Asphalt modifier and asphalt composition

Incorporating a polyolefin copolymer with epoxy groups and a carboxyl group-containing additive into asphalt maintains anti-peeling performance, addressing the durability issue of polyolefin resin modifiers under high-temperature storage.

JP7588544B2Active Publication Date: 2024-11-22SUMITOMO CHEM CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2021067751
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-13
Publication Date
2024-11-22
Estimated Expiration
2041-04-13

AI Technical Summary

Technical Problem

Polyolefin resin-based asphalt modifiers lose anti-exfoliation performance for aggregates when stored at high temperatures for extended periods, leading to reduced road durability.

Method used

Incorporating a polyolefin copolymer with epoxy groups and an additive containing an organic compound with a carboxyl group or its metal salt into the asphalt composition to maintain anti-peeling performance.

Benefits of technology

The modified asphalt composition retains anti-peeling performance against aggregates even after long-term high-temperature storage, enhancing road pavement durability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588544000001
    Figure 0007588544000001
  • Figure 0007588544000002
    Figure 0007588544000002
  • Figure 0007588544000003
    Figure 0007588544000003
Patent Text Reader

Abstract

To provide an asphalt modifier and an asphalt composition capable of maintaining a separation preventive performance to an aggregate even after a long-term storage at high temperature.SOLUTION: Disclosed is an asphalt modifier being a fused and kneaded material of a mixture including a polyolefin copolymer having an epoxy group and an additive containing at least one of an organic compound having a carboxyl group and a metal salt thereof. Also disclosed is an asphalt composition including asphalt, a polyolefin copolymer having an epoxy group and an additive containing at least one of an organic compound having a carboxyl group and a metal salt thereof.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an asphalt modifier and an asphalt composition. [Background technology]

[0002] In order to improve the heat resistance of asphalt and inhibit peeling, asphalt is sometimes modified with a modifier containing a polyolefin resin (for example, Patent Document 1). In the case of asphalt compositions used for road paving, inhibiting asphalt peeling is important in reducing damage to roads caused by peeling. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2004-35839 A Summary of the Invention [Problem to be solved by the invention]

[0004] By the way, after being mixed with asphalt, the modifier containing the polyolefin resin may be stored at high temperatures for a long period of time, for example, at 175° C. for about one week. However, long-term storage at high temperatures may cause a decrease in the anti-stripping performance for aggregates (for example, hard sandstone or limestone).

[0005] Therefore, one aspect of the present invention provides an asphalt modifier and an asphalt composition that can maintain anti-stripping performance for aggregate even after long-term storage at high temperatures. [Means for solving the problem]

[0006] One aspect of the present invention is an asphalt modifier, which is a melt-kneaded mixture containing a polyolefin copolymer having an epoxy group and an additive containing at least one of an organic compound having a carboxyl group or a metal salt thereof.

[0007] Another aspect of the present invention is an asphalt composition containing asphalt, a polyolefin copolymer having an epoxy group, and an additive including at least one of an organic compound having a carboxyl group or a metal salt thereof. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to provide an asphalt modifier and an asphalt composition that can maintain anti-stripping performance for aggregate even after long-term storage at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, embodiments of the present invention will be described in detail, however, the present invention is not limited to the following embodiments.

[0010] One embodiment of the present invention is an asphalt modifier that is a melt-kneaded mixture containing a polyolefin copolymer having an epoxy group and an additive containing at least one of an organic compound having a carboxyl group or a metal salt thereof.

[0011] The polyolefin copolymer having an epoxy group (hereinafter also referred to as "polyolefin copolymer A") may contain, for example, a monomer unit having an epoxy group and a monomer unit derived from ethylene and / or an α-olefin. The ratio of the monomer unit derived from ethylene and / or an α-olefin (the total ratio of the monomer unit derived from ethylene and the monomer unit derived from an α-olefin) may be 50 to 99.9 mass% based on the total mass of the polyolefin copolymer A. The ratio of the monomer unit having an epoxy group may be 0.1 mass% or more, 0.5 mass% or more, or 1 mass% or more, and may be 50 mass% or less, 30 mass% or less, or 20 mass% or less, based on the mass of the polyolefin copolymer A. The polyolefin copolymer A may be a random copolymer or a block copolymer.

