Low-dust sprayed concrete and low-dust spraying method using same
A low-dust shotcrete method using calcium aluminate and aluminum sulfate with minimal alkali metals and polyethylene oxide addresses dust generation issues, ensuring high safety and efficient strength development in shotcrete applications.
Patent Information
- Application Number
- JP2022550404
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-17
- Filing Date
- 2021-08-04
- Publication Date
- 2024-11-11
- Estimated Expiration
- 2041-08-04
AI Technical Summary
Existing shotcrete methods generate significant dust due to the use of alkaline materials like alkali metal aluminates and alkali metal hydroxides, which are highly reactive and difficult to handle, leading to environmental degradation and safety concerns.
A low-dust shotcrete composition using calcium aluminate and aluminum sulfate, with specific ratios and minimal alkali metal content, combined with polyethylene oxide, is mixed and conveyed through compressed air to minimize dust generation and ensure high rapid setting and strength development.
The solution provides a low-dust shotcrete method that ensures high safety, stable strength development, and reduced dust generation across varying temperatures, eliminating the need for protective gear and enhancing work efficiency.
Smart Images

Figure 0007580477000001 
Figure 0007580477000002 
Figure 0007580477000003
Abstract
Description
[Technical field]
[0001] The present invention relates to low-dust sprayed concrete and a low-dust sprayed construction method using the same. [Background technology]
[0002] In tunnel excavation work, concrete is sprayed to reinforce the ground and stabilize the excavation surface. There are two methods: dry method, in which compressed air from a compressor is supplied into a transport pipe that transports concrete sent by a piston pump, etc., and the concrete is pneumatically transported, and at the same time, powdered quick-setting agent transported by air from an quick-setting agent supplying facility is supplied to a branch pipe of the junction pipe, the concrete and the quick-setting agent are mixed, and then the concrete is sprayed from a nozzle; and wet method, in which water is added during the pneumatic transport of dry-mix concrete, powdered quick-setting agent transported by air from an quick-setting agent supplying facility is supplied to a branch pipe of the junction pipe, the concrete and the quick-setting agent are mixed, and then the concrete is sprayed from a nozzle.
[0003] These spraying methods can generate a large amount of dust when the pneumatically transported concrete is sprayed, so a method has been proposed in which a powdered dust-reducing agent such as water-soluble cellulose and polyethylene oxide is added to the concrete before it is mixed (see, for example, Patent Documents 1 and 2). Also, a method has been proposed for reducing dust by spraying a cement composition using coated fine aggregate obtained by coating fine aggregate with cement (see, for example, Patent Document 3).
[0004] However, powdered dust-reducing agents require, for example, adjusting the particle size of polyethylene oxide to an appropriate size to increase solubility. In addition, powdered dust-reducing agents dissolve in the surface water of concrete aggregates, so they tend to adhere to aggregate hoppers and form balls during mixing, making it difficult to obtain sufficient dust prevention effects. This is particularly noticeable when the surface water content of the aggregate is high.
[0005] In view of this, a powdered dust prevention agent containing an inorganic fine powder made of polyethylene oxide and talc and / or pyrophyllite has been proposed (see, for example, Patent Document 4). However, although the transportability and safety of powdered dust-reducing agents from the hopper of the weighing machine have improved, powdered dust-reducing agents have large changes in viscosity with temperature, which can lead to poor mixability with quick-setting agents and variations in the amount of dust generated and strength development in some cases.
[0006] On the other hand, examples of quick-setting additives that are used in combination with powdered dust-reducing agents include mixtures of calcium aluminate, alkali metal aluminate, and alkali metal carbonate, etc.; mixtures of calcined alum, alkali metal aluminate, and alkali metal carbonate, etc.; mixtures of calcium aluminate and 3CaO SiO2; mixtures of slaked lime, alkali metal aluminate, and alkali metal carbonate; and the like (see, for example, Patent Documents 5 to 9). These accelerators have the function of accelerating the setting of cement, and are mixed with cement concrete and sprayed onto the ground surface.
[0007] The method of adding the quick-setting agent is usually a method that generates a large amount of dust because the powder is mixed by air transportation. Therefore, the working environment may deteriorate, and it is necessary to wear protective glasses and a dust mask when spraying, and a method of construction that generates less dust has been desired. As a method of construction that generates less dust, a method has been proposed in which the quick-setting agent is made into a slurry and added and mixed with cement concrete, and then a solution of an alkali metal aluminate is separately pumped and mixed, and sprayed (see, for example, Patent Document 10). This method uses a highly alkaline liquid, which is difficult to handle, and requires protective glasses and gloves when spraying, which reduces workability.
[0008] Therefore, a quick-setting admixture that combines amorphous calcium aluminate and crystalline calcium aluminate has been proposed (see, for example, Patent Document 11). Patent Document 11 clearly states that an even better effect can be obtained by further using sodium aluminate at low temperatures. However, in recent years, from the viewpoint of blindness and chemical burns caused by strong alkalinity, it is preferable to avoid using strong alkaline raw materials such as alkali metal aluminates and alkali metal hydroxides as much as possible in quick-setting admixtures, but the current situation is that there are still many issues to be addressed in terms of high temperature conditions, costs, etc. [Prior art documents] [Patent documents]
[0009] [Patent Document 1] Japanese Patent Application Publication No. 58-15056 [Patent Document 2] JP 2004-189529 A [Patent Document 3] JP 2000-72503 A [Patent Document 4] JP 2009-78934 A [Patent Document 5] Special Publication No. 60-4149 [Patent Document 6] Japanese Patent Application Publication No. 64-051351 [Patent Document 7] Special Publication No. 56-27457 [Patent Document 8] Japanese Patent Application Publication No. 61-026538 [Patent Document 9] Japanese Patent Application Publication No. 63-210050 [Patent Document 10] Japanese Patent Application Publication No. 05-139804 [Patent Document 11] Patent No. 5026928 Summary of the Invention [Problem to be solved by the invention]
[0010] In general, highly alkaline materials used in quick-setting agents are highly reactive with cement and can have poor mixability with cement concrete containing dust-reducing agents, which can lead to variations in the strength development of the sprayed concrete and the amount of dust generated, making them difficult to apply.
