Reflective photomask blanks and reflective photomasks

The reflective photomask blank and photomask design with a ruthenium capping layer and high extinction coefficient materials in the low reflective part address shadowing and adhesion issues, improving transfer performance and stability in EUV lithography.

JP7584702B2Active Publication Date: 2024-11-15TOPPAN PHOTOMASK CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2024131670
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-15
Estimated Expiration
2041-01-08

AI Technical Summary

Technical Problem

Current EUV lithography techniques face issues such as decreased contrast and line edge roughness due to shadowing effects, leading to poor transfer performance and adhesion problems between the capping layer and low reflective parts in reflective photomasks, which are exacerbated by contaminants and hydrogen delamination.

Method used

A reflective photomask blank and photomask design utilizing a multilayer reflective film with a capping layer containing ruthenium and a low reflective part composed of materials like silver, cobalt, indium, platinum, and tellurium, along with specific oxides, nitrides, and borides, ensuring high adhesion and reduced thickness to minimize shadowing effects.

Benefits of technology

The solution enhances transfer performance and resistance to environmental contaminants, maintaining pattern stability and improving adhesion between layers, thereby reducing shadowing effects and enhancing the longevity and accuracy of pattern transfer.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007584702000002
    Figure 0007584702000002
  • Figure 0007584702000003
    Figure 0007584702000003
  • Figure 0007584702000004
    Figure 0007584702000004
Patent Text Reader

Abstract

To provide a reflective photomask blank and a reflective photomask that have high interlayer adhesion between a capping layer and a low-reflection layer, and suppress or reduce the projection effect of a reflective photomask for patterning transfer in which light with a wavelength in the extreme UV range is used as a light source.SOLUTION: A reflective photomask blank 10 according to the present embodiment comprises a substrate 1, a reflection section 5, and a low-reflection section 4. The reflection section 5 comprises a multilayered reflection film 2 and a capping layer 3. The capping layer 3 includes ruthenium (Ru). The low-reflection section 4 includes 40 at% or more of a material selected from Ag, Co, In, Pt, Sn, Ni, Te, and compounds thereof, and in a region that is at a thickness of 2 nm from the capping layer 3 side of the low-reflection section 4, includes 25 at% or more of a material belonging to a first material group, or includes 30 at% or more of a material belonging to a second material group. The total film thickness of the low-reflection section 4 is 45 nm or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a reflective photomask for use in lithography using light in the ultraviolet region as a light source, and a reflective photomask blank for producing the same. [Background technology]

[0002] In the manufacturing process of semiconductor devices, the demand for miniaturization of photolithography technology is increasing along with the miniaturization of semiconductor devices. The minimum resolution dimension of the transfer pattern in photolithography depends heavily on the wavelength of the exposure light source, and the shorter the wavelength, the smaller the minimum resolution dimension can be. For this reason, the exposure light source is being replaced from the conventional ArF excimer laser light with a wavelength of 193 nm to light in the EUV (Extreme Ultra Violet) region with a wavelength of 13.5 nm.

[0003] Light in the EUV region is absorbed at a high rate by most substances, so a reflective photomask is used as a photomask for EUV exposure (EUV mask) (see, for example, Patent Document 1). Patent Document 1 discloses an EUV photomask obtained by forming a reflective layer made of a multilayer film in which molybdenum (Mo) layers and silicon (Si) layers are alternately laminated on a glass substrate, forming an absorbing layer mainly composed of tantalum (Ta) thereon, and forming a pattern on this absorbing layer.

[0004] Furthermore, as mentioned above, EUV lithography cannot use refractive optics that utilize the transmission of light, so the optical components of the exposure machine are reflective (mirrors) rather than lenses. This creates a problem in that the incident light and reflected light on the reflective photomask (EUV mask) cannot be designed to be coaxial, so EUV lithography normally employs a method in which the optical axis is tilted 6 degrees from the vertical direction of the EUV mask, and the reflected light reflected at an angle of minus 6 degrees is guided to the semiconductor substrate. As such, in EUV lithography, the optical axis is tilted via a mirror, which is known to cause a problem known as the "projection effect," in which the EUV light incident on the EUV mask casts a shadow on the mask pattern (patterned absorbing layer) of the EUV mask.

[0005] Current EUV mask blanks use a tantalum (Ta)-based film with a thickness of 60 nm to 90 nm as the absorption layer. When performing pattern transfer exposure with an EUV mask fabricated using this mask blank, there is a risk of a decrease in contrast at the shadow edge of the mask pattern depending on the relationship between the incident direction of the EUV light and the orientation of the mask pattern. This can lead to problems such as increased line edge roughness of the transferred pattern on the semiconductor substrate and inability to form the line width to the targeted dimension, resulting in a deterioration of transfer performance.

[0006] Therefore, reflective photomask blanks are being considered in which the absorption layer is changed from tantalum (Ta) to a material with high absorption (extinction coefficient) for EUV light, or a material with high absorption is added to tantalum (Ta).For example, Patent Document 2 describes a reflective photomask blank in which the absorption layer is made of a material containing 50 atomic % (at %) or more of tantalum (Ta) as the main component, and further containing at least one element selected from tellurium (Te), antimony (Sb), platinum (Pt), iodine (I), bismuth (Bi), iridium (Ir), osmium (Os), tungsten (W), rhenium (Re), tin (Sn), indium (In), polonium (Po), iron (Fe), gold (Au), mercury (Hg), gallium (Ga), and aluminum (Al).

[0007] Furthermore, it is known that mirrors become contaminated by by-products of EUV generation (e.g., tin (Sn)) and carbon (C). Accumulation of contaminants on the mirror can reduce the reflectivity of the mirror surface, lowering the throughput of the lithography apparatus. In response to this problem, Patent Document 3 discloses a method of generating hydrogen radicals within the apparatus, reacting the hydrogen radicals with the contaminants, and removing the contaminants from the mirror.

[0008] In the method of Patent Document 3, hydrogen ions and the like are generated in addition to hydrogen radicals in the device, and these atomic hydrogens can also penetrate between the capping layer and the low-reflection portion in the photomask. The penetrated atomic hydrogen forms a high-concentration hydrogen region between the layers, and in this region, the atomic hydrogens can bond with each other to become hydrogen molecules. The hydrogen molecules thus generated become bubbles, which increase the vacancy density between the layers and can cause delamination.

[0009] In response to this problem, a reflective photomask blank that prevents delamination by providing a hydrogen absorbing layer between layers that may cause delamination has been studied. For example, the photomask blank described in Patent Document 4 discloses a method in which a hydrogen absorbing layer is provided between a multilayer reflective film and a capping layer, so that atomic hydrogen that may cause delamination is captured in the hydrogen absorbing layer. However, there is no description of delamination between the capping layer and the low reflection portion in the reflective photomask blank described in Patent Document 4. Therefore, the transfer pattern (mask pattern) formed on the absorbing layer by introduction into the EUV exposure device cannot be stably maintained, and as a result, there is a possibility that the transferability may deteriorate. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] JP 2011-176162 A [Patent Document 2] JP 2007-273678 A [Patent Document 3] JP 2011-530823 A [Patent Document 4] JP 2019-113825 A Summary of the Invention [Problem to be solved by the invention]

[0011] Therefore, an object of the present invention is to provide a reflective photomask blank and a reflective photomask that suppress or reduce the projection effect of a reflective photomask for patterning transfer using light with a wavelength in the extreme ultraviolet region as a light source, and that have high interlayer adhesion between the capping layer and the low-reflection portion. [Means for solving the problem]

[0012] In order to solve the above problems, a photomask blank according to one embodiment of the present invention is a reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising: a substrate; a reflective portion formed on the substrate for reflecting incident light; and a low-reflection portion formed on the reflective portion for absorbing incident light, the reflective portion comprising a multilayer reflective film and a capping layer, the capping layer containing at least ruthenium (Ru), the low-reflection portion containing at least one of silver (Ag), cobalt (Co), indium (In), platinum (Pt), tin (Sn), nickel (Ni), and tellurium (Te), and oxides thereof, The low-reflection portion includes at least one material selected from the group consisting of nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides at a concentration of 40 at % or more, and a region of at least 2 nm thick from the capping layer side of the low-reflection portion includes at least one material selected from the group consisting of ruthenium (Ru), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), niobium (Nb), molybdenum (Mo), technetium (Tc), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides. or contains 30 at % or more of at least one material selected from a second material group consisting of scandium (Sc), copper (Cu), yttrium (Y), zirconium (Zr), palladium (Pd), lanthanum (La), hafnium (Hf), gold (Au), beryllium (Be), magnesium (Mg), calcium (Ca), zinc (Zn), cadmium (Cd), and aluminum (Al), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boride oxynitrides thereof, and the total film thickness of the low-reflection portion is 45 nm or less.

