Piezoelectric element

The piezoelectric element with a helical chiral polymer crystal and circular configuration addresses manufacturing complexity by converting shear deformation into expansion/contraction, enabling efficient use in various devices.

JP7589570B2Active Publication Date: 2024-11-26SEIKO EPSON CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021013649
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-01-29
Publication Date
2024-11-26
Estimated Expiration
2041-01-29

AI Technical Summary

Technical Problem

Braided piezoelectric elements have a complex structure, making them difficult to manufacture and handle as piezoelectric elements.

Method used

A piezoelectric element comprising a helical chiral polymer crystal with a piezoelectric layer, first and second electrode layers, and connection portions, configured to convert shear deformation into expansion/contraction deformation, utilizing a circular shape and uniaxial orientation of the c-axis within the plane.

Benefits of technology

Facilitates easy utilization of piezoelectricity for applications such as actuators, vibration generators, and sensors by simplifying the structure and enhancing manufacturing ease while maintaining effective deformation conversion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007589570000001
    Figure 0007589570000001
  • Figure 0007589570000002
    Figure 0007589570000002
  • Figure 0007589570000003
    Figure 0007589570000003
Patent Text Reader

Abstract

To provide a piezoelectric device that facilitates the use of piezoelectricity through conversion of shear deformation into expansion and contraction deformation.SOLUTION: A piezoelectric device comprises: a piezoelectric layer including helical chiral polymer crystal showing piezoelectricity; a first electrode layer; a second electrode layer; a first connection part provided on the first electrode layer on the opposite side of the piezoelectric layer; and a second connection part provided on the second electrode layer on the opposite side of the piezoelectric layer. When seen along a thickness direction of the piezoelectric layer, an overlapping portion where the piezoelectric layer, the first electrode layer, and the second electrode layer overlap each other has a round shape, and when seen along the thickness direction of the piezoelectric layer, the first connection part and the second connection part overlap the center of the overlapping portion.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piezoelectric element. [Background technology]

[0002] Piezoelectric polymers are used in various forms because of their unique processability as polymer materials. For example, Patent Document 1 discloses a braided piezoelectric element in which a piezoelectric fiber formed from a piezoelectric polymer is wound around and covered on the surface of a conductive fiber formed from a conductive material. In such a braided piezoelectric element, a piezoelectric fiber containing a piezoelectric polymer uniaxially oriented in the fiber axis direction is used. Patent Document 1 also discloses that the winding angle of the piezoelectric fiber with respect to the conductive fiber is an oblique direction of 15° to 75°. By setting the winding angle in such a range, a shear stress is generated in the piezoelectric fiber, and a large electric signal can be extracted through the conductive fiber by the piezoelectric effect. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] International Publication No. 2016 / 175321 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the braided piezoelectric element has a complex structure and is difficult to manufacture, and the braided piezoelectric element also has a special shape, which makes it difficult to handle as a piezoelectric element. [Means for solving the problem]

[0005] The piezoelectric element according to the application example of the present invention is a piezoelectric layer having a first surface and a second surface which are in a front-back relationship and which contains a helical chiral polymer crystal exhibiting piezoelectricity; a first electrode layer provided on the first surface of the piezoelectric layer; a second electrode layer provided on the second surface of the piezoelectric layer; a first connection portion provided on the first electrode layer on the opposite side to the piezoelectric layer; a second connection portion provided on the second electrode layer on the opposite side to the piezoelectric layer; Equipped with When viewed along a thickness direction of the piezoelectric layer, an overlapping portion where the piezoelectric layer, the first electrode layer, and the second electrode layer overlap each other has a circular shape, When viewed along the thickness direction of the piezoelectric layer, the first connection portion and the second connection portion overlap with the center of the overlapping portion. And, The helical chiral polymer crystal is a crystal having a helical molecular structure, When the axis of progression of the helical structure is the c-axis, the c-axis is uniaxially oriented within the plane of the piezoelectric layer. It is characterized by: [Brief description of the drawings]

