High-strength thick steel plate with excellent formability and its manufacturing method

A controlled steel composition and hot rolling process with specific alloying elements and cooling rates produce a thick steel plate with uniform microstructure and hardness distribution, addressing non-uniformity and crack issues, enhancing strength and formability for large commercial vehicles and heavy equipment.

JP7588717B2Active Publication Date: 2024-11-22POHANG IRON & STEEL CO LTD
View PDF 13 Cites 0 Cited by

Patent Information

Application Number
JP2023524172
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-10-23
Filing Date
2021-10-20
Publication Date
2024-11-22
Estimated Expiration
2041-10-20

AI Technical Summary

Technical Problem

Existing methods for manufacturing high-strength, extra-thick steel plates face challenges in achieving a uniform microstructure during hot rolling, leading to non-uniform stress distribution, increased crack propensity, and reduced durability due to localized stress concentration and microstructural heterogeneity, especially in thick plates with a thickness of 15 to 25 mm.

Method used

A steel composition with specific alloying elements (C, Si, Mn, Cr, Al, P, S, N, Ti, Nb) and controlled hot rolling and cooling processes to achieve a microstructure comprising 90% ferrite and bainite, limited pearlite and carbides, and controlled cooling rates to ensure uniform hardness distribution, thereby enhancing yield strength and elongation.

Benefits of technology

The solution results in a thick steel plate with excellent tensile strength, yield strength, and elongation, ensuring high strength characteristics and formability, suitable for structural members in large commercial vehicles and heavy equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007588717000005
    Figure 0007588717000005
  • Figure 0007588717000006
    Figure 0007588717000006
  • Figure 0007588717000007
    Figure 0007588717000007
Patent Text Reader

Abstract

The present invention relates to a high-strength thick steel plate having excellent formability and a manufacturing method thereof, and more specifically to a high-strength thick steel plate having a uniform microstructure, excellent yield strength and elongation, and no cracks occurring during forming, and a manufacturing method thereof.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thick steel plate and a manufacturing method thereof, and more particularly to a thick steel plate having high strength properties and excellent formability, and a manufacturing method thereof. [Background technology]

[0002] Conventionally, plate materials with a thickness of 12 to 14 mm and a tensile strength of 440 MPa or more, which are manufactured by the plate rolling process, have been mainly used for structural members of commercial vehicles and heavy equipment, but recently, technology has been developed to use high-strength steel materials with a tensile strength of 550 MPa or more in order to reduce weight and increase strength. In particular, extra-thick plate materials with a thickness of 15 to 25 mm, which are used for large commercial vehicles, special vehicles, and heavy equipment parts, have been manufactured by the plate rolling process, but a method of applying the hot rolling process is required to ensure price competitiveness.

[0003] However, when high-strength extra-thick steel plate is manufactured by a hot rolling process, there are problems such as difficulty in rolling under high pressure, difficulty in forming a uniform microstructure, difficulty in securing stable yield strength, ease of cracking during manufacturing of parts, and shortened durability life due to localized stress concentration during use.

[0004] In this regard, for conventional steel materials, a technique has been proposed in which, after hot rolling in the normal austenite region, the steel is coiled at a high temperature to form a ferrite phase as the base structure and fine precipitates are formed to ensure strength and ductility, as in Patent Document 1, and a technique has been proposed in which the coiling temperature is cooled to a temperature at which a bainite phase is formed in the base structure so as not to form a coarse pearlite structure, and then the steel is coiled, as in Patent Document 2. In addition, a technique has been proposed in Patent Document 3 in which Ti, Nb, etc. are used to refine austenite grains by performing a reduction of 20 to 40% two or more times in the non-recrystallized region during hot rolling.

[0005] However, although alloying elements such as Si, Mn, Al, Mo, and Cr, which are mainly used in the above-mentioned technology for manufacturing thick high-strength steel plates, are effective in improving strength, excessive addition of these elements leads to segregation and uneven microstructure, which reduces formability, and fine cracks generated on the shear surface easily propagate in a fatigue environment, resulting in damage to the parts. In particular, as the thickness increases, the unevenness of the microstructure between the surface layer and the deeper layer increases, which increases local stress concentration and increases the propagation speed of cracks in a fatigue environment, resulting in reduced durability.

[0006] Furthermore, in order to obtain a precipitation strengthening effect by refining the crystal grains of thick plate material, it is effective to utilize precipitate-forming elements such as Ti, Nb, and V. However, if the plate material is coiled at a high temperature of 500 to 700°C, at which precipitates are likely to form, or if the cooling rate is not controlled during cooling after hot rolling, coarse carbides will form in the center of the thickness of the thick plate material, resulting in a deterioration in the quality of the sheared surface.

[0007] Furthermore, applying a rolling reduction of 20 to 40% two or more times in the unrecrystallized region during hot rolling can be easily applied to thin products, but there is a problem in that it is difficult to apply when manufacturing thick plate products, which have a smaller total rolling amount than thin products. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] Japanese Patent Publication No. 2002-322541 [Patent Document 2] Korean Patent Registration No. 10-1528084 [Patent Document 3] Japanese Patent Publication No. 1997-143570 Summary of the Invention [Problem to be solved by the invention]

[0009] One aspect of the present invention provides a high-strength thick steel plate that is excellent in yield strength and elongation and does not generate cracks during forming by ensuring a uniform microstructure during a hot rolling process of the thick steel plate, and a manufacturing method thereof.