[0013] In order to achieve the above object, a photomask according to one aspect of the present invention includes a substrate, a reflective portion formed on the substrate to reflect incident light, and a low-reflection portion formed on the reflective portion to absorb the incident light, the reflective portion includes a multilayer reflective film and a capping layer, the capping layer includes at least ruthenium (Ru), and the low-reflection portion includes at least one of silver (Ag), cobalt (Co), indium (In), platinum (Pt), tin (Sn), nickel (Ni), or a combination of these. The low-reflection portion includes at least one material selected from the group consisting of nickel (Ni), tellurium (Te), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and oxynitride boride thereof at a concentration of 40 at % or more, and the low-reflection portion includes at least one material selected from the group consisting of ruthenium (Ru), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), niobium (Nb), molybdenum (Mo), technetium (Ti), and the like in a region of at least 2 nm thick from the capping layer side. The material contains at least one material selected from a first material group consisting of tungsten (Tc), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and oxynitride boride thereof, at 25 at % or more, or contains scandium (Sc), copper (Cu), yttrium (Y), zirconium (Zr), palladium (Pb), palladium (Tc), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, and oxyborides thereof, at 25 at % or more, or contains at least one material selected from a first material group consisting of tungsten (Tc), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, and oxyboride boride thereof, at 25 at % or more. The low-reflection portion contains 30 at % or more of at least one material selected from a second material group consisting of palladium (Pd), lanthanum (La), hafnium (Hf), gold (Au), beryllium (Be), magnesium (Mg), calcium (Ca), zinc (Zn), cadmium (Cd), and aluminum (Al), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boride oxynitrides thereof, and the total film thickness of the low-reflection portion is 45 nm or less. Effect of the Invention

[0014] According to one aspect of the present invention, in patterning using light having a wavelength in the extreme ultraviolet region as a light source, the transfer performance to a semiconductor substrate is improved, and resistance to the external environment during manufacture and use of the photomask can be expected. In other words, the reflective photomask blank and the reflective photomask according to one aspect of the present invention suppress or reduce the projection effect of a reflective photomask for patterning transfer using light having a wavelength in the extreme ultraviolet region as a light source, and have high adhesion between the capping layer and the layer of the low reflection portion. [Brief description of the drawings]

[0015] [Figure 1] 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment of the present invention. [Diagram 2] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Diagram 3] 1 is a map showing the refractive index n and the extinction coefficient k at the wavelength of EUV light. [Figure 4] FIG. 11 is a schematic cross-sectional view showing a structure of a reflective photomask according to a modified example of the embodiment of the present invention. [Diagram 5] FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a material belonging to a first material group and the content (concentration) distribution of a high extinction coefficient material in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 6] FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a material belonging to a first material group and the content (concentration) distribution of a high extinction coefficient material in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 7] FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a material belonging to a first material group and the content (concentration) distribution of a high extinction coefficient material in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 8]FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a material belonging to a first material group and the content (concentration) distribution of a high extinction coefficient material in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Figure 9] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Figure 10] FIG. 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment of the present invention. [Figure 11] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 12] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 13] 1A to 1C are schematic cross-sectional views showing a manufacturing process of a reflective photomask according to an embodiment of the present invention. [Figure 14] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Figure 15] FIG. 2 is a schematic plan view showing a 64 nm line width LS pattern for transfer evaluation according to an embodiment of the present invention. [Figure 16] FIG. 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment of the present invention. [Figure 17] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Figure 18] FIG. 1 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to an embodiment of the present invention. [Figure 19] 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to an embodiment of the present invention. [Figure 20] FIG. 2 is a schematic cross-sectional view showing a structure of a reflective photomask blank according to a comparative example of the present invention. [Figure 21] FIG. 1 is a schematic cross-sectional view showing a structure of a reflective photomask according to a comparative example of the present invention. [Figure 22]FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a material belonging to a first material group and the content (concentration) distribution of a high extinction coefficient material in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to an embodiment of the present invention. [Diagram 23] FIG. 1 is a conceptual diagram showing an example of the content (concentration) distribution of a material belonging to a first material group and the content (concentration) distribution of a high extinction coefficient material in an absorption layer (low reflection portion) provided in a reflective photomask blank and a reflective photomask according to a comparative example of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, embodiments of the present invention will be described with reference to the drawings, but the present invention is not limited to the embodiments shown below. In the embodiments shown below, technically preferable limitations are imposed for carrying out the present invention, but these limitations are not essential requirements for the present invention. Fig. 1 is a schematic cross-sectional view showing the structure of a reflective photomask blank 10 according to an embodiment of the present invention. Also, Fig. 2 is a schematic cross-sectional view showing the structure of a reflective photomask 20 according to an embodiment of the present invention. Here, the reflective photomask 20 according to the embodiment of the present invention shown in Fig. 2 is formed by patterning the low reflection portion 4 of the reflective photomask blank 10 according to the embodiment of the present invention shown in Fig. 1.

[0017] (Overall structure) As shown in Fig. 1, a reflective photomask blank 10 according to an embodiment of the present invention includes a substrate 1, a multilayer reflective film 2 formed on the substrate 1, and a capping layer 3 formed on the multilayer reflective film 2. As a result, a reflective portion 5 having the multilayer reflective film 2 and the capping layer 3 is formed on the substrate 1, and a low-reflection portion 4 is provided on the reflective portion 5. The low-reflection portion 4 may be composed of an absorbing layer, or may be composed of an adhesive layer and an absorbing layer as shown in Fig. 4.

[0018] (substrate) The substrate 1 according to the embodiment of the present invention may be, for example, a flat silicon (Si) substrate, a synthetic quartz substrate, etc. The substrate 1 may be made of low thermal expansion glass containing titanium (Ti), but the present invention is not limited to these materials as long as they have a small thermal expansion coefficient.

[0019] (Multilayer reflective film) The multilayer reflective film 2 according to the embodiment of the present invention may be any film that reflects EUV light (extreme ultraviolet light) as exposure light, and may be a multilayer reflective film made of a combination of materials that have significantly different refractive indices for EUV light. The multilayer reflective film 2 may be formed by repeatedly stacking layers of a combination of molybdenum (Mo) and silicon (Si), or molybdenum (Mo) and beryllium (Be), for example, for about 40 periods.

[0020] (capping layer) The capping layer 3 according to the embodiment of the present invention is formed of a material that is resistant to dry etching performed when forming a transfer pattern (mask pattern) in the low reflection portion 4, and functions as an etching stopper that prevents damage to the multilayer reflective film 2 when etching the low reflection portion 4. The capping layer 3 is formed of a material that contains at least ruthenium (Ru). The content of ruthenium (Ru) in the capping layer 3 is preferably in the range of 30 mass% to 100 mass% with respect to the total mass of the capping layer 3, more preferably in the range of 50 mass% to 100 mass%, and even more preferably in the range of 80 mass% to 100 mass%. If the content of ruthenium (Ru) is 30 mass% or more with respect to the total mass of the capping layer 3, the function as the above-mentioned etching stopper is further improved. Although not shown, a back conductive film can be formed on the surface of the substrate 1 on which the multilayer reflective film 2 is not formed. The back conductive film is a film for fixing the reflective photomask 20 by utilizing the principle of an electrostatic chuck when the reflective photomask 20 is placed in an exposure machine.

[0021] (Low reflective part) As shown in FIG. 2, a low-reflection portion pattern 4a of a reflective photomask 20 is formed by removing a part of the low-reflection portion 4 of a reflective photomask blank 10, that is, by patterning the low-reflection portion 4. In EUV lithography, EUV light is incident at an angle and reflected by the reflection portion 5, but the low-reflection portion pattern 4a obstructs the light path, resulting in a projection effect, which may deteriorate the transfer performance onto a wafer (semiconductor substrate). This deterioration in transfer performance can be reduced by reducing the thickness of the low-reflection portion 4 that absorbs EUV light. In order to reduce the thickness of the low-reflection portion 4, it is preferable to use a material that is more absorbent for EUV light than conventional materials, that is, a material with a high extinction coefficient k at a wavelength of 13.5 nm.

