Thermally conductive resin sheet, laminated heat dissipation sheet, heat dissipation circuit board and power semiconductor device

A thermally conductive resin sheet with a high-melting-point thermoplastic resin and boron nitride aggregate particles addresses voltage and thermal conductivity issues, ensuring reliability in power semiconductor devices through enhanced moisture absorption and reflow resistance.

JP7581740B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2020163329
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-29
Publication Date
2024-11-13
Estimated Expiration
2040-09-29

AI Technical Summary

Technical Problem

Conventional thermally conductive resin sheets used in power semiconductor devices suffer from insufficient voltage resistance, thermal conductivity, and moisture absorption issues, particularly during reflow processes, leading to potential deformation and reduced reliability.

Method used

A thermally conductive resin sheet composed of a thermoplastic resin with a glass transition temperature or melting point of 300°C or higher, combined with boron nitride aggregate particles having an oil absorption of 0.95 mL/g or more, is used, and a manufacturing method involving mixing and press molding is employed to minimize orientation and enhance thermal conductivity and withstand voltage performance.

Benefits of technology

The resin sheet exhibits improved thermal conductivity, moisture absorption resistance, and reflow resistance, maintaining structural integrity and electrical performance under high temperature and humidity conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581740000003
    Figure 0007581740000003
  • Figure 0007581740000004
    Figure 0007581740000004
  • Figure 0007581740000005
    Figure 0007581740000005
Patent Text Reader

Abstract

To provide a thermally conductive resin sheet with good voltage resistance performance and thermal conductivity and excellent moisture absorption reflow resistance.SOLUTION: A thermally conductive resin sheet according to an aspect of the present invention contains thermoplastic resin and boron nitride agglomerated particles with an oil absorption capacity of 0.95 mL / g or more. A method for manufacturing a thermally conductive resin sheet according to an aspect of the present invention includes a mixing process for obtaining a mixture of a powder comprising thermoplastic resin and boron nitride agglomerated particles having an oil absorption capacity of 0.95 mL / g or more, and a press forming process for pressing the mixture to form a sheet.SELECTED DRAWING: Figure 3
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive resin sheet, a laminated heat dissipation sheet having a configuration in which a heat dissipating metal layer is laminated on the surface of the thermally conductive resin sheet, and a heat dissipation circuit board further having a configuration in which a conductive circuit is formed. [Background technology]

[0002] In recent years, power semiconductor devices used in various fields such as railways, automobiles, industry, and general home appliances are being shifted from conventional Si power semiconductors to power semiconductors using SiC, AlN, GaN, etc. in order to achieve further miniaturization, cost reduction, and efficiency improvement. Power semiconductor devices are generally used as power semiconductor modules in which a plurality of semiconductor devices are arranged on a common heat sink and packaged.

[0003] Various issues have been pointed out for practical use of such power semiconductor devices. One of these issues is the problem of heat generation from the devices. Power semiconductor devices can achieve high output and high density by operating at high temperatures. However, there are concerns that heat generation accompanying device switching may reduce the reliability of power semiconductor devices.

[0004] In recent years, particularly in the electrical and electronics fields, heat generation due to the increasing density of integrated circuits has become a major problem, and how to dissipate the heat has become an urgent issue. One method to solve this problem is to use highly thermally conductive ceramic substrates such as alumina substrates and aluminum nitride substrates as heat dissipation substrates on which power semiconductor devices are mounted. However, ceramic substrates have problems such as being easily cracked by impact, and being difficult to make into thin films and miniaturize.

[0005] Therefore, as an alternative product to the ceramic substrate, a thermally conductive resin sheet containing a resin and an inorganic filler is being considered. Among these, as an inorganic filler, hexagonal boron nitride has attracted attention from the viewpoint of thermal conductivity and the like. However, because hexagonal boron nitride particles are plate-shaped, they have high thermal conductivity in the plane direction (ab-axis direction) but low thermal conductivity in the thickness direction (c-axis direction).When this hexagonal boron nitride is blended with a resin and molded into a sheet, the hexagonal boron nitride tends to be oriented in the flow direction of the resin composition, that is, in the plane direction of the sheet, so the resulting thermally conductive resin sheet has high thermal conductivity in the plane direction but low thermal conductivity in the thickness direction.

[0006] In order to improve the anisotropy of the thermal conductivity of a thermally conductive resin sheet, studies have been conducted on reducing particle orientation by using agglomerated boron nitride particles obtained by agglomerating boron nitride particles. For example, Patent Documents 1 and 2 propose spherical agglomerates obtained by binding boron nitride particles with a binder and then spray-drying them. Moreover, Patent Document 3 proposes hexagonal boron nitride particles in which primary particles of hexagonal boron nitride are aggregated together in a pinecone shape. Furthermore, Patent Document 4 proposes a granulated powder that contains spherical secondary particles formed by agglomerating scaly boron nitride, in which the density of the primary particles in the core portion of the secondary particles is lower than the density of the primary particles in the shell portion. Patent Document 5 proposes boron nitride agglomerated particles in which primary particles of hexagonal boron nitride are agglomerated, and the primary particles in the boron nitride agglomerated particles have a house-of-cards structure. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2006-257392 A [Patent Document 2] Special Publication No. 2008-510878 [Patent Document 3] Japanese Patent Application Publication No. 09-202663 [Patent Document 4] JP 2016-044098 A [Patent Document 5] JP 2015-006985 A Summary of the Invention [Problem to be solved by the invention]

[0008] Conventional thermally conductive resin sheets sometimes lack sufficient voltage resistance and thermal conductivity.

[0009] Moreover, thermally conductive resin sheets for use in power semiconductor devices are required to have resistance to a reflow process. The reflow process is one of the processes for assembling power semiconductor modules. In this reflow process, the temperature of the components is raised rapidly to melt the solder and join the metal components together. In recent years, the operating temperature of power semiconductor devices has increased with the increase in output and density, so the solder used in the reflow process is also required to be heat resistant, and it has become common to use high-temperature solder that requires a reflow temperature of 290°C. Therefore, in the reflow process, the process of raising the temperature to around 290°C at which the high-temperature solder flows and then cooling it is repeated. Furthermore, if the components absorb moisture before the reflow process is performed, deterioration of the components during the reflow process is greatly accelerated, and the voltage resistance performance may be greatly reduced.

[0010] Therefore, an object of the present invention is to provide a thermally conductive resin sheet that has good voltage resistance performance and thermal conductivity, and is excellent in moisture absorption and reflow resistance. In this specification, "moisture absorption reflow resistance" means that even after a moisture absorption reflow test in which a thermally conductive resin sheet is laminated with a metal plate and stored under high temperature and high humidity conditions (e.g., an environment of 85°C and 85% RH for 3 days) and then a reflow test (e.g., 290°C) is performed, the thermally conductive resin sheet has high voltage resistance and does not delaminate at the interface with the metal plate or deform due to foaming. [Means for solving the problem]

[0011] A thermally conductive resin sheet according to one embodiment of the present invention contains a thermoplastic resin and agglomerated particles of boron nitride having an oil absorption of 0.95 mL / g or more. Effect of the Invention

[0012] The thermally conductive resin sheet of the present invention has good voltage resistance and thermal conductivity, and is excellent in moisture absorption and reflow resistance. [Brief description of the drawings]

[0013] [Figure 1] FIG. 2 is a conceptual diagram of a particle cross-section according to an example of a boron nitride agglomerated particle having a low oil absorption amount. [Diagram 2] 1 is a SEM photograph (a photograph substituting a drawing) of a particle surface according to an example of boron nitride agglomerated particles having a low oil absorption amount. [Diagram 3] FIG. 2 is a conceptual diagram of a particle cross-section according to an example of a boron nitride agglomerated particle having a high oil absorption amount. [Figure 4] 1 is a SEM photograph (a photograph substituted for a drawing) of a particle surface according to an example of a boron nitride agglomerated particle having a high oil absorption capacity. [Diagram 5] FIG. 1 is a schematic diagram of a house of cards structure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] An embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below, and various modifications can be made within the scope of the present invention.

[0015] 1.Resin composition The thermally conductive resin sheet of the present invention comprises a resin composition containing a thermoplastic resin and boron nitride agglomerated particles having an oil absorption of 0.95 mL / g or more. Each component will be described in detail below.

[0016] (1)Thermoplastic resin The thermoplastic resin used in the thermally conductive resin sheet of the present invention is preferably resistant to resin flow, plastic deformation, and recovery of thermal restoring strain due to a decrease in elastic modulus even under reflow conditions for a heat dissipating circuit board, for example, under conditions of 290° C. and 5 minutes. To satisfy this requirement, the thermoplastic resin preferably has a glass transition temperature (Tg) of 300° C. or higher or a melting point (Tm) of 300° C. or higher.

[0017] When the thermoplastic resin is a resin composition consisting of a combination of two or more types of thermoplastic resins that are mutually compatible, it is preferable that the glass transition temperature (Tg) of the resin composition is 300°C or higher, or the melting point (Tm) of the resin composition is 300°C or higher. On the other hand, when the thermoplastic resin is a resin composition consisting of a combination of two or more types of thermoplastic resins that are incompatible with each other, it is preferable that the glass transition temperature (Tg) of the thermoplastic resin that is the main component of the resin composition is 300°C or higher, or the melting point (Tm) of the thermoplastic resin that is the main component of the resin composition is 300°C or higher. Here, "main component" refers to the resin that has the highest mass content in the resin composition, and refers to a resin that accounts for 50 mass% or more of the resin composition, particularly 60 mass% or more, particularly 70 mass% or more, particularly 80 mass% or more, particularly 90 mass% or more, and particularly 95 mass% or more (including 100 mass%).

