Spunbond nonwoven fabric
The spunbond nonwoven fabric with a striped pattern and controlled fiber orientation addresses visibility and texture issues, providing enhanced design, strength, and flexibility for sanitary materials and cleaning sheets.
Patent Information
- Application Number
- JP2020163359
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-29
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2040-09-29
AI Technical Summary
Existing methods for imparting patterns to nonwoven fabrics result in poor pattern visibility, reduced texture, and limitations in expressing fine designs due to issues with fiber spread states or collector net closures, leading to decreased quality and physical properties.
A spunbond nonwoven fabric with a striped pattern is developed, featuring high and low brightness areas alternately arranged, controlled fiber orientation, and specific brightness and thickness differences, along with controlled basis weight and thickness, to achieve excellent design, quality, and flexibility in at least one direction.
The solution results in a nonwoven fabric with enhanced design, sufficient strength, and flexibility, suitable for sanitary materials and cleaning sheets, with improved wiping performance.
Smart Images

Figure 0007589478000002 
Figure 0007589478000003 
Figure 0007589478000004
Abstract
Description
[Technical field]
[0001] The present invention relates to a spunbond nonwoven fabric suitable for use as a sanitary material or a cleaning sheet. [Background technology]
[0002] In recent years, in the field of sanitary materials such as disposable diapers and sanitary napkins, there has been a demand for nonwoven fabrics that have excellent design properties in addition to the traditionally required properties such as texture, feel, and flexibility.
[0003] As a means for imparting design to nonwoven fabric, in addition to a simple method of imparting a pattern by thermal compression using a concave-convex roll, a method of controlling the spread and collection state of the fibers that make up the nonwoven fabric is used. For example, a method has been proposed in which any pattern is expressed on the nonwoven fabric by changing the electrically spread state of the threads that make up the nonwoven fabric and collecting them (see Patent Document 1).
[0004] Also, a manufacturing device has been proposed that can impart a pattern to a nonwoven fabric by closing a part of a collector net that collects the nonwoven fabric (see Patent Document 2). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Japanese Patent Application Publication No. 7-109658 [Patent Document 2] JP 2017-206803 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, in the method disclosed in Patent Document 1, a predetermined pattern is imparted by changing the fiber-spreading state of the nonwoven fabric, which causes problems such as poor visibility of the pattern, poor texture in areas where the fiber-spreading state is loose, and reduced quality and physical properties. In addition, since the electrical fiber-spreading state is changed, it is difficult to impart a fine pattern.
[0007] On the other hand, in the device disclosed in Patent Document 2, a part of the collector net is closed, which makes it difficult to collect yarn in some parts, resulting in a decrease in quality and physical properties. In addition, there is a problem that the size of the closed part is limited, making it difficult to express a sufficient design.
[0008] In view of the above problems, an object of the present invention is to provide a spunbonded nonwoven fabric which has excellent designability, sufficient quality and strength, and excellent flexibility in at least one direction. [Means for solving the problem]
[0009] As a result of extensive research to achieve the above-mentioned object, the inventors have discovered that in a spunbond nonwoven fabric having a striped pattern in which high luminance areas and low luminance areas are arranged alternately, by controlling the luminance profile of the striped pattern and the fiber orientation of the nonwoven fabric within specific ranges, it is possible to obtain a spunbond nonwoven fabric that is excellent not only in design but also in quality and strength, and further has excellent flexibility in at least one direction.
[0010] The present invention has been completed based on these findings, and provides the following inventions.
[0011] The spunbonded nonwoven fabric of the present invention has a striped pattern on at least one surface in which high luminance regions and low luminance regions are alternately arranged, and in an average luminance profile in a direction perpendicular to the direction in which the striped pattern is formed, the luminance difference between a peak and an adjacent bottom is 10 to 100, the pitch of the peaks is 5 mm to 60 mm, and the degree of fiber orientation based on the direction in which the striped pattern is formed is 0° to 45°. And, The weight of the spunbond nonwoven fabric is 10 g / m 2 ~100g / m 2 and The difference in basis weight between the high brightness area and the low brightness area is 5 g / m 2 ~90g / m 2 and The difference between the thickness of the spunbond nonwoven fabric in the high brightness region and the thickness of the spunbond nonwoven fabric in the low brightness region is 0.03 mm to 1 mm. do.
[0013] According to a preferred embodiment of the nonwoven fabric of the present invention, the difference between the fiber orientation degree in the high brightness region and the fiber orientation degree in the low brightness region is 0° to 5°.
[0014] According to a preferred embodiment of the nonwoven fabric of the present invention, the average single fiber diameter of the fibers constituting the spunbonded nonwoven fabric is 6.5 μm to 14.5 μm. Effect of the Invention
[0015] According to the present invention, a spunbonded nonwoven fabric having excellent design, sufficient quality and strength, and excellent flexibility in at least one direction can be obtained. Due to these characteristics, the spunbonded nonwoven fabric of the present invention can be suitably used, particularly for sanitary material applications. [Brief description of the drawings]
[0016] [Figure 1] FIG. 1 is a schematic top view illustrating a striped pattern of a spunbond nonwoven fabric of the present invention, in which high luminance areas and low luminance areas are alternately arranged. [Diagram 2] FIG. 2 is a top conceptual diagram illustrating a lattice pattern formed by overlapping stripe patterns in two different directions on the spunbonded nonwoven fabric of the present invention. [Diagram 3] FIG. 3 is a conceptual diagram illustrating and explaining the average luminance profile in a direction perpendicular to the stripe pattern of the spunbonded nonwoven fabric of the present invention in the region (3) of FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The spunbonded nonwoven fabric of the present invention has a striped pattern on at least one surface in which high luminance regions and low luminance regions are alternately arranged, and in an average luminance profile in a direction perpendicular to the direction in which the striped pattern is formed, the luminance difference between a peak and an adjacent bottom is 10 to 100, the pitch of the peaks is 5 mm to 60 mm, and the degree of fiber orientation based on the direction in which the striped pattern is formed is 0° to 45°. Furthermore, the basis weight of the spunbond nonwoven fabric is 10 g / m 2 ~100g / m 2 The difference in basis weight between the high brightness area and the low brightness area is 5 g / m 2 ~90g / m 2 and the difference between the thickness of the spunbond nonwoven fabric in the high brightness region and the thickness of the spunbond nonwoven fabric in the low brightness region is 0.03 mm to 1 mm. The components will be described in detail below, but the present invention is not limited to the scope of the following description as long as it does not depart from the gist of the present invention.
[0018] [Thermoplastic resin] In the spunbonded nonwoven fabric of the present invention, the thermoplastic resin forming the fibers constituting the spunbonded nonwoven fabric is, for example, a polyolefin resin or a polyester resin. Examples of the polyolefin resin include a polypropylene resin and a polyethylene resin, and examples of the polyester resin include a polyethylene terephthalate resin and a polylactic acid resin.
