Film suitable for capacitor applications
A film composed of syndiotactic polystyrene, polyphenylene ether, and amorphous polystyrene resins addresses the issue of poor high-temperature performance in capacitors by enhancing dielectric breakdown strength and insulation, suitable for high-temperature automotive electronics.
Patent Information
- Application Number
- JP2021071060
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-04-20
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2041-04-20
AI Technical Summary
Films containing syndiotactic polystyrene resin exhibit poor dielectric breakdown strength and insulation properties at high temperatures, which are inadequate for high-temperature applications in capacitors, particularly in automotive electronics.
A film composition comprising syndiotactic polystyrene resin, polyphenylene ether resin, and amorphous polystyrene resin, with a specific wide-angle X-ray scattering profile, is developed to enhance dielectric breakdown strength and insulation properties at high temperatures.
The film achieves higher dielectric breakdown strength and insulation properties, making it suitable for high-temperature environments and small-sized, high-capacity capacitors used in electronic and automotive applications.
Smart Images

Figure 0007582042000003 
Figure 0007582042000004 
Figure 0007582042000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a film, etc., and particularly to a film suitable for use in a capacitor. [Background technology]
[0002] Capacitors using resin films have been used in electronic devices, electric devices, etc., for example, as high-voltage capacitors, various switching power supplies, filter capacitors and smoothing capacitors for converters, inverters, etc. Resin film capacitors are also used in inverters and converters that control drive motors for electric vehicles, hybrid vehicles, etc., for which demand has been increasing in recent years.
[0003] Capacitors, particularly automotive capacitors, are increasingly being used in high-temperature environments. For example, in devices (inverters, converters, etc.) that control the drive motors of automobiles, the use of semiconductors with high heat resistance (silicon carbide semiconductors, etc.) has recently increased, and as a result, capacitors used in these devices are also required to have high heat resistance. For this reason, a resin film containing syndiotactic polystyrene is being used as one of the resin films with high heat resistance (Patent Document 1). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] International Publication No. 2016 / 080356 Summary of the Invention [Problem to be solved by the invention]
[0005] In the course of research, the present inventors have focused on heat resistance, particularly on dielectric breakdown strength at high temperatures. In addition, from the viewpoint of reliability as a film for a capacitor, a certain level of insulation is required. However, films containing syndiotactic polystyrene resins have poor dielectric breakdown strength and insulation at high temperatures.
[0006] An object of the present invention is to provide a film having higher dielectric breakdown strength and insulating properties at high temperatures. [Means for solving the problem]
[0007] In the course of research, the inventors have found that it is possible to maintain dielectric breakdown strength and insulation properties at high temperatures at a certain level or higher by adjusting the type of resin to be blended together with the syndiotactic polystyrene resin and the wide-angle X-ray scattering profile of the film. As a result of further intensive research, the inventors have found that a film having a layer containing a syndiotactic polystyrene resin, a polyphenylene ether resin, and an amorphous polystyrene resin, and having a wide-angle X-ray scattering profile (profile 1) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 2) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 3) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 4) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 5) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 6) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 7) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 8) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 9) of 4.9 nm or more, and a film having a wide-angle X-ray scattering profile (profile 1 ... -1 The inventors have found that the above-mentioned problems can be solved by using a film having a peak in the vicinity of the peak. Based on this finding, the inventors have conducted further research and have completed the present invention. That is, the present invention includes the following aspects.
[0008] Item 1. A film, The film has a layer containing a syndiotactic polystyrene-based resin, a polyphenylene ether-based resin, and an amorphous polystyrene-based resin, and The wide-angle X-ray scattering profile (profile 1) of the film was 4.9 nm. -1 having a peak near film.
[0009] Item 2. 4.9 nm of the wide-angle X-ray scattering profile (profile 2) in the TD direction of the film -1 Item 2. The film according to item 1, having a peak in the vicinity.
[0010] Item 3. 8.5 nm of Profile 1 -1 Item 3. The film according to item 1 or 2, having a peak in the vicinity.
[0011] Item 4. 9.9 nm of Profile 1 -1 4. The film according to any one of items 1 to 3, having a peak in the vicinity.
[0012] Item 5. The film according to any one of Items 1 to 4, wherein the content of the syndiotactic polystyrene resin in the film is 62% by mass or more and 93% by mass or less.
[0013] Item 6. The film according to any one of Items 1 to 5, wherein the content of the polyphenylene ether resin in the film is 6% by mass or more and 27% by mass or less.
[0014] Item 7. The film according to any one of Items 1 to 6, wherein the content of the amorphous polystyrene resin in the film is 1% by mass or more and 11% by mass or less.
[0015] Item 8. The film according to any one of Items 1 to 7, wherein the amorphous polystyrene resin is at least one selected from the group consisting of atactic polystyrene resins and styrene-based thermoplastic elastomers.
[0016] Item 9. The film according to any one of Items 1 to 8, wherein the amorphous polystyrene resin is an atactic polystyrene resin.
[0017] Item 10. The film according to any one of items 1 to 9, which is a biaxially stretched film.
[0018] Item 11. The film according to any one of items 1 to 10, which is a single-layer film.
[0019] Item 12. The film according to any one of items 1 to 11, having a thickness of 20 μm or less.
[0020] Item 13. The film according to any one of items 1 to 12, which is for a capacitor.
[0021] Item 14. A metal layer-integrated film comprising the film according to any one of items 1 to 13 and a metal layer laminated on one or both sides of the film.
[0022] Item 15. A capacitor comprising the film according to any one of items 1 to 13 or the metal layer-integrated film according to item 14. [Brief description of the drawings]
[0023] [Figure 1] FIG. 2 is an explanatory diagram of WAXS measurement. [Diagram 2] The wide-angle X-ray scattering profiles (profile 1) of the biaxially stretched films of the Examples and Comparative Examples are shown. [Diagram 3] 1 shows wide-angle X-ray scattering profiles (profile 2) in the TD direction for the biaxially stretched films of the Examples and Comparative Examples. DISCLOSURE OF THEINVENTION Effect of the Invention
[0024] According to the present invention, it is possible to provide a film having higher dielectric breakdown strength and insulating properties at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0025] In this specification, the expressions "contain" and "comprise" include the concepts of "contain", "include", "consist essentially of" and "consist only of".
[0026] When the content of each component in each raw material used is known, the content of each component in the film of the present invention is calculated from the content and the blending ratio of the raw materials. When a raw material with an unknown content is used, the content of each component in the raw material is measured by the method described in "(1-1) Measurement and calculation of the content of each component in a biaxially stretched film" in the Examples, and the content of each component in the film of the present invention is calculated from the content and the blending ratio of the raw materials. When the content of the raw materials is unknown, the content of each component in the film of the present invention is calculated by the method described in "(1-1) Measurement and calculation of the content of each component in a biaxially stretched film" in the Examples.
[0027] 1. Film In one embodiment, the present invention relates to a film, the film having a layer containing a syndiotactic polystyrene-based resin, a polyphenylene ether-based resin, and an amorphous polystyrene-based resin, and a wide-angle X-ray scattering profile (profile 1) of the film of 4.9 nm -1 The present invention relates to a film having a peak in the vicinity of the wavelength of the chromatic aberration (hereinafter, the film may be referred to as "the film of the present invention"). This will be described below.
[0028] The syndiotactic polystyrene resin is not particularly limited as long as it is a polystyrene resin having a syndiotactic structure. The syndiotactic structure means that the stereochemical structure is a syndiotactic structure, that is, that the side chains of phenyl groups and substituted phenyl groups are alternately positioned in the opposite direction to the main chain formed from carbon-carbon bonds. Tacticity is usually measured by nuclear magnetic resonance spectroscopy using carbon isotopes ( 13 The amount of the repeating unit is determined by a C-NMR method, and the amount of the repeating unit can be expressed as the proportion of a plurality of consecutive structural units, for example, a dyad for two units, a triad for three units, a pentad for five units, etc.
[0029] The syndiotactic polystyrene resin has, for example, a racemic diad and a syndiotacticity of, for example, 75% or more, preferably 85% or more.The syndiotactic polystyrene resin has, for example, a racemic pentad and a syndiotacticity of, for example, 30% or more, preferably 50% or more.
[0030] Specific examples of syndiotactic polystyrene resins include polystyrene, poly(alkylstyrene), poly(halogenated styrene), poly(halogenated alkylstyrene), poly(alkoxystyrene), poly(vinyl benzoate ester), hydrogenated polymers thereof, mixtures thereof, and copolymers containing these as main components.
[0031] Examples of poly(alkylstyrene)s include poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tertiary butylstyrene), poly(phenylstyrene), poly(vinylstyrene), poly(vinylnaphthalene), etc. Examples of poly(halogenated styrene)s include poly(chlorostyrene), poly(bromostyrene), poly(fluorostyrene), etc. Examples of poly(halogenated alkylstyrene)s include poly(chloromethylstyrene), etc. Examples of poly(alkoxystyrene)s include poly(methoxystyrene), poly(ethoxystyrene), etc.