[0018] From the above viewpoints, the thermoplastic resin preferably contains a non-crystalline thermoplastic resin having a glass transition temperature (Tg) of 300° C. or higher and / or a crystalline thermoplastic resin having a melting point (Tm) of 300° C. or higher. Among these, it is preferable that the main component of the thermoplastic resin is a non-crystalline thermoplastic resin having a glass transition temperature (Tg) of 300° C. or higher and / or a crystalline thermoplastic resin having a melting point (Tm) of 300° C. or higher, i.e., that the main component of the thermoplastic resin is 50% by mass or higher of the entire thermoplastic resin, and more preferably 60% by mass or higher, more preferably 70% by mass or higher, more preferably 80% by mass or higher, and even more preferably 90% by mass or higher (including 100% by mass).

[0019] In the present invention, the term "non-crystalline thermoplastic resin" refers to a thermoplastic resin that does not have a melting point, whereas the term "crystalline thermoplastic resin" refers to a thermoplastic resin that has a melting point.

[0020] Examples of heat-resistant amorphous thermoplastic resins available as commercially available raw materials include polycarbonate resin (Tg: 152°C), modified polyphenylene ether resin (Tg: 211°C), polysulfone resin (Tg: 190°C), polyphenylsulfone resin (Tg: 220°C), polyethersulfone resin (Tg: 225°C), polyetherimide resin (Tg: 217°C), and the like. However, none of these commercially available heat-resistant amorphous thermoplastic resins has a glass transition temperature far below 300°C or higher. Thermoplastic polyimide resins with a glass transition temperature of 300° C. or higher are commercially available. However, the moldable temperature of the thermoplastic polyimide resin is very high, and the melt viscosity at the moldable temperature is very high, making it difficult to fill a large amount of thermally conductive filler. Furthermore, since the molecular structure contains an imide group, it is highly hygroscopic, and therefore is not suitable for use as the main component of the thermoplastic resin of the present invention.

[0021] From the above, the thermoplastic resin used in the thermally conductive resin sheet of the present invention is preferably a resin mainly composed of a crystalline thermoplastic resin having a melting point of 300°C or more. By using a crystalline thermoplastic resin having a melting point of 300°C or more as the main component, the moldability is good even when a large amount of thermally conductive filler is filled, and the voids inside the sheet can be sufficiently reduced, resulting in good insulation. In addition, a crystalline thermoplastic resin having a melting point of 300°C or more is less likely to flow, plastically deform, or recover from thermal restoring strain due to a decrease in elastic modulus under reflow conditions, so that the moisture absorption reflow resistance is also good.

[0022] The melting point of the thermoplastic resin can be measured by the method specified in JIS K-7121 "Method of measuring transition temperature of plastics - Determination of melting temperature". Specifically, the thermoplastic resin composition is used as a specimen, and 10 mg of the sample is heated from -40°C to 380°C at a heating rate of 10°C / min, held at 380°C for 1 minute, cooled to -40°C at a cooling rate of 10°C / min, held at the same temperature for 1 minute, and then heated again at 10°C / min to obtain the melting point (Tpm), which is the temperature at the apex of the melting peak. The crystalline thermoplastic resin used in the present invention is one in which at least endothermic peaks due to crystalline melting can be clearly confirmed and the temperature of the apex of the main peak among the peaks is 300°C or higher. In addition, when a resin composition containing added thermally conductive fillers is measured by a differential scanning calorimeter (DSC), there is no significant difference in the melting point, except in cases where the addition of the thermally conductive filler accelerates the deterioration of the matrix resin during hot molding.

[0023] The melting point of the crystalline thermoplastic resin is more preferably 310°C or higher, more preferably 320°C or higher, and even more preferably 330°C or higher, from the viewpoint of moisture absorption reflow resistance at 290°C. On the other hand, the upper limit of the melting point is not particularly limited. From the viewpoint of moldability and productivity, it is more preferably 380°C or lower, more preferably 370°C or lower, and even more preferably 360°C or lower.

[0024] By having the melting point of the thermoplastic resin be 300° C. or higher, the elastic modulus of the resin raw material is unlikely to decrease even at the reflow condition of 290° C. Therefore, the flow deformation of the resin can be suppressed even in the reflow process, and the elastic strain of the resin layer is unlikely to be restored, so that the deterioration of the surface appearance of the thermally conductive resin sheet and the non-uniformity of the thickness of the thermally conductive resin sheet can be suppressed, and a thermally conductive resin sheet with sufficient strength can be obtained. In addition, because the elastic modulus of the resin raw material is unlikely to decrease at 290°C, even if the resin composition absorbs moisture in a humid and hot environment and moisture is present in the resin composition, the moisture in the resin composition is unlikely to expand during the reflow process or the process of mounting on a module, and foaming is unlikely to occur in the thermal conductive resin sheet, resulting in good voltage resistance performance and thermal conductivity.

[0025] It is believed that there is a relationship between the foaming in the thermally conductive resin sheet during the reflow process and the voltage resistance performance and thermal conductivity, for example, as follows. When moisture in the resin composition expands during the reflow process or the process of mounting on a module, foaming may occur inside the thermally conductive resin sheet, near the interface between the heat dissipation metal layer and the thermally conductive resin sheet, or near the interface between the conductive circuit pattern and the thermally conductive resin sheet. For example, when bubbles are generated inside the thermally conductive resin sheet, there is a risk that the voltage resistance performance will be significantly reduced. When a heat dissipating metal material is laminated on one surface of a thermally conductive resin sheet, if foaming occurs near the interface between the heat dissipating metal material and the thermally conductive resin sheet, the heat dissipating metal material may peel off, resulting in a significant decrease in thermal conductivity. Furthermore, if a conductive circuit pattern is formed on the other surface of the thermally conductive resin sheet, if foaming occurs near the interface between the conductive circuit pattern and the thermally conductive resin sheet, the conductive circuit pattern may peel off or fall off, causing abnormalities in the electrical circuit or a significant decrease in the thermal conductivity of the thermally conductive resin sheet.

[0026] Specific examples of heat-resistant crystalline thermoplastic resins include polybutylene terephthalate resin (PBT, melting point: 224°C), polyamide 6 (nylon 6, melting point: 225°C), polyamide 66 (nylon 66, melting point: 265°C), liquid crystal polymer (LCP, melting point: 320°C to 344°C), polyether ketone resin (melting point: 303°C to 400°C), polytetrafluoroethylene resin (PTFE, melting point: 327°C), tetrafluoroethylene-perfluoroalkoxyethylene copolymer resin (PFA, melting point: 302°C to 310°C), tetrafluoroethylene-hexafluoropropylene copolymer resin (FEP, melting point: 250°C to 290°C), and the like.

[0027] As the crystalline thermoplastic resin used in the present invention, liquid crystal polymers, polyether ketone resins, PTFE, and PFA are preferred because they have a melting point of 300° C. or higher. Among these crystalline thermoplastic resins having a melting point of 300° C. or higher, liquid crystal polymers and / or polyether ketone resins are particularly preferred from the viewpoint of moldability, etc. Furthermore, among these, polyether ketone resins are preferred from the viewpoint of adhesion to heat dissipating metal layers such as copper plates.

[0028] The polyether ketone resin that can be used in the present invention is a general term for thermoplastic resins having a repeating unit represented by the following formula (1) (wherein m and n are 1 or 2).

[0029] [ka]

[0030] Examples of polyetherketone resins include polyetherketone (PEK; m=1, n=1, melting point 373°C), polyetheretherketone (PEEK; m=2, n=1, melting point 343°C), polyetherketoneketone (PEKK; m=1, n=2, melting point 303°C to 400°C), polyetheretherketoneketone (PEEKK; m=2, n=2, melting point 358°C), and polyetherketoneetherketoneketone (PEKEKK; copolymer containing both m=1, n=1 structural units and m=1, n=2 structural units, melting point 387°C). All of these are available as commercially available raw materials.

[0031] Among polyether ketone resins, polyether ether ketone (PEEK) can be particularly preferably used, taking into consideration a variety of factors, including that it has a sufficiently high melting point and a relatively low molding processing temperature, allowing the molding cycle to be shortened, that it has a continuous heat resistance temperature of 200°C or higher, demonstrating that it can be used in heat-resistant applications without any problems, that various grades are available in terms of melt viscosity related to molding processability, that it has the most chemically stable structure among polyether ketone resins and is also excellent in hot water resistance and chemical resistance, and that its price has become reasonable due to its use in a wide range of applications.

[0032] When polyether ether ketone (PEEK) is used as the crystalline thermoplastic resin in the present invention, it may be blended with other thermoplastic resins. The type of the other thermoplastic resin is not particularly limited. Among them, the other thermoplastic resin is preferably a compatible resin that has the effect of compensating for the performance that is insufficient when only polyether ether ketone is used for the application of the present invention.

[0033] As the compatible resin, polyetherimide (PEI) is more preferable. Combining PEEK with PEI not only makes it possible to adjust the crystallinity (heat of crystalline fusion) of PEEK, but also, by adjusting the crystallization rate of PEEK, it is possible to increase the glass transition temperature when the resin composition is in an amorphous state (Tg of PEEK is 143°C, while Tg of PEI is 217°C). Since PEI is an amorphous resin, the melting point of the resin itself does not change even when PEEK and PEI are combined. In addition, in the present invention, by using PEI which has an imide group and is amorphous, it is possible to improve the adhesion to heat dissipating metal materials such as copper plates.

