Tank manufacturing method and tank manufacturing mold
The use of a mold with ribs forming flow paths that differ from fiber directions in the tank manufacturing process addresses the issue of incomplete resin impregnation, ensuring thorough fiber impregnation and improved manufacturing efficiency.
Patent Information
- Application Number
- JP2022079335
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2022-05-13
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2042-05-13
AI Technical Summary
In conventional tank manufacturing methods using RTM, variations in the shape of the intermediate product can cause the fibers to not be sufficiently impregnated with resin due to contact between the mold and the intermediate product, leading to incomplete resin application.
The method involves using a mold with protruding ribs on its inner surface that form flow paths different from the fiber direction, allowing resin to flow through and impregnate the fibers even when the mold and intermediate product come into contact, and ensuring the fiber width is larger than the channel width to prevent burial of fibers in the flow paths.
This approach ensures complete resin impregnation of fibers, even in areas where the mold and intermediate product contact, by creating flow paths that allow resin to flow freely and preventing fiber burial, thus enhancing the manufacturing process's efficiency and quality.
Smart Images

Figure 0007589711000001 
Figure 0007589711000002 
Figure 0007589711000003
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for manufacturing a tank and a mold for manufacturing the tank. [Background technology]
[0002] 2. Description of the Related Art Conventionally, in the manufacturing method of a tank, a technique is known in which a fiber reinforced resin layer and a resin layer are formed on the outer periphery of a liner by a resin transfer molding (RTM) method (Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2020-118288 A Summary of the Invention [Problem to be solved by the invention]
[0004] Due to variations in shape that occur in the intermediate tank product formed by wrapping fibers around the outer surface of the liner, when the mold and the intermediate product come into contact with each other, it may not be possible to sufficiently impregnate the fibers at the contact area with resin. [Means for solving the problem]
[0005] The present disclosure can be realized in the following forms.
[0006] (1) According to one embodiment of the present disclosure, a method for manufacturing a tank is provided. The method for manufacturing a tank includes a preparation step of preparing a preform in which multiple layers of fiber bundles are wound around the outer surface of a liner that forms an internal space of the tank, and a mold, and an impregnation step of injecting a resin into the mold in an arrangement state in which the preform is arranged in the mold to impregnate the fiber bundle with the resin, the mold includes a mold body portion, a plurality of ribs that protrude from the inner surface of the mold body portion and face the fiber bundle of the outermost layer in the arrangement state, and a flow path portion formed between a first rib and a second rib as the ribs adjacent to each other, through which the resin flows, and in the arrangement state, the fiber direction in which the fiber bundle in the outermost layer extends is different from the flow path direction in which the flow path portion extends. According to this embodiment, the tank is manufactured using a mold having a plurality of ribs that protrude from the inner surface of the mold body portion and a flow path portion formed by the ribs adjacent to each other. In this case, since the fiber direction and the flow path direction are different in the arrangement of the preform, it is possible to prevent the fiber bundle from being buried in the flow path section. As a result, even if the preform comes into contact with the inner surface of the mold due to the variation in shape of the preform, the fiber bundle at the contact area can be sufficiently impregnated with the resin by circulating the resin in the flow path section. (2) In the above embodiment, when the distance between the first rib and the second rib is defined as the flow path width of the flow path portion and the width of the fiber bundle is defined as the fiber width, the preparation step may include a step of winding the fiber bundle having the fiber width larger than the flow path width around the preform to form the outermost layer. According to this embodiment, the fiber width can be made larger than the flow path width in the impregnation step. This can further prevent the fiber bundle forming the outermost layer from being buried in the flow path portion. (3) In the above embodiment, the mold body may have a cylindrical body and two dome portions provided at both ends of the body, the diameter of which decreases with increasing distance from the body, and the rib may be formed on the inner surface of the body. According to this embodiment, in the state in which the preform is