[0011] The present invention aims to provide a low-dust sprayed concrete which can be used in cement concrete containing a dust-reducing agent without using materials such as alkali metal aluminates and alkali metal hydroxides as quick-setting agents, and which can achieve high quick-setting properties, high early strength development, and high mixability with cement concrete even at high temperatures, which are equal to or greater than those of quick-setting agents containing the above-mentioned materials, and which does not cause variation in the amount of dust generated due to environmental temperature and can be used in places where long-term strength development is required, as well as a low-dust sprayed construction method using the same. [Means for solving the problem]
[0012] As a result of various investigations aimed at solving the above problems, the present inventors have conceived the following invention and found that the above problems can be solved.
[0013] [1] A low-dust sprayed concrete comprising: a cement concrete containing polyethylene oxide; and a sprayed quick-setting admixture which is substantially free of alkali metal aluminates and alkali metal hydroxides and which contains calcium aluminate and aluminum sulfate, wherein the sprayed quick-setting admixture contains 5 to 105 parts by mass of aluminum sulfate per 100 parts by mass of calcium aluminate, and the content of alkaline earth metals in the aluminum sulfate is 0.007 to 4% by mass calculated as alkaline earth metal oxide. [2] The low-dust sprayed concrete according to [1], wherein the aluminum sulfate contains 0.005 to 2 mass % CaO and 0.002 to 2 mass % MgO. [3] The low-dust sprayed concrete according to [1] or [2], further comprising 5 to 105 parts by mass of an alkaline earth metal hydroxide per 100 parts by mass of the calcium aluminate. [4] The low-dust sprayed concrete according to any one of [1] to [3], further comprising at least one selected from the group consisting of alkali metal carbonates, alkaline earth metal carbonates, and alkaline earth metal sulfates. [5] The low-dust sprayed concrete according to [4], which contains the alkali metal carbonate in an amount of 1 to 30 mass %. [6] Low-dust sprayed concrete according to any one of [1] to [5], wherein the proportion of aluminum sulfate having a particle size of 10 μm or less in the aluminum sulfate is 1 to 40 mass %. [7] Low-dust sprayed concrete according to any one of [1] to [6], wherein the aluminum sulfate is a hydrate having 4 to 12 water of hydration. [8] Low-dust sprayed concrete according to any one of [1] to [7], wherein the polyethylene oxide has a mass average molecular weight of 100,000 to 5,000,000. [9] A low-dust spraying method comprising transporting the cement concrete and spraying quick-setting admixture contained in the low-dust sprayed concrete described in any one of [1] to [8] to a mixing pipe by compressed air, mixing and joining the cement concrete and the spraying quick-setting admixture in the mixing pipe, and then ejecting and spraying the mixture from a spray nozzle.
[10] A low-dust spraying method as described in [9], in which the cement concrete is transported by compressed air a distance of 4 m or more before being mixed with the spraying quick-setting admixture, and after the cement concrete and the spraying quick-setting admixture have been mixed and joined together, the concrete is transported a distance of 1.5 m or more and then discharged and sprayed from the spray nozzle. Effect of the Invention
[0014] According to the present invention, it is possible to provide a low-dust sprayed concrete which, even at high temperatures, can achieve high quick-setting properties and high early strength development with less variation than quick-setting admixtures containing the above-mentioned materials, without using materials such as alkali metal aluminates and alkali metal hydroxides, and which can be applied to locations where long-term strength development is required or where low dust generation is required, and a low-dust sprayed construction method using the same. Furthermore, compared with low-dust sprayed concrete that contains at least one of an alkali metal aluminate and an alkali metal hydroxide, high safety is ensured in handling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] [Low-dust sprayed concrete] The low-dust sprayed concrete according to the embodiment of the present invention is a mixture of cement concrete and a sprayed quick-setting admixture.
[0016] <Cement concrete> The cement for cement concrete is not particularly limited, and examples include various Portland cements such as normal, high-early-strength, extra-high-early-strength, medium-heat, and low-heat, filler cements made by mixing Portland cement with blast furnace slag, fly ash, and limestone powder, and environmentally friendly cements (eco-cement) made from municipal waste incineration ash and sewage sludge incineration ash, and these can also be used in a fine powder form. The ratio of the mixture and cement in the mixed cement is not particularly limited, and it is also possible to use a mixture of more of these admixtures than are assumed by the JIS.
[0017] The cement concrete of this embodiment contains cement and aggregate, and the aggregate preferably has low water absorption and high aggregate strength. The aggregate is not particularly limited as long as it can be sprayed, but river sand, mountain sand, sea sand, lime sand, silica sand, etc. can be used as fine aggregate, and river gravel, mountain gravel, lime gravel, etc. can be used as coarse aggregate, and crushed sand and crushed stone can also be used.
