Electroless plated fiber material and its manufacturing method and manufacturing system
The electrostatic spraying of catalyst and reducing agent solutions onto fiber materials addresses the high costs and environmental issues of traditional electroless plating by reducing solution usage and enhancing the conductivity and thickness of the plating film, thus improving manufacturing efficiency.
Patent Information
- Application Number
- JP2020114102
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-01
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2040-07-01
AI Technical Summary
Existing electroless plating processes for fiber materials are costly due to the use of large quantities of processing solutions containing precious metals and hazardous substances, leading to high manufacturing costs and environmental burdens, while also reducing manufacturing efficiency.
A method involving electrostatic spraying of catalyst and reducing agent solutions onto fiber materials, charged to specific potentials, to reduce the amount of processing solution used and improve the quality of the electroless plated fiber materials by increasing conductivity and reducing plating film thickness.
Reduces the amount of processing solution required, lowers manufacturing costs, decreases environmental impact, and enhances the conductivity and thickness of the plating film, thereby improving manufacturing efficiency.
Smart Images

Figure 0007588339000001 
Figure 0007588339000002 
Figure 0007588339000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing electrolessly plated fiber materials, which includes a step of electrolessly plating a fiber material using a solution containing metal ions and a solution containing a reducing agent. The present invention relates to an electrolessly plated fiber material produced by such a production method. The present invention also relates to a production system for electrolessly plated fiber materials, which includes an electroless plating device configured to electrolessly plate a fiber material using a solution containing metal ions and a solution containing a reducing agent. [Background technology]
[0002] In order to produce a conductive fiber material, electroless plating may be applied to the fiber material. In the electroless plating, a metal ion is reduced using a reducing agent to deposit a metal plating film on the fiber material. One example of a manufacturing technique for electroless plated fiber material includes an electroless plating process in which the fiber material is immersed in a plating solution. (See, for example, Patent Documents 1 to 3.)
[0003] Another example of a manufacturing technique for electroless plated fiber material includes an electroless plating process in which a solution containing metal ions is sprayed by electrospray onto a fiber material containing a reducing agent, thereby generating metal particles in the fiber material through a reaction between the metal ions and the reducing agent (see, for example, Patent Document 4).
[0004] Yet another example of a manufacturing technique for electrolessly plated fiber material includes an electroless plating process in which a solution containing metal ions is sprayed onto the fiber material in a state in which the material is charged to one of positive and negative potentials by electrospraying, and a solution containing a reducing agent is sprayed onto the fiber material in a state in which the material is charged to the other of positive and negative potentials by electrospraying, thereby producing metal particles in the fiber material through a reaction between the metal ions and the reducing agent (see, for example, Patent Document 5).
[0005] In one example, another example, and a further example of a manufacturing technique for electroless plated fiber material, preparation steps such as a cleaning step in which the fiber material is immersed in a cleaning solution, a tannic acid treatment step in which the fiber material is immersed in a tannic acid solution to increase the adhesion between the fiber material and the plating film, and a catalysis treatment step in which the fiber material is immersed in a catalysis treatment solution to attach a catalyst to the fiber material are carried out before the electroless plating treatment step (see, for example, Patent Documents 1 to 5). [Prior art documents] [Patent documents]
[0006] [Patent Document 1] U.S. Pat. No. 3,877,965 [Patent Document 2] Japanese Patent Application Publication No. 7-173636 [Patent Document 3] JP 2003-105552 A [Patent Document 4] International Publication No. 2015 / 060341 [Patent Document 5] International Publication No. 2015 / 060342 Summary of the Invention [Problem to be solved by the invention]
[0007] In the electroless plating process of one example of the manufacturing technique for electroless plated fiber material, and in the preparation process of one example and another example of the manufacturing technique for electroless plated fiber material, it is necessary to immerse the fiber material in various processing solutions stored in large quantities in tanks or the like. However, the processing solution may contain precious metals, and using a large amount of such processing solution increases the manufacturing cost. In addition, the used solution contains environmentally hazardous substances, and it is costly to dispose of such a solution in a manner that complies with environmental regulations. When immersing the fiber material in the processing solution, it is necessary to perform batch processing in a tank or the like that stores the solution. Using an apparatus for performing batch processing also increases the manufacturing cost. Furthermore, these factors reduce the manufacturing efficiency of electroless plated fiber material.
[0008] There is room for improvement in the quality of electroless plated fiber materials, such as increasing the electrical conductivity of electroless plated fiber materials and reducing the thickness of the plating film of electroless plated fiber materials.
[0009] In view of this situation, it is desirable to reduce the amount of processing solution used and improve the quality of the electroless plated fiber material produced in the method for producing electroless plated fiber material. Furthermore, it is desirable to increase the conductivity of the electroless plated fiber material produced, reduce the thickness of the plating film of the electroless plated fiber material produced, reduce the production cost of the electroless plated fiber material, reduce the environmental load, and improve the production efficiency of the electroless plated fiber material in the method for producing electroless plated fiber material.
[0010] In electroless plated fiber materials, it is desirable to reduce the amount of processing solution used during production and to improve the quality. In addition, it is desirable to increase the electrical conductivity, reduce the thickness of the plating film, reduce production costs, reduce the environmental load that may occur during production, and improve production efficiency.
[0011] In the manufacturing system for electroless plated fiber materials, it is desirable to reduce the amount of processing solution used and improve the quality of the electroless plated fiber materials produced. In addition, in the manufacturing system for electroless plated fiber materials, it is desirable to increase the conductivity of the electroless plated fiber materials produced, reduce the thickness of the plating film of the electroless plated fiber materials produced, reduce manufacturing costs, reduce the environmental load, and improve the manufacturing efficiency of the electroless plated fiber materials. [Means for solving the problem]
[0012] A method for producing an electrolessly plated fibrous material according to one embodiment includes a catalysis step in which a catalyst solution containing a catalyst precursor is electrostatically sprayed, while being charged to a positive or negative potential, onto a fibrous material that is grounded or charged to a potential opposite to that of the catalyst solution and that has been given moisture, and a first reducing agent solution containing a reducing agent for the catalyst precursor is electrostatically sprayed, while being charged to a positive or negative potential, onto the fibrous material that is grounded or charged to a potential opposite to that of the first reducing agent solution and that has been given moisture, thereby obtaining a catalyst-applied fibrous material in which a catalyst has been applied to the fibrous material; and an electroless plating step in which a metal ion solution containing metal ions and a second reducing agent solution containing a reducing agent for the metal ions are electrostatically sprayed, while being similarly charged to a positive or negative potential, onto the catalyst-applied fibrous material that is grounded or charged to a potential opposite to that of the metal ion solution and the second reducing agent solution and that has been given moisture, so that they react in the same electric field at the catalyst-applied fibrous material, thereby obtaining an electrolessly plated fibrous material in which a plating coating has been formed on the catalyst-applied fibrous material.
[0013] In one embodiment, the electroless plated fiber material includes a catalysis step in which a catalyst solution containing a catalyst precursor is electrostatically sprayed, while being charged to a positive or negative potential, onto a fiber material that is grounded or charged to a potential opposite to that of the catalyst solution and that has been given moisture, and a first reducing agent solution containing a reducing agent for the catalyst precursor is electrostatically sprayed, while being charged to a positive or negative potential, onto the fiber material that is grounded or charged to a potential opposite to that of the first reducing agent solution and that has been given moisture, thereby obtaining a catalyst-applied fiber material in which a catalyst has been applied to the fiber material; The catalyst-applied fiber material is produced by a manufacturing method including an electroless plating process in which a metal ion solution containing metal ions and a second reducing agent solution containing a reducing agent for the metal ions are electrostatically sprayed, each of which is charged to the same positive or negative potential, onto the catalyst-applied fiber material which is grounded or charged to a potential opposite to the potentials of the metal ion solution and the second reducing agent solution and which has been given moisture, so that they react within the same electric field in the catalyst-applied fiber material, thereby obtaining an electroless plated fiber material in which a plating coating is formed on the catalyst-applied fiber material.
[0014] A manufacturing system for electrolessly plated fibrous materials according to one embodiment includes a catalysis device configured to obtain a catalyst-applied fibrous material in which a catalyst is applied to a fibrous material, an electroless plating device configured to obtain an electrolessly plated fibrous material in which a plating film is formed on the catalyst-applied fibrous material, and a fibrous material sent to the catalysis device, wherein the catalysis device includes a catalyst nozzle configured to electrostatically spray a catalyst solution containing a catalyst precursor, while being charged to a positive or negative potential, onto the fibrous material that is grounded or charged to a potential opposite to the potential of the catalyst solution and to which moisture has been applied, and a catalyst nozzle configured to electrostatically spray a first reducing agent solution containing a reducing agent for the catalyst precursor, while being charged to a positive or negative potential, onto the fibrous material that is grounded or charged to a potential opposite to the potential of the first reducing agent solution and to which moisture has been applied. and a first reducing agent nozzle configured as described above, wherein the electroless plating apparatus has a metal ion nozzle configured to electrostatically spray a metal ion solution containing metal ions, charged to a positive or negative potential, onto the catalyst-applied fiber material, and a second reducing agent nozzle configured to electrostatically spray a second reducing agent solution containing a reducing agent for the metal ions, charged to the same potential as the metal ion solution, onto the catalyst-applied fiber material, and the electroless plating apparatus is configured to react the metal ion solution electrostatically sprayed from the metal ion nozzle and the second reducing agent solution electrostatically sprayed from the second reducing agent nozzle within the same electric field at the catalyst-applied fiber material that is grounded or charged to a potential opposite to the potentials of the metal ion solution and the second reducing agent solution and has been given moisture. Effect of the Invention
[0015] In the manufacturing method of electroless plated fiber material according to one embodiment, the amount of processing solution used can be reduced, and the quality of the electroless plated fiber material produced can be improved. Furthermore, in the manufacturing method of electroless plated fiber material according to one embodiment, the conductivity of the electroless plated fiber material produced can be increased, the thickness of the plating film of the electroless plated fiber material produced can be reduced, the manufacturing cost of the electroless plated fiber material can be reduced, the environmental load can be reduced, and the manufacturing efficiency of the electroless plated fiber material can be improved.
[0016] In the electroless plated fiber material according to one embodiment, the amount of processing solution used during production can be reduced, and the quality can be improved. In addition, in the electroless plated fiber material according to one embodiment, the electrical conductivity can be increased, the thickness of the plating film can be reduced, the production cost can be reduced, the environmental load that may occur during production can be reduced, and the production efficiency can be improved.
