Active energy ray-curable resin composition, coating film and laminate

The active energy ray-curable resin composition, formed by reacting glycerin diacrylate and isocyanate compounds, addresses the need for improved scratch resistance and adhesion in resin film coatings, providing enhanced hardness and protection for electronic and optical devices.

JP7587722B1Active Publication Date: 2024-11-20DKS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2024057555
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2024-03-29
Publication Date
2024-11-20
Estimated Expiration
2044-03-29

AI Technical Summary

Technical Problem

There is an increasing demand for active energy ray-curable resin compositions that can form coatings on resin films with improved scratch resistance and adhesion to substrates, as electronic and optical devices require higher performance.

Method used

An active energy ray-curable resin composition containing an addition reaction product of glycerin diacrylate and an isocyanate compound, with specific hydroxyl value and isocyanate compound derivatives, is used to form a coating film with high hardness and excellent adhesion.

Benefits of technology

The composition achieves a coating film with high Martens hardness, pencil hardness, and excellent scratch resistance, enhancing surface protection for resin films.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007587722000001
    Figure 0007587722000001
Patent Text Reader

Abstract

Provided is an active energy ray-curable resin composition capable of forming a coating film having high hardness and excellent scratch resistance. [Solution] The present invention provides an active energy ray-curable resin composition containing an active energy ray-curable component, the active energy ray-curable component containing an addition reaction product (X) of a monomer (M) containing glycerin diacrylate (A) and an isocyanate compound (C), the monomer (M) further containing glycerin triacrylate (B), the monomer (M) having a hydroxyl value of 5 mgKOH / g or more and 80 mgKOH / g or less, the isocyanate compound (C) being at least one selected from the group consisting of aliphatic isocyanates and derivatives thereof, and the addition reaction product (X) being contained in an amount of 15 mass% or less based on the total mass of the active energy ray-curable component.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable resin composition, a coating film, and a laminate. [Background technology]

[0002] 2. Description of the Related Art Active energy ray-curable resin compositions containing a polymerizable component that is cured by active energy rays such as ultraviolet rays can form a cured product such as a coating film when cured, and therefore are widely used in coating applications and the like.

[0003] For example, it is known that active energy ray curable resin compositions are used as coating agents for the purpose of protecting the surface of resin films and the like used in electronic devices, optical devices, and the like. Specifically, a process is carried out in which the active energy ray curable resin composition is applied to the surface of a resin film or the like to form a film, and the film is irradiated with active energy rays such as ultraviolet rays to harden the film. This process forms a coating film of the active energy ray curable resin composition on the surface of the resin film or the like. Such a coating film protects the surface of the resin film or the like, making it possible to prevent the resin film from being scratched, for example. From this perspective, various active energy ray curable resin compositions excellent in performance such as scratch resistance have been studied in order to improve the protective performance of the surface of the resin film or the like.

[0004] For example, Patent Document 1 discloses an active energy ray-curable composition containing a urethane acrylate resin having a specific structure and a photopolymerization initiator, and it is said that such a composition can form a cured coating film having high hardness and excellent scratch resistance. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2023-161761 A Summary of the Invention [Problem to be solved by the invention]

[0006] However, in recent years, with the rapid progress in improving the performance of electronic devices, optical devices, etc., there is an increasing demand for further improvement in the performance of resin films used therein. Accordingly, there is an increasing demand for coating agents (active energy ray-curable resin compositions), and there has been a demand for active energy ray-curable resin compositions capable of forming coating films on resin films that are more scratch-resistant than ever before.

[0007] The present invention has been made in view of the above, and aims to provide an active energy ray curable resin composition capable of forming a coating film having high hardness, excellent scratch resistance, and excellent adhesion to a substrate. Another aim of the present invention is to provide a coating film formed using the active energy ray curable resin composition and a laminate including the coating film. [Means for solving the problem]

[0008] Means for Solving the Problems The present inventors have conducted intensive research to achieve the above object, and as a result have found that the above object can be achieved by using an active energy ray-curable component containing glycerin triacrylate and a product obtained by reaction of glycerin diacrylate with an isocyanate compound in a predetermined ratio, thereby completing the present invention.

[0009] That is, the present invention includes, for example, the subject matter described in the following sections. Item 1 An active energy ray-curable resin composition containing an active energy ray-curable component, The active energy ray-curable component is The composition contains an addition reaction product (X) of a monomer (M) containing glycerin diacrylate (A) and an isocyanate compound (C), The monomer (M) further contains glycerin triacrylate (B), The monomer (M) has a hydroxyl value of 5 mgKOH / g or more and 80 mgKOH / g or less, The isocyanate compound (C) is at least one selected from the group consisting of aliphatic isocyanates and derivatives thereof, The active energy ray-curable resin composition contains the addition reaction product (X) in an amount of 15 mass % or less based on the total mass of the active energy ray-curable component. Section 2 Item 2. The active energy ray-curable resin composition according to item 1, wherein the derivative of the isocyanate compound (C) is at least one selected from the group consisting of an isocyanurate of an aliphatic polyisocyanate and a biuret of an aliphatic polyisocyanate. Section 3 Item 3. The active energy ray-curable resin composition according to item 1 or 2, wherein the reaction product contains the addition reaction product (X) and the glycerin triacrylate (B). Section 4 A method for producing an active energy ray-curable resin composition, comprising the steps of: The method includes a step of obtaining the active energy ray-curable component using a raw material including a monomer (M) including glycerin diacrylate (A) and glycerin triacrylate (B) and an isocyanate compound (C), The monomer (M) has a hydroxyl value of 5 mgKOH / g or more and 80 mgKOH / g or less, The isocyanate compound (C) is at least one selected from the group consisting of aliphatic isocyanates and derivatives thereof, The active energy ray curable component contains an addition reaction product (X) of the glycerin diacrylate (A) and the isocyanate compound (C), and the glycerin triacrylate (B). Section 5 Item 5. The method for producing an active energy ray-curable resin composition according to item 4, wherein the derivative of the isocyanate compound (C) is at least one selected from the group consisting of an isocyanurate of an aliphatic polyisocyanate and a biuret of an aliphatic polyisocyanate. Section 6 Item 6. The method for producing an active energy ray-curable resin composition according to Item 4 or 5, wherein the addition reaction product (X) is contained in an amount of 15 mass % or less based on the total mass of the active energy ray-curable component. Section 7 Item 4. A coating film comprising a cured product of the active energy ray-curable resin composition according to any one of items 1 to 3. Section 8 Item 8. A laminate comprising the coating film according to item 7 on a substrate. Effect of the Invention

