Silicon membrane structure for use in manufacturing a pellicle, and manufacturing method thereof

The Si membrane structure with concavo-convex or defect patterns addresses non-uniform etching issues in pellicle film manufacturing by dispersing stress, ensuring a stable self-supporting pellicle film formation.

JP7583961B2Active Publication Date: 2024-11-14NGK CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2023567498
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-12-17
Publication Date
2024-11-14
Estimated Expiration
2041-12-17

AI Technical Summary

Technical Problem

Conventional pellicle film manufacturing processes using Si substrates face issues with non-uniform etching during the conversion to a self-supporting film, leading to stress application and potential damage due to residual Si, resulting in uneven pellicle film formation.

Method used

A Si membrane structure with a concavo-convex or defect pattern is used to define individualized segments, allowing uniform etching and dispersing stress during the conversion to a self-supporting pellicle film, using a Si frame for support.

Benefits of technology

The Si membrane structure effectively disperses stress, reducing the risk of pellicle film damage and ensuring uniform etching, resulting in a stable self-supporting pellicle film.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007583961000001
    Figure 0007583961000001
  • Figure 0007583961000002
    Figure 0007583961000002
  • Figure 0007583961000003
    Figure 0007583961000003
Patent Text Reader

Abstract

Provided is a Si membrane structure (10) with which, during etching to convert a pellicle film on a Si membrane into a self-supporting film, the breakage risk of the pellicle film can be reduced by dispersing the stress applied to the pellicle film due to residual Si. The Si membrane structure includes: a Si membrane (12); and a Si frame (14) provided along the outer circumference of one surface of the Si membrane. Uneven patterns and / or defective patterns are formed on the Si frame-side surface of the Si membrane so that a plurality of segments (S) individualized from one another are defined.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a Si membrane structure for use in the manufacture of a pellicle, and a method for manufacturing a pellicle. [Background technology]

[0002] The miniaturization of semiconductor manufacturing processes is progressing year by year, and various improvements are being made to each process. In particular, in the photolithography process, EUV (extreme ultraviolet) light with a wavelength of 13.5 nm has begun to be used instead of the 193 nm wavelength of the conventional ArF exposure. As a result, the wavelength suddenly became 1 / 10 or less, and its optical characteristics became completely different. However, since there is no material with high transmittance for EUV light, for example, a pellicle film, which is a film to prevent particle adhesion on photomasks (reticles), is known.

[0003] For example, Patent Document 1 (JP Patent No. 6858817) discloses a pellicle film having a core layer including a material that is substantially transparent to EUV radiation and a cap layer including a material that absorbs IR radiation. For example, this document discloses a pellicle having a B or Be core layer covered with a Ru or Mo cap layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Patent No. 6858817 Summary of the Invention

[0005] When attempting to manufacture a pellicle film having a layered structure as disclosed in Patent Document 1, it is conceivable to form a pellicle film on a Si substrate, and then remove unnecessary portions of the Si substrate by etching to form a free-standing film. An example of such a conventional manufacturing process is shown in Figures 7A and 7B. In this conventional process, first, a Si wafer 120 is prepared (Figure 7A(a)). On both sides of this Si wafer 120, a SiO2 film 122 is formed to a thickness of 100 to 1000 nm by chemical vapor deposition (CVD) or thermal oxidation (Figure 7A(b)). Resist is applied to one or both sides of the Si wafer 120, and exposure and development are performed so that a hole in the resist of a predetermined size is formed on one side to form a resist mask 124 for SiO2 etching (Figure 7A(c)). One side of this substrate is wet-etched with hydrofluoric acid to etch away the exposed portions of the SiO2 film 122, thereby producing a SiO2 mask 122a (Figure 7A(d)). After removing the resist mask 124, the Si is etched with a TMAH (tetramethylammonium hydroxide) liquid to thin the Si wafer 120 to a thickness of 10 to 50 μm (FIG. 7A(e)). The SiO2 film 122 formed on the Si surface that is not etched is removed and cleaned with hydrofluoric acid, and the Si wafer 120 is diced to a predetermined size with a laser L (FIG. 7A(f)). In this way, a structure with a cavity 126 in the center of the Si wafer 120, that is, a Si membrane structure 110 having a Si membrane 112 and a Si frame 114 provided along its periphery, is obtained (FIG. 7B(g)). A protective layer 134 (e.g., a Ru layer having a thickness of 2 nm) is formed on the Si membrane structure 110 by sputtering (FIG. 7B(h)), a main layer 132 (e.g., a Be layer having a thickness of 30 to 50 nm) is formed thereon (FIG. 7B(i)), and a protective layer 134 (e.g., a Ru layer having a thickness of 2 nm) is further formed thereon (FIG. 7B(j)), to form the pellicle film 130. Finally, the Si membrane 112 in the region corresponding to the part to be made into a free-standing film is removed by soft etching using XeF2 gas, and the pellicle film 130 is made into a free-standing film. In this way, a pellicle 128 having a Si frame 114 and a pellicle film 130 is obtained (FIG. 7B(k)).

