Spunbond nonwoven fabric, electric wire pressure winding tape, printing substrate, and method for manufacturing spunbond nonwoven fabric
A spunbond nonwoven fabric with specific polyethylene terephthalate resin properties and thermocompression bonding addresses the challenge of combining mechanical strength and surface smoothness, achieving a fabric suitable for electric wire holding tapes and printing substrates.
Patent Information
- Application Number
- JP2024521789
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-03-29
- Filing Date
- 2024-03-27
- Publication Date
- 2024-11-13
- Estimated Expiration
- 2044-03-27
AI Technical Summary
Existing spunbond nonwoven fabrics face challenges in achieving both mechanical strength and surface smoothness through heat and pressure bonding alone, as previous methods fail to adequately address these properties.
A spunbond nonwoven fabric composed of polyethylene terephthalate resin fibers with specific crystallization and melting peak ranges, core-sheath composite structure, and thermocompression bonding to enhance strength and smoothness, using a method that includes spinning, web formation, and thermocompression bonding with controlled temperature and pressure.
The solution results in a nonwoven fabric with excellent mechanical strength and high surface smoothness, suitable for applications requiring both properties.
Smart Images

Figure 0007582558000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a spunbond nonwoven fabric, an electric wire pressure winding tape, and a printing substrate. [Background technology]
[0002] The properties required for nonwoven fabrics used in electric wire pressure wrapping tapes are tensile strength, surface smoothness to facilitate peeling from the sheath material, thinness, etc. Also, for printing substrates, in addition to mechanical strength, the surface smoothness of the nonwoven fabric is an important property in terms of printing clarity and uniform ink adhesion.
[0003] Conventionally, in order to obtain a spunbonded nonwoven fabric having excellent mechanical strength and excellent surface smoothness, bonding by heat and pressure alone was insufficient because of insufficient strength and smoothness, and it was necessary to combine it with resin processing (Patent Document 1, Patent Document 2). Meanwhile, various studies have been conducted to obtain these properties by bonding by heat and pressure alone.
[0004] Patent Document 3 proposes a method for obtaining a polyethylene terephthalate spunbond nonwoven fabric suitable for use as an electric wire pressure tape or a printing substrate, in which the reduced viscosity of polyethylene terephthalate is increased to increase the strength of the fiber itself, and the fiber has a specific flatness and fineness, thereby producing a spunbond nonwoven fabric that is high in strength and excellent in smoothness.
[0005] Patent Document 4 proposes a spunbond nonwoven fabric having an intrinsic viscosity within a specific range and a ratio of the flatness of the fiber surface layer to the inner layer within a specific range. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 55-32342 [Patent Document 2] Japanese Patent Application Publication No. 57-56564 [Patent Document 3] JP 2001-140157 A [Patent Document 4] JP 2007-197891 A Summary of the Invention [Problem to be solved by the invention]
[0007] In Patent Document 3, by using flat yarns, the gaps between the fibers are reduced and surface smoothness can be improved; however, bonding by heat and pressure alone is not sufficient in terms of strength and smoothness.
[0008] In Patent Document 4, it is possible to increase the strength of a nonwoven fabric by setting the intrinsic viscosity within a specific range, and also to improve the surface smoothness by flattening only the fibers in the surface layer of the nonwoven fabric; however, bonding by heat and pressure alone is not sufficient in terms of strength and smoothness.
[0009] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a spunbonded nonwoven fabric which has excellent surface smoothness while maintaining mechanical strength by bonding only through thermocompression. [Means for solving the problem]
[0010] As a result of intensive research conducted by the present inventors in order to achieve the above object, it has been discovered that by controlling the crystallization peak and melting peak of a spunbonded nonwoven fabric in a specific temperature range in differential scanning calorimetry, it is possible to obtain a spunbonded nonwoven fabric having excellent mechanical strength and excellent surface smoothness. The present invention has been completed based on these findings.
