Printed matter and printed matter combinations
The printed matter with a transparent base material and adhesive layer addresses transparency, adhesion, and blocking issues by using a resin film and convex particles, ensuring clear display and durability when stacked or combined.
Patent Information
- Application Number
- JP2024141229
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2024-08-22
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-22
AI Technical Summary
Existing printed materials with transparent substrates face issues of low transparency, poor adhesion between the substrate and printed layer, and blocking when stacked or combined with other materials, which diminishes their aesthetic value.
The printed matter includes a transparent base material with a resin film and an easily adhesive layer on one surface, containing a binder component and particles that form convex portions, ensuring high transparency (≤3.0%), strong adhesion, and preventing blocking.
The solution maintains high transparency, enhances adhesion, and prevents blocking, thereby preserving the aesthetic value and structural integrity of the printed materials when combined with other printed matters or objects.
Smart Images

Figure 0007586371000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to printed articles and printed article combinations. [Background technology]
[0002] Printed matter in which a picture is printed on a transparent substrate is known. The printed matter described in Patent Document 1 imitates cel drawings that were used in the production of animation in the past. Cel drawings are items in which original drawings are drawn on a transparent celluloid substrate. Digital drawing using computers has become widespread in recent years. Therefore, cel drawings are no longer used in the production of animation. On the other hand, prints imitating cel drawings are collected by enthusiasts, fans, and enthusiasts.
[0003] Printed materials using transparent substrates are used by layering them with patterned materials in which a pattern is printed on a paper substrate or the like. The pattern on the patterned material is observed through the transparent substrate of the printed material. Users can also layer multiple printed materials. When multiple printed materials are combined, the pattern on the printed material in the back is observed through the transparent substrate of the printed material in the foreground. Users can enjoy unique displays by combining multiple patterns.
[0004] In a printed matter in which a design is printed on a transparent substrate, the transparent substrate is required to have high transparency. If the transparency of the transparent substrate is low, the aesthetic value of the printed matter is reduced.
[0005] As described above, a printed matter using a transparent substrate can be treated as a printed matter combination in which the printed matter is combined with another picture or another printed matter. If the transparency of the transparent substrate is low, the picture behind the printed matter in the printed matter combination cannot be observed vividly and clearly. Therefore, the aesthetic value of the printed matter combination is reduced.
[0006] In printed matter in which a pattern is printed on a transparent substrate, the transparent substrate is also required to have adhesion to the ink to be printed. If the adhesion between the transparent substrate and the printing layer is weak, the printing layer cannot be formed on the transparent substrate. When the printed matter is combined with a patterned matter or another printed matter, it will deform (e.g., bend). If the adhesion between the transparent substrate and the printing layer is weak, the printing layer may peel off from the transparent substrate when the printed matter is used. If the printing layer peels off even partially, the aesthetic value of the printed matter will be significantly impaired.
[0007] A printed matter having a pattern printed on a transparent substrate may be exhibited in combination with an object with a pattern or another printed matter. In this exhibit, the printed matter may be attached to the object with a pattern or another printed matter by, for example, a fixing device. The printed matter may be exhibited while covered with a transparent resin plate. As described above, a printed matter using a transparent substrate may be combined with an object with a pattern or another printed matter in a different manner. Therefore, the printed matter is required to suppress blocking between the object with a pattern, another printed matter, and the resin plate. Blocking is a phenomenon in which a printed matter sticks to other adjacent members. When blocking occurs, the aesthetic value of the printed matter is significantly impaired. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Application Publication No. 10-297141 Summary of the Invention [Problem to be solved by the invention]
[0009] As described above, the transparent substrate of the printed matter is required to have high transparency and adhesion to the printed layer. At the same time, it is also necessary to suppress blocking of the printed matter. The present disclosure aims to improve the transparency of the transparent substrate, improve the adhesion between the transparent substrate and the printed layer, and suppress blocking in a printed matter including the transparent substrate and the printed layer. [Means for solving the problem]
[0010] The first printed matter according to the embodiment of the present disclosure is A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer, the easy-adhesion layer is provided only on one surface of the resin film and constitutes the second surface; the resin film constitutes the first surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; A printed matter that is used by being overlapped with another printed matter such that the front surface is in contact with the back surface of the other printed matter, or that is used by being overlapped with a resin plate such that the front surface is in contact with the resin plate.
[0011] The second printed matter according to the embodiment of the present disclosure is A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; It is resistant to a mandrel test using a 5 mm diameter mandrel with a holding time of 30 seconds x 2 times, The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
[0012] A third printed matter according to an embodiment of the present disclosure is A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; The adhesion on the second surface is rated at 2 or less by a cross-cut method; The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
[0013] A fourth printed matter according to an embodiment of the present disclosure is A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; The average thickness of the binder component is 1.0 μm or less, The particles have an average particle size of 1.0 μm or less, The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate. Effect of the Invention
[0014] According to the present disclosure, for a printed matter including a transparent substrate and a printed layer, three advantages can be achieved: improved transparency of the transparent substrate, improved adhesion between the transparent substrate and the printed layer, and suppression of blocking. [Brief description of the drawings]
[0015] [Figure 1] FIG. 1 is a cross-sectional view showing an example of a printed matter according to an embodiment of the present disclosure. [Figure 2A] FIG. 2A is a photograph showing a specific example of a printed matter. [Figure 2B] FIG. 2B is a photograph showing another specific example of a printed matter. [Figure 3A] FIG. 3A is a plan view showing an example of a design displayed on the printed matter shown in FIG. [Figure 3B] FIG. 3B is a plan view showing another example of a design displayed on the printed matter shown in FIG. [Figure 4] FIG. 4 is a plan view showing a printed matter combination including the first printed matter shown in FIG. 3A and the second printed matter shown in FIG. 3B. [Diagram 5] FIG. 5 is a cross-sectional view showing the printed product combination shown in FIG. [Figure 6] FIG. 6 is a plan view showing an example of a patterned article. [Figure 7] FIG. 7 is a plan view showing a printed matter combination including the first printed matter shown in FIG. 3A, the second printed matter shown in FIG. 3B, and the picture matter shown in FIG. [Figure 8] FIG. 8 is a cross-sectional view showing the printed product combination shown in FIG. [Figure 9A] FIG. 9A is a diagram showing one specific example of a printed product combination. [Figure 9B] FIG. 9B is a cross-sectional view taken along line IX-IX in FIG. 9A. [Figure 10A] FIG. 10A is a diagram showing another specific example of a printed product combination. [Figure 10B] FIG. 10B is a cross-sectional view taken along line XX in FIG. 10A. [Figure 11A] FIG. 11A is a diagram showing yet another specific example of a printed product combination. [Figure 11B] FIG. 11B is a cross-sectional view taken along line XI-XI in FIG. 11A. [Figure 12A] FIG. 12A is a diagram showing one specific example of a printed product combination. [Figure 12B] FIG. 12B is a cross-sectional view taken along line XII-XII in FIG. 12A. [Figure 13A] FIG. 13A is a diagram showing one specific example of a printed product combination. [Figure 13B] FIG. 13B is a cross-sectional view taken along line XIII-XIII in FIG. 13A. [Figure 14A] FIG. 14A is a diagram showing one specific example of a printed product combination. [Figure 14B] FIG. 14B is a cross-sectional view taken along line XIV-XIV in FIG. 14A. [Figure 15] FIG. 15 is a diagram illustrating a test method for evaluating the adhesion of a printed layer. [Figure 16] FIG. 16 is a photograph showing the test results of a test for evaluating the adhesion of a printed layer. [Figure 17] FIG. 17 is a photograph showing the test results of a test evaluating the adhesion of a printed layer. [Figure 18]FIG. 18 is a photograph showing the test results of a test evaluating the adhesion of a printed layer. [Figure 19] FIG. 19 is a photograph showing the test results of a test for evaluating the adhesion of a printed layer. [Figure 20] FIG. 20 is a diagram illustrating an evaluation pattern used in a test for evaluating blocking. [Figure 21] FIG. 21 is a diagram illustrating a test method for evaluating blocking in a transparent substrate. [Figure 22] FIG. 22 is a diagram illustrating the printing pattern of an evaluation printing layer used in a test for evaluating blocking in the printing layer. [Diagram 23] FIG. 23 is a diagram illustrating the printing pattern of an evaluation printing layer used in a test for evaluating blocking in the printing layer. [Figure 24] FIG. 24 is a diagram illustrating the printing pattern of an evaluation printing layer used in a test for evaluating blocking in the printing layer. [Diagram 25] FIG. 25 is a diagram illustrating the printing pattern of an evaluation printing layer used in a test for evaluating blocking in the printing layer. [Figure 26] FIG. 26 is a diagram illustrating a test method for evaluating blocking in a transparent printing layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] In this embodiment, <1> ~ <21> Regarding.
[0017] <1> A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer, The easy-adhesion layer is provided only on one surface of the resin film and constitutes the second surface, the resin film constitutes the first surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; A printed matter that is used by being overlapped with another printed matter such that the front surface is in contact with the back surface of the other printed matter, or that is used by being overlapped with a resin plate such that the front surface is in contact with the resin plate.
[0018] <2> A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; It is resistant to a mandrel test using a 5 mm diameter mandrel with a holding time of 30 seconds x 2 times, The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
[0019] <3> A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; The adhesion on the second surface is rated at 2 or less by a cross-cut method; The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
[0020] <4> A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes protrusions formed by the particles, The transparent substrate has a transmission haze of 3.0% or less; The average thickness of the binder component is 1.0 μm or less, The particles have an average particle size of 1.0 μm or less, The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
[0021] <5> The easy-adhesion layer is provided on only one surface of the resin film, The resin film constitutes the first surface. <1> ~ <4> 13. The printed matter according to any one of claims 1 to 12.
[0022] <6> It is resistant to a mandrel test using a 5 mm diameter mandrel with a holding time of 30 seconds x 2 times, <1> ~ <5> 13. The printed matter according to any one of claims 1 to 12.
[0023] <7> The adhesion on the second surface is rated at 2 or less by a cross-cut method. <1> ~ <6> 13. The printed matter according to any one of claims 1 to 12.
[0024] <8> The average thickness of the binder component is 1.0 μm or less, The particles have an average particle size of 1.0 μm or less, <1> ~ <7> 13. The printed matter according to any one of claims 1 to 12.
[0025] <9> The average thickness of the binder component is smaller than the average particle size of the particles. <1> ~ <8> 13. The printed matter according to any one of claims 1 to 12.
[0026] <10> The arithmetic mean roughness Sa of the first surface is 5.0 nm or less, The arithmetic average roughness Sa of the second surface is 5.0 nm or less. <1> ~ <9> 13. The printed matter according to any one of claims 1 to 12.
[0027] <11> The color difference of the transparent substrate before and after the light resistance test ΔE = ((ΔL * ) 2 +(Δa* ) 2 +(Δb * ) 2 ) 1 / 2 is less than or equal to 0.25, <1> ~ <10> 13. The printed matter according to any one of claims 1 to 12.
[0028] <12> The resin film is mainly composed of polyester or acrylic resin. <1> ~ <11> 13. The printed matter according to any one of claims 1 to 12.
[0029] <13> In the region where the printed layer is formed, the anti-see-through index Nt according to the anti-see-through method B (instrument method) is 85.0% or more; <1> ~ <12> 13. The printed matter according to any one of claims 1 to 12.
[0030] <14> The thickness of the printing layer is 0.40 μm or more. <1> ~ <13> 13. The printed matter according to any one of claims 1 to 12.
[0031] <15> The printing layer includes a pattern printing layer having a pattern and a white, uniform base printing layer; The pattern printed layer is located between the easy-adhesion layer and the undercoat printed layer. <1> ~ <14> 13. The printed matter according to any one of claims 1 to 12.
[0032] <16> The undercoat printing layer is provided only on the picture printing layer, The periphery of the undercoat printing layer is spaced apart from the periphery of the picture printing layer. <15> The printed matter described in.
[0033] <17> The thickness of the undercoat printing layer is 0.20 μm or more. <15> or <16> The printed matter described in.
[0034] <18> <1> ~ <17> A printed matter according to any one of claims 1 to 4, <1> ~ <17> and another printed material according to any one of claims 1 to 5. A printed material combination comprising:
[0035] <19> Further comprising a resin bag for containing the printed matter and the other printed matter. <18> 2. A printed matter combination as described in claim 1.
[0036] <20> <1> ~ <17> A printed matter according to any one of claims 1 to 4, A printed matter combination comprising:
[0037] <21> <1> ~ <17> A printed matter according to any one of claims 1 to 4, A printed matter combination comprising:
[0038] Hereinafter, the present embodiment will be described with reference to the drawings. In the drawings attached to this specification, the scale and the aspect ratio are appropriately changed and exaggerated from those of the actual objects for the convenience of understanding. Configurations shown in some drawings may be omitted in other drawings.
[0039] In this specification, terms specifying shapes and geometric conditions as well as the degree thereof, such as "parallel," "orthogonal," and "same," as well as values of lengths and angles, are not limited to their strict meanings, but are interpreted as including a range of degrees within which similar functions can be expected.
[0040] In this specification, terms such as "sheet," "film," and "plate" are not distinguished from one another solely on the basis of differences in name. For example, a "resin plate" is not distinguished from a member called a resin sheet or a resin film solely on the basis of differences in name.
[0041] In this specification, the normal direction of a sheet-like (film-like, plate-like) member means a direction parallel to the normal or perpendicular line to the sheet surface of the target sheet-like (film-like, plate-like) member. The "sheet surface (film surface, plate surface)" means a surface that coincides with the target sheet-like (film-like, plate-like) member when the target sheet-like (film-like, plate-like) member is observed as a whole.
[0042] In this specification, when multiple upper limit candidates and multiple lower limit candidates are given for a certain parameter, the numerical range of the parameter may be formed by combining any one of the upper limit candidates and any one of the lower limit candidates. As an example, consider the description "Parameter B may be A1 or more, A2 or more, or A3 or more. Parameter B may be A4 or less, A5 or less, or A6 or less." In this example, the numerical range of parameter B may be A1 or more and A4 or less, A1 or more and A5 or less, A1 or more and A6 or less, A2 or more and A4 or less, A2 or more and A5 or less, A2 or more and A6 or less, A3 or more and A4 or less, A3 or more and A5 or less, or A3 or more and A6 or less.
[0043] In order to clarify the relationship between directions between the drawings, some drawings show a first direction D1, a second direction D2, and a third direction D3 as common directions by arrows with a common symbol. The tip side of the arrow is the first side of each direction. The opposite side to the tip of the arrow is the second side of each direction. As shown in FIG. 1, a symbol with an x in a circle indicates an arrow pointing away from the paper in a direction perpendicular to the paper surface of the drawing. As shown in FIG. 3A, a symbol with a dot in a circle indicates an arrow pointing away from the paper in a direction perpendicular to the paper surface of the drawing.
[0044] The measurement methods described below, such as methods for measuring dimensions and physical properties, are not only applicable to measuring printed matter 20, but also to measuring components contained in printed matter 20, such as the transparent substrate, resin film, easy-adhesion layer, printing layer, picture printing layer, and base printing layer.