[0018] The cement concrete contained in the low-dust sprayed concrete of the present invention contains polyethylene oxide as a dust-reducing component. If the mass average molecular weight of polyethylene oxide is high, the viscosity of concrete increases and the mixability with the quick-setting agent tends to deteriorate, so the dust-reducing performance decreases, and if the molecular weight is low, it cannot affect the concrete viscosity and the dust-reducing performance decreases, so in the present invention, the mass average molecular weight of polyethylene oxide is preferably 100,000 to 5,000,000, more preferably 300,000 to 4,000,000, and even more preferably 500,000 to 3,000,000. The mass average molecular weight of polyethylene oxide can be determined by gel permeation chromatography (GPC) under the following measurement conditions. Measurement conditions: Equipment: Product name "LC-10AD" (manufactured by Shimadzu Corporation) Detector: Refractive index detector (RID) Column: Product name "SHODEX KF-804" (manufactured by Showa Denko K.K.) ·Measurement temperature: 30℃ ·Eluent:THF ·Flow rate: 1.0mL / min Sample concentration: 0.2% by mass (THF) Sample injection volume: 100μL Conversion standard: Polyethylene oxide
[0019] The content of the polyethylene oxide according to the present embodiment as described above is, for example, preferably 0.004 to 0.090 parts by mass, more preferably 0.006 to 0.085 parts by mass, and even more preferably 0.008 to 0.080 parts by mass, relative to 100 parts by mass of cement of cement concrete. By having the content of polyethylene oxide equal to or greater than the above lower limit, dust reduction performance is easily obtained. In addition, by having the content of polyethylene oxide equal to or less than the above upper limit, the mixability with the spray quick-setting admixture is improved, the initial adhesion property is improved, and rebound can be suppressed.
[0020] <Accelerating agent for spraying> The quick-setting admixture for spraying contained in the low-dust sprayed concrete according to the embodiment of the present invention contains substantially no alkali metal aluminate or alkali metal hydroxide, but contains calcium aluminate and aluminum sulfate. Since it contains substantially no alkali metal aluminate or alkali metal hydroxide, it is easy to handle, and protective glasses, gloves, etc. are not required during spraying, so workability is not impaired and high safety can be ensured. Here, examples of alkali metal aluminates include sodium aluminate and potassium aluminate, and examples of alkali metal hydroxides include sodium hydroxide and potassium hydroxide. Furthermore, "substantially free" refers to a content below the lower limit of detection by XRF measurement, specifically 0 ppm.
[0021] On the other hand, by setting the content of aluminum sulfate to 5 to 105 parts by mass per 100 parts by mass of calcium aluminate and setting the content of alkaline earth metal in the aluminum sulfate to 0.007 to 4 mass%, calculated as alkaline earth metal oxide, it is possible to obtain high quick-setting properties and high early strength development even under high temperature conditions without substantially containing alkali metal aluminate and alkali metal hydroxide.
[0022] The mixability of the spraying quick-setting admixture with cement concrete can be evaluated by the standard deviation indicating the variation in the Proctor penetration value measured at 10 points according to ASTM C403. The lower the standard deviation of the Proctor penetration value, the better the mixability, so it is preferably 8.0 or less, more preferably 7.5 or less, and even more preferably 7.0 or less.
[0023] The present embodiment will be described in detail below. In this specification, parts and percentages are based on mass unless otherwise specified.
[0024] (Calcium Aluminate) Calcium aluminate is a general term for crystalline and / or amorphous substances with CaO and Al2O3 as main components and hydration activity, which are obtained by mixing raw materials containing calcia and raw materials containing alumina, subjecting them to heat treatment such as firing in a kiln or melting in an electric furnace, and then quenching or slow cooling. It is a compound in which part of CaO or Al2O3 is replaced with alkali metal oxides, alkaline earth metal oxides, silicon oxide, titanium oxide, iron oxide, alkali metal halides, alkaline earth metal halides, alkali metal sulfates, alkaline earth metal sulfates, etc., or a substance in which a small amount of these elements exist as solid solutions or alone as contaminants in a substance mainly composed of CaO and Al2O3.
[0025] The particle size of calcium aluminate is 3,000 cm in terms of Blaine specific surface area (based on JIS R 5201 (physical testing method for cement). Hereinafter, this is also called the Blaine value). 2 / g or more is preferable, and 5,000 cm 2 / g or more is more preferable. 2 / g or more, the quick-setting property and early strength development of a sprayed material obtained by mixing the quick-setting admixture with cement concrete can be improved.
[0026] The CaO / Al2O3 molar ratio in calcium aluminate is preferably in the range of 2.0 to 2.6, more preferably in the range of 2.2 to 2.4, from the viewpoints of rapid setting property and early strength development.
[0027] (Aluminum Sulfate) The aluminum sulfate of the present invention contains an alkaline earth metal, and the content thereof (the total amount when there are multiple alkaline earth metals) is 0.007 to 4 mass %, preferably 0.01 to 2 mass %, calculated as alkaline earth metal oxide. The aluminum sulfate as described above can be obtained by mixing sulfuric acid containing an alkaline earth metal compound such as an alkaline earth metal oxide as an impurity with aluminum hydroxide. During the mixing, alkaline earth metals such as CaO and MgO may be added to obtain a desired content. In other words, in the aluminum sulfate of this specification, CaO and MgO are confirmed together with aluminum sulfate in fluorescent X-ray analysis, but in X-ray diffraction (XRD) analysis, only a broad peak of aluminum sulfate is confirmed, and no peaks that can identify CaO and MgO are confirmed. In other words, although the aluminum sulfate contains calcium and magnesium, it can be substantially regarded as being the same as aluminum sulfate.