arranged, the gap formed between the preform and the inner surface of the mold is smaller in the body than in the cylindrical portion. Therefore, by forming the rib on the inner surface of the body, the flow path of the resin can be more reliably secured using the flow path portion. Therefore, it is possible to easily impregnate the fiber bundle with the resin in the body. (4) According to another embodiment of the present disclosure, a tank manufacturing mold is provided. The tank manufacturing mold includes a mold body, a plurality of ribs facing the fiber bundle of the outermost layer in an arrangement state in which a preform protruding from the inner surface of the mold body and having a plurality of layers of fiber bundles wound around the outer surface of a liner forming an internal space of a tank is arranged in the mold, and a flow path portion formed between a first rib and a second rib as the ribs adjacent to each other, through which a resin to be impregnated in the fiber bundle flows in the arrangement state, and in the arrangement state, the fiber direction in which the fiber bundle in the outermost layer extends is different from the flow path direction in which the flow path portion extends. According to this embodiment, the tank manufacturing mold includes a plurality of ribs protruding from the inner surface of the mold body, and a flow path portion formed by the ribs adjacent to each other. In the arrangement state of the preform, the fiber direction and the flow path direction are different, so that it is possible to suppress the fiber bundle from being buried in the flow path portion. As a result, even if the preform comes into contact with the inner surface of the mold due to shape variations in the preform, the resin can be circulated through the flow path section, allowing the fiber bundles at the contact area to be sufficiently impregnated with resin. The present disclosure may be realized in various forms other than the above-described tank manufacturing method and tank manufacturing mold, for example, in the form of a tank manufacturing device including a tank manufacturing mold. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a diagram for explaining a schematic configuration of a preform and a tank. [Diagram 2] FIG. 2 is a diagram showing a schematic configuration of a tank manufacturing apparatus. [Diagram 3] 6 is a flowchart showing a method for manufacturing a tank using the manufacturing apparatus. [Figure 4] FIG. 2 is a perspective view showing the inside of the tank manufacturing mold according to the first embodiment, as seen from the outside. [Diagram 5] Cross-sectional view of FIG. 4 along line 5-5. [Figure 6] FIG. 6 is an enlarged view of the first region of FIG. 5 . [Figure 7] FIG. 3 is a diagram showing a schematic external shape of a rib in the first embodiment. [Figure 8] FIG. 4 is a diagram showing the relationship between the fiber direction and the flow path direction in the first embodiment. [Figure 9] FIG. 6 is an enlarged view of the second region of FIG. 5 . [Figure 10] FIG. 4 is a diagram for explaining a detailed configuration of a through hole. [Figure 11] FIG. 11 is a perspective view showing the inside of a tank manufacturing mold according to a second embodiment, as seen from the outside. [Figure 12] FIG. 11 is a diagram showing the relationship between the fiber direction and the flow path direction in the second embodiment. [Figure 13] FIG. 11 is a perspective view showing the inside of a tank manufacturing mold according to a third embodiment, as seen from the outside. [Figure 14] FIG. 13 is a diagram showing the relationship between the fiber direction and the flow path direction in the third embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] A. First embodiment: A-1. Preform and tank configuration: Fig. 1 is a diagram for explaining the schematic configuration of a preform 120 and a tank 100. The tank 100 shown in the right diagram of Fig. 1 is manufactured by processing the preform 120 shown in the left diagram of Fig. 1. In Fig. 1, step numbers corresponding to each process (step S1 to step S8) in the manufacturing method of the tank 100 (Fig. 3 described later) are given.
[0009] FIG. 1 shows a cross-section of the preform 120 and the tank 100 along the central axis O. FIG. 1 shows an X-axis, a Y-axis, and a Z-axis as mutually perpendicular axes. The directions of the arrows of the X-axis, Y-axis, and Z-axis indicate the positive directions along the X-axis, Y-axis, and Z-axis, respectively. The positive directions along the X-axis, Y-axis, and Z-axis are respectively the +X direction, +Y direction, and +Z direction. The directions opposite to the directions of the arrows of the X-axis, Y-axis, and Z-axis are the negative directions along the X-axis, Y-axis, and Z-axis. The negative directions along the X-axis, Y-axis, and Z-axis are respectively the -X direction, -Y direction, and -Z direction. The directions along the X-axis, Y-axis, and Z-axis, regardless of whether they are positive or negative, are called the X direction, Y direction, and Z direction, respectively.