[0010] The object of the present invention is not limited to the above-mentioned contents, and a person skilled in the art will have no difficulty in understanding further object of the present invention from the entire contents of this specification. [Means for solving the problem]

[0011] One aspect of the present invention comprises, by weight%, C: 0.05-0.15%, Si: 0.01-1.0%, Mn: 1.0-2.0%, Cr: 0.005-1.0%, Al: 0.01-0.1%, P: 0.001-0.02%, S: 0.001-0.01%, N: 0.001-0.01%, Ti: 0.005-0.11%, Nb: 0.005-0.07%, with the balance being Fe and unavoidable impurities; The R value defined by the following relational formula 1 satisfies 0.3 to 1.0, Based on the cross section, the surface layer in the range of 0 to t / 4 (where t means the thickness of the steel plate) and the deep layer in the range of t / 4 to t / 2 (excluding t / 4) each contain, in area percentage, ferrite and bainite in total at 90% or more, pearlite and carbides with a diameter of 0.5 μm or more at less than 5%, and MA phase (Martensite & Austenite) at less than 5% as a fine structure, The product of yield strength and elongation (YSxT-El) is 16000MPa·% or more. We can provide thick steel plates with a thickness of 10 mm or more. [Equation 1] R=[C]*+0.7x[Mn]+8.5x[P]+7.5x[S]-0.9x[Si]-1.5x[Nb] [C]*=[C]-[C]xQ Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) ([C], [Mn], [P], [S], [Si], [Nb] and [Ti] in the above Relational Formula 1 are the weight percentages of the corresponding alloying elements.)

[0012] The thickness of the steel plate may be 15 mm or more.

[0013] In a deep layer portion of the steel plate, the pearlite and carbides having a diameter of 0.5 μm or more may account for 3% or less by area, and the MA phase may account for 3% or less.

[0014] In the surface layer portion of the steel plate, the bainite may be 20% or less, the pearlite and carbides with a diameter of 0.5 μm or more may be less than 2%, and the MA phase may be 3% or less, in area percentage.

[0015] The difference between the average hardness value and the maximum hardness value measured at 0.5 mm intervals from a point 0.5 mm below the surface layer of the test piece to a point 0.5 mm below the back surface layer based on any line perpendicular to the thickness cross section of the steel plate may be 20 Hv or less.

[0016] Another aspect of the present invention is a step of reheating a steel slab containing, by weight, 0.05-0.15% C, 0.01-1.0% Si, 1.0-2.0% Mn, 0.005-1.0% Cr, 0.01-0.1% Al, 0.001-0.02% P, 0.001-0.01% S, 0.001-0.01% N, 0.005-0.11% Ti, 0.005-0.07% Nb, the balance being Fe and unavoidable impurities, and wherein the R value defined by the following Relation 1 is 0.3-1.0; hot rolling the reheated steel slab at a temperature range of 800 to 1150°C with a rolling reduction of 20 to 50% to a thickness of 10 mm or more, and finishing the rolling in a temperature range of Tn-50 to Tn defined by the following Relation 2: The above hot-rolled steel sheet is subjected to a CR defined by the following formula 3 up to a temperature range of 450 to 550°C. Min a step of first cooling at the above cooling rate and then coiling; and A method for manufacturing a thick steel plate may be provided, the method including a step of secondary cooling the coiled steel plate. [Equation 1] R=[C]*+0.7x[Mn]+8.5x[P]+7.5x[S]-0.9x[Si]-1.5x[Nb] [C]*=[C]-[C]xQ Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) ([C], [Mn], [P], [S], [Si], [Nb] and [Ti] in the above Relational Formula 1 are the weight percentages of the corresponding alloying elements.) [Equation 2] Tn=730+92x[C]+70x[Mn]+45x[Cr]+650x[Nb]+410x[Ti]-80x[Si]-1.4x(t-8) (The unit of Tn in the above Relational Formula 2 is °C, and [C], [Mn], [Cr], [Nb], [Ti] and [Si] are the weight percentages of the corresponding alloying elements.) (t in the above Relational Expression 2 is the thickness (mm) of the final rolled plate material.) [Equation 3] CR Min =76.6-157x[C]-25.2x[Si]-14.1x[Mn]-27.3x[Cr]+61x[Ti]+448x[Nb] (CR of the above formula 3 Min The unit is °C / s, and [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percent of the corresponding alloying elements.

[0017] The reheating can be carried out in the temperature range of 1200 to 1350°C.

[0018] The cooling rate during the primary cooling may be 80° C. / sec or less.

[0019] During the secondary cooling, the material can be air-cooled or water-cooled to a temperature range of room temperature to 200°C. Effect of the Invention

[0020] According to one aspect of the present invention, it is possible to provide a thick steel plate that is excellent in tensile strength, yield strength, and elongation, and has high strength properties while also having excellent formability, and a method for manufacturing the same.

[0021] According to another aspect of the present invention, there is provided a high strength thick steel plate for use in structural members such as wheel rims, discs, members and frames of large commercial vehicles, and a manufacturing method thereof. [Brief description of the drawings]

[0022] [Figure 1] 1 shows the product of yield strength and elongation (YSxT-El) and the difference (ΔH) between the average hardness value and the maximum hardness value in the thickness section of the inventive steel and the comparative steel. [Diagram 2] 1 shows the hardness distribution in the thickness cross section of the inventive steel and the comparative steel. [Diagram 3] 1 shows the hardness distribution in the thickness cross section of the inventive steel and the comparative steel. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] Hereinafter, preferred embodiments of the present invention will be described. The embodiments of the present invention can be modified in various ways, and the scope of the present invention should not be construed as being limited to the embodiments described below. The present embodiments are provided to further explain the present invention in detail to those skilled in the art to which the present invention pertains.

[0024] In order to solve the above-mentioned problems, the inventors of the present invention investigated the distribution of microstructures in the thickness direction and detailed changes in material properties depending on the composition, hot rolling and cooling conditions for extra thick rolled steel plates having various compositions.