[0032] Among these, particularly preferred syndiotactic polystyrene resins include polystyrene, poly(p-methylstyrene), poly(m-methylstyrene), poly(p-tertiary butylstyrene), poly(p-chlorostyrene), poly(m-chlorostyrene), poly(p-fluorostyrene), hydrogenated polystyrene, and styrene-alkylstyrene copolymers such as a copolymer of styrene and p-methylstyrene.
[0033] The molecular weight of the syndiotactic polystyrene resin is not particularly limited. For example, the mass average molecular weight (weight average molecular weight) is, for example, 10,000 to 3,000,000, preferably 50,000 to 1,000,000, more preferably 100,000 to 500,000. The mass average molecular weight is a value measured by gel permeation chromatography at 135°C using 1,2,4-trichlorobenzene as a solvent.
[0034] The melting point of the syndiotactic polystyrene resin is not particularly limited. The melting point is, for example, 200° C. or more and 320° C. or less, preferably 220° C. or more and 280° C. or less. The melting point is a melting peak temperature measured according to JIS K7121:2012.
[0035] The syndiotactic polystyrene resin can be obtained as a commercial product or can be produced by a known method. For example, the syndiotactic polystyrene resin can be obtained as "Zalec" (142ZE, 300ZC, 130ZC, 90ZC) manufactured by Idemitsu Kosan Co., Ltd.
[0036] The syndiotactic polystyrene resins can be used alone or in combination of two or more.
[0037] The content of the syndiotactic polystyrene resin in the film of the present invention is not particularly limited. The syndiotactic polystyrene resin is preferably the component with the highest content in the film of the present invention. The content of the syndiotactic polystyrene resin in the film of the present invention is preferably 62% by mass or more and 93% by mass or less, more preferably 63% by mass or more and 90% by mass or less, even more preferably 63% by mass or more and 87% by mass or less, even more preferably 65.5% by mass or more and 83% by mass or less, particularly preferably 65.5% by mass or more and 79% by mass or less, and especially preferably 67% by mass or more and 73% by mass or less, from the viewpoint of dielectric breakdown strength at high temperatures, insulating properties, etc.
[0038] The polyphenylene ether resin is not particularly limited, and is typically a polymer having a structural unit represented by the following general formula (1). The polyphenylene ether resin may be composed of one type of repeating structural unit, or may contain two or more types of repeating structural units:
[0039] [ka] [In the formula, R 1 , R 2 , R 3 and R 4 are the same or different and each represents a hydrogen atom, a halogen atom, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, an optionally substituted alkylaralkyl group, or an optionally substituted alkoxy group. The halogen atom is not particularly limited, and examples thereof include a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom.
[0040] The alkyl group includes any of linear, branched, and cyclic (preferably linear or branched, more preferably linear). The number of carbon atoms in the alkyl group (in the case of linear or branched) is not particularly limited, and is, for example, 1 to 8. The number of carbon atoms is preferably 1 to 4, more preferably 1 to 3, even more preferably 1 to 2, and even more preferably 1. The number of carbon atoms in the alkyl group (in the case of cyclic) is not particularly limited, and is, for example, 3 to 7, and preferably 4 to 6. Specific examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a tert-butyl group, a sec-butyl group, an n-pentyl group, a neopentyl group, an n-hexyl group, a 3-methylpentyl group, an n-heptyl group, and an n-octyl group.
[0041] The alkenyl group includes both linear and branched (preferably linear) alkenyl groups. The number of carbon atoms in the alkenyl group is not particularly limited and is, for example, 2 to 8. The number of carbon atoms is preferably 2 to 4. Specific examples of the alkenyl group include a vinyl group, an allyl group, a 1-propenyl group, an isopropenyl group, a butenyl group, a pentenyl group, and a hexenyl group.
[0042] The alkynyl group includes both linear and branched (preferably linear) alkynyl groups. The number of carbon atoms in the alkenyl group is not particularly limited and is, for example, 2 to 8. The number of carbon atoms is preferably 2 to 4. Specific examples of the alkynyl group include an ethynyl group, a propynyl group (e.g., a 1-propynyl group, a 2-propynyl group (propargyl group)), a butynyl group, a pentynyl group, and a hexynyl group.
[0043] The aryl group is not particularly limited, but preferably has 6 to 12 carbon atoms, more preferably 6 to 12 carbon atoms, and even more preferably 6 to 8 carbon atoms. The aryl group may be either monocyclic or polycyclic (e.g., bicyclic, tricyclic, etc.), but is preferably monocyclic. Specific examples of the aryl group include a phenyl group, a naphthyl group, a biphenyl group, a pentalenyl group, an indenyl group, an anthranyl group, a tetracenyl group, a pentacenyl group, a pyrenyl group, a perylenyl group, a fluorenyl group, and a phenanthryl group, and preferably a phenyl group.
[0044] The aralkyl group is not particularly limited, and examples thereof include aralkyl groups in which the hydrogen atoms (for example, 1 to 3, preferably 1 hydrogen atom) of the alkyl group are substituted with the aryl group. Specific examples of the aralkyl group include a benzyl group and a phenethyl group.
[0045] The alkylaryl group is not particularly limited, and examples thereof include alkylaryl groups in which the hydrogen atoms (for example, 1 to 3, preferably 1 hydrogen atom) of the aryl group are substituted with the alkyl group. Specific examples of the alkylaryl group include a tolyl group and a xylyl group.
[0046] The alkylaralkyl group is not particularly limited, and examples thereof include alkylaralkyl groups in which a hydrogen atom (for example, 1 to 3, preferably 1 hydrogen atom) on the aromatic ring of the above-mentioned aralkyl group is substituted with the above-mentioned alkyl group.
[0047] The alkoxy group is not particularly limited, and examples thereof include linear or branched (preferably linear) alkoxy groups having 1 to 8 carbon atoms, preferably 1 to 4, more preferably 1 to 3, even more preferably 1 to 2, and still more preferably 1. Examples of the alkoxy group include a methoxy group, an ethoxy group, an n-propoxy group, an isopropoxy group, an n-butoxy group, an isobutoxy group, a sec-butoxy group, and a t-butoxy group.
[0048] Examples of the substituents of the alkyl group, alkenyl group, alkynyl group, aryl group, aralkyl group, alkylaryl group, alkylaralkyl group, alkoxy group, etc. include halogen atoms, hydroxy groups, etc. The number of the substituents is not particularly limited and is, for example, 0 to 3, preferably 0 to 1, and more preferably 0.
[0049] In a preferred embodiment of the present invention, R 1 , R 2 , R 3 and R 4 are the same or different and each is a hydrogen atom, a halogen atom, or an optionally substituted alkyl group (preferably an unsubstituted alkyl group). 2 and R 3 is preferably a hydrogen atom, and R 1 and R 4 is preferably a group other than a hydrogen atom.
[0050] Specific examples of polyphenylene ether resins include poly(2,3-dimethyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-chloromethyl-1,4-phenylene ether), poly(2-methyl-6-hydroxyethyl-1,4-phenylene ether), poly(2-methyl-6-n-butyl-1,4-phenylene ether), poly(2-ethyl-6-isopropyl-1,4-phenylene ether), Poly(2-ethyl-6-n-propyl-1,4-phenylene ether), Poly(2,3,6-trimethyl-1,4-phenylene ether), Poly(2-(4'-methylphenyl)-1,4-phenylene ether), Poly(2-bromo-6-phenyl-1,4-phenylene ether), Poly(2-methyl-6-phenyl-1,4-phenylene ether), Poly(2-phenyl-1,4-phenylene ether) ether), poly(2-chloro-1,4-phenylene ether), poly(2-methyl-1,4-phenylene ether), poly(2-chloro-6-ethyl-1,4-phenylene ether), poly(2-chloro-6-bromo-1,4-phenylene ether), poly(2,6-di-n-propyl-1,4-phenylene ether), poly(2-methyl-6-isopropyl-1,4-phenylene ether), poly(2-chloro-6- Examples of the polyphenylene ether include homopolymers such as poly(methyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2,6-dibromo-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), poly(2,6-diethyl-1,4-phenylene ether), and poly(2,6-dimethyl-1,4-phenylene ether), and copolymers thereof. In addition, those modified with a modifier such as maleic anhydride or fumaric acid are also preferably used. Furthermore, copolymers obtained by graft copolymerization or block copolymerization of vinyl aromatic compounds such as styrene with the above polyphenylene ethers are also used. Among these, poly(2,6-dimethyl-1,4-phenylene ether) is particularly preferred.
