Steel sheet for cans and its manufacturing method

A steel sheet for cans with a tailored composition and manufacturing process achieves high tensile strength and elongation, addressing the strength deficiencies of existing sheets and enabling thinner, more sustainable can production.

JP7585896B2Active Publication Date: 2024-11-19JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021040182
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-03-26
Filing Date
2021-03-12
Publication Date
2024-11-19
Estimated Expiration
2041-03-12

AI Technical Summary

Technical Problem

Existing steel sheets for cans, despite having high upper yield strength and total elongation, often lack sufficient tensile strength and axial buckling strength, particularly when made thinner to reduce environmental impact and cost.

Method used

A steel composition with specific mass percentages of elements like C, Si, Mn, P, S, Al, N, Nb, Mo, B, and Cr, combined with a manufacturing process involving heating, hot rolling, cold rolling, annealing, and temper rolling, to achieve tensile strength of 500 MPa or more and elongation of 10% or more, with a metal structure comprising ferrite and pearlite or granular cementite.

Benefits of technology

The resulting steel sheet exhibits high strength and excellent workability, allowing for thinner can bodies with improved resource efficiency and cost reduction while maintaining structural integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007585896000001
    Figure 0007585896000001
  • Figure 0007585896000002
    Figure 0007585896000002
  • Figure 0007585896000003
    Figure 0007585896000003
Patent Text Reader

Abstract

To provide a steel plate for a can, which has high intensity and excellent workability, and to provide a method for manufacturing the same.SOLUTION: A steel plate for a can comprises, by mass: 0.020% or more and 0.130% or less of C; 0.04% or less of Si; 0.10% or more and 0.60% or less of Mn; 0.020% or less of P; 0.005% or more and 0.020% or less of S; 0.01% or more and 0.10% or less of Al; 0.0050% or more and 0.0180% or less of N; 0.007% or more and 0.030% or less of Nb; and 0.010% or more and 0.050% or less of Mo, with the balance comprising Fe and inevitable impurities, wherein the steel plate has tensile strength of 500 MPa or more and elongation of 10% or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a steel sheet for cans suitable for use as a material for can containers used in particular for food cans, beverage cans, etc., and a method for manufacturing the same. [Background technology]

[0002] There is a demand to reduce the amount of steel used in food and beverage cans in order to reduce environmental impact and costs, and the use of thinner steel sheets is progressing for both two-piece and three-piece cans. When steel sheets are made thinner, the strength of the can body decreases, so it is necessary to use high-strength steel sheets. Conventionally, steel sheets called DR (Double Reduced) materials have been used as high-strength steel sheets for cans. DR materials are steel sheets that are manufactured by cold rolling again (secondary rolling) after annealing. Although DR materials are high-strength, they have low elongation and poor workability, so they have not always been applicable to can body processing, which requires high workability.

[0003] In order to address these issues, there is a need for steel sheets for cans that have high strength and excellent formability. For example, Patent Documents 1 and 2 propose high-strength steel sheets for cans.

[0004] Patent Document 1 describes a steel containing, by mass%, C: 0.020% or more and 0.130% or less, Si: 0.04% or less, Mn: 0.10% or more and 1.2% or less, P: 0.007% or more and 0.100% or less, S: 0.03% or less, Al: 0.0010% or more and 0.10% or less, N: more than 0.0120% and 0.020% or less, and further containing one or more selected from Nb: 0.010% or more and 0.050% or less, Ti: 0.010% or more and 0.050% or less, and B: 0.0010% or more and 0.010% or less. has been proposed, which has a component composition including two or more of the above and the balance consisting of iron and unavoidable impurities, has a ferrite phase structure, the area ratio of the ferrite phase being 50% or more, has an upper yield strength of 480 to 700 MPa and a total elongation of 12% or more after heat treatment at 210°C for 20 minutes, and the ratio of the amount of solute N in a region from the surface to a 1 / 8 depth position in the sheet thickness direction to the amount of solute N in a region from a 3 / 8 depth position to a 4 / 8 depth position from the surface satisfies the following formula 1.