[0025] As a result, the inventors confirmed a method for making hot-rolled thick steel plate have excellent yield strength and ductility, and in particular, confirmed that uniformity is ensured in the microstructure of thick steel plate having a certain thickness or more, and that the hardness distribution in the thickness direction is constant, which led to the completion of the present invention.

[0026] The present invention will be described in detail below.

[0027] The steel composition of the present invention will be described in detail below.

[0028] In the present invention, unless otherwise specified, the percentage indicating the content of each element is based on weight.

[0029] A steel sheet according to one aspect of the present invention may contain, by weight, C: 0.05-0.15%, Si: 0.01-1.0%, Mn: 1.0-2.0%, Cr: 0.005-1.0%, Al: 0.01-0.1%, P: 0.001-0.02%, S: 0.001-0.01%, N: 0.001-0.01%, Ti: 0.005-0.11%, Nb: 0.005-0.07%, with the balance being Fe and unavoidable impurities.

[0030] Carbon (C): 0.05~0.15% Carbon (C) is the most economical and effective element for strengthening steel, and increasing the amount of carbon added increases the precipitation strengthening effect or the proportion of bainite phase, thereby increasing tensile strength. When the thickness of a hot-rolled steel sheet is increased, the cooling rate at the center of the thickness during cooling after hot rolling slows down, and if the carbon (C) content is high, coarse carbides and pearlite are likely to form. If the carbon (C) content is less than 0.05%, it is difficult to obtain a sufficient strengthening effect, and if the carbon (C) content exceeds 0.15%, there are problems in that formability and durability are reduced due to the formation of coarse carbides, pearlite phase, and band structure at the center of the thickness, and weldability is also poor.

[0031] Therefore, the carbon (C) content may be 0.05 to 0.15%, and more preferably 0.06% or more and 0.12% or less.

[0032] Silicon (Si): 0.01 to 1.0% Silicon (Si) is an element that has the effect of deoxidizing molten steel, strengthening solid solution, and delaying the formation of coarse carbides to improve formability. If the content of silicon (Si) is less than 0.01%, the effect of solid solution strengthening is poor, and the effect of delaying the formation of carbides is also slight, making it difficult to improve formability. If the content of silicon (Si) exceeds 1.0%, the phase transformation temperature increases, and during hot rolling of extremely thick plate materials in the low temperature range, coarse grains are likely to form due to localized rolling of the ferrite region in the surface layer, and red scale due to silicon (Si) is formed on the surface of the steel plate, which not only significantly deteriorates the quality of the steel plate surface, but also reduces ductility and weldability.

[0033] Therefore, the silicon (Si) content may be 0.01 to 1.0%, and more preferably 0.1% or more and 0.9% or less.

[0034] Manganese (Mn): 1.0-2.0% Manganese (Mn), like Si, is an effective element for solid solution strengthening of steel, and increases the hardening ability of steel, facilitating the formation of bainite phase during cooling after hot rolling. If the manganese (Mn) content is less than 1.0%, the above effects of addition cannot be obtained, and if the content exceeds 2.0%, the hardening ability increases significantly, making martensite phase transformation more likely to occur and promoting the formation of pearlite during high-temperature coiling. In addition, during the continuous casting process, segregation areas develop significantly in the center of the thickness during slab casting, and during cooling after hot rolling, microstructures are formed unevenly in the thickness direction, reducing formability and durability.

[0035] Therefore, the manganese (Mn) content may be 1.0 to 2.0%, and more preferably 1.1% or more.

[0036] Chromium (Cr): 0.005~1.0% Chromium (Cr) is an element that strengthens steel through solid solution, and plays a role in retarding the phase transformation of ferrite during cooling and aiding in the formation of bainite. If the chromium (Cr) content is less than 0.005%, the above effects of addition are not obtained, and if the chromium (Cr) content exceeds 1.0%, the ferrite transformation is excessively retarded, martensite phase is formed, and elongation decreases. In addition, like Mn, segregation develops significantly in the center of the thickness, making the microstructure in the thickness direction non-uniform and reducing formability and durability.

[0037] Therefore, the chromium (Cr) content may be 0.005 to 1.0%, and more preferably 0.1% or more and 0.9% or less.

[0038] Aluminum (Al): 0.01-0.1% Aluminum (Al) is an element added mainly for deoxidation. If the content of aluminum (Al) is less than 0.01%, the effect of adding it is insufficient, and if the content exceeds 0.1%, it bonds with N to form AlN, which is likely to cause corner cracks in the slab during continuous casting and defects due to the formation of inclusions.

[0039] Therefore, the aluminum (Al) content may be 0.01 to 0.1%.

[0040] Phosphorus (P): 0.001 to 0.02% Phosphorus (P) is an element that, like Si, simultaneously promotes solid solution strengthening and ferrite transformation. If the phosphorus (P) content exceeds 0.02%, embrittlement occurs due to grain boundary segregation, and fine cracks are likely to occur during forming, significantly deteriorating formability and durability. On the other hand, to reduce the P content to less than 0.001%, the manufacturing costs are high, which is economically disadvantageous, and is insufficient for obtaining strength.

[0041] Therefore, the phosphorus (P) content may be 0.001 to 0.02%.

[0042] Sulfur (S): 0.001-0.01% Sulfur (S) is an impurity present in steel, and if the sulfur (S) content exceeds 0.01%, it combines with Mn and other elements to form non-metallic inclusions, which can easily cause fine cracks during cutting of the steel, and can cause problems such as poor formability and durability. On the other hand, to reduce the sulfur content to less than 0.001%, steelmaking operations take a long time, resulting in reduced productivity.

[0043] Therefore, the content of sulfur (S) may be 0.001 to 0.01%.

