(Meth)acrylic acid copolymer
A (meth)acrylic acid-based copolymer with specific molecular weight and sulfonic acid group at the main chain end addresses the challenge of silica scale inhibition, offering effective silica scale suppression.
Patent Information
- Application Number
- JP2021010853
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-01-27
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2041-01-27
AI Technical Summary
Existing water treatment agents struggle to effectively inhibit silica scale, and there is a need for polymers made from easily available general-purpose monomers.
A (meth)acrylic acid-based copolymer containing structural units derived from (meth)acrylic acid and sulfonic acid (salt) group-containing monomers, with a weight average molecular weight of 28,000 to 56,000 and a sulfonic acid (salt) group at one end of the main chain, is developed.
The copolymer exhibits excellent ability to suppress silica scale precipitation, making it suitable as a water treatment agent or scale inhibitor.
Smart Images

Figure 0007586721000001 
Figure 0007586721000002 
Figure 0007586721000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a (meth)acrylic acid-based copolymer, and more particularly to a (meth)acrylic acid-based copolymer used for inhibiting scale such as silica scale. [Background technology]
[0002] For example, in geothermal power generation, industrial cooling water, and seawater desalination, the generation of scale such as calcium carbonate and silica can be a problem. For example, Patent Document 1 discloses that a copolymer having 2 mol % or more and 9 mol % or less of structural units derived from a sulfonic acid group-containing monomer, 91 mol % or more and 98 mol % or less of structural units derived from (meth)acrylic acid (salt), having a sulfonic acid (salt) group at at least one main chain end, and having a weight average molecular weight of 7,000 to 100,000, is excellent in calcium ion trapping ability and calcium carbonate dispersibility, and can be suitably used as a calcium carbonate scale inhibitor. For example, Patent Document 2 discloses that a copolymer having 5 mol % or more and 22 mol % or less of structural units derived from a sulfonic acid group-containing monomer, 78 mol % or more and 95 mol % or less of structural units derived from (meth)acrylic acid (salt), a sulfonic acid (salt) group at at least one main chain end, and a weight average molecular weight of 13,000 to 50,000 has excellent gel resistance and high calcium ion chelating ability, and therefore can be suitably used as a water treatment agent such as a scale inhibitor. For example, Patent Document 3 discloses that a copolymer containing 16 mol % or more and 24 mol % or less of structural units derived from a sulfonic acid group-containing monomer and 76 mol % or more and 84 mol % or less of structural units derived from (meth)acrylic acid (salt), having a sulfonic acid (salt) group at at least one main chain end and having a weight average molecular weight of 1,000 to 18,000, has excellent gel resistance and high calcium ion chelating ability, and therefore can be suitably used as a water treatment agent such as a scale inhibitor. For example, Patent Document 4 discloses that the copolymer described in the invention improves the dispersibility of hydrophobic particles and also exhibits excellent chelating ability for calcium ions, thereby enabling it to exhibit extremely good scale prevention ability for the piping and inside of geothermal power generation equipment, and therefore can be suitably used as a scale inhibitor for geothermal power generation equipment. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication No. 2014 / 054707 [Patent Document 2] JP 2012-188586 A [Patent Document 3] International Publication No. 2013 / 147171 [Patent Document 4] JP 2016-064382 A Summary of the Invention [Problem to be solved by the invention]
[0004] As described above, water treatment agents such as scale inhibitors have been proposed, but there is a demand for further improving the silica scale inhibition ability, and there has been a demand for a silica scale inhibitor that is applicable to silica scale prevention in various water treatment applications and is made of a polymer produced from a general-purpose monomer that is easily available.The present invention aims to provide a (meth)acrylic acid-based copolymer that has excellent silica scale inhibition ability and can be suitably used, for example, as a silica scale inhibitor. [Means for solving the problem]
[0005] The present inventors have conducted various investigations to achieve the above object and have arrived at the present invention. That is, the (meth)acrylic acid-based copolymer of the present disclosure is a copolymer containing structural units derived from (meth)acrylic acid (salt) and structural units derived from a sulfonic acid (salt) group-containing monomer, in which the sulfonic acid (salt) group-containing monomer accounts for 13 mol % or more relative to 100 mol % of structures derived from all monomers, the weight average molecular weight of the copolymer is 28,000 or more and 56,000 or less, and at least one main chain end of the copolymer is a sulfonic acid (salt) group. Effect of the Invention
[0006] The (meth)acrylic acid-based copolymer of the present disclosure exhibits good suppression ability against scale precipitation of silica components, etc. Therefore, the (meth)acrylic acid-based copolymer of the present disclosure can be preferably used as a water treatment agent used for suppressing scale such as silica scale, or as a scale inhibitor. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] The present invention will be described in detail below. In addition, a combination of two or more of the individual preferred embodiments of the present invention described below is also a preferred embodiment of the present invention.
