Organoaminodisilazanes for high-temperature atomic layer deposition of silicon oxide thin films

Organic aminodisilazane precursors in ALD processes address the low deposition rates and impurity issues of thermal oxidation and conventional ALD, enabling high-quality, conformal silicon oxide films at elevated temperatures.

JP7586837B2Active Publication Date: 2024-11-19VERSUM MATERIALS US LLC
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021563071
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-04-25
Filing Date
2020-04-17
Publication Date
2024-11-19
Estimated Expiration
2040-04-17

AI Technical Summary

Technical Problem

Existing thermal oxidation processes for depositing silicon oxide films in semiconductor applications have low deposition rates and result in impure, non-conformal films at high temperatures, while conventional ALD processes at these temperatures lead to CVD mode deposition, reducing film controllability and conformality.

Method used

The use of organic aminodisilazane precursors in ALD processes at temperatures above 500°C, with specific functional groups to anchor monolayers and prevent thermal decomposition, combined with oxygen sources and purge gases, to form high-quality, conformal silicon oxide films.

Benefits of technology

Achieves high-purity, conformal silicon oxide films with improved film density and purity at elevated temperatures, overcoming the limitations of conventional ALD and thermal oxidation methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007586837000001
    Figure 0007586837000001
  • Figure 0007586837000002
    Figure 0007586837000002
  • Figure 0007586837000003
    Figure 0007586837000003
Patent Text Reader

Abstract

An atomic layer deposition (ALD) process for the formation of silicon oxide at temperatures above 500° C. is provided by the method of formula I: TIFF2022530419000019.tif4978, where R 1 and R 2 is hydrogen, straight or branched C1-C 10 Alkyl groups and C6-C 10 aryl groups, with the proviso that R 1 and R 2 cannot both be hydrogen; R 3 is hydrogen, straight or branched C1-C 10 Alkyl groups and C6-C 10 aryl groups; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 is carried out using at least one organoaminodisilazane precursor that is not linked to form a cyclic ring structure.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] This application claims the benefit of U.S. Patent Application No. 62 / 838,854, filed April 25, 2019. The disclosure of U.S. Patent Application No. 62 / 838,854 is incorporated herein by reference.

[0002] Described herein are compositions and methods for the formation of silicon oxide films. More specifically, described herein are compositions and methods for the formation of silicon oxide films at one or more deposition temperatures of about 500° C. or greater and using atomic layer deposition (ALD) processes. [Background technology]

[0003] Thermal oxidation is a process commonly used to deposit high purity and highly conformal silicon oxide films, such as silicon dioxide (SiO2), in semiconductor applications. However, thermal oxidation processes have very low deposition rates, e.g., 0.03 Å / s at 700° C., which makes the thermal oxidation process impractical for high volume manufacturing processes (see, e.g., Wolf, S., “Silicon Processing for the VLSI Era Vol. 1-Process Technology”, Lattice Press, CA, 1986).

[0004] Atomic layer deposition (ALD) and plasma enhanced atomic layer deposition (PEALD) are processes used to form conformal films of silicon dioxide (SiO2) at low temperatures (<500°C). In ALD and PEALD processes, precursors and reactive gases (e.g. oxygen or ozone) are pulsed separately for a certain number of cycles to form a monolayer of silicon dioxide (SiO2) in each cycle. However, silicon dioxide (SiO2) deposited at low temperatures using these processes may contain levels of impurities, such as carbon (C), nitrogen (N), or both, that are harmful for semiconductor applications. To remedy this, one possible solution is to increase the deposition temperature to 500°C or higher. However, at these higher temperatures, conventional precursors used by the semiconductor industry self-react, thermally decompose, and deposit in chemical vapor deposition (CVD) mode rather than ALD mode. CVD mode deposition reduces conformality compared to ALD deposition, especially in high aspect ratio structures in semiconductor applications. In addition, CVD mode deposition provides less film control or smaller material thickness than ALD mode deposition.

[0005] JP2010-275602A and JP2010-225663A disclose the use of a raw material for forming a Si-containing thin film, such as silicon oxide, by a chemical vapor deposition (CVD) process at a temperature of 300-500° C. The raw material has the formula: (a) HSi(CH3)(R 1 )(NR 2 R 3 ) (where R 1 But NR 4 R 5 or a 1C-5C alkyl group; R 2 and R 4 represents a 1C-5C alkyl group or a hydrogen atom; and R 3 and R 5 each represents a 1C-5C alkyl group; or (b) HSiCl(NR 1 R 2 )(NR 3 R 4) (where R 1 and R 3 each independently represents an alkyl group having 1 to 4 carbon atoms or a hydrogen atom; and R 2 and R 4 each independently represents an alkyl group having 1 to 4 carbon atoms. The organosilicon compound has an H-Si bond.

[0006] U.S. Pat. No. 7,084,076 discloses halogenated siloxanes, such as hexachlorodisiloxane (HCDSO), which can be used in combination with pyridine as a catalyst to form silicon dioxide for ALD deposition below 500° C.

[0007] US6992019 discloses a method for catalyst-assisted atomic layer deposition (ALD) to form a silicon dioxide layer with excellent properties on a semiconductor substrate by using a first reactant component consisting of a silicon compound having at least two silicon atoms, or a tertiary amine as a catalyst component, or a combination of both, together with associated purging methods and sequencing. The precursor used is hexachlorodisilane. The deposition temperature is 25-150°C.

