Improved safety of lithium secondary batteries

By using a specific electrolyte additive and high-nickel manganese positive electrode materials, the lithium secondary battery forms a protective film, addressing gas generation and ion precipitation issues, thereby improving performance and safety under high temperatures.

JP7580852B2Active Publication Date: 2024-11-12LG ENERGY SOLUTION LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023539196
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2022-10-20
Filing Date
2022-10-21
Publication Date
2024-11-12
Estimated Expiration
2042-10-21

AI Technical Summary

Technical Problem

The generation of gas under high temperature conditions and the precipitation of metal ions on the electrode surface in lithium secondary batteries, leading to a decrease in open circuit voltage (OCV) and reduced battery performance and safety.

Method used

Incorporation of a specific electrolyte additive represented by Chemical Formula 1 and optionally Chemical Formula 2 in the non-aqueous electrolyte, along with a positive electrode active material containing high concentrations of nickel and manganese, to form a protective film on the electrode surfaces, preventing gas generation and ion leaching.

Benefits of technology

The solution effectively reduces gas generation and ion leaching, enhancing battery performance and high-temperature safety by maintaining lower resistance and higher capacity retention.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007580852000001
    Figure 0007580852000001
  • Figure 0007580852000002
    Figure 0007580852000002
  • Figure 0007580852000003
    Figure 0007580852000003
Patent Text Reader

Abstract

The present invention relates to a secondary battery with improved high-temperature safety, which uses a positive electrode active material containing high concentrations of nickel and / or manganese and a specific additive in a non-aqueous electrolyte to uniformly form a coating on the surface of the electrode during activation of the battery, thereby preventing a large amount of gas from being generated under high-temperature conditions and effectively preventing metal ions from eluting from the electrode, increasing cell resistance, and decreasing capacity, thereby effectively improving the performance and high-temperature safety of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium secondary battery with improved safety.

[0002] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0155470 dated November 12, 2021 and Korean Patent Application No. 10-2022-0135402 dated October 20, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference. [Background technology]

[0003] In recent years, secondary batteries have been widely used not only in small devices such as portable electronic devices, but also in medium- to large-sized devices such as battery packs for hybrid and electric vehicles and power storage devices. Examples of such secondary batteries include non-aqueous electrolyte batteries such as lithium ion batteries, lithium batteries, lithium ion capacitors, and sodium ion batteries.

[0004] Among such non-aqueous electrolyte batteries, lithium ion batteries are used by injecting an electrolyte into a battery cell including a positive electrode containing a positive electrode active material capable of intercalating and deintercalating lithium, and a negative electrode containing a negative electrode active material capable of intercalating and deintercalating lithium. In particular, the electrolyte uses an organic solvent in which a lithium salt is dissolved, and is important in determining the stability and performance of a lithium secondary battery.

[0005] For example, LiPF6, which is the most commonly used lithium salt in electrolytes, reacts with the electrolyte solvent to accelerate the depletion of the solvent and generate HF. The generated HF not only generates a large amount of gas under high temperature conditions, but also dissolves metal ions from the positive electrode active material. If the dissolved metal ions are generated in the form of precipitation on the surface of the negative electrode, it causes an increase in the negative electrode potential and a drop in the OCV of the cell, which reduces not only the performance of the battery but also its lifespan and high-temperature safety. Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, an object of the present invention is to provide a technology for forming a coating on the surface of an electrode to reduce the precipitation of metal ions on the surface of the electrode, thereby suppressing gas generation under high temperature conditions, while improving the OCV drop of the battery. [Means for solving the problem]

[0007] In order to solve the above-mentioned problems, in one embodiment, the present invention provides a lithium secondary battery including an electrolyte composition including an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, a non-aqueous organic solvent, a lithium salt, and an electrolyte additive for a secondary battery including a compound represented by the following Chemical Formula 1:

[0008] [ka]

[0009] In the above formula 1, R1 each independently represents a single bond, an alkylene group having 1 to 10 carbon atoms, or

[0010] [ka] wherein R2 is independently a hydrogen atom, an acrylate group, or a methacrylate group; R3 is a single bond or an alkylene group having 1 to 4 carbon atoms; and a is an integer of 1 to 10.

[0011] Specifically, each R1 independently represents a single bond, a methylene group, an ethylene group, a propylene group, or

[0012] [ka]

[0013] where R3 is a single bond or an ethylene group, and a can be an integer from 1 to 5.

[0014] More specifically, the compound represented by Chemical Formula 1 above may be one or more of the compounds represented by the following <Structural Formula 1> to <Structural Formula 8>.