[0044] Nitrogen (N): 0.001-0.01% Nitrogen (N) is a typical solid solution strengthening element along with C, and forms coarse precipitates along with Ti and Al. In general, the effect of solid solution strengthening of nitrogen (N) is superior to that of C, but there is a problem that the toughness decreases significantly as the amount of nitrogen (N) in steel increases, so the upper limit is set at 0.01%. On the other hand, to reduce the content to less than 0.001%, it takes a lot of time during steelmaking operations, and productivity decreases.

[0045] Therefore, the nitrogen (N) content may be 0.001 to 0.01%.

[0046] Titanium (Ti): 0.005 to 0.11% Titanium (Ti) is a typical precipitation strengthening element, and forms coarse TiN in steel due to its strong affinity with N. TiN has the effect of suppressing the growth of crystal grains during the heating process for hot rolling. In addition, titanium (Ti) that remains after reacting with N dissolves in steel and bonds with C to form TiC precipitates, which is useful for improving the strength of steel. If the titanium (Ti) content is less than 0.005%, the above effect cannot be obtained, and if the content exceeds 0.11%, there is a problem that the generation of coarse TiN and the coarsening of the precipitates cause local stress concentration during forming, making it easy for cracks to occur.

[0047] Therefore, the titanium (Ti) content may be 0.005 to 0.11%, and more preferably 0.01% or more and 0.1% or less.

[0048] Niobium (Nb): 0.005-0.07% Niobium (Nb), together with Ti, is a representative precipitation strengthening element, and is effective in improving the strength and impact toughness of steel by refining grains through precipitation during hot rolling and delaying recrystallization. If the niobium (Nb) content is less than 0.005%, the above effect cannot be obtained, and if the content exceeds 0.07%, there is a problem that formability and durability are reduced due to the formation of elongated grains and coarse complex precipitates caused by excessive delay in recrystallization during hot rolling.

[0049] Therefore, the niobium (Nb) content may be 0.005 to 0.07%, and more preferably 0.01% or more.

[0050] The steel material of the present invention may contain the remaining iron (Fe) and inevitable impurities in addition to the above-mentioned composition. The inevitable impurities cannot be excluded because they may be unintentionally mixed in during normal manufacturing processes. Since such impurities are known to any engineer in the field of normal steel manufacturing, the entire contents of the impurities will not be mentioned in this specification.

[0051] The steel of the present invention may have an R value defined by the following relational expression 1 of 0.3 to 1.0.

[0052] By controlling R in Relation 1, it is possible to improve the uniformity of the microstructure by minimizing the segregation of C, Mn, P, S, etc. and the formation of MnS that occurs during the solidification of steel and cooling of the slab in the continuous casting process. It is generally known that segregation of alloy elements such as C and Mn occurs in the cast structure formed during solidification, and P has the characteristic of being mainly segregated at the grain boundaries when the steel plate is maintained at high temperatures after hot rolling and cooling, which causes embrittlement of the grain system. This segregation is highly dependent on the content of the alloy elements. In particular, C and Mn form coarse carbides and pearlite structures during cooling after hot rolling, which causes a decrease in the quality of the sheared surface. In addition, Mn forms MnS, a nonmetallic inclusion, together with S, which is elongated during rolling and significantly reduces the formability of the final product. On the other hand, Si suppresses the formation of coarse carbides and has a large effect of solid solution strengthening even with a small amount of alloy, and Nb and Ti are effective in forming fine precipitates to refine the crystal grain size, and are effective in improving the above-mentioned segregation and grain boundary embrittlement problems.

[0053] In the present invention, steels having various alloy components were hot rolled to produce thick plates, and the hardness of the cross section was measured. As a result, it was confirmed that there is a correlation between the uniformity of the microstructure, the alloy components and their contents, and this led to derive Relational Formula 1.

[0054] When the R value defined by the following relational expression 1 is less than 0.3, it is difficult to secure the physical properties targeted in the present invention, whereas when the value exceeds 1.0, the non-uniformity of the microstructure increases, and the hardness value in the cross section varies greatly. More preferably, the lower limit of the R value may be 0.5, and the upper limit may be 0.8. [Equation 1] R=[C]*+0.7x[Mn]+8.5x[P]+7.5x[S]-0.9x[Si]-1.5x[Nb] [C]*=[C]-[C]xQ Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) ([C], [Mn], [P], [S], [Si], [Nb] and [Ti] in the above Relational Formula 1 are the weight percentages of the corresponding alloying elements.)

[0055] In the following, the steel microstructure of the present invention will be described in detail.

[0056] Unless otherwise specified in the present invention, the percentages expressing the fraction of the microstructure are based on the area.

[0057] In a steel satisfying the alloy composition according to one aspect of the present invention, based on a cross section, a surface layer portion in the range of 0 to t / 4 (where t means the thickness of the steel plate) and a deep layer portion in the range of t / 4 to t / 2 (excluding t / 4) can each contain, in area percentages, a total of 90% or more of ferrite and bainite, less than 5% of pearlite and carbides with a diameter of 0.5 μm or more, and less than 5% of MA phase (Martensite & Austenite) as a fine structure.

[0058] The microstructure of thick high-strength steel plates is determined during cooling. Bainite and MA (Martensite & Austenite) phases tend to form easily in the surface layer where the cooling rate is fast, whereas coarse carbides and pearlite tend to form in the deeper layer where the cooling rate is slow.

[0059] Generally, the MA phase formed in the surface layer is a hard phase and has a higher hardness than the surrounding microstructure, resulting in a non-uniform hardness distribution, which causes microcracks to occur due to the difference in hardness between the MA phase and the matrix during forming. Also, the coarse carbides and pearlite formed in the deep layer are harder than the surrounding microstructure and are brittle, which causes microcracks to occur during shear forming.

