Wiring board and manufacturing method thereof

The wiring board design addresses the peeling issues of narrow and wide conductors by using a dual insulating layer structure with specific metal layer configurations, enhancing adhesion and reducing stress transmission for improved conductor integrity.

JP7583680B2Active Publication Date: 2024-11-14KYOCERA CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021107014
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-06-28
Publication Date
2024-11-14
Estimated Expiration
2041-06-28

AI Technical Summary

Technical Problem

Existing methods struggle to maintain the integrity of both narrow and wide wiring conductors on wiring boards, with narrow conductors prone to peeling due to reduced bonding area and wide conductors experiencing poor flatness and stress-induced peeling.

Method used

A wiring board design featuring a first insulating layer with a wide wiring conductor and a second insulating layer with a narrow wiring conductor, where the wide conductor includes a base metal layer and an electroplated layer with reduced stress transmission, and the narrow conductor is embedded in a groove with a base metal layer and electroplated layer for enhanced adhesion.

Benefits of technology

The design ensures that both narrow and wide wiring conductors are less likely to peel off, improving electrical insulation reliability and reducing stress-induced peeling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583680000001
    Figure 0007583680000001
  • Figure 0007583680000002
    Figure 0007583680000002
  • Figure 0007583680000003
    Figure 0007583680000003
Patent Text Reader

Abstract

To provide a wiring board from which both a wiring conductor with a narrow width and a wiring conductor with a wide width are hardly peeled off.SOLUTION: A wiring board according to the present disclosure comprises: a first insulating layer; a second insulating layer that is located on a top face of the first insulating layer; a first wiring conductor that is located on the top face of the first insulating layer and includes a wide width pattern with a width of 150 μm or more; and a second wiring conductor that is located in a groove recessed from a top face of the second insulating layer toward the first insulating layer and includes a narrow width pattern with a width of 15 μm or less. The first wiring conductor includes a first base metal layer that is located on the first insulating layer, and a first electrolytic plating layer that is located on the first base metal layer and is in contact with the second insulating layer on its side face. The second wiring conductor includes a second base metal layer that is located on an inner wall surface of the groove, and a second electrolytic plating layer that fills the groove on the second base metal layer.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a wiring board and a manufacturing method thereof. [Background technology]

[0002] Conventionally, a semi-additive method has been used as a method for forming wiring conductors in wiring boards. The semi-additive method is a method for forming wiring conductors in the following procedure. First, a thin base metal layer is formed on the exposed surface of an insulating layer by electroless plating, sputtering, or the like. Next, a plating resist layer having openings corresponding to the pattern of the wiring conductor is formed on this base metal layer. Next, an electrolytic plating layer is formed on the base metal layer exposed in the openings of the plating resist layer. Next, the plating resist layer is peeled off and removed, and finally, the base metal layer in the portion not covered by the electrolytic plating layer is etched away.

[0003] Meanwhile, in wiring boards, the wiring conductors are becoming finer. For example, there is a demand for the width of the wiring conductor to be 15 μm or less, and for the distance between adjacent wiring conductors to be 15 μm or less. When the width of the wiring conductor is narrow, for example, 15 μm or less, the bonding area between the insulating layer and the wiring conductor via the underlying metal layer becomes small, and the wiring conductor is easily peeled off from the insulating layer. Furthermore, the electrical insulation reliability between adjacent wiring conductors is reduced.

[0004] Therefore, as described in Patent Document 1, a method for forming a wiring conductor consisting of an undercoat metal layer and an electrolytic plating layer remaining in the groove has been proposed. First, a groove corresponding to the pattern of the wiring conductor is formed to a predetermined depth on the surface of the insulating layer by laser processing. Next, a thin undercoat metal layer is formed on the surface of the insulating layer including the inner wall of the groove by electroless plating or sputtering. Next, an electrolytic plating layer is formed on this undercoat metal layer to a thickness that fills the groove. Finally, the undercoat metal layer and the electrolytic plating layer on the insulating layer are polished and removed by chemical mechanical polishing.