[0010] The active energy ray-curable resin composition of the present invention can form a coating film that has high hardness, excellent scratch resistance, and excellent adhesion to a substrate. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] Hereinafter, embodiments of the present invention will be described in detail. In this specification, the expressions "containing" and "comprise" include the concepts of "containing", "comprises", "consists essentially of" and "consists only of".

[0012] 1. Active energy ray-curable resin composition The active energy ray curable resin composition of the present invention contains an active energy ray curable component. The active energy ray curable component contains an addition reaction product (X) between a monomer (M) containing glycerin diacrylate (A) and an isocyanate compound (C). The monomer (M) further contains glycerin triacrylate (B), and the monomer (M) has a hydroxyl value of 5 mgKOH / g or more and 80 mgKOH / g or less. The isocyanate compound (C) is at least one selected from the group consisting of aliphatic isocyanates and derivatives thereof. The addition reaction product (X) is contained in an amount of 15 mass% or less based on the total mass of the active energy ray curable component.

[0013] In this specification, glycerin diacrylate will be referred to as "glycerin diacrylate (A)", glycerin triacrylate will be referred to as "glycerin triacrylate (B)", and the isocyanate compound will be referred to as "isocyanate compound (C)".

[0014] In the present specification, hereinafter, "the active energy ray-curable resin composition of the present invention" will be abbreviated to simply "the curable resin composition of the present invention".

[0015] The curable resin composition of the present invention can form a coating film having high hardness and excellent scratch resistance. In particular, the coating film obtained from the curable resin composition of the present invention is excellent in both Martens hardness and pencil hardness.

[0016] Furthermore, a coating film formed using the curable resin composition of the present invention has high adhesion to resin films.

[0017] Therefore, the curable resin composition of the present invention can be suitably used as a coating agent for substrates such as resin films.

[0018] (Active energy ray curable component) The curable resin composition of the present invention contains an active energy ray curable component as an essential component. The active energy ray curable component is a component having a property of being cured by active energy rays, particularly a property of being polymerized by active energy rays. The active energy ray referred to in the present invention is preferably ultraviolet light, and other examples include electron beams, gamma rays, carbon arc lamps, xenon lamps, and metal halide lamps. Hereinafter, the active energy ray curable component will be simply abbreviated as "curable component".

[0019] As described above, the curable component contains an addition reaction product (X) between a monomer (M) containing glycerin diacrylate (A) and an isocyanate compound (C).

[0020] Monomer (M) further contains glycerin triacrylate (B), and thus monomer (M) is a mixture of glycerin diacrylate (A) and glycerin triacrylate (B).

[0021] The hydroxyl value of the monomer (M) is 5 mgKOH / g or more and 80 mgKOH / g or less. When the hydroxyl value of the monomer (M) is in this range, the coating film obtained from the curable resin composition of the present invention has high hardness and excellent scratch resistance. When the hydroxyl value of the monomer (M) is less than 5 mgKOH / g or exceeds 80 mgKOH / g, the hardness of the coating film obtained from the curable resin composition of the present invention decreases, particularly the Martens hardness, and it becomes difficult to form a coating film having the desired scratch resistance.

[0022] The hydroxyl value of the monomer (M) is preferably 10 mgKOH / g or more, more preferably 15 mgKOH / g or more, even more preferably 20 mgKOH / g or more, and particularly preferably 25 mgKOH / g or more, and is preferably 70 mgKOH / g or less, more preferably 60 mgKOH / g or less, even more preferably 50 mgKOH / g or less, and particularly preferably 40 mgKOH / g or less.

[0023] The monomer (M) may contain other components than glycerin diacrylate (A) and glycerin triacrylate (B) as long as the hydroxyl value is 5 mgKOH / g or more and 80 mgKOH / g or less. The monomer (M) preferably contains 80 mass% or more of glycerin diacrylate (A) and glycerin triacrylate (B), more preferably 90 mass% or more, and even more preferably 95 mass% or more. It is particularly preferable that the monomer (M) consists of only glycerin diacrylate (A) and glycerin triacrylate (B).

[0024] In the monomer (M), the content ratio of glycerin diacrylate (A) and glycerin triacrylate (B) can be adjusted so that the hydroxyl value is in the range of 5 mgKOH / g or more and 80 mgKOH / g or less. For example, it is preferable that glycerin triacrylate (B) is contained in an amount of 50 mass% or more based on the total amount of glycerin diacrylate (A) and glycerin triacrylate (B).

