Powder for cold spray, cold spray film, and method for producing the film

A cold spray powder with controlled pore volume and particle size distribution for rare earth compounds addresses nozzle clogging and enhances film hardness, enabling durable coatings for semiconductor equipment.

JP7585574B2Active Publication Date: 2024-11-19MITSUI MINING & SMELTING CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2020180852
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-10-28
Publication Date
2024-11-19
Estimated Expiration
2040-10-28

AI Technical Summary

Technical Problem

Existing cold spray methods face challenges with nozzle clogging during film formation and lack of suitable supply aids for forming films with high hardness, particularly for brittle materials like ceramics, and there is a need for improved film-forming compounds and methods to address these issues.

Method used

A cold spray powder containing compounds of specific rare earth elements such as yttrium, with a specific pore volume distribution and particle size range, is used to form films with enhanced hardness and supply properties, utilizing yttrium oxide, fluoride, or oxyfluoride powders with controlled pore volumes and particle sizes to prevent nozzle clogging and improve film quality.

Benefits of technology

The solution provides cold spray films with improved hardness and reduced nozzle clogging, enabling the formation of durable and corrosion-resistant coatings suitable for semiconductor manufacturing equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585574000004
    Figure 0007585574000004
  • Figure 0007585574000005
    Figure 0007585574000005
  • Figure 0007585574000006
    Figure 0007585574000006
Patent Text Reader

Abstract

To provide a material for cold spray excellent not only in deposition property but also in supply property, by using a compound of specific rare earth such as yttrium as a compound for deposition.SOLUTION: Concerning powder for cold spray containing a compound of at least one kind of element for deposition selected from Y, Yb and Gd, in a distribution of a pore volume to a pore size measured by a mercury press-in method, at least one peak is observed in the range of the pore size of 0.3 μm or more and 2.0 μm or less, and the pore volume with the pore size less than 0.3 μm is 0.1 ml / g or more and 0.5 ml / g or less.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to powders for cold spray, cold spray films and methods for making the films. [Background technology]

[0002] The cold spray method is a system that accelerates raw material particles to near the speed of sound and causes them to collide with a substrate while still in a solid phase, forming a coating. Normally, in the cold spray method, a supersonic nozzle (Laval nozzle) is used to generate a high-speed gas flow, and powder particles are injected into the gas flow to increase the collision speed, causing the material particles to collide with the substrate at high speed. Cold spray is a coating technology classified as a type of thermal spraying. However, it differs from conventional thermal spraying in that a coating is formed by colliding raw material in a molten or semi-molten state with a substrate, whereas cold spray adheres the raw material to the substrate without melting it.

[0003] Conventionally, the cold spray method has generally been used to form metal films, which have excellent ductility, and there have been very few examples of forming ceramic films, which are brittle materials. However, in recent years, the applicant has found that it is possible to form a film by the cold spray method for powder of an yttrium compound having a specific specific surface area or more (Patent Document 1).

[0004] Meanwhile, there are reports of adding alumina powder to metal powders used in cold spraying to eliminate nozzle clogging and improve the hardness of the resulting film (for example, Non-Patent Document 1). Furthermore, Patent Document 2 describes a thermal spray powder containing yttrium oxide, which has a pore radius distribution peak of 0.2 μm or more, as a thermal spray powder that can obtain a dense coating with suppressed spitting during plasma spraying. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] WO2020 / 090528 publication [Patent Document 2] JP 2006-200005 A [Non-patent literature]

[0006] [Non-Patent Document 1] Tetsuya Sonoda et al. "Preparation and Evaluation of NiAl High Temperature Corrosion Resistant Coating by Cold Spray Method", Journal of the Japan Welding Society, Vol. 28 (2010) No. 4, pp. 376-382 Summary of the Invention [Problem to be solved by the invention]

[0007] The applicant has found that with respect to the cold spray material described in Patent Document 1, depending on the film formation conditions, there may be room for improvement in terms of material supplyability, such as the occurrence of nozzle clogging during film formation. On the other hand, Non-Patent Document 1 describes the use of alumina powder as a supply aid for the metal film-forming raw material when the metal film-forming raw material is used to form a film by the cold spray method, but does not consider what kind of supply aid is suitable when a specific rare earth compound such as yttrium is used to form a film by the cold spray method. Furthermore, Patent Document 2 does not relate to powders for cold spraying, and the document makes no mention of the pore volume with a pore diameter of less than 0.3 μm, which is essential for obtaining a coating with higher hardness than conventional cold spraying methods.

[0008] Therefore, an object of the present invention is to provide a material for cold spray that is excellent not only in film-forming properties but also in supplyability, by using a compound of a specific rare earth element such as yttrium as a film-forming compound. Another object of the present invention is to provide a film having a hardness that has heretofore been difficult to obtain as a cold spray film of a compound of a specific rare earth element such as yttrium, and a method for producing the same. [Means for solving the problem]

[0009] The present invention relates to a powder for cold spraying, which contains a compound of at least one film-forming element selected from Y, Yb, and Gd, The present invention provides a powder for cold spray, in which at least one peak is observed in the pore diameter range of 0.3 μm or more and 2.0 μm or less in the distribution of pore volume versus pore diameter measured by mercury intrusion porosimetry, and the pore volume of pores with diameters less than 0.3 μm is 0.1 ml / g or more and 0.5 ml / g or less.

[0010] The present invention also provides a cold spray film formed using the powder for cold spray.

[0011] Furthermore, the present invention provides a method for producing a film, comprising a step of performing a cold spray method using the powder.

