Controlled long chain branching in EPDM by post-reactor modification
Electron beam radiation of metallocene-catalyzed EPDM terpolymers introduces controlled long chain branches, addressing the challenges of LCB control and improving rheological properties for enhanced processability and elasticity.
Patent Information
- Application Number
- JP2021577044
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-06-26
- Filing Date
- 2020-06-18
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2040-06-18
AI Technical Summary
Existing methods for producing ethylene-propylene-diene monomer (EPDM) with long chain branches (LCBs) face challenges in controlling LCB levels, leading to undesirable crosslinking and broad molecular weight distribution, which affects the polymer's properties and processability.
A process involving electron beam radiation of metallocene-catalyzed EPDM terpolymers at specific doses to introduce controlled LCBs, resulting in branched terpolymers with improved rheological properties.
The process enhances the rheological properties of EPDM by increasing LCBs, reducing cold flow, improving elasticity, and enhancing processability without undesirable crosslinking, as evidenced by increased Mooney viscosity, relaxation area, and reduced phase angle.
Smart Images

Figure 0007581262000001 
Figure 0007581262000002 
Figure 0007581262000003
Abstract
Description
[Background technology]
[0001] Ethylene-propylene-diene monomer terpolymers (EPDM) with molecular structures containing long-chain branching (LCB) are known. LCB introduces side chains into the EPDM backbone, significantly altering the rheological and physical properties of EPDM. For example, LCB improves the elastic and shear-thinning properties of EPDM. Advantages of high-LCB EPDM compared to non-branched EPDM include reduced cold flow, improved green strength, improved collapse resistance during extrusion of hollow parts, improved foamability, faster extrusion speeds, faster mixing, reduced energy consumption in internal mixers, increased filler loading, and reduced melt fracture.
[0002] The choice of catalyst used under the polymerization and polymerization process conditions provides a method for adjusting the LCB level in EPDM structure. Ziegler-Natta (ZN) catalysts (e.g., titanium-based or vanadium-based catalysts) can introduce LCBs into EPDM during the polymerization process. However, the level of LCBs is difficult to control; for example, ZN polymerization processes tend to produce undesirable crosslinked EPDM, which leads to gel formation. ZN polymerization processes also produce EPDM with a wide compositional and molecular weight distribution.
[0003] Metallocene catalysts (e.g., zirconium-based catalysts) produce EPDM in a solution polymerization process. Metallocene catalysts generally produce EPDM with a more uniform composition distribution, narrower MWD, and a more linear molecular structure compared to ZN-catalyzed EPDM. However, metallocene catalysts typically produce lower levels of LCB compared to ZN-catalyzed EPDM.
[0004] Therefore, the art has recognized a need for high LCB EPDM. The art has further recognized a need for methods to increase LCB in metallocene-catalyzed EPDM. Summary of the Invention
[0005] Disclosed herein is a process. In one embodiment, the process includes providing a neat ethylene / propylene / non-conjugated polyene terpolymer (n-terpolymer) having a Mooney viscosity (ML(1+4) at 125°C) of less than 100 Mooney units (MU). The process includes exposing the n-terpolymer to electron beam radiation at a dose of 0.2 megarads (MRad) to 1.3 MRad. The process includes forming a branched ethylene / propylene / non-conjugated polyene terpolymer (b-terpolymer) having a Mooney viscosity at 125°C, ML(1+4), of 25 MU to 135 MU.
[0006] Also disclosed herein is a composition, in one embodiment, comprising a branched ethylene / propylene / non-conjugated polyene terpolymer (b-terpolymer) having (A) a Mooney viscosity (ML 1+4 at 125°C) of 35 MU to 120 MU, (B) a rheology ratio of 55 to 110, and (C) a phase angle δ of 20° to 39°.
[0007] definition All references herein to the Periodic Table of the Elements shall refer to the Periodic Table of the Elements, published and copyrighted 2003 by CRC Press, Inc. Also, any reference to a Group(s) shall be to the Group(s) reflected in that Periodic Table of the Elements using the IUPAC system for numbering groups.
[0008] For purposes of United States patent practice, the contents of any referenced patent, patent application, or publication are incorporated by reference in their entirety (or the equivalent United States version is so incorporated by reference), particularly with respect to the disclosure of definitions (to the extent not inconsistent with any definitions specifically provided in this disclosure) and general knowledge in the art.
[0009] Numerical ranges disclosed herein include all values (boundaries) between the lower and upper limits, and ranges including explicit values (e.g., from 1, 2, or 3 to 5, 6, or 7) also include all subranges between any two explicit values (e.g., 1-2, 2-6, 5-7, 3-7, 5-6, etc.).
[0010] Unless stated to the contrary, implicit from the context, or customary in the art, all parts and percentages are by weight and all test methods are current as of the filing date of this disclosure.
[0011] As used herein, the term "composition" refers to a mixture of materials that comprise the composition, as well as reaction products and decomposition products formed from the materials of the composition.
[0012] The terms "comprising," "including," "having," and their derivatives are not intended to exclude the presence of any additional component, step, or procedure, regardless of whether such component, step, or procedure is specifically disclosed herein. For the avoidance of doubt, all compositions claimed through the use of the term "comprising" may include any additional additive, adjuvant, or compound (whether polymeric or non-polymeric) unless stated to the contrary. In contrast, the term "consisting essentially of" excludes from the scope of any subsequent recitation any other component, step, or procedure, except those that are not essential to operability. The term "consisting of" excludes any component, step, or procedure not expressly delineated or listed. The term "or," unless expressly stated otherwise, refers to the listed members individually and in any combination. The use of the singular includes the use of the plural, and vice versa.
[0013] An "ethylene-based polymer" is a polymer containing greater than 50 weight percent polymerized ethylene monomer (based on the total amount of polymerizable monomers) and, optionally, may contain at least one comonomer. Ethylene-based polymers include ethylene homopolymers and ethylene copolymers (meaning units derived from ethylene and one or more comonomers). The terms "ethylene-based polymer" and "polyethylene" may be used interchangeably. Non-limiting examples of ethylene-based polymers (polyethylenes) include low-density polyethylene (LDPE) and linear polyethylene. Non-limiting examples of linear polyethylene include linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (ULDPE), very low-density polyethylene (VLDPE), multicomponent ethylene-based copolymers (EPE), ethylene / α-olefin multiblock copolymers (also known as olefin block copolymers (OBC)), single-site catalyzed linear low-density polyethylene (m-LLDPE), substantially linear or linear plastomers / elastomers, and high-density polyethylene (HDPE). Generally, polyethylene can be produced in gas phase, fluidized bed reactors, liquid phase slurry process reactors, or liquid phase solution process reactors using heterogeneous catalyst systems such as Ziegler-Natta catalysts, homogeneous catalyst systems comprising Group 4 transition metals and ligand structures (e.g., metallocene, nonmetallocene metal-centered, heteroaryl, heterovalent aryloxy ether, phosphinimine, etc.). Combinations of heterogeneous and / or homogeneous catalysts can also be used in either single or dual reactor configurations. In one embodiment, the ethylene-based polymer does not contain aromatic comonomers polymerized in the polymer.