[0025] The addition reaction product (X) is a product obtained by an addition reaction between the glycerin diacrylate (A) in the monomer (M) and the isocyanate compound (C). More specifically, the addition reaction product (X) is a polyaddition product obtained by polyaddition reaction of the glycerin diacrylate (A) and the isocyanate compound (C). Thus, the addition reaction product (X) is a compound containing units derived from the glycerin diacrylate (A) and units derived from the isocyanate compound (C).

[0026] In addition, since the glycerin triacrylate (B) in the monomer (M) is a compound that does not have a hydroxyl group, it does not undergo an addition reaction with the isocyanate compound (C), and therefore the addition reaction product (X) does not contain units derived from glycerin triacrylate (B).

[0027] Specifically, the addition reaction product (X) is a product obtained by reacting a hydroxyl group (OH) present in the molecule of glycerin diacrylate (A) with an isocyanate group (NCO) present in the molecule of the isocyanate compound (C). In particular, since the isocyanate compound (C) has two or more isocyanate groups as described below, the reaction between the glycerin diacrylate (A) and the isocyanate compound (C) proceeds sequentially, resulting in a polyaddition reaction.

[0028] The addition reaction product (X) is produced by the reaction of the hydroxyl group (OH) in the glycerin diacrylate (A) with the isocyanate group (NCO) in the isocyanate compound (C), and therefore contains a urethane bond (OCONH). In other words, the addition reaction product (X) contains both a urethane moiety produced by the above-mentioned reaction and an acrylate moiety derived from the glycerin diacrylate (A), and therefore can be called a urethane acrylate compound.

[0029] The isocyanate compound (C) is at least one selected from the group consisting of aliphatic isocyanates and their derivatives. In particular, the isocyanate compound (C) has two or more isocyanate groups in the molecule. It is preferable that the aliphatic isocyanate and its derivatives (aliphatic isocyanate derivatives) do not have an aromatic ring or an alicyclic ring (cyclic hydrocarbon group) in the molecule.

[0030] The aliphatic isocyanate may be, for example, a wide variety of known bifunctional or higher aliphatic isocyanates, and examples thereof include aliphatic diisocyanate compounds having 30 or less carbon atoms. Specific examples of the aliphatic isocyanate include ethylene diisocyanate, tetramethylene diisocyanate, pentamethylene diisocyanate, hexamethylene diisocyanate, 2-methyl-1,5-pentane diisocyanate, 3-methyl-1,5-pentane diisocyanate, and 2,2,4-trimethyl-1,6-hexamethylene diisocyanate. In that the hardness of the coating film obtained from the curable resin composition of the present invention is easily increased and the scratch resistance is further increased, the aliphatic isocyanate is preferably an aliphatic diisocyanate compound having 4 to 30 carbon atoms, and more preferably an aliphatic diisocyanate compound having 4 to 10 carbon atoms.

[0031] Examples of the aliphatic isocyanate derivative (same meaning as the derivative of the isocyanate compound (C)) include trifunctional or higher isocyanate compounds. Among them, the aliphatic isocyanate derivative is preferably at least one selected from the group consisting of isocyanurates of aliphatic polyisocyanates and biuret forms of aliphatic polyisocyanates, in that the hardness of the coating film obtained from the curable resin composition of the present invention is likely to be high and the scratch resistance is also improved.

[0032] An example of an isocyanurate of an aliphatic polyisocyanate is a compound in which -R-NCO is bonded to a nitrogen atom derived from an isocyanurate, and an example of a biuret of an aliphatic polyisocyanate is a compound in which -R-NCO is bonded to a nitrogen atom derived from a biuret. Here, R is an alkylene group having 30 or less carbon atoms, preferably an alkylene group having 4 to 30 carbon atoms, and more preferably an alkylene group having 4 to 10 carbon atoms.

[0033] From the above, as the isocyanate compound (C), at least one selected from the group consisting of aliphatic isocyanates, isocyanurates of aliphatic polyisocyanates, and biuret compounds of aliphatic polyisocyanates can be preferably used. The more preferred isocyanate compound (C) is an aliphatic isocyanate, which tends to form a coating film with a higher Martens hardness.

[0034] The isocyanate compound (C) used to obtain the addition reaction product (X) may be one type alone or two or more types.

[0035] The isocyanate compound (C) can be obtained, for example, by production using a known method, or can be obtained from commercial products.

[0036] The reaction method of the glycerin diacrylate (A) and the isocyanate compound (C) is not particularly limited. For example, the addition reaction product (X) can be obtained by the reaction carried out in step 1 described later.

[0037] The molecular weight of the addition reaction product (X) is, for example, preferably 450 or more and 3,000 or less, and more preferably 550 or more and 1,200 or less, calculated as the molar mass.

[0038] As described above, the curable component contains the addition reaction product (X) between the monomer (M) containing the glycerin diacrylate (A) and the isocyanate compound (C). In other words, the curable component contains the addition reaction product (X) and the glycerin triacrylate (B).

[0039] The curable component may contain other components in addition to the addition reactant (X) and glycerin triacrylate (B). The other components may include various compounds having a polymerizable double bond, particularly (meth)acrylic compounds. In this specification, "(meth)acrylic" means "acrylic" or "methacrylic".

[0040] The curable component may contain 50% by mass or more of the addition reactant (X) and glycerin triacrylate (B) in total, preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and particularly preferably 99% by mass or more. The curable component may be composed of only the addition reactant (X) and glycerin triacrylate (B). In this case, the inclusion of glycerin diacrylate (A) and / or isocyanate compound (C) that is inevitably contained in the curable component is not excluded. The glycerin diacrylate (A) and / or isocyanate compound (C) that is inevitably contained is, for example, an unreacted product of the reaction to obtain the addition reactant (X). It is preferable that the curable component does not contain a solvent, which will be described later.