[0012] Furthermore, the present invention provides a cold spray coating comprising one or more materials selected from Y5O4F7, YOF, and YF3, and having a Vickers hardness of 70 or more and 500 or less. Effect of the Invention

[0013] According to the present invention, a material for cold spraying that is excellent not only in film-forming properties but also in supplyability can be provided by using a compound of a specific rare earth element such as yttrium as a film-forming compound. Furthermore, the present invention can provide a cold spray film of a specific rare earth compound such as yttrium that has a hardness that has been difficult to obtain in the past, and a method for producing the same. [Brief description of the drawings]

[0014] [Figure 1] FIG. 4 is a schematic diagram illustrating a powder supply method during film formation in the examples. [Diagram 2] 1 is a chart showing the pore volume distribution of the powder for cold spray in Example 1. [Diagram 3] 1 is a chart showing the pore volume distribution of the powder for cold spray in Example 2. [Figure 4] 1 is a chart showing the pore volume distribution of the powder for cold spray in Comparative Example 1. [Diagram 5] 1 is a chart showing the pore volume distribution of the powder for cold spray in Comparative Example 2. [Figure 6] 1 is a chart showing the particle size distribution of the powder for cold spray in Example 1. [Figure 7] 1 is a chart showing the particle size distribution of the powder for cold spray in Example 2. [Figure 8] 1 is a chart showing the particle size distribution of a powder for cold spray in Comparative Example 1. [Figure 9] 1 is a chart showing the particle size distribution of a powder for cold spray in Comparative Example 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will now be described based on its preferred embodiments. First, the powder for cold spray of the present invention will be described. Hereinafter, "cold spray" may be abbreviated as "CS". The powder for CS of the present invention has excellent film-forming and supplying properties by the CS method, and can obtain a cold spray film (CS film) containing a specific rare earth compound with a hardness that has been difficult to obtain in the past.

[0016] (1) Compounds of rare earth elements The powder for CS of the present invention contains at least one rare earth element selected from Y, Yb, and Gd (hereinafter, "Ln 1 One of its features is that it contains compounds of the film-forming elements listed below.

[0017] In the present invention, Ln 1 The compound Ln 1 oxide of Ln 1 fluoride, or Ln 1 It is preferable that the CS powder is an oxyfluoride of Ln because it provides excellent corrosion resistance when used for coating semiconductor manufacturing equipment. In particular, it is preferable that the oxyfluoride of Ln1 fluoride, or Ln 1 It is preferable that the oxyfluoride is an oxyfluoride of the formula: Ln 1 The oxides of Ln include sesquioxides (Ln 1 2O3), as well as Ln 1 It includes complex oxides of Ln and Al. 1 The fluoride of Ln 1 It is preferably represented by F3.

[0018] Ln 1 The oxyfluorides of certain rare earth elements such as Y (Ln 1 ), oxygen (O), and fluorine (F) (hereinafter referred to as "Ln 1 -OF".) Ln 1 -OF is rare earth elements (Ln 1 ), oxygen (O), and fluorine (F) in the molar ratio Ln 1 :O:F=1:1:1 (Ln 1 OF), and other forms of rare earth oxyfluorides (Ln 1 5O4F7, Ln 1 7O6F9, Ln 1 From the viewpoint of the availability of oxyfluorides and the effect of the present invention, which is high in film forming property and supplyability, Ln 1 -OF is Ln 1 O x F y It is preferable that the formula is expressed as (0.3≦x≦1.7, 0.1≦y≦1.9). From the above viewpoint, it is more preferable that the formula is 0.35≦x≦1.65, and even more preferable that the formula is 0.4≦x≦1.6. It is more preferable that the formula is 0.2≦y≦1.8, and even more preferable that the formula is 0.5≦y≦1.5. It is also preferable that the formula is 2.3≦2x+y≦5.3, and especially 2.35≦2x+y≦5.1, and it is especially preferable that the formula is 2x+y=3. In particular, it is preferable to use the formula where x<1 and y>1 in terms of chemical stability against both fluorine-based plasma and oxygen-based plasma.

[0019] Ln 1 As the material, Y is most preferable because it is suitable as a corrosion-resistant member of semiconductor manufacturing equipment and because it is excellent in the effect of improving the supplyability according to the present invention and the resulting improvement in the hardness of the film.

[0020] (2) Pore volume distribution The powder for CS of the present invention is characterized in that, in the distribution of pore volume versus pore diameter measured by mercury intrusion porosimetry, at least one peak is observed in the pore diameter range of 0.3 μm to 2.0 μm, and the volume of pores with a pore diameter of less than 0.3 μm is 0.1 ml / g to 0.5 ml / g. Note that the pore diameter in this specification refers to the pore diameter. The present inventors have intensively studied a configuration for improving the supplyability of a powder of a specific rare earth compound such as yttrium while maintaining the film-forming property and without clogging the nozzle (supply pipe) during film formation. As a result, it has been found that a powder having a peak of pore diameters of 0.3 μm to 2.0 μm in the pore volume distribution and a pore volume of pores with diameters of less than 0.3 μm falling within the above range improves the supplyability during film formation by the CS method, and by subjecting the powder to the CS method, it is possible to improve the supplyability of the powder compared to the conventional Ln 1 It was found that the compound could produce a film with superior hardness compared to the CS film.

[0021] In the pore volume distribution, a powder having a peak in the pore diameter range of 0.3 μm to 2.0 μm and having a pore volume of less than 0.3 μm is the above-mentioned predetermined amount usually contains two or more types of particles (powders) with different particle sizes. Specifically, in the pore volume distribution, the peak in the pore diameter range of 0.3 μm to 2.0 μm is derived from the interparticle voids of primary particles of a powder with a relatively large particle size (primary particle size). Also, the pore volume within the above range in the pore diameter range of less than 0.3 μm is derived from the interparticle voids of primary particles of a powder with a relatively small particle size (primary particle size).

[0022] In the pore volume distribution of the powder for CS, the powder that gives a pore volume in the above range of pore diameters less than 0.3 μm has a relatively small primary particle size as described above, and as a result has a specific surface area of ​​a certain level or more. A high specific surface area is important for the film-forming properties of the powder for CS. On the other hand, a powder having such a specific surface area may cause clogging in an acceleration nozzle for colliding the powder with a substrate at high speed during film formation by the CS method, thereby reducing the supplying ability. In this regard, the powder for CS of the present invention contains a powder with a relatively large particle size (primary particle size) that gives a peak in the pore diameter range of 0.3 μm to 2.0 μm. The presence of this relatively large particle size (primary particle size) is a factor that affects the specific rare earth Ln 1 This improves nozzle clogging during powder supply in the CS method using a powder-based coating. This is believed to increase the hardness of the resulting CS film because the impact speed of the coating powder against the substrate during coating by the CS method remains high and stable.