[0015] [ka]

[0016] The compound represented by Chemical Formula 1 may be included in an amount of 0.01 to 5 wt % based on the total weight of the electrolyte composition.

[0017] In addition, the electrolyte composition may further include a compound represented by the following Chemical Formula 2.

[0018] [ka]

[0019] In Chemical Formula 2, R4 is independently an alkylene group having 1 to 10 carbon atoms or

[0020] [ka]

[0021] wherein R5 is hydrogen or an alkyl group having 1 to 4 carbon atoms, R6 is a single bond or an alkylene group having 1 to 4 carbon atoms, and b is an integer of 1 to 10.

[0022] As an example, the compound represented by Chemical Formula 2 may include a compound represented by Chemical Formula 3 below.

[0023] [ka]

[0024] In addition, the compound represented by Chemical Formula 2 may be included in an amount of 0.01 to 3 wt % based on the total weight of the electrolyte composition.

[0025] In addition, the lithium salts are LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, and (CF3SO2)2NLi.

[0026] The non-aqueous organic solvent may also include N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphate triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0027] In addition, the positive electrode may include one or more positive electrode active materials selected from the lithium metal oxides represented by the following Chemical Formula 4 and Chemical Formula 5.

[0028] [Chemical formula 4] Li x [Ni y Co zMn w M 1 v ]O2

[0029] [Chemical formula 5] LiM 2 p Mn (2-p) O4

[0030] In the above Chemical Formula 4 and Chemical Formula 5, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and x, y, z, w, and v are 1.0≦x≦1.30, 0.5≦y<1, 0 <z≦0.3、0<w≦0.3、0≦v≦0.1であり、y+z+w+v=1であり、M 2 is Ni, Co or Fe, and p is in the range of 0.05≦p≦0.6.

[0031] Specifically, the positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2, LiNi 0.7 Co 0.1 Mn 0.1 Al 0.1 O2, LiNi 0.7 Mn 1.3 O4, LiNi 0.5 Mn 1.5 O4 and LiNi 0.3 Mn 1.7 O4.

[0032] The negative electrode is composed of a negative electrode active material including a carbon material and a silicon material, and the silicon material is silicon (Si), silicon carbide (SiC), and silicon oxide (SiO q , where 0.8≦q≦2.5) may be included.

[0033] The silicon material may be included in an amount of 1 to 20 wt % based on the total weight of the negative electrode active material. Effect of the Invention

[0034] The secondary battery according to the present invention uses a positive electrode active material containing high concentrations of nickel and / or manganese, together with a specific additive component in a non-aqueous electrolyte, so that a coating is uniformly formed on the surface of the electrode during activation of the battery, which can prevent a large amount of gas from being generated under high temperature conditions and can effectively prevent metal ions from eluting from the electrode, increasing the cell resistance and decreasing the capacity, thereby effectively improving the performance and high temperature safety of the battery. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0035] The present invention is susceptible to various modifications and may have various embodiments, and therefore, specific embodiments are described in detail in the detailed description.

[0036] However, this is not intended to limit the invention to the particular embodiment, but should be understood to include all modifications, equivalents, or alternatives falling within the spirit and scope of the present invention.

[0037] In the present invention, terms such as "comprise" and "have" are intended to specify the presence of features, numbers, steps, operations, components, parts, or combinations thereof described in the specification, but should be understood as not precluding the presence or additional possibility of one or more other features, numbers, steps, operations, components, parts, or combinations thereof.

[0038] In addition, in the present invention, when a layer, film, region, plate, or other portion is described as being "on" another portion, this includes not only the case where it is "directly on" the other portion, but also the case where there is another portion in between. Conversely, when a layer, film, region, plate, or other portion is described as being "under" the other portion, this includes not only the case where it is "directly under" the other portion, but also the case where there is another portion in between. In addition, in the present application, being "on" can include not only the case where it is located at the top, but also the case where it is located at the bottom.

[0039] In addition, in the present invention, "including as a main component" may mean including 50 wt% or more, 60 wt% or more, 70 wt% or more, 80 wt% or more, 90 wt% or more, or 95 wt% or more of the defined component based on the total weight. For example, "including graphite as a main component as a negative electrode active material" may mean including 50 wt% or more, 60 wt% or more, 70 wt% or more, 80 wt% or more, 90 wt% or more, or 95 wt% or more of graphite based on the total weight of the negative electrode active material, and in some cases, may mean that the entire negative electrode active material is made of graphite and includes 100 wt% of graphite.

[0040] The present invention will now be described in more detail.