[0017] In the manufacturing system for electroless plated fiber material according to one embodiment, the amount of processing solution used can be reduced, and the quality of the electroless plated fiber material produced can be improved. Furthermore, in the manufacturing system for electroless plated fiber material according to one embodiment, the conductivity of the electroless plated fiber material produced can be increased, the thickness of the plating film of the electroless plated fiber material produced can be reduced, the manufacturing cost can be reduced, the environmental load can be reduced, and the manufacturing efficiency of the electroless plated fiber material can be improved. [Brief description of the drawings]
[0018] [Figure 1] FIG. 1 is a flow chart for explaining a method for producing an electrolessly plated fiber material according to the first embodiment. [Diagram 2] FIG. 2 is a front view showing a schematic diagram of a catalysis device used in the catalysis step of the method for producing an electrolessly plated fibrous material according to the first embodiment, together with a support device that supports the fibrous material. [Diagram 3] FIG. 3 is a front view showing a schematic diagram of an electroless plating apparatus used in the electroless plating step of the method for producing an electroless plated fiber material according to the first embodiment, together with a supporting device. [Figure 4] FIG. 4 is a cross-sectional view that shows a schematic diagram of a degreasing apparatus used in the degreasing step of the manufacturing method for electrolessly plated fibrous material according to the first embodiment. [Diagram 5] FIG. 5 is a cross-sectional view that shows a schematic diagram of a pretreatment device used in the pretreatment step of the method for producing an electrolessly plated fibrous material according to the first embodiment. [Figure 6]FIG. 6 is a front view showing a schematic diagram of a cleaning device used in each of the pre-, mid-, and post-cleaning steps of the method for producing electrolessly plated fiber material according to the first embodiment, together with a supporting device. [Figure 7] FIG. 7 is a schematic diagram of a manufacturing system for electrolessly plated fiber material according to the second embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] The electroless plated fiber material and its manufacturing method and manufacturing system according to the first and second embodiments are described below. In the manufacturing method and manufacturing system according to the first and second embodiments, a fiber material having a plating film in which metal is deposited by electroless plating is produced, i.e., an electroless plated fiber material.
[0020] "First embodiment" The electroless plated fiber material according to the first embodiment and the manufacturing method and manufacturing system thereof will be described.
[0021] "Outline of electroless plated fiber material and its manufacturing method" An outline of the electrolessly plated fiber material A4 and its manufacturing method according to this embodiment will be described with reference to Figures 1 to 3. As shown in Figure 1, the manufacturing method of the electrolessly plated fiber material A4 generally includes a catalysis step S5 (details of which are shown in Figure 2) and an electroless plating step S7 (details of which are shown in Figure 3).
[0022] In such a manufacturing method, as shown in Fig. 2, in the catalysis step S5, a fibrous material A2 described later is grounded, and while moisture is added to the fibrous material A2, a catalyst solution B, which is a solution containing a catalyst precursor, is electrostatically sprayed onto the fibrous material A2 in a state where it is positively charged (indicated by the sign +). However, instead of grounding the fibrous material in the catalysis step, the fibrous material can be charged to a potential opposite to that of the catalyst solution. Also, the catalyst solution can be electrostatically sprayed onto the fibrous material in a state where it is negatively charged.
[0023] In the catalysis step S5, the fiber material A2 is grounded and a first reducing agent solution C, which is a solution containing a reducing agent of a catalyst precursor, is electrostatically sprayed onto the fiber material A2 while being charged to a positive potential (indicated by the symbol +) while moisture is being added to the fiber material A2. The potential of the catalyst solution B and the potential of the first reducing agent solution C are the same.
[0024] However, in the catalysis step, instead of grounding the textile material, the textile material can be charged to a potential opposite to that of the first reducing agent solution. Also, the first reducing agent solution can be electrostatically sprayed onto the textile material in a negatively charged state. The potential of the first reducing agent solution can be made different from that of the catalytic solution.
[0025] In the catalyst application step S5, a catalyst-applied fiber material A3 is obtained by applying a catalyst to the fiber material A2. In the following, the catalyst-applied fiber material A3 is simply referred to as the fiber material A3, as necessary.
[0026] 3, in the electroless plating process S7, the catalyst-applied fiber material A3 is grounded and moisture is applied to the fiber material A3, while a metal ion solution D, which is a solution containing metal ions, and a second reducing agent solution E, which is a solution containing a reducing agent for metal ions, are electrostatically sprayed onto the fiber material A3 while each is charged to a positive potential (indicated by the symbol +), so that they react in the same electric field at the fiber material A3. The potential of the metal ion solution D is the same as the potential of the second reducing agent solution E. The potentials of the metal ion solution D and the second reducing agent solution E are also the same as the potentials of the catalyst solution B and the first reducing agent solution C.
[0027] However, instead of grounding the textile material during the electroless plating process, the textile material can be charged to a potential opposite to that of the metal ion solution and the second reducing agent solution. Also, the metal ion solution and the second reducing agent solution can be electrostatically sprayed onto the textile material while being negatively charged. The potentials of the metal ion solution and the second reducing agent solution can be different from one or both of the potentials of the catalyst solution and the first reducing agent solution.
[0028] In such an electroless plating step S7, electroless plated fiber material A4 is obtained in which a plating film is formed on fiber material A3. In the following, electroless plated fiber material A4 will be simply referred to as fiber material A4 as necessary. The electroless plated fiber material A4 according to this embodiment can be generally manufactured by such a manufacturing method.
[0029] "Details of electroless plated fiber material and its manufacturing method" The electroless plated fiber material A4 according to this embodiment and the manufacturing method thereof will be described in detail with reference to Figures 1 to 6. As shown in Figure 1, the manufacturing method of the electroless plated fiber material A4 can also include, in detail, a degreasing step S1 (details shown in Figure 4), a pre-drying step S2, a pre-treatment step S3 (details shown in Figure 5), a pre-cleaning step S4 (details shown in Figure 6), a catalyzing step S5 (details shown in Figure 2), a middle cleaning step S6 (details shown in Figure 6), an electroless plating step S7 (details shown in Figure 3), a post-cleaning step S8 (details shown in Figure 6), and a post-drying step S9.
[0030] In such a manufacturing method, as shown in Fig. 4, the fiber material A1 is degreased in a degreasing step S1. After the degreasing step S1, the fiber material A1 is dried in a pre-drying step S2, although not shown in detail. Note that if the degreasing liquid F is volatile, the pre-drying step S2 can be omitted.
[0031] As shown in Fig. 5, in the pretreatment step S3, the fibrous material A1 dried in the predrying step S2 is pretreated so as to be negatively charged in order to improve the adhesion between the pretreated fibrous material A2 described below and the plating film. In the pretreatment step S3, the fibrous material A1 is pretreated to obtain the pretreated fibrous material A2. In the following, the pretreated fibrous material A2 will be simply referred to as the fibrous material A2 as necessary. However, when one or both of the catalysis step and the electroless plating step include the operation of electrostatically spraying a negatively charged solution onto the fibrous material as described above, the pretreatment step can be omitted.
[0032] As shown in Fig. 6, after the pretreatment step S3, the pretreated fiber material A2 is washed in the pre-cleaning step S4. As shown in Fig. 2, in the catalyzing step S5, the fiber material A2 washed in the pre-cleaning step S4 is grounded, and while moisture is added to the fiber material A2, the catalyst solution B is electrostatically sprayed onto the fiber material A2 in a positively charged state. Also, in the catalyzing step S5, the fiber material A2 is grounded, and while moisture is added to the fiber material A2, the first reducing agent solution C is electrostatically sprayed onto the fiber material A2 in a positively charged state. In the catalyzing step S5, a catalyst-added fiber material A3 is obtained.
[0033] As shown in Fig. 6, after the catalysis step S5, the catalyst-added fiber material A3 is washed in the intermediate washing step S6. As shown in Fig. 3, in the electroless plating step S7, the fiber material A3 washed in the intermediate washing step S6 is grounded, and while the fiber material A3 is being moistened, a metal ion solution D and a second reducing agent solution E are electrostatically sprayed onto the fiber material A3 while being positively charged, so that they react in the same electric field at the fiber material A3. In the electroless plating step S7, an electroless plated fiber material A4 is obtained.
[0034] As shown in Fig. 6, after the electroless plating step S7, the electroless plated fiber material A4 is washed in a post-cleaning step S8. Although not specifically shown, in a post-drying step S9, the fiber material A4 washed in the post-cleaning step S8 is dried. The manufacturing method for the electroless plated fiber material may also include an annealing step of annealing the electroless plated fiber material after the post-drying step. In detail, the electroless plated fiber material A4 according to this embodiment can be manufactured by such a manufacturing method.
[0035] "Details of fiber materials" The fiber material A1 can be specifically as follows. The fiber material A1 is a thread-like material containing a polymer compound as a constituent, or a material obtained by bundling the threads (cotton, woven fabric, nonwoven fabric, paper, etc.), and there is no particular limitation on the specific material, the difference between natural and synthetic fibers, the form of the material, etc. For example, the types of fiber materials include plant fibers such as hemp and cotton, animal fibers such as wool and silk, regenerated fibers such as rayon, polyamide-based synthetic fibers such as nylon (nylon 6,6, etc.), polyester-based synthetic fibers, acrylic-based synthetic fibers, polyvinyl alcohol-based synthetic fibers, polyolefin-based synthetic fibers, polyurethane-based synthetic fibers, cellulose-based semi-synthetic fibers, protein-based semi-synthetic fibers, etc. The fiber material is more preferably a thread, a woven fabric, a nonwoven fabric, a knitted fabric, paper, or a film.
[0036] When the fiber material is thread, for example, the thickness of the thread can be about 30 denier to about 1200 denier. Furthermore, the thickness of the thread is preferably about 30 denier to about 300 denier.
[0037] Considering that moisture is added to the fiber materials A2 and A3 in the catalysis step S5 and the electroless plating step S7, it is preferable that the fiber material A1 is hydrophilic. However, the fiber material may be hydrophobic, and in this case, it is preferable that the fiber material is subjected to a treatment for imparting hydrophilicity to the fiber material, such as a surface modification treatment.
[0038] "Details of the degreasing process" As shown in Fig. 4, the degreasing step S1 can be specifically performed as follows. In the degreasing step S1, the textile material A1 is immersed in a degreasing liquid F, thereby degreasing the textile material A1. In the degreasing step S1, yarn oil, woven fabric oil, knitted fabric oil, dirt, etc. can be removed from the textile material A1.
[0039] In the degreasing step S1, a degreasing device 10 configured to be able to degrease the fibrous material A1 is used. The degreasing device 10 has a tank 11 configured to be able to store a degreasing liquid F. In the degreasing step S1, the entire fibrous material A1 is immersed in the degreasing liquid F in the tank 11.
[0040] As the degreasing liquid F, any liquid that is normally used for degreasing the fibers can be used depending on the type of the fibers. For example, the degreasing liquid F can be an organic solvent containing acetone, isopropyl alcohol, ethanol, chloroform, methanol, xylene, etc. The degreasing liquid F can also be an alkaline cleaner containing caustic soda, sodium carbonate, sodium triphosphate, sodium tripolyphosphate, sodium orthosilicate, sodium metasilicate, a nonionic surfactant, etc.
[0041] The ambient temperature of the environment in which the degreasing step S1 is carried out, i.e., the ambient temperature of the degreasing device 10, may be room temperature. The treatment temperature of the degreasing liquid F may be room temperature (about 20°C) to about 80°C. The immersion time for immersing the fiber material A1 in the degreasing liquid F may be about 1 minute to about 10 minutes. However, the ambient temperature, treatment temperature, and immersion time are not limited to these. The ambient temperature, treatment temperature, and immersion time may be appropriately adjusted so as to efficiently remove raw yarn oil, woven fabric oil, knitted fabric oil, dirt, and the like from the fiber material.
[0042] "Details of pre- and post-drying processes" Although not specifically shown, the pre- and post-drying steps S2, S9 can be as follows. In the pre-drying step S2, warm or hot air is applied to the fibrous material A1 degreased in the degreasing step S1 to dry the fibrous material A1. In the post-drying step S9, warm or hot air is applied to the electroless plated fibrous material A4 cleaned in the post-cleaning step S8 to dry the fibrous material A4.