[0012] The monomer unit having an epoxy group may be, for example, a monomer unit derived from an unsaturated carboxylic acid glycidyl ester, or a monomer unit derived from a glycidyl ether having an unsaturated group.

[0013] The unsaturated carboxylic acid glycidyl ester may be a compound represented by the following formula (1): 1 represents an alkenyl group having 2 to 18 carbon atoms, and the alkenyl group may have one or more substituents. Examples of the compound represented by formula (1) include glycidyl acrylate, glycidyl methacrylate, and glycidyl itaconic acid ester.

[0014] [ka]

[0015] The glycidyl ether having an unsaturated group may be a compound represented by the following formula (2): 2 represents an alkenyl group having 2 to 18 carbon atoms, and the alkenyl group may have one or more substituents. X represents CH 2 -O(CH 2 R 2 ) or an oxygen atom. Examples of compounds represented by formula (2) include allyl glycidyl ether, 2-methylallyl glycidyl ether, and styrene-p-glycidyl ether.

[0016] [ka]

[0017] The polyolefin copolymer A may be a copolymer further containing other monomer units derived from an ethylenically unsaturated compound in addition to the monomer units having an epoxy group and the monomer units derived from ethylene and / or α-olefin. The proportion of the other monomer units may be 0 to 50% by mass, or 10 to 40% by mass, based on the total mass of the polyolefin copolymer A.

[0018] Examples of ethylenically unsaturated compounds from which other monomer units are derived include α,β-unsaturated carboxylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate; carboxylic acid vinyl esters such as vinyl acetate, vinyl propionate, and vinyl butanoate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, propyl vinyl ether, and phenyl vinyl ether; and styrene derivatives such as styrene, methylstyrene, and ethylstyrene. "(Meth)acrylate" means acrylate or methacrylate, and the same applies to similar compounds.

[0019] Examples of polyolefin copolymer A include ethylene-glycidyl (meth)acrylate copolymer, ethylene-glycidyl (meth)acrylate-methyl (meth)acrylate copolymer, ethylene-glycidyl (meth)acrylate-ethyl (meth)acrylate copolymer, ethylene-glycidyl (meth)acrylate-normal propyl (meth)acrylate copolymer, ethylene-glycidyl (meth)acrylate-isopropyl (meth)acrylate copolymer, ethylene-glycidyl (meth)acrylate-norbutyl (meth)acrylate copolymer, ethylene-glycidyl (meth)acrylate-isobutyl (meth)acrylate copolymer, and ethylene-glycidyl (meth)acrylate-vinyl acetate copolymer. The polyolefin copolymer having an epoxy group may be an ethylene-glycidyl (meth)acrylate copolymer.

[0020] The melt flow rate of the polyolefin copolymer A may be 300g / 10min or less. When the melt flow rate is 300g / 10min or less, the molecular weight of the polyolefin copolymer A is relatively large, so that the heat resistance of the asphalt modifier tends to be excellent. From the same viewpoint, the melt flow rate of the polyolefin copolymer A may be 200g / 10min or less, 100g / 10min or less, or 50g / 10min or less. The melt flow rate of the polyolefin copolymer A may be 1g / 10min or more, or 5g / 10min or more, from the viewpoint of excellent dispersion efficiency by having the same viscosity as asphalt when mixed with asphalt. The melt flow rate of polyolefin copolymer A is a value measured by Method A (a method for calculating the extrusion rate in grams per 10 minutes (g / 10 min) from the weight of the extrudate produced in a specified time) under conditions of 190°C and a load of 2.16 kg based on JIS 7210-1:2014.