[0008] [(Meth)acrylic acid-based copolymer of the present disclosure] The (meth)acrylic acid-based copolymer of the present disclosure contains a structural unit derived from (meth)acrylic acid (salt) and a structural unit derived from a monomer containing a sulfonic acid (salt), the monomer containing a sulfonic acid (salt) group is 13 mol% or more relative to 100 mol% of the structures derived from all monomers, the weight average molecular weight of the copolymer is 28000 or more and 56000 or less, and at least one main chain end of the copolymer is a sulfonic acid (salt) group. The above copolymer may be referred to as the copolymer of the present disclosure.
[0009] <Structural unit derived from (meth)acrylic acid (salt)> In this disclosure, (meth)acrylic acid refers to acrylic acid, methacrylic acid, and salts thereof. The above salt is not particularly limited, but examples thereof include alkali metal salts, alkaline earth metal salts, transition metal salts, and ammonium salts. In the present disclosure, the structural unit derived from (meth)acrylic acid (salt) refers to a structural unit in which the carbon-carbon double bond of (meth)acrylic acid (salt) is replaced with a carbon-carbon single bond. For example, if acrylic acid is CH2=CH(COOH), the structural unit derived from acrylic acid can be represented as -CH2-CH(COOH)-. The structural unit derived from (meth)acrylic acid (salt) can be formed, for example, by radical polymerization of (meth)acrylic acid (salt). Note that the structural unit derived from (meth)acrylic acid (salt) is not limited to a structural unit formed by polymerization of (meth)acrylic acid (salt), as long as it has the same structure as the structure in which the carbon-carbon double bond of (meth)acrylic acid (salt) is replaced with a carbon-carbon single bond, and may be, for example, a structural unit formed by a post-reaction after polymerization.
[0010] The content of the structural unit derived from (meth)acrylic acid (salt) in the copolymer of the present disclosure is preferably 50 mol% or more, more preferably 60 mol% or more, and even more preferably 70 mol% or more, based on 100 mol% of the structural units derived from all monomers constituting the copolymer of the present disclosure. Also, it is preferably 87 mol% or less, more preferably 86 mol% or less, and even more preferably 82 mol% or less. The content of the structural unit derived from the (meth)acrylic acid (salt) is calculated in terms of (meth)acrylic acid. The term "in terms of (meth)acrylic acid" means that even if the structural unit derived from (meth)acrylic acid (salt) is a structural unit derived from a (meth)acrylic acid salt, the mass is calculated as (meth)acrylic acid. By being in the above range, the silica scale inhibition ability of the water treatment agent or scale inhibitor of the present disclosure tends to be improved.
[0011] <Structural unit derived from monomer containing sulfonic acid (salt) group> In the present disclosure, a sulfonic acid (salt) group-containing monomer refers to a compound that contains at least one carbon-carbon double bond and a sulfonic acid (salt) group. The at least one carbon-carbon double bond is usually radically polymerizable. The above salt is not particularly limited, but examples thereof include alkali metal salts, alkaline earth metal salts, transition metal salts, and ammonium salts. In the present disclosure, the structural unit derived from a sulfonic acid (salt) group-containing monomer refers to a structural unit in which at least one carbon-carbon double bond of a sulfonic acid (salt) group-containing monomer is replaced with a carbon-carbon single bond. Note that the structural unit derived from a sulfonic acid (salt) group-containing monomer may have the same structure as the structure in which at least one carbon-carbon double bond of a sulfonic acid (salt) group-containing monomer is replaced with a carbon-carbon single bond, and is not limited to a structural unit formed by polymerization of a sulfonic acid (salt) group-containing monomer, and may be, for example, a structural unit formed by a post-reaction after polymerization. Examples of sulfonic acid (salt) group-containing monomers include vinyl sulfonic acid and its salts, styrene sulfonic acid and its salts, (meth)allyl sulfonic acid and its salts, 3-(meth)allyloxy-2-hydroxypropanesulfonic acid and its salts, 3-(meth)allyloxy-1-hydroxypropanesulfonic acid and its salts, 2-(meth)allyloxyethylenesulfonic acid and its salts, and 2-acrylamido-2-methylpropanesulfonic acid and its salts.