[0005] According to this method, a groove for a wiring conductor having a relatively narrow width (for example, 15 μm or less) is filled well with the electrolytic plating layer. However, a groove for a wiring conductor having a relatively wide width (for example, 150 μm or more) is difficult to fill well with the electrolytic plating layer. As a result, in a wide wiring conductor, the upper surface of the wiring conductor is greatly recessed and the flatness is poor. If the thickness of the electrolytic plating layer is further increased to eliminate this recess, the stress generated when forming this electrolytic plating layer becomes large. Therefore, the stress acts largely between the inner wall of the groove for the wide wiring conductor via the base metal layer, and the wide wiring conductor is easily peeled off. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2004-149926 A DISCLOSURE OF THEINVENTION [Problem to be solved by the invention]

[0007] An object of the present disclosure is to provide a wiring board in which both narrow and wide wiring conductors are less likely to peel off. [Means for solving the problem]

[0008] The wiring board according to the present disclosure includes a first insulating layer, a second insulating layer located on the upper surface of the first insulating layer, a first wiring conductor located on the upper surface of the first insulating layer and including a wide pattern having a width of 150 μm or more, and a second wiring conductor located in a groove recessed from the upper surface of the second insulating layer toward the first insulating layer and including a narrow pattern having a width of 15 μm or less. The first wiring conductor includes a first base metal layer located on the first insulating layer, and a first electrolytic plating layer located on the first base metal layer and having a side surface in contact with the second insulating layer. The second wiring conductor includes a second base metal layer located on the inner wall surface of the groove, and a second electrolytic plating layer filled in the groove on the second base metal layer.

[0009] A method for manufacturing a wiring board according to the present disclosure includes the steps of: forming a first insulating layer; forming a first wiring conductor on an upper surface of the first insulating layer, the first wiring conductor including a wide pattern having a width of 150 μm or more, the first wiring conductor including a first base metal layer and a first electrolytic plating layer located on the first base metal layer; forming a second insulating layer covering the first insulating layer and the first wiring conductor; forming a first groove recessed from the upper surface of the second insulating layer toward the first insulating layer; forming a second base metal layer covering the upper surface of the second insulating layer and the inner wall surface of the first groove, and a second electrolytic plating layer located on the second base metal layer and having a thickness sufficient to fill the first groove; and removing at least the second base metal layer and the second electrolytic plating layer located on the second insulating layer to form a second wiring conductor including a narrow pattern having a width of 15 μm or less located in the groove. Effect of the Invention

[0010] According to the wiring board according to the present disclosure, it is possible to provide a wiring board in which both narrow and wide wiring conductors are less likely to peel off. [Brief description of the drawings]

[0011] [Figure 1] 1 is an explanatory diagram showing a cross section of a wiring board according to a first embodiment of the present disclosure. [Diagram 2] 1A to 1D are explanatory views for explaining a manufacturing process of a wiring board according to a first embodiment of the present disclosure. [Diagram 3] 1A to 1D are explanatory views for explaining a manufacturing process of a wiring board according to a first embodiment of the present disclosure. [Figure 4] 1A to 1C are explanatory views for explaining a manufacturing process of a wiring board according to a first embodiment of the present disclosure. [Diagram 5] 1A to 1C are explanatory views for explaining a manufacturing process of a wiring board according to a first embodiment of the present disclosure. [Figure 6] 1A and 1B are explanatory views for explaining a manufacturing process of a wiring board according to a first embodiment of the present disclosure. [Figure 7]FIG. 11 is an explanatory diagram showing a cross section of a wiring board according to a second embodiment of the present disclosure. [Figure 8] FIG. 11 is an explanatory diagram showing a cross section of a wiring board according to a third embodiment of the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The wiring board of the present disclosure will be described with reference to the drawings. Fig. 1 is a schematic diagram showing a cross section of a wiring board 1 according to a first embodiment of the present disclosure. The wiring board 1 according to the first embodiment includes a core layer 11, a conductor layer 12 located on the surface of the core layer 11, a build-up layer located so as to cover the core layer 11 and the conductor layer 12, and a solder resist 17 located on the surface of the build-up layer.