[0008] US Patent No. 9,460,912 discloses a method for the formation of silicon oxide-containing films at one or more deposition temperatures of about 500° C. In one embodiment, the compositions and processes are represented by the following formulae I, II (R 1 R 2 m Si(NR 3 R 4 ) n X p (I);R 1 R 2 m Si(OR 3 ) n (OR 4 ) q X p(II)), and combinations thereof. Summary of the Invention [Problem to be solved by the invention]

[0009] There is a need to develop processes for forming high quality, low impurity, highly conformal silicon oxide films using atomic layer deposition (ALD) processes or ALD-like processes, such as, but not limited to, cyclic chemical vapor deposition processes, to replace thermal-based deposition processes. Additionally, it may be desirable to develop high temperature deposition (e.g., deposition at one or more temperatures of 500° C.) in ALD or ALD-like processes to improve one or more film properties, such as purity and / or density. [Means for solving the problem]

[0010] Described herein are processes for the deposition of silicon oxide materials or films at high temperatures, e.g., at one or more temperatures of 500° C. or greater, in an atomic layer deposition (ALD) or ALD-like process.

[0011] One embodiment is a process for depositing silicon oxide comprising: a. providing a substrate in a reactor; b. introducing at least one organoaminodisilazane precursor into a reactor; c. purging the reactor with a purge gas; d. introducing an oxygen source into the reactor; and e. purging the reactor with a purge gas wherein steps b through e are repeated until a desired thickness of silicon oxide is deposited; and the process is carried out at one or more temperatures between 500 and 800° C., and at one or more pressures between 50 milliTorr (mT) and 760 Torr.

[0012] Another embodiment is a process for depositing silicon oxide, comprising the steps of: a. providing a substrate in a reactor; b. introducing at least one organoaminodisilazane precursor into a reactor; c. purging the reactor with a purge gas; d. introducing a source of oxygen into the reactor; e. purging the reactor with a purge gas; f. introducing water vapor or a hydroxyl source into the reactor; and g. purging the reactor with a purge gas wherein steps b through e are repeated until a desired thickness of silicon oxide is deposited; and the process is carried out at one or more temperatures between 500 and 800° C. and at one or more pressures between 50 milliTorr (mT) and 760 Torr. In this or other embodiments, the oxygen source is selected from the group consisting of oxygen, oxygen plasma, water vapor, water vapor plasma, hydrogen peroxide, nitrogen oxides, and ozone.

[0013] For each of the above methods, at least one organoaminodisilazane precursor described herein comprises: [ka] wherein R 1 and R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups and C6-C 10 R is independently selected from the group consisting of aryl groups; 3 is hydrogen, linear or branched C1-C 10 Alkyl groups and C6-C 10 aryl groups, where R 1 and R 2 cannot both be hydrogen; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2are not linked to form a cyclic ring structure. In one or more embodiments described above, the purge gas is selected from the group consisting of nitrogen, helium, argon, and combinations thereof.

[0014] In one or more of the embodiments described above, the oxygen source is selected from the group consisting of oxygen, a composition comprising oxygen and hydrogen, oxygen plasma, water vapor, water vapor plasma, hydrogen peroxide, nitrous oxide, ozone, and combinations thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] Described herein are compositions and processes for forming silicon oxide-containing films, such as silicon oxynitride films, stoichiometric or non-stoichiometric silicon oxide films, silicon oxide films, or combinations thereof, at one or more temperatures of 500° C. or greater in ALD or ALD-like processes, such as, but not limited to, cyclic chemical vapor deposition processes (CCVD).

[0016] A typical ALD process in the prior art uses an oxygen source or oxidant, such as oxygen, a composition containing oxygen and hydrogen, oxygen plasma, water vapor, water vapor plasma, hydrogen peroxide, nitrous oxide, and ozone directly to form silicon oxide at a process temperature of 25-500° C. The deposition process includes: a. providing a substrate in a reactor; b. introducing an organoaminodisilazane into the reactor; c. purging the reactor with a purge gas; d. introducing an oxygen source into the reactor; and e. purging the reactor with a purge gas In the prior art process, steps b through e are repeated until a film of the desired thickness is deposited.

[0017] High temperature process above 500°C, preferably above 600°C, most preferably above 650°C can provide better quality in terms of film purity and density. ALD process provides good film step coverage. However, typical organosilicon precursors used in ALD or PEALD deposit films in ALD mode only in a certain temperature range. When temperature is higher than this range, thermal decomposition of precursor occurs, which causes either gas phase reaction or continuous substrate surface reaction, which changes deposition process to CVD mode rather than the desired ALD mode.

[0018] Without being bound by theory, for ALD or ALD-like deposition processes at one or more temperatures above 500°C, above 600°C, or above 650°C, the organoaminodisilazane molecules described herein should have at least one anchoring functional group that reacts with a specific reactive site on the substrate surface to anchor a monolayer of silicon species. The anchoring functional group can be selected from organic amino groups, preferably smaller amino groups, such as dimethylamino, ethylmethylamino, or diethylamino groups. Because smaller organic amino groups allow the organoaminodisilazane to have a lower boiling point and higher reactivity. The organoaminodisilazane should further have an inactive functional group that is chemically stable to prevent further surface reactions that cause a self-limiting process. The inactive functional group is selected from different alkyl groups, such as methyl, ethyl, and phenyl groups, preferably methyl groups. The remaining groups on the surface are then oxidized to form Si-O-Si bonds and hydroxyl groups. In addition, a hydroxyl source, such as HO or water plasma, can also be introduced into the reactor to form additional hydroxyl groups as reactive sites for the next ALD cycle.

[0019] In one embodiment, at least one organoaminodisilazane precursor described herein has formula (I): [ka] wherein R 1 and R 2 is hydrogen, linear or branched C1-C 10 Alkyl groups, C3-C 10 Cyclic alkyl groups and C6-C 10 R is independently selected from the group consisting of aryl groups; 3 is hydrogen, linear or branched C1-C 10 Alkyl groups and C6-C 10 aryl groups, where R 1 and R 2 cannot both be hydrogen; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 are not linked to form a cyclic ring structure.