[0041] <Lithium secondary battery> Furthermore, in one embodiment, the present invention provides a lithium secondary battery including an electrolyte composition comprising an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode, a non-aqueous organic solvent, a lithium salt, and an electrolyte additive for a secondary battery including a compound represented by the following Chemical Formula 1:

[0042] [ka]

[0043] In the above formula 1, R1 each independently represents a single bond, an alkylene group having 1 to 10 carbon atoms, or

[0044] [ka]

[0045] wherein R2 is independently a hydrogen atom, an acrylate group, or a methacrylate group; R3 is a single bond or an alkylene group having 1 to 4 carbon atoms; and a is an integer of 1 to 10.

[0046] The lithium secondary battery according to the present invention includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, a separator interposed between the positive electrode and the negative electrode, and the nonaqueous electrolyte composition containing the lithium salt of the present invention described above.

[0047] In this case, the positive electrode contains a lithium metal oxide containing nickel and / or manganese at a high concentration / content as a positive electrode active material, and the electrolyte composition contains an electrolyte additive of a specific component, which can prevent a large amount of gas from being generated under high temperature conditions, and can effectively prevent metal ions from being eluted from the electrode, which can increase the cell resistance and reduce the capacity, thereby effectively improving the performance and high temperature safety of the battery.

[0048] Specifically, the positive electrode includes a positive electrode mixture layer produced by applying a positive electrode active material onto a positive electrode current collector, drying and pressing the positive electrode mixture layer, and may further include a conductive material, a binder, other additives, and the like as necessary.

[0049] Here, the positive electrode active material is a material that can undergo an electrochemical reaction on a positive electrode current collector, and may include at least one of lithium metal oxides represented by the following Chemical Formula 4 and Chemical Formula 5 that can reversibly intercalate and deintercalate lithium ions.

[0050] [Chemical formula 4] Li x [Ni y Co z Mn w M 1 v ]O2

[0051] [Chemical formula 5] LiM 2 p Mn (2-p) O4

[0052] In the above Chemical Formula 4 and Chemical Formula 5, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo, and x, y, z, w, and v are 1.0≦x≦1.30, 0.5≦y<1, 0 <z≦0.3、0<w≦0.3、0≦v≦0.1であり、y+z+w+v=1であり、M 2 is Ni, Co or Fe, and p is in the range of 0.05≦p≦0.6.

[0053] The lithium metal oxides represented by Chemical Formula 4 and Chemical Formula 5 are materials containing high amounts of nickel (Ni) and manganese (Mn), respectively, and have the advantage of being able to stably supply high-capacity and / or high-voltage electricity when used as positive electrode active materials. In addition, a high charging potential of about 4.0 V or more is required to form a coating on the surface of the positive electrode and / or negative electrode during activation of a secondary battery. Unlike conventional positive electrode active materials such as iron phosphate, which have a charging potential of less than 4.0 V, the lithium metal oxides have a high charging potential of about 4.0 V or more, making it easy to form a coating on the electrode.

[0054] In this case, the lithium metal oxide represented by the above chemical formula 4 is LiNi 0.8 Co 0.1 Mn 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.9 Co 0.05 Mn 0.05 O2, LiNi 0.6 Co 0.2 Mn 0.1 Al 0.1 O2, LiNi 0.6 Co 0.2 Mn 0.15 Al 0.05 O2, LiNi 0.7 Co0.1 Mn 0.1 Al 0.1 O2, etc., and the lithium metal oxide represented by the above formula 5 is LiNi 0.7 Mn 1.3 O4, LiNi 0.5 Mn 1.5 O4, LiNi 0.3 Mn 1.7 O4, etc., which may be used alone or in combination.

[0055] In addition, the positive electrode may use a positive electrode current collector that has high conductivity without inducing chemical changes in the battery. For example, stainless steel, aluminum, nickel, titanium, calcined carbon, etc. may be used, and in the case of aluminum or stainless steel, those that have been surface-treated with carbon, nickel, titanium, silver, etc. may be used. In addition, the average thickness of the current collector may be suitably 3 to 500 μm, taking into consideration the conductivity and total thickness of the positive electrode to be manufactured.

[0056] Similarly to the positive electrode, the negative electrode includes a negative electrode mixture layer produced by applying a negative electrode active material onto a negative electrode current collector, drying and pressing the negative electrode active material, and may further include a conductive material, a binder, other additives, and the like as necessary.

