Rare earth magnet and its manufacturing method

The method for manufacturing rare earth magnets by preserving an unprocessed surface and applying a rare earth rich layer only to the processed surface addresses surface damage and cost issues, enhancing magnetic properties and reducing costs.

JP7585783B2Active Publication Date: 2024-11-19TOYOTA JIDOSHA KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020218316
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-12-28
Publication Date
2024-11-19
Estimated Expiration
2040-12-28

AI Technical Summary

Technical Problem

The manufacturing process of rare earth magnets results in surface damage and reduced magnetic properties due to removal processing, leading to potential demagnetization and increased costs from diffusing rare earth elements over the entire surface.

Method used

A manufacturing method that preserves an unprocessed surface area on the magnet body and applies a rare earth rich layer only to the processed surface, using a diffusion process to restore magnetic properties while minimizing the use of expensive rare earth elements.

Benefits of technology

The method effectively suppresses deterioration of magnetic properties and reduces manufacturing costs by maintaining the integrity of the unprocessed surface and selectively applying a rare earth rich layer, ensuring sufficient torque and magnetic performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585783000001
    Figure 0007585783000001
  • Figure 0007585783000002
    Figure 0007585783000002
  • Figure 0007585783000003
    Figure 0007585783000003
Patent Text Reader

Abstract

To provide a rare earth magnet capable of suppressing the degrading of magnetic properties, and a manufacturing method.SOLUTION: A disclosed rare earth magnet includes a magnet body including the prime phase and containing rare earth element R1, transition metal element T, and boron B. A region near the corners of the magnet body of the constituent surface that constitutes the surface of the magnet body is a machined surface that has been removed, and an area in the center of the constituent surface rather than the area near the corners is not removed, i.e. a non-processed surface.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rare earth magnet and a manufacturing method thereof, and more particularly to a rare earth magnet including a magnet body containing rare earth elements, transition metal elements, and boron, and a manufacturing method thereof. [Background technology]

[0002] Rare earth magnets, for example Nd-Fe-B rare earth magnets, which have a magnet body including a main phase containing rare earth elements, transition metal elements, and boron, and a subphase that surrounds the main phase and contains more rare earth elements than the main phase, are known as high-performance magnets with excellent magnetic properties, and are used in motors such as internal magnet motors (IPM motors) installed in electric vehicles such as electric vehicles (EVs) and hybrid vehicles (HVs). In this type of rare earth magnet, the main phase exerts strong magnetism, and the subphase magnetically separates the main phases, generating coercive force, thereby obtaining high magnetic properties.

[0003] When this type of rare earth magnet is used in an actual motor, a raw material powder containing rare earth elements, transition metal elements, and boron is compressed into a shape for producing a rare earth magnet body, and the resulting compressed powder compact is sintered to obtain a sintered body, which is then shaped into the shape and dimensions to be used in the final product by removal processing such as cutting or shearing. As a result, the rare earth magnet body has subphases removed from the processed surface, or damage such as cracks or stress due to processing distortion occurs. This reduces the coercive force of the surface, causing demagnetization even with a small reverse magnetic field, and may cause sequential demagnetization, in which the magnet is demagnetized even more as the reverse magnetic field increases. This causes the magnetic properties of the surface to be lower than those of the interior, which may cause the magnetic properties of the rare earth magnet to deteriorate, and there is a high possibility that the magnetic properties of the rare earth magnet will deteriorate due to demagnetization, especially in motors for electric vehicles.

[0004] To address these problems, a technique has been applied in which a rare earth element-containing material is present on the surface of a rare earth magnet body, which is the processed surface of the magnet body, and heat treatment is performed to diffuse the rare earth element into the magnet body, thereby modifying the surface of the magnet body and recovering the magnetic properties of the rare earth magnet. For example, Patent Document 1 describes a rare earth magnet formed by machining a magnet block material, in which rare earth metal is diffused and infiltrated from the magnet surface into the magnet to a depth greater than the radius of the crystal grains exposed at the outermost surface of the magnet, thereby modifying the damaged portion caused by machining and obtaining the desired magnetic properties. Patent Document 2 describes a rare earth sintered magnet in which the magnet body is formed by sintering a compact made of raw alloy fine powder containing a rare earth element, a transition metal element, and boron, and the magnet body is covered with a chemical vapor deposition film mainly made of a rare earth element, and the surface is restored. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-304038 A [Patent Document 2] JP 2005-285859 A Summary of the Invention [Problem to be solved by the invention]

[0006] In the conventional manufacturing method of this type of rare earth magnet, after obtaining a sintered body by sintering the powder compact as described above, when forming the sintered body into a shape and size to be used in a product by removing processing to produce a magnet body, the entire surface of the sintered body is subjected to removing processing. As a result, the entire constituent surface of the magnet body becomes a processed surface. For this reason, there is a risk that subphases will be removed or damage or stress will occur on the entire surface portion of the constituent surface of the rare earth magnet body, and the magnetic properties of the entire surface portion of the constituent surface will be lower than those of the interior, resulting in significant deterioration of the magnetic properties of the rare earth magnet.

[0007] On the other hand, if rare earth elements are diffused over the entire surface of the magnet body in order to prevent such significant deterioration of the magnetic properties, the amount of expensive rare earth elements used will increase, which may lead to increased manufacturing costs.

[0008] The present invention has been made in view of the above-mentioned circumstances, and an object of the present invention is to provide a rare earth magnet capable of suppressing deterioration of the magnetic properties, and a method for manufacturing the same. [Means for solving the problem]

[0009] In order to solve the above problems, the rare earth magnet of the present invention comprises a magnet body including a main phase, which contains a rare earth element R1, a transition metal element T, and boron B, and is characterized in that the regions near the corners of the magnet body of a component surface constituting the surface of the magnet body are machined surfaces which have been removed, and a more central region of the component surface than the regions near the corners is an unmachined surface which has not been removed.