[0011] The present invention and its preferred embodiments include the following configurations. [1] A spunbond nonwoven fabric composed of fibers whose main component is a polyethylene terephthalate resin, which has a crystallization peak in the range of 100°C to 150°C and a single melting peak in the range of 250°C to 270°C when measured by differential scanning calorimetry, and has a maximum height roughness Rz of 40.0 μm or less. [2] Apparent density: 0.40 g / cm 3 More than 1.00g / cm 3 The spunbond nonwoven fabric according to the above-mentioned [1], which is as follows: [3] A wire pressure winding tape comprising the spunbond nonwoven fabric described in [1] or [2] above. [4] A printing substrate comprising the spunbond nonwoven fabric described in [1] or [2] above. [5] A method for producing the spunbonded nonwoven fabric according to the above item [1] or [2], comprising the following steps (a) to (c) in this order: Step (a): A step of spinning a core-sheath type composite fiber in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less and having an intrinsic viscosity (IV) that is 0.05 or more and 0.25 or less lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is disposed around the high-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less. Step (b): A step of drawing and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermocompressing the fiber web with a flat roll. Effect of the Invention
[0012] According to the present invention, there is provided a nonwoven fabric having excellent mechanical strength and high surface smoothness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The spunbond nonwoven fabric of the present invention is a spunbond nonwoven fabric composed of fibers mainly composed of polyethylene terephthalate resin, and has a crystallization peak in the range of 100° C. to 150° C. and a single melting peak in the range of 250° C. to 270° C. as measured by differential scanning calorimetry, and a maximum height roughness Rz of 40.0 μm or less. The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the invention, and various modifications are possible without departing from the gist of the invention.
[0014] [Polyethylene terephthalate resin] First, the spunbond nonwoven fabric of the present invention is composed of fibers containing polyethylene terephthalate resin as a main component.
[0015] The melting point of the polyethylene terephthalate resin is preferably 250°C or higher and 270°C or lower. By setting the melting point of the polyethylene terephthalate resin to 250°C or higher, it becomes easier to obtain heat resistance that can withstand practical use. Furthermore, by setting the melting point of the polyethylene terephthalate resin to 270°C or lower, it becomes easier to cool the yarn discharged from the spinneret, and it becomes easier to suppress fusion between fibers and perform stable spinning even with a thin fiber diameter. Here, the melting point of the polyethylene terephthalate resin refers to the maximum melting peak temperature obtained by measuring the polyethylene terephthalate resin by differential scanning calorimetry (DSC).
[0016] The intrinsic viscosity (IV) of the polyethylene terephthalate resin is preferably 0.40 or more and 0.70 or less. By making the intrinsic viscosity of the polyethylene terephthalate resin 0.40 or more, more preferably 0.45 or more, and even more preferably 0.50 or more, it is possible to suppress a decrease in the strength of the fibers constituting the nonwoven fabric. On the other hand, by making the intrinsic viscosity of the polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.
[0017] Additives such as crystal nucleating agents, matting agents, lubricants, pigments, mildewproofing agents, antibacterial agents, flame retardants, metal oxides, aliphatic bisamides and / or alkyl-substituted aliphatic monoamides, and hydrophilic agents can be added to the polyethylene terephthalate resin as long as they do not impair the effects of the present invention. Among them, metal oxides such as titanium oxide have the effect of improving spinnability by reducing surface friction of fibers and preventing fusion between fibers, and also improving the fusion properties of the nonwoven fabric by increasing thermal conductivity during fusion molding of the nonwoven fabric with a heated roll, thereby making it possible to obtain a spunbond nonwoven fabric with superior mechanical strength.
[0018] [fiber] The fibers constituting the nonwoven fabric are preferably core-sheath type composite fibers.
[0019] Furthermore, the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the sheath component is preferably lower than the intrinsic viscosity (IV) of the polyethylene terephthalate resin of the core component by 0.05 or more and 0.25 or less. Hereinafter, the polyethylene terephthalate resin of the sheath component in this embodiment is also called "low-viscosity polyethylene terephthalate resin", and the polyethylene terephthalate resin of the core component is also called "high-viscosity polyethylene terephthalate resin". The intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is 0.05 or more, more preferably 0.08 or more, and even more preferably 0.10 or more lower than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin, so that the spinning stress is concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. As a result, a fiber having high single fiber strength and excellent thermal adhesion can be obtained, making it easier to obtain a nonwoven fabric having excellent mechanical strength. On the other hand, when the intrinsic viscosity of the low-viscosity polyethylene terephthalate resin is smaller than the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin by not more than 0.25, preferably not more than 0.20, the single fiber strength of the core-sheath type composite fiber can be improved.