[0057] The negative electrode active material may include a carbon material and a silicon material. Specifically, the carbon material means a material mainly composed of carbon atoms, and such a carbon material may include at least one selected from the group consisting of natural graphite, artificial graphite, expanded graphite, non-graphitizable carbon, carbon black, acetylene black, and ketjen black. The silicon material means a material mainly composed of silicon atoms, and such a silicon material may include silicon (Si), silicon carbide (SiC), silicon monoxide (SiO), or silicon dioxide (SiO2) alone or in combination. When silicon monoxide (SiO) and silicon dioxide (SiO2) are uniformly mixed or composited as the silicon (Si)-containing material and included in the negative electrode composite layer, they are called silicon oxide (SiO q , where 0.8≦q≦2.5).

[0058] In addition, the silicon material may be included in an amount of 1 to 20 wt % based on the total weight of the negative electrode active material, specifically, 3 to 10 wt %, 8 to 15 wt %, 13 to 18 wt %, or 2 to 8 wt %. The present invention can maximize the energy density of the battery by adjusting the content of the silicon material within the above content range.

[0059] The negative electrode current collector is not particularly limited as long as it has high conductivity without inducing chemical changes in the battery, and may be, for example, copper, stainless steel, nickel, titanium, calcined carbon, etc., and in the case of copper or stainless steel, it may be surface-treated with carbon, nickel, titanium, silver, etc. The average thickness of the negative electrode current collector may be suitably 1 to 500 μm, taking into consideration the conductivity and total thickness of the negative electrode to be manufactured.

[0060] Meanwhile, the separator interposed between the positive and negative electrodes of each unit cell is an insulating thin film having high ion permeability and mechanical strength, and is not particularly limited as long as it is a commonly used material in the art, specifically, a material containing at least one polymer selected from polypropylene, polyethylene, and polyethylene-propylene copolymers having chemical resistance and hydrophobicity may be used. The separator may have the form of a porous polymer substrate such as a sheet or nonwoven fabric containing the above-mentioned polymer, and may have the form of a composite separator in which organic or inorganic particles are coated on the porous polymer substrate with an organic binder. The separator may have an average pore diameter of 0.01 to 10 μm and an average thickness of 5 to 300 μm.

[0061] Furthermore, the secondary battery contains the above-mentioned nonaqueous electrolyte composition according to the present invention as an electrolyte.

[0062] The electrolyte composition may be a non-aqueous electrolyte composition, which is a liquid electrolyte having a configuration including a lithium salt and an electrolyte additive in a non-aqueous organic solvent, wherein the electrolyte additive includes a compound represented by the following Chemical Formula 1:

[0063] [ka]

[0064] In the above formula 1, R1 each independently represents a single bond, an alkylene group having 1 to 10 carbon atoms, or

[0065] [ka]

[0066] wherein R2 is independently a hydrogen atom, an acrylate group, or a methacrylate group; R3 is a single bond or an alkylene group having 1 to 4 carbon atoms; and a is an integer of 1 to 10.

[0067] The compound represented by Chemical Formula 1 includes a mother nucleus having a structure in which an acrylate group is bonded to two or more oxygen atoms of a phosphate via an unsaturated hydrocarbon chain and / or an alkylene glycol unit, and thus can uniformly form an organic and / or inorganic coating on the surface of the positive electrode and / or negative electrode when the secondary battery is activated. As a result, the electrolyte additive can suppress the electrolyte from being decomposed and generating gas when the battery is exposed to high temperatures, and can improve the phenomenon of an increase in resistance and / or a decrease in capacity of the battery, thereby further improving the performance and high temperature safety of the battery.

[0068] For this purpose, in the compound represented by the above formula 1, R1 is independently a single bond, an alkylene group having 1 to 6 carbon atoms, or

[0069] [ka]

[0070] wherein each R2 is independently a hydrogen atom, an acrylate group, or a methacrylate group; R3 is a single bond, a methylene group, or an ethylene group; and a can be an integer from 1 to 10.

[0071] Specifically, each R1 independently represents a single bond, a methylene group, an ethylene group, a propylene group, or

[0072] [ka]

[0073] where R3 is a single bond or an ethylene group, and a can be an integer from 1 to 5.

[0074] As an example, the compound represented by Chemical Formula 1 above may be one or more of the compounds represented by the following <Structural Formula 1> to <Structural Formula 8>.

[0075] [ka]

[0076] As described above, the electrolyte additive contains a mother nucleus having a structure in which an acrylate group is bonded to two or more oxygen atoms of a phosphate via an unsaturated hydrocarbon chain and / or an alkylene glycol unit, and therefore can directly participate in the solvation shell of lithium ions even at low potential during battery activation, thereby uniformly forming an inorganic coating on the surface of the negative electrode through a reduction reaction, and at the same time, can uniformly form an inorganic coating on the surface of the positive electrode through an oxidation reaction.