[0043] In each of the pre- and post-drying steps S2 and S9, a drying device (not shown) configured to apply warm or hot air to the fiber materials A1 and A4 is used. However, in either the pre- and post-drying steps, the fiber materials can also be naturally dried.
[0044] "Details of the pre-treatment process" As shown in Fig. 5, the pretreatment step S3 can be specifically performed as follows. In the pretreatment step S3, the fiber material A1 is immersed in a treatment liquid G containing a treatment agent, thereby negatively charging the fiber material A1. The pretreatment step S3 can improve the adhesion between the pretreated fiber material A2 and the plating coating.
[0045] In the pretreatment step S3, a pretreatment device 20 is used that is configured to perform a pretreatment that can improve the adhesion between the fiber material A2 and the plating film. The pretreatment device 20 has a tank 21 that is configured to store a treatment liquid G. In the pretreatment step S3, the entire fiber material A2 is immersed in the treatment liquid G in the tank 21.
[0046] The treatment agent contained in the treatment liquid G can be a solution containing a substance capable of giving a negative charge to the fiber material A1, such as polyphenol compounds such as tannic acid, gallic acid, pyrogallol, and catechol. By giving a negative charge to the fiber material A1 and making it negatively charged, the adhesion of metal ions, which are catalyst precursors, to the pretreated fiber material A2 can be increased in the subsequent catalysis step S5. In addition, the adhesion between the plating film formed thereafter and the catalyst-applied fiber material A3 can be increased. When the treatment agent is tannic acid, the treatment liquid G can be called a tannic acid solution G, and the pretreatment step S3 can be called a tannic acid treatment step S3. The concentration of the treatment agent in the treatment liquid G can be about 0.1% by mass to about 5.0% by mass.
[0047] The ambient temperature of the environment in which the pretreatment step S3 is carried out, i.e., the ambient temperature of the pretreatment device 20, may be room temperature. The treatment temperature of the treatment liquid G may be room temperature (about 20°C) to about 100°C. The immersion time for immersing the fiber material A1 in the treatment liquid G may be about 1 minute to about 10 minutes. However, the ambient temperature, treatment temperature, and immersion time are not limited to these. The ambient temperature, treatment temperature, and immersion time may be appropriately adjusted so as to enhance the adhesion between the fiber material and the plating film. Note that the pretreatment step may be other treatments that are usually performed as pretreatments for electroless plating of the fiber depending on the type of fiber material, and is not limited to pretreatments using a treatment liquid.
[0048] "Details of pre-, mid- and post-cleaning processes" As shown in FIG. 6, each of the pre-, intermediate, and post-cleaning steps S4, S6, and S8 can be specifically performed as follows. In the pre-cleaning step S4, the cleaning liquid H is discharged onto the pretreated fiber material A2, thereby cleaning the fiber material A2. In the intermediate cleaning step S6, the cleaning liquid H is discharged onto the catalyst-added fiber material A3, thereby cleaning the fiber material A3. In the post-cleaning step S8, the cleaning liquid H is discharged onto the electroless plated fiber material A4, thereby cleaning the fiber material A4. In each of the pre-, intermediate, and post-cleaning steps S4, S6, and S8, a cleaning device 30 capable of discharging the cleaning liquid H onto the fiber materials A2, A3, and A4 is used. The cleaning device 30 includes a cleaning nozzle 30a having a discharge port 30b configured to discharge the cleaning liquid H.
[0049] However, in at least one of the pre-, mid-, and post-cleaning steps, the textile material may be immersed in a cleaning liquid, thereby cleaning the textile material. In this case, a cleaning device having a tank capable of storing the cleaning liquid may be used in at least one of the pre-, mid-, and post-cleaning steps.
[0050] The cleaning liquid H may be water. Such water may be distilled water, ion-exchanged water, RO (Reverse Osmosis) water, purified water such as pure water and ultrapure water, tap water, natural water, etc. The cleaning liquids H in the pre-, middle-, and post-cleaning steps may be the same as each other. However, the cleaning liquid is not limited to water. The cleaning liquids in the pre-, middle-, and post-cleaning steps S4, S6, S8 may be different from each other. One of the cleaning liquids in the pre-, middle-, and post-cleaning steps may be different from the remaining two.
[0051] Here, as shown in Fig. 6, a support device 40 that supports the fiber materials A2, A3, and A4 in each of the pre-, middle, and post-cleaning steps S4, S6, and S8 will be described. The support device 40 has two support parts 41, 42 that are arranged at a distance from each other so as to bridge the fiber materials A2 to A4. Hereinafter, one of these two support parts 41, 42 will be referred to as a first support part 41, and the other of the two support parts 41, 42 will be referred to as a second support part 42, as necessary.
[0052] The supporting device 40 has a connecting portion 43 that connects the first and second supporting portions 41, 42. The fibrous materials A2 to A4 are stretched across the first and second supporting portions 41, 42 with a predetermined tension applied thereto. At this time, it is preferable that the fibrous materials A2 to A4 are tensioned to such an extent that no slack that would cause the radial positions of the fibrous materials A2 to A4 to vary is generated. The supporting device 40 is configured to fix the fibrous materials A2 to A4 to the first and second supporting portions 41, 42. However, the supporting device may be configured to move the fibrous materials along their longitudinal direction while being supported by the first and second supporting portions.
[0053] In FIG. 6, the first support portion 41 is disposed above the second support portion 42 with a gap therebetween. The fiber materials A2 to A4 are bridged across the first and second support portions 41, 42 so as to be substantially aligned in the vertical direction. However, the arrangement of the first and second support portions is not limited thereto. For example, the first and second support portions may be disposed horizontally with a gap therebetween. In this case, the fiber materials may be bridged across the first and second support portions so as to be substantially aligned in the horizontal direction.
[0054] One or both of the two supporting parts 41, 42 are configured to have electrical conductivity and are electrically grounded. The fiber materials A2 to A4 are grounded via one or both of the two supporting parts 41, 42. In FIG. 6, the second supporting part 42 is electrically conductive and is electrically grounded. In this case, the first supporting part 41 may be either electrically conductive or non-conductive. However, instead of the second supporting part, the first supporting part may be electrically conductive and is electrically grounded. Also, both the first and second supporting parts may be grounded.
[0055] As described above, when the first support part 41 is disposed above the second support part 42 with a gap therebetween and the fibrous materials A2 to A4 are disposed substantially vertically, the discharge port 30b of the cleaning nozzle 30a of the cleaning device 30 is disposed above the first support part 41. The cleaning liquid H discharged from the discharge port 30b flows from the first support part 41 along the fibrous materials A2 to A4 to the second support part 42 due to gravity. Such cleaning liquid H can clean the fibrous materials A2 to A4.
[0056] Although details will be described later, the supporting device 40 supports the fiber materials A2 and A3 in the catalyzing step S5 and the electroless plating step S7. The supporting device 40 can also support the fiber material A4 in the post-drying step S9.
[0057] "Details of the catalysis process" As shown in Fig. 2, the catalysis step S5 can be specifically performed as follows. In the catalysis step S5, the catalyst solution B is electrostatically sprayed onto the pretreated fiber material A2 in advance, and the first reducing agent solution C is electrostatically sprayed onto the same fiber material A2 following the catalyst solution B. However, in the catalysis step, the catalyst solution and the first reducing agent solution can also be electrostatically sprayed onto the fiber material at the same time. In the catalysis step, the first reducing agent solution can also be electrostatically sprayed onto the fiber material in advance, and the catalyst solution can also be electrostatically sprayed onto the fiber material following the first reducing agent solution.
[0058] In the catalysis step S5, the fiber material A2 is supported by the support device 40. Also in the catalysis step S5, a catalysis device 50 is used that is configured to cause a reaction on the surface of the fiber material A2 that provides a catalyst for the electroless plating reaction.
[0059] The catalyst nozzle mechanism 50 has a catalyst nozzle mechanism 51 configured to be capable of electrostatically spraying the catalyst solution B. The catalyst nozzle mechanism 51 has a catalyst nozzle 51a having a spray port 51b for electrostatically spraying the catalyst solution B. The catalyst nozzle 51a is configured to be movable along the longitudinal direction of the fiber material A2, as indicated by a double-sided arrow P1. The catalyst nozzle 51a can also repeatedly move back and forth along the longitudinal direction of the fiber material A2. The catalyst nozzle mechanism 51 has a catalyst supply pipe 51c configured to allow the catalyst solution B supplied to the catalyst nozzle 51a to pass through. A power source (not shown) can be used to charge the catalyst solution B to a positive potential (or a negative potential).
[0060] In such a catalyst nozzle mechanism 51, the catalyst solution B is sprayed in the form of droplets from the spray nozzle 51b of the catalyst nozzle 51a through the catalyst supply pipe 51c. At this time, an electric field can be generated between the catalyst nozzle 51a and the fiber material A2 by the electrospray phenomenon. When the fiber material is to be charged to a potential opposite to that of the catalyst solution, the fiber material can be charged to the opposite potential using a power source.
[0061] Here, the electrospray phenomenon will be described. For example, in the electric field between the catalyst nozzle 51a of the catalyst nozzle mechanism 51 and the fiber material A2, the catalyst nozzle 51a side is set to a positive potential by using a power source or the like, and the grounded fiber material A2 side is set to about 0 kV or a negative potential. By providing a potential gradient between the catalyst nozzle 51a and the fiber material A2 in this way, the electrospray phenomenon can be generated.
[0062] Furthermore, in a configuration in which the fibrous material A2 is fixed to the first and second support parts 41, 42 of the support device 40, if the catalyst solution B is sprayed from the catalyst nozzle 51a while moving the catalyst nozzle 51a along the longitudinal direction of the fibrous material A2, the catalyst solution B can be sprayed over the entire fibrous material A2. However, in a configuration in which the support device moves the fibrous material along its longitudinal direction while supporting it with the first and second support parts as described above, the catalyst solution can be sprayed over the entire fibrous material even if the catalyst nozzle is fixed in a certain position.
[0063] The catalysis device 50 has a first reducing agent nozzle mechanism 52 configured to be able to electrostatically spray the first reducing agent solution C. The first reducing agent nozzle mechanism 52 includes a first reducing agent nozzle 52a having a spray port 52b for electrostatically spraying the first reducing agent solution C. The first reducing agent nozzle 52a is configured to be able to move along the longitudinal direction of the fiber material A2 as shown by the double-sided arrow P2. The first reducing agent nozzle 52a can also repeatedly move back and forth along the longitudinal direction of the fiber material A2. The first reducing agent nozzle mechanism 52 has a first reducing agent supply pipe 52c configured to allow the first reducing agent solution C supplied to the first reducing agent nozzle 52a to pass through. A power source (not shown) can be used to charge the first reducing agent solution C to a positive potential (or a negative potential).
[0064] In such a first reducing agent nozzle mechanism 52, the first reducing agent solution C is sprayed in the form of droplets from the spray port 52b of the first reducing agent nozzle 52a through the first reducing agent supply pipe 52c. Furthermore, an electric field can be generated between the first reducing agent nozzle 52a and the fiber material A2 by the electrospray phenomenon similar to that of the catalyst nozzle mechanism 51. When the fiber material is to be charged to a potential opposite to that of the first reducing agent solution, the fiber material can be charged to the opposite potential using a power source.