[0045] 1 to 26 are diagrams for explaining this embodiment. FIGS. 1 to 14B show specific examples of a printed matter combination 10 or a printed matter 20 according to this embodiment. FIG. 1 is a cross-sectional view showing the printed matter 20. As shown in FIG. 1, the printed matter 20 includes a front surface 21 and a back surface 22. The printed matter 20 includes a transparent substrate 30 and a printed layer 50. The printed layer 50 is formed on a portion of the transparent substrate 30. The transparent substrate 30 includes a first surface 31 and a second surface 32. The printed layer 50 is located on a portion of the second surface 32. The transparent substrate 30 includes a resin film 35 and an easy-adhesion layer 40.
[0046] In the illustrated example, the front surface 21 and the back surface 22 face each other in the first direction D1. From the front surface 21 to the back surface 22 in the first direction D1, the transparent substrate 30 and the printed layer 50 are located in this order. The front surface 21 may be formed of the transparent substrate 30. The back surface 22 may be formed of the transparent substrate 30 and the printed layer 50. A portion of the back surface 22 may be formed of the printed layer 50, and the other portion of the back surface 22 may be formed of the easy-adhesion layer 40.
[0047] In the illustrated example, the first direction D1 is a stacking direction of the transparent substrate 30 and the printed layer 50. The transparent substrate 30 and the printed layer 50 are both sheet-shaped. The printed matter 20 is also sheet-shaped. The printed matter 20 is also called a printed sheet or a printed film. The first direction D1 is a thickness direction of the printed matter 20, the transparent substrate 30, and the printed layer 50.
[0048] In the illustrated example, the first surface 31 and the second surface 32 face each other in a first direction D1. From the first surface 31 to the second surface 32 in the first direction D1, the resin film 35 and the easy-adhesion layer 40 are positioned in this order. The first surface 31 may be formed of the resin film 35. The second surface 32 may be formed of the easy-adhesion layer 40. A printed layer 50 is formed on a portion of the second surface 32.
[0049] In the illustrated example, the easy-adhesion layer 40 is located between the resin film 35 and the printed layer 50 in the first direction D1. The resin film 35, the easy-adhesion layer 40, and the printed layer 50 are located in this order from the front surface 21 to the back surface 22 in the first direction D1.
[0050] In the illustrated example, the first direction D1 is a lamination direction of the resin film 35 and the easy-adhesion layer 40. Both the resin film 35 and the easy-adhesion layer 40 are sheet-shaped. The first direction D1 is a thickness direction of the resin film 35 and the easy-adhesion layer 40.
[0051] In the illustrated example, the printed matter 20, the transparent substrate 30, the resin film 35, the easy-adhesion layer 40, and the printed layer 50 are flat. The printed matter 20, the transparent substrate 30, the resin film 35, the easy-adhesion layer 40, and the printed layer 50 extend on a plane. The printed matter 20, the transparent substrate 30, the resin film 35, the easy-adhesion layer 40, and the printed layer 50 extend in the second direction D2 and the third direction D3.
[0052] The second direction D2 and the third direction D3 are perpendicular to each other. The first direction D1 is perpendicular to the second direction D2. The first direction D1 is perpendicular to the third direction D3.
[0053] Unlike the illustrated example, the easy-adhesion layer 40 may be provided on both sides in the first direction D1 of the resin film 35. That is, the transparent substrate 30 may include the easy-adhesion layer 40, the resin film 35, and the easy-adhesion layer 40 in this order from the first surface 31 to the second surface 32 in the first direction D1.
[0054] The components included in the printed matter 20 will be described.
[0055] The transparent substrate 30 is a transparent substrate. Transparent means that the total light transmittance is 50% or more. The total light transmittance of the transparent substrate 30 may be 75% or more, 80% or more, 82% or more, 85% or more, 87% or more, 89% or more, 90% or more, or 92% or more. The total light transmittance of the transparent substrate 30 may be 100% or less, or may be less than 100%.
[0056] A light source that mimics the spectrum of D65 standard light (hereafter referred to as the D65 light source) is used to measure the total light transmittance. Before measuring the total light transmittance, the D65 light source is turned on for 15 minutes to stabilize the output of the D65 light source. The angle of incidence on the sample when measuring the total light transmittance is 0°. The test environment when measuring the total light transmittance is a temperature of 23°C ± 2°C and a relative humidity of 50% ± 5%. The sample is placed in the test environment for 16 hours before starting the test. Other measurement conditions when measuring the total light transmittance are in accordance with JIS K7361-1:1997.
[0057] The sample was large enough to cover the entire measurement window of the measuring device. The total light transmittance was the arithmetic average of three measured values. The three measured values that were the subject of the arithmetic average were the three measured values excluding the maximum and minimum values from the five measured values measured at the five measurement points included in the evaluation target. The five measurement points were located at least 10 mm apart from each other.
[0058] The incident surface when measuring the total light transmittance of the transparent substrate 30 is the first surface 31. In the printed matter 20, the printed layer 50 is located on a portion of the printed matter 20. The total light transmittance of the transparent substrate 30 is measured in the region of the printed matter 20 where the transparent substrate 30 is provided.
[0059] An upper limit may be set for the transmission haze of the transparent substrate 30. By setting an upper limit for the transmission haze of the transparent substrate 30, a pattern located behind the printed matter 20 can be observed vividly and clearly. The transmission haze of the transparent substrate 30 may be 3.0% or less, 2.5% or less, 2.0% or less, 1.6% or less, 1.4% or less, or 1.3% or less.
[0060] There is no particular lower limit set for the transmission haze of the transparent substrate 30. The transmission haze of the transparent substrate 30 may be 0 or more, or may be greater than 0.
[0061] A D65 light source is used to measure transmission haze. Before measuring transmission haze, turn on the D65 light source for 15 minutes to stabilize the output of the D65 light source. The angle of incidence on the sample when measuring transmission haze is 0°. The test environment when measuring transmission haze is a temperature of 23°C ± 2°C and a relative humidity of 50% ± 5%. The sample is placed in the test environment for 16 hours before starting the test. Other measurement conditions when measuring transmission haze are in accordance with JIS K7136:2000.
[0062] The sample was large enough to cover the entire measurement window of the measuring device. The transmitted haze was the arithmetic average of three measured values. The three measured values subject to the arithmetic average were the three measured values excluding the maximum and minimum values from the five measured values measured at the five measurement locations included in the evaluation target. The five measurement locations were located at least 10 mm apart from each other.
[0063] The incident surface when measuring the transmission haze of the transparent substrate 30 is the first surface 31. In the printed matter 20, the printed layer 50 is located on a portion of the printed matter 20. The total light transmittance of the transparent substrate 30 is measured in the region of the printed matter 20 where the transparent substrate 30 is provided.
[0064] An upper limit may be set for the arithmetic mean roughness Sa of the first surface 31. By setting an upper limit for the arithmetic mean roughness of the first surface 31, a pattern located behind the printed matter 20 can be vividly and clearly observed. The arithmetic mean roughness of the first surface 31 may be 5.0 nm or less, 4.0 nm or less, 3.0 nm or less, 2.0 nm or less, or 1.0 nm or less.
[0065] There is no particular lower limit set for the arithmetic mean roughness Sa of the first surface 31. The arithmetic mean roughness of the first surface 31 may be equal to or greater than 0 nm.
[0066] An upper limit may be set for the arithmetic mean roughness Sa on the second surface 32. By setting an upper limit for the arithmetic mean roughness on the second surface 32, a pattern located behind the printed matter 20 can be vividly and clearly observed. The arithmetic mean roughness on the second surface 32 may be 5.0 nm or less, 4.0 nm or less, 3.0 nm or less, 2.0 nm or less, or 1.0 nm or less.
[0067] There is no particular lower limit set for the arithmetic mean roughness Sa of the second surface 32. The arithmetic mean roughness of the second surface 32 may be equal to or greater than 0 nm.
[0068] The arithmetic mean roughness Sa is the three-dimensional arithmetic mean roughness defined in ISO25178. The arithmetic mean roughness Sa is an index showing surface roughness. The three-dimensional arithmetic mean roughness is the three-dimensional extension of the arithmetic mean roughness Ra related to two-dimensional roughness. The arithmetic mean roughness Sa is calculated by the following formula (i) by placing the orthogonal coordinate axes X and Y on the reference plane, the roughness curved surface as Z(x, y), and the size of the reference plane as Lx and Ly. In formula (i), A = Lx x Ly.
number
[0069] The arithmetic mean roughness is a value measured using a white light interference microscope. The measurement area using the white light interference microscope is 469.71 μm × 352.28 μm. Before measuring the arithmetic mean roughness, the light source is turned on for 15 minutes to stabilize the light source output. The test environment when measuring the arithmetic mean roughness is a temperature of 23°C ± 2°C and a relative humidity of 50% ± 5%. The sample is placed in the test environment for 16 hours before starting the test. Other measurement conditions when measuring the arithmetic mean roughness are in accordance with JIS B0601:2013.
[0070] The arithmetic mean roughness is the arithmetic mean of five measured values. The five measured values to be used for the arithmetic mean are the five measured values excluding the maximum and minimum values from the seven measured values measured at the seven measurement locations included in the evaluation object. The seven measurement locations are located at least 10 mm apart from each other.
[0071] 1, the transparent substrate 30 includes a resin film 35 and an easy-adhesion layer 40. The resin film 35 is a substrate that supports the printed layer 50. The easy-adhesion layer 40 is a layer that improves the adhesion of the printed layer 50.
[0072] The material of the resin film 35 is not particularly limited, and the material of the base material may be resin or glass. Resin is preferable because it is lightweight and easy to manufacture. In applications such as those shown in Figs. 9A to 14B to be referred to later, when the display method of the printed matter 20 is changed, the resin film 35 made of resin has excellent handleability. The resin contained in the resin film 35 may include acrylic resin, polyester, polypropylene, polystyrene, polycarbonate, and triacetyl cellulose.
[0073] The resin film 35 may contain acrylic resin as a main component. "Acrylic resin" includes both acrylic resin and methacrylic resin. The main component means a material contained in the target (e.g., the resin film 35) at the maximum mass percentage (wt%). The resin film 35 may contain acrylic resin at a mass percentage of 50% or more.
[0074] The acrylic resin contained in the resin film 35 may be any appropriate (meth)acrylic resin. Examples of (meth)acrylic resins include poly(meth)acrylic acid esters such as polymethyl methacrylate, methyl methacrylate-(meth)acrylic acid copolymers, methyl methacrylate-(meth)acrylic acid ester copolymers, methyl methacrylate-acrylic acid ester-(meth)acrylic acid copolymers, methyl (meth)acrylate-styrene copolymers (such as MS resins), and polymers having alicyclic hydrocarbon groups (for example, methyl methacrylate-cyclohexyl methacrylate copolymers, methyl methacrylate-norbornyl (meth)acrylate copolymers, etc.). Resins used in the base layer include poly(meth)acrylic acid C copolymers such as polymethyl (meth)acrylate. 1-6 It may contain alkyl.
[0075] The resin film 35 may contain polyester as a main component. The resin film 35 may contain, as the polyester, one or more of polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate.
[0076] The average thickness of the resin film 35 may be 10 μm or more and 500 μm or less, 20 μm or more and 250 μm or less, or 50 μm or more and 200 μm or less.
[0077] The "average thickness" used for the components 35, 40, and 50 included in the printed matter 20 is specified by (M1) to (M3) below.
[0078] (M1) The cross section of the printed matter 20 is imaged with a scanning transmission electron microscope (STEM) to obtain an observation image. The imaging area is determined so that the first direction D1, which is the thickness direction of the component to be measured, is aligned with the short side of the rectangular imaging area. The magnification during imaging is set to an appropriate magnification such that the thickness of the component to be measured relative to the length of the short side of the imaging area is 1 / 20 or more and 1 / 3 or less.
[0079] (M2) Measure the thickness of the component to be measured at a central position in the captured image along a direction perpendicular to the first direction D1, and at a pair of lateral positions on either side of the central position. The lateral positions are positions shifted to either side of the central position in the direction perpendicular to the first direction D1 by a length five times the thickness measurement value at the central position.
[0080] (M3) The above steps (M1) and (M2) are carried out three times for the component to be measured, and the thickness of the component to be measured is measured at a total of nine measurement positions. From the total of nine thickness measurements, the maximum measurement value, the second maximum measurement value, the minimum measurement value, and the second minimum measurement value are removed to obtain five thickness measurements. The average value of the five thickness measurements is regarded as the average thickness of the component to be measured.
[0081] Section samples with exposed cross sections for STEM observation were prepared according to the following steps (N1) to (N2).
[0082] (N1) Cut the printed matter to a desired size to create a cut sample. Then, embed the cut sample in resin to create an embedded sample. The cut sample should be a rectangular shape measuring 10 mm in length and 3 mm in width. Epoxy resin is used as the embedding resin.
[0083] The embedded sample was obtained by placing the cut sample in a silicon embedding plate, pouring in embedding resin, leaving it at room temperature for 12 hours to harden the embedding resin, and then removing the cut sample and the embedding resin from the silicon embedding plate. The embedded sample was in the shape of a block.
[0084] The epoxy resin used for embedding was a mixture of Struers' product name "Epofix" and the product name "Epofix Hardener" made by the same company in a ratio of 10:1.2. The silicon embedding plate made by Dosaka EM may be used.
[0085] (N2) The block-shaped embedded sample is cut vertically to prepare a section sample in which the cross section of the printed matter is exposed. The embedded sample is cut on a microtome using a glass knife and a diamond knife. When cutting the block-shaped embedded sample, it is first roughly cut with a glass knife. For rough trimming, a surface of approximately 100 μm in length and 20 μm in width that includes the cross section is prepared. Next, this surface is cut with a diamond knife, and the section sample floated on the water is collected with a mesh.
[0086] An example of a scanning transmission electron microscope that can be used to obtain an observation image is the ultra-high resolution field emission scanning electron microscope SU9000 manufactured by Hitachi High-Tech Corporation. When using this microscope, the BFSTEM shooting mode is used. The acceleration voltage is 30 kV. The emission current is 20 μA. The image data size is 1280 × 960 pixels. The measurement magnifications are 5000, 10000, 50000, 75000, and 100000 times.
[0087] The adhesive layer 40 includes a binder component 41 and particles 42 held by the binder component 41. The second surface 32 formed by the adhesive layer 40 includes protrusions 43 formed by the particles 42.
[0088] The protrusions 43 due to the particles 42 are protrusions 43 formed due to the particles 42. The protrusions 43 formed by the particles 42 are included in the protrusions 43 due to the particles 42. As shown in FIG. 1, the protrusions 43 may be formed by the particles 42 exposed from the binder component 41. The protrusions 43 may be formed by the particles 42 and the binder component 41 protruding on the particles 42. The protrusions 43 may be formed by the binder component 41 protruding on the particles 42.
[0089] The binder component 41 may function as a binding agent for forming a coating film. The binder component 41 may be an element that holds the particles 42. The binder component 41 holds the particles 42 contained in the adhesion layer 40, so that the adhesion layer 40 can maintain a film form. The binder component 41 may be a base material of the adhesion layer 40.
