Particle-linked ceria-based composite microparticle dispersion, its manufacturing method, and abrasive dispersion for polishing containing particle-linked ceria-based composite microparticle dispersion

The particle-linked ceria-based composite fine particle dispersion addresses low polishing rates and surface defects by connecting silica particles with a cerium-containing silica layer, providing high-speed polishing with minimal scratches and contamination on semiconductor substrates.

JP7583627B2Active Publication Date: 2024-11-14JGC CATALYSTS & CHEMICALS LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2021013423
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-11-14
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Existing ceria-based abrasive particles used in semiconductor manufacturing suffer from low polishing rates, surface defects, and impurities, leading to reduced polishing stability and increased scratches, especially during high-pressure conditions.

Method used

A particle-linked ceria-based composite fine particle dispersion is developed, where silica primary particles are connected via a cerium-containing silica layer, forming a planar structure with child ceria particles dispersed inside, enhancing mechanical contact and stability during polishing.

Benefits of technology

The dispersion achieves high-speed polishing with minimal scratches and reduced abrasive grain residue, ensuring high surface accuracy and preventing contamination on semiconductor substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583627000002
    Figure 0007583627000002
  • Figure 0007583627000003
    Figure 0007583627000003
  • Figure 0007583627000004
    Figure 0007583627000004
Patent Text Reader

Abstract

To provide ceria-based composite particulates, which can polish silica films, Si wafers and even difficult-to-process materials at high-speed, can achieve high surface accuracy at the same time, and can be particularly suitable in a dispersion for high-speed polishing.SOLUTION: A ceria-based composite particulate, which is characterized in that (i) it includes a plurality of specific silica primary fine particles connected via a cerium-containing silica layer, (ii) it has mother particles having on their surfaces a cerium-containing silica layer, and child particles dispersed inside the cerium-containing silica layer, and (iii) it has the following characteristics (1) to (3): (1) The ratio of short diameter / long diameter is in the range of 0.1 to 0.9. (2) The ratio of the projected area (T) of the stereoscopic portion of the particulate and the projected area (S) of the entire particulate, determined from scanning electron micrograph, satisfy a specific relationship. (3) Neither of the two sites α nor β on the outer edge and on the long axis of the particulate, identified from the scanning electron micrograph, has a sharp-edged projection structure.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a ceria-based composite microparticle dispersion suitable as an abrasive used in the manufacture of semiconductor devices and the like, and in particular to a ceria-based composite microparticle dispersion for planarizing a film to be polished formed on a substrate by chemical mechanical polishing (CMP), a method for producing the same, and a polishing abrasive dispersion containing the ceria-based composite microparticle dispersion. [Background technology]

[0002] Semiconductor devices such as semiconductor substrates and wiring boards have achieved high performance through higher density and miniaturization. In the manufacturing process of semiconductors, so-called chemical mechanical polishing (CMP) is applied, and specifically, it is an essential technology for shallow trench isolation, planarization of interlayer insulating films, and formation of contact plugs and Cu damascene wiring.

[0003] Generally, CMP polishing agents consist of abrasive grains and chemical components, and the chemical components play a role in promoting polishing by oxidizing or corroding the target film. On the other hand, the abrasive grains perform polishing through mechanical action, and colloidal silica, fumed silica, and ceria particles are used as abrasive grains. Ceria particles in particular have a particularly high polishing speed for silicon oxide films, and are therefore used for polishing in the shallow trench isolation process. In the shallow trench isolation process, not only the silicon oxide film but also the silicon nitride film is polished. To facilitate isolation, it is desirable that the polishing rate of the silicon oxide film is high and that of the silicon nitride film is low, and the polishing rate ratio (selectivity) is also important.

[0004] Conventionally, the method of polishing such components involves a relatively rough primary polishing process followed by a precise secondary polishing process to obtain a smooth surface or an extremely high-precision surface with few scratches or other imperfections. Regarding the abrasive used in the secondary polishing as the finish polishing, the following methods have been proposed.

[0005] For example, Patent Document 1 describes a method for producing cerium oxide ultrafine particles (average particle size: 10 to 80 nm) made of cerium oxide single crystals, which comprises mixing and stirring an aqueous solution of cerous nitrate and a base in a ratio such that the pH is 5 to 10, followed by rapidly heating to 70 to 100°C and maturing at that temperature. It further describes that this production method can provide cerium oxide ultrafine particles that are highly uniform in particle size and shape.

[0006] Non-Patent Document 1 also discloses a method for producing ceria-coated silica, which includes a production process similar to the production process for cerium oxide ultrafine particles described in Patent Document 1. This method for producing ceria-coated silica does not include the firing-dispersion process included in the production method described in Patent Document 1.

[0007] Patent Document 2 describes silica-based composite particles having a crystalline oxide layer B containing one or more elements selected from zirconium, titanium, iron, manganese, zinc, cerium, yttrium, calcium, magnesium, fluorine, lanthanum, and strontium on the surface of amorphous silica particle A. In addition, as a preferred embodiment, a silica-based composite particle is described having an amorphous oxide layer C on the surface of amorphous silica particle A, which is an amorphous oxide layer containing an element such as aluminum and is different from the amorphous silica layer, and further having a crystalline oxide layer B on the amorphous silica particle A, which contains one or more elements selected from zirconium, titanium, iron, manganese, zinc, cerium, yttrium, calcium, magnesium, fluorine, lanthanum, and strontium. It is described that such silica-based composite particles have a crystalline oxide layer B on the surface of amorphous silica particles A, so that they can improve the polishing speed, and by pre-treating silica particles, they can suppress sintering between particles during firing, improving dispersibility in polishing slurry, and they can provide an inexpensive polishing material with high polishing performance because they do not contain cerium oxide or can greatly reduce the amount of cerium oxide used.It is also described that those that have an amorphous oxide layer C between silica-based particles A and oxide layer B are particularly excellent in the effect of suppressing sintering of particles and the effect of improving polishing speed.

[0008] Furthermore, Patent Document 3 describes a silica-based composite microparticle dispersion liquid containing silica-based composite microparticles having an average particle size of 50 to 350 nm and the following characteristics [1] to [3], in which child particles mainly made of crystalline ceria are present on the surface of mother particles mainly made of amorphous silica, and the surfaces of the child particles are further coated with silica. [1] The silica-based composite microparticles have a mass ratio of silica to ceria of 100:11 to 316. [2] When the silica-based composite microparticles are subjected to X-ray diffraction, only the crystalline phase of ceria is detected. [3] The silica-based composite microparticles have a crystallite size of 10 to 25 nm in the (111) plane of the crystalline ceria, as measured by X-ray diffraction. It is also described that such silica-based composite microparticles can be used to polish even silica films, Si wafers, and other difficult-to-process materials at high speeds, while at the same time achieving high surface precision (low scratches, low surface roughness (Ra) of the substrate to be polished, etc.), and furthermore, since they do not contain impurities, it is possible to provide a silica-based composite microparticle dispersion that can be preferably used for polishing the surfaces of semiconductor devices such as semiconductor substrates and wiring substrates. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] Patent No. 2,746,861 [Patent Document 2] JP 2013-119131 A [Patent Document 3] International Publication No. 2016 / 159167 Brochure [Non-patent literature]

[0010] [Non-Patent Document 1] Seung-Ho Lee, Zhenyu Lu, SVBabu and Egon Matijevic, "Chemical mechanical polishing of thermal oxide films using silica particles coated with ceria", Journal of Materials Research, Volume 17, Issue 10, 2002, pp2744-2749 Summary of the Invention [Problem to be solved by the invention]

[0011] However, when the present inventors actually produced and examined the cerium oxide ultrafine particles described in Patent Document 1, they found that the polishing rate was low and that the particles were prone to cause defects on the surface of the polishing substrate (deterioration of surface accuracy, increased scratches, and residue of abrasive on the surface of the polishing substrate). The inventors believe that the main reason for this is that, compared to methods for producing ceria particles that include a calcination step (calcination increases the crystallinity of the ceria particles), the method for producing cerium oxide ultrafine particles described in Patent Document 1 does not include a calcination step and simply crystallizes cerium oxide particles from a liquid phase (an aqueous solution containing cerium nitrate), so the crystallinity of the cerium oxide particles produced is relatively low; further, because no calcination process is performed, the cerium oxide does not adhere to the base particles, and so the cerium oxide remains on the surface of the polishing substrate.

[0012] In addition, since the ceria-coated silica described in Non-Patent Document 1 is not fired, the actual polishing rate is thought to be low. In addition, since it is not fixed and integrated with the silica particles, it easily falls off, resulting in a decrease in the polishing rate, a lack of polishing stability, and there is also a concern that particles will remain on the surface of the polishing substrate.

[0013] Furthermore, the present inventors have found that when polishing is performed using silica-based composite particles having an oxide layer C described in Patent Document 2, impurities such as aluminum may remain on the surface of the semiconductor device, which may adversely affect the semiconductor device. Furthermore, the ceria particles described in these documents are attached to the base particles, but are not strongly fixed and therefore tend to fall off from the base particles. Furthermore, when polishing is performed using an abrasive in which crystalline ceria particles are formed on spherical silica mother particles as described in Patent Document 2, the removal rate of the silica film is high due to the chemical reaction that occurs simultaneously with the mechanical action of the ceria particles during polishing. However, under high pressure conditions, the ceria crystals may fall off, wear down, or collapse, reducing the contact area between the substrate and the ceria, which may result in a slow removal rate.

[0014] Furthermore, the silica-based composite microparticle dispersion described in Patent Document 3 is capable of exhibiting excellent polishing performance (polishing speed, high surface precision, etc.) in polishing applications. However, with the ever-increasing density and integration of semiconductor devices, there is a demand for an abrasive dispersion with even better polishing performance for semiconductor substrates, in particular an improved polishing speed.

[0015] The present invention aims to solve the above problems. That is, the present invention aims to provide a particle-linked ceria-based composite microparticle that can polish even silica films, Si wafers, and difficult-to-process materials at high speed, achieves high surface accuracy (low scratches, few abrasive grains remaining on the substrate, improved substrate Ra value, etc.), and is preferably used for polishing the surfaces of semiconductor devices such as semiconductor substrates and wiring substrates when it does not contain impurities, and is particularly suitable for high-speed polishing, a dispersion containing the particle-linked ceria-based composite microparticle, a method for producing the dispersion, and a polishing abrasive dispersion containing the particle-linked ceria-based composite microparticle dispersion. [Means for solving the problem]

[0016] The present inventors have conducted extensive research to solve the above problems and have completed the present invention. The present invention relates to the following [1] to

[12] . [1] A base particle having a cerium-containing silica layer on its surface, the base particle being composed of a plurality of primary silica particles having a particle diameter in the range of 50 to 600 nm as measured by a STEM-EDS analysis method, the primary silica particles being connected via a cerium-containing silica layer; child particles dispersed within the cerium-containing silica layer; The particle-connected ceria-based composite particles have the following characteristics (1) to (3): (1) The short diameter / long diameter ratio of the inter-particle type ceria-based composite fine particles is in the range of 0.1 to 0.9. (2) The projected area (T) of the three-dimensional part of the particle and the projected area (S) of the whole particle of the particle-linked ceria-based composite fine particles, which are determined from a scanning electron micrograph, satisfy the relationship of the following general formula (I): T / S×100=0: General formula (I) (3) Neither of the two portions α and β on the outer edge and on the major axis of the particle identified from a scanning electron micrograph of the particle-connected ceria-based composite fine particle has a pointed structure. [2] The particle-linked ceria-based composite particles according to the above [1], wherein the particle-linked ceria-based composite particles have a non-kurtosis in the range of 0.85 to 1.0. [3] The particle-linked ceria-based composite microparticles according to the above [1] or [2], having the base particle in which 4 to 10 of the primary silica microparticles are linked via the cerium-containing silica layer. [4] A particle-linked ceria-based composite microparticle dispersion in which the particle-linked ceria-based composite microparticles according to any one of the above [1] to [3] are dispersed in a solvent. [5] A particle-linked ceria-based composite microparticle dispersion comprising the particle-linked ceria-based composite microparticles according to any one of the above [1] to [3], in which a group of linked particles having the following characteristics (4) to (7) is dispersed in a solvent: (4) The average particle size of the linked particle group as measured by dynamic light scattering is 100 to 600 nm. (5) The average particle size of the primary silica particles in the connected particle group is in the range of 50 to 600 nm as measured by STEM-EDS analysis. (6) The ratio of minor axis to major axis of the connected particles is in the range of 0.1 to 0.9. (7) The sum of the projected areas of the three-dimensional portions of the particles (T') and the sum of the projected areas of the entire particles (S') obtained from a scanning electron micrograph of the group of connected particles satisfy the relationship of the following general formula (II): T' / S'×100≦30: General formula (II) [6] The particle-linked ceria-based composite fine particle dispersion according to the above [5], wherein the linked particles have a non-kurtosis in the range of 0.85 to 1.0. [7] The particle-linked ceria-based composite microparticle dispersion according to the above item [5] or [6], wherein the mother particle of the particles constituting the linked particle group is formed by linking 4 to 10 of the primary silica microparticles via the cerium-containing silica layer. [8] The particle-linked ceria-based composite microparticle dispersion according to any one of the above [5] to [7], characterized in that, among particles in the linked particle group having the base particle in which four or more of the primary silica microparticles are linked via the cerium-containing silica layer, the number ratio of particles having the base particle in which the primary silica microparticles are linked while extending in a planar shape is 60% or more. [9] The particle-linked ceria-based composite microparticle dispersion according to any one of the above [5] to [8], characterized in that the particle-linked particle group has a plurality of peaks in a particle-linked number distribution.

[10] A polishing abrasive dispersion comprising the particle-linked ceria-based composite fine particle dispersion according to any one of the above [6] to [9].

[11] A method for producing a particle-linked ceria-based composite microparticle dispersion, the method comprising the steps of: maintaining a dispersion having a solid content concentration of 1 to 20 mass%, at a pH range of 2.0 to 6.0 and a temperature range of 50 to 180°C, in which ceria-based composite microparticles having primary silica microparticles, a cerium-containing silica layer on the surfaces of the primary silica microparticles, and child particles dispersed inside the cerium-containing silica layer, the primary silica microparticles being mainly composed of amorphous silica and the child particles being mainly composed of crystalline ceria, and having an average particle diameter of 50 to 350 nm as measured by a dynamic light scattering method are dispersed in a solvent.

[12] A method for producing the particle-linked ceria-based composite microparticle dispersion according to the above item

[11] , comprising the steps of: maintaining the dispersion having a solid content concentration of 1 to 20% by mass at a pH in the range of 2.0 to 6.0 and at a temperature in the range of 50 to 180°C, and then maintaining the dispersion at a pH of 10.0 or higher and at a temperature in the range of 50 to 98°C, and then continuously or intermittently adding a silicic acid liquid thereto, thereby preparing the particle-linked silica-based microparticle dispersion in which the particles have been grown. Effect of the Invention

[0017] The particle-linked ceria-based composite microparticle dispersion of the present invention contains the particle-linked ceria-based composite microparticles that are elongated in a plane as a main component. When the particle-linked ceria-based composite microparticles that are elongated in a plane are used as abrasive grains, the stress is easily dispersed at multiple contact points with the polishing substrate compared to spherical ceria-based composite microparticles that do not have a connected structure or particle-linked ceria-based composite microparticles that have a three-dimensional branched structure, so that the occurrence of polishing scratches can be suppressed. Furthermore, the connection structure allows the dynamic contact area to be effectively obtained by the rotational movement of the abrasive grains, so that excellent polishing characteristics can be achieved. Therefore, the particle-linked ceria-based microparticle dispersion containing the particle-linked ceria-based microparticles of the present invention is useful, for example, as a raw material for abrasive grain dispersions and polishing compositions, and is particularly excellent in the effect of high polishing speed.