[0077] In addition, the compound represented by Chemical Formula 1 may be included in the electrolyte composition at a specific content. Specifically, the compound represented by Chemical Formula 1 may be included in the electrolyte composition at 0.01 to 5 wt % based on the total weight of the electrolyte composition, and more specifically, the compound represented by Chemical Formula 1 may be included in the electrolyte composition at 0.05 to 3 wt %, 0.5 to 2.5 wt %, 0.5 to 2.0 wt %, or 0.7 to 1.8 wt % based on the total weight of the electrolyte composition. The present invention can prevent the electrolyte additive from being used in an excessive amount outside the above range, which increases the resistance of the battery at high temperatures and reduces the capacity. In addition, the present invention can prevent the electrolyte additive from being used in an extremely small amount outside the above range, which causes the additive to have a weak effect.

[0078] In addition, the electrolyte composition may further include a compound represented by the following Chemical Formula 2 in addition to the electrolyte additive represented by Chemical Formula 1.

[0079] [ka]

[0080] In Chemical Formula 2, R4 is independently an alkylene group having 1 to 10 carbon atoms or

[0081] [ka]

[0082] wherein R5 is hydrogen or an alkyl group having 1 to 4 carbon atoms, R6 is a single bond or an alkylene group having 1 to 4 carbon atoms, and b is an integer of 1 to 10.

[0083] Specifically, R4 is independently a methylene group, an ethylene group, a propylene group, or

[0084] [ka]

[0085] wherein R5 is independently a hydrogen atom, a methyl group, or an ethyl group; R6 is independently a single bond or a methylene group; and b is an integer of 1 to 4.

[0086] As an example, the compound represented by Chemical Formula 2 may include a compound represented by Chemical Formula 3 below.

[0087] [ka]

[0088] The compound represented by Chemical Formula 2 contains a double bond at its terminal and participates in the formation of a coating on the surface of the electrode during activation of the battery together with the electrolyte additive, thereby suppressing the elution of metal generated from the positive electrode active material, while containing a phosphate group and an amide group, thereby improving the durability and electrical performance of the battery at high temperatures.

[0089] In this case, the compound represented by the formula 2 may be included in the electrolyte composition in a specific content. Specifically, the compound represented by the formula 2 may be included in the electrolyte composition in an amount of 0.01 to 3 wt %, more specifically, in an amount of 0.05 to 3 wt %, 0.1 to 1 wt %, or 0.3 to 0.8 wt % based on the total weight of the electrolyte composition. The present invention can prevent the use of an excessive amount of the compound represented by the formula 4 outside the above range, which increases the viscosity of the electrolyte composition and reduces the wettability of the electrodes and the separator. In addition, the present invention can prevent the use of a small amount of the electrolyte additive outside the above range, which causes the additive to have a weak effect.

[0090] Meanwhile, the lithium salt used in the electrolyte composition may be any salt used in non-aqueous electrolytes in the art without any particular limitation. Specifically, the lithium salt may be LiCl, LiBr, LiI, LiClO4, LiBF4, LiB 10 Cl 10 , LiPF6, LiCF3SO3, LiCF3CO2, LiAsF6, LiSbF6, LiAlCl4, CH3SO3Li, and (CF3SO2)2NLi.

[0091] The concentration of these lithium salts is not particularly limited, but the lower limit of the preferred concentration range is 0.5 mol / L or more, specifically 0.7 mol / L or more, more specifically 0.9 mol / L or more, and the upper limit of the preferred concentration range is 2.5 mol / L or less, specifically 2.0 mol / L or less, more specifically 1.5 mol / L or less. If the concentration of the lithium salt is below 0.5 mol / L, the ionic conductivity decreases, and the cycle characteristics and output characteristics of the nonaqueous electrolyte battery may decrease. If the concentration of the lithium salt exceeds 2.5 mol / L, the viscosity of the electrolyte for the nonaqueous electrolyte battery increases, which may also decrease the ionic conductivity, and may decrease the cycle characteristics and output characteristics of the nonaqueous electrolyte battery.

[0092] In addition, when a large amount of lithium salt is dissolved in a non-aqueous organic solvent at once, the liquid temperature may rise due to the heat of dissolution of the lithium salt. If the temperature of the non-aqueous organic solvent rises significantly due to the heat of dissolution of the lithium salt, in the case of a lithium salt containing fluorine, decomposition may be promoted and hydrogen fluoride (HF) may be generated. Hydrogen fluoride (HF) is undesirable because it causes deterioration of battery performance. Therefore, the temperature when dissolving the lithium salt in the non-aqueous organic solvent is not particularly limited, but may be adjusted to -20 to 80°C, specifically 0 to 60°C.