[0014] The terms "interpolymer" and "copolymer" refer to polymers prepared by the polymerization of at least two different types of monomers. These collective terms include both classical copolymers, i.e., polymers prepared from two different types of monomers, and polymers prepared from three or more different types of monomers, e.g., terpolymers, tetrapolymers, etc.
[0015] As used herein, the term "electron beam radiation" or ("e-beam") refers to the generation of an electron beam from a heated cathode filament (typically tungsten). Electrons emitted from the cathode are accelerated in an electric field applied between the cathode and anode. The energy gain of the electron beam is proportional to the accelerating voltage. Energy is measured in eV (electron volts), and accelerators up to 10 MeV are commercially available. Electron beam exposure dose is measured in megarads (MRad). When the electron beam enters a polymer, it ionizes and excites the molecules, resulting in the displacement of hydrogen atoms and the formation of free radicals. The combination of two free radicals forms branches. The type of branch formed by this method is H-type or tetrafunctional.
[0016] The term "entanglement molecular weight" as used herein is explained as follows: A plot of the logarithm of the structurally undeformed mechanical properties of a polymer melt plotted against the logarithm of molecular weight exhibits an initial weak linear dependence at approximately 10 kDa followed by a transition to a strong dependence on molecular weight. This "transition molecular weight" is called the "entanglement molecular weight." While polymers above the entanglement molecular weight are useful as plastics, polymers below the entanglement molecular weight exhibit characteristics of low-molecular-weight materials, typically brittle powders. For example, candle wax is a low-molecular-weight polyolefin with the same molecular structure as polyethylene.
[0017] The term "long chain branching" or ("LCB") as used herein refers to the presence of side chains on an ethylene / propylene / diene-monomer terpolymer where the side chain molecular weight exceeds the entanglement molecular weight of the polymer.
[0018] The term "polymer" refers to a material prepared by reacting (i.e., polymerizing) a set of monomers, whether the set is a homogeneous (i.e., only one type of) set of monomers or a heterogeneous (i.e., two or more types of) set of monomers. As used herein, the term polymer includes the term "homopolymer," which refers to a polymer prepared from a homogeneous set of monomers, and the term "interpolymer," which is defined below.
[0019] The term "terpolymer" refers to a polymer prepared by the polymerization of three different types of monomers.
[0020] Test Method Mooney Viscosity Test: EPDM rubber Mooney viscosity is measured using a Mooney shear disc viscometer according to ASTM 1646-04. The instrument is an Alpha Technologies Mooney Viscometer 2000. The torque required to rotate the rotor at 2 rpm is measured by a torque transducer. After closing the platen, the sample is preheated for 1 minute. The motor is then started and the torque is recorded for 4 minutes. Results are reported in Mooney units (MU) as "ML(1+4) at 125°C." The term "ML" indicates that a large rotor, "Mooney Large," is used in the viscosity test; this large rotor is a standard-sized rotor. Mooney viscosity (MV) measures the resistance of a polymer to flow at relatively low shear rates and indicates the polymer's fluidity.
[0021] Mooney relaxation area (MLRA) data are obtained from Mooney viscosity measurements in which a test sample relaxes after the rotor stops. At the end of a Mooney viscosity test, the disk stops rotating within 0.1 seconds. Relaxation data collection typically begins 1 second after the rotor stops and continues for at least 2 minutes after the rotor stops. The reported MLRA value is the integrated area under the Mooney torque relaxation time curve from 1 second to 120 seconds (MLRA(1' + 4' + 2')). The MLRA value indicates the degree of elasticity of a polymer and can be considered a stored energy term. A higher MLRA value indicates that the test sample stores more energy and requires more time to relax (i.e., dissipate the stored energy) after the applied strain is removed. More elastic polymers (e.g., polymers with longer long-chain branching) typically exhibit higher MLRA values compared to less elastic polymers (e.g., polymers with shorter long-chain branching). MLRA is reported in Mooney units-seconds (MU·s).
[0022] As used herein, the term "MLRA / ML ratio" is the ratio of Mooney relaxation area to Mooney viscosity and is an abbreviation for "MLRA / ML(1+4) at 125°C." The MLRA / ML ratio indicates the degree of melt elasticity of a polymer and is directly proportional to the degree of melt elasticity. The MLRA / ML ratio is reported in seconds.
[0023] Rubber Rheological Property Analysis (RPA): Rubber rheological property analysis is performed according to ASTM D6204 using a rotorless oscillatory shear rheometer (i.e., Rubber Process Analyzer (RPA)). RPA frequency sweep tests are performed using an Alpha Technologies RPA 2000. Test samples are cut using a Cutter 2000R. The sample size is 5 to 7 grams. The test specimen is considered to be of appropriate size (116 to 160% of the test cavity volume) if a small bead of rubber compound is extruded uniformly around the die when the die is closed. The sample is placed between two pieces of Mylar film. A frequency sweep is performed at 125°C using 5% strain for the neat terpolymer. A frequency sweep is performed at 100°C using 5% strain for the terpolymer composition. The frequency range is 0.1 radians per second (rad / s) to 100 rad / s. The stress response was analyzed in terms of amplitude and phase, from which the storage shear modulus (G'), loss shear modulus (G"), complex viscosity (V), tan delta (i.e., phase angle δ), and complex shear modulus G* were calculated. Modulus values are reported in kilopascals (kPa), phase angles are reported in degrees, and viscosity is reported in pascal-seconds (Pa s).
[0024] The term "phase angle δ" as used herein is the phase lag exhibited between an applied stress and the resulting strain imparted by that stress. For a given dynamic mechanical study, the phase angle δ is measured at a complex shear modulus G* value of 100 kPa and 125°C. When comparing the phase angles δ of a group of polymers, a reduced value of the phase angle δ generally indicates that the polymer is more elastic.
[0025] The term "Rheological Ratio" (or "RR") is calculated as the ratio of the complex viscosity at 0.1 rad / sec and 125°C to the complex viscosity at 100 rad / sec and 125°C, where RR is equal to V0.1 / V100 at 125°C.
[0026] High Temperature Gel Permeation Chromatography Test ("HT GPC Test"): The HT GPC test consisted of an infrared concentration / composition detector (IR-5 detector), a PDI 2040 laser light scattering detector (Agilent), and a 4-capillary bridge viscometer (Malvern), and was used to measure number average molecular weight (M N ), weight average molecular weight (M W ), and zeta-average molecular weight (M Z The procedure is carried out using a POLYMERCHAR (Valencia, Spain) HT GPC system, which allows the determination of the .alpha.-methyl-.beta.-methyl.beta.
[0027] The columns were four mixed A LS 20 micrometer columns (Agilent). The detector compartment was operated at 160°C and the column compartment at 150°C. The carrier solvent was 1,2,4-trichlorobenzene (TCB) containing approximately 250 ppm butylated hydroxytoluene (BHT) and was nitrogen sparged.
[0028] The HT GPC system is calibrated with 21 narrow molecular weight distribution polystyrene standards. The molecular weights of the standards range from 580 to 8,400,000 and are arranged in six "cocktail" mixtures with a separation of at least 10 between individual molecular weights. The resulting molecular weight data (M ps ) into equation (1):M pe =A(M ps ) B Polyethylene molecular weight data (M pe ), where the A value was determined iteratively and is approximately 0.42 and the B value is 1.0. A fifth-order polynomial was used to fit each polyethylene-equivalent calibration point obtained from equation (1) for each polystyrene standard to their observed elution volumes.
