Method for manufacturing polarizing plate with pressure-sensitive adhesive layer
The manufacturing method for polarizing plates with controlled alcohol content and storage conditions addresses peeling defects in harsh environments by ensuring uniform crosslinking and adhesion, enhancing durability in high-temperature, high-humidity conditions.
Patent Information
- Application Number
- JP2020189236
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-11-13
AI Technical Summary
Polarizing plates used in harsh environments, such as vehicle-mounted image display devices, experience peeling defects when exposed to changes from high-temperature, high-humidity conditions, which existing methods fail to adequately address.
A manufacturing method for polarizing plates with adhesive layers that involves forming an adhesive layer with a gel fraction of 70% or less, using alcohols like methanol, ethanol, or n-propyl alcohol, and storing the plates in controlled temperature and humidity conditions to ensure alcohol migration and crosslinking agent deactivation, thereby reducing peeling defects.
The method effectively suppresses peeling defects in polarizing plates when exposed to environmental changes from high-temperature, high-humidity conditions by ensuring adequate adhesion and crosslinking density uniformity.
Smart Images

Figure 0007589408000001 
Figure 0007589408000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a polarizing plate with a pressure-sensitive adhesive layer. [Background technology]
[0002] Liquid crystal display devices (LCDs) are widely used not only in liquid crystal televisions, but also in personal computers, mobile devices such as mobile phones, and in-vehicle applications such as car navigation systems. Typically, liquid crystal display devices have liquid crystal panels in which polarizing plates with adhesive layers are attached to both sides of a liquid crystal cell by the adhesive layers, and display is performed by controlling light from a backlight with the liquid crystal panel. In recent years, organic electroluminescence (EL) display devices have also been widely used in televisions, mobile devices such as mobile phones, and in-vehicle applications such as car navigation systems, similar to liquid crystal display devices. In organic EL display devices, a circular polarizing plate (a laminate including a polarizing element and a λ / 4 plate) may be placed on the viewing side surface of the image display panel to prevent external light from being reflected by a metal electrode (cathode) and being viewed as a mirror surface.
[0003] As described above, polarizing plates are increasingly being installed in vehicles as components of image display devices such as liquid crystal display devices and organic electroluminescence display devices. Polarizing plates used in vehicle-mounted image display devices are often exposed to various harsh environments, such as high temperature environments and high temperature and high humidity environments, compared to those used in mobile applications such as televisions and mobile phones. For this reason, it is required that defects such as the polarizing plate with an adhesive layer lifting or peeling off from the liquid crystal cell (hereinafter also referred to as "peeling defects") do not occur even when subjected to severe environmental changes.
[0004] In order to cope with such a severe environment, a technique is known that improves the hue by suppressing the dimensional change of the polarizing plate in a high-temperature environment (for example, Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2013-148806 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, even such a polarizing plate does not sufficiently suppress peeling failure when exposed to an environmental change from a high-temperature and high-humidity environment to a high-temperature environment. The present invention aims to provide a polarizing plate with a pressure-sensitive adhesive layer in which peeling failure is further suppressed even when exposed to an environmental change from a high-temperature and high-humidity environment to a high-temperature environment. [Means for solving the problem]
[0007] The present invention provides a method for producing a polarizing plate with a pressure-sensitive adhesive layer, as exemplified below. [1] Alcohol content is 4μg / cm 2 More than 230μg / cm 2 A step of producing a polarizing plate, A step of producing a polarizing plate with a pressure-sensitive adhesive layer by forming a pressure-sensitive adhesive layer having a gel fraction of 70% or less on one surface of the polarizing plate; and storing the polarizing plate with the pressure-sensitive adhesive layer in an environment having a temperature of 18° C. or higher and 28° C. or lower and a relative humidity of 40% or higher and 70% or lower for 2 days or more. [2] The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to [1], wherein the alcohol is at least one selected from the group consisting of methanol, ethanol, and n-propyl alcohol. [3] The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to [1] or [2], wherein the process for producing the polarizing plate includes a process for bonding a polarizing element obtained by adsorbing and aligning iodine in a polyvinyl alcohol-based resin layer and a transparent protective film with an adhesive layer formed from an adhesive containing alcohol. [4] The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to [3], wherein the adhesive contains a polyvinyl alcohol-based resin. [5] The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to [4], wherein the content of the alcohol in the adhesive is 100 parts by mass or more and 2000 parts by mass or less per 100 parts by mass of the polyvinyl alcohol-based resin. [6] The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to any one of [3] to [5], wherein the adhesive layer has a thickness of 0.01 to 7 μm. Effect of the Invention
[0008] According to the present invention, it is possible to produce a polarizing plate with a pressure-sensitive adhesive layer in which peeling defects are further suppressed even when the environment changes from a high-temperature and high-humidity environment to a high-temperature environment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention will be described, however, the present invention is not limited to the following embodiment.
[0010] [Process for manufacturing polarizing plates] The polarizing plate to be used contains alcohol. The polarizing plate may include a polarizing element having a dichroic dye adsorbed and oriented in a layer containing a polyvinyl alcohol-based resin, and a transparent protective film.
[0011] The amount of alcohol contained in the polarizing plate is 4 μg / cm 2 More than 230μg / cm 2 or less, preferably 13 μg / cm 2 More than 200μg / cm 2 More preferably, it is 20 μg / cm or less. 2 More than 190μg / cm 2 60μg / cm or less 2 It may be more than 100 μg / cm 2 By setting the amount of alcohol contained in the polarizing plate in this range, it is possible to ensure a sufficient amount of alcohol migration to the adhesive layer in a later step without impairing the characteristics of the polarizing element. It is desirable that the amount of alcohol contained in the polarizing plate be within the above range even immediately before the "step of storing the polarizing plate with the adhesive layer" described below.
[0012] <Polarizing element> A well-known polarizing element can be used as the polarizing element in which a dichroic dye is adsorbed and aligned in a layer containing a polyvinyl alcohol (hereinafter also referred to as "PVA")-based resin (hereinafter also referred to as a "PVA-based resin layer"). Examples of the polarizing element include a stretched film obtained by dyeing a PVA-based resin film with a dichroic dye and uniaxially stretching it, and a stretched layer obtained by using a laminated film having a coating layer formed by applying a coating liquid containing a PVA-based resin onto a base film, dyeing the coating layer with a dichroic dye, and uniaxially stretching the laminated film. The stretching may be performed after dyeing with the dichroic dye, may be performed while dyeing, or may be performed after stretching and dyeing.
[0013] PVA resins are obtained by saponifying polyvinyl acetate resins. Examples of polyvinyl acetate resins include polyvinyl acetate, which is a homopolymer of vinyl acetate, and copolymers of vinyl acetate with other monomers that can be copolymerized with it. Examples of other copolymerizable monomers include unsaturated carboxylic acids, olefins such as ethylene, vinyl ethers, and unsaturated sulfonic acids.
[0014] The saponification degree of the PVA resin is preferably about 85 mol% or more, more preferably about 90 mol% or more, and even more preferably about 99 mol% or more and 100 mol% or less. The polymerization degree of the PVA resin is, for example, 1000 to 10000, preferably 1500 to 5000. The PVA resin may be modified, and may be, for example, polyvinyl formal, polyvinyl acetal, polyvinyl butyral, etc., modified with aldehydes.
