Composite substrate, method for manufacturing composite substrate, method for manufacturing circuit substrate, method for manufacturing assembly of multiple circuit substrates, and method for manufacturing multiple circuit substrates
The composite substrate with notches or holes in metal layers on a ceramic substrate facilitates easy identification of front and back sides, addressing handling challenges and reducing defects in circuit board manufacturing.
Patent Information
- Application Number
- JP2021522819
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-05-31
- Filing Date
- 2020-05-27
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-05-27
AI Technical Summary
Existing circuit boards with ceramic substrates lack effective methods for easily identifying the front and back sides, leading to potential manufacturing defects and difficulties in handling and processing.
A composite substrate is designed with a ceramic substrate bonded to a first and second metal layer, where at least one notch or hole is formed in one or both layers to visually distinguish the front and back surfaces, and scribe lines are used for further identification and division.
The solution allows for easy identification of the front and back sides of the composite substrate, reducing manufacturing defects and enhancing processing efficiency by ensuring accurate handling and separation of circuit boards.
Smart Images

Figure 0007581196000001 
Figure 0007581196000002 
Figure 0007581196000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite substrate, a method for manufacturing a composite substrate, a method for manufacturing a circuit substrate, a method for manufacturing an assembly of a plurality of circuit substrates, and a method for manufacturing a plurality of circuit substrates. Regarding. [Background technology]
[0002] A circuit board is known in which a ceramic substrate is used as a base material and a circuit pattern is formed on one side of the substrate. Such a circuit board is excellent in terms of high thermal conductivity and high insulation properties, and is therefore used for, for example, a power module.
[0003] Patent Document 1 discloses a technique in which metal layers are bonded to both sides of a ceramic substrate having scribe lines formed on its surface to form a composite substrate, the metal layers on the surface are etched into a circuit pattern, and the composite substrate is then divided along the scribe lines to manufacture multiple circuit substrates. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2007-324301 A Summary of the Invention [Problem to be solved by the invention]
[0005] The present invention aims to provide a composite substrate comprising a ceramic substrate, a first metal layer bonded to the front side of the ceramic substrate, and a second metal layer bonded to the back side, the composite substrate having a front and back surfaces which can be easily distinguished from each other. [Means for solving the problem]
[0006] The composite substrate of the first aspect of the present invention comprises a ceramic substrate, a first metal layer bonded to a front side of the ceramic substrate, and a second metal layer bonded to a back side of the ceramic substrate, and one or both of the first metal layer and the second metal layer have at least one notch or hole formed therein to enable identification of the front and back sides of the ceramic substrate. Here, "enabling identification of the front and back surfaces" means that a person handling the composite substrate can visually identify the front and back surfaces of the composite substrate. The following are examples of the manner in which the front and back sides can be distinguished. (First embodiment) An embodiment in which at least one notch or hole is formed in one of the first metal layer and the second metal layer. (Second embodiment) At least one notch or hole is formed in both the first metal layer and the second metal layer, but the one formed in the first metal layer differs from the one formed in the second metal layer in terms of shape, position, quantity or size. (Third embodiment) At least one notch or hole is formed in both the first metal layer and the second metal layer, and those formed in the first metal layer and those formed in the second metal layer are identical or approximately identical in shape, position, quantity and size, but differ by the color, material or pattern inside the notch or hole.
[0007] A second aspect of the composite substrate of the present invention is a composite substrate in which the ceramic substrate is rectangular when viewed in the thickness direction, and the at least one notch is formed in one or both of the first metal layer and the second metal layer so as to expose at least one of the four corners of the ceramic substrate.
[0008] A third aspect of the composite substrate of the present invention is a composite substrate in which at least one notch or hole is formed in both the first metal layer and the second metal layer, and the at least one notch or hole formed in both layers differs from each other in one or more of position, size, and shape.
[0009] A fourth aspect of the present invention provides a composite substrate, wherein the at least one notch or hole functions as an alignment mark.
[0010] A fifth aspect of the present invention provides a composite substrate, wherein one of the first metal layer and the second metal layer has a circuit pattern on which an electronic component is mounted.
[0011] In a sixth aspect of the composite substrate of the present invention, the other of the first metal layer and the second metal layer functions as a heat dissipation layer.
[0012] A seventh aspect of the present invention provides a composite substrate, wherein at least one scribe line is formed on one of the front and back surfaces of the ceramic substrate.
[0013] An eighth aspect of the composite substrate of the present invention is a composite substrate, in which the at least one notch or hole is formed in one of the first metal layer and the second metal layer so that, when viewed from the thickness direction, a portion of the at least one scribe line is located inside the notch or hole.
[0014] A ninth aspect of the composite substrate of the present invention is a composite substrate, in which a circuit pattern on which electronic components are mounted is formed in each of a plurality of areas partitioned by at least one scribe line in one of the first metal layer and the second metal layer.
[0015] In a composite substrate of a tenth aspect of the present invention, a plurality of regions defined by the at least one scribe line in the other of the first metal layer and the second metal layer each function as a heat dissipation layer.
[0016] A first aspect of the present invention relates to a method for manufacturing a composite substrate in which a first metal layer and a second metal layer are bonded to the front and back sides of a ceramic substrate, and includes a notch forming step of forming at least one notch or hole in one of the first metal layer and the second metal layer to enable identification of the front and back sides of the ceramic substrate, and a bonding step of bonding the first metal layer and the second metal layer to the front and back sides of the ceramic substrate, respectively.
[0017] A method for producing a composite substrate according to a second aspect of the present invention is a method for producing a composite substrate in which a first metal layer and a second metal layer are bonded to the front and back sides of a ceramic substrate, respectively, and includes a notch forming step of forming at least one notch or hole in each of the first metal layer and the second metal layer, which allows identification of the ceramic substrate; and a bonding step of bonding the first metal layer and the second metal layer to the front and back sides of the ceramic substrate, respectively. Includes.
[0018] A third aspect of the present invention is a method for manufacturing a composite substrate, in which, in the notch forming process, at least one notch or hole that differs from the other in any one or more of position, size, and shape is formed in both of the substrates.
[0019] The method for manufacturing a circuit board of the present invention includes the method for manufacturing the composite substrate and a pattern formation process, which is performed after the bonding process, in which the front and back surfaces of the ceramic substrate are identified from the at least one notch or hole formed in one or both of the first metal layer and the second metal layer, and a circuit pattern in which electronic components are mounted on one of the first metal layer and the second metal layer is formed.
[0020] A fourth aspect of the present invention relates to a method for manufacturing a composite substrate, and includes the method for manufacturing a composite substrate, and a scribe line forming step, which is performed before the bonding step, of forming at least one scribe line on the front or back surface of the ceramic substrate.
[0021] A fifth aspect of the present invention relates to a method for manufacturing a composite substrate, and in the notch forming step, at least one notch or hole is formed in one of the first metal layer and the second metal layer so that a portion of the at least one scribe line is positioned inside the at least one notch or hole in the thickness direction during the bonding step.
[0022] The manufacturing method of an assembly of multiple circuit boards of the present invention includes the manufacturing method of the composite substrate and a pattern formation process, which is performed after the bonding process, in which the front and back surfaces of the ceramic substrate are identified from the at least one notch or hole formed in one or both of the first metal layer and the second metal layer, and a circuit pattern is formed in each of multiple areas partitioned by the at least one scribe line in one of the first metal layer and the second metal layer.
[0023] The method for manufacturing multiple circuit boards of the present invention includes a method for manufacturing an assembly of multiple circuit boards, and a dividing step of cutting the ceramic substrate along at least one scribe line to divide the assembly of multiple circuit boards. Effect of the Invention
[0024] The composite substrate of the present invention is a composite substrate comprising a ceramic substrate, a first metal layer bonded to the front side of the ceramic substrate, and a second metal layer bonded to the back side, and its front and back sides can be easily distinguished.