[0005] Patent Document 2 proposes a steel sheet for cans, characterized in that the composition, in mass%, contains C: 0.020% or more and 0.130% or less, Si: 0.04% or less, Mn: 0.10% or more and 1.20% or less, P: 0.007% or more and 0.100% or less, S: 0.030% or less, Al: 0.001% or more and 0.100% or less, N: more than 0.0120% and 0.0200% or less, Nb: 0.0060% or more and 0.0300% or less, with the balance being iron and unavoidable impurities, the upper yield strength is 460 to 680 MPa, the total elongation is 12% or more, and the absolute value of the difference between the amount of solute Nb in the region from the surface to the 1 / 8 depth position and the amount of solute Nb in the region from the 3 / 8 depth position to the 4 / 8 depth position is 0.0010 mass% or more. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] WO2016 / 157878 publication [Patent Document 2] WO2017 / 150066 publication Summary of the Invention [Problem to be solved by the invention]

[0007] The steel sheets for cans disclosed in Patent Documents 1 and 2 have high upper yield strength and high total elongation, but do not necessarily have sufficient tensile strength, or even if tensile strength is obtained, there is a problem that the can body strength (axial buckling strength) is insufficient.

[0008] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a steel sheet for cans having high strength and excellent formability, and a manufacturing method thereof. [Means for solving the problem]

[0009] In order to achieve the above object, the present invention provides the following. [1] In mass percent, C: 0.020% or more, 0.130% or less, Si: 0.04% or less, Mn: 0.10% or more, 0.60% or less, P: 0.020% or less, S: 0.005% or more, 0.020% or less, Al: 0.01% or more, 0.10% or less, N: 0.0050% or more, 0.0180% or less, Nb: 0.007% or more, 0.030% or less, Mo: 0.010% or more, 0.050% or less, The balance is Fe and unavoidable impurities, The tensile strength is 500 MPa or more, Elongation is 10% or more, Steel sheet for cans. [2] The composition is further expressed as mass percent: B: 0.0005% or more, 0.0040% or less, Cr: 0.04% or more, 0.20% or less Contains one or more of the following: The steel sheet for cans according to [1]. [3] The metal structure has ferrite and is composed of one or more of pearlite or granular cementite. The steel sheet for cans according to [1] or [2]. [4] A method for producing a steel sheet for cans according to any one of [1] to [3], A heating step of heating the steel slab having the above-mentioned composition at a heating temperature of 1100°C or higher; a hot rolling process in which the steel slab after the heating process is hot rolled under a hot rolling finishing temperature condition of 830°C or more and 950°C or less; a coiling step of coiling the hot-rolled sheet obtained in the hot rolling step at a coiling temperature of 450°C or more and 650°C or less; a cold rolling process in which the hot-rolled sheet after the coiling process is cold-rolled at a rolling ratio of 85% or more; An annealing process in which the cold-rolled sheet obtained in the cold rolling process is annealed under the condition of an annealing temperature of 700 ° C. or more and 780 ° C. or less; A temper rolling process in which the annealed sheet obtained in the annealing process is rolled under conditions of an elongation rate of 0.5% or more and 5.0% or less; The method for producing a steel sheet for cans comprising the steps of: Effect of the Invention

[0010] The steel sheet for cans of the present invention has high strength and excellent formability. According to the present invention, it becomes possible to further reduce the thickness of steel sheets used for food cans, beverage cans, etc., thereby achieving resource saving and cost reduction. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The chemical composition, properties, and manufacturing method of the steel sheet for cans according to the present invention will be described below in order. Note that the present invention is not limited to the following embodiments.

[0012] First, the composition of the steel sheet for cans of the present invention will be described. In the description of the composition, % indicating the content of each component means mass %. The steel sheet for cans of the present invention will also be simply referred to as steel sheet.

[0013] C: 0.020% or more, 0.130% or less C is an important element for improving tensile strength. By making the C content 0.020% or more, the tensile strength can be made 500 MPa or more. The C content is preferably 0.030% or more, and more preferably 0.085% or more. On the other hand, if the C content exceeds 0.130%, the elongation decreases. For this reason, the C content needs to be 0.130% or less.