[0034] The amount of PEI added is preferably 50% by mass or less, with the total amount of the resin composition being 100% by mass. By adding 50% by mass or less of PEI, the heat resistance in a moisture absorption reflow test can be maintained by the crystallinity of PEEK, while the adhesion to heat dissipating metal materials can be improved.

[0035] Various commercially available PEEK products can be used, such as "KetaSpire (registered trademark)" manufactured by Solvay, "Vestakeep (registered trademark)" manufactured by Daicel-Evonik, and "Victrex PEEK" manufactured by Victrex, which are available with various melt viscosities from various companies. These PEEK raw materials may be used in the form of a single grade, or in the form of a blend of multiple grades having different melt viscosities, etc.

[0036] The melt viscosity of the crystalline thermoplastic resin in the present invention is not particularly limited. In particular, since a relatively large amount of thermally conductive filler is blended, in order to facilitate hot molding, the melt viscosity of the crystalline thermoplastic resin is preferably 0.60 kPa·s or less, and more preferably 0.30 kPa·s or less. When the melt viscosity is within the above range, there is no need to set the temperature of the molding machine excessively high, and deterioration of the raw material can be suppressed. On the other hand, the lower limit of the melt viscosity is not particularly limited. In particular, 0.01 kPa·s or more is preferable. The melt viscosity is based on ASTM D3835 and is measured at a shear rate of 1000 s -1 These values ​​were measured at a temperature of 400°C.

[0037] From the viewpoint of long-term durability in a heated environment, the mass average molecular weight (Mw) of the crystalline thermoplastic resin is preferably 48,000 or more, more preferably 49,000 or more, and even more preferably 50,000 or more. On the other hand, from the viewpoint of moldability, it is preferably 120,000 or less, more preferably 110,000 or less, and even more preferably 100,000 or less.

[0038] The MFR of the crystalline thermoplastic resin is preferably 8 g / 10 min or more, more preferably 9 g / 10 min or more, and even more preferably 10 g / 10 min or more, from the viewpoint of moldability and the difficulty of forming voids between the resin and the added thermally conductive filler. On the other hand, from the viewpoint of long-term durability in a heated environment, the MFR is preferably 180 g / 10 min or less, more preferably 170 g / 10 min or less, and even more preferably 160 g / 10 min or less. The MFR is a value measured at 380°C and 5kgf in accordance with JIS K7210 (2014).

[0039] (2) Boron nitride agglomerated particles From the viewpoint of increasing thermal conductivity, the boron nitride agglomerated particles of the present invention preferably have an oil absorption of 0.95 mL / g or more, and more preferably 1.0 mL / g or more. In the present invention, the oil absorption can be measured in accordance with JIS K5101-13-1:2004 ("Testing methods for pigments" - Part 13: Oil absorption - Section 1: Refined linseed oil method).

[0040] The oil absorption amount of the boron nitride agglomerated particles and the thermal conductivity in the thickness direction of the thermal conductive resin sheet are thought to have a relationship, for example, as follows. The oil absorption of boron nitride agglomerated particles represents the amount of resin that penetrates into the agglomerated particles, and is also correlated with the surface condition of the agglomerated particles. For example, a low oil absorption of an agglomerated particle indicates that there are few voids inside and that the surface is less uneven. As shown in Figures 1 and 2, an agglomerated particle with less surface unevenness has a structure in which the thickness direction (c-axis direction) of the primary particles near the outermost surface of the agglomerated particle coincides with the radial direction of the agglomerated particle. While such agglomerated particles have the advantage of providing good coatability when a thermally conductive resin sheet is produced by a wet coating method, the primary particles near the outermost surface lie flat so as to cover the agglomerated particles, which may increase the thermal resistance at the interface between the agglomerated particle surface and the resin, or at the contact interface between a plurality of agglomerated particles. In addition, when multiple aggregated particles are packed so as to come into contact with each other in a thermally conductive resin sheet, the aggregated particles having the above structure conduct heat to each other at the surface portions of the aggregated particles via the thickness direction (c-axis direction) of the primary particles. Since the thermal conductivity of the primary particles is low in the thickness direction, there is a limit to the thermal conductivity of the thermally conductive resin sheet in the thickness direction. On the other hand, if the oil absorption of the agglomerated particles is large, it means that the gaps between the particles tend to be large if the internal voids are the same, and if the particle size distribution is the same, it means that the surface is uneven. As shown in Figures 3 and 4, an agglomerated particle with a large surface unevenness has a structure in which the plane direction (ab axis direction) of the primary particles near the outermost surface of the agglomerated particle coincides with the radial direction of the agglomerated particle. When such agglomerated particles are filled so that multiple agglomerated particles contact each other in a thermal conductive resin sheet, the contact area between the particles is increased compared to agglomerated particles in which the primary particles near the outermost surface lie so as to cover the agglomerated particles. Therefore, the thermal resistance between the particles is reduced, and the thermal conductivity in the thickness direction of the thermal conductive resin sheet is increased.

[0041] Boron nitride agglomerated particles having an oil absorption of 0.95 mL / g or more can be achieved, for example, by using agglomerated particles having a house-of-cards structure as described below. After obtaining boron nitride agglomerated particles by a known method, the oil absorption may be increased by subjecting the particles to a physical or chemical surface roughening treatment. The boron nitride agglomerated particles sold by various companies use primary particles of boron nitride that are relatively well crystallized during granulation, and as a result, the stable faces (ab faces) of the primary particles tend to stack together, resulting in a "cabbage structure" in which the thickness direction of the primary particles near the outermost surface of the agglomerated particles coincides with the radial direction of the agglomerated particles. Agglomerated particles with a "cabbage structure" have primary particles near the outermost surface that lie flat so as to cover the agglomerated particles, making it difficult to achieve an oil absorption of 0.95 mL / g or more.

[0042] The oil absorption of the boron nitride agglomerated particles of the present invention is preferably less than 2.0 mL / g, more preferably 1.9 mL / g or less, and even more preferably 1.8 mL / g or less. When the oil absorption is less than 2.0 mL / g, the mechanical strength of the boron nitride agglomerated particles is sufficiently maintained, resulting in good moldability. In addition, air bubbles in the thermal conductive resin sheet are easily removed during the molding process, resulting in better voltage resistance and thermal conductivity.

[0043] The boron nitride agglomerated particles of the present invention preferably have a spherical shape. "Spherical" generally means that the aspect ratio (ratio of major axis to minor axis) is 1 or more and 2 or less, preferably 1 or more and 1.75 or less, more preferably 1 or more and 1.5 or less, and even more preferably 1 or more and 1.4 or less. The aspect ratio can be determined by randomly selecting 200 or more particles from an image of the cross section of a thermally conductive resin sheet taken with a scanning electron microscope (SEM), determining the ratio of the long axis to the short axis of each particle, and calculating the average value.

[0044] From the viewpoint of improving thermal conductivity, the aggregated structure of the boron nitride aggregated particles is preferably a card house structure. The aggregate structure of the boron nitride aggregated particles can be confirmed by a scanning electron microscope (SEM).

[0045] The house of cards structure is a structure in which plate-shaped particles are stacked in a complex manner without being oriented, as described in "Ceramics 43 No. 2" (published by the Ceramic Society of Japan in 2008). More specifically, it is a structure in which the flat surface of the primary particles that form the aggregate particle is in contact with the end surface of other primary particles that exist within the aggregate particle. A schematic diagram of the house of cards structure is shown in Figure 5. The card-house structured aggregated particles have a very high breaking strength due to their structure, and do not break even during the pressurizing process performed during the molding of the thermally conductive resin sheet. Therefore, the primary particles that are usually oriented in the longitudinal direction of the thermally conductive resin sheet can be made to exist in a random direction. Therefore, by using the card-house structured aggregated particles, the proportion of the primary particles that have the ab plane oriented in the thickness direction of the thermally conductive resin sheet can be increased, so that heat can be effectively conducted in the thickness direction of the sheet, and the thermal conductivity in the thickness direction can be further increased.

[0046] The boron nitride agglomerated particles having a house-of-cards structure can be produced, for example, by the method described in International Publication No. 2015 / 119198. It is preferable that the boron nitride agglomerated particles of the present invention are not subjected to a treatment that applies force to the surface of a ball mill or the like.

[0047] When using boron nitride agglomerated particles having a house-of-card structure, the particles may be surface-treated with a surface treatment agent. The surface treatment agent may be a known surface treatment agent such as a silane coupling treatment. In general, direct affinity or adhesion is not observed between the thermally conductive filler and the thermoplastic resin, and this is also true when boron nitride agglomerated particles having a card house structure are used as the thermally conductive filler. It is believed that the attenuation of thermal conductivity at the interface can be further reduced by increasing the adhesion at the interface between the thermally conductive filler and the matrix resin by chemical treatment.

[0048] By using agglomerated particles of boron nitride as the thermally conductive filler of the present invention, the particle size can be made larger than that of a thermally conductive filler that uses primary particles as they are. By increasing the particle size of the thermally conductive filler, the number of heat transfer paths between the thermally conductive fillers passing through the thermoplastic resin with low thermal conductivity can be reduced, and therefore the increase in thermal resistance in the heat transfer paths in the thickness direction can be reduced.

[0049] From the above viewpoints, the lower limit of the maximum particle diameter Dmax on a volume basis (hereinafter also referred to as "maximum particle diameter") of the boron nitride agglomerated particles is preferably 20 μm or more, more preferably 30 μm or more, and even more preferably 50 μm or more. On the other hand, the upper limit of the maximum particle diameter Dmax is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and even more preferably 90 μm or less.