[0028] As a spraying material, aluminum sulfate contributes to adhesion to the wall surface and strength development in the very early stages. In particular, aluminum sulfate containing alkaline earth metals can provide sufficient adhesion even at room temperature to low temperature environments, and can also prevent a significant decrease in long-term strength in high temperature environments. If the content of alkaline earth metals in aluminum sulfate is less than 0.007 mass% in terms of oxide, it is difficult to develop long-term strength in high temperature environments and the initial strength development may decrease significantly, which is not preferable. In addition, if the content of alkaline earth metals exceeds 4 mass% in terms of oxide, it is not preferable because the initial strength decreases and the setting property may not be easily developed regardless of the temperature environment. In particular, the above-mentioned action can be achieved by using aluminum sulfate containing a predetermined amount of alkaline earth metal-containing substance, and the above-mentioned effect cannot be sufficiently obtained even if an alkaline earth metal oxide such as commercially available reagent calcium oxide or magnesium oxide is added and mixed later in addition to aluminum sulfate not containing an alkaline earth metal-containing substance. In addition, "low temperature" in the above "low temperature environment" refers to 5°C or below, and "high temperature" in the above "high temperature environment" refers to 25°C or above.
[0029] Here, the alkaline earth metal refers to at least any one of beryllium, magnesium, calcium, strontium, and barium. These alkaline earth metals exist together with aluminum sulfate as alkaline earth metals alone or as alkaline earth metal-containing substances such as alkaline earth metal compounds, alkaline earth metal-containing solid solutions, and alkaline earth metal-containing amorphous bodies. Specific examples of the coexistence state include alkaline earth metals, alkaline earth metal oxides (BeO, MgO, CaO, SrO, BaO, etc.), alkaline earth metal hydroxides, alkaline earth metal carbonates, and solid solutions of alkaline earth metal oxides in aluminum sulfate. Preferably, no alkaline earth metal sulfates are included.
[0030] The content of aluminum sulfate is 5 to 105 parts, preferably 10 to 90 parts, and more preferably 20 to 80 parts, relative to 100 parts of calcium aluminate. If the content of aluminum sulfate is outside the range of 5 to 105 parts, the setting property decreases.
[0031] The CaO content in aluminum sulfate is preferably 0.005 to 2%, and the MgO content is preferably 0.002 to 2%, more preferably 0.01 to 1.5%, and the MgO content is more preferably 0.008 to 1.5%. The CaO content and MgO content in aluminum sulfate can be adjusted, for example, by mixing high-purity aluminum hydroxide with sulfuric acid without removing CaO and / or MgO contained in the sulfuric acid, or by intentionally adding CaO and / or MgO.
[0032] If the CaO content is 0.005% or more, it is easier to obtain long-term strength under high temperature conditions, and if it is 2% or less, it is easier to suppress the deterioration of setting properties. Also, if the MgO content is 0.002% or more, it is easier to obtain long-term strength under high temperature conditions, and if it is 2% or less, it is easier to suppress abnormal expansion under high temperature conditions.
[0033] Aluminum sulfate can be used in the range of anhydrous salt to 14-18 hydrates, but 14-hydrates or more may not be able to be pulverized, so 12-hydrates or less is preferred. Anhydrous salts may have poor coagulation properties, so 4-hydrates or more are preferred. More preferred are 4-12 hydrates, i.e., aluminum sulfate is a hydrate with 4-12 waters of hydration. The number of water of hydration may be adjusted by, for example, dehydrating aluminum sulfate 18-hydrate by heating or the like until the desired number of water of hydration is reached.
[0034] Aluminum sulfate can be used in any form of powder, such as flakes, coarse powder, or powder, but from the viewpoint of very early strength development, powder form is preferred, and it is preferable to adjust the particle size to 10 μm or less at 1 to 40%. If the particle size is 10 μm or less at 1% or more, very early strength development is easily achieved, and if it is 40% or less, long-term strength is more easily achieved. A sieve or the like can be used to adjust the particle size to 1 to 40% of the particle size being 10 μm or less.
[0035] (Alkaline Earth Metal Hydroxides) The quick-setting admixture for spraying according to the present embodiment preferably further contains an alkaline earth metal hydroxide, which can further improve the long-term strength.
[0036] The alkaline earth metal hydroxide refers to, for example, hydroxides of beryllium, magnesium, calcium, strontium, barium, etc., and one or more of calcium hydroxide, strontium hydroxide, barium hydroxide, magnesium hydroxide, and radium hydroxide can be used. Among these, calcium hydroxide and magnesium hydroxide are preferred from the industrial viewpoint of cost and ease of handling, and carbide slag produced as a by-product when acetylene is generated from calcium carbide can also be used as calcium hydroxide. The particle size of the alkaline earth metal hydroxide is preferably 30% or less of the 250 μm residue, more preferably 10% or less of the 250 μm residue.
[0037] The content of the alkaline earth metal hydroxide is preferably 2 to 120 parts by mass, more preferably 5 to 105 parts by mass, further preferably 5 to 100 parts by mass, and particularly preferably 10 to 50 parts by mass, based on 100 parts by mass of calcium aluminate. By making the content of the alkaline earth metal hydroxide equal to or more than the lower limit, the setting property is less likely to deteriorate. In addition, by making the content of the alkaline earth metal hydroxide equal to or less than the upper limit, the long-term strength can be improved.
