodium chloride, ammonium dichlorate, magnesium sulfate, and sodium bicarbonate. In this system, the "liquid electrolyte" consists of either a "cosolvent in-salt electrolyte", an aqueous electrolyte, an organic electrolyte, or an ionic solution. In this system, the electrodes are made of stainless steel, titanium, copper, and aluminum. In this system, the electrodes are composed of conductive thin films, conductive meshes, and conductive fabrics. The electrodes and separators in this system have "perforated, separated, and isolated sections" of the electrodes, separators, and layers. In this system, the separator layer is a "cellulose" material, a paper dielectric, a "plastic dielectric", or a dielectric material. In this system, the composition of the activated carbon composite is approximately 75% to 88% "activated carbon" from low-cost carbon sources, approximately 4% to 20% "conductive additives" including carbon black, Super P, "acetylene black," furnace black, lamp black, and channel black, and approximately 3% to 12% "binders including PTFE and PVDF" (whether or not dispersed in water).

[0048] According to another embodiment of the present invention, there is provided a method of maintaining a serviceable electrostatic storage device (supercapacitor), comprising the steps of: The electrostatic storage device comprises a resealable or non-resealable container, electrodes, a separator, and a solid or liquid electrolyte; The method comprises: (a) identifying that the electrostatic storage device requires maintenance by measuring and analyzing its operational performance; (b) accessing the contents within the electrostatic storage device when the contents within include a perforated, separated, or isolated section of an electrode, separator, or layer; (c) Remove electrolyte, replace electrolyte, reinject electrolyte, or add electrolyte. (d) resealing the resealable container or placing new or additional contents in the non-resealable container and sealing the non-resealable container.

[0049] The method involves "accessing the contents inside the electrostatic storage device" through a detachable "cover."

[0050] The method includes removing a detachable cover from a container. The method includes attaching or reattaching a detachable cover to a container. The method includes accessing contents within the electrostatic storage device by separating a separable cover from a container.

[0051] The method may include replacing, repairing, refurbishing, or reusing a sealable "gasket" or "gasket material" of an electrostatic storage device.

[0052] This method may involve sealing the supercapacitor by welding or crimping. The method may include sealing or securing the electrostatic storage device in a permanent or semi-permanent manner.

[0053] The method may include maintaining an electrostatic storage device selected from the group consisting of a capacitor, an ultracapacitor, a supercapacitor, a double layer electrolytic capacitor, and a hybrid capacitor.

[0054] The method may include injecting an electrolyte into perforations in the electrostatic storage device. The method may include injecting the electrolyte so that the electrodes and the conductive energy storage material are saturated.

[0055] The method may include introducing an electrolyte into an electrostatic storage device having separations or isolated sections for electrodes, separators, or layers. The method can include introducing an electrolyte such that the electrode and the conductive energy storage material are saturated.

[0056] The method may include maintaining an electrostatic storage device that includes a resealable container.

[0057] The method can include removing contents within the electrostatic storage device. The method may include placing the contents within the electrostatic storage device into a new container, which may be resealable or non-resealable. The method may include returning the contents of the removed electrostatic storage device to the original container, which may be resealable or non-resealable. The method may include replacing, placing, or returning the contents within the electrostatic storage device back into the original container, and then sealing the container. The method may include sealing the container to complete maintenance of the electrostatic storage device.

[0058] According to another embodiment of the present invention, there is provided an electrostatic storage device comprising: (a) a container, electrodes, a separator, and a solid or liquid electrolyte capable of measuring and analyzing the operating characteristics of the electrostatic storage device to identify requirements for maintenance of the electrostatic storage device; (b) a resealable or non-resealable container that allows access to the contents within the electrostatic storage device; the interior contents include perforated, separated, or isolated sections of an electrode, separator, or layer; the electrolyte is removable and replaceable so that additional electrolyte can be added to the electrostatic storage device; The contents are placed in a non-resealable container and sealed, or an existing container is operable to be resealed.

[0059] The electrostatic storage device may include a separable cover. The detachable cover may be attachable to the container of the electrostatic storage device. The detachable cover is removable from the container. The detachable cover can be removed from the container to allow access to the internal contents for maintenance. The electrostatic storage device may include a sealable gasket. The sealable gasket may be replaceable or reusable. The electrostatic storage device may include a "gasket material." The gasket material is replaceable and reusable. The electrostatic storage device can be sealed by welding or crimping. Electrostatic storage devices can be permanently or semi-permanently sealed and fixed. The electrostatic storage device can be selected from the group of capacitors, ultracapacitors, supercapacitors, double layer electrolytic capacitors and hybrid capacitors. The electrostatic storage device may include perforations. The perforations can be filled with electrolyte so that the electrode becomes saturated. The perforations can be filled with an "electrolyte" to saturate the conductive energy storage material of the electrostatic storage device. The electrostatic storage device may include perforated, separated, or isolated sections of an electrode, separator, or layer. The electrostatic storage device may include a resealable container.

[0060] According to another embodiment of the present invention, there is provided an electrostatic storage device comprising: (a) means for providing a container, electrodes, separators, and solid and liquid electrolytes so that the operational performance of an electrostatic storage device can be measured and analyzed to identify maintenance requirements for said electrostatic storage device; (b) means for providing a resealable or non-resealable container that allows access to the contents within said electrostatic storage device; and (c) means for providing perforations, separations, or separate sections for the electrode, separator, or layer; The electrolyte is removable and replaceable so that additional electrolyte can be added to the electrostatic storage device. The contents within the electrostatic storage device can be placed into a non-resealable container and sealed, or can be manipulated to reseal an existing container.

[0061] The present disclosure also provides systems and methods for manufacturing energy storage devices, particularly supercapacitors. The present disclosure also provides a process for designing and fabricating activated carbons with preselected pore widths and pore distribution hierarchies that synergistically couple the pores of the activated carbon to electrolytes and other media (based on the size of ions, solvated ions, desolvated ions, and solvation shells). Here, the activated carbon manufacturing process involves pre-designing activated carbon with a predetermined "specific pore width and pore distribution hierarchy" (determined based on the size of the ions, ion carriers, and solvation shells that will be applied to the selected electrolyte or other medium). During the energy storage device manufacturing process, pre-designed activated carbon and selected electrolytes provide optimal and superior energy storage devices based on a hierarchical structure that matches the "ion size" and "activated carbon pore width." Additionally, preferred embodiments of the device utilize state-of-the-art co-solvents and state-of-the-art salt electrolytes, which simplify the manufacturing process. Specifically, the use of co-solvents and salt electrolytes allows manufacturing to be carried out under normal atmospheric conditions, improving safety and reducing both the cost and complexity of manufacturing energy storage devices and manufacturing facilities.

[0062] In systems and methods for manufacturing energy storage devices such as supercapacitors, the manufacturing process of "activated carbon with a predetermined pore width and pore distribution," which is influenced by ion size and the solvation shell of a specific electrolyte, provides an optimal structure and design based on "ion-pore matching" and "pore hierarchical structure."

[0063] In one embodiment, the device includes the following steps: The process of drying any carbon source. Carbonizing a suitable carbon source. The process of contacting or immersing a carbon source such as coal, petroleum, petroleum coke, or biomass with potassium hydroxide (KOH) flakes or a potassium hydroxide (KOH) solution. The above "contact / immersion time" is "about 1 hour, about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, about 12 hours, about 13 hours, about 14 hours, about 15 hours, about 16 hours, about 17 hours, about 18 hours, about 19 hours, about 20 hours, about 21 hours, about 22 hours, about 23 hours, or about 24 hours," with 12 hours being preferred. Here, the weight percent ratio range of "KOH:C" is about 1:1 wt%, about 2:1 wt%, about 3:1 wt%, about 4:1 wt%, about 51 wt%, about 6:1 wt%, about 7:1 wt%, about 8:1 wt%, about 9:1 wt%, about 10:1 wt%, about 11:1 wt%, about 12:1 wt%, with a weight percent ratio of 2 parts KOH:1 part carbon source being preferred. Water can be used to dilute the KOH base, up to a weight percent ratio of 50 parts water to 1 part KOH, with a weight percent ratio of 1 part water to 1 part KOH being preferred. The contacted carbon source is activated by a pyrolysis process under a nitrogen, helium, or argon atmosphere (nitrogen is preferred) at an activation temperature of 500°C to 1100°C for 10 minutes to 48 hours, but activation at a temperature of 800°C for 2 hours is preferred, and a temperature increase rate of 10°C per minute is preferred to produce activated carbon with a hierarchical structure and a specified pore width and pore distribution.

[0064] The activated carbon may be composed of pores with the following proportions: 1% 2% 3% 4% 5% 6% 7% 8% 9% 10% 11% 12% 13% 14% 15% 16% 17% 18% 19% 20% 21% 22% 23% 24% 25% 26% 27% 28% 29% 30% 31% 32% 33% 34% 35% 36% 37% 38% 39% 40% 41% 42% 43% 44% 45% 46% 47% 48% 49% 50% 51 %·approximately 52%·approximately 53%·approximately 54%·approximately 55%·approximately 56%·approximately 57%·approximately 58%·approximately 59%·approximately 60%·approximately 61%·approximately 62%·approximately 63%·approximately 64%·approximately 65%·approximately 66%·approximately 67%·approximately 68%·approximately 69%·approximately 70%·approximately 71%·approximately 72%·approximately 73%·approximately 74%·approximately 75%·approximately 76%·approximately 77%·approximately 78%·approximately 79%·approximately 80%·approximately 81%·approximately 82%·approximately 83%·approximately 84%·approximately 85%·approximately 86%·approximately 87%·approximately 88%·approximately 89%·approximately 90%·approximately 91%·approximately 92%·approximately 93%·approximately 94%·approximately 95%·approximately 96%·approximately 97%·approximately 98%·approximately 99%. In certain embodiments, the compositional volume of the pores has a pore width of about 2 nm (micropores) or less. Activated carbon may be porous or comprised of pores, where "compositional volume of pores" comprises the compositional volume of pores having a pore width of about 2 nm (micropores) or less, in certain embodiments, greater than about 55% and less than about 95% by volume. The activated carbon is made up of a compositional volume of "pores of about 2 nm or smaller pore width" (micropores), which in the illustrated preferred embodiment is greater than about 60% and less than about 80%. The activated carbon is composed of pores (micropores) with a pore width of about 2 nm or less, and the composition thereof is 67% by volume in a preferred embodiment. In certain embodiments, activated carbon is composed of "pores having a pore width of about 2 nm or more" (mesopores), and the composition volume of the pores is about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, about 15%, about 16%, about 17%, about 18%, about 19%, about 20%, about 21%, about 22%, about 23%, about 24%, about 25%, about 26%, about 27%, about 28%, about 29%, about 30%, about 31%, about 32%, about 33%, about 34%, about 35%, about 36%, about 37%, about 38%, about 39%, about 40%, about 41%, about 42%, about 43%, about 44%, about 45%, about 46%, about 47%, about 48%, about 49%, about 50%, about 51%, about 52%, about 53%, about 54%, about 55%, about 56%, about 57%, about 58%, about 59%, about 60%, about 61%, about 62%, about 63%, about 64%, about 65%, about 66%, about 67%, about 68%, about 69%, about 70%, about 71%, about 72%, about 73%, about 74%, about 75%, about 76%, about 77%, about 78%, about 79%, about 80%, about 81%, about 82%, about 83%, about 84%, about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96 19% approx. 20% approx. 21% approx. 22% approx. 23% approx. 24% approx. 25% approx. 26% approx. 27% approx. 28% approx. 29% approx. 30% approx. 31% approx. 32% approx. 33% approx. 34% approx. 35% approx. 36% approx. 37% approx. 38% approx. 39% approx. 40% approx. 41% approx. 42% approx. 43% approx. 44% approx. 45% approx. 46% · approx. 47% · approx. 48%, approx. 49% · approx. 50% · approx. 51% · approx. 52% · approx. 53% · approx. 54% · approx. 55% · approx. 56% · approx. 57% · approx. 58% · approx. 59% · approx. 60% · approx. 61% · approx. 62% · approx. 63% · approx. 64% · approx. 65% · approx. 66% · approx. 67% · approx. 68% · approx. 69% · approx. 70% · approx. 71% · approx. 72% · approx. 7 3%, approximately 74%, approximately 75%, approximately 76%, approximately 77%, approximately 78%, approximately 79%, approximately 80%, approximately 81%, approximately 82%, approximately 83%, approximately 84%, approximately 85%, approximately 86%, approximately 87%, approximately 88%, approximately 89%, approximately 90%, approximately 91%, approximately 92%, approximately 93%, approximately 94%, approximately 95%, approximately 96%, approximately 97%, approximately 98%, approximately 99%. In certain embodiments, the activated carbon is composed of pores with a pore width of about 2 nm or greater (mesopores) with a composition volume greater than about 5% and less than about 70% by volume. In certain embodiments, the activated carbon is composed of pores with a pore width of about 2 nm or more (mesopores), the composition volume of which is greater than about 20% by volume and less than about 40% by volume in the illustrated preferred embodiment. The activated carbon is composed of pores with a pore width of about 2 nm or larger (mesopores), with a composition volume of 32% by volume being a preferred embodiment. Furthermore, in a preferred embodiment, an average pore width between 1.8 nm and 2.7 nm is the preferred average pore width. In a particular embodiment, the composition volume of pores having a pore width of about 2 nm or more (mesopores) is "between pore widths of 2 nm and 50 nm." In an additional embodiment, the compositional volume of pores having a pore width of about 2 nm or more (mesopores) is such that the majority of mesopores have a pore width between 2 nm and 20 nm. In an additional embodiment, the compositional volume of pores (mesopores) having a pore width of about 2 nm or more is noted to be "between 2 nm and 10 nm in pore width" for the majority of mesopores. In this preferred embodiment, the composition volume of pores with a pore width of about 2 nm or more (mesopores) is between 2 nm and 5 nm in width, with most mesopores having a width of up to about 10 nm.

[0065] Activated carbon: Approximately 0.1%, approximately 0.2%, approximately 0.3%, approximately 0.4%, approximately 0.5%, approximately 0.6%, approximately 0.7%, approximately 0.8%, approximately 0.9%, approximately 1%, approximately 2%, approximately 3%, approximately 4%, approximately 5%, approximately 6%, approximately 7%, approximately 8%, approximately 9%, approximately 10%, approximately 11%, approximately 12%, approximately 13%, approximately 14%, approximately 15%, approximately 16%, approximately 17% · about 18% · about 19% · about 20% · about 21% · about 22% · about 23% · about 24% · about 25% · about 26% · about 27% · about 28% · about 29% · about 30% · about 31% · about 32% · about 33% · about 34% · about 35% pores, and in certain embodiments, the compositional volume of the pores is about 50 nm or greater (macropores). In certain embodiments, activated carbon is comprised of "pores of about 50 nm or larger in size" (macropores), the composition volume of which is greater than about 0.1% and less than about 35%. The activated carbon is composed of pores of about 50 nm or larger in size (macropores), which in this example comprise more than about 0.1% and less than about 10% by volume of the composition. The activated carbon is composed of pores of a size of about 50 nm or greater (macropores), which in a preferred embodiment make up less than 5% of the composition volume.

[0066] Additionally, energy storage devices having electrode compositions containing activated carbon may also contain "conductive additives" (carbon black, super p, furnace black, channel black, acetylene black, thermal black, lamp black, conductive carbon). In certain embodiments, the composition volume percentage is between 2% and 25% by weight of the conductive additive. In a preferred embodiment, the composition volume percentage is between 2% and 15% by weight of the conductive additive. Here, in a preferred embodiment, the "composition volume percent of the conductive additive" is about 5% by weight of "acetylene black."

[0067] Additionally, an energy storage device having an electrode composition including activated carbon may have an "electrode mix" including 2-propanol, sec-propyl alcohol, IPA, isopropyl, isopropanol, alcohol, and water. Here, in one embodiment, the composition volume percentage of the admixture is between 1 wt% and 25 wt%. In a preferred embodiment, the composition volume percentage of the admixture is between 2 wt% and 10 wt%. The preferred embodiment has a volume percent composition of the admixture of "4 wt % isopropanol."

[0068] Furthermore, the composition has a "binder" comprising a polyvinylidene fluoride (PVDF)-"polytetrafluoroethylene" (PTFE)-non-reactive thermoplastic fluoropolymer copolymer terpolymer plastic composite, with the "binder" comprising "PVDF" (ink-type electrode) and "PTFE" (free-standing electrode) being preferred embodiments. This is to form supercapacitor electrode mixtures, paints, mixtures, pastes, inks, and freestanding electrode composites. Here, in certain embodiments, the composition volume percentage is between 1% and 25% by weight of the binder. In a preferred embodiment, the composition volume percentage is between 5% and 20% by weight of the binder. The preferred embodiment has a composition volume percentage of "binder" of "approximately 10% by weight polytetrafluoroethylene (PTFE; 60% by weight dispersion in water)."

[0069] Additionally, the energy storage device includes a "current collector" that can be a variety of conductive metals, thin films, meshes, or conductive structures, including metals, stainless steel, titanium, aluminum, copper, conductive carbon, and graphene, with stainless steel and titanium being preferred. Both the "electrode admixture" and the "conductive material" may be any thickness between 0.0001 mm and 10 mm, and may be in any mesh pattern or winding.

[0070] Additionally, the energy storage device also includes an ion-permeable separator, which may include porous plastic, paper, fiber, cellulose, or an ion-permeable insulator. Both ion-permeable separators are available in a variety of thicknesses, from 0.0001 mm up to 10 mm, and in a wide range of widths, lengths, and shapes.

[0071] Furthermore, the energy storage devices include a variety of electrolytes, such as aqueous electrolytes, organic electrolytes, co-solvents in salt electrolytes, ion carrier electrolytes, ionic electrolytes, gel electrolytes, hybrid electrolytes, dry polymer electrolytes, ceramic electrolytes, and solid-state electrolyte devices, with co-solvents in salt electrolytes being preferred. This example, which is a 7.7-8.5 molar solution of sodium perchlorate (NaClO4:Sigma-Aldrich) in water-acetonitrile with a molar ratio of "1:1.5:2.5", is a preferred embodiment.

[0072] Additionally, energy storage devices include container cases of any size and shape, ranging from small circuit-sized units to very large units of kWh to several kWh.

[0073] The processing and construction of this energy storage device allows for the application of liquid electrolyte in a normal atmospheric environment. The processes and devices described herein enable safe, low-cost manufacturing processes and improved energy storage devices such as supercapacitors.

[0074] This disclosure presents systems, methods, and inventions that can be utilized to significantly improve processes, manufacturing, systems, devices, and physical energy storage devices. The present disclosure presents an invention for producing activated carbons with predetermined pore widths and pore distribution hierarchical structures, along with an invention for producing energy storage devices (especially supercapacitors). It describes a process for matching the size of the electrolyte charge carriers and the pore width of the activated carbon with a suitable electrolyte, allowing the assembly of these devices in normal atmospheric conditions. This allows for the specific control and matching of activated carbon pore width, pore distribution hierarchical structure, and desired electrolytes, leading to the fabrication of improved energy storage devices. This in turn improves the surface contact, interconnection, and propagation of electrolyte and ions within the activated carbon electrode. These improvements result in better ionic interconnection and charge transport, leading to increased energy density and performance. This is also true as the material mass loading (thickness) of the electrode material increases, which typically leads to challenges in bidirectional volumetric charge transport and volumetric ion packing, which generally result in reduced energy density and performance.

[0075] The present invention, in some embodiments, can utilize a multi-step process for manufacturing energy storage devices and components, which involves producing activated carbon materials from carbon source feedstocks with specific pore widths and pore distributions that ensure ionic and pore compatibility between the activated carbon and the electrolyte.

[0076] The multi-step process described herein may, in this example, include the following steps: drying process. The process of reducing particles to a certain size and grinding them. The carbonization process. The process of soaking in chemicals. A mixing process to ensure uniform distribution of the soaking chemicals. the drying process. A pyrolysis process to produce an activated carbon material having a predetermined pore width and pore distribution. cooling process. The process of cleaning activated carbon with additives. The process of adding electrode components to activated carbon. Mixing process of electrode components. Electrode application and freestanding electrode formation process. Optional electrode drying process. Assembly process of energy storage devices. Drying process for assembling additional options. Electrolyte impregnation process. Sealing process.

[0077] Activated carbon is typically produced from carbonaceous or lignocellulosic precursors using two existing activation techniques. 1) A method of physically and thermally activating materials using gasifying agents such as air, carbon dioxide, water vapor, and oxygen. 2) "Chemical activation" using one or more chemicals including phosphoric acid, zinc chloride, and potassium hydroxide.

[0078] Conventional activated carbon production methods typically use hydrocarbon materials such as coal or biomass, which are processed through a number of steps, including drying, carbonization, and activation. The carbonization and activation processes produce combustible gases, including hydrogen-rich product gases. These gases are typically vented from the production furnace to a separate combustion chamber where they are oxidized with air to form primarily carbon dioxide and water vapor. These may be sent to an air pollution control system to remove pollutants such as sulfur dioxide and particulates.

[0079] In one embodiment of the present invention, the present disclosure describes a continuous process for manufacturing a supercapacitor. This process comprises the following: (a) A process in which a carbon source is supplied as a raw material. (b) producing activated carbon having a predetermined pore width and pore distribution from the feedstock; (c) The process of controlling various factors that affect and result in the specific pore width and pore distribution within the formed activated carbon, including the carbon source, drying, charring, activator mixing and soaking time, activator concentration, carbon source concentration, pyrolysis reaction temperature, pyrolysis reactor atmosphere, temperature rise and fall times, cooling times, and particle size. This is to ensure optimal binding of the electrolyte for a given predetermined activated carbon pore width and pore distribution. (d) A process in which a feedstock is treated with chemicals or steam in one or more indirectly or directly heated reaction zones using an inert gas and an "activator" including at least one of KOH, water, and carbon dioxide, and mechanically connected gas inlets and gas outlets in the reaction zones to promote carbon activation. (e) removing at least a portion of the vapor or steam (which may be a separate stream of vapor or steam) from said reaction zone. (f) Recycling at least a portion of the vapor or steam or its thermally treated form into the processes described above, or recycling it as a feedstock through the processes described above, or converting it into synthesis gas (city gas). (g) removing at least a portion of said activated carbon. (h) grinding the activated carbon to a fine particle size, which can be done either before or after activation of the carbon. (i) Mixing activated carbon with conductive additives, binders, and admixtures in one or more mixing chambers. "Conductive additives" include carbon black, Super P, furnace black, channel black, acetylene black, thermal black, lamp black, and conductive carbon. "Binders" include PVDF, PTFE, non-reactive thermoplastic fluororesin, copolymers, and terpolymers. The "mixtures" include 2-propanol, sec-propyl alcohol, IPA, isopropyl, isopropanol, alcohol, and water. Supercapacitor electrode compositions are available in the form of blends, paints, mixtures, pastes, inks, and free-standing electrodes. (j) One or more extruders or sprayers are interconnected or mechanically coupled to the mixing chamber to introduce the conductive material, which may be a metal such as stainless steel, titanium, copper, aluminum, or silver, into the supercapacitor electrode composition or freestanding electrode. The electrodes may be thin films or meshes. Here, both the electrode mixture and the conductive material come in a variety of thicknesses, from 0.0001 mm up to 10 mm, and in a variety of mesh and winding patterns. (k) The extruder is equipped with or mechanically connected to nozzles, sprayer(s), scrapers, and presses to dispense the metals into the supercapacitor composition or freestanding electrode. The extruder may be metal contact or freestanding and may be equipped with a mechanical pump, compressor, gravity feed, press, auger, or press to provide a constant supply of the supercapacitor composition. (l) The device may further comprise a "mechanical feeding unit or feeder" including a winder, rollers, drum, cutter, crimper, and motor for the anode material, cathode material, and ion-permeable separator. These are mechanically coupled to the device and are used to provide a continuous supply of "ion-permeable separators" including porous plastic, paper, fiber, and ion-permeable insulators, as well as "conductive metals." These can be configured to produce energy storage devices or supercapacitor cells in which the anode-ion-permeable separator-cathode stack is wound and stacked in a continuous fashion, with multiple anode-ion-permeable separator-cathode stacked cells. (m) The device may further include a "mechanical feeding unit or feeder, including a heater and dehydrator," before the supercapacitor container or shell components. The supercapacitor container is mechanically coupled to the device, allowing for the insertion and removal of new or partially completed supercapacitor containers containing supercapacitor material at periodic or predetermined intervals. (n) A mechanical feeding unit or feeder mechanically connected to one or more extruders for energy storage containers containing energy storage materials or supercapacitor materials may have a sprayer or nozzle for dosing or injecting electrolyte. "Electrolytes" can include organic electrolytes, aqueous electrolytes, cosolvent or salt electrolytes, ion carrier electrolytes, ionic electrolytes, gel electrolytes, dry polymer electrolytes, and ceramic electrolytes. To allow the electrolyte to be dispensed under normal atmospheric conditions, a "co-solvent in a salt electrolyte" is preferred. (o) The device may include a mechanical supply unit or feeder mechanically connected to the container sealing device for an energy storage container containing the energy storage material. The sealing device may include a crimper, screw, rivet, clamp, press, weld, or seal welder to bond and secure the anode and cathode leads to the positive and negative terminals of the energy storage device. The sealing device comprises a means of sealing the container, with or without a separate seal or component. The sealing device may also include means for controlling the internal energy storage pressure (eg, vacuum). The vacuum pump is for reducing the internal pressure, including a finished energy storage cell hopper for receiving the finished energy storage device or supercapacitor cell.

[0080] A method for producing "activated carbon for use with an electrolyte" in an electrostatic energy storage device, comprising: The activated carbon is micropores having a micropore width of less than 2 nm; Mesopores having a mesopore width of 2 nm to 50 nm; and macropores having a macropore diameter of greater than 50 nm. The method includes: (a) selecting an electrolyte from the group consisting of: a "first electrolyte" having a "first average size" in which the average size of the solvated ions or desolvated ions is "1 nm or less"; A "second electrolyte" with a "second average size" in which the average size of the solvated or desolvated ions is "greater than 1 nm." (b) The process of selecting the activation temperature and activation time. When the "first electrolyte" is selected, the activation temperature is in the range of "650°C to 850°C" and the activation time is in the range of 30 minutes to 4 hours. When the "second electrolyte" is selected, the activation temperature is in the range of "750°C to 950°C" and the activation time is in the range of 30 minutes to 5 hours. (c) Activating a carbon source under an inert gas at atmospheric pressure at an activation temperature for an activation time to produce activated carbon containing more micropores than mesopores, more mesopores than macropores, and at least 0.001% macropores.

[0081] In step (c), activated carbon is produced as follows: When "first electrolyte" is selected, "50% to 95% by volume of the pores are micropores," "5% to 50% by volume of the pores are mesopores," and "0.001% to 5% by volume of the pores are macropores." Furthermore, when the "second electrolyte" is selected, "40% to 80% by volume of the pores are micropores," "20% to 60% by volume of the pores are mesopores," and "0.1% to 20% by volume of the pores are macropores."

[0082] In step (c), activated carbon is produced as follows: When the first electrolyte is selected, about 67% by volume of the pores are micropores, about 32% by volume of the pores are mesopores, and about 1% by volume of the pores are macropores.

[0083] In process (c), "The carbon source is exposed to a caustic base solution" to produce a "first powder", By "heating the first powder at the activation temperature for the activation time," the first powder is activated to generate the "second powder," "The second powder is exposed to an acidic aqueous solution" to produce "the third powder."

[0084] The method may further include at least one of drying or carbonizing the carbon source prior to step (d).

[0085] In the method of the present application, step (d) involves exposing the carbon source to a caustic basic solution, which is an aqueous solution containing potassium hydroxide.

[0086] In the method of the present application, step (d) includes contacting or immersing the carbon source in a caustic base solution in a mass ratio to the carbon source, the mass ratio being in the range of 1:1 to 12:1.

[0087] In the present method, step (d) comprises exposing the carbon source to a caustic base solution for a period ranging from 1 hour to 24 hours.

[0088] In the method of the present application, step (e) includes "heating the first powder at an activation temperature of 800°C for an activation time of 2 hours" when the electrolyte includes water, a co-solvent, and a salt.

[0089] In the present method, the co-solvent is acetonitrile.

[0090] In the present method, the salt is sodium perchlorate.

[0091] In the method of the present application, the salt molar concentration is in the range of 4 to 10M.