[0060] Therefore, in the present invention, in order to simultaneously solve the problems in the surface layer and the deep layer, the fractions of pearlite and carbides with a diameter of 0.5 μm or more are limited to less than 5%, and the fraction of the MA phase is limited to less than 5%. At this time, the fractions of pearlite, carbides with a diameter of 0.5 μm or more, and the MA phase can be applied equally to both the surface layer and the deep layer.

[0061] In the present invention, the inclusion of 90% or more of ferrite and bainite is for the purpose of suppressing the unnecessary formation of coarse carbides and pearlite, providing a uniform hardness distribution according to thickness position, and securing excellent yield strength and elongation, and if the inclusion is less than 90%, it is difficult to secure the product of yield strength and elongation (YSxT-El) value targeted in the present invention. Therefore, in the present invention, the total inclusion of 90% or more of ferrite and bainite can be used.

[0062] From the standpoint of ensuring the physical properties aimed at by the present invention, it is more preferable that in the deep layer portion, the pearlite and carbides with a diameter of 0.5 μm or more are 3% or less and the MA phase is 3% or less, and in the surface layer portion, the bainite is 20% or less, the pearlite and carbides with a diameter of 0.5 μm or more are less than 2%, and the MA phase is 3% or less.

[0063] The microstructure in the present invention has the same characteristics in the surface layer and the deep layer of the steel, and the microstructure proposed in the present invention is applied to the entire steel in the same manner. In addition, the surface layer in the present invention means a region in the range of 0 to t / 4 (t is the thickness of the steel plate) based on the cross section, and the deep layer means a region in the range of t / 4 to t / 2 (excluding t / 4).

[0064] The steel production method of the present invention will now be described in detail.

[0065] The steel according to one aspect of the present invention may be produced by reheating, hot rolling, primary cooling, coiling, and secondary cooling a steel slab satisfying the above-mentioned alloy composition.

[0066] Slab Reheat A steel slab satisfying the above-mentioned alloy composition can be reheated in the temperature range of 1200 to 1350°C.

[0067] If the reheating temperature is less than 1200°C, the precipitates are not sufficiently redissolved, the amount of precipitates formed in the process after hot rolling is reduced, and coarse TiN remains.On the other hand, if the temperature exceeds 1350°C, the strength decreases due to abnormal grain growth of austenite crystal grains.

[0068] Hot rolling The reheated steel slab can be hot rolled at a rolling reduction of 20 to 50% in a temperature range of 800 to 1150°C, and the rolling can be completed in a temperature range of Tn-50 to Tn defined by the following relational expression 2.

[0069] If the hot rolling temperature exceeds 1150°C, the temperature of the steel sheet becomes too high, the grain size becomes coarse, and the surface quality of the hot rolled steel sheet deteriorates. On the other hand, if the temperature is less than 800°C, elongated grains develop due to excessive delay in recrystallization, and anisotropy and formability become poor. If the steel sheet is rolled at a temperature below the austenite temperature range, a non-uniform microstructure develops more significantly. This makes it easier for fine cracks to occur in non-uniform areas during forming, and reduces ductility.

[0070] If the rolling end temperature exceeds Tn, the microstructure of the steel becomes coarse and non-uniform. If the temperature is less than Tn-50, in the case of an extra-thick high-strength steel plate having a thickness of 15 to 25 mm, the fine ferrite phase fraction increases due to the promotion of ferrite phase transformation in the surface layer where the temperature is relatively low, but the crystal grains have an elongated shape, which causes cracks to propagate rapidly, and a non-uniform microstructure may remain in the center, resulting in poor durability.

[0071] The rolling finish temperature determined by Relational Formula 2 in the present invention means the temperature of the hot-rolled steel sheet at the end of hot rolling. [Equation 2] Tn=730+92x[C]+70x[Mn]+45x[Cr]+650x[Nb]+410x[Ti]-80x[Si]-1.4x(t-8) (The unit of Tn in the above Relational Formula 2 is °C, and [C], [Mn], [Cr], [Nb], [Ti] and [Si] are the weight percentages of the corresponding alloying elements.) (t in the above Relational Formula 2 is the thickness (mm) of the final rolled plate material)

[0072] The reduction within the hot rolling temperature range may be 20 to 50%.

[0073] If the reduction is less than 20%, it is difficult to obtain the effect of retarding recrystallization and uneven coarse grains are likely to form, and if the reduction exceeds 50%, an excessively elongated fine structure is formed, and if carbides are formed along the grain boundaries, cracks are likely to occur along the grain boundaries during forming. In addition, the number of fine precipitates is reduced, and the effect of precipitation strengthening is also reduced.

[0074] Primary cooling and winding The above hot-rolled steel sheet is subjected to a CR defined by the following formula 3 up to a temperature range of 450 to 550°C. Min After primary cooling at the above cooling rate, the sheet can be coiled.

[0075] The temperature range from immediately after hot rolling to the cooling end temperature corresponds to the temperature range where the phase transformation of ferrite occurs during cooling, and since the cooling rate at the center of the thickness is slower than that at the surface layer of the rolled sheet, coarse ferrite phase and coarse carbide are formed at the center of the thickness, resulting in a non-uniform microstructure. Therefore, in order to prevent this, in the present invention, a specific cooling rate CR Min However, if the average cooling rate in the above temperature range exceeds 80° C. / sec, the difference in cooling rate between the surface layer and the deep layer becomes too large, and the hardness difference between the surface layer and the deep layer increases significantly, resulting in poor formability and durability.

[0076] The cooling rate determined by Relational Formula 3 in the present invention means the cooling rate of the hot-rolled steel sheet after hot rolling. [Equation 3] CR Min =76.6-157x[C]-25.2x[Si]-14.1x[Mn]-27.3x[Cr]+61x[Ti]+448x[Nb] (CR of the above formula 3 Min The unit is °C / s, and [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of the corresponding alloying elements.)