[0010] In this embodiment, the X direction is a direction along the central axis O of the tank 100. The Y direction is a direction along the direction of gravity in an arrangement posture of the tank 100 described below. The -Y direction coincides with the direction of gravity in the arrangement posture. The Y direction and the Z direction coincide with the radial direction CD of the tank 100. In the figures and explanations shown hereinafter, in the radial direction CD of the tank 100, the side approaching the central axis O is referred to as the radial inner side, and the side away from the central axis O is referred to as the radial outer side.
[0011] The tank 100 is mounted on, for example, a fuel cell vehicle and is used to store hydrogen gas under high pressure to be supplied to the fuel cell. As shown in the right diagram of FIG. 1, the tank 100 includes a liner 10, a reinforcing layer 90, a valve-side nozzle 181, and an end-side nozzle 182.
[0012] The liner 10 is a hollow container that forms an internal space 10p for storing a fluid such as hydrogen gas. The liner 10 is formed of a resin having gas barrier properties such as a polyamide resin. The central axis of the liner 10 is the same as the central axis O of the tank 100.
[0013] The reinforcing layer 90 is a layer for reinforcing the liner 10. The reinforcing layer 90 covers the outer periphery of the liner 10. The reinforcing layer 90 includes a fiber reinforced resin layer 15 and a resin layer 17.
[0014] The fiber reinforced resin layer 15 covers the outer surface 10b of the liner 10. The material forming the fiber reinforced resin layer 15 is, for example, a fiber reinforced resin such as CFRP (Carbon Fiber Reinforced Plastics). CFRP is formed by impregnating carbon fibers with a thermosetting resin such as an epoxy resin and then thermally curing the resin.
[0015] The resin layer 17 covers at least a part of the outer surface 15b of the fiber reinforced resin layer 15. The resin layer 17 is formed of the same resin as that impregnated into the fibers in the process of forming the fiber reinforced resin layer 15. In this embodiment, the fiber reinforced resin layer 15 and the resin layer 17 are formed by a resin transfer molding (RTM) method (hereinafter, RTM method) using a tank manufacturing mold 2 (FIG. 2 described later). Details of the method of forming the fiber reinforced resin layer 15 and the resin layer 17 by the RTM method will be described later. The resin layer 17 has a plurality of through holes 170 penetrating in the thickness direction. Details of the through holes 170 will be described later. The types of fiber material and thermosetting resin as materials for forming the reinforcing layer 90 are not limited to those mentioned above. The fiber material used to form the reinforcing layer 90 may include, for example, glass fiber.
[0016] The container body 95 of the tank 100 is composed of the liner 10 and the reinforcing layer 90. The container body 95 has a cylindrical portion 950, a first spherical portion 951, and a second spherical portion 952. The cylindrical portion 950 is formed by a part of the liner 10 and the reinforcing layer 90. The cylindrical portion 950 has a cylindrical shape.
[0017] The first spherical portion 951 and the second spherical portion 952 are portions of the container body 95 other than the cylindrical portion 950, and are provided at both ends of the cylindrical portion 950. Specifically, the first spherical portion 951 is provided in the cylindrical portion 950, continuous with one end 950r in the axial direction OD along the central axis O. The shape of the first spherical portion 951 is a dome shape (spherical shape) protruding from one end 950r of the cylindrical portion 950 toward the valve-side base 181. The diameter of the first spherical portion 951 decreases with increasing distance from the cylindrical portion 950. The tip portion 10r of the liner 10 in the first spherical portion 951 is curved so as to enter the internal space 10p side. The curved tip portion 10r of the liner 10 forms an opening 10d.