[0006] However, in this conventional process, when etching with XeF2 gas (FIG. 7B(k)), due to the structure and specifications of the etching apparatus, there is a problem that the Si membrane 112 corresponding to the portion to be made into a free-standing film (hereinafter referred to as the window portion) is not etched uniformly. For example, as shown in FIGS. 8A and 8B, a portion of the Si membrane 112 where the etching rate is slow occurs in the center portion of the window portion, and as a result, a portion where the pellicle film 130 has become a free-standing film and a portion where the Si membrane 112 remains may temporarily coexist. At that time, the pellicle film 130 may be subjected to non-uniform stress due to the residual Si, and the pellicle film 130 may be damaged.

[0007] The inventors have now discovered that by using a Si membrane structure having a concave-convex pattern and / or a defect pattern to define a plurality of mutually individualized segments in the Si membrane to form a pellicle film, the stress on the pellicle film caused by residual Si can be distributed during etching to make the pellicle film on the Si membrane into a free-standing film, thereby reducing the risk of damage to the pellicle film.

[0008] Therefore, an object of the present invention is to provide a Si membrane structure capable of dispersing the stress applied to the pellicle film caused by residual Si during etching to make the pellicle film on the Si membrane into a free-standing film, thereby reducing the risk of damage to the pellicle film. Another object of the present invention is to provide a method for manufacturing a pellicle capable of dispersing the stress applied to the pellicle film caused by residual Si during etching to make the pellicle film on the Si membrane into a free-standing film, thereby reducing the risk of damage to the pellicle film.

[0009] According to one aspect of the present invention, there is provided a Si membrane structure for use in the manufacture of a pellicle, comprising: A silicon membrane and A Si frame provided along an outer periphery of one surface of the Si membrane; The present invention provides a Si membrane structure, comprising: a concave-convex pattern and / or a defect pattern formed on the surface of the Si membrane facing the Si frame so as to define a plurality of segments that are individualized from each other.

[0010] According to another aspect of the present invention, A pellicle film is formed on the surface of the Si membrane structure opposite to the Si frame, and then The Si membrane is removed by etching with XeF2 gas, thereby making the pellicle membrane a free-standing membrane whose outer edge is supported by the Si frame. A method for manufacturing a pellicle is provided, comprising:

[0011] According to another aspect of the present invention, A pellicle film is formed on a surface of a Si membrane structure opposite to the Si frame, the surface being provided with a Si membrane and a Si frame provided along an outer peripheral edge of one surface of the Si membrane; A concave-convex pattern and / or a defect pattern are formed on the surface of the Si membrane facing the Si frame so as to define a plurality of segments that are individualized from each other, and then The Si membrane is removed by etching with XeF2 gas, thereby making the pellicle membrane a free-standing membrane whose outer edge is supported by the Si frame. A method for manufacturing a pellicle is provided, comprising: [Brief description of the drawings]

[0012] [Figure 1A] FIG. 2 is a bottom view showing a schematic diagram of one embodiment of a Si membrane structure according to the present invention. [Figure 1B] 1B is a cross-sectional view of the Si membrane structure shown in FIG. 1A taken along line 1B-1B. [Figure 1C] FIG. 1C is an enlarged cross-sectional view of the circled portion in FIG. 1B. [Figure 2A] FIG. 4 is a bottom view illustrating a process for manufacturing a pellicle using the Si membrane structure shown in FIGS. 1A to 1C. [Figure 2B]2B is a cross-sectional view taken along line 2B-2B of the manufacturing process shown in FIG. 2A. [Figure 2C] FIG. 2C is an example of an enlarged cross-sectional view of the circled portion (pellicle membrane) in FIG. 2B. [Diagram 3] FIG. 4 is a bottom view showing a modified example of the Si membrane structure shown in FIGS. 1A to 1C. [Figure 4A] FIG. 4 is a bottom view diagrammatically showing another embodiment of the Si membrane structure according to the present invention. [Figure 4B] 4B is a cross-sectional view of the Si membrane structure shown in FIG. 4A taken along line 4B-4B. [Figure 4C] FIG. 4C is an enlarged cross-sectional view of the circled portion (Si membrane) in FIG. 4B. [Figure 5A] FIG. 5 is a bottom view illustrating a process for manufacturing a pellicle using the Si membrane structure shown in FIGS. 4A to 4C. [Figure 5B] 5B is a cross-sectional view taken along line 5B-5B of the manufacturing process shown in FIG. 5A. [Figure 6A] 2 is a process flow diagram showing the first half of the manufacturing process of the Si membrane structure according to the present invention. [Figure 6B] 4 is a process flow diagram showing the latter half of the manufacturing process of the Si membrane structure according to the present invention. [Figure 7A] 1 is a process flow diagram showing the first half of a manufacturing process for a pellicle membrane according to the prior art. [Figure 7B] 1 is a process flow diagram showing the latter half of a pellicle membrane manufacturing process according to the prior art. [Figure 8A] FIG. 7C is a bottom view illustrating a process for manufacturing a pellicle using the Si membrane structure shown in FIG. 7B. [Figure 8B] 8B is a cross-sectional view of the manufacturing process shown in FIG. 8A along line 8B-8B. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Silicon membrane structure 1A to 1C show an example of a Si membrane structure 10 for use in manufacturing a pellicle. The Si membrane structure 10 shown in FIG. 1 includes a Si membrane 12 and a Si frame 14. The Si frame 14 is provided along the outer periphery of one surface of the Si membrane 12. A concave-convex pattern and / or a defect pattern is applied to the surface of the Si membrane 12 facing the Si frame 14 so as to define a plurality of individualized segments S. By using the Si membrane structure 10 in which the concave-convex pattern and / or the defect pattern is applied to the Si membrane 12 so as to define a plurality of individualized segments S in this way, for forming a pellicle film, the stress applied to the pellicle film due to residual Si can be dispersed during etching to make the pellicle film on the Si membrane into a self-supporting film, thereby reducing the risk of damage to the pellicle film.