[0013] The core layer 11 is formed of a resin such as an epoxy resin, a bismaleimide-triazine resin, a polyimide resin, a polyphenylene ether resin, or a liquid crystal polymer. These resins may be used alone or in combination of two or more. The core layer 11 may contain a reinforcing material such as glass cloth, and may further have insulating particles dispersed therein. The insulating particles are not limited, and examples thereof include inorganic insulating fillers such as silica, alumina, barium sulfate, talc, clay, glass, calcium carbonate, and titanium oxide. The core layer 11 has a thickness of, for example, 0.1 mm or more and 2.0 mm or less.

[0014] The conductor layer 12 is located on the main surface of the core layer 11. The conductor layer 12 is formed of a conductor such as copper, for example, copper foil or copper plating. The thickness of the conductor layer 12 is not particularly limited, and is, for example, 5 μm or more and 25 μm or less.

[0015] The core layer 11 has a through-hole conductor 11a for electrically connecting the conductor layers 12 on the upper and lower surfaces of the core layer 11. The through-hole conductor 11a is located in a through-hole penetrating the upper and lower surfaces of the core layer 11. The through-hole conductor 11a is formed of a conductor made of a metal plating such as copper plating. The through-hole conductor 11a is connected to the conductor layers 12 on both sides of the core layer 11. The through-hole conductor 11a may be formed only on the inner wall surface of the through-hole, or may be filled in the through-hole.

[0016] The build-up layer includes a first insulating layer 131, a second insulating layer 132 located on the upper surface of the first insulating layer 131, a first wiring conductor 14 located on the upper surface of the first insulating layer 131, and a second wiring conductor 15 located in a groove 151 recessed from the upper surface of the second insulating layer 132 toward the first insulating layer 131. The build-up layer has the first insulating layer 131, the second insulating layer 132, the first wiring conductor 14, and the second wiring conductor 15 as one unit, and in FIG. 1, there are four such units. The number of such units is not limited to four, and it is sufficient that there is at least one.

[0017] The first insulating layer 131 is formed of a resin such as an epoxy resin, a bismaleimide-triazine resin, a polyimide resin, a polyphenylene ether resin, or a liquid crystal polymer. These resins may be used alone or in combination of two or more. The first insulating layer 131 may have insulating particles dispersed therein. The insulating particles are not limited, and examples thereof include inorganic insulating fillers such as silica, alumina, barium sulfate, talc, clay, glass, calcium carbonate, and titanium oxide. The first insulating layer 131 has a thickness of, for example, 10 μm or more and 50 μm or less.

[0018] The second insulating layer 132 located on the upper surface of the first insulating layer 131 may be made of the same resin as that forming the first insulating layer 131, and may be made of a single resin or a combination of two or more types. Furthermore, the second insulating layer 132 may also have insulating particles dispersed therein similar to those of the first insulating layer 131. The thickness of the second insulating layer 132 is not limited, and may be thinner than the thickness of the first insulating layer 131, for example. The second insulating layer 132 has a thickness of, for example, 5 μm or more and 25 μm or less.

[0019] Core layer 11, first insulating layer 131, and second insulating layer 132 may be formed of the same resin or different resins. Furthermore, when insulating particles are dispersed in core layer 11, first insulating layer 131, and second insulating layer 132, the insulating particles may be the same or different.

[0020] The first wiring conductor 14 located on the upper surface of the first insulating layer 131 includes a wide pattern having a width of 150 μm or more. On the other hand, the first wiring conductor 14 does not include a pattern having a width of 15 μm or less. The first wiring conductor 14 mainly functions as a ground and a power source. As shown in FIG. 1, the first wiring conductor 14 includes a first base metal layer 14a and a first electrolytic plating layer 14b.

[0021] The first undercoat metal layer 14a is a base for the first wiring conductor 14, and is located on the upper surface of the first insulating layer 131. The first undercoat metal layer 14a is made of a metal such as copper. The first undercoat metal layer 14a has a thickness of, for example, 0.1 μm or more and 0.5 μm or less. The first undercoat metal layer 14a may be formed on the inner wall surface of a via hole, as shown in FIG. 1. The first undercoat metal layer 14a is formed to improve the adhesion of the first electrolytic plating layer 14b described later.