[0018] The particle-linked ceria-based microparticles of the present invention have particle-linked silica-based microparticles as base particles formed by bonding primary silica microparticles together. In such particle-linked silica-based microparticles, it is preferable that the primary silica microparticles are bonded together via a cerium-containing silica layer, which will be described later. The particle-linked ceria-based microparticle dispersion of the present invention exhibits excellent polishing performance as an abrasive dispersion, as described below. In addition, in the case of particle-linked ceria-based composite microparticles that do not contain components other than silica and ceria in the components of the particle-linked ceria-based microparticles, they are more useful when used as abrasives in polishing electronic parts, since they do not cause problems such as contamination of semiconductor substrates.

[0019] When the particle-linked ceria-based composite microparticle dispersion of the present invention is used for polishing purposes, for example as a polishing abrasive dispersion, even difficult-to-process materials such as silica films or Si wafers can be polished at high speed and at the same time high surface precision (low scratches, low surface roughness (Ra) of the polished substrate, etc.) can be achieved. The method for producing a particle-linked ceria-based composite microparticle dispersion of the present invention provides a method for efficiently producing a particle-linked ceria-based composite microparticle dispersion that exhibits such excellent performance. [Brief description of the drawings]

[0020] [Figure 1] 1 is a schematic cross-sectional view of a composite fine particle of the present invention. [Diagram 2] FIG. 2 is a diagram (schematic diagram) for explaining the neck depth. [Diagram 3] FIG. 2 is another schematic diagram of a cross section of a composite fine particle of the present invention. [Figure 4] FIG. 13 is a diagram for explaining non-kurtosis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0021] The present invention will now be described. The present invention relates to particle-linked ceria-based composite particles comprising a mother particle having a cerium-containing silica layer on its surface as well as child particles dispersed within the cerium-containing silica layer, the mother particle being composed of a plurality of primary silica particles each having a particle diameter in the range of 50 to 600 nm as measured by STEM-EDS analysis, the mother particle having the cerium-containing silica layer on its surface as well as child particles dispersed within the cerium-containing silica layer, and the particle-linked ceria-based composite particles having the following characteristics (1) to (3): (1) The short diameter / long diameter ratio of the inter-particle type ceria-based composite fine particles is in the range of 0.1 to 0.9. (2) The projected area (T) of the three-dimensional part of the particle and the projected area (S) of the whole particle of the particle-linked ceria-based composite fine particles, which are determined from a scanning electron micrograph, satisfy the relationship of the following general formula (I): T / S×100=0: General formula (I) (3) Neither of the two portions α and β on the outer edge and on the major axis of the particle identified from a scanning electron micrograph of the particle-connected ceria-based composite fine particle has a pointed structure. Such particle-linked ceria-based composite particles are hereinafter also referred to as "composite particles of the present invention" or "ceria-based composite particles of the present invention".

[0022] The present invention also relates to a particle-linked ceria-based composite microparticle dispersion, in which linked particles containing the composite microparticles of the present invention and having the following characteristics (4) to (7) are dispersed in a solvent. (4) The average particle size of the linked particle group as measured by dynamic light scattering is 100 to 600 nm. (5) The average particle size of the primary silica particles in the connected particle group is in the range of 50 to 600 nm as measured by STEM-EDS analysis. (6) The ratio of minor axis to major axis of the connected particles is in the range of 0.1 to 0.9. (7) The sum of the projected areas of the three-dimensional portions of the particles (T') and the sum of the projected areas of the entire particles (S') obtained from a scanning electron micrograph of the group of connected particles satisfy the relationship of the following general formula (II): T' / S'×100≦30: General formula (II) Such a particle-linked ceria-based composite fine particle dispersion is hereinafter also referred to as the "dispersion of the present invention." The particles contained in the dispersion of the present invention are also referred to as "the linked particle group of the present invention" hereinafter.

[0023] The linked particle group of the present invention includes the composite fine particles of the present invention, but may also include other particles that do not fall under the category of the composite fine particles of the present invention.

[0024] The present invention also relates to a method for producing a particle-linked ceria-based composite microparticle dispersion, the method comprising the steps of: maintaining a dispersion having a solid content concentration of 1 to 20 mass % in a pH range of 2.0 to 6.0 and a temperature range of 30 to 180° C., the dispersion comprising ceria-based composite microparticles having a mean particle diameter of 50 to 350 nm measured by a dynamic light scattering method, the ceria-based composite microparticles having primary silica microparticles, a cerium-containing silica layer on the surfaces of the primary silica microparticles, and child particles dispersed inside the cerium-containing silica layer, the primary silica microparticles being mainly composed of amorphous silica and the child particles being mainly composed of crystalline ceria, in a solvent, at a pH range of 2.0 to 6.0 and a temperature range of 30 to 180° C. Such a production method will be hereinafter referred to as the "production method of the present invention."

[0025] The dispersion of the present invention is preferably produced by the above-mentioned method.

[0026] Hereinafter, when the term "the present invention" is simply mentioned, it means any of the composite fine particles of the present invention, the dispersion of the present invention, the connected particle group of the present invention, and the production method of the present invention.

[0027] In this specification, unless otherwise specified, the term "ceria-based composite microparticles" refers to single-particle ceria-based composite microparticles. Such single-particle ceria-based composite microparticles do not have a connected structure of multiple ceria-based composite microparticles. Such single-particle ceria-based composite microparticles can become "particle-connected ceria-based composite microparticles" through a manufacturing method specified in this application. The single-particle ceria-based composite microparticles have an average particle diameter of 50 to 350 nm as measured by dynamic light scattering, and comprise primary silica microparticles, a cerium-containing silica layer on the surfaces of the primary silica microparticles, and child particles dispersed within the cerium-containing silica layer, the primary silica microparticles being primarily composed of amorphous silica, and the child particles being primarily composed of crystalline ceria. Similarly, unless otherwise specified, when simply referring to a "ceria-based composite fine particle dispersion," it means a dispersion in which the single-particle ceria-based composite fine particles are dispersed in a solvent.

[0028] The base particles of the particle-linked ceria-based composite microparticles in the present invention are linked bodies of primary silica microparticles (particle-linked silica microparticles) in which a plurality of primary silica microparticles having an average particle diameter in the range of 50 to 600 nm measured by STEM-EDS analysis as described above are linked via a cerium-containing silica layer, and the base particles also have the cerium-containing silica layer on their surfaces. Note that in the present application, the base particles may be referred to as "particle-linked silica microparticles".

[0029] <Composite fine particles and connected particle groups of the present invention> The composite fine particles of the present invention will now be described. The composite particles of the present invention are interlocked ceria-based composite particles that are elongated in a planar shape. The present inventors have found that when a dispersion or slurry containing interlocked ceria-based composite particles that are elongated in a planar shape is used as an abrasive, a higher polishing rate can be obtained compared to when spherical particles or interlocked ceria-based composite particles having a three-dimensional branched structure are used as an abrasive.

[0030] In the present application, the particle-linked ceria-based composite microparticles having a three-dimensional branched structure refer to particles in which the projected area (T) of the three-dimensional part of the particle and the projected area (S) of the entire particle, which are determined from a scanning electron micrograph (including a scanning transmission electron micrograph) of the particle-linked ceria-based composite microparticles, satisfy the following relational expression: T / S×100>0 In such particles, the particle-linked ceria-based composite microparticles can be said to have a significant three-dimensional structure, specifically, when the particle-linked ceria-based composite microparticles have a plurality of branched structures in which the branched structures are in a twisted positional relationship, or when the particle-linked ceria-based composite microparticles have only one branched structure and a bent structure, and the bent structure is bent in a three-dimensional direction relative to the branched structure.

[0031] In contrast, the planarly elongated particle-linked ceria-based composite microparticles in the present application are particle-linked ceria-based composite microparticles that do not have a three-dimensional branched structure. Examples of such particle-linked ceria-based composite microparticles include particle-linked ceria-based composite microparticles that have only one bent structure and particle-linked ceria-based composite microparticles that have a branched structure that does not correspond to a three-dimensional branch. Regarding the presence or absence of three-dimensional branching, when the projected area (T) of the three-dimensional portion of the particle and the projected area (S) of the entire particle, determined from a scanning electron microscope (including a scanning transmission electron microscope) photograph of the particle-linked ceria-based composite microparticles, satisfy the relationship of the following general formula (I), the particle-linked ceria-based composite microparticles can be regarded as not having a three-dimensional branched structure and as extending in a plane. T / S×100=0: General formula (I) When a dispersion or slurry containing planarly elongated particle-linked ceria-based composite microparticles is used as an abrasive, it is presumed that the planarly elongated particle-linked ceria-based composite microparticles can have a larger contact surface with the substrate to be polished, thereby improving the polishing speed and other performance properties.

[0032] The structure of the composite fine particles of the present invention is exemplified in Figure 1. Figure 1 shows an embodiment in which the primary silica fine particles constituting the mother particle (particle-linked silica fine particle) are bonded via a cerium-containing silica layer.

[0033] The primary silica particles constituting the base particle are connected in a planar manner. In other words, they do not form a three-dimensional structure. The degree of this is expressed by formula (I) or formula (II). The details of formula (II) will be explained later.

[0034] In addition, although the embodiment shown in FIG. 1 is a type in which some of the child particles are exposed to the outside, in the composite microparticles of the present invention, all of the child particles may or may not be exposed to the outside.

[0035] As shown in Fig. 1, a composite microparticle 20 of the present invention has a mother particle 10 formed by a plurality of primary silica microparticles 1 linked via a cerium-containing silica layer 12. The mother particle 10 also has a cerium-containing silica layer 12 on its surface. Furthermore, the composite microparticle 20 of the present invention has child particles 14 dispersed inside the cerium-containing silica layer 12. The black triangles in Fig. 1 are examples of measurement points X to Z at which STEM-EDS analysis, which will be described later, is performed.

[0036] In the schematic diagram of FIG. 1, the mother particle 10, the cerium-containing silica layer 12, and the child particles 14 are clearly distinguished from each other for ease of understanding. However, in reality, in the composite microparticles of the present invention, the mother particle 10, the cerium-containing silica layer 12, and the child particles 14 exist as a single unit, and it is difficult to clearly distinguish between the mother particle 10, the cerium-containing silica layer 12, and the child particles 14 except by contrast or EDS analysis in STEM-EDS. However, when a STEM-EDS analysis is performed on a cross section of the composite fine particle of the present invention and the element concentrations of Ce and Si are measured, it is possible to confirm that the particle has the structure shown in FIG.

[0037] The STEM-EDS analysis in this application is described below. [STEM-EDS analysis] When a sample containing the composite microparticle of the present invention is subjected to EDS analysis in which an electron beam is selectively irradiated to a location identified by a scanning transmission electron microscope (STEM) and the elemental concentrations of Ce and Si are measured at measurement point X on the cross section of the composite microparticle of the present invention, the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is less than 3%. Furthermore, when the element concentrations of Ce and Si are measured at the measurement point Z, the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is more than 50%. Then, when the element concentrations of Ce and Si are measured at the measurement point Y, the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is 3 to 50%. Therefore, in an element map obtained by performing STEM-EDS analysis, the primary silica particles 1 constituting the base particle 10 in the composite microparticle of the present invention and the cerium-containing silica layer 12 can be distinguished by a line where the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is 3%. Also, in an element map obtained by performing STEM-EDS analysis, the cerium-containing silica layer 12 in the composite microparticle of the present invention and the child particle 14 can be distinguished by a line where the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is 50%.

[0038] Obtaining an elemental map by performing STEM-EDS analysis in this manner and grasping the shape, size, etc. of each of the particles constituting the connected particle group of the present invention or the mother particle, child particle, and cerium-containing silica layer in the composite microparticle of the present invention is also referred to below as the "elemental mapping method." In the present invention, STEM-EDS analysis is performed at a magnification of 200,000 times unless otherwise specified.

[0039] <Mother particle> The base particles in the particles constituting the connected particle group of the present invention and the base particles in the composite fine particles of the present invention will be described below. The primary silica microparticles contained in the base particles of the particles that make up the connected particle group of the present invention and the primary silica microparticles that make up the base particles of the composite microparticles of the present invention are portions in which the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is less than 3% in an element map obtained by an element mapping method.

[0040] By obtaining an element map, it is possible to understand from the shape (contour) of the base particle that the base particle of the composite microparticle of the present invention is a form in which a plurality of primary silica microparticles are connected. In addition, since it is possible to grasp the contour of the base particle in the particle constituting the connected type particle group of the present invention or the primary silica microparticle constituting the base particle of the composite microparticle of the present invention, it is also possible to measure the number of primary silica microparticles constituting the base particle and the particle diameter of each primary silica microparticle.

[0041] The number (connection number) of primary silica fine particles contained in the mother particle in the particles constituting the connected particle group of the present invention and the number (connection number) of primary silica fine particles constituting the mother particle of the composite fine particles of the present invention are not particularly limited, but is preferably 4 to 10 per mother particle, and more preferably 4 to 8. This is because when polishing is performed using the dispersion liquid of the present invention containing such composite fine particles of the present invention, the polishing rate becomes higher.

[0042] In the connected particle group of the present invention, among particles having base particles in which four or more primary silica particles are connected, the percentage of the number of particles having base particles in which the primary silica particles are connected while extending in a plane (number of particles having base particles in which the primary silica particles are connected while extending in a plane / number of particles having base particles in which four or more primary silica particles are connected × 100) is preferably 60% or more, more preferably 70% or more, and even more preferably 80% or more. The reason is that it is easy to reduce polishing scratches due to the above-mentioned stress dispersion and to obtain a polishing rate due to dynamic contact.

[0043] The method for measuring this ratio will now be described. First, for the connected particle group of the present invention, the primary silica fine particles constituting the base particle are identified by the above-mentioned STEM-EDS method, and the base particle is further identified from its shape to measure the number of connections constituting one base particle. Then, 50 particles including base particles in which four or more primary silica fine particles are connected are identified. Next, the percentage of the number of particles having base particles in which the primary silica fine particles are connected while extending in a planar shape is determined among the identified particles having base particles in which four or more primary silica fine particles are connected. In addition, in the case where the primary silica particles are not extended on a plane, that is, as the mother particles contained in the particle-linked ceria-based composite particles having a three-dimensional branched structure, there are particles having a plurality of branched structures, in which the branched structures are in a twisted positional relationship, particles having only one branched structure and a bent structure, and the bent structure is bent in a three-dimensional direction relative to the branched structure, and other examples include aggregated particles (pyramidal or irregular shapes) and single particles (not having any connected structure). Details of the measurement method are described later in "Physical Property Test 7".