[0014] That is, as described above, in the conventional process, when etching with XeF2 gas (FIG. 7B(k)), due to the structure and specifications of the etching apparatus, there is a problem that the Si membrane 112 corresponding to the part to be made into a free-standing film (hereinafter referred to as the window part) is not etched uniformly. For example, as shown in FIGS. 8A and 8B, a part where the etching rate of the Si membrane 112 is slow occurs in the center part of the window part, and as a result, a part where the pellicle film 130 is made into a free-standing film and a part where the Si membrane 112 remains may temporarily coexist. At that time, due to the residual Si, stress is applied non-uniformly to the pellicle film 130, and the pellicle film 130 may be damaged. This problem is successfully solved by the Si membrane structure 10 according to the present invention. This is considered to be due to the following mechanism. FIGS. 2A and 2B show a process of manufacturing a pellicle 28 using the Si membrane structure 10 of the present invention. FIG. 2A shows a bottom view of the Si membrane structure 10 and the pellicle film 30 seen from below (i.e., from the side where the Si frame 14 extends), while FIG. 2B shows a cross section of the structure shown in FIG. 2A taken along line 2B-2B. As can be seen from these figures, the Si membrane 12 has a plurality of segments S that are individualized from each other, and thus the Si membrane 12 is etched in segments when the Si membrane 12 is etched with XeF2 gas. For example, etching of the recess or defect in the Si membrane 12 precedes, and the Si membrane 12 in that portion disappears first. Therefore, the stress caused by the Si membrane 12 (i.e., the residual Si) that remains in the stage immediately before the pellicle film 30 becomes a free-standing film in the latter half of the etching is dispersed. This is because, as is clear from the comparison with the conventional process shown in FIGS. 8A and 8B, the stress is different between the portion where the pellicle film 30 becomes a free-standing film and the portion where the Si membrane 12 remains, and the residual Si is dispersed in segments, so that the stress is also dispersed accordingly.

[0015] The Si membrane 12 is a membrane-like portion that functions as a temporary support layer in the region for forming the pellicle film 30 into a free-standing film. Therefore, the Si membrane 12 is a portion that should be removed by etching when forming the pellicle film 30 into a free-standing film. From this viewpoint, the thickness of the Si membrane 12 is preferably 5 to 100 μm, more preferably 5 to 50 μm, and further preferably 10 to 25 μm.

[0016] The Si frame 14 is a frame-like part provided along the outer periphery of one surface of the Si membrane, and functions to support the pellicle film 30 at the outer periphery when the pellicle film 30 is made into a free-standing film. Therefore, the Si frame 14 is a part that should be left as a border when the pellicle film 30 is made into a free-standing film. From this viewpoint, the height of the Si frame 14 is preferably 100 to 2000 μm, more preferably 200 to 800 μm, and even more preferably 400 to 750 μm. The width of the Si frame 14 is preferably 500 to 40,000 μm, more preferably 1,000 to 20,000 μm, and even more preferably 2,000 to 10,000 μm.

[0017] The Si membrane 12 and the Si frame 14 are preferably made of Si single crystals, and preferably the Si membrane 12 and the Si frame 14 form the Si membrane structure 10 as an integral body.

[0018] A concave-convex pattern and / or a defect pattern are applied to the surface of the Si membrane 12 facing the Si frame 14 so as to define a plurality of segments S that are individualized from each other. The concave-convex pattern and / or the defect pattern may be a regular pattern or an irregular pattern. For example, different patterns may be adopted for the regions of the Si membrane 12 that are easily etched and the regions that are not easily etched.

