Low Dielectric Laminate
The laminate addresses the dispersibility issue of fillers in adhesive layers by optimizing filler distribution, achieving enhanced adhesive and dielectric properties for high-frequency signal transmission.
Patent Information
- Application Number
- JP2021519686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-04
- Filing Date
- 2020-12-02
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2040-12-02
AI Technical Summary
Existing laminates for flexible printed circuit boards do not adequately address the dispersibility of fillers in the adhesive layer, leading to insufficient linear expansion and inadequate dielectric properties, which are crucial for high-frequency signal transmission.
A laminate structure with a specific distribution of fillers in the adhesive layer, where the number of fillers closer to the metal base material surface is higher than those closer to the resin base material surface, using a composition of acid-modified polyolefin, epoxy resin, and optional oligophenylene ether and polycarbodiimide, ensuring optimal dispersibility and adhesion.
The laminate exhibits excellent adhesive properties, dielectric properties, and linear expansion, providing superior dimensional stability and low dielectric constants and loss tangents for high-frequency applications.
Smart Images

Figure 0007582182000007 
Figure 0007582182000001 
Figure 0007582182000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate having low dielectric properties, and more particularly to a laminate that can be used for flexible printed wiring boards, coverlay films, and bonding sheets.
[0002] Flexible printed circuit boards (FPCs) have excellent flexibility and can accommodate the multi-functionality and miniaturization of personal computers and smartphones, and are therefore widely used to incorporate electronic circuit boards into narrow and complex interiors. In recent years, electronic devices have become smaller, lighter, more dense, and more powerful, and these trends have led to increasingly higher requirements for the performance of wiring boards (electronic circuit boards). In particular, with the increase in the speed of transmission signals in FPCs, signals are becoming increasingly high frequency, and as a result, there is an increasing demand for low dielectric properties (low dielectric constant, low dielectric loss tangent) in the high frequency range for FPCs. Patent Document 1 discloses a coverlay film (laminate) having a thermosetting adhesive layer made of a thermosetting adhesive composition containing a polyolefin resin, a carbodiimide resin, a multifunctional epoxy resin, and a filler. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-127501 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]
[0004] However, the coverlay film (laminate) described in Patent Document 1 contains a filler, but does not take into consideration the dispersibility of the filler in the adhesive layer, so the linear expansion properties of the laminate are insufficient. The present invention has been made in consideration of the above problems, and has an object to provide a laminate having excellent adhesive properties, dielectric properties, and linear expansion properties of the adhesive layer. [Means for solving the problem]
[0005] A laminate in which a metal substrate, an adhesive layer, and a resin substrate are laminated in this order, The adhesive layer contains a filler (A) and a cured product of an acid-modified polyolefin (B) and an epoxy resin (C), A laminate in which, in a cross section of the adhesive layer in a direction perpendicular to the surface of the laminate, the number a1 of the filler (A) contained in a region from the midpoint to the surface of the metal substrate is greater than the number b1 of the filler (A) contained in a region from the midpoint to the surface of the resin substrate.
[0006] The ratio of a1 to b1 is preferably a1 / b1=less than 100 / more than 0 to more than 50 / less than 50.
[0007] The filler (A) is preferably one or more selected from the group consisting of phosphorus-containing flame-retardant fillers, aluminum hydroxide, silica, titanium oxide, and carbon black. Furthermore, the adhesive layer preferably contains an oligophenylene ether (D) and / or a polycarbodiimide (E) having a number average molecular weight of 3000 or less in the cured product component.
[0008] The relative dielectric constant (ε c ) is preferably 3.0 or less, and the dielectric tangent (tan δ) is preferably 0.02 or less.
[0009] A printed wiring board comprising the laminate as a component. Effect of the Invention
[0010] The laminate of the present invention has an appropriately set dispersibility of the filler in the adhesive layer, and therefore has excellent adhesion and dielectric properties in the adhesive layer, as well as excellent linear expansion properties, making it possible to provide a laminate with good dimensional stability. [Brief description of the drawings]
[0011] [Figure 1]FIG. 1 is a cross-sectional view of the laminate in a direction perpendicular to the surface. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, the present invention will be described in more detail based on the following embodiment. However, the present invention is not limited to the following embodiment, and it is possible to carry out the present invention by making appropriate modifications within the scope of the above and below described purpose, and all of these modifications are included in the technical scope of the present invention.
[0013] <Laminate> The laminate of the present invention is formed by laminating a metal substrate, an adhesive layer, and a resin substrate in this order. The metal substrate and the adhesive layer may be directly laminated, or another substrate (layer) may be laminated therebetween. It is preferable that the metal substrate and the adhesive layer are directly laminated. Also, the adhesive layer and the resin substrate may be directly laminated, or another substrate (layer) may be laminated therebetween. It is preferable that the adhesive layer and the resin substrate are directly laminated. That is, it is preferable that the metal substrate, the adhesive layer, and the resin substrate are directly laminated (three layers: metal substrate / adhesive layer / resin substrate).
[0014] In addition, another substrate may be laminated on the laminate via an adhesive layer, for example, a four-layer structure of adhesive layer / metal substrate / adhesive layer / resin substrate, a four-layer structure of metal substrate / adhesive layer / resin substrate / adhesive layer, or a five-layer structure of adhesive layer / metal substrate / adhesive layer / resin substrate / adhesive layer.
[0015] An example of a laminate is shown in Fig. 1. The laminate 10 in Fig. 1 is formed by laminating a metal substrate 1, an adhesive layer 3, and a resin substrate 2 in this order, and the adhesive layer 3 includes a region 3a (hereinafter also referred to as adhesive layer 3a) closer to the surface of the metal substrate and a region 3b (hereinafter also referred to as adhesive layer 3b) closer to the surface of the resin substrate.