[0093] In addition, the non-aqueous organic solvent used in the electrolyte composition may be any organic solvent used in the art for non-aqueous electrolytes without any particular limitations. Specifically, examples of the non-aqueous organic solvent that can be used include aprotic organic solvents such as N-methyl-2-pyrrolidinone, ethylene carbonate (EC), propylene carbonate, butylene carbonate, dimethyl carbonate (DMC), diethyl carbonate (DEC), γ-butyrolactone, 1,2-dimethoxyethane (DME), tetrahydroxyfuran (franc), 2-methyltetrahydrofuran, dimethylsulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate, and ethyl propionate.

[0094] The non-aqueous solvent used in the present invention may be one type alone, or two or more types may be mixed in any combination and ratio according to the purpose. Among these, propylene carbonate, ethylene carbonate, fluoroethylene carbonate, diethyl carbonate, dimethyl carbonate, and ethyl methyl carbonate are particularly preferred from the viewpoints of electrochemical stability against oxidation and reduction and chemical stability against heat and reaction with solutes.

[0095] On the other hand, the electrolyte composition may further contain additives in addition to the basic components described above. As long as the gist of the present invention is not impaired, additives generally used in the nonaqueous electrolyte of the present invention may be added at any ratio. Specifically, compounds having an overcharge prevention effect, an anode film formation effect, and a cathode protection effect, such as cyclohexylbenzene, biphenyl, t-butylbenzene, vinylene carbonate, vinylethylene carbonate, difluoroanisole, fluoroethylene carbonate, propane sultone, succinonitrile, and dimethylvinylene carbonate, may be mentioned. In addition, as in the case of use in a nonaqueous electrolyte battery called a lithium polymer battery, it is also possible to use the electrolyte for a nonaqueous electrolyte battery by solidifying it with a gelling agent or a crosslinked polymer.

[0096] The present invention will now be described in more detail with reference to examples and experimental examples.

[0097] However, the following examples and experimental examples are merely illustrative of the present invention, and the contents of the present invention are not limited to the following examples and experimental examples.

[0098] <Production Examples 1 to 12. Production of Electrolyte Compositions> LiPF6 was dissolved as a lithium salt at a concentration of 1M in a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed at a volume ratio of 3:7, and the electrolyte additive represented by Chemical Formula 1 and the compound represented by Chemical Formula 3 were dissolved in the amounts shown in Table 1 below relative to the total weight of the electrolyte to prepare a non-aqueous electrolyte composition.

[0099] [Table 1]

[0100] [ka]

[0101] <Examples 1 to 12. Production of lithium secondary batteries> The positive electrode active material is LiNi with a particle size of 5 μm. 0.8 Co 0.1 Mn 0.05 Al 0.05 O2 was prepared and mixed with polyvinylidene fluoride (PVDF) as a carbon-based conductive agent and binder in a weight ratio of 94:3:3 in N-methylpyrrolidone (NMP) to form a slurry, which was then cast onto an aluminum sheet, dried in a vacuum oven at 120°C, and rolled to produce a positive electrode.

[0102] Separately, a negative electrode active material was prepared by mixing artificial graphite and silicon oxide (SiO2) in a weight ratio of 9:1. 97 parts by weight of the negative electrode active material and 3 parts by weight of styrene-butadiene rubber (SBR) were mixed with water to form a slurry, which was then cast onto a copper sheet, dried in a vacuum oven at 130°C, and rolled to produce a negative electrode.

[0103] The positive and negative electrodes obtained above were inserted into a case with a separator made of 18 μm polypropylene between them, and then the electrolyte compositions (5 ml) prepared in the above Preparation Examples 1 to 12 were poured in as shown in Table 2 below to prepare pouch-type 2.1 Ah class small lithium secondary batteries.

[0104] [Table 2]

[0105] <Comparative Example 1. Manufacture of Lithium Secondary Battery> A lithium secondary battery was manufactured in the same manner as in Example 1, except that an electrolyte was used in which LiPF6 was dissolved as a lithium salt at a concentration of 1 M in a solvent in which ethylene carbonate (EC) and ethyl methyl carbonate (EMC) were mixed in a volume ratio of 3:7 without using any electrolyte additive.

[0106] <Experimental Example> In order to evaluate the effect of reducing gas generation and the high temperature safety of the lithium secondary battery according to the present invention, the following experiment was carried out.