[0022] The first electrolytic plating layer 14b is a layer that becomes the main body of the first wiring conductor 14, and is located on the first undercoat metal layer 14a. In the first wiring conductor 14, electric charges flow around the first electrolytic plating layer 14b. The first electrolytic plating layer 14b is not limited as long as it is a layer formed by electrolytic plating, and is formed of a metal such as copper. The first electrolytic plating layer 14b has a thickness of, for example, 5 μm or more and 25 μm or less. Furthermore, the side surface of the first electrolytic plating layer 14b is in contact with the second insulating layer 132. That is, since the first undercoat metal layer 14a does not exist on the side surface of the first electrolytic plating layer 14b, stress transmitted to the second insulating layer 132 between the side surface of the first electrolytic plating layer 14b and the second insulating layer 132 can be eliminated. As a result, peeling of the first electrolytic plating layer 14b can be reduced.

[0023] In first electrolytic plated layer 14b, the arithmetic mean roughness Ra of the side surface is not limited and may be, for example, 150 nm or more and 300 nm or less. If first electrolytic plated layer 14b has an arithmetic mean roughness Ra of the side surface of 150 nm or more and 300 nm or less, first electrolytic plated layer 14b is firmly adhered to the second insulating layer, and peeling of first electrolytic plated layer 14b can be further reduced.

[0024] The second wiring conductor 15 is located in a groove 151 recessed from the upper surface of the second insulating layer 132 toward the first insulating layer 131, and includes a narrow pattern having a width of 15 μm or less. On the other hand, the second wiring conductor 15 does not include a pattern having a width of 150 μm or more. The depth of the groove 151 is not limited, and may be, for example, 5 μm or more and 25 μm or less. The second wiring conductor 15 mainly has a function for signal transmission. As shown in FIG. 1, the second wiring conductor 15 includes a second base metal layer 15a and a second electrolytic plating layer 15b. In FIG. 1, the second wiring conductor 15 appears to be wide, but the wide second wiring conductor 15 shows a cross section cut in the longitudinal direction.

[0025] Second base metal layer 15a is a base for second wiring conductor 15, and is located on the inner wall surface of groove 151. Second base metal layer 15a is made of a metal such as copper. Second base metal layer 15a has a thickness of, for example, 0.1 μm or more and 0.5 μm or less. Second base metal layer 15a is formed to improve the adhesion of second electrolytic plating layer 15b, which will be described later.

[0026] The second electrolytic plating layer 15b is a layer that becomes the main body of the second wiring conductor 15, and fills the groove 151 in which the second base metal layer 15a is formed. In the second wiring conductor 15, electric charges flow through the second electrolytic plating layer 15b. The second electrolytic plating layer 15b is not limited as long as it is a layer formed by electrolytic plating, and is formed of a metal such as copper. The second electrolytic plating layer 15b is located in the groove 151 of the second insulating layer 132 via the second base metal layer 15a on both the side and bottom surfaces. Therefore, excellent adhesion is exhibited, and peeling of the second electrolytic plating layer 15b can be reduced.

[0027] In the second insulating layer 132, the arithmetic mean roughness Ra of the inner wall surface of the groove 151 is not limited, and may be, for example, 50 nm or more and 100 nm or less. In the second insulating layer 132, if the arithmetic mean roughness Ra of the inner wall surface of the groove 151 is 50 nm or more and 100 nm or less, the second base metal layer 15a is more firmly adhered, and peeling of the second base metal layer 15a can be further reduced. The second wiring conductor 15 has a surface roughness with an arithmetic mean roughness Ra of 50 nm or more and 100 nm or less corresponding to the roughness of the inner wall surface of the groove 151. This roughness is smaller than the side roughness of the first wiring conductor 14 (first electrolytic plating layer 14b), and is advantageous in that it is possible to reduce transmission loss when a high-frequency signal is transmitted to the second wiring conductor 15.