[0092] In the present method, the molar concentrations of the co-solvent and salt electrolyte are in the range of 7-8M.

[0093] In the present method, the molar concentration of the co-solvent and salt electrolyte is 7.7.

[0094] In the present method, the salt molar concentration is in the range of 7-8M.

[0095] In the method of the present application, the "molar ratios of salt, water, and co-solvent" are "salt in the range of 0.5 to 2," "water in the range of 0.5 to 3," and "co-solvent in the range of 1.5 to 4."

[0096] In the method of the present application, the molar ratio of salt to water to co-solvent is "1:1.5:2.5" for salt to water to co-solvent, respectively.

[0097] In the method of the present application, step (e) includes heating the first powder at a "heating rate of 10° C. per minute" before heating the first powder to the activation temperature.

[0098] In the present method, step (e) includes heating the furnace / reactor to an operating temperature prior to adding the carbonaceous material for the pyrolysis process, and placing the carbonaceous material in the preheated furnace / reactor to reach the desired pyrolysis temperature.

[0099] In the method of the present application, step (e) includes "heating in the presence of an inert gas" selected from the group consisting of nitrogen, helium, and argon gas.

[0100] In the method of the present application, step (e) "optionally dries the first powder" before activating the first powder.

[0101] The method of the present application includes "drying the first powder at 60°C to 200°C" before activating the first powder.

[0102] The method of the present application includes a step of exposing the second powder to an acidic aqueous solution of hydrochloric acid with a molar concentration of 4M for 5 minutes to 24 hours, thereby producing a soaked powder.

[0103] In the method, step (f) further comprises washing the soaked powder in water to produce a washed powder, and then drying the washed powder.

[0104] A method for manufacturing an electrode includes the following steps. (g) An electrode mixture is produced containing the "activated carbon" produced by the above method, a "conductive additive," and a "binder."

[0105] In the method of the present application, step (g) includes preparing an "electrode mixture" including a "binder" selected from the group consisting of polyvinylidene fluoride (PVDF), polyvinylidene fluoride, polytetrafluoroethylene (PTFE), copolymers, and terpolymers.

[0106] In the method, step (g) includes forming an electrode mixture further comprising a mixture.

[0107] In the method of the present application, step (g) includes producing an electrode admixture including carbon black, which is a conductive additive, and alcohol, which is an admixture containing an additive for good emulsion of the carbon black.

[0108] In the method of the present application, step (g) includes preparing an electrode admixture including acetylene black as a conductive additive and isopropanol as a mixing agent.

[0109] In the method of the present application, step (g) includes preparing an electrode mixture comprising 70 to 90 wt % activated carbon, 5 to 20 wt % polytetrafluoroethylene as a binder, 1 to 10 wt % acetylene black as a conductive additive, and 0.01 to less than 0.3 wt % isopropanol as a mixing agent.

[0110] The method of the present application further includes: (h) "Combining an electrode mixture with a conductive current collector" to "produce one of an anode and a cathode." This is achieved by pressing, spraying, milling, thin-film rolling, extruding, molding, or individually thin-filming the "electrode mix" onto the current collector. (j) If necessary, drying one of the anode and cathode. This can be done through a heated chamber or by air drying at normal room temperature for a period of time. Dehumidify the room or chamber to achieve the desired humidity level.

[0111] In the method of the present application, step (h) includes "rolling the electrode mixture into a thin film" before manufacturing one of the anode and the cathode.

[0112] In the method of the present application, step (h) includes combining the "electrode mixture" with a conductive "current collector" comprising a material selected from the group consisting of stainless steel, titanium, aluminum, copper, conductive carbon, and graphene.

[0113] In the method of the present application, step (h) includes combining the "electrode mix" with an "electrically conductive current collector" comprising stainless steel.

[0114] In the method of the present application, step (j) includes drying one of the anode and cathode at 55°C for 12 hours.

[0115] 1. An electrical energy storage apparatus comprising: (k) a pair of electrodes prepared by the above method; (l) The electrolyte as described above, wherein the electrolyte is disposed between a pair of electrodes and wets the electrodes to a desired wetness or is saturated with the entire electrode mixture composition to a desired saturation.

[0116] Herein, the device further comprises an ion-permeable separator disposed between the pair of electrodes.

[0117] In this application, the device is a supercapacitor.

[0118] [Electrolyte] To compete with batteries, there is a strong demand for the development of low-cost, safe supercapacitors (SCs) that can store high energy. Activated carbon, the primary electrode material for electrochemical double-layer capacitors, is currently reaching its capacitance limit. Our strategy is to enhance the storage capacity of porous carbons by tailoring the pore width and pore distribution hierarchy to match the appropriate electrolyte, thereby increasing the accessible surface area. This is due to the limited accessible surface area of ​​carbon in organic liquid electrolytes, even for the large specific surface area carbons used in typical commercial supercapacitors (SCs). In this study, we tailor the pore width and pore distribution hierarchy to suit the appropriate electrolyte, thereby increasing the accessible surface area and improving the storage capacity of porous carbon. The present invention presents a significant advantage in matching the porosity of microporous carbon with the recently discovered "water / acetonitrile hybrid electrolyte" and good electrolyte wettability. These embodiments provide "low diffusion resistance" and "increased accessible surface area of ​​activated carbon," resulting in high capacitive performance compared to aqueous and organic electrolytes, even with thick electrodes. This aqueous / organic hybrid electrolyte containing sodium perchlorate salt (and alternative salts of the perchlorate family, such as perchlorates, organic perchlorates, ammonium, alkali metal, alkaline earth perchlorates, and transition metal perchlorates) not only offers similar advantages to aqueous liquid electrolytes in terms of cost, safety, and smaller ion size than organic liquid electrolytes, but also offers a wider stability window. By using a hybrid electrolyte on low-cost coal-derived microporous activated carbon with most pores smaller than 2 nm, a 41.2 F / g (0.3 F / cm 2 , 18.3F / cm 3 ) and 350Wh / Kg (271.3μWh / cm 2 ) can be used to fabricate supercapacitors (SCs) with the best capacitance and high energy density. To further confirm the benefits of the present invention, the capacity performance of commercially available activated carbons with large surface areas and numerous mesopores was investigated. Comparative gravimetric capacitance was found to be higher than that of the present activated carbons (39.5 F / g and 7.4 F / cm). 3 ) and the ultimate supercapacitor, which has a much lower density and volumetric capacitance.

[0119] The energy storage mechanism of electric double-layer capacitors (EDLCs), also known as supercapacitors (SCs), originates from the electrostatic adsorption and desorption of ions on a highly porous electrode surface that is accessible to electrolyte ions. Supercapacitors (SCs) are finding increasing adoption in consumer electronics and transportation technologies due to their fast charge / discharge rates, high power density, low maintenance, and long lifespan. However, supercapacitors (SCs) have a lower energy density compared to lithium-ion batteries and are not considered as a battery replacement for grid-scale applications or electric vehicles.

[0120] "Electrodes" and "electrolytes" play important roles in the formation mechanism of supercapacitors (SCs), and are therefore important for producing high-energy density and low-cost supercapacitors (SCs). On the electrode side, "activated carbon" (AC) derived from various sources is the most widely used electrode material in commercial supercapacitors (SCs) due to its high double-layer capacitance, low cost, large "specific surface area" (SSA), chemical stability, high electrical conductivity, and controllable porosity. Generally, the capacitance of the double layer increases with increasing specific surface area (SSA), but the capacitance is limited to a certain value (1200-1500 m for some activated carbons (AC)). 2 / g) BET value" (calculated using the BET method) is constant. Studies on activated carbons (AC) with different pore widths in various electrolytes have shown that there is in fact no linear relationship between capacitance and specific surface area (SSA), and that S BET It was revealed that the specific surface area (SSA) may not reflect the effective specific surface area (SSA). The type of electrolyte, surface chemistry, pore width and distribution, pore shape, pore connectivity (hierarchical structure), and other properties have a strong influence on ion accessibility and, therefore, on specific capacitance.

[0121] Generally, activated carbon (AC) has a wide range of pore widths and pore distributions, including micropores (less than 2 nm), mesopores (2-50 nm), and macropores (greater than 50 nm). Both micropores and mesopores contribute to capacitance, but the influence of pore width and pore distribution on capacitance has not been fully elucidated due to inconsistencies in research results and interpretations. Apart from the pore width, the pore shape and the way the pores are connected (hierarchical structure) vary from one activated carbon (AC) to another depending on the type of carbon source and activation method. In related research, it remains difficult to identify the optimum porosity that results in the highest capacitance. Previous studies have suggested that organic electrolytes cannot access pores smaller than 1 nm because their solvation shells are larger than 1 nm. For example, the sizes of the solvated ions of Et4NBF4 in propylene carbonate (PC) were 1.35 nm and 1.40 nm for the cation and anion, respectively.

[0122] Subsequently, researchers achieved high capacitance in microporous "carbide-derived carbon" (CDC), which has an average pore width of less than 1 nm. The researchers found that "normalized capacitance increases as the average pore width approaches the ionic size." This increase in capacitance (normalized by surface area) for sub-nm pores is explained by the partial or complete removal of the ionic solvation shell, which facilitates access to the micropore. Therefore, some have proposed using only microporous carbon and matching the pore width to the ionic size to achieve high capacitance. However, "sub-nm pore-only electrodes can have high diffusion resistance, reducing rate capability and power density," potentially compromising key advantages of supercapacitors (SCs). Furthermore, because the specific capacitance based on the whole carbon is of paramount importance, it is difficult to realize sub-nm pore-only electrodes. Therefore, although microporous carbon increases capacitance, the small proportion of wider pores may promote diffusion within the narrow pores, reducing the diffusion resistance.

[0123] The inventors' goal is to "establish a balance between micropores and mesopores," with "mesopores acting as channels for ion transport." Furthermore, the size of the mesopores is less than 5 nm, which appears to be the upper limit of the mesopore size, larger than the size of two solvated ions.

[0124] The present invention is realized by tailoring the pore width and pore distribution (hierarchical structure) of a given carbon based on the electrochemical performance using a given electrolyte, and as an improvement of the present invention, by optimizing the activation process.

[0125] On the electrolyte side, the type of electrolyte significantly affects the electrochemical performance of activated carbon (AC). Organic electrolytes are the most commonly used in commercial supercapacitors (SCs) due to their high energy density resulting from a large stability window of 2.5V to 3V. However, organic electrolytes are "moisture sensitive" and require purification and manufacturing processes in strictly controlled environments, which increases the manufacturing costs of supercapacitors (SCs). Inexpensive "aqueous electrolytes" are safe in terms of flammability and toxicity. Aqueous electrolytes typically have high capacitance but do not necessarily have superior rate capabilities or ionic conductivity compared to organic electrolytes, and their relatively narrow electrochemical stability window limits their energy density. The operating voltage is relatively low at 1 V or less in aqueous electrolytes such as acidic and alkaline solutions, but is higher in neutral electrolytes, for example, 1.6 to 1.8 V in Na2SO4.

[0126] Recently, a new "aqueous / organic hybrid electrolyte" has been developed for supercapacitors (SCs) that has moisture resistance and non-flammability similar to aqueous electrolytes. The "hybrid electrolyte" with an optimum concentration of 5 m(mol) LiTFSI in "water / acetonitrile" produced a supercapacitor (SC) with a stability window of 2.2 V. Furthermore, a strategy of using low-cost sodium perchlorate salt as the same cosolvent was adopted to obtain a new highly concentrated hybrid electrolyte (8 m salt in water / acetonitrile) for 2.5 V supercapacitors (SCs). Due to the absence of free water molecules in the hybrid electrolyte, the combination of high salt concentration and acetonitrile additive helps achieve a wider stability window than aqueous electrolytes. However, the specific capacitance of currently demonstrated activated carbon (AC)-based supercapacitors (SCs) is still lower than that of previously known SCs using organic electrolytes, presumably due to the mismatch between the electrodes and the electrolyte.

[0127] Another important advantage of the present system and method for constructing supercapacitors (SCs) is the compatibility of the electrodes with the electrolyte. One aspect of the present invention is to "maximize the accessible surface area" of activated carbon (AC) (hierarchical structure) by "matching the porosity with the electrolyte" (ionic pore matching) and increasing the energy stored in the supercapacitor (SC). There is still a trade-off between capacitance and speed performance. For example, microporous carbons exhibit high capacitance exclusively in organic electrolytes, but too narrow pores result in high diffusion resistance and large ion and solvated ion sizes, reducing rate performance. Although the presence of mesopores helps in the rapid transport of ions into the micropores, an excess of large pores leads to carbon with low packing density, resulting in low volumetric capacitance. Furthermore, electrodes constructed with low-density activated carbon (AC) require excessive electrolyte usage, resulting in a heavier supercapacitor (SC) cell and lower overall gravimetric capacitance. Therefore, there is a narrow window of balance between micropores and mesopores that provides the best capacity performance, and this needs to be determined experimentally for the chosen electrolyte. The specific features, processes, systems, methods, and ion pore matching disclosed herein are one exemplary aspect and benefit of the present invention.

[0128] Good "wettability" between the electrodes and the liquid electrolyte is another important criterion for electrode compatibility. Wettability strongly influences the penetration of electrolyte into the electrode and thus the accessible surface area. Activated carbon (AC) is generally hydrophobic, and the micropores of the carbon cannot be completely wetted by aqueous electrolytes. This indicates that aqueous electrolytes are not suitable for hydrophobic carbons. Organic electrolytes typically exhibit good affinity for hydrophobic carbon, although this is exaggerated for thick electrodes. One method to increase the affinity between porous carbon and aqueous electrolytes is to introduce "functional groups containing nitrogen or oxygen" into activated carbon (AC). However, excessive heteroatom doping leads to reduced electronic conductivity and structural defects. In the present invention, because acetonitrile is present as a co-solvent, hydrophobic activated carbon (AC) can also be wetted by the hybrid electrolyte. Nuclear magnetic resonance spectroscopy (NMR) showed that acetonitrile penetrated the micropores of the carbon, demonstrating "an affinity between the micropores and acetonitrile."

[0129] The imbalance between the electrode and electrolyte is the main cause of the insufficient energy density of activated carbon (AC)-based supercapacitors (SCs), which is due to the limited access of ions to the carbon pores (ion-pore mismatch, wetting problems) and the low packing density caused by excess pores. This embodiment of the present invention is configured to produce the desired activated carbon paired with an electrolyte to create and realize a supercapacitor with superior performance.

[0130] The invention disclosed herein describes a process for "matching the porosity of the microporous carbon to the co-solvent electrolyte" to "maximize the surface area accessible to the electrolyte ions." Sodium perchlorate is advantageous due to its low cost and small ionic size compared to common salts used in organic electrolytes, making it a desirable salt for hybrid electrolytes and a beneficial embodiment of the present invention. For the porosity of activated carbon (AC), S BET 1200m 2 It is preferable to choose a microporous carbon with more than 1000 .mu.m / g, since the micropores play an important role in double layer charge storage. Aqueous electrolytes may pass such AC compatibility tests due to the small size of their ions, but they have a low stability window and poor AC wettability. Both the organic and hybrid electrolytes meet the wettability and stability window requirements (2.7 V vs. 2.5 V), and the smaller size of the ions and solvated ions in the hybrid electrolytes leads to superior and improved devices. Now, if we use the same porous carbon in the present invention, the "hybrid electrolyte" will provide higher capacitance for its small ions and easier access to the micropores. For example, although some of the micropores are too small for the ions of the organic electrolyte to enter, "the micropores match the size of the ions in the hybrid electrolyte," which is an exemplary improvement of the present invention. Furthermore, the "hybrid electrolyte" exhibits "superior rate capability" due to the smaller ions and the low diffusion resistance of their solvation shells, which is another improvement in the present invention. That is, the hybrid electrolyte, with its small ion size, allows the use of porous carbons with smaller pores than organic-compatible carbons. This increases energy density and performance and is an exemplary advantage of the present invention. It is also useful to be able to tailor the porosity of the carbon without excessively increasing the packing density, which is another embodiment and advantage of the present invention.

[0131] One of the preferred embodiments of the present invention proposes microporous coal-derived carbon as the carbon source for activated carbon (AC) by "fine-tuning the pore width and pore distribution hierarchy" based on "KOH saturation and activation temperature" to achieve the best electrochemical performance with "hybrid electrolyte." The prepared activated carbon (AC), called "TC800" (fuel carbon activated at an activation temperature of 800°C), has a hierarchical pore structure containing "micropores up to 2 nm" and "mesopores in the range of 2 to 6 nm."

[0132] [Experimentation] While the embodiments are described below, the experiments, experimental studies, and analyses generally describe the claimed invention on a laboratory scale, and the disclosed processes, material preparations, device configurations, and compositions are intended to be adapted for large-scale commercial processes and treatments. The following sections disclose processes, actions, configurations, test results, and theory, but are not intended to limit the scope of the present invention. Those skilled in the art will be able to benefit from and utilize the processes, systems, methods and compositions of matter disclosed herein using conventional and modern methods of manufacturing, material processing and energy storage construction. These processes and compositions can be implemented and used to realize the benefits of the present invention or as additional embodiments of the disclosed invention.

[0133] [Activation of fuel coal (TC)] Raw thermal coal (TC; sub-bituminous coal from Dodds Coal Mine, Alberta, Canada) was manually crushed and "ground" with a pestle and mortar. The "fuel coal (TC) powder" was then sieved (No. 140, 106 μm openings) and then ground in a ball mill (Pulverisette 7, Fritsch GmbH) at 350 rpm for 30 min. A 2 mm zirconium oxide ball was used to measure the fine particle size (d 50 <20 μm). "Raw fuel coal (TC)" was soaked in "KOH aqueous solution" (mass ratio of KOH to fuel coal (TC) 2:1) for 12 hours and then dried in an oven at 60°C. The fuel coal (TC) / KOH was then placed in a stainless steel container and subsequently heated in a tube furnace (Lindberg / Blue M™ Mini-Mite™) under a nitrogen flow. The sample was heated at a rate of 10°C / min and held at the activation temperature (either 600, 700, or 800°C) for 2 hours. Next, the as-prepared activated carbons were immersed in a 4 M HCl solution for 8 hours, washed thoroughly with distilled water, and dried overnight in an oven at 60°C. The final products were expressed as TC600, TC700, and TC800 depending on the activation temperature.

[0134] Structural characterizations The morphology of the samples was obtained by scanning electron microscopy (SEM; Tescanmira 3 XMU), and the elemental composition was collected by energy dispersive spectrometer (EOS; X-Max detector, Oxford Instruments). X-ray diffraction (XRO; Bruker 08-Advance X-ray diffractometer) spectroscopy was used to investigate the crystal structures of raw fuel coal (TC) and activated carbon (AC) (TC600, TC700, and TC800). To obtain the porous characteristics of activated carbon (AC), "nitrogen adsorption-desorption" was measured at 77K using a quantum chromium apparatus. The apparent surface area was obtained using the Brunauer-Emmett-Teller (BET) method.

[0135] [Electrochemical characterization] The prepared electrode is an exemplified preferred embodiment of the present invention, and was prepared by mixing "85 wt% activated carbon (AC)", "10 wt% polytetrafluoroethylene" (PTFE; 60 wt% dispersion in water, MTI), "5 wt% acetylene black" (AB; MTI), and "a few drops of isopropanol". The paste was roll pressed into a thin film and die cut into circular disks with a diameter of 1.27 cm. The electrodes were manually pressed onto a woven titanium mesh of the same diameter and dried in an oven at 55°C for 12 hours. Two types of activated carbon (AC) were used to prepare the electrodes. The base materials were thermal coal (TC) (TC600, TC700, and TC800) and a commercial activated carbon (AC) called AC30 (ASAC30, AdvEn Industries Inc.). The area mass loading of the electrodes used for porosity and electrolyte studies is 3.6–4.5 mg / cm. 2 " range.

[0136] All electrochemical tests were carried out by assembling the supercapacitor (SC) in a symmetrical two-electrode system (CR2032 coin cell). Briefly, two specific electrodes were sandwiched between two stainless steel current collectors and separated by one separator (Whatman grade 1 for aqueous and hybrid electrolytes, glass fiber for organic electrolytes). In all cells, the amount of electrolyte used was approximately 80 μL.

[0137] It was found that optimizing the hybrid electrolyte salt:water:acetonitrile molar ratio to 1:1.5:2.4 resulted in an 8 m (molar concentration, mol / kg) solution, which also contains some of the present examples. In addition, in order to ensure the stability of the liquid electrolyte at room temperature, an "approximate molar ratio of 1:1.5:2.5" was used in another preferred embodiment. Namely, a 7.7 m solution of sodium perchlorate (NaClO4; Sigma-Aldrich) in water / acetonitrile, 1 M Na2SO4 (Sigma-Aldrich), and 1 M tetraethylammonium tetrafluoroborate (Et4NBF4; Sigma-Aldrich) in propylene carbonate (PC) were used as common aqueous and organic electrolytes, respectively. Supercapacitors (SCs) containing organic electrolytes were fabricated in an argon-filled glove box.

[0138] Electrochemical tests were performed using an electrochemical workstation (SP-150, BioLogic). Galvanostatic charge-discharge (GCD) measurements were performed at constant currents ranging from 1 to 700 mA, depending on the rate capability of the individual samples. The minimum threshold depends on the ionic conductivity and viscosity of the electrolyte and can be defined as the current at which the coulombic efficiency begins to decrease. The minimum GCD currents for aqueous, organic, and hybrid electrolytes were determined to be 1 mA, 2 mA, and 3-5 mA, respectively. Electrochemical impedance spectroscopy (EIS) tests were recorded at frequencies ranging from 100 kHz to 0.01 Hz with an AC amplitude of 10 mV and zero DC amplitude. Cyclic voltammetry (CV) curves were performed at scan rates ranging from 20 to 600 mV / s. Galvanostatic charge-discharge (GCD) cyclic tests were performed using a battery tester (BTS-4008-5V-50mA, Neware) and an electrochemical workstation (VMP, BioLogic).

[0139] The capacitance characteristics of the supercapacitors (SCs) were calculated based on the galvanostatic charge-discharge (GCD) curves. The cell capacitance is calculated using the formula C=IΔt / (ΔV-V IR ) where I is the discharge current. Δt is the discharge time, ΔV is the potential window, and V IR is the potential drop at the beginning of the discharge curve. Energy (E) and power (P) are respectively E=0.5C(ΔV-V IR ) 2 =0.5I(ΔV-V IR )Δt and P=E / Δt. The equivalent series resistance (ESR) of a supercapacitor (SC) is ESR=V IR Calculated from / I. These were divided by m to obtain gravimetric capacitance, energy, and power densities. where m is the total weight of both electrodes (including 30 activated carbon (AC), binder, and conductive additives). The area-specific capacitance, energy, and power density were calculated by dividing these by A. where A is the geometric area of ​​the electrode (1.266 cm 2 ) Current density is also defined as I / m or I / A. The current of the cyclic voltammetry (CV) curve is C CV Normalized to capacitance using =I / (mv). where v is the potential scan rate. [Brief explanation of the drawings]

[0140] The present invention will now be described with reference to the detailed description of the present embodiments and the drawings. [Figure 1] FIG. 1 shows a first embodiment of the system and method disclosed in this application. [Figure 2] FIG. 2 is a block diagram illustrating the functional steps of the system and method disclosed herein. [Figure 3] FIG. 3 is a diagram showing the layers and internal structure of the supercapacitor of the system and method disclosed herein. [Figure 4] FIG. 4 is a diagram showing the rows of pores inside the supercapacitor of the system and method disclosed herein. [Figure 5]Figure 5 shows a single microporous sheet with two leads inside the supercapacitor of the systems and methods disclosed herein. [Figure 6] Figure 6 shows the opposite side of a single porous sheet with multiple leads inside the supercapacitor of the systems and methods disclosed herein. [Figure 7] FIG. 1 is a diagram showing the outer housing of an embodiment of the supercapacitor of the system and method disclosed herein. [Figure 8] FIG. 10 is a diagram showing the cover of the external housing of this embodiment of the supercapacitor of the system and method disclosed herein. [Figure 9] FIG. 9 illustrates a fastener for the external housing of this embodiment of the supercapacitor of the systems and methods disclosed herein. [Figure 10] FIG. 10 illustrates the seal and gasket of the external housing of this embodiment of the supercapacitor of the system and method disclosed herein. [Figure 11] Figure 11 shows an example of the system and method disclosed herein, depicting a cylindrical supercapacitor with a pore lining, a co-solvent in the salt electrolyte, and a high surface area, low-cost, and widely available derived composite material. [Figure 12] Figure 12 shows an example of a cylindrical supercapacitor with a pore lining of the systems and methods disclosed herein. [Figure 13] FIG. 13 illustrates an example embodiment of the systems and methods disclosed herein, a cylindrical supercapacitor with a partitioned interior section. [Figure 14] FIG. 14 illustrates an example embodiment of the systems and methods disclosed herein, a layered or cubic supercapacitor with partitioned internal sections. [Figure 15] FIG. 15 is a diagram illustrating this embodiment of the present invention, which includes a single reactor multi-zone activated carbon production system and a continuous carbon material feed system with an energy storage production system. [Figure 16]Figure 16 is a block diagram of this embodiment of the present invention, which includes a continuous carbon material feed system with a single reactor multi-zone activated carbon production system and energy storage production system. [Figure 17] FIG. 17 is a block diagram of an embodiment of the present invention including a continuous carbon material feed system with a multi-reactor, multi-zone activated carbon production system and energy storage production system. [Figure 18] FIG. 18 is a block diagram of an embodiment of the present invention including an activated carbon generation system and an energy storage and generation system. [Figure 19] FIG. 19 is a block diagram of an embodiment of the present invention including an activated carbon generation system and an energy storage and generation system. [Figure 20] FIG. 20 is a block diagram of an embodiment of the invention including an energy storage and generation system with a self-sustaining electrode generation system. [Figure 21] FIG. 21 is a block diagram of an embodiment of the present invention including an energy storage production system with an ink-type / mixed electrode manufacturing system. [Figure 22] FIG. 22 is a block diagram of an embodiment of the present invention comprising a predetermined pore distribution activated carbon production system. [Figure 23] FIG. 23 is a block diagram of an embodiment of the present invention including an energy storage and generation system in which activated carbon pores and electrolyte ions are matched in size and distribution. [Figure 24] Figure 24(a), (b), and (c) show the absorption of electrolytes with and without solvent shells on the surfaces of different pore sizes (micropores <0.6 nm, micropores <15 nm, and mesopores <2.5 nm), where (a) is an organic electrolyte, (b) is an aqueous electrolyte, and (c) is a hybrid electrolyte. [Figure 25] Figure 25(a)(b)(c)(d)(e)(f) shows the effect of activation temperature on the carbon structure and supercapacitor performance of TC600, TC700, and TC800 using hybrid electrolytes. (a)(b)(c) are SEM images, (d) is XRD pattern, (e) is nitrogen adsorption / desorption isotherm, and (f) is pore distribution. [Figure 26] Figure 26(a), (b), and (c) show the performance of supercapacitors (SCs) assembled from TC800 using hybrid, organic, and aqueous electrolytes. (a) Specific capacitances obtained from the galvanostatic charge-discharge (GCD) curves of TC1, TC4, and TC5; (b) Ragone plots obtained from the galvanostatic charge-discharge (GCD) curves of TC1, TC4, and TC5; and (c) Nyquist plots obtained from electrochemical impedance spectroscopy (EIS) tests. [Figure 27] (a), (b), (c), (d), (e), and (f) show the performance of SCs constructed from TC800 electrodes using hybrid, organic, and aqueous electrolytes (a–c). (a) is the specific capacitance obtained from the GCD curves of TC1, TC4, and TC5; (b) is the Ragone plot obtained from the GCD curves of TC1, TC4, and TC5; and (c) is the Nyquist plot obtained from EIS tests. The inset photographs were taken up to 4 seconds after electrolyte application onto the electrodes, demonstrating the surface wettability of each electrolyte. Performance comparison of SCs fabricated from TC800 (TC1) and AC30 (AC1) electrodes using hybrid electrolytes (d–f). (d) is the CV plot, (e) is the gravimetric and volumetric capacitance plot, and (f) is the Ragone plot of the gravimetric and volumetric capacitance plot for TC1 and AC1. [Figure 28] (a)(b)(c)(d) Images showing the cycling characteristics of TC8 with hybrid electrolyte (TC800, 3.95 mg / cm2) over 370k GCD cycles for various currents and voltages, where (a) is the specific capacitance versus cycle number, (b) is the energy density versus cycle number, (c) is the power density versus cycle number, and (d) is a photograph of 31 green LEDs lit for 55 minutes followed by 32 red LEDs lit for 4 minutes, where the green and red LEDs are all connected in parallel and powered by one SC (supercapacitor) charged to 2.5V. [Figure 29](a)(b)(c) Images showing the performance comparison of TC1 against state-of-the-art AC-based SCs (SC1, SC2, SC3, SC4, SC5) reported in the research literature, where (a) shows the specific capacitance, (b) shows the gravimetric Ragone plot, and (c) shows the area-based Ragone plot. [Figure 30] This image shows a comparison of current literature performance studies on supercapacitors, performance results for commercially available supercapacitors, and performance results for supercapacitors fabricated using the inventive system and method disclosed herein. [Figure 31] (a) and (b) are images showing the hierarchical structure of carbon pores in various activated carbons, where (a) shows the preferred hierarchical structure of activated carbon produced by the system and method of the present invention, and (b) shows the hierarchical structure of highly microporous activated carbon. DETAILED DESCRIPTION OF THE INVENTION

[0141] [Detailed Description of the Invention] The present disclosure is intended to enable one skilled in the art to make and use the invention, and describes several alternative embodiments, adaptations, variations, alternatives, and uses. Embodiments, additional embodiments, features, and advantages of the present disclosure will become apparent to those skilled in the art upon review of the detailed description of the present disclosure in conjunction with the accompanying drawings.

