Method for producing silica particles, method for producing silica sol, polishing method, method for producing semiconductor wafer, and method for producing semiconductor device

A controlled hydrolysis and condensation reaction with alkali catalysts and specific conditions produce silica particles of 30 nm to 40 nm diameter, addressing the inconsistency in existing methods and improving polishing precision for semiconductor wafers.

JP7581910B2Active Publication Date: 2024-11-13MITSUBISHI CHEM CORP
View PDF 12 Cites 0 Cited by

Patent Information

Application Number
JP2021008422
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-02-04
Filing Date
2021-01-22
Publication Date
2024-11-13
Estimated Expiration
2041-01-22

AI Technical Summary

Technical Problem

Existing methods for producing silica particles with an average primary particle diameter of 30 nm to 40 nm for precision polishing in semiconductor manufacturing are not well-defined, leading to inconsistent results.

Method used

A method involving a hydrolysis and condensation reaction of tetraalkoxysilane using an alkali catalyst, with specific temperature and catalyst concentration controls, followed by concentration and pressurized heating of the reaction solution, to produce silica particles with the desired diameter.

Benefits of technology

The method consistently produces silica particles with an average primary particle diameter of 30 nm to 40 nm, enhancing polishing rate and smoothness for semiconductor wafers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007581910000002
    Figure 0007581910000002
  • Figure 0007581910000001
    Figure 0007581910000001
Patent Text Reader

Abstract

To provide a method for producing silica particles for obtaining silica particles with an average primary particle size of 30 nm-40 nm.SOLUTION: A method for producing silica particles includes subjecting, using an alkali catalyst, tetraalkoxysilane to a hydrolysis reaction and a condensation reaction. When a reaction temperature is defined as x°C and a concentration of the alkali catalyst in a reaction system is defined as y mass%, 0.03x-0.17≤y≤0.03x+0.03 holds from the start to finish of the reaction.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing silica particles, a method for producing a silica sol, a polishing method, a method for producing a semiconductor wafer, and a method for producing a semiconductor device. [Background technology]

[0002] Polishing methods using polishing liquids are known as methods for polishing the surfaces of materials such as metals and inorganic compounds. In particular, in the final polishing of prime silicon wafers for semiconductors and reclaimed silicon wafers, and in chemical mechanical polishing (CMP) for planarizing interlayer insulating films during semiconductor device manufacturing, forming metal plugs, forming buried wiring, and the like, the surface condition has a significant effect on the semiconductor characteristics, so the surfaces and end faces of these components are required to be polished with extremely high precision.

[0003] In such precision polishing, a polishing composition containing silica particles is adopted, and colloidal silica is widely used as the abrasive grains, which are the main component. Depending on the manufacturing method, colloidal silica is known to be produced by pyrolysis of silicon tetrachloride (fumed silica, etc.), by deionization of alkali silicate such as water glass, and by hydrolysis and condensation reaction of alkoxysilane (generally called the "sol-gel method").

[0004] Many studies have been conducted on methods for producing silica particles. For example, Patent Document 1 discloses a method for producing silica particles by hydrolysis and condensation reactions of alkoxysilane. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2005-060217 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, silica particles obtained by hydrolysis and condensation reactions are sometimes used for polishing silicon wafers, and the average primary particle size of the silica particles used for polishing silicon wafers is often 30 nm to 40 nm because suitable polishing characteristics are obtained. The reason for this is that both the polishing rate and smoothness for the polished object represented by silicon wafers are achieved.

[0007] The method for producing silica particles disclosed in Patent Document 1 does not disclose any conditions for obtaining silica particles having an average primary particle diameter of 30 nm to 40 nm, and has a problem that, depending on the production conditions, silica particles having an average primary particle diameter of 30 nm to 40 nm may not be obtained.

[0008] The present invention has been made in view of the above problems, and an object of the present invention is to provide a method for producing silica particles for obtaining silica particles having an average primary particle diameter of 30 nm to 40 nm. [Means for solving the problem]

[0009] Conventionally, suitable production conditions for obtaining silica particles having an average primary particle diameter of 30 nm to 40 nm have not necessarily been disclosed. However, as a result of intensive research, the present inventors have found that silica particles having an average primary particle diameter of 30 nm to 40 nm can be obtained by optimizing the reaction temperature and the concentration of the alkali catalyst in the reaction system, and have completed the present invention.

[0010] That is, the gist of the present invention is as follows. [1] A method for producing silica particles by hydrolysis and condensation of tetraalkoxysilane using an alkali catalyst, A method for producing silica particles, wherein the following formula (1) is satisfied from the start of the reaction to the end of the reaction, when the reaction temperature is x°C and the concentration of the alkali catalyst in the reaction system is y% by mass. 0.03x-0.17≦y≦0.03x+0.03 (1) [2] A method for producing silica particles according to [1], comprising adding a solution (B) containing a tetraalkoxysilane and a solution (C) containing an alkali catalyst to a solution (A) containing an alkali catalyst, and subjecting the tetraalkoxysilane to a hydrolysis reaction and a condensation reaction. [3] The method for producing silica particles according to [1] or [2], further comprising satisfying the following formula (2) from the start of the reaction to the end of the reaction: 25≦x≦50 (2) [4] The method for producing silica particles according to any one of [1] to [3], further comprising satisfying the following formula (3) from the start of the reaction to the end of the reaction: 0.6≦y≦1.5 (3) [5] The method for producing silica particles according to any one of [1] to [4], wherein the average primary particle diameter of the silica particles is 30 nm to 40 nm. [6] A method for producing silica particles according to any one of [1] to [5], further comprising the following step (1): Step (1): A step of concentrating the reaction solution after the hydrolysis reaction and the condensation reaction and adding a dispersion medium [7] The method for producing silica particles according to [6], further comprising the following step (2): Step (2): A step of subjecting the dispersion of silica particles obtained in step (1) to a pressurized and heated treatment. [8] A method for producing a silica sol, comprising the method for producing silica particles according to any one of [1] to [7]. [9] The method for producing a silica sol according to [8], wherein a concentration of silica particles in the silica sol is 3% by mass to 50% by mass.