[0020] The intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin is preferably 0.55 or more and 0.70 or less. By making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.55 or more, it is possible to prevent a decrease in single fiber strength. Furthermore, by making the intrinsic viscosity of the high-viscosity polyethylene terephthalate resin 0.70 or less, it is possible to stably spin even fine fibers, and to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.
[0021] The mass ratio of the sheath component in the core-sheath type composite fiber is preferably 10% by mass or more and 80% by mass or less. By making the mass ratio of the sheath component 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, the sheath components are firmly fused together during thermocompression bonding, and a spunbonded nonwoven fabric having sufficient strength for practical use can be obtained. On the other hand, by making the ratio of the sheath component 80% by mass or less, more preferably 70% by mass or less, and even more preferably 60% by mass or less, the proportion of the highly oriented core component is increased, the single fiber strength of the core-sheath type composite fiber is improved, and a spunbonded nonwoven fabric having sufficient strength for practical use can be obtained.
[0022] The composite form of the sheath-core composite fiber may be, for example, a concentric sheath-core type, an eccentric sheath-core type, an islands-in-the-sea type, etc. Among them, the sheath-core type composite form is preferred, and the concentric sheath-core type composite form is more preferred, since it has excellent spinnability, allows the fibers to be uniformly bonded together by thermocompression bonding, and allows a spunbonded nonwoven fabric with excellent mechanical strength to be produced.
[0023] The fibers preferably have an average fiber diameter of 6.0 μm or more and 20.0 μm or less. By making the average fiber diameter 6.0 μm or more, more preferably 7.0 μm or more, and even more preferably 8.0 μm or more, it is possible to prevent a decrease in spinnability, improve production stability, and obtain a spunbond nonwoven fabric having excellent mechanical strength. On the other hand, by making the average fiber diameter 20.0 μm or less, more preferably 18.0 μm or less, and even more preferably 16.0 μm or less, it is possible to obtain a spunbond nonwoven fabric having a uniform texture and sufficient strength for practical use.
[0024] In the present invention, the average fiber diameter (μm) is determined by the following method. (i) Ten small sample pieces of 10 mm x 10 mm are randomly taken from the spunbond nonwoven fabric. (ii) The surface of the collected small sample is photographed using a scanning electron microscope or the like at magnifications of 500 to 2000 times, enabling the thickness of the fibers to be measured. (iii) From the photographs of each small sample, 10 fibers are randomly selected (100 fibers in total) and their thickness is measured. Assuming that the cross section of the fiber is circular, the thickness is taken as the fiber diameter. (iv) The average fiber diameter is calculated by rounding off the arithmetic mean of those fiber diameters to one decimal place.
[0025] [Spunbond nonwoven fabric] The spunbonded nonwoven fabric of the present invention has a crystallization peak in the range of 100°C to 150°C by differential scanning calorimetry. When the spunbonded nonwoven fabric has a crystallization peak temperature in the above range, fusion between fibers during flat roll bonding is promoted, resulting in a spunbonded nonwoven fabric with excellent surface smoothness and excellent mechanical strength. On the other hand, in the case of a spunbonded nonwoven fabric that does not have a crystallization peak, fusion between fibers is difficult to occur, resulting in a spunbonded nonwoven fabric with low surface smoothness and low mechanical strength.
[0026] Furthermore, the spunbond nonwoven fabric has a single melting peak in the range of 250° C. to 270° C. as measured by differential scanning calorimetry. By having a single melting peak in this range, the fibers can be firmly thermocompressed together at a sufficient temperature without causing operational problems such as low-melting point components melting and sticking to a heated roll during thermocompression, and a spunbond nonwoven fabric having sufficient strength for practical use can be obtained.
[0027] Here, the crystallization peak temperature Tc (°C) and the melting peak temperature Tm (°C) of the spunbond nonwoven fabric are obtained by differential scanning calorimetry (DSC), and the values calculated according to the following procedure are adopted. (i) A small piece of spunbond nonwoven fabric is sampled in an amount of 0.5 mg to 5 mg. (ii) Using differential scanning calorimetry (DSC), the temperature is raised from room temperature to 280°C at a rate of 16°C / min to obtain a DSC curve. (iii) The peak top temperature of the crystallization exothermic peak is read from the DSC curve and regarded as the crystallization peak temperature Tc (°C) of the spunbond nonwoven fabric, and the peak top temperature of the melting endothermic peak is read and regarded as the melting peak temperature Tm (°C) of the spunbond nonwoven fabric.