[0006] [Figure 1] FIG. 1 is a perspective view showing a piezoelectric element according to an embodiment. [Diagram 2] 2 is a cross-sectional view of the piezoelectric element shown in FIG. [Diagram 3] FIG. 2 is a plan view of the piezoelectric element shown in FIG. [Figure 4A] FIG. 1 is a schematic diagram showing the molecular structure of polylactic acid crystals. [Figure 4B] FIG. 1 is a schematic diagram showing the molecular structure of polylactic acid crystals. [Diagram 5] FIG. 2 is a plan view showing only the laminate of FIG. [Figure 6] 6 is a plan view showing an example of a laminate including a piezoelectric element as a comparative example, in which the shape of the laminate in FIG. 5 is changed to a square. FIG. [Figure 7] 2 is a diagram showing the results of simulating the distribution of the amount of displacement of a laminate when a voltage is applied between a first electrode layer and a second electrode layer of the piezoelectric element shown in FIG. 1. FIG. [Figure 8]1 is an example of a θ-2θ profile obtained by θ-2θ measurement using an X-ray diffraction apparatus for a piezoelectric layer containing polylactic acid whose c-axis is uniaxially oriented. [Figure 9] FIG. 9 is an example of a pole figure obtained by fixing the 2θ position at 16.7° for the piezoelectric layer from which the θ-2θ profile shown in FIG. 8 was obtained. [Figure 10] FIG. 13 is a plan view showing a modified example of the piezoelectric element according to the embodiment. [Figure 11] FIG. 13 is a plan view showing a modified example of the piezoelectric element according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0007] The piezoelectric element of the present invention will now be described in detail with reference to the accompanying drawings. Fig. 1 is a perspective view showing a piezoelectric element according to an embodiment, Fig. 2 is a cross-sectional view of the piezoelectric element shown in Fig. 1, and Fig. 3 is a plan view of the piezoelectric element shown in Fig. 1.

[0008] 1. Piezoelectric element 1 and 2 includes a laminate 500 having a piezoelectric layer 200, a first electrode layer 300, and a second electrode layer 400. The piezoelectric layer 200 has a first surface 201 and a second surface 202 which are opposite surfaces. The first electrode layer 300 is provided on the first surface 201 of the piezoelectric layer 200. The second electrode layer 400 is provided on the second surface 202 of the piezoelectric layer 200.

[0009] The piezoelectric element 100 may include other components in addition to these components. For example, an adhesive layer or the like may be interposed between the piezoelectric layer 200 and the first electrode layer 300 and the second electrode layer 400. In addition, a protective film or the like may be provided to cover the laminate 500.

[0010] The laminate 500 shown in Figures 1 and 2 has a circular shape in plan view as shown in Figure 3. Specifically, the piezoelectric layer 200, the first electrode layer 300, and the second electrode layer 400 each have a circular shape in plan view and are the same size as each other.

[0011] Examples of circular shapes include perfect circles, ellipses, and ovals, but a perfect circle is preferred. A perfect circle is a shape that is circular and has a difference between the length of the major axis and the length of the minor axis that is 10% or less of the length of the major axis. The major axis is the longest axis that can be taken in a planar view, and the minor axis is an axis that passes through the midpoint of the major axis in a planar view and is perpendicular to the major axis.

[0012] A first wiring 800 and a second wiring 900 are connected to the piezoelectric element 100. One end of the first wiring 800 is connected to the center of the circular first electrode layer 300 via a first connection portion 600. One end of the second wiring 900 is connected to the center of the circular second electrode layer 400 via a second connection portion 700.

[0013] The other end of the first wiring 800 and the other end of the second wiring 900 are each connected to, for example, a power supply device (not shown). This allows a voltage to be applied between the first electrode layer 300 and the second electrode layer 400, causing the piezoelectric layer 200 to exhibit an inverse piezoelectric effect. In this case, the piezoelectric element 100 is used by being incorporated into a device such as an actuator, a vibration generating element, or an ultrasonic motor.

[0014] The other end of the first wiring 800 and the other end of the second wiring 900 may be connected to, for example, a charge detection device (not shown). This allows the charge generated by the piezoelectric effect in the piezoelectric layer 200 to be taken out from the first electrode layer 300 and the second electrode layer 400, and the charge amount to be detected by the charge detection device. Based on the detected charge amount, the force applied to the piezoelectric layer 200 can be obtained, or power required for switching or power generation can be generated. In this case, the piezoelectric element 100 is incorporated into devices such as various force sensors, such as tactile sensors and force sensors, various switches, and power generation elements. The piezoelectric element 100 may also be connected to a voltage detection device. This allows the voltage generated by the piezoelectric effect to be detected by the voltage detection device.

[0015] Examples of materials constituting the first electrode layer 300 and the second electrode layer 400 include metal materials such as simple metal elements such as gold, silver, platinum, copper, nickel, aluminum, indium, tin, zinc, and palladium, or alloys and intermetallic compounds containing these metal elements, as well as resin materials such as conductive polymers.

[0016] The average thickness t3 of the first electrode layer 300 and the average thickness t4 of the second electrode layer 400 shown in FIG. 2 are not particularly limited, but are each preferably 0.05 μm or more and 500 μm or less, and more preferably 0.50 μm or more and 300 μm or less.

[0017] For example, a bonding metal material such as solder or brazing material, a conductive paste, a conductive adhesive, or the like is used for the first connection portion 600 and the second connection portion 700. As an example, the first connection portion 600 shown in Fig. 2 is bonded or joined to both the first electrode layer 300 and the first wiring 800, and has a shape in which the diameter of the first wiring 800 is expanded. Similarly, as an example, the second connection portion 700 shown in Fig. 2 is bonded or joined to both the second electrode layer 400 and the second wiring 900, and has a shape in which the diameter of the second wiring 900 is expanded.