[0025] Furthermore, according to the method for manufacturing a composite board of the present invention, it is possible to manufacture a composite board whose front and back can be easily distinguished. Accordingly, according to the method for manufacturing a circuit board, the method for manufacturing an assembly of multiple circuit boards, and the method for manufacturing multiple circuit boards of the present invention, manufacturing defects do not occur or are unlikely to occur. [Brief description of the drawings]
[0026] [Figure 1]FIG. 4 is a flow diagram showing a method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 2A] FIG. 11 is a flow diagram of a green sheet forming process included in the method for manufacturing multiple mounting boards according to the present embodiment. [Figure 2B] FIG. 13 is a schematic diagram for explaining the molding process included in the green sheet formation process of this embodiment, in which a strip-shaped green sheet is produced from the slurry using a doctor blade molding device. [Figure 2C] This is a diagram for explaining the cutting process included in the green sheet formation process of this embodiment, and is a schematic diagram (side view) for explaining the state in which a strip-shaped green sheet is cut using a cutting device to produce single-leaf green sheets. [Figure 2D] FIG. 2D is a schematic diagram of FIG. 2C as viewed from the front side. [Diagram 3] 2 is a schematic diagram of a plurality of ceramic substrates in a stacked state manufactured by the ceramic substrate manufacturing method of the present embodiment. FIG. [Figure 4] 11A to 11C are diagrams for explaining a scribe line forming step included in the method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 5A] FIG. 11 is a flow diagram of a metal layer forming process included in the method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 5B] 11A to 11C are diagrams for explaining a metal layer forming step included in the method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 5C] 5C-5C cross-sectional view of FIG. 5B. [Figure 6] 11A to 11C are diagrams for explaining a resist printing step included in the method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 7] 11A to 11C are diagrams for explaining an etching step included in the method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 8] 11A to 11C are diagrams for explaining a dividing step included in the method for manufacturing a plurality of mounting substrates according to the present embodiment. [Figure 9] FIG. 11 is a view for explaining a metal layer forming step in the first modified example. [Figure 10] FIG. 13 is a view for explaining a metal layer forming step in the second modified example. [Figure 11] FIG. 13 is a view for explaining a metal layer forming step in the third modified example. [Figure 12] FIG. 13 is a view for explaining a metal layer forming step in the fourth modified example. [Figure 13] FIG. 13 is a diagram of a motherboard according to a fifth modified example, which is a cross-sectional view taken along the same portion as the cross-sectional view of FIG. 5C of this embodiment. [Figure 14] FIG. 23 is a view for explaining a metal layer forming step in the sixth modified example. [Figure 15A] FIG. 13 is a view for explaining a metal layer forming step in the seventh modified example. [Figure 15B] This is a cross-sectional view of FIG. 15A along line 15B-15B. [Figure 16] FIG. 23 is a view for explaining a metal layer forming step in the eighth modified example. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0027] Overview Hereinafter, the present embodiment will be described with reference to the drawings. Specifically, a manufacturing method of a plurality of mounting substrates (not shown) of the present embodiment will be described in the order of each process shown in Fig. 1 with reference to Fig. 1 etc. The ceramic substrate 40 (see Fig. 3), the motherboard 60 (one example of a composite substrate, see Figs. 5B and 5C), the aggregate substrate 60B (another example of a composite substrate, see Figs. 7 and 8), and the circuit substrate 60C (see Fig. 8) manufactured after each process will be described in the explanation of each process corresponding to the manufacturing process. Next, the effects of this embodiment will be described. Next, modified examples of this embodiment will be described with reference to, for example, FIGS. In addition, in all drawings referred to in the following description, similar components are given the same reference numerals and descriptions thereof will be omitted as appropriate.
[0028] <<Method for manufacturing a plurality of mounting substrates according to the present embodiment>> The manufacturing method S100 of multiple mounting substrates of this embodiment (hereinafter referred to as the manufacturing method S100 of this embodiment) includes, as shown in FIG. 1, a green sheet formation process S10, a sintering process S20, a scribe line formation process S30 (hereinafter referred to as the SL formation process S30), a metal layer formation process S40, a resist printing process S50, an etching process S60, a surface treatment process S70, a division process S80, and a mounting process S90, and these processes are performed in the order listed.
[0029] The relationship between the end of each step in the manufacturing method S100 of this embodiment and the product at that time is as follows. ======================================== Each process at the end of the process ======================================== Sintering step S20 Ceramic substrate 40 (see FIG. 3) SL formation process S30: Ceramic substrate 40A with SL (see FIG. 4) Metal layer formation process S40 Motherboard 60 (see FIG. 5B and FIG. 5C) Etching process S60: collective substrate 60B (see FIG. 7) Dividing step S80: Dividing a plurality of circuit boards 60C (see FIG. 8) Mounting process S90 Multiple mounting boards ======================================== In this specification, the motherboard 60 is an example of a composite board, and the aggregate board 60B is an example of an aggregate.
[0030] The description of this embodiment also includes the following embodiments of the invention. Specifically, the embodiments are as follows. (Invention relating to composite substrate) The motherboard 60 of this embodiment (an example of a composite substrate) comprises a ceramic substrate 40, a first metal layer 50A bonded to the front side of the ceramic substrate 40, and a second metal layer 50B bonded to the back side of the ceramic substrate 40, and at least one of the first metal layer 50A and the second metal layer 50B has at least one notch NT1 or hole HL2 formed in one or both of the first metal layer 50A and the second metal layer 50B to enable identification of the front and back sides of the ceramic substrate 40 (see Figures 5B, 5C, 11-12, 13, etc.). Here, the term "notch" in this specification means a part that is removed while opening at the periphery of the object being formed (specifically, one or both of the first metal layer 50A and the second metal layer 50B). The term "notch" here includes a form in which the whole part of the object in the thickness direction is removed (see reference symbol NT1 in FIG. 5B, reference symbol NT2 in FIG. 10, reference symbol NT4 in FIG. 16, etc.) and a form in which a part of the object in the thickness direction is removed (see reference symbol NT3 in FIG. 13). In this case, the "notch" can also be regarded as a depression. In contrast, the term "hole" in this specification means a part that is removed from the front or back surface of the object being formed (specifically, one or both of the first metal layer 50A and the second metal layer 50B) in the thickness direction without opening at the periphery (see reference symbol HL1 in FIG. 14, reference symbols HL1 and HL2 in FIG. 15A and FIG. 15B, etc.). The "hole" here includes a through hole that penetrates the object to be formed (see reference symbol HL1 in FIG. 14 and reference symbol HL1 in FIGS. 15A and 15B) and a non-through hole (depression) that does not penetrate the object to be formed (see reference symbol HL2 in FIGS. 15A and 15B). This non-through hole can also be considered as a depression or a groove. (Invention relating to the manufacturing method of composite substrate) The manufacturing method of the motherboard 60 (an example of a composite substrate) of this embodiment is a manufacturing method of a motherboard 60 in which a first metal layer 50A and a second metal layer 50B are bonded to the front and back sides, respectively, of a ceramic substrate 40, and includes a notch forming process of forming at least one notch or hole in one of the first metal layer 50A and the second metal layer 50B to enable identification of the front and back sides of the ceramic substrate 40, and a bonding process of bonding the first metal layer 50A and the second metal layer 50B to the front and back sides of the ceramic substrate 40, respectively (see Figures 5A, 5B, etc.). (Invention relating to the manufacturing method of circuit boards) The manufacturing method of the circuit board 60C of this embodiment includes a manufacturing method of the motherboard 60 (an example of a composite substrate) of this embodiment, and an etching process S60 (an example of a circuit pattern forming process) which is performed after the bonding process S42, in which the front and back surfaces of the ceramic substrate 40 are identified from at least one notch NT1 or hole HL1 formed in one or both of the first metal layer 50A and the second metal layer 50B, and a circuit pattern CP on which electronic components (not shown) are mounted is formed on one of the first metal layer 50A and the second metal layer 50B (see Figures 1, 7, etc.). (Invention relating to a method for manufacturing an assembly of multiple circuit boards) The manufacturing method of the aggregate substrate 60B (an example of an aggregate) of the multiple circuit substrates 60C of this embodiment includes the manufacturing method of the motherboard 60 (an example of a composite substrate) of this embodiment, and an etching process S60 (an example of a circuit pattern forming process) that is performed after the bonding process S42 and identifies the front and back surfaces of the ceramic substrate 40 from at least one notch NT1 or hole HL1 formed in one or both of the first metal layer 50A and the second metal layer 50B, and forms circuit patterns CP in each of the multiple regions partitioned by at least one scribe line SL in one of the first metal layer 50A and the second metal layer 50B (see FIG. 1, FIG. 7, etc.). The manufacturing method of the multiple circuit substrates 60C of this embodiment corresponds to the processes from the green sheet forming process S10 to the dividing process S80 in the manufacturing method S100 of this embodiment (see FIG. 1). (Invention relating to a method for manufacturing multiple circuit boards) The method for manufacturing the plurality of circuit boards 60C of the present embodiment includes the following steps: The method includes a manufacturing method for an aggregate substrate 60B (an example of an aggregate) of a plurality of circuit substrates 60C of this embodiment, and a dividing process for cutting the ceramic substrate 40 (or the ceramic substrate 40A with SL) along at least one scribe line SL to divide the aggregate substrate 60B. Each step will be described below.