[0022] FIG. 3 is a graph showing the optical constants of some metal materials with respect to the wavelength of EUV light of 13.5 nm. The horizontal axis of FIG. 3 represents the refractive index n, and the vertical axis represents the extinction coefficient k. The extinction coefficient k of tantalum (Ta), which is the main material of the conventional low-reflectivity portion 4, is 0.041. If a material having a damping coefficient k is used, it is possible to make the thickness of the low reflectivity portion 4 thinner than in the past. Materials that satisfy the above-mentioned extinction coefficient k include, for example, silver (Ag), platinum (Pt), indium (In), cobalt (Co), tin (Sn), nickel (Ni), and tellurium (Te), as shown in FIG.

[0023] The intensity of reflected light from the reflective portion 5 is Rm, and the intensity of reflected light from the low-reflective portion 4 is Ra. The optical density (OD) value, which is an index representing the contrast in light intensity between the reflective portion 5 and the low-reflective portion 4, is defined by the following formula (1). OD = -log(Ra / Rm) Equation (1) The larger the OD value, the better the contrast and the higher the transferability. For pattern transfer, OD>1 is necessary, but based on the above comparison with the conventional method, an OD value of 1.5 or more is more preferable.

[0024] As described above, compound materials mainly composed of Ta have been used for the low-reflection portion 4 of conventional EUV reflective photomasks. In this case, to obtain an OD value of 1 or more, the low-reflection portion 4 needs to be 40 nm thick or more, and to obtain an OD value of 2 or more, the low-reflection portion 4 needs to be 70 nm thick or more. The extinction coefficient k of tantalum (Ta) is 0.041, but among the materials shown in Figure 3, silver (Ag), platinum (Pt), indium (In), cobalt (Co), tin (Sn), nickel (Ni), and tellurium (Te) all have extinction coefficients of 0.041 or more, so they can be made thinner than when tantalum (Ta) is used. In particular, oxides of tin (Sn) and indium (In) are desirable candidate materials because they can be etched with chlorine-based gas.

[0025] For example, by applying a material containing tin (Sn) and oxygen (O) with an extinction coefficient k of 0.06 or more, or a material containing indium (In) and oxygen (O) to the low-reflective portion 4, it is possible to reduce the film thickness of the low-reflective portion 4 to 17 nm if the OD value is at least 1, and to reduce the film thickness of the low-reflective portion 4 to 45 nm or less if the OD value is 2 or more. However, if the film thickness of the low-reflective portion 4 exceeds 45 nm, the projection effect will be about the same as that of a low-reflective portion 4 with a film thickness of 60 nm that is formed from a conventional compound material mainly composed of Ta.

[0026] Therefore, the low reflection portion 4 in the embodiment of the present invention is characterized by containing 40 at % or more of at least one material selected from silver (Ag), cobalt (Co), indium (In), platinum (Pt), tin (Sn), nickel (Ni), tellurium (Te), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and oxynitride boride thereof (hereinafter also referred to as high extinction coefficient material) and having a film thickness of 45 nm or less. In other words, when the film thickness of the low reflection portion 4 is within the range of 45 nm or less, the projection effect can be sufficiently reduced and the transfer performance is improved compared to the conventional low reflection portion 4 formed of a compound material mainly composed of tantalum (Ta). Here, if the content of the above-mentioned high extinction coefficient material is 40 at % or more with respect to the number of atoms of the entire low reflection portion 4, it is easy to make the film thickness of the low reflection portion 4 45 nm or less. Furthermore, if the content of the high extinction coefficient material is 75 at % or less with respect to the total number of atoms in the low reflectivity portion 4, the adhesion to the capping layer 3 is improved. Note that the content of the high extinction coefficient material is preferably within a range of 45 at % to 65 at % with respect to the total number of atoms in the low reflectivity portion 4, and more preferably within a range of 50 at % to 60 at %. Furthermore, in order to transfer a fine pattern, it is desirable to have a high contrast between the intensity of light reflected from the reflective portion 5 and the low reflective portion 4. Therefore, it is more preferable that the OD value of the low reflective portion 4 is 1.5 or more.

[0027] The materials belonging to the first material group and the second material group, which will be described later, satisfy the conditions for improving the adhesion between the capping layer 3 and the low-reflection portion 4. This is because the first material group This is because the materials belonging to the first material group and the materials belonging to the second material group each have a surface free energy value close to that of ruthenium (Ru) contained in the capping layer 3. In particular, the materials belonging to the first material group have a surface free energy value closer to that of ruthenium (Ru) compared to the materials belonging to the second material group, and therefore further strengthen the adhesion between the capping layer 3 and the low-reflectivity portion 4.

[0028] The first group of materials has a surface free energy of ruthenium (Ru) ±0.5 [J / m2 The materials in the second group have a surface free energy of less than ±0.5 [J / m] based on the surface free energy of ruthenium (Ru). 2 ] or more ±2[J / m 2 ]. For this reason, the material contained in the region of the low-reflection section 4 at least 2 nm thick from the capping layer 3 side can be a material belonging to the first material group or a material belonging to the second material group, as well as a material mixed with another material; however, in order not to reduce adhesion to the capping layer 3, it is preferable that the material contains at least one material selected from the first material group or at least one material selected from the second material group in an amount of at least 25 at % or more and at least 30 at % or more, respectively.

[0029] Here, the above-mentioned first material group refers to a material group consisting of ruthenium (Ru), titanium (Ti), vanadium (V), chromium (Cr), manganese (Mn), iron (Fe), niobium (Nb), molybdenum (Mo), technetium (Tc), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), osmium (Os), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof.

[0030] Furthermore, the above-mentioned second material group refers to a material group consisting of scandium (Sc), copper (Cu), yttrium (Y), zirconium (Zr), palladium (Pd), lanthanum (La), hafnium (Hf), gold (Au), beryllium (Be), magnesium (Mg), calcium (Ca), zinc (Zn), cadmium (Cd), and aluminum (Al), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof.

[0031] If the content of at least one material selected from the first material group is 25 at % or more relative to the number of atoms of all materials constituting the region of the low-reflectivity portion 4 having a thickness of at least 2 nm from the capping layer 3 side, the adhesion between the capping layer 3 and the low-reflectivity portion 4 will be further strengthened. Note that the content of at least one material selected from the first material group is more preferably 40 at % or more relative to the number of atoms of all materials constituting the region of the low-reflectivity portion 4 having a thickness of at least 2 nm from the capping layer 3 side, and even more preferably 50 at % or more.

[0032] If the content of at least one material selected from the second material group is 30 at % or more relative to the number of atoms of all materials constituting the region of the low-reflectivity portion 4 having a thickness of at least 2 nm from the capping layer 3 side, the adhesion between the capping layer 3 and the low-reflectivity portion 4 will be further strengthened. Note that the content of at least one material selected from the second material group is more preferably 45 at % or more relative to the number of atoms of all materials constituting the region of the low-reflectivity portion 4 having a thickness of at least 2 nm from the capping layer 3 side, and even more preferably 55 at % or more.

[0033] In the above-described embodiment, the content of at least one material selected from the first material group is 25 at % or more relative to the number of atoms of the entire material constituting the region of the low reflection portion 4 having a thickness of at least 2 nm from the capping layer 3 side, or the content of at least one material selected from the second material group is 25 at % or more relative to the number of atoms of the entire material constituting the region of the low reflection portion 4 having a thickness of at least 2 nm from the capping layer 3 side. In the above description, the content of at least one material is 30 at % or more of the total number of atoms of the material constituting the region of the low-reflection portion 4 having a thickness of at least 2 nm from the capping layer 3 side, but the present invention is not limited to this. For example, the content of at least one material selected from the first material group may be 25 at % or more relative to the atomic number of materials constituting the entire low-reflection section 4 consisting of only the absorption layer, and the content of at least one material selected from the second material group may be 30 at % or more relative to the atomic number of materials constituting the entire low-reflection section 4 consisting of only the absorption layer.

[0034] That is, if the content of at least one material selected from the first material group is 25 at% or more with respect to the total number of atoms in the low-reflection portion 4, the adhesion between the capping layer 3 and the low-reflection portion 4 will be further strengthened. Also, if the content of at least one material selected from the first material group is 60 at% or less with respect to the total number of atoms in the low-reflection portion 4, there is little possibility of adversely affecting the projection effect. Note that the content of at least one material selected from the first material group is preferably within a range of 30 at% to 55 at% with respect to the total number of atoms in the low-reflection portion 4, and more preferably within a range of 35 at% to 50 at%. Furthermore, the composition of the second material group in the entire low reflectivity portion 4 is preferably in the range of 30 at % to 60 at %, more preferably in the range of 35 at % to 55 at %, and optimally in the range of 40 at % to 50 at %.