[0010] The rare earth magnet of the present invention can suppress deterioration of the magnetic properties.

[0011] The rare earth magnet may further comprise a rare earth rich layer provided on the machined surface of the magnet body.

[0012] In addition, in order to solve the above-mentioned problems, the manufacturing method of the rare earth magnet of the present invention is a method for manufacturing the above-mentioned rare earth magnet, and is characterized by comprising a molding step of obtaining a green body by compression molding a raw material powder containing a rare earth element R1, a transition metal element T, and boron B into a shape for producing the magnet body of the rare earth magnet, a sintering step of obtaining a sintered body by sintering the green body, and a processing step of producing the magnet body by removing corners of the sintered body and excess portions in their vicinity.

[0013] According to the method for producing a rare earth magnet of the present invention, deterioration of the magnetic properties of the rare earth magnet can be suppressed.

[0014] The method for producing a rare earth magnet may further include a heat treatment step of subjecting the processed surface of the magnet body to a heat treatment in the presence of a diffusion material containing rare earth element R2.

[0015] Furthermore, in order to solve the above-mentioned problems, the manufacturing method of the rare earth magnet of the present invention is characterized by comprising a recovery process of recovering the above-mentioned rare earth magnet from the motor, and a heat treatment process of performing a heat treatment on the processed surface of the magnet body of the rare earth magnet in the presence of a diffusion material containing rare earth element R2.

[0016] According to the method for producing a rare earth magnet of the present invention, it is possible to recover a rare earth magnet whose magnetic properties have been deteriorated, by restoring the magnetic properties of the magnet. Effect of the Invention

[0017] According to the present invention, the deterioration of the magnetic properties of the rare earth magnet can be suppressed. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1(a) is a schematic perspective view showing a rare earth magnet according to a first embodiment, and (b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in (a). [Diagram 2] FIG. 1(a) is a schematic perspective view showing a rare earth magnet according to the conventional technology, and FIG. 1(b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in (a). [Diagram 3] FIG. 1(a) is a schematic perspective view showing a rare earth magnet according to a second embodiment, and (b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in (a). [Figure 4] FIG. 1(a) is a schematic perspective view showing a rare earth magnet according to the conventional technology, and FIG. 1(b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in (a). [Diagram 5] FIG. 6 is a diagram showing an outline of the flow of a method for producing a rare earth magnet according to a second embodiment. [Figure 6]10(a) and 10(b) are schematic cross-sectional views illustrating the main steps of a method for producing a rare earth magnet according to a second embodiment. [Figure 7] 1(a) to 1(c) are schematic cross-sectional views illustrating the main steps of a method for producing a rare earth magnet according to a second embodiment. [Figure 8] 10(a) to 10(d) are schematic cross-sectional views illustrating the main steps of a method for producing a rare earth magnet according to a third embodiment. [Figure 9] 6 shows an SEM image of a cross section of the boundary between the magnet body and the vapor-deposited film after treatment in the rare earth magnet of Reference Example 2, and an EPMA image of the Nd content. FIG. [Figure 10] FIG. 1( a ) is a schematic cross-sectional view showing a BH curve tracer conforming to JIS C 2501, which is a measuring device used to measure the JH curve, and FIG. 1( b ) is a graph showing the procedure for applying a magnetic field when measuring the JH curve. [Figure 11] 1 is a graph showing JH curves measured for the rare earth magnets of Reference Examples 1 and 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, embodiments of the rare earth magnet and the method for producing the same of the present invention will be described. First, the outline of the rare earth magnet according to the embodiment will be described by taking the rare earth magnet according to the first embodiment as an example. Fig. 1(a) is a schematic perspective view showing the rare earth magnet according to the first embodiment, and Fig. 1(b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in Fig. 1(a). Meanwhile, Fig. 2(a) is a schematic perspective view showing a rare earth magnet according to the conventional technology, and Fig. 2(b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in Fig. 2(a).

[0020] As shown in Figures 1(a) and 1(b), the rare earth magnet 1 according to the first embodiment includes a rare earth element R1, a transition metal element T, and boron B, and is provided with a rectangular magnet body 10 including main phase grains (main phase) 10a and subphase 10b surrounding the main phase grains 10a. The main phase grains 10a are made of RFe 14The subphase 10b is a phase having a type B crystal structure, and the subphase 10b is a phase containing more rare earth element R1 than the main phase particles 10a. Regions 12A near corners 14 of the magnet body 10 of all constituent surfaces 12 constituting the surface 10s of the magnet body 10 are machined surfaces (polished surfaces) 12a that have been polished (removed), and regions 12B more central than the regions 12A near the corners 14 of all constituent surfaces 12 are unmachined surfaces 12b that have not been polished. Although not shown, the rare earth magnet 1 further includes a Ni plating or paint film formed by surface treatment on the surface 10s of the magnet body 10.

[0021] On the other hand, as shown in FIG. 2(a) and FIG. 2(b), the rare earth magnet 100 according to the conventional technology includes a rectangular magnet body 10 containing a rare earth element R1, a transition metal element T, and boron B, as in the first embodiment, and including main phase particles (main phase) 10a and subphases 10b surrounding the main phase particles 10a. However, unlike the first embodiment, the rare earth magnet 100 has the entire surface 10s of the magnet body 10, i.e., all of the constituent faces 12, as a polished processed surface (polished surface) 12a. As a result, the subphases 10b are removed from the entire surface portions of all of the constituent faces 12 of the magnet body 10, and stress due to cracks 16 or processing distortion reaching the inside of the magnet body 10 is generated. As a result, the coercive force of the surface portions of the constituent faces 12 of the magnet body 10 is significantly reduced, and the magnetic properties of the rare earth magnet 100 are significantly deteriorated.