[0038] (Other Ingredients) The quick-setting admixture for spraying according to the present embodiment may contain materials expected for normal quick-setting admixtures, if necessary. For example, a substance selected from the group consisting of an alkali metal carbonate, an alkaline earth metal carbonate, and an alkaline earth metal sulfate may be used, and at least one selected from the group consisting of an alkaline earth metal carbonate and an alkaline earth metal sulfate is preferred. At least one selected from the group consisting of an alkaline earth metal carbonate and an alkaline earth metal sulfate is preferred in terms of contributing to the enhancement of long-term strength, and is preferably 0.3 to 50 mass%, more preferably 0.6 to 45 mass%, and even more preferably 1 to 40 mass% in the quick-setting admixture for spraying. Examples of the alkaline earth metal carbonate and the alkaline earth metal sulfate include calcium carbonate and calcium sulfate.
[0039] In addition, in order to obtain a predetermined strength, particularly at 3-hour strength or 1-day strength, it is preferable to use an alkali metal carbonate. The amount of the alkali metal carbonate in the quick-setting admixture for spraying is preferably 0.3 to 50 mass%, more preferably 0.6 to 45 mass%, and even more preferably 1 to 40 mass%. When the amount of the alkali metal carbonate is equal to or more than the lower limit, a desired strength is easily obtained at the 3-hour strength or 1-day strength. When the amount of the alkali metal carbonate is equal to or less than the upper limit, a long-term strength is easily obtained. Examples of the alkali metal carbonate include sodium carbonate and potassium carbonate.
[0040] The amount of the quick-setting admixture for spraying is preferably 5 to 30 parts by mass, more preferably 6 to 25 parts by mass, and even more preferably 7 to 20 parts by mass, relative to 100 parts by mass of cement in the cement concrete. When the amount of the quick-setting admixture for spraying is equal to or more than the above lower limit, the adhesion property, setting property, and strength expression required for spraying are easily obtained. In addition, when the amount of the quick-setting admixture for spraying is equal to or less than the above upper limit, it is possible to suppress a decrease in long-term strength. The form of the quick-setting admixture for spraying according to this embodiment when mixed into cement concrete is not particularly limited, and examples thereof include powder, liquid, suspension, and slurry.
[0041] [Low dust spraying method] The low-dust spraying method of the present invention can be a wet spraying method in which water is added to cement concrete containing polyethylene oxide in a concrete manufacturing facility to prepare wet concrete, and a spraying quick-setting admixture is added just before spraying. Although there is another type of spraying method, dry spraying, in the present invention, from the viewpoint of reducing the amount of dust generated, the wet spraying method is preferable.
[0042] In the low-dust spraying method of the present invention, after a fixed amount of cement concrete is transported by a concrete pump, compressed air is added to the cement concrete by the pump, and the cement concrete is transported to a mixing pipe by the compressed air. The cement concrete is then mixed in the mixing pipe by adding a quick-setting agent for spraying. In the low-dust spraying method of the present invention, the transport distance from the addition of compressed air to the cement concrete to the addition of the quick-setting agent for spraying is preferably 4 m or more, more preferably 5 m or more, and even more preferably 6 m or more. By having the transport distance from the addition of compressed air to the cement concrete to the addition of the quick-setting agent for spraying be equal to or more than the above lower limit, the concrete strength development after spraying is less variable, and the dust reduction performance is also improved, which is preferable. In addition, the transport distance from the addition of compressed air to the cement concrete to the addition of the quick-setting agent for spraying is preferably 20 m or less, more preferably 15 m or less, and even more preferably 10 m or less. By keeping the conveying distance from when the compressed air is added to the cement concrete until the spraying quick-setting admixture is added to the concrete at or below the upper limit value, the cement concrete can be conveyed stably.
[0043] In addition, the cement concrete is transported in a fixed amount by a concrete pump and transported to a mixing pipe by compressed air by the pump. In the mixing pipe, the cement concrete is then mixed with a quick-setting agent for spraying transported by compressed air via another route, and is discharged and sprayed from a spray nozzle. The transport distance from the cement concrete and the quick-setting agent for spraying to the spray nozzle is preferably 1.5 m or more, more preferably 2.0 m or more, and even more preferably 2.5 m or more. By having the transport distance from the cement concrete and the quick-setting agent for spraying to the spray nozzle be equal to or more than the above lower limit, the quick-setting agent for spraying and the cement concrete can be mixed well, the variation in strength development is suppressed, and the dust reduction performance is also improved, which is preferable. In addition, the transport distance from the cement concrete and the quick-setting agent for spraying to the spray nozzle is preferably 10 m or less, more preferably 7.5 m or less, and even more preferably 5 m or less. By keeping the transport distance from the joining of the cement concrete and the spraying quick-setting admixture to the spray nozzle below the above upper limit value, the cement concrete and the spraying quick-setting admixture can be transported stably.
[0044] By using the low-dust sprayed concrete of the present invention, the amount of dust generation can be suppressed, and the variation in the amount of dust generation due to the environmental temperature can also be suppressed. The environmental temperature at which the low-dust sprayed concrete is sprayed by the low-dust spraying method of the present invention is preferably 5°C or higher, more preferably 7°C or higher, and even more preferably 10°C or higher. By having the environmental temperature at which the low-dust sprayed concrete is sprayed be equal to or higher than the above lower limit, moderate strength development can be obtained, and dust reduction performance can also be improved, so that the variation in dust generation due to the environmental temperature can be suppressed. In addition, the environmental temperature at which the low-dust sprayed concrete is sprayed by the low-dust spraying method of the present invention is preferably 40°C or lower, more preferably 35°C or lower, and even more preferably 33°C or lower. By having the environmental temperature at which the low-dust sprayed concrete is sprayed be equal to or lower than the above upper limit, the dust reduction performance can be improved without causing extreme strength development, and the variation in dust generation due to the environmental temperature can be suppressed.