[0050] The lower limit of the volume-based average particle diameter D50 of the boron nitride agglomerated particles is preferably 2 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and still more preferably 20 μm or more. On the other hand, the upper limit of the average particle diameter D50 is preferably 300 μm or less, more preferably 200 μm or less, even more preferably 100 μm or less, and still more preferably 80 μm or less.

[0051] By having the maximum particle size of the boron nitride agglomerated particles be equal to or less than the above upper limit, when the boron nitride agglomerated particles are contained in a matrix resin, the interface between the matrix resin and the boron nitride agglomerated particles is reduced, resulting in lower thermal resistance, high thermal conductivity being achieved, and a good quality film free of surface roughness, etc. By having the maximum particle size be equal to or more than the above lower limit, a sufficient thermal conductivity improving effect as a thermally conductive filler required for power semiconductor devices can be obtained.

[0052] It is also considered that the effect of the thermal resistance at the interface between the matrix resin and the boron nitride agglomerated particles on the thickness of the thermal conductive resin sheet becomes significant when the size of the boron nitride agglomerated particles is 1 / 10 or less of the thickness of the thermal conductive resin sheet. In particular, in the case of power semiconductor devices, thermal conductive resin sheets with thicknesses of 100 μm to 300 μm are often used, so from the viewpoint of thermal conductivity as well, it is preferable that the volume-based maximum particle size Dmax of the boron nitride agglomerated particles be larger than the above lower limit. Furthermore, by having the maximum particle diameter Dmax of the boron nitride agglomerated particles be equal to or greater than the above lower limit, not only is the increase in thermal resistance caused by the interface between the boron nitride agglomerated particles and the matrix resin suppressed, but the number of required thermal conduction paths between particles is reduced, increasing the probability that they will be connected from one side to the other in the thickness direction of the thermal conductive resin sheet. Furthermore, by having the maximum particle diameter Dmax of the boron nitride agglomerated particles be equal to or greater than the above lower limit, the interfacial area between the matrix resin and the boron nitride agglomerated particles is smaller than when the same mass of particles having a Dmax smaller than the above lower limit is used. This makes it possible to reduce the occurrence of voids that tend to occur at the interface between the matrix resin and the boron nitride agglomerated particles in the thermal conductive resin sheet, making it easier to obtain excellent voltage resistance characteristics. On the other hand, by having the volume-based maximum particle diameter Dmax of the boron nitride agglomerated particles be equal to or less than the above upper limit, protrusion of the boron nitride agglomerated particles onto the surface of the thermal conductive resin sheet is suppressed, and a good surface shape without surface roughness can be obtained. Therefore, when a sheet is produced by bonding it to a copper substrate, sufficient adhesion can be obtained and excellent voltage resistance characteristics can be obtained.

[0053] The ratio (Dmax / thickness) of the size (Dmax) of the boron nitride agglomerated particles to the thickness of the thermally conductive resin sheet is preferably 0.3 or more and 1.0 or less, more preferably 0.35 or more or 0.95 or less, and even more preferably 0.4 or more or 0.9 or less.

[0054] The maximum particle size Dmax and the average particle size D50 of the boron nitride agglomerated particles can be measured, for example, by the following method. For a sample in which boron nitride agglomerated particles are dispersed in a solvent, specifically, for a sample in which boron nitride agglomerated particles are dispersed in a pure water medium containing sodium hexametaphosphate as a dispersion stabilizer, the particle size distribution is measured using a laser diffraction / scattering particle size distribution analyzer LA-920 (manufactured by Horiba, Ltd.), and the maximum particle diameter Dmax and average particle diameter D50 of the boron nitride agglomerated particles can be obtained from the obtained particle size distribution. The maximum particle size and the average particle size can also be determined using a dry particle size distribution measuring device such as Morphologi G3 (manufactured by Malvern Instruments). The maximum particle size Dmax and average particle size D50 of the boron nitride agglomerated particles added to the thermoplastic resin can also be measured in a similar manner to that described above by dissolving and removing the thermoplastic resin in a solvent (including a heated solvent), or by swelling the thermoplastic resin to reduce the adhesive strength with the boron nitride agglomerated particles and then physically removing it, and further by heating the resin component in the atmosphere to incinerate it and remove it.

[0055] (3) Content of each ingredient The lower limit of the thermoplastic resin content in 100% by mass of the resin composition of the present invention is preferably 15% by mass or more, more preferably 20% by mass or more, while the upper limit of the thermoplastic resin content is preferably 40% by mass or less, more preferably 35% by mass or less. The lower limit of the content of the boron nitride agglomerated particles in 100% by mass of the resin composition of the present invention is preferably 60% by mass or more, more preferably 65% ​​by mass or more, while the upper limit of the content of the thermally conductive filler is preferably 85% by mass or less, more preferably 80% by mass or less. When the content of the boron nitride agglomerated particles is equal to or greater than the above lower limit, the effect of improving thermal conductivity and the effect of controlling the linear expansion coefficient due to the boron nitride agglomerated particles are satisfactorily exhibited, whereas when the content of the boron nitride agglomerated particles is equal to or less than the above upper limit, the moldability of the resin composition and the interfacial adhesion with different materials are improved.

[0056] In general, the compounding ratio of a thermally conductive resin composition is often specified by the volume fraction of the matrix resin and the boron nitride agglomerated particles (hence, the area ratio in the cross section of the thermally conductive resin sheet). The thermal conductivity in the thickness direction of the thermally conductive resin sheet is not determined only by the volume fraction, but is affected by various factors such as the above-mentioned preferred particle size, particle orientation state, and particle shape, so in the present invention, the mass fraction is used for convenience in practical compounding. In particular, when using boron nitride agglomerated particles with a house-of-cards structure, the internal structure of the particle exhibits a house-of-cards structure, and a large number of flat-shaped boron nitride primary particles oriented in the radial direction are formed on the particle surface in a protruding state, which is called a burr shape or a confetti shape, and the protrusions of adjacent house-of-cards structure particles come into physical contact with each other, forming a heat transfer path with low thermal resistance in the thickness direction. Therefore, it may not be easy to determine the volume fractions of the matrix resin and the boron nitride agglomerated particles by observation with a normal scanning electron microscope (SEM). Furthermore, when the amount of boron nitride agglomerated particles with a house-of-cards structure added is increased, the pressure applied during the hot press molding of the resin composition causes the particles to deform at the contact points, rather than contacting each other as spherical particles, and the contact points are observed to be in linear, i.e., planar, contact. When such a contact state is reached, the addition of boron nitride with a house-of-cards structure enables the formation of an efficient heat transfer path. However, even in such a case, it is not easy to determine the respective volume fractions of the matrix resin and the boron nitride agglomerated particles by SEM observation.

[0057] The resin composition of the present invention may contain other components in addition to the thermoplastic resin and the boron nitride agglomerated particles, although from the viewpoint of increasing thermal conductivity, it is preferable that the resin composition does not contain other components. Other components include various antioxidants such as phosphorus-based and phenol-based, phenol acrylate-based and other process stabilizers, heat stabilizers, hindered amine radical scavengers (HAAS), impact modifiers, processing aids, metal deactivators, copper inhibitors, antistatic agents, flame retardants, additives such as silane coupling agents that improve the affinity at the interface between the boron nitride agglomerated particles and thermoplastic resins, additives such as silane coupling agents that can be expected to increase the adhesive strength between the resin sheet and metal plate-like material, extenders, etc. When these additives are used, the amount added may be within the range of the amount usually used for these purposes.

[0058] 2.Thermal conductive resin sheet The thermally conductive resin sheet of the present invention is made of the above-mentioned resin composition and has the characteristics of excellent moisture absorption reflow resistance and being less susceptible to interfacial peeling due to thermal expansion and contraction when laminated with a metal plate.

[0059] The thermal conductivity of the thermal conductive resin sheet in the thickness direction at 25° C. is preferably 15 W / m K or more, more preferably 17 W / m K or more, and even more preferably 19 W / m K or more. When the thermal conductivity in the thickness direction is equal to or more than the above lower limit, the sheet can be suitably used in power semiconductor devices that operate at high temperatures. The thermal conductivity can be adjusted by the type of thermoplastic resin, its physical properties such as melt viscosity, the structure of the boron nitride agglomerated particles, its oil absorption and content, the method of mixing the thermoplastic resin with the boron nitride agglomerated particles, the conditions in the heating and kneading step described below, and the like.

[0060] The thermal conductivity can be measured by the following method. First, the thermal diffusivity a (mm 2 Since there are no JIS standards for thermal diffusivity and thermal conductivity of resin-based materials, measurements are made in accordance with JIS R1611-2010 (Method of measurement of thermal diffusivity, specific heat capacity, and thermal conductivity of fine ceramics by the flash method). In addition, since JIS R1611-2010 specifies that "the thickness of the sample should be 0.5 mm or more and 5 mm or less," the thickness of the resin sheet should be adjusted to 0.5 mm or more before measurement. If the thickness of the resin sheet is less than 0.5 mm, multiple sheets may be stacked to adjust the total thickness to 0.5 mm or more before measurement. Next, the density ρ (g / m) of the resin sheet was measured using the Archimedes method in accordance with JIS K6268. 3 ) is required. Furthermore, in accordance with JIS K7123, the specific heat capacity c (J / (g·K)) at 25°C is measured using a DSC measuring device. From these measured values, the thermal conductivity in the sheet thickness direction at 25° C. can be calculated as "H=a×ρ×c".