[0022] In contrast, in the rare earth magnet 1 according to the first embodiment, in all constituent surfaces 12 of the magnet body 10, only the regions 12A near the corners 14 are machined surfaces 12a, and the regions 12B closer to the center than the regions 12A near the corners 14 are unmachined surfaces 12b. In the magnet body 10, the subphases 10b are removed from the surface portions of the machined surfaces 12a, and cracks 16 reaching the inside of the magnet body 10 or stress due to machining distortion are generated, but in the surface portions of the unmachined surfaces 12b, the subphases 10b are not removed, and cracks 16 reaching the inside of the magnet body 10 or stress due to machining distortion are not generated. Thus, in the rare earth magnet 1 according to the first embodiment, a decrease in the coercive force of the surface portions of the constituent surfaces 12 of the magnet body 10 is suppressed, and deterioration of the magnetic properties of the rare earth magnet 1 can be suppressed. Specifically, in the rare earth magnet 1, demagnetization occurs even when the reverse magnetic field is small, and is suppressed from becoming large as the reverse magnetic field increases, thereby suppressing a decrease in the residual magnetic flux density. This makes it possible to obtain sufficient torque when the rare earth magnet 1 is used in a motor.

[0023] Next, the rare earth magnet according to the second embodiment will be further illustrated. Fig. 3(a) is a schematic perspective view showing the rare earth magnet according to the second embodiment, and Fig. 3(b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in Fig. 3(a). Meanwhile, Fig. 4(a) is a schematic perspective view showing a rare earth magnet according to the conventional technology, and Fig. 4(b) is a schematic cross-sectional view taken along line AA of the rare earth magnet shown in Fig. 4(a).

[0024] As shown in Figures 3(a) and 3(b), the rare earth magnet 1 according to the second embodiment, in addition to the magnet body 10 according to the first embodiment, further comprises a rare earth rich layer 20 provided on the machined surface 12a of the constituent surface 12 of the magnet body 10 so as to cover the main phase particles 10a. The surface portion of the machined surface 12a of the constituent surface 12 is modified by providing a diffusion layer 40. The rare earth rich layer 20 is not provided on the non-machined surface 12b of the constituent surface 12. Although not shown, the rare earth magnet 1 further comprises a Ni plating or paint film formed by surface treatment on the surface 10s of the magnet body 10 and the surface 20s of the rare earth rich layer 20.

[0025] On the other hand, the rare earth magnet 100 according to the prior art shown in Figures 4(a) and 4(b) includes, in addition to the magnet body 10 according to the prior art shown in Figure 2, a rare earth rich layer 20 provided on the entire machined surface 12a of the constituent surface 12 of the magnet body 10 so as to cover the main phase particles 10a. The surface portion of the entire machined surface 12a of the constituent surface 12 is modified by providing a diffusion layer 40. This makes it possible to suppress deterioration of the magnetic properties of the rare earth magnet 100 by restoring the coercive force of the surface portion of the entire machined surface 12a of the constituent surface 12. However, this increases the amount of expensive rare earth elements used, which may lead to increased manufacturing costs.

[0026] In contrast, in the rare earth magnet 1 according to the second embodiment, the rare earth rich layer 20 and diffusion layer 40 are provided only on the machined surface 12a of the constituent surfaces 12 of the magnet body 10, and are not provided on the non-machined surfaces 12b. This makes it possible to recover the coercive force of the surface portion of the machined surface 12a, which is part of the constituent surfaces 12, while suppressing an increase in manufacturing costs, thereby recovering the magnetic properties of the rare earth magnet 1.

[0027] Therefore, with the rare earth magnet according to the embodiment, it is possible to suppress the deterioration of the magnetic properties as in the first and second embodiments. Furthermore, when a rare earth rich layer is further provided on the processed surface of the magnet body as in the second embodiment, it is possible to recover the magnetic properties while suppressing an increase in manufacturing costs.

[0028] Next, the configuration of the rare earth magnet and the method of manufacturing the same according to the embodiment will be described in detail.

[0029] 1. Magnet body The magnet body is not particularly limited as long as it contains a rare earth element R1, a transition metal element T, and boron B and includes a main phase, but typically includes a main phase and a subphase surrounding the main phase.

[0030] The composition of the magnet body is not particularly limited as long as it contains a rare earth element R1, a transition metal element T, and boron B, and can be arbitrarily selected depending on the purpose, but when the magnet body is an R1-TB magnet body (R1: rare earth element, T: transition metal element, B: boron), from the viewpoint of achieving excellent magnetic properties, a composition in which the rare earth element R1 is from 27.0 mass% to 32.0 mass%, the boron B is from 0.5 mass% to 2.0 weight% and the remainder is substantially the transition metal element T is preferable. This is because having the content of the rare earth element R1 at or above the lower limit of this range can prevent the precipitation of α-Fe, which is soft magnetic, and the like, and the coercivity from decreasing, and having the content of the rare earth element R1 at or below the upper limit of this range can prevent the amount of subphase from increasing, thereby preventing the corrosion resistance from deteriorating, and can also prevent the volume ratio of the main phase from decreasing, thereby preventing the residual magnetic flux density from decreasing. In addition, when the content of boron (B) is equal to or higher than the lower limit of this range, a high coercive force can be obtained, and when the content of boron (B) is equal to or lower than the upper limit of this range, a decrease in residual magnetic flux density can be suppressed.

[0031] Among the components of the magnet body, the rare earth element R1 is not particularly limited as long as it is one or more selected from Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, but it is preferable that the main components are one or two selected from Nd and Pr, because they have a good balance of magnetic properties, are abundant in resources, and are relatively inexpensive. In addition, the transition metal element T is preferably one or more transition elements, for example, Fe or Fe and Co as essential elements.