[0019] Examples of polypropylene resins include propylene homopolymers and copolymers of propylene and various α-olefins, while examples of polyethylene resins include ethylene homopolymers and copolymers of ethylene and various α-olefins.
[0020] Among these, polypropylene-based resins are particularly preferred from the viewpoint of properties such as spinnability, strength, and flexibility.
[0021] In the polyolefin resin used in the present invention, the proportion of propylene homopolymer is preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 80% by mass or more. By setting it in the above range, good spinnability can be maintained and strength can be improved.
[0022] The polyolefin resin used in the present invention may be a mixture of two or more kinds, and a resin composition containing other olefin resins, thermoplastic elastomers, etc. may also be used.
[0023] They can also be used as composite fibers in which the above thermoplastic resins are combined. Examples of composite forms of composite fibers include concentric sheath-core type, eccentric sheath-core type, and sea-island type. Among them, the concentric sheath-core type composite form is preferred because it has excellent spinnability and can bond fibers together uniformly by thermal bonding.
[0024] To the thermoplastic resin used in the present invention, additives such as commonly used antioxidants, weather stabilizers, light stabilizers, antistatic agents, spinning agents, antiblocking agents, lubricants, nucleating agents, and pigments, or other polymers may be added as necessary, within the scope of not impairing the effects of the present invention.
[0025] The melting point of the polyolefin resin used in the present invention is preferably 80° C. to 200° C. By setting the melting point to preferably 80° C. or higher, more preferably 100° C. or higher, and even more preferably 120° C. or higher, heat resistance sufficient for practical use is easily obtained. In addition, by setting the melting point to preferably 200° C. or lower, more preferably 180° C. or lower, it becomes easy to cool the yarn discharged from the spinneret, and fusion between the fibers is suppressed, making it easy to perform stable spinning.
[0026] The melt flow rate (hereinafter, sometimes simply referred to as MFR) of the resin, which is the raw material of the spunbonded nonwoven fabric of the present invention, is preferably 30 g / 10 min to 850 g / 10 min. By setting the MFR to 30 g / 10 min or more, more preferably 60 g / 10 min or more, and even more preferably 100 g / min or more, it is possible to obtain a spunbonded nonwoven fabric having excellent spinnability during production and uniform texture. On the other hand, by setting the MFR to 850 g / 10 min or less, more preferably 600 g / 10 min or less, and even more preferably 400 g / 10 min or less, it is possible to suppress a decrease in the strength of the spunbonded nonwoven fabric.
[0027] The MFR of this resin is a value measured by ASTM D1238 (Method A). According to this standard, for example, polypropylene is measured at a load of 2.16 kg and a temperature of 230°C, and polyethylene is measured at a load of 2.16 kg and a temperature of 190°C.
[0028] Of course, it is also possible to adjust the MFR of the polyolefin resin by blending two or more resins with different MFRs in any ratio. In this case, the MFR of the resin to be blended with the main polyolefin resin is preferably 10g / 10min to 1000g / 10min, more preferably 20g / 10min to 800g / 10min, and even more preferably 30g / 10min to 600g / 10min. By making it within the above range, it is possible to prevent the blended polyolefin resin from having a partially uneven viscosity, resulting in non-uniform fineness and deterioration of spinnability.
[0029] In addition, when spinning fibers as described below, in order to prevent the occurrence of partial viscosity unevenness, to make the fiber fineness uniform, and to further reduce the fiber diameter as described below, it is also possible to adjust the MFR of the resin used by decomposing the resin. However, it is preferable not to add free radical agents such as peroxides, particularly dialkyl peroxides. When this method is used, partial viscosity unevenness occurs, making the fineness non-uniform, making it difficult to sufficiently reduce the fiber diameter, and spinnability may also be deteriorated due to viscosity unevenness and bubbles caused by decomposition gas.
[0030] In order to improve the slipperiness and flexibility of the spunbond nonwoven fabric of the present invention, the constituent fibers, which are polyolefin fibers made of polyolefin resin, may contain a fatty acid amide compound having 23 to 50 carbon atoms.
[0031] By making the carbon number of the fatty acid amide compound mixed with the polyolefin resin preferably 23 or more, more preferably 30 or more, it is possible to prevent the fatty acid amide compound from being excessively exposed on the fiber surface, to provide excellent spinnability and processing stability, and to maintain high productivity. On the other hand, by making the carbon number of the fatty acid amide compound preferably 50 or less, more preferably 42 or less, it is possible to facilitate migration of the fatty acid amide compound to the fiber surface, and to impart slipperiness and softness to the spunbonded nonwoven fabric.
[0032] Examples of the fatty acid amide compound having 23 to 50 carbon atoms used in the present invention include saturated fatty acid monoamide compounds, saturated fatty acid diamide compounds, unsaturated fatty acid monoamide compounds, and unsaturated fatty acid diamide compounds.
[0033] Specific examples of fatty acid amide compounds having 23 to 50 carbon atoms include tetradocosanoic acid amide, hexadocosanoic acid amide, octadocosanoic acid amide, nervonic acid amide, tetracosapentaenoic acid amide, nisinic acid amide, ethylene bislauric acid amide, methylene bislauric acid amide, ethylene bisstearic acid amide, ethylene bishydroxystearic acid amide, ethylene bisbehenic acid amide, hexamethylene bisstearic acid amide, hexamethylene bisbehenic acid amide, hexamethylene hydroxystearic acid amide, distearyl adipic acid amide, distearyl sebacic acid amide, ethylene bisoleic acid amide, ethylene biserucic acid amide, and hexamethylene bisoleic acid amide, and these can also be used in combination.
[0034] In the present invention, among these fatty acid amide compounds, ethylene bisstearamide, which is a saturated fatty acid diamide compound, is preferably used. Ethylene bisstearamide has excellent thermal stability and can be melt spun, and a spunbonded nonwoven fabric having excellent lubricity and flexibility can be obtained by using a fiber made of a thermoplastic resin containing this ethylene bisstearamide while maintaining high productivity.
[0035] In the present invention, the amount of the fatty acid amide compound added to the fiber is preferably 0.01% by mass to 5.0% by mass. By making the amount of the fatty acid amide compound 0.01% by mass or more, more preferably 0.1% by mass or more, it is possible to impart appropriate slipperiness and flexibility. On the other hand, by making the amount 5.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 1.0% by mass or less, it is possible to suppress a decrease in spinnability.
[0036] The amount added here refers to the mass percentage of the fatty acid amide compound added to the entire thermoplastic resin constituting the spunbonded nonwoven fabric of the present invention. For example, even when the fatty acid amide compound is added only to the sheath component constituting the core-sheath type composite fiber, the addition ratio to the entire amount of the core-sheath component is calculated.