[0031] <Green sheet forming process and sintering process> In this embodiment, the combination of the green sheet formation step S10 and the sintering step S20, which are performed in the order described above, corresponds to a method for manufacturing the ceramic substrate 40. Hereinafter, a method for manufacturing the ceramic substrate 40 of this embodiment will be described with reference to FIGS. 2A, 2B, 2C, 2D, and 3. FIG.
[0032] Here, the ceramic substrate 40 is, for example, a ceramic substrate provided in a circuit board for a power module mounted on an electric vehicle, a railroad car, or other industrial equipment. The ceramic substrate 40 is, for example, obtained by sintering the single-leaf green sheets 30 (see FIG. 2C) described later in a stacked state (see FIG. 3). The single-leaf green sheets 30 are obtained by cutting the strip-shaped green sheets 20 (see FIGS. 2B and 2C). That is, the relationship between the ceramic substrate 40 and the single-leaf green sheets 30 is the relationship between a finished product and an intermediate product (a product manufactured in a process before becoming a finished product), or the relationship between a first intermediate product and a second intermediate product (a product manufactured in a process before becoming the first intermediate product). Therefore, the single-leaf green sheets 30 of this embodiment are manufactured in the process up to the intermediate stage of the manufacturing method of the ceramic substrate 40 of this embodiment. The ceramic substrate 40 of the present embodiment is, for example, a rectangular plate (see FIG. 4).
[0033] <Green sheet formation process> The green sheet forming step S10 will be described below with reference to Figures 2A, 2B, 2C, and 2D. As shown in the flow diagram of Figure 2A, the green sheet forming step S10 of this embodiment includes a slurry preparing step S11, a molding step S12, a cutting step S13, a laminating step S14, a degreasing step S15, and a sintering step S20, which are performed in the order listed.
[0034] [Slurry preparation process] In this step, a raw material powder and an organic solvent, which will be described later, are mixed to prepare a slurry 10. The slurry 10 (see FIG. 2B) prepared in this step is formed into a belt-shaped green sheet 20 in the next step (forming step).
[0035] The raw powder of the slurry 10 is a powder containing a main component and a sintering aid, which will be described later. The main component is, for example, 80% by weight to 98.3% by mass of silicon nitride (Si 3 N 4 ), and the sintering aid is, for example, 1 weight % to 10 mass % (oxide equivalent) of at least one rare earth element and 0.7 weight % to 10 mass % (oxide equivalent) of magnesium (Mg). The alpha conversion rate of the silicon nitride powder is preferably 20% to 100%, taking into consideration the density, bending strength, and thermal conductivity of the ceramic substrate 40. Here, to clarify the meaning of "~" used in this specification, for example, "20%~100%" means "20% or more and 100% or less." Additionally, "~" used in this specification means "more than or equal to the portion before "~" and less than or equal to the portion after "~".
[0036] Silicon nitride (Si 3 N 4 The reason why the proportion of the sintering aid in the raw material powder is set to 80% by weight to 98.3% by mass, for example, is that the bending strength and thermal conductivity of the obtained ceramic substrate 40 are not too low, and the density of the ceramic substrate 40 is ensured due to a shortage of sintering aid.
[0037] For the sake of simplicity, the raw material powder of silicon nitride is referred to as Si 3 N 4powder (also known as silicon nitride powder, an example of ceramic powder), Mg raw material powder is called MgO powder, rare earth element raw material powder is called Y 2 O 3 However, the raw powder of silicon nitride and the raw powder of the sintering aid are written as Si 3 N 4 Powder and MgO powder and Y 2 O 3 It does not have to be a powder.
[0038] And, the Si compounded as described above 3 N 4 Powder, MgO powder and Y 2 O 3 The powder is mixed with a plasticizer, an organic binder, and an organic solvent to prepare the slurry 10. Therefore, the slurry 10 prepared in this step contains ceramic powder.
[0039] This concludes the description of the slurry preparation step S11.
[0040] [Molding process] Next, the molding step S12 will be described. This step is a step of producing a belt-shaped green sheet 20 from the slurry 10, as shown in FIG. 2B.
[0041] This step is performed, for example, by using a doctor blade molding apparatus 100 shown in FIG. 2B. Here, the doctor blade molding apparatus 100 includes a belt conveying mechanism 110, a molding unit 120, and a heating unit 130. The belt conveying mechanism 110 includes an upstream roller 112A, a downstream roller 112B, and a belt 114, and drives the downstream roller 112 to move the belt 114 from the upstream roller 112 to the downstream roller 112 (along the X direction). The molding unit 120 is disposed above the belt 114 (on the Z direction side of the belt 114) and faces the belt 114. The molding unit 120 includes a storage section 122 that stores the slurry 10, and a doctor blade 124.
[0042] As shown in FIG. 2B, the forming unit 120 uses the doctor blade 124 to regulate the slurry 10, which is taken out of the storage section 122 by its own weight and the adhesive force with the moving belt 114, into a sheet having a set thickness. The heating unit 130 blows hot air WC onto the slurry 10 on the belt 114, which has been cut to a set thickness, to form the slurry 10 into a sheet (evaporate the organic solvent). As a result, in the forming process, a belt-shaped green sheet 20 having a set width (the Y direction in the figure corresponds to the width direction) is produced from the slurry 10. That is, in the forming process, the slurry 10 is formed into a belt shape by doctor blade forming, and as an example, a Si 3 N 4 A belt-shaped green sheet 20 containing (ceramic) is obtained.
[0043] As an example, this step is performed after the slurry 10 produced in the slurry production step S11 is degassed and the slurry 10 is thickened. The thickness of the belt-shaped green sheet 20 produced in this step is set in consideration of the thickness of the ceramic substrate 40 to be finally manufactured. Accordingly, the control conditions (such as the distance from the belt 114) of the doctor blade 124 for controlling the slurry 10 to a set thickness are also set in consideration of the thickness of the ceramic substrate 40 to be finally manufactured.
[0044] This concludes the description of the molding step S12.
[0045] [Cutting process] Next, the cutting step S13 will be described. This step is a step of cutting the belt-shaped green sheet 20 to produce individual green sheets 30, as shown in FIG.
[0046] 2C. The cutting device 200 includes a sheet conveying mechanism 210 and a cutting section 220. The sheet conveying mechanism 210 includes a support section 212, a first conveying section 214, and a second conveying section 216. The support section 212 rotatably supports a roller 112B (see FIGS. 2B and 2C) around which the strip-shaped green sheet 20 produced in the forming step S12 is wound. The first conveying section 214 adjusts the position of the strip-shaped green sheet 20 conveyed from the support section 212 and conveys the strip-shaped green sheet 20 along the X direction (along the longitudinal direction of the strip-shaped green sheet 20) to the cutting section 220. The second conveying section 216 conveys the individual green sheet 30 produced by cutting the strip-shaped green sheet 20 in the cutting section 220 further downstream (in the X direction). The cutting section 220 also has a housing 222, an irradiation section 224, and a moving mechanism 226. The irradiation section 224, for example, irradiates laser light LB. The moving mechanism 226 scans the irradiation section 224 from one end to the other end in the short-side direction (Y direction in the figure) of the strip-shaped green sheet 20. The irradiation section 224 and the moving mechanism 226 are attached to the housing 222.