[0012] For example, a structural unit derived from a sulfonic acid (salt) group-containing monomer is represented by the following general formula (1). TIFF0007586721000001.tif37114 (In general formula (1), R1 represents a hydrogen atom or a methyl group, and X and Y each independently represent a hydroxyl group or a sulfonic acid (salt) group (provided that at least one of X and Y represents a sulfonic acid (salt) group. Sulfonic acid (salt) refers to sulfonic acid and sulfonate salts. The salts of sulfonate salts are metal salts, ammonium salts, and organic amine salts. Specifically, alkali metal salts such as sodium salts, lithium salts, and potassium salts; alkaline earth metal salts such as magnesium salts and calcium salts; transition metal salts such as iron salts; monoethanolamine salts, diethanolamine salts, etc. Examples of the salt include alkanolamine salts such as monoethylamine salts, diethylamine salts, triethylamine salts, etc.; alkylamine salts such as monoethylamine salts, diethylamine salts, triethylamine salts, etc.; salts of organic amines such as polyamines such as ethylenediamine salts, triethylenediamine salts, etc. Among these, sodium salts and potassium salts are particularly preferred. An asterisk represents an atom contained in another structural unit of the same type or different type to which the structural unit represented by general formula (1) is bonded.) The structural unit containing the atom represented by the asterisk is not particularly limited, but examples thereof include a structural unit derived from a monomer, a structural unit derived from an initiator, and a structural unit derived from a chain transfer agent. Since the scale inhibition ability of the water treatment agent or scale inhibitor of the present disclosure tends to be improved, 3-(meth)allyloxy-2-hydroxypropanesulfonic acid and its salts are preferred, and 3-allyloxy-2-hydroxypropanesulfonic acid and its sodium salt are more preferred.
[0013] The content of the structural unit derived from the sulfonic acid (salt) group-containing monomer in the copolymer of the present disclosure is 13 mol% or more, preferably 14 mol% or more, more preferably 14.5 mol% or more, based on 100 mass% of the structural units derived from all monomers constituting the copolymer of the present disclosure. Also, it is preferably 40 mol% or less, more preferably 30 mol% or less, and even more preferably 25 mol% or less. The content of the structural unit derived from the sulfonic acid (salt) group-containing monomer is calculated in terms of sodium salt. The calculation in terms of sodium salt means that even if the sulfonic acid (salt) group contained in the structural unit derived from the sulfonic acid (salt) group-containing monomer is, for example, an acid type sulfonic acid group, it is calculated as the sodium salt of the sulfonic acid group. By being in the above range, the silica scale inhibition ability of the water treatment agent or scale inhibitor of the present disclosure tends to be improved.
[0014] <Structural units derived from other monomers> The copolymer of the present disclosure may, if desired, have structural units derived from monomers other than (meth)acrylic acid (salt)-derived structural units and sulfonic acid (salt) group-containing monomers (also referred to as structural units derived from other monomers). In the present disclosure, the structural unit derived from another monomer refers to a structural unit in which at least one carbon-carbon double bond of another monomer is replaced with a carbon-carbon single bond. Note that the structural unit derived from another monomer may have the same structure as the structure in which at least one carbon-carbon double bond of the other monomer is replaced with a carbon-carbon single bond, and is not limited to a structural unit formed by polymerization of the other monomer, and may be, for example, a structural unit formed by a post-reaction after polymerization. The content of structural units derived from other monomers in the copolymer of the present disclosure is, relative to 100 mol% of structural units derived from all monomers constituting the copolymer of the present disclosure, 0 mol% or more and 15 mol% or less, preferably 0 mol% or more and 10 mol% or less, more preferably 0 mol% or more and 5 mol% or less, even more preferably 0 mol% or more and 3 mol% or less, particularly preferably 0 mol% or more and 2 mol% or less, and most preferably 0 mol%.