[0035] In addition, the content of at least one material selected from the first material group may be 25 at % or more of the atomic number of materials constituting the entire low-reflection section 4 composed of the adhesion layer and the absorption layer described below, and the content of at least one material selected from the second material group may be 30 at % or more of the atomic number of materials constituting the entire low-reflection section 4 composed of the adhesion layer and the absorption layer described below.

[0036] (First form) A first embodiment of the present invention will be described with reference to FIG. In order to facilitate etching process, it is effective to make the absorbing layer constituting the low reflectance portion 4 a film having a uniform composition. Therefore, in order to facilitate etching processability, the absorption layer is preferably a structure having a uniform composition that contains at least 40 at.% or more of one or more materials (high extinction coefficient materials) selected from silver (Ag), cobalt (Co), indium (In), platinum (Pt), tin (Sn), nickel (Ni), tellurium (Te), and their oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides, relative to the number of atoms in the entire absorption layer, and that contains at least 25 at.% or more of one or more materials selected from a first material group, or at least 30 at.% or more of one or more materials selected from a second material group.

[0037] In addition, the absorption layer according to this embodiment may be composed of multiple layers, and an HM (hard mask) layer serving as an etching mask, an AR (anti-reflection) film for improving the contrast of the inspection light, etc. may be provided on the absorption layer. Even in this case, the total thickness of the layers constituting the absorption layer is preferably 45 nm or less. That is, even if the low reflection part 4 is composed of a single layer, its thickness is preferably 45 nm or less, and even if it is divided into multiple layers, its total thickness is preferably 45 nm or less.

[0038] (Second Form) A second embodiment of the present invention will be described with reference to FIG. In order to reduce the projection effect and prevent atomic hydrogen from penetrating between the capping layer and the absorbing layer, a material with a high extinction coefficient k is added to the absorbing layer 542, as shown in FIG. In addition, it is effective to provide an adhesion layer 541 for more firmly adhering the capping layer 3 and the absorbing layer 542. The material for forming the adhesion layer 541 is preferably the same as the material for forming the absorbing layer (low reflection portion 4) shown in FIG. Therefore, it is preferable that the adhesion layer 541 has a film thickness of 2 nm or more and 20 nm or less, and contains 25 at % or more of one or more materials selected from the above-mentioned first material group, or 30 at % or more of one or more materials selected from the above-mentioned second material group. If the thickness of the adhesion layer 541 is 2 nm or more, it is possible to analyze the constituent elements (measure the content of the constituent elements) using a commercially available XPS device. Also, if the thickness of the adhesion layer 541 is 20 nm or less, it is sufficiently thin as the overall thickness of the low reflection portion 54, and the possibility of deteriorating the transfer performance (the possibility of adversely affecting the projection effect) is reduced.

[0039] (Third Form) A third embodiment of the present invention will be described with reference to FIG. The cross-sectional sidewall angle of the absorbing layer (low-reflection portion 4) after patterning is desirably a rectangular shape nearly perpendicular to the surface of the capping layer 3, and if the cross-sectional sidewall of the absorbing layer (low-reflection portion 4) has a stepped or tapered shape, there is a concern that unintended attenuation and amplification of the exposure light and changes in the reflected light intensity at the pattern end may deteriorate the transfer performance. Therefore, it is desirable that the cross section of the absorbing layer (low-reflection portion 4) after patterning has no steps.

[0040] Therefore, it is desirable to have a material having a surface free energy close to that of ruthenium (Ru) that forms the capping layer 3 contained in a large amount in the region of the low-reflectivity portion 4 facing the capping layer 3, and to have the composition ratio of that material continuously change so that it decreases toward the region of the low-reflectivity portion 4 opposite the capping layer 3 (the outermost surface side), thereby changing the composition without forming a layer boundary. Therefore, it is preferable that the low-reflectivity portion 4 on the capping layer 3 side contains 25 at % or more of one or more materials selected from the first material group, or 30 at % or more of one or more materials selected from the second material group, in a film thickness (region) of at least 2 nm or more, and that the region of the low-reflectivity portion 4 opposite the capping layer 3 (the outermost surface side) is a structure in which the composition ratio of the first material group or the second material group changes continuously so that it is lower than that of the capping layer 3 side.

[0041] Hereinafter, the distribution of the content (concentration) of the material belonging to the first material group and the content (concentration) of the high extinction coefficient material, which "change continuously," in the low-reflection section 4 will be described. Note that in this embodiment, the distribution of the content (concentration) of the material belonging to the first material group and the distribution of the content (concentration) of the material belonging to the second material group are qualitatively the same. Therefore, the description of the distribution of the content (concentration) of the material belonging to the second material group will be omitted here. In this embodiment, it is preferable that the content of the material belonging to the first material group decreases linearly (linearly), curvedly (e.g., S-curve), or exponentially from the capping layer 3 side toward the outermost surface side of the low-reflection section 4. In addition, in this embodiment, it is preferable that the content of the high extinction coefficient material increases linearly (linearly), curvedly (e.g., S-curve), or exponentially from the capping layer 3 side toward the outermost surface side of the low-reflection section 4.

[0042] Moreover, it is preferable that at least one of the materials belonging to the first material group and the high extinction coefficient material has a uniform composition in at least one of the regions on the capping layer 3 side and the outermost surface side of the low reflectivity section 4. In this embodiment, the "region on the capping layer 3 side" means the lower 10% of the entire capping layer 3, and the "outermost surface side region" means the upper 10% of the entire low reflectivity section 4. Furthermore, the point (location) where the content (concentration) of the material belonging to the first material group and the content (concentration) of the high extinction coefficient material are the same may be located on the capping layer 3 side or on the outermost surface side of the low reflectivity section 4 when the low reflectivity section 4 is divided into two equal parts in the thickness direction. Furthermore, the region on the capping layer 3 side (the lower 10% of the entire low reflectivity section 4) does not have to be made up of only materials belonging to the first material group, and the region on the outermost surface side (the upper 10% of the entire low reflectivity section 4) does not have to be made up of only high extinction coefficient materials. In other words, the region on the capping layer 3 side may contain a high extinction coefficient material, and the region on the outermost surface side may contain a material belonging to the first material group.

[0043] Hereinafter, the distribution of the content (concentration) of the material belonging to the first material group and the content (concentration) of the high extinction coefficient material in the low reflection portion 4 will be described with reference to FIGS. 5 to 8 are conceptual diagrams showing the content distribution (concentration distribution) of the material belonging to the first material group and the content distribution (concentration distribution) of the high extinction coefficient material. In each of Figs. 5 to 8, the vertical axis indicates the content (%) of the material belonging to the first material group and the high extinction coefficient material in the entire low reflection portion 4, and the horizontal axis indicates the depth direction of the entire low reflection portion 4. Figure 5 shows that the content of the material belonging to the first material group (solid line) decreases linearly from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, and the content of the high extinction coefficient material (dashed line) increases linearly from the capping layer 3 side toward the outermost surface side of the low-reflection section 4.

[0044] FIG. 6 shows a configuration in which the content of the material belonging to the first material group (solid line) decreases linearly from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, and the content of the high extinction coefficient material (dashed line) increases linearly from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, and the point (location) where the content (concentration) of the material belonging to the first material group and the content (concentration) of the high extinction coefficient material are the same is located on the capping layer 3 side when the low-reflection section 4 is divided into two equal parts in the thickness direction, and the region on the capping layer 3 side contains the high extinction coefficient material, and the region on the outermost surface side contains the material belonging to the first material group.

[0045] FIG. 7 shows a configuration in which the content of the material belonging to the first material group (solid line) exponentially decreases from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, and the content of the high extinction coefficient material (dashed line) exponentially increases from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, with the capping layer 3 side region and the outermost surface side region each having a uniform composition, and the point (location) where the content (concentration) of the material belonging to the first material group and the content (concentration) of the high extinction coefficient material are the same is located on the outermost surface side when the low-reflection section 4 is divided into two equal parts in the thickness direction.

[0046] Figure 8 shows a configuration in which the content of the material belonging to the first material group (solid line) decreases in a curved manner (drawing an inverted S-shaped curve) from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, and the content of the high extinction coefficient material (dashed line) increases in a curved manner (drawing an S-shaped curve) from the capping layer 3 side toward the outermost surface side of the low-reflection section 4, with the region on the capping layer 3 side and the region on the outermost surface side each having a uniform composition.