[0032] The magnet body is not particularly limited, but examples thereof include Nd-Fe-B magnet body and Pr-Fe-B magnet body. The magnet body may be an RTBM magnet body containing an additive element M in addition to a rare earth element R1, a transition metal element T, and boron B. The additive element M may be one or more selected from Al, Ga, Cr, Mn, Mg, Si, Cu, C, Nb, Sn, W, V, Zr, Ti, Hf, and Mo. Among these additive elements, for example, high melting point metals such as Nb, Zr, and W are preferable in that they have the effect of suppressing crystal grain growth. The composition of the magnet body is not limited to the compositions listed in this specification, and may be other compositions applicable to the present invention.

[0033] The main phase of the magnet body is R2Fe 14 This phase has a B-type crystal structure. For example, if the magnet body is an Nd-Fe-B magnet body, the main phase is NdFe 14 B. The subphase of the magnet body is a phase that contains a larger amount of the rare earth element R1 than the main phase, and exists so as to surround the main phase.

[0034] The regions of the constituent surfaces constituting the surface of the magnet body near the corners of the magnet body are processed surfaces that have been removed, and the central region of the constituent surfaces rather than the regions near the corners is an unprocessed surface that has not been removed. Here, the "corner of the magnet body" refers to a portion where at least two of the constituent surfaces constituting the surface of the magnet body intersect.

[0035] The processed surface of the magnet body is not particularly limited as long as it is a surface that has been subjected to removal processing, but typically, the removal processing removes subphases or generates damage or stress, resulting in alteration of the surface portion and deterioration of the magnetic properties of that portion. Surfaces that have been subjected to removal processing are surfaces that are newly exposed when a sintered body before being molded into a magnet body is subjected to removal processing, and examples of such surfaces include polished surfaces, ground surfaces, and cut surfaces. The surface roughness Ra of the processed surface of the magnet body is, for example, in the range of 0.1 μm to 10 μm.

[0036] The non-machined surface of the magnet body is the portion of the surface of the sintered body that is machined to obtain the magnet body that is not removed. The non-machined surface of the magnet body has a surface roughness Ra in the range of 0.5 μm to 50 μm, for example.

[0037] The shape of the magnet body is not particularly limited as long as it is a three-dimensional shape having corners, and can be a general shape of magnet body of a rare earth magnet used in motors mounted on electric vehicles, etc., but examples include polygonal shapes such as a cube or rectangular prism, and as long as it has corners, it may be a shape having curved surfaces as its constituent surfaces.

[0038] The dimensions of the magnet body are not particularly limited and may be the general dimensions of magnet bodies of rare earth magnets used in motors mounted on electric vehicles, but when the shape of the magnet body is a cube or a rectangular parallelepiped, the dimensions are preferably, for example, a width (W) of 3 mm to 30 mm, a length (L) of 5 mm to 80 mm, and a height (H) of 2 mm to 15 mm. If the dimensions of the magnet body are above the lower limit of this range, the effect of shrinkage during sintering of the compact becomes large, making it necessary to remove excess parts at the corners of the sintered body and in their vicinity. On the other hand, if the dimensions of the magnet body are below the upper limit of this range, the effect of modifying the surface part of the processed surface of the magnet body by the rare earth-rich layer becomes large.

[0039] 2. Rare earth rich layer and diffusion layer The rare earth magnet preferably further comprises a rare earth rich layer provided on the machined surface of the magnet body, which recovers the coercive force of the surface portion of the machined surface of the magnet body and restores the magnetic properties of the rare earth magnet.

[0040] The rare earth rich layer is a layer that remains after a diffusion reaction between the diffusion material containing the rare earth element R2 and the surface portion of the processed surface of the magnet body by performing a heat treatment in a state where the diffusion material containing the rare earth element R2 is present on the processed surface of the magnet body, and is a layer that is richer in the rare earth element R2 than the surface portion of the processed surface of the magnet body. In the diffusion reaction between the diffusion material and the surface portion of the processed surface of the magnet body, the rare earth element R2 diffuses from the diffusion material to the surface portion of the processed surface of the magnet body, and the constituent elements diffuse from the surface portion of the processed surface of the magnet body to the diffusion material. The rare earth rich layer is not particularly limited, but examples include a layer in which a film of the diffusion material formed on the processed surface of the magnet body by PVD, CVD, or the like remains after the diffusion reaction, and a layer formed by coating the processed surface of the magnet body with a powdered diffusion material and then diffusing the film.

[0041] The rare earth element R2 is not particularly limited as long as it is one or more selected from Sc, Y, La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, and Lu, but among them, it is preferable to use one or two elements selected from Nd, Pr, Ce, Sm, Dy, and Tb as the main component, and particularly preferable to use one or two elements selected from Dy and Tb as the main component, because it has a large effect of recovering magnetic properties such as coercivity.

[0042] The thickness of the rare earth rich layer is not particularly limited as long as it can restore the magnetic properties of the rare earth magnet, but is preferably within the range of 0.1 μm to 5 μm. By having the thickness of the rare earth rich layer be equal to or greater than the lower limit of this range, the effect of restoring the coercive force of the surface portion of the processed surface of the magnet body can be sufficiently obtained. Also, by having the thickness of the rare earth rich layer be equal to or less than the upper limit of this range, the decrease in residual magnetic flux density due to the presence of the rare earth rich layer can be suppressed, and sufficient torque can be obtained when used in a motor, and the amount of rare earth element used can be reduced, thereby reducing unnecessary costs.

[0043] When a rare earth magnet has a rare earth-rich layer, a diffusion layer is usually present on the surface of the machined surface of the magnet body. The diffusion layer is a layer formed by the diffusion of the rare earth element R2 from the diffusion material to the surface of the machined surface of the magnet body, and is a layer richer in the rare earth element R2 than the interior of the magnet body. The diffusion layer can further restore magnetic properties such as coercivity.

[0044] The thickness of the diffusion layer is not particularly limited as long as it can restore the magnetic properties of the rare earth magnet, but is preferably within the range of 0.1 μm to 5 μm, for example. By having the thickness of the diffusion layer at or above the lower limit of this range, the recovery effect of coercivity and the like can be sufficiently obtained. Also, by having the thickness of the diffusion layer at or below the upper limit of this range, deterioration of the magnetic properties due to the diffusion layer can be avoided.