[0107] a) Analysis of changes in resistance and capacity of secondary batteries after high-temperature storage The secondary batteries manufactured in the examples and comparative examples were stored at 60° C. for 12 weeks, and the changes in resistance and capacity of the batteries were observed.

[0108] Specifically, each secondary battery was activated by charging / discharging twice at 0.2C / 0.5C, and then a charge / discharge experiment was conducted once each with a charge / discharge current density of 0.5C / 0.2C, a charge cut-off voltage of 4.8V (Li / graphite), and a discharge cut-off voltage of 3.0V (Li / graphite).

[0109] The battery was then fully charged at 0.33C and 4.2V, and stored at a high temperature of 60°C while measuring the resistance and capacity of the battery every two weeks. After measuring the resistance and capacity of the battery, the battery was charged to a fully charged state and stored. The change in the resistance and capacity of the battery was calculated based on the initial resistance and capacity of the battery, and the results are shown in Table 3 below.

[0110] B) Analysis of gas generation from secondary batteries stored at high temperatures The secondary batteries manufactured in the examples and comparative examples were stored at 60° C. for 12 weeks, and the amount of gas generated from the batteries was analyzed every two weeks. Specifically, after charging / discharging the secondary batteries at activation twice at 0.2 C / 0.5 C, a charge / discharge experiment was performed once each at a charge / discharge current density of 0.5 C / 0.2 C, a charge cut-off voltage of 4.8 V (Li / graphite), and a discharge cut-off voltage of 3.0 V (Li / graphite).

[0111] Then, the secondary battery was fully charged at 0.33C and 4.2V, and stored for 12 weeks at a high temperature of 60° C. After 12 weeks, the secondary battery was degassed by applying pressure to the surface, and the amount of gas degassed was measured. The results are shown in Table 3 below.

[0112] [Table 3]

[0113] As shown in Table 3 above, the secondary batteries of the examples contain a positive electrode active material containing a high content of nickel, as well as an electrolyte composition containing the compound represented by Chemical Formula 1 as an electrolyte additive, and therefore have excellent electrical performance and safety at high temperatures. Specifically, the secondary batteries of the examples showed significantly less gas generation, less increase in battery resistance, and higher capacity retention even when exposed to high temperature conditions, compared to the secondary batteries of the comparative examples.

[0114] From these results, the secondary battery according to the present invention uses a positive electrode active material containing a high concentration of nickel and / or manganese as well as an additive of a specific component in a non-aqueous electrolyte solution to uniformly form a coating on the surface of the electrode during activation of the battery, thereby making it possible to prevent the generation of a large amount of gas under high temperature conditions and effectively prevent metal ions from eluting from the electrode, increasing the cell resistance and decreasing the capacity, thereby effectively improving the performance and high temperature safety of the battery.

[0115] Although the present invention has been described above with reference to preferred embodiments, it will be understood that a person skilled in the art or having ordinary knowledge in the art can make various modifications and variations to the present invention without departing from the spirit and technical scope of the present invention as described in the claims below.

[0116] Therefore, the technical scope of the present invention should not be limited to the contents described in the Summary of the Invention of the specification, but should be defined by the claims.

Claims

1. an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; The present invention relates to an electrolyte composition comprising a non-aqueous organic solvent, a lithium salt, a compound represented by the following Chemical Formula 1, and an electrolyte additive for a secondary battery comprising a compound represented by the following Chemical Formula 2: 【Chemistry 1】 In the above Chemical Formula 1, R 1 each independently represents a single bond, an alkylene group having 1 to 10 carbon atoms, or 【Chemistry 2】 and R 2 are each independently a hydrogen atom, an acrylate group, or a methacrylate group; R 3 is a single bond or an alkylene group having 1 to 4 carbon atoms, a is an integer from 1 to 10; 【Chemistry 3】 In Chemical Formula 2, R 4 independently represents an alkylene group having 1 to 10 carbon atoms, or 【Chemistry 4】 and R 5 is hydrogen or an alkyl group having 1 to 4 carbon atoms; R 6 is a single bond or an alkylene group having 1 to 4 carbon atoms; A lithium secondary battery, wherein b is an integer from 1 to 10.

2. R 1 each independently represents a single bond, a methylene group, an ethylene group, a propylene group, or 【Chemistry 5】 and R 3 is a single bond or an ethylene group, 2. The lithium secondary battery according to claim 1, wherein a is an integer of 1 to 5.

3. 2. The lithium secondary battery of claim 1, wherein the compound represented by Chemical Formula 1 is at least one compound selected from the following <Structural Formula 1> to <Structural Formula 8>. 【Chemistry 6】

4. 2. The lithium secondary battery according to claim 1, wherein the compound represented by Chemical Formula 1 is contained in an amount of 0.01 to 5 wt % based on the total weight of the electrolyte composition.