[0044] The particle diameter of the primary silica particles constituting the base particles of the composite particles of the present invention is 50 to 600 nm, preferably 60 to 400 nm. The particle diameter of the primary silica particles is determined by identifying the base particles (parts where the ratio (percentage) of Ce molar concentration to the sum of Ce molar concentration and Si molar concentration (Ce / (Ce+Si)×100) is less than 3%) in an element map of the composite particles of the present invention obtained by the element mapping method using STEM-EDS as described above, identifying the primary silica particles constituting the base particles from their shapes, measuring the major axis and minor axis of the primary silica particles, and taking the average value as the particle diameter of the primary silica particles (see FIG. 1). In addition, the particle diameters of 50 particles constituting the connected particle group of the present invention were measured in the same manner, and the value obtained by simply averaging them was defined as the average particle diameter of the primary silica fine particles in the connected particle group of the present invention. Details of the measurement method are described later in "Physical property test 1".

[0045] In addition, in an element map obtained by an element mapping method or in an enlarged image (including photographs and pictures) obtained by a scanning electron microscope (SEM) or a transmission electron microscope (TEM), the straight line indicating the maximum diameter of the particle is taken as the long axis, its length is measured and this value is taken as the long axis (DL), a point is determined on the long axis that divides the long axis in half, two points are found where a straight line perpendicular to this point intersects with the outer edge of the particle, and the distance between these two points is measured and taken as the short axis (DS). This method of determining the long axis (DL) and short axis (DS) of a particle is hereinafter referred to as the "long axis and short axis measurement method."

[0046] The fact that the primary silica fine particles constituting the base particles are mainly composed of amorphous silica can be confirmed, for example, by the following method. When the dispersion of the present invention is dried and then pulverized in a mortar, and an X-ray diffraction pattern is obtained using, for example, a conventionally known X-ray diffraction device (for example, RINT1400 manufactured by Rigaku Denki Co., Ltd.), no peaks of crystalline silica such as cristobalite appear. This confirms that the silica contained in the base particles is amorphous. In addition, in such a case, the primary silica fine particles constituting the base particles are considered to be mainly composed of amorphous silica. In addition, the dispersion of the present invention is dried, embedded in resin, and then sputter-coated with Pt, and a cross-sectional sample is prepared using a conventionally known focused ion beam (FIB) device. For example, when the prepared cross-sectional sample is subjected to a conventionally known TEM device and an FFT pattern is obtained using fast Fourier transform (FFT) analysis, no diffraction pattern of crystalline silica such as cristobalite appears. From this, it can be confirmed that the silica contained in the primary silica fine particles that constitute the base particle is amorphous. In such a case, the base particle is considered to be mainly composed of amorphous silica. Another method is to use a conventionally known TEM device to observe the presence or absence of lattice fringes due to the atomic arrangement of the base particles on a cross-sectional sample prepared in a similar manner. If the material is crystalline, lattice fringes according to the crystal structure are observed, and if the material is amorphous, lattice fringes are not observed. This confirms that the silica contained in the base particles is amorphous. In such a case, the primary silica fine particles that make up the base particles are considered to be mainly composed of amorphous silica.

[0047] The particles constituting the connected particle group of the present invention or the composite fine particles of the present invention may have a neck, and the thicker the neck, the more preferable it is, because this can prevent the particle from collapsing due to stress during polishing and suppress the deterioration of the polishing characteristics. In the composite fine particle of the present invention, the term "neck" refers to the outer peripheral portion corresponding to the bonding portion between adjacent primary silica fine particles in the mother particle.

[0048] The average neck depth (Lm) is preferably from 5 to 200 (unit: nm), and more preferably from 5 to 100 (unit: nm).

[0049] The average neck depth means a value determined by the following measurement. [Method of measuring average neck depth] In a scanning electron microscope photograph (magnification: 50,000 times) of the composite microparticles of the present invention contained in the dispersion of the present invention, a straight line R circumscribing both of the outermost layers of the portions corresponding to two adjacent primary silica microparticles (P and Q) as shown in Fig. 2 is obtained at an arbitrary point, and a line segment γ perpendicular to the straight line R is obtained from an outer layer point D of the junction of the portions corresponding to the two primary silica microparticles (the perpendicular point is defined as E), and the length between D and E is defined as the neck depth (L). When multiple straight lines R are obtained, the straight line R is determined so that the value of the neck depth (L) is maximized. The neck depth (L) [nm] is determined at any three points of the same composite fine particle of the present invention, and the average value (Ls) [nm] is calculated. Ls is calculated for 50 particles, and the average value is regarded as the average neck depth (Lm) [nm] of the particles constituting the connected particle group of the present invention.

[0050] <Child Particle> The child particles of the particles constituting the linked particle group of the present invention and the child particles of the composite fine particles of the present invention will be described below. The child particles in the particles constituting the connected particle group of the present invention and the child particles in the composite microparticles of the present invention are those portions in which the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) exceeds 50% in an element map obtained by an element mapping method.

[0051] In the composite fine particles of the present invention, child particles mainly composed of crystalline ceria (hereinafter also referred to as "ceria child particles") are dispersed in a cerium-containing silica layer disposed on the mother particle.

[0052] In the composite fine particles of the present invention, it is preferable that the mother particle has recesses and protrusions on its surface, and that the child particles exist relative to the mother particle in the following form (a), (b) or (c). (a) A form in which a child particle is bonded to a protruding portion of a mother particle via a part of the cerium-containing silica layer. (b) A form in which child particles are bonded to both the convex and concave portions of a mother particle via a part of the cerium-containing silica layer. (c) A form in which a child particle is bonded to a recess of a mother particle via a part of the cerium-containing silica layer. It is desirable that these forms (a), (b) and (c) exist simultaneously. This is because, when the dispersion of the present invention is used as an abrasive dispersion for polishing, since the mother particle has a step, during polishing, the child particles of form (a) first come into contact with the substrate to be polished and perform polishing. Even if the child particles of form (a) are dislodged, worn or destroyed by the polishing pressure, the ceria child particles of form (b) and (c) come into contact with the substrate to be polished next, and the contact area can be kept large, so that polishing can be performed efficiently and at a stable polishing rate. According to the production method of the present invention described later, it is easy to obtain the dispersion of the present invention containing the composite fine particles of the present invention in which child particles of the form (a), (b) or (c) are simultaneously present.

[0053] In addition, the ceria child particles may be laminated in the cerium-containing silica layer, and the shape of the ceria child particles may be, but is not limited to, a perfect sphere, an ellipse, a rectangle, or the like. Furthermore, the particle size distribution may be uniform or sharp, and steps of the ceria child particles may be formed due to the formation of protrusions or uneven shapes on the mother particles. Some of the ceria subparticles are embedded in the cerium-containing silica layer, while others are partially exposed from the cerium-containing silica layer.

[0054] The average particle size of the child particles is preferably from 10 to 25 nm, and more preferably from 12 to 23 nm. When the average particle size of the child particles exceeds 25 nm, the precursor particles having such ceria child particles tend to be sintered or coagulated after firing and to be difficult to disintegrate in the manufacturing method of the present invention. When such a dispersion of the present invention is used for polishing purposes, it is not preferable because it causes scratches on the object to be polished. When the average particle size of the child particles is less than 10 nm, it tends to be difficult to obtain a polishing rate sufficient for practical use when used for polishing purposes.

[0055] The average particle size of the child particles is determined by identifying the child particles based on the element map obtained by the element mapping method, determining the long diameter (DL) and short diameter (DS) of the child particles by the long diameter / short diameter measurement method, calculating the geometric mean value of these, and taking the simple average of the particle sizes measured for 50 child particles in this manner.

[0056] The child particles may be stacked, i.e., multiple child particles may be present within the cerium-containing silica layer on radial lines extending from the center of the parent particle. Furthermore, the child particles may be embedded in the cerium-containing silica layer or may be partially exposed to the outside of the cerium-containing silica layer. However, when the child particles are embedded in the cerium-containing silica layer, the surface of the ceria-based composite fine particle is closer to the silica surface, improving the storage stability and polishing stability and further reducing the amount of abrasive grains remaining on the substrate after polishing. Therefore, it is preferable that the child particles are embedded in the cerium-containing silica layer.

[0057] The shape of the child particles is not particularly limited. For example, they may be spherical, elliptical, or rectangular. When the dispersion of the present invention is used for polishing purposes and a high polishing rate is to be obtained, the child particles are preferably non-spherical, and more preferably rectangular.

[0058] The child particles dispersed in the cerium-containing silica layer may be in a monodisperse state, in a layered state (i.e., a state in which multiple child particles are stacked in the thickness direction of the cerium-containing silica layer), or in a state in which multiple child particles are connected to each other.

[0059] In the present invention, the child particles preferably contain crystalline ceria as a main component. The fact that the child particles are mainly composed of crystalline ceria can be confirmed, for example, by drying the dispersion of the present invention, grinding the obtained solid matter in a mortar to obtain the composite microparticles of the present invention, and then subjecting the composite microparticles to X-ray analysis using, for example, a conventionally known X-ray diffraction device (for example, RINT1400 manufactured by Rigaku Corporation), and detecting only the crystalline phase of ceria in the obtained X-ray diffraction pattern. In such a case, the child particles are considered to be mainly composed of crystalline ceria. The crystalline phase of ceria is not particularly limited, but examples thereof include cerianite and the like.

[0060] The child particles preferably contain crystalline ceria (crystalline Ce oxide) as a main component, but may contain other elements, such as elements other than cerium, and may also contain a cerium hydrate compound as a polishing promoter. However, as described above, it is preferable that only the ceria crystal phase is detected when the composite microparticles of the present invention are subjected to X-ray diffraction. That is, even if a crystal phase other than ceria is contained, the content of the crystal phase other than ceria is low or the crystal phase is dissolved in the ceria crystal, so that the content is outside the detection range by X-ray diffraction.

[0061] The average crystallite diameter of the ceria child particles is calculated using the full width at half maximum of the maximum peak appearing in the chart obtained by subjecting the particles contained in the connected particle group of the present invention or the composite fine particles of the present invention to X-ray diffraction. For example, the average crystallite diameter of the (111) plane is preferably 10 to 25 nm (full width at half maximum is 0.86 to 0.34°), more preferably 12 to 23 nm (full width at half maximum is 0.72 to 0.37°), and more preferably 15 to 22 nm (full width at half maximum is 0.58 to 0.38°). In many cases, the peak intensity of the (111) plane is the maximum, but the peak intensity of another crystal plane, for example, the (100) plane, may be the maximum. In that case, it can be calculated in the same way, and the size of the average crystallite diameter in that case may be the same as the average crystallite diameter of the (111) plane.

[0062] The method for measuring the average crystallite size of the child particles is shown below using the (111) plane (2θ=approximately 28 degrees) as an example. First, the particles contained in the connected particle group of the present invention or the composite fine particles of the present invention are pulverized using a mortar, and an X-ray diffraction pattern is obtained using, for example, a conventionally known X-ray diffractometer (for example, RINT1400 manufactured by Rigaku Denki Co., Ltd.). Then, the full width at half maximum of the peak of the (111) plane near 2θ=28 degrees in the obtained X-ray diffraction pattern is measured, and the average crystallite size can be calculated using the following Scherrer formula. D=Kλ / βcosθ D: average crystallite size (angstroms) K: Scherrer constant (K=0.94 in the present invention) λ: X-ray wavelength (1.5419 angstroms, Cu lamp) β: Full width at half maximum (rad) θ: reflection angle The measurement method is described in Physical Properties Test 12 below.

[0063] <Cerium-containing silica layer> The cerium-containing silica layer in the particles constituting the connected particle group of the present invention and the cerium-containing silica layer in the composite fine particle of the present invention will be described below.

[0064] The composite particles of the present invention have cerium-containing silica layers between a plurality of primary silica particles and on the surface of the mother particle, and child particles are dispersed within the cerium-containing silica layers. By adopting such a structure, the child particles are less likely to fall off due to the crushing process during production or the pressure during polishing, and even if some of the child particles are chipped off, most of the child particles do not fall off and remain in the cerium-containing silica layer, so that the polishing function is not reduced.

[0065] The cerium-containing silica layer in the particles constituting the connected particle group of the present invention and the cerium-containing silica layer in the composite microparticle of the present invention are portions where the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is 3 to 50% in an element map obtained by an element mapping method.

[0066] In an image (TEM image) obtained by observing the composite particles of the present invention using a transmission electron microscope, the image of the child particle appears dark on the surface of the mother particle, but a part of the cerium-containing silica layer appears as a relatively faint image around and outside the child particle, i.e., on the surface side of the composite particles of the present invention. When this part is subjected to STEM-EDS analysis to determine the Si molar concentration and Ce molar concentration of the part, it can be confirmed that the Si molar concentration is very high. Specifically, the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is 3 to 50%.

[0067] The average thickness of the cerium-containing silica layer is preferably 10 to 40 nm, and more preferably 12 to 30 nm. The average thickness of the cerium-containing silica layer is determined by drawing straight lines at any 12 points from the center of the composite microparticle of the present invention to the outermost shell, measuring the distance between the line where the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is 3% as determined from the element map obtained by performing the STEM-EDS analysis as described above, and the outermost shell of the composite microparticle of the present invention (the distance on the line passing through the center of the mother particle), and then calculating the simple average of these distances. Note that the center of the mother particle refers to the intersection of the major axis and the minor axis as described above.

[0068] The cerium-containing silica layer in the composite microparticles of the present invention is considered to promote the bonding force between the child particles (ceria microparticles mainly composed of crystalline ceria) dispersed and grown in the cerium-containing silica layer during the firing process and the mother particles. Therefore, for example, in the manufacturing method of the present invention, the calcined product dispersion obtained by firing is pre-disintegrated in a dry manner if necessary, then disintegrated in a wet manner, and then centrifuged to obtain a ceria-based composite microparticle dispersion, and the cerium-containing silica layer is considered to have the effect of preventing the child particles from coming off the mother particles. In this case, there is no problem with the localized falling off of the child particles, and it is not necessary that the entire surface of the child particles is covered with a part of the cerium-containing silica layer. It is sufficient that the child particles are strong enough not to come off the mother particles during the disintegration process. Due to this structure, it is believed that when the dispersion of the present invention is used as an abrasive, the removal rate is high and deterioration of surface accuracy and scratches are reduced.

[0069] In addition, in the composite fine particles of the present invention, at least a part of the surface of the child particles is covered with a cerium-containing silica layer, so that the --OH group of silica is present on the outermost surface (outermost shell) of the composite fine particles of the present invention. Therefore, when used as an abrasive, the composite fine particles of the present invention repel each other due to the charge of the --OH group on the polishing substrate surface, and as a result, it is considered that the adhesion to the polishing substrate surface is reduced.

[0070] In addition, ceria generally has a different potential from silica, polishing substrates, and polishing pads, and as the pH goes from alkaline to near neutral, the negative zeta potential decreases, and in the weak acid region, it has a positive potential. Therefore, at an acidic pH during polishing, ceria adheres to the polishing substrate or polishing pad due to differences in the magnitude of potential or polarity, and is likely to remain on the polishing substrate or polishing pad. On the other hand, since the composite fine particles of the present invention have silica in the outermost shell as described above, the potential becomes negative due to silica, so that the composite fine particles of the present invention maintain a negative potential from an alkaline to an acidic pH, and as a result, the abrasive grains are less likely to remain on the polishing substrate or polishing pad. When the composite fine particles of the present invention are crushed while maintaining a pH of 8.6 to 10.8 during the crushing treatment in the manufacturing method of the present invention, a part of the silica (silica in the cerium-containing silica layer) on the surface of the composite fine particles of the present invention is dissolved. If the dispersion of the present invention manufactured under such conditions is adjusted to pH<7 when applied to polishing, the dissolved silica will deposit on the composite fine particles (abrasive grains) of the present invention, and the surface of the composite fine particles of the present invention will have a negative potential. When the potential is low, silicic acid may be added to appropriately reinforce the cerium-containing silica layer.