[0021] The content of polyolefin copolymer A may be 70 mass% or more, 80 mass% or more, 85 mass% or more, or 90 mass% or more, based on the total mass of the mixture melt-kneaded to form the asphalt modifier, and may be 99.9 mass% or less, 99.5 mass% or less, 99 mass% or less, 95 mass% or less, or 90 mass% or less.

[0022] The asphalt modifier contains an additive containing at least one of an organic compound having a carboxyl group (hereinafter also referred to as "organic compound B") or a metal salt thereof. The organic compound B may contain at least one selected from the group consisting of saturated fatty acids, unsaturated fatty acids, and aromatic carboxylic acids. The metal salt may be a sodium salt, a potassium salt, a calcium salt, or the like of the organic compound B. The asphalt modifier may contain an additive containing one or more organic compounds B or metal salts thereof.

[0023] Examples of saturated fatty acids include formic acid, acetic acid, propionic acid, butanoic acid, pentanoic acid, hexanoic acid, heptanoic acid, caprylic acid, capric acid, lauric acid, myristic acid, palmitic acid, stearic acid, arachidic acid, and behenic acid. Organic compound B may contain at least one selected from the group consisting of caprylic acid, capric acid, myristic acid, stearic acid, and behenic acid, and may contain stearic acid from the viewpoint of easily maintaining anti-exfoliation performance against limestone.

[0024] Examples of unsaturated fatty acids include monounsaturated fatty acids such as crotonic acid, myristoleic acid, palmitoleic acid, sapienic acid, oleic acid, and elaidic acid; diunsaturated fatty acids such as linoleic acid, eicosadienoic acid, and docosadienoic acid; triunsaturated fatty acids such as linolenic acid (α-linolenic acid) and pinolenic acid; and tetraunsaturated fatty acids such as stearidonic acid and arachidonic acid. The number of unsaturated carbon bonds possessed by the unsaturated fatty acid may be 2 or less or 1. The organic compound B may contain oleic acid or linolenic acid.

[0025] Examples of aromatic carboxylic acids include benzoic acid, phthalic acid, isophthalic acid, terephthalic acid, and salicylic acid. Organic compound B may include benzoic acid.

[0026] The number of carboxyl groups that organic compound B has may be 3 or less, 2 or less, or 1 or less, from the viewpoint of preventing gelation when polyolefin copolymer A and organic compound B are mixed.

[0027] The number of carbon atoms in the organic compound B may be 6 or more, 8 or more, 10 or more, 14 or more, 16 or more, or 18 or more, and may be 22 or less, 20 or less, or 18 or less.

[0028] The content of the additive may be 0.1% by mass or more, 0.5% by mass or more, 1% by mass or more, 5% by mass or more, or 10% by mass or more, and 30% by mass or less, 20% by mass or less, 15% by mass or less, or 10% by mass or less, based on the total mass of the mixture to be melt-kneaded to form the asphalt modifier. The content of the organic compound B may be within the above range based on the total mass of the mixture to be melt-kneaded. The content of the metal salt of the organic compound B may be within the above range based on the total mass of the mixture to be melt-kneaded. In the process of melt-kneading, some or all of the additive may react and bond with the polyolefin copolymer A or convert to other compounds, but in this specification, the "content of the additive" means the amount of the additive introduced to form the mixture to be melt-kneaded.

[0029] The content of the additive may be 0.1 parts by mass or more, 0.4 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and 45 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, based on 100 parts by mass of the polyolefin copolymer A. The content of the organic compound B may be within the above range based on 100 parts by mass of the polyolefin copolymer A. The content of the metal salt of the organic compound B may be within the above range based on 100 parts by mass of the polyolefin copolymer A.

[0030] The asphalt modifier according to one embodiment may further contain components other than the polyolefin copolymer A and the additives. The asphalt modifier may further contain, for example, a styrene-butadiene-styrene block copolymer (hereinafter also referred to as "SBS copolymer"), a polyolefin copolymer other than the polyolefin copolymer A, and an organic compound other than the organic compound B.