[0018] The second spherical portion 952 is provided continuously to the other end 950s, which is the end opposite to the one end 950r, of the cylindrical portion 950. The second spherical portion 952 has a dome shape (spherical shape) protruding from the other end 950s of the cylindrical portion 950 toward the end side base 182. The diameter of the second spherical portion 952 decreases with increasing distance from the cylindrical portion 950.
[0019] The valve side nozzle 181 is attached to the opening 10d. The shape of the valve side nozzle 181 is generally cylindrical so as to connect the internal space 10p of the liner 10 with the outside. The valve side nozzle 181 functions as an inlet and outlet for fluids such as hydrogen gas stored in the internal space 10p.
[0020] The end side nozzle 182 is a member for closing the internal space 10p of the liner 10 on the other end 950s side. The end side nozzle 182 is provided on the second spherical portion 952 so as to be exposed to both the inside and the outside of the tank 100. The shape of the end side nozzle 182 is a cylindrical shape with a part of it being closed in order to close the internal space 10p of the liner 10.
[0021] On the other hand, as shown in the left diagram of Fig. 1, the preform 120 includes a liner 10, a fiber layer 121 in which multiple layers of fiber bundles 12 are wound around the outer surface 10b of the liner 10, a valve side nozzle 181, and an end side nozzle 182. The configurations of the liner 10, the valve side nozzle 181, and the end side nozzle 182 are the same as those of the tank 100 shown in the right diagram of Fig. 1. In other words, the preform 120 is an intermediate product in the manufacturing process of the tank 100.
[0022] The fiber layer 121 is formed by winding the fiber bundle 12 in multiple layers by at least one of helical winding and hoop winding so as to cover the outer surface 10b of the liner 10. The "fiber bundle 12" referred to here refers to an assembly of fibers in which a large number of single fibers having a diameter of about several micrometers are bundled together. The "helical winding" referred to here refers to a method of winding the fiber bundle 12 around the liner 10 so that the winding angle (fiber orientation) of the fiber bundle 12 with respect to the central axis O is greater than 0 degrees and smaller than 90 degrees. In the helical winding, for example, the fiber bundle 12 is wound so as to extend from one spherical portion (e.g., the first spherical portion 951) of the liner 10 through the cylindrical portion 950 to the other spherical portion (e.g., the second spherical portion 952). The "hoop winding" refers to a method of winding the fiber bundle 12 around the liner 10 so that the winding angle of the fiber bundle 12 with respect to the central axis O is approximately 90 degrees. In the hoop winding, the fiber bundle 12 is wound around the cylindrical portion 950 while moving the winding position parallel to the central axis O. The innermost layer 12a of the fiber layer 121 is in contact with the outer surface 10b of the liner 10. The outermost layer 12b of the fiber layer 121 forms the outer surface of the preform 120.
[0023] A-2. Tank manufacturing equipment configuration: FIG. 2 is a diagram showing a schematic configuration of a manufacturing apparatus 1 for a tank 100. FIG. 2 shows a state in which a preform 120 is arranged in a tank manufacturing mold 2. The manufacturing apparatus 1 is an apparatus for manufacturing the tank 100 shown in the right diagram of FIG. 1 from the preform 120 shown in the left diagram of FIG. 1 by the RTM method. Specifically, the manufacturing apparatus 1 impregnates a fiber layer 121 of the preform 120 with a resin by the RTM method, and then hardens the resin to manufacture the tank 100 in which a reinforcing layer 90 is formed on the outer periphery side of the liner 10. In this embodiment, the reinforcing layer 90 is formed using a thermosetting resin.
[0024] The manufacturing apparatus 1 includes a tank manufacturing mold 2, a support mechanism 208, a temperature adjustment device 40, a vacuum pump 50, a resin reservoir 64, a pressurizing device 60, a valve 62, a control device 70, and a drive mechanism 80.