[0015] The thickness of the polarizing element is preferably 3 μm or more and 35 μm or less, more preferably 4 μm or more and 30 μm or less, and even more preferably 5 μm or more and 25 μm or less. By making the thickness of the polarizing element 35 μm or less, the influence of the polyenation of the PVA resin on the deterioration of optical properties in a high temperature environment can be suppressed. By making the thickness of the polarizing element 3 μm or more, it becomes easy to make a configuration that achieves the desired optical properties.
[0016] The polarizing element preferably contains alcohol. In this embodiment, a step of bonding the polarizing element and the transparent protective film with an adhesive layer formed from an adhesive containing alcohol can be included. Therefore, it is presumed that a part of the alcohol migrates from the adhesive layer and is included in the polarizing element. The alcohol in the polarizing element may include alcohol added during the manufacturing process of the polarizing element.
[0017] (alcohol) Examples of the alcohol used in the present invention include lower alcohols having 1 to 4 carbon atoms. Specific examples include methanol, ethanol, n-propyl alcohol, isopropyl alcohol, and tert-butyl alcohol. The alcohol that may be contained in the polarizing plate or adhesive (or adhesive layer) preferably includes at least one selected from the group consisting of methanol, ethanol, n-propyl alcohol, isopropyl alcohol, and tert-butyl alcohol. These may be used alone or in combination of two or more. Preferably, at least one selected from the group consisting of methanol, ethanol, n-propyl alcohol, and isopropyl alcohol may be included. These are preferred because they have low molecular weights and can be efficiently transferred from the polarizing plate to the adhesive layer.
[0018] The method of making the polarizing element contain alcohol includes a method of immersing the PVA-based resin layer in a treatment solvent containing alcohol, or a method of spraying, flowing or dropping the treatment solvent onto the PVA-based resin layer. Among these, the method of immersing the PVA-based resin layer in a treatment solvent containing alcohol is preferably used.
[0019] The process of immersing the PVA-based resin layer in a treatment solvent containing alcohol may be performed simultaneously with the processes of swelling, stretching, dyeing, crosslinking, washing, etc. in the manufacturing method of a polarizing element described later, or may be provided separately from these processes. The process of making the PVA-based resin layer contain alcohol is preferably performed after dyeing the PVA-based resin layer with iodine, and more preferably performed simultaneously with the washing process. According to such a method, the change in hue is small, and the influence on the optical properties of the polarizing element can be reduced.
[0020] In order to incorporate alcohol into the polarizing element, the alcohol may be added both during the production of the polarizing element and to the adhesive.
[0021] (Urea compounds) The polarizing element may further include a urea-based compound. A polarizing element including a urea-based compound can further suppress the decrease in transmittance. The urea-based compound may be the same as the urea-based compound that can be included in the adhesive described later. The method for incorporating the urea-based compound in the polarizing element can be the same as the method for incorporating alcohol in the polarizing element. The urea-based compound may be included in the manufacturing process of the polarizing element, or it can be included in the polarizing element by being included in the adhesive for laminating the polarizing element and the transparent protective film described later.
[0022] (Dicarboxylic acid) The polarizing element may further include a dicarboxylic acid. A polarizing element including a dicarboxylic acid can further suppress the decrease in transmittance. The dicarboxylic acid may be the same as the dicarboxylic acid that can be included in the adhesive described later. The method for incorporating the dicarboxylic acid into the polarizing element can be the same as the method for incorporating an alcohol into the polarizing element. The dicarboxylic acid may be incorporated during the manufacturing process of the polarizing element, or it can be incorporated into the polarizing element by being incorporated into the adhesive for laminating the polarizing element and the transparent protective film described later.
[0023] (Method of manufacturing polarizing element) The method for producing the polarizing element is not particularly limited, but typical methods include a method in which a PVA-based resin film that has already been wound into a roll is sent out and stretched, dyed, crosslinked, and the like to produce the polarizing element (hereinafter referred to as "production method 1"), and a method including a step of applying a coating liquid containing a PVA-based resin onto a substrate film to form a PVA-based resin layer as a coating layer, and stretching the resulting laminate (hereinafter referred to as "production method 2").
[0024] Production method 1 can include a step of uniaxially stretching a PVA-based resin film, a step of dyeing the PVA-based resin film with a dichroic dye such as iodine to adsorb the dichroic dye, a step of treating the PVA-based resin film with the adsorbed dichroic dye with an aqueous boric acid solution, and a step of washing with water after the treatment with the aqueous boric acid solution.
[0025] The swelling step is a treatment step in which the PVA-based resin film is immersed in a swelling bath. The swelling step can remove dirt and blocking agents on the surface of the PVA-based resin film, and can also suppress uneven dyeing by swelling the PVA-based resin film. A medium mainly composed of water, such as water, distilled water, or pure water, is usually used for the swelling bath. The swelling bath may contain surfactants, alcohol, or the like, as appropriate, according to a conventional method. In order to control the potassium content of the polarizing element, potassium iodide may be used in the swelling bath. In this case, the concentration of potassium iodide in the swelling bath is preferably 1.5% by mass or less, more preferably 1.0% by mass or less, and even more preferably 0.5% by mass or less.
[0026] The temperature of the swelling bath is preferably about 10° C. to about 60° C., more preferably about 15° C. to about 45° C., and even more preferably about 18° C. to about 30° C. The immersion time in the swelling bath cannot be determined in general because the degree of swelling of the PVA-based resin film is affected by the temperature of the swelling bath, but is preferably about 5 seconds to about 300 seconds, more preferably about 10 seconds to about 200 seconds, and even more preferably about 20 seconds to about 100 seconds. The swelling step may be carried out only once, or may be carried out multiple times as necessary.
[0027] The dyeing process is a treatment process in which the PVA-based resin film is immersed in a dye bath (iodine solution), and a dichroic dye such as iodine can be adsorbed and oriented on the PVA-based resin film. The iodine solution is usually preferably an aqueous iodine solution, and contains iodine and an iodide as a dissolving agent. Examples of iodides include potassium iodide, lithium iodide, sodium iodide, zinc iodide, aluminum iodide, lead iodide, copper iodide, barium iodide, calcium iodide, tin iodide, and titanium iodide. Among these, potassium iodide is preferred from the viewpoint of controlling the potassium content in the polarizing element.
[0028] The concentration of iodine in the dye bath is preferably about 0.01% by mass to about 1% by mass, more preferably about 0.02% by mass to about 0.5% by mass, and the concentration of iodide in the dye bath is preferably about 0.01% by mass to about 10% by mass, more preferably about 0.05% by mass to about 5% by mass, and even more preferably about 0.1% by mass to about 3% by mass.
[0029] The temperature of the dye bath is preferably about 10° C. to 50° C., more preferably about 15° C. to 45° C., and even more preferably about 18° C. to 30° C. The immersion time in the dye bath cannot be determined in general because the degree of dyeing of the PVA-based resin film is affected by the temperature of the dye bath, but is preferably about 10 seconds to 300 seconds, and more preferably about 20 seconds to 240 seconds. The dyeing process may be carried out only once, or may be carried out multiple times as necessary.