[0015] Examples of the other monomers include carboxyl group-containing monomers such as maleic acid, itaconic acid, and salts thereof; unsaturated alcohols such as (meth)allyl alcohol and isoprenol, and monomers obtained by adding alkylene oxides thereto; polyalkylene glycol chain-containing monomers such as (meth)acrylic acid esters of alkoxyalkylene glycols; vinyl aromatic monomers having heterocyclic aromatic hydrocarbon groups such as vinylpyridine and vinylimidazole; dialkylaminoalkyl (meth)acrylates such as dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, and dimethylaminopropyl acrylate; dialkylaminoalkyl (meth)acrylamides such as dimethylaminoethyl acrylamide, dimethylaminoethyl methacrylamide, and dimethylaminopropyl acrylamide; allylamines such as diallyl alkylamines such as diallyl amine and diallyl dimethylamine; and quaternized products thereof; N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide, N-vinyl-N-methylformamide, N-vinyl-N-methyl N-vinyl monomers such as acetamide and N-vinyl oxazolidone; amide monomers such as (meth)acrylamide, N,N-dimethylacrylamide, N-isopropylacrylamide, and t-butylacrylamide; hydroxyl group-containing monomers such as (meth)allyl alcohol and isoprenol; (meth)acrylic acid alkyl ester monomers such as butyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and dodecyl (meth)acrylate; 2-hydroxyethyl (meth)acrylate, and 2-hydroxypropyl (meth)acrylate. (meth)acrylate hydroxyalkyl monomers such as 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxyhexyl (meth)acrylate; vinyl aryl monomers such as styrene, indene, and vinyl aniline; isobutylene, vinyl acetate, and the like; ether bond-containing monomers include vinyl ethers such as ethyl vinyl ether, butyl vinyl ether, and benzyl vinyl ether; (meth)allyl ethers such as ethyl methallyl ether, butyl methallyl ether, and benzyl methallyl ether;Examples of isoprenyl ethers include ethyl isoprenyl ether, butyl isoprenyl ether, and benzyl isoprenyl ether.
[0016] <Other structural units> The copolymer of the present disclosure is characterized in that it has a sulfonic acid (salt) group at at least one end of the polymer main chain. Having a sulfonic acid (salt) group at at least one end of the polymer main chain means having a sulfonic acid (salt) group at one or more ends of the main chain. For example, in the case of a linear polymer, there are two main chain ends, and one or both of them may have a sulfonic acid group, and for example, in the case of a polymer having a branched structure, there are three or more main chain ends, and one or more of them may have a sulfonic acid group. By having a sulfonic acid (salt) group at at least one chain end, the mass% of the sulfonic acid group at the main chain end of the copolymer is preferably 0.01% or more and 10% or less, more preferably 0.01% or more and 5% or less, relative to 100% by mass of the copolymer in which the silica scale inhibition ability is improved by having a sulfonic acid (salt) group at least one chain end. The conversion of the sulfonic acid group is calculated based on the acid group.
[0017] <Physical properties of the copolymer of the present disclosure> The copolymer of the present disclosure has a weight average molecular weight (Mw) of 28000 or more and 56000 or less, more preferably 30000 or more and 50000 or less, and even more preferably 37000 or more and 49000 or less. By being in the above range, the silica scale inhibition ability of the water treatment agent or scale inhibitor of the present disclosure tends to be further improved. The copolymer of the present disclosure contains acid groups such as carboxylic acid (salt) groups and sulfonic acid (salt) groups, and the acid groups of the copolymer of the present disclosure may be neutralized. It is preferable that the total neutralization rate of the acid groups is 1 mol% or more and 90 mol% or less. The neutralization rate can be calculated, for example, by ordinary acid-base titration.
[0018] <Method for producing the copolymer of the present disclosure> The method for producing the copolymer of the present disclosure is not particularly limited, but it is usually preferable to produce the copolymer by polymerizing structural units derived from (meth)acrylic acid (salt), a sulfonic acid (salt) group-containing monomer, and other monomers as necessary. In the process for producing the copolymer of the present disclosure, a polymerization initiator can be used in the polymerization of the monomer. In the process for producing the copolymer of the present disclosure, a chain transfer agent can be used as necessary to adjust the molecular weight.
[0019] <Chain transfer agent of the present disclosure> The chain transfer agent of the present disclosure can be used to adjust the molecular weight. For example, bisulfite (salt) such as bisulfite, metabisulfite, sodium bisulfite, potassium bisulfite, sodium metabisulfite, potassium metabisulfite, mercaptoethanol, thioglycerol, thioglycolic acid, 2-mercaptopropionic acid, 3-mercaptopropionic acid, thiomalic acid, octyl thioglycolate, octyl 3-mercaptopropionate, 2-mercaptoethanesulfonic acid, n-dodecyl mercaptan, octyl mercaptan, butyl thioglycolate, and other thiol-based chain transfer agents; halides such as carbon tetrachloride, methylene chloride, bromoform, and bromotrichloroethane; secondary alcohols such as isopropanol and glycerin; phosphorous acid, hypophosphorous acid, and salts thereof (sodium hypophosphite, potassium hypophosphite, and the like); and the like.