[10] A polishing method, comprising polishing using a polishing composition containing the silica sol obtained by the method for producing a silica sol according to [8] or [9].

[11] A method for producing a semiconductor wafer, comprising the polishing method according to

[10] .

[12] A method for manufacturing a semiconductor device, comprising the polishing method according to

[10] . Effect of the Invention

[0011] The method for producing silica particles of the present invention can provide silica particles having an average primary particle diameter of 30 nm to 40 nm. [Brief description of the drawings]

[0012] [Figure 1] 1 is a graph summarizing the production conditions of the method for producing silica particles at the start of the reaction in Examples and Comparative Examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] The present invention will be described in detail below, but the present invention is not limited to the following embodiments and can be modified and practiced in various ways within the scope of the gist. In addition, when the expression "~" is used in this specification, it is used as an expression including the numerical values ​​or physical property values ​​before and after it.

[0014] (Method of producing silica particles) The method for producing silica particles of the present invention is a method for producing silica particles by hydrolysis and condensation reaction of tetraalkoxysilane using an alkali catalyst, and satisfies the following formula (1) from the start of the reaction to the end of the reaction when the reaction temperature is x°C and the concentration of the alkali catalyst in the reaction system is y% by mass. 0.03x-0.17≦y≦0.03x+0.03 (1)

[0015] The reaction temperature refers to the temperature from the start of the hydrolysis reaction and the condensation reaction to the end of the reaction. The concentration of the alkali catalyst in the reaction system refers to the total amount of the alkali catalyst relative to the total amount of the liquid and the substances dissolved in the liquid in the reaction system in the hydrolysis reaction and the condensation reaction. The total amount of the liquid in the reaction system and the substances dissolved in the liquid is only solution (A) described later at the start of the reaction, and during the reaction it is the total amount of solution (A), solution (B), solution (C) and the alcohol produced in the reaction. The liquid in the reaction system and the substances dissolved in the liquid do not include silica particles dispersed in the liquid.

[0016] By satisfying the above formula (1) from the start of the reaction to the end of the reaction, silica particles having an average primary particle diameter of 30 nm to 40 nm can be obtained. It is preferable to satisfy the following formula (1') from the start of the reaction to the end of the reaction, and it is more preferable to satisfy the following formula (1'') from the start of the reaction to the end of the reaction. 0.03x-0.16≦y≦0.03x+0.02 (1') 0.03x-0.15≦y≦0.03x+0.01 (1'')

[0017] x is the reaction temperature (° C.), and it is preferable that x is within the range described below from the start of the reaction to the end of the reaction. x is preferably 25 to 50, and more preferably 30 to 45. When x is 25 or more, silica particles having an average primary particle size of 40 nm or less can be easily obtained. When x is 50 or less, silica particles having an average primary particle size of 30 nm or more can be easily obtained.

[0018] y is the concentration (mass%) of the alkali catalyst in the reaction system, and it is preferable that y is kept within the range described below from the start of the reaction to the end of the reaction. The total amount of the substances in the reaction system is taken as 100 mass%. y is preferably 0.6 to 1.5, and more preferably 0.7 to 1.4. When y is 0.6 or more, silica particles having an average primary particle size of 30 nm or more can be easily obtained. When y is 1.5 or less, silica particles having an average primary particle size of 40 nm or less can be easily obtained.

[0019] Examples of the alkali catalyst include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. Among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress the inclusion of metal impurities, is highly volatile, and is easy to remove after hydrolysis and condensation reactions.

[0020] In the method for producing silica particles of the present invention, it is preferable to add a solution (B) containing a tetraalkoxysilane and a solution (C) containing an alkali catalyst to a solution (A) containing an alkali catalyst, and to cause the tetraalkoxysilane to undergo a hydrolysis reaction and a condensation reaction.

[0021] Examples of the alkali catalyst in the solution (A) include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. Among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress the inclusion of metal impurities, is highly volatile, and is easy to remove after the hydrolysis reaction and the condensation reaction.

[0022] The solution (A) preferably contains water, since this allows the hydrolysis reaction and condensation reaction of the tetraalkoxysilane to proceed.

[0023] The solution (A) preferably contains a solvent other than water, since this provides excellent dispersibility of the tetraalkoxysilane in the reaction solution. Examples of the solvent other than water in the solution (A) include methanol, ethanol, propanol, isopropanol, ethylene glycol, etc. These solvents other than water may be used alone or in combination of two or more. Among these solvents other than water, alcohol is preferred, more preferably methanol or ethanol, and even more preferably methanol, because the solvent used in the hydrolysis reaction and the solvent by-produced in the condensation reaction are the same, and the convenience in production is excellent.

[0024] When the reaction temperature is x°C and the concentration of the alkali catalyst in solution (A) is z mass%, silica particles having an average primary particle size of 30 nm to 40 nm can be obtained, so it is preferable to satisfy the following formula (2), it is preferable to satisfy the following formula (2'), and it is more preferable to satisfy the following formula (2''). The total amount of solution (A) is 100 mass%. 0.03x-0.17≦z≦0.03x+0.03 (2) 0.03x-0.16≦z≦0.03x+0.02 (2') 0.03x-0.15≦z≦0.03x+0.01 (2'')

[0025] z is the concentration (mass %) of the alkali catalyst in the solution (A), and z is preferably set to the range described below at the start of the reaction. z is preferably 0.58 to 1.53, and more preferably 0.73 to 1.38. When z is 0.58 or more, silica particles having an average primary particle size of 30 nm or more can be easily obtained. When z is 1.53 or less, silica particles having an average primary particle size of 40 nm or less can be easily obtained.

[0026] The concentration of water in solution (A) is preferably 3 mass % to 25 mass %, and more preferably 7 mass % to 20 mass %, in 100 mass % of solution (A) because silica particles with an average primary particle diameter of 30 nm to 40 nm can be easily obtained.

[0027] Examples of the tetraalkoxysilane in the solution (B) include tetramethoxysilane, tetraethoxysilane, tetrapropoxysilane, and tetraisopropoxysilane. These tetraalkoxysilanes may be used alone or in combination of two or more. Among these tetraalkoxysilanes, tetramethoxysilane and tetraethoxysilane are preferred, and tetramethoxysilane is more preferred, because they undergo a fast hydrolysis reaction, are less likely to leave unreacted substances, are highly productive, and can easily produce a stable silica sol.