[0051] The number average molecular weight of the polyphenylene ether resin is not particularly limited, but from the viewpoint of extrusion moldability and continuous stretchability, it is preferably from 10,000 to 100,000, and more preferably from 15,000 to 50,000. The number average molecular weight is determined by converting the molecular weight value measured by the GPS method into the value of polystyrene.
[0052] The polyphenylene ether resin can be obtained as a commercial product or can be produced by a known method. For example, the polyphenylene ether resin can be preferably used with the Iupiace (registered trademark) series (e.g., Iupiace (registered trademark) PX100L, PX100F) manufactured by Mitsubishi Engineering Plastics Corporation or the Zylon (registered trademark) series (e.g., Zylon (registered trademark) S201A) manufactured by Asahi Kasei Corporation.
[0053] The polyphenylene ether resins may be used alone or in combination of two or more.
[0054] The content of the polyphenylene ether resin in the film of the present invention is not particularly limited. -1 Near 8.5 nm -1 Near, 9.9 nm -1 From the viewpoint of improving the peak height near the surface of the organic solvent and improving the dielectric breakdown strength and insulating properties (volume resistivity) at high temperatures, the content is preferably 6 mass% or more and 27 mass% or less, more preferably 6 mass% or more and 26 mass% or less, even more preferably 10 mass% or more and 26 mass% or less, still more preferably 15 mass% or more and 26 mass% or less, particularly preferably 15 mass% or more and 24 mass% or less, and especially preferably 17 mass% or more and 24 mass% or less.
[0055] The amorphous polystyrene resin is not particularly limited as long as it contains a styrene monomer unit and is amorphous, and known resins can be used. Examples of the amorphous polystyrene resin include atactic polystyrene resins and styrene thermoplastic elastomers.
[0056] The atactic polystyrene resin is not particularly limited as long as it is an amorphous resin having a main chain of polystyrene with an atactic structure. As the atactic polystyrene resin, it is preferable that 90% or more, more preferably 95% or more of the structural units constituting the main chain are styrene and / or styrene having a substituent on the aromatic ring.
[0057] Atactic structure means that the phenyl groups and substituted phenyl groups, which are side chains of the main chain formed by carbon-carbon bonds, have a random three-dimensional structure. Tacticity is usually measured by nuclear magnetic resonance spectroscopy using isotopes of carbon ( 13 The amount of syndiotactic polystyrene is quantified by C-NMR method, and can be expressed by the proportion of consecutive multiple structural units, for example, dyad when there are two, triad when there are three, pentad when there are five, etc. Atactic polystyrene resins are, for example, racemic dyads, and have a syndiotacticity of, for example, less than 75%, preferably 65% or less. Also, atactic polystyrene resins are, for example, racemic pentads, and have a syndiotacticity of, for example, less than 30%, preferably 25% or less.
[0058] Specific examples of atactic polystyrene resins include polystyrene, poly(alkylstyrene), poly(halogenated styrene), poly(halogenated alkylstyrene), poly(alkoxystyrene), and mixtures thereof, or copolymers containing these as main components.
[0059] Examples of poly(alkylstyrene)s include poly(methylstyrene), poly(ethylstyrene), poly(isopropylstyrene), poly(tertiary butylstyrene), poly(phenylstyrene), poly(vinylstyrene), poly(vinylnaphthalene), etc. Examples of poly(halogenated styrene)s include poly(chlorostyrene), poly(bromostyrene), poly(fluorostyrene), etc. Examples of poly(halogenated alkylstyrene)s include poly(chloromethylstyrene), etc. Examples of poly(alkoxystyrene)s include poly(methoxystyrene), poly(ethoxystyrene), etc.
[0060] Among these, particularly preferred atactic polystyrene resins include polystyrene, poly(p-methylstyrene), poly(m-methylstyrene), poly(p-tertiary butylstyrene), poly(p-chlorostyrene), poly(m-chlorostyrene), poly(p-fluorostyrene), hydrogenated polystyrene, and styrene-alkylstyrene copolymers such as a copolymer of styrene and p-methylstyrene.
[0061] The melt mass flow rate of the atactic polystyrene resin is not particularly limited and is, for example, 0.5 to 20 g / 10 min. The melt mass flow rate is preferably 2 to 15 g / 10 min, more preferably 4 to 12 g / 10 min, and even more preferably 6 to 9 g / 10 min. The melt mass flow rate is measured according to ISO1133 (conditions: 200°C, load 5 kgf, test piece is pellet).
[0062] Atactic polystyrene resins can be obtained as commercial products or can be produced by known methods. As commercial products of atactic polystyrene resins, resins generally called general-purpose polystyrene (GPPS) can be suitably used, and are available as, for example, "PSJ-Polystyrene GPPS" (HF77, 679, SGP10, etc.) manufactured by PS Japan Co., Ltd.
[0063] The atactic polystyrene resins may be used alone or in combination of two or more.
[0064] The styrene-based thermoplastic elastomer is not particularly limited, and known ones can be used. The styrene-based thermoplastic elastomer usually has a styrene monomer polymer block (Hb) as a hard segment and a conjugated diene compound polymer block or its hydrogenated block (Sb) as a soft segment. The structure of this styrene-based thermoplastic elastomer may be a diblock structure represented by Hb-Sb, a triblock structure represented by Hb-Sb-Hb or Sb-Hb-Sb, a tetrablock structure represented by Hb-Sb-Hb-Sb, or a polyblock structure in which a total of five or more Hbs and Sbs are linearly bonded.
[0065] The styrene-based monomer used in the styrene monomer polymer block (Hb) is not particularly limited, and examples thereof include styrene and its derivatives. Specifically, examples thereof include styrenes such as styrene, α-methylstyrene, 2-methylstyrene, 4-methylstyrene, 4-propylstyrene, 4-t-butylstyrene, 4-cyclohexylstyrene, 4-dodecylstyrene, 2-ethyl-4-benzylstyrene, 4-(phenylbutyl)styrene, 2,4,6-trimethylstyrene, monofluorostyrene, difluorostyrene, monochlorostyrene, dichlorostyrene, methoxystyrene, and t-butoxystyrene; vinyl group-containing aromatic compounds such as vinyl naphthalenes such as 1-vinylnaphthalene and 2-vinylnaphthalene; and vinylene group-containing aromatic compounds such as indene and acenaphthylene. Among these, styrene is preferred. The styrene-based monomer may be one type only, or two or more types.
[0066] The conjugated diene compound used in the conjugated diene compound polymer block (Sb) is not particularly limited. Examples of such conjugated diene compounds include butadiene, isoprene, 2,3-dimethylbutadiene, pentadiene, and hexadiene. Among these, butadiene is preferred. The conjugated diene compound may be one type or two or more types. Furthermore, other comonomers such as ethylene, propylene, butylene, and styrene may be copolymerized. The conjugated diene compound polymer block (Sb) may be a hydrogenated product that is partially or completely hydrogenated.
[0067] Specific examples of styrene-based thermoplastic elastomers include styrene-isoprene diblock copolymers (SI), styrene-butadiene diblock copolymers (SB), styrene-isoprene-styrene triblock copolymers (SIS), styrene-butadiene / isoprene-styrene triblock copolymers (SB / IS), and styrene-butadiene-styrene triblock copolymers (SBS), as well as hydrogenated products thereof. Examples of hydrogenated products include styrene-ethylene-butylene-styrene copolymers (SEBS), styrene-ethylene-propylene-styrene copolymers (SEPS), styrene-ethylene-ethylene-propylene-styrene copolymers (SEEPS), and styrene-butylene-butadiene-styrene copolymers (SBBS). Among these, hydrogenated products are preferred, and SEBS is particularly preferred.
[0068] The content of the styrene monomer polymer block unit (Hb) in the styrene-based thermoplastic elastomer is not particularly limited, but is, for example, 5% by mass or more and 80% by mass or less, preferably 25% by mass or more and 80% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 35% by mass or more and 60% by mass or less.
[0069] The content of the conjugated diene compound polymer block and / or its hydrogenated block (Sb) (preferably ethylene-butylene) in the styrene-based thermoplastic elastomer is not particularly limited, but is, for example, 20% by mass or more and 95% by mass or less, preferably 20% by mass or more and 75% by mass or less, more preferably 30% by mass or more and 70% by mass or less, and even more preferably 40% by mass or more and 65% by mass or less.
[0070] The melt mass flow rate of the styrene-based thermoplastic elastomer is not particularly limited and is, for example, 0.5 to 15 g / 10 min. The melt mass flow rate is preferably 1 to 10 g / 10 min, more preferably 1.5 to 5 g / 10 min, and further preferably 2 to 4 g / 10 min. The melt mass flow rate is measured according to JIS K 7210:1999 (conditions: 230°C, load 2.16 kg).