[0019] According to a preferred embodiment of the present invention, as shown in Figs. 1A to 1C, the concave-convex pattern may be a pattern in which a convex portion (or a concave portion) is located inside each of the segments S, and a concave portion (or a convex portion) is located on the outer periphery of each of the segments S. In this way, as shown in Figs. 2A and 2B, etching of the concave portion in the Si membrane 12 is performed first, and the Si membrane 12 corresponding to the concave portion can be removed first, thereby dispersing stress caused by the Si membrane 12 (i.e., residual Si) remaining at the stage immediately before the pellicle film 30 becomes a free-standing film. From this viewpoint, the thickness of the convex portion of the Si membrane 12 is preferably 5 to 100 µm, more preferably 5 to 50 µm, and even more preferably 10 to 25 µm. On the other hand, the thickness of the concave portion of the Si membrane 12 is preferably 5 to 100 µm, more preferably 5 to 50 µm, and even more preferably 10 to 25 µm. As shown in Fig. 1C, when the thickness of the recessed portion of the Si membrane 12 is X and the thickness of the protruding portion of the Si membrane 12 is Y, the ratio of X / Y is preferably 0.10 to 0.95, more preferably 0.20 to 0.90, and further preferably 0.50 to 0.85. The shape of the segment S is not limited to a rectangle such as a square as shown in Figs. 1A to 1C, but may be various shapes such as a circle, an ellipse, a diamond, etc. as shown in Fig. 3. The method of forming the uneven pattern is not particularly limited, but lithography and anisotropic wet etching may be performed so as to provide minute unevenness of different thicknesses in the shape of segments in the portion corresponding to the Si membrane 12.

[0020] According to another preferred embodiment of the present invention, the defect pattern may be composed of at least one type of defect selected from the group consisting of grooves, notches, and cracks. A Si membrane structure 10' according to this embodiment is shown in Figs. 4A to 4C. In the Si membrane structure 10' shown in these figures, a plurality of segments S, which are individualized from each other, are defined by defects such as grooves, notches, and cracks. Even in this case, as shown in Figs. 5A and 5B, etching of the defect portion D in the Si membrane 12 precedes etching of the Si membrane 12 corresponding to the defect portion D, and the stress caused by the Si membrane 12 (i.e., the residual Si) remaining at the stage immediately before the pellicle film 30 becomes a free-standing film can be dispersed. The method of forming the defect pattern is not particularly limited, but is preferably performed by laser irradiation. For example, by inducing micro-defects in the Si membrane 12 by a laser, it is possible to make it preferentially etched by XeF2. The depth of the defect D is not particularly limited, but as shown in FIG. 4C, when the thickness of the Si membrane 12 is X and the depth of the defect is Y, the ratio of Y / X is preferably 0.10 to 0.95, more preferably 0.20 to 0.90, and even more preferably 0.50 to 0.85.

[0021] 6(k), the surface of the Si frame 14 opposite to the Si membrane 12 may be covered with a SiO2 film 22. In this case, since the Si frame 14 is masked by the SiO2 film 22, even when the Si frame 14 is subjected to etching with XeF2 gas, it is possible to prevent the Si frame 14 from disappearing due to etching, and the Si frame 14 can be used as a border in the pellicle 28.

[0022] Manufacturing method for Si membrane structure 6A and 6B show an example of a manufacturing process of a Si membrane structure 10 having a concave-convex pattern. In this process, first, a Si wafer 20 is prepared on which a pellicle film is to be formed (FIG. 6A(a)). A SiO2 film 22 is formed to a thickness of 100 to 1000 nm on both sides of the Si wafer 20 by chemical vapor deposition (CVD) or thermal oxidation (FIG. 6A(b)). A resist is applied to one or both sides of the Si wafer 20, and exposure and development are performed so that a resist hole of a predetermined size is formed on one side to form a resist mask 24 for SiO2 etching (FIG. 6A(c)). One side of the substrate is wet-etched with hydrofluoric acid to etch away the exposed part of the SiO2 film 22, thereby producing a SiO2 mask 22a (FIG. 6A(d)). After removing the resist mask 24, Si is etched with a TMAH (tetramethylammonium hydroxide) solution to thin the Si wafer 20 to a predetermined thickness suitable for the Si membrane 12 (FIG. 6A(e)). Thus, a structure having a cavity 26 in the center of the Si wafer 20 is obtained. A resist 25a is applied to the surface of this structure facing the cavity 26 (FIG. 6A(f)). Exposure and development are performed to provide a pattern that defines a plurality of segments S on the surface to which the resist 25a is applied, and a resist mask 25 for SiO2 etching is obtained in a predetermined pattern (FIG. 6B(g)). Etching is performed with TMAH liquid on the surface of the Si wafer 20 masked in a predetermined pattern with the resist mask 25 on the cavity 26 side, so that the exposed portion of the Si wafer 20 is further thinned to form a recess pattern (FIG. 6B(h)). After removing the resist mask 25 (FIG. 6B(i)), the SiO2 film 22 formed on the surface of the Si that has not been etched is removed by etching with hydrofluoric acid (FIG. 6B(j)). Thus, a Si membrane structure 10 is obtained in which a concave-convex pattern is applied to the surface on the cavity 26 side to define a plurality of segments S that are individualized from each other (FIG. 6B(k)).