[0037] The amount of fatty acid amide compound added to the fiber can be measured, for example, by extracting the additive from the fiber with a solvent and quantitatively analyzing it using liquid chromatography mass spectrometry (LS / MS) etc. The extraction solvent is appropriately selected depending on the type of fatty acid amide compound, and in the case of ethylene bisstearic acid amide, for example, a method using a chloroform-methanol mixture can be mentioned.
[0038] [Fibers that make up spunbond nonwoven fabric] The fibers constituting the spunbonded nonwoven fabric of the present invention preferably have an average single fiber diameter of 6.5 μm to 14.5 μm. By making the average single fiber diameter preferably 6.5 μm or more, more preferably 7.5 μm or more, and even more preferably 8.4 μm or more, it is possible to prevent a decrease in spinnability and produce a spunbonded nonwoven fabric of good quality stably. On the other hand, by making the average single fiber diameter preferably 14.5 μm or less, more preferably 11.7 μm or less, and even more preferably 11.2 μm or less, it is possible to improve the flexibility and produce a spunbonded nonwoven fabric with high uniformity.
[0039] In the present invention, the average single fiber diameter (μm) of the fibers constituting the spunbonded nonwoven fabric is calculated by the following procedure. (1) The resin is melt-spun, pulled and stretched by an ejector, and the nonwoven fiber web is collected on a net. (2) Randomly collect 10 small samples (100 x 100 mm). (3) Take surface photographs at 500x to 1000x magnification using a microscope or electron microscope, and measure the widths of 10 fibers from each sample, a total of 100 fibers. (4) Calculate the average single fiber diameter (μm) from the average of the 100 measured values.
[0040] [Spunbond nonwoven fabric] The spunbonded nonwoven fabric of the present invention has a striped pattern in which high brightness regions and low brightness regions are alternately arranged. Here, in the present invention, the "high brightness region" refers to a region having a brightness higher than the average brightness of the spunbonded nonwoven fabric, while the "low brightness region" refers to a region having a brightness lower than the average brightness of the spunbonded nonwoven fabric. The "striped pattern" refers not only to a pattern in which high brightness regions and low brightness regions are alternately arranged in the horizontal direction of the paper as exemplified in FIG. 1, but also to a pattern (lattice pattern) in which high brightness regions and low brightness regions are alternately arranged in two directions, vertical and horizontal, of the paper as exemplified in FIG. 2. The average brightness of the spunbonded nonwoven fabric refers to a value measured and calculated by the following method. (1) Attach the spunbond nonwoven fabric to the black backing (AC card black #350). (2) Using a scanner (e.g., Fuji Xerox Co., Ltd.'s "DocuCentre-VI"), the black mount with the spunbond nonwoven fabric attached is scanned in full color at 200 dpi to create a color scanned image of the spunbond nonwoven fabric and save it in JPG format. (3) Crop the image so that each side is 150 mm long into a square. (4) Calculate the luminance (unitless) defined in the YUV color space for each pixel (Brightness of each pixel) = 0.29891 x R + 0.58661 x G + 0.11448 x B Here, R, G, and B represent the red, green, and blue intensities (each unitless) of the RGB color model, respectively. (5) The brightness of all pixels is averaged and rounded off to the first decimal place to determine the average brightness.
[0041] The spunbond nonwoven fabric of the present invention has a peak (P A ) and bottom (P B), and the luminance difference between the apex and the adjacent bottom is 10 to 100. By making the luminance difference between the apex and the adjacent bottom 10 or more, preferably 15 or more, more preferably 20 or more, a spunbonded nonwoven fabric having excellent design and excellent flexibility in at least one direction can be obtained. In addition, when used as a cleaning sheet, wiping performance can be improved. On the other hand, by making the luminance difference between the apex and the adjacent bottom 100 or less, preferably 80 or less, more preferably 60 or less, it is possible to prevent the amount of fiber in the low luminance region (2) from being excessively reduced, thereby preventing a loss of practical strength. In the present invention, the direction in which the stripe pattern is formed is the direction of the arrow (4) in FIG. 1 in the case of a pattern in which high luminance regions (1) and low luminance regions (2) are alternately arranged in one direction as shown in FIG. 1, and is the direction including more high luminance regions, that is, the direction of the arrow (4), in the case of a pattern in which high luminance regions (1) and low luminance regions (2) are alternately arranged in two directions, vertically and horizontally, on the sheet of paper as shown in FIG. 2.
[0042] In the present invention, the average luminance profile in the direction perpendicular to the stripe pattern of the spunbond nonwoven fabric is measured by the method described below. (1) Attach the spunbond nonwoven fabric to the black backing (AC card black #350). (2) Using a scanner (e.g., Fuji Xerox Co., Ltd.'s "DocuCentre-VI"), the black mount with the spunbond nonwoven fabric attached thereto is scanned at 200 dpi in full color to create a color scanned image of the spunbond nonwoven fabric, and the image is saved in JPG format. At this time, the direction in which the high-luminance area (1) is formed (the direction in which the stripe pattern is formed (4)) is set to the vertical direction of the image. In the case of a pattern in which the high-luminance area (1) and the low-luminance area (2) are alternately arranged in two directions, vertical and horizontal, on the paper surface, as shown in FIG. 2, the clearer direction is selected as the direction in which the stripe pattern is formed (in the case shown in FIG. 2, the direction in which the stripe pattern is formed is the direction indicated by the symbol 4). In the case where the clarity of the stripe patterns in two different directions is equivalent, any of the two directions, vertical and horizontal, is selected as the direction in which the stripe pattern is formed (4). (3) Trim the image so that it is a square with each side measuring 30 mm to 300 mm in length, and the size must be such that it contains at least four units of the stripe pattern, with each unit consisting of adjacent high-luminance areas (A) and low-luminance areas (B). (4) Calculate the luminance (unitless) defined in the YUV color space for each pixel (Brightness of each pixel) = 0.29891 x R + 0.58661 x G + 0.11448 x B Here, R, G, and B represent the red, green, and blue intensities (each unitless) of the RGB color model, respectively. (5) The average brightness is calculated in the vertical direction of the image (the direction in which the stripe pattern is formed), and an average brightness profile in the horizontal direction (the direction perpendicular to the stripe pattern) is created.
[0043] FIG. 3 shows an example of an average luminance profile in a direction perpendicular to the direction in which the stripe pattern of the spunbond nonwoven fabric is formed. A ) and the adjacent bottom (P B The luminance difference between the vertex and the adjacent bottom is measured using the bottom with the greater average luminance of the two bottoms adjacent to one vertex. The luminance difference is measured for five or more vertices, and the average value is rounded off to the nearest whole number, which is the luminance difference between the vertex and the adjacent bottom.
[0044] If it is difficult to determine the peaks and valleys due to unevenness in the average luminance profile, moving average processing may be performed in the horizontal direction (the direction perpendicular to the stripe pattern). In this case, to ensure that the average luminance profile is properly created, the width of the moving average is adjusted so that it is equal to or less than one-eighth the pitch of the peaks determined from the average luminance profile after processing.