[0028] A solder resist 17 is located on the surface of the build-up layer. The solder resist 17 is made of, for example, an acrylic modified epoxy resin. The solder resist 17 has a function of protecting the conductor layer 12 and the like from solder when, for example, mounting electronic components or connecting to a motherboard. The solder resist 17 has an opening for exposing a part of the first wiring conductor 14 or the second wiring conductor 15 located on the surface of the build-up layer. The part of the first wiring conductor 14 or the second wiring conductor 15 exposed from this opening functions as a pad when mounting a semiconductor element or the like.

[0029] Next, a method for producing the wiring board according to the present disclosure will be described. The method for producing the wiring board according to the present disclosure includes the following steps (a) to (f). (a) forming a first insulating layer; (b) forming a first wiring conductor on the upper surface of the first insulating layer, the first wiring conductor including a first base metal layer and a first electrolytic plating layer located on the first base metal layer, the first wiring conductor including a wide pattern having a width of 150 μm or more; (c) forming a second insulating layer covering the first insulating layer and the first wiring conductor; (d) forming a first groove recessed from the top surface of the second insulating layer toward the first insulating layer; (e) forming a second base metal layer covering the upper surface of the second insulating layer and the inner wall surface of the first groove, and a second electrolytic plating layer located on the second base metal layer and having a thickness sufficient to fill the first groove. (f) removing at least the second base metal layer and the second electrolytic plating layer located on the second insulating layer to form a second wiring conductor including a narrow pattern having a width of 15 μm or less located in the groove.

[0030] A method for manufacturing a wiring board according to the present disclosure will be described with reference to Figures 2 to 6. Figures 2 to 6 are explanatory views for explaining the manufacturing process of wiring board 1 according to the first embodiment.

[0031] First, as shown in Fig. 2(A), a core layer 11 is prepared. A conductor layer 12 is located on the main surface of the core layer 11. Furthermore, the core layer 11 has through-hole conductors 11a for electrically connecting the conductor layers 12 on the upper and lower surfaces of the core layer 11. The core layer 11, the through-hole conductors 11a, and the conductor layers 12 are as described above, and detailed description thereof will be omitted.

[0032] Next, the step of forming the first insulating layer (step (a)) will be described. As shown in FIG. 2(B), the first insulating layer 131 is formed so as to cover the core layer 11 and the conductor layer 12. The first insulating layer 131 is as described above, and detailed description will be omitted. As shown in FIG. 2(C), via holes are formed in the first insulating layer 131 as necessary. The via holes are formed by laser processing, such as a CO2 laser, a UV-YAG laser, an excimer laser, or the like.

[0033] Next, a process (step (b)) of forming a first wiring conductor including a wide pattern having a width of 150 μm or more on the upper surface of the first insulating layer, including a first base metal layer and a first electrolytic plating layer located on the first base metal layer, will be described. As shown in FIG. 2(D), a metal such as copper is deposited by electroless plating on the upper surface of the first insulating layer 131 (the surface of the first insulating layer 131 and the inner wall surface of the via hole). Palladium may be used as a catalyst when performing the electroless plating. The deposited metal finally becomes the first base metal layer 14a. The deposited metal has a thickness of, for example, 0.1 μm or more and 0.5 μm or less.

[0034] After a metal such as copper is deposited by electroless plating, the portions where the first electrolytic plating layer 14b is not to be formed are covered with resist as shown in Fig. 3(A). After covering with resist, a metal such as copper is deposited by electrolytic plating as shown in Fig. 3(B). By setting the width of the portion where the metal such as copper is deposited to 150 μm or more, a wide pattern can be formed. Next, the resist is removed as shown in Fig. 3(C), and the copper in the portion covered with the resist is removed as shown in Fig. 3(D).

[0035] In this manner, the first base metal layer 14a and the first electrolytic plating layer 14b located on the first base metal layer 14a are formed on the first insulating layer 131, and the first wiring conductor 14 is formed. The first electrolytic plating layer 14b has a thickness of, for example, 5 μm or more and 25 μm or less. The first wiring conductor 14 includes a wide pattern having a width of 150 μm or more. Furthermore, a via hole conductor 16 is formed as necessary.

[0036] The side surfaces of first electrolytic plated layer 14b may be roughened to have an arithmetic mean roughness Ra of 150 nm to 300 nm. By performing such a roughening treatment, first electrolytic plated layer 14b is firmly attached to second insulating layer 132, and peeling of first electrolytic plated layer 14b can be further reduced.