[0028] The raw materials for the silica particles may be raw materials other than tetraalkoxysilane, such as low condensates of tetraalkoxysilane. However, due to their excellent reactivity, it is preferable that, out of 100 mass% of all raw materials constituting the silica particles, tetraalkoxysilane accounts for 50 mass% or more and raw materials other than tetraalkoxysilane accounts for 50 mass% or less, and it is more preferable that tetraalkoxysilane accounts for 90 mass% or more and raw materials other than tetraalkoxysilane accounts for 10 mass% or less.

[0029] The solution (B) may contain only tetraalkoxysilane without containing a solvent, but it is preferable that the solution (B) contains a solvent, since this improves the dispersibility of the tetraalkoxysilane in the reaction liquid. Examples of the solvent in the solution (B) include methanol, ethanol, propanol, isopropanol, and ethylene glycol. These solvents may be used alone or in combination of two or more. Among these solvents, alcohol is preferred, more preferably methanol or ethanol, and even more preferably methanol, because the solvent used in the hydrolysis reaction and the solvent by-produced in the condensation reaction are the same, and the convenience in production is excellent.

[0030] The concentration of the tetraalkoxysilane in solution (B) is preferably 60% by mass to 95% by mass, more preferably 70% by mass to 90% by mass, in 100% by mass of solution (B). When the concentration of the tetraalkoxysilane in solution (B) is 60% by mass or more, the reaction liquid tends to become homogeneous. In addition, when the concentration of the tetraalkoxysilane in solution (B) is 95% by mass or less, the formation of a gel-like substance can be suppressed.

[0031] The concentration of the solvent in solution (B) is preferably 5% by mass to 40% by mass, more preferably 10% by mass to 30% by mass, in 100% by mass of solution (B). When the concentration of the solvent in solution (B) is 5% by mass or more, the generation of a gel-like substance can be suppressed. Also, when the concentration of the solvent in solution (B) is 40% by mass or less, the reaction liquid tends to become homogenous.

[0032] The addition rate of solution (B) per hour relative to the volume of solution (A) is preferably 0.05 kg / hour / L to 1.3 kg / hour / L, and more preferably 0.1 kg / hour / L to 0.8 kg / hour / L. When the addition rate of solution (B) is 0.05 kg / hour / L or more, the productivity of silica particles is excellent. Furthermore, when the addition rate of solution (B) is 1.3 kg / hour / L or less, the generation of a gel-like substance can be suppressed.

[0033] Examples of the alkali catalyst in the solution (C) include ethylenediamine, diethylenetriamine, triethylenetetraamine, ammonia, urea, ethanolamine, and tetramethylammonium hydroxide. These alkali catalysts may be used alone or in combination of two or more. Among these alkali catalysts, ammonia is preferred because it has excellent catalytic action, is easy to control the particle shape, can suppress the inclusion of metal impurities, is highly volatile, and is easy to remove after the hydrolysis reaction and the condensation reaction.

[0034] It is preferable that the solution (C) contains a solvent, since this can reduce fluctuations in the concentration of the alkali catalyst in the reaction liquid. Examples of the solvent in the solution (C) include water, methanol, ethanol, propanol, isopropanol, and ethylene glycol. These solvents may be used alone or in combination of two or more. Among these solvents, water and alcohol are preferred, and water is more preferred, because the solvents used in the hydrolysis reaction and the condensation reaction are the same as the by-products, and are convenient in production.

[0035] The concentration of the alkali catalyst in solution (C) is preferably 0.5% by mass to 10% by mass, more preferably 1% by mass to 6% by mass, based on 100% by mass of solution (C). When the concentration of the alkali catalyst in solution (C) is 0.5% by mass or more, it is easy to adjust the concentration of the alkali catalyst in the reaction liquid from the start of the reaction to the end of the reaction. In addition, when the concentration of the alkali catalyst in solution (C) is 10% by mass or less, it is possible to reduce the fluctuation of the concentration of the alkali catalyst in the reaction liquid.

[0036] The concentration of the solvent in solution (C) is preferably 90% by mass to 99.5% by mass, more preferably 94% by mass to 99% by mass, based on 100% by mass of solution (C). When the concentration of the solvent in solution (C) is 90% by mass or more, the fluctuation of the concentration of the alkali catalyst in the reaction liquid can be reduced. Also, when the concentration of the solvent in solution (C) is 99.5% by mass or less, the concentration of the alkali catalyst in the reaction liquid can be easily adjusted from the start of the reaction to the end of the reaction.

[0037] The addition rate of solution (C) per hour relative to the volume of solution (A) is preferably 0.02 kg / hour / L to 0.5 kg / hour / L, and more preferably 0.04 kg / hour / L to 0.3 kg / hour / L. When the addition rate of solution (C) is 0.02 kg / hour / L or more, the productivity of silica particles is excellent. When the addition rate of solution (C) is 0.5 kg / hour / L or less, the formation of a gel-like substance can be suppressed.

[0038] The concentration of water in the reaction system of the hydrolysis reaction and condensation reaction is preferably maintained at 3 mass% to 25 mass%, and more preferably at 7 mass% to 20 mass%, relative to the total amount (100 mass%) of the reaction system, in order to easily obtain silica particles having an average primary particle diameter of 30 nm to 40 nm.

[0039] Since the method for producing silica particles of the present invention can remove unnecessary components and add necessary components, it is preferable that the method further includes the following step (1). Step (1): A step of concentrating the reaction solution after the hydrolysis reaction and the condensation reaction and adding a dispersion medium

[0040] Examples of the dispersion medium include water, methanol, ethanol, propanol, isopropanol, and ethylene glycol. These dispersion media may be used alone or in combination of two or more. Among these dispersion media, water and alcohol are preferred, and water is more preferred, because they have excellent affinity with silica particles.

[0041] The method for producing silica particles of the present invention preferably further includes the following step (2) since the condensation degree of the silica particles can be increased. Step (2): A step of subjecting the dispersion of silica particles obtained in step (1) to a pressurized and heated treatment.

