Porous carbon and preparation method thereof, silicon-carbon negative electrode material, and preparation method of silicon-carbon negative electrode material

Porous carbon is filled and sealed through biomass carbon source heat treatment and chemical vapor deposition technology, solving the problem of excessive micropores in small and medium sizes of porous carbon, improving the performance and preparation efficiency of silicon-carbon negative electrode materials, and achieving more efficient silicon Carbon anode material preparation.

CN117776183BActive Publication Date: 2024-11-15ZHEJIANG ZHONGNING SILICON INDUSTRY CO LTD

Patent Information

Application Number
CN202311566243.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Priority Date
2022-11-22
Filing Date
2023-11-22
Publication Date
2024-11-15
Estimated Expiration
2043-11-22

AI Technical Summary

Technical Problem

It is difficult to control the pore size in the existing porous carbon preparation process, resulting in excessive micropores in small sizes, affecting the performance and industrial application of silicon carbon anode materials.

Method used

The biomass carbon source is used to prepare porous carbon crude products through heat treatment, and the pore filling and sealing treatment is carried out using chemical vapor deposition technology to control the pore size, reduce the specific surface area, and improve the mechanical properties and mechanical parameters of silicon carbon anode materials.

Benefits of technology

Effectively seal the tiny pores in porous carbon, improve the deposition efficiency and performance of silicon carbon anode material, reduce the preparation cost, and improve mechanical properties and mechanical parameters.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117776183B_ABST
    Figure CN117776183B_ABST
Patent Text Reader

Abstract

The present invention provides a porous carbon and a preparation method thereof, a silicon-carbon negative electrode material, and a preparation method of a silicon-carbon negative electrode material. The porous carbon is used to prepare a silicon-carbon negative electrode material, and the preparation method of the porous carbon includes: S100, using a biomass carbon source as a raw material, carbonizing the biomass carbon source through heat treatment, and preparing a crude porous carbon; S200, using an organic carbon source, and performing pore filling and sealing treatment on the crude porous carbon prepared by S100 through chemical vapor deposition to obtain a finished porous carbon. The biomass carbon source includes: coconut shells, straws, rice husks, wood, bamboo, bagasse, and nut shells. The present invention can seal the pores of the porous carbon that are too small in size by performing pore filling and sealing treatment on the crude porous carbon, thereby reducing the specific surface area of ​​the porous carbon. Therefore, the porous carbon of the present invention is more suitable for the preparation of silicon-carbon negative electrode materials.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of chemical processes, and in particular to porous carbon and a preparation method thereof, a silicon-carbon negative electrode material, and a preparation method of a silicon-carbon negative electrode material. Background Art

[0002] In the prior art, the preparation methods of porous carbon mainly include activation method and template method. The physical activation method mainly uses water vapor, carbon dioxide, air and other gases as activators, and contacts with carbonized materials at high temperature to activate and form pores. The chemical activation method is a method of adding chemicals such as potassium hydroxide, phosphoric acid, zinc chloride, etc. to the raw materials and heating and activating them in an inert gas medium. The chemical activation method requires the use of a large amount of alkaline particles such as potassium hydroxide and sodium hydroxide. Although the prepared porous carbon has a rich pore structure, it needs to be washed with a large amount of deionized water to reach the use level in order to make the material neutral, and magnetic adsorption is required to remove metal ions. A large amount of wastewater will be generated during the preparation process, which is easy to cause environmental pollution.

[0003] Although the template method can control the pore structure in an orderly manner, the cost of preparing the template is high, and the prepared porous carbon needs to be etched to remove the template, which has a high production cost and is difficult to industrialize. Among them, the template method is divided into a hard template method and a soft template method. The hard template method is to first synthesize a porous molecular sieve, use it as a hard template, and inject a carbon precursor into its pores to form a nano-organic / silicon composite material, and then undergo high-temperature carbonization and template etching technology to finally prepare a porous carbon material. The soft template method uses a surfactant as a template agent, and through the interaction between the surfactant and the carbon source, a porous structure is formed through self-assembly.

[0004] Using biomass carbon such as coconut shells, rice straw, etc. as raw materials, or chemical phenolic resin as raw materials, first undergoing high-temperature oxygen-insulated carbonization in a converter, and then undergoing secondary activation to form pores, we can eventually prepare porous carbon with a large number of pore structures and a high specific surface area.

[0005] Although porous carbon with high specific surface area can be used in fields such as supercapacitors and hydrogen storage adsorption, the porous carbon prepared by traditional processes contains a large number of micropores below 1nm, which cannot contribute to silane vapor deposition. In addition, a large number of micropores below 1nm will cause the porous carbon to have too high specific surface area, which will reduce the initial efficiency when preparing silicon-carbon negative electrode materials, making such porous carbon unsuitable or unable to be used as a substrate for silane vapor deposition. Summary of the invention

[0006] The technical problem to be solved by the present invention is: how to control the pore size of porous carbon and reduce the small-sized micropores of porous carbon.

[0007] To solve the above problems, the present invention provides a method for preparing porous carbon, a silicon-carbon negative electrode material, and a method for preparing a silicon-carbon negative electrode material.

[0008] The porous carbon is used to prepare a silicon-carbon negative electrode material, and the preparation method of the porous carbon includes:

[0009] S100, using a biomass carbon source as a raw material, carbonizing the biomass carbon source through heat treatment, and preparing a crude porous carbon product;

[0010] S200, using an organic carbon source, by chemical vapor deposition, to perform pore filling and sealing treatment on the crude porous carbon product prepared in S100, to obtain the finished porous carbon product.