[0047] In the cutting device 200 of this embodiment, the sheet conveying mechanism 210 conveys the strip green sheet 20 by the length of the single green sheet 30, stops the strip green sheet 20, and cuts the strip green sheet 20 by the cutting unit 220. In this case, the cutting unit 220 irradiates the irradiation unit 224 with the laser light LB while moving the irradiation unit 224 from one end side to the other end side in the short side direction of the strip green sheet 20 along the Y direction by the moving mechanism 226 (see FIG. 2). In addition, the irradiation unit 224 scanned by the moving mechanism 226 irradiates the laser light LB intermittently. Here, "intermittently" means repeating irradiation for a certain period and not irradiating for a certain period. Therefore, the moving mechanism 226 scans the irradiation unit 224 by repeating movement and stopping (see FIG. 2D). As described above, in this process, the belt-shaped green sheet 20 is cut by irradiating the laser light LB onto the belt-shaped green sheet 20 to obtain the single-leaf green sheet 30. The laser light LB may be a carbon dioxide laser light, an infrared laser light, an ultraviolet laser light, or other laser light as long as it can cut the belt-shaped green sheet 20. In addition, in the description of this process, the belt-shaped green sheet 20 is cut using the cutting device 200 shown in FIG. 2C as an example to produce the single-leaf green sheet 30, but other methods may be used as long as the single-leaf green sheet 30 can be produced from the belt-shaped green sheet 20. For example, the single-leaf green sheet 30 may be produced by punching the belt-shaped green sheet 20 by pressing using a press processing device (not shown).
[0048] This concludes the description of the cutting step S13.
[0049] [Lamination process] Next, the lamination step S14 will be described. This step is a step of laminating a plurality of single-leaf green sheets 30 in the thickness direction thereof, as shown in Fig. 3. This step is performed in order to efficiently sinter the single-leaf green sheets 30 in the subsequent step (sintering step S20).
[0050] In this step, as shown in FIG. 3, a plurality of single green sheets 30 are stacked with a non-reactive powder layer (not shown) interposed therebetween, which will be described later. Here, if the number of stacked single green sheets 30 is small, the number of sheets that can be processed at one time in a sintering furnace (not shown) in the subsequent sintering step S16 will be small (production efficiency will be low). In contrast, if the number of stacked single green sheets 30 is large, the binder contained in the single green sheets 30 will be difficult to decompose in the next step (degreasing step S15). For the above reasons, the number of stacked single green sheets 30 in this step is 8 to 100, preferably 30 to 70.
[0051] Moreover, the non-reactive powder layer in this embodiment is, for example, a boron nitride powder layer (BN powder layer) having a film thickness of about 1 μm to 20 μm. The BN powder layer has a function of easily separating the ceramic substrate 40 after the next step (sintering step S16). The BN powder layer is applied as a slurry of BN powder to one side of each green sheet 30 by, for example, spraying, brush application, roll coater, screen printing, or the like. The BN powder has a purity of 85% or more and preferably has an average particle size of 1 μm to 20 μm.
[0052] This concludes the description of the lamination step S14.
[0053] [Degreasing process] Next, the degreasing step S15 will be described. This step is for degreasing the binder and the plasticizer contained in the single green sheet 30 before the next step (sintering step S16). In this step, for example, the plurality of green sheets 30 (see FIG. 3) stacked in the stacking step S14 are held for 0.5 to 20 hours in a temperature environment of 450° C. to 750° C. As a result, the binder and plasticizer contained in the plurality of green sheets 30 are degreased.
[0054] The above is a description of the degreasing step S15. The above is a description of the green sheet forming step S10 of this embodiment.
[0055] <Sintering process> Next, the sintering step S16 will be described with reference to Fig. 3. This step is a step of sintering a plurality of single-leaf green sheets 30 (hereinafter referred to as the plurality of single-leaf green sheets 30 in Fig. 3) that have been stacked in the lamination step S14 and from which the binder and plasticizer have been degreased in the degreasing step S15, using a sintering device (not shown). When this step is completed, a plurality of ceramic substrates 40 are manufactured in a stacked state.
[0056] The above is a description of the sintering step S20. The above is also a description of the method for manufacturing the ceramic substrate 40 of the present embodiment.
[0057] There is no particular limitation on the type of ceramic substrate 40, and examples thereof include carbides, oxides, and nitrides. Specific examples include silicon carbide, alumina, silicon nitride, aluminum nitride, and boron nitride, and more preferably silicon nitride and aluminum nitride.
[0058] <Scribe line formation process> Next, the SL forming step S30 will be described with reference to Fig. 4. This step is a step of forming at least one scribe line SL (three in this embodiment as an example) on one of the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 (front surface 40A1 in this embodiment as an example). When this step is completed, a ceramic substrate 40A with an SL is manufactured (see Fig. 4). In this process, as shown in Fig. 4, a total of three straight line sections are formed on the surface 40A1 of the ceramic substrate 40 by the laser light irradiated from an irradiation unit (not shown), for example, one in the center in the width direction and two lines dividing the length direction into thirds, and the entire area of the surface 40A1 is divided into six equal areas. Here, as an example, each scribe line SL is composed of a plurality of recesses arranged in a straight line (see Fig. 5C). Therefore, the irradiation unit (for example, a carbon dioxide laser light source, a YAG laser light source, etc.) used in this process is capable of irradiating the laser light intermittently, for example. The scribe lines SL are used as cutting lines when dividing the ceramic substrate 40 into a plurality of pieces (six pieces in this embodiment) in a subsequent dividing step S80 (see FIG. 1).
[0059] This concludes the description of the SL forming step S30.
[0060] <Metal layer formation process> Next, the metal layer forming step S40 will be described with reference to Figures 5A, 5B, and 5C. As shown in the flow diagram of Figure 5A, this step includes a notch forming step S41 and a bonding step S42, which are performed in the order described.
[0061] [Notch forming process] The notch forming step S41 is a step of forming a notch NT1 in the first metal layer 50A, which is rectangular when viewed in the thickness direction and is bonded to the front surface 40A1 side of the ceramic substrate 40A with SL (see FIG. 5B). For example, this step may be performed by cutting a strip-shaped metal layer (not shown) using an apparatus such as the cutting apparatus 200 shown in FIG. 2C to produce a rectangular sheet of metal layer, and forming a notch NT1 in the sheet of metal layer using a press unit (not shown) attached to the apparatus to produce the first metal layer 50A. In contrast, in this step, no notch is formed in the second metal layer 50B, which is rectangular when viewed in the thickness direction and is bonded to the back surface 40A2 side of the ceramic substrate 40A with SL.
[0062] In addition, since the above-mentioned first metal layer 50A and second metal layer 50B are bonded to the ceramic substrate 40A with SL in a bonding step S42 described later to form layers, in this specification, the first metal layer 50A and second metal layer 50B, which are plate-shaped before being bonded to the ceramic substrate 40A with SL in the bonding step S42, will be referred to as they are. In addition, the second metal layer 50B and the ceramic substrate 40A with SL have the same shape and size of the outer periphery when viewed from the thickness direction of each. And the first metal layer 50A and the second metal layer 50B are the same in thickness, shape, size and material, except that the first metal layer 50A has a notch NT1 formed therein.
[0063] There are no particular limitations on the type of the first metal layer 50A and the second metal layer 50B, and examples thereof include copper, a copper alloy, aluminum, and an aluminum alloy.