[0023] The powder for CS of the present invention has a pore volume of Ln 1 It is preferable that the particles that provide the pore volume at a pore diameter of less than 0.3 μm contain Ln 1 The inclusion of the powder can be confirmed, for example, by observing a powder spread on a carbon tape with a scanning electron microscope (SEM) at a magnification of 1500 times, and performing a point analysis of the observed powder by energy dispersive X-ray analysis (EDX). For example, it is preferable to observe two or more types of particles having a large aggregate diameter (secondary particle diameter) and a small aggregate diameter, and to perform a point analysis on the particles having the large aggregate diameter, and it is preferable to confirm that the particles having the large aggregate diameter have a D measured by a laser diffraction / scattering particle size distribution measurement method. 50 More preferably, the particle has an aggregate diameter equivalent to more than 10 μm. An example of a particle that provides a pore volume with a pore diameter of less than 0.3 μm is the first powder described below. On the other hand, a powder that provides at least one peak in the pore volume distribution with a pore diameter of 0.3 μm to 2.0 μm is preferably a ceramic powder. A suitable example of such a powder is the second powder described below.

[0024] In the present invention, the CS powder has a pore size peak in the range of 0.3 μm or more and 2.0 μm or less, and in order to further improve supplyability, it is particularly preferable that the powder has a peak in the range of 0.6 μm or more and 1.8 μm or less, and it is even more preferable that the powder has a peak in the range of 0.8 μm or more and 1.4 μm or less.

[0025] In the present invention, it is preferable from the viewpoint of flowability that the falling point (end point) of the pore volume peak in the pore diameter range of 0.3 μm to 2.0 μm is located on the larger diameter side of the pore diameter of 0.3 μm. Here, the falling point of the peak is the pore diameter equal to or higher than the intersection point of the descending slope of the peak from the larger diameter side to the smaller diameter side and the baseline, and is the smallest pore diameter at which the log differential pore volume decreases to 70% or less of the log differential pore volume at the point 20 nm larger from that pore diameter. Regarding the pore volume distribution of the powder for CS, the ratio IB / IA of the pore volume IB of pores with diameters less than 0.3 μm to the pore volume IA in the pore diameter range of 0.3 μm or more and 2.0 μm or less is preferably 5 or less in terms of eliminating clogging during film formation and improving film hardness, more preferably 3 or less, particularly preferably 2 or less, and even more preferably 1.8 or less. The lower limit of IB / IA is preferably 0.1 or more in terms of suppressing peeling of the film from the substrate, and even more preferably 0.3 or more.

[0026] The powder for CS of the present invention has the advantage that the film hardness is excellent when the pore volume IB of pores with diameters of less than 0.3 μm is 0.1 ml / g or more, and has the advantage that a thick film can be easily obtained when the pore volume IB is 0.5 ml / g or less. From this viewpoint, the pore volume IB of pores with diameters of less than 0.3 μm is more preferably 0.12 ml / g or more and 0.4 ml / g or less, and even more preferably 0.14 ml / g or more and 0.3 ml / g or less.

[0027] In terms of eliminating clogging during film formation and of film hardness and film formability, the pore volume IA of the pores having diameters of 0.3 μm or more and 2.0 μm or less is preferably 0.05 ml / g or more and 0.25 ml / g or less, and more preferably 0.12 ml / g or more and 0.2 ml / g or less.

[0028] The powder for CS in the present invention may have at least one peak in the pore volume distribution at a pore diameter of less than 0.3 μm. Alternatively, it may have a broad protuberance at a pore diameter of less than 0.3 μm. When the powder for CS in the present invention has at least one peak in the pore volume distribution at a pore diameter of less than 0.3 μm, the peak position may be in the range of 5 nm or more and less than 300 nm, and more preferably in the range of 10 nm or more and 200 nm or less.

[0029] The CS powder having the above pore volume distribution can be obtained by a suitable production method described later.

[0030] (3) BET specific surface area In order to obtain film-forming property, supply property and high film hardness based thereon, it is preferable that the BET specific surface area of ​​the CS powder is within a specific range. 2 / g or more 30m 2 / g, and preferably less than 5m 2 / g or more 25m 2 / g or less is more preferable, and 7.5m 2 / g or more 20m 2 It is particularly preferable that the molecular weight is not more than 1 / g.

[0031] The powder for CS having the above BET specific surface area can be obtained by a suitable production method described later.

[0032] (4) Particle size distribution The powder for CS preferably has at least one peak in the volumetric particle size distribution measured by a laser diffraction / scattering particle size distribution measuring method in the range of 1 μm to 10 μm. A powder with a particle size of 1 μm to 10 μm is likely to give a peak in the pore size range of 0.3 μm to 2.0 μm in the pore volume distribution. By adopting such a configuration, the powder for CS can further increase the fluidity. From the viewpoint of further improving the above-mentioned effect, the powder for CS preferably has at least one peak in the volumetric particle size distribution measured by a laser diffraction / scattering particle size distribution measuring method in the range of 1 μm to 10 μm, particularly in the range of 1.5 μm to 8 μm, and more preferably in the range of 2 μm to 5 μm. In this specification, the particle size distribution of the powder for CS by the laser diffraction / scattering particle size distribution measurement method is measured on a sample that has not been subjected to ultrasonic pretreatment.

[0033] The powder for CS preferably has at least one peak in the volumetric particle size distribution measured by a laser diffraction / scattering particle size distribution measuring method in the range of more than 10 μm to 100 μm. In the above particle size distribution, the secondary particles having a particle size peak in the range of more than 10 μm to 100 μm tend to provide a pore volume in the above range for pore diameters of less than 0.3 μm in the above-mentioned pore volume distribution. The secondary particles of such a particle size are preferable because they have fluidity and excellent film-forming properties. From this viewpoint, the powder for CS preferably has at least one peak in the range of more than 10 μm to 100 μm in the volumetric particle size distribution measured by a laser diffraction / scattering particle size distribution measuring method, particularly in the range of 20 μm to 80 μm, and even more preferably in the range of 25 μm to 50 μm. The secondary particles having the above-mentioned secondary particle size may be a granulated powder obtained by a granulation process, or may be an agglomerated powder in which primary particles are aggregated without going through a granulation process. Granulated powders are sometimes called granules.

