Wet-laid nonwoven fabric for semipermeable membrane support and method for producing same
A wet-laid nonwoven fabric production method using polyester fibers and controlled heating and pressing processes addresses the strength loss issue in wet conditions, preventing curling and ensuring stable semipermeable membrane application.
Patent Information
- Application Number
- JP2020215561
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-12-24
- Publication Date
- 2024-11-20
- Estimated Expiration
- 2040-12-24
AI Technical Summary
Nonwoven fabrics used as supports for semipermeable membranes suffer significant strength loss when wet, leading to curling and deformation during the drying process after coating with a polymer solution.
A method involving the production of a wet-laid nonwoven fabric using polyester fibers, with specific heating and pressing processes to maintain tensile strength, reducing the tensile strength reduction rate to 10% or less in a wet state, achieved through controlled heating and pressing steps.
The method effectively suppresses curling and maintains strength in the nonwoven fabric during the drying process, ensuring stable application of semipermeable membranes.
Smart Images

Figure 0007587414000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a wetlaid nonwoven fabric, and more particularly to a wetlaid nonwoven fabric for use as a semipermeable membrane support for use in semipermeable membranes having a separation function, such as ultrafiltration membranes, microfiltration membranes, and reverse osmosis (RO) membranes, and a method for producing the same. [Background technology]
[0002] In recent years, the applications of semipermeable membranes have been increasing, including the removal of impurities from drinking / industrial water, desalinization of seawater, removal of germs from food, wastewater treatment, and in the biochemistry field. Currently, the main markets are Europe, the US, China, and Korea, but in the future, it is expected that they will also be used in water treatment to alleviate water shortages in the Middle East and improve hygiene, and production and usage volumes both in Japan and overseas are continuing to increase.
[0003] In general, a semipermeable membrane is produced by a method of coating and fixing a solution of a polymer that is a raw material of the semipermeable membrane on a support such as a nonwoven fabric or a woven fabric. There is also a method of coating a solution of a polymer on the support in advance to form a support layer, and then forming a semipermeable membrane.
[0004] Therefore, the nonwoven fabric or other support must be such that when a polymer solution is applied to the non-coated surface, defects such as film defects or pinholes due to strike-through or fluffing of the support do not occur.
[0005] As the material for the semipermeable membrane, various polymers such as regenerated cellulose, cellulose derivatives, polyvinyl alcohol, polysulfone, polyamide, etc. are selected according to the application. However, the membrane itself is weak in strength and cannot withstand the high pressure of 1 to 10 MPa when used alone for ultrafiltration or reverse osmosis. Therefore, it is necessary to generate the membrane on a support such as a nonwoven fabric that is strong and has high liquid permeability.
[0006] In order to obtain the required liquid permeability, tensile strength, wet strength, and durability, the support generally used is a nonwoven fabric in which synthetic fibers such as polyester or polyolefin are formed into a sheet by a wet or dry process and then heated and pressurized to melt and bond the synthetic fibers together.
[0007] Nonwoven fabrics as semipermeable membrane supports and their manufacturing methods are publicly known. For example, a semipermeable membrane support has been proposed that is made of a main fiber made of polyester fiber and a binder fiber, and is manufactured by heating and pressurizing the nonwoven fabric after papermaking, and that has a tensile strength ratio of 2:1 to 1:1 in the papermaking flow direction and the width direction, and that has a surface roughness of the front and back sides of the support that is 15% or more larger than the back side roughness, so that the support can be transported with rolls without bending in the width direction even when a semipermeable membrane liquid is applied thereto, and can be treated in a coagulation washing tank without any problems (see, for example, Patent Document 1).
[0008] Also, a nonwoven fabric has been proposed that has little warping and excellent dimensional stability under high temperature conditions by providing a difference in smoothness between the front and back sides (see, for example, Patent Document 2).
[0009] Also proposed is a separation membrane comprising a separation membrane body and a flow path material, the flow path material containing at least 50 to 97% by weight of a polyolefin resin and 3 to 50% by weight of a thermoplastic elastomer resin, the polyolefin resin having a crystallinity of 20 to 50% (see, for example, Patent Document 3). [Prior art documents] [Patent documents]
[0010] [Patent Document 1] JP 2002-095937 A [Patent Document 2] Patent No. 4668210 [Patent Document 3] JP 2015-27666 A Summary of the Invention [Problem to be solved by the invention]
[0011] However, the nonwoven fabrics of Patent Documents 1 to 3 have a problem that their strength is significantly reduced when they become wet during the process of providing a semipermeable membrane. If the strength of the nonwoven fabric is significantly reduced in a wet state, the nonwoven fabric under tension may curl when the surface coated with the polymer solution (membrane-forming surface) is dried, causing problems such as deformation of the semipermeable membrane.