[0142] In this specification and claims, the singular forms "a," "an," and "the" may include the plural unless the context clearly dictates otherwise. Unless expressly indicated otherwise, all technical, scientific and descriptive terms used herein have the same meaning as commonly used terms and forms by one of ordinary skill in the art.

[0143] Unless otherwise expressly stated, all references expressing reaction conditions, stoichiometries, component concentrations, and the like used in the specification and claims are to be understood as including all instances by the term "about." Additionally, unless indicated otherwise, the numerical parameters and ranges set forth in the specification and claims are expressed as approximations that may vary depending upon particular or alternative analytical techniques.

[0144] In this disclosure, the term "macropore" refers to a "pore having a pore width greater than 50 nm." In the present disclosure, the term "mesopore" refers to "pores having a pore width of about 2 nm to about 50 nm." In this disclosure, the term "micropore" refers to a "pore having a pore width of less than about 2 nm."

[0145] In the present description, the term "carbon source" is intended to mean a material (raw material, product, or reaction intermediate) that contains the element carbon. Carbon sources are renewable on time scales of days, months, years, decades, centuries, thousands of years, millions of years, or longer.

[0146] In this description, the term "reagent" is used in its broadest sense. Reagents can be fuels, chemicals, materials, compounds, additives, mixtures of ingredients, solvents, etc. A reagent is not necessarily a chemical substance that causes or reacts with a chemical reaction. A reagent may or may not be a chemical reactant that is consumed in a particular reaction. A reagent may also be a chemical catalyst for a particular reaction. Reagents may be used to adjust the mechanical, physical, and / or hydrodynamic properties of the material, or some reagents may be absent.

[0147] A "carbon source" as provided herein typically contains about half of its weight as carbon, and generally is about 50 weight percent or less biomass. Depending on the specific feedstock composition, the carbon source may contain at least 40 weight percent carbon, at least 45 weight percent carbon, at least 50 weight percent carbon, at least 55 weight percent carbon, at least 60 weight percent carbon, at least 65 weight percent carbon, at least 70 weight percent carbon, at least 75 weight percent carbon, at least 80 weight percent carbon, at least 85 weight percent carbon, at least 90 weight percent carbon, at least 95 weight percent carbon, at least 96 weight percent carbon, at least 97 weight percent carbon, at least 98 weight percent carbon, or at least 99 weight percent carbon.

[0148] Notwithstanding the foregoing, the term "carbon source" is used herein for practical purposes only to describe the materials that are processed to construct the present system in various alternative embodiments. Any limitations on specific carbon content, carbon concentration, or carbon composition are not implied by the terms themselves, but only by reference to specific embodiments or equivalents thereof. For example, materials with low initial carbon content subjected to the present systems and methods can produce highly improved carbon sources compared to "starting materials" that can provide high yields of carbon source. However, it is not relevant for relatively low carbon source starting materials having low purity carbon, which may include carbon sources having less than about 50 weight percent carbon. The carbon source may also be a raw material or mixture that contains carbon or that can be converted to carbon. Basically, the carbon source can contain carbon, hydrogen, and oxygen. The claimed systems, methods and devices are capable of handling a wide range of feedstocks of different types, sizes and moisture contents.

[0149] Carbon sources may include, for example, plants and plant-derived materials, vegetation, agricultural waste, forestry waste, wood waste, paper waste, animal waste, poultry waste, municipal solid waste, biomass, wood harvest residues, softwood chips, hardwood chips, tree branches, tree stumps, knots, leaves, bark, auger waste, paper pulp, cellulose, wheat straw, rice straw, sugarcane bagasse, switchgrass, miscanthus, livestock manure, municipal solid waste, municipal sewage, commercial waste, pumice, almond shells, pecan shells, coconut shells, coffee grounds, grass pellets, hay pellets, wood pellets, cardboard, paper, carbohydrates, plastics, cloth, carbon-containing feedstock fuels such as fossil fuels other than biomass, coal, petroleum coke, and mixtures of biomass and fossil fuels such as mixtures of biomass and coal. In this example, the carbon source raw material is or includes coal, oil shale, crude oil, asphalt, petroleum coke, and other crude processed solids. Carbon sources may include waste tires, recycled plastic, recycled paper, and other waste and recycled materials.

[0150] FIG. 1 is a diagram of a first embodiment of the present system and method, showing the components necessary to achieve the maintainability of an electrostatic storage device (supercapacitor) 135 made from inexpensive and abundant materials such as thermal coal, petroleum coke, and biomass. Conventional capacitors are designed to be disposable and non-maintainable. This is due to several factors, including the typically small physical size, the number of supercapacitors used as a single device or unit, and the prohibitive cost of maintaining these devices. With the advent of large supercapacitor 135-based systems for grid-scale energy storage, the ability to maintain supercapacitors 135 is now becoming a viable and economical alternative to disposables, with the goal of extending the life and operational performance of the supercapacitors. This is achieved by the present systems and methods. Furthermore, the use of supercapacitors in grid-scale applications allows for low cost availability and low potential energy density for fabrication, eliminating the need for premium materials to maximize energy density and compete with battery technology on physical size.

[0151] The first embodiment utilizes a "resealable container 15," meaning that the container 15 can be opened and closed at the discretion of the user. This allows the supercapacitor 135 to be opened and then resealed after maintenance is complete. Such a configuration can be achieved in several ways, utilizing a main supercapacitor housing 15 or container 15, gaskets 65 or seals 65, separable covers 25, fasteners 35, and "internal contents 99" of the supercapacitor 135 suitable for receiving maintenance.

[0152] In another embodiment, a "non-resealable container 15" may be used, and the "internal contents 99" may be removed and placed in another additional container 15. The supercapacitor 135 utilizes a perforated "separator and electrode layer 99." These perforations allow electrolyte (not shown) to be injected and saturate the entire internal contents 99 of the supercapacitor 135 when the supercapacitor 135 is to be serviced. These perforations solve the problem of uniformly and completely saturating the electrodes and conductive materials with the "contents 99" inside the supercapacitor.

[0153] The components of the supercapacitor 135 and their natural property of storing charge as an electrostatic field reduce degradation of the elements of the supercapacitor 135 . Specifically, activated carbon, obtained from a low-cost carbon source (not shown), is a highly stable element that is frequently used, robust, and provides a very long operational life. Furthermore, the metal components of each cell of the supercapacitor 135 are typically formed of the same metal to prevent charge from simply being stored electrostatically and to prevent the cell from operating electrically. Galvanic cells degrade the metal elements that store the charge over time, so preventing the formation of galvanic cells can prevent major failures of the metals used in the electrodes caused by corrosion and degradation of the electrolyte (not shown). Designing the electrodes to prevent or minimize corrosion results in stable cells with extremely long operating life. Such minimal degradation can be achieved by using high-quality conductive materials with long life such as stainless steel, chromium, and graphene, to name a few non-limiting examples.

[0154] The above design and operation methodology realizes advantages of supercapacitors that are not available from conventional batteries or currently available supercapacitors. This includes extending the operational life of each cell by allowing maintenance to be performed on components of the cell that require maintenance. This is achieved by providing access to these components, allowing proper identification of faulty or failed components, and enabling uniform and proper maintenance of those components. Furthermore, the use of low-cost, abundant carbon sources can reduce the cost of the device, a key factor in commercial success. Furthermore, the use of widely available carbon sources allows for rapid scalability of the technology, a critical factor for success.

[0155] A first exemplary maintenance technique involves the use of sodium perchlorate, of the general formula NACL04, and a mixture of sodium perchlorate and sodium perchlorate of the general formula CH3CN. The solution is to add electrolytes such as acetonitrile (TIFF0007580089000002.tif5977) and "co-solvents in salt electrolytes" containing water. In some embodiments, the electrolyte has a molar ratio of about 7-8 and consists of 1 part sodium perchlorate, 1.5 parts water, and 2.4 parts acetonitrile, but can also include the common salt lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), sodium chloride, ammonium dichlorate, magnesium sulfate, and sodium bicarbonate. In variants, the liquid electrolyte includes "a cosolvent in an electrolyte salt, an aqueous electrolyte, an organic electrolyte, or an ionic fluid." In the first embodiment, the electrolyte is introduced into the "perforatings 85" and "internal layers 99 of the device," and then, with these layers aligned, an injector (not shown) injects the electrolyte (not shown) into these columns, saturating the conductive elements 99 throughout the device.

[0156] The manner and shape of the perforation 85 is not necessarily critical and may include any number of different holes, slits, configurations, shapes, or combinations thereof. The perforations 85 may be pre-formed in each sheet prior to assembly, and further, the perforations 85 may be formed before the assembled, complete serviceable device 135 is sealed. The perforations 85 may be pre-formed in the separator separating the anode and cathode, or the separator may be unperforated depending on the desired results.

[0157] FIG. 1 illustrates a maintainable electrostatic storage device 135, in this example a supercapacitor 135, including a container 15, a detachable cover 25 that is the lid of the container, a fastener 35, a lead insulating holder 175, lead wires 115, and a gasket 65 or seal 65. The supercapacitor section 99 may include a supercapacitor 135 made up of a double layer electrolytic capacitor 125 that includes "perforations 85." The "supercapacitor maintenance" operation is performed by removing fasteners 35 and container cover 25 to access section 99 of the capacitor, and then "injecting electrolyte into perforations 85" of double layer electrolytic capacitor 125. Providing such a novel and stable electrolyte can fundamentally refresh the supercapacitor 135 and extend the life of the supercapacitor 135. Through research and experimentation using supercapacitor 135, the inventors have determined that there are two main causes of premature failure of supercapacitor 135. These main causes include the electrolyte (not shown) and the metal that makes up electrode 115. Generally, the electrodes, separator, container 15, and carbon material (not shown) that make up the remainder of the cell are stable almost indefinitely. By maintaining the supercapacitor 135 components as they fail or wear out over time, a device can be created that provides benefits over a long period of time, potentially even multiple generations. Although this embodiment uses a double layer electrolytic capacitor 125 as an example, the benefits of the present system and method for providing the robustness and long life of these devices can be applied to many other types of capacitors 135, including hybrid capacitors (not shown). While a supercapacitor 135 for charging is given as an example, possible alternative embodiments are further referenced herein and may be described and implemented with reference to the section "Storage Devices," and the referenced possible alternative embodiments are further referenced herein and may be described and implemented with reference to the section "Applications" as well as the section "Implementations."

[0158] FIG. 2 is a block diagram showing the functional steps of the system and method of the present invention. FIG. 2 includes identifying supercapacitors 135 and other maintainable devices 135 comprised of low-cost carbon sources and co-solvents in a salt electrolyte, testing the devices 205 to determine if they require maintenance (225), and either removing the devices from operation (235) or restoring them to operation (215) depending on whether the devices require maintenance. If the device is removed from operation (235), the process of servicing the device involves opening (245) the device, accessing (255) the contents inside the device, servicing (265) the device (including servicing 275 the liquid electrolyte of the device), sealing (285) the device after servicing is complete, and returning (215) the device to operation. The maintainable device 135 may include a variety of different electrostatic storage devices or accumulators, including supercapacitors 135, solid electrolytic capacitors, and hybrid capacitors (not shown) are non-limiting examples. Testing (205) of the device can be accomplished in many ways, including capacitance testing, voltage testing, timing-based testing, thermal testing, fade and stability testing, current absorption testing, and other tests to verify that the maintainable device 135 is operating with desired operating characteristics and performance. Once a serviceable device 135 is identified (225) as needing maintenance, the device 135 must be removed from operation (235) to perform the maintenance. At this stage, the device 135 is usually opened (245) for maintenance, but by directly incorporating the maintenance system and maintenance components required for maintaining the device into the maintainable device 135, maintenance can be performed without opening the device. Supercapacitors 135 typically have a very long lifespan, said to be capable of lasting 1 to 2 million cycles, which, combined with their low storage capacity, generally makes maintenance uneconomical. With the advent of very large systems and the development of energy storage methods with supercapacitors135 with kilowatt-hour capacities, the advantages of achieving maintainable devices135, extending operational life and reducing construction costs have become apparent. Through research, the inventors have determined that the presence of certain structures and materials within the device contributes to the premature failure of the device. Additionally, the inventors have identified applications that would benefit from using low-cost, widely available materials to lower the cost per unit of energy storage in these devices, including grid storage, electric vehicles, electronic appliances, and electrical and electronic devices.

[0159] Among the causes of failure of the supercapacitor 135, the most frequent one is "instability of the electrolyte (not shown)." In some embodiments, an electrolyte, essentially formed of a soluble material (not shown) in a solution (not shown) that acts as an ionically conductive additive, begins to lose stability and separate over time. This may include gas evolution and evaporation, as well as separation of solids into solution. The common point is that the electrolyte becomes unstable or inappropriate and the supercapacitor 135 fails or does not operate in an optimal manner. By allowing the liquid electrolyte to be maintained (275), the operating life and performance of the supercapacitor 135 can be extended. This is highly beneficial given that other forms of energy storage, especially at grid scale, lack the ability to maintain or extend their operational lifespan. An example of this is lithium ion, which typically requires replacement of the entire lithium ion storage solution after 2000-8000 cycles. Longer lifespans bring economic and environmental benefits. This is to achieve the amount of energy storage necessary for our civilization to fully transition away from hydrocarbons, and furthermore, the economic benefit of extending the operational life of a supercapacitor 135 such as a maintainable device 135 is that the maintainable storage device 135 does not have to be replaced as frequently. Reference is made to a supercapacitor 135 for charging, but possible alternative embodiments are additionally referenced herein and are described and implemented with reference to the section "Storage Devices," and possible alternative embodiments are additionally referenced herein and are described and implemented with reference to the "Applications" section as well as the "Implementations" section.

[0160] FIG. 3 shows the layers and interior of a supercapacitor 135 combined to clearly show the "perforation columns" of the present system and method. A common configuration for large capacitance supercapacitors has traditionally been a wound cylindrical configuration. Winding the layers of the supercapacitor 135 together during fabrication, while a mainstream manufacturing process, makes maintaining the electrolyte (not shown) more difficult. Although this specification describes maintaining the interior region of the capacitor by drilling 85 and isolation, this is not a requirement and the electrolyte can be maintained by conventional injection and isolation methods. The double layer electrolytic capacitor 125 is constructed from materials such as conductor 45, separator 95, leads 115, perforations 85, and a low-cost compound with a high surface area (not shown). These materials are typically formed by dosing or applying a high surface area, low cost compound (not shown) to a conductor 45 with a layer of separator 95. Then, another high surface area compound (not shown) is dosed on the separated conductor 45, saturated with an electrolyte such as a "co-solvent in salt electrolyte" (not shown), and stacked, wound, or layered. Such a configuration is beneficial when used in the systems and methods of the present invention, particularly by stacking the layers of the double layer electrolytic capacitor 125 so that the injector can saturate all layers, which is highly advantageous as it simplifies the maintenance process. The layered perforation 85 configuration of FIG. 3 allows for efficient maintenance of the electrolyte (not shown) and provides a system in which many individual supercapacitor cells can be maintained simultaneously. Because the present system and method provides significant economic benefits, simplified maintenance is a key feature for implementing maintenance of large numbers of cells 135 and systems.

[0161] FIG. 4 is a diagram showing a row of perforations 85 within the supercapacitor of the present system and method. FIG. 4 is intended to represent the rows of perforations 85 in this non-limiting example of a double layer electrolytic capacitor 125. In FIG. 4, the conductor 45 and separator 95 are perforated with uniform rows of perforations 85, which allows electrolyte (not shown) to be injected at uniform intervals throughout the double layer electrolytic capacitor 125 during maintenance. The leads 115 are separated by insulating separators 75 to prevent bridging. The advantage of the perforations 85 is that they allow for the injection of electrolytes and cleaning agents without separating the layers of the supercapacitor, even for larger supercapacitors 135 and typical commercial-scale supercapacitors. The elimination of the need to separate layers during maintenance reduces the risk of damage to the capacitor, such as carbon elements (not shown) peeling off from the conductive electrodes. Additionally, the uniform distribution of the rows of perforations 85 allows the liquid electrolyte to saturate outward, completely saturating all of the conductive spaces of capacitor 135, thereby providing optimal performance after maintenance.

[0162] FIG. 5 shows a single "perforated membrane 85" with two leads 115 within the supercapacitor of the present system and method, with the leads having an anode and cathode with opposing or perpendicular faces. The "thin membrane with perforations 85" includes conductors 45, perforations 85, and leads 115. For this perforation design to be most effective when single sheets are assembled as shown in Figure 5, they must be stacked and the rows aligned so that the injector can reach the rows without damaging the capacitor's internal material. In this example, the perforations are circular, but a variety of shapes can be used and the distance between the perforations may vary depending on a number of factors, including the viscosity of the liquid electrolyte (not shown). Of course, in some cases it may be beneficial to provide perforations 85 directly in the separator material so that the separator material can distribute the electrolyte throughout the conductive material 45 . This can be achieved by incorporating small perforations 85 into the separator channels that act as distribution pathways for the electrolyte (not shown).

[0163] FIG. 6 shows a single perforated sheet 85 with four leads inside the supercapacitor of the present system and method, covered with a high surface area, low cost, abundant "admixture 55" such as activated carbon derived from coal, petroleum coke, or biomass. 6 includes conductor 45, perforation 85, and lead wire 115. FIG. Certain configurations may benefit from having multiple leads from the electrodes 115 (anode and cathode), allowing for more diverse assembly and connection layouts, including multiple assembled top capacitors as well as multiple final connection configurations for each layer, with the leads 115 located on the same, opposite, or perpendicular faces of the container. This multiple-lead configuration can benefit the performance of the supercapacitor because the use of multiple opposing or perpendicular leads for both the anode and cathode (positive terminal, negative terminal, current collector) "provides low charge spreading resistance." This low diffusion resistance can be attributed to the short distance that charge travels within the cell. A non-limiting example of this configuration is a cylindrical supercapacitor with a positive anode and a negative cathode on both the top and bottom of the supercapacitor. In this non-limiting example, the positive and negative connections can be made individually to the top and bottom anodes and cathodes, or the positive and negative connections can be made simultaneously to the top and bottom anodes and cathodes. When both the anode and cathode are simultaneously connected to the positive and negative terminals of the appropriate polarity leads, this configuration results in very low diffusion resistance during charging and discharging, allowing supercapacitor operation in a series circuit or series connection. This multi-lead configuration can benefit all forms of supercapacitors, batteries, and energy storage devices. Some non-limiting examples of batteries and supercapacitors are referenced throughout this specification and are incorporated herein by reference.

[0164] FIG. 7 shows a container 15, which is the outer housing of this embodiment of the supercapacitor of the present system and method. This shows the "lead insulation holder 175" with its own perforations 85 as well as the inner section 99 and perforations 85 for fasteners.

[0165] Although the particular housing 15 is shown as having a cubic shape by way of example, it is possible to employ different geometric configurations, such as the circular configurations used in common commercial supercapacitors, and still utilize the benefits of the present systems and methods.

[0166] The container 15 may also be equipped with different locking mechanisms (not shown) to allow an operator access to the contents inside the supercapacitor, and may consist of various circular locks such as twist-off lids, locking handles, and various types of sealing engagements, using the housing 15 as some non-limiting examples. Some housings 15 include "inlets" and "outlets" (not shown) to allow maintenance of the electrolyte (not shown) and various other components while the contents inside the supercapacitor remain contained within the casing 15. Additionally, some embodiments allow the contents inside the supercapacitor to be removed for servicing.

[0167] The serviceable supercapacitor container 15 may include interlocking features that may include, but are not limited to, flanges, guides, ribs, sliders, grooves, and other variations thereof, some of which are not shown. Here, the components inside the supercapacitor can function as a cartridge within the housing 15 for removal, maintenance and reinstallation. It may be advantageous to use an internal encapsulation mechanism such as a plastic bag or vacuum bag (not shown), an example being a polycarbonate bag to seal the supercapacitor material. This can be achieved by placing the supercapacitor material in a bag, then evacuating the air and applying a vacuum, and then storing the sealed bag in container 15. This operation allows the internal components of the supercapacitor to be removed without actually creating a vacuum within the serviceable container unit 15 . This also allows the outer container 15 to be constructed from a variety of materials, providing flexibility in construction, for example having thin side walls with a reinforced base, and allowing the use of inexpensive materials such as steel, molded plastic, composites, etc.

[0168] In one embodiment, the shape of the serviceable container 15 is a parallelogram having a first set of opposing parallel straight sides and a second set of opposing parallel straight sides, with the illustrated square being particularly preferred. As previously mentioned, a variety of shapes and variations can be used.

[0169] FIG. 8 is a diagram illustrating the "cover 25" of the external housing (FIG. 7) of this embodiment of the supercapacitor of the systems and methods disclosed herein, showing perforations 85 for fasteners (see FIG. 9). Although perforations 85 are used in this example, the removable cover 25 may also be attached to the container by, for example, a hinge, locking mechanism, or arms (not shown). The removable cover 25 may be a suitably shaped groove or channel to slide into place. The removable cover 25 may also be circular with grooves / channels to function as a screw-on lid. The removable cover 25 may be pressed into place with a seal and recessed so that it can be held in place using a pin or insert. There are many variations that do not depart from the scope and intent of the present system and method that allow the container to have a detachable or removable cover 25 that allows access to the contents inside the capacitor for maintenance.

[0170] FIG. 9 illustrates a "fastener 35" for the outer housing of a supercapacitor embodiment of the present systems and methods, including a bolt 185 and a nut 195. In this example, bolts 185 and nuts 195 are employed as examples of mechanisms for constructing a resealable container, however, many different types of mechanisms can be used, including locking arms, screw tops, permanent or non-permanent welds, stackable cartridges, interlocking frames, grooves or channels, crimps, clamps, press seals, riveting, and vacuum seals, to name a few non-limiting examples.

[0171] FIG. 10 shows an external housing seal 65 or "gasket 65" having perforations 85 for a supercapacitor embodiment of the present systems and methods. A variety of different types of seals can be utilized for engagement between the container housing and the removable cover, and although a radial seal 65 is shown in the described invention, an axial seal (not shown) may also be used. There are many different configurations that seals can take and be used in, including stepped configurations, compressible seals, square or rounded corners, rigid seals and injectable seals. The seal is intended to provide an airtight seal 65 for the container, ensuring stable operation and a long expected life of the liquid electrolyte (not shown). An inwardly facing radial seal 65 may also be used, which may be a permanent, replaceable seal 65 that can be replaced during maintenance. An example of a permanent seal is a "weld seal" where the container is physically welded to itself as a single unit. It may also be a material that acts as a permanent weld, such as an injectable sealant, as some non-limiting examples.

[0172] Many types of seal configurations and variations thereof may be utilized with assemblies according to the present disclosure.

[0173] FIG. 11 illustrates an example embodiment of a cylindrical double layer electrolytic capacitor section as a device having a "wound inner layer with perforations 85" and a "separator 75" of the system and method disclosed herein. The double layer electrolytic capacitor section includes a cylindrical container 15, a lead insulating holder 175, an optional "plurality of leads 115" including multiple output leads and electrical connections on the opposite or perpendicular surfaces, perforations 85, and an electrical connector 215. FIG. 11 demonstrates the improvements added to make it maintainable, including a “co-solvent in salt electrolyte 205” and a high surface area, low cost composite material 55. In this particular case, the cylindrical container 15 is a complete unit, for example permanently welded or fixed. In this particular embodiment, maintenance requires that the contents inside the double layer electrolytic capacitor 125 be disconnected and possibly extracted. Many different embodiments may be employed such as screw tops, removable lids, other forms of press seals, crimp lock lids, and built-in features to allow for maintenance, some of which are not shown. Although reference is made to an upper capacitor 135 for charging, possible alternative embodiments are further referenced and described herein and implemented with reference to the "Storage devices" section, and further possible alternative embodiments are further referenced and described herein and implemented with reference to the "Applications" section as well as the "Implementations" section.

[0174] FIG. 12 shows an example of a cylindrical double-layer electrolytic capacitor 125, which is a device having a "perforated and wound inner layer 85" and a "separator 75" according to the present system and method. This includes the cylindrical container 15, the lead insulating holder 175, and the optional plurality of leads 115, including the plurality of output leads and the electrical connections on the opposite or perpendicular side. FIG. 12 shows that the additional refinements are useful. In this particular example, the cylindrical housing 15 is a permanently welded or fixed complete unit. In this particular example, maintenance requires disconnecting and possibly extracting the contents inside the double layer electrolytic capacitor 125. Many different embodiments may be employed such as screw tops, removable covers, other forms of press seals, crimp lock lids, and built-in features to allow for maintenance, some of which are not shown. Although reference is made to a supercapacitor 135 for charging, possible alternative embodiments are further referenced and described herein and implemented with reference to the "Storage devices" section, and further possible alternative embodiments are further referenced and described herein and implemented with reference to the "Applications" section as well as the "Implementations" section.

[0175] FIG. 13 illustrates an embodiment of a cylindrical double layer electrolytic capacitor 125 having a partitioned interior section 95 of the present system and method. It comprises a conductor 45 with separation 95, a container 15 and a container cover 25. It should be noted that this is a wound capacitor, including the lead insulating holder 175, the leads 115, and the top of the supercapacitor 135, although general arrangements including multiple leads 115 arranged on opposing or perpendicular surfaces are also possible. FIG. 13 demonstrates a wound-up supercapacitor 125 that has been modified to use maintainable, widely available, low-cost materials for its construction. In this particular example, the cylindrical container housing 15 is a permanently welded or fastened complete unit. In this particular example, maintenance requires disconnecting and possibly extracting the contents inside the double layer electrolytic capacitor 125. Many different embodiments may be employed such as screw tops, removable lids, other forms of press seals, crimp lock lids, and built-in features to allow for maintenance, some of which are not shown. Although reference is made to a supercapacitor 135 for charging, possible alternative embodiments are further referenced and described herein and implemented with reference to the "Storage devices" section, and further possible alternative embodiments are further referenced and described herein and implemented with reference to the "Applications" section as well as the "Implementations" section.

[0176] FIG. 14 illustrates an embodiment of a layered, cubic-shaped supercapacitor 135 having separate "sections 95" within the supercapacitor of the present system and method. This particular configuration includes a container 15, lead insulating holder 175, and leads 115, with the interior of the supercapacitor separated by "separations 95." FIG. 14 shows a cube-shaped supercapacitor with lead insulating holder 175 and lead wires 115, but the supercapacitor may have a more conventional arrangement with leads on the opposite or vertical surfaces. Figure 14 is intended to demonstrate that, with additional improvements, supercapacitors are practical and can be constructed using widely available, low-cost materials, and the electrolyte is a "salt co-solvent," improving safety compared to organic electrolytes, which tend to be highly reactive and toxic. In this particular example, the cube-shaped container 15 is a permanently welded or fastened complete unit. In this particular example, maintenance requires disconnecting and possibly extracting the contents inside the double layer electrolytic capacitor 125. Many different embodiments may be employed such as screw tops, removable lids, other forms of press seals, crimp lock lids, and built-in features to allow for maintenance, some of which are not shown.