[0025] The tank manufacturing mold 2 includes a pair of a first mold 21 and a second mold 22 that form a mold body 20, a placement chamber 200 that places the preform 120, a plurality of ribs 23 (not shown), and a flow path portion 27 (not shown). The details of the ribs 23 and the flow path portion 27 (not shown) will be described later.
[0026] The first die 21 and the second die 22 face each other. The first die 21 is disposed lower in the direction of gravity (-Y direction side) than the second die 22. Therefore, in this embodiment, the first die 21 is a lower die, and the second die 22 is an upper die. In the following, when there is no need to distinguish between the first die 21 and the second die 22, they will simply be referred to as the "mold body 20."
[0027] The first mold 21 is a fixed mold installed on a pedestal or the like. The first mold 21 has a first mold opposing wall 211, a first mold bottom wall 212, a first mold recess 215, a first mold tube portion 218, and a first gate 219. The first mold opposing wall 211 is a wall surface facing the second mold 22. The first mold bottom wall 212 is a wall surface facing the first mold opposing wall 211 in parallel with a gap therebetween. The first mold bottom wall 212 is fixed to, for example, a pedestal (not shown). The first mold recess 215 is a recess in which a part of the first mold opposing wall 211 is recessed toward the first mold bottom wall 212 side. The first mold recess 215 has a first mold bottom surface 216 and two first mold connection surfaces 217m, 217n, and is shaped such that the +Y direction side where the second mold 22 is located is open. The first mold connection surfaces 217 are located on both ends of the first mold bottom surface 216. The first mold pipe section 218 is a gas flow path formed inside the first mold 21 in order to evacuate the placement chamber 200 with the vacuum pump 50. The first gate 219 is an opening formed in the first mold bottom surface 216 of the first mold recess 215. In other words, the first mold pipe section 218 enables vacuum degassing by the vacuum pump 50 via the first gate 219.
[0028] The second die 22 is a movable die configured to be able to be pressed toward the first die 21. The second die 22 has a second die opposing wall 221, a second die top wall 222, a second die recess 225, a second die tube portion 228, and a second gate 229. The second die opposing wall 221 is a wall surface facing the first die opposing wall 211. The second die top wall 222 is a surface facing the second die opposing wall 221 in parallel with a gap. The second die recess 225 is a recess in which a part of the second die opposing wall 221 is recessed toward the second die top wall 222 side. The second die recess 225 has a second die top surface 226 and two second die connection surfaces 227m, 227n, and is shaped such that the -Y direction side where the first die 21 is located is open. The second die connection surfaces 227 are located on both end sides of the second die top surface 226. That is, the inner surface 20a of the mold body 20 is formed by the first mold bottom surface 216 and the first mold connection surface 217 of the first mold recess 215, and the second mold top surface 226 and the second mold connection surface 227 of the second mold recess 225. The second mold pipe portion 228 is a flow path formed inside the second mold 22 to allow the resin supplied from the resin reservoir 64 to flow to the placement chamber 200. The second gate 229 is an opening formed in the second mold top surface 226 of the second mold recess 225. That is, the second mold pipe portion 228 communicates the valve 62 and the resin reservoir 64 side with the placement chamber 200 side via the second gate 229. In FIG. 2, the direction in which the resin flows (hereinafter, the flow direction) is indicated by an arrow.
[0029] The placement chamber 200 is a space for placing the preform 120 between the first die 21 and the second die 22. The placement chamber 200 is an internal space of the tank manufacturing mold 2 that is formed by the first die recess 215 and the second die recess 225 when the first die 21 and the second die 22 are clamped together (hereinafter, referred to as the mold clamped state). In other words, the placement chamber 20 is formed inside the mold main body 20 when the mold main body 20 is in the mold clamped state.
[0030] The first mold recess 215 and the second mold recess 225 are each formed to have a shape that matches the shape of the preform 120. Specifically, the tank manufacturing mold 2 includes a cylindrical body portion 205 and two dome portions 201, 202 that are provided on both ends of the body portion 205 and that decrease in shape with increasing distance from the body portion 205.