[0028] The spunbond nonwoven fabric has a maximum height roughness Rz of 40.0 μm or less. By making the maximum height roughness Rz 40.0 μm or less, preferably 35.0 μm or less, and more preferably 33.0 μm or less, localized irregularities can be eliminated from the nonwoven fabric surface, resulting in a nonwoven fabric with excellent surface smoothness.
[0029] In the present invention, the maximum height roughness Rz refers to a value measured and calculated by the following method. (i) 10 cm x 10 cm of long fiber nonwoven fabric is randomly taken from 10 locations. (ii) For randomly sampled nonwoven fabric, a surface roughness meter (for example, Mitutoyo Corporation's "Surftest SJ-210") is used to measure a range of 21 mm in the width direction of the long-fiber nonwoven fabric sheet in accordance with JIS B0610:2001 "Geometric characteristic specifications of products (GPS) - Surface shape: Profile curve method - Definition and display of rolling circle waviness" under conditions of λc = 2.5 mm, λs = 8 μm, and a measurement speed of 0.5 mm / s. The maximum height roughness Rz is measured in 0.1 μm units for 10 points of each sample on each side. (iii) The above measured values are arithmetically averaged for each surface, rounded off to one decimal place, and the value of the surface with the highest value is regarded as the maximum height roughness Rz.
[0030] The spunbond nonwoven fabric of the present invention preferably has an arithmetic mean roughness Ra of 4.5 μm or less. By having an arithmetic mean roughness Ra of 4.5 μm or less, more preferably 4.0 μm or less, and even more preferably 3.5 μm or less, the entire surface of the nonwoven fabric becomes smooth, resulting in a nonwoven fabric with excellent smoothness.
[0031] In the present invention, the arithmetic mean roughness Ra refers to a value measured and calculated by the following method. (i) 10 cm x 10 cm of long fiber nonwoven fabric is randomly taken from 10 locations. (ii) For randomly sampled nonwoven fabric, a surface roughness tester (for example, Mitutoyo Corporation's "Surftest SJ-210") is used to measure a range of 21 mm in the width direction of the long-fiber nonwoven fabric sheet in accordance with JIS B0610:2001 "Product geometric characteristic specifications (GPS) - Surface shape: Profile curve method - Definition and display of rolling circle waviness" under conditions of λc = 2.5 mm, λs = 8 μm, and a measurement speed of 0.5 mm / s, and the arithmetic mean roughness Ra is measured in units of 0.1 μm on each side of 10 points of each sample. (iii) The measured values on both sides (total of 20 points) are calculated by arithmetic average, and this is rounded off to one decimal place to obtain the arithmetic average roughness Ra.
[0032] The spunbond nonwoven fabric of the present invention has a tensile strength per unit area of 5.00 (N / 5cm) / (g / m 2It is preferable that the tensile strength is 5.00 (N / 5cm) / (g / m 2 ) or more, more preferably 5.50 (N / 5cm) / (g / m 2 ) or more, more preferably 5.80 (N / 5cm) / (g / m 2 ) or more, a minimum tensile strength can be obtained, which is preferable.
[0033] In the present invention, the tensile strength per unit area of the spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) shall be the value determined by the following method in accordance with JIS L1913:2010 "Testing methods for general long-fiber nonwoven fabrics", 6.3 "Tensile strength and elongation". (i) Three samples measuring 30 cm x 5.0 cm are taken from the nonwoven fabric at equal intervals in both the longitudinal direction (MD) and cross direction (CD). (ii) A load is applied until the sample breaks, with a grip distance of 20 cm and a tensile speed of 100±10 mm / min. (iii) The strength of the sample at maximum load is taken as the tensile strength (N / 5 cm), and the average of three points in each of the MD and CD is calculated. The sum of these average values is the tensile strength of the spunbond nonwoven fabric. (iv) The tensile strength per unit area of the spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) and round off to the third decimal place.