[0037] Next, a process (c) of forming a second insulating layer that covers the upper surface of the first insulating layer and the first wiring conductor will be described. The second insulating layer 132 is formed so as to cover the first insulating layer 131 and the first wiring conductor 14, as shown in FIG. 4(A).

[0038] Next, a step (step (d)) of forming a first groove recessed from the upper surface of the second insulating layer toward the first insulating layer will be described. As shown in FIG. 4(B), the first groove 151a is formed in the second insulating layer 132 at a position where the second wiring conductor 15 is to be formed. The method of forming the first groove 151a is not limited, and the first groove 151a is formed by laser processing such as an excimer laser, a CO2 laser, a UV-YAG laser, or the like. It is preferable to adopt an excimer laser because the first groove 151a is easily formed with a uniform depth. The depth of the first groove 151a is not limited, and may be, for example, 5 μm or more and 25 μm or less. As shown in FIG. 4(B) and FIG. 4(C), a via hole may be formed in the second insulating layer 132 as necessary, and a via hole penetrating from the second insulating layer 132 to the first insulating layer 131 may be formed.

[0039] When forming the first groove 151a, a groove forming process may be performed so that the inner wall surface of the first groove 151a has an arithmetic mean roughness Ra of 50 nm to 100 nm. In this case, too, using an excimer laser makes it easy to form the inner wall surface to a predetermined roughness. By forming the first groove 151a in this manner, the second undercoat metal layer 15a is firmly attached to the first insulating layer and the second insulating layer, and peeling of the second undercoat metal layer 15a can be further reduced.

[0040] Next, we will explain the process (step (e)) of forming a second base metal layer covering the upper surface of the second insulating layer and the inner wall surface of the first groove, and a second electrolytic plating layer located on the second base metal layer and having a thickness sufficient to fill the first groove.

[0041] As shown in FIG. 5(A), a second undercoat metal layer 15a is formed on the upper surface of the second insulating layer 132 (the surface of the second insulating layer 132 and the inner wall surface of the via hole) and the inner wall surface of the first groove 151a. The second undercoat metal layer 15a is formed, for example, by depositing a metal such as copper by electroless plating. Palladium may be used as a catalyst when performing the electroless plating. The second undercoat metal layer 15a has a thickness of, for example, 0.1 μm or more and 0.5 μm or less.

[0042] After forming the second undercoat metal layer 15a, as shown in Fig. 5(B), a second electrolytically plated layer 15b is formed on the second undercoat metal layer 15a to a thickness sufficient to fill the first grooves 151a. The second electrolytically plated layer 15b is made of a metal such as copper.

[0043] Next, we will explain the process (process (f)) of removing at least the second base metal layer and the second electrolytic plating layer located on the second insulating layer and forming a second wiring conductor including a narrow pattern having a width of 15 μm or less located in the groove.

[0044] As shown in FIG. 5C, at least the second undercoat metal layer 15a and the second electrolytic plating layer 15b located on the second insulating layer 132 are removed. In this removing step, a part of the second insulating layer 132 may also be removed as necessary. For example, when the width of the first groove 151a near the opening exceeds 15 μm, a part of the second insulating layer 132 may be removed until the width of the first groove 151a becomes 15 μm or less, including the second undercoat metal layer 15a and the second electrolytic plating layer 15b located on the second insulating layer 132. In this manner, the second wiring conductor 15 including a narrow pattern having a width of 15 μm or less located in the groove 151 is formed.

[0045] 6(A), a build-up layer having a desired number of layers is formed on the upper surfaces of the core layer 11 and the conductor layer 12. As described above, the build-up layer includes a first insulating layer 131, a second insulating layer 132 located on the upper surface of the first insulating layer 131, a first wiring conductor 14 located on the upper surface of the first insulating layer 131, and a second wiring conductor 15 located in a groove 151 recessed from the upper surface of the second insulating layer 132 toward the first insulating layer 131.