[0090] The material of the binder component 41 is not particularly limited. The binder component 41 may contain a resin. The resin contained in the binder component 41 may be a natural resin or a synthetic resin. The binder component 41 may contain a thermoplastic resin. The binder component 41 may contain a cured resin. The cured resin is a cured product of a curable resin composition. The curable resin may be a thermosetting resin or an ionizing radiation curable resin. The ionizing radiation curable resin may be an ultraviolet ray curable resin or an electron beam curable resin. Examples of the resin contained in the binder component 41 include thermoplastic resins such as polyester, polyurethane, and (meth)acrylic resin, and thermosetting resins.
[0091] The material of the particles 42 is not particularly limited. The particles 42 may be inorganic particles. The particles 42 may be organic particles. The easy-adhesion layer 40 may contain both organic particles and inorganic particles as the particles 42. Examples of the material of the inorganic particles include silica, alumina, zirconia, and titania. Examples of the material of the organic particles include polymethyl methacrylate, polyacrylic-styrene copolymer, melamine resin, polycarbonate, polystyrene, polyvinyl chloride, benzoguanamine-melamine-formaldehyde condensate, silicone, fluorine-based resin, and polyester-based resin.
[0092] The easy-adhesion layer 40 may be prepared by a wet method. The easy-adhesion layer 40 may be prepared using an easy-adhesion layer coating liquid for forming the easy-adhesion layer 40. The easy-adhesion layer 40 may be prepared by drying or curing the coating film of the easy-adhesion layer coating liquid. The easy-adhesion layer coating liquid for preparing the easy-adhesion layer 40 may contain a binder component 41, particles 42, a solvent, an additive, a crosslinking agent, etc. The convex portion 43 can be formed on the second surface 32 by adjusting the blending ratio of the particles 42, the average particle size of the particles 42, the material of the binder component 41, the material of the particles 42, the type of solvent contained in the easy-adhesion layer coating liquid, and the drying conditions of the coating film of the easy-adhesion layer coating liquid.
[0093] The easy-adhesion layer 40 may be produced by co-extrusion together with the resin film 35. By co-extrusion, the transparent substrate 30 including the resin film 35 and the easy-adhesion layer 40 can be produced.
[0094] An upper limit may be set for the average thickness of the binder component 41. By setting an upper limit for the average thickness of the binder component 41, it is possible to stably form the convex portions 43. The average thickness of the binder component 41 may be 1.0 μm or less, 0.8 μm or less, 0.5 μm or less, 0.3 μm or less, or 0.25 μm or less.
[0095] There is no particular lower limit for the average thickness of the binder component 41 as long as the particles 42 can be held by the binder component 41. The average thickness of the binder component 41 may be greater than 0 μm, may be 0.01 μm or more, or may be 0.02 μm or more.
[0096] The average thickness of the binder component 41 is the average thickness of the adhesive layer 40 in the region where the particles 42 are not present and the protrusions 43 are not formed. The average thickness of the binder component 41 is specified by the above-mentioned (M1) to (M3). That is, the arithmetic mean value of the five thickness measurements of the adhesive layer 40 in the region where the particles 42 are not present and the protrusions 43 are not formed, obtained by the above-mentioned (M1) to (M3), is the average thickness of the binder component 41.
[0097] However, when the imaging region is determined in (M1), the adhesive layer 40 located at the center along the direction perpendicular to the first direction D1 does not include particles 42 and does not include protrusions. In addition, in (M2), when the adhesive layer 40 includes at least one of the particles 42 and the protrusions 43 at any side position, the thickness of the adhesive layer 40 is measured at a position adjacent to the side position that does not include particles 42 and does not include protrusions.
[0098] An upper limit may be set for the average particle diameter of the particles 42. By setting an upper limit for the average particle diameter of the particles 42, protrusions 43 of an appropriate size can be formed. Protrusions 43 of an appropriate size can reduce the transmission haze of the printed matter 20. In other words, by setting an upper limit for the average particle diameter of the particles 42, the image behind the transparent substrate 30 can be observed vividly and clearly. The average particle diameter of the particles 42 may be 1.0 μm or less, 0.80 μm or less, 0.70 μm or less, 0.60 μm or less, or 0.5 μm or less.
[0099] A lower limit may be set for the average particle diameter of the particles 42. By setting a lower limit for the average particle diameter of the particles 42, protrusions 43 of an appropriate size can be formed. Protrusions 43 of an appropriate size can effectively suppress blocking, as described below. The average particle diameter of the particles 42 may be 0.010 μm or more, 0.030 μm or more, 0.040 μm or more, or 0.050 μm or more.
[0100] The average particle size of the particles 42 is determined by the following (M4) to (M6).
[0101] (M4) Obtain an observation image by photographing the cross section of the printed matter 20 with a scanning transmission electron microscope (STEM). The observation image of the cross section of the printed matter 20 is obtained in the same manner as when measuring the average thickness.
[0102] (M5) The largest particle located in the observed image is selected, and the particle diameter is measured. The particle diameter is the distance between two lines that is the maximum distance between the two lines when the cross section of the particle is sandwiched between the two lines. In other words, the particle diameter is the maximum length of the particle in the observed image. The particle diameter is specified as the particle diameter (maximum length) of each particle. In other words, the particle diameter is the primary particle diameter.
[0103] (M6) The above steps (M4) and (M5) are carried out nine times for the same optical sheet to be measured, to measure the particle diameters of a total of nine particles. From the total of nine particle diameter measurements, the largest measurement value, the second largest measurement value, the smallest measurement value, and the second smallest measurement value are removed to obtain five particle diameter measurements. The average value of the five particle diameter measurements is regarded as the average particle diameter of the particles 42.
[0104] 2A and 2B are images of a cross section of a printed matter 20 measured using a scanning transmission electron microscope. Fig. 2A shows a transparent substrate according to Example 1, which will be described later. Fig. 2B shows a transparent substrate according to Example 2, which will be described later.
[0105] The average thickness of the binder component 41 may be smaller than the average particle diameter of the particles 42. According to this example, the convex portions 43 of the particles 42 can be stably formed on the second surface 32. The convex portions 43 on the second surface 32 can suppress blocking, as described below.
[0106] The printed layer 50 is a layer formed by printing. The printed layer 50 may be formed by drying or curing a coating of ink. The printing for forming the printed layer 50 is not particularly limited. The printed layer 50 may be formed by inkjet printing, offset printing, silk printing, or gravure printing.
[0107] The printed layer 50 may include a binder component and a colorant held by the binder component.
[0108] The binder component may be a resin. The binder component may include a thermoplastic resin. The binder component may include a resin cured product. The resin cured product is a cured product of a curable resin composition. The curable resin may be a thermosetting resin or an ionizing radiation curable resin. The ionizing radiation curable resin may be an ultraviolet ray curable resin or an electron beam curable resin. Examples of resins contained in the binder component include ultraviolet ray curable resins such as polyester, polyurethane, and (meth)acrylic resin.
[0109] The colorant may be a pigment, a dye, or a combination of a pigment and a dye.
[0110] The printed layer 50 is formed with a pattern. The printed layer 50 displays a pattern. The pattern is not particularly limited. The printed layer 50 may include patterns such as figures, patterns, designs, colors, pictures, photographs, characters, marks, pictograms, symbols, letters, numbers, etc. In the printed matter 20 used in combination with another printed matter 20 or a patterned object 60 having a pattern, the printed matter 20 may include a pattern related to animation. The pattern related to animation may include a pattern such as a character, a building, a facility, belongings, letters, patterns, designs, colors, etc.
[0111] Fig. 3A shows a first printed matter 20A including a character design. Fig. 3B shows a second printed matter 20B including a character design. The first printed matter 20A and the second printed matter 20B differ in the facial expression and arrangement of the character design.
[0112] A lower limit may be set for the anti-see-through index Nt of the printed matter 20 in the area where the printing layer 50 is formed, measured by the anti-see-through B method (instrumental method). The anti-see-through index Nt is an index that indicates the degree of anti-see-through. When the anti-see-through index Nt is high, the anti-see-through property is high. In other words, when the anti-see-through index Nt is high, the printed matter 20 is less likely to transmit the color behind it. By increasing the anti-see-through property, the printed matter 20 can suppress the influence of the color behind it and vividly display the image in the desired color. The anti-see-through index Nt may be 85.0% or more, 90.0% or more, 91.0% or more, or 92.0% or more.
[0113] The anti-transparency index Nt can be increased by increasing the thickness of the printed layer 50, adding a dark color material to the printed layer 50, combining a picture printed layer with a base printed layer, etc. When a base printed layer is provided to increase the anti-transparency property, the thickness of the base printed layer may be 10 μm or more, or may be 20 μm or more.
[0114] There is no particular upper limit set for the anti-see-through index Nt of the printed matter 20 in the region where the printed layer 50 is formed, measured by the anti-see-through B method (instrumental method). The anti-see-through index Nt may be equal to or less than 100%.
[0115] The anti-transparency index Nt is the brightness (L * ) when using a white backing (L * The value of the anti-see-through index Nt is expressed as a percentage. The unit of the anti-see-through index Nt is "%". * ) is measured on the print 20 to be evaluated placed on a backing. * ) is measured using reflected light.
[0116] Lightness (L * When measuring the lightness (L) of the printed matter 20, the back surface 22 faces the backing, and the front surface 21 serves as the incident surface and the reflecting surface. * ) and lightness when using a white backing (L * The lightness (L) of the evaluation object is measured at the same measurement position by exchanging the white backing and the black backing. * ) and lightness when using a white backing (L * ) to calculate the anti-transparency index.
[0117] Lightness (L * Before measuring the light source, turn on the light source for 15 minutes to stabilize the light source output. The measurement wavelength is 400 nm to 700 nm. * The test environment for measuring the anti-transparency index Nt is 20°C ± 15°C and 60% ± 20% relative humidity. The sample is placed in the test environment for 16 hours before the start of the test. Other measurement conditions for measuring the anti-transparency index Nt are in accordance with JIS L1923:2017.
[0118] A measurement sample is obtained from the evaluation object. The measurement sample is approximately a square shape measuring 7 cm x 7 cm. The anti-see-through index Nt is measured at three measurement points on the measurement sample. The arithmetic mean value of the three anti-see-through index values is the anti-see-through index Nt of the evaluation object. The three measurement points are located at positions at least 10 mm apart from each other on the measurement sample.
[0119] A lower limit may be set for the thickness of the printed layer 50. By setting a lower limit for the thickness of the printed layer 50, the influence of the color of the pattern behind the printed layer 50 can be reduced, and the pattern of the printed layer 50 can be displayed vividly in the desired color. By setting a lower limit for the thickness of the printed layer 50, the easy-adhesion layer 40 constituting the back surface 22 together with the printed layer 50 can be prevented from contacting other adjacent members. The occurrence of blocking can be prevented by preventing the easy-adhesion layer 40, which is prone to blocking, from contacting other members. The thickness of the printed layer 50 may be 0.40 μm or more, 2.0 μm or more, 25 μm or more, or 35 μm or more.
[0120] An upper limit may be set for the thickness of the printed layer 50. By setting an upper limit for the thickness of the printed layer 50, the printed matter 20 can be made thinner. The thickness of the printed layer 50 may be 600 μm or less, 200 μm or less, 150 μm or less, or 8.0 μm or less.
[0121] As shown in FIG. 1, the printing layer 50 may include a picture printing layer 51 and a base printing layer 52. The picture printing layer 51 is a layer formed with a picture displayed by the printing layer 50. The picture printing layer 51 includes a picture. The picture printing layer 51 displays a picture. The base printing layer 52 is a uniform layer of a single color. The base printing layer 52 may be a uniform layer of white color. The base printing layer 52 is a base layer displayed by the picture printing layer 51. The base printing layer 52 allows the picture printing layer 51 to vividly display the picture.
[0122] The pattern-printed layer 51 may be formed by printing inks of cyan, magenta, yellow, and black. The thickness of the pattern-printed layer 51 may be appropriately set so as to display a desired pattern. The thickness of the pattern-printed layer 51 may be 0.20 μm or more and 200 μm or less, 1 μm or more and 100 μm or less, or 15 μm or more and 40 μm or less.
[0123] A lower limit may be set for the thickness of the base printing layer 52. By setting a lower limit for the thickness of the base printing layer 52, the influence of the color of the pattern behind the printing layer 50 can be reduced, and the pattern of the pattern printing layer 51 can be displayed vividly in the desired color. The thickness of the base printing layer 52 may be 0.20 μm or more, 1 μm or more, 10 μm or more, or 20 μm or more.
[0124] An upper limit may be set for the thickness of the base printing layer 52. By setting an upper limit for the thickness of the base printing layer 52, the printed matter 20 can be made thinner. The thickness of the base printing layer 52 may be 400 μm or less, 200 μm or less, 100 μm or less, or 40 μm or less.
[0125] 1, the base printing layer 52 may be provided only on the picture printing layer 51. The peripheral edge 52a of the base printing layer 52 may be separated from the peripheral edge 51a of the picture printing layer 51. According to this example, when the printed matter 20 is observed from the front surface 21, the base printing layer 52 is concealed by the picture printing layer 51. By concealing the base printing layer 52, the picture displayed by the picture printing layer 52 can be displayed vividly and clearly.
[0126] A method of using the printed matter 20 having the above configuration will be described with reference to the drawings.
[0127] The printed matter 20 includes a transparent substrate 30 and a printing layer 50. A pattern is formed on the printing layer 50. The printed matter 20 displays the pattern formed on the printing layer 50.
[0128] In the example shown in FIG. 1, the printing layer 50 includes a picture printing layer 51 and a base printing layer 52. The base printing layer 52 is a monochromatic layer. The base printing layer 52 may be a monochromatic layer of constant thickness. The base printing layer 52 may be, for example, a uniform white layer. The base printing layer 52 is located behind the picture printing layer 51, allowing the picture printing layer 51 to display a picture vividly and clearly. The viewer can observe the picture of the picture printing layer 51 vividly and clearly.
[0129] 1, the picture-printed layer 51 is located between the transparent substrate 30 and the base printed layer 52 in a first direction D1, which is the stacking direction. The printed matter 20 displays the picture of the picture-printed layer 51 facing a first side in the first direction D1. An observer observes the picture of the picture-printed layer 51 through the transparent substrate 30.
[0130] In the illustrated example, the transparent substrate 30 covers the printed layer 50 and the picture printed layer 51. Therefore, the transparent substrate 30 can protect the printed layer 50 and the picture printed layer 51. In other words, the transparent substrate 30 can prevent damage and deterioration of the picture.
[0131] As shown in FIG. 1, the base printing layer 52 may be provided only on the picture printing layer 51. The peripheral edge 52a of the base printing layer 52 may be separated from the peripheral edge 51a of the picture printing layer 51. According to the example shown in FIG. 1, when the printed matter 20 is observed from the surface 21, the base printing layer 52 is concealed by the picture printing layer 51. Since the base printing layer 52 is not observed at the peripheral edge 51a of the picture printing layer 51, the outline of the picture becomes clear. The viewer can clearly see the picture displayed by the picture printing layer 51. The aesthetic value of the printed matter 20 can be improved.