[0012] In view of such problems, an object of the present disclosure is to provide a wetlaid nonwoven fabric for semipermeable membrane supporting material, which is less likely to curl after thermal drying by reducing the decrease in strength in a wet state, and a method for producing the same. [Means for solving the problem]
[0013] The method for producing a wet nonwoven fabric for a semipermeable membrane support according to the present invention comprises the steps of: preparing a fiber raw material slurry containing only polyester fibers as a fiber component; making the fiber raw material slurry into a paper and dewatering it to obtain a wet sheet; drying the wet sheet to obtain a dry sheet; a first heating and pressurizing step of heating the dry sheet in a thermal calendar device set to a heating condition of 200° C. to 260° C. while pressing both sides to obtain a sheet that has been subjected to a heating and pressurizing treatment; a temperature-reducing step of lowering the temperature of the sheet that has been subjected to the heating and pressurizing treatment; and a second heating and pressurizing step of, when the temperature of the sheet that has been subjected to the temperature-reducing step is 135° C. to 156° C., pressing both sides of the sheet again in a thermal calendar device set to a heating condition of 200° C. to 260° C. to obtain a sheet that has been subjected to a second heating and pressurizing treatment, wherein the sheet that has been subjected to the second heating and pressurizing treatment is a wet nonwoven fabric having a tensile strength reduction rate X in a wet state represented by (Equation 1) to (Equation 3) of 10% or less. . (Equation 1) The decrease rate of tensile strength in the wet state in the machine direction (MD) M (%) = (A MD -B MD ) / A MD ×100 A MD : Tensile strength in machine direction (MD) (JIS P8113:2006) B MD : Wet tensile strength in machine direction (MD) (JIS P8135:1998) (Equation 2) The decrease rate of tensile strength in the wet state in the cross (CD) direction C (%) = (A CD -B CD ) / A CD ×100 A CD : Tensile strength in transverse (CD) direction (JIS P8113:2006) B CD : Wet tensile strength in transverse (CD) direction (JIS P8135:1998) (Equation 3) Decrease rate of tensile strength in wet state X (%) = (decrease rate M + decrease rate C) / 2
[0014] In the method for producing a wetlaid nonwoven fabric for semipermeable membrane supporting material according to the present invention, in the second heating and pressing step for obtaining a sheet subjected to the second heating and pressing treatment, the sheet that has been subjected to the temperature-lowering step at 135° C. or higher and 156° C. or lower is preferably a sheet immediately before being cooled to less than 135° C. in the temperature-lowering step, or a sheet that has been cooled to less than 135° C. in the temperature-lowering step and then heated again to 135° C. or higher. A wetlaid nonwoven fabric having an increased crystallinity of polyester fibers can be produced.
[0015] In the method for producing a wetlaid nonwoven fabric for a semipermeable membrane support according to the present invention, it is preferable that the polyester fibers contain polyester fibers having a primary crystallization temperature of 115° C. or higher. A wetlaid nonwoven fabric having a further increased crystallinity of the polyester fibers can be produced. In the method for producing a wetlaid nonwoven fabric for a semipermeable membrane support according to the present invention, it is preferable that the sheet tension in the first heating and pressing step and the second heating and pressing step is higher than the sheet tension in the drying step.
[0016] The wet-laid nonwoven fabric for semipermeable membrane supporting material according to the present invention is A semi-finished product containing only polyester fiber as a fiber component. A wet-laid nonwoven fabric for a membrane support, comprising: The polyester fiber includes a main fiber and a binder fiber, the main fiber being a polyethylene terephthalate fiber, The wetlaid nonwoven fabric has a front surface and a back surface that have been subjected to a heat and pressure treatment, and is characterized in that the rate of decrease X in tensile strength in a wet state, which is expressed by (Equation 1) to (Equation 3), is 10% or less. (Equation 1) The decrease rate of tensile strength in the wet state in the machine direction (MD) M (%) = (A MD -B MD ) / A MD ×100 A MD : Tensile strength in machine direction (MD) (JIS P8113:2006) B MD : Wet tensile strength in machine direction (MD) (JIS P8135:1998) (Equation 2) The decrease rate of tensile strength in the wet state in the cross (CD) direction C (%) = (A CD -B CD ) / A CD ×100 A CD : Tensile strength in transverse (CD) direction (JIS P8113:2006) B CD : Wet tensile strength in transverse (CD) direction (JIS P8135:1998) (Equation 3) Decrease rate of tensile strength in wet state X (%) = (decrease rate M + decrease rate C) / 2
[0017] In the wetlaid nonwoven fabric for semipermeable membrane support according to the present invention, the polyester fibers preferably include polyester subject fibers and polyester binder fibers, and the polyester binder fibers are melt-bonded to the polyester subject fibers at least on the front and back surfaces of the wetlaid nonwoven fabric, and the polyester subject fibers are melt-bonded to each other. After papermaking, a drying process is performed to melt-bond the polyester binder fibers to the polyester subject fibers, and a heating and pressing process is further performed to melt-bond the polyester subject fibers to each other, thereby increasing the strength of the wetlaid nonwoven fabric.
[0018] In the wetlaid nonwoven fabric for semipermeable membrane support according to the present invention, the mass of the polyester binder fibers relative to the total mass of the polyester subject fibers and the polyester binder fibers is preferably 20% by mass or more and 38% by mass or less. By setting such a blending ratio, the wetlaid nonwoven fabric can be suitably heated and pressurized, and an appropriate amount of fiber can be left in the wetlaid nonwoven fabric, thereby stabilizing the quality of the wetlaid nonwoven fabric in a wet state.
[0019] In the wetlaid nonwoven fabric for semipermeable membrane support according to the present invention, the wetlaid nonwoven fabric preferably contains only polyethylene terephthalate fibers as a fiber component, which is excellent in heat resistance, chemical resistance, economical efficiency, and variety.