[0042] The pressure of the pressurized heat treatment is preferably 0.10 MPa to 2.3 MPa, more preferably 0.14 MPa to 1.0 MPa. When the pressure of the pressurized heat treatment is 0.10 MPa or more, the degree of condensation of the silica particles can be increased. When the pressure of the pressurized heat treatment is 2.3 MPa or less, the silica particles can be produced without significant changes in the average primary particle size, average secondary particle size, and association ratio, and the dispersion stability of the silica sol is excellent. Pressurization can be achieved by heating the silica particle dispersion in a sealed state to above the boiling point of the dispersion medium. When the silica particle aqueous dispersion is heated to 100°C or higher in a sealed state, the pressure becomes the saturated water vapor pressure at that temperature.

[0043] The temperature of the pressure and heat treatment is preferably 100° C. to 220° C., and more preferably 110° C. to 180° C. When the temperature of the pressure and heat treatment is 100° C. or higher, the degree of condensation of the silica particles can be increased. When the temperature of the pressure and heat treatment is 220° C. or lower, silica particles can be produced without significant changes in the average primary particle size, average secondary particle size, and association ratio, and the dispersion stability of the silica sol is excellent.

[0044] The time of the pressurized heat treatment is preferably 0.25 hours to 10 hours, and more preferably 0.5 hours to 8 hours. When the time of the pressurized heat treatment is 0.25 hours or more, the degree of condensation of the silica particles can be increased. When the time of the pressurized heat treatment is 10 hours or less, the silica particles can be produced without significant changes in the average primary particle size, the average secondary particle size, and the association ratio, and the dispersion stability of the silica sol is excellent.

[0045] The pressurized heat treatment is preferably carried out in an aqueous dispersion because it can increase the degree of condensation of the silica particles without significantly changing the average primary particle size, the average secondary particle size, and the association ratio.

[0046] The pH when the pressure heat treatment is carried out in the aqueous dispersion is preferably 6.0 to 8.0, more preferably 6.5 to 7.8. When the pH when the pressure heat treatment is carried out in the aqueous dispersion is 6.0 or more, gelation of the silica sol can be suppressed. When the pH when the pressure heat treatment is carried out in the aqueous dispersion is 8.0 or less, the degree of condensation of the silica particles can be increased without significantly changing the average primary particle size, the average secondary particle size, and the association ratio.

[0047] (Physical properties of silica particles) The average primary particle diameter of the silica particles is preferably 30 nm to 40 nm, more preferably 32 nm to 38 nm. When the average primary particle diameter of the silica particles is 30 nm or more, the polishing rate for the polished object, such as a silicon wafer, is excellent. When the average primary particle diameter of the silica particles is 40 nm or less, the smoothness of the polished object, such as a silicon wafer, is excellent, and the silica particles are stable in the dispersion liquid, suppressing the sedimentation of the silica particles.

[0048] The average primary particle size of the silica particles is measured by the BET method. Specifically, the specific surface area of ​​the silica particles is measured using an automatic specific surface area measuring device, and the average primary particle size is calculated using the following formula (3). Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 )) ··· (3)

[0049] The average primary particle size of the silica particles can be set according to the above-mentioned conditions.

[0050] The average secondary particle diameter of the silica particles is preferably 50 nm to 90 nm, more preferably 60 nm to 80 nm. When the average secondary particle diameter of the silica particles is 50 nm or more, the polishing rate for the polished object, such as a silicon wafer, is excellent. When the average secondary particle diameter of the silica particles is 90 nm or less, the smoothness of the polished object, such as a silicon wafer, is excellent, and the silica particles are stable in the dispersion liquid, suppressing the sedimentation of the silica particles.

[0051] The average secondary particle size of the silica particles is measured by a DLS method, specifically, using a dynamic light scattering particle size measuring device.

[0052] The average secondary particle size of the silica particles can be set according to the above-mentioned conditions.

[0053] The association ratio of the silica particles is preferably 1.0 to 4.0, more preferably 1.1 to 3.0. When the association ratio of the silica particles is 1.0 or more, the polishing rate for the polished object, typically a silicon wafer, is excellent, and the productivity of the silicon wafer is excellent. When the association ratio of the silica particles is 4.0 or less, the surface roughness and scratches of the polished object, typically a silicon wafer, during polishing can be reduced, and the aggregation of the silica particles can be suppressed.

[0054] The association ratio of the silica particles is calculated using the following formula (4) from the average primary particle diameter measured by the above-mentioned measurement method and the average secondary particle diameter measured by the above-mentioned measurement method. Association ratio=average secondary particle diameter / average primary particle diameter... (4)

[0055] The surface silanol group density of silica particles is 0.1 / nm 2 ~10 pieces / nm 2 is preferable, and 0.5 particles / nm 2 ~7.5 pieces / nm 2 More preferably, 2.0 particles / nm 2 ~7.0 pieces / nm 2 More preferably, the surface silanol group density of the silica particles is 0.1 / nm 2 When the surface silanol group density of the silica particles is 10 / nm or more, the silica particles have a suitable surface repulsion, and the dispersion stability of the silica sol is excellent. 2 When the amount is equal to or less than this, the silica particles have an appropriate surface repulsion, and aggregation of the silica particles can be suppressed.

[0056] The surface silanol group density of the silica particles is measured by the Sears method, specifically, under the following conditions. Take a silica sol equivalent to 1.5 g of silica particles, add pure water to make the liquid volume 90 mL, add 0.1 mol / L hydrochloric acid aqueous solution until the pH becomes 3.6 in an environment of 25°C, add 30 g of sodium chloride, gradually add pure water to completely dissolve the sodium chloride, and finally add pure water until the total volume of the test liquid is 150 mL to obtain the test liquid. The obtained test liquid is placed in an automatic titrator, and 0.1 mol / L aqueous sodium hydroxide solution is added dropwise to measure the titer A (mL) of 0.1 mol / L aqueous sodium hydroxide solution required to change the pH from 4.0 to 9.0. The consumption amount V (mL) of 0.1 mol / L sodium hydroxide solution required for the pH to change from 4.0 to 9.0 per 1.5 g of silica particles was calculated using the following formula (5), and the surface silanol group density ρ (particles / nm 2 ) is calculated. V=(A×f×100×1.5) / (W×C) ··· (5) A: The amount (mL) of 0.1 mol / L sodium hydroxide solution required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles f: Potency of the 0.1 mol / L sodium hydroxide solution used C: Concentration of silica particles in silica sol (mass%) W: Amount of silica sol collected (g) ρ = (B × N A ) / (10 18 ×M×S BET ) ··· (6) B: The amount of sodium hydroxide (mol) required to change the pH from 4.0 to 9.0 per 1.5 g of silica particles calculated from V N A : Avogadro's number (pieces / mol) M: Silica particle amount (1.5g) S BET : The specific surface area (m2) of silica particles measured when calculating the average primary particle size 2 / g)