[0034] (5) First powder and second powder The powder for CS of the present invention is Ln 1 and has a particle size distribution of more than 10 μm and less than 100 μm in terms of volumetric particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method. 50 (particle size at which the cumulative volume from the small diameter side according to a laser diffraction / scattering particle size distribution measurement method is 50%), and 50 It is preferable that the second powder contains a second powder having the following formula: 50 In terms of film-forming and supplying properties, the D of the first powder is preferably 1.5 μm or more and 8 μm or less, and more preferably 2 μm or more and 5 μm or less. 50 From the viewpoint of film-forming and supplying properties, the thickness is preferably from 20 μm to 80 μm, and more preferably from 25 μm to 50 μm. In the present specification, the D of the first powder by the laser diffraction / scattering particle size distribution measurement method 50 shall be determined on samples that have not been subjected to ultrasonic pretreatment. The first powder may be in the form of a granule or an agglomerated powder.

[0035] The first powder is Ln 1 The first powder has a compound of the formula (I) and is a powder for forming a CS film. The first powder has a peak in the particle size distribution of the powder for CS in the range of more than 10 μm to 100 μm. From the viewpoint of both film forming property and supply property, the first powder has a BET specific surface area of ​​10 m. 2 / g or more 50m 2 / g or less, and 2 / g or more 30m 2 It is more preferable that the molecular weight is not more than 1 / g.

[0036] The second powder acts as a supply aid. The second powder provides a peak in the range of 1 μm to 10 μm in the above particle size distribution of the CS powder. The second powder has a BET specific surface area of ​​1 m 2 / g or more 10m 2 / g or less is preferable in terms of excellent supplyability of the powder for CS, and 2 / g or more 5m 2It is more preferable that the molecular weight is not more than 1 / g. In the present specification, the D 50 shall be determined on samples that have not been subjected to ultrasonic pretreatment. The form of the second powder is not particularly limited, but it is preferable that it is not granular in view of improving supplyability.

[0037] The second powder is a ceramic powder, Ln 1 This is preferable in terms of improving nozzle clogging when forming a film from the compound by the CS method and improving film hardness, and is particularly preferable in terms of preventing impurity contamination of silicon wafers by at least one of rare earth compounds, silicon compounds, and aluminum compounds. The phrase "the second powder is composed of at least one of rare earth compounds, silicon compounds, and aluminum compounds" preferably means that the second powder has at least one of rare earth compounds, silicon compounds, and aluminum compounds as a main phase, specifically, when the second powder is subjected to X-ray diffraction measurement under the following conditions, the main peak is derived from a rare earth compound, a silicon compound, or an aluminum compound.

[0038] Rare earth element Ln in the rare earth compound constituting the second powder 2 The rare earth elements Ln constituting the second powder include 16 elements, namely, scandium (Sc), yttrium (Y), lanthanum (La), cerium (Ce), praseodymium (Pr), neodymium (Nd), samarium (Sm), europium (Eu), gadolinium (Gd), terbium (Tb), dysprosium (Dy), holmium (Ho), erbium (Er), thulium (Tm), ytterbium (Yb) and lutetium (Lu). 2 The rare earth elements Ln 2 Oxides of rare earth elements Ln 2 Fluorides of rare earth elements Ln 2 The rare earth elements Ln 2 Oxides of rare earth elements Ln 2 Fluorides of rare earth elements Ln 2The oxyfluorides of the above-mentioned 16 rare earth elements Ln 2 The oxides, fluorides, and oxyfluorides of the above can be used without any particular limitation.

[0039] Rare Earth Elements Ln 2 The oxides of cerium (Ce), praseodymium (Pr), and terbium (Tb) are classified as sesquioxides (Ln 2 2O3, Ln 2 may be the rare earth elements mentioned above). Cerium oxide is usually CeO2 and praseodymium oxide is usually Pr6O 11 and terbium oxide is usually Tb4O7. 2 The oxide may be a composite oxide of two or more rare earth elements, or a composite oxide of a rare earth element and Al or the like.

[0040] Rare Earth Elements Ln 2 The fluoride of Ln 2 It is preferably represented by F3. Also, the rare earth element Ln 2 For the oxyfluorides of the rare earth elements, the rare earth elements have been expanded to the above 16 types, but the specific rare earth elements Ln 1 That is, what was said about Ln 2 The oxyfluorides of rare earth elements (Ln 2 ), oxygen (O), and fluorine (F) (hereinafter referred to as "Ln 2 -OF".) Ln 2 -OF is rare earth elements (Ln 2 ), oxygen (O), and fluorine (F) in the molar ratio Ln 2 :O:F=1:1:1 (Ln 2 OF), and other forms of rare earth oxyfluorides (Ln 2 5O4F7, Ln 2 7O6F9, Ln 2 4O3F6, etc.) may be used. From the viewpoint of achieving the effect of ease of production and high supplyability of oxyfluorides, Ln 2 -OF is Ln 2 O x F yIt is preferable that the formula is expressed as (0.3≦x≦1.7, 0.1≦y≦1.9). From the above viewpoint, it is more preferable that the formula is 0.35≦x≦1.65, and even more preferable that the formula is 0.4≦x≦1.6. It is more preferable that the formula is 0.2≦y≦1.8, and even more preferable that the formula is 0.5≦y≦1.5. It is also preferable that the formula is 2.3≦2x+y≦5.3, and especially 2.35≦2x+y≦5.1, and it is especially preferable that the formula is 2x+y=3. In particular, it is preferable to use the formula where x<1 and y>1 in terms of chemical stability against both fluorine-based plasma and oxygen-based plasma.

[0041] The second powder of rare earth elements Ln 2 The compound is the film-forming element Ln 1 The rare earth element Ln of the second powder may be the same as or different from the compound of the first powder. 2 The compound is the film-forming element Ln 1 It is preferable that the compound is the same as the compound mentioned above, since the film composition can be easily constituted of a single compound. In the present invention, the second powder may constitute the obtained CS film, or may act only as an auxiliary agent for improving the supplyability, without constituting a film.

[0042] The silicon compound may be SiO2.

[0043] Aluminum compounds include Al2O3, AlF3, and AlOF.

[0044] The second powder is Ln 2 Among these compounds, it is preferable to use a compound of at least one rare earth element selected from Y, Y, and Gd in terms of suitability for use in corrosion-resistant coating members for semiconductor devices and in terms of raw material cost, and it is preferable to use a fluoride or oxyfluoride of at least one rare earth element selected from Y, Yb, and Gd, and it is particularly preferable to use a compound of Y in terms of chemical and physical stability against plasma. Also, it is preferable to use Al2O3 as the second powder in terms of improving the hardness of the film.