[0014] Si:0.04% or less If a large amount of Si is added, the surface treatment property deteriorates due to surface concentration, and the corrosion resistance decreases, so the content must be 0.04% or less. The Si content is preferably 0.03% or less. On the other hand, since Si contributes to improving the tensile strength, it is preferable to add 0.01% or more.

[0015] Mn: 0.10% or more, 0.60% or less Mn contributes to improving tensile strength through solid solution strengthening, and a tensile strength of 500 MPa or more can be obtained. In order to obtain such an effect, the Mn content must be 0.10% or more. The Mn content is preferably 0.30% or more. On the other hand, if the Mn content exceeds 0.60%, the elongation decreases. Therefore, the upper limit of the Mn content must be 0.60%. The Mn content is preferably 0.55% or less.

[0016] P:0.020% or less If a large amount of P is contained, excessive hardening and central segregation cause deterioration in workability and corrosion resistance. Therefore, the upper limit of the P content is set to 0.020%. On the other hand, since P contributes to improving tensile strength, the P content is preferably 0.005% or more. The P content is more preferably 0.010% or more.

[0017] S: 0.005% or more, 0.020% or less S forms sulfides in steel and reduces castability. Therefore, the S content is set to 0.020% or less. If the S content is less than 0.005%, pitting corrosion may occur depending on the contents of the can, so the S content must be 0.005% or more. It is preferably more than 0.010%. More preferably, it is 0.011% or more.

[0018] Al: 0.01% or more, 0.10% or less Al is useful as a deoxidizing element and contributes to improving the cleanliness of steel. For this reason, it is necessary to contain 0.01% or more of Al. On the other hand, if Al is contained in excess, excessive AlN is generated, so that the amount of solute N decreases and the tensile strength decreases, so the Al content must be 0.10% or less. The Al content is preferably 0.08% or less, and more preferably 0.04% or less.

[0019] N: 0.0050% or more, 0.0180% or less N contributes to improving tensile strength by existing as solid solution N. Furthermore, when Mo is added, the strength of the can body can be improved by increasing the N content. For this reason, the N content must be 0.0050% or more. On the other hand, if it is contained in excess, elongation decreases due to the formation of coarse nitrides, so the N content must be 0.0180% or less.

[0020] Nb: 0.007% or more, 0.030% or less Nb is an important element that improves tensile strength by refining ferrite grains and forming carbides, and in order to obtain such effects, the Nb content must be 0.007% or more. The Nb content is preferably 0.010% or more. On the other hand, if the Nb content exceeds 0.030%, the recrystallization temperature becomes excessively high, making it difficult to achieve both tensile strength and elongation. Therefore, the Nb content is set to 0.030% or less.

[0021] Mo: 0.010% or more, 0.050% or less Mo is an important element in the present invention, and contributes to improving tensile strength by refining ferrite grains and forming carbonitrides. Furthermore, it contributes not only to improving tensile strength but also to improving the axial buckling strength of the can body. Therefore, Mo must be contained at 0.010% or more. The Mo content is preferably 0.020% or more. On the other hand, if Mo is contained at more than 0.050%, not only will such effects saturate, but grain boundary segregation will become excessive and elongation will decrease. Therefore, the upper limit of the Mo content must be 0.050%, and it is preferably 0.045% or less.

[0022] The steel sheet for cans of the present invention may have a composition containing the above-mentioned components with the balance being Fe and unavoidable impurities.

[0023] In addition to the above-mentioned chemical composition, the steel sheet for cans of the present invention preferably further contains at least one of B: 0.0005% to 0.0040% and Cr: 0.04% to 0.20%.

[0024] B: 0.0005% or more, 0.0040% or less B has the effect of refining ferrite grains and increasing tensile strength. For this reason, the B content is preferably 0.0005% or more. Furthermore, from the viewpoint of improving strength and elongation by finely dispersing pearlite and granular cementite, it is even more preferable to make it more than 0.0020%. If excessive B is added, the amount of solid-solubilized N decreases due to the formation of BN, and the tensile strength decreases, so the content is preferably 0.0040% or less.