[0020] Among these, in the production of the copolymer according to the present disclosure, it is preferable to use bisulfites (salts) in order to incorporate a sulfonic acid group into at least one main chain end. This allows efficient introduction of a sulfonic acid group into at least one main chain end of the copolymer obtained. One type of chain transfer agent may be used, or two or more types may be used. The amount of chain transfer agent added is not limited as long as the monomers can be polymerized well, but is preferably 0.001 to 0.02 mol per mol of the monomer mixture to be copolymerized.
[0021] <Polymerization initiator of the present disclosure> In the process of producing the copolymer of the present disclosure, a polymerization initiator is usually used. Known polymerization initiators can be used. For example, persulfates such as sodium persulfate, potassium persulfate, and ammonium persulfate, hydrogen peroxide, dimethyl 2,2-'azobis(2-methylpropionate), 2,2'-azobis(isobutyronitrile), 2,2'-azobis(2-methylbutyronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), 2,2'-azobis(isobutyric acid) dimethyl, 4,4'-azobis(4-cyanovaleric acid), 2,2'-azobis(2-methylpropionate), Examples of the usable peroxides include azo compounds such as 2,2'-azobis[N-(2-carboxyethyl)-2-methylpropionamidine] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane] disulfate dihydrate, and 1,1'-azobis(cyclohexane-1-carbonitrile), as well as organic peroxides such as benzoyl peroxide, lauroyl peroxide, peracetic acid, di-t-butyl peroxide, and cumene hydroperoxide. Among these, persulfates are preferred, and by combining the above chain transfer agent, sulfonic acid groups can be efficiently introduced into the polymer main chain terminals.
[0022] [Uses of the Copolymer of the Present Disclosure] The copolymer of the present disclosure can exhibit high performance in aqueous applications and can be preferably used as a scale inhibitor for use in geothermal power generation processes, oil well and gas well processes, seawater desalination processes or waste liquid concentration processes using forward osmosis membranes or reverse osmosis membranes, boiler water circulation systems, cooling water circulation systems, and the like. The copolymer of the present disclosure can be preferably used as a scale inhibitor for, for example, silica scale or calcium carbonate, and is most preferably used as a scale inhibitor for silica scale.
[0023] [Water treatment agent of the present disclosure] The water treatment agent of the present disclosure includes the copolymer of the present disclosure. The water treatment agent of the present disclosure preferably includes the copolymer of the present disclosure in an amount of, for example, 1% by mass to 70% by mass. More preferably, the amount is 1% by mass to 50% by mass, even more preferably, 1% by mass to 40% by mass, most preferably, 1% by mass to 30% by mass, and even more preferably, 1% by mass to 20% by mass. The water treatment agent of the present disclosure may contain components other than the copolymer of the present disclosure. Examples of components other than the copolymer of the present disclosure include solvents such as water, pH adjusters such as alkalis and acids, oxygen scavengers, anticorrosives, chelating agents, phosphonic acids (salts) such as aminotrimethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, and salts thereof, carboxyl-containing polymers other than the copolymer of the present disclosure, surfactants, defoamers, pitch control agents, slime control agents, and the like. The water treatment chemical of the present disclosure is not particularly limited, but can be preferably used, for example, as a scale inhibitor for preventing scale from occurring in various types of water.
[0024] [Scale inhibitor of the present disclosure] The scale inhibitor of the present disclosure includes the copolymer of the present disclosure. The scale inhibitor of the present disclosure preferably includes, for example, 1% by mass or more and 100% by mass or less of the copolymer of the present disclosure. More preferably, the content is 1% by mass or more and 80% by mass or less, and most preferably, the content is 1% by mass or more and 50% by mass or less. The scale inhibitor of the present disclosure may contain components other than the copolymer of the present disclosure. Examples of components other than the copolymer of the present disclosure include solvents such as water, pH adjusters such as alkalis and acids, oxygen scavengers, anticorrosive agents, chelating agents, phosphonic acids (salts) such as aminotrimethylenephosphonic acid, 1-hydroxyethylidene-1,1-diphosphonic acid, and salts thereof, carboxyl-containing polymers other than the copolymer of the present disclosure, surfactants, defoamers, pitch control agents, slime control agents, and the like. The scale inhibitor of the present disclosure is not particularly limited, but can be preferably used as, for example, a scale inhibitor for silica scale or calcium carbonate. The scale inhibitor of the present disclosure is particularly excellent in terms of silica scale inhibition ability, and can therefore be preferably used as a silica scale inhibitor.