[0061] The lower limit of the thickness of the thermally conductive resin sheet is preferably 50 μm or more, more preferably 60 μm or more, and even more preferably 70 μm or more, while the upper limit of the thickness is preferably 300 μm or less, more preferably 200 μm or less, and even more preferably 160 μm or less. By making the thickness of the thermally conductive resin sheet 50 μm or more, sufficient voltage resistance characteristics can be ensured. On the other hand, by making the thickness 300 μm or less, it is possible to achieve a smaller and thinner device, particularly when the thermally conductive resin sheet is used in a power semiconductor device, and the thinning of the film can reduce the thermal resistance in the thickness direction, compared to insulating thermally conductive layers made of ceramic materials.

[0062] In the thermally conductive resin sheet of the present invention, in order to reduce the anisotropy of thermal conductivity and increase the thermal conductivity in the thickness direction, it is preferable to reduce the orientation of the primary particles of the boron nitride agglomerated particles. The orientation of the primary particles can be evaluated by measuring the thermally conductive resin sheet by X-ray diffraction and calculating the ratio I(002) / I(100), where I(002) is the diffraction peak intensity of the (002) plane and I(100) is the diffraction peak intensity of the (100) plane. The ratio "I(002) / I(100)" is preferably 20 or less, more preferably 17 or less, and even more preferably 15 or less. If the ratio exceeds 20, the boron nitride agglomerated particles collapse in the melt-kneading step or are excessively crushed in the pressing step, resulting in a large number of primary particles that are parallel to the surface direction of the thermal conductive resin sheet or form a small angle with the surface direction. In this case, even if the content of boron nitride agglomerated particles is increased, it is difficult to increase the thermal conductivity in the thickness direction. The lower limit of the ratio "I(002) / I(100)" is not particularly limited. For example, when using boron nitride agglomerated particles having a house-of-cards structure, the ratio "I(002) / I(100)" of the particles alone is about 4.5 to 6.6, so 4.5 is considered to be the lower limit, except when intentional orientation is performed.

[0063] 3. Manufacturing method of thermally conductive resin sheet An example of the method for producing the thermally conductive resin sheet of the present invention will now be described. An example of the method for producing the thermally conductive resin sheet of the present invention includes a method including a mixing step and a press molding step.

[0064] A conventional manufacturing method is to obtain a thermally conductive resin film by applying a slurry in which a matrix resin and a thermally conductive filler are dispersed in a solvent to a substrate (wet coating method). However, air bubbles may be included during coating on the substrate, or if the solvent is not dried sufficiently, foaming may occur due to the residual solvent in the coating film, which may result in a decrease in voltage resistance. In particular, when using boron nitride agglomerated particles with a large oil absorption, the slurry is likely to thicken due to the many irregularities on the agglomerated particle surface, and air bubbles are more likely to be included during kneading with the resin or coating on the substrate, which means that air bubbles are likely to remain in the resin film, which may result in a decrease in voltage resistance. In addition, in the above-mentioned wet coating method, when the amount of the thermally conductive filler added is increased in order to increase the thermal conductivity, streaks may occur during coating, resulting in poor productivity. These streaks are particularly likely to occur when boron nitride agglomerated particles, which have a high oil absorption, are used.

[0065] In the manufacturing method of the present invention, the thermoplastic resin is pressed into the voids in the boron nitride agglomerated particles by forming the sheet at a temperature at which the thermoplastic resin exhibits fluidity, so that the sheet is less likely to contain air bubbles. In addition, since the sheet can be obtained without using a solvent in the present invention, there is no foaming caused by residual solvent. Therefore, the manufacturing method of the present invention can improve the voltage resistance performance of the thermal conductive resin sheet. Furthermore, since the manufacturing method of the present invention does not involve a coating step, no streaks are generated even when agglomerated particles of boron nitride having a high oil absorption are used, and productivity is good.

[0066] As described in the examples of Patent Documents 4 and 5, it was common to use a thermosetting resin as a matrix resin in the past, and therefore wet coating methods were often used to manufacture thermally conductive resin sheets. In this wet coating method, if the aggregated particle surface is uneven, the above-mentioned problems often occur, so it is considered preferable to use aggregated particles with as little unevenness on the aggregated particle surface as possible, i.e., aggregated particles with a small oil absorption. On the other hand, from the viewpoint of thermal conductivity, it is preferable that the agglomerated particle surface has many projections and recesses in order to increase the contact area between the particles, that is, the agglomerated particles have a large oil absorption. As described above, when the conventional manufacturing method is used, there is a trade-off between the improvement of voltage resistance and productivity and the improvement of thermal conductivity in terms of oil absorption. According to the manufacturing method of the present invention, agglomerated particles with a large oil absorption can be used without having to consider the problems associated with wet coating methods, and therefore it is possible to improve the voltage resistance and productivity while also increasing thermal conductivity.

[0067] (1)Mixing process In the mixing step, powder made of a thermoplastic resin and boron nitride agglomerated particles having an oil absorption of 0.95 mL / g or more are stirred and mixed at room temperature. A conventional manufacturing method involves heating, melting and kneading a matrix resin and a thermally conductive filler. However, this melting and kneading can cause shear fracture of the thermally conductive filler. In particular, when using boron nitride agglomerated particles with a high oil absorption, shear fracture is likely to occur because of the many irregularities on the surface. Therefore, in the present invention, instead of performing heating, melting and kneading, powder made of a thermoplastic resin and boron nitride agglomerated particles having an oil absorption of 0.95 mL / g or more are stirred and mixed at room temperature, making it possible to reduce the occurrence of shear fracture and increase the thermal conductivity of the resulting sheet.

[0068] (2) Press molding process In the press molding step, the mixture obtained in the mixing step is pressed to be formed into a sheet.

[0069] As the press molding method, various known press machines for molding thermoplastic resins can be used. From the viewpoint of preventing deterioration of the resin during the hot pressing, it is particularly preferable to use a vacuum press capable of reducing the amount of oxygen in the press during heating, or a press equipped with a nitrogen replacement device.

[0070] In the press molding process, it is preferable to set the pressurizing pressure not only for the purpose of forming the molten kneaded material into a sheet body of uniform thickness, but also for the purpose of bonding the added thermally conductive filler particles together to form a heat path, and for the purpose of eliminating voids and gaps in the sheet. From this viewpoint, the pressure in the press molding step, as the actual pressure applied to the sample, is usually 8 MPa or more, preferably 9 MPa or more, more preferably 10 MPa or more, and is preferably 50 MPa or less, more preferably 40 MPa or less, and further preferably 30 MPa or less. By setting the pressure during pressing to the upper limit or less, it is possible to prevent the thermally conductive filler from being crushed, and a thermally conductive resin sheet having high thermal conductivity can be obtained. Also, by setting the pressing pressure to the lower limit or more, contact between the thermally conductive filler particles is improved, making it easier to form a thermally conductive path, and a sheet having high thermal conductivity can be obtained. In addition, since the voids in the resin sheet can be reduced, a thermally conductive resin sheet having a high breakdown voltage can be obtained even after a moisture absorption reflow test.

[0071] The temperature of the press machine in the press molding process is preferably set to a temperature at which the thermoplastic resin exhibits fluidity, for example, the melting point of the thermoplastic resin as the main component + 30° C. For example, when a polyether ketone resin is used as the main component, the temperature of the press machine is preferably set to 370° C. to 440° C., and more preferably 380° C. or higher or 420° C. or lower. By performing press molding at this temperature range, the obtained thermally conductive resin sheet can be given good thickness uniformity and high thermal conductivity due to good contact between the added boron nitride agglomerated particles. If the molding temperature is 370°C or higher, the resin viscosity is reduced to a level sufficient for shaping processing, and the molded thermally conductive resin sheet can be given sufficient thickness uniformity. On the other hand, if the set temperature of the press machine is 440°C or lower, deterioration of the resin itself and deterioration of the physical properties of the molded thermally conductive resin sheet can be suppressed.

[0072] The pressurization time is usually 30 seconds or more, preferably 1 minute or more, more preferably 3 minutes or more, and even more preferably 5 minutes or more, and is preferably 1 hour or less, more preferably 30 minutes or less, and even more preferably 15 minutes or less. By being equal to or less than the upper limit, the manufacturing process time of the thermally conductive resin sheet can be reduced, and the cycle time can be shortened compared to a thermally conductive resin sheet using a heat-resistant thermosetting resin, which tends to reduce production costs. Also, by being equal to or more than the lower limit, the thermally conductive resin sheet can have a sufficiently uniform thickness, and internal gaps and voids can be sufficiently removed, preventing unevenness in thermal conductivity performance and voltage resistance characteristics.

[0073] 4.Laminated heat dissipation sheet The laminated heat dissipation sheet of the present invention is obtained by laminating a heat dissipation metal layer containing a heat dissipation material on one surface of the above-mentioned thermally conductive resin sheet of the present invention. The heat dissipating material is not particularly limited as long as it is made of a material having good thermal conductivity. In particular, in order to increase the thermal conductivity in the laminated structure, it is preferable to use a heat dissipating metal material, and more preferably to use a flat metal material. The type of metal material is not particularly limited, but among them, a copper plate, an aluminum plate, an aluminum alloy plate, etc. are preferable because they have good thermal conductivity and are relatively inexpensive.

[0074] When a flat metal material is used as the heat dissipating metal material in the laminated heat dissipation sheet, the thickness of the metal material is preferably 0.03 to 6 mm, and more preferably 0.1 mm or more or 5 mm or less, in order to ensure sufficient heat dissipation.