[0177] Although reference is made to supercapacitors for charging, possible alternative embodiments are further referenced and described herein and realized with reference to the "Storage devices" section, and further possible alternative embodiments are further referenced and described herein and realized with reference to the "Applications" section as well as the "Implementations" section.

[0178] Applications The present systems are described with reference to examples, and in some embodiments, the methods contained herein can utilize various types of capacitors and supercapacitors, which are referenced in the following non-limiting examples of the present invention. This includes but is not limited to: energy generation, storage and conditioning methods and systems; energy recovery methods and systems involving a supply current such as alternating current or direct current; photovoltaic, solar, wind, wind turbine, wave and tidal energy generators; piezoelectric, thermoelectric, environmental, RF, fuel cell, electrochemical; existing inductive sources such as wind turbines, hydroelectric, geothermal, charcoal, natural gas, nuclear, wave / tidal energy and liquid gases such as oxygen; pressure-based systems; regenerative breaks; regenerative turbines; recovery systems such as momentum-based energy recovery, pressure-based energy recovery, temperature-based energy recovery, kinetic-based energy recovery, contraction and expansion-based energy recovery, discharge recovery and build-up energy recovery; electrostatic charge storage, inductive storage, capacitive storage and potential difference, non-limiting examples are electromagnets and electro-magnetic diffusion. The most notable application areas are energy storage systems, regenerative braking and recovery systems, solar and wind power generation, and energy generation and distribution systems.

[0179] Applications and systems for using this technology, which extend the useful operation of devices through the use of maintainable, low-cost electrical accumulators or electrostatic storage devices, are referred to as embodiments of the present invention. Non-limiting examples include the following: Transportation, including vehicles, transport equipment, air transport equipment, sea transport equipment, speed transport equipment, airplane turbines, trains, skytrains, bullet trains, linear motor cars, machinery, equipment, elevators, escalators, cranes, bridges, ramps, factories, equipment, machinery, agricultural equipment, machinery, lifting equipment, museums, park vehicles and equipment, flying vehicles, flying cars, helicopters, quadcopters, drones, electric bicycles, motorcycles, tricycles, semi-trucks, passenger transport, commercial vehicles. Harvesting systems could benefit high-power consuming devices such as lasers, particle accelerators, and devices that generate and manage electromagnetic and magnetic fields. Additionally, power generation facilities, generators, and power utilization may benefit from incorporating configurations of the present systems and methods, which may be of great benefit to many practical implementations. Selected embodiments of the present systems and methods may be scaled up for large-scale industrial applications, used in conjunction with baseload power sources, energy storage, and energy backup systems, which may benefit significantly from the present systems.

[0180] Implementations The device applications and potential uses may be non-limiting examples for embodiments of energy storage devices ranging from nano-sized to commercial industrial sizes. Some notable examples are energy storage systems, transportation, regeneration and recovery systems in cars, trucks, planes, ships, trains, airships, automobiles and machinery. Generation and storage, production, transmission, and other embodiments may include, but are not limited to, existing generation and storage systems. These include solar power, piezoelectric power, thermoelectric power, energy harvesting, RF power, fuel cell power, electrochemical power, wind turbines, hydroelectric power, geothermal power, coal, natural gas, nuclear power, and wave / tidal energy.

[0181] Storage devices Because the claimed systems and methods take advantage of the natural physical properties and operation of capacitors (electrostatic storage devices) and other electrical components, a wide range of possible alternatives can be used to achieve the novelty and usefulness of the claimed systems and methods. Non-limiting examples of the present invention include the following. Storage batteries, electrostatic storage batteries and storage devices, batteries and electrochemical storage devices (including hybrids), magnetic field storage devices such as inductors, and coils, and electrostatic storage devices may be substituted for or used in conjunction with the present invention and are claimed herein.

[0182] Such devices can be used in a number of different storage devices in the systems and methods referred to herein as embodiments of the present invention. The accumulator may include a variety of storage device configurations and may include circuits that operate with polarized capacitors, non-polarized capacitors, devices, and may include accumulator balancing and balancing ICs (integrated circuits). Non-limiting examples include single bulk storage devices such as capacitors and ultracapacitors, multi-cell configurations, multi-cell configurations, multi-storage devices and multiple multi-storage devices, perforated storage devices, single layer, multi-layer devices, and magnetic field storage devices. Also, ceramic, paraelectric, ferroelectric, mixed oxide, class 1, class 2, multilayer, decoupling, suppression, high voltage power supply, power thin film, thin film, nanostructured crystalline thin film, composite ink / paste, cross-linked gel electrolyte, electrolyte, metallized, plastic, polypropylene, polyester, polyphenylene sulfide, polyethylene naphthalate, polytetrafluoroethylene, RFI, EMI, snubber, motor run, AC capacitor, electrolytic, aluminum, tantalum, niobium, non-solid, solid manganese oxide, solid conductive polymer, bipolar, axial, SMD, chip Radial, hybrid capacitor, supercapacitor, double layer, pseudocapacitor, hybrid capacitor, electrochemical capacitor, ultracapacitor, electric double layer capacitor, APowerCAP®, BestCap®, BoostCap®, Cap-XX®, DLC·AP®, EneCapTen®, EVerCAP®, DynaCap®, Faradcap®, GreenCap®, GoldCap®, HYCAP®, Kapton capacitor, Skelcap Capacitors and ceramic capacitors include, but are not limited to, Super capacitors, SuperCaps, PAS capacitors, PowerStors, pseudocaps, ultracapacitors, double layer lithium ion, class X, class Y, carbon capacitors, graphene capacitors, graphite capacitors, integrated capacitors, nanoscale capacitors, glass capacitors, vacuum capacitors, SF6 gas filled capacitors, printed circuit board capacitors, conductive line capacitors, mica capacitors, air gap capacitors, variable capacitors, tunable capacitors, trimmer capacitors, superdielectric capacitors, and high energy density capacitors.

[0183] "Pyrolysis" and "pyrolyze" generally refer to the thermal decomposition of carbon materials. In pyrolysis, less oxygen is present than is required for complete combustion of the material, such as less than about 30%, less than about 20%, less than about 10%, less than about 5%, less than about 1%, less than about 0.5%, less than about 0.1%, or less than about 0.01%. In additional embodiments, the pyrolysis can be carried out in the absence of oxygen.

[0184] Physical changes that may occur during pyrolysis may include any of the following: (i) Heat transfer from the heat source and the temperature rise of the feed material. (ii) Pyrolysis reactions at high temperatures release volatile materials and form charcoal. (iii) Heat flow from the volatile material to the cold solid feedstock results in heat transfer between the hot volatile material and the cold unpyrolyzed or partially pyrolyzed feedstock. (iv) Condensation of volatile materials in the colder parts of the feedstock, which can lead to secondary reactions that produce tar. (v) An autocatalytic secondary pyrolysis reaction may occur during or simultaneously with the primary pyrolysis reaction. (vi) Additionally, thermal decomposition, reformation, water-gas shift reactions, free volatile recombination, and dehydration may occur, some of which are a function of residence time, temperature, and pressure, and some of which may be affected by residence time, temperature, and pressure.

[0185] The "pyrolysis" is carried out at least in part to "dehydrate the feedstock." In additional embodiments, pyrolysis removes greater than about 50%, greater than about 75%, greater than about 90%, greater than about 95%, or greater than about 99% of the water from the feedstock.

[0186] The beneficial aspects of the present system and method can be used in many different applications. An example of this is the use of the "ion-pore matching hierarchical structure" and systems and methods disclosed herein as a method for producing improved activated carbon for the removal and reduction of contaminants contained in and emitted from gases, liquids, electronic missions, water bodies, effluents, and emissions, as well as many other sources.

[0187] FIG. 15 illustrates an embodiment of the present invention, including: A continuous "carbon source material supply system 110" of carbon source 100 consisting of a multi-zone configuration of a single "pyrolysis reactor / zone 220" to produce carbonized activated carbon material of a predetermined pore structure, and an "energy storage device stacking system 500." The device configuration in this embodiment includes a mechanically coupled or operatively associated "energy storage device stack system 500," and also includes an "electrode preparation system / zone 400" operatively associated with the system 500 for producing carbonized activated carbon of the predetermined pore structure described above. The carbon source processing system may include various features, embodiments, and controllable parameters as described throughout this disclosure.

[0188] Some of the functionality described herein includes systems, processes, and devices, including: Treatment of various carbon sources100. Some exemplary features of the system may include: The process involves determining the desired pore width and hierarchical structure of the final activated carbon in order to control the device to produce the desired result product. A grinding section (not shown) for grinding the carbon source 100 into a fine powder. A "carbon source material supply system 110" for the carbon source 100, comprising a material supply unit or hopper 130 for containing the carbon source, and an auger 121 or alternative supply mechanism or means. A soaking / mixing zone 190 for the carbon source 100, including an inlet 156, an outlet 157, a gas inlet 150a, a gas outlet 151a, and a soaking container or equivalent. Optional inert atmosphere. A thermally controlled "drying and preheating zone 200a" including "gas inlets 150b and 150c" and "gas outlets 151b and 151c." A "pyrolysis reactor / zone 220" and a "gas phase separation section / zone 250" for pyrolyzing the carbon source 100, including an "inlet 158" and an "outlet 159." A "cooling and washing zone / section 240" including "inlets 152a-152b" for liquid and vapor phase cooling and "outlets 153a-153b" for liquid / vapor / heat recovery systems for washing the pyrolytic carbon and introducing additives. "Drying zone 200b" for "drying pyrolytic activated carbon having a predetermined pore structure." One or more "electrode mixing systems / zones 401" can be positioned throughout the device to mix "pyrolyzed activated carbon of predetermined pore structure" with "additional energy storage electrode material" or "mixture 107." The "electrode mixing system / zone 401" includes one or more "inlets 402a and 402b," and further has an "electrode mixture balancer" and "outlets 402c and 402d." "Outlets 402c-402d" can be used to balance the internal pressure or to remove samples of mixtures such as supercapacitor materials. Additionally, the device includes an "activated carbon material supply system 120." The Activated Carbon Material Supply System 120 transports activated carbon and electrode mixture throughout the device and into the Electrode Mix Storage Hopper 404 . The "electrode mixture storage hopper 404" includes an "electrode mixture system device 405" and an "electrode mixture supply system 406." An "electrode mix delivery system 406" delivers the electrode mix to the device 400 for fabricating and laminating energy storage devices. The energy storage device fabrication and stacking device 400 may include numerous components necessary for its operation, and for ease of understanding, only the necessary functional components are shown, with all other additional functional components and operating systems being incorporated herein by reference, although omitted. The energy storage device manufacturing device may include an electrode mixture injector 407, an electrode applicator 408, an electrode mixture overflow recirculation system 409, a device winding and stacking system 411, rollers 412a and 412b, tensioners 413a and 413b, and drive mechanism(s) and motor(s) 414. Additionally, the energy storage device manufacturing device may include a connecting belt gear direct connect drive mechanism 415. The energy storage device manufacturing system may further include an electrode drying system / zone 420, an electrolyte injector 433, an electrolyte mixing system 431 and storage tank, and an electrolyte system / zone containing the electrolyte. The energy storage device manufacturing device system may further include a conduit 432 and an "attachment and sealing system / zone 450," which may also include a "welding and sealing device 451," as described below. The "welding and sealing device 451" uses a welder, sealer, crimper, press, and seal to produce, for example, a "finished energy storage device 460." The Energy Storage Device Stacking System 500 is used, for example, to fabricate supercapacitors and batteries.

[0189] In this embodiment, the closed "carbon source material supply system 110" includes a "material supply hopper 130," a "material transfer mechanical system 110," and deoxygenation (purge) manifolds and mechanical systems 150a, 150b, 150c, 151a, 151b, and 151c.

[0190] In this embodiment, the “material supply hopper 130 ” may be any suitable open or closed atmosphere container configured to contain the carbon source material 100 . In certain embodiments, the "screw or auger 121" is operatively rotated by a drive source, such as, but not limited to, a motor or other mechanically operable device (not shown). In an additional embodiment, the carbon source material 100 is fed into a "carbon source material feeding system 110" implemented by a gravity feed system. In certain embodiments, the Carbon-Source Material Supply System 110 can be configured such that the screw or auger 121 is enclosed in a suitable container. In additional embodiments, the containers described may be generally cylindrical in shape. In additional embodiments, the "carbon source material supply system 110" can include screws, augers, conveyors, drums, screens, chutes, drop chambers, and pneumatic conveying devices, and the "carbon source material supply system 110" can include rotary airlocks and double or triple flap airlocks (not shown).

[0191] In certain embodiments, the carbon source material 100 is fed into the "carbon source material feed system 110" from a carbon source material feed hopper 130, and the rotation of an auger or screw moves the raw carbon source material 100 toward the deoxygenation manifold. When the carbon source material 100 reaches the deoxygenation manifold, the air surrounding the raw carbon source material 100 in the Carbon Source Material Supply System 110 contains approximately 21% oxygen. In additional embodiments, the deoxygenation manifold may be located adjacent to or around the Carbon Source Material Supply System 110. In certain embodiments, the oxygen-enclosing manifold or container of the Carbon-Source Material Supply System 110 may include multiple gas inlet ports 151a, 151b, 151c and multiple gas outlet ports 150a, 150b, 150c.

[0192] In certain embodiments, the deoxygenation manifold may have at least one gas inlet line 123a and at least one gas outlet line 122a. In an additional embodiment, at least one gas inlet line 123a of the deoxygenation manifold is in operative communication and mechanically connected with each of the plurality of gas inlet ports 151a, 151b, and 151c. In an additional embodiment, at least one gas outlet line 122a of the deoxygenation manifold is in operative communication and mechanically connected with each of the plurality of gas outlet ports 150a, 150b, and 150c. In certain embodiments, the gas inlet line 123a can be configured to pump the inert gas 123 to the gas inlet ports 151a, 151b, and 151c. In certain embodiments, the inert gas 123 is nitrogen, argon, or helium, and is substantially oxygen-free. In an additional embodiment, the inert gas 123 is introduced counter-currently to the carbon source material.

[0193] In certain embodiments, the introduction of an inert gas 123 into the sealed Carbon Source Material Supply System 110 may be done to force ambient air 122 out of the sealed system. In certain embodiments, during operation, an inert gas 123 is introduced into the first gas inlet port 151a, causing oxygen-enriched ambient air 122 to be forced out of the outlet port 150a. At this point, the desired level of oxygen may not be achieved, such as less than about 2% oxygen, less than about 1% oxygen, less than about 0.5% oxygen, less than about 0.2%, less than about 0.1% oxygen, or the like. In additional embodiments, additional inert gas 123 must be injected to "exclude the necessary or desired amount of oxygen 122" from the air surrounding the carbon source material 100 in the closed system. In additional embodiments, the second gas inlet port 151b can cooperate with the injection at the first gas inlet port 151a to pump inert gas 123 into the containment system, thereby partially or substantially eliminating the remaining oxygen 122. After injecting the inert gas 123 once, twice or multiple times to remove the oxygen 122 from the sealed system, the desired result of "reducing the oxygen content" can be achieved. In an additional embodiment, if the desired oxygen level is not achieved after the second injection of inert gas 123, inert gas 123 can be used during a third injection 151, and any remaining unwanted oxygen 122 can be removed from the gas outlet 150c of the sealed system. Additional inlets and outlets may be incorporated as needed. In an additional embodiment, oxygen 122 levels are monitored throughout the Carbon Source Material Supply System 110 and the amount and location of inert gas 123 injection is calibrated to ensure desired performance, safety, and a predetermined pore structure of the carbonized activated carbon material 105 as a result of the process.

[0194] In certain embodiments, the gas inlet ports 151a, 151b, and 151c and the corresponding gas outlet ports 150a, 150b, and 150c, respectively, are slightly offset from one another relative to a perpendicular bisecting plane passing through the Carbon-Source Material Supply System 110. In certain embodiments, the inlet ports 151a, 151b, 151c and the corresponding outlet ports 150a, 150b, 150c can be offset by an amount corresponding to the pitch of the auger 121 in the Carbon Source Material Supply System 110. In an additional embodiment, after the atmosphere surrounding the raw carbon source material 100 has been deoxygenated 122 to a predetermined or sufficient level, the raw carbon source material 100 can be fed from the Carbon Source Material Feed System 110 to one or more Pyrolysis Reactors / Zones 220. In additional embodiments, oxygen levels can be monitored throughout the Carbon Source Material Supply System 110 to calibrate the amount and location of inert gas 123 injection to achieve a predetermined and desired oxygen level.

[0195] In additional embodiments, the device includes multiple gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, 402d and multiple gas extraction probes 156, 150a, 150b, 150c, 158, 152a, 152b, 154a, 154b, 402a, 402b positioned at various points throughout the device. In additional embodiments, any one of gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, and 402d and any one of gas extraction probes 156, 150a, 150b, 150c, 158, 152a, 152b, 154a, 154b, 402a, and 402b correspond to a different one of the multiple zones. In alternative embodiments, the device includes any suitable number of gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, 402d and any suitable number of gas extraction probes 156, 150a, 150b, 150c, 158, 152a, 152b, 154a, 154b, 402a, 402b. In certain embodiments, each of the multiple zones has one gas introduction probe 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, 402d and two or more gas extraction probes 156, 150a, 150b, 150c, 158, 152a, 152b, 154a, 154b, 402a, 402b.

[0196] In an alternative embodiment, the "drying zones 200a-200b" are associated with gas introduction probes 151b-151c and gas extraction probes 150b-150c. In additional embodiments, gas introduction probes 151b and 151c introduce nitrogen, argon, or helium 123 into the "drying zones 200a and 200b," and gas extraction probes 150b and 150c extract gas 122 from the "drying zones 200a and 200b." In certain embodiments, the gas introduction probes 151b and 151c may be configured to introduce the gas mixture 123 into the "drying zones 200a and 200b." In an additional embodiment, the extracted gas 122 may be oxygen. In an alternative embodiment, the gas extraction probes 150b-150c extract gas 122 from the "drying zones 200a-200b" and reuse the extracted gas in a heat or energy recovery system.

[0197] In certain embodiments, the "preheat zone 210" can associate gas introduction probes 151b and 151c and gas extraction probes 150b and 150c. In additional embodiments, gas introduction probes 151b and 151c introduce nitrogen, argon, or helium 123 into the preheating zone 210, and gas extraction probes 150b and 150c extract gas 122 from the drying and preheating zone 200a. In additional embodiments, gas introduction probes 151b-151c may introduce a mixture of gases 123 into the "preheat zone 210." In additional embodiments, the gas 122 extracted from the gas extraction probes 150b-150c may include carbon-rich off-gas. In additional embodiments, gases extracted from the Preheat Zone 210 or Pyrolysis Reactor / Zone 220 may be treated and then reintroduced into, for example, a carbon recovery unit or the material in the Pyrolysis Reactor / Zone 220. In additional embodiments, gases 122 extracted from multiple zones of the device can be used for energy recovery in drying, processing, and gas heaters, or even pyrolysis in trimming reactors and carbon enrichment units.

[0198] In certain embodiments, the Pyrolysis Reactor / Zone 220 can be associated with a Gas Introduction Probe 159 and a Gas Extraction Probe 158 . In additional embodiments, a gas introduction probe 159 introduces nitrogen, argon, or helium 123 into the Pyrolysis Reactor / Zone 220. Additionally, a gas extraction probe 158 extracts gases from the Pyrolysis Reactor / Zone 220 . In an additional embodiment, the gas introduction probe 159 is configured to introduce a mixture of gases 123 into the Pyrolysis Reactor / Zone 220 . In additional embodiments, the gas 122 extracted from the gas extraction probe 158 may include carbon-rich off-gas, syngas, or city gas. In certain embodiments, the carbon-rich gas 122 extracted from the Pyrolysis Reactor / Zone 220 can be used and reintroduced into the material at a later stage in the process. In an additional embodiment, the gases 122 extracted from the Preheat Zone 210 and the gases 122 extracted from the Pyrolysis Reactor / Zone 220 can be combined at any point in the process before being reintroduced into the material.

[0199] In another embodiment, the cooling and scrubbing zone / section 240 can be associated with gas introduction probes 152a and 152b and gas extraction probes 153a and 153b. In additional embodiments, the gas introduction probes 152a and 152b introduce nitrogen, argon, or helium 123 into the cooling and rinsing zone / section 240. Additionally, gas extraction probes 153a and 153b can extract gas from the "cooling and washing zone / section 240." In various embodiments, gas introduction probes 152a-152b can introduce a mixture of gases 123 into the "cooling and scrubbing zone / section 240." In various embodiments, the gas extraction probes 153a-153b extract the gas 122 from the "cooling and scrubbing zone / section 240" so that it can be reused in a heat or energy recovery system.

[0200] In certain embodiments, the gas introduction probes 152a-152b and gas extraction probes 153a-153b may operate in conjunction with a controller and multiple sensors to regulate the level and concentration of gas 123 introduced and extracted from each device zone.

[0201] In certain embodiments, the gas inlet probes 152a-152b and the gas outlet probes 153a-153b are made of suitable piping and are constructed to withstand high temperature fluctuations. In certain embodiments, the gas introduction probes 152a-152b and the gas extraction probes 153a-153b may include a plurality of openings through which the gases 123 and 122 to be introduced and extracted may pass. In certain embodiments, multiple openings may be located beneath the inlet and gas extraction probes 152a-152b. In additional embodiments, each of the plurality of openings extends over a length within an individual zone or within multiple zones.

[0202] In additional embodiments, gas introduction probes 152a-b can extend from one side of the device through each zone or multiple zones. In certain such embodiments, each of the gas introduction probes 152a-152b can extend from one side of the device to a respective zone of the device. In an additional embodiment, a gas catalyst can be added to increase the fixed carbon level. In certain such embodiments, the multiple openings for each gas introduction probe 152a-152b may be located only in each zone associated with that particular gas introduction probe 152a-152b.

[0203] In certain embodiments, each of the gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, and 402d can extend into a respective zone from the left side of the base soak and mix zone 190. In this example, gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, and 402d extend through the device or "electrode mixing system / zone 401." Additionally, the introduction probes described above can be configured to terminate in zones such as the base "soaking and mixing zone 190," "drying zone 200a," "preheating zone 210," "pyrolysis reactor / zone 220," "cooling and washing zone / section 240," "drying zone 200b," "electrode mixing system / zone 401," a specific zone, all zones, or selected zones.

[0204] In certain embodiments, the gas introduction probes may all extend through the Preheat Zone 210, with the Preheat Zone Gas Introduction Probes terminating in the Drying and Preheat Zone 200a. In certain such embodiments, the remaining gas introduction probes may extend through the "pyrolysis reactor / zone 220." The "pyrolysis reactor / zone 220" has a pyrolysis zone gas introduction probe that can terminate within the pyrolysis reactor / zone 220. In additional embodiments, the gas extraction probe can be configured similarly to the gas introduction probe. In additional embodiments, the gas introduction probe and the gas extraction probe can originate from either side of the device.

[0205] In certain embodiments, the gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, and 402d may be arranged concentrically with one another to reduce space. This can be used in a multi-port configuration. In the above embodiment, each of the inlet probes or ports 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, and 402d may have a smaller diameter than the preceding inlet probe or port. For example, in the above embodiment, gas introduction probes 159·151a in base soaking / mixing zone 190 may have the largest inner diameter. The gas introduction probes 151b and 151c of the "Preheat Zone 210" and "Drying Zone 200a" are positioned within the inner diameter of the gas introduction probes 159 and 151a of the base "Soaking and Mixing Zone 190", and the gas introduction probe 159 of the "Pyrolysis Reactor / Zone 220" is positioned within the inner diameter of the precoat. The gas introduction probes 151b and 151c of the "preheating zone 210", "drying zone 200a", and the gas introduction probes 153a and 153b of the "cooling and washing zone / section 240" are arranged within the gas introduction probe 159 of the "pyrolysis reactor / zone 220". Therefore, the gas introduction probes 155a and 155b of the "drying zone 200b" are disposed within the gas introduction probes 153a and 153b of the "cooling and cleaning zone / section 240", and therefore the gas introduction probes 402c and 402d of the "electrode mixing system / zone 401" are disposed within the gas introduction probes 155a and 155b of the "drying zone 200a". In the above embodiment, suitable connectors can be attached to each of the gas introduction probes 159, 151a, 151b, 151c, 159, 153a, 153b, 155a, 155b, 402c, and 402d on the outside of the device. This is to control the air injected into each gas introduction probe individually or in concert.

[0206] In the particular embodiment described, a concentric or near-concentric arrangement may be preferred, with the outermost "gas introduction probes" only exposed before being terminated in each zone. Thus, in the above embodiment, the individual introductions into the gas zones can be controlled independently of each other, and only a single continuous gas introduction probe line is required. For such an embodiment, the gas extraction probes 156, 150a, 150b, 150c, 158, 152a, 152b, 154a, 154b, 156, 150a, 150b, 150c, 158, 152a, 152b, 154a, 154b, 402a, 402b may also have a concentric or nearly concentric configuration similar to that of the gas introduction probe.

[0207] In certain embodiments, the device may include a "single pyrolysis reactor 220" having two or more separate zones. Although multiple zones are shown in certain embodiments, any number of zones may be used in other embodiments. In additional embodiments, each zone can be connected to at least one other zone via a carbon source material transport unit 110 . In an additional embodiment, the carbon source material delivery unit 110 can control the atmosphere and temperature conditions.

[0208] In this example, the carbon source material 100, such as coal or petroleum coke, is optionally dried, ground and sized by passing it through a mesh or the like outside of the Pyrolysis Reactor / Zone 220. The carbon source material 100 is then introduced into the “soaking and mixing zone 190 ” with an oxygen-containing atmosphere (optional) created prior to introduction into the carbon source hopper 130 . Such operation can optionally be achieved using a Carbon Source Material Supply System 110. The Carbon Source Material Supply System 110 can be controlled to reduce the oxygen 122 level in the ambient air of the device to about 3%, about 2%, about 1%, about 0.1% or less. As the level of oxygen 122 within the device decreases, raw carbon material 100 enters the "soak and mix zone 190" via the sealed "carbon source material supply system 110." In one such embodiment, the Carbon Source Material Supply System 110 may include a sealed jacket or sleeve. Steam or off-gas from the Pyrolysis Reactor 220 is used to directly heat the carbon source material 100 through a sealed jacket or sleeve. The steam or off-gas from the "pyrolysis reactor 220" is then used to preheat and pyrolyze the carbon source material 100 by a process gas heater or heat exchanger (not shown).

[0209] Subsequently, in this example, a water-containing "additive," such as the non-limiting example of KOH, is thoroughly and evenly distributed throughout the carbon source material 100 prior to preheating or pyrolysis. The soak time in the soaking / mixing zone 190 is approximately 10 minutes, approximately 20 minutes, approximately 30 minutes, approximately 40 minutes, approximately 50 minutes, approximately 1 hour, approximately 1.5 hours, approximately 2 hours, approximately 3 hours, approximately 4 hours, approximately 5 hours, approximately 6 hours, approximately 7 hours, approximately 8 hours, approximately 9 hours, approximately 10 hours, approximately 11 hours, approximately 12 hours, approximately 13 hours, approximately 14 hours, approximately 15 hours, approximately 16 hours, approximately 17 hours, approximately 18 hours, approximately 19 hours, approximately 20 hours, approximately 21 hours, approximately 22 hours, approximately 23 hours, approximately 24 hours. Approximately 25 hours, approximately 26 hours, approximately 27 hours, approximately 28 hours, approximately 29 hours, approximately 30 hours, approximately 31 hours, approximately 32 hours, approximately 33 hours, approximately 34 hours, approximately 35 hours, approximately 36 hours, approximately 37 hours, approximately 38 hours, approximately 39 hours, approximately 40 hours, approximately 41 hours, approximately 42 hours, approximately 43 hours, approximately 44 hours, approximately 45 hours, approximately 46 hours, approximately 47 hours, approximately 48 hours, approximately 49 hours, approximately 50 hours, with around 12 hours being ideal.

[0210] Next, in this embodiment, the presoaked carbon source 100 enters the "drying and preheating zone 200a," where the temperature of the "carbon source 100" is increased from near ambient temperature to about 100°C, about 150°C, or about 200°C. In additional embodiments, the temperature remains below 200°C. In additional embodiments, the "drying and preheating zone 200a" may include a mechanism (not shown) for capturing and venting off-gases from the pre-soaked carbon source 100 while it is being heated. In an additional embodiment, the off-gas can optionally be extracted for later use. In additional embodiments, the heating sources used for the various mechanical systems are electric and gas. In additional embodiments, the heat source used for the various zones may be waste gas from other reactors in the device or from an external source. In additional embodiments, heat may be provided from an indirect source.