[0132] As described above, an upper limit is set for the transmission haze of the transparent substrate 30. By setting the transmission haze of the transparent substrate 30 to 3.0% or less, it is possible to effectively prevent the transparent substrate 30 from degrading the pattern. Therefore, an observer can see through the transparent substrate 30 and clearly and vividly observe the pattern of the printing layer 50.
[0133] The total light transmittance of the transparent substrate 30 may be set to the above-mentioned lower limit. The above-mentioned lower limit of the total light transmittance can further improve the transparency of the transparent substrate 30. An observer can observe the pattern of the printing layer 50 more vividly and clearly through the transparent substrate 30.
[0134] The above-mentioned upper limit may be set for the arithmetic mean roughness Sa on the first surface 31 of the transparent substrate 30. The above-mentioned upper limit of the arithmetic mean roughness Sa can further improve the transparency of the transparent substrate 30. An observer can see through the transparent substrate 30 and observe the pattern of the printed layer 50 more vividly and clearly.
[0135] Similarly, the above-mentioned upper limit may be set for the arithmetic mean roughness Sa on the second surface 32 of the transparent substrate 30. The above-mentioned upper limit of the arithmetic mean roughness Sa can further improve the transparency of the transparent substrate 30. An observer can see through the transparent substrate 30 and observe the pattern of the printing layer 50 more vividly and clearly.
[0136] Fig. 3A is a plan view showing a first printed matter 20A as an example of the printed matter 20. Fig. 3B is a plan view showing a second printed matter 20B as an example of the printed matter 20. Fig. 3A and Fig. 3B are each a plan view showing the printed matter 20 from a first side in a first direction D1.
[0137] 3A and 3B, the printed layer 50 is provided on a portion of the transparent substrate 30. Therefore, the observer can observe the back of the printed matter 20 in the region where the printed layer 50 is not provided. Since the transparent substrate 30 has excellent transparency, the observer can clearly observe the back of the printed matter 20 through the transparent substrate 30.
[0138] As mentioned in the Background Art section, cel drawings were used in the production of animation in the past. Cel drawings are original drawings on a transparent celluloid substrate. Nowadays, digital drawing by computer has become widespread. Therefore, cel drawings are no longer used in the production of animation.
[0139] On the other hand, the printed matter 20 including the transparent substrate 30 and the printed layer 50 may have high commercial value among enthusiasts, fans, and enthusiasts due to the rarity of cel drawings. In order to satisfy the desires of enthusiasts, fans, and enthusiasts, it is important that the printed matter 20 has aesthetic value, and it is essential for the printed matter 20 that the transparent substrate 30 has high transparency. The printed matter 20 according to this embodiment, in which the transparent substrate 30 has high transparency, attracts enthusiasts, fans, and enthusiasts, and becomes a collection item for enthusiasts, fans, and enthusiasts.
[0140] The printed matter 20 can be observed behind through the area of the transparent substrate 30 that is not covered with the printing layer 50. Thus, like a traditional cel painting, the printed matter 20 can be handled in combination with another printed matter 20 and / or a picture object 60 including a design. The printed matter 20, together with the other printed matter 20 and / or the picture object 60 including a design, constitutes a printed matter combination 10. The printed matter combination 10 may include the printed matter 20 and another printed matter 20. The printed matter combination 10 may include the printed matter 20 and the picture object 60. The printed matter combination 10 may include the printed matter 20, another printed matter 20, and the picture object 60.
[0141] 4 and 5 show an example of a printed matter combination 10. The printed matter combination 10 shown in Fig. 4 and Fig. 5 includes a plurality of printed matters 20. As shown in Fig. 5, one printed matter 20 is overlapped with another printed matter 20 in the first direction D1. Each of the plurality of printed matters 20 includes a transparent substrate 30 and a printing layer 50.
[0142] The printed matter combination 10 shown in Figures 4 and 5 includes a first printed matter 20A shown in Figure 3A and a second printed matter 20B shown in Figure 3B. The first printed matter 20A and the second printed matter 20B are each a specific example of the printed matter 20.
[0143] In the printed matter combination 10 shown in Figures 4 and 5, one printed matter 20B is overlapped with another printed matter 20B such that the front surface 21 of one printed matter 20B contacts the back surface 22 of the other printed matter 20A. In other words, one printed matter 20A is overlapped with another printed matter 20B such that the back surface 22 of one printed matter 20A contacts the front surface 21 of the other printed matter 20B.
[0144] 4 and 5, in a printed matter combination 10 including a plurality of printed matters 20, the pattern of a printed matter 20 (second printed matter 20B) located in the back is observed through the transparent substrate 30 of a printed matter 20 (first printed matter 20A) located in the front. According to the printed matters 20 and printed matter combination 10 including a transparent substrate 30 having high transparency, the patterns included in each of the plurality of printed matters 20 can be observed simultaneously. In other words, a user can combine patterns in a unique way and can enjoy appreciating the plurality of patterns that have been uniquely combined.
[0145] "Located in front" means that it is located close to the observer (user) in the first direction D1. "Located in front" means that of two printed materials 20 overlapped in the first direction D1, the printed material 20 that is located close to the observer (user) in the first direction D1. "Located behind" means that it is located far from the observer (user) in the first direction D1. "Located behind" means that of two printed materials 20 overlapped in the first direction D1, the printed material 20 that is located far from the observer (user) in the first direction D1.
[0146] 4 and 5, the printed product combination 10 may include three printed products 20. The printed product combination 10 may include four or more printed products 20.
[0147] 6 is a plan view showing one specific example of a patterned object 60 that is placed over the printed matter 20. The patterned object 60 includes a pattern. The patterned object 60 displays a pattern. The patterned object 60 does not have to include a transparent area. The patterned object 60 may include a transparent area. The patterned object 60 may have a pattern formed over its entire area. The patterned object 60 may have a pattern formed only in a portion of it.
[0148] The patterned object 60 may be a printed paper. The printed paper may include a printing base material and a pattern printed layer on the printing base material. The printing base material is not particularly limited and may be paper, a resin film, glass, or a wooden board. Unlike the transparent base material 30, the printing base material does not have to be transparent. The pattern printed layer may be configured in the same manner as the printing layer 50. The patterned object 60 may be photographic paper. The patterned object 60 may be a photograph.
[0149] 7 and 8 show another example of the printed matter combination 10. The printed matter combination 10 shown in Fig. 7 and Fig. 8 includes a printed matter 20 and a picture object 60. As shown in Fig. 8, the printed matter 20 is overlapped with the picture object 60 in the first direction D1. As shown in Fig. 8, the printed matter 20 is overlapped with the picture object 60 such that the back surface 22 of the printed matter 20 is in contact with the picture object 60.
[0150] 7 and 8 includes a first printed matter 20A, a second printed matter 20B, and a picture object 60. The second printed matter 20B is located between the first printed matter 20A and the picture object 60 in the first direction D1.
[0151] In the printed matter combination 10 shown in Figures 7 and 8, the pattern of the patterned object 60 is observed through the transparent substrate 30 of the first printed matter 20A and the transparent substrate 30 of the second printed matter 20B. The pattern of the second printed matter 20B is observed through the transparent substrate 30 of the first printed matter 20A. With the printed matter 20 and printed matter combination 10 including the transparent substrate 30 with high transparency, the patterns included in the printed matter 20 and the patterned object 60 can be observed simultaneously. In other words, the user can combine patterns in their own way and enjoy appreciating the multiple patterns that have been combined in their own way.
[0152] 7 and 8, the print combination 10 may include a single print 20 along with the picture object 60. The print combination 10 may include three prints 20 along with the picture object 60. The print combination 10 may include four or more prints 20 along with the picture object 60.
[0153] In the examples shown in Figures 4, 5, 7, and 8, the multiple patterns displayed by the printed matter 20 and the picture object 60 included in the printed matter combination 10 do not overlap. In other words, the multiple patterns displayed by the printed matter combination 10 are shifted from each other in a direction perpendicular to the first direction D1. Two or more patterns displayed by the printed matter combination 10 may partially overlap each other.
[0154] In the printed product combination 10 in which two or more patterns partially overlap each other, a printed product 20 may be used whose anti-see-through index Nt according to the anti-see-through method B (instrumental method) has been adjusted as described above. The printed product 20 located in the foreground may have an anti-see-through index Nt according to the anti-see-through method B (instrumental method) of 85.0% or more in the area where the printed layer 50 is formed. According to this example, the printed product 20 located in the foreground can clearly display the pattern in the desired vivid color without being affected by the pattern of the printed product 20 located behind it.
[0155] In the printed matter combination 10 in which two or more patterns partially overlap each other, the base printing layer 52 is provided only on the pattern printing layer 51, and the peripheral edge 52a of the base printing layer 52 may be separated from the peripheral edge 51a of the pattern printing layer 51. According to this example, the base printing layer 52 is not observed between the two patterns that are displayed partially overlapping each other. Therefore, the two patterns can be observed without feeling strange.
[0156] The usage forms of the printed matter 20 and the printed matter combination 10 will be described. Figs. 9A to 14B are diagrams showing usage forms of the printed matter 20 and the printed matter combination 10. The usage forms shown in Figs. 9A to 14B can be applied to the printed matter combination 10 including a plurality of printed matters 20. The usage forms shown in Figs. 9A to 14B can be applied to the printed matter combination 10 including the printed matter 20 and the picture object 60. The usage forms shown in Figs. 9A to 14B can be applied to the printed matter combination 10 including a plurality of printed matters 20 and the picture object 60. In the usage forms shown in Figs. 9A to 14B, the number of printed matters 20 included in the printed matter combination 10 is not particularly limited.
[0157] As shown in Figures 9A and 9B, the printed matter combination 10 may include a fastener 71. The printed matter 20 and the picture object 60 included in the printed matter combination 10 may be fixed to each other using the fastener 71. As shown in Figures 3A and 3B, the printed matter 20 may have a hole 24. As shown in Figure 6, the picture object 60 may have a hole 24. The hole 24 may penetrate the printed matter 20. The fastener 71 passes through the hole 24 to fix the printed matter 20 and the picture object 60 to each other.
[0158] In the illustrated example, three holes 24 are provided in each of the printed matter 20 and the picture object 60. The printed matter combination 10 secures the printed matter 20 and the picture object 60 to each other with three fasteners 71. The printed matter 20 and the picture object 60 have a rectangular shape in a plan view. The three holes 24 are provided near the upper edges of the printed matter 20 and the picture object 60. The three holes 24 are arranged along the upper edges. However, the arrangement and number of the holes 24 and the arrangement and number of the fasteners 71 may be changed.
[0159] As shown in FIG. 10A and FIG. 10B, the printed matter combination 10 may include a fixing tool 71 and a resin plate 72. The resin plate 72 has an elongated shape. The resin plate 72 is provided near the upper edge and extends along the upper edge. The fixing tool 71 passes through a hole in the resin plate 72 and further passes through the holes 24 in the printed matter 20 and the picture object 60. The fixing tool 71, together with the resin plate 72, fixes the printed matter 20 and the picture object 60 included in the printed matter combination 10 to each other. The printed matter combination 10 shown in FIG. 10A and FIG. 10B has a pair of resin plates 72. The printed matter 20 and the picture object 60 included in the printed matter combination 10 are sandwiched from both sides in the first direction D1 by the pair of resin plates 72. One of the pair of resin plates 72 can be omitted.
[0160] 9A to 10B, the printed matter 20 and the patterned object 60 are fixed to each other near their upper edges. Therefore, by turning over the printed matter 20 or the patterned object 60 included in the printed matter combination 10, the pattern or the combination of patterns displayed by the printed matter combination 10 can be changed.
[0161] As shown in FIG. 11A and FIG. 11B, the printed matter combination 10 may include a fixing device 71 and a resin plate 72. The resin plate 72 has a size that covers the entire surface of the printed matter 20 and the picture object 60. The printed matter combination 10 has a pair of resin plates 72. The printed matter 20 and the picture object 60 included in the printed matter combination 10 are sandwiched by the pair of resin plates 72 from both sides in the first direction D1. The fixing device 71 passes through the pair of resin plates 72 and fixes the pair of resin plates 72 to each other. In the example shown in FIG. 11A and FIG. 11B, the fixing device 71 does not pass through the printed matter 20 and the picture object 60. Therefore, it is possible to suppress the fixing device 71 from damaging the printed matter 20 and the picture object 60.
[0162] 11A and 11B, the resin plate 72 covers the printed matter 20 and the picture-patterned object 60 from both sides in the first direction D1. Therefore, the resin plate 72 can protect the printed matter 20 and the picture-patterned object 60. In other words, the resin plate 72 can suppress damage and deterioration of the picture.
[0163] As shown in FIG. 12A and FIG. 12B, the printed matter combination 10 may include a case 73. The case 73 includes a pair of resin plates 73a. The pair of resin plates 73a has a rectangular shape in a plan view. The pair of resin plates 73a are joined to each other on three sides. The pair of resin plates 73a form an opening leading to the inside on one side. As shown in FIG. 12A and FIG. 12B, the printed matter 20 and the picture object 60 are accommodated between the pair of resin plates 73a. The printed matter 20 and the picture object 60 are sandwiched by the pair of resin plates 73a from both sides in the first direction D1. The resin plate 73a has a size that covers the entire surface of the printed matter 20 and the picture object 60. The printed matter 20 and the picture object 60 can be inserted and removed from the case 73 by passing through the opening.
[0164] 12A and 12B, the resin plate 73a covers the printed matter 20 and the patterned object 60 from both sides in the first direction D1. Therefore, the resin plate 73a can protect the printed matter 20 and the patterned object 60. In other words, the resin plate 73a can suppress damage and deterioration of the pattern.
[0165] As shown in FIGS. 13A and 13B, the printed matter combination 10 may include a display device 75. The display device 75 includes a display frame 75a and a resin plate 75b. The resin plate 75b can be attached to the display frame 75a. The resin plate 75b can be removed from the display frame 75a. The printed matter 20 and the picture object 60 are housed between the display frame 75a and the resin plate 75b. The printed matter 20 and the picture object 60 are sandwiched from both sides in the first direction D1 by the display frame 75a and the resin plate 75b. The resin plate 75b has a size sufficient to cover the entire surfaces of the printed matter 20 and the picture object 60.
[0166] 13A and 13B, the resin plate 75b covers the printed matter 20 and the patterned object 60 from both sides in the first direction D1. Therefore, the resin plate 75b can protect the printed matter 20 and the patterned object 60. In other words, the resin plate 75b can suppress damage and deterioration of the pattern.
[0167] In the example shown in Fig. 10A to Fig. 13B, the resin plates 72, 73a, 75b may be transparent. In the printed matter combination 10 shown in Fig. 10A to Fig. 12B, the printed matter 20 and the patterned matter 60 are observed through the resin plates 72, 73a, 75b located in front of the printed matter 20 and the patterned matter 60. The transmission haze of the resin plates 72, 73a, 75b may be the same as the transmission haze of the transparent substrate 30 described above. The total light transmittance of the resin plates 72, 73a, 75b may be the same as the total light transmittance of the transparent substrate 30 described above. The material of the resin plates 72, 73a is not particularly limited. The resin plates 72, 73a, 75b may contain polyester, acrylic resin, polystyrene, polycarbonate, or glass as a main component.