[0029] M N , M W , and M Z is calculated according to the following equation:
number
[0030] For irradiated terpolymers (i.e., terpolymers exposed to electron beam treatment), candidates for HT GPC analysis are randomly selected and cut into sections. Each HT GPC analyte is prepared using a blend of sections cut from various terpolymers to overcome any radiation heterogeneity within individual terpolymer samples. HT GPC analytes are prepared at a concentration of approximately 2.0 milligrams per milliliter (mL) using approximately 60 milligrams of cut sections and 30 mL of TCB dissolved in a glass vial with an aluminum foil-lined cap. The analytes are heated at 150 °C for 3 hours with gentle stirring and then transferred to an injection vial at high temperature. The solution in the injection vial is then heated at 160 °C for 30 minutes before injection. The injection volume is 200 microliters, and the flow rate is 1.0 mL / min. The analytes are filtered through an in-line filter during injection to remove insoluble material.
[0031] As used herein, the term "initial analyte" is the mass of analyte injected into the HT GPC system. As used herein, the term "filtered analyte" is the mass of analyte that exits the in-line filter and is recovered from the IR-5. The weight fraction of the "soluble fraction" is the result of dividing the filtered analyte by the initial analyte. For samples that contain an insoluble fraction, the value reported is for only the soluble portion of the analyte.
[0032] 4. The capillary bridge viscometer measures the intrinsic viscosity (η) of the analyte. The g' value of the analyte is calculated as η 直鎖状 Calculate as η divided by (i.e., g' = η / η 直鎖状 ), where η 直鎖状 is the intrinsic viscosity of a linear polymer with the same molecular weight.
[0033] Mass Recovery Test: The mass recovery (M-REC) is calculated using the analyte quantity values obtained from the HT GPC test by the formula M-REC=100×[(initial analyte−filtered analyte) / initial analyte].
[0034] It is understood that polymers with internal crosslinks form insoluble gels that are quantitatively detectable by mass recovery analysis. It is further understood that polymers exhibiting 85% or greater mass recovery are free of internal crosslinks.
[0035] The g' value of the irradiated terpolymer is used to calculate the amount of long-chain branching. The change in g' value (i.e., the ratio of the g' value of the irradiated terpolymer divided by the g' value of the same non-irradiated terpolymer) was calculated according to the pioneering work on long-chain branching by Zimm and Stockmeyer, "The Dimensions of Chain Molecules Containing Branches and Rings," BH Zimm, WH Stockmeyer, The Journal of Chemical Physics, Vol. 17, pages 1301-1314, 1949, the entire contents of which are incorporated herein by reference. The g' values used in the standard were converted to g' values using the following equation with an empirical value of 0.5: g ε =g' Based on the calculated g' values, the long chain branches per chain of each resin were calculated based on the linear correlation between the number of branches in tetrafunctional (H-type) branched polymers and the g value by Zimm and Stockmayer.
[0036] Monomer Content Test: The ethylene and propylene content of the terpolymers on a weight percent basis is determined by Fourier Transform Infrared (FTIR) analysis according to ASTM D3900. The ENB content of the terpolymers on a weight percent basis is determined by Fourier Transform Infrared (FTIR) analysis according to ASTM D6047.
[0037] Residual Elemental Analysis Testing: Residual elemental analysis is performed using both inductively coupled plasma atomic emission spectroscopy (ICP-AES) and X-ray fluorescence (XRF) techniques. For ICP-AES analysis, the sample is weighed into a quartz tube, and 1 mL of water and 3 mL of nitric acid are added to the sample. The sample is placed in a 115°C hot block for 30 minutes. The sample is then placed in an UltraWave microwave oven and digested at 250°C. After microwave digestion, the sample is diluted and analyzed for aluminum, calcium, chromium, titanium, and vanadium on a Perkin Elmer ICP. For XRF analysis, the sample is plaqued in a hot press at 260°F. The sample is then rinsed with distilled water, then acetone, and the chlorine content is measured by XRF. Results are reported in parts per million (ppm).
[0038] Density is measured according to ASTM D792, Method B. Results are reported in grams per cubic centimeter (g / cc or g / cm 3 ) to record. DETAILED DESCRIPTION OF THE INVENTION
[0039] process The present disclosure provides a process. In one embodiment, the process includes providing an ethylene / propylene / non-conjugated polyene terpolymer. The terpolymer is neat and has a Mooney viscosity of less than 100 Mooney units, where the Mooney viscosity test condition is ML(1+4) at 125°C. The process includes exposing the neat terpolymer to electron beam radiation. The neat terpolymer is exposed to electron beam radiation at a dose of 0.2 megarads (MRad) to 1.3 MRad. The process includes forming a branched ethylene / propylene / non-conjugated polyene terpolymer. The branched terpolymer has a Mooney viscosity of 25 Mooney units to 135 Mooney units.
[0040] The process includes providing a terpolymer. In one embodiment, the terpolymer is an ethylene / α-olefin / non-conjugated polyene, which comprises, in polymerized form, ethylene, an α-olefin, and a non-conjugated polyene. Suitable examples of α-olefins include C3-C20 α-olefins or C3-C8 α-olefins. Suitable examples of non-conjugated polyenes include C4-C40 non-conjugated dienes.
[0041] In one embodiment, the α-olefin is a C3-C8 aliphatic α-olefin. In a further embodiment, the α-olefin is selected from the group consisting of propylene, 1-butene, 1-hexene, and 1-octene.
[0042] In one embodiment, the α-olefin is propylene.
[0043] In one embodiment, the non-conjugated polyene is an acyclic diene or a cyclic diene.Non-limiting examples of acyclic dienes include straight-chain acyclic dienes, such as 1,4-hexadiene and 1,5-heptadiene, and branched-chain acyclic dienes, such as 5-methyl-1,4-hexadiene, 2-methyl-1,5-hexadiene, 6-methyl-1,5-heptadiene, 7-methyl-1,6-octadiene, 3,7-dimethyl-1,6-octadiene, 3,7-dimethyl-1,7-octadiene, 5,7-dimethyl-1,7-octadiene, and 1,9-decadiene, and mixed isomers of dihydromyrcene. Non-limiting examples of cyclic dienes include monocyclic dienes such as 1,4-cyclohexadiene, 1,5-cyclooctadiene, and 1,5-cyclododecadiene, polycyclic alicyclic fused and bridged ring dienes such as tetrahydroindene and methyltetrahydroindene, alkenyl, alkylidene, cycloalkenyl, and cycloalkylidene norbornenes such as 5-methylene-2-norbornene (MNB), 5-ethylidene-2-norbornene (ENB), 5-vinyl-2-norbornene, 5-propenyl-2-norbornene, 5-isopropylidene-2-norbornene, 5-(4-cyclopentenyl)-2-norbornene, and 5-cyclohexylidene-2-norbornene.