[0045] In the spunbonded nonwoven fabric of the present invention, the distance between adjacent vertices in the average luminance profile in the direction perpendicular to the stripe pattern, i.e., the pitch of the vertices, is 5 mm to 60 mm. By making the pitch of the vertices of the average luminance profile 5 mm or more, preferably 8 mm or more, more preferably 10 mm or more, it is possible to obtain a spunbonded nonwoven fabric that is excellent in design and excellent in flexibility in at least one direction. In addition, in applications such as cleaning sheets, it is possible to improve wiping performance. On the other hand, by making the pitch of the vertices of the average luminance profile 60 mm or less, preferably 45 mm or less, more preferably 30 mm or less, it is possible to obtain a spunbonded nonwoven fabric that has improved design and has small flexibility variations by arranging the low luminance regions (B) that are easily bent at narrow intervals. In addition, in applications as cleaning sheets, it is possible to reduce variation in wiping performance.
[0046] The pitch (mm) of the apexes of the average luminance profile is determined by measuring the pitch of adjacent apexes at five or more locations, and rounding off the average value (mm) to the nearest whole number.
[0047] The spunbonded nonwoven fabric of the present invention has a fiber orientation of 45° or less relative to the direction in which the stripe pattern is formed. By setting the fiber orientation to 45° or less, preferably 35° or less, and more preferably 30° or less relative to the direction in which the stripe pattern is formed, it is possible to obtain a spunbonded nonwoven fabric having good texture and excellent design properties.
[0048] The degree of fiber orientation based on the formation direction of the stripe pattern in the lattice pattern as exemplified in FIG. 2 is measured as follows, using a stripe pattern with the same formation direction as the stripe pattern used to create the above average brightness profile as a reference. (1) Five 20 mm long test pieces, each containing a striped pattern unit consisting of adjacent high luminance and low luminance areas, are taken at equal intervals across the width of the spunbond nonwoven fabric. (2) Using a scanning electron microscope, take surface photographs of the center of the high and low basis weight regions for each sample. The magnification should be 500x or more, and a magnification that includes at least 20 fibers should be selected. (3) On each surface photograph, draw a guide line at any position perpendicular to the direction of the stripe pattern. For all fibers that intersect with the guide line, measure the inclination of the fibers near the intersection with the guide line, with the direction of the stripe pattern as the reference (0°). However, do not measure fibers with unclear outlines. (4) In each of the high basis weight region and low basis weight region, the inclination angle (-90° to 90°) of 20 fibers in each photograph, for a total of 200 fibers, is measured, and the absolute value is averaged to one decimal place to obtain the degree of fiber orientation based on the direction in which the stripe pattern of the spunbond nonwoven fabric (as a whole) is formed.
[0049] The basis weight of the spunbond nonwoven fabric of the present invention is 10 g / m 2 ~100g / m 2 The weight is preferably 10 g / m 2 More preferably, it should be 13 g / m or more. 2 More preferably, it should be 15 g / m 2 By adjusting the weight to the above value, a spunbond nonwoven fabric having a mechanical strength sufficient for practical use can be obtained. On the other hand, the weight per unit area is preferably 100 g / m 2 Less than 50 g / m 2 More preferably, 30 g / m or less 2 By using the following, it is possible to obtain a spunbond nonwoven fabric having appropriate flexibility suitable for use as a nonwoven fabric for sanitary materials.
[0050] In the present invention, the basis weight of the spunbond nonwoven fabric is determined in accordance with "6.2 Mass per unit area" of JIS L1913:2010 "Testing methods for general nonwoven fabrics" and is measured by the following procedure. (1) Take three test pieces measuring 20 cm x 25 cm per meter of sample width. (2) Measure the mass (g) of each at standard conditions. (3) The average value is 1m 2 Mass per unit (g / m 2 )
[0051] The spunbond nonwoven fabric of the present invention has a basis weight difference between the high brightness area and the low brightness area of 5 g / m 2 ~100g / m 2 The difference in weight between the high brightness area and the low brightness area is preferably 5 g / m 2 More preferably, 10 g / m 2 More preferably, 20 g / m 2 By setting the above, the shading of the striped pattern consisting of high brightness and low brightness regions becomes clear, and a spunbond nonwoven fabric having excellent design and excellent flexibility in at least one direction can be obtained. In addition, when used as a cleaning sheet, wiping performance can be improved. On the other hand, the basis weight difference between the high brightness region and the low brightness region is preferably 100 g / m 2 More preferably, the thickness is set to 90 g / m or less. 2 Less than 80 g / m, more preferably 80 g / m 2 By setting it to the value below, it is possible to prevent the amount of fiber in the low brightness region from being excessively reduced, which would result in a decrease in strength.
[0052] In addition, the spunbonded nonwoven fabric of the present invention has a striped pattern by precisely controlling the distribution of basis weight. Generally, there is a method of applying a striped pattern to a low-brightness region by adopting a part having regular openings, but the strength of the nonwoven fabric is easily reduced by having openings, and depending on the application, liquid is easily allowed to pass through the openings. There is also a method of applying a pattern processing to a high-brightness region and a low-brightness region using an engraved roll with a different pattern, but this does not cause a basis weight difference and makes it difficult to apply extreme unevenness. Therefore, it is difficult to obtain a spunbonded nonwoven fabric that has excellent flexibility in one direction while maintaining sufficient strength as in the present invention.
[0053] The thickness of the spunbond nonwoven fabric of the present invention is preferably 0.05 mm to 1.5 mm. By setting the thickness to preferably 0.05 mm to 1.5 mm, more preferably 0.08 mm to 1.0 mm, and even more preferably 0.10 mm to 0.8 mm, it is possible to provide a spunbond nonwoven fabric that has flexibility and appropriate cushioning properties and is suitable for use as a spunbond nonwoven fabric for sanitary materials, particularly for use in disposable diapers.
[0054] In the present invention, the thickness (mm) of the spunbond nonwoven fabric is determined in accordance with "5.1 Thickness" of JIS L1906:2000 "Testing methods for general long-fiber nonwoven fabrics" and is measured by the following procedure. (1) For each of the high-luminance and low-luminance areas, a pressure probe with a diameter of 10 mm is used to measure the thickness at 10 points per meter at equal intervals across the width of the nonwoven fabric with a load of 10 kPa to an accuracy of 0.01 mm. (2) The average thickness of the 20 points measured in the high brightness and low brightness areas is rounded off to the third decimal place.