[0016] The method for producing the laminate is not particularly limited, but can be performed, for example, by the following method. First, an adhesive composition a containing a filler (A), an acid-modified polyolefin (B) and an epoxy resin (C) is applied to the surface of the metal substrate 1, and dried to produce an adhesive layer 3a. Then, an adhesive composition b containing less filler (A) than the adhesive composition a is applied to the surface, and dried to produce an adhesive layer 3b. Then, a resin substrate 2 is laminated and heat-treated (cured) to obtain a laminate. Conversely, the adhesive composition b is applied to the surface of the resin substrate 2, dried to produce an adhesive layer 3b, and then an adhesive composition a is applied and dried to produce an adhesive layer 3a, and then the metal substrate 1 is laminated and heat-treated (cured) to obtain the laminate.
[0017] When the laminate is used as a component of a printed wiring board, it is preferable to form a conductor circuit thereon.
[0018] <Adhesive layer> The adhesive layer of the present invention contains a filler (A) and a cured product of an acid-modified polyolefin (B) and an epoxy resin (C), and the number a1 of the filler (A) in the adhesive layer 3a is greater than the number b1 of the filler (A) in the adhesive layer 3b.
[0019] The ratio (a1 / b1) of the number a1 of the adhesive layers 3a to the number b1 of the adhesive layers 3b is preferably less than 100 / more than 0 to more than 50 / less than 50. In order to improve the linear expansion properties, the ratio is more preferably 99 / 1 to 51 / 49, even more preferably 98 / 2 to 52 / 48, still more preferably 97 / 3 to 53 / 47, particularly preferably 96 / 4 to 54 / 46, and most preferably 95 / 5 to 55 / 45.
[0020] The adhesive layer 3a and the adhesive layer 3b are arranged such that the adhesive layer 3a is located on the metal substrate 1 side and the adhesive layer 3b is located on the resin substrate 2 side from the midpoint of the length (film thickness of the adhesive layer 3) in the direction perpendicular to the surface of the laminate. The midpoint here refers to the intermediate position between the surface of the adhesive layer that contacts the metal substrate 1 and the surface that contacts the resin substrate 2, and refers to the position that is 50% from the metal substrate 1 and 50% from the resin substrate 2 when the film thickness of the adhesive layer is 100%. That is, the adhesive layer 3a is located within 50% of the adhesive layer 3 from the metal substrate 1. The adhesive layer 3b is located within 50% of the adhesive layer 3 from the resin substrate 2. The boundary between the adhesive layer 3a and the adhesive layer 3b may be clear, or may be indistinct and integrated.
[0021] The film thickness (thickness) of the adhesive layer is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 15 μm or more, and particularly preferably 20 μm or more, because the adhesive strength is good. Also, the film thickness (thickness) of the adhesive layer is preferably 200 μm or less, more preferably 150 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm, because the adhesive layer can be given flexibility.
[0022] The number of fillers (A) can be measured using an electron microscope. Specifically, the laminate is cut in a direction perpendicular to its surface, and the number of fillers (A) contained in the adhesive layer 3a region and the adhesive layer 3b region on the cut surface is visually counted. The number of fillers (A) contained in the adhesive layer is proportional to the content of fillers (A) contained in the adhesive composition applied to the resin substrate or metal substrate. Note that fillers (A) with a major axis of less than 15 nm are not counted because their linear expansion effect is weak.
[0023] <Filler (A)> The filler (A) used in the present invention (hereinafter, simply referred to as component (A)) is not particularly limited as long as it has a low linear expansion effect when its dispersibility in the adhesive layer is appropriately set. Among them, it is preferable to use one or more types selected from the group consisting of phosphorus-containing flame-retardant fillers, aluminum hydroxide, silica, titanium oxide, and carbon black.
[0024] The phosphorus-containing flame-retardant filler is not particularly limited as long as it contains a phosphorus atom in its structure. Examples of the phosphorus-containing flame-retardant filler include phosphinic acid derivatives and phosphazene compounds, with phosphinic acid derivatives being preferred and phenanthrene-type phosphinic acid derivatives being more preferred. Examples of phenanthrene-type phosphinic acid derivatives include 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (Sanko Co., Ltd., trade name: HCA), 10-benzyl-10-hydro-9-oxa-10-phosphaphenanthrene-10-oxide (Sanko Co., Ltd., trade name: BCA), 10-(2,5-dihydroxyphenyl)-10-H-9-oxa-10-phosphaphenanthrene-10-oxide (Sanko Co., Ltd., trade name: HCA-HQ), and finely ground 10-(2,5-dihydroxyphenyl)-10-H-9-oxa-10-phosphaphenanthrene-10-oxide (Sanko Co., Ltd., trade name: HCA-HQ-HS). These can be used alone or in combination of two or more. Among them, HCA-HQ-HS is preferred.
[0025] Commercially available aluminum hydroxide products include Hidilite (registered trademark) H42M, Hidilite H43M, and Hidilite H42STV manufactured by Showa Denko K.K., and B1403 and B1403T manufactured by Nippon Light Metal Co., Ltd. These may be used alone or in combination of two or more. Among them, Hidilite H42M manufactured by Showa Denko K.K. is preferred.
[0026] Commercially available silica products include S0-C1, S0-C2, S0-C3, S0-C4, S0-C5, and S0-C6 manufactured by Admattex Co., Ltd., and FB-3SDC manufactured by Denka Co., Ltd. These may be used alone or in combination of two or more. Among these, FB-3SDC manufactured by Denka Co., Ltd. is preferred.
[0027] Commercially available titanium oxide products include TIPAQUE (registered trademark) CR-60 manufactured by Ishihara Sangyo Kaisha, Ltd. and JR-403 manufactured by Teika Co., Ltd. These may be used alone or in combination of two or more. Among these, JR-403 manufactured by Teika Co., Ltd. is preferred.