[0045] From the viewpoint of improving supplyability while maintaining film-forming properties, the amount of the first powder in the CS powder is preferably 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, and particularly preferably 30% by mass or more and 70% by mass or less. The amount of the first powder is also preferably 10% by mass or more and 90% by mass or less, preferably 20% by mass or more and 80% by mass or less, and particularly preferably 30% by mass or more and 70% by mass or less, based on the total amount of the first powder and the second powder.

[0046] From the viewpoint of improving supplyability while maintaining film-forming properties, the amount of the second powder in the CS powder is preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and particularly preferably 30% by mass to 70% by mass. The amount of the second powder is also preferably 10% by mass to 90% by mass, more preferably 20% by mass to 80% by mass, and particularly preferably 30% by mass to 70% by mass, based on the total amount of the first powder and the second powder.

[0047] The amount of powders other than the first powder and the second powder in the powder for CS is preferably 10 mass % or less, more preferably 5 mass % or less, and even more preferably 2 mass % or less.

[0048] Next, a preferred method for producing the powder for CS of the present invention will be described. 50 and mixing the first and second powders having the above compositions. The mixing ratio may be the preferred ratio described above. The first powder can be produced by a conventionally known method, for example, a method similar to the method for producing a rare earth compound powder described in Patent Document 1. The manufacturing method of the second powder is also not particularly limited, but the second powder is preferably Ln 2 A preferred production method for the case where the oxyfluoride or fluoride is the above will be described below.

[0049] The second powder is Ln2 A suitable method for producing the rare earth oxyfluoride or fluoride is to mix a rare earth fluoride and a rare earth oxide, sinter the mixture at 600° C. to 1000° C., and then pulverize the mixture to obtain D 50 is between 1 μm and 10 μm. The firing temperature is more preferably 700° C. or higher and 900° C. or lower. The firing atmosphere may be air.

[0050] (6) Film formation by CS method Next, a film forming method using the CS method will be described. In this film formation method, the CS powder of the present invention is used as a raw material powder, and the raw material powder is heated and accelerated by a heated and pressurized gas, and caused to collide with a substrate to form a film. The deposition apparatus used in deposition by the CS method includes a generator that generates high-temperature, high-pressure gas, a gas acceleration unit that receives the high-temperature, high-pressure gas from the generator and accelerates the gas, and a substrate holding unit that holds the substrate. The raw material powder is injected into the high-temperature, high-pressure gas flow, causing the raw material powder to collide with the substrate.

[0051] The gas temperature in the high-temperature / high-pressure gas generating section is preferably 150°C or higher in order to facilitate adhesion of rare earth compound particles to the substrate, and is preferably 800°C or lower in order to prevent contamination by metal impurities from the acceleration nozzle. From these viewpoints, the gas temperature is more preferably 160°C or higher and 750°C or lower, and particularly preferably 180°C or higher and 700°C or lower.

[0052] The gas pressure in the high-temperature / high-pressure gas generating section is preferably 0.1 MPa or more since the particles are easily attached to the substrate, and is preferably 10 MPa or less since it is easy to prevent the phenomenon in which the particles are difficult to collide with the substrate due to shock waves generated near the substrate surface. From this viewpoint, the gas pressure is more preferably 0.2 MPa or more and 8 MPa or less, and particularly preferably 0.3 MPa or more and 6 MPa or less.

[0053] The gas acceleration section can be an acceleration nozzle, and the shape and structure thereof are not limited. The substrate may be made of metal such as aluminum, aluminum alloy, stainless steel, or carbon steel; ceramics such as graphite, quartz, or alumina; or plastics. The gas may be compressed air, nitrogen, helium, or the like.

[0054] The position of the substrate in the substrate holder may be any position that is exposed to the high-temperature, high-pressure gas flow. The substrate holder and substrate may be fixed, but it is preferable to move the substrate and / or the gun vertically and / or horizontally to expose the entire substrate to the high-temperature, high-pressure gas flow and form a uniform film. The distance between the source powder ejection portion and the substrate (hereinafter also referred to as the "film formation distance") is preferably, for example, 10 mm or more and 50 mm or less in terms of ease of film formation, and more preferably 15 mm or more and 45 mm or less.

[0055] The thickness of the film obtained above is preferably 20 μm or more in terms of obtaining sufficient halogen plasma resistance by coating the components of the semiconductor manufacturing equipment, and is preferably 500 μm or less in terms of economical viewpoints and thickness suitable for use. From this viewpoint, 100 μm or more and 300 μm or less are more preferable. Furthermore, from the viewpoint of durability against physical sputtering action applied to the film during etching, the film obtained by the present invention preferably has a Vickers hardness of 70 or more, more preferably 90 or more, and even more preferably 100 or more. From the viewpoint of ease of production, the upper limit of the Vickers hardness is 500. The method for measuring the Vickers hardness can be the method described in the examples below.

[0056] The film obtained above is Ln 1 Preferably, Ln 1 The coating or powder consists of oxyfluorides or fluorides of Ln 1 The compound consisting of Ln 1 Specifically, when the film or powder is subjected to X-ray diffraction measurement under the following conditions, the main peak is Ln1 It is preferable that the coating obtained above is composed of one or more selected from Y5O4F7, YOF and YF3, because the coating obtained above is preferably composed of one or more selected from Y5O4F7, YOF and YF3, since the CS film composed of these compounds has a relatively high hardness, is chemically stable against any of fluorine-based plasma, chlorine-based plasma and oxygen-based plasma, and is suitable as a corrosion-resistant coating for members such as chambers of semiconductor manufacturing equipment.

[0057] The coating obtained as described above can be used for coating components of various plasma processing devices and chemical plants in addition to components of semiconductor manufacturing equipment. EXAMPLES

[0058] The present invention will be described in more detail below with reference to examples. However, the scope of the present invention is not limited to such examples. Unless otherwise specified, "%" means "mass %." The BET specific surface areas described below were all measured by the method described below. Figures 1 to 9 show the pore volume distributions and particle size distributions of Examples 1 and 2 and Comparative Examples 1 and 2.