[0055] In the spunbonded nonwoven fabric of the present invention, the difference between the thickness of the spunbonded nonwoven fabric in the high brightness region and the thickness of the spunbonded nonwoven fabric in the low brightness region (hereinafter, sometimes simply referred to as "thickness difference between the high brightness region and the low brightness region") is preferably 0.03 mm to 1 mm. By making the thickness difference between the high brightness region and the low brightness region preferably 0.03 mm or more, more preferably 0.06 mm or more, and even more preferably 0.1 mm or more, the shading of the stripe pattern can be made clearer, and a spunbonded nonwoven fabric having excellent design and excellent flexibility in at least one direction can be obtained. In addition, when used as a cleaning sheet, the wiping performance can be improved. On the other hand, by making the thickness difference between the high brightness region and the low brightness region preferably 1 mm or less, more preferably 0.9 mm or less, and even more preferably 0.8 mm or less, the amount of fiber in the low brightness region can be prevented from being excessively reduced, which can prevent the strength from being reduced.
[0056] In the present invention, the thickness difference (mm) between the high-luminance area and the low-luminance area of the spunbond nonwoven fabric is determined in accordance with JIS L1906:2000 "Testing methods for general long-fiber nonwoven fabrics" (5.1 Thickness) and is measured by the following procedure. (1) For each of the high-luminance and low-luminance areas, a pressure probe with a diameter of 10 mm is used to measure the thickness at 10 points per meter at equal intervals across the width of the nonwoven fabric with a load of 10 kPa to an accuracy of 0.01 mm. (2) For each of the high-luminance and low-luminance areas, the average of the thicknesses of the 10 points is rounded off to two decimal places to determine the thickness of the high-luminance and low-luminance areas. (3) The absolute value of the difference in thickness between the high brightness area and the low brightness area is calculated.
[0057] In cases where it is difficult to measure the thickness difference between the high-luminance and low-luminance areas using the above method using a 10 mm diameter pressure probe due to reasons such as a narrow pitch of the stripe pattern, the thickness of the cross section may be measured using an optical microscope.
[0058] The apparent density of the spunbond nonwoven fabric of the present invention is 0.05 g / cm 3 ~0.3g / cm 3 The apparent density of the spunbond nonwoven fabric is preferably 0.3 g / cm 3 More preferably, 0.25 g / cm 3 More preferably, it should be 0.20 g / cm or less. 3 By setting the density to the range below, it is possible to prevent the fibers from being densely packed and the flexibility of the spunbonded nonwoven fabric from being impaired.
[0059] On the other hand, the apparent density of the spunbond nonwoven fabric is preferably 0.05 g / cm 3 More preferably, it is 0.08 g / cm 3 More preferably, it is 0.10 g / cm 3 By doing so, it is possible to obtain a spunbond nonwoven fabric which is suppressed from causing fluff or delamination and has sufficient strength and ease of handling for practical use.
[0060] In the present invention, the apparent density (g / cm 3 ) is calculated from the above unrounded basis weight and thickness according to the following formula, and rounded off to the third decimal place. Apparent density (g / cm 3 )=[Weight (g / m 2 )] / [Thickness (mm)]×10 -3 .
[0061] The spunbonded nonwoven fabric of the present invention preferably has a bending resistance in at least one direction of 30 mm or less. By setting the bending resistance to preferably 30 mm or less, more preferably 28 mm or less, and even more preferably 26 mm or less, the spunbonded nonwoven fabric for sanitary materials, particularly suitable for use in disposable diapers, can be obtained with a suitable degree of flexibility. In addition, from the viewpoint of ensuring ease of handling as a spunbonded nonwoven fabric, the bending resistance is preferably 10 mm or more. The bending resistance can be adjusted by the pitch of the stripe pattern, the degree of fiber orientation based on the direction of formation of the stripe pattern, the basis weight, the single fiber diameter, and the heat compression conditions (compression rate, temperature, line pressure, etc.), etc.
[0062] The bending resistance of spunbond nonwoven fabrics shall be the value measured in accordance with "6.7 Bending resistance (JIS method and ISO method)" of "JIS L1913:2010 General nonwoven fabric test methods" and "6.7.4 Gurley method."
[0063] The spunbonded nonwoven fabric of the present invention has a fiber orientation degree of 0° to 45° based on the direction in which the stripe pattern is formed. Here, "fiber orientation degree based on the direction in which the stripe pattern is formed" refers to the difference (°) between the fiber orientation angle and the direction in which the stripe pattern is formed (4) as exemplified in Fig. 1, and is a value shown in the range of 0° to 90°. By setting the fiber orientation degree based on the direction in which the stripe pattern is formed to 45° or less, preferably 35° or less, and more preferably 30° or less, it is possible to obtain a spunbonded nonwoven fabric having good texture, excellent design, and excellent strength.
[0064] In addition, in the spunbond nonwoven fabric of the present invention, the difference in fiber orientation between the high brightness region and the low brightness region is preferably 0° to 5°. By setting the difference in fiber orientation between the high brightness region (A) and the low brightness region (B) to preferably 0° to 5°, more preferably 0° to 4°, and even more preferably 0° to 3°, the difference in the fiber orientation state becomes smaller compared to the high brightness region and the low brightness region, making it possible to maintain good texture even at the boundary between these regions, improving the design and preventing a decrease in strength.
[0065] The degree of fiber orientation based on the direction in which the stripe pattern of the spunbonded nonwoven fabric is formed is determined by the following procedure. (1) Five 20 mm long test pieces, each containing a striped pattern unit consisting of adjacent high luminance and low luminance areas, are taken at equal intervals across the width of the spunbond nonwoven fabric. (2) Using a scanning electron microscope, take surface photographs of the center of the high and low basis weight regions for each sample. The magnification should be 500x or more, and a magnification that includes at least 20 fibers should be selected. (3) On each surface photograph, draw a guide line at any position perpendicular to the direction of the stripe pattern. For all fibers that intersect with the guide line, measure the inclination of the fibers near the intersection with the guide line, with the direction of the stripe pattern as the reference (0 degrees). However, do not measure fibers with unclear outlines. (4) In each of the high and low basis weight regions, the inclination angle (-90° to 90°) of 20 fibers in each photograph, for a total of 100 fibers, is measured, and the average of the absolute values is rounded off to the first decimal place to determine the fiber orientation of the high and low basis weight regions. The average of the absolute values of the inclination angles of 200 fibers in the high and low basis weight regions combined is rounded off to the first decimal place to determine the fiber orientation based on the direction in which the stripe pattern of the spunbond nonwoven fabric (as a whole) is formed.
[0066] [Manufacturing method of spunbond nonwoven fabric] Next, a preferred embodiment of the method for producing the spunbonded nonwoven fabric of the present invention will be specifically described.
[0067] The spunbond nonwoven fabric of the present invention is a long fiber nonwoven fabric produced by the spunbond method. The method for producing the nonwoven fabric is not particularly limited, but examples thereof include the spunbond method, flash spinning method, wet method, carding method, and airlaid method. In particular, the spunbond method is excellent in productivity and mechanical strength, and can suppress fluffing and fiber dropout, which are likely to occur in short fiber nonwoven fabrics. In addition, the collected spunbond nonwoven fiber web or heat-pressed spunbond nonwoven fabric (both are written as S) is laminated in multiple layers with SS, SSS, and SSSS, which is a preferred embodiment because it improves productivity and uniformity of texture.