[0031] The asphalt modifier can further improve heat resistance and peeling resistance by containing polyolefin copolymer A and SBS copolymer. The content of the SBS copolymer in the asphalt modifier may be, for example, 0.5 mass% or more, 1.0 mass% or more, or 2.0 mass% or more based on the total mass of the mixture melt-kneaded to form the asphalt modifier, and may be 10 mass% or less, 8 mass% or less, or 5 mass% or less. The content of the SBS copolymer in the asphalt modifier may be, for example, 0.5 mass parts or more, 10 mass parts or more, 100 mass parts or more, 600 mass parts or more, 1000 mass parts or more, or 1400 mass parts or more based on the total 100 mass parts of polyolefin copolymer A and additives in the mixture melt-kneaded to form the asphalt modifier, and may be 5000 mass parts or less, 4200 mass parts or less, 3800 mass parts or less, or 3400 mass parts or less.

[0032] The total content of polyolefin copolymer A and additives in the mixture melt-kneaded to form the asphalt modifier may be 90 mass% or more, 95 mass% or more, or 99 mass% or more based on the total mass of the melt-kneaded mixture, or may be substantially 100 mass% (an embodiment in which the melt-kneaded mixture consists of polyolefin copolymer A and additives).

[0033] The asphalt modifier can be obtained by kneading a mixture containing polyolefin copolymer A and additives with a mixer or the like while heating it. That is, the asphalt modifier can be produced by a method including a step of melt-kneading a mixture containing polyolefin copolymer A and additives. The heating temperature of the mixture when obtaining the asphalt modifier may be, for example, 100 to 250°C, or 150 to 200°C.

[0034] During the process of melt-kneading the mixture, at least a part of the organic compound B or its metal salt contained in the additive reacts with the polyolefin copolymer A or other components, and a structural change that increases the fluidity of the mixture is thought to occur in the melt-kneaded product (asphalt modifier). However, the details of such a reaction are not clear, and it is difficult and impractical to directly identify the melt-kneaded product (asphalt modifier) ​​itself by its structure or characteristics. In addition, a part of the organic compound B or its metal salt may remain unreacted in the melt-kneaded product (asphalt modifier). The polyolefin copolymer A in the asphalt modifier may be modified by reaction with the organic compound B or its metal salt.

[0035] The asphalt modifier according to one embodiment may be stored and used as a material set including a first agent containing the polyolefin copolymer A and a second agent containing an additive containing at least one of an organic compound B or a metal salt thereof. The first agent and the second agent of the material set are mixed, and the resulting mixture is melt-kneaded to obtain the asphalt modifier.

[0036] When the first and second agents of the material set are mixed to obtain a mixture, the amount of the second agent added may be, based on the total mass of the resulting mixture, 0.1 mass% or more, 0.5 mass% or more, 1 mass% or more, 5 mass% or more, or 10 mass% or more, and may be 30 mass% or less, 20 mass% or less, 15 mass% or less, or 10 mass% or less.

[0037] When the first and second agents of the material set are mixed to obtain a mixture, the amount of the second agent added per 100 parts by mass of the first agent may be 0.1 parts by mass or more, 0.4 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and may be 45 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less.

[0038] The asphalt modifier according to one embodiment can be mixed with asphalt to obtain an asphalt composition containing the asphalt modifier and asphalt. The asphalt composition may be a melt-kneaded mixture containing asphalt, polyolefin copolymer A, and an additive containing at least one of an organic compound B or a metal salt thereof. That is, another embodiment of the present invention is an asphalt composition that is a melt-kneaded mixture containing asphalt, a polyolefin copolymer having an epoxy group, and an additive containing at least one of an organic compound having a carboxyl group or a metal salt thereof.