[0046] Finally, as shown in FIG. 6(B), solder resist 17 is formed so as to be located on the surface of the build-up layer. Solder resist 17 is formed by covering the surface of the build-up layer with a film of, for example, acrylic modified epoxy resin, and curing it. The solder resist 17 is as described above, and a detailed description will be omitted. In this manner, the wiring board 1 according to the first embodiment is obtained.

[0047] Next, another wiring board according to the present disclosure will be described with reference to Fig. 7. Fig. 7 is an explanatory diagram showing a cross section of a wiring board 2 according to a second embodiment of the present disclosure. In the wiring board 2 shown in Fig. 7, the same members as those in the first wiring board 1 are given the same reference numerals, and detailed description thereof will be omitted.

[0048] In the wiring board 1 according to the first embodiment, the bottom surface of the second wiring conductor 15 (the bottom surface of the second base metal layer 15a) is in contact with the first insulating layer 131. On the other hand, in the wiring board 2 according to the second embodiment, the bottom surface of the second wiring conductor 25 (the bottom surface of the second base metal layer 25a) is not in contact with the first insulating layer 131. That is, the second wiring conductor 25 (the second base metal layer 25a and the second electrolytic plating layer 25b) is contained within the second insulating layer 132. In this way, the wiring board 2 according to the second embodiment differs from the wiring board 1 according to the first embodiment in the arrangement of the second wiring conductor 25.

[0049] When palladium is used as a catalyst in forming the first undercoat metal layer 14a and the second undercoat metal layer 25a by electroless plating, palladium may remain. If palladium remains, migration is likely to occur near the boundary between the first insulating layer 131 and the second insulating layer 132 between the adjacent second wiring conductors 25 (second undercoat metal layer 25a) or between the second wiring conductor 25 and the first wiring conductor 14. If the second wiring conductor 25 is contained within the second insulating layer 132 as in the wiring board 2 according to the second embodiment, the second undercoat metal layer 25a will be separated from the boundary between the first insulating layer 131 and the second insulating layer 132. As a result, migration near the boundary can be reduced, and insulation reliability is further improved.

[0050] In the method for manufacturing the wiring board 2 according to the second embodiment, for example, in the step (step (d)) of forming the first groove described above, the depth of the first groove 151a may be adjusted so that the bottom surface of the first groove 151a fits within the second insulating layer 132. The depth of the first groove 151a may be appropriately set depending on the thickness of the second insulating layer 132.

[0051] Next, still another wiring board of the present disclosure will be described with reference to Fig. 8. Fig. 8 is an explanatory diagram showing a cross section of a wiring board 3 according to a third embodiment of the present disclosure. In the wiring board 3 shown in Fig. 8, the same members as those in the first wiring board 1 are given the same reference numerals, and detailed description thereof will be omitted.

[0052] In the wiring board 1 according to the first embodiment, the upper surface of the first wiring conductor 14 (the upper surface of the first electrolytically plated layer 14b) is not covered with the second insulating layer 132. On the other hand, in the wiring board 3 according to the third embodiment, at least a portion of the upper surface of the first wiring conductor 34 (the upper surface of the first electrolytically plated layer 14b) is not exposed from the second insulating layer 132 and is covered with the second insulating layer 132. In this way, the wiring board 3 according to the third embodiment differs from the wiring board 1 according to the first embodiment in the arrangement of the first wiring conductor 34.

[0053] For example, a small gap may exist near the boundary between the second insulating layer 132 and the insulating layer located thereon, and migration may occur if adjacent wiring conductors are exposed at the boundary. That is, migration is likely to occur near the boundary between the first wiring conductor 34 (first electrolytic plating layer 14b) and the second insulating layer 132. When at least a part of the upper surface of the first wiring conductor 34 is covered with the second insulating layer as in the wiring board 3 according to the third embodiment, the upper surface of the first electrolytic plating layer 14b is separated from the boundary between the upper surface of the second insulating layer 132 and the insulating layer located thereon. As a result, migration can be reduced between the upper surface of the first electrolytic plating layer 14b and the upper surface of the second insulating layer 132, and insulation reliability is further improved.