[0071] In order to adjust the electric potential of the child particles, it is possible to adjust the electric potential using a polymer organic material such as polyacrylic acid, but in the present invention, the silica that is softly attached to the surface adjusts the electric potential, so the use of organic materials is reduced and defects caused by organic materials (residual organic materials, etc.) on the substrate are less likely to occur. In addition, since this softly attached silica has not undergone a baking process, it is a low-density, soft, and easily soluble silica layer. This easily soluble silica layer has an adhesive effect with the substrate, and is effective in improving the polishing rate. This easily soluble silica layer can be confirmed by maintaining the dispersion of the present invention at pH 9 and measuring the silica concentration in the solution obtained by solid-liquid separation. In the dispersion of the present invention, silica may be present in a variety of forms, and may not constitute the composite microparticles of the present invention, but may be present dispersed or dissolved in the solvent, or attached to the surface of the composite microparticles of the present invention.

[0072] The composite fine particles of the present invention have the above-mentioned mother particles, the cerium-containing silica layer, and the child particles. The particles constituting the connected particle group of the present invention include the composite fine particles of the present invention. In the particles constituting the connected particle group of the present invention and in the composite fine particles of the present invention, the mass ratio of silica (SiO2) to ceria (CeO2) is preferably 100:11-316, more preferably 100:30-230, even more preferably 100:30-150, and even more preferably 100:60-120. The mass ratio of silica to ceria is generally considered to be the same as the mass ratio of mother particles to child particles. If the amount of child particles relative to the mother particles is too small, the mother particles or composite fine particles may bond to each other, resulting in the generation of coarse particles. In this case, the polishing agent (polishing slurry) containing the dispersion of the present invention may cause defects (deterioration of surface accuracy such as an increase in scratches) on the surface of the polishing substrate. In addition, if the amount of ceria relative to silica is too large, not only will the cost become expensive, but resource risks will also increase. Furthermore, fusion between particles will progress. As a result, the roughness of the substrate surface will increase (deterioration of surface roughness Ra), scratches will increase, and free ceria will remain on the substrate, and it will also be likely to cause problems such as adhesion to wastewater piping of the polishing device. In addition, the silica to be calculated for the mass ratio of silica (SiO2) to ceria (CeO2) refers to all the silica (SiO2) contained in the particles constituting the connected particle group of the present invention or the composite microparticles of the present invention. Therefore, it refers to the total amount of the silica component constituting the mother particle, the silica component contained in the cerium-containing silica layer arranged on the surface of the mother particle, and the silica component that can be contained in the child particle.

[0073] The silica (SiO2) and ceria (CeO2) contents (mass%) of the particles constituting the connected particle group of the present invention and the composite microparticles of the present invention are determined by first determining the solids concentration of the dispersion of the present invention by subjecting it to ignition loss at 1000°C and then weighing it. Next, the content (mass%) of cerium (Ce) contained in a predetermined amount of particles constituting the connected particle group of the present invention is determined by ICP plasma emission spectrometry and converted into oxide mass% (CeO2 mass% etc.). Then, the components other than CeO2 constituting the particles constituting the connected particle group of the present invention are considered to be SiO2, and the SiO2 mass% can be calculated. In the production method of the present invention, the mass ratio of silica to ceria can also be calculated from the amounts of the silica source material and the ceria source material used when preparing the dispersion of the present invention. This is applicable when the process is not one in which ceria or silica is dissolved and removed, and in such a case, the amounts of ceria or silica used and the analytical values ​​show good agreement. The measurement method is described in Physical Properties Test 11 below.

[0074] [Composite fine particles and connected particle groups of the present invention] The minor axis / major axis ratio of the particles constituting the connected particle group of the present invention and the composite fine particles of the present invention is 0.1 to 0.9, preferably 0.1 to 0.7, and more preferably 0.1 to 0.65. When the dispersion liquid of the present invention containing the composite microparticles of the present invention has such a short diameter / long diameter ratio, when the dispersion liquid of the present invention containing the composite microparticles of the present invention is used for polishing purposes, the polishing rate for the substrate to be polished can be improved and at the same time, the surface roughness on the substrate to be polished can be reduced.

[0075] Here, the minor axis / major axis ratio is a value obtained by determining the major axis (DL) and minor axis (DS) by a major axis / minor axis measurement method in a photographic projection obtained by photographing the particles constituting the connected particle group of the present invention or the composite fine particles of the present invention at a magnification of 300,000 times (or 500,000 times) using a transmission electron microscope, calculating the minor axis / major axis ratio (DS / DL) for any 50 particles, and averaging these values.

[0076] The projected area (T) of the three-dimensional part of the composite fine particle of the present invention and the projected area (S) of the whole particle determined from a scanning electron micrograph satisfy the relationship of the following general formula (I). T / S×100=0: General formula (I) In other words, this means that the particles have no three-dimensional portions and the composite fine particles of the present invention are configured in a planar shape.

[0077] The method for measuring the projected area (T) of the solid part of the particle and the projected area (S) of the whole particle is the same as that described later in "Physical Property Test 5: Calculation of Formula (II)".

[0078] Neither of the two sites α and β, which are on the outer edge and on the major axis of the particle identified from a scanning electron micrograph of the composite fine particle of the present invention, has a pointed structure.

[0079] The structures of the site α and the site β will be described with reference to FIG. Fig. 3 is a schematic diagram of a cross section of a composite microparticle of the present invention, and shows a particle identified from a scanning electron microscope photograph. In Fig. 3, a composite microparticle 20 of the present invention has a mother particle 10 formed by connecting a plurality of primary silica microparticles 1, a cerium-containing silica layer 12 between the primary silica microparticles 1 and on the surface of the mother particle 10, and a child particle 14 dispersed inside the cerium-containing silica layer 12. In addition, DL, which is indicated by a dotted line in FIG. 3, represents the long axis. The composite fine particle 20 of the present invention shown in FIG. 3 does not have a pointed structure at two sites α and β which are on the outer edge of the particle and on the major axis DL. Here, the structure of the pointed portion will be described. First, the long axis DL is determined from a scanning electron micrograph. Next, the intersection points between the major axis DL and the outer edge of the composite microparticle of the present invention are determined and designated as α and β, respectively. The part including the intersection point α is designated as portion α, and the part including the intersection point β is designated as portion β. Next, two tangents are drawn that pass through the intersection point α and circumscribe the outer edge of the composite fine particle of the present invention (that is, the outer edge of the cerium-containing silica layer or the child particle) (these are called tangents D1 and D2). Here, the positions of the outer edge that circumscribes the two tangents are selected so that the angle between the two tangents (the angle on the side including the long axis DL; this angle is designated as Fα) is maximum. Next, similarly, the angle Fβ between the two tangents is measured for the intersection point β. When both Fα and Fβ are 120 degrees or more, the composite fine particle of the present invention does not have a pointed structure.

[0080] The particles constituting the connected particle group of the present invention and the particle-linked ceria-based composite microparticles of the present invention are characterized in that they have a non-pointed particle outer shape. Specifically, the particles constituting the connected particle group of the present invention and the particle-linked ceria-based composite microparticles of the present invention preferably have a non-pointedness in the range of 0.85 to 1.0, more preferably 0.87 to 1.0.

[0081] The non-kurtosis will be explained with reference to Fig. 4. Fig. 4 is a schematic diagram of a cross section of a composite microparticle of the present invention, similar to Fig. 3. The center P of the primary silica microparticle closest to the site α is determined, and a line segment A perpendicular to the tangent line D1 from the center P is defined. Similarly, a line segment B perpendicular to the tangent line D2 from the center P is defined. Also, a line segment C connecting the center P and the intersection point α is defined. Then, the length a of the line segment A, the length b of the line segment B, and the length c of the line segment C are determined, and the non-kurtosis value (Nsv) is calculated by the following formula. (Nsv)=(a+b+c) / 3 Next, the non-kurtosis degree (Nsd) is calculated by dividing (Nsv) by the length (T) of the longest line segment among line segments A, B, and C. (Nsd)=(Nsv) / T Specifically, the non-kurtosis (Nsd) is calculated for both the portion α side and the portion β side of one particle, and the average value is regarded as the non-kurtosis of the particle. With regard to the non-kurtosis of the particles constituting the connected particle group of the present invention, the non-kurtosis of 20 particles is determined, and the average value is calculated to be the non-kurtosis of the particles constituting the connected particle group of the present invention.

[0082] The average particle size of the particles constituting the linked particle group of the present invention or the particle size of the composite fine particles of the present invention is preferably 100 to 600 nm, more preferably 100 to 500 nm. When the average particle size of the particles constituting the linked particle group of the present invention or the particle size of the composite fine particles of the present invention is in such a range, the polishing rate is increased when used as an abrasive, which is preferable. The average particle diameter of the composite microparticles of the present invention means the value obtained by determining the major axis and minor axis using a major axis / minor axis measurement method in a photographic projection obtained by photographing the composite microparticles of the present invention at a magnification of 300,000 times (or 500,000 times) using a transmission electron microscope, and calculating the geometric mean value of these. The average particle size of the particles constituting the linked particle group of the present invention is determined by a dynamic light scattering method. For example, the average particle size can be measured by the cumulant method using a conventionally known particle size measuring device (e.g., ELSZ-1000, manufactured by Otsuka Electronics Co., Ltd.). The measurement method is described in Physical Property Test 3 below.

[0083] The particles constituting the linked particle group of the present invention contained in the dispersion of the present invention preferably have a plurality of peaks in the distribution of the number of linked particles. Usually, polishing with an abrasive dispersion is performed using a polishing pad. There are unevenness and pores of various sizes on the surface of the polishing pad, and it is known that the polishing rate can be increased if the abrasive grains are adequately held in the unevenness and pores. For example, when the ceria-based composite fine particles in the connected particle group of the present invention have multiple peaks in the connection number distribution, they are easily held in the unevenness and pores, which is desirable for increasing the polishing rate. In the present application, the number of connections of the primary silica fine particles was measured (specifically, the measurement method is described in Physical Property Test 2 below), and the number of peaks in the connection number distribution was counted. This measurement method is described in Physical Property Test 8 below. Furthermore, when the particle size distribution of the linked particle group of the present invention contained in the dispersion of the present invention is determined by dynamic light scattering, the particle size distribution also preferably has multiple peaks for the same reasons as in the case of the linkage number distribution described above.

[0084] The projected area (T') of the three-dimensional portion of a particle constituting the connected particle group of the present invention and the projected area (S') of the entire particle, which are determined from a scanning electron micrograph, satisfy the relationship of the following general formula (II). T' / S'×100≦30: General formula (II) In other words, this means that the particles have few three-dimensional portions, and the particles constituting the connected particle group of the present invention are mainly configured in a planar shape.

[0085] In general formula (II), T' / S'×100 is 0 to 30 (i.e., 0≦T' / S'×100≦30), preferably 0.1 to 25 (i.e., 0.1≦T' / S'×100≦25), and more preferably 3 to 20 (i.e., 0.1≦T' / S'×100≦20). In this case, when the dispersion liquid of the present invention containing the linked particle group of the present invention is used as an abrasive, the polishing rate becomes higher.

[0086] Here, the projected area (T') of the solid portion of the particle and the projected area (S') of the entire particle are values ​​obtained by determining the projected area (T) of the solid portion of the particle and the projected area (S) of the entire particle for each of 50 particles using the method described above, and then calculating the geometric mean value.

[0087] The particles constituting the connected particle group of the present invention or the composite fine particles of the present invention have a specific surface area of ​​4 to 100 m 2 / g, and 5 to 70m 2 It is more preferable that the molecular weight is / g.

[0088] Here, a method for measuring the specific surface area (BET specific surface area) will be described. First, a dried sample (0.2 g) is placed in a measurement cell and degassed in a nitrogen gas flow at 250°C for 40 minutes, then the sample is kept at liquid nitrogen temperature in a mixed gas flow of 30% nitrogen by volume and 70% helium by volume to allow the nitrogen to be adsorbed in equilibrium on the sample. Next, the temperature of the sample is gradually raised to room temperature while the mixed gas is being passed through, and the amount of nitrogen desorbed during this period is detected, and the specific surface area of ​​the sample is measured using a calibration curve created in advance. Such a BET specific surface area measurement method (nitrogen adsorption method) can be carried out using, for example, a conventionally known surface area measurement device. In the present invention, the specific surface area means a value obtained by measurement in this manner, unless otherwise specified.

[0089] The contents of the elements Na, Ag, Al, Ca, Cr, Cu, Fe, K, Mg, Ni, Ti, Zn and Zr (hereinafter sometimes referred to as "specific impurity group 1") in the particles constituting the connected particle group of the present invention and in the composite microparticles of the present invention are each preferably 5000 ppm or less, more preferably 1000 ppm or less, more preferably 100 ppm or less, more preferably 50 ppm or less, more preferably 25 ppm or less, more preferably 5 ppm or less, and even more preferably 1 ppm or less. In addition, the content of each of the elements U, Th, Cl, NO3, SO4 and F (hereinafter sometimes referred to as "specific impurity group 2") in the particles constituting the connected particle group of the present invention and in the composite fine particles of the present invention is preferably 5 ppm or less.

[0090] Here, the content of specific impurity group 1 or specific impurity group 2 in the particles constituting the connected particle group of the present invention, the composite fine particles of the present invention, and the silica-based fine particles described below means the content relative to the dry amount. The content in terms of the dry amount means the ratio (percentage) of the weight of the measurement target (specific impurity group 1 or specific impurity group 2) to the mass of the solid content contained in the target. The impurity content of the base particles is roughly the same as the impurity content of the silica-based microparticles if there is no contamination due to contamination, etc.

[0091] Generally, silica-based fine particles prepared using water glass as a raw material contain the specific impurities of group 1 and group 2 derived from the raw water glass in a total amount of several thousand ppm. In the case of a dispersion liquid in which particles containing such silica-based fine particles are dispersed in a solvent, it is possible to reduce the content of the specific impurity group 1 and the specific impurity group 2 by carrying out an ion exchange treatment, but even in that case, the specific impurity group 1 and the specific impurity group 2 remain at a total of several ppm to several hundred ppm. Therefore, when using silica-based fine particles made from water glass, impurities are sometimes reduced by acid treatment or the like. In contrast, in the case of a dispersion in which silica-based microparticles synthesized using alkoxysilane as a raw material are dispersed in a solvent, the content of each element in the specific impurity group 1 is preferably 100 ppm or less, more preferably 20 ppm or less, and the content of each element and each anion in the specific impurity group 2 is preferably 20 ppm or less, more preferably 5 ppm or less.