[0041] (Active energy ray-curable resin composition) Next, the curable resin composition of the present invention will be described. The curable resin composition of the present invention contains the above-mentioned curable component as an essential component. That is, the curable resin composition of the present invention is a mixture containing at least the addition reaction product (X) and glycerin triacrylate (B).

[0042] In the curable resin composition of the present invention, the addition reaction product (X) is contained in an amount of 15 mass% or less based on the total mass of the curable components. This allows the coating film obtained from the curable resin composition of the present invention to have high hardness and excellent scratch resistance. If the content of the addition reaction product (X) exceeds 15 mass% based on the total mass of the curable components, the hardness of the coating film obtained from the curable resin composition of the present invention decreases, particularly the Martens hardness, and it becomes difficult to obtain the desired scratch resistance.

[0043] In the curable resin composition of the present invention, the addition reaction product (X) is contained in an amount of preferably 1 mass % or more, more preferably 5 mass % or more, even more preferably 7 mass % or more, and particularly preferably 8 mass % or more, based on the total mass of the curable components.

[0044] The curable resin composition of the present invention may contain other components as long as the curable component is an essential component. Examples of other components include a solvent, a polymerization initiator, a polymerization inhibitor, a photosensitizer, a light stabilizer, a silane coupling agent, an ultraviolet absorber, a catalyst, a leveling agent, a defoaming agent, a polymerization accelerator, an antioxidant, a flame retardant, an infrared absorber, an antistatic agent, a slip agent, a plasticizer, a dispersant, and the like.

[0045] The solvent may be added, for example, for the purpose of improving the coating property of the curable resin composition of the present invention. Examples of the solvent include chlorine-based hydrocarbons such as chloroform and 1,2-dichloroethane; ether compounds such as diethyl ether and tetrahydrofuran; aliphatic hydrocarbons such as hexane and heptane; alicyclic hydrocarbons such as cyclohexane; aromatic hydrocarbons such as benzene, toluene and xylene; ketone compounds such as acetone and methyl ethyl ketone; ester compounds such as vinyl acetate; alcohols such as methanol, ethanol, isopropyl alcohol and t-butanol; formamides such as N,N-dimethylformamide and N,N-dimethylacetamide; pyrrolidones such as 2-pyrrolidone and N-methylpyrrolidone; dimethyl sulfoxide, etc.

[0046] The amount of the solvent contained in the curable resin composition of the present invention is not particularly limited. For example, the amount of the solvent can be adjusted so that the total concentration of the curable components is 1 to 100 mass %, and in consideration of coatability, the amount is preferably about 5 to 50 mass %.

[0047] The polymerization initiator may be, for example, a wide variety of known polymerization initiators. The polymerization initiator may be either a thermal decomposition polymerization initiator or a photopolymerization initiator, and is preferably a photopolymerization initiator in terms of ease of film formation.

[0048] Examples of photopolymerization initiators include aromatic ketones such as benzophenone, aromatic compounds such as anthracene and α-chloromethylnaphthalene, and sulfur compounds such as diphenyl sulfide and thiocarbamate. Examples of polymerization initiators using active energy rays such as ultraviolet rays other than visible light include acetophenone, acetophenone benzyl ketal, 1-hydroxycyclohexyl phenyl ketone, 2,2-dimethoxy-1,2-diphenylethan-1-one, xanthone, fluorenone, benzaldehyde, fluorene, anthraquinone, triphenylamine, carbazole, 3-methylacetophenone, 4-chlorobenzophenone, 4,4'-dimethoxybenzophenone, 4,4'-diaminobenzophenone, benzoin propyl ether, benzoin ethyl ether, benzyl dimethyl ketal, 1-(4-isopropylphenyl)-2-hydroxy-2-methylpropan-1-one, 2-hydroxy-2-methyl-1- Examples of the phenylpropan-1-one include thioxanthone, diethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-propan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1,4-(2-hydroxyethoxy)phenyl-(2-hydroxy-2-propyl)ketone, 2,4,6,-trimethylbenzoyldiphenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, and oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone).

[0049] The content of the polymerization initiator contained in the curable resin composition of the present invention is not particularly limited, and may be 0.01 to 10 parts by mass, preferably 0.03 to 5 parts by mass, based on 100 parts by mass of the total amount of the curable components. Alternatively, the content of the polymerization initiator may be 0.1 to 1% by mass based on the total amount of the addition reaction product (X).

[0050] The curable resin composition of the present invention preferably contains 50 mass% or more of the curable component, more preferably 80 mass% or more, even more preferably 90 mass% or more, and particularly preferably 95 mass% or more, based on the total mass excluding the solvent.

[0051] (Method for producing active energy ray-curable resin composition) The method for producing the curable resin composition of the present invention is not particularly limited, and for example, a known method for producing an active energy ray-curable resin composition can be widely adopted. Preferably, the curable resin composition of the present invention can be produced by a production method including the following step 1. Step 1: A step of obtaining the active energy ray-curable component using a raw material containing a monomer (M) including glycerin diacrylate (A) and glycerin triacrylate (B) and an isocyanate compound (C).

[0052] In step 1, a raw material containing a monomer (M) including glycerin diacrylate (A) and glycerin triacrylate (B) and an isocyanate compound (C) is used.

[0053] In step 1, the reaction using the raw material is specifically an addition reaction (polyaddition) of glycerin diacrylate (A) and an isocyanate compound (C). By carrying out such a reaction, an addition reaction (polyaddition) of glycerin diacrylate (A) and an isocyanate compound (C) occurs, and the addition reaction product (X) is generated.