[0047] In the above embodiment, the low-reflection portion 4 has an increased content of compound material (high extinction coefficient material) having high absorbency for EUV light from the capping layer 3 side toward the outermost surface side of the low-reflection portion 4, and an decreased content of compound material (material belonging to the first material group or material belonging to the second material group) having a value close to the surface free energy of ruthenium (Ru) contained in the capping layer 3 from the capping layer 3 side toward the outermost surface side of the low-reflection portion 4, thereby reducing shadowing and strengthening adhesion between the capping layer 3 and the low-reflection portion 4. As a result, the dimensional accuracy and shape accuracy of the pattern transferred onto the wafer are improved. Moreover, a photomask that can be used for a long period of time can be produced. In this embodiment, the distribution of the contents of the materials belonging to the first material group and the high extinction coefficient material is not limited to the above-mentioned distribution, and may be a combination of the above distributions.

[0048] The material constituting the low-reflection portion 4 may contain, for example, beryllium (Be), calcium (Ca), scandium (Sc), vanadium (V), manganese (Mn), iron (Fe), copper (Cu), germanium (Ge), arsenic (As), strontium (Sr), technetium (Tc), rhodium (Rh), barium (Ba), tungsten (W), rhenium (Re), osmium (Os), gold (Au), etc., which can improve roughness, in-plane dimensional uniformity, and in-plane uniformity of the transferred image, and can be a sufficiently amorphous material. In addition, the material constituting the low-reflection portion 4 can contain, for example, silver (Ag), cobalt (Co), indium (In), platinum (Pt), tin (Sn), nickel (Ni), tellurium (Te), etc., so that the material has an extinction coefficient k greater than that of tantalum (Ta), which is the conventional main material.

[0049] In addition, the material constituting the low-reflection portion 4 may contain, for example, tantalum (Ta), chromium (Cr), titanium (Ti), aluminum (Al), silicon (Si), zirconium (Zr), vanadium (V), hafnium (Hf), niobium (Nb), yttrium (Y), lead (Pb), gallium (Ga), etc., making it less likely to react with hydrogen radicals and making it more resistant to hydrogen radicals. In addition, the material constituting the low-reflection portion 4 may contain, for example, tantalum (Ta), chromium (Cr), titanium (Ti), aluminum (Al), vanadium (V), hafnium (Hf), etc., so that an oxide film 6 having hydrogen radical resistance can be formed to cover the exposed surface of the low-reflection portion 4, as shown in FIG. 9.

[0050] In addition, the material constituting the low-reflection portion 4 can contain, for example, aluminum (Al), chromium (Cr), zirconium (Zr), etc., so that the material has low reactivity with chemicals such as SPM and APM that are commonly used for mask cleaning, and can be made more resistant to cleaning. Furthermore, the material constituting the low-reflection portion 4 contains, for example, silicon nitride (SiN), tantalum oxide (TaO), or the like, and can be a material that has high light absorption at wavelengths of 190 nm to 260 nm and improves the contrast of the inspection light. In addition, the material constituting the low-reflection portion 4 can contain, for example, cobalt (Co), ruthenium (Ru), iridium (Ir), gold (Au), palladium (Pd), platinum (Pt), molybdenum (Mo), etc., and can be a material that has a refractive index n of less than 0.95 for a wavelength of 13.5 nm and improves phase shifting properties. Although examples of the effects of the materials that can be contained in the low-reflectivity portion 4 have been described above, the effects of each material are not limited to the above examples, and each material may have a plurality of effects.

[0051] Furthermore, since the reflective photomask 20 is exposed to an environment in which atomic hydrogen such as hydrogen radicals and hydrogen ions exists, unless the material has high interlayer adhesion to atomic hydrogen, it cannot withstand long-term use. In this embodiment, hydrogen plasma is generated using microwave plasma with a power of 1 kW in a vacuum of 0.36 millibars (mbar) or less, and after exposure to a hydrogen radical-rich environment for a certain period of time, the reflective photomask 20 is cut and the cross sections of the capping layer 3 and the low-reflectivity portion 4 are observed with a TEM (transmission electron microscope), and a material in which no voids are visually observed is determined to be a material with high interlayer adhesion to atomic hydrogen. The TEM observation results for voids shown in Table 1 below were obtained by observing an area of ​​200 nm multiple times at a magnification of 600,000 times. When voids were not observed with the naked eye, they were evaluated as "○", and when they were observed with the naked eye, they were evaluated as "×".

[0052] Examples of the reflective photomask blank and the reflective photomask according to the present invention will be described below. [Example 1] 10, a multilayer reflective film 12 is formed by stacking 40 layers of a laminate film made of a pair of silicon (Si) and molybdenum (Mo) on a synthetic quartz substrate 11 having low thermal expansion characteristics. The thickness of the multilayer reflective film 12 is 280 nm. Next, a capping layer 13 made of ruthenium (Ru) was formed as an intermediate film to a thickness of 2.5 nm on the multilayer reflective film 12. As a result, a reflective portion 16 having the multilayer reflective film 12 and the capping layer 13 was formed on the substrate 11.

[0053] Next, the absorbing layer 14 was formed on the capping layer 13 with a homogeneous material of tin oxide (high extinction coefficient material) and tantalum oxide (material belonging to the first material group) in a ratio of 75:25, so as to have a thickness of 40 nm. The atomic ratio of tin (Sn) and oxygen (O) was measured by EDX (energy dispersive X-ray analysis) and found to be 1:2.5. In addition, the crystallinity of the absorbing layer 14 was measured by XRD (X-ray diffraction) and found to be amorphous. As a result, the absorbing layer 14 was formed on the reflecting portion 16.

[0054] Next, a back surface conductive film 15 made of chromium nitride was formed to a thickness of 100 nm on the side of the substrate 11 on which the multilayer reflective film 12 was not formed, thereby producing the reflective photomask blank 100 of Example 1. A multi-target sputtering device was used to deposit each film on the substrate 11. The thickness of each film was controlled by the sputtering time.

[0055] Next, a method for producing the reflective photomask 200 will be described with reference to FIGS. As shown in FIG. 11, a positive chemically amplified resist (SEBP9012: manufactured by Shin-Etsu Chemical Co., Ltd.) was spin-coated to a thickness of 120 nm on the absorption layer 14 of the reflective photomask blank 100, and baked at 110° C. for 10 minutes to form a resist film 17. Next, a predetermined pattern was drawn on the resist film 17 formed of a positive chemically amplified resist by an electron beam lithography machine (JBX3030: manufactured by JEOL Ltd.). After that, a baking process was performed at 110° C. for 10 minutes, and then a spray development (SFG3000: manufactured by Sigma Meltec Co., Ltd.) was performed. As a result, a resist pattern 17a was formed as shown in FIG.

[0056] Next, the absorbing layer 14 was patterned by dry etching mainly using a chlorine-based gas to form a low reflection portion pattern 14a, as shown in FIG. Next, the remaining resist pattern 17a was peeled off to produce a reflective photomask 200 according to this embodiment as shown in FIG. Next, the reflective photomask 200 according to this embodiment was immersed in sulfuric acid at 80° C. for 10 minutes, and then immersed in a cleaning tank filled with a cleaning solution of ammonia, 30% by mass hydrogen peroxide, and water in a ratio of 1:1:20 for 10 minutes using 500 W megasonics, and washed with running water for 10 minutes. After that, the film thickness was measured with an AFM (atomic force microscope) and compared with the film thickness at the time of film formation, but no change was observed in the film thickness.

[0057] In this embodiment, the low reflection portion pattern 14a formed in the absorber layer 14 includes a 64 nm line-and-space (LS) pattern, a 200 nm line-width LS pattern for measuring the film thickness of the absorber layer 14 using an AFM, and a 4 mm square low reflection portion removed portion for measuring the EUV reflectance on a reflective photomask 200 for transfer evaluation. The 64 nm line-width LS pattern was designed in each of the x and y directions as shown in FIG. 15 so that the influence of the projection effect caused by oblique irradiation of EUV can be easily seen.