[0092] In the present invention, the contents of Na, Ag, Al, Ca, Cr, Cu, Fe, K, Mg, Ni, Ti, Zn, Zr, U, Th, Cl, NO3, SO4, and F in the base particles are values ​​determined by measurement using the following methods. ·Na and K: Atomic absorption spectrometry Ag, Al, Ca, Cr, Cu, Fe, Mg, Ni, Ti, Zn, Zr, U and Th: ICP-MS (Inductively Coupled Plasma Atomic Emission Spectroscopy Mass Analysis) ·Cl: Potentiometric titration method NO3, SO4 and F: Ion chromatograph

[0093] <Dispersion of the Present Invention> The dispersion of the present invention will now be described. The dispersion of the present invention is one in which the linked particle group of the present invention as described above is dispersed in a solvent.

[0094] The dispersion of the present invention contains water and / or an organic solvent as a solvent. As the solvent, it is preferable to use water such as pure water, ultrapure water, and ion-exchanged water. Furthermore, the dispersion of the present invention can be suitably used as a polishing slurry by adding at least one additive selected from the group consisting of a polishing accelerator, a surfactant, a pH adjuster, and a pH buffer as an additive for controlling the polishing performance.

[0095] In addition, examples of solvents that can be used in the dispersion liquid of the present invention include alcohols such as methanol, ethanol, isopropanol, n-butanol, and methyl isocarbinol; ketones such as acetone, 2-butanone, ethyl amyl ketone, diacetone alcohol, isophorone, and cyclohexanone; amides such as N,N-dimethylformamide and N,N-dimethylacetamide; ethers such as diethyl ether, isopropyl ether, tetrahydrofuran, 1,4-dioxane, and 3,4-dihydro-2H-pyran; glycol ethers such as 2-methoxyethanol, 2-ethoxyethanol, 2-butoxyethanol, and ethylene glycol dimethyl ether; 2- Organic solvents that can be used include glycol ether acetates such as methoxyethyl acetate, 2-ethoxyethyl acetate, and 2-butoxyethyl acetate; esters such as methyl acetate, ethyl acetate, isobutyl acetate, amyl acetate, ethyl lactate, and ethylene carbonate; aromatic hydrocarbons such as benzene, toluene, and xylene; aliphatic hydrocarbons such as hexane, heptane, isooctane, and cyclohexane; halogenated hydrocarbons such as methylene chloride, 1,2-dichloroethane, dichloropropane, and chlorobenzene; sulfoxides such as dimethyl sulfoxide; and pyrrolidones such as N-methyl-2-pyrrolidone and N-octyl-2-pyrrolidone. These may be mixed with water.

[0096] The solid content concentration in the dispersion of the present invention is preferably in the range of 0.3 to 50% by mass.

[0097] It is preferable that the dispersion of the present invention, when subjected to cationic colloid titration, gives a streaming potential curve in which the ratio (ΔPCD / V) of the streaming potential change (ΔPCD) represented by the following formula (1) to the amount (V) of the cationic colloid titrant added at the tip is −110.0 to −5.0. ΔPCD / V=(IC) / V Equation (1) C: streaming potential at the knick (mV) I: Streaming potential at the beginning of the streaming potential curve (mV) V: Amount of the cationic colloid titrant added in the knick (ml)

[0098] Here, the cationic colloid titration is carried out by adding a cationic colloid titrant to 80 g of the dispersion of the present invention, the solid content of which has been adjusted to 1% by mass. As the cationic colloid titrant, a 0.001N polydiallyldimethylammonium chloride solution is used.

[0099] The streaming potential curve obtained by this cationic colloid titration is a graph in which the amount (ml) of cationic titrant added is plotted on the X-axis and the streaming potential (mV) of the dispersion of the present invention is plotted on the Y-axis. A knick is a point (inflection point) where the streaming potential changes suddenly in the streaming potential curve obtained by cationic colloid titration. The streaming potential at the inflection point is C (mV), and the amount of cationic colloid titrant added at the inflection point is V (ml). The starting point of the streaming potential curve is the streaming potential in the dispersion of the present invention before titration. Specifically, the starting point is the point where the amount of cationic colloid titrant added is 0. The streaming potential at this starting point is I (mV).

[0100] When the above ΔPCD / V value is -110.0 to -5.0, the polishing rate of the polishing agent is further improved when the dispersion of the present invention is used as a polishing agent. It is considered that this ΔPCD / V reflects the degree of coverage of the child particles with the cerium-containing silica layer on the surface of the composite fine particles of the present invention and / or the degree of exposure of the child particles on the surface of the composite fine particles, or the presence of silica that is easily detached. The present inventor presumes that when the ΔPCD / V value is within the above range, the child particles are less likely to be detached during wet disintegration, and the polishing rate is also high. Conversely, when the absolute value of the ΔPCD / V value is larger than -110.0, the surface of the composite fine particles is entirely covered with the cerium-containing silica layer, so that child particles are less likely to fall off during the disintegration process, but silica is less likely to be detached during polishing, and the polishing rate decreases. On the other hand, when the absolute value is smaller than -5.0, it is considered that falling off occurs easily. The present inventor presumes that when it is within the above range, the surface of the child particles is moderately exposed during polishing, so that child particles are less likely to fall off, and the polishing rate is further improved. ΔPCD / V is more preferably from −100.0 to −5.0, and further preferably from −100.0 to −10.0.

[0101] The dispersion of the present invention preferably has a negative streaming potential before the start of cationic colloid titration, i.e., when the titration amount is zero, when its pH value is in the range of 3 to 8. This is because, when this streaming potential is maintained at a negative potential, the abrasive grains (ceria-based composite fine particles) are unlikely to remain on the polishing substrate, which also exhibits a negative surface potential.

[0102] <Production Method of the Present Invention> The production method of the present invention will now be described. In the manufacturing method of the present invention, for example, a ceria-based composite microparticle dispersion liquid in which single-particle ceria-based composite microparticles are dispersed in a solvent is used as a raw material. The ceria-based composite microparticle dispersion liquid in the present application is obtained by, for example, maintaining a dispersion liquid (solid content concentration of 1 to 20% by mass) in which ceria-based composite microparticles (average particle diameter of 50 to 350 nm measured by dynamic light scattering method) having silica primary microparticles (preferably consisting of a single silica-based microparticle), a cerium-containing silica layer on the surface of the silica primary microparticles, and child particles dispersed inside the cerium-containing silica layer, the silica primary microparticles being mainly composed of amorphous silica, and the child particles being mainly composed of crystalline ceria, dispersed in a solvent, at a pH range of 2.0 to 6.0 and a temperature range of 30 to 180°C (preferably 50 to 180°C).

[0103] The dispersion of the present invention is preferably produced by the production method of the present invention. In the production method of the present invention, first, a silica-based fine particle dispersion is prepared.

[0104] The form of the silica-based fine particles is not particularly limited. The silica-based fine particles are mainly composed of amorphous silica, similar to the above-mentioned primary silica fine particles. Here, the definition of the main component is the same as in the case of the primary silica fine particles.

[0105] The average particle size of the silica-based fine particles in the silica-based fine particle dispersion used as the raw material here is smaller than that of the particle-linked ceria-based composite fine particles in the particle-linked ceria-based composite fine particle dispersion obtained by the production method of the present invention.Silica-based fine particles in the range of 50 to 600 nm are preferably used. The average particle diameter of the silica-based microparticles in this silica-based microparticle dispersion is determined by determining the long and short diameters using a long and short diameter measurement method based on a photographic projection obtained by photographing using a scanning electron microscope, and taking the average of these as the particle diameter of the particle. After measuring the particle diameters of 50 particles, the average value is calculated from these.

[0106] In addition, the higher the uniformity of the particle diameter of the silica-based fine particles used as raw material, the higher the durability of the finally obtained particle-linked ceria-based composite fine particles, and the better the polishing performance. If the particle diameter of the primary silica fine particles constituting the particle-linked ceria-based composite fine particles varies widely, for example, when the particle-linked ceria-based composite fine particles are used as polishing abrasives, the particle-linked ceria-based composite fine particles may break, and furthermore, polishing scratches may occur frequently due to stress concentration on the polishing substrate.

[0107] The coefficient of variation (CV value) in the particle size distribution of the silica-based fine particles is preferably 30% or less, more preferably 20% or less. When silica-based fine particles having a coefficient of variation in particle size distribution within this range are used as raw materials, the coefficient of variation in the particle size distribution of primary silica fine particles in the particle-linked ceria-based composite fine particles finally obtained is also approximately the same as that of the raw material, which is preferable in terms of obtaining better polishing performance. The coefficient of variation in the particle size distribution of primary silica fine particles in the particle-linked ceria-based composite fine particles is preferably 30% or less, more preferably 20% or less. Furthermore, when the silica-based fine particles used as the raw material have a high degree of uniformity in the average particle size, the particle size distribution of the finally obtained particle-linked ceria-based composite fine particles can be easily converged to a multiple peak shape.

[0108] The minor axis / major axis ratio of the silica-based fine particles in the silica-based fine particle dispersion used as the raw material is preferably 0.1 or more and less than 1.0, and more preferably 0.1 or more and 0.7 or less. The ratio of the minor axis to the major axis of the silica-based microparticles in this silica-based microparticle dispersion is determined by determining the major axis and minor axis using a major axis and minor axis measurement method based on a photographic projection obtained by photographing using a scanning electron microscope, and then calculating the simple average value of the major axis and minor axis of 50 particles.

[0109] When preparing the dispersion of the present invention for use in polishing semiconductor devices and the like by the manufacturing method of the present invention, it is preferable to use a silica-based microparticle dispersion in which silica-based microparticles produced by hydrolysis of alkoxysilane are dispersed in a solvent as the silica-based microparticle dispersion. When using other conventionally known silica-based microparticle dispersions (such as silica-based microparticle dispersions prepared from water glass as a raw material) as raw material, it is preferable to purify the raw water glass or the acidic silicic acid liquid obtained from water glass by a known method before use, or to acid-treat the obtained silica-based microparticle dispersion and further deionize it before use. In this case, the content of Na, Ag, Al, Ca, Cr, Cu, Fe, K, Mg, Ni, Ti, Zn, U, Th, Cl, NO3, SO4 and F contained in the silica-based microparticles is reduced, specifically, it can be 100 ppm or less. Specifically, the silica-based fine particles in the silica-based fine particle dispersion liquid, which is the raw material, preferably satisfy the following conditions (a) and (b). (a) The content of Na, Ag, Al, Ca, Cr, Cu, Fe, K, Mg, Ni, Ti and Zn is each 100 ppm or less. (b) The contents of U, Th, Cl, NO3, SO4 and F are each 5 ppm or less.

[0110] In addition, silica-based fine particles having a suitable reactivity with cerium (dissolved weight of silica-based fine particles per weight of ceria) are preferably used. By adding a cerium salt aqueous solution to the silica-based fine particles, a part of the silica is dissolved by the cerium salt (cerium hydroxide, etc.), the size of the silica-based fine particles is reduced, and a precursor of a cerium-containing silica layer containing microcrystals of cerium is formed on the surface of the dissolved silica-based fine particles. At this time, if the silica-based fine particles are made of amorphous silica that is highly reactive with cerium, the precursor of the cerium-containing silica layer becomes thick, and the cerium-containing silica layer formed by firing becomes thick or the silica ratio of the layer becomes excessively high, making it difficult to disintegrate in the disintegration process. In addition, if the silica-based fine particles are made of amorphous silica that is extremely low in reactivity with cerium, the cerium-containing silica layer is not sufficiently formed, and the ceria child particles are easily dropped off. When the reactivity with cerium is appropriate, the dissolution of excess silica is suppressed, the cerium-containing silica layer has an appropriate thickness, which prevents the child particles from falling off, and its strength is thought to be greater than the strength between the composite fine particles, which is desirable because it facilitates crushing.

[0111] Next, an aqueous cerium salt solution and an aqueous alkali solution are added to the silica-based fine particle dispersion liquid, and while maintaining the pH of the silica-based fine particle dispersion liquid in the range of 7.0 to 9.0, the aqueous cerium salt solution and the aqueous alkali solution are added continuously or intermittently to prepare a precursor particle dispersion liquid.

[0112] The type of cerium salt is not limited here, but cerium chloride, nitrate, sulfate, acetate, carbonate, metal alkoxide, etc. can be used. Specific examples include cerium (I) nitrate, cerium carbonate, cerium (I) sulfate, and cerium (I) chloride. Among them, trivalent cerium salts such as cerium (I) nitrate, cerium (I) chloride, and cerium carbonate are preferred. This is because crystalline cerium oxide and cerium hydroxide are generated from the solution that becomes supersaturated at the same time as neutralization, and these are rapidly coagulated and deposited on silica-based fine particles, and ultimately CeO2 ultrafine particles are formed in a monodisperse state. Furthermore, trivalent cerium salts react moderately with silica-based fine particles, making it easy to form a cerium-containing silica layer. In addition, trivalent cerium, which is highly reactive with the silica film formed on the polishing substrate, is easily formed in the ceria crystals, making it preferable. However, sulfate ions, chloride ions, nitrate ions, etc. contained in these metal salts are corrosive. Therefore, if desired, it is necessary to remove them to 5 ppm or less in a post-process after preparation by washing. On the other hand, carbonates are preferably used because they are released as carbon dioxide gas during preparation, and alkoxides are decomposed to form alcohols.

[0113] The aqueous alkali solution to be added together with the aqueous cerium salt solution may be any known alkali, such as an aqueous ammonia solution, an aqueous solution of an alkali hydroxide, an aqueous solution of an alkaline earth metal, or an aqueous solution of an amine.

[0114] The amount of cerium metal salt added to the silica-based microparticle dispersion is preferably an amount such that the mass ratio of silica to ceria in the resulting ceria-based composite microparticles is in the range of 100:11 to 316, similar to the case of the composite microparticles of the present invention described above.

[0115] The amount of the alkaline aqueous solution to be added is the amount that maintains the pH at 7.0 to 9.0.

[0116] In addition, the time for adding the cerium salt aqueous solution and the alkaline aqueous solution to the silica-based fine particle dispersion is preferably 0.5 to 24 hours. If this time is too short, the CeO2 ultrafine particles aggregate and become difficult to react with silica on the surface of the silica-based fine particles, which is undesirable because it tends to form particles that are difficult to disintegrate in the disintegration process after firing. Conversely, if this time is too long, the reaction does not proceed any further in the formation of the CeO2 ultrafine particle-containing layer, making it uneconomical. After the addition of the cerium metal salt, the mixture may be aged at 0 to 80° C. if desired. This is because aging promotes the reaction of the cerium compound and has the effect of adhering the free CeO2 ultrafine particles that have not adhered to the silica-based fine particles onto the silica-based fine particles.

[0117] By such a treatment, a dispersion liquid (precursor particle dispersion liquid) containing particles (precursor particles) which are the precursors of the composite fine particles of the present invention can be obtained. It is possible to obtain particles having an average crystallite size of 2.5 nm or more and less than 10 nm of CeO2 ultrafine particles contained in the precursor particles.

[0118] The obtained precursor particle dispersion may be diluted with pure water or ion-exchanged water or concentrated before being subjected to the next treatment. The precursor particle dispersion may be deionized using a cation exchange resin, an anion exchange resin, an ultrafiltration membrane, an ion exchange membrane, or by centrifugation.

[0119] The solid content concentration in the precursor particle dispersion is preferably 1 to 27% by mass.

[0120] Next, the obtained precursor particle dispersion liquid is dried and then fired at 800 to 1200°C.