[0020] In the wet-laid nonwoven fabric for semipermeable membrane supporting material according to the present invention, the sheet density of the wet-laid nonwoven fabric is 0.5 g / cm 3 It is preferable that the above is satisfied. This can improve the suitability of the semipermeable membrane coating solution for application to the wetlaid nonwoven fabric. Effect of the Invention
[0021] By using the wetlaid nonwoven fabric for semipermeable membrane support of the present disclosure, the decrease in strength when the fabric is in a wet state during the process of providing the semipermeable membrane is reduced, and as a result, curling during the drying process after semipermeable membrane coating is suppressed. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, the present invention will be described in detail with reference to the embodiments, but the present invention is not limited to these descriptions. Various modifications of the embodiments may be made as long as the effects of the present invention are achieved.
[0023] The nonwoven fabric for semipermeable membrane support according to this embodiment is mainly composed of polyester fibers. As the polyester fibers, polyethylene terephthalate fibers, polyethylene naphthalate fibers, polytributylene terephthalate fibers, etc. can be used. In addition to polyester fibers, fibers spun from synthetic resins such as polyethylene, polypropylene, polyacrylate, polyurethane, polyvinyl chloride, polyvinylidene chloride, polyethylene fluoride, polyaramid, polyimide, polyacrylonitrile, and nylon can be used within a range that does not impair the effects of the present invention. Furthermore, fibers made from regenerated cellulose such as rayon, cellulose derivatives such as cellulose acetate and nitrocellulose, and natural products such as polylactic acid, polybutyric acid, and polysuccinic acid, which have been actively researched in recent years for biochemical applications, can also be used. The wet-laid nonwoven fabric for semipermeable membrane support according to this embodiment contains polyester fibers as a fiber component in a range of 90% by mass or more and 100% by mass or less. From the viewpoint of increasing the stability of quality, it is preferable that the blending ratio of polyester fibers is high, and more preferably 95% by mass or more. In this embodiment, it is preferable to use only polyester fibers, and more preferably to use only polyethylene terephthalate fibers, because of their heat resistance, chemical resistance, low cost, and wide variety of fiber diameters and properties.
[0024] In this embodiment, polyester fibers, which are the main components of the nonwoven fabric for semipermeable membrane support, are divided into main fibers and binder fibers. Polyester fibers that are not intended for melt adhesion at low temperatures are called main fibers. Regarding the shape of the main fibers, if a fiber diameter is small, the pore size of the completed sheet becomes smaller, and if a fiber diameter is large, the strength of the sheet increases. If a fiber having a short fiber is used, the dispersibility in water in the wet papermaking process improves, and if a fiber having a long fiber is used, the strength of the sheet increases. In this embodiment, the main fiber is preferably used with a thickness of 0.05 to 5.0 decitex, preferably 0.1 to 2.0 decitex, and a length of 1 to 8 mm, preferably 3 to 6 mm. In addition, the cross-sectional shape of the main fiber can be appropriately selected as necessary, and is not limited in this embodiment. The polyester fiber main fiber has a melting point of about 220 to 260°C, preferably 230 to 255°C.
[0025] If necessary, it is also possible to blend as the main fiber a pulp-like raw material, for example wood pulp for papermaking, or synthetic resin pulp such as polyethylene, polypropylene, acrylic, or aramid, or inorganic fibers such as glass fiber, silica fiber, or alumina fiber. Even when blending these main fibers, the wetlaid nonwoven fabric must contain polyester fiber in the range of 90% by mass or more and 100% by mass or less as a fiber component.
[0026] The wetlaid nonwoven fabric for semipermeable membrane supporting material according to this embodiment can also be blended with inorganic fillers such as calcium carbonate, talc, kaolin, etc., as required.
[0027] In this embodiment, binder fibers can be used to obtain sufficient sheet strength during the sheet forming process and winding process. The binder fibers generally refer to synthetic fibers with a melting point about 20°C or more lower than that of the main fiber, preferably 25°C or more lower, and have the effect of melting and bonding the surface by heating in the drying process after papermaking, and imparting tensile strength to the sheet that enables operation. However, since the tensile strength of the fiber itself is inferior to that of the main fiber, it is necessary to set a blending ratio that balances ease of operation and strength of the finished product. In this embodiment, the blending amount of polyester binder fibers is preferably 20 to 38 mass% of the total polyester fibers (total amount of polyester main fiber and polyester binder fiber), and more preferably 25 to 35 mass%. Within this range, heat and pressure treatment can be suitably performed, and an appropriate amount of fiber can be left, so that the quality can be stabilized in a wet state. If the binder fiber is less than 20 mass%, the strength is weak at the papermaking stage of the wet nonwoven fabric, and a stable base paper cannot be obtained. On the other hand, if the binder fiber content exceeds 38% by mass, the material can be fused satisfactorily in the heating and pressurizing step, but since a large amount of amorphous fiber is present, it may be difficult to maintain strength in a wet state.
[0028] There are binder fibers in which all of the constituent resins are melted, and types in which only the surface is melted, having a double structure with an inner and outer side, that is, a core-sheath structure, and all of these can be used in the present embodiment. Polyester unstretched fibers having a melting point of about 200 to 260°C, preferably 210 to 250°C, are preferably used. In addition, the thickness, length, cross-sectional shape, etc. can be selected according to the purpose, as in the case of the main fiber. The binder fiber is preferably of the same or similar resin composition as the main fiber, but a different resin composition can also be used according to the required characteristics. In addition, vinylon binder fibers, which have the property of dissolving under moist and hot conditions, are also preferably used. Furthermore, wood pulp for papermaking, which has self-adhesiveness due to hydrogen bonding, can also be used as a binder. Even when a binder fiber other than polyester binder fiber is blended, it is necessary for the wetlaid nonwoven fabric to satisfy the requirement that the fiber component contains polyester fiber in the range of 90% by mass to 100% by mass.