[0020] In one preferred embodiment, at least one organoaminodisilazane precursor described herein has formula (IA): [ka] wherein R 1 and R 2 is selected from C1 to C6 alkyl groups; R 3 is hydrogen, a linear or branched C1-C6 alkyl group, and a C6-C 10 aryl groups; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 are not linked to form a cyclic ring structure.

[0021] In the above formula and throughout this specification, the term "alkyl" refers to a straight or branched chain functional group having 1 to 10, 3 to 10, or 1 to 6 carbon atoms. Exemplary straight chain alkyl groups include methyl, ethyl, n-propyl (n-Pr or Pr n Exemplary branched alkyl groups include, but are not limited to, iso-propyl (i-Pr or Pri ), isobutyl (i-Bu or Bu i ), sec-Butyl (s-Bu or Bu s ), tert-Butyl (t-Bu or Bu t ), iso-pentyl, tert-pentyl, isohexyl, and neohexyl. In certain embodiments, the alkyl group can have one or more functional groups attached to the alkyl group, such as, but not limited to, an alkoxy group, a dialkylamino group, or a combination thereof. In other embodiments, the alkyl group does not have one or more functional groups attached to the alkyl group. The alkyl group can be saturated or alternatively unsaturated.

[0022] In the formula above and throughout this specification, the term "cyclic alkyl" refers to a cyclic functional group having 3 to 10 carbon atoms. Exemplary cyclic alkyl groups include, but are not limited to, cyclobutyl, cyclopentyl, cyclohexyl, and cyclooctyl groups.

[0023] In the above formula and throughout this specification, the term "aryl" refers to an aromatic cyclic functional group having 3 to 10 carbon atoms, 5 to 10 carbon atoms, or 6 to 10 carbon atoms. Exemplary aryl groups include, but are not limited to, phenyl, benzyl, chlorobenzyl, tolyl, and o-xylyl.

[0024] In certain embodiments, the substituent R in formula I 1 and R 2 may be linked together to form a ring structure. As will be appreciated by those of skill in the art, R 1 and R 2 When both are linked together to form a ring, R 1 is R 2and vice versa. In these embodiments, the ring structure may be unsaturated (e.g., cyclic alkyl ring) or saturated (e.g., aryl ring). Furthermore, in these embodiments, the ring structure may be substituted or unsubstituted. Exemplary cyclic ring groups include, but are not limited to, pyrrolidino, 2-methylpyrrolidino, 2,5-dimethylpyrrolidino, piperidino, 2,6-dimethylpiperidino, pyrrolyl, and imidazolyl groups. However, in other embodiments, the substituent R 1 and R 2 are not linked.

[0025] In certain embodiments, the silicon film deposited using the methods described herein is formed in the presence of oxygen using an oxygen source, an oxygen-containing reagent or precursor. The oxygen source can be introduced into the reactor in the form of at least one oxygen source, and may be incidentally present in other precursors used in the deposition process. Suitable oxygen source gases can include, for example, water (H2O) (e.g., deionized water, purified water and / or distilled water), oxygen (O2), oxygen plasma, ozone (O3), N2O, NO2, carbon monoxide (CO), carbon dioxide (CO2), and combinations thereof. In certain embodiments, the oxygen source comprises an oxygen source introduced into the reactor at a flow rate of about 1 to about 2000 standard cubic centimeters (sccm) or about 1 to about 1000 sccm. The oxygen source can be introduced for a time ranging from about 0.1 to about 100 seconds. In one particular embodiment, the oxygen source comprises water having a temperature of 10°C or higher. In the embodiment where the film is deposited by ALD or cyclic CVD process, the precursor pulse can have a pulse duration longer than 0.01 seconds, the oxygen source can have a pulse duration shorter than 0.01 seconds, while the water pulse can have a pulse duration shorter than 0.01 seconds.In yet another embodiment, the purge period between pulses can be as short as 0 seconds, or pulse continuously without purge in between.The oxygen-containing source or reagent is provided in a molecular amount less than 1:1 ratio to the silicon precursor, so that at least some carbon is retained in the as-deposited dielectric film.

[0026] In certain embodiments, the silicon oxide film further comprises nitrogen. In these embodiments, the film is deposited in the presence of a nitrogen-containing source using the methods described herein. The nitrogen-containing source may be introduced into the reactor in the form of at least one nitrogen-containing source gas and / or may be present incidentally in other precursors used in the deposition process. Suitable nitrogen-containing source gases may include, for example, ammonia, hydrazine, monoalkylhydrazine, dialkylhydrazine nitrogen, nitrogen / hydrogen, ammonia plasma, nitrogen plasma, nitrogen / hydrogen plasma, and mixtures thereof. In certain embodiments, the nitrogen-containing source comprises an ammonia plasma or a hydrogen / nitrogen plasma source gas introduced into the reactor at a flow rate of about 1 to about 2000 square cubic centimeters (sccm) or about 1 to about 1000 sccm. The nitrogen-containing source may be introduced for a time period ranging from about 0.1 to about 100 seconds. In embodiments where the film is deposited by ALD or cyclic CVD process, the precursor pulse may have a pulse duration longer than 0.01 seconds, the nitrogen-containing source may have a pulse duration shorter than 0.01 seconds, while the water pulse may have a pulse duration shorter than 0.01 seconds. In yet another embodiment, the purge period between the pulses may be as short as 0 seconds, or pulsed continuously with no purge in between.

[0027] The deposition methods disclosed herein may include one or more purge gases. Purge gases used to purge unconsumed reactants and / or reaction by-products include, but are not limited to, argon (Ar), nitrogen (N2), helium (He), neon, hydrogen (H2), and mixtures thereof. In certain embodiments, a purge gas, such as Ar, is fed into the reactor at a flow rate of about 10 to about 2000 sccm for about 0.1 to 1000 seconds, thereby purging unreacted materials and any by-products that may remain in the reactor.