[0028] Examples of commercially available carbon black products include Good Flowability #MA100 and General Purpose Color #44 manufactured by Mitsubishi Chemical Corporation. These may be used alone or in combination of two or more. Among these, Good Flowability #MA100 is preferred.
[0029] The content of the filler (A) is preferably 0.1 parts by mass or more relative to 100 parts by mass of the acid-modified polyolefin (B). Since the linear expansion property is good, the content is more preferably 0.5 parts by mass or more, and even more preferably 1 part by mass or more. Also, since the adhesiveness is good, the content is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less.
[0030] The shape of the filler (A) is not particularly limited, but at least one selected from the group consisting of spherical fillers, needle-like fillers, rod-like fillers, fibrous fillers, flat fillers, scaly fillers, and plate-like fillers is preferred. Among these, the use of spherical fillers can reduce uneven distribution of stress concentration, and furthermore, distortion during thermal expansion can be easily reduced. In addition, as long as it is selected from the group consisting of spherical fillers, needle-like fillers, rod-like fillers, fibrous fillers, flat fillers, scaly fillers, and plate-like fillers, one type may be used or multiple types may be used in combination.
[0031] The filler (A) preferably has a major axis of 15 nm or more. By having a major axis of 15 nm or more, the linear expansion property is easily improved. Therefore, the major axis of the filler (A) is more preferably 20 nm or more, even more preferably 50 nm or more, and even more preferably 0.1 μm or more. On the other hand, the upper limit of the major axis of the filler (A) is not particularly limited, and may be, for example, 50 μm or less, 30 μm or less, 10 μm or less, 5 μm or less, or 3 μm or less.
[0032] <Acid-modified polyolefin (B)> The acid-modified polyolefin (B) used in the present invention (hereinafter, simply referred to as component (B)) is not limited, but is preferably one obtained by grafting at least one of α,β-unsaturated carboxylic acid and its acid anhydride to a polyolefin resin. The polyolefin resin refers to a polymer mainly composed of a hydrocarbon skeleton, such as a homopolymer of an olefin monomer exemplified by ethylene, propylene, butene, butadiene, isoprene, etc., or a copolymer with other monomers, and a hydrogenated or halogenated product of the obtained polymer. In other words, the acid-modified polyolefin is preferably one obtained by grafting at least one of α,β-unsaturated carboxylic acid and its acid anhydride to at least one of polyethylene, polypropylene, and propylene-α-olefin copolymer.
[0033] Propylene-α-olefin copolymer is a copolymer of propylene as a main component with α-olefin. As the α-olefin, for example, one or more of ethylene, 1-butene, 1-heptene, 1-octene, 4-methyl-1-pentene, vinyl acetate, etc. can be used. Among these α-olefins, ethylene and 1-butene are preferred. The ratio of the propylene component to the α-olefin component in the propylene-α-olefin copolymer is not limited, but the propylene component is preferably 50 mol% or more, more preferably 70 mol% or more.
[0034] Examples of at least one of α,β-unsaturated carboxylic acids and their acid anhydrides include maleic acid, itaconic acid, citraconic acid, and their acid anhydrides. Among these, acid anhydrides are preferred, and maleic anhydride is more preferred. Specifically, maleic anhydride-modified polypropylene, maleic anhydride-modified propylene-ethylene copolymer, maleic anhydride-modified propylene-butene copolymer, maleic anhydride-modified propylene-ethylene-butene copolymer, etc. can be mentioned, and these acid-modified polyolefins can be used alone or in combination of two or more.
[0035] From the viewpoint of heat resistance and adhesion to resin substrates and metal substrates, the acid value of the acid-modified polyolefin (B) is preferably 5 mgKOH / g or more, more preferably 6 mgKOH / g or more, and even more preferably 7 mgKOH / g or more. By making it equal to or more than the lower limit, compatibility with the epoxy resin (C) is improved, and excellent adhesive strength can be expressed. In addition, the crosslinking density is high, and solder heat resistance is good. The upper limit is preferably 40 mgKOH / g or less, more preferably 30 mgKOH / g or less, and even more preferably 20 mgKOH / g or less. By making it equal to or less than the upper limit, adhesion is good.
[0036] The number average molecular weight (Mn) of the acid-modified polyolefin (B) is preferably in the range of 10,000 to 50,000. More preferably, it is in the range of 15,000 to 45,000, even more preferably, it is in the range of 20,000 to 40,000, and particularly preferably, it is in the range of 22,000 to 38,000. By making it equal to or more than the lower limit, the cohesive force becomes good and excellent adhesiveness can be exhibited. On the other hand, by making it equal to or less than the upper limit, excellent flowability and operability can be obtained.
[0037] The acid-modified polyolefin (B) is preferably a crystalline acid-modified polyolefin. The term "crystalline" as used herein refers to a polyolefin that shows a clear melting peak during heating from -100°C to 250°C at a rate of 20°C / min using a differential scanning calorimeter (DSC).
[0038] The melting point (Tm) of the acid-modified polyolefin (B) is preferably in the range of 50°C to 120°C, more preferably in the range of 60°C to 100°C, and most preferably in the range of 70°C to 90°C. By making it equal to or higher than the lower limit, the cohesive force derived from crystals becomes good, and excellent adhesiveness and solder heat resistance can be exhibited. In addition, by making it equal to or lower than the upper limit, excellent solution stability and flowability are achieved, and operability during adhesion is good.
[0039] The heat of fusion (ΔH) of the acid-modified polyolefin (B) is preferably in the range of 5 J / g to 60 J / g. More preferably, it is in the range of 10 J / g to 50 J / g, and most preferably, it is in the range of 20 J / g to 40 J / g. By making it equal to or greater than the lower limit, the cohesive force derived from crystals becomes good, and excellent adhesiveness and solder heat resistance can be exhibited. In addition, by making it equal to or less than the upper limit, excellent solution stability and flowability are obtained, and operability during adhesion is good.