[0029] In this embodiment, the sheet density is 0.5 g / cm 3 In order to improve the applicability of the semipermeable membrane coating liquid to the wet nonwoven fabric, it is necessary to increase the sheet density of the nonwoven fabric substrate and reduce the air permeability. The sheet density is preferably 0.6 g / cm or more. 3 More preferably, 0.7 g / cm or more is more preferable, and even more preferably 0.7 g / cm 3 That's it. 0.5g / cm 3 If the density is less than 1.2 g / cm, the coating liquid will penetrate too much into the nonwoven fabric substrate, resulting in uneven coating layer and surface. In addition, the coating liquid will penetrate in the Z-axis direction, which may lead to defects in the film or pinholes. The upper limit of the sheet density is, for example, 1.2 g / cm. 3 That's all.
[0030] The air permeability of the wetlaid nonwoven fabric according to the present embodiment is preferably 50 Pa to 3000 Pa, more preferably 80 Pa to 1500 Pa, as a pressure loss at a surface air velocity of 5.3 cm / sec. of the wetlaid nonwoven fabric. Here, the pressure loss is an index showing the air permeability of the wetlaid nonwoven fabric, and the higher the pressure loss, the lower the air permeability. If the pressure loss is less than 50 Pa, as described above, the coating liquid of the semipermeable membrane will penetrate too much into the nonwoven fabric substrate sheet, causing the coating layer and the surface to become nonuniform, and may also cause strike-through. On the other hand, if the pressure loss is greater than 3000 Pa, the coating liquid will not easily penetrate into the nonwoven fabric substrate sheet, causing the coating layer to adhere poorly to the surface of the nonwoven fabric substrate sheet, and the coating layer may easily peel off from the substrate sheet.
[0031] As a method for producing a wet-laid nonwoven fabric for semipermeable membranes, a so-called wet papermaking method is used, in which fibers are dispersed in water, then the fibers are layered on a papermaking wire, and water is removed from below the wire to form a sheet. The type of papermaking machine used here is not limited in this embodiment, and for example, a sheet-fed papermaking device or a continuous papermaking machine such as a fourdrinier papermaking machine, a short-wire papermaking machine, a cylinder papermaking machine, an inclined wire papermaking machine, a gap former, or a delta former can be used. At this time, in order to obtain a wet-laid synthetic nonwoven fabric for semipermeable membrane supports with few defects, it is desirable to form the sheet as uniformly and with good texture as possible.
[0032] Since the paper-made sheet contains a large amount of moisture, it is dried in a drying zone. The drying method is not particularly limited, but hot air drying, infrared drying, drum drying, drying with a Yankee dryer, etc. are preferably used. The drying temperature is preferably 100 to 160°C.
[0033] Although the wetlaid nonwoven fabric after the papermaking process and the drying process has some adhesion due to softening of the binder fibers, it is insufficient in strength as a semipermeable membrane support as it is and has poor suitability for coating of the semipermeable membrane. Therefore, in order to obtain sufficient strength as a semipermeable membrane support, a heating and pressurizing treatment is performed at a temperature near the melting point of the main fiber, for example, at a temperature of -55°C to +5°C relative to the melting point of the main fiber, thereby not only melt-bonding the binder fibers but also melt-bonding the main fiber to increase the strength. This treatment can be performed using various heat and pressure processing devices, but a thermal calendar device is generally effective. For example, a method using a metal roll nip calendar that can be treated at a temperature of 200°C or higher, or a soft nip calendar of metal roll / resin roll can be used if the resin roll has high heat resistance. The temperature condition is preferably in the range of 200°C to 260°C, and more preferably 205°C to 240°C. In the heating and pressing process, sufficient heat is applied to appropriately melt the polyester main fiber, so that the main fiber is sufficiently fused to each other, and the decrease in strength in a wet state can be reduced. If the temperature in the heating and pressing process in the thermal calendar device is less than 200°C, the heat is insufficient, and there is a risk that the decrease in strength in a wet state cannot be suppressed. On the other hand, if the temperature condition exceeds 260°C, the main fiber melts, but it becomes easy to adhere to the roll in the heating and pressing process, and not only the surface of the nonwoven fabric becomes rough, but also the roll becomes dirty, making it impossible to perform stable heating and pressing. In addition to the temperature during the heating and pressing process, the suppression of the decrease in strength in a wet state is also affected by the pressing conditions and sheet tension. Although it depends on the heating temperature, as a pressing condition, the higher the linear pressure, the easier it is to suppress the decrease in strength in a wet state. For example, when the temperature is 200 to 260°C, the linear pressure is preferably in the range of 50 to 250 kN / m, and more preferably 100 to 230 kN / m. In addition, the higher the sheet tension, the easier it is to suppress the decrease in strength in a wet state. It is preferable to set the sheet tension in the heating and pressing step higher than that in the drying step. Furthermore, in order to achieve uniform performance throughout the nonwoven fabric, it is desirable to perform the treatment with a temperature profile and linear pressure profile as uniform as possible. The roll diameter of the thermal calendaring device is appropriately selected depending on parameters such as the substrate to be heat-pressurized, nip pressure, and speed.