[0025] [Scale prevention method of the present disclosure] The scale prevention method of the present disclosure uses a water treatment agent or a scale inhibitor of the present disclosure, or a copolymer of the present disclosure. The scale prevention method of the present disclosure preferably includes a step of adding a water treatment agent or a scale inhibitor of the present disclosure, or a copolymer of the present disclosure, to a system to be prevented from scaling. Also, preferably, the method includes a step of controlling the amount of the copolymer of the present disclosure in the system to be prevented from scaling so that it is within a predetermined range. The content of the copolymer of the present disclosure in the system to be prevented from scaling is preferably 0.1 ppm or more and 500 ppm or less, and more preferably 0.1 ppm or more and 300 ppm or less. EXAMPLES
[0026] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. In addition, unless otherwise specified, "parts" means "parts by mass" and "%" means "% by mass". <Weight average molecular weight measurement conditions (GPC)> Equipment: Tosoh Corporation HLC8320 Column: SHODEX Asahipak GF-310-HQ, Showa Denko Corporation; GF-710-HQ, GF-1G-7B Column temperature: 40℃ Flow rate: 0.5ml / min Calibration curve: Polyacrylic acid standard manufactured by American Polymer Standards Corporation Eluent: 0.1N sodium acetate
[0027] <Synthesis Example 1> 251.5g of pure water and 0.031g of Mohr's salt were charged into a 3L SUS reaction vessel equipped with a reflux condenser and a stirrer (paddle blade), and the temperature was raised to 85°C while stirring to prepare a polymerization reaction system. Next, 517.5g of an 80% aqueous acrylic acid solution (hereinafter also referred to as "80% AA"), 533.2g of a 40% aqueous solution of sodium 3-allyloxy-2-hydroxypropanesulfonate (hereinafter also referred to as "40% HAPS"), 179.3g of a 15% aqueous sodium persulfate solution (hereinafter also referred to as "15% NaPS"), and 18.6g of a 32.5% aqueous sodium hydrogensulfite solution (hereinafter also referred to as "32.5% SBS") were dropped from separate nozzles into the polymerization reaction system maintained at 85°C under stirring. The drop time of each solution was 180 minutes for 80% AA, 140 minutes for 40% HAPS, 200 minutes for 15% NaPS, and 170 minutes for 32.5% SBS. The drop speed of each solution was constant, and each solution was continuously dropped. After the drop of 15% NaPS was completed, the reaction solution was kept at 85°C (aged) for another 30 minutes to complete the polymerization. In this way, a polymer aqueous solution (1) with a solid content concentration of 44.8% was obtained. The weight average molecular weight of the polymer (1) was 37,000. The composition ratio of the charged polymer was the same as that of the produced polymer.
[0028] <Synthesis Example 2> 250.78g of pure water and 0.031g of Mohr's salt were charged into a 3L SUS reaction vessel equipped with a reflux condenser and a stirrer (paddle blade), and the temperature was raised to 85°C while stirring to prepare a polymerization reaction system. Next, 508.9g of 80% AA, 524.3g of 40% HAPS, 176.3g of 15% NaPS, and 39.7g of 10% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 85°C under stirring. The drop times of each solution were 180 minutes for 80% AA, 140 minutes for 40% HAPS, 200 minutes for 15% NaPS, and 170 minutes for 10% SBS. The drop speed of each solution was constant, and each solution was dropped continuously. After the drop of 15% NaPS was completed, the reaction solution was maintained (aged) at 85°C for another 30 minutes to complete the polymerization. In this way, an aqueous polymer solution (2) with a solid content of 44.5% was obtained. The weight average molecular weight of the polymer (2) was 49000. The composition ratio of the charged polymer and the produced polymer was the same.