[0034] Tensile strength per unit area of spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) = [tensile strength of spunbond nonwoven fabric (N / 5cm)] / weight (g / m 2 ).
[0035] The apparent density of the spunbond nonwoven fabric of the present invention is 0.40 g / cm 3 More than 1.00g / cm 3 It is preferable that the apparent density is 0.40 g / cm or less. 3 or more, preferably 0.42 g / cm 3 More preferably, 0.45 g / cm 3By setting the apparent density at 1.00 g / cm or more, a spunbond nonwoven fabric having both thinness and mechanical strength can be obtained. 3 Less than 0.95 g / cm 3 Less than or equal to 0.90 g / cm 3 By setting the thickness to the range below this, it is possible to provide a certain level of breathability, and for example, when used as a printing substrate, this is preferred because it allows ink to easily penetrate into the interior of the nonwoven fabric.
[0036] The apparent density (g / cm) of the spunbond nonwoven fabric is 3 ) is the basis weight (g / m2) of the spunbond nonwoven fabric described below. 2 ) is converted into units by the thickness (mm) of the spunbond nonwoven fabric described later, and then divided to obtain the result (g / cm 3 The thickness (mm) of the spunbond nonwoven fabric is calculated by the following procedure. (i) Take three pieces of spunbond nonwoven fabric that are 10 cm wide in the longitudinal direction. (ii) Using a pressure probe with a diameter of 10 mm, measure the thickness of the spunbond nonwoven fabric at 10 equally spaced points per meter across the width of the fabric with a load of 10 kPa to an accuracy of 0.01 mm. (iii) The arithmetic average of the measured values obtained above is calculated for each of the three spunbond nonwoven fabrics sampled, and the arithmetic average is then rounded to two decimal places to calculate the average for each of the three spunbond nonwoven fabrics.
[0037] The basis weight (g / m 2 ) is calculated using the following procedure. (i) Take three pieces of spunbond nonwoven fabric measuring 30 cm x 50 cm. (ii) Measure the mass of each sample and calculate the average of the measured values as the mass per unit area (g / m 2 ) and round off to the first decimal place to calculate the weighting. [Manufacturing method of spunbond nonwoven fabric] The spunbonded nonwoven fabric of the present invention can be preferably produced by the method for producing the spunbonded nonwoven fabric of the present invention, which is a method for producing the spunbonded nonwoven fabric of the present invention and includes the following steps (a) to (c) in this order:
[0038] [Step (a): Fiber spinning step] In step (a), a core-sheath type composite fiber is spun in which a low-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less and having an intrinsic viscosity (IV) lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate resin by 0.05 to 0.25, is disposed around a high-viscosity polyethylene terephthalate resin having a melting point of 250°C or more and 270°C or less.
[0039] That is, in the sheath-core composite fiber, it is preferable that the high-viscosity polyethylene terephthalate resin is the core component and the low-viscosity polyethylene terephthalate resin is the sheath component. By making the difference between the intrinsic viscosity of the core component and the intrinsic viscosity of the sheath component 0.05 or more, more preferably 0.10 or more, spinning stress is concentrated on the core component during spinning, promoting the orientation of the core component and suppressing the orientation of the sheath component. On the other hand, by making the difference between the intrinsic viscosity of the core component and the intrinsic viscosity of the sheath component 0.25 or less, preferably 0.20 or less, the single fiber strength of the sheath-core composite fiber can be improved, and rapid softening during thermocompression bonding can be suppressed, thereby suppressing sticking to a heated roll during production.
[0040] The core-sheath type composite fiber is preferably melted at a temperature not lower than its melting point but not higher than 70°C above the melting point, and is preferably melt-extruded from a spinneret having a temperature not lower than its melting point but not higher than 70°C above the melting point.
[0041] The shape of the outlet hole of the spinneret from which the core-sheath type composite fiber is extruded may be circular, elliptical, polygonal, multi-lobed, or a combination of these shapes in accordance with the cross-sectional shape of the fiber. Among these, a circular shape is more preferred from the viewpoint of efficiently obtaining bonding points between the fibers and firmly bonding the fibers together by thermocompression bonding.
[0042] [Step (b): Step of forming a fiber web] In step (b), the spun core-sheath type composite fiber is pulled and stretched by an ejector, and deposited on a moving net conveyor to form a fiber web.