[0034] Here, we will discuss the decrease in strength of nonwoven fabrics in a wet state. Generally, resins such as polyethylene terephthalate and methacrylic resins have some degree of water absorption. In crystalline resins, the degree of crystallinity is also related to the moisture content, and generally, the higher the degree of crystallinity, the less likely it is to absorb water. This is because the polymer chains are properly arranged, making it difficult for water molecules to penetrate into the crystalline structure. On the other hand, amorphous resins are relatively easy to absorb water, and this moisture weakens the hydrogen bonds between the polymers, causing loosening between the molecules. This loosening between the molecules in the amorphous part results in a decrease in the strength of the fiber in a wet state. If the strength of the nonwoven fabric when wet is too low, it will be more likely to become distorted when a semipermeable membrane is provided, and as a result, it will be more likely to curl during the drying process after the semipermeable membrane is applied. In order to obtain a nonwoven fabric that is less susceptible to loss of strength in a wet state, it is conceivable to use synthetic fibers with a high degree of crystallinity in advance. However, such a nonwoven fabric is prone to insufficient strength in both dry and wet states because the fibers are less likely to fuse together when subjected to heat and pressure treatment. In addition, the density is low, making the semipermeable membrane more susceptible to defects and pinholes.
[0035] In this embodiment, by carrying out the above-mentioned heating and pressurizing treatment, the reduction rate X of the tensile strength in a wet state represented by (Equation 1) to (Equation 3) is set to 15% or less, more preferably 10% or less, and further preferably 6% or less. (Equation 1) The decrease rate of tensile strength in the wet state in the machine direction (MD) M (%) = (A MD -B MD ) / A MD ×100 A MD : Tensile strength in machine direction (MD) (JIS P8113:2006) B MD : Wet tensile strength in machine direction (MD) (JIS P8135:1998) (Equation 2) The decrease rate of tensile strength in the wet state in the cross (CD) direction C (%) = (A CD -B CD ) / A CD ×100 A CD: Tensile strength in transverse (CD) direction (JIS P8113:2006) B CD : Wet tensile strength in transverse (CD) direction (JIS P8135:1998) (Equation 3) Decrease rate of tensile strength in wet state X (%) = (decrease rate M + decrease rate C) / 2
[0036] By adopting such a configuration, it is possible to suppress the decrease in strength of the nonwoven fabric in a wet state, and as a result, the occurrence of curling in the drying process after semipermeable membrane coating is suppressed. If the decrease rate X of the tensile strength in the wet state exceeds 15%, the decrease in strength when wet is large, and the nonwoven fabric cannot withstand the contraction force due to the aggregation of the semipermeable membrane in the drying process after semipermeable membrane coating, and as a result, the occurrence of curling in the nonwoven fabric cannot be suppressed. In addition, the nonwoven fabric after semipermeable membrane coating may be wound into a roll while still in a wet state, and deformation and distortion due to the reduced stress at that time are affected, and as a result, the occurrence of curling in the nonwoven fabric cannot be suppressed. The smaller the decrease rate X of the tensile strength in the wet state, the better, but in reality, the lower limit is about 0.5%.
[0037] As mentioned above, the heat and pressure treatment is very effective in producing a semipermeable membrane support. The heat and pressure treatment using a heat and pressure processing device may be performed once or multiple times, but it is preferable to perform the treatment twice from the viewpoint of efficiently increasing the crystallinity and productivity. As mentioned above, the heat and pressure treatment is preferably performed at a temperature of 200°C or higher. If the nonwoven fabric is treated at such a high temperature, the nonwoven fabric becomes soft and is likely to be distorted or wrinkled, probably because the heat deformation temperature of the polyester fiber is exceeded. Therefore, when the heat and pressure treatment is performed twice, after the first heat and pressure treatment is completed and before the second heat and pressure treatment is performed, the temperature of the nonwoven fabric itself is generally lowered with a cooling roll or the like to prevent the nonwoven fabric from becoming too soft. Specifically, it is common to lower the temperature of the nonwoven fabric to 100°C or less before the second heat and pressure treatment. However, it was found that when the temperature of the nonwoven fabric is lowered by a cooling roll or the like, the crystallinity of the polyester fiber is not easily increased even if a relatively large amount of heat is applied during the second heating and pressurizing treatment, and the decrease rate X of the tensile strength in the wet state tends to increase. In addition, if the amount of heat is insufficient at this time, the amount of heat transferred in the Z-axis direction of the nonwoven fabric is insufficient, so that only the fibers near the surface of the nonwoven fabric are fused, and many of the fibers in the middle layer remain as they are or are in a semi-melted state, which may result in a large decrease rate X of the tensile strength in the wet state. For this reason, in this embodiment, when the heating and pressurizing treatment is performed twice, it is preferable that the surface temperature of the nonwoven fabric immediately before the second heating and pressurizing treatment is 130°C or higher. More preferably, it is 135°C or higher. If the surface temperature of the nonwoven fabric is less than 130°C, it may be difficult to keep the decrease rate X of the tensile strength in the wet state to 15% or less. The polyester fibers to be blended preferably contain polyester fibers having a primary crystallization temperature of 115° C. or more, and more preferably contain polyester fibers having a primary crystallization temperature of 115° C. or more and less than 130° C. A wetlaid nonwoven fabric having an even higher degree of crystallinity of the polyester fibers can be produced.The method for raising the surface temperature of the nonwoven fabric to 130° C. or higher immediately before the second heating and pressurizing treatment is not particularly limited, but it is preferable to carry out the first heating and pressurizing treatment at 200° C. or higher, for example, to raise the surface temperature of the nonwoven fabric to 130° C. or higher, and then to carry out the second heating and pressurizing treatment immediately, i.e., before the surface temperature of the nonwoven fabric drops below 130° C. Also, for example, if the first heating and pressurizing treatment is carried out at 200° C. or higher and the surface temperature of the nonwoven fabric is raised to 130° C. or higher, but then the temperature drops below 130° C., the nonwoven fabric may be heated to 130° C. or higher and then the second heating and pressurizing treatment may be carried out.