[0211] Subsequently, after preheating in the "Drying and Preheating Zone 200a", the "Carbon Source Material Supply System 110" transfers the preheated carbon source 100 to another "Pyrolysis Reactor / Zone 220" (optional). In additional embodiments, first zone 200a and "pyrolysis reactor / zone 220" are the same reactor. In additional embodiments where the first zone 200a is separate from the Pyrolysis Reactor / Zone 220, the Carbon Source Material Supply System 110 can penetrate the Pyrolysis Reactor / Zone 220 through a high temperature steam seal system, such as, by way of non-limiting example, an airlock (not shown). This allows the carbon source 100 to permeate the "pyrolysis reactor / zone 220" while preventing gas and heat loss and oxygen ingress. In additional embodiments, the temperature inside the "pyrolysis reactor / zone 220" is heated to about 100°C, about 200°C, about 300°C, about 400°C, about 500°C, about 600°C, about 700°C, about 800°C, about 900°C, about 1000°C, or about 1100°C, with "800°C for 2 hours" being preferred. In additional embodiments, the Pyrolysis Reactor / Zone 220 may include an Output Port 159 for capturing and discharging gases 122 released from the preheated carbon source material 100, for example, during pyrolysis. In an additional embodiment, the gas 122 is extracted and optionally stored for later use. In additional embodiments, the off-gas 122 from the Pyrolysis Reactor / Zone 220 and the off-gas 122 from multiple zones of the device can be combined into a single gas stream. Once carbonized, the carbon source material 100 becomes a pyrolyzed activated carbon having a predetermined pore structure 105, which in certain embodiments can be transported out of the pyrolysis reactor / zone 220 by an activated carbon material delivery system 120. The feeding system is similar to the "carbon source material feeding system 110" and can enter the "cooling and washing zone / section 240" (optional) for cooling and washing. At this stage, it is preferable to "wash the activated carbon with water and any additives," and a non-limiting example of a preferred "additive" is "HCl." In certain embodiments, the cleaning and cooling is accomplished for a specific, controlled amount of time, eg, a "soak time." For example, about 10 minutes, about 20 minutes, about 30 minutes, about 40 minutes, about 50 minutes, about 1 hour, about 1.5 hours, about 2 hours, about 3 hours, about 4 hours, about 5 hours, about 6 hours, about 7 hours, about 8 hours, about 9 hours, about 10 hours, about 11 hours, about 12 hours, about 13 hours, about 14 hours, about 15 hours, about 16 hours, about 17 hours, about 18 hours, about 19 hours, about 20 hours, about 21 hours, about 22 hours, about 23 hours, about 24 hours, about 25 hours The recommended time is approximately 26 hours, approximately 26 hours, 27 hours, approximately 28 hours, approximately 29 hours, approximately 30 hours, approximately 31 hours, approximately 32 hours, approximately 33 hours, approximately 34 hours, approximately 35 hours, approximately 36 hours, approximately 37 hours, approximately 38 hours, approximately 39 hours, approximately 40 hours, approximately 41 hours, approximately 42 hours, approximately 43 hours, approximately 44 hours, approximately 45 hours, approximately 46 hours, approximately 47 hours, approximately 48 hours, approximately 49 hours, and approximately 50 hours, with "approximately 8 hours of soaking" being preferred. In certain embodiments, the "cooling and washing zone / section 240" may be the same as the "pyrolysis reactor / zone 220" or may be a separate reactor or zone from the "pyrolysis reactor / zone 220."

[0212] In this example, when the pyrolytic activated carbon 105 of a predetermined pore hierarchical structure enters the "cooling and washing zone / section 240," the material is cooled (actively or passively) to a specific temperature. In an additional embodiment, the temperature of the activated carbon 105 of predetermined pore structure is cooled in an inert atmosphere "cooling and washing zone / section 240." In an additional embodiment, the "cooling and washing zone / section 240" water-cools the activated carbon material 105 of a predetermined pore structure. The "cooling and washing zone / section 240" may be a mechanical mechanism containing "additives such as HCl" that allow the material to be submerged for a specified and extended period of time. The activated carbon material 105 of a predetermined pore structure is cooled in the "cooling and washing zone / section 240" where it reaches a temperature at which it will not spontaneously ignite when exposed to normal atmospheric or oxygenated air. In additional embodiments, the "cooling and washing zone / section 240" reduces the temperature of the activated carbon material to below 200°C or about 150°C to about 100°C. In this embodiment, the device may also include an optional mixing system for mixing the activated carbon material 105 with a coolant and an additive, which allows for uniform cooling of the carbon material. Additionally, cooling can be accomplished by direct or indirect means and can involve the use of water, other liquids, or additives. Additionally, the cooling process can be carried out by direct or indirect means with air or other gases, or a combination of both.

[0213] In certain embodiments, the cooling mechanism may be separate from the Pyrolysis Reactor / Zone 220 and mechanically connected to the Activated Carbon Material Supply System 120 . In an additional embodiment, the cooling mechanism is located after the Pyrolysis Reactor / Zone 220. In additional embodiments, the cooling mechanism may be the same as the Pyrolysis Reactor / Zone 220 or may be incorporated within the Pyrolysis Reactor / Zone 220. In additional embodiments, the cooling mechanism comprises, by way of non-limiting example, a screw, an auger 121, or a conveyor, illustratively a belt conveyor. In certain embodiments, the cooling mechanism may be a drum, a screen pan, a countercurrent bed, a vertical tower, a jacketed paddle, a cooling screw, or a combination thereof. The cooling mechanism may be direct or indirect cooling means, may utilize water or other liquids or additives, may utilize gases directly or indirectly, or any combination of the above. In additional embodiments, the cooler may include a water spray mechanism, inlet ports 152a and 152b (with and without additives), a "chilled inert gas flow mechanism," and outlet ports 153a and 153b, which may be "liquid nitrogen" or, if below ignition or flammable temperatures, "ambient air." In additional embodiments, heat can be recovered during this cooling process, in one example by capturing flash steam produced by the water spray or superheated steam produced when saturated steam is introduced, mixing them together, and then heating them with activated carbon material 105.

[0214] In this example, a "raw carbon source material 100," such as coal, petroleum coke, oil, or biomass, is introduced into a "pyrolysis reactor / zone 220" with a low oxygen content atmosphere. This operation can optionally be accomplished using the Carbon Source Material Supply System 110 described above. By using the "carbon source material supply system 110," the oxygen level in the ambient air within the system can be reduced to about 3%, about 2%, about 1%, or about 0.1% or less, thereby making it suitable for a "combustion-free pyrolysis process." Raw carbon source material 100 can be introduced into the device in a sealed "carbon source material supply system 110", optionally after oxygen levels have been reduced. In additional embodiments, the "carbon source material supply system 110" may include an encapsulated jacket(s) or sleeve(s) through which steam or off-gas from the reactor is transported and used to preheat the carbon source material 100.

[0215] In additional embodiments, the Raw Carbon Source Material 100 can first travel from the Carbon Source Material Supply System 110 through an optional Drying and Preheating Zone 200a or Preheating Zone 210 / preheating area of ​​the device. In an additional embodiment, the raw material can be heated in an optional "Drying and Preheating Zone 200a" to remove water and other moisture, combustible gases, and tars, which can be done as a separate zone before passing through the "Preheating Zone 210." In additional embodiments, the interior of the optional "drying and preheating zone 200a" may be heated to a temperature from about ambient temperature to about 100°C, about 150°C, or even to about 200°C. Water or moisture removed from the raw carbon source material 100 can exit any "drying and preheating zone 200a" or area, for example, through exit ports 150b-150c. In additional embodiments, the optional "drying and preheating zone 200a" can be adapted to extract steam and moisture (122). In an additional embodiment, the water droplets, steam, and moisture from the optional "drying and preheating zone 200a" can optionally be extracted for later use. The water droplets, steam, or vapor extracted from the optional Drying and Preheating Zone 200a can be used in a suitable waste heat recovery system and in combination with the Carbon Source Material Supply System 110. The steam and moisture 122 used in the Carbon Source Material Supply System 110 can be used to preheat the raw carbon source material 100 while oxygen levels are eliminated within the Carbon Source Material Supply System 110. In additional embodiments, the reactor does not include a drying zone 220, as the carbon source material 100 is dried outside of the "pyrolysis reactor / zone 220."

[0216] In additional embodiments, the dried carbon source material 100 re-enters the "preheat zone 210" where the temperature of the dried carbon source material 100 is increased from the ambient temperature range to a temperature range of about 100°C to about 150°C to about 200°C. In an additional embodiment, the temperature does not exceed 200° C. in the "preheat zone 210." If the preheat zone is too hot or not hot enough, the dry carbon source material 100 will be treated in a non-ideal manner before being introduced into the Pyrolysis Reactor / Zone 220. The "preheating zone 210" may include output mechanisms 150b-150c for capturing exhaust gases from the dry carbon source material 100 during preheating for reuse now or at a later date. In an additional embodiment, the off-gas can optionally be extracted for later use. In additional embodiments, the heating sources used in the various zones may be electric or gas. In additional embodiments, the heat source used in the various zones may be waste gas from other zones of the device or from an external source. In additional embodiments, the heat may be indirect.

[0217] After processing in the Preheat Zone 210, the Carbon Source Material Feed System 110 delivers the preheated material to the Pyrolysis Reactor / Zone 220 to undergo the pyrolysis process. In additional embodiments, the Carbon Source Material Supply System 110 can penetrate the Pyrolysis Reactor / Zone 220 through a high temperature steam seal system (not shown), including, but not limited to, an airlock (not shown). This allows the material delivery system to enter the high temperature Pyrolysis Reactor / Zone 220 while preventing or minimizing gas leakage and oxygen ingress. In additional embodiments, the interior of the "pyrolysis reactor / zone 220" is heated to a temperature of about 100°C, about 200°C, about 300°C, about 400°C, about 500°C, about 600°C, about 700°C, about 800°C, about 900°C, about 1000°C, or about 1100°C, with a ramp rate of 10°C per minute at 800°C being preferred. In an additional embodiment, the "pyrolysis reactor / zone 220" includes an outlet port 158 ​​and an inlet port 159 similar to the "preheating zone 210" to capture and vent gases released from the "pyrolysis reactor / zone 220" while the preheated carbon source material 100 is being carbonized. In an additional embodiment, the gas can optionally be extracted for later use at the operator's discretion. In an additional embodiment, the off-gas from the Preheat Zone 210 and the off-gas from the Pyrolysis Reactor / Zone 220 can be combined into a single gas stream. Once carbonized, the carbonized carbon source material 105 exits the pyrolysis reactor / zone 220 and then enters the cooling and washing zone / section 240.

[0218] In an additional embodiment, raw carbon source material 100 and dried, preheated, or carbonized activated carbon material having a predetermined pore structure 105 travel along a continuous "carbon source material feed system 110" or system through a "pyrolysis reactor / zone 220." In additional embodiments, the Carbon Source Material Supply System 110 can deliver various carbon source materials 100 at different points in the process. In an additional embodiment, the process of transporting material through the Pyrolysis Reactor / Zone 220 is a continuous process. In certain embodiments, the velocity of the Carbon Source Material Supply System 110 is suitably calibrated, calculated, and controlled by an associated controller or processor (not shown) to ensure uninterrupted operation of the Carbon Source Material Supply System 110 as material moves through the device or Pyrolysis Reactor / Zone 220. In certain embodiments, the operation of the Carbon Source Material Supply System 110 may be segmented and may include multiple separate augers (not shown) or additional carbon material supply mechanisms as described herein, and the Carbon Source Material Supply System 110 may be controlled by an associated controller or processor. By operating the individual carbon material supply mechanisms, the "carbon source material supply system 110" can control the transfer rate of the carbon source material 100 between zones, stages, or reactors depending on the optimal residence time of the carbon source material 100 within a particular zone, stage, or reactor of the device.

[0219] In additional embodiments, a controller (not shown) associated with the Pyrolysis Reactor / Zone 220 can be configured to adjust the rate of the Carbon Source Material Supply System 110 based on feedback sensors and detected gases from the FTIR (optional), measurement parameters, temperature gauges, the Pyrolysis Reactor / Zone 220, or other suitable variables in the reaction process. In additional embodiments, suitable moisture, temperature, and gas sensors in communication with the controller and processor can be incorporated into or mechanically connected to the pyrolysis reactor 220, or between the pyrolysis reactor 220 and the zones, or at any suitable location along the Carbon Source Material Supply System 110 or device. In additional embodiments, the controller processor can use information obtained from sensors and gauges to optimize the speed and efficiency of a device or processing system. In an additional embodiment, the controller associated with the Pyrolysis Reactor / Zone 220 is configured to operate the Carbon Source Material Supply System 110.

[0220] In additional embodiments, a controller associated with one or more of the Pyrolysis Reactors / Zones 220 can be configured to monitor gas concentrations, gas temperatures, and moisture within the Carbon Source Material Supply System 110 and / or within the Pyrolysis Reactors / Zones 220. In additional embodiments, the controller may be configured to adjust the speed of the Carbon Source Material Supply System 110, the input of gas 123 to the material supply unit 110, or the heat applied to the material 100 in the Carbon Source Material Supply System 110 based on one or more readings obtained from the various sensors.

[0221] In an additional embodiment, the device is enclosed in a kiln shell to control and manipulate the large amounts of heat required for the pyrolysis reactor / zone 220 processes and reactions to occur. In additional embodiments, the kiln shell of the device may comprise several insulating chambers surrounding multiple zones. In certain embodiments, the kiln includes multiple separate zones for the devices. In an additional embodiment, each zone of the device includes at least one inlet and at least one outlet. In additional embodiments, within each zone, the inlets and outlets can be adjusted to control the flow of carbon feedstock 100, gases 122-123, and heat into, out of, or into the zone. A supply of inert gas 123 can be introduced into the inlets 151a, 151b, and 151c, and the removed air 122 can be extracted through the corresponding outlets 150a, 150b, and 150c. In additional embodiments, one or more outlets of a zone within the device are connected to one or more other inlets or other outlets within the device.

[0222] In an additional embodiment, raw carbon source material 100 is deoxygenated in the Carbon Source Material Supply System 110 before being introduced into the device (specifically, the first zone and / or optional Drying and Preheating Zone 200a). The "drying and preheating zone 200a" may include inlets 151b and 151c and outlets 150b and 150c. In an additional embodiment, the "drying and preheating zone 200a" is heated to a temperature of about 80°C to about 200°C to reduce water and other moisture from the carbon source material 100. The carbon source material 100 is then moved to the same preheating zone where the material 100 is preheated.

[0223] In an additional embodiment, the optionally dried and preheated carbon source material 100 is then transferred to a "pyrolysis reactor / zone 220" for carbonization. In certain embodiments, carbonization occurs at a temperature of from about 200°C to about 1100°C. For example, approximately 200°C, approximately 210°C, approximately 220°C, approximately 230°C, approximately 240°C, approximately 250°C, approximately 260°C, approximately 270°C, approximately 280°C, approximately 290°C, approximately 300°C, approximately 310°C, approximately 320°C, approximately 330°C, approximately 340°C, approximately 350°C, approximately 360°C, approximately 370°C, approximately 380°C, approximately 390°C, approximately 400°C, approximately 410°C, approximately 420°C, approximately 430°C, approx. 440°C, approx. 450°C, approx. 460°C, approx. 470°C, approx. 480°C, approx. 490°C, approx. 500°C, approx. 510°C, approx. 520°C, approx. 530°C, approx. 540°C, approx. 550°C, approx. 560°C, approx. 570°C, approx. 580°C, approx. 590°C, approx. 600°C, approx. 610°C, approx. 620°C, approx. 630°C, approx. 640°C, approx. 650°C, approx. 660°C, approx. 670°C, approx. 680°C, approx. 690°C, approx. 700°C, approx. 710°C, approx. 720°C, approx. 730°C, approx. 740°C, approx. 750°C, approx. 760°C, approx. 770°C, approx. 780°C, approx. 790°C, approx. 800°C, approx. 810°C, approx. 820°C, approx. 830°C, approx. 840°C, approx. 850°C, approx. 860°C, approx. 870°C, approx. 880°C, approx. 890°C, approx. 900°C, approx. 910°C, about 920°C, about 930°C, about 940°C, about 950°C, about 960°C, about 970°C, about 980°C, about 990°C, about 1000°C, about 1010°C, about 1020°C, about 1030°C, about 1040°C, about 1050°C, about 1060°C, about 1070°C, about 1080°C, about 1090°C, and about 1100°C, with about 800°C being preferred.

[0224] In an additional embodiment, the carbonization zone of the Pyrolysis Reactor / Zone 220 is configured so that the gases 122 produced during carbonization can be extracted and stored for later use. In an additional embodiment, the gases 122 produced during carbonization are optionally extracted for current or later use. In additional embodiments, the carbonization temperature is selected and maintained to maximize the carbon content of the carbonized carbon source material 100 while reducing or eliminating the production of methane (CH4).

[0225] In additional embodiments, the “pyrolysis reactor / zone 220 ” may include at least one inlet and multiple outlet ports 158 . In additional embodiments, one of the outlet ports 158 can be connected to further processing equipment such as a collection system, an acid hydrogenation unit, a distillation column, etc. In additional embodiments, the Pyrolysis Reactor / Zone 220 can process the off-gas 122 coming from the Preheat Zone 210 or the Pyrolysis Reactor / Zone 220 to produce a condensate or concentrated gas. In further embodiments, the condensate may include polar compounds such as, by way of non-limiting example, acetic acid, methanol, and furfural. In additional embodiments, the enriched gases produced in the Pyrolysis Reactor / Zone 220 may include at least non-polar gases. In additional embodiments, the gas Pyrolysis Reactor 220 may include a Fractionation Column. In additional embodiments, the acetic acid is sent via a line or channel to an optional "acid hydrogenation unit." In an additional embodiment, the methanol-furfural is sent to a distillation and processing unit via an optional additional line channel.

[0226] In additional embodiments, the carbon recovery unit may also include an input connected to a "pyrolysis reactor / zone 220." In an additional embodiment, the gas 122 withdrawn from the carbon recovery unit is optionally used in an energy recovery system capable of carbon enrichment. Additionally, in various embodiments, gas 122 may be withdrawn from one or more zones of the device and optionally used in an energy recovery system or a system for carbon disposal.

[0227] As mentioned above, high oxygen levels in the ambient air surrounding the carbon source material 100 during processing can result in undesirable combustion and oxidation of the carbon source material 100. This can significantly reduce the quantity and quality of the final activated carbon material 105. In additional embodiments, the Carbon Source Material Supply System 110 may be a closed system comprising one or more manifolds configured to remove oxygen 122 from the air surrounding the raw carbon source material 100 and the Pyrolysis Reactor / Zone 220. In additional embodiments, oxygen levels of about 0.5% to about 1.0% can be used for preheating, pyrolysis, carbonization, and cooling. The closed "carbon source material supply system 110" is configured with the goal of reducing the oxygen level to about 3% or less, about 2% or less, about 1% or less, or about 0.5% or less throughout the process. As the oxygen level drops, the carbon source material 100 is transported along a "carbon source material supply system 110" within the device. In additional embodiments, preheating the inert gas throughout the recovery process and then introducing the preheated inert gas 123 into the device reactor and trimming reactor can improve system efficiency and reduce energy consumption.

[0228] In an additional embodiment, a trimming reactor (not shown) can be included in the system. In an additional embodiment comprising a trimming reactor (not shown), the pyrolyzed material from the device is fed to a separate additional reactor (not shown) for further pyrolysis, where heated inert gas 123 is introduced to produce products with higher carbon levels. In additional embodiments, this secondary processing occurs in containers such as, but not limited to, drums, tanks, barrels, bins, totes, pipes, sacks, presses, and roll-off containers. In an additional embodiment, a final container can be used for transporting the carbonized material 105. In an additional embodiment, the inert gas 123 is heated via a heat exchanger (not shown) that obtains heat from the gas 123 extracted from the device and is combusted in a process gas heater.

[0229] In an additional embodiment, the Heat, Steam, and Gases 123 recovered from the Pyrolysis Reactor / Zone 220 is sent to the Carbon Source Material Supply System 110 where it is jacketed and isolated from direct contact with the Carbon Source Material 100. However, the heat, steam, and gases 123 recovered from the pyrolysis reactor / zone 220 can be used to indirectly heat the carbon source material 100 prior to introduction into the pyrolysis reactor / zone 220 and / or the drying zone.

[0230] In an alternative embodiment, the heat, steam, and gases 123 recovered from the Drying Zones 200a-200b or the Pyrolysis Reactor / Zone 220 may be directed to the Carbon Source Material Supply System 110, which may be jacketed or otherwise isolated from direct contact with the carbon source material 100. This allows for indirect heating of the carbon source material 100 prior to its introduction into the Pyrolysis Reactor / Zone 220.

[0231] In additional embodiments, the carbonized activated carbon material 105 of predetermined pore structure may be moved to a "cooling and washing zone / section 240" for passive or active cooling. In additional embodiments, the predetermined pore structure carbonized activated carbon material 105 is cooled to a temperature of about 10°C, about 20°C, about 30°C, or about 40°C. In an additional embodiment, the predetermined pore structure carbonized activated carbon material 105 can be moved to a "cooling and washing zone / section 240." The predetermined pore structure carbonized activated carbon material 105 is cooled and washed to remove additives, specifically bases such as KOH. In an additional embodiment, the carbonized activated carbon material 105 of predetermined pore structure is transferred to a "cooling and washing zone / section 240" where it is cooled and washed with "additives such as water and hydrochloric acid (HCl)."

[0232] In this embodiment, when the predetermined pore structure carbonized activated carbon material 105 is introduced into the "cooling and washing zone / section 240", the carbonized material 105 is cooled to a predetermined temperature range of about 20°C or 30°C, which is approximately room temperature. In additional embodiments, the device includes multiple "cooling and washing zones / sections 240." In an additional embodiment, the "cooling and washing zone / section 240" can cool the carbonized material 105 to below 200°C. In an additional embodiment, the "cooling and washing zone / section 240" may include a mixer auger to agitate the carbonized material 105 to cool and wash it uniformly. In additional embodiments, one or more of the multiple "cooling and washing zones / sections 240" may be external to the device.

[0233] In additional embodiments, the carbonized activated carbon material 105 of a predetermined pore structure can exit the Cooling and Washing Zone / Section 240 along the Activated Carbon Material Supply System 120 and then enter a carbon recovery unit (not shown).

[0234] In an additional embodiment, the carbonized activated carbon material 105 of a predetermined pore structure is dried in the first or second Drying Zone 200a / 200b and then transported along the Activated Carbon Material Supply System 120, exiting the Cooling and Washing Zone / Section 240 and into the Electrode Mixing System / Zone 401.

[0235] At this point, the carbonized activated carbon material 105 of predetermined pore structure may be in a powdered state or may be pulverized to produce a fine powder. The grinding or pulverization may occur within the "Electrode Mixing System / Zone 401" or in a separate pulverizing device. In certain embodiments, grinding and pulverizing the carbonized activated carbon material 105 of predetermined pore structure can be performed before or after activating the carbon.

[0236] In one embodiment, activated carbon can be mixed with electrode materials in one or more mixing chambers to create an electrode mix. Some non-limiting examples of "electrode materials" include "conductive additives," "binders," and "admixtures." Some non-limiting examples of "conductive additives" include carbon black, super p, furnace black, channel black, acetylene black, thermal black, lamp black, conductive carbon, and the like. Some non-limiting examples of "binders" include PVDF, PTFE, non-reactive thermoplastic fluoropolymers, copolymers, terpolymers, and the like. Some non-limiting examples of "mixtures" include 2-propanol, 2-propyl alcohol, IPA, isopropyl, "isopropanol", alcohol, and water. Some non-limiting examples of electrode compositions may be in the form of admixtures, paints, mixtures, pastes, inks, free-standing electrodes, and the like.

[0237] In certain embodiments, the "electrode mixing system / zone 401" is interconnected or mechanically connected to an "electrode preparation system / zone 400" comprising one or more extruders 407 / sprayers for introducing the electrode mixture composition. In yet another embodiment, the Electrode Preparation System / Zone 400 forms a free-standing electrode that is formed, pressed, applied, and then attached to a current collector. The electrode mix composition can be applied, pressed, and contacted to a conductive current collector material such as: These metals include stainless steel, titanium, copper, aluminum, and silver, and can be thin films or meshes, with thicknesses ranging from 0.0001 mm to 10 mm, and with a variety of mesh patterns and windings. Additionally, electrode mixtures and freestanding electrodes are available in a variety of thicknesses ranging from 0.0001 mm to 10 mm, as listed below. たとえば、about 0.05mm·about 0.1mm·about 0.15 mm·about 0.2mm·about 0.25mm·about 0.3mm·about 0.35mm·about 0.4mm·about 0.45mm·about 0.5mm·about 0.55mm·about 0.6mm·about 0.65mm·about 0.7mm·about 0.75mm·about 0.8mm·about 0.85mm·about 0.9mm·about 0.95mm·about 1.0mm·about 1.25mm·about 1.5mm · About 1.75mm· About 2.0mm· About 2.25mm· About 2.5mm· About 2.75mm· About 3.0mm· About 3.25mm· About 3.5mm· About 3.75mm· About 4.0mm· About 4.25mm· About 4.5mm· About 4.75mm· About 5.0mm· About 6.0mm· About 7.0mm· About 8.0mm· About 9.0mm· About 10.0mmでもよい。 また, about 1mg / cm 2 About 1.25 mg / cm 2 About 1.5 mg / cm 2 About 1.75 mg / cm 2 About 2 mg / cm 2 About 2.25 mg / cm 2 About 2.5 mg / cm 2 About 2.75 mg / cm 2 About 3mg / cm 2 About 3.25 mg / cm 2 About 3.5 mg / cm 2 About 3.75 mg / cm 2 About 4 mg / cm 2 About 4.25 mg / cm 2 About 4.5 mg / cm 2 About 4.75 mg / cm 2 About 5mg / cm 2 About 5.25 mg / cm 2 About 5.5 mg / cm 2 About 5.75 mg / cm 2 About 6 mg / cm 2 About 6.25 mg / cm 2 About 6.5 mg / cm 2 About 6.75 mg / cm 2 About 7 mg / cm 2 About 7.25 mg / cm 2 About 7.5 mg / cm 2 About 7.75 mg / cm 2 About 8mg / cm 2About 8.25 mg / cm 2 About 8.5 mg / cm 2 About 8.75 mg / cm 2 About 9 mg / cm 2 About 9.25 mg / cm 2 About 9.5 mg / cm 2 About 9.75 mg / cm 2 About 10mg / cm 2 About 10.25 mg / cm 2 About 10.5 mg / cm 2 About 10.75 mg / cm 2 About 11 mg / cm 2 About 11.25 mg / cm 2 About 11.5 mg / cm 2 About 11.75 mg / cm 2 About 12 mg / cm 2 About 12.25 mg / cm 2 About 12.5 mg / cm 2 About 12.75 mg / cm 2 About 13 mg / cm 2 About 13.25 mg / cm 2 About 13.5 mg / cm 2 About 13.75 mg / cm 2 About 14 mg / cm 2 About 14.25 mg / cm 2 About 14.5 mg / cm 2 About 14.75 mg / cm 2 About 15mg / cm 2 About 16 mg / cm 2 About 17 mg / cm 2 About 18 mg / cm 2 About 19 mg / cm 2 About 20mg / cm 2 About 21 mg / cm 2 About 22 mg / cm 2 About 23mg / cm 2 About 24 mg / cm 2 About 25mg / cm 2 About 30mg / cm 2 About 35mg / cm 2 About 40mg / cm 2 About 45mg / cm 2 About 50mg / cm 2is also acceptable, approximately 3.6 to 10.5 mg / cm 2 is preferred.

[0238] In additional embodiments, the "electrode preparation system / zone 400" comprises or is mechanically connected to an applicator system, such as, but not limited to, a nozzle, sprayer, clapper, or press, which allows for the application of the electrode composition mixture and freestanding electrodes. The applicator system may be applied directly to the metal, may be in direct contact with the metal, or may be a freestanding configuration. In additional embodiments, the "electrode preparation system / zone 400" further includes mechanical pumps, compressors, gravity feeds, presses, augers, and pressures to provide a consistent supply of the electrode mix composition described above.