[0023] Supplementally, as described later, after the pellicle film 30 is formed on the Si membrane structure 10, the main region (i.e., the region to be made into a free-standing film) other than the outer edge portion is removed by etching. Therefore, in order to perform etching efficiently and in a short time, it is desirable to thin the thickness of the Si membrane 12 in the region to be made into a free-standing film in advance. For this reason, it is desirable to form a mask of a predetermined shape on the Si wafer 20 using a normal semiconductor process, etch the Si wafer 20 by wet etching, and thin the thickness of the main region of the Si wafer 20 (particularly the Si membrane) to a predetermined thickness. The Si wafer 20 that has been subjected to the wet etching is washed and dried to prepare the Si membrane structure 10 having the cavity 26 formed by wet etching. Note that the wet etching mask may be made of any material that is corrosion-resistant against a wet etching solution for Si, and for example, SiO2 is preferably used. In addition, the wet etching solution is not particularly limited as long as it can etch Si. For example, TMAH (tetramethylammonium hydroxide) is preferable because it can perform very good etching by anisotropic etching of Si when used under appropriate conditions.

[0024] Manufacturing method of a pellicle 2A, 2B, 5A, and 5B, the pellicle 28 can be preferably manufactured while reducing the risk of breakage by using the Si membrane structure 10 of the present invention. Specifically, after forming the pellicle film 30 on the Si membrane 12 of the Si membrane structure 10, the unnecessary portion of the Si membrane 12 is removed by etching to make the pellicle film 30 a free-standing film, thereby manufacturing the pellicle 28. Therefore, as described above, the main portion of the pellicle film 30 is in the form of a free-standing film with no Si membrane 12 remaining.

[0025] (1) Formation of pellicle film 30 A pellicle film 30 is formed on the surface of the Si membrane structure 10 opposite to the Si frame 14. FIG. 2C shows an example of the pellicle film 30. The pellicle film 30 preferably has a main layer 32 made of at least one metal selected from the group consisting of Ni, Al, Be, Cr, and Ga. These metals have the advantage that they are not easily eroded by XeF2 gas when the Si membrane 12 is etched away with XeF2 gas to form the pellicle film 30 into a free-standing film. This is supported by the fact that the boiling points of the fluorides of Ni, Al, Be, Cr, and Ga are extremely high, at 1750°C (NiF2), 1260°C (AlF3), 1169°C (BeF2), 1100°C (CrF2), and 950°C (GaF3), compared to the boiling point of XeF2, which is 114°C. A high boiling point means a low vapor pressure, which means that it is more difficult to etch with XeF2 gas. From the viewpoint of an EUV transmitting film, Be is particularly preferable. Since Be has a higher EUV transmittance than Si and C, it exhibits a practically high EUV transmittance (for example, 93% or more). In addition, it is preferable that the pellicle film 30 further includes a protective layer 34 that covers at least one side (preferably both sides) of the main layer 32 from the viewpoint of protecting the main layer 32. When the main layer 32 is made of Be, preferable examples of materials constituting the protective layer 34 include beryllium nitride, beryllium oxide, and beryllium fluoride.

[0026] The pellicle film 30 may be formed by any film forming method. One example of a preferred film forming method is a sputtering method. For example, when a three-layer structure of beryllium nitride / beryllium / beryllium nitride is produced, it is preferable that the beryllium film as the main layer 32 is produced by sputtering using a pure Be target, and the beryllium nitride film as the protective layer 34 is produced by reactive sputtering. This reactive sputtering can be performed, for example, by introducing nitrogen gas into the chamber during sputtering using a pure Be target, so that beryllium and nitrogen react to produce beryllium nitride. As another method, beryllium nitride can also be produced by forming a beryllium film, and then irradiating it with nitrogen plasma to cause a nitriding reaction of beryllium to produce beryllium nitride. In any case, the synthesis method of beryllium nitride is not limited to these. It is preferable to use different beryllium targets for forming the beryllium nitride film and beryllium targets for forming the beryllium film, but it is also possible to use the same target for forming the beryllium nitride film and the beryllium film. The beryllium nitride film and the beryllium film may be formed in a single-chamber sputtering apparatus as in the examples described below, or the beryllium nitride film and the beryllium film may be formed in separate chambers using a two-chamber sputtering apparatus.

[0027] (2) Self-supporting film The Si membrane 12 is removed by etching with XeF2 gas, thereby forming the pellicle film 30 into a free-standing film whose outer edge is supported by the Si frame 14. The unnecessary portion of the Si membrane 12 other than the outer edge portion to be left as a border of the Si membrane structure 10 on which the pellicle 28 is formed is removed by etching, forming the pellicle film 30 into a free-standing film. The etching of Si may be performed by any method, but is preferably performed by etching using XeF2. In this manner, the pellicle 28 having the Si frame 14 and the pellicle film 30 is obtained.