[0028] Each step of supplying precursors, oxygen sources, nitrogen-containing sources and / or other precursors, source gases and / or reagents can be performed with varying times for supplying them to vary the stoichiometric composition of the resulting dielectric film.

[0029] Energy is provided to at least one of silicon precursor, oxygen-containing source, or combination thereof to induce reaction and form a dielectric film or coating on the substrate.Such energy can be provided by, but not limited to, heat, plasma, pulsed plasma, helicon plasma, high-density plasma, inductively coupled plasma, X-ray, electron beam, photon, remote plasma method, and combinations thereof.In certain embodiments, a secondary radio frequency source can be used to modify the plasma characteristics at the substrate surface.In embodiments where deposition includes plasma, the plasma generation process can include a direct plasma generation process, where plasma is generated directly in the reactor, or alternatively, a remote plasma generation process, where plasma is generated outside the reactor and fed into the reactor.

[0030] At least one silicon precursor can be transported to a reaction chamber, for example, to a cyclic CVD or ALD reactor, in a variety of ways. In one embodiment, a liquid transport system can be utilized. In an alternative embodiment, a unit that combines liquid transport and flash evaporation processes, such as a turbo vaporizer manufactured by MSP Corporation of Shoreview, MN, can be used to allow low volatility materials to be transported volumetrically, which results in reproducible transport and deposition without pyrolysis of the precursor. In liquid transport formulations, the precursors described herein can be transported in a substantially liquid form, or alternatively, can be used in solvent formulations or compositions that include the precursors. Thus, in certain embodiments, precursor formulations can include at least one solvent component with suitable properties that can be desirable and advantageous in a given end-use application that forms a film on a substrate.

[0031] In the composition comprising a solvent and at least one organoaminodisilazane precursor having formula I or IA described herein, for the embodiment in which at least one organoaminodisilazane precursor having formula I or IA is used, the solvent or mixture thereof selected does not react with the silicon precursor. The amount (wt%) of the solvent in the composition is 0.5wt% to 99.5wt% or 10wt% to 75wt%. In this or other embodiment, the solvent has a boiling point (bp) close to the boiling point (bp) of the at least one organoaminodisilazane precursor of formula I, or the difference between the boiling point of the solvent and the boiling point of the at least one organoaminodisilazane precursor of formula I is less than 40°C, less than 30°C, less than 20°C, or less than 10°C. Alternatively, the difference between the boiling points is a range that has any one or more of the following endpoints: 0, 10, 20, 30, or 40°C as endpoints. Examples of suitable ranges of the bp difference include, but are not limited to, 0 to 40° C., 20 to 30° C., or 10 to 30° C. Examples of suitable solvents in the composition include, but are not limited to, ethers (e.g., 1,4-dioxane, dibutyl ether), tertiary amines (e.g., pyridine, 1-methylpiperidine, 1-ethylpiperidine, N,N'-dimethylpiperazine, N,N,N',N'-tetramethylethylenediamine), nitriles (e.g., benzonitrile), alkanes (e.g., octane, nonane, dodecane, ethylcyclohexane), aromatic hydrocarbons (e.g., toluene, mesitylene), tertiary amino ethers (e.g., bis(2-dimethylaminoethyl) ether) or mixtures thereof.

[0032] As described above, the purity level of at least one organoaminodisilazane precursor of formula I is high enough to be acceptable for reliable semiconductor manufacturing.In certain embodiments, at least one organoaminodisilazane precursor of formula I described herein contains less than 2 wt%, less than 1 wt%, or less than 0.5 wt% of one or more of the following impurities: free amine, free halide or halide ion, and higher molecular weight species.Higher purity levels of the organoaminodisilazanes described herein can be obtained through one or more of the following processes: purification, adsorption, and / or distillation.

[0033] In one embodiment of the method described herein, a cyclic deposition process, such as ALD-like, ALD or PEALD, can be used, in which deposition is carried out using at least one organoaminodisilazane precursor of formula I and an oxygen source. ALD-like processes are defined as cyclic CVD processes, but which provide highly conformal silicon oxide films.

[0034] In certain embodiments, the gas lines connecting the precursor canister to the reaction chamber are heated to one or more temperatures depending on the process requirements, and the container of at least one organoaminodisilazane precursor of Formula I is maintained at one or more temperatures for bubbling. In other embodiments, a solution containing at least one organoaminodisilazane precursor of Formula I is injected into a vaporizer maintained at one or more temperatures for direct liquid injection.

[0035] A flow of argon and / or other gases can be used as a carrier gas to facilitate transporting vapor of at least one organoaminodisilazane precursor of Formula I to the reaction chamber during the precursor pulse. In certain embodiments, the reaction chamber process pressure is about 1 Torr.

[0036] In a typical ALD or ALD-like process, e.g., a CCVD process, a substrate, e.g., a silicon oxide substrate, is initially exposed to an organoaminodisilazane and heated in a heater stage in a reaction chamber to allow the complex to chemisorb to the surface of the substrate.

[0037] A purge gas, such as argon, purges unabsorbed excess complex from the process chamber. After sufficient purging, an oxygen source is introduced into the reaction chamber to react with the absorbed surface, and then another gas purge is applied to remove reaction by-products from the chamber. The process cycle can be repeated to achieve the desired film thickness. In some cases, pumping can be substituted for purging with an inert gas, or both can be used to remove unreacted silicon precursor.

[0038] In this or other embodiments, the steps of the methods described herein can be performed in various orders, sequentially, simultaneously (e.g., during at least a portion of another step), and in any combination. Each step of supplying the precursor and oxygen source gas can be performed for different durations to vary the stoichiometric composition of the resulting dielectric film.