[0043] In step (b), the spun fibers are preferably pulled and stretched by an ejector, and the fibers are deposited on a moving net conveyor to form a fiber web. In this case, the spinning speed for pulling the fibers is preferably 3000 m / min or more and 6000 m / min or less.
[0044] [Step (c): Step of thermocompressing the fiber web] In step (c), the fiber web is heat-pressed with a flat roll.
[0045] The fiber web can be heat-pressed to obtain the intended spunbonded nonwoven fabric.
[0046] The method for thermocompression bonding the fiber web is by using a pair of flat rolls. By performing thermocompression bonding with flat rolls, unlike bonding with an embossing roll, localized unevenness is eliminated, the maximum height roughness of the surface can be reduced, and a nonwoven fabric with excellent surface smoothness can be obtained.
[0047] As for the surface material of the flat roll, a preferred embodiment is one in which a metal roll is paired with a metal roll in order to obtain a sufficient thermocompression effect.
[0048] The surface temperature of the flat roll during thermocompression bonding is preferably set to a temperature 10°C to 100°C lower than the melting point (hereinafter sometimes referred to as Tm (°C)) of the polyethylene terephthalate resin used (i.e., (Tm-100)°C to (Tm-10)°C). By setting the surface temperature of the thermoroll to (Tm-100)°C or higher, more preferably (Tm-90)°C or higher, it is possible to obtain a spunbonded nonwoven fabric having a strength sufficient for practical use by performing moderate thermocompression bonding. Furthermore, by setting the surface temperature of the flat roll to (Tm-10)°C or lower, more preferably (Tm-15)°C or lower, it is possible to prevent excessive thermocompression bonding and prevent the spunbonded nonwoven fabric from partially taking on a film-like sheet form.
[0049] The linear pressure of the flat roll during thermocompression bonding is preferably 90 N / cm or more and 1000 N / cm or less. By setting the linear pressure for thermocompression bonding to 90 N / cm or more, a spunbonded nonwoven fabric having excellent mechanical strength can be obtained. By setting the linear pressure for thermocompression bonding to 1000 N / cm or less, excessive fusion between the fibers can be prevented.
[0050] [Electrical wire pressure winding tape] The electric wire pressure winding tape of the present invention includes the nonwoven fabric. This makes it possible to obtain an electric wire pressure winding tape that is thin, has good mechanical strength, and has excellent surface smoothness. The electric wire pressure winding tape of the present invention refers to a tape that is disposed between an electric wire cable and a sheath that covers the cable and that winds the electric wire cable. The electric wire pressure winding tape of the present invention can be post-processed to impart functions such as semiconductivity and water absorption to the nonwoven fabric.
[0051] The applications of the electric wire pressure winding tape of the present invention are not particularly limited, and the tape can be used in various fields. Specific examples of applications of the electric wire pressure winding tape of the present invention include power cables for power transmission and communication cables.
[0052] [Printing base material] The printing substrate of the present invention contains the nonwoven fabric. In this way, a printing substrate having excellent mechanical strength, good surface smoothness, and excellent printability can be obtained. The printing substrate is preferably a substrate for commercial printing such as inkjet printing, laser printing, flexographic printing, letterpress printing, gravure printing, offset printing, and thermal transfer printing. The printing substrate of the present invention can also be subjected to post-processing to improve functions such as flame retardancy and concealment.
[0053] The application of the printing substrate of the present invention is not particularly limited, and it can be used in various fields. Specific examples of the application of the printing substrate of the present invention include wallpaper, posters, labels, etc. EXAMPLES
[0054] Next, the nonwoven fabric of the present invention will be specifically described based on examples, although the present invention is not limited to these examples.
[0055] [Measurement method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were performed according to the above-mentioned methods.
[0056] (1) Melting point of polyethylene terephthalate resin (℃) Measurement was performed using a differential scanning calorimeter (PerkinElmer, "DSC-2") at a temperature rise rate of 16°C / min, and the temperature at which the extreme value was obtained in the obtained melting endothermic curve was taken as the melting point.
[0057] (2) Intrinsic viscosity (IV) of polyethylene terephthalate resin The intrinsic viscosity (IV) of the polyethylene terephthalate resin was measured by the following method.