[0038] If the amount of heat during the heating and pressurizing treatment is insufficient, the amount of heat in the Z-axis direction of the nonwoven fabric will be insufficient, so that only the fibers near the surface of the nonwoven fabric will fuse, and the fibers in the middle layer will remain as they are or will be in a semi-melted state. In this case, there is a risk of the strength decreasing when the semipermeable membrane becomes wet during the process of processing.
[0039] In the multiple heat and pressure treatment, the same heat and pressure device may be used repeatedly for the first and second treatments onward, or multiple heat and pressure devices may be used for continuous treatment, or a calender device with multiple heat calender rolls arranged in the height direction may be used. The treatment temperature for the first and second treatments onward is preferably the same as or higher than the first treatment in order to promote fiber melting and crystallization of the support, but this is not essential.
[0040] In the method of continuously treating the fibers by disposing a plurality of heat and pressure devices, it is preferable to dispose at least one metal roll / metal roll hard nip calendar. More preferably, two or more are disposed. If only a metal roll / resin roll soft nip calendar is used, the remelting effect of the fibers is weak, and the strength in the wet state cannot be maintained. If heat and pressure treatment is performed with a hard nip calendar at least once, the fiber melting and crystallization are promoted to a certain extent by the hard nip effect, and a sufficient amount of heat can be applied even in combination with a soft nip calendar. EXAMPLES
[0041] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. In the examples, "parts" and "%" respectively refer to "parts by mass" and "% by mass" calculated on a solid content basis, unless otherwise specified.
[0042] <Example 1> (Preparation of fiber raw material slurry) 70 kg of polyester subject fiber (product name: EP133, manufactured by Kuraray Co., Ltd., stretched fiber, crystallization temperature 230-260°C, melting point 255°C) having a thickness of 1.45 decitex and a cut length of 5 mm and 30 kg of polyester binder fiber (product name: TR07N, manufactured by Teijin Fibers Limited, unstretched fiber, primary crystallization temperature 115-130°C, secondary crystallization temperature 220-260°C, melting point 255°C) having a thickness of 1.2 decitex and a cut length of 5 mm were added to water so that the mass blending ratio of the polyester subject fiber to the polyester binder fiber was 70:30, and the mixture was dispersed for 5 minutes using a disperser. Further water was then added to obtain a fiber slurry having a fiber concentration of 0.03%.
[0043] (Sheet Creation) The resulting fiber slurry was used to make paper using a short-wire papermaking machine, and the paper was dried using a cylinder dryer at a surface temperature of 120°C to produce a paper with a basis weight of 55 g / m 2 With this goal in mind, we obtained a nonwoven fabric sheet.
[0044] (heat and pressure treatment) The nonwoven fabric sheet was subjected to a heat and pressure treatment using a metal roll / metal roll hard nip thermal calendar device equipped with a metal roll having a face length of 1170 mm and a roll diameter of 450 mm (circumference length of 1413 mm) under the conditions of a roll surface temperature of 235°C, a roll clearance of 80 µm, a linear pressure of 150 kN / m, a processing speed of 5 m / min, and a paper passing number of two times, to obtain a basis weight of 55.0 g / m. 2 , thickness 0.071mm, sheet density 0.77g / cm 3 The surface temperature of the nonwoven fabric before the second heating and pressurizing treatment was 141°C before decreasing to 130°C.
[0045] < reference Example 2> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the mass blending ratio of the polyester subject fibers to the polyester binder fibers was set to 62:38 and the roll surface temperature in the heat and pressure treatment was changed to 205° C. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 56.0 g / m 2 , thickness 0.061mm, sheet density 0.92g / cm 3 The surface temperature of the nonwoven fabric before the second heating and pressurizing treatment was 132°C before dropping to 130°C.
[0046] <Example 3> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the mass blending ratio of the polyester subject fibers to the polyester binder fibers was set to 65:35 and the roll surface temperature in the heat and pressure treatment was changed to 210° C. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 54.0 g / m 2 , thickness 0.059mm, sheet density 0.92g / cm 3 The surface temperature of the nonwoven fabric before the second heating and pressurizing treatment was 155°C before decreasing to 130°C.
[0047] <Example 4> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the mass blending ratio of the polyester subject fibers to the polyester binder fibers was 80:20 and the roll surface temperature in the heat and pressure treatment was changed to 235° C. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 57.0 g / m 2 , thickness 0.056mm, sheet density 1.02g / cm 3 The surface temperature of the nonwoven fabric before the second heat and pressure treatment was 156°C before decreasing to 130°C.
[0048] < reference Example 5> A wetlaid nonwoven fabric for semipermeable membrane supporting material was obtained in the same manner as in Example 1, except that the blending ratio of polyester main fiber, polyester binder fiber, and unbeaten LBKP was changed to 62:30:8 by mass. Basis weight: 56.0 g / m 2 , thickness 0.065mm, sheet density 0.86g / cm 3The surface temperature of the nonwoven fabric before the second heat and pressure treatment was 143°C before dropping to 130°C.