[0039] The asphalt contained in the asphalt composition is not particularly limited, and may be, for example, natural asphalt such as straight asphalt for paving, lake asphalt, etc., semi-blown asphalt, straight asphalt modified with blown asphalt, tar-modified straight asphalt, or a combination thereof.

[0040] The asphalt content may be 90 mass% or more, 95 mass% or more, 99 mass% or more, 99.5 mass% or more, or 99.9 mass% or less, 99.8 mass% or less, or 99.7 mass% or less, based on the total mass of the mixture that is melt-blended to form the asphalt composition.

[0041] The content of polyolefin copolymer A may be 0.1 mass% or more, 0.2 mass% or more, or 0.25 mass% or more, and may be 4.99 mass% or less, 3 mass% or less, 1 mass% or less, 0.5 mass% or less, or 0.3 mass% or less, based on the total mass of the mixture melt-kneaded to form the asphalt composition.

[0042] The content of the additive may be 0.0005% by mass or more, 0.001% by mass or more, 0.003% by mass or more, 0.01% by mass or more, 0.02% by mass or more, or 0.03% by mass or more, based on the total mass of the mixture melt-kneaded to form the asphalt composition, and may be 1% by mass or less, 0.5% by mass or less, 0.1% by mass or less, 0.05% by mass or less, or 0.03% by mass or less. The content of the organic compound B may be within the above range, based on the total mass of the mixture melt-kneaded. The content of the metal salt of the organic compound B may be within the above range, based on the total mass of the mixture melt-kneaded.

[0043] The content of the additive may be 0.1 parts by mass or more, 0.4 parts by mass or more, 1 part by mass or more, 5 parts by mass or more, or 10 parts by mass or more, and 45 parts by mass or less, 30 parts by mass or less, 20 parts by mass or less, or 15 parts by mass or less, based on 100 parts by mass of the polyolefin copolymer A. The content of the organic compound B may be within the above range based on 100 parts by mass of the polyolefin copolymer A. The content of the metal salt of the organic compound B may be within the above range based on 100 parts by mass of the polyolefin copolymer A.

[0044] The total content of polyolefin copolymer A and the additives may be 0.1 mass% or more, 0.2 mass% or more, or 0.3 mass% or more, based on the total mass of the mixture melt-kneaded to form the asphalt composition, and may be 10 mass% or less, 5 mass% or less, 1 mass% or less, 0.5 mass% or less, or 0.3 mass% or less.

[0045] The asphalt composition can be obtained by melt-kneading a mixture containing asphalt and the asphalt modifier. The asphalt composition can also be obtained by melt-kneading a mixture containing asphalt, polyolefin copolymer A, and an additive containing at least one of organic compound B or a metal salt thereof. The temperature during melt-kneading may be, for example, 100 to 250°C or 150 to 200°C. The time for melt-kneading may be, for example, 0.01 to 6 hours.

[0046] The asphalt composition can be used, for example, by mixing with aggregate, and can be used as an asphalt composition for road paving containing the asphalt composition and aggregate. That is, another embodiment of the present invention is an asphalt composition for road paving containing the asphalt composition and aggregate.

[0047] The type and content of aggregate can be appropriately adjusted within the range generally adopted in the field of road paving. Examples of aggregate may be crushed stone, crushed sand, and crushed stone and crushed sand of sedimentary rock (e.g., hard sandstone, limestone). The content of aggregate may be, for example, 1000 to 10000 parts by mass per 100 parts by mass of the asphalt composition. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples, although the present invention is not limited to these examples.