[0045] In the low-dust spraying method of the present invention, the cement concrete is transported in a fixed quantity by a concrete pump, combined with compressed air, combined with the spraying quick-setting agent, and sprayed. Either hose or metal piping can be used for the section, and either can be used as long as it is made of a commonly used material. EXAMPLES
[0046] [Experimental Example 1] The measuring methods for each physical property and the materials used are as follows. (Spraying test) Cement concrete was prepared at a test temperature of 30°C, consisting of 360 kg of cement, 216 kg of water, 1,050 kg of sand, 650 kg of gravel, and 180 g of dust-reducing component A. The prepared cement concrete was pumped at 12 m per hour using a concrete pump (Shintech, MKW-25SMT). 3 The pump transports the material at a rate of 10 m per minute. 3The cement concrete was then mixed with the compressed air at a flow rate of 4 m per minute so that the cement concrete was sprayed with 9 parts by mass of the quick-setting agent (spraying quick-setting agent) with the content shown in Table 1 at 100 parts by mass of cement. 3 The concrete was transported under these transport conditions and mixed together to obtain low-dust sprayed concrete. After the cement concrete and spraying accelerator were mixed together, the low-dust sprayed concrete was transported over a 3m pipe to the spraying nozzle and sprayed onto a steel plate. The Proctor penetration value 5 minutes after spraying the low-dust sprayed concrete was measured at 10 points according to ASTM C403, and the average value and standard deviation were calculated. The compressive strength (JIS R 5201, the same below) was measured at 10 minutes, 3 hours, and 28 days after spraying. In addition, the rebound rate of the spraying and the amount of dust 10 m behind the spraying point were measured using the method described below. Each of the spray quick-setting admixtures having the content ratios shown in Table 1 was prepared by mixing the respective materials.
[0047] (Rebound rate) Excavation cross section: 15m 2 The rebound was measured when the concrete was sprayed for 3 minutes over a 1m wide area within a circumferential angle of 45° to 90° of the mock tunnel (a surface where sprayed concrete had been applied in advance and scraped off to make it smooth after hardening), and the rebound rate from the low-dust sprayed concrete used was calculated using the following formula. The rebound rate was calculated as follows: (kg of low-dust shotcrete that fell) / (kg of low-dust shotcrete used for spraying) x 100 (%). The rebound rate is preferably 20% or less.
[0048] (Amount of dust) Excavation cross section: 15m 2During 10 minutes of spraying on a 1m wide area (surface where sprayed concrete had been applied in advance and scraped off to make it smooth after hardening) in the circumferential range of 45° to 90° of the simulated tunnel, the amount of dust was measured every minute at a position 10m behind the spraying area using a Shibata Scientific Digital Dust Meter LD-3K2. The dust amount (mg / m3) was calculated using a mass conversion coefficient of 0.002 for the count value of the dust meter. 3 ) was calculated.
[0049] (Materials used) Cement: Ordinary Portland cement, manufactured by Denka Sand: River sand, density 2.64g / cm 3 , coarse grain rate (FM) 2.83 Gravel: River gravel, density 2.67g / cm 3 Water: Tap water Dust reduction component A: Polyethylene oxide, mass average molecular weight 1.8 million, commercially available product Calcium aluminate: CaO / Al2O3 molar ratio: 2.24, Blaine specific surface area: 5900 cm 2 / g, CaO source: quicklime (CaO: 95%), Al2O3 source: natural bauxite (Al2O3: 85%), manufacturing method: melted in an electric furnace, quenched and crushed into glass powder, vitrification rate: 90%, the sum of CaO and Al2O3 is 96% Alkaline earth metal hydroxide a: Calcium hydroxide (industrial product), calcium hydroxide content 98%, Blaine specific surface area 10,500 cm 2 / g, AS-A: Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides. Particle size of 10 μm or less: 20%, 8.5% hydrate
[0050] [Table 1]
[0051] From the test results in Table 1, if the amount of aluminum sulfate in the spray quick-setting admixture is 4 parts by mass, Mean and standard deviation of Proctor penetration valuesIt can be seen that the setting time and compressive strength are significantly lower than those of the Examples. It can also be seen that when the amount of aluminum sulfate blended is 110 parts by mass, the setting time and compressive strength are lower than those of the Examples. From the above results, it is preferable that the content of aluminum sulfate in the quick-setting admixture is 5 to 105 parts by mass, and particularly 5 to 100 parts by mass.
[0052] [Experimental Example 2] Experimental Example 2 was the same as Experimental Example 1, except that the aluminum sulfate contained in the spray quick-setting admixture was changed to that shown in Table 2. The aluminum sulfate used contained 0.006% to 4.5% alkaline earth metal, calculated as metal oxide, and the abbreviations for these metals are shown below.