[0011] In any of the above technical solutions, the biomass carbon source includes at least one of the following or a combination thereof: coconut shell, straw, rice husk, wood, bamboo, bagasse, and nut shell.

[0012] In any of the above technical solutions, the organic carbon source includes at least one of the following or a combination thereof: methane, ethane, propane, acetylene, ethylene, propylene, and toluene.

[0013] In any of the above technical solutions, S100 specifically includes:

[0014] S110, subjecting the biomass carbon source to a first-stage heat treatment in a protective atmosphere and then cooling it;

[0015] S120, subjecting the biomass carbon source to a second-stage heat treatment under a condition of passing water vapor and then cooling the biomass carbon source to obtain a crude porous carbon product;

[0016] The first-stage heat treatment is used to carbonize the biomass carbon source and form pores, and the second-stage heat treatment is used to enlarge the pores of the biomass carbon source.

[0017] In any of the above technical solutions, the second-stage heat treatment enlarges the pores of the biocarbon source to 1 to 3 nm.

[0018] In any of the above technical solutions, the BET specific surface area of ​​the crude porous carbon is greater than or equal to 1800 m 2 ·g -1 , for example, 1800~2000m 2 ·g -1 For example, the proportion of mesopores (>2 nm) in the crude porous carbon is less than or equal to 15%.

[0019] In any of the above technical solutions, the temperature range of the first-stage heat treatment is 750°C to 850°C, and the temperature range of the second-stage heat treatment is 850°C to 900°C. The temperature range of the first-stage heat treatment is preferably 770°C to 850°C. The time of the first-stage heat treatment is preferably 2 to 5 hours, for example, 2.5 hours. The time of the second-stage heat treatment is preferably 3 to 6 hours, for example, 5 hours.

[0020] In any of the above technical solutions, between S110 and S120, it also includes: washing and drying the biomass carbon source that has undergone the first-stage heat treatment and cooling.

[0021] In any of the above technical solutions, after S120, the method further includes: washing and drying the crude porous carbon product that has undergone the second-stage heat treatment and cooling.

[0022] In any of the above technical solutions, S200 specifically includes:

[0023] S210, performing air flow pulverization on the crude porous carbon product so that the particle size of the crude porous carbon product satisfies DV50 of 5 μm to 8 μm;

[0024] S220, sending the crude porous carbon into a fluidized bed reactor, using an organic carbon source, performing chemical vapor deposition under a pressure condition of 0.2 MPa to 0.3 MPa and a temperature condition of 700° C. to 800° C. to obtain the finished porous carbon.

[0025] In S220 of any of the above technical solutions, the temperature condition of the chemical vapor deposition is preferably 720-800°C, for example, 740-760°C.

[0026] In S220 of any of the above technical solutions, the chemical vapor deposition is carried out for 1 to 3 hours under the pressure of 0.2 MPa to 0.3 MPa and the temperature of 700° C. to 800° C. The BET specific surface area of ​​the obtained porous carbon product is 1300 to 1700 m 2 ·g -1 , for example, 1400 to 1600 m 2 ·g -1 For example, the proportion of mesopores (>2 nm) in the obtained porous carbon product is greater than or equal to 18%.

[0027] In any of the above technical solutions, after the pore filling and sealing treatment, the pores with a size of less than 1 nm in the finished porous carbon product are sealed.

[0028] The present invention provides a porous carbon, and the porous carbon is obtained by using the method described in any of the above technical solutions.

[0029] The present invention also provides a silicon-carbon negative electrode material, which is prepared by using the finished porous carbon product obtained by any of the above technical solutions.

[0030] The present invention provides a silicon-carbon negative electrode material. The silicon-carbon negative electrode material is prepared by silane vapor deposition using porous carbon as a raw material. The porous carbon is obtained by the method described in any of the above technical solutions.

[0031] The present invention provides a method for preparing a silicon-carbon negative electrode material, comprising the following steps: introducing a silicon source gas into the finished porous carbon product in a fluidized state to perform chemical vapor deposition to deposit silicon on the porous carbon, and then introducing a carbon source gas to perform chemical vapor deposition to deposit carbon on the porous carbon.

[0032] In any of the above technical solutions, the temperature for depositing silicon on porous carbon by chemical vapor deposition is 650-850° C., the pressure of silicon source gas is 0.1-0.8 MPa, and the time is 3-10 hours, for example, 8 hours.

[0033] In any of the above technical solutions, the temperature of depositing carbon on the porous carbon by chemical vapor deposition is 600-800° C., the time is 1-5 hours, and the pressure of depositing carbon on the porous carbon by chemical vapor deposition is 0-0.3 MPa.

[0034] In any of the above technical solutions, the silicon source gas is silane gas and / or halogenated silane gas. The silane gas is monosilane gas and / or disilane gas; and the halogenated silane gas is chlorosilane gas.

[0035] In any of the above technical solutions, the carbon source gas used when depositing carbon on porous carbon by chemical vapor deposition is one or any combination of methane, ethane, propane, acetylene, ethylene, propylene, and toluene.

[0036] Beneficial Effects

[0037] In the process of preparing porous carbon, the present invention adopts an organic carbon source and closes the tiny pores (especially the pores below 1 nm) in the 1 nm porous carbon by chemical vapor deposition, thereby reducing the specific surface area of ​​the porous carbon (can be reduced to 1500 m 2 / g or less). Porous carbon can be used as a raw material for preparing silicon-carbon negative electrode materials. By means of silane vapor deposition, silicon can be deposited on the surface of the porous carbon matrix to obtain a silicon-carbon negative electrode material. However, tiny pores (especially pores below 1 nm) cannot contribute to silane vapor deposition, and a large number of micropores below 1 nm will cause the porous carbon to have too high a specific surface area, affecting the mechanical properties and mechanical parameters of the silicon-carbon negative electrode material. Therefore, during the preparation of the porous carbon, the crude porous carbon obtained by S100 is subjected to pore filling and sealing treatment, so that the tiny pores in the porous carbon can be closed, thereby improving the deposition efficiency in the process of preparing the silicon-carbon negative electrode material by chemical vapor deposition, saving organic carbon sources, and improving the mechanical properties and mechanical parameters of the silicon-carbon negative electrode material.