[0239] In additional embodiments, the Electrode Preparation System / Zone 400 includes an electrode mix feed system 406 and may also include a mechanical feed system and a Device Winding and Stacking System 411 . In further particular embodiments, the Electrode Preparation System / Zone 400 may include a feeder, a winder, rollers 412a and 412b, a drum, a cutter, a crimper, a drive mechanism or motor 414, a connecting belt 415, gears, a direct connection, and tensioners 413a and 413b. Additionally, for the anode material, cathode material, and ion-permeable separator, "electrode preparation system / zone 400" includes an electrode mixing injector 407, an electrode applicator 408, an electronic electrode mixing overflow system 409, "electrode drying system / zone 420," and "electrolyte injection system / zone 430." The "electrolyte injection system / zone 430" includes the "electrolyte mixing system 431", the storage tank, liquid electrolyte conduit 432, the electrolyte injector 433, and the "adhesion and sealing system / zone 450". The "Attachment and Sealing System / Zone 450" may include a welder 451, a sealer, a crimper, a press, and a seal, and forms part of the energy storage device production system 500. In alternative embodiments, the “attachment and sealing system / zone 450 ” can be mechanically connected to or disconnected from the energy storage device manufacturing system 500 . In an additional embodiment, the Energy Storage Device Manufacturing System 500 may further include an energy storage device hopper 462 for storing or stacking the energy storage devices 460 .

[0240] In an additional embodiment, an "electrode preparation system / zone 400" may be used to continuously supply the "conductive metal 45" described above. In an additional embodiment, an "electrode preparation system / zone 400" can be used to provide a continuous supply of conductive metal 45 coated with an electrode mix, ink, paint, paste, or composition. In an additional embodiment, the Electrode Preparation System / Zone 400 can provide a continuous supply of Electrode Mix to form a free-standing electrode.

[0241] In an additional embodiment, the Electrode Preparation System / Zone 400 provides a continuous supply of Conductive Metal 45 for immobilizing and contacting the Conductive Metal 45 with the free-standing electrode / electrode mixture. In an additional embodiment, the Electrode Preparation System / Zone 400 may provide a continuous supply of ion permeable separators 95 . In an additional embodiment, the "electrode preparation system / zone 400" allows for a continuous supply of conductive metal 45, electrode mixture composition, and ion-permeable separator 95 for layering / multi-layering. In an additional embodiment, the "electrode preparation system / zone 400" allows for layering of energy storage devices. In additional embodiments, the "electrode preparation system / zone 400" allows for layering of energy storage devices having the following layer structure: Two conductive metal current collectors 45 with electrode mixture applied to opposite surfaces. Two conductive metal current collectors 45 with opposing faces in contact with the free-standing electrodes. Two ion-permeable separators 95 between the two current collectors and the electrode composite. In an additional embodiment, the Electrode Preparation System / Zone 400 allows for the fabrication of a double layer electrolytic capacitor 460 . In an additional embodiment, the Electrode Preparation System / Zone 400 allows for the fabrication of a supercapacitor 460 . In an additional embodiment, the Electrode Preparation System / Zone 400 allows for the fabrication of an energy storage device 460.

[0242] In additional embodiments, the "electrode preparation system / zone 400" is configured to fabricate a continuously wound or stacked (anode, ion-permeable separator, cathode, ion-permeable separator) energy storage device 460 or supercapacitor cell 460. In additional embodiments, the electrode preparation system / zone 400 can be configured to provide a layered structure with multiple anodes 45, multiple ion-permeable separators 95, and multiple cathodes 45, which can be stacked or grouped into cells. Additionally, in certain embodiments, the stacked, laminated, or wound energy storage device may have an anode lead connected and may also have a cathode lead connected. In certain embodiments, the anode and cathode leads may be connected to the energy storage device terminals 115 and may protrude from the energy storage device 460.

[0243] In certain embodiments, the ion-permeable separator 95 includes, but is not limited to, porous plastic, paper, cellulose, glass, fiber, sheet, spray, ion-permeable insulators and separators.

[0244] In an additional embodiment of the "electrode preparation system / zone 400," the device may further include a "mechanical feeding unit or feeder" for the supercapacitor container shell. A mechanical feeding unit or feeder may be mechanically connected to the device and may be used to allow the insertion and removal of supercapacitor containers consisting of new or partially completed containers containing supercapacitor material at regular or predetermined intervals.

[0245] In additional embodiments, the "electrode preparation system / zone 400" may include a mechanical feeding unit or feeder for placing layered or wound energy storage device "internal contents" (e.g., energy storage material or supercapacitor material) into the energy storage container. In additional embodiments, the "electrode preparation system / zone 400" may be mechanically connected to one or more electrolyte injectors 433 and may further include spray nozzles. In an additional embodiment, the "electrode preparation system / zone 400" dispenses / injects (433) electrolyte into an energy storage container containing energy storage / supercapacitor material. The electrolytes include organic electrolytes, aqueous electrolytes, co-solvents, salt electrolytes, ion carrier electrolytes, ionic electrolytes, gel electrolytes, dry polymer electrolytes, and ceramic electrolytes, with "co-solvents in salt electrolytes" being preferred.

[0246] In this embodiment, the "electrode preparation system / zone 400" can inject / inject (433) the electrolyte into the energy storage device in a typical atmospheric environment. In this example, the "electrode preparation system / zone 400" introduces / injects (433) electrolyte into the "energy storage device" in a typical atmospheric environment. In this example, the "electrode preparation system / zone 400" introduces and injects (433) the electrolyte into the "supercapacitor" in a general atmospheric environment.

[0247] In addition, in the "electrode preparation system / zone 400" of this embodiment, the device may also include a mechanical supply unit or feeder for an energy storage container containing energy storage material / electrolyte. In this embodiment, the Electrode Preparation System / Zone 400 may be mechanically connected to the container sealing device. The "sealing device" may include a crimper, screw, rivet, clamp, press, weld, or seal, or may include a welder 451 for joining or securing the anode and cathode leads to the positive and negative terminals of the energy storage device, and for enclosing or sealing the energy storage device 460. In this embodiment, the "electrode preparation system / zone 400" may include a sealing device and may also include a sealing means for the container with or without a separate seal or component.

[0248] Also in this embodiment, the Electrode Preparation System / Zone 400 may include means for controlling the internal energy storage pressure, for example, for vacuum. In certain embodiments, the "electrode preparation system / zone 400" may include a vacuum pump to reduce the internal pressure of the energy storage device.

[0249] In this embodiment, the "electrode preparation system / zone 400" may include an "energy storage cell hopper 462" for receiving completed energy storage devices 460 or completed supercapacitor cells 460.

[0250] In this embodiment, the "electrode preparation system / zone 400" may include a controller processor (not shown) associated with controlling the operation and parameters of the "electrode preparation system / zone 400." In additional embodiments, the controller processor can be configured to regulate the speed and control of a number of systems, including the following non-limiting examples: Non-limiting examples include anode metal 45 supply, cathode metal 45 supply, ion permeable separator 95 supply, electrode mix and electrode material feed system 406, electrode mix applicator 408, electrode mix measurement and electrode mix recirculation system 409, electrode drying 420, rollers 412a and 412b, tensioners 413a and 413b, winding speed, winding length, stacking speed, stacking length, motor 414, drive system 415, container loading, container filling, container transport, liquid electrolyte mixing 431, liquid electrolyte injection 432 and 433, liquid electrolyte measurement, anode and cathode connection, anode and cathode terminal connection, attachment 450, container sealing 451, container crimping, container closure, vacuum control, energy storage device 460 assembly, supercapacitor 460 assembly, and hopper 462 storage and control. The controller can be based on one or more inputs, sensors, feedback sensors, measurement parameters, measurements, timers, timed processes, temperature gauges, or other suitable assembly parameters. In additional embodiments, moisture, temperature, and gas sensors in communication with the controller processor are incorporated into or mechanically connected to each zone, between zones, or at any suitable location within or along the energy storage device manufacturing system 500 device. In additional embodiments, the controller processor may use information obtained from sensor gauges. This optimizes the speed and efficiency of devices, processing systems, machine parts, feeding systems, mixing systems, assembly systems and materials based on readings taken by various sensors.

[0251] FIG. 16 is a functional block diagram of an embodiment of the present invention including a Carbon Source Material Supply System 110, a single reactor, multiple zones, and a System / Zone 380 for Producing Hierarchical Activated Carbon with Predetermined Pore Structure. The device configuration of this embodiment includes a fully mechanically coupled and operably connected "energy storage device manufacturing system 390" having an "electrode preparation system / zone 400" in communication with a "predetermined pore structure hierarchical activated carbon manufacturing system / zone 380." Here, the present invention is achieved by a series of steps and alternative steps including:

[0252] In this example, activated carbon with a hierarchical structure of an improved predetermined pore structure and a completed energy storage device were fabricated through the following process. This is a process in which the device parameters are controlled to produce the desired result product, ultimately determining the desired "pore width and hierarchical structure of activated carbon." Drying the optional carbon source 200a. Feeding the carbon source material 100 to a "sizing and grinding system 180" (optional). The process of milling a carbon source material 100 to produce a milled carbon source material 101. A process of feeding a carbon source material 100 into a chemical base "soak tank / system 190" or a process of feeding a pulverized carbon material 101 into a chemical base "soak tank / system 190" or a process of adding a pulverized carbon material 101 into a chemical base "soak tank / system 190". A process 110 in which the "carbon source material 100" or "ground carbon source material 101" is soaked in a basic chemical or aqueous solution to produce a "base-soaked carbon source material 102." A process of supplying a carbon source material 100 by the "carbon source material supply system 110", or a process of placing a pulverized carbon source material 101 into the "drying and preheating zone 200a" (optional), or a process of supplying a carbon source material 102 soaked in a base by the "carbon source material supply system 110" to the "drying and preheating zone 200a" (optional). Drying the base-soaked carbon source material 102 or carbon source material 100 in a drying system / zone 200 (optional). The process of removing chemicals such as water 126 and base from the "base-soaked carbon source material 102." A process for producing "dry carbon source material 103." The process of recovering and reusing heat using the "Heat Recovery System 310." The process of feeding the "dry carbon material 103" to an optional first zone (preheat reactor) 210 by the "carbon source material feeding system 110". The process of "preheating" the dry carbon source material 103 in a first zone (preheat reactor) 210 to produce a "preheated carbon source material 104." The process of discharging the water 126 and gas via line 160. The "carbon source material supply system 110" supplies the "preheated carbon source material 104" to a second zone (pyrolysis reactor) 220 (optional), and the two undergo pyrolysis. A process of preheating dry material 103 undergoing pyrolysis in a second zone (pyrolysis reactor) 220 or preheating material 104 undergoing pyrolysis to produce an "activated carbon material 105 having a predetermined pore structure hierarchy." Optionally, monitoring the second zone (pyrolysis reactor) 220 by FTIR 290 (optional). feeding activated carbon material 105 containing additives such as HCl to a third zone (cooling and washing reactor) 230 (optional) by an "activated carbon material feeding system 120" for cooling and washing. Discharging gas from the first zone (preheat reactor) 210 through line 160. Discharging gas from the second zone (pyrolysis reactor) 220 via line 160. Discharging the gas through line 160 from a second line 160 connected to a single line 161 . Discharging the gas into "phase separator 250" via combined line 161. The process of "capturing polar compounds 128" from exhaust gases, which can then be used immediately for heat and energy recovery as needed, or stored for later use. Transferring acetic acid from the phase separator 250 via line 160 to an acid hydrogenation unit 280. The process of converting acetic acid into ethanol 127 (optional). Optionally, feeding the cooled and washed activated carbon material 106 to an activated carbon recovery unit 300 via an activated carbon material feeding system 120. Optionally, removing the final activated carbon product 350 produced in the Predetermined Pore Structure Hierarchical Activated Carbon Production System / Zone 380 from the Activated Carbon Recovery Unit 300. Optionally, recover energy 310 via an "activated carbon recovery unit 300." A process of cooling / washing the activated carbon material 106 produced in the "system for producing hierarchical activated carbon with a predetermined pore structure / zone 380" by the "activated carbon material supply system 120" in the "electrode mixing system / zone 401" of the "energy storage device manufacturing system 390". and mixing additional electrode components with the activated carbon material 105·106 having a hierarchical structure of predetermined pore structure to produce an electrode composite mixture in an “electrode mixing system / zone 401.” feeding the electrode composite mixture 107 into an "electrode preparation system / zone 400." The process of preparing an electrode 108 in an "electrode preparation system / zone 400" and feeding the electrode 108 to an "electrode drying system / zone 420" (optional) or feeding the electrode to a "device winding and stacking system 411" that includes an ion-permeable separator. feeding the prepared electrode 109 into an "electrolyte input system / zone 430." placing the completed energy storage device actuation mechanism 109 into the energy storage device container. The process of adding electrolyte 435 supplied from "electrolyte mixing system 431" to "electrolyte addition system / zone 430". The process of sealing and encapsulating the energy storage device assembly 461 in the "attachment and sealing system / zone 450" to the completed energy storage device assembly 461. Optionally, applying a vacuum to the sealed / enclosed completed energy storage device assembly 461 or fabricating the completed energy storage device 460.

[0253] In the embodiment shown in Figure 16, the improved "activated carbon having a hierarchical structure of predetermined pore structure" and "finished energy storage device" includes:

[0254] In this example, the carbon source material 100 is fed into an optional "sizing and grinding system 180." In this embodiment, the enclosed "carbon source material supply system 110" includes a material supply hopper (not shown), a material transfer mechanical system 110, and a deoxygenation manifold or mechanical system (not shown).

[0255] In this embodiment, the material feed hopper may be any suitable open or closed atmosphere container configured to receive the carbon source material 100 . The material feed hopper may be mechanically connected and operatively associated with the "carbon source material feed system 110," which in certain embodiments may be a screw and auger system rotated by a non-limiting example drive source such as a motor or other mechanically operable device (not shown).

[0256] In an additional embodiment, the carbon source material 100 is fed to a "carbon source material feeding system 110" which is implemented as a gravity feed system. In certain embodiments, the carbon-source material supply system 110 is configured so that the screw auger is properly enclosed. In additional embodiments, the "enclosure" may be generally cylindrical. In additional embodiments, the "carbon-source material supply system 110" can include screws, augers, conveyors, drums, screens, chutes, drop chambers, pneumatic conveying devices, and may also have rotary airlocks, double and triple flap airlocks (not shown).

[0257] In certain embodiments, the carbon source material 100 is fed from a carbon source material feed hopper into the "carbon source material feed system 110," and the rotation of an auger or screw transports the raw carbon source material 100 toward the deoxygenation manifold. When the carbon source material 100 reaches the deoxygenation manifold, the raw carbon source material 100 in the "carbon source material supply system 110" is surrounded by air containing approximately 21% oxygen. In additional embodiments, the deoxygenation manifold may be located adjacent to or near the Carbon Source Material Supply System 110. In certain embodiments, the "deoxygenation manifold" or "carbon source material supply system 110 enclosure" may include multiple gas inlet ports and multiple gas outlet ports.

[0258] In certain embodiments, an "oxigen purge manifold" can have at least one gas inlet line and at least one gas outlet line. In additional embodiments, at least one gas inlet line of the deoxygenation manifold can be in operable communication and mechanical connection with each of the plurality of gas inlet ports. In an additional embodiment, at least one gas outlet line of the deoxygenation manifold can be in operative communication and mechanical connection with each of the plurality of gas outlet ports. In certain embodiments, the gas inlet line can be configured to deliver an inert gas to the gas inlet port. In particular embodiments, the inert gas is substantially oxygen-free nitrogen, argon, or helium. In an additional embodiment, the inert gas is introduced counter-currently to the carbon source material.

[0259] In certain embodiments, an inert gas may be introduced into the sealed Carbon Source Material Supply System 110 to push ambient air out of the sealed system. In certain embodiments, during operation, when inert gas is introduced into the first gas inlet port, a quantity of oxygen-enriched ambient air is exhausted through the outlet port. At this point, the desired oxygen level (about 2% or less, about 1% or less, about 0.5% or less, about 0.2% or less, about 0.1% or less) may not be achieved.

[0260] In additional embodiments, an inert gas must be additionally injected to remove the necessary or desired amount of oxygen from the air surrounding the carbon source material 100 in the sealed system. In an additional embodiment, the second gas inlet port can inject an inert gas into the sealed system in conjunction with the injection through the first gas inlet port to remove some or most of the remaining oxygen from the sealed system. After injecting inert gas once, twice or multiple times to eliminate oxygen, the desired result of "reducing the oxygen content" can be achieved. In an additional embodiment, if the desired oxygen level is still not reached after the second inert gas injection, a third inert gas injection can be performed, and the gas outlet can remove any remaining unwanted oxygen from the sealed system. Additional inlets and outlets may be provided as required. In an additional embodiment, oxygen levels are monitored throughout the "carbon source material supply system 110" and the amount and location of inert gas injection are calibrated to ensure the desired performance, safety, and production of activated carbon material 105 with a predetermined hierarchical pore structure.

[0261] In certain embodiments, each gas inlet port and its corresponding gas outlet port are slightly offset from one another with respect to a perpendicular bisector plane passing through the carbon source material supply system 110 . In certain embodiments, the inlet ports and corresponding outlet ports can be offset on the Carbon Source Material Feed System 110 by an amount that corresponds approximately to the pitch of the augers in the Carbon Source Material Feed System 110. In an additional embodiment, the atmosphere surrounding the feedstock 100 may be deoxygenated to a predetermined or sufficient level before being fed from the carbon source material feed system 110 to one or more pyrolysis reactors / zones 220. In additional embodiments, oxygen levels can be monitored throughout the Carbon Source Material Supply System 110 to calibrate the amount and location of inert gas injection to achieve the desired oxygen levels.

[0262] In additional embodiments, the device includes multiple gas introduction and extraction probes positioned at various points throughout the device. In additional embodiments, each one of the gas introduction probes and each one of the gas extraction probes corresponds to a different one of the plurality of zones. In alternative embodiments, the device may have any suitable number of gas introduction probes and gas extraction probes, and in certain embodiments, may have one gas introduction probe and two or more gas extraction probes for multiple zones.

[0263] In this example, a carbon material 100 is pulverized to produce a pulverized carbon source material 101 . The carbon source material 100 is fed into a chemical base soak tank / system 190 . Alternatively, the ground carbon source material 101 is fed into a chemical "base steep tank / system 190." Alternatively, the ground carbon material 101 is fed into a separate chemical "base dip tank / system 190" (optional).

[0264] In this example, the carbon source material 100, such as coal or petroleum coke, is optionally dried, crushed, and sized, for example by passing through a mesh, outside the Pyrolysis Reactor / Zone 220, after which the carbon source material 100 is introduced into the Steeping and Mixing Zone 190, optionally using an oxygen-containing atmosphere, before being introduced into the carbon source hopper. This can optionally be achieved using a Carbon Source Material Supply System 110. The Carbon Source Material Supply System 110 can control the oxygen level in the ambient air of the device to be about 3% or less, about 2% or less, about 1% or less, or about 0.1% or less. Once the oxygen level within the device is reduced, raw carbon material 100 enters the "soak and mix zone 190" via a sealed "carbon source material supply system 110." In one such embodiment, the carbon-source material supply system 110 may include an encapsulated jacket sleeve. The vapors and off-gas from the "pyrolysis reactor / zone 220" are used to preheat and pyrolyze the carbon source material 100, either by directly heating the carbon source material 100 or by a process gas heater or heat exchanger (not shown) to preheat and pyrolyze the carbon source material 100.

[0265] Next, in this example, a water-containing additive (such as, but not limited to, KOH) is thoroughly and uniformly distributed throughout the carbon source material for a period of time prior to preheating and pyrolysis. The immersion time in the "immersion and mixing zone 190" is as follows: 10 minutes, 20 minutes, 30 minutes, 40 minutes, 50 minutes, 1 hour, 1.5 hours, 2 hours, 3 hours, 4 hours, 5 hours, 6 hours, 7 hours, 8 hours, 9 hours, 10 hours, 11 hours, 12 hours, 13 hours, 14 hours, 15 hours, 16 hours, 17 hours, 18 hours, 19 hours, 20 hours, 21 hours, 22 hours, 23 hours, 24 hours, 25 hours Approximately 26 hours, approximately 27 hours, approximately 28 hours, approximately 29 hours, approximately 30 hours, approximately 31 hours, approximately 32 hours, approximately 33 hours, approximately 34 hours, approximately 35 hours, approximately 36 hours, approximately 37 hours, approximately 38 hours, approximately 39 hours, approximately 39 hours, approximately 40 hours, approximately 41 hours, approximately 42 hours, approximately 43 hours, approximately 44 hours, approximately 45 hours, approximately 46 hours, approximately 47 hours, approximately 48 hours, approximately 49 hours, approximately 50 hours, with around 12 hours being ideal.

[0266] In this example, a carbon source material 100 or pulverized carbon material 101 is soaked in a basic chemical or aqueous base to produce a "base-soaked carbon source material 102" (110). The carbon source material 100 and pulverized carbon material 101 are supplied to an optional drying and preheating zone 200a by the carbon source material supply system 110.

[0267] In an alternative embodiment, the drying zone is associated with a gas introduction probe and a gas extraction probe. In an additional embodiment, a gas introduction probe introduces "nitrogen, argon, or helium" into the drying zone, and a gas extraction probe extracts gas from the drying zone. In certain embodiments, the gas introduction probe introduces a mixture of gases into the drying zone. In an additional embodiment, the extracted gas may be oxygen. In another embodiment, a gas extraction probe extracts gas from the drying zone for reuse in a heat and energy recovery system.

[0268] In certain embodiments, the "preheat zone 210" can be associated with a gas introduction probe and a gas extraction probe. In additional embodiments, a gas introduction probe introduces nitrogen, argon, or helium into the preheat zone 210 and a gas extraction probe extracts gas from the preheat zone 210 . In additional embodiments, the gas introduction probe can be configured to introduce a mixture of gases into the preheat zone 210 . In additional embodiments, the gas extracted from the gas extraction probe may include carbon-rich off-gas. In additional embodiments, gases extracted from the Preheat Zone 210 or Pyrolysis Reactor / Zone 220 may be reintroduced into the material at a later stage in the process, such as in a carbon recovery unit or Pyrolysis Reactor / Zone 220. In additional embodiments, gas extracted from multiple zones of the device is used for energy recovery in a drying, treatment, and gas preheater or for further pyrolysis in a trimming reactor or carbon enrichment unit.

[0269] In another embodiment, the base-soaked carbon source material 102 is fed to the Drying and Preheating Zone 200a (optional) by the Carbon Source Material Feed System 110. Drying system / zone 200 (optional) dries the base-soaked carbon source material 102 or carbon source material 100 . Chemicals such as water 126 and base are removed from the carbon source material 102 that has been soaked in the basic chemical. Preparation of dry carbon source material (103). Heat recovery and reuse through the "Heat Recovery System 310." A "carbon source material supply system 110" supplies dry carbon material 103 to a first zone (preheat reactor) 210 (optional). Dry carbon source material 103 is preheated in a first zone (preheat reactor) 210 (optional) to produce preheated carbon source material 104. Water 126 and gas are discharged via line 160 .

[0270] In certain embodiments, the device may include a single "pyrolysis reactor / zone 220" having two or more distinct zones. In certain embodiments, multiple zones are shown; however, in alternative embodiments, any different number of zones may be used. In additional embodiments, each zone can be connected to at least one other zone via a material transfer unit 110 . In additional embodiments, the material transfer unit 110 can control the atmospheric and temperature conditions.

[0271] Next, in this embodiment, the "pre-soaked carbon source 100" is introduced into the "drying and preheating zone 200a," where the internal temperature of the carbon source 100 is increased from near ambient temperature to approximately 100°C, 150°C, or 200°C. In additional embodiments, the temperature remains below 200°C. In an additional embodiment, the "drying and preheating zone 200a" may include a mechanism (not shown) for capturing and venting off-gas from the pre-soaked carbon source 100 during preheating. In an additional embodiment, the off-gas can be extracted for later use. In additional embodiments, the heating sources used for the various mechanical systems are electric and gas. In additional embodiments, the heating source used for the various reactors may be waste gas from another reactor in the device or gas from an external source. In an additional embodiment, the heat may be from an indirect heat source.

[0272] In this example, the carbon material 104 preheated by the "carbon source material supply system 110" is supplied to a second zone (pyrolysis reactor) 220 (optional) for pyrolysis.

[0273] In certain embodiments, the "pyrolysis reactor / zone 220" can be associated with a gas introduction probe and a gas extraction probe. In additional embodiments, a gas introduction probe introduces nitrogen, argon, or helium into the Pyrolysis Reactor / Zone 220, and a gas extraction probe extracts gases from the Pyrolysis Reactor / Zone 220. In an additional embodiment, the gas introduction probe is configured to introduce a mixture of gases into the pyrolysis zone. In additional embodiments, the gas extracted from the gas extraction probe may include carbon-rich off-gas. In certain embodiments, the carbon-rich gas extracted from the Pyrolysis Reactor / Zone 220 may be reintroduced into the material at a later stage in the process. In an additional embodiment, gases extracted from the Preheat Zone 210 and gases extracted from the Pyrolysis Reactor / Zone 220 can be combined at any stage in the process before being reintroduced into the material.

[0274] In this embodiment, in the second zone (pyrolysis reactor) 220, a "predetermined pore structure carbonized activated carbon material 105" is produced by the preheated material 104 undergoing pyrolysis and the dried material 103 undergoing pyrolysis. An FTIR 290 (optional) can monitor the second zone (pyrolysis reactor) 220 (optional).

[0275] Subsequently, after preheating in the Drying and Preheating Zone 200a, the Carbon Source Material Delivery System 110 transfers the preheated carbon source 100 to any other Pyrolysis Reactor / Zone 220. In additional embodiments, first zone 200a and "pyrolysis reactor / zone 220" are the same reactor. In additional embodiments where the first zone 200a is separate from the Pyrolysis Reactor / Zone 220, the Carbon Source Material Supply System 110 can penetrate the Pyrolysis Reactor / Zone 220 through a high temperature steam seal system, such as, by way of non-limiting example, an airlock (not shown). This allows the carbon source 100 to permeate the "pyrolysis reactor / zone 220" while preventing gas, heat loss, and oxygen ingress. In additional embodiments, the interior of the "pyrolysis reactor / zone 220" is heated to a temperature of about 100°C, about 200°C, about 300°C, about 400°C, about 500°C, about 600°C, about 700°C, about 800°C, about 900°C, about 1000°C, or about 1100°C, with "800°C for 2 hours at a ramp rate of 10°C per minute" being preferred. In additional embodiments, the Pyrolysis Reactor / Zone 220 may include an Output Port to capture and discharge gases evolved from the preheated carbon source material 100, for example, while undergoing pyrolysis. In an additional embodiment, the gas is extracted and optionally stored for later use. In an additional embodiment, the off-gas from the Pyrolysis Reactor / Zone 220 and the off-gas from multiple zones of the device can be combined into a single gas stream. Upon carbonization, the carbon source material 100 becomes a "hierarchically structured pyrolytic activated carbon 105 of predetermined pore structure" that is transported out of the "pyrolysis reactor / zone 220" by the "activated carbon material delivery system 120." In certain embodiments, the “activated carbon material supply system 120 ” is the same system as the carbon source supply system 110 . The "hierarchically structured pyrolytic activated carbon 105 having a predetermined pore structure" is introduced into an optional "cooling and washing zone / section 240" for cooling and washing. In the "cooling and washing zone / section 240," the activated carbon is preferably washed with "water and optional additives," a non-limiting example of a preferred additive being "HCl." In certain embodiments, the cleaning and cooling can be accomplished for a specific, controlled amount of time (eg, soak time). For example, soaking times are approximately 10 minutes, approximately 20 minutes, approximately 30 minutes, approximately 40 minutes, approximately 50 minutes, approximately 1 hour, approximately 1.5 hours, approximately 2 hours, approximately 3 hours, approximately 4 hours, approximately 5 hours, approximately 6 hours, approximately 7 hours, approximately 8 hours, approximately 9 hours, approximately 10 hours, approximately 11 hours, approximately 12 hours, approximately 13 hours, approximately 14 hours, approximately 15 hours, approximately 16 hours, approximately 17 hours, approximately 18 hours, approximately 19 hours, approximately 20 hours, approximately 21 hours, approximately 22 hours, approximately 23 hours, approximately 24 hours. Time: about 25 hours, about 26 hours, about 27 hours, about 28 hours, about 29 hours, about 30 hours, about 31 hours, about 32 hours, about 33 hours, about 34 hours, about 35 hours, about 36 hours, about 37 hours, about 38 hours, about 39 hours, about 40 hours, about 41 hours, about 42 hours, about 43 hours, about 44 hours, about 45 hours, about 46 hours, about 47 hours, about 48 hours, about 49 hours, about 50 hours, and "about 8 hours" is preferred. In certain embodiments, the "cooling and washing zone / section 240" may be the same zone / system as the "pyrolysis reactor / zone 220" or a different zone / system.