[0068] In the spunbonding method, first, molten thermoplastic resin is spun from a spinneret as long fibers, which are then drawn by compressed air using an ejector, and the fibers are collected on a moving net to obtain a nonwoven fiber web. The nonwoven fiber web is then subjected to a thermal bonding treatment to obtain a spunbonded nonwoven fabric.
[0069] The shapes of the spinneret and ejector are not particularly limited, and various shapes such as round, rectangular, etc. can be used. Among them, a combination of a rectangular spinneret and a rectangular ejector is preferably used because it uses a relatively small amount of compressed air, is excellent in energy cost, is less likely to cause fusion or abrasion between the yarns, and is easy to open the yarns.
[0070] In the present invention, the polyolefin resin is melted in an extruder, metered, and fed to a spinneret to be spun into long fibers. The spinning temperature when melting and spinning the polyolefin resin is preferably 200° C. to 270° C., more preferably 210° C. to 260° C., and even more preferably 220° C. to 250° C. By setting the spinning temperature within the above range, a stable molten state can be achieved, and excellent spinning stability can be obtained.
[0071] The back pressure of the spinneret is preferably 0.1 MPa to 6.0 MPa. By setting the back pressure to preferably 0.1 MPa to 6.0 MPa, more preferably 0.3 MPa to 6.0 MPa, and even more preferably 0.5 MPa to 6.0 MPa, it is possible to prevent the discharge uniformity from deteriorating, resulting in variation in fiber diameter, and to prevent the spinneret from becoming larger in size in order to increase pressure resistance. The back pressure of the spinneret can be adjusted by the nozzle hole diameter, nozzle hole depth, spinning temperature, etc. of the spinneret, and among these, the nozzle hole diameter has a large contribution.
[0072] The spun long fiber yarn is then cooled. Methods for cooling the spun yarn include, for example, forcibly blowing cold air onto the yarn, naturally cooling at the ambient temperature around the yarn, and adjusting the distance between the spinneret and the ejector. Alternatively, a combination of these methods can be used. The cooling conditions can be appropriately adjusted in consideration of the discharge rate per hole of the spinneret, the spinning temperature, the ambient temperature, and the like.
[0073] Next, the cooled and solidified yarn is pulled and stretched by compressed air jetted from an ejector.
[0074] The spinning speed is preferably 3500 to 6500 m / min, more preferably 4000 to 6500 m / min, and even more preferably 4500 to 6500 m / min. By setting the spinning speed at 3500 to 6500 m / min, high productivity is achieved, and the orientation and crystallization of the fibers progresses, making it possible to obtain long fibers with high strength. Normally, when the spinning speed is increased, the spinnability deteriorates and it is not possible to stably produce filaments, but as described above, by using a polyolefin-based resin having a specific MFR range, it is possible to stably spin the intended polyolefin fiber.
[0075] The obtained long fibers are then collected on a moving net to obtain a nonwoven fiber web. In the spunbonded nonwoven fabric of the present invention, the dispersion of the fibers is controlled by blowing air from the outside or using a baffle plate with irregularities between the time when the yarn is ejected from the ejector and collected on the collecting net, and the fibers are collected on the collecting net in a state where regular coarse and dense variations are intentionally generated, so that a striped pattern consisting of high brightness areas and low brightness areas can be formed on the spunbonded nonwoven fabric. When controlling the dispersion of the fibers by blowing air from the outside, the shape of the striped pattern can also be changed over time by changing the air flow rate over time.
[0076] The stripe pattern of the spunbonded nonwoven fabric of the present invention is preferably formed by continuous high brightness regions in the longitudinal direction and continuous low brightness regions in the longitudinal direction. The longitudinal direction means the flow direction of the collecting net and the winding direction of the nonwoven fabric roll. In this way, it is easy to control the dispersion of the fibers, and it is possible to obtain a spunbonded nonwoven fabric that is excellent in design and has excellent flexibility in at least one direction. On the other hand, when a stripe pattern is formed that is continuous in the width direction, it is difficult to form a stripe pattern consisting of clear high brightness regions and clear low brightness regions at narrow intervals because the yarn is ejected from the ejector at a high speed.
[0077] When producing a spunbonded nonwoven fabric having a lattice pattern formed by providing a continuous stripe pattern in the width direction as well as the length direction, it is effective to combine the above-mentioned method of controlling the dispersion of fibers with the method of closing a part of the collection net. In this way, a spunbonded nonwoven fabric having excellent design can be obtained.
[0078] In the present invention, it is also a preferred embodiment to temporarily bond the nonwoven fiber web by contacting one side of the nonwoven fiber web on a net with a hot flat roll, which can prevent the surface layer of the nonwoven fiber web from turning over or being blown away while being transported on the net, thereby improving transportability from collecting the yarns to thermocompression bonding.
[0079] The resulting nonwoven fibrous web can then be thermally bonded to obtain the intended spunbonded nonwoven fabric.
[0080] The method for thermally bonding the nonwoven fiber web is not particularly limited, and examples include methods of thermally bonding the nonwoven fiber web using various rolls, such as a thermal embossing roll in which the surfaces of a pair of upper and lower rolls are engraved (with uneven portions), a thermal embossing roll consisting of a combination of a roll with one flat (smooth) surface and a roll with the other roll having engraving (with uneven portions), and a thermal calendar roll consisting of a pair of upper and lower flat (smooth) rolls, as well as ultrasonic bonding in which the web is thermally welded by ultrasonic vibration of a horn.
[0081] Among these, a preferred embodiment is to use a heat embossing roll having engraved (uneven portions) on the surface of a pair of upper and lower rolls, or a heat embossing roll consisting of a combination of a roll with one flat (smooth) surface and a roll with engraved (uneven portions) on the surface of the other roll, because this has excellent productivity, imparts strength in the partial heat-bonded parts, and allows the non-bonded parts to retain the texture and feel unique to nonwoven fabric.
[0082] As for the surface material of the hot embossing roll, a preferred embodiment is to use a pair of metal rolls in order to obtain a sufficient thermocompression effect and to prevent the engraving (convex and concave portions) of one embossing roll from being transferred to the surface of the other roll.
[0083] The embossed adhesion area ratio by such a hot embossing roll is preferably 5 to 30%. By setting the adhesion area to preferably 5% or more, more preferably 8% or more, and even more preferably 10% or more, it is possible to obtain a strength that can be practically used as a spunbonded nonwoven fabric. On the other hand, by setting the adhesion area to preferably 30% or less, more preferably 25% or less, and even more preferably 20% or less, it is possible to obtain a suitable flexibility as a spunbonded nonwoven fabric for sanitary materials, particularly suitable for use in disposable diapers. Even when ultrasonic bonding is used, it is preferable that the adhesion area ratio is in the same range.