[0168] 14A and 14B, the printed product combination 10 may include a bag 74. The printed product 20 may be handled while contained in the bag 74. For example, the printed product 20 may be distributed while contained in the bag 74, or may be sold while contained in the bag 74. The bag 74 used during distribution or sale may be transparent or non-transparent. The bag 74 may contain a polyolefin such as polyethylene or polypropylene as a main component.
[0169] As shown in the above examples of use, the printed matter 20 using the transparent substrate 30 can be treated as a printed matter combination 10 by combining it with a picture object 60 or another printed matter 20. If the transparency of the transparent substrate 30 is low, the picture behind the printed matter 20 in the printed matter combination 10 cannot be observed vividly and clearly, and the aesthetic value of the printed matter combination is reduced.
[0170] The transparent substrate 30 is also required to have good adhesion to the printed layer 50. If the adhesion between the transparent substrate and the printed layer is poor, the printed layer 50 cannot be formed on the transparent substrate 30. The printed matter 20 may be deformed (e.g., curved) when combined with a picture object 60 or another printed matter 20. If the adhesion between the transparent substrate 30 and the printed layer 50 is poor, the printed layer 50 may peel off from the transparent substrate 30. If the printed layer 50 peels off even partially, the aesthetic value of the printed matter 20 is significantly impaired.
[0171] Furthermore, the printed matter 20 may be viewed in combination with a picture object 60 or another printed matter 20. In this application, the printed matter 20 may be displayed in contact with the picture object 60 or another printed matter 20 using a fixture 71 or the like. The printed matter 20 may also be maintained in contact with a resin plate 72, 73a, 75b, or a bag 74. If the printed matter 20 is maintained in contact with another printed matter 20, a picture object 60, a resin plate 72, 73a, 75b, or a bag 74 for a long period of time, blocking may occur between the printed matter 20 and these members.
[0172] Blocking is a phenomenon in which a printed matter sticks to another member to which it is in close contact. If the printed matter is forcibly peeled off from the other member when blocking occurs, damage occurs to the printed matter 20, such as the peeling off of a part of the printed matter, for example, a part of the easy-adhesion layer or a part of the printing layer, the transfer of a part of the other member to the printed matter, or the scratching of the printed matter. If the printed matter 20 is damaged, the commercial value of the printed matter 20 is significantly reduced.
[0173] As described above, high transparency of the transparent substrate 30, adhesion between the transparent substrate 30 and the adhesive layer 40, and prevention of damage due to blocking are required for the printed matter 20. In the present embodiment, as described below, efforts are made to simultaneously satisfy these three requirements.
[0174] In this embodiment, the printed matter 20 includes a front surface 21 and a back surface 22. The printed matter 20 includes a transparent substrate 30 and a printed layer 50. The transparent substrate 30 includes a first surface 31 constituting the front surface 21, and a second surface 32 opposite to the first surface 31. The transparent substrate 30 includes a resin film 35 and an easy-adhesion layer 40 constituting the second surface 32. The printed layer 50 is located on a portion of the easy-adhesion layer 40 constituting the second surface 32. By forming the easy-adhesion layer 40 on the second surface 32 of the transparent substrate 30, the adhesion between the transparent substrate 30 and the printed layer 50 can be improved.
[0175] However, the easy-adhesion layer 40, together with the printed layer 50, constitutes the back surface 22 of the printed matter 20. The easy-adhesion layer 40 has the property of improving adhesion. Therefore, the back surface 22 of the printed matter 20 constituted by the easy-adhesion layer 40 is prone to blocking with another printed matter 20, a picture-patterned object 60, etc. Improving adhesion between the printed layer 50 and the transparent substrate 30 and suppressing blocking of the printed matter 20 are usually conflicting issues.
[0176] According to this embodiment, the easy-adhesion layer 40 includes not only the binder component 41 that can contribute to improving adhesion with the printing layer 50, but also the particles 42 held by the binder component 41. While the transmission haze of the transparent substrate 30 is set to 3.0% or less, the second surface 32 includes the convex portions 43 due to the particles 42. That is, the convex portions 43 are formed due to the particles 42. For example, the particles 42 exposed from the binder component 41 may form the convex portions 43. The binder component 41 may be raised on the particles 42 to form the convex portions 43.
[0177] Since the second surface 32 of the transparent substrate 30 includes the convex portion 43, the back surface 22 formed by the easy-adhesion layer 40 is prevented from coming into surface contact with another printed matter 20 or a picture-patterned object 60. Therefore, the back surface 22 formed by the second surface 32 of the easy-adhesion layer 40 is effectively prevented from blocking with another printed matter 20 or a picture-patterned object 60. Damage to the printed matter 20 due to blocking is prevented.
[0178] On the other hand, the adhesion between the printed layer 50 formed by printing and the transparent substrate 30 is improved by the adhesion layer 40. Furthermore, by thinning the thickness of the binder component 41 of the adhesion layer 40 for the purpose of improving adhesion to the printed layer 50 to such an extent that the convex portions 43 are formed, blocking between the adhesion layer 40 of the printed matter 20 and other members adjacent to the printed matter 20, such as another printed matter 20, a picture-patterned object 60, a resin plate, etc., can be suppressed.
[0179] As another means for suppressing blocking, it is possible to cover the easy-adhesion layer and the printed layer with a separate layer such as a coating layer and a dry laminate layer. Alternatively, it is possible to perform a surface treatment for suppressing adhesion on the printed matter, such as a fluorine coating. However, these treatments have an adverse effect on the printed matter's ability to display the image vividly and clearly.
[0180] In addition, the formation of the convex portion on the second surface may reduce transparency, in other words, the transmissive observation property of the pattern. In this embodiment, the transmissive haze of the transparent substrate 30 is maintained at 3.0% or less. By disposing the particles 42 in the vicinity of the surface layer portion forming the second surface 32 of the transparent substrate 30, the transmissive haze is kept at 3.0% or less, and the convex portion 43 caused by the particles 42 can be formed. That is, the transmissive haze can be sufficiently reduced while the convex portion 43 is formed. In other words, the transmissive haze is mainly due to the external haze caused by the convex portion 43, and the internal haze is reduced. As a result, the damage caused by blocking can be suppressed while the decrease in transparency is sufficiently suppressed.
[0181] In addition, by forming the convex portion 43, a gap can be formed between the back surface 22 of the printed matter 20 and a member adjacent to the printed matter 20. Therefore, even if a minute foreign matter gets mixed in, the foreign matter can be prevented from immediately damaging the back surface 22.
[0182] A printed material 20 according to the present embodiment (e.g., the second printed material 20B shown in FIGS. 5 and 8) that is used overlapping another printed material 20 with its front surface 21 in contact with its rear surface 22 may have the following feature (A). A printed material 20 according to the present embodiment (e.g., the first printed material 20A shown in FIG. 11B and the printed materials 20 shown in FIGS. 12B and 13B) that is used overlapping the resin plates 72, 73a, 75b with its front surface 21 in contact with the resin plates 72, 73a, 75b may have the following feature (A). (A): The easy-adhesion layer 40 is provided on only one surface of the resin film 35 , and the resin film 35 constitutes the first surface 31 .
[0183] As described above, the easy-adhesion layer 40 usually makes blocking more likely to occur. In feature (A), the easy-adhesion layer 40 is formed only on one of a pair of surfaces of the resin film 35. According to feature (A), when two printed matter 20 are superimposed, it is possible to prevent the easy-adhesion layer 40 of one printed matter 20 from coming into contact with the easy-adhesion layer of the other printed matter 20. Therefore, according to the printed matter 20 having feature (A), the occurrence of blocking with the other printed matter 20 can be effectively suppressed.
[0184] According to the feature (A), it is possible to prevent the easy-adhesion layer 40 of the printed matter 20 from coming into contact with the resin plates 72, 73a, 75b that are overlaid on the printed matter 20. The resin plates 72, 73a, 75b can come into contact with the resin film 35 that constitutes the front surface 21, rather than with the easy-adhesion layer 40 that constitutes the back surface 22. Therefore, according to the printed matter 20 having the feature (A), it is possible to effectively suppress the occurrence of blocking with the resin plates 72, 73a, 75b.
[0185] As described above, according to feature (A), it is possible to prevent the aesthetic value of printed matter 20, which is used by being overlapped with another printed matter 20, from being impaired by having front surface 21 contacting back surface 22 of the other printed matter 20. According to feature (A), it is possible to prevent the aesthetic value of printed matter 20, which is used by being overlapped with resin plates 72, 73a, 75b, from being impaired by having front surface 21 contacting resin plates 72, 73a, 75b.
[0186] The printed matter 20 according to the present embodiment (e.g., the first printed matter 20A shown in Figs. 5 and 8) used overlapping another printed matter 20 with the back surface 22 in contact with the front surface 21 of the other printed matter 20 may have the following feature (B). The printed matter 20 according to the present embodiment (e.g., the second printed matter 20B shown in Figs. 8 and 11B, and the printed matter 20 shown in Figs. 12B and 13B) used overlapping a picture-containing object 60 with the back surface 22 in contact with the picture-containing object 60 may have the following feature (B). The printed matter 20 according to the present embodiment (e.g., the printed matter 20 in Figs. 11B, 12B, and 13B when the picture-containing object 60 is omitted) used overlapping the resin plates 72, 73a, and 75a with the back surface 22 in contact with the resin plates 72, 73a, and 75a may have the following feature (B). (B): The printed matter 20 is resistant to a mandrel test using a mandrel with a diameter of 5 mm and a holding time of 30 seconds twice.
[0187] The mandrel test evaluates the adhesion between the printed layer 50 and the easy-adhesion layer 40. The adhesion between the printed layer 50 and the easy-adhesion layer 40 is evaluated as being stronger when the printed layer 50 and the easy-adhesion layer 40 can withstand a mandrel test using a mandrel with a smaller diameter. The printed matter may be able to withstand a mandrel test using a mandrel with a diameter of 2 mm and a holding time of 30 seconds x 2 times.
[0188] The mandrel test is performed as follows.
[0189] First, an evaluation print layer is formed on the second surface 32 formed by the easy-adhesion layer 40 of the transparent substrate 30. The evaluation print layer is formed by printing cyan, magenta, yellow, black, and white inks. The printing is inkjet printing. Cyan, magenta, yellow, and black all have an ink concentration of 100%. The ink concentration of white is 200%. In other words, white is obtained by forming a layer of 100% ink concentration twice. The inks of each color are the UV-curable ink "LUS-170" series manufactured by Mimaki Engineering Co., Ltd. UV-curable ink is ink that hardens when exposed to ultraviolet light. After printing, the UV-curable ink is fixed by exposure to ultraviolet light.
[0190] From the printed matter containing the transparent substrate and the evaluation printing layer, an evaluation sample with a long side of 100 (approximately ±1 mm) x a short side of 15 (approximately ±1 mm) is cut out using a single-edged trimming razor manufactured by Nisshin EM.
[0191] The evaluation sample is manually wound around a mandrel of a specified diameter with the short side parallel to the central axis of the mandrel. The evaluation sample is in contact with the outer circumferential surface of the mandrel over a central angle of 180 degrees. In other words, the evaluation sample is wound around the mandrel in a U-shape. The evaluation sample is held in this state around the mandrel for 30 seconds.
[0192] After 30 seconds have elapsed, remove the evaluation sample from the mandrel. After removing the evaluation sample from the mandrel, spread the evaluation sample flat for an appropriate period within a range of 1 to 10 seconds.
[0193] Thereafter, the evaluation sample is wound around the mandrel in the same manner as the previous time. That is, the evaluation sample is wound around the mandrel by hand so that the short side is parallel to the central axis of the mandrel. The evaluation sample is brought into contact with the outer peripheral surface of the mandrel over a range of a central angle of 180 degrees. That is, the evaluation sample is wound around the mandrel in a U-shape. The evaluation sample is held in the wound state around the mandrel for 30 seconds.
[0194] After that, the evaluation sample is removed from the mandrel and checked for peeling of the evaluation printing layer from the transparent substrate. Three evaluation samples are cut out from one evaluation object, and if no peeling occurs in any of the three evaluation samples after the mandrel test, it is determined that the sample has resistance to the mandrel test.
[0195] The test environment for the mandrel test shall be 23°C ± 2°C and 50% ± 5% relative humidity. The evaluation sample shall be placed in the test environment for 16 hours before the start of the test.
[0196] According to the feature (B), the adhesion between the printed layer 50 and the transparent substrate 30 can be improved. Therefore, even when the printed layer 50 of the printed matter 20 comes into contact with another member, or when the printed matter 20 is deformed, such as curved, in order to combine the printed matter 20 with another member, the printed layer 50 can be prevented from peeling off from the transparent substrate 30. The printed matter 20 having the feature (B) is suitable for a printed matter 20 that is used by being layered on another printed matter 20, with the back surface 22 being in contact with the front surface 21 of the other printed matter 20. The printed matter 20 having the feature (B) is suitable for a printed matter 20 that is used by being layered on a patterned object 60, with the back surface 22 being in contact with the patterned object 60 including a pattern. A printed matter 20 having characteristic (B) is suitable for a printed matter 20 that is used by overlapping with a resin plate 72, 73a, 75a with the back surface 22 in contact with the resin plate 72, 73a, 75a (for example, a printed matter 20 in which the picture object 60 is omitted in Figures 11B, 12B, and 13B).
[0197] As described above, according to feature (B), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping another printed matter 20 from being impaired by having the back surface 22 come into contact with the front surface 21 of the other printed matter 20. According to feature (B), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping the picture object 60 including a pattern from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a. According to feature (B), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping the resin plates 72, 73a, 75a from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a.
[0198] The printed matter 20 according to the present embodiment (e.g., the first printed matter 20A shown in Figs. 5 and 8) used overlapping another printed matter 20 with the back surface 22 in contact with the front surface 21 of the other printed matter 20 may have the following feature (C). The printed matter 20 according to the present embodiment (e.g., the second printed matter 20B shown in Figs. 8 and 11B, and the printed matter 20 shown in Figs. 12B and 13B) used overlapping a picture-containing object 60 with the back surface 22 in contact with the picture-containing object 60 may have the following feature (C). The printed matter 20 according to the present embodiment (e.g., the printed matter 20 in Figs. 11B, 12B, and 13B when the picture-containing object 60 is omitted) used overlapping the resin plates 72, 73a, and 75a with the back surface 22 in contact with the resin plates 72, 73a, and 75a may have the following feature (C). (C): The adhesion on the second surface is rated 2 or less by the cross-cut method.
[0199] The cross-cut test evaluates the adhesion of the printed layer and the easy-adhesion layer. The adhesion in the cross-cut test is evaluated on a six-point scale from "0" to "5." The lower the evaluation number, the higher the adhesion of the printed layer and the easy-adhesion layer. The adhesion on the second surface may be 1 or less, or 0, in the evaluation by the cross-cut test.
[0200] The cross-cut test is carried out as follows: In the cross-cut test, the conditions not described below are in accordance with JIS K5600-5-6:1999.
[0201] First, an evaluation printing layer is formed on the second surface 32 constituted by the easy-adhesion layer 40 of the transparent substrate 30. The evaluation printing layer is prepared in the same manner as the evaluation printing layer described in the method for preparing the evaluation sample used in the mandrel test described above.