[0077] If the cooling end temperature and the coiling temperature exceed 550°C, a pearlite phase is formed in a band structure or a large amount of coarse carbides are formed, resulting in a decrease in formability and durability of the steel. If the temperature is less than 450°C, an excessive amount of martensite and MA phases are formed, resulting in a decrease in formability and durability.

[0078] Secondary cooling The coiled steel sheet may be secondarily cooled to a temperature range of room temperature to 200° C., and the secondarily cooling may be air-cooling or water-cooling.

[0079] In the present invention, air cooling means cooling in air at room temperature at a cooling rate of 0.001 to 10°C / hour. Even if the cooling rate exceeds 10°C / hour, water cooling may be used since it is possible to suppress transformation of some untransformed phases in the steel into the MA phase if the above coiling temperature and primary cooling conditions are satisfied. In the present invention, water cooling means cooling by inserting the coil into a water bath at room temperature. However, in order to control the cooling rate to less than 0.001°C / hour, separate heating and heat retention equipment is required, which is economically disadvantageous, so the lower limit of the cooling rate may be 0.001°C / hour.

[0080] The steel plate of the present invention manufactured as described above may be a thick steel plate having a thickness of 10 mm or more, more preferably 15 mm or more, and may be a thick steel plate with an upper limit of 25 mm. The steel plate of the present invention may have a difference between an average hardness value and a maximum hardness value measured at 0.5 mm intervals from a point 0.5 mm below the surface layer of a test piece to a point 0.5 mm below the back surface layer of the test piece, based on an arbitrary line perpendicular to the thickness cross section, of 20 Hv or less, more specifically, the average hardness value may be 160 to 300 Hv. In addition, the product of yield strength and elongation (YSxT-El) is 16000 MPa·% or more, and the steel plate may have excellent formability while being high in strength.

[0081] The present invention will be described in more detail below with reference to examples. However, it should be noted that the following examples are merely intended to illustrate and explain the present invention in more detail, and are not intended to limit the scope of the present invention. EXAMPLES

[0082] Table 1 below shows the steel composition and final hot-rolled sheet thickness for each steel type. Table 2 below shows the rolling finish temperature (FDT), total reduction (%), coiling temperature (CT), cooling rate (CR*) up to the coiling temperature which is the cooling finish temperature after hot rolling, Tn and Tn-50 defined by Relation 2, and the minimum cooling rate (CR*) defined by Relation 3 for the steel types shown in Table 1. MinThe reheating temperature not disclosed in Table 2 was 1250°C, the hot rolling temperature was 800 to 1150°C, and the cooling rate of the steel sheet after coiling was 1°C / hour.

[0083] [Table 1] [Equation 1] R=[C]*+0.7x[Mn]+8.5x[P]+7.5x[S]-0.9x[Si]-1.5x[Nb] [C]*=[C]-[C]xQ Q = ([Nb] / 93 + [Ti] / 48) / ([C] / 12) ([C], [Mn], [P], [S], [Si], [Nb] and [Ti] in the above Relational Formula 1 are the weight percentages of the corresponding alloying elements.)

[0084] [Table 2] [Equation 2] Tn=730+92x[C]+70x[Mn]+45x[Cr]+650x[Nb]+410x[Ti]-80x[Si]-1.4x(t-8) (The unit of Tn in the above Relational Formula 2 is °C, and [C], [Mn], [Cr], [Nb], [Ti] and [Si] are the weight percentages of the corresponding alloying elements.) (t in the above Relational Expression 2 is the thickness (mm) of the final rolled plate material.) [Equation 3] CR Min =76.6-157x[C]-25.2x[Si]-14.1x[Mn]-27.3x[Cr]+61x[Ti]+448x[Nb] (CR of the above formula 3 Min The unit is °C / s, and [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of the corresponding alloying elements.)

[0085] Tables 3 and 4 below show the microstructural characteristics and mechanical properties of the steel grades.

[0086] The microstructures in Table 3 are the results of analysis at a point 0.5 mm beneath the surface layer of the hot-rolled sheet and at a deep layer. In the present invention, the surface layer refers to the range of 0 to t / 4 based on the thickness t, and the deep layer refers to the range of t / 4 to t / 2 (excluding t / 4). The microstructures of the surface layer in Table 3 are the results of analysis at a point 0.5 mm beneath the surface layer, and the microstructures of the deep layer are the results of analysis at t / 2, which is the center of the thickness. The area fraction of the MA phase was measured by etching using the Lepera etching method, and then analyzed at 1000x magnification using an optical microscope and an image analyzer. The area fractions of the martensite & austenite phase (MA), ferrite phase (F), bainite phase (B), and pearlite phase (P) were analyzed at 3000x and 5000x magnification using a scanning electron microscope (SEM). Here, ferrite (F) is polygonal ferrite with an equiaxed crystal shape, and bainite (B) refers to ferrite phases observed in the low temperature range, such as bainite, acicular ferrite, and bainitic ferrite. The area fraction of pearlite (P) refers to the sum of the area fractions of pearlite and carbides of 0.5 μm or more.

[0087] In Table 4, YS, TS, and T-El mean 0.2% off-set yield strength, tensile strength, and elongation at break, and are the results of testing JIS No. 5 standard test pieces taken parallel to the rolling direction. The hardness of the cross section of the test piece was also measured and shown. The hardness was measured with a Micro-Vickers tester at 0.5 mm intervals from a point 0.5 mm directly below the surface layer of the test piece to a point 0.5 mm directly below the back surface layer, based on an arbitrary line perpendicular to the thickness cross section of the test piece, and a load of 500 g was applied. Table 4 shows the maximum hardness value and average hardness value in the thickness cross section among the measured hardness values, and the difference between the two hardness values. Peak (number) means the number of parts where the difference between the hardness value at the thickness point and the average hardness value exceeds 20 Hv.

