Explosion-proof sheet manufacturing method based on explosion value optimization, explosion-proof sheet and battery shell

Through the stamping process, the explosion-proof marks are formed and combined with high-temperature annealing treatment, the problem of poor explosion-proof marks in stainless steel battery shells is solved, low-cost and high-stability explosion value control is achieved, and the safety and performance of the battery is ensured.

CN118976816APending Publication Date: 2024-11-19SHENZHEN EVERWIN PRECISION TECHNOLOGY CO LTD

Patent Information

Application Number
CN202411041318.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When the explosion-proof marks of existing stainless steel battery shells are made by laser etching or stamping, the process is complex, the cost is high, and the stability and consistency are poor, resulting in unstable burst value and difficult to meet the needs of low cost and high stability.

Method used

The stamping process is used to form explosion-proof marks on the stainless steel explosion-proof sheet blank, and the hardness and stress of the marking area are reduced by high-temperature annealing. Annealing is combined with a 3D printed vacuum heat treatment furnace to achieve a more stable burst value.

Benefits of technology

The process flow is simplified, the cost is reduced, and the stability and consistency of explosion-proof marks are improved, so that the blasting value is around 1.2MPa, meeting the customer's blasting value requirements and avoiding the risk of excessive expansion or failure of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118976816A_ABST
    Figure CN118976816A_ABST
Patent Text Reader

Abstract

The invention discloses an explosion-proof sheet manufacturing method based on explosion value optimization, an explosion-proof sheet and a battery shell. The explosion-proof sheet manufacturing method based on explosion value optimization comprises the following steps: taking an explosion-proof sheet blank; an anti-explosion nick is formed in the anti-explosion piece blank; and carrying out high-temperature annealing treatment on the anti-explosion sheet blank, so that the hardness of the anti-explosion nick area of the anti-explosion sheet blank is reduced to 100-200 HV. According to the explosion-proof sheet blank and the manufacturing method thereof, the hardness of the explosion-proof nick area can be reduced to 100 HV to 200 HV by performing high-temperature annealing on the explosion-proof sheet blank, so that the stress of the explosion-proof nick area can be removed, the hardness of the explosion-proof nick area can be softened, a relatively small explosion-proof nick and a relatively stable explosion value are realized, and the requirements of customers on the explosion value range are met.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of new energy batteries, and in particular relates to a method for manufacturing an explosion-proof sheet based on explosion value optimization, an explosion-proof sheet and a battery shell. Background Art

[0002] In recent years, new energy batteries have developed rapidly, and power battery shells and energy storage battery shells are developing towards large capacity and low cost. The advantages of stainless steel battery shells, such as easy welding, high strength, and material restrictions, make up for the shortcomings of aluminum and tinplate battery shells. The explosion-proof valve of the stainless steel battery shell is generally provided with explosion-proof notches. In order to ensure the stability of the explosion value of the stainless steel explosion-proof valve, the explosion-proof notches are generally made by laser etching or stamping. However, the process of making explosion-proof notches by laser etching is more complicated, costly, and has poor stability and consistency. If the explosion-proof notches are made by stamping, the material accumulation in the explosion-proof notch area will increase the density and hardness due to stamping, which will make it more difficult to blast. Summary of the invention

[0003] In view of the above-mentioned deficiencies in the prior art, the technical problem to be solved by the present invention is to provide a method for manufacturing an explosion-proof plate based on explosion value optimization, an explosion-proof plate and a battery housing.

[0004] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0005] A method for manufacturing an explosion-proof disk based on burst value optimization comprises the following steps:

[0006] S100, taking a bursting disk blank;

[0007] S200, forming explosion-proof notches on the explosion-proof sheet blank;

[0008] S300, performing high temperature annealing treatment on the explosion-proof sheet blank to reduce the hardness of the explosion-proof notch area of ​​the explosion-proof sheet blank to 100 HV to 200 HV.

[0009] Furthermore, the explosion-proof disc blank is a stainless steel sheet.

[0010] Furthermore, in the step S200, an explosion-proof notch is formed on the explosion-proof sheet blank by a stamping process, and the hardness of the explosion-proof notch region of the explosion-proof sheet blank after stamping is 300 HV to 400 HV.

[0011] Furthermore, the cross-sectional shape of the explosion-proof notch is trapezoidal, "U"-shaped or "V"-shaped, and the residual thickness value of the explosion-proof notch is 0.03 mm to 0.05 mm.