[0276] In this example, a "raw carbon source material 100," such as coal, petroleum coke, oil, or biomass, is introduced into the "pyrolysis reactor / zone 220" in an atmosphere with low oxygen content, optionally achieved by the "carbon source material supply system 110" described above. The Carbon Source Material Supply System 110 can be used to reduce the oxygen level in the ambient air within the system to about 3%, about 2%, about 1%, about 0.1% or less, resulting in pyrolysis without combustion. Raw carbon source material 100, after the oxygen level has been reduced, is introduced into the device in a sealed "carbon source material supply system 110." In an additional embodiment, the "carbon source material supply system 110" may include an encapsulated jacket or sleeve through which steam or off-gas from the reactor is routed and utilized to preheat the carbon source material 100.

[0277] In an additional embodiment, raw carbon source material 100 first travels from the Carbon Source Material Supply System 110 through optional Drying and Preheating Zones 200a and 210 of the device. In an additional embodiment, a "drying and preheating zone 200a" (optional) can heat the raw materials to remove water and other moisture, which can be a separate zone or can be sent to a separate "preheating zone 210." In additional embodiments, the interior of the optional "drying and preheating zone 200a" may be heated to a temperature from about ambient temperature to about 100°C, about 150°C, or about 200°C. The water or moisture removed from the raw carbon source material 100 can, in one example, be discharged from the "drying and preheating zone 200a" (optional) through an exit port. In an additional embodiment, the "drying and preheating zone 200a" (optional) can be adapted to extract vapor, steam, and moisture. In an additional embodiment, the vapor / steam / moisture from the "Drying / Preheating Zone 200a" (optional) can optionally be extracted for later use. The moisture, vapor, or steam extracted from the optional Drying and Preheating Zone 200a can be used in a suitable waste heat recovery system and in conjunction with the Carbon Source Material Supply System 110. In an additional embodiment, the vapor, steam, or moisture used in the Carbon Source Material Supply System 110 can be used to preheat the raw carbon source material 100 while oxygen levels are being excluded within or by the Carbon Source Material Supply System 110. In an additional embodiment, the carbon source material 100 is dried outside of the “pyrolysis reactor / zone 220” if the pyrolysis reactor does not include a drying zone 220.

[0278] In an additional embodiment, the dried carbon source material 100 enters a "preheat zone 210" where it is raised from a temperature range of about ambient to a temperature range of about 100°C to about 150°C to about 200°C. In an additional embodiment, the temperature does not exceed 200° C. in the "preheat zone 210." If the preheat zone is too hot or not hot enough, the dry carbon source material 100 may be processed in a non-ideal manner before entering the Pyrolysis Reactor / Zone 220. The "preheat zone 210" may include an output mechanism for capturing off-gases exhausted from the dry carbon source material 100 while it is being preheated and reusing them now or at a later date. In an additional embodiment, the off-gas can optionally be extracted for later use. In additional embodiments, the heating sources used for the various zones may be electric or gas. In additional embodiments, the heating source used for the various zones may be waste gas from other zones of the device or from an external source. In an additional embodiment, the heat may be indirect heat.

[0279] In this example, after processing in the Preheating Zone 210, the Carbon Source Material Supply System 110 transfers the preheated material to the Pyrolysis Reactor / Zone 220 where it undergoes the pyrolysis process. In additional embodiments, the Carbon Source Material Supply System 110 can penetrate the Pyrolysis Reactor / Zone 220 through a high temperature steam seal system (not shown), which may include, but is not limited to, an airlock (not shown). This allows the material delivery system to enter the hot Pyrolysis Reactor / Zone 220 while preventing and minimizing gas escape and oxygen ingress. In additional embodiments, the interior of the "pyrolysis reactor / zone 220" is heated to a temperature of about 100°C, about 200°C, about 300°C, about 400°C, about 500°C, about 600°C, about 700°C, about 800°C, about 900°C, about 1000°C, or about 1100°C, with about 800°C being preferred. In additional embodiments, the "pyrolysis reactor / zone 220" may include inlet and outlet ports similar to the "preheat zone 210" for capturing and venting gases released from the preheated carbon during carbonization of the carbon source feedstock 100. In an additional embodiment, the gas can optionally be extracted for later use at the operator's discretion. In an additional embodiment, the off-gas from the Preheat Zone 210 and the off-gas from the Pyrolysis Reactor / Zone 220 can be combined into a single gas stream. Once carbonized, the carbonized carbon source material 105 is discharged from the Pyrolysis Reactor / Zone 220 and then transferred to the Cooling and Washing Zone / Section 240.

[0280] In an additional embodiment, the raw carbon source material 100, and further dried carbon source material, preheated carbon source material, and / or activated carbon material having a hierarchical structure of predetermined pore structure 105, travels along a continuous carbon source material feed system 110 and through a pyrolysis reactor / zone 220. In additional embodiments, the Carbon Source Material Supply System 110 delivers different carbon source materials 100 at different stages in the process. In an additional embodiment, the process of moving material through the Pyrolysis Reactor / Zone 200 is a continuous process. In certain embodiments, the speed of the Carbon Source Material Supply System 110 can be appropriately calibrated, calculated, and controlled by an associated controller processor (not shown) so that operation of the Carbon Source Material Supply System 110 does not need to be interrupted as material moves through the device and the Pyrolysis Reactor / Zone 220. In certain embodiments, the "carbon source material supply system 110" may be operationally partitioned and may include multiple separate augers (not shown) and additional carbon material supply mechanisms, controlled by an associated controller and processor (not shown). Operation of the individual carbon material supply mechanisms of the "carbon source material supply system 110" can be implemented to control the rate at which the carbon source material 100 progresses between zones, stages, or reactors depending on the amount of time the carbon source material 100 remains in a particular zone, stage, or reactor of the device.

[0281] In additional embodiments, a controller (not shown) associated with one or more of the Pyrolysis Reactors / Zones 220 adjusts the rate of the Carbon Source Material Supply System 110 based on one or more feedback sensors, gases detected by an FTIR (optional), FTIR during the reaction, measured parameters, temperature gauges, the Pyrolysis Reactor / Zone 220, and other suitable variables during the reaction. In additional embodiments, suitable moisture, temperature and gas sensors in communication with the controller processor may be provided or mechanically connected within the Pyrolysis Reactor / Zone 220, between the zones and the Pyrolysis Reactor 220, or at any suitable location along the Carbon Source Material Supply System 110 or device. In additional embodiments, the controller processor can use information obtained from the sensor gauges to optimize the speed and efficiency of the device processing system. In an additional embodiment, a controller associated with one or more Pyrolysis Reactors / Zones 220 is configured to operate the Carbon Source Material Supply System 110.

[0282] In additional embodiments, a controller associated with one or more of the Pyrolysis Reactors / Zones 220 can monitor the concentration, temperature, and moisture of gases within the Carbon Source Material Supply System 110 and within the Pyrolysis Reactors / Zones 220. In additional embodiments, the controller may adjust the speed of the Carbon Source Material Supply System 110, the introduction of gas into the Carbon Source Material Supply System 110, and the heat applied to the material 100 in the Carbon Source Material Supply System 110 based on one or more readings obtained from various sensors.

[0283] In an additional embodiment, the device is enclosed in a kiln shell to control and manipulate the large amounts of heat required for the pyrolysis reactor / zone 220 process / reaction to occur. In additional embodiments, the kiln shell of the device may include several insulating chambers that enclose multiple zones. In certain embodiments, the furnace includes multiple separate zones for the devices. In additional embodiments, each zone of the device includes at least one inlet and at least one outlet. In additional embodiments, within each zone, inlets and outlets are configured to be adjustable to control the flow of carbon source material 100, gas flow, and heat flow into and out of the zone. An inert gas can be introduced into an inlet and the displaced air can be extracted through an outlet corresponding to that inlet. In additional embodiments, one or more outlets of a zone within the device are connected to one or more other inlets or outlets within the device.

[0284] In an additional embodiment, raw carbon source material 100 is deoxygenated in the "carbon source material supply system 110" before being introduced into the device (specifically the first zone, "drying and preheating zone 200a"). The "drying and preheating zone 200a" may have an entrance and an exit. In an additional embodiment, the "drying and preheating zone 200a" can be heated to a temperature of about 80°C to about 200°C to reduce water and other moisture from the carbon source material 100. The carbon source material 100 can then be moved to a preheating zone (which may be the same zone as the drying zone 200a) where the material 100 is preheated.

[0285] In additional embodiments, the optionally dried and preheated carbon source material 100 can then be transferred to a "pyrolysis reactor / zone 220" for carbonization. In certain embodiments, carbonization can occur at a temperature of from about 200°C to about 1100°C. For example, approximately 200°C, approximately 210°C, approximately 220°C, approximately 230°C, approximately 240°C, approximately 250°C, approximately 260°C, approximately 270°C, approximately 280°C, approximately 290°C, approximately 300°C, approximately 310°C, approximately 320°C, approximately 330°C, approximately 340°C, approximately 350°C, approximately 360°C, approximately 370°C, approximately 380°C, approximately 390°C, approximately 400°C, approximately 410°C, approximately 420°C, approximately 430°C, approx. 440°C, approx. 450°C, approx. 460°C, approx. 470°C, approx. 480°C, approx. 490°C, approx. 500°C, approx. 510°C, approx. 520°C, approx. 530°C, approx. 540°C, approx. 550°C, approx. 560°C, approx. 570°C, approx. 580°C, approx. 590°C, approx. 600°C, approx. 610°C, approx. 620°C, approx. 630°C, approx. 640°C, approx. 650°C, approx. 660°C, approx. 670°C, approx. 680°C, approx. 690°C, approx. 700°C, approx. 710°C, approx. 720°C, approx. 730°C, approx. 740°C, approx. 750°C, approx. 760°C, approx. 770°C, approx. 780°C, approx. 790°C, approx. 800°C, approx. 810°C, approx. 820°C, approx. 830°C, approx. 840°C, approx. 850°C, approx. 860°C, approx. 870°C, approx. 880°C, approx. 890°C, approx. 900°C, approx. 910°C, about 920°C, about 930°C, about 940°C, about 950°C, about 960°C, about 970°C, about 980°C, about 990°C, about 1000°C, about 1010°C, about 1020°C, about 1030°C, about 1040°C, about 1050°C, about 1060°C, about 1070°C, about 1080°C, about 1090°C, and about 1100°C, with about 800°C being preferred.

[0286] In an additional embodiment, the carbonization zone of the Pyrolysis Reactor / Zone 220 can extract the gases 122 produced during carbonization and store them for later use if desired. In an additional embodiment, the gases 122 produced during carbonization are extracted for current or later use. In additional embodiments, the carbonization temperature is selected and maintained to maximize the carbon content of the carbonized carbon source material 100 while reducing or eliminating the production of methane (CH4).

[0287] In additional embodiments, the "pyrolysis reactor / zone 220" may include at least one inlet port and multiple outlet ports. In additional embodiments, one of the outlet ports can be connected to further processing equipment such as a collector, an acid hydrogenation unit, a distillation column, etc. In an additional embodiment, the Pyrolysis Reactor / Zone 220 can process the off-gas coming from the Preheat Zone 210 and Pyrolysis Reactor / Zone 220 to produce a condensate or concentrated gas. In further embodiments, the condensate may include polar compounds, examples of which include, but are not limited to, acetic acid, methanol, and furfura. In additional embodiments, the enriched gas produced by the Pyrolysis Reactor / Zone 220 may include at least non-polar gases. In additional embodiments, the "pyrolysis reactor / zone 220" for the gas may include a fractionation column. In additional embodiments, the acetic acid can be transported via a line or channel to an acid hydrogenation unit (optional). In additional embodiments, the methanol-furfural can be transported to the distillation and processing unit via an optional additional line channel.

[0288] In an additional embodiment, the carbon recovery unit may also include an inlet connected to the Pyrolysis Reactor / Zone 220. In additional embodiments, the gas extracted from the carbon recovery unit is optionally used in an energy recovery system or carbon concentration system. Additionally, in various embodiments, gases may be exhausted from one or more zones of the device and optionally used in an energy recovery system or system for further carbon processing.

[0289] High oxygen levels in the ambient air surrounding the feedstock 100 during processing can result in combustion and oxidation of the feedstock 100, dramatically reducing the quantity and quality of the final activated carbon material 105. In an additional embodiment, the Carbon Source Material Supply System 110 may remove oxygen within the Pyrolysis Reactor / Zone 220, which may include one or more manifolds that exclude oxygen from the air surrounding the raw carbon source material 100. In additional embodiments, oxygen levels of about 0.5% to about 1.0% can be used for preheating, pyrolysis, carbonization, and cooling. The closed Carbon Source Material Supply System 110 is designed to reduce oxygen levels to about 3% or less, about 2% or less, about 1% or less, or about 0.5% throughout the process. As the oxygen level drops, the carbon source material 100 is transported along a "carbon source material supply system 110" within the device. In an additional embodiment, the inert gas is preheated through the recovery process and then introduced into the device reactor and trimming reactor, improving system efficiency and reducing energy consumption.

[0290] In additional embodiments, a trimming reactor (not shown) may be included in the system. In an additional embodiment having a trimming reactor (not shown), the pyrolyzed material from the device can be fed to another additional reactor (not shown) for further pyrolysis, where heated inert gas can be introduced to produce a product with stable high carbon levels. In additional embodiments, this secondary processing can occur in a container such as, but not limited to, a drum, tank, barrel, bin, tote, pipe, sack, press, or roll-off container. In an additional embodiment, a final container can be used for transport of the carbonized source material 105. In an additional embodiment, the inert gas can be heated via a heat exchanger (not shown) that can obtain heat from gases extracted from the device and can be combusted in a process gas heater.

[0291] In an additional embodiment, the heat, steam, and gases recovered from the Pyrolysis Reactor / Zone 220 are sent to the Carbon Source Material Supply System 110, where they are enclosed within a jacket or isolated from direct contact with the carbon source material 100 and used to indirectly heat the carbon source material 100 prior to introduction into the Pyrolysis Reactor / Zone 220 or drying zone.

[0292] In an alternative embodiment, the heat, steam, and gases recovered from the Drying Zones 200a and 200b and the Pyrolysis Reactor / Zone 220 are sent to the Carbon Source Material Supply System 110 where they are jacketed or otherwise isolated from direct contact with the carbon source material 100. This may indirectly heat the feed material 100 before it is introduced into the Pyrolysis Reactor / Zone 220 .

[0293] In this embodiment, the "activated carbon material supply system 120" supplies activated carbon material 105 to a third zone (cooling and washing reactor) 230 (optional) for cooling and washing. The "cooling and cleaning reactor 230" may contain additives such as HCl. Gas is discharged from the first zone, "preheat zone 210," through line 160.

[0294] In this example, as the hierarchical activated carbon product 105 of a given pore structure enters the "cooling and washing zone / section 240," the material is cooled (actively or passively) to a specified temperature. In an additional embodiment, the temperature of the activated carbon 105 of a given pore structure is reduced in a "cooling and washing zone / section 240" within an inert atmosphere. In an additional embodiment, the "cooling and washing zone / section 240" is a mechanical mechanism that can "water-cool activated carbon material 105 having a hierarchical structure of a predetermined pore structure" and contains "an additive such as HCl" that soaks the material for a specified / extended period of time. The predetermined pore structure carbon material 105 may be cooled in a "cooling and washing zone / section 240." In the "Cooling and Cleaning Zone / Section 240", the temperature reaches a level where it will not spontaneously ignite even when exposed to normal air or air containing oxygen. In additional embodiments, the "cooling and washing zone / section 240" reduces the temperature of the carbon source material to between 200°C and about 150°C and below about 100°C. In this embodiment, the device may include an optional mixing system for mixing the activated carbon material 105, the coolant, and the additives, thereby allowing for uniform cooling of the carbon source material. Additionally, cooling can be by direct or indirect means, and may involve the use of water, other liquids, or additives. Furthermore, the cooling process can be performed by direct means, indirect means using air or other gases, or a combination of both.

[0295] In certain embodiments, the cooling mechanism is separate from the Pyrolysis Reactor / Zone 220 and can be mechanically connected to the Activated Carbon Material Supply System 120 . In an additional embodiment, the cooling mechanism is located after the Pyrolysis Reactor / Zone 220. In additional embodiments, the cooling mechanism may be the same mechanism as the Pyrolysis Reactor / Zone 220 or may be incorporated into the Pyrolysis Reactor / Zone 220. In additional embodiments, the cooling mechanism is a non-limiting example of a screw, auger, a conveyor, particularly a belt conveyor, and in certain embodiments, a drum, a screen, a pan, a countercurrent bed, a vertical tower, a jacketed paddle, a cooled screw, combinations thereof, direct or indirect means, water, other liquids, additives, gas, direct or indirect means, or any combination of the above. In additional embodiments, the cooling mechanism may include a water spray mechanism, an inlet port (with or without additives), a cooled inert gas flow mechanism, an outlet port which may be liquid nitrogen or atmospheric air (or air if below ignition or flammable temperatures). In additional embodiments, heat can be recovered during this process, for example by capturing the flash steam generated by the water spray and the superheated steam generated when saturated steam is introduced, and then heating it with activated carbon material 105.

[0296] In an additional embodiment, the carbonized activated carbon material 105 of predetermined pore structure can be transported to a "cooling and washing zone / section 240" where it is passively or actively cooled. In additional embodiments, the "hierarchically structured activated carbon material 105 of predetermined pore structure" can be cooled to a temperature of about 10°C, about 20°C, about 30°C, or about 40°C. In an additional embodiment, the activated carbon material 105 having a hierarchical structure of predetermined pore structure is moved to a "cooling and washing zone / section 240" where it is simultaneously cooled and washed to remove additives, specifically bases such as KOH. In an additional embodiment, the carbonized activated carbon material 105 of predetermined pore structure is transferred to a "cooling and washing zone / section 240" where it is cooled and simultaneously "washed with additives such as water and HCl."

[0297] In this embodiment, when activated carbon material 105 having a hierarchical structure with a predetermined pore structure enters the "cooling and washing zone / section 240", the carbonized material 105 is allowed to cool to a predetermined temperature range of approximately 20°C to 30°C, which is normal room temperature. In additional embodiments, the device includes multiple "cooling and washing zones / sections 240." In an additional embodiment, the "cooling and washing zone / section 240" can cool the carbonized material 105 to below 200°C. In an additional embodiment, the "cooling and washing zone / section 240" may include a mixer auger to agitate the carbonized material 105 to uniformly cool and wash it. In additional embodiments, one or more of the multiple "cooling and washing zones / sections 240" may be external to the device.

[0298] In an additional embodiment, the activated carbon material 105 having a hierarchical structure of predetermined pore structure is conveyed from the Cooling and Washing Zone / Section 240 along the Activated Carbon Material Supply System 120 and then transported to a carbon recovery unit (not shown).

[0299] In an additional embodiment, the activated carbon material 105 having a hierarchical structure of predetermined pore structures can be transported along the activated carbon material supply system 120, exiting the cooling and washing zone / section 240, and then to the electrode mixing system / zone 401.

[0300] In this example, gas exits the second zone (pyrolysis reactor) 220 through line 160 . A second line 160 connected to a single line 161 exhausts the gas passing through the line 160 . The gas is discharged through a connected line 161 to a "phase separator 250." Polar compounds 128 are captured from the exhaust gas and, if desired, used immediately for heat and energy recovery or stored for later use. Acetic acid is transferred from Phase Separator 250 to Acid Hydrogenation Unit 280 via line 160. Acetic acid is converted into ethanol 127.

[0301] In another embodiment, the "cooling and scrubbing zone / section 240" can be associated with a gas introduction probe and a gas extraction probe. In additional embodiments, a gas introduction probe can introduce nitrogen, argon, or helium into the cooling and scrubbing zone / section 240, and a gas extraction probe can extract gas from the cooling and scrubbing zone / section 240. In various embodiments, a gas introduction probe can introduce a mixture of gases into the "cooling and scrubbing zone / section 240." In various embodiments, a gas extraction probe extracts gas from the "cooling and scrubbing zone / section 240" for reuse in a heat and energy recovery system.

[0302] In certain embodiments, the gas introduction probe and gas extraction probe can operate in conjunction with a controller and multiple sensors to regulate the level and concentration of gas introduced to and extracted from each device zone.

[0303] In certain embodiments, the gas introduction probe and gas extraction probe may be made of suitable piping and made to withstand high temperature fluctuations. In certain embodiments, the gas introduction probe and gas extraction probe may include multiple openings for introducing and extracting gas. In certain embodiments, multiple openings can be located on the underside of the inlet and gas extraction probe. In an additional embodiment, each of the plurality of openings extends through a respective zone.

[0304] In additional embodiments, a gas introduction probe may extend from one side of the device through each zone. In certain such embodiments, each gas introduction probe can extend from one side of the device to each zone of the device. In an additional embodiment, a gaseous catalyst can be added to increase the fixed carbon level. In certain such embodiments, the multiple openings for each gas introduction probe may be located only in each zone associated with that particular gas introduction probe.

[0305] In certain embodiments, each gas introduction probe can extend from the left side of the base "soak and mix zone 190" to one each zone, in this example the gas introduction probes extend through the device to or through the device. Therefore, the introduction probe may terminate at the base "Soaking and Mixing Zone 190", "Drying and Preheating Zone 200a", "Preheating Zone 210", "Pyrolysis Reactor / Zone 220", "Cooling and Washing Zone / Section 240", "Drying Zone 200b", "Electrode Mixing System / Zone 401", specific zones, all zones, selected zones, etc.

[0306] In certain embodiments, the gas introduction probe may include a preheat zone gas introduction probe that passes through the "preheat zone 210" and terminates in the "drying and preheat zone 200a." In certain such embodiments, the remaining gas introduction probes may extend through the Pyrolysis Reactor / Zone 220, with the pyrolysis zone gas introduction probes terminating within the Pyrolysis Reactor / Zone 220. In additional embodiments, the gas extraction probe can be configured similarly to the gas introduction probe. In additional embodiments, the gas introduction probe and gas extraction probe may originate from either side of the device.

[0307] In certain embodiments, the gas introduction probes can be arranged concentrically to conserve available space in a multi-port configuration. In the above embodiment, each inlet probe / port may have a smaller diameter than the previous inlet probe / port. For example, in the above embodiment, the gas introduction probe in the base "soaking and mixing zone 190" can have the largest inner diameter, so the gas introduction probes in the "preheating zone 210" and "drying zone 200a" are positioned within the inner diameter of the gas introduction probe in the base "soaking and mixing zone 190." Additionally, the gas inlet probe of the "pyrolysis reactor / zone 220" is positioned within the inner diameter of the gas inlet probe of the preheating and drying zone. Also, the gas introduction probe of the "cooling and cleaning zone / section 240" is disposed within the gas introduction probe 159 of the "pyrolysis reactor / zone 220". The gas introduction probe of the "drying zone 200b" is disposed within the "cooling and washing zone / section 240." The gas introduction probe of the electrode mixing system zone 401 is disposed in the gas introduction probe in the "drying and preheating zone 200a." In the above embodiment, suitable connectors can be attached to each gas introduction probe external to the device to allow for individual or cooperative control of the air injected into each gas introduction probe.

[0308] In certain embodiments, a concentric or near-concentric arrangement may be preferred, with the outermost gas introduction probes exposed in each zone before being terminated. Thus, in the above embodiment, the individual introductions to the gas zones can be controlled independently of each other, requiring only a single continuous gas introduction probe line. Similar concentric or near-concentric configurations can be applied to the gas extraction probe.

[0309] In this embodiment, the "cooled and washed activated carbon material 106" is supplied to the "activated carbon recovery unit 300" via the "activated carbon material supply system 120". The activated carbon product 350 produced in the "Predetermined Pore Structure Hierarchical Activated Carbon Production System / Zone 380" is removed from the "Activated Carbon Recovery Unit 300." Optionally, energy 310 is recovered by an Activated Carbon Recovery Unit 300.

[0310] In this embodiment, the cooled / washed activated carbon material 106 is produced in a "predetermined pore structure hierarchical activated carbon production system / zone 380" by an "activated carbon material supply system 120" and fed into an "electrode mixing system / zone 401" within an "energy storage device production system 390." Additional electrode materials and the hierarchically structured activated carbon material 105-106 of predetermined pore structure are mixed together in an electrode mixing system / zone 401 to form an electrode composite mix.

[0311] The "activated carbon material 105 having a hierarchical structure of a predetermined pore structure" may be in a powder state at this point, or may be pulverized to form a fine powder. The grinding or pulverization can be performed within the electrode mixing system / zone 401 or in a separate milling device. In certain embodiments, grinding and pulverization can be performed before activation or after activation of the carbon.

[0312] In this embodiment, the electrode mix can be made by mixing activated carbon with electrode components in one or more mixing chambers. Non-limiting examples of "electrode ingredients" include "conductive additives, binders, admixtures," and the like. Non-limiting examples of conductive additives include carbon black, super p, furnace black, channel black, acetylene black, thermal black, ion black, and conductive carbon. Non-limiting examples of "binders" include PVDF, PTFE, non-reactive thermoplastic fluoropolymers, copolymers, and terpolymers. Non-limiting examples of "mixtures" include 2-propanol·sec-propyl alcohol·IPA·isopropyl·isopropanol·alcohol·water. Non-limiting examples of electrode compositions may be in the form of an admixture, paint, mixture, paste, ink, or free-standing electrode.

[0313] In this example, the "electrode mixture 107" is supplied to the "electrode preparation system / zone 400." The electrodes 108 are prepared in the "electrode preparation system / zone 400."

[0314] In certain embodiments, the "electrode mixing system / zone 401" can be interconnected or mechanically connected to an "electrode preparation system / zone 400" having one or more extruders / sprayers for introducing the electrode mixture. In yet another embodiment, the Electrode Preparation System / Zone 400 can form a freestanding electrode that is formed, pressed, applied, and then attached to a current collector. The electrode mixture composition can be applied, pressed, and contacted to an "electrically conductive current collector material" such as: Possible metals for the "conductive current collector material" include stainless steel, titanium, copper, aluminum, and silver, which may be thin films or meshes, and which come in thicknesses ranging from 0.0001mm to 10mm, with a variety of mesh patterns and windings. Additionally, the electrode mix and freestanding electrodes can be of various thicknesses ranging from 0.0001 mm to 10 mm. たとえば、about 0.05mm·about 0.1mm·about 0.15mm·about 0.2mm·about 0.25mm·about 0.3mm·about 0.35mm·about 0.4mm·about 0.45mm·about 0.5mm·about 0.55mm·about 0.6mm·about 0.65mm·about 0.7mm·about 0.75mm·about 0.8mm·about 0.85mm·about 0.9mm·about 0.95mm·about 1.0mm·about 1 .25mm·about 1.5mm·about 1.75mm·about 2.0mm·about 2.25mm·about 2.5mm·about 2.75mm·about 3.0mm·about 3.25mm·about 3.5mm·about 3.75mm·about 4.0mm·about 4.25mm·about 4.5mm·about 4.75mm·about 5.0mm·about 6.0mm·about 7.0mm·about 8.0mm·about 9.0mm·about 10.0mmである。 また, about 1mg / cm 2 About 1.25 mg / cm 2 About 15mg / cm 2 About 1.75 mg / cm 2 About 2 mg / cm 2 About 2.25 mg / cm 2 About 2.5 mg / cm 2 About 2.75 mg / cm 2 About 3mg / cm 2 About 3.25 mg / cm 2 About 3.5 mg / cm 2 About 3.75 mg / cm 2 About 4 mg / cm 2 About 4.25 mg / cm 2 About 4.5 mg / cm 2 About 4.75 mg / cm 2 About 5mg / cm 2 About 5.25 mg / cm 2 About 5.5 mg / cm 2 About 5.75 mg / cm 2 About 6 mg / cm 2 About 6.25 mg / cm 2 About 6.5 mg / cm 2 About 6.75 mg / cm 2 About 7 mg / cm 2 About 7.25 mg / cm 2 About 7.5 mg / cm 2 About 7.75 mg / cm 2 About 8mg / cm 2About 8.25 mg / cm 2 About 8.5 mg / cm 2 About 8.75 mg / cm 2 About 9 mg / cm 2 About 9.25 mg / cm 2 About 9.5 mg / cm 2 About 9.75 mg / cm 2 About 10mg / cm 2 About 1025mg / cm 2 About 10.5 mg / cm 2 About 10.75 mg / cm 2 About 11 mg / cm 2 About 11.25 mg / cm 2 About 115mg / cm 2 About 11.75 mg / cm 2 About 12 mg / cm 2 About 12.25 mg / cm 2 About 12.5 mg / cm 2 About 12.75 mg / cm 2 About 13 mg / cm 2 About 13.25 mg / cm 2 About 13.5 mg / cm 2 About 13.75 mg / cm 2 About 14 mg / cm 2 About 14.25 mg / cm 2 About 14.5 mg / cm 2 About 14.75 mg / cm 2 About 15mg / cm 2 About 16 mg / cm 2 About 17 mg / cm 2 About 18 mg / cm 2 About 19 mg / cm 2 About 20mg / cm 2 About 21 mg / cm 2 About 22 mg / cm 2 About 23 mg / cm 2 About 24 mg / cm 2 About 25mg / cm 2 About 30mg / cm 2 About 35mg / cm 2 About 40mg / cm 2 About 45mg / cm 2 About 50mg / cm 2and "approximately 3.6 to 10.5 mg / cm 2 " is preferred.