[0044] In one embodiment, the non-conjugated polyene does not contain heteroatoms. As used herein, the term "heteroatom" refers to an atom other than carbon or hydrogen. Heteroatoms can be non-carbon atoms from groups IV, V, VI, and VII of the periodic table. Non-limiting examples of heteroatoms include F, N, O, P, B, S, and Si.
[0045] In one embodiment, the non-conjugated polyene is ENB.
[0046] In one embodiment, the terpolymer contains only one type of non-conjugated polyene, which is inactive or does not contain heteroatoms.
[0047] In one embodiment, the terpolymer is an ethylene / propylene / norbornene terpolymer. In a further embodiment, the terpolymer is an ethylene / propylene / ENB terpolymer. As used herein, the term "EPDM" refers to an ethylene / propylene / ENB terpolymer having only three monomers, with ENB being the only diene in the terpolymer.
[0048] In one embodiment, the terpolymer is a neat terpolymer. As used herein, the term "neat" refers to a material that has no oil in or on its structure. As used herein, the term "neat" refers interchangeably to a material that is "oil-free." In one embodiment, the EPDM is neat EPDM (i.e., "n-EPDM").
[0049] In one embodiment, the n-EPDM used herein is produced using a metallocene catalyst as described in U.S. Pat. No. 8,101,696, the entire contents of which are incorporated herein by reference.
[0050] The n-EPDM has a Mooney viscosity of less than 100 MU. In one embodiment, the n-EPDM has a Mooney viscosity of 20 MU, or 30 MU, or 40 MU, or 50 MU, or 60 MU, or 65 MU, or 70 MU, to 80 MU, or 85 MU, or 90 MU, or 99 MU. In a further embodiment, the n-EPDM has a Mooney viscosity of 20-99 MU, or 30-99 MU, or 60-80 MU.
[0051] In one embodiment, the n-EPDM has a Mooney Relaxation Area (MLRA) of 25 Mooney units-seconds (MUs), or 30 MUs, or 180 MUs, to 280 MUs, or 475 MUs, or 510 MUs, or 550 MUs. In further embodiments, the n-EPDM has a MLRA of 25 to 550 MUs, or 30 to 475 MUs, or 180 to 280 MUs.
[0052] In one embodiment, the n-EPDM has an MLRA / ML ratio of from 0.5 seconds, or 1 second, or 2 seconds, or 3 seconds, or 3.3 seconds, to 4 seconds, or 4.5 seconds, or 5 seconds, or 6 seconds, or 6.5 seconds, or 7 seconds, or 7.5 seconds, or 8 seconds. In further embodiments, the n-EPDM has an MLRA / ML ratio of 0.5 to 8 seconds, or 2 to 6.6 seconds, or 3 to 6 seconds.
[0053] In one embodiment, the n-EPDM has a rheology ratio (RR) of from 20, or 25, or 30, or 35, to 40, or 45, or 50, or 55, or 60, or 65. In further embodiments, the n-EPDM has a RR of 20-65, or 25-60, or 30-55.
[0054] The n-EPDM has a phase angle δ of 41° or greater. In one embodiment, the n-EPDM has a phase angle δ of 41°, or 45°, or 50°, to 60°, or 70°, or 85°. In a further embodiment, the n-EPDM has a phase angle δ of 41° to 85°, or 45° to 70°, or 50° to 60°.
[0055] In one embodiment, the n-EPDM contains from 50 weight percent (wt%), or 55 wt%, or 60 wt%, or 68 wt%, to 70 wt%, or 72 wt%, or 74 wt%, or 80 wt% polymerized ethylene. In further embodiments, the n-EPDM contains 50-80 wt%, or 60-74 wt%, or 68-72 wt% polymerized ethylene. In one embodiment, the n-EPDM contains from 23 wt%, or 25 wt%, to 27 wt%, or 30 wt%, or 35 wt%, or 38 wt% polymerized propylene. In further embodiments, the n-EPDM contains 23-38 wt%, or 25-35 wt%, or 25-30 wt% polymerized propylene. In one embodiment, the n-EPDM contains from 0.5%, or 1%, or 2%, or 3%, or 3.5%, or 4%, or 4.5%, or 4.7% to 5.1%, or 5.5%, or 6%, or 7%, or 8%, or 8.5%, or 9% by weight of polymerized ENB. In further embodiments, the n-EPDM contains 0.5-9%, or 0.5-8.5%, or 0.5-7%, or 4-5% by weight of polymerized ENB. The weight percentages are based on the total weight of the n-EPDM.
[0056] In one embodiment, the n-EPDM has a molecular weight distribution (MWD) of from 1.8, or 2.0, or 2.2, or 2.4, or 2.6 to 3.1, or 3.2, or 3.5, or 4.0, or 5.0. In further embodiments, the n-EPDM has an MWD of from 1.8 to 5.0, or from 2.0 to 4.0, or from 2.2 to 3.5, or from 2.3 to 3.1.
[0057] The n-EPDM may comprise a combination of two or more embodiments described herein.
[0058] The terpolymer may comprise a combination of two or more embodiments described herein.
[0059] The process includes exposing a terpolymer (e.g., n-EPDM) to electron beam radiation. In one embodiment, the terpolymer (e.g., n-EPDM) is exposed to a radiation dose of 0.2 megarads (MRad), or 0.3 MRad, or 0.4 MRad, to 0.5 MRad, or 0.6 MRad, or 0.7 MRad, or 0.8 MRad, or 0.9 MRad, or 1 MRad, or 1.1 MRad, or 1.2 MRad, or 1.3 MRad, or 1.5 MRad. In further embodiments, the terpolymer (e.g., n-EPDM) is exposed to a radiation dose of 0.2-1.3 MRad, or 0.3-1.2 MRad, or 0.3-0.9 MRad, or 0.3-0.7 MRad, or 0.4-0.5 MRad.
[0060] In one embodiment, the terpolymer (e.g., n-EPDM) is exposed for an exposure time of 1 millisecond, or 2 milliseconds, or 4 milliseconds, or 6 milliseconds, or 8 milliseconds, or 10 milliseconds, to 12 milliseconds, or 14 milliseconds, or 18 milliseconds, or 20 milliseconds, or 30 milliseconds, or 100 milliseconds. In further embodiments, the terpolymer (e.g., n-EPDM) is exposed for an exposure time of 1 to 100 milliseconds, or 2 to 30 milliseconds, or 4 to 20 milliseconds, or 10 to 20 milliseconds.
[0061] In one embodiment, the process utilizes a linear electron beam accelerator. The terpolymer is exposed to electron beam radiation in an ambient air environment. The linear electron beam accelerator operates in an energy range of 4.5 MeV, with a beam power of 150 kW across the entire energy range, a beam energy spread of ±10 percent, and an average current of 30 milliamps (mA).
[0062] The process includes forming a branched terpolymer (i.e., b-terpolymer). The branched terpolymer is interchangeably referred to as an irradiated terpolymer. The branched terpolymer is a branched ethylene / α-olefin / non-conjugated polyene terpolymer. The α-olefin of the branched ethylene / α-olefin / non-conjugated polyene terpolymer is any α-olefin described herein. The non-conjugated polyene of the branched ethylene / α-olefin / non-conjugated polyene terpolymer is any non-conjugated polyene described herein. In one embodiment, the branched terpolymer is a branched ethylene / propylene / ENB terpolymer. As used herein, the term "b-EPDM" refers to a branched ethylene / propylene / ENB terpolymer.