[0058] [Example 2] 16, an adhesion layer 241 made of tantalum oxide (a material belonging to a first material group) was formed on the capping layer 13 to a thickness of 2 nm. The atomic ratio of tantalum (Ta) to oxygen (O) was found to be 1:1.9 when measured by EDX (energy dispersive X-ray analysis). In addition, it was found to be amorphous when measured by XRD (X-ray diffraction). Next, an absorption layer 242 made of tin oxide (high extinction coefficient material) was deposited to a thickness of 38 nm on the layer deposited on the capping layer 13. As a result, the total thickness of the low reflection portion 24 was 40 nm. However, in the low reflectance portion 24, tantalum oxide and tin oxide are separated into upper and lower layers, and the film is not one whose composition changes continuously. The atomic ratio of tin (Sn) to oxygen (O) was measured by EDX (energy dispersive X-ray analysis) to be 1:2.5. In addition, measurement by XRD (X-ray diffraction) revealed that the material was amorphous. A reflective photomask blank 101 and a reflective photomask 201 having a low-reflection pattern 24a of Example 2 shown in Figures 16 and 17 were produced in the same manner as in Example 1, except for the formation of the adhesion layer 241 and the absorption layer 242.

[0059] [Example 3] As shown in Fig. 18, a material containing tantalum (Ta) and oxygen (O) was formed on the capping layer 13 to a thickness of 2 nm. The atomic ratio of tantalum (Ta) to oxygen (O) was found to be 1:1.9 when measured by EDX (energy dispersive X-ray analysis). In addition, it was found to be amorphous when measured by XRD (X-ray diffraction). Next, on the layer formed on the capping layer 13, a film of a material containing tantalum (Ta), tin (Sn) and oxygen (O) was formed to a thickness of 38 nm. In this manner, the absorbing layer 34 was formed on the capping layer 13 . The absorbing layer 34 was formed by continuously changing the sputtering target voltage so as to prevent the generation of layer boundaries during film formation.

[0060] In addition, when the composition was analyzed by XPS (X-ray photoelectron spectroscopy), it was found that the composition change was observed as shown in Fig. 22. That is, the content (solid line) of tantalum (Ta) and oxygen (O) belonging to the first material group is 25 at% or more with respect to the total number of atoms in the absorbing layer 34, and decreases in a curved manner (drawing an inverted S-shaped curve) from the capping layer 13 side toward the outermost surface side of the absorbing layer 34, and the content (dashed line) of tin (Sn) and oxygen (O) belonging to the high extinction coefficient material is 40 at% or more with respect to the total number of atoms in the absorbing layer 34, and increases in a curved manner (drawing an S-shaped curve) from the capping layer 13 side toward the outermost surface side of the absorbing layer 34. Furthermore, the composition is uniform in the region on the capping layer 13 side and the region on the outermost surface side of the absorbing layer 34. However, since the depth resolution of the XPS used in this experiment is 2 nm, the composition change in the depth direction within a 2 nm thick range on the capping layer 13 side of the absorbing layer 34 could not be measured.

[0061] On the side of the absorbing layer 34 opposite to the capping layer 13 side (the outermost surface side), the atomic ratio of tantalum (Ta), tin (Sn), and oxygen (O) was found to be 0:1:1.25 when measured by EDX (energy dispersive X-ray analysis).In addition, when measured by XRD (X-ray diffraction device), it was found to be amorphous. A reflective photomask blank 102 and a reflective photomask 202 having a low reflection portion pattern 34a of Example 3 shown in FIGS. 18 and 19 were produced in the same manner as in Example 1, except for the formation of the absorbing layer 34.

[0062] [Example 4] A reflective photomask blank 100 and a reflective photomask 200 having a low-reflection portion pattern 14a of Example 4 shown in Figures 10 and 14 were produced in the same manner as in Example 1, except that tantalum oxide (a material belonging to the first material group) was changed to zirconium oxide (a material belonging to the second material group). The ratio of tin oxide (high extinction coefficient material) to zirconium oxide (material belonging to the second material group) in the absorbing layer 14 formed on the capping layer 13 was 75:25. The atomic ratio of tin (Sn) to oxygen (O) was measured by EDX (energy dispersive X-ray analysis) and found to be 1:2.5. The crystallinity of the absorbing layer 14 was measured by XRD (X-ray diffraction) and found to be amorphous.

[0063] [Example 5] A reflective photomask blank 101 and a reflective photomask 201 having a low-reflection portion pattern 24a of Example 5 shown in Figures 16 and 17 were produced in the same manner as in Example 2, except that tantalum oxide (a material belonging to the first material group) was changed to zirconium oxide (a material belonging to the second material group). The ratio of the number of zirconium (Zr) atoms to oxygen (O) atoms in the layer formed on the capping layer 13 was found to be 1:1.9 when measured by EDX (energy dispersive X-ray analysis), and was found to be amorphous when measured by XRD (X-ray diffraction). Next, an absorption layer 242 made of tin oxide (high extinction coefficient material) was formed to a thickness of 38 nm on the layer formed on the capping layer 13. As a result, the total thickness of the low reflection portion 24 was 40 nm. However, in the low reflectance portion 24, zirconium oxide and tin oxide are separated into upper and lower layers, and the film is not one whose composition changes continuously. The atomic ratio of tin (Sn) to oxygen (O) was 1:2.5 when measured by EDX (energy dispersive X-ray analysis), and was found to be amorphous when measured by XRD (X-ray diffraction).

[0064] [Example 6] A reflective photomask blank 102 of Example 6 and a reflective photomask 202 having a low-reflection portion pattern 34a shown in Figures 18 and 19 were produced in the same manner as in Example 3, except that tantalum oxide (a material belonging to the first material group) was changed to zirconium oxide (a material belonging to the second material group). The ratio of the number of zirconium (Zr) atoms to oxygen (O) atoms in the layer formed on the capping layer 13 was found to be 1:1.9 when measured by EDX (energy dispersive X-ray analysis), and was found to be amorphous when measured by XRD (X-ray diffraction). Furthermore, on the side of the absorbing layer 34 opposite to the capping layer 13 side (the outermost surface side), the atomic ratio of zirconium (Zr), tin (Sn), and oxygen (O) was found to be 0:1:1.25 when measured by EDX (energy dispersive X-ray analysis). Also, when measured by XRD (X-ray diffraction device), it was found to be amorphous.

[0065] [Example 7] The reflective photomask blank 101 of Example 2 and the reflective photomask 201 having the low-reflection pattern 24a shown in Figures 16 and 17 were produced in the same manner as in Example 2, except that the adhesion layer 241 formed of tantalum oxide (a material belonging to the first material group) and having a thickness of 2 nm was changed to an adhesion layer 241 formed of zirconium oxide (a material belonging to the second material group) and having a thickness of 20 nm.

[0066] [Comparative Example 1] On the capping layer 13, the absorbing layer 14 was formed from a homogeneous material of tin oxide (high extinction coefficient material) and tantalum oxide (material belonging to the first material group) in a ratio of 90:10, with a thickness of 40 nm. The atomic ratio of tin (Sn) to oxygen (O) was measured by EDX (energy dispersive X-ray analysis) to be 1:2.5. In addition, the crystallinity of the absorbing layer 14 was measured by XRD (X-ray diffraction) and found to be amorphous. A reflective photomask blank 100 and a reflective photomask 200 of Comparative Example 1 shown in FIGS. 10 and 14 were produced in the same manner as in Example 1, except for the formation of the absorbing layer 14.

[0067] [Comparative Example 2] An adhesion layer 241 made of tantalum oxide was formed on the capping layer 13 to a thickness of 16 nm. The atomic ratio of tantalum (Ta) to oxygen (O) was found to be 1:1.9 when measured by EDX (energy dispersive X-ray analysis). In addition, it was found to be amorphous when measured by XRD (X-ray diffraction). Next, an absorbing layer 242 made of tin oxide was deposited to a thickness of 36 nm on the layer deposited on the capping layer 13. As a result, the total thickness of the low reflection portion 24 was 52 nm. However, in the low reflectance portion 24, tantalum oxide and tin oxide are separated into upper and lower layers, and the film is not one whose composition changes continuously. The atomic ratio of tin (Sn) to oxygen (O) was measured by EDX (energy dispersive X-ray analysis) to be 1:2.5. In addition, measurement by XRD (X-ray diffraction) revealed that the material was amorphous. A reflective photomask blank 101 and a reflective photomask 201 of Comparative Example 2 shown in FIGS. 16 and 17 were produced in the same manner as in Example 1, except for the formation of the adhesive layer 241 and the absorbing layer 242.