[0045] 3.Rare earth magnets The uses of rare earth magnets are not particularly limited, but examples of rare earth magnets include those used in motors such as internal magnet motors (IPM motors) mounted on electric vehicles such as electric vehicles (EVs) and hybrid vehicles (HVs), actuators for hard disk drives, motors for mobile phones, etc. Among them, rare earth magnets used in motors mounted on electric vehicles are preferable.

[0046] 4. Manufacturing method of rare earth magnets The manufacturing method of the rare earth magnet according to the embodiment is a method of manufacturing the rare earth magnet according to the embodiment, and is characterized by comprising a molding step of obtaining a green body by compression molding a raw material powder containing a rare earth element R1, a transition metal element T, and boron B into a shape for producing the magnet body of the rare earth magnet, a sintering step of obtaining a sintered body by sintering the green body, and a processing step of producing the magnet body by removing corners and excess portions in the vicinity of the corners of the sintered body.

[0047] Here, an overview of the method for manufacturing a rare earth magnet according to the embodiment will be described by taking as an example the method for manufacturing a rare earth magnet according to the second embodiment shown in Fig. 3. Fig. 5 is a diagram showing a schematic flow of the method for manufacturing a rare earth magnet according to the second embodiment. Figs. 6(a) to 7(c) are schematic cross-sectional views showing the main steps of the method for manufacturing a rare earth magnet according to the second embodiment.

[0048] In the manufacturing method of the rare earth magnet according to the second embodiment, first, as shown in FIG. 5, the rare earth element R1, transition metal element T, boron B, and other additive elements are weighed out according to the composition of the magnet body of the rare earth magnet to be manufactured, and these raw materials are mixed and placed in a crucible (weighing and mixing process).

[0049] Next, as shown in Figure 5, the crucible is placed in a vacuum melting furnace, and high frequency waves are applied to the crucible to melt the raw materials and homogeneously alloy them. The molten metal is then poured into a mold to produce an ingot (alloying process).

[0050] Next, as shown in Fig. 5, the ingot is pulverized in several steps using a jet mill or the like until it is pulverized into raw powder with an average particle size of about several microns (pulverization process). At this time, in order to prevent the raw powder from oxidizing, the powder is protected in a nitrogen or argon atmosphere while being pulverized.

[0051] 5 and 6(a), raw material powder 5 containing rare earth element R1, transition metal element T, and boron B is compression molded into a shape for producing a magnet body of the rare earth magnet according to the second embodiment to obtain a green body 50 (molding process). Specifically, raw material powder 5 is press molded in a die to which a magnetic field is applied. This aligns the crystal orientation of raw material powder 5 in the direction of the external magnetic field, improving the magnetic properties in the orientation direction.

[0052] 5 and 6(b), the green body 50 is sintered to obtain a sintered body 60 (sintering step). Specifically, the green body 50 is sintered in a vacuum sintering furnace to obtain the sintered body 60. During this process, as a result of the shape change accompanying the shrinkage of the green body 50, the sintered body 60 has excess parts 60c at and near the corners that are not needed for the magnet body to be manufactured.

[0053] Next, as shown in FIG. 5, a test is performed to measure magnetic properties such as residual magnetic flux density and coercive force of the sintered body 60, and the sintered body 60 that passes the test is sent to the next step (magnetic property test step).

[0054] 5 and 7(a), the corners of the sintered body 60 and excess parts 60c in their vicinity are polished (removed) to produce the magnet body 10 of a rare earth magnet (machining step). At this time, the surface newly exposed by polishing the sintered body 60 becomes the machined surface (polished surface) 12a of the magnet body 10, and the surface of the magnet body 10 other than the machined surface 12a becomes the unmachined surface 12b. The magnet body 10 contains a rare earth element R1, a transition metal element T, and boron B, and includes main phase particles (main phase) 10a and a subphase 10b that exists so as to surround the main phase particles 10a.

[0055] Next, as shown in Figs. 5 and 7(b), a heat treatment is performed in the presence of a diffusion material 30 containing a rare earth element R2 on the machined surface 12a of the magnet body 10 (heat treatment step). As a result, as shown in Fig. 7(c), the rare earth element R2 is diffused from the diffusion material 30 into the surface portion of the machined surface 12a of the magnet body 10 to generate a diffusion layer 40, thereby modifying the surface portion of the machined surface 12a of the magnet body 10. The diffusion material 30 is then left after the diffusion reaction with the surface portion of the machined surface 12a of the magnet body 10 to form a rare earth rich layer 20. At this time, for example, if the magnet body 10 is a Nd-Fe-B magnet body, the rare earth element R2 is diffused into the main phase particles (NdFe 14 B) By diffusing and reacting with the surface region of 10a, new (Nd,R2)2Fe 14B is generated. Furthermore, the surfaces of the main phase grains 10a are covered with an Nd-rich layer (rare earth-rich layer) 20. As a result, the coercive force of the surface portion of the machined surface 12a of the magnet body 10 is restored, and the magnetic properties of the magnet body 10 are restored. Furthermore, in the process in which the rare earth element R2 diffuses, cracks 16 reaching the inside of the magnet body 10, generated by the polishing process, or stress due to processing distortion, disappear. As a result, the coercive force inside the magnet body 10 is also restored.

[0056] 5, various types of surface treatments are applied to the magnet body 10 provided with the rare earth rich layer 20 depending on the environment in which it will be used (surface treatment process). Specifically, for example, if the magnet body 10 is an Nd-Fe-B based magnet body, it is generally prone to rust, so is Ni plated or painted.

[0057] 5, the magnet body 10 after the surface treatment is inspected (inspection process). Specifically, the dimensions and appearance of the magnet body 10 are inspected. In addition, magnetic properties are measured, corrosion resistance tests are performed, strength measurements are performed, etc. according to the product specifications.