[0071] The styrene-based thermoplastic elastomer can be obtained as a commercial product or can be produced by a known method. As the styrene-based thermoplastic elastomer, for example, the Tuftec (registered trademark) series (e.g., H1517, etc.) manufactured by Asahi Kasei Corporation, and the Septon (registered trademark) series (e.g., 8000 series) manufactured by Kuraray Co., Ltd. can be suitably used.
[0072] The styrene-based thermoplastic elastomers can be used alone or in combination of two or more.
[0073] The amorphous polystyrene resins may be used alone or in combination of two or more.
[0074] The content of the amorphous polystyrene-based resin is not particularly limited, but it is preferable that the content of the resin in the film of the present invention is lower than that of the syndiotactic polystyrene-based resin (preferably lower than each of the syndiotactic polystyrene-based resin and the polyphenylene ether-based resin).
[0075] The content of the amorphous polystyrene resin in the film of the present invention is not particularly limited. -1 Near 8.5 nm -1 Near, 9.9 nm -1 From the viewpoint of improving the peak height near the surface of the organic solvent and improving the dielectric breakdown strength and insulating properties (volume resistivity) at high temperatures, the content is preferably 1 mass% or more and 11 mass% or less, more preferably 2 mass% or more and 11 mass% or less, even more preferably 3 mass% or more and 11 mass% or less, still more preferably 4 mass% or more and 11 mass% or less, particularly preferably 5 mass% or more and 11 mass% or less, especially more preferably 6 mass% or more and 10.5 mass% or less, especially more preferably 6.5 mass% or more and 10.0 mass% or less, and especially still more preferably 7 mass% or more and 9.5 mass% or less.
[0076] The wide-angle X-ray scattering profile (profile 1) of the film of the present invention is 4.9 nm -1 In profile 1, from the viewpoint of dielectric breakdown strength and insulation properties at high temperatures, the peak is around 8.5 nm. -1 Near and / or 9.9 nm -1 It is preferable that the peak is around 8.5 nm. -1 Near and 9.9 nm -1 It is preferable to have a peak in the vicinity.
[0077] From the viewpoint of dielectric breakdown strength and insulating properties at high temperatures, the wide-angle X-ray scattering profile (profile 2) in the TD direction of the film of the present invention is 4.9 nm -1 From the same viewpoint, it is preferable that the peak is in the vicinity of 8.5 nm. -1 Near and / or 9.9 nm -1 It is preferable that the peak is around 8.5 nm. -1 Near and 9.9 nm -1 It is preferable to have a peak in the vicinity.
[0078] These peaks shown in wide-angle X-ray measurements are presumed to originate from the α crystals of syndiotactic polystyrene resins, as referenced in Polymer, Vol. 135 (2018) pp. 103-110.
[0079] The presence or absence of each of the above peaks in Profile 1 and Profile 2 is determined as follows.
[0080] WAXS measurements WAXS measurements are performed using the NANO-Viewer X-ray scattering measurement device manufactured by Rigaku Corporation (Figure 1). A sample is cut out from the film so that two directions (an arbitrary direction (direction 1) and a direction perpendicular to direction 1 (direction 2)) (in the case of a biaxially stretched film, direction 1 is the MD direction and direction 2 is the TD direction) can be identified, and the sample is set in the sample cell with direction 1 as the vertical direction and direction 2 as the horizontal direction, and measurements are performed under the following conditions. If the thickness of the sample is less than 8 μm, the sample is stacked after aligning the directions (direction 1, direction 2) to obtain a total thickness of 8 to 20 μm. Detector: 2D detector PILATUS-100K Sample-detector distance: 72.67mm Wavelength (λ): 0.154nm (CuKα line) Current strength: 40kV, 30mA Mode of use: NANO-Viewer extended mode Measurement location: Any 3 locations on the sample Exposure time: 600 seconds for each of three locations Wavenumber (q) region: 2~20[nm -1 ].
[0081] The two-dimensional scattering image obtained by the above WAXS measurement is subjected to the following data processing using the data analysis program FIT2D manufactured by the European Synchrotron Radiation Research Facility (ESRF).
[0082] Wide angle X-ray scattering profile The two-dimensional scattering image obtained by WAXS measurement is circularly averaged to convert the data into one dimension, and the WAXS profile is obtained by subtracting 0.8 times the values measured and calculated in the same manner except that no sample is set as dark current correction for the detector and empty cell scattering correction, to obtain a one-dimensional wide-angle X-ray scattering profile (profile 1). The horizontal axis of the profile is the wave number q (nm -1 ).
[0083] Wide-angle X-ray scattering profile in the TD direction For the two-dimensional scattering image obtained by WAXS measurement, the positive direction of the X-axis is set as 0°, and the region from 150 to 210° is cut out to calculate the sector average and convert the data into one dimension. For the obtained WAXS profile, the dark current correction of the detector and the empty cell scattering correction are subtracted by multiplying the values measured and calculated in the same manner except that no sample is set by 0.8 to obtain a one-dimensional wide-angle X-ray scattering profile in the TD direction (profile 2).
[0084] Peak Height 4.9 nm in Profile 1 and Profile 2, respectively -1 Near 8.5 nm -1 Near and 9.9 nm -1 The presence or absence of a peak in each vicinity is judged as follows.
[0085] The following (2), (3), and (4) are extracted from the measured values. (2) 4.9±0.3 nm -1 The maximum value in the range of measurements (3) 8.5±0.3 nm -1 The maximum value in the range of measurements (5) 9.9±0.3 nm -1 The maximum value in the range of measurements The following (1) and (4) are calculated as the average value of the two most recent measurement values that sandwich the values below. (1) 4.5 nm -1 Value of (4) 9.3 nm -1 Value of Calculate the peak height using the following formula. 4.9 nm -1 Nearby: (2)-(1) above 8.5 nm -1 Nearby: (3)-(4) above 9.9 nm -1 Nearby: (5)-(4) above.
[0086] (Evaluation Criteria) Regarding Profile 1, A peak is judged to be present when the peak height is 6 or more. The peak height is preferably 8 or more, more preferably 10 or more, particularly preferably 15 or more, and even more preferably 17 or more.
[0087] Regarding Profile 2, A peak is judged to have a peak when the peak height is 10 or more. The peak height is preferably 13 or more, more preferably 15 or more, particularly preferably 19 or more, and even more preferably 22 or more.
[0088] By producing a film so that the peak height is equal to or greater than the above-mentioned value, the dielectric breakdown strength and insulating properties (volume resistivity) are improved, which is preferable. The peak height is adjusted by changing the state of the crystals of syndiotactic polystyrene generated in the film by adjusting the above-mentioned resin mixing ratio, stretching temperature, etc.
[0089] The film of the present invention may contain other resins, additives, etc. in addition to the above components.
[0090] The other resin is not particularly limited. When the film of the present invention contains other resin, the content of the other resin is, for example, 10% by mass or less, 5% by mass or less, 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less. Examples of the other resin include polypropylene resins.
[0091] The additives are not particularly limited, and may be, for example, components that can be blended into a resin film (particularly a resin film for a capacitor), specifically, for example, antioxidants, chlorine absorbents, lubricants, plasticizers, flame retardants, colorants, inorganic particles, etc. When the film of the present invention contains additives, the content of the additives in the film of the present invention is, for example, 10% by mass or less, 5% by mass or less, 1% by mass or less, 0.5% by mass or less, or 0.1% by mass or less. The film of the present invention is a resin composition, and the resin composition can be produced by a method including a step of forming a resin composition (sometimes referred to as the "resin composition of the present invention" in this specification) containing a syndiotactic polystyrene resin, a polyphenylene ether resin, and an amorphous polystyrene resin into a film. For example, the resin composition of the present invention can be extruded into a film (the film of the present invention obtained by this method is sometimes referred to as the "unstretched film of the present invention") and biaxially stretching the unstretched film of the present invention (the film of the present invention obtained by this method is sometimes referred to as the "biaxially stretched film of the present invention") to obtain the film of the present invention. Details of the production method will be described below. The above peak in the wide-angle X-ray scattering profile can be obtained by adjusting the production conditions, particularly the resin composition, the longitudinal stretching temperature, the transverse stretching temperature, and the heat setting temperature after the transverse stretching.
[0092] The composition of the resin composition of the present invention is the same as that of the film of the present invention.
[0093] The state of the resin composition of the present invention is not particularly limited. Examples of the state of the resin composition of the present invention include a solid state (e.g., an aggregate of resin masses (the size of which is not particularly limited, and which also includes pellets and powders)) and a liquid state (e.g., a molten mixture of each component).
[0094] The resin composition of the present invention preferably contains a blend resin (including a polymer alloy) obtained by blending some or all of the components in a molten state.
[0095] The resin composition of the present invention preferably contains modified polyphenylene ether as a blend resin containing polyphenylene ether resin. The modified polyphenylene ether is a resin obtained by melt-kneading (polymer alloying) a polyphenylene ether resin and another resin. The modified polyphenylene ether is preferable because it has excellent melt flowability and extrusion moldability.