[0054] The raw material used in step 1 can be prepared by mixing the monomer (M) and the isocyanate compound (C) in a given ratio.

[0055] The hydroxyl value of the monomer (M) contained in the raw material is 5 mgKOH / g or more and 80 mgKOH / g or less. When the hydroxyl value of the monomer (M) is in this range, the curable resin composition obtained by the production method of the present invention can form a coating film having high hardness and excellent scratch resistance.

[0056] When the hydroxyl value of the monomer (M) contained in the raw material is less than 5 mgKOH / g or exceeds 80 mgKOH / g, the coating film of the curable resin composition obtained by the production method of the present invention will have reduced hardness, particularly reduced Martens hardness, and it will also be difficult to form a coating film having the desired scratch resistance.

[0057] The hydroxyl value of the monomer (M) is preferably 10 mgKOH / g or more, more preferably 15 mgKOH / g or more, even more preferably 20 mgKOH / g or more, and particularly preferably 25 mgKOH / g or more, and is preferably 70 mgKOH / g or less, more preferably 60 mgKOH / g or less, even more preferably 50 mgKOH / g or less, and particularly preferably 40 mgKOH / g or less.

[0058] The monomer (M) may contain other components than glycerin diacrylate (A) and glycerin triacrylate (B) as long as the hydroxyl value is 5 mgKOH / g or more and 80 mgKOH / g or less. The monomer (M) preferably contains 80 mass% or more of glycerin diacrylate (A) and glycerin triacrylate (B), more preferably 90 mass% or more, and even more preferably 95 mass% or more. It is particularly preferable that the monomer (M) consists of only glycerin diacrylate (A) and glycerin triacrylate (B).

[0059] In the monomer (M), the content ratio of glycerin diacrylate (A) and glycerin triacrylate (B) can be adjusted so that the hydroxyl value is in the range of 5 mgKOH / g or more and 80 mgKOH / g or less. For example, it is preferable that glycerin triacrylate (B) is contained in an amount of 50 mass% or more based on the total amount of glycerin diacrylate (A) and glycerin triacrylate (B).

[0060] The monomer (M) containing glycerin diacrylate (A) and glycerin triacrylate (B) can be obtained from commercial products, such as M-930 from the Aronix (registered trademark) series manufactured by Toagosei Co., Ltd.

[0061] The isocyanate compound (C) contained in the raw material is at least one selected from the group consisting of aliphatic isocyanates and their derivatives. The derivative of the isocyanate compound (C) is at least one selected from the group consisting of isocyanurates of aliphatic polyisocyanates and biuret forms of aliphatic polyisocyanates, as described above.

[0062] The isocyanate compound (C) contained in the raw material can be preferably at least one selected from the group consisting of aliphatic isocyanates, isocyanurates of aliphatic polyisocyanates, and biuret compounds of aliphatic polyisocyanates. The more preferred isocyanate compound (C) is an aliphatic isocyanate, and in this case, the curable resin composition obtained by the manufacturing method of the present disclosure is likely to form a coating film with a higher Martens hardness. The isocyanate compound (C) contained in the raw material can be one type alone or two or more types.

[0063] The addition reaction (polyaddition) of the glycerin diacrylate (A) and the isocyanate compound (C) performed in step 1 can be carried out using a wide variety of known polyaddition reactions. For example, the reaction conditions for reacting a known alcohol compound with an isocyanate compound can be widely used in the present invention.

[0064] For example, an addition reaction product (X) can be obtained by reacting glycerin diacrylate (A) in a monomer (M) with an isocyanate compound (C) in the presence of a catalyst. Since the glycerin triacrylate (B) in the monomer (M) does not have a hydroxyl group, the glycerin triacrylate (B) does not react with the isocyanate compound (C). Therefore, the glycerin triacrylate (B) remains even after the polyaddition reaction.

[0065] As the catalyst, for example, an organic tin compound can be used, and specific examples include tin octoate, dibutyltin dilaurate, dioctyltin dineodecane, dioctyltin dilaurate, manganese, cobalt, lead, bismuth stannate, lead stannate, zirconium octoate, zinc octoate, dibutyltin-bis-o-phenylphenylene, dibutyltin-S,S-dibutyldithio-carbonate, triphenylantimony dichloride, dibutyltin maleate, dibutyltin diacetate, dibutyltin dilaurate mercaptide, triethylenediamine, bismuth stearate, lead stearate, dimethyltin dichloride, etc. The amount of the catalyst used can usually be adjusted in the range of 0.001 to 5 parts by weight per 100 parts by weight of the total of glycerin diacrylate (A) and isocyanate compound (C).

[0066] The reaction for obtaining the addition product (X) can be carried out in the presence of a polymerization inhibitor. As the polymerization inhibitor, a wide variety of known polymerization inhibitors such as hydroquinone monomethyl ether can be used.

[0067] The reaction temperature for obtaining the addition reaction product (X) is not particularly limited, and can be, for example, about 30 to 100° C., preferably 50 to 80° C. The reaction time is also not particularly limited, and can be set to an appropriate range depending on the reaction temperature. For example, the reaction can be carried out until the amount of free isocyanate becomes 10% by mass or less, preferably 5% by mass or less, more preferably 0.1% by mass or less, based on the amount of the isocyanate compound (C) used.

[0068] The raw materials used in step 1 may contain other components in addition to glycerin diacrylate (A), glycerin triacrylate (B), and the isocyanate compound (C). The other components include the above-mentioned catalyst, polymerization inhibitor, etc., and also polymerizable monomers that are added as necessary.