[0059] <Example 1> [1st powder] The first powder was prepared according to the following procedure. 1.6 kg of yttrium oxide powder was dissolved in 10 kg of 30% aqueous acetic acid solution heated to 100° C. The resulting solution was cooled, and the precipitated yttrium acetate hydrate was fired at 650° C. in an air atmosphere. Yttrium oxide powder was obtained by this process. The obtained yttrium oxide powder was dispersed in pure water at a concentration of 70 g / L, and 50% hydrofluoric acid was added thereto so that 25 g of hydrogen fluoride was obtained per 100 g of yttrium oxide, and the mixture was stirred at 25° C. for 24 hours to obtain an yttrium oxyfluoride precursor. The obtained precursor was dehydrated and then dried at 120° C. for 24 hours in an air atmosphere. The obtained dried powder was calcined at 400° C. for 5 hours in an air atmosphere, and then crushed in a pin mill to obtain an yttrium oxyfluoride powder. The obtained yttrium oxyfluoride powder was dispersed in pure water at a concentration of 35%, and then granulated using a FOC-16 spray dryer manufactured by Okawara Kakakuki Co., Ltd. to obtain yttrium oxyfluoride (Y5O4F7) granulated powder (granules). The operating conditions of the spray dryer were slurry supply rate: 245 ml / min, atomizer rotation speed: 20,000 min -1 The inlet temperature was 250°C.

[0060] [Second powder] As the second powder, alumina powder DTS-A35-10 / 0 manufactured by Fujimi Incorporated was used.

[0061] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to obtain a mixed powder for CS. In the mixed powder for CS obtained in Example 1, the ratio IB / IA of the pore volume IB to the pore volume IA was 5 or less. In the powder for CS, the falling point (end point) of the pore volume peak in the pore diameter range of 0.3 μm to 2.0 μm was located on the larger diameter side than the pore diameter of 0.3 μm. In addition, in the distribution of the pore volume, a pore volume peak was observed in the pore diameter range of 10 nm to 200 nm.

[0062] <Example 2> [1st powder] The first powder was the same as that used in Example 1. [Second powder] The second powder was prepared according to the following procedure. 1.0 kg of yttrium oxide powder manufactured by Nippon Yttrium Co., Ltd. and 1.1 kg of yttrium fluoride powder were mixed using an Ishikawa-type mixing and crushing machine manufactured by Ishikawa Kogyo Co., Ltd., and sintered at 900°C for 24 hours in an air atmosphere. The sintered product was coarsely crushed using a mass colloider manufactured by Masuko Sangyo Co., Ltd. Pure water was added to the coarsely crushed product to make a 30% slurry, and then it was milled using a ball mill. 50 The resulting pulverized product was dried at 150° C. for 24 hours in an air atmosphere, and then finely crushed using a pin mill to obtain the desired second powder.

[0063] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to prepare a mixed powder for CS.

[0064] <Example 3> [1st powder] The first powder was prepared according to the following procedure. 1.6 kg of yttrium oxide powder was dissolved in 10 kg of 30% aqueous acetic acid solution heated to 100° C. The resulting solution was cooled, and the precipitated yttrium acetate hydrate was fired at 650° C. in an air atmosphere. By this process, yttrium oxide powder was obtained. The obtained yttrium oxide powder was dispersed in pure water at a concentration of 70 g / L, and 50% hydrofluoric acid was added thereto so that 18 g of hydrogen fluoride was added per 100 g of yttrium oxide, and the mixture was stirred at 25° C. for 24 hours to obtain an yttrium oxyfluoride precursor. The obtained precursor was dehydrated and then dried at 120° C. for 24 hours in an air atmosphere. The obtained dried powder was calcined at 400° C. for 5 hours in an air atmosphere, and then crushed in a pin mill to obtain an yttrium oxyfluoride powder. The obtained yttrium oxyfluoride powder was dispersed in pure water at a concentration of 35%, and then granulated using a FOC-16 spray dryer manufactured by Okawara Kakakuki Co., Ltd. to obtain yttrium oxyfluoride (YOF) granulated powder (granules). The operating conditions of the spray dryer were slurry supply rate: 245 ml / min, atomizer rotation speed: 20,000 min -1 The inlet temperature was 250°C.

[0065] [Second powder] The second powder was prepared according to the following procedure. 1.0 kg of yttrium oxide powder manufactured by Nippon Yttrium Co., Ltd. and 0.6 kg of yttrium fluoride powder were mixed using an Ishikawa-type mixing and crushing machine manufactured by Ishikawa Kogyo Co., Ltd., and sintered at 900°C for 24 hours in an air atmosphere. The sintered product was coarsely crushed using a mass colloider manufactured by Masuko Sangyo Co., Ltd. Pure water was added to the coarsely crushed product to make a 30% slurry, and then it was milled using a ball mill. 50The resulting pulverized product was dried at 150° C. for 24 hours in an air atmosphere, and then finely crushed using a pin mill to obtain the desired second powder.

[0066] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to prepare a mixed powder for CS.

[0067] <Example 4> [1st powder] The first powder was prepared according to the following procedure. 1.6 kg of yttrium oxide powder was dissolved in 10 kg of 30% acetic acid aqueous solution heated to 100° C. The resulting solution was cooled, and the precipitated yttrium acetate hydrate was fired in an air atmosphere at 650° C. By this process, yttrium oxide powder was obtained. The obtained yttrium oxide powder was dispersed in pure water at a concentration of 70 g / L, and 50% hydrofluoric acid was added thereto so that 35 g of hydrogen fluoride was added per 100 g of yttrium oxide, and the mixture was stirred at 25° C. for 24 hours to obtain an yttrium oxyfluoride precursor. The obtained precursor was dehydrated and then dried at 120° C. for 24 hours in an air atmosphere. The obtained dried powder was calcined at 400° C. for 5 hours in an air atmosphere, and then crushed with a pin mill to obtain a powder containing yttrium oxyfluoride and yttrium fluoride. The obtained powder was dispersed in pure water at a concentration of 35%, and then granulated using a spray dryer manufactured by Okawara Kakakuki Co., Ltd., FOC-16 type, to obtain yttrium oxyfluoride (Y5O4F7) and YF3 granulated powder (granules). The operating conditions of the spray dryer were slurry supply rate: 245 ml / min, atomizer rotation speed: 20,000 min -1 The inlet temperature was 250°C. The obtained powder was subjected to X-ray diffraction measurement under the following conditions. The main phase was found to be Y5O4F7(YO 0.8 F 1.4 ) and the subphase was YF3.