[0088] [Table 3]

[0089] [Table 4]

[0090] As shown in Table 4, invention steels 1 to 7, which have the alloy composition, production method and satisfy the relational expressions 1 to 3 proposed in the present invention, ensured all of the mechanical properties targeted by the present invention.

[0091] FIG. 1 shows the product of yield strength and elongation and the difference between the average hardness and maximum hardness of the thickness cross section for the inventive steel and the comparative steel. It can be seen that the difference in hardness for the inventive steel is 20 Hv or less, and the YSxT-El value is 16,000 MPa·% or more.

[0092] Figures 2 and 3 show the distribution of hardness values ​​in the thickness cross section of the invention steel and the comparative steel, respectively. In the case of the comparative steel, the hardness value at the center of the thickness is relatively low compared to the surface layer, and it can be confirmed that there is a large difference depending on the position in the thickness.

[0093] Comparative steels 1 to 4 are cases where the relational formula 1 proposed in the present invention is not satisfied. Comparative steel 1 is a case where the C content satisfies the range of the present invention, but exceeds the proposed range of relational formula 1 considering segregation. Therefore, excessive pearlite is formed in the deep and surface layers of the microstructure, and a high hardness difference is observed locally when the hardness is measured in the thickness direction. The ductility is also insufficient, and the results are outside the range proposed in the present invention. Comparative steels 2 and 3 are cases where the Mn content is outside the range of the Mn component proposed in the present invention and at the same time, the relational formula 1 is not satisfied. Comparative steel 2 has a low Mn content, so segregation in the thickness direction of the rolled plate, coarse carbides, and non-uniform pearlite are not formed, but the yield strength and tensile strength are insufficient, and the properties aimed at in the present invention are not obtained. Comparative steel 3 has an excessive Mn content, and the hardening ability is high, so bainite is formed in the surface layer, while pearlite is excessively formed in the deep layer, and elongated MnS inclusions are also observed. In particular, when the hardness was measured in the thickness direction, a high hardness difference was observed locally, and the ductility was also insufficient. Comparative steel 4 is a case in which the P content is outside the range proposed in the present invention and at the same time does not satisfy Relational Formula 1. The microstructure of comparative steel 4 satisfies the range proposed in the present invention, and the strength and elongation were also good, but when the hardness was measured, a local hardness difference was observed in one part, which is likely to cause brittleness when used after part manufacturing.

[0094] Comparative steel 5 satisfied the relational expression 1, but did not satisfy the range of the Si content of the present invention. It was confirmed that coarse ferrite was formed in the surface layer of the microstructure, and MA phases were also formed in the surface layer and deep layer. In addition, the surface layer showed a slightly low hardness value, and the product of yield strength and elongation was outside the range targeted by the present invention. This is because the phase transformation temperature was increased by the excessive addition of Si, ferrite was formed in the surface layer during hot rolling, and rolling was performed in the two-phase region, and some untransformed ferrite was formed from the MA phase.

[0095] Comparative steel 6 satisfies the range of the alloy composition of the present invention, but does not satisfy the relational formula 1. In this case, no segregation of the composition was observed, and the MA phase and coarse carbides in the microstructure were hardly formed, and only fine pearlite was observed around the grain boundaries. Therefore, the hardness distribution in the thickness direction was relatively uniform. However, the strength value targeted in the present invention could not be secured.

[0096] Comparative steels 7 and 8 are cases where the relational expression 2 and the reduction ratio are not satisfied. Comparative steel 7 is a case where rolling was completed in a temperature range that satisfied the relational expression 2, but the reduction ratio was insufficient, and a non-uniform microstructure was formed during cooling. Therefore, the structural fraction of the microstructure satisfied the present invention, but coarse grains were mixed in the ferrite matrix structure, and low yield strength was observed. Steels having such a microstructure may have poor durability during use of parts. Comparative steel 8 is a case where the relational expression 2 and the reduction ratio conditions are not satisfied. Due to the large reduction amount, an excessively elongated microstructure was formed in the surface layer due to delayed recrystallization during rolling, while equiaxed ferrite and pearlite were mainly formed in the deep layer, and the microstructure was composed of a non-uniform microstructure depending on the thickness position, which caused a decrease in the durability of the part and also a decrease in elongation.

[0097] Comparative steels 9 and 10 are cases where the coiling temperature conditions are not met. Comparative steel 9 is a case where the cooling end temperature and coiling temperature are higher than the temperature range proposed in the present invention, and pearlite is formed locally, and a pearlite band structure is observed especially in the deep layer. As a result, a locally high hardness difference is observed when hardness is measured in the thickness direction. Comparative steel 10 is a case where the cooling end temperature and coiling temperature are lower than the range proposed in the present invention. Comparative steel 10 is a case where an excessive amount of bainite is formed in the microstructure of the surface layer, and the elongation is insufficient.

[0098] Comparative steel 11 does not satisfy the cooling rate condition of the cooling rate relational expression 3, that is, the cooling rate during cooling after hot rolling is lower than the range of the present invention. Pearlite and coarse carbides are formed in the deep thickness layer, and a high hardness difference is observed locally.

[0099] Comparative steels 12 and 13 are cases where the conditions of reduction amount and cooling end temperature are not satisfied. In comparative steel 12, the reduction amount is insufficient in the temperature region where recrystallization is delayed during hot rolling, the coiling temperature is low, the grain size of ferrite is nonuniform, and bainite is excessively formed in the microstructure of the surface layer. Pearlite is also observed locally in the deep layer, which resulted in low elongation. Comparative steel 13 is a case where the reduction amount is insufficient in the temperature region where recrystallization is delayed, the coiling temperature is high, and the cooling rate does not satisfy Relation 3. As a result, it was confirmed that the microstructure is nonuniform, pearlite is formed in a band structure, and the yield strength is low.