[0058] Next, the magnet body 10 is magnetized (magnetization process) as shown in Fig. 5. Through the above, the rare earth magnet 1 according to the second embodiment shown in Fig. 3 is manufactured. Furthermore, as shown in Fig. 5, the manufactured rare earth magnet is packaged and shipped (packaging and shipping process).

[0059] In the method for producing a rare earth magnet according to the second embodiment, the magnet body 10 of the rare earth magnet 1 is produced by polishing only the corners of the sintered body 60 and the excess parts 60c in their vicinity, so that the subphases 10b are not removed from the surface parts of the non-machined faces 12b of the magnet body 10, and cracks 16 reaching the inside of the magnet body 10 or stress due to machining distortion are not generated. This prevents a decrease in the coercive force of the surface parts of the constituent faces 12 of the magnet body 10, and prevents deterioration of the magnetic properties of the rare earth magnet 1. Furthermore, a diffusion layer 40 can be generated only on the surface part of the machined face 12a of the magnet body 10 to modify that part, and further a rare earth rich layer 20 can be formed on the machined face 12a of the magnet body 10. This prevents an increase in manufacturing costs and restores the magnetic properties of the rare earth magnet 1.

[0060] The manufacturing method for the rare earth magnet according to the first embodiment shown in FIG. 1 described above differs from the manufacturing method for the rare earth magnet according to the second embodiment only in that no heat treatment step is performed, and the steps subsequent to the surface treatment step are performed on a magnet body 10 that does not have a rare earth rich layer 20.

[0061] Therefore, the manufacturing method of the rare earth magnet according to the embodiment can suppress deterioration of the magnetic properties of the rare earth magnet. Also, when the manufacturing method further includes a heat treatment step of performing a heat treatment on the processed surface of the magnet body in the presence of a diffusion material containing rare earth element R2, it is possible to recover the magnetic properties of the rare earth magnet while suppressing an increase in manufacturing costs.

[0062] Next, the method for producing a rare earth magnet according to the embodiment will be described in detail.

[0063] (1) Molding process In the compacting step, raw material powder containing rare earth element R1, transition metal element T, and boron B is compression-molded into a shape for producing the magnet body of the rare earth magnet, thereby obtaining a compact.

[0064] The composition of the raw material powder is similar to the composition of the magnet body described above in "1. Magnet body," and therefore a description thereof will be omitted here.

[0065] The method of compression molding the raw material powder is not particularly limited, but magnetic field molding in which the raw material powder is press molded in a mold to which a magnetic field is applied is preferred. The magnetic field molding method may be a perpendicular magnetic field press in which a magnetic field is applied perpendicular to the pressing direction, or a parallel magnetic field press in which a magnetic field is applied parallel to the pressing direction. The magnetic field molding may be performed, for example, in a magnetic field in the range of 500 kA / m to 2000 kA / m, at a pressure in the range of 100 MPa to 200 MPa.

[0066] The shape and dimensions of the compact compressed from the raw material powder are not particularly limited, so long as they are suitable for producing a magnet body of a rare earth magnet; they will usually correspond to the shape and dimensions of the magnet body, and can be determined taking into account shrinkage that occurs when the compact is sintered.

[0067] (2) Sintering process In the sintering step, the green body is sintered to obtain a sintered body.

[0068] The sintering atmosphere is preferably, for example, a vacuum atmosphere or an inert gas atmosphere such as argon or helium. The sintering temperature and sintering time are not particularly limited and need to be adjusted depending on various conditions such as the composition of the raw material powder, the pulverization method during preparation, and the particle size distribution, but may be, for example, sintered for 5 hours at a temperature in the range of 900° C. to 1150° C. The heating method for sintering is not particularly limited, but examples include resistance heating and high-frequency induction heating.

[0069] In the sintering process, the green body shrinks as it is baked. The volumetric shrinkage rate of the green body varies depending on the raw material powder, the green body molding conditions, the sintering conditions, etc., but generally, the dimensions of the sintered body are about 70% to 80% of the green body, and the volume of the sintered body is about 50% of the green body.

[0070] (3) Processing process In the processing step, the corners of the sintered body and excess parts in their vicinity are removed to produce the magnet body. As a result, the surface newly exposed by the removal processing of the sintered body becomes the processed surface of the magnet body, and the surface of the magnet body other than the processed surface becomes the non-processed surface.

[0071] The method for removing the corners of the sintered body and the excess parts in their vicinity is not particularly limited as long as it is a processing method that removes a part of the sintered body, and examples include polishing, grinding, cutting, etc. The shape and dimensions of the magnet body produced in the processing step are similar to those of the magnet body described above in "1. Magnet body", so description thereof will be omitted here.

[0072] (4) Heat treatment process and aging treatment process The manufacturing method of the rare earth magnet preferably further comprises a heat treatment step of performing a heat treatment on the processed surface of the magnet body in the presence of a diffusion material containing the rare earth element R2. By diffusing the rare earth element R2 from the diffusion material into the surface portion of the processed surface of the magnet body, the surface portion of the processed surface of the magnet body can be modified and the magnetic properties of the rare earth magnet can be restored.

[0073] The method of providing the diffusion material containing the rare earth element R2 on the processed surface of the magnet body is not particularly limited, but includes a method of forming a film of the diffusion material on the processed surface of the magnet body by PVD, CVD, etc., a method of powdering the diffusion material and coating the processed surface of the magnet body, etc. More specifically, the method includes a method of forming a sputtered film or vapor deposition film of the rare earth element R2, or a sputtered film or vapor deposition film of an alloy containing the rare earth element R2, by PVD, CVD, etc., a method of coating the processed surface of the magnet body with a powder of the rare earth element R2, a powder of a compound such as an oxide, fluoride, oxyfluoride, hydride, hydroxide, etc. of the rare earth element R2, a powder of an alloy containing the rare earth element R2, etc., and a method of disposing the magnet body in a powder.