[0049] 1. Raw materials (1) Asphalt Straight asphalt (hereinafter referred to as "StAs"): StAs, manufactured by ENEOS Corporation, penetration: 60-80° (2) Resin Resin A: Ethylene / glycidyl methacrylate copolymer (hereinafter referred to as "EGMA copolymer"). Sumitomo Chemical Co., Ltd., glycidyl methacrylate content 19% by mass, MFR 7g / 10min (190°C, 2.16kg load) Resin B: Ethylene / methacrylic acid copolymer (manufactured by DuPont-Mitsui Polychemicals Co., Ltd., N1525, methacrylic acid modification rate: 15% by weight, MFR 25g / 10min (190°C, 2.16kg load)) Resin C: Ethylene / methyl acrylate / octadecyl acrylate copolymer (3) Additives Stearic acid (Tokyo Chemical Industry Co., Ltd.) Stearyl alcohol (Tokyo Chemical Industry Co., Ltd.) Benzoic acid (Tokyo Chemical Industry Co., Ltd.) Oleic acid (Tokyo Chemical Industry Co., Ltd.) Capric acid (Tokyo Chemical Industry Co., Ltd.) Myristic acid (Tokyo Chemical Industry Co., Ltd.) Behenic acid (Tokyo Chemical Industry Co., Ltd.) α-Linolenic acid (Tokyo Chemical Industry Co., Ltd.) Stearyl alcohol (Tokyo Chemical Industry Co., Ltd.) Calcium stearate (manufactured by Sakai Chemical Industry Co., Ltd.) Polyphosphoric acid (Aldrich) Caprylic acid (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.)

[0050] 2. Preparation of Asphalt Modifier The resin and additives in the amounts shown in Table 1 were added to a Labo Plastomill manufactured by Toyo Seiki Co., Ltd. equipped with a small mixer with a capacity of 100 mL, and the mixture was melt-kneaded at 150°C, 80 rpm, and 5 minutes to obtain the asphalt modifiers of Examples 1 to 3.

[0051] 3. Preparation of asphalt composition Examples 1 to 3 400g of StAs was heated in an oven at 180°C for 30 minutes. The stirring part of a homomixer MARKII2.5 type was inserted into the StAs softened by heating, and the asphalt modifiers of Examples 1 to 3 were added while gradually increasing the rotation speed of the stirring part. The mixture obtained by adding the asphalt modifiers of Examples 1 to 3 was melt-kneaded for 1 hour at a rotation speed of 7000 rpm while heating to 180°C. The formed molten kneaded product was cooled to room temperature over a day and night to obtain an asphalt composition. The amount of the asphalt modifier added was adjusted so that the amounts of the resin and additives used to prepare the asphalt modifier were the contents (unit: parts by mass) shown in Table 1. The contents shown in Table 1 are values ​​assuming that the total of the asphalt, resin, and additives is 100 parts by mass.

[0052] Examples 4 to 17, Comparative Examples 1 to 9 400g of StAs was heated in an oven at 180°C for 30 minutes. The stirring part of a homomixer MARKII2.5 type was inserted into the StAs softened by heating, and the mixture obtained by adding the resin and additives while gradually increasing the rotation speed of the stirring part was melt-kneaded for 1 hour at a rotation speed of 7000 rpm while heating to 180°C. The formed molten kneaded product was cooled to room temperature over a day and night to obtain an asphalt composition. The amounts of the resin and modifier added were adjusted so that the amounts of the resin and additives used to prepare the asphalt modifier were the contents (unit: parts by mass) shown in Tables 1 to 3. The contents shown in Tables 1 to 3 are values ​​assuming that the total of the asphalt, resin, and additives is 100 parts by mass.

[0053] 4. Evaluation Approximately 150 g of the prepared asphalt composition was placed in a 160 mL aluminum can and stored in an oven at 175°C for 1 or 7 days. After storage, the asphalt composition was collected, and the strippability of the asphalt composition stored for 0, 1, and 7 days was evaluated by the following test in accordance with JPI-5S-27-86 "Test method for strippability of asphalt coatings". The asphalt composition stored for 0 days was the asphalt composition immediately after it was prepared.