[0030] The crosslinking step is a treatment step in which the PVA-based resin film dyed in the dyeing step is immersed in a treatment bath (crosslinking bath) containing a boron compound, and the boron compound crosslinks the polyvinyl alcohol-based resin film, allowing iodine molecules or dye molecules to be adsorbed to the crosslinked structure. Examples of the boron compound include boric acid, borate salts, and borax. The crosslinking bath is generally an aqueous solution, but may also be a mixed solution of water and an organic solvent miscible with water. The crosslinking bath preferably contains potassium iodide from the viewpoint of controlling the potassium content in the polarizing element.
[0031] In the crosslinking bath, the concentration of the boron compound is preferably about 1% by mass to about 15% by mass, more preferably about 1.5% by mass to about 10% by mass, and more preferably about 2% by mass to about 5% by mass. When potassium iodide is used in the crosslinking bath, the concentration of potassium iodide in the crosslinking bath is preferably about 1% by mass to about 15% by mass, more preferably about 1.5% by mass to about 10% by mass, and more preferably about 2% by mass to about 5% by mass.
[0032] The temperature of the crosslinking bath is preferably about 20° C. to about 70° C., more preferably about 30° C. to about 60° C. The immersion time in the crosslinking bath cannot be determined in general because the degree of crosslinking of the PVA resin film is affected by the temperature of the crosslinking bath, but is preferably about 5 seconds to about 300 seconds, more preferably about 10 seconds to about 200 seconds. The crosslinking step may be carried out only once, or may be carried out multiple times as necessary.
[0033] The stretching process is a process for stretching the PVA-based resin film at least in one direction to a predetermined magnification. In general, the PVA-based resin film is uniaxially stretched in the conveying direction (longitudinal direction). There are no particular limitations on the stretching method, and either a wet stretching method or a dry stretching method can be used. The stretching process may be carried out only once, or may be carried out multiple times as necessary. The stretching process may be carried out at any stage in the production of a polarizing element.
[0034] The treatment bath (stretching bath) in the wet stretching method can usually use a solvent such as water or a mixed solution of water and an organic solvent miscible with water. The stretching bath preferably contains potassium iodide from the viewpoint of controlling the content of potassium in the polarizing element. When potassium iodide is used in the stretching bath, the concentration of potassium iodide in the stretching bath is preferably about 1% by mass to 15% by mass, more preferably about 2% by mass to 10% by mass, and more preferably about 3% by mass to 6% by mass. The treatment bath (stretching bath) can contain a boron compound from the viewpoint of suppressing film breakage during stretching. When a boron compound is contained, the concentration of the boron compound in the stretching bath is preferably about 1% by mass to 15% by mass, more preferably about 1.5% by mass to 10% by mass, and more preferably about 2% by mass to 5% by mass.
[0035] The temperature of the stretching bath is preferably about 25° C. to about 80° C., more preferably about 40° C. to about 75° C., and even more preferably about 50° C. to about 70° C. The immersion time in the stretching bath cannot be determined in general because the degree of stretching of the PVA-based resin film is affected by the temperature of the stretching bath, but is preferably about 10 seconds to about 800 seconds, and more preferably about 30 seconds to about 500 seconds. The stretching treatment in the wet stretching method may be performed together with one or more treatment steps of a swelling step, a dyeing step, a crosslinking step, and a washing step.
[0036] Examples of the dry stretching method include a roll-to-roll stretching method, a heated roll stretching method, a compression stretching method, etc. The dry stretching method may be carried out together with a drying step.
[0037] The total stretching ratio (cumulative stretching ratio) applied to the polyvinyl alcohol-based resin film can be appropriately set depending on the purpose, but is preferably about 2 to 7 times, more preferably about 3 to 6.8 times, and even more preferably about 3.5 to 6.5 times.
[0038] The cleaning step is a treatment step in which the polyvinyl alcohol-based resin film is immersed in a cleaning bath, and foreign matter remaining on the surface of the polyvinyl alcohol-based resin film can be removed. The cleaning bath is usually made of a medium mainly composed of water, such as water, distilled water, or pure water. In addition, from the viewpoint of controlling the potassium content in the polarizing element, it is preferable to use potassium iodide in the cleaning bath. In this case, the concentration of potassium iodide in the cleaning bath is preferably about 1% by mass or more and 10% by mass or less, more preferably about 1.5% by mass or more and 4% by mass or less, and even more preferably about 1.8% by mass or more and 3.8% by mass or less.
[0039] The temperature of the cleaning bath is preferably about 5° C. to about 50° C., more preferably about 10° C. to about 40° C., and even more preferably about 15° C. to about 30° C. The immersion time in the cleaning bath cannot be determined in general because the degree of cleaning of the PVA-based resin film is affected by the temperature of the cleaning bath, but is preferably about 1 second to about 100 seconds, more preferably about 2 seconds to about 50 seconds, and even more preferably about 3 seconds to about 20 seconds. The cleaning step may be carried out only once, or may be carried out multiple times as necessary.
[0040] The drying step is a step of drying the PVA-based resin film washed in the washing step to obtain a polarizing element. The drying can be performed by any appropriate method, for example, natural drying, air drying, or heat drying.
[0041] The manufacturing method 2 can be produced through the steps of applying a coating solution containing a PVA resin onto a substrate film, uniaxially stretching the resulting laminated film, dyeing the PVA resin layer of the uniaxially stretched laminated film with a dichroic dye to adsorb it to form a polarizing element, treating the film with the adsorbed dichroic dye with an aqueous boric acid solution, and washing with water after the treatment with the aqueous boric acid solution. The substrate film used to form the polarizing element may be used as a protective layer for the polarizing element. If necessary, the substrate film may be peeled off and removed from the polarizing element.
[0042] <Transparent protective film> The transparent protective film (hereinafter, simply referred to as "protective film") used in this embodiment is attached to at least one surface of the polarizing element via an adhesive layer. This transparent protective film is attached to one or both surfaces of the polarizing element, but is preferably attached to both surfaces.
[0043] The protective film may have other optical functions at the same time, and may be formed into a laminated structure in which multiple layers are laminated. The thickness of the protective film is preferably thin from the viewpoint of optical properties, but if it is too thin, the strength decreases and the processability is poor. The appropriate thickness is 5 μm or more and 100 μm or less, preferably 10 μm or more and 80 μm or less, and more preferably 15 μm or more and 70 μm or less.
[0044] The protective film may be a cellulose acylate film, a film made of a polycarbonate resin, a film made of a cycloolefin resin such as norbornene, a (meth)acrylic polymer film, a polyester resin film such as polyethylene terephthalate, etc. When a protective film is attached to both sides of a polarizing element using a water-based adhesive such as a PVA adhesive, it is preferable that the protective film on at least one side is either a cellulose acylate film or a (meth)acrylic polymer film in terms of moisture permeability, and among these, a cellulose acylate film is preferable.
[0045] At least one of the protective films may have a retardation function for the purpose of compensating for a viewing angle. In that case, the protective film itself may have a retardation function, may have a separate retardation layer, or may be a combination of both. The film having a retardation function may be directly attached to the polarizing element via an adhesive, or may be attached via a pressure-sensitive adhesive or adhesive via another protective film attached to the polarizing element.