[0040] The method for producing the acid-modified polyolefin (B) is not particularly limited, and examples thereof include a radical graft reaction (i.e., a reaction in which radical species are generated on a polymer that is to become the main chain, and an unsaturated carboxylic acid and an acid anhydride are graft polymerized using the radical species as a polymerization initiation point).
[0041] As the radical generator, although not particularly limited, it is preferable to use an organic peroxide.As the organic peroxide, although not particularly limited, peroxides such as di-tert-butyl peroxyphthalate, tert-butyl hydroperoxide, dicumyl peroxide, benzoyl peroxide, tert-butyl peroxybenzoate, tert-butyl peroxy-2-ethylhexanoate, tert-butyl peroxypivalate, methyl ethyl ketone peroxide, di-tert-butyl peroxide, lauroyl peroxide, etc.; azonitriles such as azobisisobutyronitrile, azobisisopropionitrile, etc. can be mentioned.
[0042] <Epoxy resin (C)> The epoxy resin (C) used in the present invention (hereinafter, also simply referred to as component (C)) is not particularly limited as long as it has a glycidyl group in the molecule, but preferably has two or more glycidyl groups in the molecule. Specifically, it is not particularly limited, but at least one selected from the group consisting of biphenyl type epoxy resin, naphthalene type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, novolac type epoxy resin, alicyclic epoxy resin, dicyclopentadiene type epoxy resin, tetraglycidyl diaminodiphenylmethane, triglycidyl paraaminophenol, tetraglycidyl bisaminomethylcyclohexanone, N,N,N',N'-tetraglycidyl-m-xylylenediamine, and epoxy-modified polybutadiene can be used. Preferably, it is a biphenyl type epoxy resin, a novolac type epoxy resin, a dicyclopentadiene type epoxy resin, or an epoxy-modified polybutadiene. More preferably, it is a dicyclopentadiene type epoxy resin or a novolac type epoxy resin.
[0043] The content of the epoxy resin (C) is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, even more preferably 1 part by mass or more, and particularly preferably 2 parts by mass or more, relative to 100 parts by mass of the acid-modified polyolefin (B). By making it equal to or more than the lower limit, a sufficient curing effect can be obtained, and excellent adhesiveness and solder heat resistance can be exhibited. In addition, it is preferably 60 parts by mass or less, more preferably 50 parts by mass or less, even more preferably 40 parts by mass or less, and particularly preferably 35 parts by mass or less. By making it equal to or less than the upper limit, low dielectric properties are improved. That is, by making it within the above range, an adhesive layer having excellent adhesiveness, solder heat resistance, and low dielectric properties can be obtained.
[0044] The cured product of the acid-modified polyolefin (B) and the epoxy resin (C) (hereinafter, simply referred to as the cured product) refers to a cured product obtained by reacting the (B) component with the (C) component. When the adhesive layer as a whole is taken as 100% by mass, the cured product is preferably contained in an amount of 40% by mass or more. Since the strength of the adhesive layer is improved, the cured product is more preferably contained in an amount of 50% by mass or more, even more preferably contained in an amount of 60% by mass or more, even more preferably contained in an amount of 70% by mass or more, and particularly preferably contained in an amount of 75% by mass or more.
[0045] The curing conditions for components (B) and (C) are not particularly limited, but are preferably 100 to 200° C., more preferably 110 to 180° C., and even more preferably 120 to 150° C. The curing time may be set appropriately, and is preferably about 1 to 10 hours, more preferably 2 to 8 hours, and even more preferably 3 to 5 hours.
[0046] The curable component of the adhesive layer preferably further contains an oligophenylene ether (D) having a number average molecular weight of 3000 or less and a polycarbodiimide (E).
[0047] <Oligophenylene ether (D)> The oligophenylene ether (D) used in the present invention (hereinafter, simply referred to as component (D)) has a number average molecular weight (Mn) of 3000 or less, and preferably has a structural unit represented by the following general formula (1) and / or a structural unit represented by the following general formula (2). By including component (D), the solder heat resistance of the adhesive layer is improved.
[0048] [ka] In the general formula (1), R1, R2, R3, and R4 are each preferably independently a hydrogen atom, an alkyl group which may be substituted, an alkenyl group which may be substituted, an alkynyl group which may be substituted, an aryl group which may be substituted, an aralkyl group which may be substituted, or an alkoxy group which may be substituted. The "alkyl group" of the alkyl group which may be substituted is, for example, a linear or branched alkyl group having 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms. More specifically, examples of the "alkenyl group" include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, and a hexyl group, and more preferably a methyl group or an ethyl group. The "alkenyl group" of the alkenyl group which may be substituted is, for example, an ethenyl group, a 1-propenyl group, a 2-propenyl group, a 3-butenyl group, a pentenyl group, and a hexenyl group, and more preferably an ethenyl group or a 1-propenyl group. Examples of the "alkynyl group" of the alkynyl group which may be substituted include, for example, an ethynyl group, a 1-propynyl group, a 2-propynyl (propargyl) group, a 3-butynyl group, a pentynyl group, and a hexynyl group, and more preferably an ethynyl group, a 1-propynyl group, or a 2-propynyl (propargyl) group. Examples of the "aryl group" of the aryl group which may be substituted include, for example, a phenyl group, a naphthyl group, and more preferably a phenyl group. Examples of the "aralkyl group" of the aralkyl group which may be substituted include, for example, a benzyl group, a phenethyl group, a 2-methylbenzyl group, a 4-methylbenzyl group, an α-methylbenzyl group, a 2-vinylphenethyl group, and a 4-vinylphenethyl group, and more preferably a benzyl group. Examples of the "alkoxy group" of the alkoxy group which may be substituted include, for example, a linear or branched alkoxy group having 1 to 6 carbon atoms, preferably 1 to 3 carbon atoms. Examples include a methoxy group, an ethoxy group, a propoxy group, an isopropoxy group, a butoxy group, a sec-butoxy group, a tert-butoxy group, a pentyloxy group, and a hexyloxy group, and a methoxy group or an ethoxy group is more preferable.When the above alkyl group, aryl group, alkenyl group, alkynyl group, aralkyl group, and alkoxy group are substituted, they may have one or more substituents. Examples of such substituents include halogen atoms (e.g., fluorine atom, chlorine atom, bromine atom), alkyl groups having 1 to 6 carbon atoms (e.g., methyl group, ethyl group, propyl group, isopropyl group, butyl group, isobutyl group, sec-butyl group, tert-butyl group, pentyl group, hexyl group), aryl groups (e.g., phenyl group, naphthyl group), alkenyl groups (e.g., ethenyl group, 1-propenyl group, 2-propenyl group), alkynyl groups (e.g., ethynyl group, 1-propynyl group, 2-propynyl group), aralkyl groups (e.g., benzyl group, phenethyl group), and alkoxy groups (e.g., methoxy group, ethoxy group). Among them, it is preferable that R1 and R4 are methyl groups, and R2 and R3 are hydrogen.