[0057] The method for measuring and calculating the surface silanol group density of the silica particles was based on "GW Ears, Jr., Analytical Chemistry, Vol. 28, No. 12, pp. 1981-1983 (1956)," "Haba Shinichi, Development of Abrasives for Semiconductor Integrated Circuit Processes, Doctoral Dissertation, Kochi University of Technology, pp. 39-45, March 2004," "Patent No. 5967118," and "Patent No. 6047395."

[0058] The surface silanol group density of the silica particles can be set within a desired range by adjusting the conditions for the hydrolysis reaction and condensation reaction of the alkoxysilane.

[0059] The metal impurity content of the silica particles is preferably 5 ppm or less, and more preferably 2 ppm or less.

[0060] When polishing silicon wafers for semiconductor devices, metallic impurities adhere to and contaminate the surface of the workpiece to be polished, adversely affecting the characteristics of the wafer and diffusing into the interior of the wafer, degrading its quality, resulting in a significant decrease in the performance of semiconductor devices manufactured from such wafers. In addition, when metal impurities are present on silica particles, coordination interactions occur between the acidic surface silanol groups and the metal impurities, changing the chemical properties (acidity, etc.) of the surface silanol groups and the three-dimensional environment of the silica particle surface (e.g. the ease of aggregation of silica particles), thereby affecting the polishing rate.

[0061] The metal impurity content of silica particles is measured by inductively coupled plasma mass spectrometry (ICP-MS). Specifically, a silica sol containing 0.4 g of silica particles is accurately weighed, sulfuric acid and hydrofluoric acid are added, and the mixture is heated, dissolved, and evaporated. Pure water is added to the remaining sulfuric acid droplets so that the total amount is exactly 10 g to create a test solution, which is then measured using an inductively coupled plasma mass spectrometry device. The target metals are sodium, potassium, iron, aluminum, calcium, magnesium, zinc, cobalt, chromium, copper, manganese, lead, titanium, silver, and nickel, and the sum of the contents of these metals is the metal impurity content.

[0062] The metal impurity content of the silica particles can be reduced to 5 ppm or less by obtaining the silica particles through hydrolysis and condensation reactions using alkoxysilane as the main raw material. In the method of deionizing alkali silicate such as water glass, sodium and other impurities derived from the raw material remain, making it extremely difficult to reduce the metal impurity content of silica particles to 5 ppm or less.

[0063] Examples of the shape of silica particles include spherical, chain-like, cocoon-like (also called lump-like or peanut-like), irregular shapes (for example, wart-like, bent, branched, etc.) etc. Among these silica particle shapes, when it is desired to reduce the surface roughness or scratches of a polished object, such as a silicon wafer, during polishing, a spherical shape is preferred, and when it is desired to increase the polishing rate of a polished object, such as a silicon wafer, an irregular shape is preferred.

[0064] Silica particles preferably have no pores because they have excellent mechanical strength and storage stability. The presence or absence of pores in the silica particles is confirmed by multipoint BET analysis using adsorption isotherms with nitrogen as the adsorption gas.

[0065] (Method of producing silica sol) The method for producing a silica sol of the present invention includes the method for producing silica particles of the present invention.

[0066] The silica sol may be produced by using the dispersion of silica particles obtained by the method for producing silica particles of the present invention as is, or by removing unnecessary components from the dispersion of silica particles obtained and adding necessary components.

[0067] The silica sol preferably contains silica particles and a dispersion medium. Examples of the dispersion medium in silica sol include water, methanol, ethanol, propanol, isopropanol, ethylene glycol, etc. These dispersion mediums in silica sol may be used alone or in combination of two or more. Among these dispersion mediums in silica sol, water and alcohol are preferred, and water is more preferred, because they have excellent affinity with silica particles.

[0068] The content of silica particles in the silica sol is preferably 3% by mass to 50% by mass, more preferably 4% by mass to 40% by mass, and even more preferably 5% by mass to 30% by mass, based on the total amount of the silica sol (100% by mass). When the content of silica particles in the silica sol is 3% by mass or more, the polishing rate for a polished object such as a silicon wafer is excellent. When the content of silica particles in the silica sol is 50% by mass or less, the aggregation of silica particles in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent.

[0069] The content of the dispersion medium in the silica sol is preferably 50% by mass to 97% by mass, more preferably 60% by mass to 96% by mass, and even more preferably 70% by mass to 95% by mass, based on the total amount of the silica sol (100% by mass). When the content of the dispersion medium in the silica sol is 50% by mass or more, the aggregation of silica particles in the silica sol or polishing composition can be suppressed, and the storage stability of the silica sol or polishing composition is excellent. In addition, when the content of the dispersion medium in the silica sol is 97% by mass or less, the polishing rate for the polished object, typically a silicon wafer, is excellent.

[0070] The content of silica particles and dispersion medium in the silica sol can be set within a desired range by removing unnecessary components from the components in the obtained dispersion of silica particles and adding necessary components.

[0071] In addition to the silica particles and the dispersion medium, the silica sol may contain other components such as an oxidizing agent, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, and an antibacterial and biocide, as necessary, within the range that does not impair the performance of the silica sol. In particular, it is preferable to include an antibacterial biocide in the silica sol, since this provides excellent storage stability of the silica sol.

[0072] Examples of antibacterial biocides include hydrogen peroxide, ammonia, quaternary ammonium hydroxide, quaternary ammonium salt, ethylenediamine, glutaraldehyde, methyl p-hydroxybenzoate, sodium chlorite, etc. These antibacterial biocides may be used alone or in combination of two or more. Among these antibacterial biocides, hydrogen peroxide is preferred because it has excellent affinity with silica sol. Biocides also include those commonly referred to as bactericides.