[0018] Examples of materials constituting the first connection portion 600 and the second connection portion 700 include metal materials such as simple metal elements such as gold, silver, platinum, copper, nickel, aluminum, indium, tin, zinc, and palladium, or alloys and intermetallic compounds containing these metal elements, as well as resin materials such as conductive polymers.

[0019] The constituent materials of the first connecting portion 600 and the second connecting portion 700 may be the same as the constituent materials of the first electrode layer 300 and the second electrode layer 400, or may be different.

[0020] The average thickness t2 of the piezoelectric layer 200 is not particularly limited, but is preferably 10 μm to 5000 μm, more preferably 30 μm to 1000 μm, and even more preferably 50 μm to 500 μm, so that the piezoelectric layer 200 has sufficient piezoelectric performance.

[0021] The piezoelectric layer 200 includes a helical chiral polymer crystal exhibiting piezoelectricity. A helical chiral polymer is a polymer whose molecular structure has a helical structure and has molecular optical activity. A helical chiral polymer crystal is a crystal of such a helical chiral polymer.

[0022] Examples of helical chiral polymers include polypeptides, cellulose derivatives, polylactic acid, polypropylene oxide, and poly-β-hydroxybutyric acid.

[0023] As described above, the helical chiral polymer crystal used in this embodiment is a crystal having a helical molecular structure, and in particular, when the axis of progression of the helical structure is the c-axis, it is preferable that the crystal is uniaxially oriented in the plane of the piezoelectric layer 200.

[0024] In such a piezoelectric layer 200, the c-axis of the helical chiral polymer is uniaxially oriented in-plane, so that it is possible to produce large polarization in the thickness direction of the piezoelectric layer 200. Therefore, it is possible to obtain a piezoelectric layer 200 in which application of an electric field and extraction of electric charge can be performed more efficiently using the first electrode layer 300 and the second electrode layer 400.

[0025] The piezoelectric layer 200 containing a helical chiral polymer whose c-axis is uniaxially oriented in-plane can be manufactured by an existing film manufacturing method such as a uniaxial stretching method. Specifically, the piezoelectric layer 200 can be manufactured by a method including a step of melt-kneading raw materials, forming them into a sheet by an extrusion molding method, and a step of uniaxially stretching the obtained sheet to obtain a stretched film. According to such a method, a stretched film in which the c-axis of the helical chiral polymer is uniaxially oriented in-plane can be obtained. This method is excellent in mass productivity, and therefore the cost of the piezoelectric layer 200 can be easily reduced.

[0026] Of these, the helical chiral polymer crystal is preferably a polylactic acid crystal. Since the polylactic acid crystal has a relatively high mechanical strength and excellent moldability, it is particularly useful as the helical chiral polymer crystal contained in the piezoelectric layer 200. In other words, by including the polylactic acid crystal, the mechanical strength and moldability of the piezoelectric layer 200 can be easily improved.

[0027] In the following, polylactic acid will be used as an example of a helical chiral polymer. Polylactic acid L (PLLA) and polylactic acid D (PDLA) are known as polylactic acids having optical activity. Here, polylactic acid L, particularly α-phase polylactic acid L, which is the most stable crystalline phase of polylactic acid L, will be used as an example. In the following explanation, polylactic acid L in α-phase will be simply referred to as "polylactic acid".

[0028] 4A and 4B are schematic diagrams each showing the molecular structure of a polylactic acid crystal. As shown in Figures 4A and 4B, the molecular structure of polylactic acid crystals has a helical structure. The crystal system of polylactic acid crystals is a rectangular crystal (orthorhombic crystal), and the length of the a-axis of the unit cell is about 1.06 nm, the length of the b-axis is about 0.61 nm, and the length of the c-axis is about 2.88 nm. Note that Figure 4A illustrates a plane of the polylactic acid crystal that includes the a-axis and the c-axis, and Figure 4B illustrates a plane of the polylactic acid crystal that includes the a-axis and the b-axis.

[0029] The piezoelectric layer 200 may contain polylactic acid crystals, but preferably contains polylactic acid crystals as a main material. The content of polylactic acid crystals in the piezoelectric layer 200 is preferably 30% by mass or more, more preferably 50% by mass or more, and even more preferably 70% by mass or more. In addition to polylactic acid crystals, the piezoelectric layer 200 may contain, for example, amorphous polylactic acid. In addition to the above-mentioned α-phase L-type polylactic acid, the piezoelectric layer 200 may contain L-type polylactic acid of metastable phases such as α' phase and β phase, or D-type polylactic acid.