[0202] The cut interval is 2 mm, and 11 cuts are made along two perpendicular directions. 2Each crosscut has an area of approximately 2 mm by approximately 2 mm. The cutting is performed manually. A single blade cutting tool is used for cutting.
[0203] Next, place the adhesive tape on the cross-cut portion. Then, rub the tape against the evaluation print layer with a finger to bring the tape into contact with the cross-cut portion of the evaluation print layer. Next, as specified in JIS K5600-5-6:1999, grab the end of the tape at an angle close to 60° and remove it from the evaluation print layer in 0.5 seconds to 1.0 seconds. The tape used is "Cellotape (registered trademark)" (24 mm wide, 0.053 mm thick, adhesive strength 4.74 N / 10 mm) manufactured by Nichiban Co., Ltd.
[0204] The cross-cut areas transferred to the tape are then observed to confirm which of the classifications 0 to 5 specified in JIS K5600-5-6:1999 each sample falls into. Three evaluation samples are cut out from one evaluation object, and the largest classification among the test results of the three evaluation samples after the cross-cut test is determined as the classification of that evaluation object.
[0205] The test environment for the cross-cut method test shall be a temperature of 23°C ± 2°C and a relative humidity of 50% ± 5%. The evaluation sample shall be placed in the test environment for 16 hours before the start of the test.
[0206] According to the feature (C), the adhesion between the printed layer 50 and the transparent substrate 30 can be improved. Therefore, even when the printed layer 50 of the printed matter 20 comes into contact with another member, or when the printed matter 20 is deformed, such as curved, in order to be combined with another member, the printed layer 50 can be prevented from peeling off from the transparent substrate 30. The printed matter 20 having the feature (C) is suitable for a printed matter 20 that is used by being layered on another printed matter 20, with the back surface 22 being in contact with the front surface 21 of the other printed matter 20. The printed matter 20 having the feature (C) is suitable for a printed matter 20 that is used by being layered on a patterned object 60, with the back surface 22 being in contact with the patterned object 60 including a pattern. A printed matter 20 having characteristic (C) is suitable for a printed matter 20 that is used by overlapping with a resin plate 72, 73a, 75a so that the back surface 22 is in contact with the resin plate 72, 73a, 75a (for example, a printed matter 20 in which the picture object 60 is omitted in Figures 11B, 12B, and 13B).
[0207] As described above, according to feature (C), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping another printed matter 20 from being impaired by having the back surface 22 come into contact with the front surface 21 of the other printed matter 20. According to feature (C), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping the picture object 60 including a pattern from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a. According to feature (C), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping the resin plates 72, 73a, 75a from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a.
[0208] The printed matter 20 according to the present embodiment (e.g., the first printed matter 20A shown in Figs. 5 and 8) used overlapping another printed matter 20 with the back surface 22 in contact with the front surface 21 of the other printed matter 20 may have the following feature (D). The printed matter 20 according to the present embodiment (e.g., the second printed matter 20B shown in Figs. 8 and 11B, and the printed matter 20 shown in Figs. 12B and 13B) used overlapping a picture-containing object 60 with the back surface 22 in contact with the picture-containing object 60 may have the following feature (D). The printed matter 20 according to the present embodiment (e.g., the printed matter 20 in Figs. 11B, 12B, and 13B when the picture-containing object 60 is omitted) used overlapping the resin plates 72, 73a, and 75a with the back surface 22 in contact with the resin plates 72, 73a, and 75a) may have the following feature (D). (D): The average thickness of the binder component 41 is 1.0 μm or less, and the average particle size of the particles 42 is 1.0 μm or less.
[0209] According to feature (D), the convex portions 43 formed by the particles 42 can be stably provided on the second surface 32 of the transparent substrate 30. Since the second surface 32 includes the convex portions 43, the back surface 22 of the printed matter 20 formed by the second surface 32 is effectively prevented from blocking with another printed matter 20, another picture object 60, the resin plates 72, 73a, 75a, etc.
[0210] The adhesion layer 40 improves the adhesion between the printed layer 50 formed by printing and the transparent substrate 30. Furthermore, by thinning the thickness of the binder component 41 of the adhesion layer 40 for the purpose of improving adhesion to the printed layer 50 to such an extent that the convex portions 43 are formed, blocking between the adhesion layer 40 of the printed matter 20 and other members adjacent to the printed matter 20, such as another printed matter 20, a picture-patterned object 60, a resin plate, etc., can be suppressed.
[0211] In particular, according to feature (D), extremely minute protrusions 43 can be provided on the second surface 32. By making the size of the protrusions 43 approximately the wavelength of visible light or less than the wavelength of visible light, scattering of visible light by the protrusions 43 can be effectively suppressed. Therefore, the transmission haze of the transparent substrate 30 can be reduced, and the transparency of the transparent substrate 30 can be improved. On the other hand, even the minute protrusions 43 can contribute to suppressing blocking of the easy-adhesion layer 40 with other members.
[0212] As described above, according to feature (D), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping another printed matter 20 from being impaired by having the back surface 22 come into contact with the front surface 21 of the other printed matter 20. According to feature (D), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping the picture object 60 including a pattern from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a. According to feature (D), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping the resin plates 72, 73a, 75a from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a.
[0213] The color difference ΔE of the transparent substrate 30 before and after the light resistance test may be 0.25 or less. The color difference ΔE is calculated by the following formula. ΔE = ((ΔL * ) 2 +(Δa * ) 2 +(Δb * ) 2 ) 1 / 2 In the formula, "ΔL * " is the difference between before and after the light resistance test. * a * b * L in color space * The difference between the values is the "Δa * " is the difference between before and after the light resistance test. * a * b * a in color system * The difference between the values is "Δb * " is the difference between before and after the light resistance test. * a * b * b in color system *It is the difference in values.
[0214] The transparent substrate 30 having a color difference ΔE of 0.25 or less before and after the light fastness test has excellent weather resistance. Therefore, the transparent substrate 30 can display the image vividly in the appropriate color for a long period of time. The user can enjoy observing the printed matter for a long period of time. The color difference ΔE can be reduced, for example, by including a weather resistance agent such as an ultraviolet absorber or a light stabilizer in the transparent substrate 30 or by using a material with high weather resistance for the transparent substrate 30.
[0215] The light resistance test is carried out under the following conditions.
[0216] First, an evaluation printing layer is formed on the second surface 32 constituted by the easy-adhesion layer 40 of the transparent substrate 30. The evaluation printing layer is prepared in the same manner as the evaluation printing layer described as the method for preparing the evaluation sample used in the mandrel test and cross-cut method test described above.
[0217] When evaluating the color difference of the transparent substrate 30 included in the printed matter 20, an evaluation print layer is formed on the back surface of the printed matter 20. In this example, the L * Value, a * value and b * The incident area on the first surface 31 when the value is measured is an area of the printed matter 20 on which the printed layer 50 is not formed.
[0218] In the light resistance test, the evaluation sample is placed in a test chamber set under the following conditions for 30 hours. ·Temperature: 36℃ ·Humidity 50%RH Black panel temperature 53℃ ·Irradiation conditions: 100,000lux / hour Test duration: 30 hours
[0219] L * Value, a * value, and b * The value is measured under the following conditions and method.
[0220] L for transparent substrate 30* a * b * In the color space. * Value, a * value, and b * Values are CIE 1976 L * a * b * It is defined in the color space L * Value, a * value and b * The value is measured by a spectrophotometer. * Value, a * value and b * The value is a value measured by reflected light with the first surface 31 of the transparent substrate 30 as the incident surface. White wood-free paper is placed behind the evaluation sample. In other words, the white wood-free paper is brought into contact with the second surface 32 of the transparent substrate 30 to be evaluated.
[0221] Using a 2° field of view, the reflectance is measured at 10 nm intervals in the range of 400 nm to 700 nm. * a * b * L in color space * Value, a * value and b * Measure the value. L * Value, a * value and b * The values are measured using a D65 light source.
[0222] L * Value, a * value and b * Before measuring the value, turn on the light source of the measuring device for 15 minutes to stabilize the light source output. * Value, a * value and b * The test environment for measuring the values is 23°C ± 2°C and 50% ± 5% relative humidity. The evaluation sample is placed in the test environment for 16 hours before the start of the test.
[0223] L * Value, a * value, and b *The L value is measured for each of three evaluation samples before the light fastness test. The arithmetic mean of the three measured values is the L value for the evaluation sample before the light fastness test. * Value, a * value, and b * value.
[0224] L * Value, a * value, and b * The L value is measured for three evaluation samples after the light fastness test. The arithmetic mean of the three measured values is the L value for the evaluation sample after the light fastness test. * Value, a * value, and b * value.
[0225] L before and after light resistance test * Value, a * value, and b * From the value, the color difference for the evaluation object is determined.
[0226] In the present embodiment described above, the printed matter 20 includes a front surface 21 and a back surface 22. The printed matter 20 includes a transparent substrate 30 and a printed layer 50. The transparent substrate 30 includes a first surface 31 constituting the front surface 21 and a second surface 32 facing the first surface 31. The transparent substrate 30 includes a resin film 35 and an easy-adhesion layer 40 constituting the second surface 32. The printed layer 50 is located on a portion of the second surface 32 and constitutes the back surface 22 together with a portion of the easy-adhesion layer 40. The easy-adhesion layer 40 includes a binder component 41 and particles 42 held by the binder component 41. The second surface 32 includes a convex portion 43 formed by the particles 42. The transparent substrate 30 has a transmission haze of 3.0% or less.
[0227] According to this embodiment, by providing the easy-adhesion layer 40 on a transparent substrate having a sufficiently low transmission haze, it is possible to ensure the adhesion between the transparent substrate 30 and the printed layer 50 while realizing high transparency. The second surface 32 formed by the easy-adhesion layer 40 includes a convex portion 43 formed by the particles 42. The second surface 32 formed by the easy-adhesion layer 40 is prevented from blocking with a member adjacent to the printed matter 20 by the convex portion 43. The second surface 32 formed by the easy-adhesion layer 40 is prevented from being scratched by foreign matter or the like by the convex portion 43. The easy-adhesion layer 40 and the convex portion 43 can be factors that deteriorate transparency, but the low transmission haze of the transparent substrate can absorb the effect of the deterioration of transparency of the printed matter 20. As a result, according to the printed matter 20 according to this embodiment, it is possible to simultaneously realize high transparency of the transparent substrate 30, adhesion between the transparent substrate 30 and the easy-adhesion layer 40, and damage suppression due to blocking. The printed matter 20 is capable of displaying images with high aesthetic value, and is therefore suitable for displaying images related to animation that is popular among enthusiastic fans, enthusiasts, and enthusiasts.
[0228] The printed matter 20 according to this embodiment may have one or more of the following configurations (A) to (D).
[0229] (A): The easy-adhesion layer 40 is provided on only one surface of the resin film 35 , and the resin film 35 constitutes the first surface 31 .
[0230] (B): The printed matter 20 is resistant to a mandrel test using a mandrel with a diameter of 5 mm and a holding time of 30 seconds twice.
[0231] (C): The adhesion on the second surface is rated 2 or less by the cross-cut method.
[0232] (D): The average thickness of the binder component 41 is 1.0 μm or less, and the average particle size of the particles 42 is 1.0 μm or less.
[0233] According to the feature (A), it is possible to prevent the aesthetic value of the printed matter 20, which is used by being overlapped with another printed matter 20, from being impaired by having the front surface 21 come into contact with the back surface 22 of the other printed matter 20. According to the feature (A), it is possible to prevent the aesthetic value of the printed matter 20, which is used by being overlapped with the resin plates 72, 73a, 75b, from being impaired by having the front surface 21 come into contact with the resin plates 72, 73a, 75b.
[0234] According to feature (B), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with another printed matter 20 from being impaired by having the back surface 22 come into contact with the front surface 21 of the other printed matter 20. According to feature (B), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with the picture-patterned object 60 including a pattern from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a. According to feature (B), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with the resin plates 72, 73a, 75a from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a.
[0235] According to feature (C), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with another printed matter 20 from being impaired by having the back surface 22 come into contact with the front surface 21 of the other printed matter 20. According to feature (C), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with the picture object 60 including a pattern from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a. According to feature (C), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with the resin plates 72, 73a, 75a from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a.
[0236] According to feature (D), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with another printed matter 20 from being impaired by having the back surface 22 come into contact with the front surface 21 of the other printed matter 20. According to feature (D), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with the picture-patterned object 60 including a pattern from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a. According to feature (D), it is possible to prevent the aesthetic value of the printed matter 20 used by overlapping with the resin plates 72, 73a, 75a from being impaired by having the back surface 22 come into contact with the resin plates 72, 73a, 75a.
[0237] Although the present embodiment has been described with reference to specific examples, the above-mentioned specific examples do not limit the present embodiment. The above-mentioned embodiment can be embodied in various other specific examples, and various omissions, substitutions, changes, additions, etc. can be made without departing from the spirit of the embodiment. EXAMPLES
[0238] The present disclosure will be described in more detail with reference to examples, but the present disclosure is not limited to the following examples.
[0239] <<<1. Creation of printed matter>>> Transparent substrates according to Examples 1 and 2 and Comparative Examples 1 to 6 were produced.
[0240] <<Example 1>> The commercially available transparent substrate according to Example 1 included a resin film and an easy-adhesion layer. The resin film constituted the first surface of the transparent substrate. The easy-adhesion layer was formed on one surface of the resin film and was in contact with the resin film. The easy-adhesion layer constituted the second surface of the transparent substrate.
[0241] In the transparent substrate according to Example 1, the resin film was made of polyethylene terephthalate and had a thickness of 100 μm.
[0242] In the transparent substrate according to Example 1, the easy-adhesion layer contained a binder component and silica particles. The second surface of the transparent substrate contained protrusions formed by particles. The binder component was a resin. The average particle diameter of the silica particles was 20 nm or more and 70 nm or less. The average particle diameter was measured multiple times. The thickness of the easy-adhesion layer was 20 nm or more and 30 nm or less.
[0243] <<Example 2>> The commercially available transparent substrate according to Example 2 included a resin film and an easy-adhesion layer. The resin film constituted the first surface of the transparent substrate. The easy-adhesion layer was formed on one surface of the resin film and was in contact with the resin film. The easy-adhesion layer constituted the second surface of the transparent substrate.
[0244] In the transparent substrate according to Example 2, the resin film was made of polyethylene terephthalate and had a thickness of 100 μm.
[0245] In the transparent substrate according to Example 2, the easy-adhesion layer contained a binder component and silica particles. The second surface of the transparent substrate contained protrusions formed by particles. The binder component was a resin. The average particle diameter of the silica particles was 100 nm or more and 400 nm or less. The average particle diameter was measured multiple times. The thickness of the easy-adhesion layer was 70 nm or more and 80 nm or less.
[0246] <<Comparative Example 1>> The commercially available transparent substrate according to Comparative Example 1 included a first easy-adhesion layer, a resin film, and a resin layer in this order. The first easy-adhesion layer, the resin film, and the resin layer were located in this order from the first surface to the second surface in the first direction. The first easy-adhesion layer was formed on the other surface of the resin film and was in contact with the resin film. The first easy-adhesion layer constituted the first surface of the transparent substrate. The resin layer was formed on one surface of the resin film and was in contact with the resin film.