[0046] <Adhesive layer> It is preferable to use an adhesive containing alcohol as the adhesive constituting the adhesive layer for bonding the protective film to the polarizing element. The adhesive can be a water-based adhesive, a solvent-based adhesive, an active energy ray curing adhesive, etc., but it is preferable to use a water-based adhesive from the viewpoint of containing alcohol, and it is preferable to contain a PVA-based resin. By using an adhesive containing alcohol, it is also possible to suppress the decrease in transmittance of the polarizing plate in a high temperature environment.
[0047] The thickness of the adhesive when applied can be set to any value, for example, so that an adhesive layer having a desired thickness is obtained after curing or heating (drying). The thickness of the adhesive layer made of the adhesive is preferably 0.01 μm or more and 7 μm or less, more preferably 0.01 μm or more and 5 μm or less, even more preferably 0.01 μm or more and 2 μm or less, and most preferably 0.01 μm or more and 1 μm or less.
[0048] The following description of the adhesive is a description of the preferred range in the case where alcohol is not contained in the polarizing element during the production of the polarizing element. When alcohol is contained in the polarizing element, the following values may be adjusted appropriately. Specific examples of the alcohol may be the same as those contained in the polarizing element described above. In the process of forming an adhesive layer through a drying process when adhering the polarizing element and the protective film, it is acceptable if part of the alcohol migrates from the adhesive layer to the polarizing element, etc.
[0049] In the case where the adhesive is an aqueous adhesive containing a PVA-based resin, the alcohol content in the adhesive is preferably 30 parts by mass or more and 2000 parts by mass or less, more preferably 100 parts by mass or more and 2000 parts by mass or less, even more preferably 500 parts by mass or more and 1800 parts by mass or less, and most preferably 800 parts by mass or more and 1500 parts by mass or less, relative to 100 parts by mass of the PVA-based resin. If the alcohol content is less than 30 parts by mass, the peeling suppression effect in the change from a high-temperature and high-humidity environment to a high-temperature environment may not be sufficiently obtained. On the other hand, if the alcohol content exceeds 2000 parts by mass, the hue may deteriorate. By setting the alcohol content in the adhesive within the above range, the drying efficiency can be increased in the drying process after laminating the protective film on the polarizing element via the adhesive, and it becomes easy to adjust the alcohol content in the polarizing plate to a desired amount.
[0050] In a configuration in which a transparent protective film is bonded to both sides of a polarizing element via an adhesive layer, of the adhesive layers on both sides of the polarizing element, only the adhesive layer on one side may be a layer containing alcohol, but it is preferable that the adhesive layers on both sides are layers containing alcohol.
[0051] In order to meet the demand for thinner polarizing plates, polarizing plates having a transparent protective film only on one side of a polarizing element have been developed. In this configuration, the transparent protective film is also laminated via an adhesive layer containing alcohol. As a method for producing a polarizing plate having a transparent protective film only on one side of such a polarizing element, a method is considered in which a polarizing plate having a transparent protective film attached to both sides via an adhesive layer is first produced, and then one of the transparent protective films is peeled off. When such a production method is used, only one of the adhesive layers may contain alcohol, but it is preferable that both adhesive layers on both sides are layers containing alcohol. When an adhesive layer containing alcohol is used on only one side of a polarizing element, it is preferable that the adhesive layer on the film side that is not peeled off contains alcohol.
[0052] (Water-based adhesive) As the aqueous adhesive, any suitable aqueous adhesive may be used, but preferably, an aqueous adhesive containing a PVA resin (PVA adhesive) is used. From the viewpoint of adhesiveness, the average polymerization degree of the PVA resin contained in the aqueous adhesive is preferably about 100 to 5500, more preferably 1000 to 4500. From the viewpoint of adhesiveness, the average saponification degree is preferably about 85 mol% to 100 mol%, more preferably 90 mol% to 100 mol%.
[0053] The PVA resin contained in the aqueous adhesive is preferably one containing an acetoacetyl group, because it has excellent adhesion between the PVA resin layer and the protective film and excellent durability. The acetoacetyl group-containing PVA resin can be obtained, for example, by reacting a PVA resin with diketene by any method. The acetoacetyl group modification degree of the acetoacetyl group-containing PVA resin is typically 0.1 mol% or more, preferably about 0.1 mol% or more and 20 mol% or less. The resin concentration of the aqueous adhesive is preferably 0.1 mass% or more and 15 mass% or less, more preferably 0.5 mass% or more and 10 mass% or less.
[0054] The water-based adhesive may contain a crosslinking agent. Known crosslinking agents may be used as the crosslinking agent. Examples of the crosslinking agent include water-soluble epoxy compounds, dialdehydes, and isocyanates.
[0055] When the PVA-based resin is an acetoacetyl group-containing PVA-based resin, the crosslinking agent is preferably any one of glyoxal, glyoxylate, and methylolmelamine, more preferably any one of glyoxal and glyoxylate, and particularly preferably glyoxal.
[0056] (Active energy ray curing adhesive) The active energy ray curable adhesive is an adhesive that is cured by irradiation with active energy rays such as ultraviolet rays, and examples thereof include an adhesive containing a polymerizable compound and a photopolymerization initiator, an adhesive containing a photoreactive resin, and an adhesive containing a binder resin and a photoreactive crosslinking agent. Examples of the polymerizable compound include photopolymerizable monomers such as photocurable epoxy monomers, photocurable acrylic monomers, and photocurable urethane monomers, and oligomers derived from these monomers. Examples of the photopolymerization initiator include compounds containing a substance that generates active species such as neutral radicals, anion radicals, and cation radicals when irradiated with active energy rays such as ultraviolet rays.
[0057] (Urea compounds) The adhesive may further contain at least one urea-based compound selected from urea, urea derivatives, thiourea, and thiourea derivatives. The adhesive layer made of the adhesive contains a urea-based compound, which can further improve high-temperature durability. In the process of forming the adhesive layer through a drying process when adhering the adhesive to the protective film, a part of the urea-based compound may migrate from the adhesive layer to the polarizing element or the like. Urea-based compounds include water-soluble and poorly water-soluble compounds, and both types of urea-based compounds can be used. When a poorly water-soluble urea-based compound is used in a water-soluble adhesive, it is preferable to devise a dispersion method so that haze increase or the like does not occur after the adhesive layer is formed.
[0058] When the adhesive is an aqueous adhesive containing a PVA-based resin, the amount of the urea-based compound added is preferably 0.1 parts by mass or more and 400 parts by mass or less, more preferably 1 part by mass or more and 200 parts by mass or less, and even more preferably 3 parts by mass or more and 100 parts by mass or less, relative to 100 parts by mass of PVA.
[0059] (urea derivative) The urea derivative is a compound in which at least one of the four hydrogen atoms of the urea molecule is substituted with a substituent. In this case, the substituent is not particularly limited, but is preferably a substituent consisting of a carbon atom, a hydrogen atom, and an oxygen atom. Some urea derivatives have low solubility in water, but have sufficient solubility in alcohol. In this case, one of the preferred embodiments is to dissolve a urea compound in alcohol to prepare an alcohol solution of the urea compound, and then add the alcohol solution of the urea compound to an aqueous PVA solution to prepare the adhesive.