[0068] [Second powder] The second powder was prepared according to the following procedure. 1.0 kg of yttrium oxide powder manufactured by Nippon Yttrium Co., Ltd. and 2.6 kg of yttrium fluoride powder were mixed using an Ishikawa-type mixing and crushing machine manufactured by Ishikawa Kogyo Co., Ltd., and sintered at 900°C for 24 hours in an air atmosphere. The sintered product was coarsely crushed using a mass colloider manufactured by Masuko Sangyo Co., Ltd. Pure water was added to the coarsely crushed product to make a 30% slurry, and then it was milled using a ball mill. 50 The resulting pulverized material was dried at 150°C for 24 hours in an air atmosphere, and then finely crushed using a pin mill to obtain the desired second powder. The obtained second powder was subjected to X-ray diffraction measurement under the following conditions, and it was found that the main phase was Y5O4F7(YO 0.8 F 1.4 ) and the subphase was YF3.

[0069] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to prepare a mixed powder for CS.

[0070] <Example 5> [1st powder] A precipitate of yttrium fluoride was obtained by reacting 2.2 kg of an aqueous solution of yttrium nitrate having a concentration of 300 g / L in terms of yttrium oxide with 0.5 kg of 50% hydrofluoric acid. The precipitate was dehydrated and washed, and then dried at 150° C. for 24 hours in an air atmosphere. The dried powder was crushed in a grinder to obtain yttrium fluoride powder. The obtained powder was dispersed in pure water at a concentration of 35%, and then granulated using a spray dryer manufactured by Okawara Kakakuki Co., Ltd., FOC-16, to obtain yttrium fluoride powder (granules). The operating conditions of the spray dryer were slurry supply rate: 245 ml / min, atomizer rotation speed: 20,000 min -1 The inlet temperature was 250°C. The obtained powder was subjected to X-ray diffraction measurement under the following conditions, and it was found that the main phase was YF3.

[0071] [Second powder] The second powder was prepared according to the following procedure. The [first powder] of this example was sintered at 900°C for 24 hours in an air atmosphere to obtain a sintered product, which was then crushed using a mass colloider manufactured by Masuko Sangyo Co., Ltd. Pure water was added to the resulting crushed product to make a 30% slurry, which was then crushed using a ball mill. 50 The resulting pulverized product was dried at 150° C. for 24 hours in an air atmosphere, and then finely crushed using a pin mill to obtain the desired second powder.

[0072] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to prepare a mixed powder for CS.

[0073] <Example 6> [1st powder] The first powder was prepared according to the following procedure. 1.6 kg of yttrium oxide powder was dissolved in 10 kg of 30% acetic acid aqueous solution heated to 100° C. The resulting solution was cooled, and the precipitated yttrium acetate hydrate was fired in an air atmosphere at 650° C. By this process, yttrium oxide powder was obtained. The obtained yttrium oxide powder was dispersed in pure water at a concentration of 70 g / L, and 50% hydrofluoric acid was added thereto so that 25 g of hydrogen fluoride was added per 100 g of yttrium oxide, and the mixture was stirred at 25° C. for 24 hours to obtain an yttrium oxyfluoride precursor. The obtained precursor was dehydrated and then dried in an air atmosphere at 120° C. for 24 hours. The obtained dried powder was calcined in an air atmosphere at 900° C. for 5 hours, and then crushed in a pin mill to obtain an yttrium oxyfluoride powder. The obtained dry powder was dispersed in pure water at a concentration of 35%, and then granulated using a spray dryer manufactured by Okawara Kakakuki Co., Ltd., FOC-16 type, to obtain yttrium oxyfluoride (Y5O4F7) granulated powder (granules). The operating conditions of the spray dryer were slurry supply rate: 245 ml / min, atomizer rotation speed: 20,000 min -1 The inlet temperature was 250°C.

[0074] [Second powder] The second powder was prepared according to the following procedure. 1.0 kg of yttrium oxide powder manufactured by Nippon Yttrium Co., Ltd. and 1.1 kg of yttrium fluoride powder were mixed using an Ishikawa-type mixing and crushing machine manufactured by Ishikawa Kogyo Co., Ltd., and sintered at 900°C for 24 hours in an air atmosphere. The sintered product was coarsely crushed using a mass colloider manufactured by Masuko Sangyo Co., Ltd. Pure water was added to the coarsely crushed product to make a 30% slurry, and then it was milled using a ball mill. 50 The resulting pulverized product was dried at 150° C. for 24 hours in an air atmosphere, and then finely crushed using a pin mill to obtain the desired second powder.

[0075] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to prepare a mixed powder for CS.

[0076] <Comparative Example 1> [1st powder] The first powder was the same as that used in Example 1. In this example, the second powder was not used, and 500 g of the first powder was used as the powder for CS.

[0078] <Comparative Example 2> [1st powder] The first powder was that described in Example 1.

[0079] [Second powder] As the second powder, alumina powder DTS-A150-45-45 / 10 manufactured by Fujimi Incorporated was used.

[0080] 500 g of the first powder and 500 g of the second powder obtained above were shaken in a vinyl bag for 3 minutes to prepare a mixed powder for CS.

[0081] The specific surface area and particle size of the first powder, second powder, and CS powder obtained in the examples and comparative examples were measured by the following method. The pore volume of the CS powder was also measured by the following method. The compositions of the first powder and second powder were also confirmed by the following method. The measurement results of the first powder and second powder are shown in Table 1, and the results of the CS powder are shown in Table 2. <Measurement Method of BET Specific Surface Area> The measurement was carried out by the BET one-point method using the fully automatic specific surface area meter Macsorb model-1201 manufactured by Mounttech Co., Ltd. The gas used was a nitrogen-helium mixed gas (30 vol% nitrogen).

[0082] <Conditions for X-ray Diffraction Measurement> ·Apparatus: UltimaIV (manufactured by Rigaku Corporation) ·X-ray source: CuKα ray ·Tube voltage: 40 kV ·Tube current: 40 mA ·Scan speed: 2 degrees / min ·Step: 0.02 degrees ·Scan range: 2θ = 10 degrees to 90 degrees For the powder to be measured, 50 g was collected, placed in an agate mortar, and ethanol in an amount sufficient to completely immerse the powder was dropped, followed by manual pulverization in the agate mortar for 10 minutes. After drying, the fraction passing through a sieve with an opening of 250 μm or less was subjected to X-ray diffraction measurement.