[0075] Regarding adhesion to heat-dissipating metal materials, the surface of the metal material on the side to be laminated with the thermally conductive resin sheet may be subjected to surface treatments such as soft etching, burnt plating, oxidation-reduction treatment, etc., surface roughening treatments, plating treatments with various metals and metal alloys to ensure adhesion durability, organic surface treatments including silane coupling treatments such as amino-based and mercapto-based, and surface treatments with organic-inorganic composite materials, etc. By carrying out these surface treatments, it is possible to further improve the initial adhesive strength, the durability of the adhesive strength, and the effect of suppressing interfacial peeling after a moisture absorption reflow test.

[0076] On the other hand, the side of the heat dissipating metal material opposite to the side laminated with the thermally conductive resin sheet does not have to be a simple flat plate, and may be subjected to processing such as increasing the surface area in order to ensure a contact area with the cooling medium, which may be a gas or liquid. Examples of processing for increasing the surface area include increasing the surface area by roughening the surface with blasting processing, etc., directly forming V-shaped or rectangular grooves or various shapes of unevenness on the heat dissipating metal material by cutting or pressing, joining another metal material that has been further processed to increase the surface area to the heat dissipating metal layer made of a flat metal material by casting processing, diffusion bonding, bolt fastening, soldering, brazing, etc., or embedding a metal pin, etc. Furthermore, it is also possible to directly press-laminated a thermally conductive resin sheet onto a heat dissipating metal layer having a cavity for passing a cooling medium. However, since the pressing pressure between the thermally conductive resin sheet and the heat dissipating metal plate is relatively high, in these cases, it is preferable to integrate the laminated and integrated flat metal material and the thermally conductive resin sheet with a grooved metal plate or a metal layer having a cavity for passing a refrigerant in a later process by soldering, brazing, bolt fastening, etc.

[0077] Regarding the lamination and integration of the heat dissipating metal material and the thermally conductive resin sheet in the laminated heat dissipation sheet, press molding, which is a batch process, can be preferably used. In this case, the press equipment and press conditions are the same as the range of press molding conditions for obtaining the above-mentioned thermally conductive resin sheet.

[0078] 5. Heat dissipation circuit board The heat dissipating circuit board of the present invention has the above-mentioned laminated heat dissipation sheet, that is, has a configuration in which the above-mentioned heat dissipating metal layer is laminated on one surface of the thermally conductive resin sheet of the present invention, and a circuit board is formed on the surface of the thermally conductive resin sheet other than the heat dissipating metal layer by, for example, etching treatment or the like.

[0079] The heat dissipating circuit board is preferably configured as an integrated structure of "heat dissipating metal layer / thermally conductive resin sheet / conductive circuit". The state before the circuit etching is, for example, an integrated structure of "heat dissipating metal layer / thermally conductive resin sheet / conductive circuit forming metal layer", in which the conductive circuit forming metal layer is flat and formed on the entire surface of one side of the thermally conductive resin sheet, or formed on a partial area.

[0080] The material of the conductive circuit-forming metal layer is not particularly limited. In particular, it is generally preferable to form the conductive circuit-forming metal layer from a copper thin plate having a thickness of 0.05 mm to 1.2 mm in terms of electrical conductivity, etching properties, cost, and the like.

[0081] The dielectric breakdown voltage of the heat dissipating circuit board is preferably 40 kV / mm or more, more preferably 50 kV / mm or more, even more preferably 60 kV / mm or more, and even more preferably 80 kV / mm or more. By having a dielectric breakdown voltage of 40 kV / mm or more, even if the thermal conductive resin sheet has a thickness of, for example, 100 μm, a dielectric breakdown voltage of 4 kV or more can be obtained, and if the dielectric breakdown voltage is 80 kV / mm or more, a dielectric breakdown voltage of 4 kV or more can be obtained even if the thickness is 50 μm. Therefore, while using a thin thermal conductive resin layer that is advantageous in terms of thermal resistance, it has sufficient voltage resistance performance and can suppress the occurrence of dielectric breakdown when a high voltage is applied.

[0082] 6. Power Semiconductor Devices The thermally conductive resin sheet of the present invention and the laminated heat dissipation sheet of the present invention can be suitably used as a heat dissipation sheet for a power semiconductor device, and a highly reliable power semiconductor module can be realized. The power semiconductor device is a power semiconductor device that uses the above-mentioned thermally conductive resin sheet or the above-mentioned laminated heat dissipation sheet, and the above-mentioned thermally conductive resin sheet or the above-mentioned laminated heat dissipation sheet is mounted on a power semiconductor device apparatus as a heat dissipation circuit board. The power semiconductor device has a high thermal conductivity and hence a heat dissipation effect, which allows it to achieve high output and high density with high reliability. In a power semiconductor device, conventionally known materials can be appropriately used for the aluminum wiring, sealing material, packaging material, heat sink, thermal paste, solder, and other materials other than the thermally conductive resin sheet or laminated heat dissipation sheet.

[0083] <Explanation of terms> In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In addition, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the intention that "greater than X is preferable" or "less than Y is preferable." In the present invention, the term "sheet" conceptually encompasses a sheet, a film, and a tape. EXAMPLES

[0084] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not exceeded.

[0085] <Examples 1 and 2 and Comparative Examples 1 to 3> The materials used, the production methods, and the measurement conditions and evaluation methods for the thermally conductive resin sheets in Examples 1 and 2 and Comparative Examples 1 to 3 are as follows.

[0086] [Materials used] (thermoplastic resin) Thermoplastic resin 1: Polyether ether ketone "KetaSpire KT-880FP" (manufactured by Solvay, melting point: 343°C, melt viscosity: 0.15 kPa·s (400°C), average particle size (D50): 30.0 to 45.0 μm, MFR: 86 g / 10 min, mass average molecular weight (Mw): 58,000 was used.

[0087] (thermosetting resin) Thermosetting resin 1: Epoxy resin composition (8.74 parts by mass of bisphenol F type epoxy resin (manufactured by Mitsubishi Chemical Corporation, mass average molecular weight in terms of polystyrene: 60,000), 10.93 parts by mass of hydrogenated bisphenol A type liquid epoxy resin (manufactured by Mitsubishi Chemical Corporation), 2.62 parts by mass of p-aminophenol type liquid epoxy resin (manufactured by Mitsubishi Chemical Corporation), 5.73 parts by mass of phenolic resin curing agent "MEH-8000H" (manufactured by Meiwa Chemical Industry Co., Ltd.), 0.48 parts by mass of 1-cyanoethyl-2-undecylimidazole "C11Z-CN" (manufactured by Shikoku Chemical Industry Co., Ltd., molecular weight 275) as a curing catalyst) was used.

[0088] (Thermal conductive filler) The thermally conductive fillers are as follows: Thermally conductive filler 1: Boron nitride agglomerated particles with a house-of-cards structure (oil absorption: 1.12 mL / g, average particle size (D50): 35 μm, maximum particle size Dmax: 90 μm) Thermally conductive filler 2: boron nitride agglomerated particles with a house-of-cards structure (oil absorption: 1.00 mL / g, average particle size (D50): 34 μm, maximum particle size Dmax: 90 μm) Thermally conductive filler 3: boron nitride agglomerated particles with a house-of-cards structure (oil absorption: 0.82 mL / g, average particle size (D50): 34 μm, maximum particle size Dmax: 90 μm)

[0089] Thermally conductive filler 1 was prepared by the method described below.

[0090] (raw materials) The raw materials used were 10,000 g of hexagonal boron nitride (hereinafter referred to as "raw h-BN powder") having a half-width of the (002) plane peak of 2θ = 0.67° and an oxygen concentration of 7.5 wt% as measured by powder X-ray diffraction measurement (Cu-Kα), 11,496 g of binder (Taki Chemical Industry Co., Ltd.'s "Taxeram M160L", solids concentration 21% by mass), and 250 g of surfactant (Kao Corporation's "ammonium lauryl sulfate", solids concentration 14% by mass).

[0091] (Preparation of Slurry) The raw material h-BN powder was weighed out in the above amount into a resin bottle, and then the binder was added in the above amount. Furthermore, the surfactant was added in the above amount, and then zirconia ceramic balls were added and the mixture was stirred on a pot mill rotating table for 1 hour to obtain a BN slurry. The viscosity of this slurry was 810 mPa s.

[0092] (granulation) The BN slurry was spray-dried using a spray dryer (FOC-20 manufactured by Okawara Kakoki Co., Ltd.) at a disk rotation speed of 20,000 to 23,000 rpm and a drying temperature of 80° C. to obtain spherical BN granulated particles.

[0093] (pyrolysis) The BN granulated particles were heat-treated in an air atmosphere at 700° C. for 5 hours to obtain precursor particles.

[0094] (Preparation of boron nitride agglomerated particles) The precursor particles were filled in a circular graphite crucible with a lid in the shape of a disk, the atmosphere in the furnace was replaced with nitrogen gas at normal pressure at room temperature, the temperature was raised to 2000°C at a rate of 83°C / hour while passing nitrogen gas, and after reaching 2000°C, the temperature was maintained for 5 hours while passing nitrogen gas, and then cooled to room temperature. The part that had been in contact with the graphite was removed from the sintered material removed from the crucible, and the material was manually crushed using a mortar and pestle, and then treated with a roll mill to obtain spherical agglomerated particles of boron nitride having a card house structure. The obtained boron nitride agglomerated particles were sieved using a sieve with an opening size of 90 μm, and only the particles that passed through the sieve were used as thermally conductive filler 1.