[0121] The drying method is not particularly limited. It can be dried using a conventionally known dryer. Specifically, a box dryer, band dryer, spray dryer, etc. can be used.

[0122] The drying time is not particularly limited, but is preferably 1 to 64 hours, and more preferably 3 to 24 hours.

[0123] Preferably, the pH of the precursor particle dispersion before drying is set to 6.0 to 7.0, because the surface activity can be suppressed when the pH of the precursor particle dispersion before drying is set to 6.0 to 7.0.

[0124] After drying, the firing temperature is 800 to 1200°C, preferably 1000 to 1100°C, more preferably 1010 to 1090°C, and even more preferably 1030 to 1090°C. When firing is performed in such a temperature range, the crystallization of ceria proceeds sufficiently, and the cerium-containing silica layer in which the ceria child particles are dispersed has an appropriate film thickness, the cerium-containing silica layer is firmly bonded to the silica primary fine particles, and the child particles dispersed in the cerium-containing silica layer are less likely to fall off. Furthermore, firing in such a temperature range makes it difficult for cerium hydroxide and the like to remain. If the temperature is too high, the crystals of ceria may grow abnormally, the cerium-containing silica layer may become too thick, the amorphous silica constituting the silica primary fine particles may crystallize, or the particles may fuse together.

[0125] The firing time is not particularly limited, but is preferably 1 to 20 hours, and more preferably 2 to 10 hours.

[0126] After a roughly powdery sintered body is thus obtained, a solvent is added to the sintered body, and the sintered body is subjected to a wet crushing treatment in the pH range of 8.6 to 10.8 to obtain a dispersion of crushed sintered body. Here, the fired body may be dry-disintegrated before being subjected to the wet disintegration treatment, and then the fired body may be wet-disintegrated.

[0127] As the dry disintegration device, a conventionally known device can be used, for example, an attritor, a ball mill, a vibration mill, a vibration ball mill, etc. Conventionally known wet disintegration devices can be used, and examples of such devices include batch bead mills such as basket mills, horizontal, vertical, and annular continuous bead mills, sand grinder mills, ball mills, rotor-stator homogenizers, ultrasonic dispersion homogenizers, and wet media agitation mills (wet disintegrators) such as impact crushers that collide fine particles in a dispersion liquid. Examples of beads used in wet media agitation mills include beads made from raw materials such as glass, alumina, zirconia, steel, flint, and organic resins.

[0128] The solvent used when the fired body is wet-disintegrated is water and / or an organic solvent. For example, it is preferable to use water such as pure water, ultrapure water, or ion-exchanged water.

[0129] In the wet disintegration, an aqueous alkali solution such as an aqueous ammonia solution is appropriately added so that the pH is in the range of 8.6 to 10.8. If the pH is maintained within this range during wet disintegration, the dispersion of the present invention can be more easily obtained in the end, in which the ratio (ΔPCD / V) of the streaming potential change (ΔPCD) to the amount of cationic colloid titrant added (V) at the knick, as expressed by the above formula (1), is −110.0 to −15.0. When such a dispersion of the present invention is used as an abrasive, the polishing rate is further improved. The inventors of the present invention presume that this is because the cerium-containing silica layer on the surface of the composite fine particle of the present invention becomes appropriately thin, and the child particles are appropriately exposed on a part of the surface of the composite fine particle of the present invention, thereby improving the polishing rate and controlling the falling off of the ceria child particles. Furthermore, they presume that during disintegration, the silica in the cerium-containing silica layer dissolves and is deposited again, forming a soft and easily soluble silica layer on the outermost layer, and that this easily soluble silica layer improves the frictional force by adhesion to the substrate, thereby improving the polishing rate. It is also presumed that because the cerium-containing silica layer is thin or peeled off, child particles tend to be detached to some extent during polishing. ΔPCD / V is more preferably -100.0 to -15.0, and even more preferably -100.0 to -20.0.

[0130] If the fired powder is merely loosened without going through a wet crushing step, or if it is dispersed in a solvent and then stirred, ultrasonically dispersed, or dry crushed or pulverized, or if the wet crushing step is carried out outside the specified pH range, it is difficult for ΔPCD / V to fall within the range of -110 to -5 (preferably -100.0 to -15), and it is difficult to form a soft and easily soluble silica layer. In addition, the ceria elementary particles are not exposed, and the polishing rate tends to be low.

[0131] The solid content concentration of the crushed fired body dispersion is not particularly limited, but is preferably in the range of, for example, 0.3 to 50 mass %.

[0132] Next, it is preferable to subject the sintered product dispersion to a centrifugal separation process at a relative centrifugal acceleration of 300 G or more, and then remove the sedimented components.

[0133] Specifically, it is preferable to classify the sintered crushed dispersion liquid by centrifugation. The relative centrifugal acceleration in the centrifugation is preferably 300G or more. After the centrifugation, it is preferable to remove the sedimentation components. There is no particular upper limit to the relative centrifugal acceleration, but it is preferable to use it at 10,000G or less in practice.

[0134] By such a treatment, a dispersion liquid can be obtained in which ceria-based composite microparticles are dispersed in a solvent, the primary silica microparticles being mainly composed of amorphous silica, the child particles being mainly composed of crystalline ceria, and the ceria-based composite microparticles having an average particle diameter of 50 to 350 nm as measured by dynamic light scattering.

[0135] In the manufacturing method of the present invention, a particle-linked ceria-based composite microparticle dispersion can be obtained by subjecting a dispersion having a solid content concentration of 1 to 20 mass %, in which such ceria-based composite microparticles are dispersed in a solvent, to a treatment including a step of maintaining the dispersion at a pH range of 2.0 to 6.0 and a temperature range of 30 to 180°C (preferably 50 to 180°C).

[0136] The methods for adjusting the conditions such as the solid content, pH, and temperature may be the same as those described above.

[0137] It is preferable to maintain the dispersion having a solid content concentration of 1 to 20% by mass at a pH of 2.0 to 6.0 and at a temperature of 30 to 180°C (preferably 50 to 180°C) and then maintain the pH at 10.0 or higher and the temperature at 50 to 98°C, and add a silicic acid liquid continuously or intermittently to the dispersion. In this case, the bonded portion (neck portion) of the resulting particle-linked ceria-based composite microparticles grows, and the bond between the ceria-based composite microparticles constituting the particle-linked ceria-based composite microparticles becomes stronger. As described above, the alkaline aqueous solution may be added for the purpose of maintaining the pH within the above range.

[0138] By the production method of the present invention, the particle-linked ceria-based composite fine particle dispersion of the present invention can be obtained.

[0139] <Polishing abrasive dispersion liquid> The liquid containing the dispersion of the present invention can be preferably used as a polishing abrasive dispersion (hereinafter also referred to as "polishing abrasive dispersion of the present invention"). In particular, it can be preferably used as a polishing abrasive dispersion for planarizing a semiconductor substrate on which an SiO2 insulating film is formed. In addition, it can be preferably used as a polishing slurry by adding a chemical component to control the polishing performance.

[0140] The abrasive polishing dispersion of the present invention has excellent effects such as high polishing rate when polishing semiconductor substrates and the like, less scratches on the polished surface during polishing, and less abrasive residue on the substrate.

[0141] The abrasive dispersion for polishing of the present invention contains water and / or an organic solvent as a solvent. As the solvent, it is preferable to use water such as pure water, ultrapure water, and ion-exchanged water. Furthermore, the abrasive dispersion for polishing of the present invention can be suitably used as a polishing slurry by adding at least one additive selected from the group consisting of a polishing accelerator, a surfactant, a heterocyclic compound, a pH adjuster, and a pH buffer as an additive for controlling the polishing performance.

[0142] <Polishing accelerator> The polishing abrasive dispersion of the present invention can be used as polishing slurry by adding a conventionally known polishing accelerator as necessary, depending on the type of polishing material.Examples of such accelerators include hydrogen peroxide, peracetic acid, urea peroxide, and mixtures thereof.When using the polishing agent composition containing such a polishing accelerator as hydrogen peroxide, when the polishing material is metal, the polishing speed can be effectively improved.

[0143] Other examples of the polishing accelerator include inorganic acids such as sulfuric acid, nitric acid, phosphoric acid, oxalic acid, and hydrofluoric acid, organic acids such as acetic acid, and the sodium salts, potassium salts, ammonium salts, and amine salts of these acids, and mixtures thereof. In the case of a polishing composition containing these polishing accelerators, when polishing a polished material consisting of multiple components, the polishing rate of a specific component of the polished material can be accelerated, and a flat polished surface can be finally obtained.

[0144] When the abrasive grain dispersion liquid for polishing of the present invention contains a polishing accelerator, the content thereof is preferably 0.1 to 10 mass %, and more preferably 0.5 to 5 mass %.

[0145] <Surfactant and / or hydrophilic compound> In order to improve the dispersibility and stability of the polishing abrasive dispersion of the present invention, a cationic, anionic, nonionic, or amphoteric surfactant or hydrophilic compound can be added. Both the surfactant and the hydrophilic compound have the effect of reducing the contact angle with the polished surface and promoting uniform polishing. As the surfactant and / or hydrophilic compound, for example, those selected from the following group can be used.

[0146] Examples of the anionic surfactant include carboxylates, sulfonates, sulfates, and phosphates. Examples of the carboxylates include soaps, N-acylamino acid salts, polyoxyethylene or polyoxypropylene alkyl ether carboxylates, and acylated peptides. Examples of the sulfonates include alkyl sulfonates, alkylbenzene and alkylnaphthalene sulfonates, naphthalene sulfonates, sulfosuccinates, α-olefin sulfonates, and N-acylsulfonates. Examples of the sulfates include sulfated oils, alkyl sulfates, alkyl ether sulfates, polyoxyethylene or polyoxypropylene alkyl allyl ether sulfates, and alkylamide sulfates. Examples of the phosphates include alkyl phosphates, and polyoxyethylene or polyoxypropylene alkyl allyl ether phosphates.

[0147] Examples of cationic surfactants include aliphatic amine salts, aliphatic quaternary ammonium salts, benzalkonium chloride salts, benzethonium chloride, pyridinium salts, and imidazolinium salts; examples of amphoteric surfactants include carboxybetaine type, sulfobetaine type, aminocarboxylate salts, imidazolinium betaine, lecithin, and alkylamine oxide.

[0148] Examples of nonionic surfactants include ether type, ether ester type, ester type, and nitrogen-containing type, and examples of the ether type include polyoxyethylene alkyl and alkylphenyl ether, examples of the ether ester type include polyoxyethylene ether of glycerin ester, examples of the ester type include polyethylene glycol fatty acid ester, and examples of the nitrogen-containing type include fatty acid alkanolamide, etc. Other examples include fluorine-based surfactants.

[0149] The surfactant is preferably an anionic surfactant or a nonionic surfactant, and the salt includes ammonium salts, potassium salts, sodium salts, etc., with ammonium salts and potassium salts being particularly preferred.

[0150] Further examples of other surfactants, hydrophilic compounds, etc. include esters such as glycerin esters; ethers such as polyethylene glycol; polysaccharides such as alginic acid; amino acid salts such as ammonium glycine salt; polycarboxylic acids and their salts such as polyaspartic acid; vinyl polymers such as polyvinyl alcohol; sulfonic acids and their salts such as ammonium methyl taurate salt; and amides such as propionamide.

[0151] When the substrate to be polished is a glass substrate or the like, any surfactant can be suitably used. However, when the substrate is a silicon substrate for a semiconductor integrated circuit or the like, and the influence of contamination by alkali metals, alkaline earth metals, halides, or the like must be avoided, it is preferable to use an acid or an ammonium salt-based surfactant.

[0152] When the polishing abrasive dispersion of the present invention contains a surfactant and / or a hydrophilic compound, the total content thereof is preferably 0.001 to 10 g, more preferably 0.01 to 5 g, and particularly preferably 0.1 to 3 g, per liter of the polishing abrasive dispersion.

[0153] The content of the surfactant and / or hydrophilic compound is preferably 0.001 g or more per liter of the polishing abrasive grain dispersion in order to obtain a sufficient effect, and is preferably 10 g or less in order to prevent a decrease in the polishing rate.

[0154] The surfactant or hydrophilic compound may be used alone or in combination with two or more kinds.

[0155] <Heterocyclic compounds> Regarding the abrasive grain dispersion liquid of the present invention, when the substrate to be polished contains metal, a heterocyclic compound may be contained for the purpose of forming a passive layer or a dissolution inhibition layer on the metal to suppress the erosion of the substrate to be polished. Here, the "heterocyclic compound" is a compound having a heterocyclic ring containing one or more heteroatoms. The heteroatom means an atom other than a carbon atom or a hydrogen atom. The heterocyclic ring means a cyclic compound having at least one heteroatom. The heteroatom means only an atom that forms a constituent part of the ring system of the heterocyclic ring, and does not mean an atom that is located outside the ring system, separated from the ring system by at least one non-conjugated single bond, or is a part of a further substituent of the ring system. Preferred examples of the heteroatom include a nitrogen atom, a sulfur atom, an oxygen atom, a selenium atom, a tellurium atom, a phosphorus atom, a silicon atom, and a boron atom, but are not limited thereto. As examples of the heterocyclic compound, imidazole, benzotriazole, benzothiazole, tetrazole, etc. can be used. More specifically, 1,2,3,4-tetrazole, etc. can be mentioned, but are not limited thereto.

[0156] Regarding the content when a heterocyclic compound is blended in the abrasive grain dispersion liquid of the present invention, it is preferably 0.001 to 1.0% by mass, more preferably 0.001 to 0.7% by mass, and even more preferably 0.002 to 0.4% by mass.

[0157] <pH adjuster> If necessary, such as to enhance the effects of the above additives, an acid or a base and their salt compounds can be added to adjust the pH of the polishing composition.

[0158] When adjusting the abrasive grain dispersion liquid of the present invention to pH 7 or higher, an alkaline substance is used as the pH adjuster. Desirably, amines such as sodium hydroxide, aqueous ammonia, ammonium carbonate, ethylamine, methylamine, triethylamine, and tetramethylamine are used.

[0159] When adjusting the abrasive grain dispersion liquid of the present invention to a pH of less than 7, an acidic substance is used as the pH adjuster. For example, mineral acids such as hydrochloric acid and nitric acid, and hydroxy acids such as acetic acid, lactic acid, citric acid, malic acid, tartaric acid, and glyceric acid are used.

[0160] <pH buffer> In order to keep the pH value of the abrasive grain dispersion liquid of the present invention constant, a pH buffer may be used. As the pH buffer, for example, phosphates and borates or organic acid salts such as ammonium dihydrogen phosphate, diammonium hydrogen phosphate, ammonium tetraborate tetrahydrate, etc. can be used.

[0161] Also, as the solvent of the abrasive grain dispersion liquid of the present invention, for example, alcohols such as methanol and ethanol; ketones such as acetone; amides such as N,N-dimethylformamide; ethers such as diethyl ether; glycol ethers such as 2-methoxyethanol; glycol ether acetates such as 2-methoxyethyl acetate; esters such as methyl acetate and ethyl acetate; aromatic hydrocarbons such as benzene, toluene, and xylene; aliphatic hydrocarbons such as hexane, heptane, isooctane, and cyclohexane; halogenated hydrocarbons such as methylene chloride; sulfoxides such as dimethyl sulfoxide; pyrrolidones such as N-methyl-2-pyrrolidone and N-octyl-2-pyrrolidone and other organic solvents can be used. These may be used by mixing with water.