[0063] In one embodiment, the process comprises forming a gel-free branched terpolymer. In a further embodiment, the process comprises forming a gel-free b-EPDM.
[0064] In one embodiment, the branched terpolymer (e.g., b-EPDM) has a Mooney viscosity of 25 MU, or 35 MU, or 45 MU, or 55 MU, or 75 MU, or 95 MU, or 100 MU, or 105 MU, or 110 MU, to 115 MU, or 120 MU, or 122 MU, or 125 MU, or 130 MU, or 135 MU. In a further embodiment, the b-EPDM has a Mooney viscosity of 25 to 135 MU, or 35 to 120 MU, or 45 to 110 MU. The irradiated terpolymer (e.g., b-EPDM) has an increased Mooney viscosity compared to the non-irradiated terpolymer.
[0065] In one embodiment, the branched terpolymer (e.g., b-EPDM) has a Mooney Relaxation Area (MLRA) of 220 MU·s, or 280 MU·s, or 315 MU·s, to 940 MU·s, or 1800 MU·s, or 2300 MU·s. In a further embodiment, the b-EPDM has an MLRA of 220 to 2300 MU·s, or 280 to 1800 MU·s, or 315 to 940 MU·s. The irradiated terpolymer (e.g., b-EPDM) has an increased MLRA compared to a non-irradiated terpolymer (e.g., n-EPDM).
[0066] In one embodiment, the branched terpolymer (e.g., b-EPDM) has an MLRA / ML ratio of 7, 8, 9, or 10 seconds to 12, 13, 15, 20, 24, 26, or 30 seconds. In further embodiments, the b-EPDM has an MLRA / ML value of 7 to 30 seconds, or 7 to 26 seconds, or 10 to 15 seconds. The irradiated terpolymer (e.g., b-EPDM) has an increased MLRA / ML ratio compared to the non-irradiated terpolymer. Without being bound by theory, the MLRA / ML ratio is considered to be the relaxation time related to the degree of melt elasticity of the terpolymer. Long-chain branching (LCB) may slow the relaxation of the terpolymer, increasing the MLRA / ML ratio. The increased MLRA / ML ratio indicates that the irradiated non-terpolymer contains more LCB than the non-irradiated n-EPDM (e.g., n-EPDM).
[0067] In one embodiment, the branched terpolymer (e.g., b-EPDM) has a rheology ratio (RR) of 55, or 60, or 70, or 80, or 90, or 95, or 100, to 105 or 110. In further embodiments, the b-EPDM has an RR of 55 to 110, or 60 to 105, or 70 to 100, or 80 to 95. The irradiated terpolymer (e.g., b-EPDM) has an increased RR value compared to the non-irradiated terpolymer. Without being bound by theory, an increased RR value indicates that the irradiated terpolymer is more shear thinning than the non-irradiated n-EPDM. An increased RR value indicates that the irradiated terpolymer contains more LCB than the non-irradiated n-EPDM.
[0068] In one embodiment, the branched terpolymer (e.g., b-EPDM) has a phase angle δ of 20°, or 22°, or 25°, or 27°, or 29°, to 30°, or 31°, or 32°, or 35°, or 37°, or 39°. In a further embodiment, the b-EPDM has a phase angle δ of 20° to 39°, or 22° to 37°, or 25° to 35°. Without being bound by theory, it is believed that the irradiated terpolymer (e.g., b-EPDM) has a decreased phase angle δ value compared to non-irradiated n-EPDM. The decreased phase angle δ value indicates that the irradiated terpolymer is more elastic than non-irradiated n-EPDM.
[0069] In one embodiment, the branched terpolymer (e.g., b-EPDM) has a density of from 0.85 g / cc or greater, or 0.86 g / cc, to 0.88 g / cc or less, or 0.89 g / cc. In a further embodiment, the b-EPDM has a density of from 0.85 to less than 0.89 g / cc, or from 0.86 to 0.88 g / cc.
[0070] In one embodiment, the branched terpolymer (e.g., b-EPDM) contains vanadium. In one embodiment, the b-EPDM has a vanadium content of from 0 parts per million (ppm) or greater, or 0.1 ppm, to less than 0.7 ppm or 0.82 ppm, or to 0.9 ppm. In further embodiments, the b-EPDM has a vanadium content of 0 to 0.9 ppm, or 0 to less than 0.82 ppm. In one embodiment, the b-EPDM contains vanadium in an amount less than 0.82 ppm.
[0071] In one embodiment, the branched terpolymer (e.g., b-EPDM) contains chlorine. In one embodiment, the b-EPDM has a chlorine content of 0 parts per million (ppm) or greater, or 10 ppm, to 15 ppm or 30 ppm. In a further embodiment, the b-EPDM has a chlorine content of 0 to 30 ppm or 0 to 15 ppm.
[0072] In one embodiment, the branched terpolymer (e.g., b-EPDM) comprises from 54 weight percent (wt%), or 55 wt%, or 60 wt%, or 65 wt%, or 68 wt%, to 72 wt% polymerized ethylene; from 23 wt%, or 25 wt%, or 30 wt%, or 40 wt%, or 50 wt%, or 55 wt% polymerized propylene; and from 0.3 wt%, or 0.5 wt%, or 1 wt%, or 2 wt%, or 3 wt%, or 3.5 wt%, or 4 wt%, or 4.5 wt%, or 4.7 wt%, to 5.1 wt%, or 5.5 wt%, or 6 wt%, or 7 wt%, or 8 wt%, or 8.6 wt% polymerized ENB. In further embodiments, the b-EPDM contains 54-72 wt. %, or 60-68 wt. % polymerized ethylene, 23-55 wt. %, or 25-50 wt. % polymerized propylene, and 0.3-8.6 wt. %, or 0.5-8 wt. % polymerized ENB. The weight percentages are based on the total weight of the b-EPDM. Without being bound by theory, it is believed that the irradiated terpolymer (e.g., b-EPDM) has a negligible reduction in ENB content compared to non-irradiated n-EPDM. The lack of a reduction in ENB content indicates the absence of crosslinking in the irradiated terpolymer.
[0073] In one embodiment, the branched terpolymer (e.g., b-EPDM) has an MWD of from 2.3, or 2.6, or 3.0, or 3.3, to 4.2, or 5.6, or 6. In a further embodiment, the b-EPDM has an MWD of from 2.3 to 6, or from 2.6 to 5.6, or from 3.3 to 4.2.
[0074] In one embodiment, the branched terpolymer (e.g., b-EPDM) has a mass recovery determined by HT GPC testing. In one embodiment, the b-EPDM has a mass recovery of 80% or greater. In further embodiments, the b-EPDM has a mass recovery of 80%, or 85%, or 90%, to 95%, or 96%, or 97%, or 98%, or 99%, or 100%. In other embodiments, the b-EPDM has a mass recovery of 80% to 100%, or 85% to 100%, or 97% to 100%.