[0012] Furthermore, in the step S200, a notch groove is first formed on the explosion-proof disc blank by a stamping process, and then an explosion-proof notch is formed in the notch groove by a stamping process.

[0013] Furthermore, in the step S300, the high temperature annealing treatment of the explosion-proof disk blank includes the following sub-steps:

[0014] S310, placing the explosion-proof sheet blank into a vacuum furnace, and evacuating the vacuum furnace;

[0015] S320, raising the temperature in the vacuum furnace uniformly to 900°C to 1300°C;

[0016] S330, keeping warm for a predetermined time;

[0017] S340, allowing the temperature in the vacuum furnace to naturally drop to 200°C to 300°C;

[0018] S350, filling the vacuum furnace with argon gas to rapidly reduce the temperature in the vacuum furnace to 70°C to 90°C;

[0019] S360. Take out the explosion-proof disk blank from the vacuum furnace.

[0020] Furthermore, in the step S310, the vacuum furnace is a 3D printing vacuum heat treatment furnace; the vacuuming time is 40min to 50min, and the vacuum degree in the vacuum furnace after vacuuming is less than 0.1pa; in the step S320, the heating rate is 3°C / min to 4°C / min, and in the step S330, the insulation time is 2 hours.

[0021] Furthermore, the explosion-proof notch is runway-shaped, including a first semicircular notch and a second semicircular notch symmetrically arranged, and two straight-segment widening notches connecting the first semicircular notch and the second semicircular notch at corresponding end points.

[0022] A bursting-proof disk is manufactured by a bursting-value-optimized bursting-proof disk manufacturing method.

[0023] A battery casing, wherein an explosion-proof valve of the battery casing comprises an explosion-proof piece.

[0024] In the present invention, a stamping process is used to form explosion-proof notches, which are more stable and more consistent, and the process is simple, with fewer steps and low production cost. By high-temperature annealing the explosion-proof sheet blank, the stress and hardness in the explosion-proof notch area are reduced by high-temperature annealing to achieve a smaller and more stable burst value to meet the customer's requirements for the explosion value range. A 3D printing vacuum heat treatment furnace can be used, which can be fully automatically controlled by a computer program during the entire annealing process, with stable power, effectively solving the problem of unstable burst value and overall large burst value of explosion-proof valves made of stainless steel explosion-proof sheets. By selecting a reasonable residual thickness value of the explosion-proof notch 200, the tearing pressure value of the explosion-proof notch 200 can be stabilized at about 1.2MPa. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0026] Figure 1 The present invention is a flow chart of an embodiment of a method for manufacturing a burst-proof disk based on burst value optimization.

[0027] Figure 2 It is a schematic diagram of the structure after explosion-proof notches are formed on the explosion-proof sheet blank.

[0028] Figure 3 for Figure 2 Top view of the .

[0029] Figure 4 for Figure 3 AA section view.

[0030] Figure 5 for Figure 4 Enlarged view of point B in the middle.

[0031] Figure 6 Flow chart of high temperature annealing treatment.

[0032] The accompanying drawings in the specification are as follows:

[0033] Explosion-proof disc blank 100 , notch groove 110 , explosion-proof notch 200 , first semicircular arc notch 211 , second semicircular arc notch 212 , first straight line segment notch 221 , second straight line segment notch 222 . DETAILED DESCRIPTION

[0034] The following describes the implementation methods of the present invention through specific examples. The illustrations provided in the following embodiments are only used to schematically illustrate the basic concept of the present invention. The following embodiments and features in the embodiments may be combined with each other without conflict.

[0035] See also Figure 1 , Figure 1 This is a flow chart of an embodiment of a method for manufacturing a burst-proof disk based on burst value optimization of the present invention. The method for manufacturing a burst-proof disk based on burst value optimization of this embodiment includes the following steps:

[0036] S100, taking an explosion-proof sheet blank 100. In this embodiment, the explosion-proof sheet blank 100 is a stainless steel sheet. The stainless steel sheet has the advantages of easy welding, high strength, and no material limitation, etc., which makes up for the shortcomings of aluminum and tinplate materials.