[0038] When preparing silicon-carbon negative electrode materials, the present invention deposits silicon and then deposits carbon for coating, which can effectively avoid direct contact between silicon and electrolyte in the negative electrode material after preparing the battery, prevent the electrolyte and silicon from reacting, and thus effectively improve product performance. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 This is a BET specific surface area test report of the porous carbon prepared in Example 5 without acetylene treatment;

[0040] Figure 2 This is the BET specific surface area test report of the porous carbon product prepared in Example 5;

[0041] Figure 3 This is the BET specific surface area spectrum of the silicon-carbon negative electrode material prepared in Example 11;

[0042] Figure 4 This is the BET specific surface area spectrum of the silicon-carbon negative electrode material prepared in Example 12;

[0043] Figure 5 This is the BET specific surface area spectrum of the silicon-carbon negative electrode material prepared in Comparative Example 1;

[0044] Figure 6 This is the BET specific surface area spectrum of the silicon-carbon negative electrode material prepared in Comparative Example 2;

[0045] Figure 7 The first cycle charge and discharge curve of the electrochemical performance test of the battery using the silicon-carbon negative electrode material prepared in Example 11;

[0046] Figure 8 The first cycle charge and discharge curve spectrum of the electrochemical performance test of the battery using the silicon-carbon negative electrode material prepared in Example 12;

[0047] Fig. 9The first cycle charge and discharge curve spectrum of the electrochemical performance test of the battery using the silicon-carbon negative electrode material prepared in Comparative Example 1;

[0048] Fig.10 The first cycle charge and discharge curve spectrum of the electrochemical performance test of the battery using the silicon-carbon negative electrode material prepared in Comparative Example 2;

[0049] Fig.11 The test curve of the capacity retention rate of the battery using the silicon-carbon negative electrode material prepared by Example 11;

[0050] Fig.12 This is a test curve of the capacity retention rate of a battery using the silicon-carbon negative electrode material prepared in Comparative Example 1. DETAILED DESCRIPTION

[0051] In order to more clearly understand the above-mentioned purpose, features and advantages of the present invention, the present invention is further described in detail below in conjunction with specific embodiments. It should be noted that the embodiments of the present application and the features in the embodiments can be combined with each other without conflict.

[0052] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and therefore, the protection scope of the present invention is not limited by the specific embodiments disclosed below. The following technical features of the embodiments of the present invention may be combined with each other without conflict.

[0053] The present invention provides a method for preparing porous carbon. The porous carbon is used to prepare silicon-carbon negative electrode materials, and the method for preparing the porous carbon comprises:

[0054] S100, using a biomass carbon source as a raw material, carbonizing the biomass carbon source through heat treatment, and preparing a crude porous carbon product;

[0055] S200, using an organic carbon source, by chemical vapor deposition, to perform pore filling and sealing treatment on the crude porous carbon product prepared in S100, to obtain the finished porous carbon product.

[0056] In the above-mentioned embodiment, the biomass carbon source has the advantages of low cost and easy availability. The use of the biomass carbon source to prepare porous carbon can achieve the beneficial effect of green environmental protection.

[0057] In some embodiments of the present invention, the biomass carbon source includes at least one of the following or a combination thereof: coconut shell, straw, rice husk, wood, bamboo, bagasse, and nut shell.

[0058] It can be understood that the heat treatment can carbonize the biomass carbon source.

[0059] In some embodiments of the present invention, the temperature range of the heat treatment is 700°C to 900°C.

[0060] In some embodiments of the present invention, preferably, the temperature range of the heat treatment is 750°C to 850°C.

[0061] In some embodiments of the present invention, further preferably, the temperature range of the heat treatment is 800°C.

[0062] It can be understood that the heat treatment may include only one stage of heat treatment, or may include two or more stages of heat treatment.

[0063] In some implementations of the present invention, S100 specifically includes:

[0064] S110, subjecting the biomass carbon source to a first-stage heat treatment in a protective atmosphere and then cooling it;

[0065] S120, subjecting the biomass carbon source to a second-stage heat treatment under a condition of passing water vapor and then cooling the biomass carbon source to obtain a crude porous carbon product;

[0066] The first-stage heat treatment is used to carbonize the biomass carbon source and form pores, and the second-stage heat treatment is used to enlarge the pores of the biomass carbon source.

[0067] Illustratively, in some embodiments of the present invention, after the first-stage heat treatment, the pores of the biomass carbon source are 1 nm to 3 nm, and after the second-stage heat treatment, the pores of the crude porous carbon are less than 5 nm.

[0068] In some embodiments of the present invention, the temperature range of the first-stage heat treatment is 750°C to 850°C, and the temperature range of the second-stage heat treatment is 850°C to 900°C.

[0069] In some embodiments of the present invention, preferably, the temperature range of the first-stage heat treatment is 780°C to 820°C, and the temperature range of the second-stage heat treatment is 870°C to 890°C.

[0070] In some embodiments of the present invention, further preferably, the temperature range of the first-stage heat treatment is 800°C, and the temperature range of the second-stage heat treatment is 880°C.

[0071] In some embodiments of the present invention, between S110 and S120, the process further includes: washing and drying the biomass carbon source that has undergone the first-stage heat treatment and cooling.