[0065] Furthermore, in a configuration in which the fibrous material A2 is fixed to the first and second support parts 41, 42 of the support device 40, if the first reducing agent solution C is sprayed from the first reducing agent nozzle 52a while moving the first reducing agent nozzle 52a along the longitudinal direction of the fibrous material A2, the first reducing agent solution C can be sprayed onto the entire fibrous material A2. However, in a configuration in which the support device moves the fibrous material along its longitudinal direction while supporting it with the first and second support parts as described above, the first reducing agent solution can be sprayed onto the entire fibrous material even if the first reducing agent nozzle is fixed at a certain position.
[0066] Regarding the relationship between the catalyst nozzle mechanism 51 and the first reducing agent nozzle mechanism 52, the catalyst nozzle 51a and the first reducing agent nozzle 52a are configured to be movable so as not to hinder each other's movement along the fibrous material A2. In FIG. 2, the catalyst nozzle 51a and the first reducing agent nozzle 52a are arranged to be shifted from each other in the circumferential direction of the fibrous material A2. The catalyst nozzle 51a and the first reducing agent nozzle 52a can be arranged so that their discharge ports 51b, 52b face in opposing directions while facing the fibrous material A2. In this case, the distance in the longitudinal direction of the fibrous material A2 between the discharge ports 51b, 52b can also be changed according to the movement of the catalyst nozzle 51a and the first reducing agent nozzle 52a in the longitudinal direction of the fibrous material A2 separately.
[0067] However, the catalyst nozzle and the first reducing agent nozzle may be arranged to be spaced apart in the longitudinal direction of the fibrous material. The catalyst nozzle and the first reducing agent nozzle may be interchanged such that when one of them is arranged at an electrostatic spraying position close to the fibrous material for electrostatic spraying of the fibrous material, the other of them is retracted from the electrostatic spraying position.
[0068] For example, catalyst solution B may be a solution in which a salt or a complex compound of platinum, gold, silver, palladium, or the like, or a mixture of two or more of these, is dissolved. The salt may be a nitrate, sulfate, chloride, acetate, or the like. Therefore, catalyst solution B contains metal ions of platinum, gold, silver, palladium, or the like, which are catalyst precursors.
[0069] In particular, in order to reduce the surface tension of the droplets sprayed from the catalyst nozzle 51a, the catalyst solution B may contain lower alcohols having 1 to 3 carbon atoms, such as methanol, ethanol, isopropyl alcohol, etc.; ketones, such as acetone, methyl ethyl ketone, etc.; or a mixture of two or more of these. The concentration of the catalyst precursor in the catalyst solution B may be appropriately adjusted. For example, the concentration of the catalyst precursor may be in the range of about 0.01 mol / L or more and about 5 mol / L or less.
[0070] The reducing agent contained in the first reducing agent solution C can be selected to be optimal for the catalyst precursor species to be reduced. Examples of the reducing agent include hydroxymethanesulfinic acid, thioglycolic acid, sulfurous acid, or salts thereof such as sodium salts, potassium salts, and ammonium salts, ascorbic acid, citric acid, sodium hydrosulfite, thiourea, dithiothreitol, hydrazines, formaldehydes, boron hydrides, or a mixture of two or more of these.
[0071] Examples of hydrazines include hydrazine, hydrazine hydrate, hydrazine salts, hydrazine substituent derivatives or their salts, etc. Specific examples include hydrazine hydrate, hydrazine monohydrochloride, hydrazine dihydrochloride, hydrazine sulfate, hydrazine hydrobromide, hydrazine carbonate, methylhydrazine, phenylhydrazine, tert-butylhydrazine hydrochloride, carbohydrazide, etc.
[0072] Examples of formaldehydes include formaldehyde, paraformaldehyde, etc., or a mixture of two or more of these. Boron hydrides refer to reducing compounds having a boron-hydrogen bond, and specific examples include sodium borohydride, potassium borohydride, lithium borohydride, sodium cyanotrihydroborate, lithium triethylborohydride, tetrahydrofuran-borane complex, dimethylamine-borane complex, diphenylamine-borane complex, pyridine-borane complex, etc. In particular, the reducing agent is preferably ascorbic acid or a hydrazine.
[0073] The amount of reducing agent added in the first reducing agent solution C can be appropriately adjusted according to the type of reducing agent, the concentration of the catalyst precursor in the catalyst solution B, etc. For example, the amount of reducing agent added is preferably in the range of 1 to 2 times the chemical equivalent of the catalyst precursor. If the amount of reducing agent added is less than the chemical equivalent, the reduction reaction to the catalyst may not proceed sufficiently. On the other hand, there is no problem if the amount of reducing agent added exceeds twice the chemical equivalent, but the cost will increase.
[0074] The catalyst solution B and the first reducing agent solution C may be aqueous solutions or water-soluble solutions compatible with each other. As an example, the solvent used for each of the catalyst solution B and the first reducing agent solution C may be water, ethanol, DMF (N,N-dimethylformamide), acetone, or a mixture of two or more of these. In particular, the solvent used for each of the catalyst solution B and the first reducing agent solution C may be water, or an aqueous solution of water and a water-soluble solvent such as ethanol, DMF, or acetone. In addition, it is preferable that the solvents used for each of the catalyst solution B and the first reducing agent solution C are the same type.
[0075] In each of the catalyst nozzle 51a and the first reducing agent nozzle 52a, the diameter of the spray ports 51b, 52b can be about 0.03 mm or more, preferably about 0.05 mm or more, more preferably about 0.1 mm or more, and can be about 1.0 mm or less, preferably about 0.5 mm or less, more preferably about 0.3 mm or less. The atmospheric temperature of the environment in which the catalysis step S5 is performed, i.e., the ambient temperature of the catalysis device 50, can be room temperature.
[0076] In the catalysis step S5, the distance between the spray nozzle 51b of the catalyst nozzle 51a and the fiber material A2, and the distance between the spray nozzle 52b of the first reducing agent nozzle 52a and the fiber material A2 can each be approximately 5 mm or more, preferably approximately 7 mm or more, more preferably approximately 10 mm or more, and can be approximately 40 mm or less, preferably approximately 30 mm or less, more preferably approximately 20 mm or less.
[0077] In the catalysis step S5, the amount of the catalyst solution B sprayed from the catalyst nozzle 51a per unit time and the amount of the first reducing agent solution C sprayed from the first reducing agent nozzle 52a per unit time can be about 3 μL / min or more, preferably about 5 μL / min or more, more preferably about 7 μL / min or more, and about 50 μL / min or less, preferably about 30 μL / min or less, more preferably about 20 μL / min or less. In the catalysis step S5, the positive potential on the catalyst nozzle 51a side and the positive potential on the first reducing agent nozzle 52a side can be about +2.0 kV or more, preferably about +3.0 kV or more, more preferably about +4.5 kV or more, and about +10.0 kV or less, preferably about +8 kV or less, more preferably about +7 kV or less.
[0078] Furthermore, in the catalysis step S5, water I is discharged onto the fibrous material A2, thereby providing moisture to the fibrous material A2. By providing moisture to the fibrous material A2, the fibrous material A2 can be reliably grounded. The catalysis device 50 has a first moisture supply mechanism 53 configured to supply water I to the fibrous material A2. The first moisture supply mechanism 53 has a first moisture supply nozzle 53a having a discharge port 53b configured to discharge water I. The supply of water I to the fibrous material A2 may be performed continuously or intermittently throughout the execution of the catalysis step S5.
[0079] In the catalysis step S5, the water I for adding moisture to the fiber material A2 may be purified water such as distilled water, ion-exchanged water, RO (Reverse Osmosis) water, pure water, ultrapure water, etc. However, the water is not limited to these.
[0080] As described above, when the first support part 41 is disposed above the second support part 42 with a gap therebetween and the fibrous material A2 is disposed substantially along the vertical direction, the discharge port 53b of the first moisture supply nozzle 53a is disposed above the first support part 41. The water I discharged from the discharge port 53b flows from the first support part 41 along the fibrous material A2 to the second support part 42 due to gravity. Such water I can provide moisture to the fibrous material A2.
[0081] However, when the support device is configured to move the fiber material along its longitudinal direction while supporting the fiber material with the first and second support parts as described above, the first moisture supply mechanism can be configured to have a tank configured to be able to store water. In this case, the fiber material can pass through the water in the tank of the first moisture supply mechanism immediately before being sprayed with the catalyst solution or immediately before being sprayed with the first reducing agent solution, or both.
[0082] Furthermore, a catalytic metal coating, such as a metal palladium or platinum coating, can be formed on the fiber material A2 by the catalysis step S5. The amount of catalyst applied to the fiber material A2 can be appropriately adjusted so that an electroless plated fiber material A4 having a desired electrical resistance value, a desired plating metal coating thickness, etc. can be obtained in the subsequent electroless plating step S7.
[0083] "Details of the electroless plating process" 3, the electroless plating process S7 can be specifically performed as follows: In the electroless plating process S7, the metal ion solution D and the second reducing agent solution E, each positively charged, are electrostatically sprayed onto the catalyst-applied fiber material A3 at the same time so that they react with each other in the same electric field at the catalyst-applied fiber material A3.
[0084] In the electroless plating step S7, the fiber material A3 is supported by the supporting device 40. In the electroless plating step S7, an electroless plating device 60 configured to perform an electroless plating process on the fiber material A3 is also used.
[0085] The electroless plating apparatus 60 has a metal ion nozzle mechanism 61 configured to be able to electrostatically spray the metal ion solution D. The metal ion nozzle mechanism 61 has a metal ion nozzle 61a having a spray port 61b that electrostatically sprays the metal ion solution D. The metal ion nozzle 61a is configured to be able to move along the longitudinal direction of the fiber material A3, as indicated by the double-sided arrow Q1. The metal ion nozzle mechanism 61 has a metal ion supply pipe 61c configured to allow the metal ion solution D supplied to the metal ion nozzle 61a to pass through. A power source (not shown) can be used to charge the metal ion solution D to a positive potential (or negative potential).
[0086] In such a metal ion nozzle mechanism 61, the metal ion solution D is sprayed in the form of droplets from the spray port 61b of the metal ion nozzle 61a through the metal ion supply pipe 61c. At this time, an electric field can be generated between the metal ion nozzle 61a and the fiber material A3 by the electrospray phenomenon similar to that of the catalyst nozzle mechanism 51 described above. When the fiber material is to be charged to a potential opposite to that of the metal ion solution, the fiber material can be charged to the opposite potential using a power source.
[0087] Furthermore, in a configuration in which the fibrous material A3 is fixed to the first and second support parts 41, 42 of the supporting device 40, if the metal ion nozzle 61a is moved along the longitudinal direction of the fibrous material A3 while spraying the metal ion solution D from the metal ion nozzle 61a, the metal ion solution D can be sprayed onto the entire fibrous material A3. However, in a configuration in which the supporting device moves the fibrous material along its longitudinal direction while supporting it with the first and second support parts as described above, the metal ion solution can be sprayed onto the entire fibrous material even if the metal ion nozzle is fixed at a certain position.