[0064] [Joining process] The bonding step S42 is a step of bonding the first metal layer 50A and the second metal layer 50B to the front surface 40A1 side and the back surface 40A2 side of the ceramic substrate 40A with SL, respectively. In this case, the first metal layer 50A and the second metal layer 50B are bonded to the front surface 40A1 side and the back surface 40A2 side, respectively, via a brazing material (not shown). Specifically, a paste-like active metal brazing material is uniformly applied to the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 by a roll coater method, a screen printing method, a transfer method, or the like, and the first metal layer 50A and the second metal layer 50B are bonded to the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 by an active metal method, respectively, via the uniformly applied paste-like active metal brazing material. Here, in this step, the screen printing method is preferable in terms of uniformly applying the paste-like brazing material. In addition, in this case, it is preferable to control the viscosity of the paste-like active metal brazing material to 5 Pa·s to 20 Pa·s. An excellent active metal brazing material in a paste form can be obtained by blending an organic solvent amount in the range of 5% by mass to 25% by mass and a binder amount in the range of 2% by mass to 15% by mass. The heating temperature for bonding may be, for example, 700°C to 900°C. The atmosphere in the heating furnace may be an inert gas such as nitrogen. The bonded body may be heated under reduced pressure below atmospheric pressure or in vacuum. The heating furnace may be a continuous type in which a plurality of bonded bodies are continuously supplied and heated, or may be a type in which one or a plurality of bonded bodies are heated in a batch manner. The bonded body may be heated while pressing the bonded body in the stacking direction. In this embodiment, when the first metal layer 50A is joined to the SL-equipped ceramic substrate 40A via a brazing material, a part of the scribe line SL is located inside the notch NT1 (see FIG. 5B). That is, the notch forming step S41 in this embodiment is a step of forming the notch NT1 in the first metal layer 50A, which is one of the first metal layer 50A and the second metal layer 50B, so that a part of the scribe line SL is located inside the notch NT1 when viewed from the thickness direction of the SL-equipped ceramic substrate 40A during the joining step S42.
[0065] As described above, the process is performed in the order of the notch forming process S41 and the bonding process S42, and when the process is completed, the motherboard 60 is manufactured (see FIGS. 5B and 5C). 5B, the shape of the notch NT1 formed in the notch forming step S41 is rectangular, but the shape of the notch NT1 does not have to be rectangular as long as a part of the scribe line SL is located inside the notch NT1 at the end of the bonding step S42. For example, the shape may be an arc, a triangle, or another shape.
[0066] This concludes the description of the metal layer forming step S40.
[0067] (Motherboard explanation) Next, the motherboard 60 of this embodiment manufactured at the end of the metal layer forming step S40 will be described with reference to FIGS. 5B and 5C. As described above, the motherboard 60 of this embodiment comprises a ceramic substrate 40, a first metal layer 50A bonded to the front side of the ceramic substrate 40, and a second metal layer 50B bonded to the back side of the ceramic substrate 40, and one or both of the first metal layer 50A and the second metal layer 50B (in this embodiment, the first metal layer 50A) have a notch NT1 formed therein that enables the front side 40A1 and the back side 40A2 of the ceramic substrate 40 to be identified. Moreover, a scribe line SL is formed on one of the front surface 40A1 and the back surface 40A2 (front surface 40A1 in this embodiment) of the ceramic substrate 40 included in the motherboard 60 of this embodiment. That is, the ceramic substrate 40 included in the motherboard 60 of this embodiment is a ceramic substrate 40A with a scribe line SL formed on the front surface 40A1. The notch NT1 is formed in one of the first metal layer 50A and the second metal layer 50B (first metal layer 50A in this embodiment) so that a part of the scribe line SL is located inside the notch NT1 when viewed from the thickness direction of the motherboard 60 (see FIG. 5B).
[0068] In this embodiment, the notch NT1 is formed in only one of the first metal layer 50A and the second metal layer 50B (an example of the above-mentioned first embodiment). Therefore, based on the premise that the surface on which the notch NT is formed is the front surface, the notch NT1 in this embodiment has the function of making it possible to distinguish the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40. In this embodiment, the notch NT1 is formed in the first metal layer 50A so that a part of the scribe line SL is located inside the notch NT1. Therefore, based on the premise that the surface of the ceramic substrate 40 on which the scribe line SL is formed is the front surface, the notch NT1 in this embodiment has the function of enabling the front surface 40A1 and back surface 40A2 of the ceramic substrate 40 to be distinguished from each other.
[0069] <Resist printing process> Next, the resist printing step S50 will be described with reference to FIG. 6. This step is a step of covering the first metal layer 50A of the motherboard 60 with a photosensitive resist film PRF, and forming resist patterns PRP corresponding to each circuit pattern CP described later in six areas partitioned by three scribe lines SL in the first metal layer 50A. Specifically, in this step, as an example, an exposure device (not shown) is used to print the resist pattern PRP on the resist film PRF (the resist pattern PRP is hardened, and the parts of the resist film PRF other than the resist pattern PRP are left unhardened). As a result, a motherboard 60A with PRP is manufactured. Since the notch NT1 is formed in the first metal layer 50A, the worker in this process can easily identify the first metal layer 50A of the notched motherboard 60A. Also, the resist pattern PRP (circuit pattern CP) is not formed in the portion of the first metal layer 50A where the notch NT1 is formed.
[0070] This concludes the description of the resist printing step S50.
[0071] <Etching process> Next, the etching step S60 (one example of a circuit pattern forming step) will be described with reference to FIG. 7. This step is a step of removing the uncured resist film PRF in the resist film PRF of the motherboard 60A with PRP, etching the portion where the first metal layer 50A is exposed, and then removing the remaining resist pattern PRP to form a circuit pattern CP. As a result, the motherboard 60A with PRP before this step becomes an aggregate substrate 60B in which a circuit pattern CP is formed in each of six areas partitioned by three scribe lines SL. Furthermore, when the aggregate substrate 60B is formed, all of the three scribe lines SL formed in the SL forming step S30 are exposed due to the etching of the first metal layer 50A. Accordingly, the portion in the first metal layer 50A where the notch NT1 is formed disappears. That is, the notch NT1 that does not function in the aggregate substrate 60B disappears in this step. Then, in a mounting step S90 described later, electronic components (not shown) such as ICs, capacitors, resistors, etc. are mounted on each circuit pattern CP formed in this step. That is, this step is performed after the bonding step S42, and is a step of identifying the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 from the notch NT1 formed in one or both of the first metal layer 50A and the second metal layer 50B (the first metal layer 50A in this embodiment), and forming a circuit pattern CP on which electronic components (shown) are mounted on one of the first metal layer 50A and the second metal layer 50B (the first metal layer 50A in this embodiment). Furthermore, after this process, a circuit pattern CP on which electronic components (not shown) are mounted is formed in each of a plurality of (six in this embodiment) areas partitioned by at least one scribe line SL (three in this embodiment) in one of the first metal layer 50A and the second metal layer 50B (first metal layer 50A in this embodiment) of the motherboard 60 of this embodiment (see Figures 5B and 5C). In the above description, the etching step S60 is an example of a circuit pattern forming step, but the combination of the resist printing step S50 and the etching step S60 may also be considered as an example of a circuit pattern forming step.
[0072] This concludes the description of the etching step S60.
[0073] <Surface treatment process> Next, the surface treatment step S70 will be described. In this step, the resist remaining on the surface of the metal layer of the etched collective board is removed, and an anti-rust treatment to prevent rusting of the metal layer and Ni-P plating or Ag plating are performed by electroless plating. A solder resist is printed on the circuit pattern of the collective board in order to prevent solder from protruding. This is a step of covering the surface of the surface of the collective board 60B on which the multiple (six in this embodiment) circuit patterns CP are formed, except for the joint parts where the electronic components are joined, with a protective layer (not shown) such as solder resist, and performing a surface treatment on the parts other than the joint parts. In addition, in this step, the joint parts where the electronic components are joined are plated, for example, by electrolytic plating, and the surface treatment of the joint parts is performed. Here, in the above description, the product at the end of the etching step S60 is the collective board 60B, but the product at the end of the surface treatment step S70, that is, the collective board 60B covered with a protective layer, may be regarded as the collective board.
[0074] This concludes the description of the surface treatment step S70.
[0075] <Dividing process> Next, the dividing step S80 will be described with reference to Fig. 8. This step is a step of cutting the aggregate substrate 60B (or the ceramic substrate 40A with SL) along a plurality of scribe lines SL (three in this embodiment as an example) to divide the aggregate substrate 60B into a plurality of circuit substrates 60C (six in this embodiment as an example). That is, this step is a step of cutting the ceramic substrate 40 along at least one scribe line SL (three in this embodiment as an example) to divide the aggregate substrate 60C into a plurality of circuit substrates 60B.