[0095] Thermally conductive filler 2 was prepared by dry-treating thermally conductive filler 1 obtained by the above method for 10 minutes in a bead mill using nylon balls with a diameter of 10 mm, to obtain spherical agglomerated particles in which the primary particles on the surface of the agglomerated particles were bent so as to cover the agglomerated particles.

[0096] Thermally conductive filler 3 was made by dry-treating thermally conductive filler 1 obtained by the above method for 30 minutes in a bead mill using nylon balls with a diameter of 10 mm, resulting in spherical agglomerated particles in which the primary particles on the surface of the agglomerated particles were bent and folded to cover the agglomerated particles. As shown in Figure 2, the SEM image of a single agglomerated particle indicates that the agglomerated particle itself is not broken or damaged, and the internal house-of-cards structure is also maintained.

[0097] The oil absorption of the boron nitride agglomerated particles was measured in accordance with JIS K5101-13-1:2004 ("Testing methods for pigments" - Part 13: Oil absorption - Section 1: Refined linseed oil method), specifically by the following method. Weigh out 2 g of boron nitride agglomerated particle powder onto a watch glass, and drip refined linseed oil onto the powder from a 10 mL burette. After each drip, use a spatula to knead the refined linseed oil into the boron nitride agglomerated particle powder. Repeat this process until the mixture of linseed oil and powder becomes a single lump. After this, drip one drop at a time, and knead with the spatula each time until the mixture of linseed oil and powder becomes uniformly smooth and hard without cracking or separating, which is the end point. The measured value converted to 1 g of powder is the oil absorption. If the oil absorption is large and the above procedure is difficult to perform with 2 g of sample, use 1 g of sample and repeat the same procedure.

[0098] The maximum particle size Dmax and the average particle size D50 of the boron nitride agglomerated particles are values ​​measured by the following method. A sample was prepared by ultrasonically dispersing 20 mg of boron nitride agglomerated particles in 10 mL of pure water medium containing sodium hexametaphosphate, and the particle size distribution was measured using a laser diffraction / scattering particle size distribution analyzer LA-920 (manufactured by Horiba, Ltd.). From the particle size distribution obtained, the maximum particle diameter Dmax and average particle diameter D50 of the boron nitride agglomerated particles were calculated.

[0099] [Preparation of Thermally Conductive Resin Sheets of Examples 1 and 2 and Comparative Example 1] The matrix resin powder and the thermally conductive filler powder were mixed at room temperature, and the resulting powder mixture was pressed for 10 minutes in a high-temperature vacuum press (Kitagawa Seiki Co., Ltd.) at a press temperature of 395°C and a press surface pressure of 10 MPa to obtain a thermally conductive resin sheet having a size of 15 cm square and a thickness of 150 μm, and a thermally conductive resin sheet having a size of 15 cm square and a thickness of 500 μm. At this time, the thickness of the sheet was adjusted by adjusting the amount of powder. The 150 μm thick thermally conductive resin sheet was used as a specimen for a moisture absorption reflow test described later, and the 500 μm thick thermally conductive resin sheet was used as a specimen for measuring thermal conductivity described later.

[0100] Here, the above 10 minutes means that the inside of the vacuum press was preheated to 150°C, the powder mixture was put there as a press charge composition, a light pressure of several MPa was applied to the powder mixture while operating the vacuum pump, the temperature inside the press was set to 395°C, and after 40 minutes of heating, the press surface pressure was set to 10 MPa for 10 minutes. After 10 minutes had passed, the temperature inside the press was again set to 150°C, and when the internal temperature approached 150°C, the vacuum was released and the thermally conductive resin sheet was taken out.

[0101] The above press-loaded configuration refers to a configuration necessary for one batch press, in which a frame-shaped spacer 6 mm thick, with outer edges 20 cm long and wide, and with an internal opening of 15 cm x 15 cm long and wide is placed on the lower plated plate, the powdered mixture in the amount required to obtain a 150 μm-thick pressed sheet or a 500 μm-thick pressed sheet is scattered inside the spacer, and a drop lid 14.6 cm long and wide, with a thickness of 5.85 mm (when a 150 μm-thick sample is taken) or a thickness of 5.50 mm (when a 500 μm-thick sample is taken), is fitted into the 15 cm x 15 cm opening, and the upper plated plate is placed on top.

[0102] [Preparation of thermally conductive resin sheets of Comparative Examples 2 and 3] The thermally conductive filler was added so that the total amount of the epoxy resin composition and the thermally conductive filler was 100% by mass, and then 37.2% by mass of a mixed solution of methyl ethyl ketone and cyclohexanone (mixing ratio (volume ratio) 1:1) was added and mixed so that the total solid content concentration of the epoxy resin composition and the thermally conductive filler was 62.8% by mass, to obtain a coating slurry (coating liquid for sheets). When mixing these, after manual mixing, stirring was performed for 2 minutes using a self-rotating stirrer "Awatori Rentaro AR-250". The coating slurry obtained above was applied onto a polyethylene terephthalate film (hereinafter also referred to as "PET film") having a thickness of 38 μm by the doctor blade method, and after heating and drying at 60° C. for 120 minutes, it was pressed at a press temperature of 42° C. and a press surface pressure of 15 MPa for 10 minutes to obtain an uncured epoxy resin sheet-shaped molding. This epoxy resin sheet-shaped molding was used as a specimen for the moisture absorption reflow test described later.

[0103] In addition, a thermally conductive resin sheet having a thickness of 500 μm used for measuring thermal conductivity described later was prepared by the following method. The uncured epoxy resin sheet-like molded body was cut into a size of 10 cm×10 cm, and four of the molded bodies were stacked to prepare a press-prepared structure. Using the same spacer and drop lid as those used to obtain a 500 μm-thick sheet in Example 1 and Comparative Example 1, the press was performed at a press temperature of 175° C. and a press surface pressure of 10 MPa for 1 hour to obtain a thermally conductive resin sheet having a thickness of 500 μm. The excess thickness of the laminated uncured epoxy resin sheet-like molded body was absorbed by the empty volume between the sheet size of 10 cm×10 cm and the spacer size of 15 cm×15 cm.

[0104] <Measurement conditions and evaluation methods> The thermally conductive resin sheets of Examples 1 and 2 and Comparative Examples 1 to 3 were measured and evaluated by the following methods.

[0105] [Thermal conductivity at 25℃] The thermal conductive resin sheets (specimens) having a thickness of 500 μm obtained in Examples 1 and 2 and Comparative Examples 1 to 3 were cut into measurement samples each having a size of 10 mm square. A laser light absorbing spray (Fine Chemical Japan's "Black Guard Spray FC-153") was thinly applied to both sides of the sample and dried, and the thermal diffusivity a (mm 2 The measurement was carried out on five points cut out from the same sheet, and the arithmetic average value was calculated.

[0106] Next, the density ρ (g / m) of the resin sheet was measured using a specific gravity measuring instrument (manufactured by A&D Co., Ltd.) according to the Archimedes method in accordance with JIS K6268. 3 In addition, the specific heat capacity c (J / (g K)) at 25°C was measured using a DSC measuring device (ThermoPlusEvo DSC8230, Rigaku Corporation) in accordance with JIS K7123. From these measured values, the thermal conductivity in the sheet thickness direction at 25° C. was calculated as "H=a×ρ×c."

[0107] The thermal diffusivity a (mm 2 As there are no JIS standards for the thermal diffusivity and thermal conductivity of resin-based materials, JIS R1611-2010 (Method of measurement of thermal diffusivity, specific heat capacity, and thermal conductivity of fine ceramics by the flash method) was used as a reference, and as this standard specifies that "the thickness of the sample shall be 0.5 mm or more and 5 mm or less," only the thickness of the sample used for thermal conductivity measurement was adjusted to 0.5 mm for measurement.

[0108] [Breakdown voltage (BDV) before moisture absorption and reflow test] (Making a heat dissipation circuit board) The thermally conductive resin sheets having a thickness of 150 μm produced in Examples 1 and 2 and Comparative Example 1 were cut into a size of 40 mm×80 mm to prepare thermally conductive resin sheets for circuit boards. On the other hand, one copper plate measuring 40 mm x 80 mm and having a thickness of 2000 μm to serve as a metal plate material for heat dissipation, and one copper plate measuring 40 mm x 80 mm and having a thickness of 500 μm to serve as a copper plate for forming a conductive circuit were prepared for each thermally conductive resin sheet for the circuit board. One side of a 2000 μm thick copper plate and one side of a 500 μm thick copper plate were each polished with #100 sandpaper in advance to roughen the surface, and the thermally conductive resin sheet for circuit boards was sandwiched between the copper plates of different thicknesses so that the roughened surface faced the thermally conductive resin sheet for circuit boards. The copper plates were pressed at a press temperature of 390°C and a press surface pressure of 13 MPa for 10 minutes to obtain a laminated heat dissipation sheet consisting of "heat dissipating metal plate material (copper plate) / thermal conductive resin sheet / copper plate for forming conductive circuits."

[0109] On the other hand, for Comparative Examples 2 and 3, which are thermally conductive resin sheets made of thermosetting resin, a 150 μm thick epoxy resin sheet-like molded body that was uncured or in which the curing reaction had progressed only slightly was sandwiched between the above-mentioned roughened metal plate material for heat dissipation (copper plate) and a copper plate for forming a conductive circuit, and vacuum pressed for 30 minutes at a press temperature of 175° C. and a press surface pressure of 10 MPa to complete the curing reaction of the thermosetting resin, thereby obtaining a laminated heat dissipation sheet consisting of "metal plate material for heat dissipation (copper plate) / thermally conductive resin sheet / copper plate for forming a conductive circuit."