[0037] S200, please refer to Figure 2 , forming an explosion-proof notch 200 on the explosion-proof disc blank 100. In this embodiment, the explosion-proof notch 200 is formed on the explosion-proof disc blank 100 by a stamping process. Of course, the notch groove 110 can also be formed on the explosion-proof disc blank 100 by a stamping process, and then the explosion-proof notch 200 is formed in the notch groove 110 by a stamping process. The explosion-proof notch 200 can be arranged near the outer edge of the groove bottom of the notch groove 110. After stamping, the area of ​​the explosion-proof notch 200 causes material accumulation due to stamping, and the density increases and the hardness becomes harder. At this time, the hardness of the explosion-proof notch 200 area of ​​the explosion-proof disc blank 100 is generally 300HV to 400HV, resulting in a large blasting value, which will affect the stability of the blasting.

[0038] See also Figure 3 In this embodiment, the explosion-proof notch 200 is in the shape of a runway, including a symmetrically arranged first semicircular notch 211 and a second semicircular notch 212, a first straight line segment notch 221 connecting the first end of the first semicircular notch 211 and the first end of the second semicircular notch 212, and a second straight line segment notch 222 connecting the second end of the first semicircular notch 211 and the second end of the second semicircular notch 212. Of course, the explosion-proof notch 200 may also be in other shapes such as an ellipse.

[0039] See also Figure 4 and Figure 5 In this embodiment, the cross-sectional shape of the explosion-proof notch 200 is a trapezoid; of course, in other embodiments, the cross-sectional shape of the explosion-proof notch 200 may also be other shapes such as a "V" shape or a "U" shape. The value of the lower bottom width of the cross-sectional area of ​​the explosion-proof notch 200 is in the range of 0 to 0.5 mm. When the cross-sectional shape of the explosion-proof notch 200 is a trapezoid, the angle a between the waist of the trapezoid and the vertical direction (i.e., the height of the trapezoid) and the value of the lower bottom width W1 of the trapezoid will also have a certain influence on the tearing pressure value of the explosion-proof structure. The value of the angle a between the waist of the trapezoid and the height of the trapezoid is in the range of 5° to 60°, preferably 25°≤a≤45°, and the value of the lower bottom width W of the trapezoid is preferably 0.03mm≤W≤0.08mm.

[0040] Please continue reading Figure 4 and Figure 5 , the tearing pressure value at the explosion-proof notch 200 is mainly affected by the residual thickness value d1 of the explosion-proof notch 200; the residual thickness value of the explosion-proof notch 200 is defined as the remaining thickness of the explosion-proof sheet blank 100 after thinning at the explosion-proof notch 200. By selecting a suitable residual thickness value d1, the tearing pressure range of the explosion-proof notch 200 can be limited. If the residual thickness value d1 of the explosion-proof notch 200 is small, the strength of the enclosed area of ​​the explosion-proof notch 200 will be greatly reduced. When the explosion-proof sheet collides with other products during movement, it is very likely that the explosion-proof notch 200 will be broken, so that the external gas enters the battery through the rupture of the explosion-proof sheet and reacts chemically with the material of the battery cell, which will cause the battery to fail, and there may even be a battery explosion accident. If the value of t is large, when the internal pressure of the battery reaches the upper limit pressure, the pressure relief port formed by tearing from the explosion-proof notch 200 will be relatively small, so that the gas inside the battery cannot be discharged in time, and it may also cause the battery to over-expand and cause an explosion. In this embodiment, the residual thickness of the explosion-proof notch 200 is 0.03 mm to 0.05 mm.

[0041] When selecting the residual thickness value d1 of the explosion-proof notch 200, it is also necessary to consider the influence of the thickness d1 of the explosion-proof disk blank 100. In this embodiment, the thickness of the explosion-proof disk blank 100 is 0.15 mm to 0.3 mm.

[0042] S300, the explosion-proof sheet blank 100 is subjected to high temperature annealing treatment to remove stress, so that the hardness of the explosion-proof notch 200 region of the explosion-proof sheet blank 100 is reduced to 100HV to 200HV, thereby obtaining an explosion-proof sheet. The high temperature annealing process can reduce the stress and hardness of the explosion-proof notch 200 region of the explosion-proof sheet, thereby achieving a smaller and more stable explosion value to meet the explosion value requirements of the battery shell.

[0043] See also Figure 6 In this step, annealing the explosion-proof disk blank 100 may include the following sub-steps:

[0044] S310, placing the explosion-proof sheet blank 100 into a vacuum furnace, and evacuating the vacuum furnace. In this embodiment, the vacuum furnace adopts a 3D printing vacuum heat treatment furnace, and the vacuuming time is 40min to 50min. After the vacuuming, the vacuum degree in the vacuum furnace is less than 0.1Pa. In this embodiment, after evacuating for 40min to 50min, the vacuum degree in the vacuum furnace is about 0.05Pa.