[0058] Dissolve 8 g of sample in 100 mL of orthochlorophenol, and measure the relative viscosity η using an Ostwald viscometer at 25°C. r was calculated by the following formula. η r =η / η0=(t×d) / (t0×d0) where η is the viscosity of the polymer solution, η0 is the viscosity of orthochlorophenol, t is the drop time of the solution (sec), and d is the density of the solution (g / cm 3 ), t0 is the fall time of orthochlorophenol (sec), and d0 is the density of orthochlorophenol (g / cm 3 ) respectively. Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula: Intrinsic viscosity (IV)=0.0242η r +0.2634.
[0059] (3) Average fiber diameter (μm) The average fiber diameter of the fibers was calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.
[0060] (4) Crystallization peak temperature (Tc) of spunbond nonwoven fabric The crystallization peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a PerkinElmer "DSC-2" differential scanning calorimeter.
[0061] (5) Melting peak temperature (Tm) of spunbond nonwoven fabric The melting peak temperature of the spunbond nonwoven fabric was calculated by the above-mentioned method using a differential scanning calorimeter "DSC-2" manufactured by PerkinElmer Co., Ltd.
[0062] (6) Maximum surface roughness Rz (μm) of spunbond nonwoven fabric The maximum surface height roughness of the spunbond nonwoven fabric was calculated by the above-mentioned method using a Mitutoyo Corporation "Surftest SJ-210" surface roughness meter.
[0063] (7) Weight of spunbond nonwoven fabric (g / m 2 ) The basis weight of the spunbond nonwoven fabric was calculated by the method described above.
[0064] (8) Thickness of spunbond nonwoven fabric (mm) The thickness of the spunbonded nonwoven fabric was calculated by the method described above.
[0065] (9) Apparent density of spunbond nonwoven fabric (g / cm 3 ) The apparent density of the spunbond nonwoven fabric was calculated by the method described above.
[0066] (10) Tensile strength per unit area of spunbond nonwoven fabric ((N / 5cm) / (g / m 2 )) The tensile strength per unit area of the spunbond nonwoven fabric was measured by the above-mentioned method using Baldwin's "RTG-1250".
[0067] (11) Arithmetic mean surface roughness Ra (μm) of spunbond nonwoven fabric The arithmetic mean surface roughness Ra of the spunbond nonwoven fabric was measured by the above-mentioned method using a Mitutoyo Corporation "Surftest SJ-210" surface roughness meter.
[0068] [Resin used] The resins used in the examples and comparative examples are described in detail below. · Polyethylene terephthalate resin A (PET_A): Polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.65, and a melting point of 255°C. · Polyethylene terephthalate resin B (PET_B): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.51 and a melting point of 255°C. Polyethylene terephthalate resin C (PET_C): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.70 and a melting point of 255°C. · Polyethylene terephthalate resin D (PET_D): Polyethylene terephthalate dried to a moisture content of 50 mass ppm or less, with an intrinsic viscosity (IV) of 0.56 and a melting point of 255°C. · Polyethylene terephthalate resin E (PET_E): Polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.45, and a melting point of 255°C. · Polyethylene terephthalate resin F (PET_F): Polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.62, and a melting point of 255°C. Polyethylene terephthalate resin G (CO-PET): Copolymerized polyethylene terephthalate that has been dried to a moisture content of 50 mass ppm or less, has an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C.
[0069] [Example 1] (The process of spinning fibers) Polyethylene terephthalate resin A and polyethylene terephthalate resin B were each melted at a temperature of 295° C. Then, concentric core-sheath composite fibers were spun from a circular extrusion hole with polyethylene terephthalate resin A as the core component and polyethylene terephthalate resin B as the sheath component at a spinneret temperature of 295° C. and a core:sheath weight ratio of 80:20.
[0070] (Step of forming a fiber web) The fiber spun by the above process was drawn at a spinning speed of 5000 m / min, and the basis weight of the resulting nonwoven fabric was 35.0 g / m 2 A fiber web consisting of fibers with an average fiber diameter of 10.1 μm was formed by depositing the mixture on a net conveyor whose moving speed was adjusted so that the diameter of the fibers was 10.1 μm.