[0049] <Comparative Example 1> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the mass blending ratio of the polyester subject fibers to the polyester binder fibers was 60:40 and the roll surface temperature in the heat and pressure treatment was changed to 195° C. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 57.0 g / m 2 , thickness 0.056mm, sheet density 1.02g / cm 3 The surface temperature of the nonwoven fabric before the second heating and pressurizing treatment was 126°C.
[0050] <Comparative Example 2> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the mass blending ratio of the polyester main fiber and the polyester binder fiber was 50:50 and the roll surface temperature in the heat and pressure treatment was changed to 200° C. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 52.0 g / m 2 , thickness 0.057mm, sheet density 0.91g / cm 3 The surface temperature of the nonwoven fabric before the second heating and pressurizing treatment was 120°C.
[0051] <Comparative Example 3> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the number of times of paper passing in the heat and pressure treatment was changed to one. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 56.0 g / m 2 , thickness 0.062mm, sheet density 0.90g / cm 3 Thus, a nonwoven fabric for semipermeable membrane supporting material was obtained.
[0052] <Comparative Example 4> A wet-laid nonwoven fabric for semipermeable membrane supporting materials was obtained in the same manner as in Example 1, except that the roll surface temperature in the heating and pressurizing treatment was changed to 210°C, and the nonwoven fabric was cooled using a cooling roll before the second heating and pressurizing treatment. The obtained wet-laid nonwoven fabric for semipermeable membrane supporting materials had a basis weight of 54.0 g / m 2 , thickness 0.051mm, sheet density 1.06g / cm 3The surface temperature of the nonwoven fabric before the second heating and pressurizing treatment was 100°C.
[0053] The following evaluations were carried out for the Examples and Comparative Examples, and the results are shown in Table 1 together with an outline of the manufacturing method of the nonwoven fabric.
[0054] (decrease rate of tensile strength in wet state X) The sheets obtained in each Example and Comparative Example are used to prepare test pieces with a test width of 15 mm and a test length (average distance between gripping lines) of 180 mm. Then, in accordance with JIS P8113:2006 Paper and Paperboard - Test Method for Tensile Properties, the extension speed of the test pieces is adjusted to 20 mm / min, and the tensile strength (A) is measured in both the longitudinal direction (A longitudinal) and the transverse direction (A transverse). Next, in accordance with JIS P8135:1998 Wet Tensile Strength Test Method, the test pieces prepared in the same manner as for tensile strength (A) are immersed in distilled water for 1 hour, after which the test pieces are taken out of the water and placed on blotting paper, another blotting paper is placed on the test pieces, and the excess water is removed by lightly pressing the blotting paper, and the wet tensile strength (B) is measured. All measurements were performed in an environment of 23°C and 50% RH. From the obtained values of (A longitudinal), (A transverse), (B longitudinal), and (B transverse), the reduction rates M and C of tensile strength in the longitudinal and transverse directions in a wet state were calculated using (Equation 1) and (Equation 2), and the reduction rate X, which is the average value of the reduction rate M in the longitudinal direction and the reduction rate C in the transverse direction, was further calculated using (Equation 3). (Equation 1) The decrease rate of tensile strength in the wet state in the machine direction (MD) M (%) = (A MD -B MD ) / A MD ×100 A MD : Tensile strength in machine direction (MD) (JIS P8113:2006) B MD : Wet tensile strength in machine direction (MD) (JIS P8135:1998) (Equation 2) The decrease rate of tensile strength in the wet state in the cross (CD) direction C (%) = (A CD -B CD ) / A CD ×100 A CD : Tensile strength in transverse (CD) direction (JIS P8113:2006) BCD : Wet tensile strength in transverse (CD) direction (JIS P8135:1998) (Equation 3) Decrease rate of tensile strength in wet state X (%) = (decrease rate M + decrease rate C) / 2
[0055] (moisture) The water droplets on the surface of the sample immersed in water for the wet tensile strength test were lightly wiped off with filter paper, the mass was measured, and the sample was dried in a hot air dryer at 105°C for 2 hours, and the bone dry mass was measured. The difference in mass between the wet sample and the bone dry sample was divided by the wet sample.
[0056] (Curl evaluation) The wet nonwoven fabric for semipermeable membrane support obtained in each Example and Comparative Example was cut to a size of 300 mm wide and 300 mm long, and a 20% solution of polysulfone resin in DMF (dimethylformamide) was applied to the wet nonwoven fabric for semipermeable membrane support using a Mayer bar #12 so that the coating layer thickness was 0.05 mm, and then the fabric was immersed in water to solidify the coating layer and replace the solvent with water. Thereafter, a polyfunctional amine aqueous solution was sprayed onto the wet coated surface, and then a polyfunctional acid halogen was sprayed and interfacially polymerized to form a membrane with a thickness of 20 nm, and the semipermeable membrane was formed by hot air drying under conditions of 150 ° C. x 5 minutes. After drying, the semipermeable membrane was immediately placed on a flat place with the semipermeable membrane facing up and left to stand, and the curl height of the four corners was measured and evaluated by the average value of the four points. The largest curl was rated as 4, the smallest curl was rated as 1, and 1 and 2 were considered to be acceptable. Evaluation criteria 1: 0~30mm or less. Curl is small and good. 2: Between 30mm and 50mm. Curling is visible, but no practical problems. 3: 50mm or more. When the film is rolled up, the edges are bent and wrinkled. 4: It becomes cylindrical. It is in a roll and cannot be wound up.