[0025] Cr: 0.04% or more, 0.20% or less Cr has the effect of increasing tensile strength by forming carbides and refining ferrite grains. Therefore, the Cr content is preferably 0.04% or more. Even if it is contained in excess, the effect is saturated, so it is preferably 0.20% or less.

[0026] Next, the steel sheet properties of the steel sheet for cans of the present invention will be described.

[0027] Tensile strength: 500MPa or more In order to ensure sufficient strength for a thin-walled can body, the tensile strength of the steel sheet must be 500 MPa or more, and is preferably 550 MPa or more.

[0028] Elongation: 10% or more In order to ensure good formability without cracking during necking, flange processing, bead processing, etc. of the can body, the elongation must be 10% or more, and is preferably 12% or more. In the present invention, the tensile strength and elongation are evaluated in accordance with JIS Z 2241 after JIS No. 5 tensile test pieces are taken from the rolling direction and aged at 210°C for 20 minutes.

[0029] The thickness of the steel sheet for cans of the present invention is not particularly limited, but is preferably 0.50 mm or less. Since the steel sheet for cans of the present invention can be made thinner, it is more preferable to set the thickness to 0.30 mm or less from the viewpoints of resource saving and cost reduction.

[0030] Steel plate structure (optimal conditions): The metal structure has ferrite and is composed of at least one of pearlite and granular cementite. High strength and high elongation can be achieved by dispersing at least one of pearlite (P) and granular cementite (θ) in addition to the ferrite (α) structure. If martensite (M) or bainite (B) is contained, the strength may become excessive and the elongation may decrease, so it is preferable not to contain these structures. For this reason, the metal structure preferably consists of at least one of pearlite (P) and granular cementite (θ) in addition to the ferrite (α) structure. The steel sheet structure is cut from the steel sheet so that a vertical cross section parallel to the rolling direction of the steel sheet can be observed, and the observation surface of the sample is polished and then etched with nital to reveal the structure, and the steel sheet structure is photographed at a position halfway through the sheet thickness at a magnification of 3000 times using a scanning electron microscope to distinguish the steel sheet structure.

[0031] Next, the manufacturing method of the steel sheet for cans of the present invention will be described. The manufacturing method of the steel sheet for cans of the present invention is characterized by having a heating step of heating a steel slab having the above-mentioned composition at a heating temperature of 1100°C or more, a hot rolling step of hot rolling the steel slab after the heating step under the condition of a hot rolling finishing temperature of 830°C to 950°C, a coiling step of coiling the hot rolled sheet obtained in the hot rolling step under the condition of a coiling temperature of 450°C to 650°C, a cold rolling step of cold rolling the hot rolled sheet after the coiling step under the condition of a rolling reduction of 85% or more, an annealing step of annealing the cold rolled sheet obtained in the cold rolling step under the condition of an annealing temperature of 700°C to 780°C, and a temper rolling step of rolling the annealed sheet obtained in the annealing step under the condition of an elongation ratio of 0.5% to 5.0%. The steel sheet for cans produced by the following production method may be appropriately subjected to steps such as a plating step of applying Sn plating, Ni plating, Cr plating or the like, a chemical conversion treatment step, and a resin film coating step such as lamination.

[0032] Heating temperature: 1100℃ or more A steel slab having the above-mentioned composition is heated at a heating temperature of 1100°C or higher (heating step). If the heating temperature of the steel slab before hot rolling is too low, coarse nitrides may be generated and elongation may decrease, so the heating temperature of the steel slab is set to 1100°C or higher. The heating temperature of the steel slab is preferably 1150°C or higher.

[0033] Hot rolling finishing temperature: 830℃ to 950℃ The steel slab after the heating process is subjected to hot rolling under the condition of a hot rolling finishing temperature of 830°C or more and 950°C or less (hot rolling process). If the hot rolling finishing temperature (finishing temperature of hot rolling) exceeds 950°C, the ferrite crystal grains in the hot rolled sheet become coarse, and the ferrite crystal grains after cold rolling, annealing, and temper rolling become coarse, and the tensile strength decreases. For this reason, the upper limit of the hot rolling finishing temperature is set to 950°C. On the other hand, if the finishing temperature of hot rolling is less than 830°C, coarse Nb carbides are formed during hot rolling, and the tensile strength decreases. For this reason, the lower limit of the hot rolling finishing temperature is set to 830°C. The preferable lower limit of the hot rolling finishing temperature is 850°C.