[0053] AS-I: Aluminum sulfate containing 0.003% by mass of CaO, 0.002% by mass of MgO, and 0.005% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5 hydrate AS-C: Aluminum sulfate containing 0.005% by mass of CaO, 0.002% by mass of MgO, and 0.007% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5 hydrate AS-E: Aluminum sulfate containing 0.006% by mass of CaO, 0.004% by mass of MgO, and 0.010% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5 hydrate AS-O: Aluminum sulfate containing 0.8% by mass of CaO, 0.5% by mass of MgO, and 1.3% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5% hydrate AS-Ca; Aluminum sulfate containing 1% by mass of CaO, 1% by mass of MgO, and 2.0% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5 hydrate AS-Ki: Aluminum sulfate containing 1.3% by mass of CaO, 1.1% by mass of MgO, and 2.4% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5% hydrate AS-Q: Aluminum sulfate containing 1.6% by mass of CaO, 1.8% by mass of MgO, and 3.4% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5% hydrate AS-Ke; Aluminum sulfate containing 2.1% by mass of CaO, 2.3% by mass of MgO, and 4.4% by mass of alkaline earth metals calculated as alkaline earth metal oxides; particle size of 10 μm or less: 20%, 8.5% hydrate
[0054] [Table 2]
[0055] From the test results in Table 2, it can be seen that the comparative example containing 0.005% alkaline earth metal in terms of alkaline earth metal oxide has a slower Proctor initial and final setting time compared to the examples. The compressive strength is also reduced. The comparative example containing 4.4% alkaline earth metal in terms of alkaline earth metal oxide also has a slower Proctor initial and final setting time compared to the examples. The average value and standard deviation of the penetration value decreased significantly. From the above results, it is preferable that the aluminum sulfate in the quick-setting admixture contains 0.007 to 4% alkaline earth metal calculated as alkaline earth metal oxide.
[0056] [Experimental Example 3] Experimental Example 3 was the same as Experimental Example 1, except that the composition of the spray quick-setting admixture was changed to that shown in Table 3.
[0057] [Table 3]
[0058] From the above results, the content of calcium hydroxide in the quick-setting admixture is preferably 5 parts by mass to 100 parts by mass per 100 parts by mass of calcium aluminate.
[0059] [Experimental Example 4] Experimental Example 4 was the same as Experimental Example 1, except that the aluminum sulfate contained in the spray quick-setting admixture was changed to that shown in Table 4. The aluminum sulfate used was as follows:
[0060] AS-Co: Aluminum sulfate containing 0.004% by mass of CaO, 0.5% by mass of MgO, and 0.504% by mass of alkaline earth metal oxide equivalent, particle size 10 μm or less: 20%, 8.5 hydrate AS-Sa: Aluminum sulfate containing 3% by mass of CaO, 0.5% by mass of MgO, and 3.5% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size of 10 μm or less: 20%, 8.5% hydrate AS-Si: Aluminum sulfate containing 0.5% by mass of CaO, 0.001% by mass of MgO, and 0.501% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 8.5 hydrate AS-S; Aluminum sulfate containing 0.5% by mass of CaO, 2% by mass of MgO, and 2.5% by mass of alkaline earth metals calculated as alkaline earth metal oxides; particle size 10 μm or less: 20%, 8.5% hydrate
[0061] [Table 4]
[0062] It can be seen from Table 4 that the amount of alkaline earth metal oxide contained in aluminum sulfate is preferably such that CaO is 0.005% by mass to 2% by mass, and MgO is 0.002% by mass to 2% by mass.
[0063] [Experimental Example 5] Experimental Example 5 was the same as Experimental Example 1, except that a spray quick-setting admixture was prepared consisting of 100 parts by mass of calcium aluminate, 50 parts by mass of alkaline earth metal hydroxide A, 50 parts by mass of aluminum sulfate (AS-A), and the types and amounts of alkaline earth metal carbonates and alkaline earth metal sulfates shown in Table 5, as in Experimental Example 1. The alkaline earth metal carbonates and alkaline earth metal sulfates used were as follows:
[0064] Alkaline earth metal carbonate: Magnesium carbonate industrial product, Blaine value 2,800 cm 2 / g Alkaline earth metal carbonate I: Calcium carbonate industrial product, Blaine value 3,000 cm 2 / g Alkaline earth metal sulfate α: Magnesium sulfate industrial product, Blaine value 3,500 cm 2 / g Alkaline earth metal sulfate β: Calcium sulfate industrial product, Blaine value 4,500 cm 2 / g
[0065] [Table 5]
[0066] [Experimental Example 6] Experimental Example 6 was the same as Experimental Example 1, except that a spray quick-setting admixture was prepared consisting of 100 parts by mass of calcium aluminate as in Experimental Example 5, 50 parts by mass of alkaline earth metal hydroxide A, 50 parts by mass of aluminum sulfate (AS-A), 10 parts by mass of alkaline earth metal carbonate B, 10 parts by mass of alkaline earth metal sulfate β, and the types and amounts of alkali metal carbonates shown in Table 6. The alkali metal carbonates used were as follows:
[0067] Alkaline metal carbonate A: Sodium carbonate industrial product, sodium carbonate content 98%, Blaine 1,000 cm 2 / g Alkaline metal carbonate I: Potassium carbonate industrial product, Potassium carbonate content 97%, Blaine 1,500cm 2 / g Alkaline metal carbonate: Lithium carbonate industrial product, lithium carbonate content 98%, Blaine 800cm 2 / g
[0068] [Table 6]
[0069] [Experimental Example 7] Experimental Example 7 was the same as Experimental Example 1, except that the aluminum sulfate contained in the spray quick-setting admixture was changed to that shown in Table 7. The aluminum sulfate used was as follows:
[0070] AS-Si: Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size of 10 μm or less: 0.5%, 8.5% hydrate AS-S; Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides; Particle size 10 μm or less: 1.0%, 8.5% hydrate AS-Ce: Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 40%, 8.5% hydrate AS-SO: Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 41%, 8.5% hydrate
[0071] [Table 7]