[0084] The bonding area referred to here means the proportion of the bonded area to the entire spunbonded nonwoven fabric. Specifically, in the case of thermal bonding using a pair of uneven rolls, it means the proportion of the portion (bonded area) where the convex parts of the upper roll and the convex parts of the lower roll overlap and contact the nonwoven fiber web to the entire spunbonded nonwoven fabric. In addition, in the case of thermal bonding using an uneven roll and a flat roll, it means the proportion of the portion (bonded area) where the convex parts of the uneven roll contact the nonwoven fiber web to the entire spunbonded nonwoven fabric. In addition, in the case of ultrasonic bonding, it means the proportion of the portion (bonded area) that is thermally welded by ultrasonic processing to the entire spunbonded nonwoven fabric.
[0085] The shape of the bonded portion formed by the hot embossing roll or ultrasonic bonding is not particularly limited, but for example, a circle, an ellipse, a square, a rectangle, a parallelogram, a rhombus, a regular hexagon, and a regular octagon can be used. It is preferable that the bonded portions are uniformly present at regular intervals in the longitudinal direction (transport direction) and the width direction of the spunbonded nonwoven fabric. In this way, the variation in strength of the spunbonded nonwoven fabric can be reduced.
[0086] The surface temperature of the hot embossing roll during thermal bonding is preferably 50°C to 10°C lower than the melting point of the thermoplastic resin used (hereinafter, sometimes referred to as Tm (°C)) (i.e., (Tm-50°C) to (Tm-10°C)). By setting the surface temperature of the hot roll to preferably -50°C (i.e., Tm-50°C, the same applies below) or higher than the melting point of the thermoplastic resin, and more preferably -45°C (Tm-45°C) or higher, a spunbonded nonwoven fabric with a strength that can be used in practical applications can be obtained by moderately thermal bonding. In addition, by setting the surface temperature of the hot embossing roll to preferably -10°C (Tm-10°C) or lower than the melting point of the thermoplastic resin, and more preferably -15°C (Tm-15°C) or lower, excessive thermal bonding can be suppressed, and moderate flexibility suitable for use as a spunbonded nonwoven fabric for sanitary materials, particularly for use in disposable diapers, can be obtained.
[0087] The linear pressure of the hot embossing roll during thermal bonding is preferably 50 to 500 N / cm. By setting the linear pressure of the roll to preferably 50 N / cm or more, more preferably 100 N / cm or more, and even more preferably 150 N / cm or more, it is possible to obtain a spunbonded nonwoven fabric having a strength suitable for practical use by moderate thermal bonding. On the other hand, by setting the linear pressure of the hot embossing roll to preferably 500 N / cm or less, more preferably 400 N / cm or less, and even more preferably 300 N / cm or less, it is possible to obtain a moderate flexibility suitable for use as a spunbonded nonwoven fabric for sanitary materials, particularly for use in disposable diapers.
[0088] In the present invention, for the purpose of adjusting the thickness of the spunbonded nonwoven fabric, thermal compression bonding can be performed using a thermal calendar roll consisting of a pair of upper and lower flat rolls before and / or after thermal bonding using the above-mentioned thermal embossing roll. The pair of upper and lower flat rolls refers to metal rolls or elastic rolls with no irregularities on the roll surfaces, and a pair of metal rolls or a pair of metal rolls and elastic rolls can be used.
[0089] The elastic roll here refers to a roll made of a material having elasticity compared to a metal roll. Examples of the elastic roll include so-called paper rolls such as paper, cotton, and aramid paper, and resin rolls made of urethane resin, epoxy resin, silicon resin, polyester resin, hard rubber, and mixtures of these resins. EXAMPLES
[0090] Next, the spunbond nonwoven fabric of the present invention will be specifically described based on examples. However, the present invention is not limited to only these examples. In addition, in the measurement of each physical property, unless otherwise specified, the measurement was performed based on the above-mentioned method.
[0091] [Measurement method] (1) Resin melt flow rate (MFR) (g / 10 min): The MFR of the resin was measured under conditions of a load of 2.16 kg and a temperature of 230°C.
[0092] (2) Average single fiber diameter (μm) of fibers constituting the spunbond nonwoven fabric: The average single fiber diameter of the fibers constituting the spunbond nonwoven fabric was measured using an electron microscope "VHX-D500" manufactured by Keyence Corporation according to the above-mentioned method.
[0093] (3) Spinning speed (m / min): From the above average single fiber diameter and the solid density of the resin used, the mass per 10,000 m of length was calculated as the average single fiber fineness (dtex) by rounding off to the first decimal place. The spinning speed was calculated based on the average single fiber fineness and the amount of resin discharged from a single hole of the spinneret set under each condition (hereinafter abbreviated as single hole discharge amount) (g / min) according to the following formula. Spinning speed (m / min) = (10,000 × [single-hole output (g / min)]) / [average single fiber fineness (dtex)].
[0094] (4) Average luminance of spunbond nonwoven fabric, average luminance profile in the direction perpendicular to the stripe pattern of the spunbond nonwoven fabric: In measuring the average brightness of the spunbond nonwoven fabric and the average brightness profile in the direction perpendicular to the stripe pattern of the spunbond nonwoven fabric, a color multifunction printer "DocuCentre-VI C4471 PFS" (manufactured by Fuji Xerox Co., Ltd.) was used for image scanning. Then, the brightness difference between the top of the average brightness profile and the adjacent bottom was calculated using the above method.
[0095] (5) Fiber orientation degree (°) based on the direction of the stripe pattern of the spunbond nonwoven fabric, and the difference between the fiber orientation degree in the high-brightness area and the fiber orientation degree in the low-brightness area (°): Using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation, the fiber orientation degree based on the direction of the stripe pattern formation was measured using the method described above (simply referred to as "fiber orientation degree" in Table 1), and the difference in fiber orientation degree between the high-brightness area and the low-brightness area (simply referred to as "difference in fiber orientation degree" in Table 1).
[0096] (6) Bending resistance of spunbond nonwoven fabric (mm): The bending resistance of the spunbond nonwoven fabric was measured in the CD direction (cross direction) according to the method described in "6.7 Bending resistance (JIS method and ISO method)" of "6.7.4 Gurley method" of JIS L1913:2010 "General nonwoven fabric test methods."
[0097] (7) Design of the striped pattern (points): A sample cut to a size of 200 mm x 200 mm was taken from the spunbond nonwoven fabric, and 10 panelists each evaluated the design of the striped pattern of the spunbond nonwoven fabric using the following 5-point scale. The scores judged by each panelist were then averaged and rounded off to the nearest whole number to determine the design of the striped pattern. The design is preferably 4 points or more, and more preferably 5 points. 5 points: Very good (The stripe pattern is clearly visible all the way to the borders, giving the impression of excellent design.) 4 points: Good (between 5 and 3 points) 3 points: Average (The boundaries are unclear in some places, but the stripe pattern is clearly visible and has a good design.) 2 points: Poor (between 1 and 3 points) 1 point: Very bad (the pattern is not visible or is unclear, and it feels like it lacks design).