[0069] By carrying out a reaction (polyaddition reaction) using the above raw materials, the reaction between glycerin diacrylate (A) and the isocyanate compound (C) proceeds, and an addition reaction product (X) is generated. As described above, glycerin triacrylate (B) does not have a hydroxyl group, so it remains unreacted. Therefore, a curable component containing the addition reaction product (X) and glycerin triacrylate (B) is obtained by the reaction using the above raw materials.

[0070] The molecular weight of the addition reaction product (X) is, for example, preferably 450 or more and 3,000 or less, and more preferably 550 or more and 1,200 or less, calculated as the molar mass.

[0071] The curable component obtained in step 1 may be mixed with a solvent, a photopolymerization initiator, and the like as necessary to obtain the curable resin composition of the present invention.

[0072] The curable component (active energy ray curable component) obtained in step 1 contains an addition reaction product (X) in an amount of 15 mass% or less based on the total mass of the curable component. This allows the curable resin composition obtained by the production method of the present invention to form a coating film having high hardness and excellent scratch resistance. If the content of the addition reaction product (X) exceeds 15 mass% based on the total mass of the curable component, the hardness of the coating film decreases, particularly the Martens hardness, and it becomes difficult to obtain the desired scratch resistance.

[0073] The addition reaction product (X) is contained in an amount of preferably 1 mass % or more, more preferably 5 mass % or more, further preferably 7 mass % or more, and particularly preferably 8 mass % or more, based on the total mass of the curable component.

[0074] (Paint film) A coating film can be formed by using the curable resin composition of the present invention or the curable resin composition obtained by the manufacturing method of the present invention. Specifically, a coating liquid is prepared by adding a solvent, a polymerization initiator, etc. to the curable resin composition as necessary, and the coating liquid is applied to a substrate to form a film, and the film is cured to form a coating film on the substrate. That is, the coating film contains a cured product of the curable resin composition of the present invention.

[0075] The substrate is not particularly limited, and may be, for example, any of various known resin films. The type of film is also not particularly limited, and may be a wide variety of resin films, such as a polyethylene terephthalate film, a polyethylene film, or an acrylic film.

[0076] The method of applying the coating liquid obtained from the curable resin composition of the present invention onto a substrate is not particularly limited, and a wide variety of known application methods can be used. For example, the coating can be performed using a known coating device, such as a blade coater, an air knife coater, a roll coater, a bar coater, a gravure coater, a microgravure coater, a rod blade coater, a lip coater, a die coater, or a curtain coater.

[0077] The method of curing the coating formed on the substrate is not particularly limited, and examples thereof include a method of irradiating the coating with active energy rays. The active energy rays are preferably ultraviolet rays, and other examples include electron beams, gamma rays, carbon arc lamps, xenon lamps, and metal halide lamps. The method and conditions of irradiating the active energy rays are also not limited, and can be the same as known. Examples of ultraviolet ray generating sources include low pressure mercury lamps, high pressure mercury lamps, ultra-high pressure mercury lamps, xenon lamps, gallium lamps, metal halide lamps, sunlight, and ultraviolet lamps such as LEDs.

[0078] The thickness of the coating film is not particularly limited and can be set within an appropriate range depending on the intended use.

[0079] The coating film obtained from the curable resin composition of the present invention contains a cured product of the active energy ray curable resin composition, and therefore has high hardness and excellent scratch resistance, particularly excellent in both Martens hardness and pencil hardness. The coating film obtained from the curable resin composition of the present invention has high Martens hardness as well as pencil hardness, which makes it possible to achieve scratch resistance superior to that of conventional coating films. In addition, the coating film formed using the curable resin composition of the present invention also has high adhesion to resin films.

[0080] Therefore, the curable resin composition of the present invention is suitable for use as a coating agent for forming a coating film on a substrate such as a resin film.

[0081] The coating film can be used to form various laminates, and examples thereof include a laminate having the coating film on a substrate. By providing the coating film, such a laminate is likely to prevent the substrate surface from being scratched.

[0082] In specifying the invention included in the present disclosure, the configurations (properties, structures, functions, etc.) described in each embodiment of the present disclosure may be combined in any manner. In other words, the present disclosure includes all subject matter consisting of all combinations of the configurations that can be combined as described in this specification. EXAMPLES

[0083] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the embodiments of these examples.

[0084] Example 1 The raw materials were prepared according to the composition of Example 1 shown in Table 1. Specifically, the raw materials used in step 1 were prepared by mixing 3.6 parts by mass of hexamethylene diisocyanate (hereinafter, HDI) as the isocyanate compound (C), 0.05 parts by mass of hydroquinone monomethyl ether as a polymerization inhibitor, 0.03 parts by mass of dioctyltin dineodecane as a catalyst, and 96.4 parts by mass of monomer M (Toagosei Co., Ltd. "Aronix (registered trademark) M-930") having a hydroxyl value of 30 mgKOH / g and consisting of glycerin diacrylate (A) and glycerin triacrylate (B) in a flask.

[0085] Next, the raw materials in the flask were heated to 70°C to carry out a reaction. The reaction was carried out until the amount of free isocyanate was 0.1 mass% or less based on the amount of the isocyanate compound (C) charged. Through this reaction, a composition containing an active energy ray-curable component containing urethane acrylate (addition reaction product (X)), which is a reaction product of glycerin diacrylate (A) and the isocyanate compound (C) in the monomer M, and glycerin triacrylate (B) was obtained (step 1).

[0086] Example 2 As shown in Table 1, a composition containing an active energy ray-curable component was obtained in the same manner as in Example 1, except that the isocyanate compound (C) was changed from HDI to 1,5-pentamethylene diisocyanate (hereinafter, PDI) to prepare the raw materials.