[0028] (3) Transformation According to another aspect of the present invention, a conventional type Si membrane structure not having the above-mentioned uneven pattern and / or defect pattern may be used, and the uneven pattern and / or defect pattern may be formed after the formation of the pellicle film and before the etching of the Si membrane. In this aspect, first, as shown in FIG. 7B, a Si membrane structure 110 having the same configuration as described above except that it does not have the uneven pattern and / or defect pattern is prepared, and a pellicle film 130 is formed on the surface opposite to the Si frame 114. Next, an uneven pattern and / or defect pattern (not shown) is formed on the surface of the Si membrane 112 facing the Si frame 114 so as to define a plurality of segments that are individualized from each other as described above. Thereafter, the Si membrane 112 is etched and removed with XeF2 gas, thereby making the pellicle film 130 a free-standing film whose outer edge is supported by the Si frame 114. In this aspect, the defect pattern is preferably formed by laser irradiation. With laser irradiation, the defect pattern can be efficiently formed on the Si membrane 112 on which the pellicle film 130 has already been formed, without damaging the pellicle film 130. In this embodiment, multiple segments S that are individualized to each other are formed in the Si membrane 112, and as in the embodiment described above, when etching the pellicle film 130 to make it into a free-standing film, the stress on the pellicle film 130 caused by residual Si can be distributed, reducing the risk of damage to the pellicle film 130.

[0029] EUV permeable membrane In a preferred embodiment of the present invention, the pellicle film 30 is an EUV (extreme ultraviolet) transmitting film. As shown in FIG. 2C, the pellicle film 30 according to this embodiment preferably comprises a main layer 32 and a protective layer 34 covering at least one side (preferably both sides) of the main layer 32. In this embodiment, the main layer 32 is preferably made of metal beryllium, while the protective layer 34 is preferably made of beryllium nitride. In this way, by combining the main layer 32 made of metal beryllium with the protective layer 34 made of beryllium nitride, it is possible to provide an EUV transmitting film that combines a practical level of high EUV transmittance (for example, 93% or more) and durability in a low-pressure hydrogen atmosphere environment.

[0030] The main layer 32 according to this embodiment is preferably made of metallic beryllium. However, the main layer 32 does not need to be made entirely of metallic beryllium, and it is sufficient that the main layer 32 is preferably made of 99% by weight or more, more preferably 99.5% by weight or more, and even more preferably 99.8% by weight or more of the main layer 32 is made of metallic beryllium. This contributes to realizing a practical level of high EUV transmittance while ensuring the basic functions of a pellicle film (such as the function of preventing particle adhesion). From this perspective, the thickness of the main layer 32 is preferably 10 to 70 nm, more preferably 15 to 50 nm, and even more preferably 20 to 35 nm.

[0031] The protective layer 34 according to this embodiment is a layer for protecting the main layer 32, which is a metal beryllium layer. Therefore, the protective layer 34 may cover at least one side of the main layer 32, but it is preferable to cover both sides of the main layer 32 with the protective layer. The protective layer 34 is preferably made of beryllium nitride. However, the main layer 32 does not need to be completely made of beryllium nitride, and it is sufficient that 99% by weight or more, preferably 99.5% by weight or more, and more preferably 99.8% by weight or more of the main layer 32 is made of beryllium nitride. Beryllium nitride has a high EUV transmittance, so that the EUV transmittance is higher than that of a beryllium film having a Ru layer formed thereon when compared at the same thickness. According to theoretical calculations, the transmittance is 85.8% when a 3-nm-thick Ru film is formed on both sides of a 30-nm-thick beryllium film, but the transmittance is 91.1% when a 3-nm-thick beryllium nitride film is formed on both sides of a 30-nm-thick beryllium film. When a 2 nm thick beryllium nitride layer and a 1 nm thick gradient composition layer (a layer composed of a nitrogen concentration gradient region described later) are formed on both sides of a 30 nm thick beryllium film, the transmittance exceeds 91.1%. By forming dense beryllium nitride layers on both sides of the beryllium layer, it is possible to suppress reaction with XeF2 gas used in etching a Si substrate described later. In addition, since beryllium is a highly reactive material, it is easily oxidized to form beryllium oxide, but the formation of beryllium nitride can suppress oxidation. As described above, the advantages of using a beryllium nitride layer as the protective layer 34 are increased EUV transmittance, protection of the beryllium film (main layer 32) in the etching process, and prevention of oxidation.

[0032] The thickness of the protective layer 34 in this embodiment is preferably 5 nm or less, and more preferably 3 nm or less. Considering that protective layers of 3 nm in thickness are formed on both sides of the main layer 32, a 3 nm thick beryllium nitride film has an EUV transmittance of 95%, which is significantly higher than the 90% of a Ru film. There is no particular limit to the lower limit of the thickness of the protective layer 34, but it is typically 1 nm or more. Note that in this specification, the term "beryllium nitride" refers not only to a stoichiometric composition such as Be3N2, but also to a composition having a stoichiometric composition such as Be3N 2-xIt means an inclusive composition that also allows a non-stoichiometric composition such as (where 0 < x < 2).