[0162] The solid content concentration contained in the abrasive grain dispersion liquid of the present invention is preferably in the range of 0.3 to 50% by mass. If this solid content concentration is too low, the required polishing rate may not be achieved. On the contrary, when the solid content concentration is too high, there are few cases where the polishing rate is further improved.

Examples

[0163] Regarding the particles contained in the particle-linked ceria-based composite particle dispersion liquid obtained in the examples described later and the dispersion liquid obtained in the comparative examples, the following physical property tests and polishing property tests were conducted.

[0164] <Physical property test 1: Average particle size of primary silica particles in connected particle group> First, for the dispersions obtained in the respective Examples and Comparative Examples, element maps were obtained by the element mapping method described above using STEM-EDS. Next, the mother particles (parts where the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) is less than 3%) were identified in the element map, and the primary silica microparticles that constituted the mother particles in the element map were identified from their shapes. Next, the major axis and minor axis of the primary silica fine particles were measured by a major axis / minor axis measuring method, and the simple average value was taken as the particle size of the primary silica fine particles (see FIG. 1). In this manner, the particle diameters of the primary silica fine particles among 50 particles contained in the dispersion were measured, and the value obtained by simple averaging was regarded as the average particle diameter of the primary silica fine particles among the particles (the connected particle group of the present invention) contained in the dispersion. In the examples and comparative examples, a STEM-EDS (product number: JEM2100, manufactured by JEOL Ltd.) was used. (In Comparative Example 1, the same measurement was performed on single-particle ceria-based composite fine particles.)

[0165] <Physical property test 2: Number of connected primary silica particles in the connected particle group of the present invention> For the dispersions obtained in each of the Examples and Comparative Examples, the base particles were identified by element mapping, and the primary silica particles constituting the base particles were identified from their shapes, and the number of connected primary silica particles constituting one base particle was measured. Then, the number of linked primary silica particles was measured for 50 base particles, and the geometric mean value was calculated, and the obtained value was regarded as the number of linked particles in the dispersion.

[0166] <Physical property test 3: Measurement of average particle size of connected particle group of the present invention> The average particle size of the particle-linked ceria-based composite microparticle dispersion obtained in each Example and Comparative Example was determined by dynamic light scattering. Specifically, the average particle size of the particle-linked ceria-based composite microparticles contained in the particle-linked ceria-based composite microparticle dispersion was measured by the cumulant method using a particle size measuring device ELSZ-1000 manufactured by Otsuka Electronics Co., Ltd. In Comparative Example 1, the same measurement was carried out on single-particle ceria-based composite fine particles.

[0167] <Physical property test 4: Short diameter / long diameter ratio of particle-connected ceria-based composite fine particles> The particles constituting the linked particle group contained in the particle-linked ceria-based composite microparticle dispersion obtained in each Example and Comparative Example were photographed by a transmission electron microscope (TEM) at a magnification of 300,000 times (or 500,000 times), and the major axis (DL) and minor axis (DS) of 50 or more particles in the obtained photographic projection were measured by a major axis / minor axis measurement method, and the geometric mean values ​​were calculated and the obtained values ​​were regarded as the major axis (DL) and minor axis (DS) of the particle-linked ceria-based composite microparticle.The minor axis / major axis ratio was then calculated. In Comparative Example 1, the same measurement was carried out on single-particle ceria-based composite fine particles.

[0168] <Physical property test 5: Calculation of formula (II)> Images or photographs of the particles constituting the linked particle group contained in the particle-linked ceria-based composite microparticle dispersion obtained in each Example and Comparative Example were obtained using a scanning electron microscope at 50,000 magnifications, and the projected area (S) of the entire particle was determined from the SEM image using image analysis software (e.g., Avizo ver. 6.0 manufactured by Visualization Sciences Group). Furthermore, the three-dimensional parts on the same particle were visually determined, and only those three-dimensional parts were specified and the projected area (T) of the three-dimensional parts was determined using the same software. Next, for 50 randomly selected particles, the projected area (T) of the solid portion and the projected area (S) of the entire particle were determined in the same manner, and the geometric mean value was calculated and the obtained value was defined as the projected area (T') of the solid portion of the particles constituting the connected particle group and the projected area (S') of the entire particle. Then, the value of T' / S' x 100 was calculated. In Comparative Example 1, the same calculation was carried out for single-particle ceria-based composite fine particles.

[0169] <Physical property test 6: Measurement of non-peakedness> The non-peak value and non-peak degree of the particles constituting the connected particle group contained in the particle-linked ceria-based composite microparticle dispersion liquid obtained in each Example and Comparative Example were measured by preparing images or photographs of the particles constituting the connected particle group contained in the particle-linked ceria-based composite microparticle dispersion liquid obtained in each Example and Comparative Example, which were obtained by using a scanning electron microscope at a magnification of 50,000 times, and measuring them by the above-mentioned method. Note that in Comparative Example 1, the single-particle ceria-based composite microparticle was similarly measured.

[0170] <Physical property test 7: Proportion of connected particles that are elongated in a plane> A method for measuring the proportion of connected particles extending in a planar manner will be described for the particles constituting the connected particle group contained in the particle-connected ceria-based composite microparticle dispersion obtained in each Example and Comparative Example. For the particles constituting the connected particle group, the mother particles are identified by the STEM-EDS method as in the physical property test 1, and the primary silica microparticles constituting the mother particles are identified from their shapes to measure the number of connections constituting one mother particle. Then, 50 particles including mother particles in which four or more primary silica microparticles are connected are identified. Next, the proportion (percentage) of the number of particles having mother particles in which the primary silica microparticles are connected while extending in a planar manner is calculated among the particles having mother particles in which four or more primary silica microparticles are connected. Whether or not the primary silica fine particles are extended in a planar shape is judged according to the above-mentioned criteria.

[0171] <Physical property test 8: Number of peaks in the linkage number distribution> For the particle-linked ceria-based composite microparticle dispersions obtained in each Example and Comparative Example, the number of links of the primary silica microparticles was measured for 50 base particles in the same manner as in the method described in Physical Property Test 2, and the number of peaks in the linkage number distribution (X-axis: linkage number, Y-axis: number of particles having each linkage number) was counted. Note that in Comparative Example 1, the same measurement was performed on single-particle ceria-based composite microparticles.

[0172] <Physical property test 9: Measurement of the coefficient of variation of particle size distribution of silica-based fine particles> The silica-based microparticle dispersion liquid (silica concentration 0.05% by mass) used as the raw material was photographed with a scanning electron microscope (SEM) at a magnification of 50,000 times, the average particle size of 50 silica-based microparticles was measured, their standard deviation was calculated, and the standard deviation was divided by the average value to calculate the coefficient of variation (CV value) [%] in the particle size distribution of the silica-based microparticles. The scanning electron microscope used was the aforementioned JEOL Ltd., product number: JEM2100. Note that in Comparative Example 1, the same measurement was performed on single-particle ceria-based composite microparticles.

[0173] <Physical property test 10: Measurement of average neck depth (Lm)> The average neck depth of the connected particle group of the present invention obtained in each of the examples and comparative examples was measured by the above-mentioned method.

[0174] <Physical property test 11: Measurement of the ratio of SiO2 content to CeO2 content (parts by mass)> The methods for measuring the CeO2 content and SiO2 content in the particles contained in the particle-linked ceria-based composite microparticle dispersions obtained in the Examples and Comparative Examples will be described. First, the particle-linked ceria-based composite microparticle dispersion was subjected to 1000°C ignition loss to determine the mass of the solid content, and then the Si content was measured by the standard addition method using an ICP plasma emission spectrometer (e.g., SPS5520, manufactured by SII) to calculate the SiO2 mass%. Next, the CeO2 content (mass%) was calculated assuming that the solid content component other than SiO2 was CeO2. Then, the ratio (mass parts) of the SiO2 content to the CeO2 content was calculated. Note that in Comparative Example 1, the same measurement was performed on single-particle ceria-based composite microparticles.

[0175] <Physical property test 12: Measurement of crystal type and average crystallite size> The particle-linked ceria-based composite microparticle dispersions obtained in the examples and comparative examples were dried using a conventionally known dryer, and the resulting powder was ground in a mortar for 10 minutes. The X-ray diffraction pattern was obtained using an X-ray diffractometer (Rigaku Corporation, RINT1400) to identify the crystal type. In addition, the full width at half maximum of the peak of the (111) plane (near 2θ=28 degrees) in the obtained X-ray diffraction pattern was measured, and the average crystallite size was calculated by the above-mentioned Scherrer formula. In Comparative Example 1, the same measurement was performed on the single-particle ceria-based composite fine particles.

[0176] <Polishing performance test 1: Measurement of polishing speed> A polishing abrasive dispersion liquid containing the particle-linked ceria-based composite microparticle dispersion liquid obtained in each of the Examples and Comparative Examples was prepared. The solid content of the polishing abrasive dispersion liquid was 0.6 mass %, and the pH was adjusted to 5.0 by adding nitric acid. Next, a SiO2 insulating film (thickness 1 μm) substrate produced by thermal oxidation was prepared as a substrate to be polished. Next, the substrate to be polished was set in a polishing apparatus (NF300, manufactured by Nanofactor Co., Ltd.), and polishing was performed using a polishing pad ("IC-1000 / SUBA400 concentric type" manufactured by Nitta Haas Corporation) with a substrate load of 0.5 MPa, a table rotation speed of 90 rpm, and a polishing abrasive dispersion liquid supplied at a rate of 50 ml / min for 1 minute. The weight change of the substrate before and after polishing was determined, and the polishing rate was calculated. In Comparative Example 1, the same measurement was carried out on single-particle ceria-based composite fine particles.

[0177] <Polishing performance test 2: Number of scratches> A polishing abrasive dispersion liquid containing the particle-linked ceria-based composite microparticle dispersion liquid obtained in each of the Examples and Comparative Examples was prepared. The solid content of the polishing abrasive dispersion liquid was set to 9 mass %, and the pH was adjusted to 2.0 by adding nitric acid. Next, the aluminum hard disk substrate was set in a polishing device (NF300, manufactured by Nanofactor Co., Ltd.) and polished using a polishing pad (Polytex φ12, manufactured by Nitta Haas Co., Ltd.) with a substrate load of 0.05 MPa, a table rotation speed of 30 rpm, and a polishing abrasive dispersion liquid for 5 minutes supplied at a rate of 20 ml / min. The substrate was then observed over the entire surface at Zoom 15 using an ultrafine defect visualization macro device (product name: Maicro-Max, manufactured by VISION PSYTEC Co., Ltd.). 2 The number of scratches (linear marks) present on the polished substrate surface corresponding to the number of scratches was counted and totaled, and the result was evaluated according to the following criteria. Number of linear scratches Evaluation Less than 50 "Very few" Between 50 and 80 "Few" 80 or more "Many" At least 80 or more, so many that the total cannot be counted. In Comparative Example 1, the same measurement was carried out on single-particle ceria-based composite fine particles.

[0178] [Example 1] Preparation of <Silica-based microparticle dispersion (average particle size of silica-based microparticles: 43 nm)> 12,090 g of ethanol and 6,363.9 g of orthosilicate were mixed to obtain a mixed solution a1. Next, 6,120 g of ultrapure water and 444.9 g of 29% ammonia water were mixed to obtain a mixed solution b1. Next, 192.9 g of ultrapure water and 444.9 g of ethanol were mixed to prepare a bed water. The water was then adjusted to 75°C while stirring, and mixed liquid a1 and mixed liquid b1 were added simultaneously to the water so that the addition would be completed in 10 hours for each. After the addition was completed, the liquid temperature was kept at 75°C for 3 hours for aging, and the solid content was adjusted to obtain 9,646.3 g of a silica-based microparticle dispersion in which silica-based microparticles with a SiO2 solid content of 19% by mass and an average particle diameter of 43 nm measured by a long and short diameter measurement method using a scanning electron microscope photograph were dispersed in a solvent.

[0179] Preparation of silica-based microparticle dispersion (average particle size of silica-based microparticles: 80 nm) 2,733.3 g of methanol and 1,822.2 g of ethyl orthosilicate were mixed to obtain a mixed solution a2. Next, 1,860.7 g of ultrapure water and 40.6 g of 29% ammonia water were mixed to obtain a mixed liquid b2. Next, 59 g of ultrapure water and 1,208.9 g of methanol were mixed to prepare a bed of water, and 922.1 g of the silica-based fine particle dispersion in which the silica-based fine particles having an average particle size of 60 nm obtained in the previous step were dispersed in a solvent was added. The bed water containing the silica-based microparticle dispersion was adjusted to 65°C while stirring, and mixed liquid a2 and mixed liquid b2 were added simultaneously so that the addition would be completed within 18 hours for each. After the addition was completed, the liquid temperature was kept at 65°C for 3 hours for aging, and then the solid concentration (SiO2 solid concentration) was adjusted to 19 mass%, and 3,600 g of high-purity silica-based microparticle dispersion was obtained. The silica-based fine particles contained in this high-purity silica-based fine particle dispersion had an average particle diameter of 80 nm as measured by a long and short diameter measuring method using scanning electron micrographs.

[0180] Next, 114 g of cation exchange resin (SK-1BH manufactured by Mitsubishi Chemical Corporation) was gradually added to 1,053 g of this high-purity silica-based fine particle dispersion (average particle diameter of silica-based fine particles: 108 nm), and the mixture was stirred for 30 minutes to separate the resin. The pH at this time was 5.1. Ultrapure water was added to the obtained silica-based fine particle dispersion liquid to obtain 6,000 g of A-1 liquid having a SiO2 solid content concentration of 3 mass %.

[0181] Next, ion-exchanged water was added to cerium (III) nitrate hexahydrate (Kanto Chemical Co., Ltd., 4N high-purity reagent) to obtain a B-1 solution having a CeO2 content of 2.5% by mass.

[0182] Next, A-1 liquid (6,000 g) was heated to 50°C, and B-1 liquid (8,453 g, equivalent to 117.4 parts by mass of CeO2 per 100 parts by mass of SiO2) was added thereto over 18 hours while stirring. During this time, the liquid temperature was maintained at 50°C, and 3% ammonia water was added as necessary to maintain the pH at 7.9 to 8.7. During the addition of B-1 liquid and during aging, air was blown into the mixed liquid, and the redox potential was maintained at a positive value. After the addition of B-1 liquid was completed, the liquid temperature was raised to 93°C and aged for 4 hours. After aging, the mixture was left to cool indoors and cooled to room temperature, after which it was washed while replenishing ion-exchanged water through an ultrafiltration membrane. The precursor particle dispersion obtained after washing had a solids concentration of 7% by mass, a pH of 9.1 (at 25°C), and an electrical conductivity of 67 μs / cm (at 25°C).

[0183] Next, a 5% by mass aqueous solution of acetic acid was added to the obtained precursor particle dispersion liquid to adjust the pH to 6.5, and the mixture was dried in a dryer at 100°C for 16 hours, and then fired in a muffle furnace at 1088°C for 2 hours to obtain a powder.