[0088] The electroless plating apparatus 60 has a second reducing agent nozzle mechanism 62 configured to be able to electrostatically spray the second reducing agent solution E. The second reducing agent nozzle mechanism 62 is configured similarly to the first reducing agent nozzle mechanism 52, except that the second reducing agent nozzle mechanism 62 electrostatically sprays the second reducing agent solution E instead of the first reducing agent solution C. The second reducing agent nozzle 62a, spray port 62b, and second reducing agent supply pipe 62c of the second reducing agent nozzle mechanism 62 correspond to the first reducing agent nozzle 52a, spray port 52b, and first reducing agent supply pipe 52c of the first reducing agent nozzle mechanism 52, respectively.
[0089] The second reducing agent nozzle 62a is movable along the longitudinal direction of the fiber material A3, as indicated by the double-sided arrow Q2. A power source (not shown) can be used to charge the second reducing agent solution E to a positive potential (or a negative potential). When the fiber material is to be charged to a potential opposite to that of the second reducing agent solution, the power source can be used to charge the fiber material to the opposite potential.
[0090] In the electroless plating apparatus, the first reducing agent nozzle mechanism may be used instead of the second reducing agent nozzle mechanism. In this case, the first reducing agent nozzle mechanism is used in common in the catalysis apparatus and the electroless plating apparatus.
[0091] Regarding the relationship between the metal ion nozzle mechanism 61 and the second reducing agent nozzle mechanism 62, the metal ion nozzle 61a and the second reducing agent nozzle 62a are configured to be movable so as not to hinder each other's movement along the fiber material A3. In Fig. 3, the metal ion nozzle 61a and the second reducing agent nozzle 62a are arranged to be shifted from each other in the circumferential direction of the fiber material A3. Furthermore, the metal ion nozzle 61a and the second reducing agent nozzle 62a can be arranged to maintain a state in which they face each other while facing their discharge ports 61b, 62b toward the fiber material A3.
[0092] The metal ions contained in the metal ion solution D may be ions of a desired metal to be plated on the fiber material A3. Thus, the metal ion solution D may be, for example, a solution of a salt or a complex compound of platinum, gold, silver, copper, tin, nickel, iron, palladium, zinc, iron, cobalt, tungsten, ruthenium, indium, molybdenum, or the like, or a mixture of two or more of these, dissolved in a suitable solvent. The salt may be a nitrate, sulfate, chloride, acetate, or the like.
[0093] In particular, in order to reduce the surface tension of the droplets sprayed from the metal ion nozzle 61a, the metal ion solution D may contain lower alcohols having 1 to 3 carbon atoms, such as methanol, ethanol, isopropyl alcohol, etc.; ketones, such as acetone, methyl ethyl ketone, etc.; or a mixture of two or more of these. The concentration of the metal ions in the metal ion solution D may be appropriately adjusted. For example, the concentration of the metal ions may be in the range of 0.01 mol / L or more and 5 mol / L or less.
[0094] The reducing agent contained in the second reducing agent solution E can be selected so as to be optimal for the type of metal ions to be reduced. Examples of the reducing agent contained in the second reducing agent solution E include the same reducing agents as those contained in the first reducing agent solution C.
[0095] The amount of reducing agent added in the second reducing agent solution E can be appropriately adjusted depending on the type of reducing agent, the concentration of metal ions in the metal ion solution D, etc. For example, the amount of reducing agent added is preferably in the range of 1 to 2 times the chemical equivalent of the metal ions. If the amount of reducing agent added is less than the chemical equivalent, the reduction reaction to the metal ions may not proceed sufficiently. On the other hand, there is no problem if the amount of reducing agent added exceeds twice the chemical equivalent, but the cost will increase.
[0096] The metal ion solution D and the second reducing agent solution E may be aqueous solutions or water-soluble solutions compatible with each other. As an example, the solvent used for each of the metal ion solution D and the second reducing agent solution E may be water, ethanol, DMF, acetone, or a mixture of two or more of these. In particular, the solvent used for each of the metal ion solution D and the second reducing agent solution E may be water or an aqueous solution of water and a water-soluble solvent such as ethanol, DMF, or acetone. In addition, it is preferable that the solvents used for each of the metal ion solution D and the second reducing agent solution E are the same type.
[0097] Furthermore, in the electroless plating step S7, water J is discharged onto the fibrous material A3, thereby providing moisture to the fibrous material A3. The electroless plating apparatus 60 has a second moisture supply mechanism 63 configured to supply water J to the fibrous material A3. The second moisture supply mechanism 63 has a second moisture supply nozzle 63a having a discharge port 63b configured to discharge water J. The supply of water J to the fibrous material A3 may be performed continuously or intermittently throughout the execution of the electroless plating step S7.
[0098] In each of the metal ion nozzle 61a and the second reducing agent nozzle 62a, the diameter of the spray ports 61b, 62b can be about 0.03 mm or more, preferably about 0.05 mm or more, more preferably about 0.1 mm or more, and can be about 1.0 mm or less, preferably about 0.5 mm or less, more preferably about 0.3 mm or less. The atmospheric temperature of the environment in which the electroless plating step S7 is performed, i.e., the ambient temperature of the electroless plating apparatus 60, can be room temperature.
[0099] In the electroless plating process S7, the distance between the spray nozzle 61b of the metal ion nozzle 61a and the fiber material A3, and the distance between the spray nozzle 62b of the second reducing agent nozzle 62a and the fiber material A3 can each be approximately 5 mm or more, preferably approximately 7 mm or more, and more preferably approximately 10 mm or more, and can be approximately 40 mm or less, preferably approximately 30 mm or less, and more preferably approximately 20 mm or less.
[0100] In the electroless plating step S7, the amount of the metal ion solution D sprayed from the metal ion nozzle 61a per unit time and the amount of the second reducing agent solution E sprayed from the second reducing agent nozzle 62a per unit time can be about 3 μL / min or more, preferably about 5 μL / min or more, more preferably about 7 μL / min or more, and can be about 50 μL / min or less, preferably about 30 μL / min or less, more preferably about 20 μL / min or less. In the electroless plating step S7, the positive potential on the metal ion nozzle 61a side and the positive potential on the second reducing agent nozzle 62a side can be about +2.0 kV or more, preferably about +3.0 kV or more, more preferably about +4.5 kV or more, and can be about +10.0 kV or less, preferably about +8 kV or less, more preferably about +7 kV or less.
[0101] In the electroless plating step S7, the water J for providing moisture to the fiber material A3 may be purified water such as distilled water, ion-exchanged water, RO water, pure water, ultrapure water, etc. The water J used in the electroless plating step S7 may be the same type as the water I used in the catalyzing step S5. In addition, the water J used in the electroless plating step S7 may be a different type from the water I used in the catalyzing step S5. However, the water is not limited to this.
[0102] In the electroless plating apparatus, the first moisture supply mechanism may be used instead of the second moisture supply mechanism. In this case, the first moisture supply mechanism is used in common in the catalysis device and the electroless plating apparatus.
[0103] As described above, when the first support part 41 is disposed above the second support part 42 with a gap therebetween and the fibrous material A3 is disposed substantially along the vertical direction, the discharge port 63b of the second moisture supply nozzle 63a is disposed above the first support part 41. The water J discharged from the discharge port 63b flows from the first support part 41 along the fibrous material A3 to the second support part 42 due to gravity. Such water J can provide moisture to the fibrous material A3.
[0104] However, when the supporting device is configured to move the fiber material along its longitudinal direction while supporting the fiber material with the first and second supporting parts as described above, the second moisture supply mechanism can be configured to have a tank configured to store water. In this case, the fiber material can pass through the water in the tank of the second moisture supply mechanism immediately before being sprayed with the metal ion solution and the second reducing agent solution.
[0105] The electroless plating step S7 allows a desired plated metal coating to be formed on the catalytic metal coating applied to the fiber material A3. In the electroless plated fiber material A4 on which the plated metal coating is formed by the electroless plating step S7, the thickness of the plated metal coating can be reduced while the electrical resistance is lowered compared to the prior art. For example, the prior art includes a commercially available silver-plated conductive thread having an electrical resistance of about 2.0 Ω / cm and a thickness of about 2.1 μm. For example, the electrical resistance of the plated metal coating of the electroless plated fiber material A4 can be set to about 2.0 Ω / cm or less and the thickness of the plated metal coating can be set to about 0.4 μm or less.
[0106] "Manufacturing system for electroless plated fiber materials" 2 to 6, a manufacturing system for electrolessly plated fiber material A4 capable of implementing the manufacturing method for electrolessly plated fiber material A4 according to this embodiment is configured as follows. That is, the manufacturing system generally includes a catalyzing apparatus 50 and an electroless plating apparatus 60. The catalyzing apparatus 50 is configured to be capable of implementing the catalyzing step S5. The electroless plating apparatus 60 is configured to be capable of implementing the electroless plating step S7.
[0107] Further, the manufacturing system may specifically include a degreasing device 10, a pretreatment device 20, a cleaning device 30, a supporting device 40, the catalysis device 50, the electroless plating device 60, and a drying device (not shown). The degreasing device 10 is configured to be capable of carrying out a degreasing step S1. The pretreatment device 20 is configured to be capable of carrying out a pretreatment step S3. The cleaning device 30 is configured to be capable of carrying out pre-, middle-, and post-cleaning steps S4, S6, and S8. The supporting device 40 is configured to be capable of supporting the fiber materials A2 to A4. The drying device is configured to be capable of carrying out pre- and post-drying steps S2 and S9.
[0108] In addition, when the manufacturing method of electroless plated fiber material includes an annealing treatment step, the manufacturing system of electroless plated fiber material can include an annealing treatment device configured to be able to perform the annealing treatment step. For example, the annealing treatment device can have a heating mechanism configured to be able to heat the fiber material. The heating mechanism can be a hot air circulating oven. In this case, the annealing treatment device can also function as a drying device. Such an apparatus can also be called a drying and annealing treatment device.
[0109] As described above, the method for producing electrolessly plated fiber material A4 according to this embodiment comprises electrostatically spraying a catalyst solution B containing a catalyst precursor, while it is charged to a positive or negative potential, onto fiber material A2 which is grounded or charged to a potential opposite to that of the catalyst solution B and to which moisture has been added, and electrostatically spraying a first reducing agent solution C containing a reducing agent for the catalyst precursor, while it is charged to a positive or negative potential, onto fiber material A2 which is grounded or charged to a potential opposite to that of the first reducing agent solution C and to which moisture has been added, thereby producing a metal ion-containing electroless plated fiber material A4. The method includes an electroless plating process S7 in which solution D and a second reducing agent solution E containing a reducing agent for the metal ions are electrostatically sprayed onto the catalyst-applied fiber material A3, which is grounded or charged to a potential opposite to the potentials of the metal ion solution D and the second reducing agent solution E and has been moistened, while each of them is charged to the same positive or negative potential, so that they react within the same electric field in the catalyst-applied fiber material A3, thereby obtaining an electroless plated fiber material A4 in which a plating coating is formed on the catalyst-applied fiber material A3.