5. The lithium secondary battery according to claim 1 , wherein the compound represented by Chemical Formula 2 includes a compound represented by Chemical Formula 3: 【Chemistry 7】

6. 2. The lithium secondary battery according to claim 1, wherein the compound represented by Chemical Formula 2 is contained in an amount of 0.01 to 3 wt % based on the total weight of the electrolyte composition.

7. Lithium salts include LiCl, LiBr, LiI, and LiClO. 4 , LiBF 4 , LiB 10 C 10 , LiPF 6 , LiCF 3 SO 3 , LiCF 3 CO 2 , LiAsF 6 , LiSbF 6 , LiAlCl 4 , C.H. 3 SO 3 Li and (CF 3 SO 2 ) 2 2. The lithium secondary battery according to claim 1, comprising one or more selected from the group consisting of NLi.

8. The non-aqueous organic solvent includes N-methyl-2-pyrrolidinone, ethylene carbonate, propylene carbonate, butylene carbonate, dimethyl carbonate, diethyl carbonate, γ-butyrolactone, 1,2-dimethoxyethane, tetrahydroxyfuran, 2-methyltetrahydrofuran, dimethyl sulfoxide, 1,3-dioxolane, formamide, dimethylformamide, dioxolane, acetonitrile, nitromethane, methyl formate, methyl acetate, phosphoric acid triester, trimethoxymethane, dioxolane derivatives, sulfolane, methylsulfolane, 1,3-dimethyl-2-imidazolidinone, propylene carbonate derivatives, tetrahydrofuran derivatives, ethers, methyl propionate and ethyl propionate. The lithium secondary battery according to claim 1.

9. The lithium secondary battery according to claim 1 , wherein the positive electrode comprises at least one positive electrode active material selected from the group consisting of lithium metal oxides represented by the following Chemical Formula 4 and Chemical Formula 5: [Chemical formula 4] Li x [Ni y Co z Mn w M 1 v ]O 2 [Chemical formula 5] LiM 2 p Mn (2-p) O 4 In the above Chemical Formula 4 and Chemical Formula 5, M 1 is one or more elements selected from the group consisting of W, Cu, Fe, V, Cr, Ti, Zr, Zn, Al, In, Ta, Y, La, Sr, Ga, Sc, Gd, Sm, Ca, Ce, Nb, Mg, B, and Mo; x, y, z, w and v are each 1.0≦x≦1.30, 0.5≦y<1, 0<z≦0.3, 0<w≦0.3, 0≦v≦0.1, and y+z+w+v=1; M 2 is Ni, Co or Fe, p is in the range of 0.05≦p≦0.

6.

10. The positive electrode active material is LiNi 0.8 Co 0.1 Mn 0.1 O 2 , LiNi 0.6 Co 0.2 Mn 0.2 O 2 , LiNi 0.9 Co 0.05 Mn 0.05 O 2 , LiNi 0.6 Co 0.2 Mn 0.1 A 0.1 O 2 , LiNi 0.6 Co 0.2 Mn 0.15 A 0.05 O 2 , LiNi 0.7 Co 0.1 Mn 0.1 A 0.1 O 2 , LiNi 0.7 Mn 1.3 O 4 , LiNi 0.5 Mn 1.5 O 4 and LiNi 0.3 Mn 1.7 O 4 The lithium secondary battery according to claim 9 , comprising one or more selected from the group consisting of:

11. The negative electrode is composed of a negative electrode active material including a carbon material and a silicon material, The silicon materials include silicon (Si), silicon carbide (SiC) and silicon oxide (SiO q 2. The lithium secondary battery according to claim 1 , wherein q is selected from the group consisting of 0.8≦q≦2.

5.

12. The lithium secondary battery according to claim 11, wherein the silicon material is contained in an amount of 1 to 20 wt % based on the total weight of the negative electrode active material.

Citation Information

Patent Citations

  • Nonaqueous electrolyte and nonaqueous electrolyte secondary battery using the same

    JP2012084384A

  • Nonaqueous electrolytic solution, electrode, and electrochemical device comprising nonaqueous electrolytic solution and electrode

    JP2012119092A

  • Secondary batteries containing electrolyte additives

    JP2015525452A

  • Gel polymer electrolyte and electrochemical device containing the same

    JP2016503572A

  • Non-aqueous electrolyte for lithium secondary battery and lithium secondary battery comprising the same

    KR1020210031158A