[0096] Examples of other resins constituting the modified polyphenylene ether include polystyrene-based resins, styrene-based thermoplastic elastomers, polypropylene-based resins, polyphenylene sulfide-based resins, polyamide-based resins, etc. Among these, polystyrene-based resins (preferably amorphous polystyrene-based resins, more preferably atactic polystyrene-based resins and / or styrene-based thermoplastic elastomers) are preferred.
[0097] The composition ratio of each resin constituting the modified polyphenylene ether is not particularly limited, and can be appropriately adjusted according to the type of resin.The content of polyphenylene ether-based resin in the modified polyphenylene ether is, for example, 40% by mass or more and 95% by mass or less, preferably 50% by mass or more and 90% by mass or less, more preferably 60% by mass or more and 85% by mass or less, even more preferably 65% by mass or more and 80% by mass or less, and even more preferably 65% by mass or more and 75% by mass or less, and the content of other resin in the modified polyphenylene ether is, for example, 5% by mass or more and 60% by mass or less, preferably 10% by mass or more and 50% by mass or less, more preferably 15% by mass or more and 40% by mass or less, even more preferably 20% by mass or more and 35% by mass or less, and even more preferably 25% by mass or more and 35% by mass or less.
[0098] The modified polyphenylene ether can be obtained as a commercial product or can be produced by a known method. As commercial products, for example, Iupiace (registered trademark) series (e.g. Iupiace (registered trademark) AH91) manufactured by Mitsubishi Engineering Plastics Corporation, Zylon (registered trademark) series (e.g. Zylon (registered trademark) 1000H) manufactured by Asahi Kasei Corporation, and Noryl (registered trademark) series manufactured by SHPP Japan LLC can be suitably used.
[0099] The modified polyphenylene ethers may be used alone or in combination of two or more.
[0100] The content of the modified polyphenylene ether is not particularly limited as long as the content of each component in the resin composition of the present invention is a predetermined amount. The content of the modified polyphenylene ether in the resin composition of the present invention is, for example, 5% by mass or more and 38% by mass or less, preferably 8% by mass or more and 35% by mass or less, more preferably 15% by mass or more and 35% by mass or less, and even more preferably 25% by mass or more and 35% by mass or less.
[0101] The blended resin can be obtained by melt-kneading each component. As a method of melt-kneading, a melt kneader of a single screw type, a twin screw type, or a multi-screw type having more than one screw can be used, and among them, a twin screw type melt kneader is preferably used because of its good kneading properties. In the case of the twin screw type, both the same-rotation and counter-rotation kneading types can be used, but the same-rotation direction is preferable from the viewpoint of suppressing resin deterioration. The ratio of the diameter and length of the screw (L / D) is preferably 20 or more, more preferably 25 or more, and even more preferably 28 or more. There is no upper limit to L / D, but from the viewpoint of suppressing resin deterioration, it is 100 or less, preferably 80 or less.
[0102] The temperature during melt kneading is preferably 250° C. to 350° C., more preferably 280° C. to 330° C., in order to balance the suppression of resin deterioration and dispersibility. During melt kneading, it is preferable to purge the kneader with an inert gas such as nitrogen in order to suppress the deterioration of the resin.
[0103] The method of extruding the resin composition of the present invention is not particularly limited, and a known extrusion molding method can be adopted. For example, the solid resin composition of the present invention supplied to an extruder is heated to a molten state, filtered through a filter, extruded into a film using a T-die, and solidified by contact with a cooling roll set to a predetermined surface temperature. After being molded into a film, the unstretched film of the present invention can be made into a roll by winding it around a core.
[0104] The resin composition of the present invention is preferably mixed before melting. The mixing method is not particularly limited, but examples thereof include a method in which a plurality of resin lumps (pellets, etc.) are dry-blended using a mixer or the like.
[0105] The resin composition of the present invention is preferably dried before melting. The drying conditions are not particularly limited. The drying temperature is not particularly limited, but is, for example, 70 to 150°C, preferably 80 to 130°C. The drying time can be appropriately adjusted depending on the drying temperature, and is, for example, 2 to 50 hours, preferably 3 to 20 hours. The moisture content after drying is, for example, 1 to 200 ppm, preferably 5 to 100 ppm.
[0106] The resin composition of the present invention is usually melted in an extruder. Examples of the extruder include a single screw type, a twin screw type, and a multi-screw type having three or more screws. In the case of two or more screws, the screw rotation type may be, for example, a same-direction rotation or a counter-direction rotation. The melting temperature is preferably 280 to 320°C, preferably 285 to 315°C, and more preferably 290 to 310°C. In order to suppress deterioration during kneading and mixing of the resin, it is preferable to purge the kneader with an inert gas such as nitrogen.
[0107] The resin composition of the present invention in a molten state may be filtered.
[0108] The temperature during extrusion through a T-die is not particularly limited, but is preferably 280 to 320°C, preferably 285 to 315°C, and more preferably 290 to 310°C.
[0109] The method of contacting the film-like material extruded from the T-die with a cooling roll to solidify it is not particularly limited, and examples thereof include air knife, electrostatic pinning, elastic roll nip, metal roll nip, elastic metal roll nip, etc. The surface temperature of the cooling roll is not particularly limited, and is, for example, 40 to 100°C, preferably 45 to 90°C.
[0110] The thickness of the unstretched film of the present invention is not particularly limited, but is, for example, 10 to 200 μm.
[0111] The method for biaxially stretching the unstretched film of the present invention is not particularly limited, and a known biaxial stretching method, such as a batch-type stretching method or a roll-type stretching method, can be adopted. In one embodiment of the present invention, a batch-type method can be adopted. For example, the unstretched film of the present invention is heated to a predetermined temperature (longitudinal stretching temperature) and stretched longitudinally in the machine direction (MD), then stretched transversely in the width direction (TD) at a predetermined temperature (transverse stretching temperature), followed by heat setting at a predetermined temperature, relaxing in the width direction, and cooling.
[0112] The longitudinal stretching temperature is preferably 130 to 175° C., more preferably 135 to 170° C., further preferably 142 to 168° C., and even further preferably 147 to 165° C. The longitudinal stretching ratio is preferably 2 to 4 times, more preferably 2.3 to 3.5 times, and further preferably 2.6 to 3.5 times.
[0113] The transverse stretching temperature is preferably 130 to 175° C., more preferably 135 to 170° C., even more preferably 142 to 168° C., and still more preferably 147 to 165° C. The transverse stretching ratio is preferably 2.5 to 4.5 times, more preferably 2.9 to 4.3 times, even more preferably 3.2 to 4.1 times, and still more preferably 3.2 to 3.9 times.
[0114] The transverse stretching temperature (preferably the transverse stretching temperature and the longitudinal stretching temperature) is preferably determined based on the T value, which serves as an index. The T value is a value calculated by the formula 1: T = content of polyphenylene ether resin in the film (mass%) x 1.2 + 132. The transverse stretching temperature (preferably the transverse stretching temperature and the longitudinal stretching temperature) is preferably within the range of T-5°C to T+10°C, more preferably within the range of T-4°C to T+8°C, even more preferably within the range of T-3°C to T+6°C, still more preferably within the range of T-2°C to T+4°C, and particularly preferably within the range of T-1.2°C to T+2°C. By setting the stretching temperature within this range, it is possible to obtain a 4.9 nm in wide-angle X-ray scattering profile. -1 Near 8.5 nm -1 Near, 9.9 nm -1 This is preferable from the viewpoint of improving the peak height near the surface of the film and improving the dielectric breakdown strength and insulating properties (volume resistivity) at high temperatures.
[0115] The heat fixing temperature is preferably 200 to 260° C., more preferably 205 to 245° C. The heat fixing time is preferably 5 to 50 seconds, more preferably 9.2 to 35 seconds. By setting the heat fixing temperature and time within this range, -1 Near 8.5 nm -1 Near, 9.9 nm -1 This is preferable from the viewpoint of improving the peak height near the surface of the film and improving the dielectric breakdown strength and insulating properties (volume resistivity) at high temperatures.
[0116] The relaxation (relaxation) rate in the width direction is preferably 2 to 6%.
[0117] The thickness of the film of the present invention is not particularly limited, but is, for example, 30 μm or less, 20 μm or less. The thickness is preferably thinner from the viewpoint of reducing the volume of the capacitor and increasing the electrostatic capacitance. From this viewpoint, the thickness is preferably 10 μm or less, more preferably 9.5 μm or less, even more preferably 8 μm or less, even more preferably 6 μm or less, particularly preferably 5 μm or less, especially preferably 4 μm or less, and particularly preferably 3 μm or less. In addition, from the viewpoint of further increasing the dielectric breakdown strength and slit processing suitability and further improving the continuous film forming property, the thickness is, for example, 1 μm or more, preferably 1.5 μm or more, more preferably 1.8 μm or more, even more preferably 2 μm or more, even more preferably 2.3 μm or more, and particularly preferably 2.5 μm or more. The range of the thickness of the film of the present invention can be set by arbitrarily combining the above upper and lower limits.