[0073] The content of the antibacterial biocide in the silica sol is preferably 0.0001% by mass to 10% by mass, more preferably 0.001% by mass to 1% by mass, based on the total amount of the silica sol (100% by mass). When the content of the antibacterial biocide in the silica sol is 0.0001% by mass or more, the storage stability of the silica sol is excellent. When the content of the antibacterial biocide in the silica sol is 10% by mass or less, the inherent performance of the silica sol is not impaired.

[0074] The pH of the silica sol is preferably 6.0 to 8.0, more preferably 6.5 to 7.8. When the pH of the silica sol is 6.0 or more, the dispersion stability is excellent and the aggregation of the silica particles can be suppressed. Also, when the pH of the silica sol is 8.0 or less, dissolution of the silica particles is prevented and the long-term storage stability is excellent. The pH of the silica sol can be adjusted to a desired range by adding a pH adjuster.

[0075] (polishing composition) The silica particles obtained by the method for producing silica particles of the present invention can be suitably used as a polishing composition. The polishing composition preferably contains the above-mentioned silica sol and a water-soluble polymer.

[0076] The water-soluble polymer enhances the wettability of the polishing composition to the object to be polished, such as a silicon wafer. The water-soluble polymer is preferably a polymer having a functional group with high water affinity, and the functional group with high water affinity has a high affinity with the surface silanol group of the silica particles, so that the silica particles and the water-soluble polymer are stably dispersed in the polishing composition in a closer vicinity. Therefore, when polishing the object to be polished, such as a silicon wafer, the effects of the silica particles and the water-soluble polymer function synergistically.

[0077] Examples of the water-soluble polymer include cellulose derivatives, polyvinyl alcohol, polyvinylpyrrolidone, copolymers having a polyvinylpyrrolidone skeleton, and polymers having a polyoxyalkylene structure.

[0078] Examples of cellulose derivatives include hydroxyethyl cellulose, hydrolyzed hydroxyethyl cellulose, hydroxypropyl cellulose, hydroxyethyl methyl cellulose, hydroxypropyl methyl cellulose, methyl cellulose, ethyl cellulose, ethyl hydroxyethyl cellulose, and carboxymethyl cellulose. An example of the copolymer having a polyvinylpyrrolidone skeleton is a graft copolymer of polyvinyl alcohol and polyvinylpyrrolidone. Examples of polymers having a polyoxyalkylene structure include polyoxyethylene, polyoxypropylene, and copolymers of ethylene oxide and propylene oxide.

[0079] These water-soluble polymers may be used alone or in combination of two or more. Among these water-soluble polymers, cellulose derivatives are preferred, and hydroxyethyl cellulose is more preferred, because they have high affinity with the surface silanol groups of silica particles and act synergistically to impart good hydrophilicity to the surface of the polished object.

[0080] The mass average molecular weight of the water-soluble polymer is preferably 1,000 to 3,000,000, more preferably 5,000 to 2,000,000, and even more preferably 10,000 to 1,000,000. When the mass average molecular weight of the water-soluble polymer is 1,000 or more, the hydrophilicity of the polishing composition is improved. When the mass average molecular weight of the water-soluble polymer is 3,000,000 or less, the affinity with silica sol is excellent, and the polishing rate for the object to be polished, typified by a silicon wafer, is excellent.

[0081] The mass average molecular weight of the water-soluble polymer is measured by size exclusion chromatography using a 0.1 mol / L NaCl solution as the mobile phase, in terms of polyethylene oxide.

[0082] The content of the water-soluble polymer in the polishing composition is preferably 0.02% by mass to 10% by mass, more preferably 0.05% by mass to 5% by mass, based on the total amount of the polishing composition (100% by mass). When the content of the water-soluble polymer in the polishing composition is 0.02% by mass or more, the hydrophilicity of the polishing composition is improved. Furthermore, when the content of the water-soluble polymer in the polishing composition is 10% by mass or less, the aggregation of silica particles during preparation of the polishing composition can be suppressed.

[0083] In addition to the silica sol and the water-soluble polymer, the polishing composition may contain other components, such as a basic compound, a polishing accelerator, a surfactant, a hydrophilic compound, a preservative, an antifungal agent, a pH adjuster, a pH buffer, a surfactant, a chelating agent, and an antibacterial and biocide, as necessary, within the range that does not impair the performance of the polishing composition. In particular, it is preferable to include a basic compound in the polishing composition, since it is possible to perform chemical polishing (chemical etching) by applying a chemical action to the surface of an object to be polished, such as a silicon wafer, and because a synergistic effect with the surface silanol groups of the silica particles can improve the polishing speed of an object to be polished, such as a silicon wafer.

[0084] Examples of the basic compound include organic basic compounds, alkali metal hydroxides, alkali metal hydrogen carbonates, alkali metal carbonates, and ammonia. These basic compounds may be used alone or in combination of two or more. Among these basic compounds, ammonia, tetramethylammonium hydroxide, tetraethylammonium hydroxide, ammonium hydrogen carbonate, and ammonium carbonate are preferred because they are highly soluble in water and have excellent affinity with silica particles and water-soluble polymers, and ammonia, tetramethylammonium hydroxide, and tetraethylammonium hydroxide are more preferred, with ammonia being even more preferred.

[0085] The content of the basic compound in the polishing composition is preferably 0.001% by mass to 5% by mass, more preferably 0.01% by mass to 3% by mass, based on the total amount of the polishing composition (100% by mass). When the content of the basic compound in the polishing composition is 0.001% by mass or more, the polishing speed of the object to be polished, such as a silicon wafer, can be improved. In addition, when the content of the basic compound in the polishing composition is 5% by mass or less, the stability of the polishing composition is excellent.

[0086] The pH of the polishing composition is preferably 8.0 to 12.0, more preferably 9.0 to 11.0. When the pH of the polishing composition is 8.0 or more, the aggregation of silica particles in the polishing composition can be suppressed, and the dispersion stability of the polishing composition is excellent. When the pH of the polishing composition is 12.0 or less, the dissolution of silica particles can be suppressed, and the stability of the polishing composition is excellent. The pH of the polishing composition can be adjusted to a desired range by adding a pH adjuster.