[0049] [ka] In general formula (2), R 11 ,R 12 ,R 13 ,R 14 ,R 15 ,R 16 ,R 17 ,R 18 are preferably each independently a hydrogen atom, an optionally substituted alkyl group, an optionally substituted alkenyl group, an optionally substituted alkynyl group, an optionally substituted aryl group, an optionally substituted aralkyl group, or an optionally substituted alkoxy group. The definition of each substituent is as described above. Examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, and a hexyl group, and a methyl group is preferable. Among them, R 13 , R 14 , R 17 and R 18 is a methyl group, and R 11 , R 12 , R 15 and R 16is preferably hydrogen. Also, -A- is preferably a linear, branched or cyclic divalent hydrocarbon group having 20 or less carbon atoms, or oxygen. The number of carbon atoms in A is more preferably 1 to 15, and even more preferably 2 to 10. Also, examples of the divalent hydrocarbon group in A include a methylene group, an ethylene group, an n-propylene group, an n-butylene group, a cyclohexylene group, and a phenylene group, and among these, a phenylene group is preferable. Oxygen is particularly preferable.
[0050] The component (D) may be a modified polyphenylene ether functionalized in part or in whole with an ethylenically unsaturated group such as a vinylbenzyl group, an epoxy group, an amino group, a hydroxy group, a mercapto group, a carboxyl group, or a silyl group. Furthermore, it is preferable that both ends have a hydroxy group, an epoxy group, or an ethylenically unsaturated group. Examples of the ethylenically unsaturated group include alkenyl groups such as ethenyl groups, allyl groups, methacrylic groups, propenyl groups, butenyl groups, hexenyl groups, and octenyl groups, cycloalkenyl groups such as cyclopentenyl groups and cyclohexenyl groups, and alkenylaryl groups such as vinylbenzyl groups and vinylnaphthyl groups. In addition, both ends may be the same functional group or different functional groups. From the viewpoint of highly controlling the balance between low dielectric tangent and reduction of resin residue, it is preferable that both ends are hydroxy groups or vinylbenzyl groups, and it is more preferable that both ends are hydroxy groups or vinylbenzyl groups.
[0051] As a compound having a structural unit represented by general formula (1), a compound represented by general formula (3) is particularly preferred. [ka] In formula (3), n is preferably 3 or more, more preferably 5 or more, and is preferably 23 or less, more preferably 21 or less, and even more preferably 19 or less.
[0052] Moreover, as the compound having a structural unit represented by general formula (2), a compound represented by general formula (4) is particularly preferable. [ka] In formula (4), n is preferably 2 or more, more preferably 4 or more, and is preferably 23 or less, more preferably 20 or less, and further preferably 18 or less.
[0053] The number average molecular weight of component (D) must be 3000 or less, more preferably 2700 or less, and even more preferably 2500 or less. The number average molecular weight of component (D) is preferably 500 or more, and more preferably 700 or more. By setting the number average molecular weight of component (D) to the lower limit or more, the flexibility of the adhesive layer can be improved. On the other hand, by setting the number average molecular weight of component (D) to the upper limit or less, the solubility in organic solvents can be improved.
[0054] The content of the (D) component is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 15 parts by mass or more, relative to 100 parts by mass of the (B) component. Also, it is preferably 100 parts by mass or less, more preferably 80 parts by mass or less, even more preferably 60 parts by mass or less, and particularly preferably 50 parts by mass or less. By keeping it within the above range, an adhesive layer with excellent adhesion and solder heat resistance can be obtained.
[0055] <Polycarbodiimide (E)> The polycarbodiimide (E) (hereinafter also simply referred to as component (E)) used in the present invention is not particularly limited as long as it has a carbodiimide group in the molecule. A polycarbodiimide having two or more carbodiimide groups in the molecule is preferred. By using a polycarbodiimide, the carboxyl group of the acid-modified polyolefin (B) reacts with the carbodiimide group, enhancing the interaction between the adhesive layer and the substrate, and improving the adhesiveness. In addition, the solder heat resistance of the adhesive layer is improved.
[0056] The content of the (E) component is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, and even more preferably 2 parts by mass or more, relative to 100 parts by mass of the (B) component. By making it equal to or more than the lower limit, an interaction with the substrate is exhibited, and the adhesiveness becomes good. In addition, it is preferably 20 parts by mass or less, more preferably 15 parts by mass or less, and even more preferably 10 parts by mass or less. By making it equal to or less than the upper limit, excellent dielectric properties can be exhibited. In other words, by making it within the above range, an adhesive layer having excellent low dielectric properties in addition to adhesiveness and solder heat resistance can be obtained.