[0098] [Example 1] A homopolymer polypropylene resin with a melt flow rate (MFR) of 40g / 10min and a melting point of 160°C was melted in an extruder and spun at a spinning temperature of 230°C and a single hole output of 0.55g / min. The spun yarn was cooled and solidified, and then pulled and stretched in a rectangular ejector with compressed air at an ejector pressure of 0.30MPa. The fibers were then ejected from the ejector outlet, and air was supplied from compressed air nozzles arranged at regular intervals adjacent to the ejector outlet, controlling the dispersion of the fibers to form coarse and dense fibers at regular intervals, which were then collected on a moving net. This produced a nonwoven fiber web made of polypropylene long fibers.
[0099] The nonwoven fiber web thus formed was then thermally bonded using a pair of upper and lower heat embossing rolls consisting of an upper roll and a lower roll under the conditions of a line pressure of 300 N / cm and a thermal bonding temperature of 130°C, resulting in an average basis weight of 15 g / m. 2 A spunbond nonwoven fabric of this type was obtained. (Upper roll): Metal embossed roll with polka dot pattern engraved on it, with a 16% adhesive area ratio (Lower roll): Metal flat roll The obtained spunbond nonwoven fabric was evaluated and the results are shown in Table 1.
[0100] [Example 2] Except for changing the injection pressure of the compressed air arranged adjacent to the outlet of the ejector, a spunbonded nonwoven fabric was obtained in the same manner as in Example 1. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0101] [Example 3] A spunbonded nonwoven fabric was obtained in the same manner as in Example 2, except that the interval between the compressed air nozzles arranged adjacent to the outlet of the ejector was changed. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0102] [Example 4] A spunbonded nonwoven fabric was obtained in the same manner as in Example 2, except that the interval between the compressed air nozzles arranged adjacent to the outlet of the ejector was changed. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0103] [Example 5] The conveying speed of the net that collects the yarn ejected from the ejector was changed to increase the average basis weight of the spunbond nonwoven fabric to 20 g / m 2 A spunbonded nonwoven fabric was obtained in the same manner as in Example 2, except that the injection pressure of the compressed air arranged adjacent to the outlet of the ejector was changed. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0104] [Example 6] In Example 2, a net for collecting the yarn ejected from the ejector was provided with continuous sealed portions in the CD direction to form a lattice pattern on the spunbonded nonwoven fabric. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0105] [Comparative Example 1] A spunbonded nonwoven fabric was obtained in the same manner as in Example 1, except that the injection pressure of the compressed air arranged adjacent to the outlet of the ejector was set to 0 MPa. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0106] [Comparative Example 2] A spunbonded nonwoven fabric was obtained in the same manner as in Example 1, except that the injection pressure of the compressed air arranged adjacent to the outlet of the ejector was set to one-fourth of the condition in Example 1. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0107] [Comparative Example 3] In Comparative Example 1, an electric fiber spreading device was installed at the outlet of the ejector with reference to JP-A-7-109658, and a striped pattern was formed on the spunbonded nonwoven fabric. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0108] [Comparative Example 4] In Comparative Example 1, a net for collecting the yarn ejected from the ejector was provided with continuous sealed portions in the CD direction to form a striped pattern on the spunbonded nonwoven fabric, with reference to JP 2017-206803 A. The evaluation results of the obtained spunbonded nonwoven fabric are shown in Table 1.
[0109] [Table 1]
[0110] The spunbonded nonwoven fabrics of Examples 1 to 6, which are formed with a striped pattern in which high brightness regions and low brightness regions are alternately arranged, and in which in the average brightness profile in the direction perpendicular to the striped pattern, the brightness difference between the apex and the adjacent bottom is 10 to 100, the pitch of the apex is 5 mm to 60 mm, and the fiber orientation based on the formation direction of the striped pattern is 45° or less, were excellent in design and excellent in unidirectional flexibility. On the other hand, the spunbonded nonwoven fabric without a striped pattern of Comparative Example 1, the nonwoven fabric of Comparative Example 2 with a small brightness difference between the apex and the adjacent bottom, the nonwoven fabric of Comparative Example 3 with a wide apex pitch, and the spunbonded nonwoven fabric of Comparative Example 4 with a narrow apex pitch and a fiber orientation of more than 45° based on the formation direction of the striped pattern, were inferior in design and flexibility.
[0111] Although the present invention has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention. [Industrial Applicability]
[0112] The spunbond nonwoven fabric of the present invention has excellent design, sufficient quality and strength, and excellent flexibility in at least one direction, and therefore can be suitably used for sanitary material applications such as disposable paper diapers, napkins, etc. In addition, since it has a striped pattern, it also has excellent wiping performance, and can be suitably used as a cleaning sheet. [Explanation of symbols]
[0113] 1: High brightness area 2: Low brightness area 3: Area for measuring the average luminance profile in the direction perpendicular to the stripe pattern direction 4: Direction of stripe pattern formation 5: Orthogonal to the stripe pattern direction
Claims
1. A spunbond nonwoven fabric having a striped pattern in which high luminance regions and low luminance regions are alternately arranged on at least one surface, wherein in an average luminance profile in a direction perpendicular to the formation direction of the striped pattern, the luminance difference between a peak and an adjacent bottom is 10 to 100, the pitch of the peaks is 5 mm to 60 mm, and the degree of fiber orientation based on the formation direction of the striped pattern is 0° to 45°, and further The spunbond nonwoven fabric has a basis weight of 10 g / m 2 to 100 g / m 2 , the difference in basis weight between the high luminance area and the low luminance area is 5 g / m 2 to 90 g / m 2 ; The difference between the thickness of the spunbond nonwoven fabric in the high brightness region and the thickness of the spunbond nonwoven fabric in the low brightness region is 0.03 mm to 1 mm.
2. The spunbond nonwoven fabric according to claim 1, wherein the difference between the fiber orientation degree in the high brightness region and the fiber orientation degree in the low brightness region is 0° to 5°.
3. 3. The spunbonded nonwoven fabric according to claim 1, wherein the average single fiber diameter of the fibers constituting the spunbonded nonwoven fabric is 6.5 μm to 14.5 μm.
Citation Information
Patent Citations
Nonwoven filament cloth having pattern and its production
JP1995109658A
wipe
JP2005526548A
Nonwoven fabric, absorbent article including the nonwoven fabric and method for producing the nonwoven fabric
JP2012214938A
Apparatus and method for producing nonwoven fabric composed of endless filament
JP2017206803A
Non-woven fabric
WO2007148497A1