[0034] Winding temperature: 450℃ to 650℃ The hot-rolled sheet obtained in the hot rolling process is coiled at a coiling temperature of 450°C or more and 650°C or less (coiling process). If the coiling temperature exceeds 650°C, alloy carbides such as Nb carbide become coarse and the tensile strength decreases. For this reason, the coiling temperature needs to be 650°C or less. The coiling temperature is preferably 620°C or less. On the other hand, if the coiling temperature is less than 450°C, the precipitation of alloy carbides such as Nb is suppressed and the tensile strength decreases, so the lower limit of the coiling temperature is set to 450°C. The coiling temperature is preferably 470°C or more.

[0035] After that, the hot-rolled sheet after the coiling step is preferably pickled (pickling step). Pickling may be performed under conditions that can remove surface scale, and the scale may be removed by a method other than pickling.

[0036] Cold rolling ratio: 85% or more The hot-rolled sheet after the coiling process or pickling process is subjected to cold rolling at a rolling reduction of 85% or more (cold rolling process). Cold rolling refines the ferrite grains after annealing and improves the tensile strength. To achieve this effect, the rolling reduction of the cold rolling is set to 85% or more. The rolling reduction is preferably 87% or more. If the cold rolling reduction is too high, the in-plane anisotropy of the steel sheet increases and can forming properties may deteriorate, so the cold rolling reduction is preferably set to 91.2% or less.

[0037] Annealing temperature: 700℃ to 780℃ The cold-rolled sheet obtained in the cold rolling process is annealed under the condition of an annealing temperature of 700°C or more and 780°C or less (annealing process). In order to obtain high elongation by recrystallization annealing, it is necessary to set the annealing temperature to 700°C or more. The annealing temperature is preferably 720°C or more. On the other hand, if the annealing temperature exceeds 780°C, in addition to the alloy carbides such as Nb carbides becoming coarse, the ferrite crystal grains also become coarse, the tensile strength decreases, and the can body strength also decreases. Therefore, the upper limit of the annealing temperature needs to be 780°C. The annealing temperature is preferably 760°C or less. As the annealing method, continuous annealing is preferable from the viewpoint of uniformity of the material. The annealing time is not particularly limited, but is preferably 10s or more. From the viewpoint of fine graining of ferrite crystal grains, the annealing time is preferably 60s or less. In order to disperse at least one of pearlite and granular cementite in addition to the ferritic structure, the average cooling rate from 700° C. to 500° C. in the cooling step after annealing is preferably less than 100° C. / s, more preferably less than 30° C. / s.

[0038] Elongation rate: 0.5% or more and 5.0% or less The annealed sheet obtained in the annealing process is rolled under conditions of an elongation rate of 0.5% or more and 5.0% or less (temper rolling process). Temper rolling after annealing adjusts the surface roughness and corrects the sheet shape, and also improves the tensile strength by introducing strain into the steel sheet. To obtain such effects, the lower limit of the rolling rate (elongation rate) of the temper rolling is set to 0.5%. The elongation rate is preferably 1.2% or more. On the other hand, if the elongation rate exceeds 5.0%, excessive strain is introduced and the uniform elongation decreases. For this reason, the upper limit of the elongation rate is set to 5.0%. The elongation rate is preferably 3.0% or less. EXAMPLES

[0039] Steel slabs were obtained by melting steels containing the components of Steel Nos. 1 to 11 shown in Table 1 with the balance being Fe and unavoidable impurities. The obtained steel slabs were heated under the conditions shown in Table 2, hot rolled, coiled, pickled to remove scale, cold rolled, annealed in a continuous annealing furnace, and temper rolled to obtain steel sheets for cans (Steel Sheets Nos. 1 to 16).