[0076] When this step is completed, a plurality of circuit boards 60C are manufactured. In this embodiment, the first metal layer 50A becomes the circuit pattern CP of each circuit board 60C through the steps up to this point. In contrast, the area of the second metal layer 50B defined by the three scribe lines SL becomes the metal layer on the opposite side of the circuit board 60C on which the circuit pattern CP is formed through the steps up to this point. Then, when using a mounting board (not shown) manufactured through a mounting step S90 described later, this metal layer functions as a heat dissipation layer for dissipating heat generated by electronic components mounted on the circuit pattern CP. Then, after this step, the other of the first metal layer 50A and the second metal layer 50B (the second metal layer 50B in this embodiment) of the motherboard 60 (see FIGS. 5B and 5C) of this embodiment functions as a heat dissipation layer in a plurality of areas (six in this embodiment) defined by at least one scribe line SL (three in this embodiment).
[0077] This concludes the description of the division step S80.
[0078] <Mounting process> Next, the mounting process will be described. This process is a process of mounting electronic components (not shown) on each circuit board 60C (see FIG. 8). In this process, a mounting device (not shown) is used to attach solder (not shown) to the joints of the circuit pattern CP (see FIG. 8) of each circuit board 60C where the electronic components are to be joined, and the joint terminals of the electronic components are joined to the joints.
[0079] When this step is completed, a plurality of mounting boards are manufactured. In the above description, this step is a step following the dividing step S80, but the dividing step S80 may be performed after this step. That is, the manufacturing method S100 of this embodiment may be performed in the order of the surface treatment step S70, the mounting step S90, and the dividing step S80.
[0080] This concludes the description of the mounting process S90. After the manufacture of the plurality of mounting boards, for example, an inspection device (not shown) is used to inspect the circuit pattern CP, inspect the operation of the electronic components, and so on. This concludes the description of the manufacturing method S100 of this embodiment.
[0081] Effect of this embodiment Next, the effects of this embodiment will be described.
[0082] In this embodiment, a first metal layer 50A of a motherboard 60 has a notch NT1 formed therein. Therefore, in the resist printing step S50, the front and back of the motherboard 60 can be easily identified. Accordingly, according to the metal layer forming step S40 of this embodiment (the manufacturing method for the motherboard 60 of this embodiment), it is possible to manufacture a motherboard 60 whose front and back can be easily identified. Furthermore, according to the manufacturing method for the plurality of circuit boards 60C of this embodiment (S10 to S80 in FIG. 1) and the manufacturing method S100 of this embodiment, manufacturing defects do not occur or are unlikely to occur.
[0083] In addition, in the present embodiment, the means for identifying the front and back of the motherboard 60 is not, for example, a mark (such as a printed pattern) affixed to the first metal layer 50A. If the means for identification were the above-mentioned mark, there is a risk that the mark will be rubbed off or otherwise removed during any step of the manufacturing method of this embodiment. In contrast, in the case of this embodiment, the notch NT1, which is a means for distinguishing between the front and back of the motherboard 60, will not disappear due to rubbing or the like. Therefore, in this embodiment, the front and back of the motherboard 60 can be more reliably identified than in the case where the means for identifying the front and back of the motherboard 60 is a mark attached to the first metal layer 50A.
[0084] As described above, the notch NT1 in this embodiment can be formed during the manufacture of the first metal layer 50 A. Specifically, when a strip-shaped metal layer (not shown) is cut using an apparatus such as the cutting apparatus 200 shown in FIG. 2C to manufacture a rectangular sheet of metal layer, the notch NT1 may be formed in the sheet of metal layer using a press unit (not shown) attached to the apparatus to manufacture the first metal layer 50 A. Therefore, according to this embodiment, the notch NT1, which is a means for identifying the front and back of the motherboard 60, can be formed easily or at low cost.
[0085] Moreover, the notch NT1 in this embodiment is formed in a portion of the first metal layer 50A other than the portion where the circuit pattern CP is formed (see FIG. 7). Therefore, the portion of the first metal layer 50A where the notch NT1 is formed is eliminated in the etching step S60. Therefore, according to this embodiment, the effects of the notch NT1 do not remain on the multiple circuit boards 60C and multiple mounting boards that are manufactured.
[0086] Moreover, in this embodiment, the first metal layer 50A is joined to the ceramic substrate 40A with SL so that a part of the scribe line SL is located inside the notch NT1 (see FIG. 5B). Therefore, in the case of this embodiment, the front and back of the motherboard 60 can be identified by directly visually checking the scribe lines SL in the resist printing step S50.
[0087] The above is a description of the effects of this embodiment. Also, the above is a description of this embodiment.
[0088] <<Variations>> As described above, one example of the present invention has been described with reference to the above-mentioned embodiment (see Figs. 1 to 8), but the present invention is not limited to the above-mentioned embodiment. The technical scope of the present invention also includes, for example, the following forms (modifications).
[0089] For example, in the description of the present embodiment, silicon nitride is used as an example of the ceramic powder, but the ceramic powder may be another ceramic powder, for example, aluminum nitride.
[0090] In addition, in the description of the molding step S12 (see FIG. 2A) included in the green sheet formation step S10 of this embodiment, the molding step S12 is performed using doctor blade molding. However, the molding step S12 may be performed by other methods as long as the slurry 10 can be molded into the strip-shaped green sheet 20. For example, the molding step S12 may be performed by extrusion molding.
[0091] In addition, in the explanation of the cutting step S13 (see FIG. 2A) included in the green sheet forming step S10 of this embodiment, the strip green sheet 20 is cut while moving the irradiation unit 224 from one end side to the other end side in the short side direction of the strip green sheet 20. However, as long as the strip green sheet 20 can be cut to obtain a single green sheet 30 as a result, the cut portion of the strip green sheet 20 does not have to be a straight line portion extending from one end side to the other end side in the short side direction of the strip green sheet 20 as in this embodiment. For example, the strip green sheet 20 may be cut so that the single green sheet 30 is separated (or hollowed out) from the strip green sheet 20 by making a hole in the strip green sheet 20 in the shape of the single green sheet 30. In other words, the single green sheet 30 obtained by cutting the strip green sheet 20 may have at least a part of the entire end surface as a cut surface.
[0092] In the present embodiment, the scribe line SL has been described as a plurality of recesses arranged in a straight line (see FIG. 5C). However, as long as the scribe line SL can fulfill its function, it may be, for example, a continuous groove, a plurality of recesses having different lengths, widths, etc.
[0093] In addition, in this embodiment, the multiple scribe lines SL have been described as being three scribe lines SL (see FIG. 4). However, the multiple scribe lines SL may be at least one scribe line SL.
[0094] In addition, in this embodiment, the multiple scribe lines SL are described as dividing the motherboard 60 into six equal parts (see FIG. 4). However, the multiple scribe lines SL do not have to divide the motherboard 60 into equal parts.
[0095] In the present embodiment, the first metal layer 50A and the second metal layer 50B are described as being equivalent in thickness, shape, size, and material, except that the notch NT1 is formed in the first metal layer 50A. However, the first metal layer 50A and the second metal layer 50B may have different thicknesses.
[0096] In the present embodiment, the circuit pattern CP is formed on the first metal layer 50A in which the notch NT1 is formed (see FIGS. 6 and 7). However, the circuit pattern CP may be formed on the second metal layer 50B in which the notch NT1 is not formed. In other words, the notch NT1, which enables identification of the front and back sides of the ceramic substrate 40 (motherboard 60), may be formed on either the first metal layer 50A or the second metal layer 50B.
[0097] In the present embodiment, the notch NT1 has been described as being formed in one place on the first metal layer 50A (see FIG. 5B). However, a plurality of notches NT1 may be formed on the first metal layer 50A. That is, it is sufficient that at least one notch NT1 is formed that enables the front and back sides of the ceramic substrate 40 (motherboard 60) to be distinguished from each other.
[0098] Also, at least one or more notches NT1 may be formed in each of the first metal layer 50A and the second metal layer 50B, and the number of notches NT1 formed in each layer may be different. For example, two notches NT1 may be formed in the first metal layer 50A, and one notch NT1 may be formed in the second metal layer 50B (an example of the second embodiment described above). In this case, based on the premise that two notches are formed on the front side of the motherboard 60, the two notches NT1 formed in the first metal layer 50A and the one notch NT1 formed in the second metal layer 50B make it possible to distinguish the front and back sides of the ceramic substrate 40 (motherboard 60).