[0075] In one embodiment, the process comprises: (1) providing a neat ethylene / propylene / norbornene terpolymer comprising: (i) 50 to 80 weight percent polymerized ethylene; (ii) 23 to 38 weight percent polymerized propylene; and (iii) 0.5 to 9 weight percent polymerized ENB, wherein the weight percentages are based on the total weight of the terpolymer; (2) exposing the neat ethylene / propylene / norbornene terpolymer to electron beam radiation at a radiation dose of 0.3-0.7 MRad; (3) forming a branched ethylene / propylene / norbornene terpolymer, wherein the branched ethylene / propylene / norbornene terpolymer is (A) Mooney viscosity of 35 to 120 MU, or 45 to 110 MU, or 55 to 105 MU; (B) a rheology ratio at 125°C of 55 to 110, or 60 to 105, or 70 to 100; and (C) forming a phase angle δ of 28° to 39°, or 22° to 37°, or 25° to 35°. The process may include two or more embodiments disclosed herein. composition
[0076] The present disclosure provides a composition. In one embodiment, the composition comprises a branched ethylene / propylene / non-conjugated polyene terpolymer. The branched terpolymer has a Mooney viscosity (ML 1+4 at 125°C) of 35 Mooney Units (MU) to 120 MU. The branched terpolymer has a rheology ratio of 55 to 110. The branched terpolymer has a phase angle δ of 20° to 39°.
[0077] In one embodiment, the branched terpolymer is a branched ethylene / propylene / ENB terpolymer (ie, b-EPDM) as previously described herein.
[0078] In one embodiment, the b-EPDM is neat b-EPDM. In a further embodiment, the b-EPDM is neat and gel-free b-EPDM.
[0079] In one embodiment, the composition comprises the branched terpolymer (e.g., b-EPDM) in an amount of from 5 wt%, or 10 wt%, or 15 wt%, to 18 wt%, or 30 wt%, or 50 wt%, based on the total weight of the composition. In further embodiments, the composition comprises the branched terpolymer (e.g., b-EPDM) in an amount of 5-50 wt%, or 10-30 wt%, or 15-18 wt%, based on the total weight of the composition.
[0080] In one embodiment, the composition comprises a neat branched terpolymer (e.g., b-EPDM) having 68 to 72 wt. % polymerized ethylene and 4.7 to 5 wt. % polymerized ENB, wherein the branched terpolymer has the following properties: (i) a Mooney viscosity ML(1+4) at 125°C of 36 to 121 MU, and / or (ii) a rheological ratio (RR) V0.1 / V100 at 125°C of 62 to 102; and / or (iii) a phase angle δ between 31° and 36°, and / or (iv) a Mooney relaxation area (MLRA) of 240 to 1795 MU·s, and / or (v) having one, some, or all of the MLRA / ML ratios between 7 and 15 seconds;
[0081] In one embodiment, the composition comprises a neat branched terpolymer (e.g., b-EPDM) having 69 to 71 wt. % polymerized ethylene and 0.3 to 0.35 wt. % polymerized ENB, wherein the branched terpolymer has the following properties: (i) a Mooney viscosity ML(1+4) at 125°C of 56 to 63 MU, and / or (ii) a rheological ratio (RR) V0.1 / V100 at 125°C of 64 to 87, and / or (iii) a phase angle δ between 31° and 37°, and / or (iv) a Mooney relaxation area (MLRA) of 348–630 MU·s, and / or (v) having one, some, or all of the MLRA / ML ratios between 7 and 10 seconds;
[0082] In one embodiment, the composition comprises a neat branched terpolymer (e.g., b-EPDM) having 54-55 wt. % polymerized ethylene and 8-9 wt. % polymerized ENB, the branched terpolymer having the following properties: (i) a Mooney viscosity ML(1+4) at 125°C of 37 to 103 MU, and / or (ii) a rheological ratio (RR) V0.1 / V100 at 125°C of 57 to 107; and / or (iii) a phase angle δ between 32° and 38°, and / or (iv) a Mooney Relaxation Area (MLRA) of 315 to 2005 MU·s, and / or (v) having one, some, or all of the following MLRA / ML ratios between 8 and 20 seconds;
[0083] In one embodiment, the composition has a vanadium content of from 0 parts per million (ppm) or greater, or 0.1 ppm, to less than 0.7 ppm or 0.82 ppm, or to 0.9 ppm. In a further embodiment, the b-EPDM has a vanadium content of 0 to 0.9 ppm, or 0 to less than 0.82 ppm. In one embodiment, the composition contains vanadium in an amount less than 0.82 ppm.
[0084] In one embodiment, the composition has a chlorine content of from 0 parts per million (ppm) or greater, or 10 ppm, to 15 ppm or 30 ppm. In a further embodiment, the b-EPDM has a chlorine content of 0 to 30 ppm or 0 to 15 ppm. additives
[0085] The composition may optionally include one or more additives.
[0086] In one embodiment, the composition comprises b-EPDM and an oil. The b-EPDM can be any b-EPDM disclosed herein above. The oil can include, but is not limited to, petroleum oils, such as aromatic oils and naphthenic oils; polyalkylbenzene oils; organic acid monoesters, such as alkyl and alkoxyalkyl oleates and stearates; organic acid diesters, such as dialkyl, dialkoxyalkyl, and alkylaryl phthalates, terephthalates, sebacates, adipates, and glutarates; glycol diesters, such as tri-, tetra-, and polyethylene glycol dialkanates; trialkyl trimellitates; trialkyl, trialkoxyalkyl, alkyl diaryl, and triaryl phosphates; chlorinated paraffin oils; coumarone-indene resins; pine tar; vegetable oils, such as castor oil, tall oil, rapeseed oil, and soybean oil, and their esters and epoxidized derivatives; and combinations thereof. In a further embodiment, the oil is selected from the group consisting of SUNPAR 2280, PARALUX 6001, HYDROBRITE 550, and CALSOL 5550.
[0087] In one embodiment, the composition comprises oil in an amount from 5%, or 15%, or 20% to 30%, or 40%, or 70% by weight based on the total weight of the composition, hi further embodiments, the composition comprises oil in an amount from 5-70%, or 15-40%, or 20-30% by weight based on the total weight of the composition.
[0088] The oil may comprise a combination of two or more embodiments described herein.
[0089] In one embodiment, the composition comprises b-EPDM and an additive. The b-EPDM can be any b-EPDM previously disclosed herein. Suitable additives include, but are not limited to, fillers, antioxidants and antiozonants, UV stabilizers, flame retardants, colorants or pigments, curing agents (e.g., sulfur, peroxides), accelerators, coagents, processing aids, blowing agents, plasticizers, and combinations thereof.
[0090] Fillers include, but are not limited to, carbon black; aluminum, magnesium, calcium, sodium, potassium silicates, and mixtures thereof; calcium, magnesium carbonate, and mixtures thereof; silicon oxide, calcium, zinc, iron, titanium, and aluminum; calcium sulfate, barium, lead; polyethylene glycol (PEG); sulfur; stearic acid; sulfonamides; alumina trihydrate; magnesium hydroxide; precipitated silica; fumed silica; natural fibers; synthetic fibers; and combinations thereof.