[0039] One particular embodiment of the method described herein for depositing a silicon oxide film on a substrate comprises: a. providing a substrate in a reactor; b. introducing into a reactor at least one organoaminodisilazane precursor described herein having formula I; c. purging the reactor with a purge gas; d. introducing an oxygen source into the reactor; and e. purging the reactor with a purge gas Steps b to e are repeated until a silicon oxide film of a desired thickness is deposited.

[0040] In one particular embodiment of the methods and compositions described herein, the organoaminodisilazane has the following formula IA: [ka] wherein R 1 and R 2 is selected from C1 to C6 alkyl groups; R 3 is hydrogen, a linear or branched C1-C6 alkyl group, and a C6-C 10 aryl groups; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 are not linked to form a cyclic ring structure. Table 1 below shows the structure of an exemplary silicon precursor having a fixed functional group, i.e., an organic amino group, and an inert functional group selected from an alkyl group, preferably a methyl or Me group. Without being bound by theory, the Si-Me group is more stable than the ethyl group at temperatures above 500° C., thus providing an inert functional group that prevents further surface reactions, resulting in a self-limiting ALD or ALD-like process, especially at temperatures above 600° C.

[0041] Table 1. Organoaminodisilazane precursors having at least one anchoring functional group and at least one inert functional group (e.g., three methyl groups), where R 3 is selected from hydrogen, methyl and methyl, which provide a low boiling point, thus allowing the organoaminodisilazane precursor to be easily transported into a reaction chamber for deposition of silicon oxide. [Table 1-1] [Table 1-2] [Table 1-3] [Table 1-4]

[0042] Organoaminodisilazane compounds having formula I or IA can be synthesized, for example, by catalytic dehydrocoupling of an unsymmetrical disilazane or a chlorinated unsymmetrical disilazane, as shown below, with an organic amine (eg, formula (1) or (2)). [ka] [ka]

[0043] Unsymmetric or chlorinated unsymmetric disilazanes can be prepared by treatment of a symmetric disilazane, of formula (3) below, with dimethylchlorosilane or dimethyldichlorosilane, respectively. [ka]

[0044] The catalyst used in the method of the present invention of formula (1) is a catalyst that promotes the formation of silicon-nitrogen bonds.Exemplary catalysts that can be used with the method described herein include, but are not limited to, alkaline earth metal catalysts; main group, transition metal, lanthanide and actinide catalysts that do not contain halides; and main group, transition metal, lanthanide and actinide catalysts that contain halides, and pure precious metals, such as ruthenium, platinum, palladium, rhodium, osmium, can also be attached to the carrier.The carrier is a solid with a large surface area.Typical carrier materials include, but are not limited to, alumina, MgO, zeolite, carbon, monolith cordierite, diatomaceous earth, silica gel, silica / alumina, ZrO and TiO2.Preferred carriers are carbon (e.g., platinum on carbon, palladium on carbon, ruthenium on carbon), alumina, silica and MgO.

[0045] Preferably, the composition comprising the organoaminodisilazane compound having formula I or IA according to the present invention and the silicon precursor compound having formula I or IA according to the present invention is substantially free of halide ions.As used herein, the term "substantially free" means less than 5 ppm (by weight) as measured by ion chromatography (IC), preferably less than 3 ppm as measured by IC, more preferably less than 1 ppm as measured by IC, and most preferably 0 ppm as measured by IC, when referring to halide ions (or halides), such as chloride (i.e. chloride-containing species, such as HCl, or silicon compounds having at least one Si-Cl bond), fluoride, bromide and iodide.Chloride is known to act as a decomposition catalyst for organoaminodisilazane compounds having formula I or IA.A significant amount of chloride in the final product may cause the silicon precursor compound to decompose.The slow decomposition of organoaminodisilazane compounds may directly affect the deposition process of the film, making it difficult for semiconductor manufacturers to meet the film specifications. In addition, the shelf life or stability is negatively affected by the higher decomposition rate of the organoaminodisilazane compound having formula I or IA, thereby making it difficult to guarantee a shelf life of 1 to 2 years. Thus, the accelerated decomposition of the organoaminodisilazane compound having formula I or IA brings about safety and performance concerns regarding the formation of these flammable and / or spontaneously combusting gaseous by-products. Preferably, the organoaminodisilazane compound having formula I or IA is substantially free of metals. As used herein, the term "substantially free" means less than 5 ppm (by weight), preferably less than 3 ppm, more preferably less than 1 ppm, and most preferably 0.1 ppm, as measured by ICP-MS, with respect to Li, Na, K, Mg, Ca, Al, Fe, and Nin. In some embodiments, the organoaminodisilazane compound having formula I or IA is metal-free. Preferably, the organoaminodisilazane compounds having Formula I or IA, when used as precursors to deposit high quality silicon oxide or carbon doped silicon oxide, have a purity of 98 wt% or greater, more preferably 99 wt% or greater, as measured by GC.

[0046] Another embodiment of the method described herein introduces a hydroxyl or OH source, such as H2O vapor, after the oxidation step. The purpose of this embodiment is to redistribute reactive sites or anchoring functional groups that anchor the organoaminodisilazane to the surface to form a monolayer. The deposition step is a. providing a substrate in a reactor; b. introducing into a reactor one of the organoaminodisilazane precursors described above; c. purging the reactor with a purge gas; d. introducing an oxidant into the reactor; e. purging the reactor with a purge gas; f. introducing water vapor or a hydroxyl source into the reactor; and g. purging the reactor with a purge gas Steps b to g are repeated until a desired thickness is deposited.

[0047] In an alternative embodiment described herein, the depositing step comprises: a. providing a substrate in a reactor; b. introducing into a reactor one of the organoaminodisilazane precursors described above; c. purging the reactor with a purge gas: d. introducing a source of oxygen into the reactor; e. purging the reactor with a purge gas; f. introducing water vapor or an OH source into the reactor; and g. purging the reactor with a purge gas Steps b to g are repeated until a desired thickness is deposited.