[0071] (Process for thermocompression bonding of fiber web) Subsequently, the formed fiber web was heat-pressed using a pair of hot flat rolls consisting of an upper roll and a lower roll under the conditions of a surface temperature of the hot flat roll of 180°C and a linear pressure of 686 N / cm to obtain a spunbonded nonwoven fabric. Top roll: Metal flat roll Bottom roll: metal flat roll.
[0072] The obtained spunbond nonwoven fabric was evaluated and the results are shown in Table 1.
[0073] [Example 2] In the fiber spinning process, the polyethylene terephthalate resin A was changed to polyethylene terephthalate resin C. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0074] [Example 3] In the fiber spinning process, the polyethylene terephthalate resin A was changed to polyethylene terephthalate resin D. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0075] [Example 4] In the fiber spinning process, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin E. A spunbonded nonwoven fabric was obtained using the same procedures and conditions as in Example 2. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0076] [Comparative Example 1] In the fiber spinning process, polyethylene terephthalate resin B was replaced with polyethylene terephthalate resin A to form a single component fiber. In addition, in the process of thermocompression bonding the fiber web, the surface temperature of the hot flat roll was set to 250° C. Other than that, a spunbonded nonwoven fabric was obtained under the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0077] [Comparative Example 2] In the fiber spinning process, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin G. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0078] [Comparative Example 3] In the fiber spinning process, polyethylene terephthalate resin B was changed to polyethylene terephthalate resin F. A spunbonded nonwoven fabric was obtained under the same procedures and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0079] [Comparative Example 4] In the process of thermocompression bonding of the fiber web, the upper roll was changed from a metal flat roll to a metal round pattern embossed roll (bonding rate 16%). Except for this, a spunbonded nonwoven fabric was obtained under the same procedure and conditions as in Example 1. The physical properties of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0080] [Table 1]
[0081] The spunbonded nonwoven fabrics of Examples 1 to 4 had high tensile strength and excellent mechanical strength, and also had a low arithmetic mean roughness Ra and excellent surface smoothness.
[0082] On the other hand, the spunbond nonwoven fabrics of Comparative Examples 1 to 4 had high arithmetic mean roughness Ra and were not excellent in surface smoothness (Comparative Examples 1 to 4), or had low tensile strength and insufficient mechanical strength (Comparative Example 1).
Claims
1. A spunbond nonwoven fabric composed of fibers containing a polyethylene terephthalate resin as a main component, the spunbond nonwoven fabric having a crystallization peak in the range of 100°C or more and 150°C or less, a single melting peak in the range of 250°C or more and 270°C or less, measured by differential scanning calorimetry, and having a maximum height roughness Rz of 40.0 μm or less.
2. Apparent density: 0.40 g / cm 3 1.00g / cm or more 3 2. The spunbond nonwoven fabric of claim 1, wherein:
3. A wire pressure winding tape comprising the spunbond nonwoven fabric according to claim 1 or 2.
4. A printing substrate comprising the spunbond nonwoven fabric according to claim 1 or 2.
5. A method for producing the spunbonded nonwoven fabric according to claim 1 or 2, comprising the following steps (a) to (c) in this order: Step (a): A step of spinning a core-sheath type composite fiber in which a low-viscosity polyethylene terephthalate-based resin having a melting point of 250° C. or more and 270° C. or less and having an intrinsic viscosity (IV) that is 0.05 or more and 0.25 or less lower than the intrinsic viscosity (IV) of the high-viscosity polyethylene terephthalate-based resin is disposed around the high-viscosity polyethylene terephthalate-based resin having a melting point of 250° C. or more and 270° C. or less. Step (b): A step of drawing and stretching the spun core-sheath type composite fiber by an ejector and depositing it on a moving net conveyor to form a fiber web. Step (c): A step of thermocompressing the fiber web with a flat roll.
Citation Information
Patent Citations
Spun-bond nonwoven fabric
JP2001140157A
Composite nonwoven fabric for patch
JP2008163538A
Area-bonded nonwoven fabric manufactured from a single polymer system
JP2010537068A
Short-cut fiber for wet-laid nonwoven fabric
JP2014037644A
Polyester long fiber nonnwoven fabric for pressswinding electric cable and method of manufacturing same
JP1980032342A