[0060] Specific examples of urea derivatives include mono-substituted ureas such as methylurea, ethylurea, propylurea, butylurea, isobutylurea, N-octadecylurea, 2-hydroxyethylurea, hydroxyurea, acetylurea, allylurea, 2-propynylurea, cyclohexylurea, phenylurea, 3-hydroxyphenylurea, (4-methoxyphenyl)urea, benzylurea, benzoylurea, o-tolylurea, and p-tolylurea. Examples of 2-substituted ureas include 1,1-dimethylurea, 1,3-dimethylurea, 1,1-diethylurea, 1,3-diethylurea, 1,3-bis(hydroxymethyl)urea, 1,3-tert-butylurea, 1,3-dicyclohexylurea, 1,3-diphenylurea, 1,3-bis(4-methoxyphenyl)urea, 1-acetyl-3-methylurea, 2-imidazolidinone (ethyleneurea), and tetrahydro-2-pyrimidinone (propyleneurea). Examples of 4-substituted ureas include tetramethylurea, 1,1,3,3-tetraethylurea, 1,1,3,3-tetrabutylurea, 1,3-dimethoxy-1,3-dimethylurea, 1,3-dimethyl-2-imidazolidinone, and 1,3-dimethyl-3,4,5,6-tetrahydro-2(1H)-pyrimidinone.
[0061] (Thiourea derivatives) A thiourea derivative is a compound in which at least one of the four hydrogen atoms of a thiourea molecule is substituted with a substituent. In this case, the substituent is not particularly limited, but is preferably a substituent consisting of a carbon atom, a hydrogen atom, and an oxygen atom.
[0062] Specific examples of thiourea derivatives include mono-substituted thioureas such as N-methylthiourea, ethylthiourea, propylthiourea, isopropylthiourea, 1-butylthiourea, cyclohexylthiourea, N-acetylthiourea, N-allylthiourea, (2-methoxyethyl)thiourea, N-phenylthiourea, (4-methoxyphenyl)thiourea, N-(2-methoxyphenyl)thiourea, N-(1-naphthyl)thiourea, (2-pyridyl)thiourea, o-tolylthiourea, and p-tolylthiourea. Examples of 2-substituted thioureas include 1,1-dimethylthiourea, 1,3-dimethylthiourea, 1,1-diethylthiourea, 1,3-diethylthiourea, 1,3-dibutylthiourea, 1,3-diisopropylthiourea, 1,3-dicyclohexylthiourea, N,N-diphenylthiourea, N,N'-diphenylthiourea, 1,3-di(o-tolyl)thiourea, 1,3-di(p-tolyl)thiourea, 1-benzyl-3-phenylthiourea, 1-methyl-3-phenylthiourea, N-allyl-N'-(2-hydroxyethyl)thiourea, and ethylenethiourea. Examples of 3-substituted thioureas include trimethylthiourea. Examples of 4-substituted thioureas include tetramethylthiourea and 1,1,3,3-tetraethylthiourea.
[0063] Among the urea-based compounds, urea derivatives or thiourea derivatives are preferred, and urea derivatives are more preferred, in that they can further suppress the decrease in transmittance in a high-temperature environment when used in an image display device having an interlayer filling configuration. Among the urea derivatives, mono- or di-substituted ureas are preferred, and mono-substituted ureas are more preferred. Di-substituted ureas include 1,1-substituted ureas and 1,3-substituted ureas, and 1,3-substituted ureas are more preferred.
[0064] (Dicarboxylic acid) The adhesive may further contain a dicarboxylic acid. By using an adhesive containing a dicarboxylic acid, the decrease in transmittance of the polarizing plate in a high temperature environment can be suppressed. Examples of dicarboxylic acids include oxalic acid, malonic acid, succinic acid, glutaric acid, adipic acid, pimelic acid, suberic acid, azelaic acid, sebacic acid, phthalic acid, isophthalic acid, terephthalic acid, tartaric acid, glutamic acid, malic acid, maleic acid, fumaric acid, itaconic acid, muconic acid, 1,4-cyclohexanedicarboxylic acid, 1,4-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, 2,7-naphthalenedicarboxylic acid, 4,4-biphenyldicarboxylic acid, 2,5-pyridinedicarboxylic acid, 3,5-pyridinedicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenylmethanedicarboxylic acid, oxaloacetic acid, methylfumaric acid, and 2,6-pyridinedicarboxylic acid. Among these, it is preferable to use citric acid, malic acid, maleic acid, or tartaric acid. These dicarboxylic acids can be used alone or in combination of two or more.
[0065] [Method of manufacturing polarizing plate] The method for producing a polarizing plate is not particularly limited, but may include, for example, a step of laminating a first transparent protective film, a polarizing element, and a second transparent protective film by providing an adhesive layer between each layer, and then adhering them to each other through a drying step. At least one adhesive layer is preferably an alcohol-containing adhesive. The step of producing a polarizing plate preferably includes a step of bonding a polarizing element formed by adsorbing and orienting iodine in a polyvinyl alcohol-based resin layer and a transparent protective film with an adhesive layer formed from an alcohol-containing adhesive. In addition, a peelable surface protective film may be laminated on at least one side of the produced polarizing plate to protect the surface. In addition, when surface protective films are laminated on both sides of the polarizing plate, the surface protective film on the adhesive forming side may be peeled off before forming the adhesive in the next step.
[0066] [Process for producing a polarizing plate with an adhesive layer] Next, a step of forming a pressure-sensitive adhesive layer on the produced polarizing plate is carried out. The pressure-sensitive adhesive layer used has a gel fraction of 70% or less.
[0067] <Adhesive layer> The adhesive layer may be composed of one layer or two or more layers, but is preferably composed of one layer. The adhesive layer may be composed of an adhesive composition mainly composed of (meth)acrylic resin, rubber resin, urethane resin, ester resin, silicone resin, or polyvinyl ether resin. Among them, an adhesive composition having a (meth)acrylic resin as a base polymer, which is excellent in transparency, weather resistance, heat resistance, etc., is preferable. The adhesive composition may be of an active energy ray curing type or a heat curing type.
[0068] As the (meth)acrylic resin (base polymer) used in the pressure-sensitive adhesive composition, a polymer or copolymer containing one or more monomers of (meth)acrylic acid esters such as butyl (meth)acrylate, ethyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, etc. is preferably used. A polar monomer is preferably copolymerized in the base polymer. Examples of the polar monomer include monomers having a carboxyl group, a hydroxyl group, an amide group, an amino group, an epoxy group, etc., such as a (meth)acrylic acid compound, a 2-hydroxypropyl (meth)acrylate compound, a hydroxyethyl (meth)acrylate compound, a (meth)acrylamide compound, an N,N-dimethylaminoethyl (meth)acrylate compound, and a glycidyl (meth)acrylate compound.
[0069] The adhesive composition may contain only the base polymer, but usually further contains a crosslinking agent. Examples of the crosslinking agent include a divalent or higher metal ion that forms a carboxylate metal salt with a carboxyl group, a polyamine compound that forms an amide bond with a carboxyl group, a polyepoxy compound or polyol that forms an ester bond with a carboxyl group, and a polyisocyanate compound that forms an amide bond with a carboxyl group. Among them, a polyisocyanate compound is preferred.