[0033] For the pellicle film 30 according to this aspect, it is preferable that the main region for transmitting EUV is in the form of a self-supporting film. That is, it is preferable that only the substrate (for example, Si substrate) used during film formation remains as a border at the outer edge of the pellicle film 30. That is, the substrate (for example, Si substrate) does not remain in the main region other than the outer edge portion. That is, it is preferable that the main region is composed of only the main layer 32 and the protective layer 34.

[0034] The pellicle film 30 according to this aspect can have a high EUV transmittance at a practical level, preferably having an EUV transmittance of 91% or more, more preferably 92% or more, and even more preferably 93% or more. Since the higher the EUV transmittance, the more desirable it is, the upper limit value is not particularly limited. However, the EUV transmittance of the pellicle film 30 can typically be 99% or less, more typically 98% or less, and even more typically 95% or less.

Example

[0035] The present invention will be supplemented and explained by the following examples. Note that the following examples do not apply an uneven pattern and / or a defect pattern to the Si membrane structure, but since they have content common to the present invention other than that, they are positioned as reference examples for assisting the understanding of the present invention.

[0036] Example 1 (Reference) According to the procedures shown in FIGS. 2A and 2B, a composite self-supporting film (EUV transmission film) having a three-layer structure of beryllium nitride / beryllium / beryllium nitride was produced as follows.

[0037] (1) Preparation of Si membrane structure A Si wafer 120 with a diameter of 8 inches (20.32 cm) was prepared (FIG. 7A(a)). A SiO2 film 122 was formed to a thickness of 50 nm on both sides of the Si wafer 120 by thermal oxidation (FIG. 7A(b)). Resist was applied to both sides of the Si wafer 120, and exposure and development were performed to form a resist hole of 110 mm x 145 mm on one side to form a resist mask 124 for SiO2 etching (FIG. 7A(c)). One side of the substrate was wet-etched with hydrofluoric acid to etch away the exposed part of the SiO2 film 122, thereby producing a SiO2 mask 122a (FIG. 7A(d)). The resist mask 124 for SiO2 etching was removed by an ashing device (FIG. 7A(e)). Then, Si was etched with TMAH liquid. The etching rate was measured in advance, and this etching was performed only for the etching time required to achieve the target Si membrane thickness of 50 μm (FIG. 7A(e)). Finally, the SiO2 film 122 formed on the surface that was not etched was removed and washed with hydrofluoric acid (FIG. 7B(f)). The outer shape of the structure thus obtained may be diced with a laser L to a desired shape as necessary (FIG. 7A(f)). In this way, a cavity 126 of 110 mm x 145 mm was provided in the center of the 8-inch (20.32 cm) Si wafer 120, and a Si membrane structure 110 in which the thickness of the Si membrane 112 in the cavity 26 portion is 50 μm was prepared (FIG. 7B(g)).

[0038] (2) Formation of pellicle membrane A composite film having a three-layer structure of beryllium nitride / beryllium / beryllium nitride was formed on the Si membrane structure 110 obtained in (1) above as follows (FIGS. 7B(h)-(j)). First, the Si membrane structure 110 was set in a sputtering device, and a pure Be target was attached. The chamber was evacuated, and the internal pressure was adjusted to 0.5 Pa, and the flow rate ratio of argon gas and nitrogen gas was adjusted to 1:1 to perform reactive sputtering. The reactive sputtering was terminated when the time came for 2 nm of beryllium nitride to be deposited. Next, sputtering was performed using only argon gas without introducing nitrogen gas, and sputtering was terminated when the time came for 25 nm of beryllium to be deposited. Thereafter, reactive sputtering was performed while introducing nitrogen gas again as in the first step, and reactive sputtering was terminated when the time came for 2 nm of beryllium nitride to be deposited. In this way, a pellicle film 130 of beryllium nitride 2 nm / beryllium 25 nm / beryllium nitride 2 nm was formed as an EUV-transmitting film.

[0039] (3) Self-supporting film The Si membrane structure 110 with the pellicle film 130 prepared in (2) above was set in the chamber of a XeF2 etcher capable of processing 8-inch (20.32 cm) substrates. The chamber was evacuated sufficiently. At this time, if moisture remains in the chamber, it reacts with the XeF2 gas to produce hydrofluoric acid, which may cause corrosion of the etcher or unexpected etching, so a sufficient vacuum was drawn. If necessary, the chamber was repeatedly evacuated and nitrogen gas was introduced to reduce the remaining moisture. When a sufficient vacuum was achieved, the valve between the XeF2 raw material cylinder and the spare chamber was opened. As a result, XeF2 sublimated and XeF2 gas was accumulated in the spare chamber as well. When a sufficient amount of XeF2 gas had accumulated in the spare chamber, the valve between the spare chamber and the chamber was opened, and XeF2 gas was introduced into the chamber. The XeF2 gas decomposed into Xe and F, and the F reacted with Si to produce SiF4. Since the boiling point of SiF4 is -95°C, the generated SiF4 quickly evaporated, causing a reaction between the newly exposed Si membrane 112 and F. When the Si etching progressed and the amount of F in the chamber decreased, the chamber was evacuated and XeF2 gas was introduced into the chamber again to perform etching. In this way, the vacuuming, introduction of XeF2 gas, and etching were repeated, and etching was continued until the Si membrane 112 corresponding to the part to be made into a free-standing membrane disappeared. Etching was stopped when the unnecessary part of the Si membrane disappeared. In this way, a composite free-standing membrane with a Si border was obtained as a pellicle membrane 130 (EUV-transmitting membrane) (Figure 7B(k)).