[0030] Fig. 5 is a plan view showing only the laminate 500 of Fig. 1. Fig. 6 is a plan view showing an example of a laminate including a piezoelectric element as a comparative example, which is a plan view showing a laminate 500' obtained by changing the shape of the laminate 500 of Fig. 5 to a square.

[0031] In the laminate 500' shown in Fig. 6, the c-axis of the helical chiral polymer, for example the c-axis of polylactic acid, is oriented along the orientation direction Dc. In such a laminate 500', when a shear stress parallel to the c-axis is applied, as shown by the two arrows in Fig. 6, a rotational motion of the electric dipole of C=O is induced in the helical structure, and polarization appears in a direction intersecting with the shear plane including the two applied shear stress vectors S1. In other words, polarization appears in a direction intersecting with the plane on which the laminate 500' extends.

[0032] When an electric field is applied to the laminate 500' exhibiting such piezoelectricity in a direction intersecting the shear plane, shear deformation occurs in the laminate 500' due to the inverse piezoelectric effect. If the laminate 500' before deformation is a square as shown by the dashed line in FIG. 6, the laminate 500' after deformation becomes a parallelogram as shown by the solid line. This shear deformation is a deformation based on stress represented by two shear stress vectors S1, but since the action lines of the two shear stress vectors S1 are different from each other, it is not easy to utilize this deformation in a piezoelectric element including the laminate 500'. Specifically, the vertices P1, P2, P3, and P4 of the laminate 500' are displaced parallel to the shear stress vector S1 as shown by the displacements d1, d2, d3, and d4 in FIG. 6. Conventionally, piezoelectric elements utilizing shear deformation have been realized by processing into a special shape such as a braided piezoelectric element, but there were problems in terms of the complexity of the structure and the difficulty of manufacturing.

[0033] Therefore, in the piezoelectric element 100 according to this embodiment, as shown in Fig. 5, the overlapping portion 10 where the piezoelectric layer 200, the first electrode layer 300, and the second electrode layer 400 overlap each other, i.e., the laminate 500, is made circular. In Fig. 5, the laminate 500 is particularly made to be a perfect circle. When an electric field is applied to such a laminate 500 in a direction intersecting the shear plane, shear deformation occurs due to the inverse piezoelectric effect based on the shear stress vector S1 similar to that of the laminate 500' shown in Fig. 6. At this time, since the laminate 500 is circular, the shear deformation is converted into expansion and contraction deformation.

[0034] Specifically, in the laminate 500' of FIG. 6, the action lines of the displacements d1 and d4 occurring at the two vertices P1 and P4 facing each other are different from each other. Specifically, the direction of the displacement d1 and the direction of the displacement d4 are on different straight lines. More specifically, when a reference line (not shown) is drawn connecting the vertices P1 and P4, the angle between the direction of the displacement d1 and the reference line, and the angle between the direction of the displacement d4 and the reference line are each more than 20°. In addition, the action lines of the displacements d2 and d3 occurring at the other two vertices P2 and P3 facing each other are also different from each other. Specifically, the direction of the displacement d2 and the direction of the displacement d3 are on different straight lines. More specifically, when a reference line (not shown) is drawn connecting the vertices P2 and P3, the angle between the direction of the displacement d2 and the reference line, and the angle between the direction of the displacement d3 and the reference line are each more than 20°.

[0035] In contrast, in the laminate 500 of FIG. 5, the action lines of the displacements d5 and d8 occurring at the outer edge E are almost overlapped with each other. The displacement d5 is a displacement at the intersection P5 of the reference line L1 and the outer edge E of the laminate 500 before deformation. The displacement d8 is a displacement at the intersection P8 of the reference line L1 and the outer edge E of the laminate 500 before deformation. The action lines of the displacements d5 and d8 are almost overlapped with each other when the angle between the direction of the displacement d5 and the reference line L1 and the angle between the direction of the displacement d8 and the reference line L1 are each 20° or less. The reference line L1 is a straight line that forms an angle of 45° with respect to the orientation direction Dc and passes through the center O of the laminate 500 before deformation.

[0036] 5, the lines of action of the displacements d6 and d7 occurring at the outer edge E of the laminate 500 are almost overlapping each other. The displacement d6 is a displacement at an intersection P6 between the reference line L2 and the outer edge E of the laminate 500 before deformation. The displacement d7 is a displacement at an intersection P7 between the reference line L2 and the outer edge E of the laminate 500 before deformation. The lines of action of the displacements d6 and d7 are almost overlapping each other when the angle between the direction of the displacement d6 and the reference line L2 and the angle between the direction of the displacement d7 and the reference line L2 are each 20° or less. The reference line L2 is a straight line that is perpendicular to the reference line L1 and passes through the center O of the laminate 500 before deformation.