[0100] Although the present invention has been described in detail with reference to the embodiments, other embodiments different from the above are possible, and therefore the technical spirit and scope of the claims set forth below are not limited to the embodiments.

Claims

1. In weight percent, it contains C: 0.05-0.15%, Si: 0.01-1.0%, Mn: 1.0-2.0%, Cr: 0.005-1.0%, Al: 0.01-0.1%, P: 0.001-0.02%, S: 0.001-0.01%, N: 0.001-0.01%, Ti: 0.005-0.11%, and Nb: 0.005-0.07%, with the balance being Fe and inevitable impurities; The R value defined by the following relational expression 1 satisfies 0.3 to 1.0, Based on the cross section, a surface layer portion in the range of 0 to t / 4 (where t means the thickness of the steel plate) and a deep layer portion in the range of t / 4 to t / 2 (excluding t / 4) each contain, in area percentage, ferrite and bainite in total at 90% or more, pearlite and carbides with a diameter of 0.5 μm or more at less than 5%, and MA phase (Martensite & Austenite) at less than 5% as a fine structure, The product of yield strength and elongation (YSxT-El) is 16000 MPa% or more, A thick steel plate having a thickness of 10 to 25 mm. [Relationship 1] R=[C]*+0.7x[Mn]+8.5x[P]+7.5x[S]-0.9x[Si]-1.5x[Nb] [C]*=[C]-[C]xQ Q=([Nb] / 93+[Ti] / 48) / ([C] / 12) (In the above Relational Formula 1, [C], [Mn], [P], [S], [Si], [Nb] and [Ti] are the weight percentages of the corresponding alloy elements.)

2. The thick steel plate according to claim 1, wherein the thickness of the steel plate is 15 to 25 mm.

3. 2. The thick steel plate according to claim 1, wherein the pearlite and carbides having a diameter of 0.5 μm or more are 3% or less and the MA phase is 3% or less, in terms of area %, in a deep layer portion of the steel plate.

4. 2. The thick steel plate according to claim 1, wherein, in area %, in a surface layer portion of the steel plate, the bainite is 20% or less, the pearlite and carbides having a diameter of 0.5 μm or more are less than 2%, and the MA phase is 3% or less.

5. 2. The thick steel plate according to claim 1, wherein the difference between the average hardness value and the maximum hardness value measured at 0.5 mm intervals from a point 0.5 mm directly below the surface layer of the test piece to a point 0.5 mm directly below the back surface layer with respect to an arbitrary line perpendicular to the thickness cross section of the steel plate is 20 Hv or less.

6. reheating a steel slab containing, by weight, 0.05-0.15% C, 0.01-1.0% Si, 1.0-2.0% Mn, 0.005-1.0% Cr, 0.01-0.1% Al, 0.001-0.02% P, 0.001-0.01% S, 0.001-0.01% N, 0.005-0.11% Ti, and 0.005-0.07% Nb, with the balance being Fe and unavoidable impurities, and satisfying an R value defined by the following Relation 1 of 0.3-1.0; hot rolling the reheated steel slab at a temperature range of 800 to 1150° C. with a rolling reduction of 20 to 50% to a thickness of 10 to 25 mm, and finishing the rolling in a temperature range of Tn-50 to Tn defined by the following Relation 2: The hot-rolled steel sheet is subjected to a CR defined by the following Relation 3 up to a temperature range of 450 to 550°C. Min A step of first cooling at the above cooling rate and then winding; and The method of manufacturing a thick steel plate further comprises a step of secondary cooling the coiled steel plate. [Relationship 1] R=[C]*+0.7x[Mn]+8.5x[P]+7.5x[S]-0.9x[Si]-1.5x[Nb] [C]*=[C]-[C]xQ Q=([Nb] / 93+[Ti] / 48) / ([C] / 12) (In the above Relational Formula 1, [C], [Mn], [P], [S], [Si], [Nb] and [Ti] are the weight percentages of the corresponding alloy elements.) [Relationship 2] Tn=730+92x[C]+70x[Mn]+45x[Cr]+650x[Nb]+410x[Ti]-80x[Si]-1.4x (t-8) (The unit of Tn in the above Relational Formula 2 is ° C., and [C], [Mn], [Cr], [Nb], [Ti] and [Si] are the weight percentages of the corresponding alloy elements.) (t in the above Relational Formula 2 is the thickness (mm) of the final rolled plate material.) [Relationship 3] CR Min =76.6-157x[C]-25.2x[Si]-14.1x[Mn]-27.3x[Cr]+61x[Ti]+448x[Nb] (CR in the above Relational Formula 3 Min The units are °C / s, and [C], [Si], [Mn], [Cr], [Ti] and [Nb] are the weight percentages of the corresponding alloying elements.)

7. The method for producing a thick steel plate according to claim 6, wherein the reheating is performed in a temperature range of 1200 to 1350°C.

8. The method for producing a thick steel plate according to claim 6, wherein the cooling rate during the primary cooling is 80°C / sec or less.

9. The method for producing a thick steel plate according to claim 6, wherein the secondary cooling is performed by air cooling or water cooling to a temperature range of room temperature to 200°C.

Citation Information

Patent Citations

  • Engineering steel with thickness greater than 26mm and vertical engineering steel greater than or equal to 500MPa and production method thereof

    CN103343300A

  • Production of high tensile strength steel plate having extremely fine structure

    JP1997143570A

  • High formability high tensile hot rolled steel sheet having excellent material uniformity, production method therefor and working method therefor

    JP2002322541A

  • Steel material excellent in fatigue crack propagation property, manufacturing method therefor, and determination method of steel material excellent in fatigue crack propagation property

    JP2015127444A

  • Steel sheet for LPG tank and manufacturing method therefor

    JP2016148105A