[0045] Compared with the previous annealing of aluminum, the annealing of stainless steel explosion-proof disks requires higher temperature and longer time. The entire annealing process requires higher temperature control requirements and a cycle of nearly 17 hours, which is difficult to control. In this embodiment, a 3D printing vacuum heat treatment furnace is used, and the entire annealing process can be fully automatically controlled by a computer program with stable power. It is an effective solution to solve the problem of unstable burst value and overall large burst value of explosion-proof valves made of stainless steel explosion-proof disks, and can stabilize the tearing pressure value of the explosion-proof notch 200 at about 1.2MPa.

[0046] S320, uniformly raising the temperature in the vacuum furnace to 900°C to 1300°C. In this embodiment, the temperature in the vacuum furnace is raised at a heating rate of 3°C / min to 4°C / min, and the final temperature in the vacuum furnace after the heating is 1100°C.

[0047] S330, heat preservation for a predetermined time. In this step, the temperature in the vacuum furnace is maintained at 1100° C. for 2 hours.

[0048] S340, allowing the temperature in the vacuum furnace to naturally drop to 200° C. to 300° C. In this step, there is no need to intervene in the vacuum furnace.

[0049] S350, fill the vacuum furnace with argon gas to quickly reduce the temperature in the vacuum furnace to 70°C to 90°C. After filling with argon gas for about 2 hours, the temperature in the vacuum furnace can be reduced to 70°C to 90°C.

[0050] S360, taking out the explosion-proof disk blank 100 from the vacuum furnace, that is, the finished explosion-proof disk.

[0051] As shown in Table 1, it is a comparison table of explosion value test data for three cases: an explosion-proof disk unit that has not been annealed, an explosion-proof disk unit that has been annealed, and an explosion-proof disk unit that has been annealed and welded to a battery cell.

[0052] Table 1

[0053]

[0054] From the test data in Table 1, it can be seen that the explosion value of the explosion-proof plate monomer is greatly reduced through high-temperature annealing treatment, with the reduction rate exceeding 50%. In addition, the explosion value of the explosion-proof plate after high-temperature annealing treatment after being welded to the battery cell is around 1.2MPa, meeting customer requirements.

[0055] In this embodiment, a stamping process is used to form the explosion-proof notch 200 on the explosion-proof disc blank 100. The explosion-proof notch 200 is more stable and has better consistency. The process is simple, the number of steps is small, and the manufacturing cost is low. By performing high-temperature annealing on the explosion-proof disc blank 100 after stamping, the hardness of the explosion-proof notch 200 area can be reduced from 300HV to 400HV to 100HV to 200HV, thereby eliminating the stress in the explosion-proof notch 200 area and softening the hardness of the explosion-proof notch 200 area.

[0056] By using a 3D printed vacuum heat treatment furnace, the entire annealing process of nearly 17 hours can be fully automatically controlled by a computer program, with stable power. This can effectively solve the problem of unstable bursting value and overall large bursting value of explosion-proof valves made of stainless steel explosion-proof disks, and can stabilize the tearing pressure value of the explosion-proof notch 200 at around 1.2MPa.

[0057] In addition, explosion-proof notch 200 needs to reach a stable bursting value of about 1.2 MPa. In addition to ensuring the hardness of the explosion-proof notch 200 area, explosion-proof notch 200 is also required to have a stable residual thickness value. In this embodiment, when the residual thickness value of explosion-proof notch 200 is 0.03mm-0.05mm, CPK (Comp l ex Process Capability in ndex; an indicator used by modern enterprises to indicate process capability) reaches 1.33, which meets the requirements.

[0058] The present invention also discloses an explosion-proof piece, which is manufactured by the explosion-proof piece manufacturing method based on burst value optimization of any of the above embodiments.

[0059] The present invention also discloses a battery housing, which is a housing of a secondary battery, which can be a power battery or an energy storage battery, and the explosion-proof valve of the secondary battery housing can include an explosion-proof disc made by the explosion-proof disc manufacturing method based on explosion value optimization in any of the above embodiments. Of course, the battery housing also includes a bottom shell and a top cover, as well as electrodes arranged on the top cover and other structures necessary for conventional battery housings, which are all prior art and will not be described in detail here.