[0110] The electroless plating fiber material A4 according to this embodiment is produced by electrostatically spraying a catalyst solution B containing a catalyst precursor, while it is charged to a positive or negative potential, onto a fiber material A2 that is grounded or charged to a potential opposite to that of the catalyst solution B and that has been given moisture, and electrostatically spraying a first reducing agent solution C containing a reducing agent for the catalyst precursor, while it is charged to a positive or negative potential, onto the fiber material A2 that is grounded or charged to a potential opposite to that of the first reducing agent solution C and that has been given moisture, thereby producing a metal ion solution D containing metal ions and a metal ion solution C containing the metal ions. and an electroless plating step S7 in which a catalyst-applied fiber material A3 having a plating film formed thereon is electrostatically sprayed with a second reducing agent solution E containing a reducing agent of the metal ion type and a reducing agent of the metal ion type, the second reducing agent solution E being charged to the same positive or negative potential, and the catalyst-applied fiber material A3 being grounded or charged to a potential opposite to the potentials of the metal ion solution D and the second reducing agent solution E and being moistened, so that the reaction occurs within the same electric field in the catalyst-applied fiber material A3, thereby obtaining an electroless plated fiber material A4 in which a plating film is formed on the catalyst-applied fiber material A3.
[0111] The manufacturing system for electrolessly plated fibrous material A4 according to this embodiment includes a catalysis device 50 configured to obtain a catalyst-applied fibrous material A3 in which a catalyst is applied to a fibrous material A2, and an electroless plating device 60 configured to obtain an electroless plated fibrous material A4 in which a plating film is formed on the catalyst-applied fibrous material A3. The catalysis device 50 includes a catalyst nozzle 51a configured to electrostatically spray a catalyst solution B containing a catalyst precursor, while being charged to a positive or negative potential, onto the fibrous material A2 which is grounded or charged to a potential opposite to the potential of the catalyst solution B and to which moisture has been applied, and a first reducing agent solution C containing a reducing agent for the catalyst precursor, while being charged to a positive or negative potential, onto the fibrous material A2 which is grounded or charged to a potential opposite to the potential of the first reducing agent solution C and to which moisture has been applied. The electroless plating apparatus 60 has a metal ion nozzle 61a configured to electrostatically spray a metal ion solution D containing metal ions in a state charged to a positive or negative potential onto the catalyst-applied fiber material A3, and a second reducing agent nozzle 62a configured to electrostatically spray a second reducing agent solution E containing a reducing agent for the metal ions in a state charged to the same potential as the metal ion solution D onto the catalyst-applied fiber material A3, and the electroless plating apparatus 60 is configured to react the metal ion solution D electrostatically sprayed from the metal ion nozzle 61a and the second reducing agent solution E electrostatically sprayed from the second reducing agent nozzle 62a within the same electric field at the catalyst-applied fiber material A3 which is grounded or charged to a potential opposite to the potentials of the metal ion solution D and the second reducing agent solution E and to which moisture has been applied.
[0112] In the electroless plating process S7 and the electroless plating device 60, the metal ion solution D and the second reducing agent solution E are charged to the same potential when electrostatically sprayed. Therefore, the metal ion solution D and the second reducing agent solution E do not collide with each other until they reach the fibrous material A3. After that, when the metal ion solution D and the second reducing agent solution E reach the grounded fibrous material A3, they lose their charge. At this time, the metal ion solution D and the second reducing agent solution E come into contact, mix, and react for the first time. Therefore, on the fibrous material A3, the metal ions of the metal ion solution D are efficiently reduced by the reducing agent of the second reducing agent solution E, and as a result, a plating film in which metal is precipitated can be efficiently formed on the fibrous material A3. In particular, the electroless plated fibrous material A4 having such a plating film can have its conductivity increased and the thickness of the plating film can be reduced. Therefore, the quality of the electroless plated fibrous material A4 can be improved.
[0113] In such electroless plated fiber material A4 and its manufacturing method and manufacturing system, the amount of processing solution electrostatically sprayed in each of the catalyzing step S5 and the catalyzing device 50 can be reduced compared to the amount of processing solution used for immersion as in the prior art. Also, the amount of processing solution electrostatically sprayed in each of the electroless plating step S7 and the electroless plating device 60 can be reduced compared to the amount of processing solution used for immersion as in the prior art. In addition, such a reduction in the amount of processing solution used can reduce manufacturing costs, reduce environmental load, and improve the manufacturing efficiency of the electroless plated fiber material A4. In the plating process using a conventional plating bath, the concentration of the substance in the plating bath changes over time, making it difficult to control the concentration of the plating bath. In the present invention, the processing solution is electrostatically sprayed, so that the problem of controlling the concentration of the plating bath can also be solved.
[0114] "Second embodiment" A description will be given of an electroless plated fiber material and a manufacturing method and system thereof according to a second embodiment. The fiber material A1 used in this embodiment is similar to the fiber material A1 used in the first embodiment.
[0115] "Outline of electroless plated fiber material and its manufacturing method" An outline of the electroless plated fiber material A4 and its manufacturing method according to this embodiment will be described with reference to Figures 1 and 7. The manufacturing method of the electroless plated fiber material A4 according to this embodiment generally includes a catalyzing step S5 and an electroless plating step S7 similar to the first embodiment.
[0116] Furthermore, in the manufacturing method of electrolessly plated fiber material A4 according to this embodiment, fiber material A2, catalyst-applied fiber material A3, and electrolessly plated fiber material A4 are integrated so as to extend from the position where catalyzing step S5 is performed toward the position where electroless plating step S7 is performed. The integrated fiber materials A2-A4 are transported from the position where catalyzing step S5 is performed toward the position where electroless plating step S7 is performed. Electrolessly plated fiber material A4 according to this embodiment can be generally manufactured by such a manufacturing method.
[0117] "Details of electroless plated fiber material and its manufacturing method" 1 and 7, the electroless plated fiber material A4 according to this embodiment and the manufacturing method thereof will be described in detail. The manufacturing method of the electroless plated fiber material A4 according to this embodiment also includes, in detail, the degreasing step S1, pre-drying step S2, pre-treatment step S3, pre-cleaning step S4, catalyzing step S5, intermediate cleaning step S6, electroless plating step S7, post-cleaning step S8, and post-drying step S9, which are similar to those of the first embodiment. Note that, if the degreasing liquid F is volatile, the pre-drying step S2 can be omitted.
[0118] Furthermore, in the manufacturing method of electrolessly plated fibrous material A4 according to this embodiment, fibrous material A1, pretreated fibrous material A2, catalyst-applied fibrous material A3, and electrolessly plated fibrous material A4 are integrated so as to extend from the position where the degreasing step S1 is performed toward the position where the post-drying step S9 is performed. The integrated fibrous materials A1-A4 are transported from the position where the degreasing step S1 is performed toward the position where the post-drying step S9 is performed. In detail, electrolessly plated fibrous material A4 according to this embodiment can be manufactured by such a manufacturing method.
[0119] "Manufacturing system for electroless plated fiber materials" A manufacturing system for electrolessly plated fiber material A4 according to this embodiment will be described with reference to Fig. 7. The manufacturing system generally includes a catalyzing device 150, an electroless plating device 170, and a transport device 200. The catalyzing device 150 is configured to be capable of carrying out a catalyzing step S5. The electroless plating device 170 is configured to be capable of carrying out an electroless plating step S7. The transport device 200 is configured to be capable of transporting fiber materials A1 to A4.
[0120] The manufacturing system may also include, in detail, a degreasing device 110, a pre-drying device 120, a pre-treatment device 130, a pre-cleaning device 140, the catalysis device 150, an intermediate cleaning device 160, the electroless plating device 170, a post-cleaning device 180, a post-drying device 190, and the conveying device 200. The degreasing device 110 is configured to be able to perform the degreasing step S1. The pre-drying device 120 is configured to be able to perform the pre-drying step S2. The pre-treatment device 130 is configured to be able to perform the pre-treatment step S3. The pre-cleaning device 140 is configured to be able to perform the pre-cleaning step S4. The intermediate cleaning device 160 is configured to be able to perform the intermediate cleaning step S6. The post-cleaning device 180 is configured to be able to perform the post-cleaning step S8. The post-drying device 190 is configured to be able to perform the post-drying step S9. The conveying device 200 conveys the fiber materials A1 to A4 so that they pass through the degreasing device 110, the pre-drying device 120, the pre-treatment device 130, the pre-cleaning device 140, the catalysis device 150, the intermediate cleaning device 160, the electroless plating device 170, the post-cleaning device 180, and the post-drying device 190 in that order.
[0121] "Details of the degreasing equipment" 7, the degreasing device 110 can be configured as follows. In the above-described manufacturing system, the degreasing device 110 has a tank 111 configured to be able to store a degreasing liquid F. The degreasing device 110 has a degreasing roll 112 disposed in the degreasing liquid F stored in the tank 111. The fibrous material A1 passes through the tank 111 while being guided by the degreasing roll 112 so as to be immersed in the degreasing liquid F.
[0122] "Details of pre-drying device" 7, the pre-drying device 120 can be configured as follows. The pre-drying device 120 is configured to apply warm or hot air to the fiber material A1 after it has passed through the degreasing device 110. The fiber material A1 is dried when it passes through the pre-drying device 120. Note that if the degreasing liquid F is volatile, the pre-drying device 120 can be omitted.
[0123] "Details of pretreatment device" 7, the pre-treatment device 130 can be configured as follows. The pre-treatment device 130 has a tank 131 configured to store the treatment liquid G. The pre-treatment device 130 has a plurality of pre-treatment rolls 132 arranged in the treatment liquid G stored in the tank 131. The fibrous material A1 after passing through the pre-drying device 120 passes through the tank 131 while being guided by the plurality of pre-treatment rolls 132 so as to move around in the treatment liquid G to be immersed in the treatment liquid G. In the pre-treatment device 130, a pre-treated fibrous material A2 is obtained, which is a state in which the fibrous material A1 has been pre-treated.
[0124] "Details of pre-cleaning device" 7, the pre-cleaning device 140 can be configured as follows. The pre-cleaning device 140 has a tank 141 configured to store a cleaning liquid H. The pre-cleaning device 140 has a pre-cleaning roll 142 disposed in the cleaning liquid H stored in the tank 141. The pretreated fiber material A2 after passing through the pre-treatment device 130 passes through the tank 141 while being guided by the pre-cleaning roll 142 so as to be washed with the cleaning liquid H. In the pre-cleaning device 140, the fiber material A2 is grounded by the cleaning liquid H in the tank 141, and as a result, the fiber material A2 located in the subsequent catalysis device 150 is also grounded.
[0125] Furthermore, in the pre-cleaning device 140, moisture is imparted to the fiber material A2 by the cleaning liquid H in the tank 141, and as a result, moisture is also imparted to the fiber material A2 located in the subsequent catalyzed device 150. Such cleaning liquid H can be the same as the water I used in the subsequent catalyzed device 150.
[0126] "Details of the catalysis device" 7, the catalyst device 150 can be configured as follows. The catalyst device 150 has a catalyst nozzle 151a configured similarly to the catalyst nozzle 51a of the first embodiment. The catalyst nozzle 151a has a spray nozzle 151b similar to the spray nozzle 51b of the catalyst nozzle 51a of the first embodiment.
[0127] The catalyst nozzle mechanism 150 includes a catalyst nozzle mechanism 151 having a plurality of catalyst nozzles 151a. The catalyst nozzle mechanism 151 has a plurality of catalyst supply pipes 151c configured to feed the catalyst solution B to each of the plurality of catalyst nozzles 151a. However, the catalyst nozzle mechanism may also be configured to have one catalyst nozzle and one catalyst supply pipe that feeds the catalyst solution thereto.