[0068] [Comparative Example 3] A material containing tantalum (Ta), tin (Sn), and oxygen (O) was deposited on the capping layer 13 to a thickness of 2 nm. The atomic ratio of tantalum (Ta), tin (Sn), and oxygen (O) was found to be 3.5:25.7:70.8 when measured by EDX (energy dispersive X-ray analysis). In addition, it was found to be amorphous when measured by XRD (X-ray diffraction). Next, a film of tantalum (Ta), tin (Sn) and oxygen (O) was formed to a thickness of 38 nm on the layer formed on the capping layer 13. In this manner, the absorbing layer 34 was formed on the capping layer 13 . The absorbing layer 34 was formed by continuously changing the sputtering target voltage so as to prevent the generation of layer boundaries during film formation.

[0069] Furthermore, composition analysis was performed by XPS (X-ray photoelectron spectroscopy), and it was found that the composition changes as shown in Fig. 23 were observed. That is, the content (solid line) of tantalum (Ta) and oxygen (O) belonging to the first material group is 25 at % or less with respect to the total number of atoms in the absorption layer 34. The composition is uniform in the region on the substrate 11 side and the region on the outermost surface side of the absorption layer 34. However, since the depth resolution of the XPS used in this experiment is 2 nm, the composition change in the depth direction within a 2 nm thick range on the capping layer 13 side of the absorbing layer 34 could not be measured. On the side of the absorbing layer 34 opposite to the capping layer 13 side (the outermost surface side), the atomic ratio of tantalum (Ta), tin (Sn), and oxygen (O) was found to be 0:1:1.25 when measured by EDX (energy dispersive X-ray analysis).In addition, when measured by XRD (X-ray diffraction device), it was found to be amorphous. A reflective photomask blank 102 and a reflective photomask 202 of Comparative Example 3 shown in FIGS. 18 and 19 were produced in the same manner as in Example 1, except for the formation of the absorbing layer 34.

[0070] [Comparative Example 4] 20, the absorbing layer 441 was formed of tantalum nitride and was deposited to a thickness of 58 nm. The outermost layer 442 was formed of tantalum oxide and was deposited to a thickness of 2 nm. This comparative example is based on the assumption of a conventional reflective photomask made of an existing film mainly composed of tantalum. However, the tantalum nitride and tantalum oxide are separated into an upper layer and a lower layer, and the film does not have a continuously changing composition. A reflective photomask blank 103 and a reflective photomask 203 having a low-reflection pattern 44a of Comparative Example 4 shown in Figures 20 and 21 were produced in the same manner as in Example 1, except for the formation of the absorption layer 441 and the outermost layer 442.

[0071] The reflectance Rm of the reflective region and the reflectance Ra of the low-reflecting region of the reflective photomask produced in the above-mentioned Examples and Comparative Examples were measured using a reflectance measuring device using EUV light. The reflectance Rm was measured in a 4 mm square low-reflecting portion removed area. From the measurement results, the OD value was calculated using the above-mentioned formula (1).

[0072] (Wafer exposure evaluation) Using an EUV exposure tool (NXE3300B, manufactured by ASML), the low reflection portion patterns 14a, 24a, 34a, and 44a of the reflective photomask produced in the examples and comparative examples were transferred and exposed onto a semiconductor wafer coated with an EUV positive chemically amplified resist. At this time, the exposure dose was adjusted so that the LS pattern in the x direction in FIG. 15 was transferred as designed. After that, the transferred resist pattern was observed and line width was measured using an electron beam dimension measuring device to confirm the resolution. In this case, the HV-bias was rated as "△" for the existing film with a thickness of 6.1 nm, "○" for less than 6.1 nm, and "◎" for 4.9 nm or less, while the OD value was rated as "○" for 1.5 or more, and "◎" for 2 or more. For HV-bias, if the evaluation was "△" or higher, there were no problems with use, so it was deemed to have passed. For OD value, if the evaluation was "○" or higher, there were no problems with use, so it was deemed to have passed. The evaluation results are shown in Table 1.

[0073] [Table 1]

[0074] In Table 1, in Comparative Example 4, the resist pattern dimensions on the wafer and the mask characteristics of a photomask in a Ta-based existing film, in which the absorption layer 441 is tantalum nitride with a thickness of 58 nm and the outermost layer 442 is tantalum oxide with a thickness of 2 nm, are shown. In the case of the reflective photomask 203 of Comparative Example 4, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 1.5, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias (horizontal-vertical dimension difference) was 6.1 nm, and although the image was resolved, the shadowing effect was large, resulting in low transferability.

[0075] In Table 1, in Example 1, the absorber layer 14 is made of a material consisting of tin oxide and tantalum oxide (mixture ratio 75:25) and has a thickness of 40 nm. The graph shows the mask characteristics and the method for producing the mask. In the case of the reflective photomask 200 of Example 1, no voids were observed by visual observation from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 2.4, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 5.3 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0076] Table 1 shows the resist pattern dimensions on the wafer and the mask characteristics for a photomask in Example 2, in which the absorption layer 242 is made of tin oxide and has a thickness of 38 nm, and the adhesion layer 241 is made of tantalum oxide and has a thickness of 2 nm. In the case of the reflective photomask 201 in Example 2, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 2.7, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 5.4 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0077] In Table 1, in Example 3, a layer of tantalum oxide having a thickness of 2 nm was formed on the capping layer 13, and a layer of a material containing tantalum (Ta), tin (Sn), and oxygen (O) having a thickness of 38 nm was formed on the layer formed on the capping layer 13 by continuously changing the target voltage of sputtering, thereby forming an absorption layer 34 having a total thickness of 40 nm on the capping layer 13. The resist pattern dimensions on the wafer and the mask characteristics are shown for the photomask. In the case of the reflective photomask 202 of Example 3, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 2.1, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 4.9 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0078] Table 1 shows the resist pattern dimensions on the wafer and the mask characteristics of a photomask in Example 4, in which the absorbing layer 14 is made of a material consisting of tin oxide and zirconium oxide (mixture ratio 75:25) and has a film thickness of 40 nm. In the case of the reflective photomask 200 of Example 4, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 1.7, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 4.5 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0079] Table 1 shows the resist pattern dimensions on the wafer and the mask characteristics for a photomask in Example 5, in which the absorption layer 242 is made of tin oxide and has a thickness of 38 nm, and the adhesion layer 241 is made of zirconium oxide and has a thickness of 2 nm. In the case of the reflective photomask 201 of Example 5, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 2.6, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 5.5 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0080] In Table 1, in Example 6, a layer of zirconium oxide having a thickness of 2 nm is formed on the capping layer 13, and a layer of a material containing zirconium (Zr), tin (Sn) and oxygen (O) having a thickness of 38 nm is formed on the layer formed on the capping layer 13 by continuously changing the target voltage of sputtering, thereby forming an absorption layer 34 having a total thickness of 40 nm on the capping layer 13. The resist pattern dimensions on the wafer and the mask characteristics are shown for the photomask. In the case of the reflective photomask 202 of Example 6, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 1.6, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 4.5 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0081] Table 1 shows the resist pattern dimensions on the wafer and the mask characteristics for a photomask in Example 7, in which the absorption layer 242 is made of tin oxide and has a thickness of 20 nm, and the adhesion layer 241 is made of zirconium oxide and has a thickness of 20 nm. In the case of the reflective photomask 201 of Example 7, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 1.7, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 4.6 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0082] In Table 1, Comparative Example 1 shows the resist pattern dimensions on the wafer and the mask characteristics of a photomask in which the absorbing layer 14 is made of a material consisting of tin oxide and tantalum oxide (mixture ratio 90:10) and has a film thickness of 40 nm. In the case of the reflective photomask 200 of Comparative Example 1, TEM observation of the mask cross section showed the presence of voids that were visually observed, and the interlayer adhesion was not favorable. The OD value was 2.4, and a contrast that allowed pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 5.4 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0083] Table 1 shows the resist pattern dimensions on the wafer and the mask characteristics for a photomask in Comparative Example 2, in which the absorption layer 242 is tin oxide with a thickness of 36 nm and the adhesion layer 241 is tantalum oxide with a thickness of 16 nm. In the case of the reflective photomask 201 in Comparative Example 2, no voids were visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was good. The OD value was 2.0, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 7.6 nm, and pattern transferability was inferior to that of Comparative Example 4.

[0084] In Table 1, in Comparative Example 3, a layer having a thickness of 2 nm is formed on the capping layer 13 using a material containing tantalum (Ta), tin (Sn), and oxygen (O) (3.5:25.7:70.8), and a layer having a thickness of 38 nm is formed on the layer formed on the capping layer 13 using a material containing tantalum (Ta), tin (Sn), and oxygen (O) by continuously changing the target voltage of sputtering, thereby forming an absorption layer 34 having a total thickness of 40 nm on the capping layer 13. The resist pattern dimensions on the wafer and the mask characteristics are shown for the photomask. In the case of the reflective photomask 202 of Comparative Example 3, there were voids visually observed from the TEM observation of the mask cross section, and the interlayer adhesion was not favorable. The OD value was 2.5, and a contrast capable of pattern transfer was obtained. As a result of patterning using EUV light, the HV bias was 5.4 nm, and superior pattern transferability was obtained compared to Comparative Example 4.