[0247] In the transparent substrate according to Comparative Example 1, the resin film was made of polyethylene terephthalate and had a thickness of 125 μm.
[0248] In the transparent substrate according to Comparative Example 1, the first easy-adhesion layer contained a binder component. The binder component was a resin. The first easy-adhesion layer did not contain particles. The first surface constituted by the first easy-adhesion layer did not contain a convex portion. The average thickness of the first easy-adhesion layer was 40 μm.
[0249] In the transparent substrate according to Comparative Example 1, the resin layer contained a binder component and silica particles. The binder component was a resin. The average particle diameter of the silica particles was about 60 nm. The thickness of the easy-adhesion layer was about 86 nm.
[0250] <<Comparative Example 2>> The commercially available transparent substrate according to Comparative Example 2 included a resin film and an easy-adhesion layer. The resin film constituted the first surface of the transparent substrate. The easy-adhesion layer was formed on one surface of the resin film and was in contact with the resin film. The easy-adhesion layer constituted the second surface of the transparent substrate.
[0251] In the transparent substrate according to Comparative Example 2, the resin film was made of polyethylene terephthalate and had a thickness of 100 μm.
[0252] The easy-adhesion layer contained a binder component. The binder component was a resin. The easy-adhesion layer did not contain particles. The second surface formed by the easy-adhesion layer did not contain any convex portions. The average thickness of the easy-adhesion layer was 25 μm.
[0253] <<Comparative Example 3>> The transparent substrate according to Comparative Example 3 was E5100 available from Toyobo Co., Ltd. The transparent substrate according to Comparative Example 3 was a resin film having one surface subjected to a corona treatment. The resin film was made of polyethylene terephthalate. The thickness of the resin film was 100 μm.
[0254] <<Comparative Example 4>> The transparent substrate according to Comparative Example 4 was E5101 available from Toyobo Co., Ltd. The transparent substrate according to Comparative Example 4 was a resin film having one surface subjected to a corona treatment. The resin film was made of polyethylene terephthalate. The thickness of the resin film was 100 μm.
[0255] <<Comparative Example 5>> The transparent substrate according to Comparative Example 5 was T60 available from Toray Industries, Inc. The transparent substrate according to Comparative Example 5 was a resin film that had not been subjected to a surface treatment. The resin film was made of polyethylene terephthalate. The thickness of the resin film was 150 μm.
[0256] <<Comparative Example 6>> The transparent substrate according to Comparative Example 6 was T60 available from Toray Industries, Inc. The transparent substrate according to Comparative Example 6 was a resin film that had not been subjected to a surface treatment. The resin film was made of polyethylene terephthalate. The thickness of the resin film was 100 μm.
[0257] <<<2. Measurement and Evaluation>>> Measurements, tests, and evaluations of the printed matter of the examples and comparative examples were carried out as described below. The environment in which the measurements, tests, and evaluations were carried out was set to a temperature of 23°C ± 2°C and a relative humidity of 50% ± 5%, unless otherwise specified. Before the start of the measurements, tests, and evaluations, the evaluation samples were placed in the above-mentioned environment for 16 hours. The evaluation samples were visually checked for the absence of any abnormalities such as dust or scratches.
[0258] <<2-1. Total light transmittance>> Evaluation samples measuring 5-6 cm x 5-6 cm were cut out from the transparent substrates according to the examples and comparative examples. The total light transmittance (%) of the transparent substrates according to each example was measured using the method described above. A haze meter "HM-150" manufactured by Murakami Color Research Laboratory was used to measure the total light transmittance. The samples were placed so as to cover the entire area of a 20φ measurement window of the measurement device. The measurement results of the total light transmittance are shown in the "Total Light Transmittance" column of Table 1.
[0259] <<2-2.Transmission haze>> Evaluation samples measuring 5-6 cm x 5-6 cm were cut out from the transparent substrates according to the examples and comparative examples. The transmission haze (%) of the transparent substrates according to each example was measured using the method described above. A haze meter "HM-150" manufactured by Murakami Color Research Laboratory was used to measure the transmission haze. The samples were placed so as to cover the entire area of a 20φ measurement window of the measurement device. The measurement results of the transmission haze are shown in the "Transmission Haze" column of Table 1.
[0260] <<2-3. Mandrel test>> A mandrel test was carried out as described above.
[0261] First, a print layer for evaluation was formed on the second surface of the transparent substrate of each of the examples and the comparative examples to obtain a print of each example. The print layer for evaluation was produced by the method described above. An evaluation sample of 100 mm x 15 mm was cut out from the print of each example. A single-edged trimming razor manufactured by Nissin EM Co., Ltd. was used to cut out the evaluation sample.
[0262] The mandrel test was carried out on the evaluation samples according to each example by the method described above. For the mandrel test, a cylindrical mandrel set / stand "Model 1500" manufactured by Elcometer was used. Mandrels with a diameter of 5 mm and a diameter of 2 mm were used for the mandrel test.
[0263] The mandrel test results of the printed matter of each example were evaluated using the method described above. The evaluation results are shown in the "Mandrel" column of Table 1. Examples that were resistant to the mandrel test are indicated with an "A" in the "Mandrel" column. Examples that were not resistant to the mandrel test are indicated with a "B" in the "Mandrel" column. Note that the results using a mandrel with a diameter of 5 mm and the results using a mandrel with a diameter of 2 mm were evaluated to be the same.
[0264] <<2-4. Cross-cut method test>> A test was carried out by the cross-cut method as described above.
[0265] First, a printed layer for evaluation was formed on the second surface of the transparent substrate of each of the examples and the comparative examples, thereby obtaining a printed matter of each example. The printed layer for evaluation was produced by the method described above.
[0266] Next, the evaluation printing layer was cut into 400 mm 2 100 cross-cuts were made in the area. The single blade cutting tool used was an OLFA universal M-thick type (blade thickness: 0.45 mm).
[0267] Thereafter, the cross-cut portion was brought into contact with tape by the method described above, and then the tape was peeled off from the cross-cut portion. The tape used was "Scotch tape" manufactured by Nichiban Co., Ltd. (24 mm wide, 0.053 mm thick, adhesive strength 4.74 N / 10 mm).
[0268] Next, the test results of the printed matter of each example were evaluated by the cross-cut method using the method described above. The evaluation results of transmission haze are shown in the "Cross-cut" column of Table 1. The "Cross-cut" column shows the classification to which each example falls among the classifications specified in JIS K5600-5-6:1999.
[0269] <<2-5. Arithmetic mean roughness Sa>> Evaluation samples were cut out from the transparent substrates according to the examples and the comparative examples. The size of the evaluation samples was set to a size that could maintain smoothness. Specifically, the size of the samples was set to within 2 cm x 5 cm. The arithmetic mean roughness Sa (μm) of the first surface of the transparent substrate according to each example was measured by the above-mentioned method. The arithmetic mean roughness Sa (μm) of the second surface of the transparent substrate according to each example was measured. The arithmetic mean roughness Sa (μm) was measured using a white light interference type layer cross section measuring device "Vert Scan R5500GML-A150-AC" manufactured by Ryoka Systems Co., Ltd. Other measurement conditions were as follows. Data analysis was performed using software vertscan2.0. A 1 / 3 inch XC-XC-HR50 manufactured by SONY was used as a CCD camera. Single-field measurement Objective lens: x10 (field of view: 469.71 x 352.28um) Tube lens: 1x Zoom Lens: No Relay Wavelength selection filter: 530 white Measurement mode: Wave mode View size: 640 x 480 pixels Polarizing filter: No Interpolation: None
[0270] The measured value of the arithmetic mean roughness Sa (μm) of the first surface is shown in "First surface roughness Sa" in Table 1. The measured value of the arithmetic mean roughness Sa (μm) of the second surface is shown in Table 1 as "Second surface roughness Sa."
[0271] <<2-6. Color difference before and after light fastness test>> The color difference before and after the light fastness test was measured by the method described above.
[0272] First, an evaluation sample for each example was obtained by forming an evaluation print layer on the second surface of the transparent substrate for each example and comparative example. The evaluation print layer was prepared in the same manner as in the preparation of the evaluation sample for the mandrel test and the cross-cut method test. For the evaluation sample for each example, L * Value, a * value, and b * The values were measured.
[0273] Next, a light resistance test was carried out on the evaluation samples according to the above-mentioned method. For the light resistance test, a "flat tray type xenon light resistance tester (Xe=3)" manufactured by Q-LAB was used. After that, the evaluation samples according to the examples after the light resistance test were * Value, a * value, and b * The values were measured.
[0274] L before and after light resistance test * Value, a * value, and b * The method for measuring the value is as described above. * Value, a * value, and b *The values were measured using a spectrophotometer "CM-700d" manufactured by Konica Minolta Sensing Co., Ltd. The high-quality paper placed behind the evaluation sample was "PPC paper High White" manufactured by Otsuka Shokai Co., Ltd.
[0275] L before and after light resistance test * Value, a * value, and b * The color difference ΔE was calculated from the measured values. The color difference ΔE values are shown in the "Color difference" column of Table 1.
[0276] <<2-7. Transparency of transparent substrates>> The transparent substrates according to Examples 1 and 2 and Comparative Examples 1 to 6 were used to evaluate the transparency of the printed layer.
[0277] A total of four samples measuring 5-6 cm x 5-6 cm were cut out from the transparent base material of each example to be evaluated. For each example, the four samples were stacked in the same orientation to prepare an evaluation sample. The fluorescent light was observed while it was on through the evaluation sample. The fluorescent light was installed at a height of 4 m from the floor. The evaluator's line of sight was set at a height of about 160 cm from the floor. The evaluator observed the fluorescent light at about 45° above the horizontal direction. The evaluation sample was placed at a position about 30 cm from the evaluator's eyes, close to the fluorescent light. The evaluation sample was placed so that the first surface faced the evaluator and the second surface faced the fluorescent light. The evaluators were 20 healthy individuals in their 30s with eyesight of 0.7 or higher.
[0278] The observation results were evaluated according to the following criteria. The evaluation results are shown in the "Transparency" column of Table 1.
[0279] A: 15 or more evaluators were able to clearly identify the outline of the fluorescent light. B: 5 to 14 evaluators were able to clearly identify the outline of the fluorescent light. C: Four or fewer evaluators were able to clearly identify the outline of the fluorescent light.
[0280] <<2-8. Adhesion of the printing layer>> The transparent substrates according to Examples 1 and 2 and Comparative Examples 4 to 6 were used to evaluate the adhesion of the printed layer.
[0281] A print layer for evaluation was formed on the second surface of the transparent substrate for each example to obtain a print for each example. The print layer for evaluation was prepared in the same manner as in preparing the evaluation samples used in the mandrel test and the cross-cut test. Evaluation samples with short sides of 15 mm and long sides of 40 mm were cut out from the obtained print. A universal M-thick cutter (blade thickness: 0.45 mm) manufactured by OLFA was used to cut out the evaluation samples.
[0282] As shown in FIG. 15, the evaluation sample 20S was folded so that the evaluation printed layer 53 was on the inside. The axis of folding passed through the center of the long side and was along the short side. The folded evaluation sample 20S was placed between two acrylic plates 81 and 82. A 500g weight 83 was placed on the acrylic plate 81 located above. The acrylic plate 82 located below was placed on a surface plate. That is, as shown in FIG. 15, the acrylic plate 82, the folded evaluation sample 20S, the acrylic plate 81, and the weight 83 were placed in this order from the surface plate upward.
[0283] The upper acrylic plate 81 was pressed toward the lower acrylic plate 82 by the weight 83. The weight 83 was placed on the acrylic plate 81 for one minute. After one minute had elapsed, the weight 83 was removed from the acrylic plate 81.
[0284] After removing the weight 83, the evaluation sample was spread out and peeling of the evaluation printed layer from the transparent substrate was examined. When evaluating whether or not the evaluation printed layer had peeled from the transparent substrate, the printed matter was observed from the front side. When evaluating whether or not the evaluation printed layer had peeled from the transparent substrate, the printed matter was also observed from the back side. FIG. 16 shows a photograph of the evaluation sample of Example 1 observed from the front side. FIG. 17 shows a photograph of the evaluation sample of Example 1 observed from the back side. FIG. 18 shows a photograph of the evaluation sample of Comparative Example 6 observed from the front side. FIG. 19 shows a photograph of the evaluation sample of Comparative Example 6 observed from the back side.
[0285] The evaluation results are shown in the "Adhesion of printed layer" column in Table 1. An "A" is indicated in the "Adhesion of printed layer" column for examples in which peeling of the evaluation printed layer did not occur. A "B" is indicated in the "Adhesion of printed layer" column for examples in which peeling of the evaluation printed layer occurred. For each example, adhesion tests were performed on three evaluation samples. If peeling of the evaluation printed layer occurred in even one of the three evaluation samples prepared for each example, it was evaluated as "peeling has occurred." If peeling of the evaluation printed layer did not occur in any of the three evaluation samples prepared for each example, it was evaluated as "no peeling has occurred."
[0286] The test environment was set to a temperature of 18° C. to 19° C. and a relative humidity of 50% to 55%. Before the start of the test, the evaluation sample was placed in the above-mentioned test environment for 16 hours.
[0287] <<2-9. Blocking on the back surface formed by an easy-adhesion layer>> Using the transparent substrates according to the examples and comparative examples, blocking on the back surface formed with the easy-adhesion layer was evaluated.
[0288] First, three evaluation transparent substrates 30S were cut out from the transparent substrate according to each example. The evaluation transparent substrate 30S was made into a rectangular shape with chamfered corners. The length of the long side of the rectangular shape was 85.5 mm. The length of the short side of the rectangular shape was 54.0 mm. The size of the evaluation transparent substrate 30S was a so-called card size.
[0289] Next, an evaluation pattern section 60S was prepared. The evaluation pattern section 60S was prepared by forming an evaluation pattern layer 61S on a matte coated paper 62. The evaluation pattern layer 61S was prepared by offset printing UV curable ink and fixing the UV curable ink at the time of printing by ultraviolet irradiation. As shown in FIG. 20, the evaluation pattern section 60S included first to ninth regions A1 to A9.
[0290] In the first area A1, black, cyan, magenta, and yellow inks were printed in that order. The ink density of cyan was set to 100%. The ink density of magenta, yellow, and black was set to 83%.
[0291] In the second area A2, black, cyan, magenta, and yellow inks were printed in that order. The ink density of magenta was 100%. The ink density of cyan, yellow, and black was 83%.
[0292] In the third area A3, black, cyan, magenta, and yellow inks were printed in that order. The ink density of yellow was set to 100%. The ink density of cyan, magenta, and black was set to 83%.
[0293] In the fourth area A4, black, cyan, magenta, and yellow inks were printed in that order. The ink density of black was 100%. The ink density of cyan, magenta, and yellow was 83%.
[0294] In the fifth area A5, only cyan was printed with 100% ink concentration. In the sixth area A6, only magenta was printed with 100% ink concentration. In the seventh area A7, only yellow was printed with 100% ink concentration. In the eighth area A8, only black was printed with 100% ink concentration. In the ninth area A9, no printing was performed. Therefore, the matte coated paper 62 was exposed in the ninth area A9 of the evaluation pattern portion 60S.