[0057] [Table 1]
[0058] As is clear from the results shown in Table 1, the wetlaid nonwoven fabrics for semipermeable membrane supporting materials in Examples 1 to 5 were excellent in the curl evaluation.
Claims
1. A method for producing a fiber raw material slurry containing only polyester fibers as a fiber component, A step of making the fiber raw material slurry into paper and dewatering it to obtain a wet sheet; a drying step of drying the wet sheet to obtain a dry sheet; a first heating and pressing step of heating the dried sheet with a thermal calendar device set at a heating condition of 200° C. to 260° C. while pressing both sides of the dried sheet to obtain a heated and pressed sheet; A temperature reducing step of reducing the temperature of the sheet subjected to the heating and pressurizing treatment; and a second heating and pressing step of heating the sheet again while pressing both sides of the sheet with a thermal calendar device set to a heating condition of 200° C. to 260° C. when the temperature of the sheet after the temperature lowering step is 135° C. to 156° C. to obtain a sheet that has been subjected to a second heating and pressing treatment, The sheet subjected to the second heating and pressurizing treatment is a wet-laid nonwoven fabric having a tensile strength reduction rate X in a wet state represented by (Equation 1) to (Equation 3) of 10% or less. (Equation 1) The decrease rate of tensile strength in the wet state in the machine direction (MD) M (%) = (A MD -B MD ) / A MD ×100 A MD : Tensile strength in machine direction (JIS P8113:2006) B MD : Wet tensile strength in machine direction (MD) (JIS P8135:1998) (Equation 2) The decrease rate of tensile strength in the cross (CD) direction in a wet state C (%) = (A CD -B CD ) / A CD ×100 A CD : Tensile strength in transverse (CD) direction (JIS P8113:2006) B CD : Wet tensile strength in transverse (CD) direction (JIS P8135:1998) (Equation 3) Decrease rate of tensile strength in a wet state X (%) = (decrease rate M + decrease rate C) / 2
2. The method for producing a wet-laid nonwoven fabric for semipermeable membrane supporting material according to claim 1, characterized in that in the second heating and pressurizing step for obtaining a sheet subjected to the second heating and pressurizing treatment, the sheet that has been subjected to the temperature-reducing step at 135°C or higher and 156°C or lower is a sheet immediately before being cooled to less than 135°C in the temperature-reducing step, or a sheet that has been once cooled to less than 135°C in the temperature-reducing step and then heated again to 135°C or higher.
3. 3. The method for producing a wet-laid nonwoven fabric for a semipermeable membrane supporting material according to claim 1, wherein the polyester fibers contain polyester fibers having a primary crystallization temperature of 115° C. or higher.
4. A method for producing a wet nonwoven fabric for a semipermeable membrane support described in any one of claims 1 to 3, characterized in that the sheet tension in the first heating and pressing process and the second heating and pressing process is higher than the sheet tension in the drying process.
5. A wet-laid nonwoven fabric for semipermeable membrane supports, comprising only polyester fibers as a fiber component, The polyester fiber includes a subject fiber and a binder fiber, The subject fiber is a polyethylene terephthalate fiber, The front and back surfaces of the wetlaid nonwoven fabric are heat-pressurized treated surfaces, A wet-laid nonwoven fabric for semipermeable membrane supporting bodies, characterized in that the rate of decrease in tensile strength in a wet state, expressed by (Equation 1) to (Equation 3), is 10% or less. (Equation 1) The decrease rate of tensile strength in the wet state in the machine direction (MD) M (%) = (A MD -B MD ) / A MD ×100 A MD : Tensile strength in machine direction (JIS P8113:2006) B MD : Wet tensile strength in machine direction (MD) (JIS P8135:1998) (Equation 2) The decrease rate of tensile strength in the cross (CD) direction in a wet state C (%) = (A CD -B CD ) / A CD ×100 A CD : Tensile strength in transverse (CD) direction (JIS P8113:2006) B CD : Wet tensile strength in transverse (CD) direction (JIS P8135:1998) (Equation 3) Decrease rate of tensile strength in a wet state X (%) = (decrease rate M + decrease rate C) / 2
6. 6. The wetlaid nonwoven fabric for a semipermeable membrane support according to claim 5, wherein the polyester fibers comprise polyester subject fibers and polyester binder fibers, and the polyester binder fibers are melt-bonded to the polyester subject fibers at least on the front and back surfaces of the wetlaid nonwoven fabric, and the polyester subject fibers are melt-bonded to each other.
7. 7. The wetlaid nonwoven fabric for a semipermeable membrane supporting material according to claim 6, wherein the mass of the polyester binder fibers is 20% by mass or more and 38% by mass or less based on the total mass of the polyester subject fibers and the polyester binder fibers.
8. The wetlaid nonwoven fabric for semipermeable membrane supporting bodies according to any one of claims 5 to 7, characterized in that the wetlaid nonwoven fabric contains only polyethylene terephthalate fibers as a fiber component.
9. The sheet density of the wet-laid nonwoven fabric is 0.5 g / cm 3 The wet-laid nonwoven fabric for semipermeable membrane supporting materials according to any one of claims 5 to 8, characterized in that
Citation Information
Patent Citations
Semipermeable membrane support and its manufacturing method
JP2002095937A
Method for producing nonwoven fabric
JP2006089872A
Nonwoven fabric for semipermeable membrane support
JP2014151238A
Separation membrane and separation membrane element
JP2015027666A
Semipermeable membrane support
JP2016140785A