[0070] Examples of the polyisocyanate compound include polyisocyanate compounds, trimers of polyisocyanate compounds, urethane prepolymers having isocyanate groups at their terminals obtained by reacting a polyisocyanate compound with a polyol compound, trimers of the urethane prepolymers, etc. Examples of the polyisocyanate compound include 2,4-tolylene diisocyanate, 2,5-tolylene diisocyanate, 1,3-xylylene diisocyanate, 1,4-xylylene diisocyanate, diphenylmethane-4,4'-diisocyanate, 3-methyldiphenylmethane diisocyanate, hexamethylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane-4,4'-diisocyanate, dicyclohexylmethane-2,4'-diisocyanate, and lysine isocyanate.
[0071] The polyisocyanate compound may be used alone or in combination of two or more, but the total content is preferably 0.01 to 2 parts by weight, more preferably 0.02 to 2 parts by weight, and even more preferably 0.05 to 1.5 parts by weight, per 100 parts by weight of the base polymer. The polyisocyanate compound may be appropriately contained in consideration of the cohesive strength, prevention of peeling in durability tests, and the like.
[0072] As commercially available isocyanate compounds, for example, L45 (manufactured by Soken Chemical Engineering Co., Ltd.), TD75 (manufactured by Soken Chemical Engineering Co., Ltd.), BXX5627 (manufactured by Toyochem Co., Ltd.), X-301-422SK (manufactured by Saiden Chemical Engineering Co., Ltd.), and Coronate L (manufactured by Tosoh Corporation) can be suitably used.
[0073] The active energy ray curable adhesive composition has a property of being cured by irradiation with active energy rays such as ultraviolet rays and electron beams, and has a property of being able to adhere to an adherend such as a film even before irradiation with active energy rays, and is able to adjust the adhesive strength by being cured by irradiation with active energy rays. The active energy ray curable adhesive composition is preferably an ultraviolet ray curable type. The active energy ray curable adhesive composition further contains an active energy ray polymerizable compound in addition to a base polymer and a crosslinking agent. If necessary, a photopolymerization initiator, a photosensitizer, etc. may be contained.
[0074] The pressure-sensitive adhesive composition can contain additives such as microparticles for imparting light scattering properties, beads (resin beads, glass beads, etc.), glass fibers, resins other than the base polymer, tackifiers, fillers (metal powders and other inorganic powders, etc.), antioxidants, UV absorbers, dyes, pigments, colorants, defoamers, corrosion inhibitors, and photopolymerization initiators.
[0075] The adhesive layer can be formed by applying the organic solvent dilution of the adhesive composition on the surface of a substrate film or a polarizing plate and drying it.The substrate film is generally a thermoplastic resin film, and a typical example thereof is a separate film that has been subjected to a release treatment.The separate film can be, for example, a film made of a resin such as polyethylene terephthalate, polybutylene terephthalate, polycarbonate, or polyarene, and the surface on which the adhesive layer is formed is subjected to a release treatment such as silicone treatment.
[0076] The process for producing a polarizing plate with a pressure-sensitive adhesive layer may include a process for directly applying a pressure-sensitive adhesive composition to a release-treated surface of a separate film to form a pressure-sensitive adhesive layer, and laminating the pressure-sensitive adhesive layer with a separate film on the surface of the polarizing plate via the pressure-sensitive adhesive layer. The process for producing a polarizing plate with a pressure-sensitive adhesive layer may include a process for directly applying a pressure-sensitive adhesive composition to a surface of a polarizing plate to form a pressure-sensitive adhesive layer, and laminating a separate film on the outer surface of the pressure-sensitive adhesive layer.
[0077] When providing the pressure-sensitive adhesive layer on the surface of the polarizing plate, it is preferable to subject the bonding surface of the polarizing plate and / or the bonding surface of the pressure-sensitive adhesive layer to a surface activation treatment such as plasma treatment or corona treatment, and it is more preferable to subject the layer to corona treatment.
[0078] Alternatively, a pressure-sensitive adhesive composition may be applied onto a second separate film to form a pressure-sensitive adhesive layer, a separate film may be laminated onto the formed pressure-sensitive adhesive layer to prepare a pressure-sensitive adhesive sheet, and the pressure-sensitive adhesive layer with the separate film after peeling the second separate film from the pressure-sensitive adhesive sheet may be laminated onto a polarizing plate. The second separate film used has a weaker adhesion to the pressure-sensitive adhesive layer than the separate film and is therefore easier to peel off.
[0079] The thickness of the pressure-sensitive adhesive layer is not particularly limited, but is, for example, preferably from 1 μm to 100 μm, more preferably from 3 μm to 50 μm, and may be 20 μm or more.
[0080] The adhesive layer used in the process of producing a polarizing plate with an adhesive layer has a gel fraction in a predetermined range. It is considered that the larger the gel fraction of the adhesive layer, the more crosslinking reaction has progressed in the adhesive layer, and it can be used as a guide for crosslink density. The gel fraction of the adhesive layer is 70% or less, preferably 50% or less, and more preferably 30% or less. Most preferably, the gel fraction is substantially 0%. The gel fraction being substantially 0% means that the gel fraction is 5% or less. If the gel fraction exceeds 70%, the peeling suppression effect may become insufficient when exposed to an environmental change from a high-temperature and high-humidity environment to a high-temperature environment. It is desirable that the gel fraction of the adhesive layer is in the above range even immediately before the "process of storing the polarizing plate with an adhesive layer" described later.
[0081] The method for obtaining a pressure-sensitive adhesive layer having a gel fraction in a predetermined range is not particularly limited, and a known method can be applied. Specifically, a pressure-sensitive adhesive layer having a desired gel fraction can be obtained by adjusting the drying temperature and drying time of the pressure-sensitive adhesive. As detailed conditions, for example, when the drying temperature is 70°C or higher and lower than 100°C, a desired pressure-sensitive adhesive layer can be obtained by setting the drying time to 30 seconds or more and 5 minutes or less. The gel fraction of the pressure-sensitive adhesive layer immediately after the preparation in this manner is substantially 0%, and it is most preferable to laminate the pressure-sensitive adhesive layer immediately after the preparation on a polarizing plate.
[0082] [Process for storing polarizing plate with adhesive layer] The produced polarizing plate with the adhesive layer is stored for 2 days or more in an environment where the temperature is 18° C. or more and 28° C. or less and the relative humidity is 40% or more and 70% or less. When the polarizing plate with the adhesive layer is a long plate produced continuously by roll-to-roll, it may be stored in the state of being wound up on a roll.
[0083] The storage temperature is preferably 20° C. or higher and 26° C. or lower. The storage humidity is preferably 50% or higher and 60% or lower. The storage period is preferably 3 days or longer, more preferably 5 days or longer, and most preferably 7 days or longer. The upper limit of the storage period is not particularly limited, but can be, for example, 365 days or shorter.