[0072] After the first-stage heat treatment, the carbonized material contains a large amount of microporous structures and has a high ash content and metal impurities. Therefore, it is necessary to remove the ash and metal impurities by washing and drying.

[0073] In some embodiments of the present invention, after S120, the process further includes: washing and drying the crude porous carbon product that has undergone the second-stage heat treatment and cooling.

[0074] After the second stage heat treatment, the porous carbon needs to be washed and dried to remove impurities caused by chemical vapor deposition for subsequent processing.

[0075] It can be understood that the chemical vapor deposition using an organic carbon source is for the purpose of performing pore filling and sealing treatment on the crude porous carbon product obtained by S100.

[0076] In some embodiments of the present invention, the organic carbon source includes at least one of the following or a combination thereof: methane, ethane, propane, acetylene, ethylene, propylene, and toluene.

[0077] By performing pore filling and sealing treatment on the crude porous carbon obtained in S100 during the porous carbon preparation process, the tiny pores in the porous carbon can be sealed, the deposition efficiency in the process of preparing silicon-carbon negative electrode materials by chemical vapor deposition can be improved, the organic carbon source can be saved, and the mechanical properties and mechanical parameters of the silicon-carbon negative electrode materials can be improved.

[0078] In some implementations of the present invention, S200 specifically includes:

[0079] S210, performing air flow pulverization on the crude porous carbon product so that the particle size of the crude porous carbon product satisfies DV50 of 5 μm to 8 μm;

[0080] S220, sending the crude porous carbon into a fluidized bed reactor, using an organic carbon source, performing chemical vapor deposition under a pressure condition of 0.2 MPa to 0.3 MPa and a temperature condition of 700° C. to 800° C. to obtain the finished porous carbon.

[0081] In some embodiments of the present invention, after the pore filling and sealing treatment, the pores with a size of less than 1 nm in the finished porous carbon product are sealed.

[0082] Example 1

[0083] A porous carbon is prepared in an embodiment of the present invention, and its preparation method is as follows. Coconut shell is used as a raw material for preparing porous carbon. In a converter, under a nitrogen atmosphere, it is heated to 750°C to 850°C for carbonization. At this time, the carbonized material contains a large number of microporous structures and has a high ash content and metal impurities. After ultrasonic cleaning and drying, it is put into the converter again, and water vapor is introduced at 850-900°C for secondary activation and pore formation. After some pores are enlarged to 1-3nm, ultrasonic cleaning and drying are performed again. The activated porous carbon is pulverized by air flow to make the particle size (DV50) between 5 and 8μm. The pulverized porous carbon is added to a fluidized bed reactor. When the reaction pressure is controlled at 0.2-0.3MPa and the reaction temperature is controlled at 700-800°C, acetylene is introduced for decomposition, pore filling and deposition, and the micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. The BET specific surface area of ​​the pulverized porous carbon in this embodiment is about 1820m before acetylene treatment. 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1450m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 11.6% before treatment and increased to 18.8% after treatment, indicating that the micropores were significantly reduced.

[0084] Example 2

[0085] A porous carbon is prepared in an embodiment of the present invention, and its preparation method is as follows. Straw is used as a raw material for preparing porous carbon, and is heated to 750°C to 800°C in a converter under a nitrogen atmosphere for carbonization. After ultrasonic cleaning and drying, it is put into the converter again, and water vapor is introduced at 850°C to 880°C for secondary activation and pore formation. After some pores are enlarged to 1-3nm, ultrasonic cleaning and drying are performed again. The activated porous carbon is subjected to air flow pulverization to make the particle size (DV50) between 6μm and 7μm. The pulverized porous carbon is added to a fluidized bed reactor, and the reaction pressure is controlled at 0.2 to 0.3MPa, and the reaction temperature is controlled at 740°C to 760°C. Methane is introduced for decomposition, pore filling and deposition, and micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. In this embodiment, the pulverized porous carbon has a BET specific surface area of ​​about 1810m before methane treatment. 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1433m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 13.3% before treatment and increased to 19.1% after treatment, indicating that the micropores were significantly reduced.

[0086] Example 3

[0087] A porous carbon is prepared in an embodiment of the present invention, and its preparation method is as follows. Nut shells are used as raw materials for preparing porous carbon, and are heated to 780°C to 800°C in a converter under an argon atmosphere for carbonization. After ultrasonic cleaning and drying, they are put into the converter again, and water vapor is introduced at 880°C to 900°C for secondary activation and pore formation. After some pores are enlarged to 1-3nm, ultrasonic cleaning and drying are performed again. The activated porous carbon is pulverized by air flow to make the particle size (DV50) between 6μm and 7μm. The pulverized porous carbon is added to a fluidized bed reactor, and ethane is introduced to decompose and fill the pores and deposit them when the reaction pressure is controlled at 0.2 to 0.3MPa and the reaction temperature is controlled at 740°C to 760°C. The micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. The BET specific surface area of ​​the pulverized porous carbon in this embodiment before ethane treatment is about 1878m 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1492m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 11.3% before treatment and increased to 19.2% after treatment, indicating that the micropores were significantly reduced.