[0054] In the method for manufacturing the wiring board 3 according to the third embodiment, for example, in the step (step (f)) of forming the second wiring conductors described above, at least second base metal layer 15a and second electrolytic plating layer 15b located on second insulating layer 132 may be removed so as not to expose at least a portion of the upper surface of first wiring conductor 34. If necessary, the vicinity of the upper surface of second insulating layer 132 may be removed. [Explanation of symbols]

[0055] 1, 2, 3 Wiring board 11 Core layer 11a Through hole conductor 12 Conductor layer 131 First insulating layer 132 Second insulating layer 14, 34 First wiring conductor 14a First base metal layer 14b First electrolytic plating layer 15, 25 Second wiring conductor 151, 251 groove 15a, 25a 2nd base metal layer 15b, 25b Second electrolytic plating layer 16 Via hole conductor 17 Solder resist

Claims

1. A first insulating layer; a second insulating layer located on an upper surface of the first insulating layer; a first wiring conductor located on an upper surface of the first insulating layer and including a wide pattern having a width of 150 μm or more; a second wiring conductor located in a groove recessed from an upper surface of the second insulating layer toward the first insulating layer and including a narrow pattern having a width of 15 μm or less; Equipped with the first wiring conductor has a first base metal layer located on the first insulating layer and a first electrolytic plating layer located on the first base metal layer, a side surface of the first electrolytic plating layer being in direct contact with the second insulating layer, the second wiring conductor includes a second base metal layer located on an inner wall surface of the groove, and a second electrolytic plating layer filling the groove on the second base metal layer. Wiring board.

2. The wiring board according to claim 1 , wherein the first electrolytic plating layer has an arithmetic mean roughness Ra of the side surface of the wiring board in a range of 150 nm to 300 nm.

3. 3. The wiring board according to claim 1, wherein the second insulating layer has an inner wall surface of the groove having an arithmetic mean roughness Ra of 50 nm or more and 100 nm or less.

4. 4. The wiring board according to claim 1, wherein the second wiring conductor is contained within the second insulating layer.

5. 5. The wiring board according to claim 1, wherein at least a portion of an upper surface of the first wiring conductor is covered with the second insulating layer.

6. forming a first insulating layer; forming a first wiring conductor including a wide pattern having a width of 150 μm or more on an upper surface of the first insulating layer, the first wiring conductor including a first base metal layer and a first electrolytic plating layer located on the first base metal layer; forming a second insulating layer covering an upper surface of the first insulating layer and the first wiring conductor; forming a first groove recessed from an upper surface of the second insulating layer toward the first insulating layer; forming a second undercoat metal layer covering an upper surface of the second insulating layer and an inner wall surface of the first groove, and a second electrolytic plating layer located on the second undercoat metal layer and having a thickness sufficient to fill the first groove; a step of removing at least the second undercoat metal layer and the second electrolytic plating layer located on the upper surface of the second insulating layer to form a second wiring conductor including a narrow pattern having a width of 15 μm or less located in the groove; A method for manufacturing a wiring board comprising the steps of:

7. The method according to claim 6 , wherein in the step of forming the first wiring conductor, a roughening treatment is performed on the side surface of the first electrolytic plating layer to give an arithmetic mean roughness Ra of 150 nm or more and 300 nm or less.

8. The manufacturing method according to claim 6 or 7, wherein in the step of forming the first groove, a groove forming process is performed such that an arithmetic mean roughness Ra of an inner wall surface of the first groove is 50 nm or more and 100 nm or less.

9. 9. The manufacturing method according to claim 6, wherein in the step of forming the first groove, a bottom surface of the first groove is formed within the second insulating layer.

10. The manufacturing method according to any one of claims 6 to 9, wherein in the step of forming the second wiring conductor, at least the second base metal layer and the second electrolytic plating layer located on the second insulating layer are removed so that at least a portion of the upper surface of the first wiring conductor is not exposed.

Citation Information

Patent Citations

  • Method of forming embedded wiring

    JP2004149926A

  • Method of manufacturing wiring board

    JP2009099964A

  • Circuit board and method for manufacturing the same

    JP2011003884A

  • Wiring board and method of manufacturing the same, and electronic component device

    JP2016219559A

  • Wiring board and manufacturing method thereof