[0118] The thickness of the film of the present invention, such as the unstretched film of the present invention or the biaxially stretched film of the present invention, is measured using an outside micrometer (high-precision digital micrometer MDH-25MB, manufactured by Mitutoyo Corporation) in accordance with JIS K 7130:1999 Method A.
[0119] The layer structure of the film of the present invention is not particularly limited. The film of the present invention may be a single layer consisting of one layer, or may be a plurality of layers having the same or different compositions. The film of the present invention is preferably a film consisting of one or more film-like molded layers of the resin composition of the present invention, and more preferably a single-layer film (a film consisting of one film-like molded layer of the resin composition of the present invention).
[0120] The film of the present invention has high dielectric breakdown strength at high temperatures. The dielectric breakdown strength is measured according to the method described in the Examples below. The dielectric breakdown strength of the film of the present invention in a 150° C. environment is preferably 350 V. DC / μm or more, preferably 370V DC / μm or more, more preferably 380V DC / μm or more, even more preferably 390V DC / μm or more, and especially preferably 400V DC / μm or more, and more preferably 410V DC / μm or more, and more preferably 415V DC / μm or more. There is no particular upper limit. For example, DC / μm, 620V DC / μm, 600V DC / μm, 580V DC / μm, 560V DC / μm, 540V DC / μm, 520V DC / μm, or 500V DC / μm.
[0121] The film of the present invention has high insulating properties. The insulating properties are evaluated by measuring the volume resistivity according to the method in the Examples described later. The volume resistivity of the film of the present invention is preferably 1×10 15 Ω·cm or more, preferably 3×10 15 Ω cm or more, more preferably 1×10 16 Ω cm or more, more preferably 2×10 16 The upper limit is not particularly limited, but is 1×10 18 Ω cm or 1×10 17 Ω cm.
[0122] The use of the film of the present invention is not particularly limited. The film of the present invention can be used, for example, as a heat-resistant film by taking advantage of its heat resistance. In addition, the film of the present invention (particularly the biaxially stretched film of the present invention) can be suitably used as a film for a capacitor that can exhibit its characteristics. In particular, the film of the invention (particularly the biaxially stretched film of the present invention) can be extremely suitably used in a capacitor that is used in a high-temperature environment, is small, and has a high capacity (for example, 5 μF or more, preferably 10 μF or more, and more preferably 20 μF or more).
[0123] 2. Metal layer integrated film In one aspect, the present invention relates to a metal layer-integrated film (sometimes referred to as the "metal layer-integrated film of the present invention" in this specification) having the film of the present invention and a metal layer laminated on one or both sides of the film. This will be described below.
[0124] The film of the present invention can have a metal layer (e.g., an electrode) attached to one or both sides thereof in order to process it into a capacitor. Such a metal layer is not particularly limited as long as the capacitor intended by the present invention can be obtained, but since a capacitor is required to be small and lightweight, it is preferable to form (laminated) a metal layer directly on one or both sides of the film of the present invention to form a metal layer-integrated film.
[0125] Examples of methods for laminating a metal layer on the surface of the film of the present invention include vacuum plating such as metal vapor deposition and sputtering, coating and drying of a metal-containing paste, and pressure bonding of metal foil or metal powder. Among these, in order to meet the further demand for smaller and lighter capacitors, vacuum vapor deposition and sputtering are preferred, and from the viewpoints of productivity and economy, vacuum vapor deposition is preferred. Examples of vacuum vapor deposition include the crucible method and the wire method, but are not particularly limited as long as the capacitor intended by the present invention can be obtained, and the most suitable method can be selected as appropriate.
[0126] The metal used in the metal layer may be, for example, a single metal such as zinc, lead, silver, chromium, aluminum, copper, or nickel, a mixture of two or more of these, or an alloy of these. In consideration of the environment, economy, and capacitor performance, zinc and aluminum are preferred.
[0127] From the viewpoint of the electrical characteristics of the capacitor, the film resistance of the metal layer is preferably about 1 to 100 Ω / □. Within this range, a higher value is desirable from the viewpoint of self-healing characteristics, and the film resistance is more preferably 5 Ω / □ or more, and even more preferably 10 Ω / □ or more. Furthermore, from the viewpoint of safety as a capacitor, the film resistance is more preferably 50 Ω / □ or less, and even more preferably 30 Ω / □ or less.
[0128] When forming an electrode (metal vapor deposition film) by vacuum vapor deposition, the film resistance can be measured during vapor deposition, for example, by a four-terminal method known to those skilled in the art. The film resistance of the metal vapor deposition film can be adjusted, for example, by adjusting the output of the evaporation source to adjust the amount of evaporation.
[0129] When forming a metal deposition film on one side of the film, a certain width is not deposited from one end of the film to form an insulating margin so that the film will become a capacitor when rolled up. Furthermore, in order to strengthen the bond between the metal layer integrated film and the metallikon electrode, it is preferable to form a heavy edge structure on the end opposite the insulating margin, and the film resistance of the heavy edge is usually about 1 to 8 Ω / □, and preferably about 1 to 5 Ω / □. The thickness of the metal film of the heavy edge is not particularly limited, but is preferably 1 to 200 nm.
[0130] There is no particular restriction on the deposition pattern (margin pattern) of the metal deposition film to be formed, but from the viewpoint of improving the characteristics such as the safety of the capacitor, it is preferable to form the fuse as a pattern including a so-called special margin such as a fishnet pattern, a T-margin pattern, etc. When the metal deposition film is formed on at least one side of the film of the present invention in a deposition pattern including a special margin, the safety of the obtained capacitor is improved, and it is also effective and preferable from the viewpoint of preventing the destruction and short circuit of the capacitor.
[0131] The margin can be formed by any known method without any restriction, such as a tape method in which masking is performed with tape during deposition, or an oil method in which masking is performed by applying oil.
[0132] A protective layer may be provided on the metal layer-integrated film of the present invention for the purpose of physical protection of the metal vapor deposition film, prevention of moisture absorption, prevention of oxidation, etc. As the protective layer, silicone oil, fluorine oil, etc. can be preferably used.
[0133] The metal layer-integrated film of the present invention can be processed into the capacitor of the present invention described below. The metal layer-integrated film of the present invention can also be used as a barrier film against oxygen and other gases.
[0134] 3. Capacitor In one aspect, the present invention relates to a capacitor (sometimes referred to as "the capacitor of the present invention" in this specification) including the film of the present invention or the metal layer-integrated film of the present invention. This will be described below.
[0135] In such capacitors, the film of the present invention can be used as a dielectric film for a capacitor by, for example, (i) using the above-mentioned metal layer integrated film, or (ii) laminating the film of the present invention having no electrodes with another conductor (for example, metal foil, the film of the present invention having one or both sides metallized, paper having one or both sides metallized, other plastic films, etc.).
[0136] In the process of producing a capacitor, a film is wound. For example, two pairs of the metal layer-integrated films of the present invention are overlapped and wound so that the metal films in the metal layer-integrated film of the present invention and the film of the present invention are alternately stacked, and further, the insulating margins are on opposite sides. In this case, it is preferable to stack the two pairs of the metal layer-integrated films of the present invention with a shift of 1 to 2 mm. The winding machine used is not particularly limited, and for example, an automatic winding machine 3KAW-N2 type manufactured by Kaito Seisakusho Co., Ltd. can be used.
[0137] The film winding process is not limited to the above method, and other methods may be used, for example, a double-sided vapor-deposited film of the present invention (in which case the heavy edges are arranged at the opposite ends of the front and back surfaces) and a non-vapor-deposited film of the present invention (2 to 3 mm narrower than the double-sided vapor-deposited film of the present invention) may be alternately laminated and wound.
[0138] When producing a flat capacitor, after winding, the resulting wound product is usually pressed. Pressing promotes tightening of the capacitor and element formation. From the viewpoint of controlling and stabilizing the interlayer gap, the optimum pressure to be applied varies depending on the thickness of the film of the present invention, and is generally 2 to 20 kg / cm. 2 It is.
[0139] Next, metal is sprayed onto both end faces of the winding to provide metallikon electrodes, thereby completing a capacitor.