[0315] In additional embodiments, the "electrode preparation system / zone 400" comprises or is mechanically connected to an applicator system for administering the electrode composition mixture and freestanding electrodes. Non-limiting examples of applicator systems include nozzles, sprayers, scrapers, and presses. A free-standing electrode is a free-standing structure that can be applied directly to a metal and that can make direct contact with the metal. In additional embodiments, the "electrode preparation system / zone 400" further includes mechanical pumps, compressors, gravity feeds, presses, augers, and pressures to provide a constant supply of electrode admixture composition.

[0316] In an additional embodiment, the device may include an analyzer to determine the ionic size of the electrolyte and the ideal pore width and pore distribution of the final hierarchical structured activated carbon pores prior to initiation of the process. In an additional embodiment, the device may perform a process to determine the ideal pore width and pore distribution desired for the pores of the final hierarchically structured activated carbon prior to initiating or during the process.

[0317] In additional embodiments, the Electrode Preparation System / Zone 400 may include an electrode mix feed system 406, which may further include a mechanical feed system and a Device Winding and Stacking System 411. Additionally, in certain embodiments, the "electrode preparation system / zone 400" can include a feeder, a winder, a roller drum, a cutter, a crimper, a drive mechanism or motor, a connecting belt, gears, a direct connection, tensioners for the anode material, the cathode material, and the ion-permeable separator, an electrode mix injector, an electrode applicator, an electrode mix overflow system, an "electrode drying system / zone 420," an "electrolyte zone / system including the electrolyte mixing system 431 and storage tank," an electrolyte conduit, and an electrolyte injector. Additionally, the “electrode preparation system / zone 400 ” may include a “bonding and sealing system / zone 450 ” having a welder-sealer-crimper-press-seal that forms part of the energy storage device manufacturing system 500 . Also, in alternative embodiments, the "electrode preparation system / zone 400" can be mechanically connected to or separated from the energy storage device manufacturing system 500. In an additional embodiment, the energy storage device manufacturing system 500 may further include an “energy storage device hopper” for storing the energy storage devices 460 to accommodate the energy storage devices 460 .

[0318] In an additional embodiment, a continuous supply of conductive metal can be provided by the Electrode Preparation System / Zone 400. In an additional embodiment, the Electrode Preparation System / Zone 400 can provide a continuous supply of conductive metal coated electrode mixes, inks, paints, pastes, and compositions. In an additional embodiment, the Electrode Preparation System / Zone 400 can provide a continuous supply of electrode mixture to form a free-standing electrode.

[0319] In additional embodiments, an "electrode preparation system / zone 400" can be used to provide a continuous supply of "conductive metal" for securing and assembling the "contact between the conductive metal and the freestanding electrode or electrode mixture," and can further include an additional drying process or moisture removal. In an additional embodiment, an "Electrode Preparation System / Zone 400" can be used for a continuous supply of ion-permeable separators or separators. In an additional embodiment, an "electrode preparation system / zone 400" can be used to provide a continuous supply of conductive metals, electrode admixture compositions, and ion-permeable separators for layering. In an additional embodiment, the "electrode preparation system / zone 400" can be used to layer energy storage devices. In additional embodiments, the "electrode preparation system / zone 400" can be used to layer an energy storage device having the following layer structure: Two conductive metal current collectors with an electrode mixture applied to opposite sides. Two conductive metal current collectors with opposing sides in contact with free-standing electrodes. Two ion-permeable separators positioned between the two coated conductive metal current collectors and the electrode composite. In an additional embodiment, the Electrode Preparation System / Zone 400 allows for the fabrication of a double layer electrolytic capacitor 460 . In an additional embodiment, the Electrode Preparation System / Zone 400 allows for the fabrication of a supercapacitor 460 . In an additional embodiment, the Electrode Preparation System / Zone 400 can create an energy storage device 460 .

[0320] In this example, the electrode 108 is fed to an "electrode drying system / zone 420" (optional) or alternatively to a "device winding and laminating system 411" where it is rolled into a thin film.

[0321] In additional embodiments, the "electrode preparation system / zone 400" may be configured to produce a continuously wound or stacked (anode-ion permeable separator-cathode) energy storage device 460 or supercapacitor cell 460. In an additional embodiment, the "electrode preparation system / zone 400" can provide a layered structure in which multiple anodes, multiple ion-permeable separators, and multiple cathodes are stacked or grouped for each cell. Additionally, in certain embodiments, a stacked, laminated, or wound energy storage device may have a "lead connected to an anode" and may also have a "lead connected to a cathode." In certain embodiments, the anode and cathode leads can be connected to terminals of the energy storage device 460 that protrude from the energy storage device 460.

[0322] In certain embodiments, "ion-permeable separator" can include, but is not limited to, porous "plastic," paper, "cellulose," fiber, glass, and ion-permeable insulators / separators.

[0323] In this example, the prepared electrodes 109 are fed into an "electrolyte input system / zone 430." The completed energy storage device actuation mechanism 109 is placed into the energy storage device container.

[0324] In additional embodiments, the Electrode Preparation System / Zone 400 may further include mechanical feeding units or feeders for the supercapacitor containers or shells. A mechanical feeding unit or feeder may be mechanically connected to the device. Additionally, mechanical feeding units or feeders are used to facilitate the insertion and removal of supercapacitor containers (new or partially completed containers containing supercapacitor material) at regular or predetermined intervals.

[0325] In additional embodiments, the "electrode preparation system / zone 400" may include a mechanical feeding unit or feeder for placing the "contents" (energy storage material or supercapacitor material) inside the energy storage device layered or wound within the energy storage container.

[0326] In this embodiment, an electrolyte 435 supplied from an "electrolyte mixing system 431" is introduced into an "electrolyte introduction system / zone 430."

[0327] In additional embodiments, the "electrode preparation system / zone 400" may be mechanically connected to one or more electrolyte injectors and may further include spray nozzles. In an additional embodiment, the "electrode preparation system / zone 400" dispenses or injects electrolyte into an energy storage container containing energy storage or supercapacitor materials. The electrolyte may be an organic electrolyte, an aqueous electrolyte, a co-solvent, a salt electrolyte, an ion carrier electrolyte, an ionic electrolyte, a gel electrolyte, a dry polymer electrolyte, or a ceramic electrolyte, with a "co-solvent in a salt electrolyte" being preferred.

[0328] In additional embodiments, the "electrode preparation system / zone 400" may include a mechanical feeding unit or feeder for placing the "contents" (energy storage material or supercapacitor material) inside the layered or wound energy storage device into the energy storage container. In additional embodiments, the "electrode preparation system / zone 400" may be mechanically connected to one or more electrolyte injectors 433 and may further include a spray nozzle. In an additional embodiment, the "electrode preparation system / zone 400" can inject / inject (433) electrolyte into an energy storage container containing energy storage / supercapacitor materials. The "electrolyte" includes organic electrolytes, aqueous electrolytes, co-solvents, salt electrolytes, ion carrier electrolytes, ionic electrolytes, gel electrolytes, dry polymer electrolytes, and ceramic electrolytes, with "co-solvents in salt electrolytes" being preferred.

[0329] In this embodiment, the "electrode preparation system / zone 400" allows the electrolyte to be injected (433) and injected into the energy storage device in a general atmospheric environment. In this example, the Electrode Preparation System / Zone 400 injects electrolyte into the Energy Storage Device (433) in a typical atmospheric environment. In this example, the "electrode preparation system / zone 400" injects / injects electrolyte into the "supercapacitor" (433) in a general atmospheric environment.

[0330] The "electrode preparation system / zone 400" of this embodiment may also include a mechanical supply unit or feeder for the energy storage containers containing the energy storage material and electrolyte. In this embodiment, the "electrode preparation system / zone 400" is mechanically connected to a container sealing device, which may include a crimper, a screw, a rivet, a clamp, a press, a weld, or a seal. Welder 451 connects or attaches the anode and cathode leads to the positive and negative terminals of the energy storage device and encapsulates and seals energy storage device 460 . In this embodiment, the "electrode preparation system / zone 400" may comprise a sealing device and may include a sealing means for the container with or without a separate sealing component.

[0331] Also in this embodiment, the Electrode Preparation System / Zone 400 may have a means to control the internal energy storage pressure, for example, for vacuum. In certain embodiments, the "electrode preparation system / zone 400" may include a vacuum pump to reduce the internal pressure of the energy storage device.

[0332] In this embodiment, the "electrode preparation system / zone 400" may include an "energy storage cell hopper 462" for storing the manufactured energy storage devices 460 or supercapacitor cells 460.

[0333] In this embodiment, the "electrode preparation system / zone 400" may include a controller / processor (not shown) that controls the operation and parameters of the "electrode preparation system / zone 400." In additional embodiments, the controller processor can be configured to regulate the speed and control of a number of systems, including the following non-limiting examples: For example, anode metal feed, cathode metal feed, ion permeable separator feed, electrode mixing, electrode material feed system 406, electrode mix applicator 408, electrode mix measurement, electrode mix recirculation system 409, electrode drying 420, rollers 412a and 412b, tensioners 413a and 413b, winding speed, winding length, stacking speed, stacking length, motor 414, drive system 415, container loading, container transport, container movement, liquid electrolyte mixing 431, liquid electrolyte injection 432 and 433, liquid electrolyte measurement, anode and cathode connection, anode and cathode terminal connection, attachment 450, container sealing 451, container crimping, container closure, vacuum control, energy storage device assembly 460, supercapacitor assembly 460, and hopper storage and control 462. The controller can be based on one or more inputs, sensors, feedback sensors, measurement parameters, measurements, timers, timed processes, thermometers, or other suitable assembly parameters. In additional embodiments, suitable moisture, temperature, and gas sensors in communication with the controller processor may be provided or mechanically connected within and between each zone at any suitable location within or along the energy storage device manufacturing system 500. In additional embodiments, the controller processor can optimize the speed and efficiency of devices, processing systems, machine parts, feeding systems, mixing systems, assembly systems, and materials based on information obtained from sensors and gauges. This is based on one or more readings taken by various sensors.

[0334] Also in this embodiment, the Electrode Preparation System / Zone 400 may have a means to control the internal energy storage pressure, for example, for vacuum. In certain embodiments, the Electrode Preparation System / Zone 400 may include a vacuum pump to reduce the internal pressure.

[0335] FIG. 17 is a functional block diagram of this embodiment of the invention, including a continuous carbon source material supply system 110, with multiple reactors, multiple zones, and a hierarchical activated carbon production system / zone 380 with a predetermined pore structure. The device configuration in this embodiment includes a mechanically coupled or operatively associated "energy storage device manufacturing system 390." The "energy storage device manufacturing system 390" includes an "electrode preparation system / zone 400" and is in operative communication with the "predetermined pore structure hierarchical activated carbon manufacturing system / zone 380." Here, the present invention can be achieved by a series of steps or alternative steps including:

[0336] In this example, the improved "hierarchical activated carbon with a predetermined pore structure" and "finished energy storage device" have the following: A process for determining the desired pore width and hierarchical structure of the final activated carbon in order to control a device-controllable system that produces the desired result product. Optional Carbon Source Drying Step 200a. Feeding the carbon source material 100 into an optional "sizing and grinding system 180." A process of pulverizing a carbon material 100 to produce a pulverized carbon source material 101. The process of feeding a carbon source material 100 to a chemical base soak tank / system 190, or feeding a pulverized carbon material 101 to a chemical base soak tank / system 190, or feeding a pulverized carbon material 101 to any chemical base soak tank / system 190. A process 110 in which the carbon source material 100 or ground carbon source material 101 is soaked in a basic chemical or aqueous solution to produce a "base-soaked carbon source material 102." A process of supplying a carbon source material 100 by the "carbon source material supply system 110", a process of supplying a pulverized carbon material 101 to the "drying and preheating zone 200a" (optional), or a process of supplying a base-soaked carbon material 102 to the "drying and preheating zone 200a" (optional) by the "carbon source material supply system 110". Drying the base-soaked carbon source material 102 or carbon source material 100 in a drying system / reactor 200 (optional). The process of removing chemicals such as water 126 and base from the base-soaked carbon source material 102. A process for producing a dry carbon source material 103. The process of recovering and reusing heat using the "Heat Recovery System 310." Feeding dry carbon source material 103 to a first zone (preheat reactor) 210 (optional) by a "carbon source material feeding system 110." Preheating the dried carbonaceous material 103 in a first zone (preheat reactor) 210 to produce a preheated carbonaceous material 104. The process of discharging the water 126 and gas through line 160. feeding the preheated carbon material 104 by the "carbon source material feeding system 110" into a second zone (pyrolysis reactor) 220 (optional) to undergo pyrolysis. In a "second zone (pyrolysis reactor) 220," preheated material 104 undergoes pyrolysis or dry carbon source material 103 undergoes pyrolysis to "produce activated carbon material 105 having a hierarchical structure of predetermined pore structure." Monitoring the second zone (pyrolysis reactor) 220 by FTIR 290 (optional). feeding activated carbon material 105 to a third zone (cooling and washing reactor) 230 (optional) by the "activated carbon material feeding system 120" for cooling and washing. Discharging gas from the first preheat zone (reactor) 210 via line 160. Discharging gas from the second zone (pyrolysis reactor) 220 via line 160. Discharging the gas from the second line 160 via line 160, which may be combined into a single line 161. Discharging the gas to "phase separator 250" via combined line 161. The process of capturing polar compounds 128 from exhaust gases, which can be immediately used for heat and energy recovery, if desired, or stored for later use. Transferring acetic acid from the phase separator 250 via line 160 to an acid hydrogenation unit 280. Process for converting acetic acid to ethanol 127 (Optional). The cooled and washed activated carbon material 106 is supplied to the activated carbon recovery unit 300 via the activated carbon material supply system 120. Optionally, removing the final activated carbon product 350 produced in the Predetermined Pore Structure Hierarchical Activated Carbon Production System / Zone 380 from the Activated Carbon Recovery Unit 300. Optionally, recovering energy 310 using an "activated carbon recovery unit 300." A process in which the "activated carbon material supply system 120" supplies the "cooled and washed activated carbon material 106" produced in the "hierarchical structure activated carbon production system with a predetermined pore structure / zone 380" to the "electrode mixing system / zone 401" in the "energy storage device production system 390." A process of mixing the added electrode components and the "activated carbon material 105-106 having a hierarchical structure of a predetermined pore structure" together in the "electrode mixing system / zone 401" to form an "electrode composite mixture." The process of supplying "electrode composite admixture 107" to "electrode preparation system / zone 400." The process of preparing the electrode 108 in the "electrode preparation system / zone 400." Feeding the electrodes 108 to an "electrode drying system / zone 420" (optional) or alternatively feeding the electrodes to a "device winding and stacking system 411" that includes an ion-permeable separator. feeding the prepared electrode 109 into an "electrolyte input system / zone 430." The process of placing the completed energy storage device actuation mechanism 109 into an "energy storage device container." A process 435 of feeding electrolyte supplied from the "electrolyte mixing system 431" into the "electrolyte feeding system / zone 430". The process of sealing or encapsulating the "completed energy storage device assembly 461" within the "attachment and sealing system / zone 450." Optionally, introducing a vacuum into the sealed energy storage device assembly 461 or, alternatively, producing a completed energy storage device 460.

[0337] In the embodiment of FIG. 17, the improved "activated carbon having a hierarchical structure of a predetermined pore structure" and "finished energy storage device" comprises:

[0338] In this example, the carbon source material 100 is fed into a "sizing and grinding system 180" (optional). In this embodiment, the closed "carbon source material supply system 110" includes a "material supply hopper (not shown)", a "material transfer mechanical system 110", a deoxygenation manifold, and a mechanical system (not shown).

[0339] In this embodiment, the material feed hopper may be any suitable open or closed atmosphere container configured to receive the carbon source material 100 . The material feed hopper may be mechanically connected or operatively linked to a "carbon source material feed system 110." In certain embodiments, the "carbon source material supply system 110" may be a screw and auger system that is rotated by a non-limiting example of a drive source, such as a motor or other mechanically operable device (not shown).

[0340] In an additional embodiment, the carbon source material 100 can be fed into a "carbon source material feeding system 110," which can be accomplished with a gravity feed system. In certain embodiments, the Carbon Source Material Supply System 110 can be configured to provide a screw auger within a suitable enclosure. In an additional embodiment, the enclosure may be generally cylindrical. In additional embodiments, the "carbon-source material supply system 110" can include screws, augers, conveyors, drums, screens, chutes, drop chambers, pneumatic conveying devices, and may also include rotary airlocks, double flap airlocks, and triple flap airlocks (not shown).

[0341] In certain embodiments, the carbon source material 100 is fed into the "carbon source material feed system 110" from a carbon source material feed hopper, and the rotation of the auger screw moves the raw carbon source material 100 towards the deoxygenation manifold. When the carbon source material 100 reaches the deoxygenation manifold, the air surrounding the raw carbon source material 100 in the Carbon Source Material Supply System 110 may contain approximately 21% oxygen. In additional embodiments, the deoxygenation manifold may be located adjacent to or around the Carbon Source Material Supply System 110. In certain embodiments, the deoxygenation manifold or "container of the carbon source material supply system 110" can include multiple gas inlet ports and multiple gas outlet ports.

[0342] In certain embodiments, the deoxygenation manifold can have "at least one gas inlet line and at least one gas outlet line." In an additional embodiment, at least one gas inlet line of the deoxygenation manifold can be in operable communication with and mechanically connected to each of the plurality of gas inlet ports. In an additional embodiment, at least one gas outlet line of the deoxygenation manifold can be in operable communication with and mechanically connected to each of the plurality of gas outlet ports. In certain embodiments, the gas inlet line delivers an "inert gas" to the gas inlet port. In a particular embodiment, the inert gas is substantially oxygen-free and is "nitrogen, argon, or helium." In an additional embodiment, the inert gas is introduced countercurrently to the carbon source material.

[0343] In certain embodiments, the introduction of an inert gas into the sealed Carbon Source Material Supply System 110 may be performed to exclude ambient air from the sealed system. In certain embodiments, during operation of the Carbon Source Material Supply System 110, when an inert gas is introduced into the first gas inlet port, a volume of oxygen-enriched ambient air is forced out the outlet port. At this point, the desired oxygen level of about 2% or less, about 1% or less, about 0.5% or less, about 0.2% or less, or about 0.1% or less may not be achieved.

[0344] In an addition...

Claims

1. 1. A method for producing a low-cost activated carbon having a majority of pores less than 2 nm for use with a hybrid electrolyte comprising water, acetonitrile and sodium perchlorate salt in a device for storing electrical energy, the method comprising the steps of: The activated carbon is a plurality of pores having micropores with a micropore diameter of less than 2 nm, mesopores with a mesopore diameter in the range of 2 nm to 50 nm, and macropores with a macropore diameter of greater than 50 nm; The method comprises: (a) selecting the hybrid electrolyte comprising water, acetonitrile, and sodium perchlorate salt from the group consisting of: (i) a first electrolyte having a first average size of solvated ions of 1 nm or less; (ii) a second electrolyte having a second average size of solvated ions greater than 1 nm; (b) selecting an activation temperature and an activation time as follows: (iii) If the first electrolyte is selected, the activation temperature ranges from 650 degrees Celsius to 850 degrees Celsius, and the activation time ranges from 30 minutes to 4 hours. (iv) If the second electrolyte is selected, the activation temperature ranges from 750 degrees Celsius to 950 degrees Celsius, and the activation time ranges from 30 minutes to 5 hours. (c) activating the carbon source in the presence of at least about an inert gas at about atmospheric pressure and at an activation temperature for an activation time, the plurality of pores comprises more micropores than mesopores and more mesopores than macropores, and at least 0.001% by volume of the pores are macropores; The process (c) comprises: (v) if a first electrolyte is selected, 0.1% to 5% by volume of the pores are macropores; a volume percentage of mesopores that varies within a range of 5 volume % to 49.9 volume % of the pores, the sum of the volume percentage of the mesopores and the volume percentage of the macropores being 50% or less; Micropores that increase or decrease within a range of 50% by volume to 94.9% by volume of the pores, the remaining volume percentage being the micropores when the volume percentage of the macropores and the volume percentage of the mesopores are subtracted from the volume percentage of the pores in the activated carbon; (vi) If a second electrolyte is selected, 0.1% to 20% by volume of the pores are macropores; a volume percentage of mesopores that varies within a range of 20 volume % to 49.9 volume % of the pores, the sum of the volume percentage of the mesopores and the volume percentage of the macropores being 50% or less; The micropores increase or decrease within a range of 50% by volume to 79.9% by volume of the pores, and the remaining volume percentage, obtained by subtracting the volume percentage of the macropores and the volume percentage of the mesopores from the volume percentage of the pores in the activated carbon, is the micropores. A method for producing activated carbon.

2. The method for producing activated carbon according to claim 1, Step (c) produces activated carbon; (vii) when the first electrolyte is selected, the first pore width of the first primary mesopore is between 2 nm and 6 nm; (viii) when the second electrolyte is selected, the second primary mesopore has a second pore width of 2 nm to 10 nm; A method for producing activated carbon.

3. The method for producing activated carbon according to claim 1 or 2, The hybrid electrolyte comprising water, acetonitrile, and sodium perchlorate salt is at least one of a cosolvent in a salt electrolyte, an aqueous electrolyte, an organic electrolyte, and an ionic solution. A method for producing activated carbon.

4. The method for producing activated carbon according to claim 1, Step (c) is (d) forming a first powder by exposing the carbon source to an activator and then drying the carbon source; (e) activating the first powder by heating the first powder at an activation temperature for an activation time in the presence of an inert gas to form a second powder; (f) washing the second powder; (g) after step (f), exposing the second powder to an acidic aqueous solution to produce an infused powder; (h) washing the soaked powder to produce a washed powder; (i) drying the washed powder; have A method for producing activated carbon.

5. The method for producing activated carbon according to claim 4, Prior to step (d), the method further comprises at least one of drying and carbonizing the carbon source. A method for producing activated carbon.

6. The method for producing activated carbon according to claim 4 or 5, Step (d) comprises exposing the carbon source to an activator caustic solution in a mass ratio of caustic solution to carbon source ranging from 1:1 to 12:

1. A method for producing activated carbon.

7. The method for producing activated carbon according to claim 4 or 5, Step (e) comprises heating the first powder at an activation temperature, where the hybrid electrolyte comprises water, a co-solvent and a salt at a molar concentration in the range of 4-10 M, the co-solvent being acetonitrile and the salt being sodium perchlorate. A method for producing activated carbon.

8. The method for producing activated carbon according to claim 4 or 5, Step (e) is heating in the presence of an at least substantially inert gas selected from the group consisting of nitrogen, helium, and argon gas. A method for producing activated carbon.

9. The method for producing activated carbon according to claim 4 or 5, Step (f) includes exposing the second powder to an acidic aqueous solution including at least one of an organic acid, citric acid, and hydrochloric acid. A method for producing activated carbon.

10. A method for manufacturing an electrode, comprising the steps of: (k) preparing an electrode mixture comprising the activated carbon prepared by the method for preparing activated carbon according to claim 1, a conductive additive, and a binder; Equipped A method for manufacturing an electrode.

11. The method for producing an electrode according to claim 10, The process (k) is forming an electrode mixture including a binder having one or more of polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), copolymers, and terpolymers; A method for manufacturing an electrode.

12. 12. The method for producing an electrode according to claim 10 or 11, The process (k) is Forming an electrode mix comprising 75-90% by weight of activated carbon, 5-15% by weight of binder, and 1-10% by weight of conductive additive. A method for manufacturing an electrode.

13. 13. The method of claim 12, further comprising the steps of: Step (k) produces an electrode mixture in which the binder is polytetrafluoroethylene and the conductive additive is acetylene black. A method for manufacturing an electrode.

14. The method for producing an electrode according to claim 10 or 11, Step (k) includes producing an electrode mixture further comprising a mixture; (m) forming one of an anode or a cathode by combining the electrode mix with a conductive current collector; (n) drying one of the anode and the cathode; Also includes A method for manufacturing an electrode.

15. 12. The method for producing an electrode according to claim 10 or 11, (p) winding the electrode mixture into a thin film; (q) producing one of an anode or a cathode by combining the electrode mixture with a conductive current collector that is conductive when the electrode mixture is wound into a film. A method for manufacturing an electrode.

16. 16. The method for producing an electrode according to claim 14 or 15, The process (h) is an electrode mixture; a conductive current collector comprising a material selected from the group consisting of stainless steel, titanium, aluminum, copper, conductive carbon, and carbon; By combining the above, one of the anode and the cathode is generated. A method for manufacturing an electrode.

17. 1. An electrical energy storage device, comprising: (r) a pair of electrodes produced by the method of claim 10 or 11; (s) a hybrid electrolyte comprising water, acetonitrile, and sodium perchlorate salt disposed between a pair of electrodes; (t) an ion-permeable separator disposed between the pair of electrodes; Equipped An electrical energy storage device comprising:

18. 20. The electrical energy storage device of claim 17, The ion-permeable separator material is at least one of a cellulose dielectric and a plastic dielectric.

1. An electrical energy storage device comprising:

19. 19. An electrical energy storage device according to claim 17 or 18, The device is a supercapacitor. An electrical energy storage device comprising:

20. 19. An electrical energy storage device according to claim 17 or 18, a container, a set of electrodes, and a hybrid electrolyte comprising water, acetonitrile, and sodium perchlorate salt; the electrostatic storage device is capable of identifying when it requires maintenance by measuring and analyzing its operational performance; the container provides access to the interior contents of the electrostatic storage device; The electrostatic storage device comprises: Maintenance and Maintenance and Removal and Exchange and re-injecting the hybrid electrolyte; and removing the hybrid electrolyte; and adding additional said hybrid electrolyte; Operable to receive at least one of An electrical energy storage device comprising:

21. 21. The electrical energy storage device of claim 20, The internal contents are perforations that saturate the electrode / conductive energy storage material when electrolyte is injected into said interior contents; have An electrical energy storage device comprising:

22. 22. The electrical energy storage device according to claim 20 or 21, The container is resealable An electrical energy storage device comprising:

23. 22. The electrical energy storage device according to claim 20 or 21, The contents may be removed from the container during maintenance, after which the contents are placed into one of the containers, a new container, and then sealed to complete the maintenance. An electrical energy storage device comprising:

Citation Information

Patent Citations

  • Electrode for electric double layer capacitor

    JP1995220985A

  • Carbonaceous material, method for producing and electric double layer capacitor using the carbonaceous material

    JP2001089119A

  • Energy storage devices

    JP2017520125A

  • Electric double layer capacitor

    JP2018092978A

  • Regeneration electrolyte for power storage device, power storage device regenerated therewith, and regeneration method of power storage device

    WO2015163279A1