[0087] Example 3 As shown in Table 1, a composition containing an active energy ray-curable component was obtained in the same manner as in Example 1, except that the isocyanate compound (C) was changed to 7.2 parts by mass of HDI nurate ("Coronate HXR" manufactured by Tosoh Corporation), which is an HDI derivative, instead of HDI, and the amount of monomer M used was changed to 92.8 parts by mass to prepare the raw material.

[0088] Example 4 As shown in Table 1, a composition containing an active energy ray-curable component was obtained in the same manner as in Example 1, except that the isocyanate compound (C) was changed to 6.8 parts by mass of PDI nurate ("STABIO (registered trademark) D-376N" manufactured by Mitsui Chemicals), which is a PDI derivative, instead of HDI, and the amount of monomer M used was changed to 93.2 parts by mass to prepare the raw material.

[0089] Example 5 As shown in Table 1, a composition containing an active energy ray-curable component was obtained in the same manner as in Example 1, except that the isocyanate compound (C) was changed to 6.4 parts by mass of HDI biuret (Duranate 24A-100 manufactured by Asahi Kasei Corporation), which is an HDI derivative, instead of HDI, and the amount of monomer M used was changed to 93.6 parts by mass to prepare the raw material.

[0090] Comparative Example 1 The raw material was prepared according to the composition of Comparative Example 1 shown in Table 1. Specifically, 12.1 parts by mass of HDI as an isocyanate compound (C), 0.05 parts by mass of hydroquinone monomethyl ether as a polymerization inhibitor, 0.03 parts by mass of dioctyltin dineodecane as a catalyst, and 87.9 parts by mass of a monomer consisting of glycerin diacrylate (A) and glycerin triacrylate (B) were mixed in a flask to prepare the raw material used in step 1. The monomer consisting of glycerin diacrylate (A) and glycerin triacrylate (B) was prepared by mixing 54.1 parts by mass of the monomer M and 33.8 parts by mass of monomer m (Toagosei Co., Ltd. "Aronix (registered trademark) M-920", hydroxyl group 240 mg KOH / g) to prepare a mixed monomer 1 having a hydroxyl group of 111 mg KOH / g.

[0091] Next, the raw materials in the flask were heated to 70°C to carry out a reaction. The reaction was carried out until the amount of free isocyanate was 0.1 mass% or less based on the amount of the isocyanate compound (C) charged. This reaction yielded a composition containing an active energy ray-curable component that contained urethane acrylate (addition reaction product (X)), which is a reaction product of glycerin diacrylate (A) and the isocyanate compound (C) in the mixed monomer, and glycerin triacrylate (B).

[0092] Comparative Example 2 A composition containing an active energy ray-curable component was obtained in the same manner as in Comparative Example 1, except that 75.4 parts by mass of Toagosei's "Aronix (registered trademark) M-920" (hydroxyl value 240 mg KOH / g) was used instead of mixed monomer 1, and the amount of HDI was changed to 24.6 parts by mass to prepare the raw materials.

[0093] Comparative Example 3 A composition containing an active energy ray-curable component was obtained in the same manner as in Comparative Example 1, except that 94.9 parts by mass of Toagosei's "Aronix (registered trademark) M-930" (hydroxyl value 30 mgKOH / g) was used instead of mixed monomer 1, and 5.1 parts by mass of isophorone diisocyanate (IPDI), which is an alicyclic isocyanate, was used instead of HDI as the isocyanate compound (C).

[0094] Comparative Example 4 A composition containing an active energy ray-curable component was obtained in the same manner as in Comparative Example 1, except that 95.6 parts by mass of Toagosei's "Aronix (registered trademark) M-930" (hydroxyl value 30 mgKOH / g) was used instead of the mixed monomer 1, and 4.4 parts by mass of xylene diisocyanate (XDI), an aromatic isocyanate, was used instead of HDI as the isocyanate compound (C).

[0095] (Evaluation method) A coating film was prepared by the following method using the composition obtained in each of the Examples and Comparative Examples, and the Martens hardness, scratch resistance, pencil hardness and adhesion to the substrate were evaluated using the obtained coating film.

[0096] [Preparation of coating film] Methyl ethyl ketone was added to the composition obtained in each Example and Comparative Example to prepare a solution with a solid content concentration of 40% by mass. To this solution, 3% by mass of "Omnirad 184" manufactured by IGM Resins BV was added as a polymerization initiator relative to the active energy ray curable component to obtain a coating liquid. The coating liquid was applied to a 100 μm thick PET film ("Cosmoshine A4360" manufactured by Toyobo Co., Ltd.) so that the film thickness in a dry state would be about 3 μm, and then dried in an oven at 80° C. for 1 minute to form a film on the PET film. Thereafter, a high-pressure mercury lamp (80 W / cm×1 lamp) was used under a nitrogen atmosphere with an integrated illuminance of 600 mJ / cm 2 The coating was cured by irradiating the coating with light at a temperature of 100° C. to obtain a laminate in which a coating film was formed on the PET film.

[0097] [Martens hardness HM] The Martens hardness of the coating film was evaluated by measuring the microhardness by an indentation test using a microhardness tester (product number: ENT-1100a) manufactured by Elionix. The indentation test was performed with an indentation load of 0.3 mN. The indentation test was performed in accordance with the indentation test method in accordance with ISO14577-1, and the Martens hardness HM of the coating film was measured and evaluated according to the following criteria. ≪Judgment criteria≫ A: Martens hardness HM is 360N / mm 2 Thus, it has an extremely high Martens hardness. B: Martens hardness HM is 340~360N / mm 2 and has a high Martens hardness. C: Martens hardness HM is 320~340N / mm 2 and the Martens hardness is low. D: Martens hardness HM is 320N / mm 2and the Martens hardness is extremely low.