[0057] The adhesive layer of the present invention preferably has a relative dielectric constant (εc) of 3.0 or less at a frequency of 1 GHz. More preferably, it is 2.6 or less, and even more preferably, it is 2.3 or less. There is no particular lower limit, but in practical use, it is 2.0. Moreover, the dielectric constant (εc) over the entire frequency range of 1 GHz to 30 GHz is preferably 3.0 or less, more preferably 2.6 or less, and even more preferably 2.3 or less.
[0058] The adhesive layer of the present invention preferably has a dielectric loss tangent (tan δ) of 0.02 or less at a frequency of 1 GHz. More preferably, it is 0.01 or less, and even more preferably, it is 0.008 or less. There is no particular lower limit, but in practice, it is 0.0001. Moreover, the dielectric loss tangent (tan δ) over the entire frequency range of 1 GHz to 30 GHz is preferably 0.02 or less, more preferably 0.01 or less, and even more preferably 0.05 or less.
[0059] In the present invention, the dielectric constant (εc) and the dielectric loss tangent (tan δ) can be measured as follows. For example, a metal layer is formed on both sides of the adhesive layer by a thin film method such as vapor deposition or sputtering, or by applying a conductive paste to form a capacitor, and the capacitance is measured to calculate the dielectric constant (εc) and the dielectric loss tangent (tan δ) from the thickness and area. In addition, when measuring the dielectric constant and the dielectric loss tangent of the adhesive layer from the laminate, the metal substrate and / or the resin substrate may be removed before the measurement, or the laminate, the adhesive layer / metal substrate, or the adhesive layer / resin substrate may be measured as is, and then the dielectric constant and the dielectric loss tangent of the metal substrate and / or the resin substrate may be subtracted therefrom.
[0060] <Resin substrate> The resin substrate is not particularly limited as long as it is a substrate made of a resin material that can be coated with the adhesive composition, dried, and used to produce a laminate. Examples of the resin substrate include polyester resin, polyamide resin, polyimide resin, polyamideimide resin, liquid crystal polymer, polyphenylene sulfide, syndiotactic polystyrene, polyolefin resin, and fluorine resin. Film-like resin is preferred.
[0061] The thickness of the resin substrate is not particularly limited, but is preferably 5 μm or more, more preferably 10 μm or more, and even more preferably 20 μm or more, because the strength of the laminate is improved. Also, the thickness is preferably 200 μm or less, more preferably 100 μm or less, and even more preferably 50 μm or less, because the processing efficiency during circuit fabrication is improved.
[0062] <Metal base material> The metal substrate may be any conventionally known conductive material that can be used for a circuit board. Examples of the material include various metals such as SUS, copper, aluminum, iron, steel, zinc, and nickel, as well as their alloys, plated products, and metals treated with other metals such as zinc and chromium compounds. Metal foil is preferred, and copper foil is more preferred.
[0063] The thickness of the metal substrate is not particularly limited, but is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 10 μm or more, in order to obtain sufficient electrical performance of the circuit, and is preferably 50 μm or less, more preferably 30 μm or less, and even more preferably 20 μm or less, in order to improve the processing efficiency during circuit fabrication.
[0064] The metal substrate is usually provided in a rolled form. The form of the metal substrate used in producing the printed wiring board of the present invention is not particularly limited. When a ribbon-shaped metal substrate (metal foil) is used, its length is not particularly limited. Its width is also not particularly limited, but is preferably about 250 to 500 cm.
[0065] The metal substrate may be subjected to a surface treatment such as an itro treatment, a plasma treatment, a blast treatment, a primer treatment, or an anchor agent treatment.
[0066] <Printed wiring board> The printed wiring board in the present invention includes the laminate of the present invention as a component. The printed wiring board is manufactured by a conventionally known method such as a subtractive method using a metal-clad laminate. If necessary, the printed wiring board is a general term for so-called flexible circuit boards (FPCs), flat cables, circuit boards for tape automated bonding (TAB), etc., in which a conductor circuit formed by metal foil is partially or entirely covered with a cover film, screen printing ink, etc.
[0067] The printed wiring board of the present invention may have any laminate structure that can be used as a printed wiring board. For example, the printed wiring board may be composed of a laminate (resin substrate / adhesive layer / metal substrate) / adhesive layer / cover film layer.
[0068] <Example> The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the examples. In the examples and comparative examples, parts simply indicate parts by mass.
[0069] (Physical property evaluation method)
[0070] Acid value: Acid-modified polyolefin (B) The acid value (mgKOH / g) in the present invention was measured by dissolving the acid-modified polyolefin (B) in toluene and titrating it with a methanol solution of sodium methoxide using phenolphthalein as an indicator.
[0071] Number average molecular weight (Mn) The number average molecular weight in the present invention is a value measured by gel permeation chromatography (hereinafter, GPC, standard substance: polystyrene resin, mobile phase: tetrahydrofuran, column: Shodex KF-802 + KF-804L + KF-806L, column temperature: 30°C, flow rate: 1.0 ml / min, detector: RI detector) manufactured by Shimadzu Corporation.
[0072] Melting point, heat of fusion The melting point and heat of fusion in the present invention are values measured using a differential scanning calorimeter (hereinafter, DSC, manufactured by TA Instruments Japan, Q-2000) from the top temperature and area of the melting peak when the material is heated to melt at a rate of 20°C / min, cooled to resinify, and then heated to melt again.