[0128] The catalysis device 150 also has a first reducing agent nozzle 152a configured similarly to the first reducing agent nozzle 52a of the first embodiment. The first reducing agent nozzle 152a has a spray port 152b similar to the spray port 52b of the first reducing agent nozzle 52a of the first embodiment.
[0129] The catalysis device 150 includes a first reducing agent nozzle mechanism 152 having a plurality of first reducing agent nozzles 152a. The first reducing agent nozzle mechanism 152 has a plurality of first reducing agent supply pipes 152c configured to feed the first reducing agent solution C to the plurality of first reducing agent nozzles 152a, respectively. However, the first reducing agent nozzle mechanism may also be configured to have one first reducing agent nozzle and one first reducing agent supply pipe that feeds the first reducing agent solution thereto.
[0130] The multiple catalyst nozzles 151a and the multiple first reducing agent nozzles 152a are aligned in the transport direction of the fibrous material A2 passing through the catalysis device 150. The catalyst nozzle mechanism 151 and the first reducing agent nozzle mechanism 152 are aligned in the transport direction of the fibrous material A2 passing through the catalysis device 150. The catalyst nozzle mechanism 151 is preferably located upstream of the first reducing agent nozzle mechanism 152 in the transport direction of the fibrous material A1. The catalyst nozzle mechanism 151 and the first reducing agent nozzle mechanism 152 can also be fixed.
[0131] However, the positions of the catalyst nozzle mechanism and the first reducing agent nozzle mechanism are not limited thereto. The catalyst nozzle mechanism may be located downstream of the first reducing agent nozzle mechanism in the conveying direction of the fiber material. One or both of the catalyst nozzle mechanism and the first reducing agent nozzle mechanism may be movable.
[0132] After passing through the pre-cleaning device 140, the pretreated fiber material A2 is electrostatically sprayed with the catalyst solution B by the catalyst nozzle mechanism 151, and is electrostatically sprayed with the first reducing agent solution C by the first reducing agent nozzle mechanism 152. At this time, the fiber material A2 passing through the catalyzation device 150 is grounded by the above-mentioned pre-cleaning device 140 and the intermediate cleaning device 160 described below. Furthermore, moisture is imparted to this fiber material A2 by the above-mentioned pre-cleaning device 140. In the catalyzation device 150, a catalyst-imparted fiber material A3 in which a catalyst has been imparted to the fiber material A2 is obtained.
[0133] "Details of the intermediate cleaning device" 7, the intermediate cleaning device 160 can be configured as follows. The intermediate cleaning device 160 has a tank 161 configured to store a cleaning liquid H. The intermediate cleaning device 160 has an intermediate cleaning roll 162 disposed in the cleaning liquid H stored in the tank 161. The catalyst-imparted fiber material A3 after passing through the catalyzing device 150 passes through the tank 161 while being guided by the intermediate cleaning roll 162 so as to be washed with the cleaning liquid H. In the intermediate cleaning device 160, the fiber material A3 is grounded by the cleaning liquid H in the tank 161, and as a result, the fiber material A2 located in the preceding catalyzing device 150 and the fiber material A3 located in the subsequent electroless plating device 170 are also grounded.
[0134] Furthermore, in the intermediate cleaning device 160, moisture is imparted to the fibrous material A3 by the cleaning liquid H in the tank 161, and as a result, moisture is also imparted to the fibrous material A3 located in the subsequent electroless plating device 170. Such cleaning liquid H can be the same as the water J used in the subsequent electroless plating device 170.
[0135] "Details of electroless plating equipment" 7, the electroless plating apparatus 170 can be configured as follows. The electroless plating apparatus 170 has a metal ion nozzle 171a configured similarly to the metal ion nozzle 61a of the first embodiment. The metal ion nozzle 171a has a spray port 171b similar to the spray port 61b of the metal ion nozzle 61a of the first embodiment.
[0136] The electroless plating apparatus 170 includes a metal ion nozzle mechanism 171 having a plurality of metal ion nozzles 171a. The metal ion nozzle mechanism 171 has a plurality of metal ion supply pipes 171c configured to supply a metal ion solution D to each of the plurality of metal ion nozzles 171a. However, the metal ion nozzle mechanism can also be configured to have one metal ion nozzle and one metal ion supply pipe that supplies the metal ion solution to the nozzle.
[0137] The electroless plating apparatus 170 has a second reducing agent nozzle 172a configured similarly to the second reducing agent nozzle 62a of the first embodiment. The second reducing agent nozzle 172a has a spray port 172b similar to the spray port 62b of the second reducing agent nozzle 62a of the first embodiment.
[0138] The electroless plating apparatus 170 includes a second reducing agent nozzle mechanism 172 having a plurality of second reducing agent nozzles 172a. The second reducing agent nozzle mechanism 172 has a plurality of second reducing agent supply pipes 172c configured to supply the second reducing agent solution E to the plurality of second reducing agent nozzles 172a, respectively. However, the second reducing agent nozzle mechanism may also be configured to have one second reducing agent nozzle and one second reducing agent supply pipe that supplies the second reducing agent solution thereto.
[0139] Regarding the relationship between the metal ion nozzle mechanism 171 and the second reducing agent nozzle mechanism 172, the metal ion nozzle 171a and the second reducing agent nozzle 172a are fixed. In Fig. 7, the metal ion nozzle 171a and the second reducing agent nozzle 172a are arranged to be shifted from each other in the circumferential direction of the fiber material A3. Furthermore, the metal ion nozzle 171a and the second reducing agent nozzle 172a can be arranged to maintain a state in which they face each other while facing their discharge ports 171b, 172b toward the fiber material A3.
[0140] After passing through the intermediate cleaning device 160, the catalyst-imparted fiber material A3 is electrostatically sprayed with a metal ion solution C by the metal ion nozzle mechanism 171, and with a second reducing agent solution E by the second reducing agent nozzle mechanism 172. At this time, the fiber material A3 passing through the electroless plating device 170 is grounded by the intermediate cleaning device 160 and the post-cleaning device 180 described below. Furthermore, moisture is imparted to this fiber material A2 by the intermediate cleaning device 160. In the electroless plating device 170, electroless plated fiber material A4 is obtained, which is in a state where a plating film is formed on the fiber material A3.
[0141] "Details of the post-cleaning device" 7, the post-cleaning device 180 can be configured as follows. The post-cleaning device 180 has a tank 181 configured to store cleaning liquid H. The post-cleaning device 180 has a post-cleaning roll 182 disposed in the cleaning liquid H stored in the tank 181. The electroless plated fiber material A4 after passing through the electroless plating device 170 passes through the tank 181 while being guided by the post-cleaning roll 182 so as to be cleaned by the cleaning liquid H. In the post-cleaning device 180, the fiber material A4 is grounded by the cleaning liquid H in the tank 181, and as a result, the fiber material A3 located in the preceding electroless plating device 170 is grounded.
[0142] "Details of post-drying device" 7, the post-drying device 190 can be configured as follows. The post-drying device 190 is configured to apply warm or hot air to the fiber material A4 after passing through the post-cleaning device 180. The fiber material A4 is dried when passing through the post-drying device 190.
[0143] The post-drying device 190 may be configured to also perform an annealing process. For example, the post-drying device 190 may have a heating mechanism configured to heat the fiber material A4. The heating mechanism may be a hot air circulating oven. In this case, such a device may be called a drying and annealing device. However, an annealing device may be provided separately from the post-drying device.
[0144] "Details of the transport device" 7, the conveying device 200 can be configured as follows. The conveying device 200 has an unwinding roll 201 configured to unwind the fibrous material A1. The conveying device 200 has a take-up roll 202 configured to take up the electrolessly plated fibrous material A4. Between the unwinding roll 201 and the take-up roll 202, the fibrous material A1, the pretreated fibrous material A2, the catalyst-applied fibrous material A3, and the electrolessly plated fibrous material A4 extend integrally.
[0145] The fibrous material A1 unwound from the unwinding roll 201 passes from the degreasing device 110 to the pretreatment device 130, and then changes into the pretreated fibrous material A2. After passing through the pretreatment device 130, the pretreated fibrous material A2 passes from the pre-cleaning device 140 to the catalyzing device 150, and then changes into the catalyzed fibrous material A3. After passing through the catalyzing device 150, the catalyzed fibrous material A3 passes from the intermediate cleaning device 160 to the electroless plating device 170, and then changes into the electroless plated fibrous material A4. After passing through the electroless plating device 170, the electroless plated fibrous material A4 passes from the post-cleaning device 180 to the post-drying device 190, and then is taken up by the take-up roll 202.
[0146] As described above, the manufacturing method and manufacturing system for electroless plated fiber material A4 according to this embodiment can obtain the same effects as those of the manufacturing method and manufacturing system for electroless plated fiber material A4 according to embodiment 1. In addition to these effects, the manufacturing method and manufacturing system according to this embodiment can obtain the following effects.
[0147] In the manufacturing method of electrolessly plated fiber material A4 in this embodiment, the fiber material A2, the catalyst-added fiber material A3, and the electrolessly plated fiber material A4 are transported from the position where the catalysis process S5 is performed to the position where the electroless plating process S7 is performed in an integrated state extending from the position where the catalysis process S5 is performed toward the position where the electroless plating process S7 is performed.
[0148] The manufacturing system for electrolessly plated fiber material A4 in this embodiment includes a conveying device 200 that is configured to convey the fiber material A2, the catalyst-added fiber material A3, and the electrolessly plated fiber material A4 from the catalysis device 150 to the electroless plating device 170 in a state in which the fiber material A2, the catalyst-added fiber material A3, and the electroless plated fiber material A4 are integrated so as to extend from the catalysis device 150 toward the electroless plating device 170.
[0149] In such a manufacturing method and manufacturing system, the fiber materials A2 to A4 can be efficiently transported, thereby improving the manufacturing efficiency.
[0150] Furthermore, the fibrous material A1, the pretreated fibrous material A2, the catalyst-applied fibrous material A3, and the electrolessly plated fibrous material A4 are integrated so as to extend from the position where the degreasing step S1 is performed toward the position where the post-drying step S9 is performed. When the fibrous materials A1 to A4 thus integrated are transported from the position where the degreasing step S1 is performed toward the position where the post-drying step S9 is performed, the fibrous materials A1 to A4 can be transported efficiently. This can improve the manufacturing efficiency.
[0151] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and the present invention can be modified and changed based on the technical concept thereof. EXAMPLES
[0152] Examples and Comparative Examples will be described. In the Examples, as shown in Figures 2 to 6, electroless plated fiber material A4 was produced from fiber material A1 made of 6,6-nylon. In the Comparative Examples, electroless plated fiber material was also produced from fiber material made of 6,6-nylon. The thickness of fiber material A1 in Example 1 and the fiber material in the Comparative Examples were both 70 denier.
[0153] "Example" First, examples will be described. In Example 1, electroless plated fiber material A4 was manufactured using the manufacturing method according to the first embodiment. Specifically, in the degreasing step S1, the fiber material A1 was immersed in a degreasing liquid F, thereby degreasing the fiber material A1. An acetone solution F was used as the degreasing liquid F. The atmospheric temperature in the degreasing step S1 was room temperature. The immersion time for immersing the fiber material A1 in the acetone solution F was 1 minute. In the pre-drying step S2, hot air was applied to the fiber material A1 degreased in the degreasing step S1, thereby drying the fiber material A1.