[0099] In the present embodiment, it has been described that the notch NT1 is formed in the first metal layer 50A in the metal layer forming step S40, the circuit pattern CP is formed in the first metal layer 50A in the etching step S60, and the second metal layer 50B becomes a plurality of heat dissipation layers when a plurality of circuit boards 60C are manufactured in the dividing step S80. However, the notch NT1 may be formed in the second metal layer 50B, and the circuit pattern CP may be formed in the second metal layer 50B.
[0100] Also, in the present embodiment, the first metal layer 50A having the notch NT1 formed therein is bonded to the ceramic substrate 40 (see the flow diagram of FIG. 5A). However, as in a modified example (first modified example) of the metal layer forming step shown in FIG. 9, the notch NT1 may be formed in the first metal layer 50A after the first metal layer 50A is bonded to the ceramic substrate 40. That is, it is sufficient that the notch NT1 that enables the front and back surfaces of the motherboard 60 to be identified is formed before the resist printing step S50.
[0101] In the present embodiment, the notches NT1 have been described as being formed at positions overlapping parts of the scribe lines SL in the first metal layer 50A (see FIG. 5B). However, as in a modified example (second modified example) of the metal layer forming step shown in FIG. 10, the notches NT2 may be formed at positions other than the positions overlapping parts of the scribe lines SL in the first metal layer 50A. For example, as in this modified example, the notches NT2 may be formed in at least one of the four corners of the first metal layer 50A. Unlike the case of this modified example, the four notches NT2 may be formed in at least one of the four corners. In addition, in the case of this modified example, the notches NT2 may be used as, for example, an alignment mark.
[0102] 10, as an example, the notches NT2 are also formed at the four corners of the second metal layer 50B. In this modification, for example, the notches NT2 of the first metal layer 50A and the notches NT2 of the second metal layer 50B may be different in size from each other (an example of the second aspect described above). According to this modification, the difference in size between the notches NT2 of the first metal layer 50A and the notches NT2 of the second metal layer 50B can be recognized, making it possible to identify the front and back sides of the motherboard 60.
[0103] 10, a notch NT2 is formed at each of the four corners of both the first metal layer 50A and the second metal layer 50B. That is, in the case of the second modification, the notch NT2 is formed at the same portion as viewed from the thickness direction in both the first metal layer 50A and the second metal layer 50B. Here, in the description of the second modification, for example, it is sufficient that the notch NT2 of the first metal layer 50A and the notch NT2 of the second metal layer 50B are different in size from each other. 11, the shape of the notch NT2 in the first metal layer 50A (rectangular as an example) and the shape of the notch NT2 in the second metal layer 50B (triangular as an example) may be different from each other (one example of the second aspect described above). According to the third modification, it is possible to distinguish the front and back sides of the motherboard 60 by recognizing the difference between the shape of the notch NT2 in the first metal layer 50A and the shape of the notch NT2 in the second metal layer 50B. In the case of the third modified example, the notch NT2 of the first metal layer 50A and the notch NT2 of the second metal layer 50B are formed at the same position when viewed from the thickness direction of the ceramic substrate 40. However, based on the premise that the side on which the rectangular notch NT2 is formed is the front surface of the ceramic substrate 40 or the side on which the triangular notch NT2 is formed is the back surface, the notch NT2 of the third modified example has the function of enabling the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 to be distinguished from each other.
[0104] Also, the SL formation step S30 has been described as being performed before the metal layer formation step S40 of this embodiment (see FIGS. 1 and 4). However, as in the case of a modified example (fourth modified example) of the metal layer formation step shown in FIG. 12, the first metal layer 50A and the second metal layer 50B may be bonded to a motherboard 60 on which no scribe line SL is formed without performing the SL formation step S30. In this case, it is sufficient that at least one notch NT1 is formed in one or both of the first metal layers 50A and 50B. In the case of the fourth modified example, if the mounting step S90 is performed without performing the dividing step S80 after the surface treatment step S70 (see FIG. 1), one mounting board is manufactured from one motherboard 60.
[0105] 5B, 5C, etc., the cutout NT1 of the present embodiment is formed by removing the entire portion of the first metal layer 50A in the thickness direction. However, the cutout NT1 of the present embodiment may be formed by removing a portion of the portion of the ceramic substrate 40 in the thickness direction, like the cutout NT3 of the fifth modified example shown in FIG. 13 (an example of the first aspect described above).
[0106] 5B, 5C, etc., the notch NT1 of this embodiment is formed by removing the entire thickness direction portion of the first metal layer 50A. However, the notch NT1 of this embodiment may be formed as a through hole that does not open at the periphery of the ceramic substrate 40 but penetrates the ceramic substrate 40 in the thickness direction, like the hole HL1 of the sixth modified example shown in FIG. 14 (an example of the first aspect described above). In the case of the sixth modified example, on the premise that the side on which the hole HL1 is formed is the front surface of the ceramic substrate 40, the hole HL1 of the fifth modified example has a function of enabling the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 to be distinguished from each other. In the sixth modified example, the shape of the hole HL1 is circular when viewed in the thickness direction of the first metal layer 50A, but the shape of the hole HL1 when viewed in the thickness direction does not have to be circular. Furthermore, hole HL1 and hole HL2 described later can be manufactured by forming hole HL1 or hole HL2 in a sheet of metal layer using a press unit (not shown) to manufacture the first metal layer 50A or the second metal layer 50B, similar to the method of forming notch NT1 in this embodiment.
[0107] 15A and 15B, in a state in which the first metal layer 50A and the second metal layer 50B constitute the motherboard 60, holes HL1 and HL2 of the same size and shape may be formed in the first metal layer 50A and the second metal layer 50B at the same position as viewed from the thickness direction (an example of the third embodiment described above). However, in the case of the seventh modification, the hole HL1 formed in the first metal layer 50A is a through hole, and the hole HL2 formed in the second metal layer 50B is a non-through hole. In the case of the seventh modification, based on the premise that the side where the hole HL1 (through hole) is formed is the front surface of the ceramic substrate 40 and the side where the hole HL2 (non-through hole) is formed is the back surface, one or both of the holes HL1 and HL2 in the seventh modification have the function of enabling identification of the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40. In this case, the color, material or pattern within holes HL1, HL2, which is the side where hole HL1 (through hole) is formed, differs from the color, material or pattern within HL2, which is the side where hole HL2 (non-through hole) is formed, in that the color and material within hole HL1 is the color and material of ceramic substrate 40, and the color and material within hole HL2 is the metal color and metal material. In the seventh modified example, the holes HL1 and HL2 are each circular when viewed in the thickness direction, but they do not have to be circular as long as they have the same size and shape when viewed in the thickness direction.
[0108] 16, in a state in which the first metal layer 50A and the second metal layer 50B constitute the motherboard 60, a plurality of notches NL4 of the same size and shape are formed in each of them at the same position when viewed from the thickness direction (an example of the third embodiment described above). Even in this case, if a feature that enables the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 to be distinguished from each other can be visually recognized from the plurality of notches NT4 in the ceramic substrate 40, the plurality of notches NT4 can be said to be notches that enable the front surface 40A1 and the back surface 40A2 of the ceramic substrate 40 to be distinguished from each other. In the eighth modified example, the scribe lines SL (an example of a pattern) formed on the front surface 40A1 of the ceramic substrate 40 are visible from some of the multiple cutouts NT4, and therefore the scribe lines SL correspond to the above-mentioned feature. From the above, based on the premise that the side on which the scribe line SL is formed within the notch NT1 is the surface of the ceramic substrate 40, the multiple notches NT4 formed in each of the first metal layer 50A and the second metal layer 50B of the eighth modified example have the function of making it possible to distinguish between the surface 40A1 and the back surface 40A2 of the ceramic substrate 40. In the eighth modified example, a plurality of notches NT4 are formed in each metal layer, but each metal layer may have only one notch NT4 formed therein. Also, the notch NT4 in the eighth modified example may be, for example, the hole HL1 (through hole) in the sixth modified example.
[0109] As described above, the above-mentioned embodiment (see FIGS. 1 to 8) and several modified examples (see, for example, FIGS. 9 to 16) have been described separately, but a form that falls within the technical scope of the present invention may be a form that combines one of these with some technical elements of the other forms. For example, the four notches NT2 in the first metal layer 50A of the motherboard 60 (see FIG. 10) of the second modified example may be the notches NT1 (see FIG. 5B) of the above-mentioned embodiment.