[0073] Peel strength (adhesion) Adhesive composition b described below was applied to a 12.5 μm thick polyimide film (Apical (registered trademark), manufactured by Kaneka Corporation) so that the thickness after drying would be 12.5 μm, and dried at 130° C. for 3 minutes. Next, adhesive composition a was applied to the adhesive composition b surface so that the thickness after drying would be 12.5 μm, and dried at 130° C. for 3 minutes. The adhesive film (B stage product) thus obtained was laminated to a rolled copper foil (BHY series, manufactured by JX Metals Corporation) with a thickness of 18 μm. The lamination was performed at 160° C. and 40 kgf / cm so that the shiny side of the rolled copper foil was in contact with the adhesive layer. 2The samples were pressed under a pressure of 10000 for 30 seconds to bond the adhesive. They were then heat treated at 140°C for 4 hours to harden the adhesive, and a sample for peel strength evaluation was obtained. The sample for peel strength evaluation was subjected to a 90° peel test at 25°C and a pulling speed of 50 mm / min to measure the peel strength. This test indicates the adhesive strength at room temperature. <Evaluation criteria> ◎:1.0N / mm or more ○: 0.8N / mm or more and less than 1.0N / mm △: 0.5N / mm or more and less than 0.8N / mm ×: Less than 0.5N / mm
[0074] Solder heat resistance Samples were prepared in the same manner as in the peel strength test described above, and 2.0 cm x 2.0 cm sample pieces were aged at 23°C for 2 days, then floated in a molten solder bath at 280°C for 10 seconds, and the presence or absence of any changes in appearance such as blistering was confirmed. <Evaluation criteria> ◎: No swelling ○: Some swelling △: Many swellings ×: Swelling and discoloration
[0075] Dielectric constant (εc) and dielectric tangent (tanδ) The adhesive composition b described below was applied to a 100 μm thick Teflon (registered trademark) sheet so that the thickness after drying and curing was 12.5 μm, and dried at 130 ° C for 3 minutes. Next, the adhesive composition a was applied to the adhesive composition b surface so that the thickness after drying was 12.5 μm, and dried at 130 ° C for 3 minutes. Then, after curing by heat treatment at 140 ° C for 4 hours, the Teflon (registered trademark) sheet was peeled off to obtain a test adhesive layer sheet. The obtained test adhesive layer sheet was cut into strips of 8 cm × 3 mm to obtain a test sample. The dielectric constant (εc) and dielectric loss tangent (tan δ) were measured using a network analyzer (manufactured by Anritsu Corporation) by a cavity resonator perturbation method under conditions of a temperature of 23 ° C and a frequency of 1 GHz. The obtained relative dielectric constant and dielectric loss tangent were evaluated as follows. <Evaluation criteria for dielectric constant> ◎: 2.3 or less ○: More than 2.3 and 2.6 or less △: More than 2.6 and less than 3.0 ×:Over 3.0 <Evaluation criteria for dielectric tangent> ◎: 0.008 or less ○: More than 0.008 and 0.01 or less △: More than 0.01 and less than 0.02 ×: More than 0.02
[0076] Number of fillers (A) The laminate was cut in a direction perpendicular to its surface, and the cut surface was photographed using an electron microscope. The amount of filler particles contained in the adhesive layer 3a and adhesive layer 3b regions on the cut surface was visually counted. Note that fillers (A) with a major axis of less than 15 nm were not counted because their linear expansion properties had a small effect.
[0077] Linear expansion Using a thermomechanical analyzer (Hitachi High-Tech Science Corporation, "TMA-7100"), the test sample with a total film thickness of 25 μm used in the above-mentioned relative dielectric constant measurement was cut into a length of 1.5 cm and introduced into the device. The temperature was raised from 20°C to 250°C under conditions of a load of 5 g and a heating rate of 10°C / min. Based on the obtained data on temperature and dimensional change, the average linear expansion coefficient at 30°C was calculated and used to evaluate the low expansion property of the test sample. <Evaluation criteria for linear expansion coefficient> The evaluation criteria are values at 30°C. ◎: 500ppm or less ○: More than 500 ppm and less than 550 ppm △: Over 550 ppm and 600 ppm or less ×: More than 600 ppm
[0078] Production Example of Resin Composition (F-1) 30 parts by mass of filler (A-1), 100 parts by mass of acid-modified polyolefin (B-1), 20 parts by mass of epoxy resin (C-1), 382 parts by mass of methylcyclohexane, 39 parts by mass of methyl ethyl ketone, and 11 parts by mass of toluene were mixed together and stirred uniformly to obtain a resin composition (F-1).
[0079] Production Examples of Resin Compositions (F-2) to (F-23) Resin compositions (F-2) to (F-23) were produced in the same manner as for resin composition (F-1).
[0080] Example 1 Resin composition (F-12) was applied to a polyimide (PI) film (manufactured by Toray DuPont, product name Kapton EN50) so that the thickness after drying would be 12.5 μm, and dried at 130° C. for 3 minutes. Next, resin composition (F-11) was applied to a thickness after drying of 12.5 μm, and dried at 130° C. for 3 minutes. Next, a copper foil (manufactured by JX Nippon Oil & Gas Exploration Co., Ltd., BHY, thickness 18 μm) was laminated so that the glossy side was in contact with the resin composition (F-11) layer, and the laminate was dried at 160° C. with a pressure of 40 kgf / cm 2 The laminate was pressed for 30 seconds under a pressure of 1000 psi, and then bonded. The laminate was then heat-treated at 140°C for 4 hours to harden the laminate, obtaining a laminate. The ratio of the number of fillers (A) contained in the adhesive layer 3a and the adhesive layer 3b was a1 / a2 = 52 / 48 (30 / 28). The results are shown in Table 2.
[0081] Examples 2 to 13, Comparative Examples 1 to 3 Examples 2 to 13 and Comparative Examples 1 to 3 were carried out in the same manner as in Example 1. The results are shown in Table 2.