[0060] The above embodiments only express the preferred implementation modes of the present invention, and the descriptions thereof are relatively specific and detailed, but they cannot be understood as limiting the scope of the invention patent. It should be pointed out that, for those of ordinary skill in the art, several variations and improvements can be made without departing from the concept of the present invention, and these all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for manufacturing explosion-proof disks based on explosion value optimization, It is characterized in that The following steps are involved: S100, taking a bursting disk blank; S200, forming explosion-proof notches on the explosion-proof sheet blank; S300, performing high temperature annealing treatment on the explosion-proof sheet blank to reduce the hardness of the explosion-proof notch area of ​​the explosion-proof sheet blank to 100 HV to 200 HV.

2. The method for producing an explosion-proof disk based on explosion value optimization according to claim 1, Features: The explosion-proof disk blank is a stainless steel sheet.

3. The method for manufacturing an explosion-proof disk based on burst value optimization according to claim 1, Features: In the step S200, an explosion-proof notch is formed on the explosion-proof sheet blank by a stamping process, and the hardness of the explosion-proof notch region of the explosion-proof sheet blank after stamping is 300 HV to 400 HV.

4. The method for manufacturing an explosion-proof disk based on explosion value optimization according to claim 1, Features: The cross-sectional shape of the explosion-proof notch is a trapezoid, a "U" shape or a "V" shape, and the residual thickness value of the explosion-proof notch is 0.03 mm to 0.05 mm.

5. The method for manufacturing an explosion-proof disk based on explosion value optimization according to claim 1, Features: In the step S200, a notch groove is first formed on the explosion-proof disk blank by a stamping process, and then an explosion-proof notch is formed in the notch groove by a stamping process.

6. A method for manufacturing an explosion-proof disk based on burst value optimization according to any one of claims 1 to 5, It is characterized in that In the step S300, the high temperature annealing treatment of the explosion-proof disk blank comprises the following sub-steps: S310, placing the explosion-proof sheet blank into a vacuum furnace, and evacuating the vacuum furnace; S320, raising the temperature in the vacuum furnace uniformly to 900°C to 1300°C; S330, keeping warm for a predetermined time; S340, allowing the temperature in the vacuum furnace to naturally drop to 200°C to 300°C; S350, filling the vacuum furnace with argon gas to rapidly reduce the temperature in the vacuum furnace to 70°C to 90°C; S360. Take out the explosion-proof disk blank from the vacuum furnace.

7. The method for manufacturing an explosion-proof disk based on burst value optimization according to claim 6, Features: In the step S310, the vacuum furnace is a 3D printing vacuum heat treatment furnace; the vacuuming time is 40min to 50min, and the vacuum degree in the vacuum furnace is less than 0.1pa after vacuuming; in the step S320, the heating rate is 3°C / min to 4°C / min, and in the step S330, the insulation time is 2 hours.

8. The method for producing an explosion-proof disk based on burst value optimization according to any one of claims 1 to 7, Features: The explosion-proof notch is in the shape of a runway, and includes a first semicircular notch and a second semicircular notch that are symmetrically arranged, and two straight-segment widening notches that connect the first semicircular notch and the second semicircular notch at corresponding end points.

9. An explosion-proof disk, Features: The explosion-proof disk is manufactured by the explosion-proof disk manufacturing method based on explosion value optimization as described in any one of claims 1 to 8.

10. A battery casing, Features: The explosion-proof valve of the battery casing includes the explosion-proof disk as claimed in claim 9.

Citation Information

Patent Citations

  • Power battery explosion-proof valve with stable structure and machining process thereof

    CN111740065A

  • Power battery explosion-proof valve structure and processing technology thereof

    CN111916615A

  • Manufacturing method of battery shell with anti-explosion nicks, battery and electric equipment

    CN117283145A

  • Anti-exposure valve plate, manufacturing method of anti-exposure valve plate, battery shell and manufacturing method of battery shell

    CN119927578A

  • Battery explosion-proof valve plate and manufacturing method thereof

    CN121507300A

Cited By

  • Automatic testing system and method for explosion-proof valve

    CN119827138A

  • An automatic testing system and method for an explosion-proof flap

    CN119827138B

  • Anti-exposure valve plate, manufacturing method of anti-exposure valve plate, battery shell and manufacturing method of battery shell

    CN119927578A

  • Battery explosion-proof valve plate and manufacturing method thereof

    CN121507300A

  • Explosion-proof valve plate having optimized bursting value and manufacturing method, and battery case and manufacturing method

    WO2026026536A1