[0048] Yet another embodiment uses hydrogen peroxide or oxygen plasma to remove inactive functional groups, or groups such as methyl. The deposition process is as follows: a. providing a substrate in a reactor; b. introducing into a reactor one of the organoaminodisilazane precursors described above; c. purging the reactor with a purge gas; d. introducing ozone, hydrogen peroxide or oxygen plasma into the reactor; and e. Purging the reactor with a purge gas. Here, steps b to e are repeated until the desired thickness is deposited.

[0049] The process temperatures for the methods described herein are one or more of the following ranges: 500°C to 1000°C; 500°C to 750°C; 600°C to 750°C; 600°C to 800°C; or 650°C to 800°C.

[0050] The deposition pressure ranges from one or more of 50 milliTorr (mT) to 760 Torr or 500 mT to 100 Torr. The purge gas can be selected from an inert gas, such as nitrogen, helium, or argon. The oxidizer is selected from oxygen, a composition containing oxygen and hydrogen, hydrogen peroxide, molecular oxygen derived from a plasma process, or ozone. EXAMPLES

[0051] Example 1: Preparation of 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane

[0052] Dimethyldichlorosilane (1.13 moles, 146 g) was added to heptamethyldisilazane (1.13 moles, 198 g) via addition funnel in a 1 L flask. The mixture was stirred and heated to about 60° C. When the reaction was complete as determined by GC analysis, the reaction mixture was distilled. Under reduced pressure (68° C. / 25 Torr), 157 g of 1-chloro-1,1,2,3,3,3-hexamethyldisilazane was obtained in 71% yield.

[0053] A solution of dimethylamine (2M) in THF (1.0 mole, 500 mL) was slowly added via addition funnel to a mixture of 1-chloro-1,1,2,3,3,3-hexamethyldisilazane (0.67 mole, 131 g), triethylamine (0.80 mole, 81 g), and hexane. After the addition was complete, the resulting slurry was stirred and then heated at about 50° C. for 2 hours. The mixture was filtered, the solvent was removed under reduced pressure, and the crude product was purified by distillation to give 93.0 g of 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane in 68% yield (bp was 185° C.).

[0054] Comparative Example 2: Atomic Layer Deposition of Silicon Oxide Films Using Dimethylaminotrimethylsilane

[0055] Atomic layer deposition of silicon oxide films was performed using the following silicon precursor: dimethylaminotrimethylsilane (DMATMS). The deposition was performed in a laboratory-scale ALD processing tool. The silicon precursor was delivered to the chamber by vapor extraction. All gases (e.g., purge and reactant gases, or precursor and oxygen sources) were preheated to 100° C. before entering the deposition region. Gas and precursor flow rates were controlled using fast-acting ALD diaphragm valves. The substrate used in the deposition was a 12-inch long silicon strip. A thermocouple was attached to the sample holder to check the substrate temperature. The deposition was performed using ozone as the oxygen source gas. The deposition parameters are given in Table 2. Table 2: Process for atomic layer deposition of silicon oxide films with ozone using DMATMS. [Table 2]

[0056] Steps 2-6 were repeated until the desired thickness was reached. The thickness and refractive index of the films were measured using a FilmTek 2000SE ellipsometer by fitting the reflectance data from the films to a predefined physical model (e.g., Lorentz Oscillator model). Wet etch rates were performed using a 1 wt% solution of 49 wt% hydrofluoric (HF) acid in deionized water. For each batch, the solution concentration was confirmed using a thermal oxide wafer as a reference. The wet etch rate of a typical thermal oxide wafer for a 1 wt% HF solution in H2O is 0.5 Å / s. The film thickness before and after etching was used to calculate the wet etch rate. Carbon and nitrogen concentrations in the films were analyzed by dynamic secondary ion mass spectrometry (SIMS) method. The % of non-uniformity was calculated from six measurements using the following formula: Non-uniformity (%) = ((max-min) / (2·average)). The density of the films was characterized using X-ray reflectometry (XRR). Table 3 summarizes the properties of SiO2 films deposited with a fixed dose (8 s) of DMATMS precursor at wafer temperatures between 600 and 650 °C. Table 3: Properties of silicon oxide films deposited using DMATMS [Table 3] The film density for silicon oxide deposited from DMATMS is 2.08-2.23 g / cc.

[0057] Example 3: 1-Dimethylamino-1,1,2,3,3,3-hexamethyldisilazane vs. DMATMS Precursor Thermal Stability

[0058] 1-Dimethylamino-1,1,2,3,3,3-hexamethyldisilazane and DMATMS as silicon precursors were introduced into the ALD chamber with the following steps: (a) introducing the silicon precursor for 12 seconds; (b) purging with nitrogen gas. Steps (a) and (b) were repeated for 300 cycles. FilmTek 2000SE ellipsometer was used to measure the thickness and refractive index (RI) of the film by fitting the reflectance data from the film to a predefined physical model (e.g., Lorentz Oscillator model). Table 4 summarizes the films formed by thermal deposition of the silazane precursors at temperatures of 600°C and 650°C, respectively, showing that 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane has slightly less decomposition than DMATMS and is therefore a better precursor for high temperature ALD applications. Table 4: Pyrolysis of silazane precursors versus DMATMS [Table 4]

[0059] Example 4: Atomic layer deposition of silicon oxide films using 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane

[0060] Atomic layer deposition of silicon oxide films was performed using the following silicon precursor: 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane. Deposition was performed in a laboratory-scale ALD processing tool. The silicon precursor was transported into the chamber by vapor extraction. The deposition process and parameters are given in Table 2. Steps 2-6 were repeated for 500 cycles until the desired thickness was reached. The deposition process parameters, deposition rate, refractive index, and wet etch rate (WER) using a 1% solution of 49% hydrofluoric (HF) acid in deionized water are given in Table 5. Table 5: Summary of process parameters and results for 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane [Table 5] It is seen that the silicon precursor, 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane, results in a slightly higher deposition rate (Å / cycle) and lower WER than DMATMS at a given temperature.