[0087] The polishing composition can be obtained by mixing the silica sol obtained by the silica sol manufacturing method of the present invention, a water-soluble polymer, and, as necessary, other components. However, taking into consideration storage and transportation, the composition may be prepared at a high concentration and then diluted with water or the like immediately before polishing.

[0088] (polishing method) The polishing method of the present invention is a method of polishing using a polishing composition containing the silica sol obtained by the method for producing a silica sol of the present invention. As the polishing composition, it is preferable to use the above-mentioned polishing composition. A specific example of the polishing method is a method in which the surface of a silicon wafer is pressed against a polishing pad, the polishing composition of the present invention is dropped onto the polishing pad, and the surface of the silicon wafer is polished.

[0089] (Method of manufacturing semiconductor wafers) The method for producing a semiconductor wafer of the present invention includes the polishing method of the present invention, and the specific polishing method is as described above. Examples of semiconductor wafers include silicon wafers and compound semiconductor wafers.

[0090] (Method of manufacturing semiconductor devices) The method for producing a semiconductor device of the present invention includes the polishing method of the present invention, and the specific polishing method is as described above.

[0091] (Application) The silica particles obtained by the method for producing silica particles of the present invention and the silica sol obtained by the method for producing a silica sol of the present invention can be suitably used for polishing purposes, such as polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing (chemical mechanical polishing) in the planarization process when producing integrated circuits, polishing synthetic quartz glass substrates used for photomasks and liquid crystals, polishing magnetic disk substrates, and the like, and among these, they can be particularly suitably used for polishing silicon wafers and chemical mechanical polishing. EXAMPLES

[0092] The present invention will be described in more detail below using examples. However, the present invention is not limited to the description of the following examples as long as it does not deviate from the gist of the present invention.

[0093] (Measurement of average primary particle size) The dispersions of silica particles obtained in the examples and comparative examples were dried at 150°C, and the specific surface area of ​​the silica particles was measured using an automatic specific surface area measuring device "BELSORP-MR1" (model name, Microtrack BEL Co., Ltd.). The density was calculated to be 2.2 g / cm using the following formula (3). 3 The average primary particle size was calculated. Average primary particle diameter (nm) = 6000 / (specific surface area (m 2 / g) x density (g / cm 3 )) ··· (3)

[0094] (Average secondary particle size) The average secondary particle size of the silica particles in the dispersions obtained in the examples and comparative examples was measured using a dynamic light scattering particle size measurement device "Zetersizer Nano ZS" (model name, manufactured by Malvern Instruments).

[0095] (Calculation of association ratio) The association ratio was calculated from the measured average primary particle size and average secondary particle size using the following formula (5). Association ratio = average secondary particle diameter / average primary particle diameter (5)

[0096] [Example 1] A solution (B) of tetramethoxysilane and methanol mixed at a volume ratio of 2.3:1, and a solution (C) of 3 mass% aqueous ammonia solution were prepared. A reaction vessel equipped with a thermometer, a stirrer, a supply pipe, and a distillation line was charged with a solution (A) of methanol, pure water, and ammonia mixed in advance. The concentration of water in solution (A) was 15 mass%, and the concentration of ammonia in solution (A) was 0.9 mass%. While maintaining the temperature of the reaction solution at 30°C, 100% by volume of solution (B) and 33% by volume of solution (C) were dropped at a constant rate over 297 minutes into 74% by volume of solution (A), to obtain a dispersion of silica particles. The ammonia concentrations in the reaction system at the start and end of the reaction are shown in Table 1. The temperature of the obtained silica particle dispersion was increased to remove methanol and ammonia while adjusting the liquid volume by adding pure water so that the silica particle content was approximately 20 mass %, thereby obtaining a silica particle dispersion with a silica particle content of approximately 20 mass %. The evaluation results of the obtained silica particles are shown in Table 1.

[0097] [Example 2] The same operation as in Example 1 was carried out, except that the ammonia concentration in solution (A) was changed to 1.0 mass%, the holding temperature of the reaction solution was changed to 35°C, the volume ratio of solution (A), solution (B), and solution (C) was changed to 82 volume%:100 volume%:27 volume%, the constant-speed dropping time was changed to 150 minutes, and the ammonia concentration in the reaction system at the start and end of the reaction was changed as shown in Table 1, to obtain a dispersion of silica particles with a silica particle content of approximately 20 mass%. The evaluation results of the obtained silica particles are shown in Table 1.

[0098] [Example 3] Except for changing the holding temperature of the reaction solution to 37°C and the ammonia concentration in the reaction system at the start and end of the reaction as shown in Table 1, the same operation as in Example 2 was carried out to obtain a dispersion of silica particles with a silica particle content of approximately 20 mass%. The evaluation results of the obtained silica particles are shown in Table 1.

[0099] [Example 4] Except for changing the ammonia concentration in solution (A) to 1.1% by mass and the ammonia concentrations in the reaction system at the start and end of the reaction as shown in Table 1, the same operation as in Example 3 was carried out to obtain a dispersion of silica particles with a silica particle content of approximately 20% by mass. The evaluation results of the obtained silica particles are shown in Table 1.

[0100] [Example 5] Except for changing the holding temperature of the reaction solution to 39°C and the ammonia concentration in the reaction system at the start and end of the reaction as shown in Table 1, the same operation as in Example 2 was carried out to obtain a dispersion of silica particles with a silica particle content of approximately 20 mass%. The evaluation results of the obtained silica particles are shown in Table 1.

[0101] [Example 6] The same operation as in Example 1 was carried out, except that the ammonia concentration in solution (A) was changed to 1.2 mass%, the holding temperature of the reaction solution was changed to 40°C, the volume ratio of solution (A), solution (B), and solution (C) was changed to 73 volume%:100 volume%:34 volume%, the constant speed dropping time was changed to 298 minutes, and the ammonia concentration in the reaction system at the start and end of the reaction was changed as shown in Table 1, to obtain a dispersion of silica particles with a silica particle content of approximately 20 mass%. The evaluation results of the obtained silica particles are shown in Table 1.