[0295] The inks used in the preparation of the evaluation pattern layer 61S were DC R2 DP Black S, DC R2 DP Indigo S, DC RTX2 Red N, and DC R2 DP Yellow L, all manufactured by DICG Corporation.
[0296] As shown in Fig. 21, an acrylic plate 92, an evaluation pattern portion 60S, an evaluation transparent substrate 30S, an evaluation transparent substrate 30S, an acrylic plate 91, and a weight 93 were stacked from bottom to top in this order and placed in a constant temperature chamber. The environment in the constant temperature chamber was set to a temperature of 60°C and a relative humidity of 90%. The standing time was 300 hours.
[0297] The thickness of the acrylic plate 91 was 3 mm. The acrylic plate 91 had the same shape in plan view as the evaluation pattern portion 60S and the evaluation transparent substrate 30S. The thickness of the acrylic plate 92 was 3 mm. The acrylic plate 92 had the same shape in plan view as the evaluation pattern portion 60S and the evaluation transparent substrate 30S. All three evaluation transparent substrates 30S were arranged so that the easy-adhesion layer 40 faced downward and the resin film 35 faced upward. The evaluation pattern portion 60S was arranged so that the evaluation pattern layer 61S faced upward and the matte coated paper 62 faced downward. The weight 93 was 500 g. A load of 500 g corresponds to the weight of about 10 books.
[0298] After 300 hours of standing, the three evaluation transparent substrates 30S and the evaluation picture portion 60S were removed from the constant temperature chamber. The presence or absence of blocking between the acrylic plate 91 and the evaluation transparent substrate 30S was examined. The presence or absence of blocking between two adjacent evaluation transparent substrates 30S was examined. The presence or absence of blocking between the evaluation transparent substrates 30S and the evaluation picture portion 60S was examined.
[0299] The evaluation results of blocking between the acrylic plate 91 and the evaluation transparent substrate 30S are shown in "Blocking P1" in Table 1. The evaluation results of blocking between two adjacent evaluation transparent substrates 30S are shown in "Blocking P2" in Table 1. The evaluation results of blocking between the evaluation transparent substrate 30S and the evaluation pattern portion 60S are shown in "Blocking P3" in Table 1.
[0300] If no blocking occurs, "Blocking P1", "Blocking P2", and "Blocking P3" are marked with "A". If blocking occurs, "Blocking P1", "Blocking P2", and "Blocking P3" are marked with "B".
[0301] For "Blocking P2," if blocking occurred on either of the two contact surfaces, it was rated as "B." For "Blocking P2," if blocking did not occur on either of the two contact surfaces, it was rated as "A."
[0302] <<2-10. Blocking of printed matter>> Using the transparent substrates according to the Examples and Comparative Examples, evaluation prints were produced. Blocking on the back surface of the evaluation print layer of the evaluation prints was evaluated.
[0303] First, three evaluation transparent substrates 30S were prepared for each example by the method described in <<2-9. Blocking on the back surface constituted by the easy-adhesion layer>>. An evaluation printed layer was formed on the easy-adhesion layer 40 of the evaluation transparent substrate 30S to obtain an evaluation printed matter including the evaluation transparent substrate 30S and the evaluation printed layer. The evaluation printed layer was produced by inkjet printing a UV-curable ink on the evaluation transparent substrate and fixing the UV-curable ink by ultraviolet irradiation during printing. A first evaluation printed matter, a second evaluation printed matter, and a third evaluation printed matter were produced for each example. The first evaluation printed matter, the second evaluation printed matter, and the third evaluation printed matter were different from each other in the pattern of the evaluation printed layer.
[0304] In the first evaluation printed matter 20SA, cyan, magenta, yellow, and black inks were printed on the second surface of the evaluation transparent substrate 30S. The cyan, magenta, yellow, and black inks were printed in the areas filled in in Fig. 22. The ink concentration of each of the cyan, magenta, yellow, and black colors was 100%.
[0305] Next, white ink was printed in the filled-in areas in FIG. 23. The thin lines shown in FIG. 23 were also printed using white ink. The line width of the thin lines was 0.15 mm. The white ink concentration was 200%. Specifically, white was printed once with an ink concentration of 200%. In this manner, the evaluation printed layer 50SA of the first evaluation printed matter 20SA was produced.
[0306] In the second evaluation printed matter 20SB, cyan, magenta, yellow, and black inks were printed in that order over the entire area of the second surface of the evaluation transparent substrate 30S. The ink concentration of cyan, magenta, yellow, and black was 100%. Next, white ink was printed over the entire area of the second surface of the evaluation transparent substrate 30S. The ink concentration of white was 200%. Specifically, white was printed once with an ink concentration of 200%. In this manner, the evaluation printed layer 50SB of the second evaluation printed matter 20SB was produced.
[0307] In the third evaluation printed matter 20SC, cyan, magenta, yellow, and black inks were printed in that order on the second surface of the evaluation transparent substrate 30S. The cyan, magenta, yellow, and black inks were printed in the areas that are filled in in Fig. 24. The ink concentration of cyan, magenta, yellow, and black was 100%.
[0308] Next, white ink was printed in the filled-in area in FIG. 25. The thin lines shown in FIG. 25 were also printed using white ink. The white ink concentration was 200%. Specifically, white was printed once with an ink concentration of 200%. In this way, the evaluation printed layer 50SC of the third evaluation printed matter 20SC was produced.
[0309] The inks of each color used to prepare the evaluation printing layer 50S were the UV-curable inks "LUS-170" series manufactured by Mimaki Engineering Co., Ltd.
[0310] As a result of the above, a first evaluation print 20SA, a second evaluation print 20SB, and a third evaluation print 20SC were obtained for each example.
[0311] As shown in Fig. 26, an acrylic plate 92, an evaluation pattern portion 60S, a first evaluation print 20SA, a second evaluation print 20SB, a third evaluation print 20SC, an acrylic plate 91, and a weight 93 were stacked from bottom to top in this order and placed in a constant temperature chamber. The environment in the constant temperature chamber was set to a temperature of 60°C and a relative humidity of 90%. The leaving time was 300 hours.
[0312] The acrylic plate 91, the acrylic plate 92, the weight 93, and the evaluation pattern part 60S were the same as those used in <<2-9. Blocking on the back surface constituted by the easy-adhesion layer>>. The three evaluation prints 20SA, 20SB, and 20SC were all arranged so that the evaluation print layer faced downward and the evaluation transparent substrate 30S faced upward. The evaluation pattern part 60S was arranged so that the evaluation pattern layer 61S faced upward and the matte coated paper 62 faced downward.
[0313] In the first evaluation print 20SA and the third evaluation print 20SC, a portion of the back surface was composed of an easy-adhesion layer. However, because the evaluation print layer 50S was thick, the easy-adhesion layer did not come into strong contact with the adjacent members in the thermo-hygrostat.
[0314] After 300 hours of standing, the three evaluation prints 20SA, 20SB, 20SC and the evaluation pattern portion 60S were removed from the constant temperature chamber. The presence or absence of blocking between the acrylic plate 91 and the first evaluation print 20SA was examined. The presence or absence of blocking between two adjacent evaluation prints 20S was examined. The presence or absence of blocking between the third evaluation print 20SC and the evaluation pattern portion 60S was examined.
[0315] The evaluation results of blocking between the acrylic plate 91 and the first evaluation printed matter 20SA are shown in "Blocking P4" in Table 1. The evaluation results of blocking between two adjacent evaluation printed matters 20S are shown in "Blocking P5" in Table 1. The evaluation results of blocking between the third evaluation printed matter 20SC and the evaluation picture portion 60S are shown in "Blocking P6" in Table 1.
[0316] If no blocking occurred, "Blocking P4," "Blocking P5," and "Blocking P6" were marked with an "A." If blocking occurred, "Blocking P4," "Blocking P5," and "Blocking P6" were marked with a "B."
[0317] For "Blocking P5," if blocking occurred on either of the two contact surfaces, it was rated as "B." For "Blocking P5," if blocking did not occur on either of the two contact surfaces, it was rated as "A."
[0318] <<2-11. Thickness of binder components and average particle size>> The thickness of the binder component and the average particle size of the particles were measured by the methods described above.
[0319] First, a section sample of the transparent substrate was prepared by the method described above. When preparing the section sample, a silicon embedding plate manufactured by Dosaka EM was used as the silicon embedding plate. The microtome used to prepare the sections was an "Ultramicrotome EM UC7" manufactured by Leica Microsystems. The cutting conditions using the diamond knife were "SPEED: 1.40 mm / s" and "FEED: 80 nm". A collodion film-attached mesh "Cat No; 651" manufactured by Nissin EM was used as the mesh for collecting the section sample.
[0320] As described above, the observation images of the sections of each example were obtained using a scanning transmission electron microscope. The scanning transmission electron microscope used was SU-9000 manufactured by Hitachi High-Tech Corporation. The imaging mode used was BFSTEM. The acceleration voltage was 30 kV. The images were captured at an emission current of 20 μA. The image data size was 1280 × 960 pixels. The measurement magnifications were 5,000 times, 10,000 times, 50,000 times, 75,000 times, and 100,000 times.
[0321] 2A is a photograph showing an observed image of a section for Example 1. FIG. 2B is a photograph showing an observed image of a section for Example 2.
[0322] Using the above-mentioned method, the thickness (μm) of the binder component and the average particle size (μm) of the particles were measured from the cross-sectional observation images for each example. The measurement results of the thickness (μm) of the binder component are shown in the "Thickness" column of Table 1. The measurement results of the average particle size (μm) of the particles are shown in the "Average Particle Size" column of Table 1.
[0323] [Table 1] [Explanation of symbols]
[0324] D1: first direction, D2: second direction, D3: third direction, 10: combination of printed matter, 20: printed matter, 20A: first printed matter, 20B: second printed matter, 20S: evaluation printed matter, 20SA: first evaluation printed matter, 20SB: second evaluation printed matter, 20SC: third evaluation printed matter, 21: front surface, 22: back surface, 24: hole, 30: transparent substrate, 30S: evaluation transparent substrate, 31: first surface, 32: second surface, 35: resin film, 40: easy-adhesion layer, 41: binder component, 42 : Particle, 43: Convex portion, 50: Printed layer, 50S: Evaluation printed layer, 50SA: First evaluation printed layer, 50SB: Second evaluation printed layer, 50SC: Third evaluation printed layer, 51: Picture printed layer, 51a: Edge, 52: Base printed layer, 52a: Edge, 53: Evaluation printed layer, 55: Resin plate, 60: Picture object, 71: Fixing device, 72: Resin plate, 73: Case, 73a: Resin plate, 74: Bag, 74a: Resin film, 75: Display device, 75a: Display frame, 75b: Resin plate
Claims
1. A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer, The easy-adhesion layer is provided on only one surface of the resin film and constitutes the second surface, The resin film constitutes the first surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes a protrusion due to the particles, The transparent substrate has a transmission haze of 3.0% or less; A printed matter that is used by being overlapped with another printed matter such that the front surface is in contact with the back surface of the other printed matter, or that is used by being overlapped with a resin plate such that the front surface is in contact with the resin plate.
2. A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes a protrusion due to the particles, The transparent substrate has a transmission haze of 3.0% or less; It has resistance to a mandrel test using a mandrel with a diameter of 5 mm and a holding time of 30 seconds x 2 times, The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
3. A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes a protrusion due to the particles, The transparent substrate has a transmission haze of 3.0% or less; The adhesion on the second surface is rated at 2 or less by a cross-cut method; The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
4. A printed matter having a front surface and a back surface, A transparent substrate and a printing layer are included. the transparent base material includes a first surface constituting the surface and a second surface opposite to the first surface, The transparent substrate includes a resin film and an easy-adhesion layer that constitutes the second surface, The printing layer is located on a portion of the second surface and constitutes the back surface together with a portion of the easy-adhesion layer, The easy-adhesion layer includes a binder component and particles held by the binder component, the second surface includes a protrusion due to the particles, The transparent substrate has a transmission haze of 3.0% or less; The average thickness of the binder component is 1.0 μm or less, The particles have an average particle size of 1.0 μm or less, The printed matter is used by being layered on another printed matter with the back surface in contact with the front surface of the other printed matter, used by being layered on a picture-containing object with the back surface in contact with the picture-containing object, or used by being layered on a resin plate with the back surface in contact with the resin plate.
5. The easy-adhesion layer is provided on only one surface of the resin film, The printed matter according to any one of claims 2 to 4, wherein the resin film constitutes the first surface.
6. 5. The printed matter according to claim 1, 3 or 4, which has resistance to a mandrel test using a mandrel having a diameter of 5 mm and a holding time of 30 seconds x 2 times.
7. The printed matter according to claim 1 , 2 or 4 , wherein the adhesion on the second surface is rated at 2 or less by a cross-cut method.
8. The average thickness of the binder component is 1.0 μm or less, The printed matter according to any one of claims 1 to 3, wherein the particles have an average particle size of 1.0 µm or less.
9. The printed matter according to any one of claims 1 to 4, wherein an average thickness of the binder component is smaller than an average particle diameter of the particles.
10. The first surface has an arithmetic average roughness Sa of 5.0 nm or less, The printed matter according to any one of claims 1 to 4, wherein the second surface has an arithmetic mean roughness Sa of 5.0 nm or less.
11. The color difference of the transparent substrate before and after the light resistance test ΔE=((ΔL * ) 2 + (Δa * ) 2 + (Δb * ) 2 ) 1/2 The printed matter according to any one of claims 1 to 4, wherein is 0.25 or less.
12. The printed matter according to any one of claims 1 to 4, wherein the resin film is mainly composed of a polyester or acrylic resin.
13. The printed matter according to any one of claims 1 to 4, wherein the anti-see-through index Nt in the region where the printed layer is formed is 85.0% or more according to the anti-see-through B method (instrumental method).
14. The printed matter according to any one of claims 1 to 4, wherein the printed layer has a thickness of 0.40 µm or more.
15. The printing layer includes a pattern printing layer having a pattern and a white, uniform base printing layer; The printed matter according to any one of claims 1 to 4, wherein the picture printed layer is located between the easy-adhesion layer and the base printed layer.
16. The undercoat printing layer is provided only on the picture printing layer, The printed matter according to claim 15 , wherein the periphery of the underprinting layer is spaced apart from the periphery of the picture printing layer.
17. The printed matter according to claim 15, wherein the undercoat printing layer has a thickness of 0.20 μm or more.
18. A printed matter according to any one of claims 1 to 4, A printed product combination comprising: another printed product according to any one of claims 1 to 4.
19. The printed matter combination according to claim 18, further comprising a plastic bag that contains the printed matter and the other printed matter.
20. The printed matter according to claim 1; A printed matter combination comprising the resin plate according to claim 1.
21. A printed matter according to any one of claims 2 to 4, A printed matter combination comprising the picture object according to any one of claims 2 to 4.
Citation Information
Patent Citations
Printed matter like picture-on-celluloid
JP1998297141A
Recording sheet with glossy film
JP2008213488A
Patterned film and display body
JP2014071220A
Laminate, method for manufacturing the same, and display
JP2020163856A
Cel display kit and cel display panel
JP3239038U