[0091] Antioxidants and antiozonants include, but are not limited to, hindered phenols, bisphenols, and thiobisphenols; and substituted hydroquinones.
[0092] In one embodiment, the composition comprises b-EPDM and calcium carbonate. In one embodiment, the calcium carbonate is present in an amount of from 5 wt. %, or 15 wt. %, or 20 wt. %, to 30 wt. %, or 40 wt. %, or 70 wt. %, based on the total weight of the composition. In further embodiments, the calcium carbonate is present in an amount of 5-70 wt. %, or 15-40 wt. %, or 20-30 wt. %, based on the total weight of the composition.
[0093] In one embodiment, the composition comprises b-EPDM and carbon black. In one embodiment, the carbon black is present in an amount of from 5 wt%, or 15 wt%, or 20 wt%, to 30 wt%, or 40 wt%, or 70 wt%, based on the total weight of the composition. In further embodiments, the carbon black is present in an amount of 5-70 wt%, or 15-40 wt%, or 20-30 wt%, based on the total weight of the composition.
[0094] In one embodiment, the composition comprises a total additive load excluding calcium carbonate and carbon black. In one embodiment, the total additive load is present in an amount of from 0.5 wt%, or 1 wt%, or 2 wt%, to 4 wt%, or 5 wt%, or 10 wt%, based on the total weight of the composition. In further embodiments, the total additive load is present in an amount of 0.5-10 wt%, or 1-5 wt%, or 2-4 wt%, based on the total weight of the composition.
[0095] The additive may comprise two or more embodiments disclosed herein.
[0096] The total additive loading may include two or more embodiments disclosed herein.
[0097] In one embodiment, the composition comprises the branched terpolymer (e.g., b-EPDM) in an amount of from 5 wt%, or 10 wt%, or 15 wt%, to 18 wt%, or 30 wt%, or 50 wt%, based on the total weight of the composition. In further embodiments, the composition comprises the branched terpolymer (e.g., b-EPDM) in an amount of 5-50 wt%, or 10-30 wt%, or 15-18 wt%, based on the total weight of the composition.
[0098] The composition may comprise two or more embodiments disclosed herein.
[0099] The composition can be used to form articles, non-limiting examples of which include belts, cables, extruder profiles, hoses, moldings, roofing membranes, sponges, tires, weatherstripping, and wire.
[0100] The invention is further illustrated by the following examples, in which all parts and percentages are by weight unless otherwise specified. [Example]
[0101] The raw materials used to formulate the comparative samples ("CS") and inventive examples ("IE") are shown in Table 1 below. [Table 1]
[0102] Comparative samples CS1, CS4, CS9, CS12, CS15, CS18, and CS19 are non-irradiated base neat EPDM and are used as received. Comparative samples CS7 and CS8 are ZN-catalyzed neat EPDM and are used as received. See Table 2.
[0103] Branched EPDM (b-EPDM) is produced by irradiating neat EPDM in air using a DYNAMITRON linear electron beam accelerator for exposure times of 10-20 milliseconds (ms) (Table 2). The operating parameters of the electron beam accelerator are an energy range of 4.5 MeV, a beam power over the full energy range of 150 kW, a beam energy spread of ±10 percent, and an average current of 30 milliamperes (mA).
[0104] Comparative samples CS2 and CS3 are produced by irradiating CS1. Comparative samples CS6, CS11, CS14, and CS17 are produced by irradiating CS4, CS9, CS12, and CS15, respectively.
[0105] Invention examples IE1 and IE2 are produced by irradiating with CS1. Invention examples IE3 and IE4 are produced by irradiating with CS4. Invention examples IE5 and IE6 are produced by irradiating with CS9 and CS12, respectively. Invention examples IE7 and IE8 are produced by irradiating with CS15. Invention examples IE9 and IE10 are produced by irradiating with CS18. Invention examples IE11 and IE12 are produced by irradiating with CS19.
[0106] Table 2 summarizes the results of irradiation on a range of properties for comparative samples and inventive examples. Table 2 includes the vanadium content (V) and chlorine content (Cl) from residual elemental analysis testing. The abbreviation NM indicates that the property was not measured for the indexed sample. [Table 2]
[0107] Table 2 shows that b-EPDM has increased MV values compared to base EPDM. For NORDEL 4760, NORDEL 4770, NORDEL 4785, and NORDEL 6565, the MV increased by 59.5 MU to 81.1 MU (IE4), 69.4 MU to 107.4 MU (IE5), 83.8 MU to 120.4 MU (IE6), and 66 MU to 103 MU (IE12), respectively, after irradiation at a 0.7 MRad dose. The MV values for CS6 (163.1 MU), CS11 (162.2 MU), and CS14 (165.1 MU) were accompanied by evidence of macrogel formation, indicating undesired crosslinking of b-EPDM after irradiation at a 1.5 MRad dose.
[0108] Applicant unexpectedly discovered that irradiating NORDEL 4770 (IE5) at a dose of 0.7 MRad changed the MV from 69.4 MU to 107.4, the RR from 42.5 to 102.2, and the phase angle δ from 48 to 31. Irradiating NORDEL 4785 (IE6) at a dose of 0.7 MRad changed the MV from 83.8 MU to 120.4, the RR from 43.7 to 99.8, and the δ from 50 to 33.
[0109] Table 2 summarizes the electron beam irradiation results for molecular weight distribution (MWD) and mass recovery (M-REC) values. Applicants unexpectedly discovered that irradiating NORDEL 4725 (IE1), NORDEL 4785 (IE6), and NORDEL 3745 (IE7) at a 0.7 MRad exposure dose produced b-EPDM with 100 percent mass recovery. 100% mass recovery indicates the presence of chain branching in the b-EPDM without the presence of crosslinking.