[0082] [Table 1]
[0083] [Table 2]
[0084] The filler (A), acid-modified polyolefin (B), epoxy resin (C), oligophenylene ether (D) and polycarbodiimide (E) used in Table 1 are as follows. <Filler (A)> Filler (A-1): Phosphorus-based flame-retardant filler (HCA-HQ-HS, manufactured by Sanko Co., Ltd., spherical, particle size: 1.5 μm) Filler (A-2): Aluminum hydroxide (Hijilite H42M manufactured by Showa Denko K.K., particle size: 1.0 μm) Filler (A-3): Silica (FB-3SDC manufactured by Denka Co., Ltd., spherical, particle size: 3 μm) Filler (A-4): Titanium oxide (TIPAQUE CR-50, manufactured by Ishihara Sangyo Kaisha, Ltd., particle size: 0.25 μm) Filler (A-5): Carbon black (Mitsubishi Chemical Corporation carbon black with good flowability #MA100, spherical, particle size: 24 nm) <Epoxy resin (C)> Epoxy resin (C-1): Dicyclopentadiene type epoxy resin: HP-7200 (DIC, epoxy equivalent 259g / eq) Epoxy resin (C-2): Epoxy modified polybutadiene resin: JP-100 (manufactured by Nippon Soda Co., Ltd.) <Oligophenylene ether (D)> Oligophenylene ether (D-1): Oligophenylene ether styrene modified product: OPE-2St 1200 (a compound having the structure of general formula (4) of Mn1000 manufactured by Mitsubishi Gas Chemical Co., Ltd.) Oligophenylene ether (D-2): Oligophenylene ether: SA90 (SABIC Mn1800 compound having the structure of general formula (3)) <Polycarbodiimide (E)> Polycarbodiimide resin (E-1): V-09GB (Nisshinbo Chemical Co., Ltd., carbodiimide equivalent: 216g / eq)
[0085] <Acid-modified polyolefin (B)> Manufacturing Example 1 In a 1L autoclave, 100 parts by mass of propylene-butene copolymer (Mitsui Chemicals' "Tafmer (registered trademark) XM7080"), 150 parts by mass of toluene, 19 parts by mass of maleic anhydride, and 6 parts by mass of di-tert-butyl peroxide were added, and the temperature was raised to 140 ° C., followed by stirring for another 3 hours. After that, the obtained reaction liquid was cooled and poured into a container containing a large amount of methyl ethyl ketone to precipitate a resin. Then, the liquid containing the resin was centrifuged to separate and purify the acid-modified propylene-butene copolymer in which maleic anhydride was graft-polymerized, (poly)maleic anhydride, and low molecular weight substances. Then, the mixture was dried under reduced pressure at 70 ° C. for 5 hours to obtain a maleic anhydride-modified propylene-butene copolymer (B-1, acid value 19 mg KOH / g, number average molecular weight 25,000, Tm 80 ° C., △H 35 J / g).
[0086] Manufacturing Example 2 A maleic anhydride-modified propylene-butene copolymer (B-2, acid value 7 mgKOH / g, number average molecular weight 35,000, Tm 82°C, △H 25 J / g) was obtained by the same procedure as in Production Example 1, except that the amount of maleic anhydride added was changed to 6 parts by mass. [Industrial Applicability]
[0087] The laminate of the present invention has good adhesive properties, dielectric properties and linear expansion properties, and is therefore useful for flexible printed wiring board applications, particularly FPC applications which require low dielectric properties (low dielectric constant, low dielectric tangent) in the high frequency range. [Explanation of symbols]
[0088] 1 Metal base material 2. Resin substrate 3 Adhesive layer 3a Adhesive layer 3a 3b Adhesive layer 3b 10 Laminate
Claims
1. A laminate in which a metal substrate, an adhesive layer, and a resin substrate are laminated in this order, The adhesive layer contains a filler (A) and a cured product of an acid-modified polyolefin (B) and an epoxy resin (C), The content of the filler (A) is 0.1 parts by mass or more and 50 parts by mass or less based on 100 parts by mass of the acid-modified polyolefin (B), The major axis of the filler (A) is 15 nm or more and 5 μm or less, A laminate in which, in a cross section of the adhesive layer in a direction perpendicular to the surface of the laminate, the number a1 of the filler (A) contained in a region from the midpoint to the surface of the metal substrate is greater than the number b1 of the filler (A) contained in a region from the midpoint to the surface of the resin substrate.
2. The laminate according to claim 1, wherein the ratio of a1 to b1 is a1 / b1=less than 100 / more than 0 to more than 50 / less than 50.
3. 3. The laminate according to claim 1, wherein the filler (A) is at least one selected from the group consisting of phosphorus-containing flame-retardant fillers, aluminum hydroxide, silica, titanium oxide and carbon black.
4. The laminate according to any one of claims 1 to 3, further comprising an oligophenylene ether (D) having a number average molecular weight of 3,000 or less in a cured product component of the adhesive layer.
5. The laminate according to any one of claims 1 to 4, further comprising a polycarbodiimide (E) in the cured product component of the adhesive layer.
6. The laminate according to any one of claims 1 to 5, wherein the adhesive layer has a relative dielectric constant (εc) of 3.0 or less and a dielectric loss tangent (tan δ) of 0.02 or less at 1 GHz.
7. A printed wiring board comprising the laminate according to any one of claims 1 to 6 as a component.
Citation Information
Patent Citations
Metal base board and its manufacture
JP1998242607A
Insulating adhesive sheet and its application
JP2006045388A
Multilayered adhesive film, coverlay film using it, and multilayered adhesive film with copper foil
JP2009084507A
Cell packaging material, method for producing the same, and cell
JP2016192397A
Thermosetting adhesive composition, adhesive film, coverlay film, and flexible printed wiring board