[0088] Example 4

[0089] A porous carbon is prepared in an embodiment of the present invention, and its preparation method is as follows. Rice husk is used as a raw material for preparing porous carbon, and is heated to 780°C to 800°C in a converter under an argon atmosphere for carbonization. After ultrasonic cleaning and drying, it is put into the converter again, and water vapor is introduced at 880°C to 900°C for secondary activation and pore formation. After some pores are enlarged to 1-3nm, ultrasonic cleaning and drying are performed again. The activated porous carbon is pulverized by air flow to make the particle size (DV50) between 6μm and 7μm. The pulverized porous carbon is added to a fluidized bed reactor, and the reaction pressure is controlled at 0.2 to 0.3MPa, and the reaction temperature is controlled at 740°C to 760°C. Propane is introduced for decomposition, pore filling and deposition, and the micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. In this embodiment, the pulverized porous carbon has a BET specific surface area of ​​about 1954m before propane treatment. 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1558m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 13.1% before treatment and increased to 19.6% after treatment, indicating that the micropores were significantly reduced.

[0090] Example 5

[0091] The method for preparing porous carbon of this embodiment comprises the following steps:

[0092] Coconut shell is used as the raw material for preparing porous carbon. In a converter, under a nitrogen atmosphere, it is heated to 800°C for carbonization. The carbonization time is 2.5 hours. At this time, the carbonized material contains a large number of microporous structures and has a high ash content and metal impurities. After ultrasonic cleaning and drying, the carbonized material is put into the converter again, and water vapor is introduced at 880°C for secondary activation and pore formation. After secondary activation and pore formation at 880°C for 5 hours, some pores are expanded to 1-3nm, and then ultrasonic cleaning and drying are performed again. The activated porous carbon is pulverized by air flow to make the particle size (DV50) between 5 and 8μm. The pulverized porous carbon is added to a fluidized bed reactor. When the reaction pressure is controlled at 0.2MPa and the reaction temperature is controlled at 750°C, acetylene is introduced for 1 hour for decomposition, filling and deposition, and the micropores less than 1nm are filled with closed pores. After the reaction is completed, the product is collected and packaged. In this embodiment, the pulverized porous carbon adopts a BET specific surface area of ​​about 1820m before acetylene treatment. 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1450m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated, which was about 11.6% before treatment and increased to 18.8% after treatment, indicating that the micropores were significantly reduced; The BET specific surface area test reports of porous carbon before and after treatment are shown in Figure 1 and Figure 2 .

[0093] Example 6

[0094] The method for preparing porous carbon of this embodiment comprises the following steps:

[0095] Straw is used as a raw material for preparing porous carbon. It is heated to 770°C in a converter under a nitrogen atmosphere for carbonization, and the carbonization time is 5 hours. After ultrasonic cleaning and drying, the carbonized material is put into the converter again, and water vapor is introduced at 870°C for secondary activation and pore formation. After secondary activation and pore formation at 870°C for 3 hours, some pores are expanded to 1-3nm, and then ultrasonic cleaning and drying are performed again. The activated porous carbon is air-flow crushed to make the particle size (DV50) between 6μm and 7μm. The crushed porous carbon is added to a fluidized bed reactor. When the reaction pressure is controlled at 0.3MPa and the reaction temperature is controlled at 740℃, methane is introduced for 3 hours for decomposition, pore filling and deposition, and micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. In this embodiment, the BET specific surface area of ​​the crushed porous carbon before methane treatment is about 1810m 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1433m 2 ·g -1; The proportion of mesopores (>2nm) was calculated to be about 13.3% before treatment and increased to 19.1% after treatment, indicating that the micropores were significantly reduced.

[0096] Example 7

[0097] The method for preparing porous carbon of this embodiment comprises the following steps:

[0098] Nut shells are used as raw materials for preparing porous carbon. In a converter, under an argon atmosphere, they are heated to 780°C for carbonization, and the carbonization time is 4 hours. After ultrasonic cleaning and drying, the carbonized material is put into the converter again, and water vapor is introduced at 880°C for secondary activation and pore formation. The secondary activation and pore formation are carried out at 880°C to 900°C for 6 hours. After some pores are enlarged to 1-3nm, ultrasonic cleaning and drying are carried out again. The activated porous carbon is pulverized by air flow to make the particle size (DV50) between 6μm and 7μm. The pulverized porous carbon is added to a fluidized bed reactor. When the reaction pressure is controlled at 0.2MPa and the reaction temperature is controlled at 740°C, ethane is introduced for 2 hours for decomposition, pore filling and deposition, and the micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. In this embodiment, the BET specific surface area of ​​the pulverized porous carbon before ethane treatment is about 1878m 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1492m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 11.3% before treatment and increased to 19.2% after treatment, indicating that the micropores were significantly reduced.

[0099] Example 8

[0100] The method for preparing porous carbon of this embodiment comprises the following steps:

[0101] Rice husk is used as a raw material for preparing porous carbon. It is heated to 800°C in a converter under an argon atmosphere for carbonization for 2 hours. After ultrasonic cleaning and drying, the carbonized material is put into the converter again. At 900°C, water vapor is introduced for secondary activation and pore formation. After secondary activation and pore formation at 900°C for 3 hours, some pores are expanded to 1-3nm, and then ultrasonic cleaning and drying are performed again. The activated porous carbon is pulverized by air flow to make the particle size (DV50) between 6μm and 7μm. The pulverized porous carbon is added to a fluidized bed reactor. When the reaction pressure is controlled at 0.3MPa and the reaction temperature is controlled at 740°C, propane is introduced for 2 hours for decomposition, pore filling and deposition, and micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. In this embodiment, the BET specific surface area of ​​the pulverized porous carbon before propane treatment is about 1954m 2 ·g -1The BET specific surface area of ​​the treated porous carbon product is about 1558m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 13.1% before treatment and increased to 19.6% after treatment, indicating that the micropores were significantly reduced.