[0098] [Scratch resistance] The coating film formed on the surface of the laminate was subjected to a load of 250 g / cm using #0000 steel wool. 2 After the test, the surface of the laminate was visually inspected and the scratch resistance was evaluated according to the following criteria. ≪Judgment criteria≫ A: The number of scratches is 2 or less, and the material has excellent scratch resistance. B: The number of scratches is 3 or more and 4 or less, and the scratch resistance is poor. C: The number of scratches is 5 or more, and the scratch resistance is extremely poor.

[0099] [Pencil hardness] The pencil hardness of the coating film on the surface of the laminate was measured in accordance with JIS K5600-5-4:1999.

[0100] [Adhesion to substrate] For the coating surface formed on the laminate surface, 100 2 mm x 2 mm grids were made by cutting the surface of the cured coating with a cutter knife, and cellophane adhesive tape was attached on top of them and then rapidly peeled off three times. The number of grids remaining without peeling off was counted and the adhesion to the substrate (PET film) was evaluated according to the following criteria. ≪Judgment criteria≫ A: 80 or more grids remained, and the adhesion to the substrate was extremely excellent. B: The number of remaining grids was 50 or more and less than 80, and the adhesion to the substrate was excellent. C: Fewer than 50 cross-cut marks remained, and adhesion to the substrate was poor.

[0101] Table 1 shows the preparation conditions for the compositions obtained in each Example and Comparative Example, particularly the blending conditions for obtaining the active energy ray-curable component. Note that the blank spaces in Table 1 mean that the corresponding raw material was not used, and the types are indicated using the abbreviations shown in each Example and Comparative Example.

[0102] Table 1 also shows the content ratio of the addition reaction product (X) (urethane acrylate) to the total mass of the active energy ray curable components (in Table 1, this is expressed as "content ratio (mass %) of the addition reaction product (X) to the entire resin"). The content ratio of the addition reaction product (X) (urethane acrylate) to the total mass of the active energy ray curable components was calculated by the following formula (1). Mass ratio of the addition reactant (X) = mass of the addition reactant (X) / {mass of the addition reactant (X) + mass of unreacted glycerin diacrylate (A) + mass of glycerin triacrylate (B)} x 100 (1) Here, the glycerin diacrylate (A) and glycerin triacrylate (B) in monomer M can be calculated based on these hydroxyl values ​​and the hydroxyl value of monomer M. From this calculation, the masses of glycerin diacrylate (A) and glycerin triacrylate (B) can be calculated. The mass of glycerin diacrylate (A) reacting with isocyanate (C) can be calculated by "the amount of substance of isocyanate (C) x the number of functional groups of isocyanate (C) x the molar mass of glycerin diacrylate (A)". The mass of the addition reactant (X) can be calculated from "the mass of isocyanate (C) + the mass of glycerin diacrylate (A) reacting with isocyanate (C)". The mass of unreacted glycerin diacrylate (A) can be calculated by "the mass of glycerin diacrylate (A) - the mass of glycerin diacrylate (A) reacting with isocyanate (C)". Based on the above calculation results, the content ratio of the addition reaction product (X) (urethane acrylate) relative to the total mass of the active energy ray-curable components can be derived from the above formula (1).

[0103] Furthermore, Table 1 shows the evaluation results (Martens hardness, scratch resistance, pencil hardness, and adhesion to substrate) of the coating films obtained from the compositions of the respective Examples and Comparative Examples.

[0104] It can be seen from Table 1 that the coating films obtained using the compositions prepared in each Example have high hardness, excellent scratch resistance, and also high adhesion to the substrate.

[0105] [Table 1]

Claims

1. A method for producing an active energy ray-curable resin composition, comprising the steps of: The method includes a step of obtaining an active energy ray-curable component using a raw material including a monomer (M) including glycerin diacrylate (A) and glycerin triacrylate (B) and an isocyanate compound (C), The monomer (M) contains 80% by mass or more of the glycerin triacrylate (B), In the step, the glycerin diacrylate (A) and the isocyanate compound (C) are subjected to an addition reaction to generate an addition reaction product (X), The monomer (M) has a hydroxyl value of 10 mgKOH / g or more and 50 mgKOH / g or less, The isocyanate compound (C) is at least one selected from the group consisting of aliphatic isocyanates and derivatives thereof, and the aliphatic isocyanate does not have an aromatic ring or an alicyclic ring in the molecule, the active energy ray-curable component contains the addition reaction product (X) and the glycerin triacrylate (B), The method for producing an active energy ray-curable resin composition, wherein the addition reaction product (X) is contained in an amount of 14.6 mass% or less based on the total mass of the active energy ray-curable component.

2. 2. The method for producing an active energy ray-curable resin composition according to claim 1, wherein the derivative of the isocyanate compound (C) is at least one selected from the group consisting of an isocyanurate of an aliphatic polyisocyanate and a biuret of an aliphatic polyisocyanate.

3. A method for producing a coating film containing a cured product of an active energy ray-curable resin composition, comprising the steps of: A step of producing the active energy ray-curable resin composition by the production method according to claim 1 or 2; A method for producing a coating film, comprising: a step of obtaining the cured product by curing the active energy ray-curable resin composition.

Citation Information

Patent Citations

  • Two-piece golf ball

    JP1993345050A

  • Active energy ray-curable composition, cured coating and laminated film

    JP2023161761A

  • Curable composition, active-energy-ray-curable composition, and active-energy-ray-curable coating composition

    WO2022225041A1

  • Laminate

    WO2024063128A1