[0029] <Synthesis Example 3> 250.8g of pure water and 0.031g of Mohr's salt were charged into a 3L SUS reaction vessel equipped with a reflux condenser and a stirrer (paddle blade), and the temperature was raised to 85°C while stirring to prepare a polymerization reaction system. Next, 457.2g of 80% AA, 609.7g of 40% HAPS, 165.2g of 15% NaPS, and 17.2g of 32.5% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 85°C under stirring. The drop times of each solution were 180 minutes for 80% AA, 140 minutes for 40% HAPS, 200 minutes for 15% NaPS, and 170 minutes for 32.5% SBS. The drop speed of each solution was constant, and each solution was dropped continuously. After the drop of 15% NaPS was completed, the reaction solution was maintained (aged) at 85°C for another 30 minutes to complete the polymerization. In this way, an aqueous polymer solution (3) with a solid content of 43.6% was obtained. The weight average molecular weight of the polymer (3) was 37000. The composition ratio of the charged polymer and the produced polymer was the same.
[0030] <Synthesis Example 4> In a 3L SUS reaction vessel equipped with a flow condenser and a stirrer (paddle blade), 462.6g of pure water and 0.031g of Mohr's salt were charged, and the temperature was raised to 85°C while stirring to prepare a polymerization reaction system. Next, 674.3g of 80% AA, 238.0g of 40% HAPS, 103.1g of 15% NaPS, and 21.9g of 32.5% SBS were dropped from separate nozzles into the polymerization reaction system maintained at 85°C under stirring. The drop times of each solution were 180 minutes for 80% AA, 155 minutes for 40% HAPS, 200 minutes for 15% NaPS, and 170 minutes for 32.5% SBS. The drop speed of each solution was constant, and each solution was dropped continuously. After the drop of 80% AA was completed, the reaction solution was maintained (aged) at 85°C for another 30 minutes to complete the polymerization. In this way, an aqueous polymer solution (4) with a solid content of 43.6% was obtained. The weight average molecular weight of the polymer (4) was 44000. The composition ratio of the charged polymer and the produced polymer was the same.
[0031] <Synthesis Example 5> 611.3g of ion-exchanged water was charged into a 5L SUS reactor equipped with a reflux condenser and agitator, and the temperature was raised to the boiling point reflux state while stirring. Next, 57.6g of 80%AA, 1145·9g of 37% sodium acrylate (hereinafter also referred to as "37%SA"), 502.9g of 40%HAPS, 132.2g of 15%NaPS, 19.0g of 35% hydrogen peroxide solution (hereinafter also referred to as "35%H2O2"), and 367.9g of ion-exchanged water were dropped from separate nozzles into the polymerization reaction system under stirring at the boiling point reflux state. The dropping time of each solution was 120 minutes for 80%AA and 37%SA, 90 minutes for 40%HAPS and ion-exchanged water, 140 minutes for 15%NaPS, and 120 minutes for 35%H2O2. In this way, a polymer aqueous solution (5) with a solid content of 50.2% was obtained. The weight average molecular weight of the polymer (5) was 5000. The composition ratio of the charged polymer and the produced polymer was the same.
[0032] <Synthesis Example 6> In a 5L SUS reaction vessel equipped with a reflux condenser and an agitator, 1620g of ion-exchanged water was charged, and the temperature was raised to a boiling point reflux state while stirring. Next, 455g of 80% AA and 133g of 15% NaPS were dropped from separate nozzles into the polymerization reaction system in a boiling point reflux state while stirring. The dropping time of each solution was 180 minutes for 80% AA, 185 minutes for 15% NaPS, and 170 minutes for ion-exchanged water. After the dropping of the 15% NaPS solution was completed, the reaction solution was kept in a boiling point reflux state (ripening) for another 30 minutes to complete the polymerization. In this way, a polymer aqueous solution (6) with a solid content of 45.7% was obtained. The weight average molecular weight of the polymer (6) was 10,000. The composition ratio of the charged polymer and the produced polymer was the same.