[0110] It is specifically intended that the present disclosure is not limited to the embodiments and examples contained herein, but includes modifications of the embodiments, including portions of the embodiments and combinations of elements of different embodiments that fall within the scope of the following claims. It should be noted that the present invention includes the following aspects. [Aspect 1] A process comprising: providing a neat ethylene / propylene / non-conjugated polyene terpolymer (n-terpolymer) having a Mooney viscosity (ML(1+4) at 125°C) of less than 100 Mooney Units (MU); exposing the n-terpolymer to electron beam radiation at a radiation dose of 0.2 megarads (MRad) to 1.3 MRad; forming a branched ethylene / propylene / non-conjugated polyene terpolymer (b-terpolymer) having a Mooney viscosity ML(1+4) at 125°C of 25 MU to 135 MU. [Aspect 2] the n-terpolymer having a rheology ratio of 20 to 65, and the process 2. The process of embodiment 1, comprising forming a b-terpolymer having a rheology ratio of 55 to 110. [Aspect 3] the n-terpolymer has a phase angle δ of 41° or greater, and the process The process of any of embodiments 1-2, comprising forming a b-terpolymer having a phase angle δ between 20° and 39°. [Aspect 4] The process of any one of embodiments 1-3, comprising forming a b-terpolymer having a mass recovery of 85 percent or greater. [Aspect 5] providing an n-terpolymer comprising 0.5 to 9.0 weight percent norbornene; forming a b-terpolymer comprising 0.3 to 8.6 weight percent norbornene. [Aspect 6] A neat ethylene / propylene / norbornene terpolymer (n-EPDM) is provided, the n-EPDM comprising: (i) 50% to 80% by weight of ethylene; (ii) 23 to 38 weight percent propylene, and (iii) comprising 0.5 to 9.0 weight percent norbornene; exposing the n-EPDM to electron beam radiation at a radiation dose of 0.3 MRad to 0.7 MRad; forming a branched ethylene / propylene / norbornene terpolymer (b-EPDM), the b-EPDM comprising: (A) Mooney viscosity ML(1+4) at 125°C of 35MU to 120MU, (B) rheological ratios between 55 and 110, and (C) forming a nanotube having a phase angle δ between 25° and 39°. [Aspect 7] Aspect 7. The process of any of aspects 1-6, comprising providing n-EPDM, wherein the n-EPDM comprises only one type of non-conjugated polyene, and the non-conjugated polyene does not comprise heteroatoms. [Aspect 8] 1. A composition comprising: a branched ethylene / propylene / non-conjugated polyene terpolymer (b-terpolymer), wherein the b-terpolymer is (A) Mooney viscosity (ML 1+4) at 125°C of 35MU to 120MU; (B) rheological ratios between 55 and 110, and (C) A composition having a phase angle δ of 20° to 39°. [Aspect 9] The composition of embodiment 8, wherein the b-terpolymer is neat. [Aspect 10] 10. The composition of any one of embodiments 8-9, wherein the b-terpolymer has a mass recovery of 80 percent or greater. [Aspect 11] 11. The b-terpolymer of any of embodiments 8-10, comprising less than or equal to 0.82 parts per million (ppm) of vanadium, as measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES). [Aspect 12] (i) 54 to 72 weight percent ethylene; (ii) 23 to 55 weight percent propylene, and (iii) The b-terpolymer of any one of embodiments 8-11, comprising 0.3 to 8.6 weight percent norbornene. [Aspect 13] 13. The b-terpolymer of any one of embodiments 8 to 12, having a density of 0.85 g / cc or greater and less than 0.89 g / cc. [Aspect 14] 14. The b-terpolymer of any one of embodiments 8 to 13, having a chlorine content of from 0 to 30 parts per million (ppm). [Aspect 15] 15. The b-terpolymer of any of aspects 8-14, comprising providing an n-EPDM, wherein the n-EPDM comprises only one type of non-conjugated polyene, and the non-conjugated polyene does not comprise heteroatoms.
Claims
1. A process comprising: providing a neat ethylene / propylene / non-conjugated polyene terpolymer (n-terpolymer) having a Mooney viscosity (ML(1+4) at 125° C.) of less than 100 Mooney Units (MU); exposing the n-terpolymer to electron beam radiation at a radiation dose of 0.2 megarads (MRad) to 1.3 MRad; forming a branched ethylene / propylene / non-conjugated polyene terpolymer (b-terpolymer) having a Mooney viscosity ML(1+4) at 125° C. of 25 MU to 135 MU.
2. the n-terpolymer has a rheology ratio of 20 to 65; the process comprising forming a b-terpolymer having a rheology ratio of 55 to 110; 2. The process of claim 1, wherein the rheological ratio is calculated as the ratio of the complex viscosity at 0.1 rad / sec and 125° C. to the complex viscosity at 100 rad / sec and 125° C.
3. the n-terpolymer has a phase angle δ of 41° or greater; the process comprising forming a b-terpolymer having a phase angle δ of 20° to 39°; 3. The process according to claim 1, wherein the phase angle δ is measured at a complex shear modulus G* of 100 kPa and at 125°C.
4. The process of any of claims 1 to 3, comprising forming a b-terpolymer having a mass recovery of 85 percent or greater.
5. providing an n-terpolymer comprising 0.5 to 9.0 weight percent 5-ethylidene-2-norbornene (ENB); forming a b-terpolymer comprising 0.3 to 8.6 weight percent ENB.
6. A neat ethylene / propylene / ENB terpolymer (n-EPDM) is provided, the n-EPDM comprising: (i) 50% to 80% by weight of ethylene; (ii) 23 to 38 weight percent propylene, and (iii) 0.5 to 9.0 weight percent of 5-ethylidene-2-norbornene (ENB); exposing the n-EPDM to electron beam radiation at a radiation dose of 0.3 MRad to 0.7 MRad; forming a branched ethylene / propylene / ENB terpolymer (b-EPDM), the b-EPDM comprising: (A) Mooney viscosity ML(1+4) at 125° C. from 35 MU to 120 MU; (B) a rheology ratio of 55 to 110, wherein said rheology ratio is calculated as the ratio of the complex viscosity at 0.1 rad / sec and 125° C. to the complex viscosity at 100 rad / sec and 125° C.; and (C) a phase angle δ of 25° to 39°, said phase angle δ being measured at a complex shear modulus G* of 100 kPa and at 125°C; Having, forming The process according to any one of claims 1 to 4, comprising:
7. 7. The process of any one of claims 1 to 6, comprising providing an n-EPDM, said n-EPDM comprising only one non-conjugated polyene, said non-conjugated polyene comprising no heteroatoms.
8. 1. A composition comprising: branched ethylene / propylene / non-conjugated polyene terpolymers (b-terpolymers); The b-terpolymer is (A) Mooney viscosity ML(1+4) at 125° C. from 35 MU to 120 MU; (B) a rheology ratio of 55 to 110, wherein said rheology ratio is calculated as the ratio of the complex viscosity at 0.1 rad / sec and 125° C. to the complex viscosity at 100 rad / sec and 125° C.; and (C) a phase angle δ of 20° to 39°, said phase angle δ being measured at a complex shear modulus G* of 100 kPa and at 125°C; having The b-terpolymer is (i) 68% to 72% by weight of ethylene; (ii) 23 to 30 weight percent propylene, and (iii) A composition comprising 0.3 to 5.1 weight percent 5-ethylidene-2-norbornene (ENB).
9. The composition of claim 8, wherein the b-terpolymer is neat.
10. The composition of any of claims 8 to 9, wherein the b-terpolymer has a mass recovery of 85 percent or greater.
11. The composition of claim 8, wherein the b-terpolymer contains less than 0.82 parts per million (ppm) vanadium as measured by inductively coupled plasma atomic emission spectroscopy (ICP-AES).
12. The composition of claim 8, wherein the b-terpolymer has a density of 0.85 g / cc or more and less than 0.89 g / cc.
13. The composition of claim 8, wherein the b-terpolymer has a chlorine content of from 0 parts per million (ppm) to 30 parts per million (ppm).
Citation Information
Patent Citations
High-melt-strength ethylene polymer, its production and its use
JP1994093033A
Polyolefin-based resin composition and insulated wire and thermally contracting tube using the same
JP1997059392A
Ethylene / α-olefin / non-conjugated polyene-based compositions and foams formed therefrom
JP2015535551A
ETHYLENE / α-OLEFIN / NON-CONJUGATED POLYENE COPOLYMER, PRODUCTION METHOD THEREFOR, AND USE THEREFOR
WO2015122495A1
Resin composition and use of same
WO2016158661A1