[0110] Furthermore, the copper plate for forming the conductive circuit of each of the laminated heat dissipation sheets was etched and patterned to obtain a heat dissipation circuit board. The pattern was such that two copper plates for the conductive circuit with a circular pattern of φ25 mm remained on a thermally conductive resin sheet of 40 mm × 80 mm.

[0111] (Measurement of dielectric breakdown voltage (BDV)) The heat dissipation circuit boards prepared using the thermally conductive resin sheets obtained in Examples 1 and 2 and Comparative Examples 1 to 3 by the above method were immersed in Fluorinert FC-40 (manufactured by 3M), and a φ25mm electrode was placed on the φ25mm copper plate patterned by etching on the heat dissipation circuit board using an ultra-high voltage withstand voltage tester 7470 (manufactured by Keisoku Gijutsu Kenkyusho Co., Ltd.), a voltage of 0.5kV was applied, and the voltage was increased by 0.5kV every 60 seconds, and measurements were performed until dielectric breakdown occurred. The measurements were performed at a frequency of 60Hz and a voltage increase rate of 1000V / sec.

[0112] If the breakdown voltage per unit thickness (converted value for a thickness of 1 mm) was 60 kV / mm or more, it was marked as "〇 (good)", if it was 40 kV / mm or more but less than 60 kV / mm, it was marked as "△ (not good)", and if it was less than 40 kV / mm, it was marked as "× (poor)". The measurement results are shown in Table 1. The evaluation of the dielectric breakdown voltage (BDV) before the moisture absorption reflow test can be used as an evaluation of the voltage resistance performance.

[0113] [Breakdown voltage after moisture absorption reflow test (BDV)] (Measurement of dielectric breakdown voltage (BDV)) Using the thermally conductive resin sheets obtained in Examples 1 and 2 and Comparative Examples 1 to 3, the heat dissipating circuit boards prepared in the same manner as in the above [Breakdown voltage before moisture absorption reflow test (BDV)] were stored in an environment of 85°C and 85% RH for 3 days using a thermohygrostat SH-221 (manufactured by Espec Corporation), and then heated from room temperature to 290°C in 12 minutes in a nitrogen atmosphere within 30 minutes, held at 290°C for 10 minutes, and then cooled to room temperature (moisture absorption reflow test). Thereafter, the heat dissipating circuit board was immersed in Fluorinert FC-40 (manufactured by 3M Corporation), and a φ25mm electrode was placed on a φ25mm copper plate patterned by etching on the heat dissipating circuit board using an ultra-high voltage withstand voltage tester 7470 (manufactured by Keisoku Gijutsu Kenkyusho Co., Ltd.), and a voltage of 0.5kV was applied, and the voltage was increased by 0.5kV every 60 seconds, and measurements were performed until dielectric breakdown occurred. The measurements were carried out at a frequency of 60 Hz and a voltage rise rate of 1000 V / sec.

[0114] If the breakdown voltage per unit thickness (converted value for a thickness of 1 mm) was 60 kV / mm or more, it was marked as "〇 (good)", if it was 40 kV / mm or more but less than 60 kV / mm, it was marked as "△ (not good)", and if it was less than 40 kV / mm, it was marked as "× (poor)". The measurement results are shown in Table 1. The evaluation of the dielectric breakdown voltage (BDV) after the moisture absorption reflow test can be used as an evaluation of the moisture absorption reflow resistance.

[0115] [Observation of sample condition after moisture absorption reflow test] The heat dissipating circuit boards produced in Examples 1 and 2 and Comparative Examples 1 to 3 were subjected to a moisture absorption reflow test in the same manner as above, and then the interface between the copper electrode with a diameter of 25 mm patterned by the above etching and the thermally conductive resin sheet was observed using an ultrasonic imaging device FinSAT (FS300III) (manufactured by Hitachi Power Solutions). The measurement was performed using a probe with a frequency of 50 MHz, a gain of 30 dB, a pitch of 0.2 mm, and by placing the sample in water. Those that did not show peeling, lifting, or voids at the interface were marked as "○ (good)", and those that showed peeling, lifting, or voids at the interface were marked as "× (poor)". The evaluation results are also shown in Table 1. The evaluation of interfacial peeling after the moisture absorption reflow test can be made as an evaluation of whether or not interfacial peeling due to thermal expansion and thermal contraction and deformation due to foaming of the thermal conductive resin sheet are likely to occur when the thermal conductive resin sheet is laminated with a metal plate and subjected to a reflow process.

[0116] [Table 1]

[0117] Comparing Examples 1 and 2 with Comparative Example 1, it was found that the thermal conductivity was significantly improved by using boron nitride agglomerated particles having an oil absorption of 0.95 mL / g or more. In addition, when comparing the breakdown voltage values ​​before and after the moisture absorption reflow test between Examples 1 and 2 and Comparative Examples 2 and 3, it was found that the use of a thermoplastic resin having a melting point of 300°C or higher as the matrix resin improved the voltage resistance performance and moisture absorption reflow resistance. Furthermore, in Examples 1 and 2, it was found that by using a manufacturing method including a mixing step of mixing a powder made of a thermoplastic resin with boron nitride agglomerated particles having an oil absorption of 0.95 mL / g or more, and a press molding step of pressing the mixture to form a sheet, it was possible to achieve both high voltage resistance performance and high thermal conductivity. In Comparative Example 2, epoxy resin and boron nitride agglomerated particles with high oil absorption were used to form a sheet by a conventional wet coating method. The surface of the boron nitride agglomerated particles was very uneven, so streaks were generated when the film was coated, and the sheet also contained many air bubbles, which is thought to have reduced the voltage resistance performance. Due to the influence of the air bubbles in the sheet, the thermal conductivity was also inferior to that of Example 2, which contained the same amount of the same filler. In Comparative Example 3, epoxy resin and boron nitride agglomerated particles with low oil absorption were used to form a sheet by a conventional wet coating method. Because the surface of the boron nitride agglomerated particles was less uneven, streaks caused by coating were reduced and the voltage resistance performance was within the acceptable range, but the moisture absorption reflow resistance was poor and the thermal conductivity was also low.

Claims

1. A thermally conductive resin sheet comprising a thermoplastic resin, boron nitride, and spherical agglomerated particles of boron nitride, the thermally conductive resin sheet having an oil absorption of 0.95 mL / g or more.

2. A thermally conductive resin sheet comprising a thermoplastic resin and spherical agglomerated particles of boron nitride (excluding those having a structure having a core made of a substance other than boron nitride at the center and a card-house-shaped shell made of boron nitride surrounding the core) having an oil absorption of 0.95 mL / g or more.

3. The thermally conductive resin sheet according to claim 1 or 2, wherein the thermoplastic resin has a melting point of 300° C. or higher.

4. The thermally conductive resin sheet according to any one of claims 1 to 3, wherein the thermoplastic resin contains a polyether ketone resin.

5. The thermally conductive resin sheet according to any one of claims 1 to 4, wherein the boron nitride agglomerated particles have an oil absorption of less than 2.0 mL / g.

6. The thermally conductive resin sheet according to any one of claims 1 to 5, wherein the boron nitride agglomerated particles have a house of cards structure.

7. The thermally conductive resin sheet according to any one of claims 1 to 6, comprising 15% by mass or more and 40% by mass or less of the thermoplastic resin and 60% by mass or more and 85% by mass or less of the boron nitride agglomerated particles.

8. The thermally conductive resin sheet according to any one of claims 1 to 7, having a thickness of 50 µm or more and 300 µm or less.

9. The thermally conductive resin sheet according to any one of claims 1 to 8, having a thermal conductivity in the thickness direction at 25 ° C. of 15 W / m · K or more.

10. A laminated heat dissipation sheet comprising a heat dissipation metal layer laminated on one surface of the thermally conductive resin sheet according to any one of claims 1 to 9.

11. A heat dissipating circuit board comprising the laminated heat dissipating sheet according to claim 10.

12. 12. The heat dissipation circuit board according to claim 11, further comprising a conductive circuit formed on the other surface of the thermally conductive resin sheet.

13. A power semiconductor device comprising the heat dissipation circuit board according to claim 11 or 12.

14. A method for producing a thermally conductive resin sheet, comprising: a mixing step of obtaining a mixture of a powder made of a thermoplastic resin and spherical agglomerated particles of boron nitride having an oil absorption of 0.95 mL / g or more, the agglomerated particles being made of boron nitride; and a press molding step of pressing the mixture to form a sheet.

15. A method for producing a thermally conductive resin sheet, comprising: a mixing step of obtaining a mixture of a powder made of a thermoplastic resin and spherical agglomerated particles of boron nitride (excluding those having a structure having a core made of a substance other than boron nitride at the center surrounded by a card-house-shaped shell made of boron nitride) having an oil absorption of 0.95 mL / g or more; and a press molding step of pressing the mixture to form a sheet.

Citation Information

Patent Citations

  • Melamine borate particle, its production and use thereof and production of hexagonal boron nitride powder

    JP1997202663A

  • Improved boron nitride composition and polymer-based composition blended therewith

    JP2006257392A

  • Thermally conductive composition and method for producing the same

    JP2008510878A

  • Aggregated boron nitride particle, composition containing aggregated boron nitride particle, and three-dimensional integrated circuit having layer comprising composition

    JP2013241321A

  • Boron nitride aggregated particle, composition containing boron nitride aggregated particle, and three-dimensional integrated circuit having layer comprising the composition

    JP2015006985A