[0037] Furthermore, the directions of the displacements d5 and d8 are substantially opposite to each other, and the directions of the displacements d6 and d7 are also substantially opposite to each other. By such a mechanism, in the laminate 500, the shear deformation is converted into the expansion and contraction deformation.

[0038] 5 has a circular shape in plan view, the directions of displacements d5, d6, d7, and d8 intersect with the outer edge E at a large angle, specifically, the angles between the directions of displacements d5, d6, d7, and d8 shown by arrows in Fig. 5 and the outer edge E are preferably 70° or more and 90° or less. This makes it difficult for the outer edge E of the stacked body 500 to interfere with other members when the displacement of the stacked body 500 is used in a device or the like, improving ease of use.

[0039] In the expansion and contraction deformation shown in Fig. 5, when an electric field is applied to the piezoelectric layer 200 so that displacements d5 and d8 occur at the intersections P5 and P8 approaching the center O as shown in Fig. 5, displacements d6 and d7 occur at the intersections P6 and P7 moving away from the center O. Conversely, although not shown, when an electric field is applied to the piezoelectric layer 200 so that displacements occur at the intersections P5 and P8 moving away from the center O, displacements occur at the intersections P6 and P7 moving toward the center O.

[0040] On the other hand, the center O of the laminate 500 hardly displaces. Therefore, even if the center O is fixed, there is almost no effect on the expansion and contraction deformation of the laminate 500. Therefore, in the piezoelectric element 100 according to this embodiment, in order to fix the laminate 500, the first connection portion 600 and the second connection portion 700 are provided at positions overlapping the center O in a plan view.

[0041] The first connection portion 600 is provided on the side of the first electrode layer 300 opposite the piezoelectric layer 200, and is preferably a member having a higher rigidity than the first electrode layer 300. The second connection portion 700 is also provided on the side of the second electrode layer 400 opposite the piezoelectric layer 200, and is preferably a member having a higher rigidity than the second electrode layer 400. By sandwiching the laminate 500 between such members with high rigidity, the laminate 500 can be fixed with a simple structure without affecting the expansion and contraction deformation.

[0042] Moreover, the first connection part 600 electrically connects the first wiring 800 and the first electrode layer 300. The second connection part 700 electrically connects the second wiring 900 and the second electrode layer 400. Therefore, a voltage can be applied to the first electrode layer 300 and the second electrode layer 400 by the first wiring 800 and the second wiring 900, and the charge taken out by the first electrode layer 300 and the second electrode layer 400 can be sent to the first wiring 800 and the second wiring 900. In addition, the first connection part 600 and the second connection part 700 are hardly displaced as described above. Therefore, in the above structure, it is possible to reduce breakage or detachment of the first wiring 800 and the second wiring 900 due to vibration.

[0043] Furthermore, when the piezoelectric layer 200 is viewed in the thickness direction, the first connection portion 600 overlaps with the center O of the laminate 500 and is configured to be smaller than the first electrode layer 300. The first connection portion 600 overlapping with the center O means that the center O is located inside the range of the first connection portion 600. Furthermore, the first connection portion 600 being smaller than the first electrode layer 300 means that the first connection portion 600 is contained inside the range of the first electrode layer 300.

[0044] Furthermore, when the piezoelectric layer 200 is viewed in the thickness direction, the second connection portion 700 overlaps with the center O of the laminate 500 and is configured to be smaller than the second electrode layer 400. The second connection portion 700 overlapping with the center O means that the center O is located inside the range of the second connection portion 700. Additionally, the second connection portion 700 being smaller than the second electrode layer 400 means that the second connection portion 700 is contained inside the range of the second electrode layer 400.

[0045] With the above configuration, the laminate 500 can be fixed at any position in space by the first wiring 800 and the second wiring 900 via the first connecting portion 600 and the second connecting portion 700, and is electrically connected to the first wiring 800 and the second wiring 900. This makes the piezoelectric element 100 an element suitable for use in various devices, taking advantage of the piezoelectricity that accompanies expansion and contraction deformation.

[0046] Here, FIG. 7 is a diagram showing the results of simulating the distribution of the amount of displacement of the laminate 500 when a voltage is applied between the first electrode layer 300 and the second electrode layer 400 of the piezoelectric element 100 shown in FIG. 1. For the simulation, analysis simulation software Femtet made by Murata Software Co., Ltd. was used. In this simulation, the laminate 500 having a perfect circle is fixed by the first connection part 600 and the second connection part 700 (not shown), and when an electric field is applied to the piezoelectric layer 200 containing polylactic acid crystals in this state, the amount of displacement of each point of the laminate 500 is calculated. In FIG. 7, the orientation direction Dc of the piezoelectric layer 200 is indicated by an arrow. In addition, in FIG. 7, the outer edge of the laminate 500 before deformation is indicated by a solid line, and the amount of displacement of each point in the laminate 500 after deformation is indicated by a shading pattern.