[0084] Although the details of the mechanism by which the polarizing plate with the adhesive layer manufactured by the manufacturing method of the present invention can suppress the peeling failure even when it is exposed to an environmental change from a high-temperature and high-humidity environment to a high-temperature environment are unclear, it is presumed as follows. In general, the adhesive layer is stored for at least two days until the crosslinking reaction stabilizes in an environment of, for example, a temperature of 23°C and a relative humidity of 55%. During this time, it is presumed that the crosslinking reaction proceeds uniformly in the thickness direction in the adhesive layer. However, the polarizing plate used in the manufacturing method of the present invention contains a predetermined amount of alcohol, and is subjected to a storage process after the adhesive layer is formed on the polarizing plate. It is presumed that alcohol migrates from the polarizing plate to the adhesive layer during such storage. As a result, it is presumed that alcohol is present in the adhesive layer in the thickness direction closer to the polarizing plate. The migrated alcohol reacts with the crosslinking agent to deactivate the crosslinking agent, and the crosslinking reaction can be suppressed. It is presumed that the adhesive layer after being stored in this way has a low crosslinking density near the polarizing plate in the thickness direction, and the crosslinking density increases as it moves away from the polarizing plate. Since the storage modulus of the pressure-sensitive adhesive layer is low near the polarizing plate and increases as it moves away from the polarizing plate, on the one hand, it can relieve the stress caused by the dimensional change of the polarizing plate, and on the other hand, it can ensure sufficient adhesion to the display device to which the polarizing plate is attached. Therefore, it is presumed that peeling failure can be suppressed even when the pressure-sensitive adhesive layer is exposed to an environmental change from a high temperature and high humidity environment to a high temperature environment.
[0085] The gel fraction of the adhesive layer at the time of use in a display device (which may be the time of completion of the process of storing the polarizing plate with the adhesive layer) is 60% or more, preferably 70% or more, and most preferably 80% or more. If the gel fraction is less than 60%, peeling is likely to occur in a high-temperature environment. The gel fraction can usually be less than 100%.
[0086] Therefore, if the gel fraction of the adhesive layer when formed into a polarizing plate is 70% or more, the crosslinking reaction has already progressed sufficiently, and the effect of deactivating the crosslinker due to the migration of alcohol in the polarizing plate is not fully achieved, and it is presumed that the effect of suppressing peeling when exposed to an environmental change from a high temperature and high humidity environment to a high temperature environment is not fully achieved. EXAMPLES
[0087] The present invention will be specifically described below based on examples. The materials, reagents, amounts of substances and their ratios, operations, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the present invention is not limited to the following examples.
[0088] (1) Measurement of the thickness of the polarizing element: The measurements were made using a Nikon digital micrometer "MH-15M."
[0089] (2) Measurement of the amount of alcohol (methanol) in the polarizing plate: The polarizing plate was cut into 1 cm squares to obtain samples for evaluation. 5 mL of ultrapure water was added to the samples, which were then heated at 70°C for 30 minutes and stirred. After that, measurements were performed using the GC-FID method under the following conditions. (Gas Chromatography Analysis Conditions) Column: DB-WAX 30m x 0.250mm x 0.25μm, ID (Agilent Technologies) or equivalent Carrier gas: Helium, 1.0 mL / min Column temperature: 40°C (held for 5 minutes) → Raise temperature at 20°C / min → 240°C (held for 10 minutes) Injection port temperature: 240°C, injection volume: 1 μL, split ratio: 50:1 Detector temperature: 240℃, Detector: FID
[0090] (3) Measurement of gel fraction of adhesive layer The gel fraction in the pressure-sensitive adhesive layer of the present invention is a value measured according to the following (a) to (d). (a) An adhesive layer having an area of approximately 8 cm x approximately 8 cm is bonded to a metal mesh made of SUS304 having an area of approximately 10 cm x approximately 10 cm (its weight is represented as Wm). (b) The laminate obtained in (a) above is weighed, and its mass is designated as Ws. Next, the laminate is folded four times so as to encase the adhesive layer and stapled, and then weighed, and its mass is designated as Wb. (c) The mesh stapled in (b) above is placed in a glass container, 60 mL of ethyl acetate is added to soak it, and the glass container is then stored at room temperature for 3 days. (d) Remove the mesh from the glass container, dry it at 120°C for 24 hours, and then weigh it. The mass is designated as Wa, and the gel fraction is calculated according to the following formula. Gel fraction (mass%) = [{Wa-(Wb-Ws)-Wm} / (Ws-Wm)] x 100
[0091] <Preparation of Polarizing Element> A 60 μm thick polyvinyl alcohol resin film with an average degree of polymerization of about 2400 and a degree of saponification of 99.9 mol% or more was immersed in pure water at 21.5°C for 79 seconds, and then immersed in an aqueous solution containing 1.0 mM iodine with a weight ratio of potassium iodide / boric acid / water of 2 / 2 / 100 at 23°C for 151 seconds. Then, the film was immersed in an aqueous solution containing 1.0 mM iodine with a weight ratio of potassium iodide / boric acid / water of 2.5 / 4 / 100 at 60.8°C for 76 seconds. Then, the film was immersed in an aqueous solution containing 1.0 mM iodine with a weight ratio of potassium iodide / boric acid / water of 3 / 5.5 / 100 at 45°C for 11 seconds. Then, the film was dried at 38°C to obtain a polarizing element with a thickness of 22 μm in which iodine was adsorbed and aligned in the polyvinyl alcohol. The stretching was mainly performed in the steps of iodine dyeing and boric acid treatment, and the total stretching ratio was 5.85 times.
[0092] [Preparation of Adhesives 1 and 2] (Preparation of PVA solution A for adhesive) 50 g of a modified PVA resin containing acetoacetyl groups ("Gohsenex Z-410" manufactured by Mitsubishi Chemical Corporation) was dissolved in 950 g of pure water, heated at 90°C for 2 hours, and then cooled to room temperature to obtain a PVA solution for adhesive (hereinafter referred to as "PVA solution A").
[0093] (Preparation of Adhesives 1 and 2) The PVA solution A prepared above, pure water, maleic acid, a 40 mass % glyoxal solution, and methanol were mixed in amounts as shown in Table 1 to prepare adhesives 1 and 2.
[0094] [Table 1]
[0095] <Preparing the transparent protective film> [Transparent protective film 1] A cellulose acylate film KC8UX2MSW (manufactured by Konica Minolta, Inc., film thickness 80 μm) was used. The cellulose acylate film was immersed in a 1.5 mol / L NaOH aqueous solution (saponification solution) kept at 55° C. for 2 minutes, and then washed with water. Thereafter, the film was immersed in a 0.05 mol / L sulfuric acid aqueous solution at 25° C. for 30 seconds, and then passed through a water washing bath under running water for 30 seconds to neutralize the film. Then, the film was drained three times with an air knife to remove water, and then it was allowed to stay in a drying zone at 70° C. for 15 seconds to dry and perform saponification treatment. [Transparent protective film 2] A cycloolefin polymer film ZB12 series (manufactured by Zeon Corporation, film thickness 52 μm) was used. Both sides of the cycloolefin polymer film were coated with a 40 W·min / m 2 The corona treatment was carried out under the following conditions.