[0083] <Pore Volume by Mercury Intrusion Method> AutoPore IV manufactured by Micromeritics was used. The pore diameter range of 0.001 μm or more and 100 μm or less was measured. The cumulative volume in the range where the pore diameter is less than 0.3 μm was defined as the pore volume IB, and the cumulative volume in the range where the pore diameter is 0.3 μm or more and 2 μm or less was defined as the pore volume IA.

[0084] <D 50 And Measurement Method of Particle Size Distribution> D 50 For D and the particle size distribution, the powder was introduced into the chamber of the sample circulator of Microtrac 3300EXII manufactured by Nikkiso Co., Ltd. containing a 0.2 mass% aqueous solution of sodium hexametaphosphate until the apparatus determined that the concentration was appropriate, and then measured. Since the powder was introduced into the chamber of the sample circulator of Microtrac 3300EXII, no dispersion treatment was performed using an external ultrasonic dispersing device, and the ultrasonic dispersion attached to the inside of Microtrac 3300EXII was not performed either.

[0085] The CS powders obtained in the Examples and Comparative Examples were subjected to the following evaluations. The results are shown in Table 3. <Film formation evaluation> The film formation evaluation was carried out according to the following procedure. The deposition device used was a high-pressure cold spray device, CGT-KINETICS4000, and the substrate was 25 mm x 25 mm x 5 mm aluminum A5052 that had been roughened using steel grit GH10 (manufactured by Shinto Kogyo Co., Ltd.). Nitrogen was used as the working gas. The gas pressure was 3.0 MPa, the gas temperature was 500°C, and the deposition distance was 25 mm. The gun scanning speed was 10 mm / s. Powder was fed to the nozzle using the device shown in Figure 1, according to the following procedure. First, 0.5 kg of powder was placed in powder feeder 11, which was then vibrated to feed it into tube 12. The powder fed to tube 12 was carried to nozzle 14 by being carried by gas fed from gas pipe 13, and then ejected from nozzle 14 toward substrate 15. Regarding nozzle clogging during application, the powder supplyability (supply stability) when a single layer was formed on the surface of the above-mentioned aluminum substrate was observed and classified according to the following criteria. ◯: No clogging occurred during film formation. ×: Clogging occurred temporarily during film formation, or clogging occurred and film formation could not be continued.

[0086] Regarding the film formability, the cross section of the film was polished with diamond slurry, and then the cross section of the film and the substrate-film interface were observed using a scanning electron microscope, and classified according to the following criteria. ◯: A thick film having a thickness of 100 μm or more was obtained without cracks or peeling from the substrate. ×: A thick film having a thickness of 100 μm or more was obtained, but cracks were observed in the film or peeling from the substrate, or the film was not deposited sufficiently to form a thick film having a thickness of 100 μm or more.

[0087] The hardness of the film was measured at 10 points under the following conditions and evaluated as the average value. Equipment: Shimadzu HMV-1 Pressure: HV0.1 ·Holding time: 10 seconds

[0088] 50 g of the membrane was taken, placed in an agate mortar, and an amount of ethanol was dropped onto it so that the membrane was completely immersed. The membrane was then crushed by hand with an agate pestle for 10 minutes, dried, and the membrane that had passed through a sieve with an opening of 250 μm or less was subjected to X-ray diffraction measurement under the above conditions.

[0089] [Table 1]

[0090] [Table 2]

[0091] [Table 3] [Explanation of symbols]

[0092] 11 Powder Feeder 12 Tubes 13 Gas piping 14 Nozzles 15 Base material

Claims

1. A powder for cold spray containing a compound of at least one film-forming element selected from Y, Yb, and Gd, A powder for cold spray, in which at least one peak is observed in a pore size range of 0.3 μm or more and 2.0 μm or less in a distribution of pore volume versus pore size measured by mercury intrusion porosimetry, and the pore volume of pores with a pore size of less than 0.3 μm is 0.1 ml / g or more and 0.5 ml / g or less.

2. BET specific surface area is 3m 2 / g or more 30m 2 2. The powder for cold spray according to claim 1, wherein the molecular weight is less than 1 / g.

3. The powder for cold spray according to claim 1 or 2, wherein at least one peak is observed in the range of 1 μm or more and 10 μm or less in a volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method.

4. The powder for cold spray according to claim 3, further comprising at least one peak observed in a range of more than 10 μm and not more than 100 μm in a volume-based particle size distribution measured by a laser diffraction / scattering particle size distribution measurement method.

5. The particle size (D) of the film-forming element is 50% of the total volume from the small diameter side measured by a laser diffraction / scattering particle size distribution measurement method. 50 ) is more than 10 μm and 100 μm or less, and at least one of a rare earth compound, a silicon compound, and an aluminum compound, and D measured by a laser diffraction / scattering particle size distribution measurement method is 50 The powder for cold spray according to any one of claims 1 to 4, further comprising a second powder having a particle size of 1 µm or more and 10 µm or less.

6. The powder for cold spray according to any one of claims 1 to 5, wherein the compound of at least one element selected from Y, Yb, and Gd is a fluoride or oxyfluoride.

7. The powder for cold spray according to any one of claims 1 to 6, comprising a compound of Y.

8. The powder for cold spray according to claim 5 , wherein the proportion of the second powder is 10% by mass or more and 90% by mass or less.

9. A method for producing a film, comprising a step of performing a cold spray method using the powder according to any one of claims 1 to 8.

10. Y 5 O 4 F 7 , YOF and YF 3 The method for producing a film according to claim 9, which produces a cold spray film consisting of one or more selected from the following and having a Vickers hardness of 70 or more and 500 or less.

Citation Information

Patent Citations

  • Method for producing coating film with the use of aerosol, particulate mixture therefor, coating film and composite material

    JP2005314801A

  • Powder for thermal spraying

    JP2006200005A

  • Powder for flame spray and flame spray material

    JP2016138309A

  • Material for spray coating, sprayed coating, and member with sprayed coating

    JP2018076546A

  • Material for cold spraying

    WO2020090528A1