[0061] Although the present disclosure has been described with reference to certain preferred embodiments, those skilled in the art will recognize that various modifications can be made without departing from the scope of the invention, and that permeants can substitute elements thereof. In addition, many modifications can be made to adapt a particular situation or material to the teachings of the invention without departing from the essential scope thereof. Therefore, it is not intended that the invention be limited to the particular embodiments, but it is intended that the invention include all embodiments falling within the scope of the appended claims. The present invention can be embodied in the following manner. (Appendix 1) 1. A process for depositing a silicon oxide film on a substrate, comprising: a) providing a substrate in a reactor; b) the following formula IA: [ka] wherein R 1 and R 2 But, C 1 ~C 6 R is independently selected from alkyl groups; 3 is hydrogen, linear or branched C 1 ~C 6 Alkyl group and C 6 ~C 10 aryl groups; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 but not linked to form a cyclic ring structure; c) purging the reactor with a purge gas to purge unconsumed reactants and / or reaction by-products; d) introducing an oxygen source into the reactor to react with the precursor to form a silicon oxide film; and e) purging the reactor with a purge gas to purge unconsumed reactants and / or reaction by-products. wherein steps b through e are repeated until a desired thickness of the silicon oxide film is deposited, and is conducted at one or more temperatures between 500 and 800° C., and at one or more pressures between 50 milliTorr (mT) and 760 Torr. (Appendix 2) The at least one organic aminodisilazane precursor is selected from the group consisting of 1-dimethylamino-1,1,3,3,3-pentamethyldisilazane, 1-diethylamino-1,1,3,3,3-pentamethyldisilazane, 1-methylethylamino-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolidino-1,1,3,3,3-pentamethyldisilazane, 1-(2-methylpyrrolidino)-1,1,3,3,3-pentamethyldisilazane, 1-(2,5-dimethylpyrrolidino)-1,1,3,3,3-pentamethyldisilazane, 1-piperidino-1,1,3,3,3- Pentamethyldisilazane, 1-(2,6-dimethylpiperidino)-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolyl-1,1,3,3,3-pentamethyldisilazane, 1-imidazolyl-1,1,3,3,3-pentamethyldisilazane, 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-diethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-methylethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-pyrrolidino-1,1,2,3,3,3-hexamethyldisilazane, 1 -(2-Methylpyrrolidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-(2,5-dimethylpyrrolidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-piperidino-1,1,2,3,3,3-hexamethyldisilazane, 1-(2,6-dimethylpiperidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-pyrrolyl-1,1,2,3,3,3-hexamethyldisilazane, 1-imidazolyl-1,1,2,3,3,3-hexamethyldisilazane, 1-dimethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane 1-Diethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-Methylethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-Pyrrolidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-(2-Methylpyrrolidino)-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-2,5-Dimethylpyrrolidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-Piperidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-(2,6-dimethylpiperidino)-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolyl-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-imidazolyl-2-ethyl-1,1,3,3,3-pentamethyldisilazane, and mixtures thereof. (Appendix 3) 2. The process of claim 1, wherein the purge gas is selected from the group consisting of nitrogen, helium, argon, and mixtures thereof. (Appendix 4) 2. The process of claim 1, wherein the oxygen source is selected from the group consisting of oxygen, peroxide, oxygen plasma, water vapor, water vapor plasma, hydrogen peroxide, an ozone source, and mixtures thereof. (Appendix 5) 2. The process of claim 1, wherein the oxygen-containing source comprises a plasma. (Appendix 6) 6. The process of claim 5, wherein the plasma is generated in situ. (Appendix 7) 6. The process of claim 5, wherein the plasma is generated remotely. (Appendix 8) The silicon oxide film has a thickness of about 2.0 g / cm 3 The process of claim 4, wherein the density is equal to or greater than 1. (Appendix 9) 2. The process of claim 1, wherein the silicon oxide film further comprises carbon. (Appendix 10) The silicon oxide film has a thickness of at least about 1.8 g / cm 3 10. The process of claim 9, wherein the crystalline cellulose has a density of (Appendix 11) 10. The process of claim 9, wherein the carbon content of the silicon oxide film is at least 0.5 atomic weight percent (at %) as measured by X-ray photoelectron spectroscopy. (Appendix 12) 1. A composition for depositing a silicon oxide film or a carbon-doped silicon oxide film using a vapor deposition process, comprising:

change

Claims

1. 1. A process for depositing a silicon oxide film on a substrate, comprising: a) providing a substrate in a reactor; b) a compound of formula IA: 【Chemistry 1】 wherein R 1 and R 2 But, C 1 ~C 6 R is independently selected from alkyl groups; 3 is hydrogen, linear or branched C 1 ~C 6 Alkyl group and C 6 ~C 10 aryl groups; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 but not linked to form a cyclic ring structure; c) purging the reactor with a purge gas to purge unconsumed reactants and / or reaction by-products; d) introducing an oxygen source into the reactor to react with the precursor to form a silicon oxide film; and e) purging the reactor with a purge gas to purge unconsumed reactants and / or reaction by-products. wherein steps b through e are repeated until a desired thickness of said silicon oxide film is deposited, and is conducted at one or more temperatures between 500 and 800° C., and at one or more pressures between 50 milliTorr (mT) and 760 Torr.