[0102] Example 9

[0103] The method for preparing porous carbon of this embodiment comprises the following steps:

[0104] Coconut shell is used as a raw material for preparing porous carbon. In a converter, under a nitrogen atmosphere, it is heated to 850°C for carbonization. The carbonization time is 2 hours. After ultrasonic cleaning and drying, the carbonized material is put into the converter again. At 850°C, water vapor is introduced for secondary activation and pore formation. After secondary activation and pore formation at 850°C for 3 hours, some pores are expanded to 1-3nm, and then ultrasonic cleaning and drying are performed again. The activated porous carbon is air-flow crushed to make the particle size (DV50) between 5 and 8μm. The crushed porous carbon is added to a fluidized bed reactor. When the reaction pressure is controlled at 0.25MPa and the reaction temperature is controlled at 720°C, acetylene is introduced for 3 hours for decomposition, pore filling and deposition, and micropores less than 1nm are filled and closed. After the reaction is completed, the product is collected and packaged. In this embodiment, the crushed porous carbon adopts a BET specific surface area of ​​about 1982m before acetylene treatment. 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1534m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 12.8% before treatment and increased to 19.8% after treatment, indicating that the micropores were significantly reduced.

[0105] Example 10

[0106] The preparation method of porous carbon in this embodiment is different from the preparation method of porous carbon in Example 9 in that: in this embodiment, after adding the crushed porous carbon to the fluidized bed reactor, the temperature when acetylene is introduced for reaction is controlled to be 800°C. The BET specific surface area of ​​the crushed porous carbon in this embodiment before acetylene treatment is about 1982 m 2 ·g -1 The BET specific surface area of ​​the treated porous carbon product is about 1498m 2 ·g -1 ; The proportion of mesopores (>2nm) was calculated to be about 12.8% before treatment and increased to 20.7% after treatment, indicating that the micropores were significantly reduced.

[0107] Embodiment 11

[0108] The silicon-carbon negative electrode material of this embodiment is prepared using the porous carbon product prepared in Example 5 as a raw material. The specific preparation method includes the following steps:

[0109] The finished porous carbon product is put into a fluidized bed reactor, and nitrogen is introduced to make the porous carbon in a fluidized state. The temperature is controlled at 800°C and the pressure of the monosilane gas is 0.5 MPa. Monosilane gas is introduced for chemical vapor deposition. During this process, monosilane and porous carbon are fully mixed, and the generated silicon is deposited in the pores on the porous carbon. After deposition for 5 hours, acetylene gas is introduced for chemical vapor deposition at 700°C and 0.1 MPa, and the generated carbon is deposited on the porous carbon to coat the porous carbon. The coating time is 1 hour to prepare a silicon-carbon negative electrode material.

[0110] Example 12

[0111] The silicon-carbon negative electrode material of this embodiment is prepared using the porous carbon product prepared in Example 6 as a raw material. The specific preparation method includes the following steps:

[0112] The finished porous carbon product is put into a fluidized bed reactor, and nitrogen is introduced to fluidize the porous carbon. The temperature is controlled at 850°C and the pressure of monosilane gas is 0.8 MPa. Monosilane gas is introduced for chemical vapor deposition. During this process, monosilane and porous carbon are fully mixed, and the generated silicon is deposited in the pores on the porous carbon. After deposition for 3 hours, acetylene gas is introduced for chemical vapor deposition at 800°C and 0.3 MPa, and the generated carbon is deposited on the porous carbon to coat the porous carbon. The coating time is 3 hours to prepare a silicon-carbon negative electrode material.

[0113] Embodiment 13

[0114] The silicon-carbon negative electrode material of this embodiment is prepared using the porous carbon product prepared in Example 7 as a raw material. The specific preparation method includes the following steps:

[0115] The finished porous carbon product is put into a fluidized bed reactor, and nitrogen is introduced to make the porous carbon in a fluidized state. The temperature is controlled at 650°C and the pressure of monosilane gas is 0.1 MPa. Monosilane gas is introduced for chemical vapor deposition. During this process, monosilane and porous carbon are fully mixed, and the generated silicon is deposited in the pores on the porous carbon. After deposition for 10 hours, acetylene gas is introduced at 700°C and normal pressure for chemical vapor deposition, and the generated carbon is deposited on the porous carbon to coat the porous carbon. The coating time is 5 hours to prepare a silicon-carbon negative electrode material.

[0116] Embodiment 14

[0117] The silicon-carbon negative electrode material of this embodiment is prepared using the porous carbon product prepared in Example 8 as a raw material. The specific preparation method includes the following steps:

[0118] The finished porous carbon product is put into a fluidized bed reactor, and nitrogen is introduced to fluidize the porous carbon. The temperature is controlled at 700°C and the pressure of the monosilane gas is 0.3 MPa. Monosilane gas is introduced for chemical vapor deposition. During this process, monosilane and porous carbon are fully mixed, and the generated silicon is deposited in the pores on the porous carbon. After deposition for 6 hours, acetylene gas is introduced for chemical vapor deposition at 600°C and 0.1 MPa, and the generated carbon is deposited on the porous carbon to coat the porous carbon. The coating time is 5 hours to prepare a silicon-carbon negative electrode material.

[0119] Embodiment 15

[0120] The silicon-carbon negative electrode material of this embodiment is prepared using the porous carbon product prepared in Example 9 as a raw material. The specific preparation method includes the following steps:

[0121] The finished porous carbon product is put into a fluidized bed reactor, and nitrogen is introduced to make the porous carbon in a fluidized state. The temperature is controlled at 750°C and the pressure of monosilane gas is 0.4MPa. Monosilane gas is introduced for chemical vapor deposition. Monosilane and porous carbon need to be fully mixed and silicon is deposited in the pores. After deposition for 4 hours, acetylene gas is introduced for chemical vapor deposition at 750°C and 0.1MPa to generate carbon deposits on the porous carbon to coat the porous carbon. The coating time is 2 hours to prepare a silicon-carbon negative electrode material.