[0102] [Comparative Example 1] The same operation as in Example 2 was carried out except that the holding temperature of the reaction liquid was changed to 30° C., to obtain a dispersion liquid of silica particles with a silica particle content of about 20 mass %. The evaluation results of the obtained silica particles are shown in Table 1.

[0103] [Comparative Example 2] Except for changing the ammonia concentration in solution (A) to 0.8% by mass and the ammonia concentrations in the reaction system at the start and end of the reaction as shown in Table 1, the same operation as in Example 2 was carried out to obtain a dispersion of silica particles with a silica particle content of approximately 20% by mass. The evaluation results of the obtained silica particles are shown in Table 1.

[0104] [Comparative Example 3] Except for changing the ammonia concentration in solution (A) to 1.1% by mass and the ammonia concentrations in the reaction system at the start and end of the reaction as shown in Table 1, the same operation as in Example 2 was carried out to obtain a dispersion of silica particles with a silica particle content of approximately 20% by mass. The evaluation results of the obtained silica particles are shown in Table 1.

[0105] [Comparative Example 4] Except for changing the ammonia concentration in solution (A) to 0.9% by mass and the ammonia concentrations in the reaction system at the start and end of the reaction as shown in Table 1, the same operation as in Example 3 was carried out to obtain a dispersion of silica particles with a silica particle content of approximately 20% by mass. The evaluation results of the obtained silica particles are shown in Table 1.

[0106] [Comparative Example 5] The same operation as in Example 1 was carried out, except that the ammonia concentration in solution (A) was changed to 1.0 mass%, the holding temperature of the reaction solution was changed to 40°C, the constant rate dropping time was changed to 298 minutes, and the ammonia concentration in the reaction system at the start and end of the reaction was changed as shown in Table 1, to obtain a dispersion of silica particles with a silica particle content of approximately 20 mass%. The evaluation results of the obtained silica particles are shown in Table 1.

[0107] [Comparative Example 6] The same operation as in Example 1 was carried out, except that the ammonia concentration in solution (A) was changed to 1.1% by mass, the holding temperature of the reaction solution was changed to 45°C, the volume ratio of solution (A), solution (B), and solution (C) was changed to 83% by volume:100% by volume:26% by volume, the constant-speed dropping time was changed to 150 minutes, and the ammonia concentration in the reaction system at the start and end of the reaction was changed as shown in Table 1, to obtain a dispersion of silica particles with a silica particle content of approximately 20% by mass. The evaluation results of the obtained silica particles are shown in Table 1.

[0108] [Table 1]

[0109] As can be seen from Table 1, the silica particles produced under conditions satisfying formula (1) as in Examples 1 to 6 had an average primary particle size of 30 nm to 40 nm. On the other hand, the silica particles produced under conditions not satisfying formula (1), such as those in Comparative Examples 1 to 6, did not have an average primary particle size of 30 nm to 40 nm.

[0110] FIG. 1 is a graph summarizing the production conditions of the method for producing silica particles at the start of the reaction in the examples and comparative examples. As can be seen from the graph, in order to achieve an average primary particle size of 30 nm to 40 nm, it is necessary to satisfy formula (1). [Industrial Applicability]

[0111] The silica particles obtained by the method for producing silica particles of the present invention and the silica sol obtained by the method for producing a silica sol of the present invention can be suitably used for polishing purposes, such as polishing semiconductor materials such as silicon wafers, polishing electronic materials such as hard disk substrates, polishing (chemical mechanical polishing) in the planarization process when producing integrated circuits, polishing synthetic quartz glass substrates used for photomasks and liquid crystals, polishing magnetic disk substrates, and the like, and among these, they can be particularly suitably used for polishing silicon wafers and chemical mechanical polishing.

Claims

1. A method for producing silica particles by hydrolysis and condensation of tetraalkoxysilane using an alkali catalyst, comprising the steps of: A method for producing silica particles, in which when the reaction temperature is x°C and the concentration of the alkali catalyst in the reaction system is y% by mass, the following formula (1) is satisfied from the start of the reaction to the end of the reaction, a solution (B) containing a tetraalkoxysilane and a solution (C) containing an alkali catalyst are added to a solution (A) containing an alkali catalyst, and the tetraalkoxysilane is subjected to a hydrolysis reaction and a condensation reaction. 0.03x-0.17≦y≦0.03x+0.03 (1)

2. The method for producing silica particles according to claim 1 , further satisfying the following formula (2) from the start of the reaction to the end of the reaction: 25≦x≦50 (2)

3. The method for producing silica particles according to claim 1 or 2, further satisfying the following formula (3) from the start of the reaction to the end of the reaction: 0.6≦y≦1.5 (3)

4. The method for producing silica particles according to any one of claims 1 to 3, wherein the average primary particle diameter of the silica particles is 30 nm to 40 nm.

5. The method for producing silica particles according to any one of claims 1 to 4, further comprising the following step (1): Step (1): A step of concentrating the reaction solution after the hydrolysis reaction and the condensation reaction and adding a dispersion medium

6. The method for producing silica particles according to claim 5 , further comprising the following step (2): Step (2): A step of subjecting the dispersion of silica particles obtained in step (1) to a pressurized and heated treatment.

7. A method for producing a silica sol, comprising a method for producing silica particles described in any one of claims 1 to 6.

8. The method for producing a silica sol according to claim 7, wherein the concentration of silica particles in the silica sol is 3% by mass to 50% by mass.

9. A polishing method, comprising polishing using a polishing composition containing a silica sol obtained by the method for producing a silica sol described in claim 7 or 8.

10. A method for manufacturing a semiconductor wafer, comprising the polishing method described in claim 9.

11. A method for manufacturing a semiconductor device, comprising the polishing method described in claim 9.

Citation Information

Patent Citations

  • Colored spherical silica particles and production thereof

    JP1995010523A

  • Silica sol and manufacturing method therefor

    JP2005060217A

  • Silica sol and manufacturing method therefor

    JP2005060219A

  • Method for producing silica-based oxide particle

    JP2007070163A

  • Suspension of spherical silica particles, its manufacturing process and spherical silica particles

    JP2007261902A