[0033] <Silica scale inhibition rate evaluation test> Sodium silicate aqueous solution: Add ion-exchanged water to 2.129 g of sodium metasilicate nonahydrate (manufactured by Aldrich) to make a total of 150 g. Magnesium sulfate aqueous solution: Add ion-exchanged water to 8.115 g of magnesium sulfate heptahydrate (manufactured by Wako Pure Chemical Industries, Ltd.) to make a total of 1000 g. Boric acid buffer: 7.42 g of boric acid (Kanto Chemical Co., Ltd.) and 19.07 g of sodium borate decahydrate (Wako Pure Chemical Industries, Ltd.) are mixed to prepare boric acid buffer. 73 g of deionized water was placed in a container, and while stirring, 2 g of the boric acid buffer, 10 g of the sodium silicate aqueous solution, 5 g of the polymer aqueous solution diluted to a polymer concentration of 1000 ppm, and 10 g of the magnesium sulfate aqueous solution were added, and the mixture was left in a warm bath at 60°C for 5 hours. After leaving the mixture for 5 hours, the test liquid was suction filtered using a suction filtration device and a filter paper with 0.1 μm openings. The obtained filtrate was measured by XR-F to measure the Si concentration in terms of SiO2. Silica scale inhibition rate (%) = SiO2 after test (ppm) / SiO2 concentration before test (ppm) x 100 The silica scale inhibition rate was judged according to the following criteria. <Inhibition rate evaluation criteria> Over 90%: ◎ 70~90%:○ 30~70%:△ Less than 30%: × <Example 1> The above silica scale inhibition rate test was carried out on 5 g of a 1000 ppm aqueous solution of the polymer (1) obtained in Synthesis Example 1. <Example 2> The above-mentioned silica scale inhibition rate evaluation test was carried out on 5 g of a 1000 ppm aqueous solution of the polymer (2) obtained in Synthesis Example 2. <Example 3> The above-mentioned silica scale inhibition rate evaluation test was carried out on 5 g of a 1000 ppm aqueous solution of the polymer (3) obtained in Synthesis Example 3. <Comparative Example 1> The above-mentioned silica scale inhibition rate evaluation test was carried out on 5 g of a 1000 ppm aqueous solution of the polymer (4) obtained in Synthesis Example 4. <Comparative Example 2> The above silica scale inhibition rate evaluation test was carried out on 5 g of a 1000 ppm aqueous solution of the polymer (5) obtained in Synthesis Example 5. <Comparative Example 3> The above silica scale inhibition rate evaluation test was carried out on 5 g of a 1000 ppm aqueous solution of the polymer (6) obtained in Synthesis Example 6. <Comparative Example 4> The evaluation test was carried out in the same manner as in the above silica scale inhibition rate evaluation test, except that the aqueous polymer solution was not added.
[0034] The experimental results of Examples 1 to 3 and Comparative Examples 1 to 4 are shown in Table 1.
[0035] [Table 1] In Table 1, "composition" indicates the structural units derived from acrylic acid (salt) / structural units derived from sulfonic acid (salt) groups. The results in Table 1 show that the copolymer of the present disclosure has excellent silica scale inhibition ability.
Claims
1. A copolymer comprising a structural unit derived from (meth)acrylic acid (salt) and a structural unit derived from a sulfonic acid (salt) group-containing monomer, The structural unit derived from the sulfonic acid (salt) group-containing monomer is represented by general formula (1): A silica scale inhibitor comprising a (meth)acrylic acid-based copolymer, the weight average molecular weight of which is 28,000 or more and 56,000 or less, the structural units derived from a monomer containing a sulfonic acid (salt) group being 13 mol % or more relative to 100 mol % of all monomer-derived structures, the copolymer having a sulfonic acid (salt) group at at least one main chain end. 【Chemistry 1】 (In general formula (1), R 1 represents a hydrogen atom or a methyl group, and X and Y each independently represent a hydroxyl group or a sulfonic acid (salt) group (provided that at least one of X and Y represents a sulfonic acid (salt) group). An asterisk represents an atom contained in another structural unit of the same type or different type to which the structural unit represented by general formula (1) is bonded.
2. The silica scale inhibitor according to claim 1, wherein the structural unit derived from the sulfonic acid (salt) group-containing monomer is a structural unit derived from 3-allyloxy-2-hydroxypropanesulfonic acid or a salt thereof.
3. A silica scale inhibitor as described in claim 1 or 2, wherein the copolymer contains structural units derived from (meth)acrylic acid (salt) in an amount of 50 mol % or more and 87 mol % or less relative to 100 mol % of structures derived from all monomers.
Citation Information
Patent Citations
(METH)acrylic acid-based copolymer, and method for producing the same
JP2012188586A
Treatment method of cooling water system
JP2013212435A
Carboxyl group-containing polymer composition
JP2014047352A
Processing method of cooling water system
JP2015025160A
Scale inhibitor for geothermal power generation
JP2016064382A