[0054] First, No. 6 crushed stone (hard sandstone or limestone) was classified using a 13 mm sieve and a 10 mm sieve to prepare aggregates with particle sizes of 10 to 13 mm. The aggregates were washed with water and then dried in a hot air dryer set at 150 ° C until they reached a certain weight. An asphalt composition heated to a temperature lower than a temperature 80 ° C higher than the softening point of the asphalt composition was applied to the dried aggregates, and the surface of the aggregates was completely covered with the asphalt composition. The ratio of the asphalt composition to 100 g of aggregate was set to 5.5 ± 0.2 g. The obtained asphalt-coated sample was spread on a glass plate and immersed in 80 ° C. hot water for one week. After immersing in 80 ° C. hot water for one week, the ratio of the area of ​​the part where the asphalt composition was not peeled off was measured. The measurement results are shown in Tables 1 to 3. In addition, "-" in the tables means that it was not measured.

[0055] [Table 1]

[0056] [Table 2]

[0057] [Table 3]

[0058] From Tables 1 to 3, by comparing Examples 1 to 17 and Comparative Examples 1 to 7, it was possible to maintain anti-stripping performance against aggregates even after long-term storage at high temperatures by containing an additive containing at least one of a polyolefin copolymer having an epoxy group and an organic compound having a carboxyl group or a metal salt thereof in the asphalt composition. Also, from a comparison between Examples 1 to 17 and Comparative Example 8, when the asphalt composition does not contain an additive containing at least one of an organic compound having a carboxyl group or a metal salt thereof, it was not possible to maintain anti-stripping performance against aggregates after long-term storage at high temperatures. Also, from a comparison between Examples 1 to 17 and Comparative Example 9, when the asphalt composition contains an inorganic acid component instead of an organic compound having a carboxyl group or a metal salt thereof, it gelled when stored at high temperatures, so it was not possible to evaluate the peelability and it was not possible to maintain anti-stripping performance against aggregates.

Claims

1. A polyolefin copolymer having an epoxy group; an additive containing at least one of an organic compound having a carboxyl group and a metal salt thereof; A melt-kneaded product of a mixture containing The organic compound has 6 to 20 carbon atoms, The asphalt modifier, wherein the organic compound comprises at least one selected from the group consisting of saturated fatty acids and unsaturated fatty acids.

2. The asphalt modifier of claim 1 , wherein the organic compound comprises stearic acid.

3. The asphalt modifier according to claim 1 or 2, wherein the content of the additive is 0.1 to 30 mass% based on the total mass of the mixture to be melt-kneaded.

4. Asphalt and The asphalt modifier according to any one of claims 1 to 3, An asphalt composition comprising:

5. A first agent containing a polyolefin copolymer having an epoxy group; A second agent containing an additive containing at least one of an organic compound having a carboxyl group or a metal salt thereof; A material set comprising: The organic compound has 6 to 20 carbon atoms, The asphalt modifier, wherein the organic compound comprises at least one selected from the group consisting of saturated fatty acids and unsaturated fatty acids.

6. The asphalt modifier of claim 5 , wherein the organic compound comprises stearic acid.

7. Asphalt and A polyolefin copolymer having an epoxy group; an additive containing at least one of an organic compound having a carboxyl group and a metal salt thereof; A melt-kneaded product of a mixture containing The organic compound has 6 to 20 carbon atoms, The asphalt composition, wherein the organic compound comprises at least one selected from the group consisting of saturated fatty acids and unsaturated fatty acids.

8. The asphalt composition of claim 7, wherein the organic compound comprises stearic acid.

9. The asphalt composition according to claim 7 or 8, wherein the content of the additive is 0.01 to 1 mass% based on the total mass of the mixture to be melt-kneaded.

Citation Information

Patent Citations

  • Vibration-damping composition

    JP1989101369A

  • Reformed asphalt composition

    JP1996199073A

  • Asphalt modifying agent and asphalt composition containing the same agent

    JP1999029665A

  • Asphalt modifier and asphalt composition containing the modifier

    JP2004035839A

  • Modified asphalt using epoxide-containing polymers

    JP2019500464A