[0122] Example 16

[0123] The method for preparing the silicon-carbon negative electrode material of this embodiment is different from the method for preparing the silicon-carbon negative electrode material of Example 15 only in that the porous carbon used in this embodiment is the porous carbon product prepared in Example 10.

[0124] Comparative Example 1

[0125] The preparation method of the silicon-carbon negative electrode material in this comparative example is different from the preparation method of the silicon-carbon negative electrode material in Example 10 only in that the porous carbon crushed in Example 5 (i.e., porous carbon that has not been subjected to closed-pore treatment) is used as raw material in this comparative example.

[0126] Comparative Example 2

[0127] The preparation method of the silicon-carbon negative electrode material in this comparative example is different from the preparation method of the silicon-carbon negative electrode material in Example 11 only in that this comparative example uses the pulverized porous carbon in Example 6 (i.e., porous carbon that has not been subjected to closed-pore treatment) as raw material.

[0128] Comparative Example 3

[0129] The preparation method of the silicon-carbon negative electrode material in this comparative example is different from the preparation method of the silicon-carbon negative electrode material in Example 12 only in that this comparative example uses the pulverized porous carbon in Example 7 (i.e., porous carbon that has not been subjected to closed-pore treatment) as raw material.

[0130] Comparative Example 4

[0131] The preparation method of the silicon-carbon negative electrode material in this comparative example is different from the preparation method of the silicon-carbon negative electrode material in Example 13 only in that this comparative example uses the pulverized porous carbon in Example 8 (i.e., porous carbon that has not been subjected to closed-pore treatment) as raw material.

[0132] Comparative Example 5

[0133] The preparation method of the silicon-carbon negative electrode material in this comparative example is different from the preparation method of the silicon-carbon negative electrode material in Example 14 only in that this comparative example uses the pulverized porous carbon in Example 9 (i.e., porous carbon that has not been subjected to closed-pore treatment) as raw material.

[0134] Comparative Example 6

[0135] The method for preparing the silicon-carbon negative electrode material of this comparative example is different from the method for preparing the silicon-carbon negative electrode material of comparative example 1 only in that after the silicon deposition is completed, the material of this comparative example is taken out as the silicon-carbon negative electrode material.

[0136] Experimental example

[0137] 1) BET specific surface area test

[0138] The BET specific surface areas of the silicon-carbon negative electrode materials prepared in Examples 11 to 16 and Comparative Examples 1 to 6 were measured respectively, and the results are shown in Table 1; the BET specific surface area spectra of the silicon-carbon negative electrode materials of Examples 11 to 16 and Comparative Examples 1 to 2 are shown in Figures 3 to 6 .

[0139] Table 1 BET specific surface area of ​​porous carbon before and after carbon source gas treatment

[0140]

[0141]

[0142] It can be seen from the data in Table 1 that when preparing the silicon-carbon negative electrode in Examples 11 to 16, porous carbon was treated with an organic carbon source gas, and the BET specific surface area decreased significantly compared with Comparative Examples 1 to 6, indicating that the pores of the porous carbon have been closed.

[0143] 2) Electrochemical performance test

[0144] The silicon-carbon negative electrode materials prepared in Examples 11 to 16 and Comparative Examples 1 to 6 were used as negative electrode materials to prepare negative electrode sheets, lithium sheets were used as counter electrodes, and LiPF 6 As electrolyte salt (concentration in electrolyte is 1 mol / L), silicon-carbon negative electrode material: CMC / SBR: conductive agent = 80:10:10 is used to prepare negative electrode plates, button batteries are prepared by the same process, and then the first discharge specific capacity and the first coulomb efficiency of the button batteries are tested (0-2.0 V, 0.1 C / 0.1 C); the silicon-carbon negative electrode materials prepared in Examples 11-16 and Comparative Examples 1-6 are compounded with graphite to form a negative electrode material with a capacity of 500 mAh / g for a full battery 300-cycle performance test (2.75-4.2 V, room temperature, 1 C / 1 C), and the prepared full battery is LiPF 6 As electrolyte salt (concentration of 1 mol / L in electrolyte), ternary material is used as positive electrode material, and the test results are shown in Table 2; the electrochemical performance test of button cells using silicon-carbon negative electrode materials prepared in Examples 11 to 16 and Comparative Examples 1 to 2 is shown in the first cycle charge and discharge curves. Figures 7-10 The test curve of the capacity retention rate of the full battery prepared with silicon-carbon negative electrode materials using Example 11 and Comparative Example 1 is shown in Figures 11-12 .

[0145] Table 2 Button battery performance test results

[0146]

[0147] From the data in Table 2, it can be seen that the capacity of the silicon-carbon negative electrode material prepared by porous carbon before and after being treated with organic carbon source gas does not change much, there is no loss, but the first coulomb efficiency is greatly improved. In terms of cycle performance, the button battery using silicon-carbon negative electrode material prepared by porous carbon without treating organic carbon source gas maintains a capacity of about 82% after 300 cycles, but the button battery using silicon-carbon negative electrode material prepared by porous carbon treated with organic carbon source gas maintains a capacity of about 91% after 300 cycles. Therefore, the first coulomb efficiency and cycle performance of the button battery using silicon-carbon negative electrode material prepared by porous carbon treated with organic carbon source gas are significantly improved.