[0074] The rare earth element R2 is the same as the rare earth element R2 described above in "2. Rare earth rich layer and diffusion layer," and therefore a description thereof will be omitted here.

[0075] The atmosphere in which the heat treatment is performed is preferably, for example, a vacuum atmosphere or an inert gas atmosphere. The temperature of the heat treatment is not particularly limited as long as it can restore the magnetic properties of the rare earth magnet, but is preferably in the range of the sintering temperature of the magnet body or lower, and more specifically, for example, is preferably in the range of 500°C to 1000°C. By setting the heat treatment temperature to the upper limit or lower of these ranges, problems such as the structure of the magnet body being altered and high magnetic properties being unable to be obtained can be avoided. In addition, by setting the heat treatment temperature to the lower limit or higher of this range, the surface portion of the processed surface can be sufficiently modified. The time of the heat treatment is not particularly limited as long as it can restore the magnetic properties of the rare earth magnet, but is preferably, for example, in the range of 10 minutes to 1 hour. By setting the heat treatment time to the lower limit or higher of this range, the surface portion of the processed surface can be sufficiently modified. In addition, by setting the heat treatment time to the upper limit or lower of this range, a decrease in productivity can be avoided and the thermal influence on the magnet body can be reduced.

[0076] When the method for manufacturing a rare earth magnet includes a heat treatment step, it is preferable that the method further includes an aging treatment step of subjecting the magnet body to an aging treatment after the heat treatment step, because this optimizes the structure of the magnet body and increases the recovery effect of magnetic properties such as coercivity.

[0077] The atmosphere in which the aging treatment is carried out is preferably, for example, a vacuum atmosphere or an inert gas atmosphere. The temperature of the aging treatment is preferably, for example, in a range lower than the temperature of the heat treatment, specifically, for example, in a range of 400°C to 600°C. This is because the magnetic properties such as the coercive force can be sufficiently restored. The time of the aging treatment is preferably, for example, in a range of 1 minute to 10 hours.

[0078] In addition, in the heat treatment step, the temperature and time of the heat treatment may be optimized so that the heat treatment also serves as the aging treatment, and thus the aging treatment step may be omitted in part or in whole.

[0079] (5)Other The manufacturing method of the rare earth magnet according to the embodiment may comprise a recovery step of recovering from a motor a rare earth magnet comprising the magnet body described above in "1. Magnet body", and a heat treatment step of performing a heat treatment on the machined surface of the magnet body of the rare earth magnet in the presence of a diffusion material containing rare earth element R2. This is because it is possible to regenerate a rare earth magnet with restored magnetic properties from a rare earth magnet whose magnetic properties such as coercivity have deteriorated due to its use in a motor.

[0080] As an example of the method for producing a rare earth magnet according to the embodiments, a method for producing a rare earth magnet according to a third embodiment will be further illustrated. Figures 8(a) to 8(d) are schematic cross-sectional views showing the main steps of the method for producing a rare earth magnet according to the third embodiment.

[0081] In the method for producing a rare earth magnet according to the third embodiment, as shown in FIG. 8(a), a sintered body 60 is produced in the same manner as in the method for producing a rare earth magnet according to the second embodiment shown in FIG. 6 and FIG. 7. Next, as shown in FIG. 8(b), in a processing step, the corners of the sintered body 60 and excess parts 60c in the vicinity thereof are polished, and the sintered body 60 is cut along two surfaces parallel to the top and side surfaces of the sintered body 60, respectively, to produce magnet body 10 in which the sintered body 60 is divided into four. Next, as shown in FIG. 8(c), in a heat treatment step, a heat treatment is performed in a state in which a diffusion material 30 containing a rare earth element R2 is present on the processed surface (polished surface) 12a and the processed surface (cut surface) 12a' of the constituent surface 12 of the magnet body 10. As a result, as shown in FIG. 8(d), a diffusion layer 40 is generated by diffusing the rare earth element R2 from the diffusion material 30 into the surface portions of the processed surfaces 12a, 12a' of the magnet body 10, and the surface portions of these surfaces are modified. The diffusion material 30 is left behind after the diffusion reaction to form the rare earth rich layer 20 .

[0082] In the manufacturing method for a rare earth magnet according to the third embodiment, subphases 10b are not removed from the surface portions of non-machined surfaces 12b excluding machined surfaces 12a, 12a' of constituent surfaces 12 of magnet body 10, and stress due to cracks 16 or machining distortion is not generated. Furthermore, by modifying the surface portions of machined surfaces 12a, 12a' of magnet body 10 and forming rare earth-rich layers 20, the coercive force of these surface portions can be restored.

[0083] The method for producing a rare earth magnet according to the embodiment may further include a weighing and mixing step, an alloying step, a crushing step, a magnetic property testing step, a surface treatment step, an inspection step, a magnetization step, etc., in addition to the molding step, sintering step, processing step, and heat treatment step, as in the flow of Fig. 5. If the method for producing a rare earth magnet includes an aging treatment step and a surface treatment step, the aging treatment step is a step prior to the surface treatment step. EXAMPLES

[0084] The rare earth magnet and the method for producing the same of the present invention will be described more specifically below with reference to the following Reference Examples.

[0085] [Reference example 1] First, a sintered body was prepared before being molded into an Nd-Fe-B magnet body. Next, all surfaces of the sintered body were polished to obtain a rectangular magnet body with a width (W) of 5 mm, length (L) of 20 mm, and height (H) of 3 mm. In this way, a rare earth magnet was produced that had a magnet body with all of its component surfaces being machined surfaces that had been entirely removed.

[0086] [Reference example 2] First, the magnet body obtained in Reference Example 1 was prepared, and the magnet body was placed in an alloy powder containing Nd, so that all of the entire constituent surfaces of the magnet body were placed in the alloy powder containing Nd. This allowed the diffusion material containing the alloy powder containing Nd to be present on all of the constituent surfaces of the magnet body.