[0096] <Preparation of polarizing plate> [Preparation of polarizing plate 1] A transparent protective film 1 was laminated on one side of a polarizing element and a transparent protective film 2 was laminated on the other side of the polarizing element using a roll laminator via adhesive 1, and then heat treatment was performed at 60°C for 10 minutes to dry the adhesive, thereby obtaining a polarizing plate 1. The thickness of the adhesive layer of polarizing plate 1 was 50 nm on both sides of the polarizing element. A surface protective film was laminated on the transparent protective film 1 side of the polarizing plate thus produced. The surface protective film was a surface protective film laminated with an acrylic pressure-sensitive adhesive layer (thickness 15 μm) formed on a polyester resin film (thickness 38 μm).
[0097] [Preparation of polarizing plate 2] Polarizing plate 2 was produced in the same manner as polarizing plate 1 except that adhesive 2 was used, and a surface protective film was attached to the surface of transparent protective film 1.
[0098] [Preparation of Adhesive Composition] The following acrylic base polymer (G-1), isocyanate crosslinking agent (G-2), and silane coupling agent (G-3) were prepared.
[0099] (H-1) Copolymer of butyl acrylate, methyl acrylate, acrylic acid and hydroxyethyl acrylate (H-2) Ethyl acetate solution of trimethylolpropane adduct of tolylene diisocyanate (solids concentration 75%) ("Coronate L" (product name, manufactured by Tosoh Corporation) (H-3) 3-Glycidoxypropyltrimethoxysilane, liquid ("KBM-403" (trade name), manufactured by Shin-Etsu Chemical Co., Ltd.)
[0100] 100 parts by mass of the acrylic base polymer (H-1), 0.2 parts by mass of an isocyanate crosslinking agent (H-2), and 0.2 parts by mass of a silane coupling agent (H-3) were mixed, thoroughly stirred, and diluted with ethyl acetate to obtain a pressure-sensitive adhesive composition.
[0101] [Preparation of adhesive layer] The obtained solution of the acrylic adhesive composition was applied to the release-treated surface of a release-treated polyethylene terephthalate film so that the thickness of the adhesive layer after drying was 25 μm, and then dried at 90° C. for 3 minutes to form an adhesive layer. The gel fraction of the obtained adhesive layer was 0%.
[0102] [Preparation of polarizing plate 1 with adhesive layer] The above-mentioned adhesive layer was immediately attached to the transparent protective film 2 side of the polarizing plate 1 to prepare the polarizing plate 1 with the adhesive layer. The obtained polarizing plate 1 with the adhesive layer was stored for 7 days in an environment at a temperature of 23° C. and a relative humidity of 50%. The methanol content of the polarizing plate before laminating the adhesive layer was 75 μg / cm 2 The gel fraction of the pressure-sensitive adhesive layer after storage was 75%.
[0103] [Preparation of polarizing plate 2 with adhesive layer] A polarizing plate 2 with an adhesive layer was produced in the same manner as in the production of the polarizing plate 1 with an adhesive layer, except that the polarizing plate 1 used in the polarizing plate 1 with an adhesive layer was changed to the polarizing plate 2. The obtained polarizing plate 2 with an adhesive layer was stored for 7 days in an environment at a temperature of 23°C and a relative humidity of 50%. The methanol content of the polarizing plate before laminating the adhesive layer was 0 μg / cm 2 The gel fraction of the adhesive layer after storage was 80%. The reason for the difference in gel fraction between polarizing plates with adhesive layer 1 and 2 is presumably because polarizing plate with adhesive layer 1 contains alcohol, which resulted in a lower gel fraction near the polarizing plate.
[0104] [Preparation of polarizing plate 3 with adhesive layer] A release-treated polyethylene terephthalate film was further laminated on the side of the pressure-sensitive adhesive layer that did not have the polyethylene terephthalate film. The resulting pressure-sensitive adhesive layer with release-treated polyethylene terephthalate films laminated on both sides was stored for 7 days in an environment at a temperature of 23°C and a relative humidity of 50%. The gel fraction of the pressure-sensitive adhesive layer after storage was 81%. One of the release-treated polyethylene terephthalate films on the pressure-sensitive adhesive layer after storage was peeled off and attached to the transparent protective film 2 side of polarizing plate 1 to produce polarizing plate 3 with a pressure-sensitive adhesive layer. The methanol content of the polarizing plate before laminating the pressure-sensitive adhesive layer was 75 μg / cm 2 It was.
[0105] <Durability evaluation> (Preparation of evaluation samples) The polarizing plates 1 to 3 with adhesive layers were cut to a size of 110 mm x 60 mm so that the absorption axis of the polarizing plate was parallel to the long side, and were attached to non-alkali glass ("EAGLE XG" manufactured by Corning, size 120 mm x 70 mm) via the adhesive layer. Then, the polarizing plates were heated at 50°C and subjected to a pressure of 5 kgf / cm. 2 (490.3 kPa) for 15 minutes, and then left to stand for 24 hours in an environment with a temperature of 23°C and a relative humidity of 55% to obtain an evaluation sample.
[0106] The evaluation samples thus prepared were stored in an environment with a temperature of 50°C and a relative humidity of 95% for 24 hours, and then in an environment with a temperature of 95°C for 96 hours, after which the evaluation samples were checked for any lifting or peeling. The results are shown in Table 2.
[0107] [Table 2]
Claims
1. Alcohol content is 4 μg / cm 2 More than 230μg / cm 2 A step of producing a polarizing plate, A step of producing a polarizing plate with a pressure-sensitive adhesive layer by forming a pressure-sensitive adhesive layer having a gel fraction of 5% or less on one surface of the polarizing plate; storing the pressure-sensitive adhesive layer-attached polarizing plate in an environment having a temperature of 18° C. or higher and 28° C. or lower and a relative humidity of 40% or higher and 70% or lower for 2 days or more; The step of producing the polarizing plate includes a step of bonding a polarizing element obtained by adsorbing and aligning iodine in a polyvinyl alcohol-based resin layer and a transparent protective film with an adhesive layer formed from an adhesive containing the alcohol, The method for producing a polarizing plate with a pressure-sensitive adhesive layer, wherein the alcohol is at least one selected from the group consisting of methanol, ethanol, and n-propyl alcohol.
2. The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to claim 1 , wherein the adhesive comprises a polyvinyl alcohol-based resin.
3. 3 . The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to claim 1 , wherein the adhesive has a content of the alcohol of 100 parts by mass or more and 2000 parts by mass or less with respect to 100 parts by mass of the polyvinyl alcohol-based resin.
4. The method for producing a polarizing plate with a pressure-sensitive adhesive layer according to any one of claims 1 to 3, wherein the adhesive layer has a thickness of 0.01 to 7 µm.
5. A method for manufacturing a polarizing plate with an adhesive layer described in any one of claims 1 to 4, wherein the gel fraction of the adhesive layer is 60% or more at the time when the storage process is completed.
Citation Information
Patent Citations
Polarizing plate, method for manufacturing the same, and IPS mode liquid crystal display device using the same
JP2011227418A
Polarizing film and manufacturing method thereof and polarizer
JP2013148806A
Optical film with adhesive and image display device
JP2016151580A
Adhesive composition for polarizer
JP2017019974A
Polarizing plate and liquid crystal display
WO2007102327A1