[0148] In the present invention, the terms "first", "second", and "third" are used for descriptive purposes only and should not be understood as indicating or implying relative importance; the term "plurality" refers to two or more, unless otherwise clearly defined. The terms "installed", "connected", "connected", "fixed", etc. should be understood in a broad sense. For example, "connected" can be a fixed connection, a detachable connection, or an integral connection; "connected" can be a direct connection or an indirect connection through an intermediate medium. For those of ordinary skill in the art, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.

[0149] In the description of this specification, the description of the terms "one embodiment", "some embodiments", "specific embodiments", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in a suitable manner in any one or more embodiments or examples. The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. A method for preparing a silicon-carbon negative electrode material, characterized in that: The following steps are involved: Passing silicon source gas into porous carbon in a fluidized state to perform chemical vapor deposition to deposit silicon on the porous carbon, and then passing carbon source gas into porous carbon to perform chemical vapor deposition to deposit carbon on the porous carbon, to obtain; The porous carbon is used to prepare a silicon-carbon negative electrode material, and the preparation method of the porous carbon includes: S100, using a biomass carbon source as a raw material, carbonizing the biomass carbon source through heat treatment, and preparing a crude porous carbon product; S200, using an organic carbon source, by chemical vapor deposition, the crude porous carbon prepared by S100 is subjected to pore filling and sealing treatment to obtain the finished porous carbon; the finished porous carbon has pores larger than 2 nm accounting for greater than or equal to 18%.

2. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The biomass carbon source includes at least one of the following or a combination thereof: coconut shell, straw, rice husk, wood, bamboo, bagasse, nut shell; The organic carbon source includes at least one of the following or a combination thereof: methane, ethane, propane, acetylene, ethylene, propylene, and toluene.

3. The method for preparing a silicon-carbon negative electrode material according to any one of claims 1 to 2, characterized in that: S100 specifically includes: S110, subjecting the biomass carbon source to a first-stage heat treatment in a protective atmosphere and then cooling; S120, subjecting the biomass carbon source to a second-stage heat treatment under a condition of passing water vapor and then cooling the biomass carbon source to obtain a crude porous carbon product; The first-stage heat treatment is used to carbonize the biomass carbon source and form pores, and the second-stage heat treatment is used to enlarge the pores of the biomass carbon source.

4. The method for preparing the silicon-carbon negative electrode material according to claim 3, characterized in that: The second stage heat treatment enlarges the pores of the biocarbon source to 1-3 nm.

5. The method for preparing the silicon-carbon negative electrode material according to claim 3, characterized in that: The temperature range of the first stage heat treatment is 750°C to 850°C, and the temperature range of the second stage heat treatment is 850°C to 900°C.

6. The method for preparing the silicon-carbon negative electrode material according to claim 5, characterized in that: The time of the first-stage heat treatment is 2 to 5 hours; the time of the second-stage heat treatment is 3 to 6 hours.

7. The method for preparing the silicon-carbon negative electrode material according to claim 3, characterized in that: Between S110 and S120, the method further includes: washing and drying the biomass carbon source after the first-stage heat treatment and cooling; After S120, the method further includes: washing and drying the crude porous carbon product that has undergone the second-stage heat treatment and cooling.

8. The method for preparing a silicon-carbon negative electrode material according to any one of claims 1 to 2, characterized in that: S200 specifically includes: S210, performing air flow pulverization on the crude porous carbon product so that the particle size of the crude porous carbon product satisfies DV50 of 5 μm to 8 μm; S220, sending the crude porous carbon into a fluidized bed reactor, using an organic carbon source, performing chemical vapor deposition under a pressure condition of 0.2 MPa to 0.3 MPa and a temperature condition of 700° C. to 800° C. to obtain the finished porous carbon.

9. The method for preparing the silicon-carbon negative electrode material according to claim 8, characterized in that: After the pore filling and sealing treatment, the pores with a size of less than 1 nm in the finished porous carbon are sealed.

10. The method for preparing the silicon-carbon negative electrode material according to claim 8, characterized in that: The chemical vapor deposition time is 1 to 3 hours under the pressure conditions of 0.2 MPa to 0.3 MPa and the temperature conditions of 700° C. to 800° C.

11. The method for preparing the silicon-carbon negative electrode material according to claim 1, characterized in that: The temperature for depositing silicon on porous carbon by chemical vapor deposition is 650~850℃, the pressure of silicon source gas is 0.1~0.8MPa, and the time is 3~10h.

12. The method for preparing the silicon-carbon negative electrode material according to claim 1 or 11, characterized in that: The temperature of depositing carbon on porous carbon by chemical vapor deposition is 600~800℃ and the time is 1~5h.

13. A silicon-carbon negative electrode material, characterized in that: The silicon-carbon negative electrode material is obtained by the method as described in any one of claims 1 to 12.

Citation Information

Patent Citations

  • Mesoporous carbon / silicon composite anode material and preparation method thereof

    CN102867944A

  • A silicon-carbon composite negative electrode material and a preparation method thereof

    CN109004203A

  • Biomass porous carbon material and preparation and application thereof

    CN110526244A

  • Lithium ion battery negative electrode material, lithium ion battery and preparation method and application of lithium ion battery negative electrode material

    CN112670484A

  • Process for preparing electroactive materials for metal-ion batteries

    CN113508474A

Cited By

  • Expansion-resistant lithium battery pole piece material for unmanned aerial vehicle and preparation method of expansion-resistant lithium battery pole piece material

    CN120657064A

  • Unmanned aerial vehicle resistant expansion lithium battery pole piece material and preparation method thereof

    CN120657064B

  • Preparation method of pitch-based porous carbon for high-performance silicon carbon

    CN120922872A

  • A method for preparing pitch-based porous carbon for high-performance silicon-carbon applications

    CN120922872B

  • Preparation method of porous carbon composite material with mesoporous structure

    CN122212136A