[0040] The obtained steel sheets for cans were evaluated for tensile strength and elongation. In addition, the steel sheet structure was identified and the axial buckling strength of the can body was evaluated. The evaluation methods were as follows. (Evaluation of tensile strength and elongation) From the obtained steel sheets for cans, JIS No. 5 tensile test pieces were taken along the rolling direction, and after aging heat treatment at 210° C. for 20 minutes, the tensile strength and elongation were evaluated in accordance with JIS Z 2241. (Evaluation of steel sheet structure) A sample was cut out from the obtained steel sheet for cans so that a vertical cross section parallel to the rolling direction of the steel sheet could be observed. The observation surface of the sample was polished and then etched with nital to reveal the structure. The steel sheet structure was photographed at a position halfway through the sheet thickness at a magnification of 3000 times using a scanning electron microscope and identified. (Evaluation of the axial buckling strength of can bodies) From the obtained steel plate for cans, blanks were cut with the plate width direction as the can circumferential direction, welded to a can height of 104 mm and an outside diameter of 52.3 mm, necked and flanged, and then the top and bottom of the can were tightened to produce a can body. A load was applied to the can body in the can height direction, and the load at which the can body buckled was measured. If it was 3500N or more, the axial buckling strength was deemed good and marked with ◯, and if it was less than 3500N, it was marked with ×.

[0041] The evaluation results are shown in Table 3.

[0042] [Table 1]

[0043] [Table 2]

[0044] [Table 3]

[0045] The inventive examples all had a tensile strength of 500 MPa or more, an elongation of 10% or more, and good axial buckling of the can body. Therefore, they are high-strength and highly formable steel sheets for cans. On the other hand, the comparative examples were inferior in at least one of tensile strength, elongation, and axial buckling strength.

Claims

1. In mass percent, C: 0.020% or more, 0.130% or less, Si: 0.04% or less, Mn: 0.10% or more, 0.60% or less, P: 0.020% or less, S: 0.005% or more, 0.020% or less, Al: 0.01% or more, 0.10% or less, N: 0.0050% or more, 0.0180% or less, Nb: 0.007% or more, 0.030% or less, Mo: 0.010% or more, 0.050% or less, The balance is Fe and unavoidable impurities. The tensile strength after aging heat treatment at 210°C for 20 minutes is 500 MPa or more, The elongation after the aging heat treatment is 10% or more. Steel sheet for cans.

2. The composition of the components is further expressed as follows, in mass%: B: 0.0005% or more, 0.0040% or less, Cr: 0.04% or more, 0.20% or less Contains one or more of the following: The steel sheet for cans according to claim 1.

3. The metal structure has ferrite and is composed of at least one of pearlite and granular cementite. The steel sheet for cans according to claim 1 or 2.

4. The method for producing a steel sheet for cans according to any one of claims 1 to 3, A heating step of heating a steel slab having the above-mentioned composition at a heating temperature of 1100°C or higher; A hot rolling process in which the steel slab after the heating process is hot rolled under a hot rolling finishing temperature condition of 830°C to 950°C; a coiling step of coiling the hot-rolled sheet obtained in the hot rolling step at a coiling temperature of 450° C. or more and 650° C. or less; a cold rolling process in which the hot-rolled sheet after the coiling process is cold-rolled at a rolling ratio of 85% or more; An annealing step of annealing the cold-rolled sheet obtained in the cold rolling step under the condition of an annealing temperature of 700 ° C. or more and 780 ° C. or less; A temper rolling process in which the annealed sheet obtained in the annealing process is rolled under the condition of an elongation rate of 0.5% or more and 5.0% or less; The method for producing a steel sheet for cans comprising the steps of:

Citation Information

Patent Citations

  • High-strength steel sheet for can manufacturing and method for manufacturing the same

    JP2009084687A

  • Steel plate for high strength high workability can and method for manufacturing the same

    JP2013028842A

  • High-strength steel sheet for cans and method for producing the same

    JP2021091966A

  • Method for producing a corrosion-resistant steel sheet

    US20160002748A1

  • Steel sheet for cans and method for manufacturing steel sheet for cans

    WO2016157878A1