[0047] As shown in Fig. 7, when the c-axis of polylactic acid is uniaxially oriented in the in-plane orientation direction Dc, the piezoelectric element 100 expands in a direction obliquely intersecting the orientation direction Dc, i.e., in the direction shown by the dashed line in Fig. 7, and deforms so as to contract in a direction intersecting the orientation direction Dc. Also, since the shading in Fig. 7 changes along the direction obliquely intersecting the orientation direction Dc, the displacement amounts of the points shown in Fig. 7 are distributed so as to be inclined along the direction obliquely intersecting the orientation direction Dc.

[0048] From the above simulation results, it is understood that in the piezoelectric element 100, shear deformation can be converted into expansion and contraction deformation.

[0049] Moreover, the in-plane uniaxial orientation of the c-axis of the helical chiral polymer in the piezoelectric layer 200 can be identified by acquiring and analyzing an X-ray diffraction profile of the piezoelectric layer 200. Specifically, first, a θ-2θ measurement is performed on the piezoelectric layer 200 using an X-ray diffractometer to acquire a θ-2θ profile.

[0050] FIG. 8 shows an example of a θ-2θ profile obtained by θ-2θ measurement in an X-ray diffraction apparatus for a piezoelectric layer containing polylactic acid whose c-axis is uniaxially oriented. When the c-axis of polylactic acid is uniaxially oriented, peaks corresponding to the (200) and (110) planes of polylactic acid are observed in the θ-2θ profile as shown in FIG. 8. These peaks are observed at 2θ=16.7°±1.0°. Note that this peak position is the peak position obtained by θ-2θ measurement using characteristic X-rays of CuKα1 with a wavelength of 1.5404 Å.

[0051] Next, a pole figure is obtained for this peak. FIG. 9 shows an example of a pole figure obtained by fixing the 2θ position at 16.7° for the piezoelectric layer from which the θ-2θ profile shown in FIG. 8 was obtained. In this pole figure, as shown by the dashed arrow in FIG. 9, contour lines indicating the diffraction intensity extend in a line shape so as to pass through the center where ψ=0°. If such contour line characteristics can be recognized in the pole figure shown in FIG. 9, it can be determined that the c-axis of polylactic acid is uniaxially oriented in the plane of the piezoelectric layer.

[0052] As described above, the piezoelectric element 100 according to this embodiment includes the piezoelectric layer 200, the first electrode layer 300, the second electrode layer 400, the first connection portion 600, and the second connection portion 700. The piezoelectric layer 200 has a first surface 201 and a second surface 202 that are opposite each other, and contains helical chiral polymer crystals that exhibit piezoelectricity. The first electrode layer 300 is provided on the first surface 201 of the piezoelectric layer 200. The second electrode layer 400 is provided on the second surface 202 of the piezoelectric layer 200. The first connection portion 600 is provided on the side of the first electrode layer 300 opposite the piezoelectric layer 200. The second connection portion 700 is provided on the side of the second electrode layer 400 opposite the piezoelectric layer 200.

[0053] When viewed along the thickness direction of the piezoelectric layer 200, an overlapping portion 10 where the piezoelectric layer 200, the first electrode layer 300, and the second electrode layer 400 overlap each other, i.e., the laminate 500, has a circular shape. When viewed along the thickness direction of the piezoelectric layer 200, the first connection portion 600 and the second connection portion 700 overlap the center O of the laminate 500 (the center of the overlapping portion 10).

[0054] According to this configuration, since the overlapping portion 10 has a circular shape, it is possible to convert the shear deformation caused by the piezoelectricity of the helical chiral polymer crystal into expansion and contraction deformation, thereby realizing a piezoelectric element 100 that makes it easy to utilize the piezoelectricity of the helical chiral polymer crystal.

[0055] Furthermore, it is preferable that the first connection portion 600 is smaller than the first electrode layer 300 when viewed along the thickness direction of the piezoelectric layer 200, and the second connection portion 700 is smaller than the second electrode layer 400 when viewed along the thickness direction of the piezoelectric layer 200.

[0056] Because the first connecting portion 600 and the second connecting portion 700 have the above-mentioned characteristics, the first connecting portion 600 and the second connecting portion 700 can fix the laminate 500 without hindering the expansion and contraction deformation occurring in the piezoelectric layer 200.

[0057] Such a piezoelectric element 100 is used in various devices that utilize expansion and contraction deformation, such as actuators, vibration generating elements, ultrasonic motors, tactile sensors, force sensors, power generating elements, and various switches.