[0154] As shown in FIG. 5, in the pretreatment step S3, the fiber material A1 dried in the pre-drying step S2 was immersed in a treatment liquid G, thereby performing a pretreatment to give a negative charge to the fiber material A1 in order to improve the adhesion between the fiber material A2 and the plating coating after this treatment. A tannic acid solution G containing tannic acid was used as the treatment liquid G, and a tannic acid treatment step S3 was performed as the pretreatment step S3. The concentration of tannic acid in the tannic acid solution G was 5% by weight. The temperature of the tannic acid solution G was 50° C. The immersion time for which the fiber material A1 was immersed in the tannic acid solution G was 5 minutes.
[0155] 6, after the pretreatment step S3, in the pre-cleaning step S4, the pretreated fiber material A2 was washed with a cleaning liquid H. As the cleaning liquid H, purified water was used.
[0156] As shown in Fig. 2, in the catalysis step S5, the fiber material A2 washed in the pre-cleaning step S4 was grounded, and while the fiber material A2 was being moistened, the catalyst solution B, which was positively charged, was electrostatically sprayed onto the fiber material A2. In the electrostatic spraying of the catalyst solution B, the catalyst solution B was prepared by dissolving palladium acetate in the solvent acetonitrile. The concentration of palladium acetate in the catalyst solution B was 0.1 mol / L.
[0157] The amount of catalyst solution B sprayed from catalyst nozzle 51a per unit time was 0.03 mL / min, and catalyst solution B was sprayed onto 30 cm of fiber material A2 for 5 minutes at this spray amount. The potential on the catalyst nozzle 51a side was +5 kV. The distance between spray port 51b of catalyst nozzle 51a and fiber material A2 was 1 cm. Purified water was supplied to fiber material A2 to provide moisture to fiber material A2.
[0158] Furthermore, after electrostatic spraying of the catalyst solution B, the fiber material A2 was grounded, and while moisture was being added to the fiber material A2, the first reducing agent solution C, positively charged, was electrostatically sprayed onto the fiber material A2. In electrostatic spraying of the first reducing agent solution C, hydrazine was used as the catalyst contained in the first reducing agent solution C. The concentration of hydrazine in the first reducing agent solution C was 1.0 mol / L. As the solvent for the first reducing agent solution C, a solution consisting of 50% ethanol and 50% water was used.
[0159] The amount of the first reducing agent solution C sprayed from the first reducing agent nozzle 52a per unit time was 0.03 mL / min, and the first reducing agent solution C was sprayed onto 30 cm of the fiber material A2 for 5 minutes at this amount. The potential on the side of the first reducing agent nozzle 52a was +5 kV. The distance between the spray port 52b of the first reducing agent nozzle 52a and the fiber material A2 was 1 cm. Purified water was supplied to the fiber material A2 to provide moisture to the fiber material A2.
[0160] 6, after the catalyzation step S5, in the intermediate washing step S6, the catalyst-imparted fiber material A3 was washed with a washing liquid H. As the washing liquid H, purified water was used.
[0161] As shown in Fig. 3, in the electroless plating process S7, the catalyst-added fiber material A3 washed in the intermediate washing process S6 was grounded, and while moisture was being added to the fiber material A3, the metal ion solution D and the second reducing agent solution E, each positively charged, were electrostatically sprayed onto the fiber material A3 so that they reacted in the same electric field at the fiber material A3. The metal ion solution D was prepared by dissolving silver nitrate in a mixed solvent consisting of ethanol and water. The concentration of silver nitrate in the metal ion solution D was 0.3 mol / L.
[0162] The amount of the metal ion solution D sprayed from the metal ion nozzle 61a per unit time was 0.03 mL / min, and the metal ion solution D was sprayed onto 30 cm of the fiber material A3 for 15 minutes at this amount. The potential on the metal ion nozzle 61a side was +5 kV. The distance between the spray port 61b of the metal ion nozzle 61a and the fiber material A3 was 1 cm.
[0163] Hydrazine was used as the reducing agent contained in the second reducing agent solution E. The concentration of hydrazine in the second reducing agent solution E was 0.5 mol / L. As a solvent for the second reducing agent solution E, a mixed solution of ethanol and water was used.
[0164] The amount of the second reducing agent solution E sprayed from the second reducing agent nozzle 62a per unit time was 0.03 mL / min, and the second reducing agent solution E was sprayed onto 30 cm of the fiber material A3 for 15 minutes at this amount. The potential on the side of the second reducing agent nozzle 62a was +5 kV. The distance between the spray port 62b of the second reducing agent nozzle 62a and the fiber material A3 was 1 cm.
[0165] 6, after the electroless plating step S7, in the post-cleaning step S8, the electroless plated fiber material A4 was washed with a cleaning liquid H. As the cleaning liquid H, purified water was used.
[0166] In the post-drying step S9, hot air was applied to the fiber material A4 cleaned in the post-cleaning step S8, thereby drying the fiber material A4. Thereafter, the electrical resistance of a plurality of electrolessly plated fiber materials A4 was measured.
[0167] "Comparative Example" Next, a comparative example will be described. In the comparative example, first, the degreasing process, pre-drying process, pre-treatment process, pre-cleaning process, catalyzation process, and intermediate cleaning process were performed in the same manner as in the example. Then, the catalyst-added fiber material washed in the intermediate cleaning process was immersed in a second reducing agent solution. A metal ion solution was electrostatically sprayed in a positively charged state using an electrospray onto the catalyst-added fiber material immersed in the second reducing agent solution, thereby obtaining an electroless plated fiber material. Furthermore, this electroless plated fiber material was subjected to a post-cleaning process and a post-drying process in the same manner as in the example. Then, the electrical resistance of a plurality of electroless plated fiber materials was measured.
[0168] "Comparison between Examples and Comparative Examples" The electrical conductivity of the electroless plated fiber materials obtained in the comparative examples was significantly inferior to that of the electroless plated fiber materials A4 obtained in the examples. That is, the electroless plated fiber materials A4 obtained in the examples showed sufficient electrical conductivity. On the other hand, in the comparative examples, even if the time for electrostatically spraying the metal ion solution in a positively charged state using electrospray was increased, the electroless plated fiber materials obtained in the comparative examples showed almost no electrical conductivity. Therefore, it was confirmed that the electroless plating step S7 in the examples, particularly in comparison with the comparative examples, gave electroless plated fiber materials A4 with sufficient electrical conductivity.
[0169] Furthermore, the electrical resistance of the electroless plated fiber materials A4 obtained in the examples was 1.0 Ω / cm to 1.5 Ω / cm. In contrast, the electrical resistance of commercially available electroless plated fiber materials was about 2.0 Ω / cm. Therefore, it was confirmed that the electroless plated fiber materials A4 obtained in the examples have conductive performance equal to or greater than that of commercially available electroless plated fiber materials. [Explanation of symbols]
[0170] A2…Pretreated fiber material (fiber material) A3: Catalyzed fiber material (fiber material) A4...Electroless plating fiber material (fiber material) B...Catalyst solution C…First reducing agent solution D: Metal ion solution E…Second reducing agent solution S5…catalyzation step S7: Electroless plating process 50,150...Catalyzer 51a, 151a...Catalyst nozzle 52a, 152a...First reducing agent nozzle 60,170...Electroless plating equipment 61a, 171a...Nozzle for metal ions 62a, 172a...Second reducing agent nozzle 200...Transportation device
Claims
1. a catalyzing step of electrostatically spraying a catalyst solution containing a catalyst precursor, while the catalyst solution is charged to a positive or negative potential, onto a fibrous material that is grounded or charged to a potential opposite to that of the catalyst solution and that has been given moisture, and electrostatically spraying a first reducing agent solution containing a reducing agent for the catalyst precursor, while the first reducing agent solution is charged to a positive or negative potential, onto the fibrous material that is grounded or charged to a potential opposite to that of the first reducing agent solution and that has been given moisture, thereby obtaining a catalyst-applied fibrous material in which a catalyst has been applied to the fibrous material; an electroless plating process in which a metal ion solution containing metal ions and a second reducing agent solution containing a reducing agent for the metal ions are electrostatically sprayed onto the catalyst-applied fiber material, which is grounded or charged to a potential opposite to that of the metal ion solution and the second reducing agent solution and is moistened, with the metal ion solution and the second reducing agent solution both charged to a positive potential or the metal ion solution and the second reducing agent solution both charged to a negative potential, thereby obtaining an electroless plated fiber material in which a plating film is formed on the catalyst-applied fiber material; Including, In the electroless plating step, the metal ion solution and the second reducing agent solution are electrostatically sprayed onto the catalyst-applied fiber material while maintaining the metal ion solution and the second reducing agent solution facing each other. A method for producing electroless plated fiber materials.
2. A method for producing electrolessly plated fiber material as described in claim 1, wherein the fiber material, the catalyst-applied fiber material, and the electrolessly plated fiber material are transported from the position where the catalyzation process is performed to the position where the electroless plating process is performed in a unified state extending from the position where the catalyzation process is performed to the position where the electroless plating process is performed.
3. a catalyst-imparting device configured to obtain a catalyzed fiber material in which a catalyst is imparted to the fiber material; an electroless plating apparatus configured to obtain an electroless plated fiber material in which a plating film is formed on the catalyst-applied fiber material; Equipped with the catalyzing device has a catalyst nozzle configured to electrostatically spray a catalyst solution containing a catalyst precursor, the catalyst solution being charged to a positive or negative potential, onto the fibrous material that is grounded or charged to a potential opposite to that of the catalyst solution and that has been given moisture, and a first reducing agent nozzle configured to electrostatically spray a first reducing agent solution containing a reducing agent for the catalyst precursor, the first reducing agent solution being charged to a positive or negative potential, onto the fibrous material that has been given moisture, the first reducing agent nozzle being grounded or charged to a potential opposite to that of the first reducing agent solution, The electroless plating apparatus has a metal ion nozzle configured to electrostatically spray a metal ion solution containing metal ions onto the catalyst-applied fiber material in a state where the metal ion solution is charged to a positive potential or a negative potential, and a second reducing agent nozzle configured to electrostatically spray a second reducing agent solution containing a reducing agent for the metal ions onto the catalyst-applied fiber material in a state where the second reducing agent solution is charged to a positive potential when the metal ion solution is at a positive potential, or to a negative potential when the metal ion solution is at a negative potential, An electroless plated fiber material manufacturing system, wherein the electroless plating apparatus is configured to maintain the outlet of the metal ion nozzle and the outlet of the second reducing agent nozzle facing each other while pointing them toward the catalyst-applied fiber material.
4. A manufacturing system for electroless plated fiber material as described in claim 3, comprising a conveying device configured to convey the fiber material, the catalyst-applied fiber material, and the electroless plated fiber material from the catalysis device to the electroless plating device in a state where they are integrated so as to extend from the catalysis device toward the electroless plating device.
Citation Information
Patent Citations
Apparatus for electrostatically coating wire body
JP1984039361A
Production of electroless-plated fiber
JP1995173636A
Pretreatment method for electroless plating and conductive material formed by using the same
JP2003105552A
Manufacturing method of fiber conductor and fiber conductor obtained thereby
JP2011236512A
Plated fiber and production method thereof
JP2015214735A