[0087] Next, the magnet body, with the diffusion material present on all of its component surfaces, was subjected to a heat treatment in a vacuum atmosphere at 900°C for 30 minutes. Next, the heat-treated magnet body was subjected to an aging treatment in a vacuum atmosphere at 550°C for 60 minutes. This produced a rare earth magnet comprising the magnet body and the layer of the evaporated film after the treatment.

[0088] [SEM observation and EPMA measurement] The cross section of the boundary between the magnet body and the layer after the processing of the vapor-deposited film in the rare earth magnet of Reference Example 2 was observed with an SEM (scanning electron microscope). At the same time, the Nd amount at each position on the cross section was measured with an EPMA (electron probe microanalyzer). Figure 9 shows an SEM image of the cross section of the boundary between the magnet body and the layer after the processing of the vapor-deposited film in the rare earth magnet of Reference Example 2, and an EPMA image of the Nd amount.

[0089] It can be seen from the SEM image and EPMA image of the Nd content in Figure 9 that a Nd-rich layer (rare earth-rich layer) is formed on the machined surface of the magnet body. This suggests that Nd diffuses into the surface portion of the machined surface of the magnet body, generating a diffusion layer, which modifies the surface portion of the machined surface of the magnet body.

[0090] [Evaluation of magnetic properties] The JH curves were measured when a reverse magnetic field was applied and then removed for the rare earth magnets of Reference Examples 1 and 2. Figure 10(a) is a schematic cross-sectional view showing a BH curve tracer conforming to JIS C 2501, which is the measuring device used to measure the JH curves, and Figure 10(b) is a graph showing the procedure for applying a magnetic field when measuring the JH curves.

[0091] In measuring the JH curve, first, a magnetic field H of 5T (magnetic field H ≈ 4000kA / m) was applied to the rare earth magnet using a pulse magnetization method to magnetize the rare earth magnet. Next, using a BH curve tracer shown in Fig. 10(a), the magnetic field H was changed from +1600kA / m to a reverse magnetic field of -1600kA / m, and then the magnetic polarization J [T] was measured in the process of changing the magnetic field H from the reverse magnetic field of -1600kA / m to 0kA / m, as shown in Fig. 10(b). Fig. 11 is a graph showing the JH curves measured for the rare earth magnets of Reference Examples 1 and 2.

[0092] 11, it can be seen that the rare earth magnet of Reference Example 1 is demagnetized even when the reverse magnetic field is small, and is demagnetized more significantly as the reverse magnetic field becomes larger, whereas the rare earth magnet of Reference Example 2 is not demagnetized as much as Reference Example 1 when the reverse magnetic field is small. It can also be seen that the amount of demagnetization of the rare earth magnet of Reference Example 2 is about half that of the rare earth magnet of Reference Example 1. Furthermore, the JH curve for the rare earth magnet of Reference Example 2 confirms that the magnetic polarization J is high, at about 1.12 T, when the magnetic field H is -900 kA / m.

[0093] Although the embodiments of the present invention have been described in detail above, the present invention is not limited to the above-described embodiments, and various design modifications can be made without departing from the spirit of the present invention as described in the claims. [Explanation of symbols]

[0094] 1 Rare earth magnets 10 Magnet body 10a Main phase particles (main phase) 10b Vice-phase 10s surface 12 Composition 12A Area near corners 12a Processed surface (polished surface) 12a' Processed surface (cut surface) 12B Central Area 12b Unmachined surface 14 Corner 16 Crack 20 Rare Earth Rich Layer 40 Diffusion Layer 5 Raw material powder 50 Molded body 60 Sintered body 60c Corners and excess parts in the vicinity 30 Diffusion Materials

Claims

1. The magnet body includes a rare earth element R1, a transition metal element T, and boron B, and includes a main phase; The shape of the magnet body is a rectangular parallelepiped having six flat rectangular constituent surfaces, a corner region of each of at least two flat rectangular constituent surfaces of the six flat rectangular constituent surfaces of the magnet body is a processed surface that has been removed by processing, the corner region is a portion where the at least two flat rectangular constituent surfaces of the magnet body intersect, A rare earth magnet, characterized in that a central region of each of the at least two flat rectangular constituent faces of the magnet body, which is more central than the corner regions, is an unmachined surface that has not been removed.

2. 2. The rare earth magnet according to claim 1, further comprising a rare earth rich layer provided on the machined surface of the magnet body.

3. A method for producing the rare earth magnet according to claim 1 or 2, comprising the steps of: a molding step of obtaining a green body by compression molding a raw material powder containing a rare earth element R1, a transition metal element T, and boron B into a shape for producing the magnet body of the rare earth magnet; a sintering step of obtaining a sintered body by sintering the molded body; a processing step of fabricating the magnet body by removing corners of the sintered body and excess portions in the vicinity thereof; A method for producing a rare earth magnet comprising the steps of:

4. 4. The method for producing a rare earth magnet according to claim 3, further comprising a heat treatment step of subjecting the processed surface of the magnet body to a heat treatment in the presence of a diffusion material containing the rare earth element R2.

5. a recovery step of recovering the rare earth magnet according to claim 1 from the motor; a heat treatment process for performing a heat treatment on the processed surface of the magnet body of the rare earth magnet in the presence of a diffusion material containing a rare earth element R2; A method for producing a rare earth magnet, comprising:

Citation Information

Patent Citations

  • Method of manufacturing r-fe-b sintered magnet having thin thickness

    JP1998064746A

  • Method for manufacturing rare-earth permanent magnet

    JP2003100537A

  • Micro high-performance rare-earth magnet for micro product and its manufacturing method

    JP2004304038A

  • Rare-earth magnet and its manufacturing method

    JP2005285859A

  • Rotor for magnet-embedded motors and magnet-embedded motor

    JP2010119190A