[0184] 310 g of the powder obtained after firing and 430 g of ion-exchanged water were placed in a 1 L beaker with a handle, to which a 3% aqueous ammonia solution was added, and the mixture was irradiated with ultrasound for 10 minutes in an ultrasonic bath while stirring to obtain a suspension with a pH of 10 (temperature: 25°C). Next, 595g of φ0.25mm quartz beads were put into a crusher (LMZ06, manufactured by Ashizawa Finetech Co., Ltd.) that had been previously cleaned and operated with water, and the above suspension was further filled into the charge tank of the crusher (filling rate 85%). Considering the ion-exchanged water remaining in the crushing chamber and piping of the crusher, the concentration during crushing was 25% by mass. Then, wet crushing and crushing were performed under the conditions of a disk peripheral speed of 12 m / sec, 25 passes, and a residence time per pass of 0.43 minutes. In addition, 3% aqueous ammonia was added for each pass so that the pH of the suspension during crushing and crushing was maintained at 10.1. In this way, a ceria-based composite microparticle dispersion with a solid content concentration of 22% by mass was obtained.

[0185] The ceria-based composite microparticle dispersion liquid thus obtained, having a solid content concentration of 22% by mass, was centrifuged for 1 minute at a relative centrifugal acceleration of 1700 G in a centrifuge (manufactured by Hitachi Koki Co., Ltd., model number "CR21G") to remove the sedimented components, thereby obtaining a ceria-based composite microparticle dispersion liquid (average particle size (by dynamic light scattering method) 134 nm, solid content concentration 20.5% by mass). 1178 g of pure water was added to 390 g of this ceria-based composite fine particle dispersion (solid content concentration: 20.5% by mass) to dilute it to a solid content concentration of 5.1% by mass. 40 g of cation exchange resin SK1BH was added to 1568 g of this ceria-based composite microparticle dispersion, and the mixture was stirred for 60 minutes to carry out cation exchange. After the cation exchange, the resin was separated using a mesh to obtain a ceria-based composite microparticle dispersion (cation exchange product). From this ceria-based composite microparticle dispersion (cation-exchanged product, solid content concentration 5.1% by mass), 784 g was divided into small portions, to which 24 g of ammonium acetate aqueous solution (acetic acid concentration 7% by mass) was added as a pH buffer to adjust the pH to 4.5, and heat treatment (90°C, 5 hours) was performed to obtain a particle-linked ceria-based composite microparticle dispersion. The average particle diameter of this particle-linked ceria-based composite microparticle dispersion measured by dynamic light scattering was 303 nm. Next, 500 g of the particle-linked ceria-based composite microparticle dispersion (heat-treated product) was divided into small portions, and 25 g of anion exchange resin (SANUP B) was added thereto and stirred for 60 minutes to carry out anion exchange. Subsequently, the resin was separated using a mesh to obtain a particle-linked ceria-based composite microparticle dispersion (anion exchange product).

[0186] For the particle-linked ceria-based composite microparticles contained in the particle-linked ceria-based composite microparticle dispersion (anion-exchanged product) thus obtained, an elemental map was obtained by STEM-EDS analysis (200,000 times magnification) using the method described in [STEM-EDS analysis] above. From this elemental map, it was confirmed that the particle-linked ceria-based composite microparticles according to this embodiment have a mother particle in which a plurality of primary silica microparticles are linked, a cerium-containing silica layer on the surface of the mother particle, and child particles dispersed inside the cerium-containing silica layer. The particle-linked ceria-based fine particle dispersion thus obtained was subjected to physical property tests 1 to 12 and polishing performance tests 1 and 2. The results are shown in Table 1.

[0187] For the dispersion obtained in Example 1, an element map was obtained by the same method as in Physical Property Test 1, and then the particle diameter was calculated by simply averaging the long and short diameters of the primary silica microparticles obtained by the long and short diameter measurement method to find a particle diameter of 101 nm. In a photographic projection diagram obtained by the same method as in Physical Property Test 4, the short diameter / long diameter ratio was calculated from the long diameter (DL) and short diameter (DS) measured by the long and short diameter measurement method to find a particle diameter of 0.8. As in Physical Property Test 5, an image obtained at 50,000 times magnification using a scanning electron microscope or an SEM image in a photograph was used to calculate the projected area (S) of an entire particle using image analysis software. Furthermore, the three-dimensional parts on the particle were visually determined, and only the three-dimensional parts were specified to calculate the projected area (T) of the three-dimensional part using the same software. The T / S calculated from this was 0, and it was confirmed that there were particles in which neither the portion α nor the portion β had a pointed structure (both Fα and Fβ were 120° or more).

[0188] [Example 2] A ceria-based composite fine particle dispersion (average particle size (measured by dynamic light scattering) 134 nm, solid content concentration 20.5% by mass) was obtained in the same manner as in Example 1. 402 g of pure water was added to 390 g of this ceria-based composite fine particle dispersion (solid content concentration: 20.5% by mass) to dilute it to a solid content concentration of 10.1% by mass. 40 g of cation exchange resin SK1BH was added to 792 g of this ceria-based composite microparticle dispersion, and the mixture was stirred for 60 minutes to carry out cation exchange. After the cation exchange, the resin was separated using a mesh to obtain a ceria-based composite microparticle dispersion (cation exchange product). From this ceria-based composite microparticle dispersion (cation-exchanged product, solid content concentration 10.1% by mass), 700 g was divided into small portions, to which 43 g of ammonium acetate aqueous solution (acetic acid concentration 7% by mass) was added as a pH buffer to adjust the pH to 4.5, and heat treatment (90°C, 16 hours) was performed to obtain a particle-linked ceria-based composite microparticle dispersion. The average particle diameter of this particle-linked ceria-based composite microparticle dispersion measured by dynamic light scattering was 406 nm.

[0189] For the dispersion obtained in Example 2, an element map was obtained by the same method as in Physical Property Test 1, and then the particle diameter was calculated by simply averaging the long and short diameters of the primary silica microparticles obtained by the long and short diameter measurement method to find a particle diameter of 101 nm. In a photographic projection diagram obtained by the same method as in Physical Property Test 4, the short diameter / long diameter ratio was calculated from the long diameter (DL) and short diameter (DS) measured by the long and short diameter measurement method to find a particle diameter of 0.5. As in Physical Property Test 5, the projected area (S) of an entire particle was calculated using an image obtained at 50,000 times magnification using a scanning electron microscope or an SEM image in a photograph, and further the three-dimensional parts on the particle were visually determined, and only the three-dimensional parts were specified to find the projected area (T) of the three-dimensional part using the same software. The T / S calculated from this was 0, and it was confirmed that there were particles in which neither the portion α nor the portion β had a pointed structure (both Fα and Fβ were 120° or more).

[0190] [Comparative Example 1] [Preparation of silica-based microparticle dispersion] 3,986 g of ion-exchanged water was added to 300 g of fumed silica (AEROSIL50, manufactured by Nippon Aerosil Co., Ltd.), and wet-disintegrated and pulverized using high-purity silica beads having a diameter of 0.25 mm (manufactured by Daiken Chemical Industry Co., Ltd. and bead mill LMZ06, manufactured by Ashizawa Finetech Co., Ltd.) to obtain 4,286 g of a silica-based microparticle dispersion with a solid content of 7% by mass. 3387.7g of ultrapure water and 29.7g of 3% ammonia were added to 2571g of the silica-based particle dispersion obtained above and mixed to obtain 6000g of a dispersion with a SiO2 solid content concentration of 3 mass% (hereinafter also referred to as A-2 liquid). The average particle diameter of the silica-based particles contained in this A-2 liquid (silica-based particle dispersion) (measurement method: long diameter and short diameter measurement method using scanning electron microscope photographs) was 32nm.

[0191] Next, ion-exchanged water was added to cerium nitrate (III) hexahydrate (Kanto Chemical Co., Ltd., 4N high-purity reagent) to obtain an aqueous solution of cerium nitrate with a CeO2 content of 3.0% by mass (hereinafter, also referred to as B-2 solution).

[0192] Next, A-2 solution (6000 g) was kept at 10°C and B-2 solution (7,186 g, CeO2 dry2 15.6 g) was added thereto over 18 hours while stirring. During this time, the liquid temperature was maintained at 10°C, and 3% ammonia water was added as necessary to maintain the pH at 7.9 to 8.7. After the addition was completed, the liquid was aged for 4 hours at a liquid temperature of 10°C. During the addition of B-2 solution and aging, air was blown into the prepared liquid while mixing, and the redox potential was maintained at 100 to 300 mV. After that, washing was performed while replenishing ion-exchanged water through an ultrafiltration membrane. The precursor particle dispersion obtained after washing had a solid content of 4.7% by mass, a pH of 8.2 (at 25° C.), and an electrical conductivity of 19 μs / cm (at 25° C.).

[0193] Next, the obtained precursor particle dispersion liquid was dried in a dryer at 120° C. for 16 hours, and then calcined in a muffle furnace at 1075° C. for 2 hours to obtain a powder (calcined body).

[0194] 300 g of ion-exchanged water was added to 100 g of the powder (calcined body) obtained after calcination, and the pH was adjusted to 10.1 using a 3% aqueous ammonia solution. The mixture was then wet-pulverized (batch-type benchtop sand mill manufactured by Kampe Co., Ltd.) with φ0.25 mm quartz beads (manufactured by Daiken Chemical Industry Co., Ltd.) for 120 minutes. After crushing, the beads were separated by passing the mixture through a 44-mesh wire screen. The solid content of the resulting crushed sintered body dispersion was 5.9% by mass and the weight was 1148 g. During crushing, an aqueous ammonia solution was added to keep the pH at 10.1.

[0195] The disintegrated dispersion was then centrifuged at 1700 G for 102 seconds in a centrifuge (manufactured by Hitachi Koki Co., Ltd., model number "CR21G"), and the light liquid was collected to obtain a ceria-based composite fine particle dispersion.

[0196] For the ceria-based composite microparticles contained in the ceria-based composite microparticle dispersion thus obtained, an elemental map was obtained by STEM-EDS analysis (200,000 times magnification) in the same manner as in Example 1. From this elemental map, it was confirmed that the ceria-based composite microparticle dispersion of Comparative Example 1 is a ceria-based composite microparticle dispersion in which single-particle ceria-based composite microparticles each having a cerium-containing silica layer on the surface of a primary silica microparticle and a child particle dispersed inside the cerium-containing silica layer are dispersed in a solvent. The thus obtained dispersion of single-particle ceria-based microparticles was subjected to physical property tests 1 to 12 and polishing performance tests 1 and 2. The results are shown in Table 1.

[0197] [Table 1]

Claims

1. a base particle which is formed by connecting a plurality of primary silica particles having a particle diameter in the range of 50 to 600 nm as measured by STEM-EDS analysis via a cerium-containing silica layer, and which also has the cerium-containing silica layer on its surface; child particles which are dispersed within the cerium-containing silica layer and which are portions in which the ratio (percentage) of the Ce molar concentration to the sum of the Ce molar concentration and the Si molar concentration (Ce / (Ce+Si)×100) exceeds 50% in an element map obtained by an element mapping method; The ceria-based composite fine particles have the following characteristics (1) to (3): A particle-linked ceria-based composite fine particle dispersion in which a group of linked particles having the characteristics described in the following (4) to (7) is dispersed in a solvent. (1) The inter-particle type ceria-based composite fine particles have a minor axis / major axis ratio in the range of 0.1 to 0.

9. (2) The projected area (T) of the three-dimensional part of the particle and the projected area (S) of the whole particle of the particle-linked ceria-based composite fine particles, which are determined from a scanning electron micrograph, satisfy the relationship of the following general formula (I): T / S×100=0: General formula (I) (3) Neither of the two regions α and β on the outer edge and on the long axis of the particle identified from a scanning electron microscope photograph of the particle-linked ceria-based composite microparticles has a pointed structure, and therefore the particle outer shape of the particle-linked ceria-based composite microparticles is sharp. (4) The average particle size of the linked particle group is 100 to 600 nm as measured by dynamic light scattering. (5) The average particle size of the primary silica particles in the connected particle group is in the range of 50 to 600 nm as measured by STEM-EDS analysis. (6) The ratio of minor axis to major axis of the connected particles is in the range of 0.1 to 0.

9. (7) The sum of the projected areas of the three-dimensional portions of the particles (T') and the sum of the projected areas of the entire particles (S') determined from a scanning electron micrograph of the group of connected particles satisfy the relationship of the following general formula (II): T' / S'×100≦30: General formula (II)

2. 2. The particle-linked ceria-based composite fine particle dispersion according to claim 1, wherein the linked particles have a non-kurtosis in the range of 0.85 to 1.

0.

3. 3. The particle-linked ceria-based composite microparticle dispersion according to claim 1, wherein a mother particle of the particles constituting the linked particle group is formed by linking 4 to 10 of the silica primary microparticles via the cerium-containing silica layer.

4. The particle-linked ceria-based composite microparticle dispersion according to any one of claims 1 to 3, characterized in that, among particles in the linked particle group having the base particle in which four or more of the primary silica microparticles are linked via the cerium-containing silica layer, the number ratio of particles having the base particle in which the primary silica microparticles are linked while extending in a planar shape is 60% or more.

5. 5. The particle-linked ceria-based composite microparticle dispersion according to claim 1, wherein a distribution of the number of linked particles constituting the linked particle group has a plurality of peaks.

6. 6. A polishing abrasive dispersion comprising the particle-linked ceria-based composite fine particle dispersion according to claim 1.

7. 6. A method for producing a particle-linked ceria-based composite microparticle dispersion according to any one of claims 1 to 5, comprising a step of maintaining a dispersion having a solid content concentration of 1 to 20 mass%, in a pH range of 2.0 to 6.0 and a temperature range of 30 to 180°C, in which ceria-based composite microparticles having a mean particle diameter of 50 to 350 nm measured by a dynamic light scattering method are dispersed in a solvent, the dispersion having a solid content concentration of 1 to 20 mass%, at a pH range of 2.0 to 6.0 and a temperature range of 30 to 180°C, the ceria-based composite microparticles having a mean particle diameter of 50 to 350 nm measured by a dynamic light scattering method ... and a solid content concentration of 1 to 20 mass%, in a solvent, the ceria-based composite microparticles having a mean particle diameter of 50 to 350 nm measured by a dynamic light scattering method, and a solid content concentration of 1 to 20 mass%, at a pH range of 2.0 to 6.0 and a temperature range of 30 to 180°C.

8. 8. The method for producing a particle-linked ceria-based composite microparticle dispersion according to claim 7, wherein the dispersion having a solid content concentration of 1 to 20% by mass is maintained at a pH in the range of 2.0 to 6.0 and a temperature in the range of 30 to 180° C., and then maintained at a pH of 10.0 or higher and a temperature in the range of 50 to 98° C., and then a silicic acid liquid is continuously or intermittently added thereto, thereby preparing the particle-linked ceria-based composite microparticles having grown particles.

Citation Information

Patent Citations

  • Non-spherical combined silica sol and method for producing the same

    JP2009137791A

  • Silica-based composite particle and production method thereof

    JP2013119131A

  • Silica-based composite fine particle fluid dispersion, method for producing same and polishing slurry including silica-based composite fine particle fluid dispersion

    JP2017193692A

  • Silica-based composite fine particle dispersion, method for producing the same, and abrasive particle dispersion for polishing containing the same

    JP2017197429A

  • Ceria-based composite fine particle dispersion, production method thereof, and polishing abrasive grain dispersion comprising ceria-based composite fine particle dispersion

    JP2019089670A