[0040] Example 2 (reference) A composite free-standing membrane was produced in the same manner as in Example 1, except that the composite membrane was formed as follows.

[0041] (Formation of composite membrane) The Si membrane structure with the cavity formed obtained in Example 1 (1) was placed in a sputtering device, and a beryllium film was formed to a thickness of 1 nm. Then, by generating plasma while introducing nitrogen gas into the chamber, the generated nitrogen plasma was reacted with the formed beryllium film to form beryllium nitride. Next, a beryllium film was formed to a thickness of 26 nm on the formed beryllium nitride film, and after the film formation, nitrogen gas was introduced into the chamber again while generating plasma, and the surface became beryllium nitride. In this way, a beryllium film with a thickness of 25 nm and a beryllium nitride film with a thickness of 1.5 nm on both sides (a composite film of beryllium nitride 1.5 nm / beryllium 25 nm / beryllium nitride 1.5 nm) was formed.

[0042] EUV transmittance The pellicle films prepared in Examples 1 and 2 were irradiated with EUV light, and the amount of transmitted EUV light was measured by a sensor. The EUV transmittance was calculated by comparing the measured value with the amount of EUV light directly measured by a sensor without an EUV-transmitting film. As a result, the EUV transmittance of the pellicle film prepared in Example 1 was 93.0%, which was almost the same as the theoretically calculated value of 93.3%. The EUV transmittance of the pellicle film prepared in Example 2 was 93.5%, which was close to the theoretically calculated value of 94.1%. It is assumed that the difference between these measured values ​​and theoretical values ​​is due to an error in the film thickness.

Claims

1. A Si membrane structure for use in the manufacture of a pellicle, comprising: A silicon membrane; A Si frame provided along an outer periphery of one surface of the Si membrane; A Si membrane structure comprising: a concave-convex pattern and / or a defect pattern formed on the surface of the Si membrane facing the Si frame so as to define a plurality of segments that are individualized from each other.

2. 2. The Si membrane structure according to claim 1, wherein the concave-convex pattern is a pattern in which convex portions are located inside each of the segments and concave portions are located on the outer periphery of each of the segments.

3. 3. The Si membrane structure according to claim 1, wherein the defect pattern is composed of at least one type of defect selected from the group consisting of a groove, a notch, and a crack.

4. The surface of the Si frame opposite to the Si membrane is SiO 2 The Si membrane structure according to any one of claims 1 to 3, which is covered with a film.

5. A pellicle film is formed on the surface of the Si membrane structure according to any one of claims 1 to 4 opposite to the Si frame, and then The Si membrane was treated with XeF 2 The pellicle membrane is then removed by etching with a gas, thereby forming a free-standing membrane whose outer edge is supported by the Si frame. A method for manufacturing a pellicle, comprising:

6. A pellicle film is formed on a surface of a Si membrane structure opposite to the Si frame, the Si membrane structure including a Si membrane and a Si frame provided along an outer peripheral edge of one surface of the Si membrane; A concave-convex pattern and / or a defect pattern are formed on the surface of the Si membrane facing the Si frame so as to define a plurality of segments that are individualized from each other, and then The Si membrane was treated with XeF 2 The pellicle membrane is then removed by etching with a gas, thereby forming a free-standing membrane whose outer edge is supported by the Si frame. A method for manufacturing a pellicle, comprising:

7. The method for manufacturing a pellicle according to claim 6 , wherein the defect pattern is formed by laser irradiation.

8. The method for manufacturing a pellicle according to any one of claims 5 to 7, wherein the pellicle membrane has a main layer composed of at least one metal selected from the group consisting of Ni, Al, Be, Cr and Ga.

9. The method for manufacturing a pellicle according to any one of claims 5 to 7, wherein the pellicle membrane comprises a main layer and a protective layer covering at least one side of the main layer.

10. A method for manufacturing a pellicle as described in claim 9, wherein the main layer is composed of at least one metal selected from the group consisting of Ni, Al, Be, Cr and Ga.

Citation Information

Patent Citations

  • Filter window, lithography projection apparatus, method of manufacturing filter window, method of manufacturing device and device manufactured by the method

    JP2005043895A

  • Compound semiconductor substrate, pellicle film, and production method of compound semiconductor substrate

    JP2017150064A

  • Pellicle for extreme ultraviolet lithography and method for manufacturing same

    JP2019091001A

  • Film for use in a lithographic apparatus and a lithographic apparatus including such a film

    JP6858817B2