2. The at least one organoaminodisilazane precursor may be selected from the group consisting of 1-dimethylamino-1,1,3,3,3-pentamethyldisilazane, 1-diethylamino-1,1,3,3,3-pentamethyldisilazane, 1-methylethylamino-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolidino-1,1,3,3,3-pentamethyldisilazane, 1-(2-methylpyrrolidino)-1,1,3,3,3-pentamethyldisilazane, 1-(2,5-dimethylpyrrolidino)-1,1,3,3,3-pentamethyldisilazane, 1-piperidino-1,1,3,3,3- Pentamethyldisilazane, 1-(2,6-dimethylpiperidino)-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolyl-1,1,3,3,3-pentamethyldisilazane, 1-imidazolyl-1,1,3,3,3-pentamethyldisilazane, 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-diethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-methylethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-pyrrolidino-1,1,2,3,3,3-hexamethyldisilazane, 1 -(2-methylpyrrolidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-(2,5-dimethylpyrrolidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-piperidino-1,1,2,3,3,3-hexamethyldisilazane, 1-(2,6-dimethylpiperidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-pyrrolyl-1,1,2,3,3,3-hexamethyldisilazane, 1-imidazolyl-1,1,2,3,3,3-hexamethyldisilazane, 1-dimethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane 1-diethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-methylethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-(2-methylpyrrolidino)-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-2,5-dimethylpyrrolidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-piperidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-(2,6-dimethylpiperidino)-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolyl-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-imidazolyl-2-ethyl-1,1,3,3,3-pentamethyldisilazane, and mixtures thereof.

3. 2. The process of claim 1, wherein the purge gas is selected from the group consisting of nitrogen, helium, argon, and mixtures thereof.

4. 2. The process of claim 1, wherein the oxygen source is selected from the group consisting of oxygen, peroxide, oxygen plasma, water vapor, water vapor plasma, hydrogen peroxide, an ozone source, and mixtures thereof.

5. The process of claim 1 , wherein the oxygen source comprises a plasma.

6. The process of claim 5 , wherein the plasma is generated in situ.

7. The process of claim 5 , wherein the plasma is generated remotely.

8. The silicon oxide film has a thickness of about 2.0 g / cm 3 The process of claim 4 having a density of at least about 100%.

9. The process of claim 1 , wherein the silicon oxide film further comprises carbon.

10. The silicon oxide film has a thickness of at least about 1.8 g / cm 3 The process of claim 9 having a density of

11. 10. The process of claim 9, wherein the carbon content of the silicon oxide film is at least 0.5 atomic weight percent (at %) as measured by X-ray photoelectron spectroscopy.

12. 1. A composition for depositing a silicon oxide film or a carbon-doped silicon oxide film using a vapor deposition process, comprising: 【Chemistry 2】 wherein R 1 and R 2 But, C 1 ~C 6 alkyl group; R 3 is hydrogen, linear or branched C 1 ~C 6 Alkyl group and C 6 ~C 10 aryl groups; R 1 and R 2 are linked together to form a cyclic ring structure, or R 1 and R 2 but are not linked to form a cyclic ring structure.

13. The at least one silicon precursor is selected from the group consisting of 1-dimethylamino-1,1,3,3,3-pentamethyldisilazane, 1-diethylamino-1,1,3,3,3-pentamethyldisilazane, 1-methylethylamino-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolidino-1,1,3,3,3-pentamethyldisilazane, 1-(2-methylpyrrolidino)-1,1,3,3,3-pentamethyldisilazane, 1-(2,5-dimethylpyrrolidino)-1,1,3,3,3-pentamethyldisilazane, and 1-piperidino-1,1,3,3,3-pentamethyldisilazane. Disilazane, 1-(2,6-dimethylpiperidino)-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolyl-1,1,3,3,3-pentamethyldisilazane, 1-imidazolyl-1,1,3,3,3-pentamethyldisilazane, 1-dimethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-diethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-methylethylamino-1,1,2,3,3,3-hexamethyldisilazane, 1-pyrrolidino-1,1,2,3,3,3-hexamethyldisilazane, 1-(2- 1-(2,5-dimethylpyrrolidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-piperidino-1,1,2,3,3,3-hexamethyldisilazane, 1-(2,6-dimethylpiperidino)-1,1,2,3,3,3-hexamethyldisilazane, 1-pyrrolyl-1,1,2,3,3,3-hexamethyldisilazane, 1-imidazolyl-1,1,2,3,3,3-hexamethyldisilazane, 1-dimethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane Silazane, 1-diethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-methylethylamino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-pyrrolidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-(2-methylpyrrolidino)-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-2,5-dimethylpyrrolidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-piperidino-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-(2,The composition according to claim 12, wherein the silyl group is selected from the group consisting of 1-pyrrolyl-2-ethyl-1,1,3,3,3-pentamethyldisilazane, 1-imidazolyl-2-ethyl-1,1,3,3,3-pentamethyldisilazane, and combinations thereof.

14. 13. The composition of claim 12, wherein the at least one silicon precursor is substantially free of one or more impurities selected from the group consisting of halides, metal ions, metals, and combinations thereof.

15. 15. The composition of claim 14, which is substantially free of one or more impurities selected from the group consisting of halide compounds, metal ions, metals, and combinations thereof.

16. The composition of claim 15 , wherein the halide compound comprises a chloride-containing species.

17. 17. The composition of claim 16, wherein the chloride concentration is less than 50 ppm as measured by IC.

18. 17. The composition of claim 16, wherein the chloride concentration is less than 10 ppm as measured by IC.

19. 17. The composition of claim 16, wherein the chloride concentration is less than 5 ppm as measured by IC.

Citation Information

Patent Citations

  • Surface treatment agent and surface treatment method

    JP2011049468A

  • High temperature atomic layer deposition of silicon oxide thin films

    JP2013236073A

  • High temperature atomic layer deposition of silicon oxide thin films

    US20130295779A1

  • Trisilylamine Derivatives as Precursors for High Growth Rate Silicon-Containing Films

    US20190085452A1