[0058] Furthermore, the piezoelectric element 100 can be electrically and mechanically connected to the laminate 500 by the first connecting portion 600 and the second connecting portion 700. Therefore, when the piezoelectric element 100 is incorporated into various devices, the fixing structure of the piezoelectric element 100 can be simplified. As a result, by using the piezoelectric element 100, the degree of freedom in designing the device can be easily increased.

[0059] Moreover, it is preferable that the first connecting portion 600 has a higher rigidity than the first electrode layer 300, and the second connecting portion 700 has a higher rigidity than the second electrode layer 400. This makes the first connecting portion 600 and the second connecting portion 700 particularly resistant to deformation, and allows the laminate 500 to be fixed more stably.

[0060] The rigidity of the first connection portion 600 is higher than that of the first electrode layer 300, which means that the bending rigidity of the first connection portion 600 is higher than that of the first electrode layer 300. Similarly, the rigidity of the second connection portion 700 is higher than that of the second electrode layer 400, which means that the bending rigidity of the second connection portion 700 is higher than that of the second electrode layer 400. The bending rigidity is expressed as the product of Young's modulus and the second moment of area, and the second moment of area is smaller if the thickness is smaller in the bending direction. Therefore, in this embodiment, the thickness of the first connection portion 600 and the second connection portion 700 is made sufficiently thicker than that of the first electrode layer 300 and the second electrode layer 400 in the thickness direction of the laminate 500.

[0061] 2, when the thickness of the first connection portion 600 is t6, the thickness t6 is preferably at least twice the average thickness t3 of the first electrode layer 300, and more preferably at least 10 times and at most 1000 times. This makes it possible to make the bending rigidity of the first connection portion 600 greater than the bending rigidity of the first electrode layer 300.

[0062] Furthermore, when the thickness of the second connection portion 700 is t7, the thickness t7 is preferably at least twice the average thickness t4 of the second electrode layer 400, and more preferably at least 10 times and at most 1000 times. This makes it possible to make the bending rigidity of the second connection portion 700 greater than the bending rigidity of the second electrode layer 400.

[0063] 3, the radius of the laminate 500 (overlapping portion 10) is R1, and the circle having a radius of r1 from the center O is C1. The radius r1 is 20% of the radius R1. When viewed along the thickness direction of the piezoelectric layer 200, the first connection portion 600 is preferably disposed inside the circle C1 as shown in FIG.

[0064] With this configuration, it is possible to prevent the area occupied by the first connection portion 600 from becoming larger than necessary. In other words, the area occupied by the first connection portion 600 can be set to a size that is necessary and sufficient for fixing the laminate 500. This makes it possible to realize a piezoelectric element 100 that can effectively utilize the piezoelectricity that accompanies expansion and contraction deformation.

[0065] Although not shown, it is preferable that the second connection portion 700 is also disposed inside the circle C1, thereby making it possible to prevent the area occupied by the second connection portion 700 from becoming larger than necessary.

[0066] The radius r1 is preferably less than 20% of the radius R1, and more preferably less than 15% of the radius R1.

[0067] 2. Variations Next, a piezoelectric element according to a modified example will be described.

[0068] 10 and 11 are plan views showing modified examples of the piezoelectric element 100 according to the embodiment.

[0069] The following describes the modified example, but in the following description, the differences from the above embodiment will be mainly described, and the description of the similarities will be omitted. Note that in Figures 10 and 11, the same reference numerals are used for the same configurations as the above embodiment.

[0070] The piezoelectric element 100A shown in FIG. 10 is similar to the piezoelectric element 100 according to the above embodiment, except that the shape of the piezoelectric layer 200A is different from that of the first electrode layer 300.

[0071] That is, the piezoelectric layer 200A shown in Fig. 10 has a square shape in plan view. The first electrode layer 300 and the second electrode layer (not shown) are each contained within the range of the piezoelectric layer 200A. Therefore, the overlapping portion 10 where the piezoelectric layer 200A, the first electrode layer 300, and the second electrode layer overlap each other is circular, as in the above embodiment. Therefore, the piezoelectric element 100A shown in Fig. 10 also has the effect of converting shear deformation into expansion and contraction deformation, that is, the same effect as in the above embodiment.

[0072] In this way, the first electrode layer 300 shown in Fig. 10 and the second electrode layer (not shown) are each circular. This provides the above-mentioned effects, and has the advantage that the piezoelectric layer 200A shown in Fig. 10 can be easily manufactured since it can have any shape. Therefore, the shape of the piezoelectric layer 200A is not limited to a square, and may be any shape.

[0073] The piezoelectric element 100B shown in FIG. 11 is similar to the piezoelectric element 100 according to the above embodiment, except that the shape of the first electrode layer 300B is different from that of the piezoelectric layer 200.