[0140] The capacitor is further subjected to a predetermined heat treatment. That is, in the present invention, the process includes a step of subjecting the capacitor to a heat treatment (hereinafter, sometimes referred to as "thermal aging"). The heat treatment temperature is not particularly limited, but is, for example, 80 to 210°C. The method of subjecting the capacitor to heat treatment may be appropriately selected from known methods including, for example, a method using a thermostatic bath under a vacuum atmosphere or a method using high-frequency induction heating. The time for which the heat treatment is performed is preferably 30 minutes or more, more preferably 10 hours or more, from the viewpoint of obtaining mechanical and thermal stability, but more preferably 20 hours or less, from the viewpoint of preventing molding defects such as heat wrinkles and molding. The effect of thermal aging is obtained by performing the heat treatment. Specifically, the gap between the films constituting the capacitor based on the metal layer-integrated film of the present invention is reduced, and corona discharge is suppressed. In addition, the internal structure of the film of the present invention is changed. When the wide-angle X-ray scattering profile of the film after the heat treatment is measured, the wave number q is 4.9 nm -1 Near 8.5 nm -1 Near, 9.9 nm -1 The peak height around 5.6 nm is increased, confirming the growth of crystals. -1Near 10.0 nm -1 Near 11.1 nm -1 Near 12.7 nm -1 A peak may be observed around 5.6 nm. -1 Near 10.0 nm -1 Near 11.1 nm -1 Near 12.7 nm -1 The peak around is presumed to be derived from δ crystals of syndiotactic polystyrene resin, referring to Polymer, Vol. 135 (2018) pp. 103-110 and the like. δ crystals are generally crystal structures that are easily observed when crystallized from a solvent such as toluene, but in the film of the present invention, it is presumed that the polyphenylene ether resin and the amorphous polystyrene resin grow δ crystals. As a result of the growth of these crystals, it is presumed that the dielectric breakdown voltage and insulating properties (volume resistivity) are improved, and the voltage resistance of the capacitor is improved.
[0141] If the heat treatment temperature is lower than the predetermined temperature or the aging time is short, the above-mentioned effects of heat aging cannot be sufficiently obtained, whereas if the heat treatment temperature is higher than the predetermined temperature or the aging time is long, the film of the present invention may suffer from thermal decomposition, oxidative degradation, or the like.
[0142] Lead wires are usually welded to the metallikon electrodes of the heat-aged capacitor. In order to impart weather resistance, particularly to prevent deterioration due to humidity, the capacitor is preferably encapsulated in a case and potted with epoxy resin.
[0143] The capacitor of the present invention using the film of the present invention can be suitably used in high-temperature environments, and can be a small-sized capacitor with a high capacity (for example, 5 μF or more, preferably 10 μF or more, and more preferably 20 μF or more). Therefore, the capacitor of the present invention can be used as a high-voltage capacitor, a filter capacitor and a smoothing capacitor for various switching power sources, converters, inverters, etc., which are used in electronic devices and electric devices. In addition, the capacitor of the present invention can be suitably used as an inverter capacitor, a converter capacitor, etc., which control the drive motor of electric vehicles and hybrid vehicles, which have become increasingly popular in recent years. EXAMPLES
[0144] The present invention will be described in detail below based on examples, but the present invention is not limited to these examples.
[0145] (1)Measurement method The various measurement methods are as follows.
[0146] (1-1) Measurement and calculation of the content of each component in biaxially stretched film The content of each component in the biaxially stretched films of the Examples and Comparative Examples was calculated from the content and the blending ratio of the raw materials when the content of each component in each raw material used was known. When a modified polyphenylene ether with an unknown content of the component was used as the raw material, the content of each component in the raw material was measured by the following method, and calculated from the content and the blending ratio of the raw materials. When the content of the raw material was unknown, the content of each component in the biaxially stretched film was measured by the following method.
[0147] The raw material or biaxially stretched film was dissolved in 1,1,2,2-tetrachloroethane-d2 to prepare the measurement sample. 1 H-NMR measurement and 13 C-NMR measurements were performed. 1 H-NMR measurement, and 13 The conditions for C-NMR measurement are shown below.
[0148] 13 In the C-NMR measurement, the components were identified based on the measured signals. 1 The integrated intensity ratio (molar ratio) per H atom of each component was determined from the signals measured by H-NMR measurement, and converted to a weight ratio using the formula weight of each component to determine the contents of the polyphenylene ether component, styrene component, and ethylene-butylene component.
[0149] Here, the content of the polyphenylene ether resin in the biaxially stretched film is equal to the content of the polyphenylene ether component determined as above.
[0150] [ 1 H-NMR measurement] Measurement device: AVANCE III-600 with Cryo Probe manufactured by Bruker Biospin Measurement frequency: 600MHz Measurement solvent: 1,1,2,2-tetrachloroethane-d2 Measurement temperature: 300K Chemical shift standard: 1,1,2,2-tetrachloroethane-d2( 1 H;6.00ppm) [ 13 C-NMR measurement] Measurement device: AVANCE III-600 with Cryo Probe manufactured by Bruker Biospin Measurement frequency: 150MHz Measurement solvent: 1,1,2,2-tetrachloroethane-d2 Measurement temperature: 300K Chemical shift standard: 1,1,2,2-tetrachloroethane-d2( 13 C;73.78 ppm).
[0151] (1-2) Wide-angle X-ray scattering analysis For the biaxially stretched films of the Examples and Comparative Examples, the presence or absence of a peak at a predetermined position in the wide-angle X-ray scattering profile was judged as follows.
[0152] (1-2-1) WAXS measurement WAXS measurements were performed using the NANO-Viewer X-ray scattering measurement device manufactured by Rigaku Corporation (Figure 1). A sample was cut out from the film so that two directions (MD direction (direction 1) and TD direction (direction 2)) could be identified, and it was set in the sample cell with direction 1 as the vertical direction and direction 2 as the horizontal direction, and measurements were performed under the following conditions. Detector: 2D detector PILATUS-100K Sample-detector distance: 72.67mm Wavelength (λ): 0.154nm (CuKα line) Current strength: 40kV, 30mA Mode of use: NANO-Viewer extended mode Measurement location: Any 3 locations on the sample Exposure time: 600 seconds for each of three locations Wavenumber (q) region: 2~20[nm -1 ].
[0153] The two-dimensional scattering image obtained by the above WAXS measurement was subjected to the following data processing using the data analysis program FIT2D manufactured by the European Synchrotron Radiation Research Facility (ESRF).
[0154] (1-2-2) Wide-angle X-ray scattering profile The two-dimensional scattering image obtained by WAXS measurement was subjected to a circular average calculation to convert the data into one dimension, and the WAXS profile was obtained. The dark current correction for the detector and the empty cell scattering correction were calculated in the same manner except that no sample was set, and multiplied by 0.8. This was used to obtain a one-dimensional wide-angle X-ray scattering profile (profile 1). The horizontal axis of the profile is the wave number q (nm -1 ).
[0155] (1-2-3) Wide-angle X-ray scattering profile in the TD direction The two-dimensional scattering image obtained by WAXS measurement was cut out from the region of 150 to 210° with the positive direction of the X-axis set as 0°, and the sector average was calculated to convert the data into one dimension. The dark current correction of the detector and the empty cell scattering correction of the obtained WAXS profile were subtracted from the values measured and calculated in the same manner except that no sample was set, multiplied by 0.8, to obtain a one-dimensional wide-angle X-ray scattering profile in the TD direction (profile 2).
[0156] (1-2-4) Peak presence / absence determination 4.9 nm in Profile 1 and Profile 2, respectively -1 Near 8.5 nm -1 Near and 9.9 nm -1 The presence or absence of each nearby peak was judged as follows.
[0157] The following (2), (3), and (4) were extracted from the measured values. (2) 4.9±0.3 nm -1 The maximum value in the range of measurements (3) 8.5±0.3 nm -1 The maximum value in the range of measurements (5) 9.9±0.3 nm -1 The maximum value in the range of measurements The following (1) and (4) were calculated as the average value of the two most recent measured values that sandwiched the values below. (1) 4.5 nm -1 Value of (4) 9.3 nm -1 Value of The peak height was calculated using the following formula. 4.9 nm -1 Nearby: (2)-(1) above 8.5 nm -1 Nearby: (3)-(4) above 9.9 nm -1 Nearby: (5)-(4) above.
[0158] (Evaluation Criteria) Regarding Profile 1, A peak was determined to have a height of 6 or more.
[0159] Regarding Profile 2, A peak was determined to have a height of 10 or more.
[0160] (2) Preparation of resin composition and film (2-1)Resin used (A) Syndiotactic polystyrene resin (sPS) A1: Zarec (registered trademark) 90ZC manufactured by Idemitsu Kosan Co., Ltd. (BC) Modified polyphenylene ether resin BC1: Modified polyphenylene ether resin (manufactured by SHPP Japan LLC, a mixed resin of polyphenylene ether resin and amorphous polystyrene).
[0161] (2-2) Method for Producing Resin Composition and Film In the following production process, the T value, which is an index of the longitudinal stretching temperature and the transverse stretching temperature, was calculated according to the formula 1: T=content of polyphenylene ether resin in film (mass %)×1.2+132.