[0072] [Experimental Example 8] Experimental Example 8 was the same as Experimental Example 1, except that the aluminum sulfate contained in the spray quick-setting admixture was changed to that shown in Table 7. The aluminum sulfate used was as follows:
[0073] AS-Ta: Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 18-hydrate AS-Chi: Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 14-hydrate AS-T; Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 12-hydrate AS-TE; Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides, particle size 10 μm or less: 20%, 10.5 hydrate AS-t; Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides; particle size 10 μm or less: 20%, 4.0 hydrate AS-Na; Aluminum sulfate containing 0.9% by mass of CaO, 0.7% by mass of MgO, and 1.6% by mass of alkaline earth metals calculated as alkaline earth metal oxides; Particle size 10 μm or less: 20%; Anhydrous salt
[0074] [Table 8]
[0075] [Experimental Example 9] Experimental Example 9 was the same as Experimental Example 1, except that the dust-reducing components contained in the cement concrete were changed to those shown in Table 9. The dust-reducing components used were as follows:
[0076] Dust reduction component B: Polyethylene oxide, mass average molecular weight 100,000, commercially available product Dust reduction component C: Polyethylene oxide, mass average molecular weight 1 million, commercially available product Dust reduction component D: Polyethylene oxide, mass average molecular weight 3 million, commercially available product Dust reduction component E: Polyethylene oxide, mass average molecular weight 5 million, commercially available product Dust reduction component F: Polyethylene oxide, mass average molecular weight 6 million, commercially available product Dust-reducing ingredient G: Dust-reducing agent whose main ingredient is methylcellulose, commercially available product
[0077] [Table 9]
[0078] [Experimental Example 10] Experimental Example 10 was the same as Experimental Example 1, except that the content of dust-reducing component A contained in the cement concrete was changed to that shown in Table 10.
[0079] [Table 10]
[0080] [Experimental Example 11] Experimental Example 11 was the same as Experimental Example 1, except that after the compressed air was joined to the cement concrete, the distance traveled before mixing with the spraying quick-setting admixture was changed to that shown in Table 11.
[0081] [Table 11]
[0082] [Experimental Example 12] Experimental Example 12 was the same as Experimental Example 1, except that the distance over which the cement concrete and the spraying quick-setting admixture were transported after being mixed and joined was changed to that shown in Table 12.
[0083] [Table 12]
[0084] [Experimental Example 13] Experimental Example 13 was the same as Experimental Example 1, except that the environmental temperature at which spraying was performed after the cement concrete and the spraying quick-setting admixture were mixed together was changed to that shown in Table 13.
[0085] [Table 13] [Industrial Applicability]
[0086] The quick-setting admixture for spraying of the present invention can be suitably used for cement concrete to be sprayed onto exposed natural ground surfaces such as tunnels and slopes of roads, railways, and water channels.
Claims
1. A cement concrete containing polyethylene oxide having a mass average molecular weight of 100,000 to 5,000,000; a spraying quick-setting admixture that is substantially free of alkali metal aluminates and alkali metal hydroxides and contains calcium aluminate and aluminum sulfate; The sprayed quick-setting admixture has an aluminum sulfate content of 5 to 105 parts by mass relative to 100 parts by mass of the calcium aluminate, and the aluminum sulfate has a magnesium and calcium content of 0.007 to 4 mass% in terms of oxide.
2. 2. The low-dust sprayed concrete according to claim 1, wherein the aluminum sulfate contains 0.005 to 2% by mass of CaO and 0.002 to 2% by mass of MgO.
3. 3. The low-dust sprayed concrete according to claim 1 or 2, further comprising 5 to 105 parts by mass of an alkaline earth metal hydroxide per 100 parts by mass of the calcium aluminate.
4. The low-dust sprayed concrete according to any one of claims 1 to 3, further comprising at least one selected from the group consisting of alkali metal carbonates, alkaline earth metal carbonates, and alkaline earth metal sulfates.
5. 5. The low-dust sprayed concrete according to claim 4, which contains the alkali metal carbonate, and the content of the alkali metal carbonate is 1 to 30 mass %.
6. The low-dust sprayed concrete according to any one of claims 1 to 5, wherein the proportion of aluminum sulfate having a particle size of 10 μm or less in the aluminum sulfate is 1 to 40 mass%.
7. 7. The low-dust sprayed concrete according to claim 1, wherein the aluminum sulfate is a hydrate having 4 to 12 water of hydration.
8. The low-dust sprayed concrete according to any one of claims 1 to 7, wherein the mass average molecular weight of the polyethylene oxide is 100,000 to 5,000,000.
9. A low-dust spraying method comprising the steps of: transporting the cement concrete and the spraying quick-setting admixture contained in the low-dust sprayed concrete according to any one of claims 1 to 8 to a mixing pipe by compressed air; mixing and joining the cement concrete and the spraying quick-setting admixture in the mixing pipe; and ejecting and spraying the mixed concrete from a spray nozzle.
10. A low-dust spraying method as described in claim 9, in which the cement concrete is transported by compressed air a distance of 4 m or more before being mixed with the spray quick-setting admixture, and after the cement concrete and the spray quick-setting admixture have been mixed and joined together, the cement concrete is transported a distance of 1.5 m or more, and then discharged and sprayed from the spray nozzle.
Citation Information
Patent Citations
JP1975026928A
Parity prediction system of shifter
JP1981027457A
Aid for dry spray art
JP1983015056A
Production of 2-acylphenol compound
JP1985004149A
accelerator
JP1986026538A