[0085] Comparing Examples 1 to 7 with the existing film (Comparative Example 4), the adhesion of each of the reflective photomasks of Examples 1 to 7 was equivalent to that of the reflective photomask using the existing film, and the pattern transferability was improved. Note that, since each of the reflective photomasks of Examples 1 to 7 was superior to that of the existing film (Comparative Example 4) in both adhesion and pattern transferability, the judgment results were indicated as "◯" and "◎" and treated as "passed." Furthermore, each of the reflective photomasks of Comparative Examples 1 to 3 was inferior to that of the existing film (Comparative Example 4) in either adhesion or pattern transferability, and the judgment results were indicated as "×" and treated as "failed."

[0086] As a result, a reflective photomask having a low reflection portion including an absorption layer made of a material having a high k value on a capping layer containing at least ruthenium (Ru), and having a material having a surface free energy value close to that of ruthenium (Ru) in at least a 2 nm thick region from the capping layer side of the low reflection portion, has excellent transferability and radiation resistance, reduces the projection effect, and is a photomask with a long life and high transfer performance. In other words, a reflective photomask having a low reflection portion including an absorption layer made of a material having a high k value on a capping layer containing at least ruthenium (Ru) has excellent transferability and radiation resistance, reduces the projection effect, and is a photomask with a long life and high transfer performance. A reflective photomask having a low-reflection portion including an absorption layer composed of, for example, a reflective layer having a material with a surface free energy value close to that of ruthenium (Ru) in a region at least 2 nm thick from the capping layer side of the low-reflection portion has the property of suppressing or reducing the projection effect and strengthening the interlayer adhesion between the capping layer and the low-reflection portion. [Industrial Applicability]

[0087] The reflective photomask blank and reflective photomask according to the present invention can be suitably used for forming fine patterns by EUV exposure in the manufacturing process of semiconductor integrated circuits and the like. [Explanation of symbols]

[0088] 1. Circuit board 2...Multilayer reflective film 3. Capping layer 4...Low reflective area 4a Low reflection pattern (absorption pattern) 5...Reflector 6...Oxide film 10. Reflective photomask blank 20. Reflective photomask 11... Circuit board 12...Multilayer reflective film 13. Capping layer 14 Absorption layer (low reflection part) 14a Low reflection pattern (absorption pattern) 24...Low reflective area 241... Adhesion layer 242...Absorption layer 24a Low reflection pattern 34 Absorption layer (low reflection part) 34a Low reflection pattern (absorption pattern) 44...Low reflective area 441...Absorption layer 442...uppermost layer 44a Low reflection pattern 54...Low reflective area 541... Adhesion layer 542...Absorption layer 54a Low reflection pattern 15 Back conductive film 16...Reflector 17. Resist film 17a Resist pattern 100···Reflective Photomask Blank 200···Reflective photomask 101 Reflective photomask blank 201 Reflective photomask 102 Reflective photomask blank 202 Reflective photomask 103 Reflective photomask blank 203 Reflective photomask

Claims

1. A reflective photomask blank for producing a reflective photomask for pattern transfer using extreme ultraviolet light as a light source, comprising: A substrate; a reflecting portion formed on and in contact with the substrate to reflect incident light; a low-reflection portion formed on and in contact with the reflection portion to absorb incident light, the reflective portion includes a multilayer reflective film and a capping layer; The capping layer includes at least ruthenium (Ru), The low-reflection portion contains 40 at % or more of at least one material selected from platinum (Pt), nickel (Ni), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boride oxynitrides thereof, A region of the low reflectivity portion having a thickness of at least 2 nm from the capping layer side contains at least one material selected from a first material group consisting of ruthenium (Ru), titanium (Ti), chromium (Cr), manganese (Mn), niobium (Nb), molybdenum (Mo), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof, at a concentration of 25 at % or more; or containing 30 at % or more of at least one material selected from a second material group consisting of yttrium (Y), zirconium (Zr), palladium (Pd), hafnium (Hf), beryllium (Be), zinc (Zn), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof; A reflective photomask blank, wherein the total film thickness of the low reflection portion is 45 nm or less.

2. The low-reflection portion includes an absorption layer formed on the capping layer, or includes an adhesion layer formed on the capping layer and an absorption layer formed thereon, The absorption layer contains 40 at % or more of at least one material selected from platinum (Pt), nickel (Ni), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof; The absorption layer and the adhesion layer contain at least one material selected from the first material group at 25 at % or more, or 2. The reflective photomask blank according to claim 1, comprising at least one material selected from the second material group in an amount of 30 at % or more.

3. Even if the low-reflection portion is made of a single layer, the thickness of the layer is 45 nm or less, The low-reflection portion contains at least one material selected from the first material group at 25 at % or more, or 3. The reflective photomask blank according to claim 1, comprising at least one material selected from the second material group in an amount of 30 at % or more.

4. Even if the low reflection portion is divided into a plurality of layers, the total thickness of the layers is 45 nm or less, the adhesion layer provided on the capping layer side of the low reflection portion has a film thickness in the range of 2 nm to 20 nm, The adhesion layer contains at least one material selected from the first material group at 25 at % or more, or 3. The reflective photomask blank according to claim 1, comprising at least one material selected from the second material group in an amount of 30 at % or more.

5. A substrate; a reflecting portion formed on and in contact with the substrate to reflect incident light; a low-reflection portion formed on and in contact with the reflection portion to absorb incident light, the reflective portion includes a multilayer reflective film and a capping layer; The capping layer includes at least ruthenium (Ru), The low-reflection portion contains 40 at % or more of at least one material selected from platinum (Pt), nickel (Ni), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boride oxynitrides thereof, A region of the low reflectivity portion having a thickness of at least 2 nm from the capping layer side contains at least one material selected from a first material group consisting of ruthenium (Ru), titanium (Ti), chromium (Cr), manganese (Mn), niobium (Nb), molybdenum (Mo), rhodium (Rh), tantalum (Ta), tungsten (W), rhenium (Re), and iridium (Ir), as well as oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof, at a concentration of 25 at % or more; or containing 30 at % or more of at least one material selected from a second material group consisting of yttrium (Y), zirconium (Zr), palladium (Pd), hafnium (Hf), beryllium (Be), zinc (Zn), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof; A reflective photomask, wherein the total film thickness of the low reflection portion is 45 nm or less.

6. The low-reflection portion includes an absorption layer formed on the capping layer, or includes an adhesion layer formed on the capping layer and an absorption layer formed thereon, The absorption layer contains 40 at % or more of at least one material selected from platinum (Pt), nickel (Ni), and oxides, nitrides, fluorides, borides, oxynitrides, oxyborides, and boron oxynitrides thereof; The absorption layer and the adhesion layer contain at least one material selected from the first material group at 25 at % or more, or 6. The reflective photomask according to claim 5, comprising at least one material selected from the second material group in an amount of 30 at % or more.

7. Even if the low-reflection portion is made of a single layer, the thickness of the layer is 45 nm or less, The low-reflection portion contains at least one material selected from the first material group at 25 at % or more, or 7. The reflective photomask according to claim 5, wherein the at least one material selected from the second material group is contained in an amount of 30 at % or more.

8. Even if the low reflection portion is divided into a plurality of layers, the total thickness of the layers is 45 nm or less, the adhesion layer provided on the capping layer side of the low reflection portion has a film thickness in the range of 2 nm to 20 nm, The adhesion layer contains at least one material selected from the first material group at 25 at % or more, or 7. The reflective photomask according to claim 5, wherein the at least one material selected from the second material group is contained in an amount of 30 at % or more.

Citation Information

Patent Citations

  • Reflective mask blanks, reflective mask, and manufacturing method of semiconductor device

    JP2007273678A

  • Reflection type mask blank and reflection type mask and production methods for them, and production method for semiconductor

    JP2008118143A

  • Reflective mask blank for EUV lithography

    JP2011035104A

  • Reflection type photomask, reflection type photomask blank, and method of manufacturing the same

    JP2011176162A

  • Radiation source, lithography apparatus, and device manufacturing method

    JP2011530823A