[0110] This application claims priority based on Japanese Patent Application No. 2019-102590, filed May 31, 2019, the disclosure of which is incorporated herein in its entirety. [Explanation of symbols]
[0111] 10 Slurry 20 Strip-shaped green sheet 30 Green Sheets 40 Ceramic Substrate 40A Ceramic board with SL 40A1 Surface 40A2 back 50A 1st metal layer 50B 2nd metal layer 60 Motherboard (an example of a composite board) Motherboard with 60A PRP 60B Aggregate substrate (an example of an aggregate) 60C circuit board 100 Doctor blade molding device 110 Belt conveyor mechanism 112 Lola 112A Roller 112B Lola 114 Belt 120 Molding Unit 122 Storage unit 124 Doctor Blade 130 Heating unit 200 Cutting device 210 Sheet transport mechanism 212 Support part 214 First conveyor section 216 Second conveyor section 220 Cutting section 222 Case 224 Irradiation unit 226 Moving mechanism CP circuit pattern HL1 hole (through hole) HL2 hole (non-through hole) LB laser light NT1 cutout NT2 cutout NT3 cutout NT4 cutout PRF resist film PRP resist pattern S10 Green sheet forming process S11 Slurry preparation process S12 Molding process S13 Cutting process S14 Lamination process S15 Degreasing process S16 Sintering process S20 Sintering process S30 SL formation process (scribe line formation process) S40 Metal layer formation process S41 Notch forming process S42 Joining process S50 Resist printing process S60 Etching process S70 Surface treatment process S80 splitting process S90 Mounting process S100 Manufacturing method for mounting board SL Scribe Line WC Hot air
Claims
1. A ceramic substrate; a first metal layer bonded to a front surface side of the ceramic substrate; a second metal layer bonded to a rear surface side of the ceramic substrate; Equipped with At least one notch or hole is formed in one or both of the first metal layer and the second metal layer, which allows identification of the front and back surfaces of the ceramic substrate; When the hole is formed, no hole is formed in a portion of the ceramic substrate that overlaps the hole, A composite substrate, wherein when the notch is formed, the notch is provided in a portion of the periphery of the metal layer having the notch, of the first metal layer and the second metal layer.
2. A ceramic substrate; a first metal layer bonded to a front surface side of the ceramic substrate; a second metal layer bonded to a rear surface side of the ceramic substrate; Equipped with At least one notch is formed in one or both of the first metal layer and the second metal layer, which allows identification of the front and back surfaces of the ceramic substrate; The ceramic substrate is rectangular when viewed in its thickness direction, A composite substrate, wherein the at least one notch is formed in one or both of the first metal layer and the second metal layer so as to expose at least one of four corners of the ceramic substrate.
3. The first metal layer and the second metal layer each have at least one notch or hole formed therein; The at least one notch or hole formed in both of the first and second substrates is different from the other in any one or more of position, size, and shape. The composite substrate according to claim 1 or 2.
4. The at least one notch or hole functions as an alignment mark. The composite substrate according to any one of claims 1 to 3.
5. A circuit pattern on which electronic components are mounted is formed on one of the first metal layer and the second metal layer. The composite substrate according to any one of claims 1 to 4.
6. The other of the first metal layer and the second metal layer functions as a heat dissipation layer. The composite substrate according to claim 5 .
7. A ceramic substrate; a first metal layer bonded to a front surface side of the ceramic substrate; a second metal layer bonded to a rear surface side of the ceramic substrate; Equipped with At least one notch or hole is formed in one or both of the first metal layer and the second metal layer, which allows identification of the front and back surfaces of the ceramic substrate; At least one scribe line is formed on one of the front and back surfaces of the ceramic substrate, A composite substrate, wherein the at least one notch or hole is formed in one of the first metal layer and the second metal layer so that a portion of the at least one scribe line is located inside the notch or hole when viewed in the thickness direction of the ceramic substrate.
8. a circuit pattern on which an electronic component is mounted is formed in each of a plurality of regions defined by the at least one scribe line in one of the first metal layer and the second metal layer; The composite substrate according to claim 7 .
9. a plurality of regions defined by the at least one scribe line in the other of the first metal layer and the second metal layer each function as a heat dissipation layer; The composite substrate according to claim 8 .
10. A method for manufacturing a composite substrate in which a first metal layer and a second metal layer are bonded to a front side and a back side of a ceramic substrate, respectively, comprising the steps of: a notch forming step of forming at least one notch or hole in one or both of the first metal layer and the second metal layer, the notch or hole enabling identification of the front and back surfaces of the ceramic substrate; a bonding step of bonding the first metal layer and the second metal layer to a front side and a back side of the ceramic substrate, respectively; Including, When the hole is formed, no hole is formed in a portion of the ceramic substrate that overlaps the hole, A method for manufacturing a composite substrate, wherein when the notch is formed, the notch is provided in a portion of the periphery of the metal layer having the notch, of the first metal layer and the second metal layer.
11. A method for manufacturing a composite substrate in which a first metal layer and a second metal layer are bonded to a front side and a back side of a ceramic substrate, respectively, comprising the steps of: a notch forming step of forming at least one notch in one or both of the first metal layer and the second metal layer, respectively, that allows identification of the front and back surfaces of the ceramic substrate; a bonding step of bonding the first metal layer and the second metal layer to a front side and a back side of the ceramic substrate, respectively; Including, The ceramic substrate is rectangular when viewed in its thickness direction, A method for manufacturing a composite substrate, wherein the at least one notch is formed in one or both of the first metal layer and the second metal layer so as to expose at least one of four corners of the ceramic substrate.
12. In the notch forming step, the at least one notch or hole that is different from the other in any one or more of position, size, and shape is formed in both of the substrates. A method for producing the composite substrate according to claim 11.
13. A method for manufacturing a composite substrate in which a first metal layer and a second metal layer are bonded to a front side and a back side of a ceramic substrate, respectively, comprising the steps of: a notch forming step of forming at least one notch or hole in one of the first metal layer and the second metal layer, respectively, which allows identification of the front and back surfaces of the ceramic substrate; a bonding step of bonding the first metal layer and the second metal layer to a front side and a back side of the ceramic substrate, respectively; Including, At least one scribe line is formed on one of the front and back surfaces of the ceramic substrate, A method for manufacturing a composite substrate, wherein the at least one notch or hole is formed in one of the first metal layer and the second metal layer so that a portion of the at least one scribe line is located inside the notch or hole when viewed in the thickness direction of the ceramic substrate.
14. A method for producing a composite substrate according to any one of claims 10 to 13, a pattern forming step, which is performed after the bonding step, of identifying a front surface and a back surface of the ceramic substrate from the at least one notch or hole formed in one or both of the first metal layer and the second metal layer, and forming a circuit pattern on one of the first metal layer and the second metal layer for mounting an electronic component; Including, A method for manufacturing a circuit board.
15. a scribe line forming step, which is a step performed before the bonding step, of forming at least one scribe line on the front or back surface of the ceramic substrate; Including, A method for producing a composite substrate according to any one of claims 10 to 12.
16. A method for producing a composite substrate according to claim 13 or 15; a pattern forming step, which is performed after the bonding step, of identifying a front surface and a back surface of the ceramic substrate from the at least one notch or hole formed in one or both of the first metal layer and the second metal layer, and forming a circuit pattern in each of a plurality of regions partitioned by the at least one scribe line in one of the first metal layer and the second metal layer; Including, A method for manufacturing an assembly of multiple circuit boards.
17. A method for manufacturing an assembly of a plurality of circuit boards according to claim 16; a dividing step of cutting the ceramic substrate along the at least one scribe line to divide the assembly of the plurality of circuit substrates; Including, A method for manufacturing a plurality of circuit boards.
Citation Information
Patent Citations
Ceramics circuit substrate
JP2001168482A
Method of manufacturing module structure, circuit board and method of fixing the same
JP2004096035A
Method for manufacturing nitride ceramics circuit board
JP2007324301A
Wiring board and electronic apparatus using the same
JP2008211159A
Method of manufacturing copper-clad resin composite ceramic board
JP2011166040A