[0074] That is, the first electrode layer 300B shown in FIG. 11 has a square shape in plan view. Although not shown, the second electrode layer also has the same shape in plan view as the first electrode layer 300B. Furthermore, the piezoelectric layer 200 is contained inside the range of the first electrode layer 300B. Therefore, the overlapping portion 10 where the piezoelectric layer 200, the first electrode layer 300B, and the second electrode layer overlap each other is circular, as in the above embodiment. Therefore, the piezoelectric element 100B shown in FIG. 11 also has the effect of converting shear deformation into expansion and contraction deformation, that is, the same effect as in the above embodiment.

[0075] In this way, the piezoelectric layer 200 shown in Fig. 11 has a circular shape. This provides the above-mentioned effect, and has the advantage that the first electrode layer 300B shown in Fig. 11 and the second electrode layer (not shown) can be of any shape, making them easy to manufacture. Therefore, the shapes of the first electrode layer 300B and the second electrode layer are not limited to squares and may be any shape.

[0076] Although not shown in FIG. 11, the first electrode layer 300B shown in FIG.

[0077] 11, the piezoelectric layer 200 is disposed inside the first electrode layer 300B and the second electrode layer and is protected from the outside. Therefore, the piezoelectric element 100B has an advantage that the piezoelectric layer 200 is less susceptible to damage and is therefore more reliable.

[0078] The piezoelectric element of the present invention has been described above based on the illustrated embodiment, but the piezoelectric element of the present invention is not limited to the embodiment. For example, the various parts of the embodiment may be replaced with any configuration having similar functions, or any component may be added to the embodiment. [Explanation of symbols]

[0079] 10...overlapped portion, 100...piezoelectric element, 100A...piezoelectric element, 100B...piezoelectric element, 200...piezoelectric layer, 200A...piezoelectric layer, 201...first surface, 202...second surface, 300...first electrode layer, 300B...first electrode layer, 400...second electrode layer, 500...laminated body, 500'...laminated body, 600...first connection portion, 700...second connection portion, 800...first wiring, 900...second wiring, C1...circle, Dc...orientation direction, E...outer Edge, L1...reference line, L2...reference line, O...center, P1...vertex, P2...vertex, P3...vertex, P4...vertex, P5...intersection, P6...intersection, P7...intersection, P8...intersection, R1...radius, S1...stress vector, d1...displacement, d2...displacement, d3...displacement, d4...displacement, d5...displacement, d6...displacement, d7...displacement, d8...displacement, r1...radius, t2...average thickness, t3...average thickness, t4...average thickness, t6...thickness, t7...thickness

Claims

1. a piezoelectric layer having a first surface and a second surface which are in a front-back relationship and which contains helical chiral polymer crystals exhibiting piezoelectricity; a first electrode layer provided on the first surface of the piezoelectric layer; a second electrode layer provided on the second surface of the piezoelectric layer; a first connection portion provided on a side of the first electrode layer opposite to the piezoelectric layer; a second connection portion provided on the second electrode layer on a side opposite to the piezoelectric layer; Equipped with When viewed along a thickness direction of the piezoelectric layer, an overlapping portion where the piezoelectric layer, the first electrode layer, and the second electrode layer overlap each other has a circular shape, When viewed along a thickness direction of the piezoelectric layer, the first connection portion and the second connection portion overlap with a center of the overlapping portion, The helical chiral polymer crystal is a crystal having a helical molecular structure, A piezoelectric element, characterized in that, when the axis of progression of the helical structure is defined as a c-axis, the c-axis is uniaxially oriented within the plane of the piezoelectric layer.

2. the first connection portion has a higher rigidity than the first electrode layer; The piezoelectric element according to claim 1 , wherein the second connection portion has a rigidity higher than that of the second electrode layer.

3. the first connection portion is smaller than the first electrode layer when viewed in a thickness direction of the piezoelectric layer; The piezoelectric element according to claim 1 , wherein the second connection portion is smaller than the second electrode layer when viewed in a thickness direction of the piezoelectric layer.

4. 4. The piezoelectric element according to claim 1, wherein the first connection portion is disposed inside a circle having a radius that is 20% of the radius of the overlapping portion.

5. 5. The piezoelectric element according to claim 1, wherein the helical chiral polymer crystal is a polylactic acid crystal.

6. 6. The piezoelectric element according to claim 1, wherein the first electrode layer and the second electrode layer are circular.

7. 7. The piezoelectric element according to claim 1, wherein the piezoelectric layer has a circular shape.

Citation Information

Patent Citations

  • Piezo-electric transformer element

    JP1998084143A

  • Piezoelectric transformer

    JP2000315828A

  • Flexible piezoelectric element

    JP2002076459A

  • Piezoelectric sheet, method for manufacturing piezoelectric sheet, and manufacturing apparatus

    WO2010147074A1

  • Pressing sensor and electronic device

    WO2016027818A1