[0162] [Example 1] [Preparation of unstretched sheet] A1 and BC1 were mixed so that the content of each component was as shown in Table 1, and the resulting resin composition was placed in a vacuum oven and dried at 120°C for 5 hours. The dried raw material was placed in a twin-screw type film-forming machine (2D30W2 manufactured by Toyo Seiki Seisakusho Co., Ltd.) together with nitrogen gas. After melting at a cylinder temperature of 300°C, it was extruded from a T-die at 300°C. The molten resin was solidified by contacting a mirror-finished metal roll (cooling roll) with a silicon rubber roll with a surface temperature of 50°C using a silicon rubber roll with a surface temperature of 50°C, and formed into a film to obtain an unstretched film. The extrusion amount and take-up speed were adjusted so that the thickness of the center of the unstretched film was about 98 μm and the thickness after stretching was the target value.
[0163] [Preparation of stretched film] An unstretched sheet was introduced into an oven of a batch-type stretching machine (Bruckner batch-type biaxial stretching machine KARO IV) set at 140 ° C (longitudinal stretching temperature) and preheated for 125 seconds. Then, in the same oven, the unstretched sheet was longitudinally stretched in the machine direction (MD) at a stretching speed of 100% / sec to a ratio of 2.8 times. Then, in the same oven, it was preheated at 140 ° C (transverse stretching temperature) for 30 seconds, and then in the same oven, it was transversely stretched in the width direction of the unstretched sheet at a stretching speed of 100% / sec to a ratio of 3.4 times. Next, the stretched film was introduced into an oven set at 210 ° C and heated (heat treated) for 10 seconds, and then the transverse stretching ratio was relaxed to 3.2 times. The heat-treated film was discharged out of the oven and cooled at room temperature for 10 seconds to obtain a biaxially stretched film. The extrusion amount and take-up speed were finely adjusted so that the thickness of the film was the thickness in Table 1.
[0164] [Example 2] A biaxially stretched film was obtained in the same manner as in Example 1, except that a resin composition obtained by mixing A1 and BC1 so that each component had a content shown in Table 1 was used, and the stretching conditions were the conditions shown in Table 1.
[0165] [Example 3] A biaxially stretched film was obtained in the same manner as in Example 1, except that a resin composition obtained by mixing A1 and BC1 so that each component had a content shown in Table 1 was used, and the stretching conditions were the conditions shown in Table 1.
[0166] [Comparative Example 1] A biaxially stretched film was obtained in the same manner as in Example 1, except that A1 was used instead of the resin composition and the stretching conditions were as shown in Table 1.
[0167] [Comparative Example 2] A biaxially stretched film was obtained in the same manner as in Example 1, except that a resin composition obtained by mixing A1 and BC1 so that each component had a content shown in Table 1 was used, and the stretching conditions were the conditions shown in Table 1.
[0168] (3) Measurement and evaluation of film characteristics (3-1) Measurement of dielectric breakdown strength at high temperatures The dielectric breakdown strength of the biaxially stretched films of the examples and comparative examples at high temperatures was evaluated as follows. A measuring device conforming to JIS C2151:2006, 17.2.2 (flat electrode method) was prepared. However, as the lower electrode, conductive rubber (E12S10 manufactured by Seiwa Electric Co., Ltd.) was used instead of the elastic body described in JIS C2151:2006, 17.2.2, and aluminum foil was not wrapped around it. The measurement environment was a forced circulation oven set at a temperature of 150°C, and the electrodes and films were used after being adjusted in the oven for 30 minutes. A DC power source was used, and the voltage was increased from 0V at a rate of 100V / sec, and the moment the current value exceeded 5mA was regarded as the moment of breakdown. The dielectric breakdown voltage was measured 20 times, and the dielectric breakdown voltage value V DC Divide by the film thickness (μm), and the top two and bottom two points are excluded from the 20 calculation results to obtain the average of 16 points, which is the dielectric breakdown strength (V DC / μm).
[0169] (3-2) Measurement of volume resistivity The volume resistivity of the biaxially stretched films of the Examples and Comparative Examples was measured as follows.
[0170] <Volume resistivity> <Measurement of volume resistivity ρV> The specific measurement procedure for volume resistivity is described below, but unless otherwise specified, the measurement conditions were based on JIS C 2139-3-1:2018 as follows.
[0171] First, place the volume resistivity measuring jig (hereinafter simply referred to as the jig) in a thermostatic chamber at 40°C. The jig was configured as follows. A DC power supply and a DC ammeter were connected to the jig.
[0172] <Volume resistivity measuring tool> Main electrode (50mm diameter) Counter electrode (diameter 85 mm) An annular guard electrode (outer diameter 80 mm, inner diameter 70 mm) surrounding the main electrode Each electrode was made of gold-plated copper, and conductive rubber was attached to the surface that came into contact with the sample. The conductive rubber used was EC-60BL (W300) manufactured by Shin-Etsu Silicone Co., Ltd., and the glossy side of the conductive rubber was attached so that it was in contact with the gold-plated copper.
[0173] Next, the resin films of the examples and comparative examples (hereinafter also referred to as samples) were set in a jig in a thermostatic chamber. Specifically, the main electrode and the guard electrode were attached to one side of the sample, and the counter electrode was attached to the other side, and the sample and each electrode were attached to each other under a load of 5 kgf. Then, the sample was left to stand for 30 minutes.
[0174] Next, a voltage was applied to the sample using a DC power source so that the potential gradient was 100 V / μm.
[0175] After the voltage was applied, the current value was read one minute later, and the volume resistivity was calculated using the following formula: The voltage was applied using a Keithley 2290-10 (DC power source), and the current value was measured using a Keithley 2635B (DC ammeter).
[0176] Volume resistivity = [(effective electrode area) x (applied voltage)] / [(sample thickness) x (current value)] Here, the effective electrode area was calculated by the following formula.
[0177] (Effective electrode area) = Pi × [[[(main electrode diameter) + (guard electrode inner diameter)] / 2] / 2] 2 This was repeated three times, and the arithmetic average value calculated to one significant digit was taken as the volume resistivity (Ω·cm).
[0178] (4) Measurement and evaluation results The measurement results of the content of each component in the biaxially stretched films of the Examples and Comparative Examples, the stretching conditions during film production, the thickness of the films, and the measurement and evaluation results of the film characteristics are shown in Table 1. Furthermore, the profile 1 measured above is shown in Figure 2, and the profile 2 is shown in Figure 3.
[0179] [Table 1]
[0180] From the above, a film is provided, the film having a layer containing a syndiotactic polystyrene-based resin, a polyphenylene ether-based resin, and an amorphous polystyrene-based resin, and the wide-angle X-ray scattering profile (profile 1) of the film is within 4.9 nm -1 It was found that the films (Examples 1 to 3) having a peak around this range had high dielectric breakdown strength at high temperatures and good insulating properties.
Claims
1. A film, the film has a layer containing a syndiotactic polystyrene-based resin, a polyphenylene ether-based resin, and an amorphous polystyrene-based resin; The content of resins other than the resin is 0% by mass or more and 5% by mass or less, and The wide-angle X-ray scattering profile (profile 1) of the film was 4.9 nm -1 having a peak near film.
2. The wide-angle X-ray scattering profile (profile 2) of the film in the TD direction was 4.9 nm. -1 The film of claim 1 having a peak near
3. Profile 1: 8.5 nm -1 3. The film of claim 1, having a peak near
4. Profile 1: 9.9 nm -1 The film according to any one of claims 1 to 3, having a peak in the vicinity.
5. The film according to any one of claims 1 to 4, wherein the content of the syndiotactic polystyrene resin in the film is 62% by mass or more and 93% by mass or less.
6. The film according to any one of claims 1 to 5, wherein the content of the polyphenylene ether resin in the film is 6% by mass or more and 27% by mass or less.
7. The film according to any one of claims 1 to 6, wherein the content of the amorphous polystyrene resin in the film is 1% by mass or more and 11% by mass or less.
8. The film according to any one of claims 1 to 7, wherein the amorphous polystyrene resin is at least one selected from the group consisting of atactic polystyrene resins and styrene-based thermoplastic elastomers.
9. The film according to any one of claims 1 to 8, wherein the amorphous polystyrene resin is an atactic polystyrene resin.
10. The film according to any one of claims 1 to 9, which is a biaxially stretched film.
11. The film of any one of claims 1 to 10, which is a monolayer film.
12. The film according to any one of claims 1 to 11, having a thickness of 20 µm or less.
13. The film according to any one of claims 1 to 12, which is for use in a capacitor.
14. A metal layer-integrated film comprising the film according to any one of claims 1 to 13 and a metal layer laminated on one or both sides of the film.
15. A capacitor comprising the film according to any one of claims 1 to 13 or the metal layer-integrated film according to claim 14.
Citation Information
Patent Citations
Biaxial oriented film for electric insulation
JP2014088530A
Alignment film