[0031] The body portion 205 accommodates the cylindrical portion 950 of the preform 120. The body portion 205 is a portion of the mold body portion 20 that includes the first mold bottom surface 216 and the second mold top surface 226. Therefore, in a state in which the preform 120 is placed in the placement chamber 200 (hereinafter, the placement state) and in a mold clamping state, both the first mold bottom surface 216 and the second mold top surface 226 face the cylindrical portion 950 of the preform 120.
[0032] The first dome portion 201 accommodates the first spherical portion 951 of the preform 120. The first dome portion 201 is a portion of the mold body 20 that includes the first mold connection surface 217m and the second mold connection surface 227m. Therefore, when the preform 120 is arranged and the mold body 20 is clamped, both the first mold connection surface 217m and the second mold connection surface 227m face the first spherical portion 951 of the preform 120.
[0033] The second dome portion 202 accommodates the second spherical portion 952 of the preform 120. The second dome portion 202 is a portion of the mold body 20 that includes the first mold connection surface 217n and the second mold connection surface 227n. Therefore, when the preform 120 is arranged and the mold body 20 is clamped, both the first mold connection surface 217n and the second mold connection surface 227n face the second spherical portion 952 of the preform 120.
[0034] In a state where the preform 120 is placed in the placement chamber 200 (hereinafter, the placement state) and in a clamped state, the first mold bottom surface 216 and the second mold top surface 226 both face the cylindrical portion 950 of the preform 120. In addition, in the placement state of the preform 120, the first mold connection surface 217 and the second mold connection surface 227 both face the spherical portions 951, 952.
[0035] In the arrangement state of the preform 120, the support mechanism 208 supports the preform 120 from both ends, that is, one end 120r where the valve-side nozzle 181 is located and the other end 120s where the end-side nozzle 182 is located.
[0036] The temperature adjustment device 40 controls the temperature of the tank manufacturing mold 2. In response to a command from the control device 70, the temperature adjustment device 40 sets the temperature of the mold body 20 to a temperature lower than the curing temperature of the resin, for example, until the impregnation of the fiber layer 121 with the resin is completed. Then, after the impregnation of the fiber layer 121 with the resin is completed, the temperature adjustment device 40 sets the temperature of the mold body 20 to a temperature equal to or higher than the curing temperature of the resin. In addition, when the reinforcing layer 90 is formed of a resin other than a thermosetting resin, the manufacturing apparatus 1 may include a curing device for curing the resin and a control device for the curing device instead of the temperature adjustment device 40. In the case of forming the reinforcing layer 90 with a photocurable resin that is cured by ultraviolet light or the like, the manufacturing apparatus 1 includes, for example, a light source that irradiates ultraviolet light as a curing device and a control device that controls the lighting of the light source.
[0037] The vacuum pump 50 is a degassing device for evacuating and degassing the placement chamber 200 when the preform 120 is placed therein and the mold body 20 is clamped. The operation of the vacuum pump 50 is controlled by the control device 70.
[0038] The resin reservoir 64 is a reservoir chamber that reserves the resin to be supplied to the placement chamber 200. The resin reservoir 64 is connected to the second mold pipe portion 228 via a valve 62. The resin reservoir 64 is also connected to a pressurizing device 60.
[0039] The pressurizing device 60 pressurizes the resin stored in the resin reservoir 64, thereby causing the resin to flow from the resin reservoir 64 to the placement chamber 200. The pressurizing device 60 is disposed upstream in the flow direction from the resin reservoir 64. The driving of the pressurizing device 60 is controlled by the control device 70.
[0040] The valve 62 is an opening / closing valve for switching between a flow state in which the resin flows from the resin reservoir 64 to the second mold pipe section 228 and a non-flow state in which the resin does not flow from the resin reservoir 64 to the second mold pipe section 228. The valve 62 is disposed downstream in the flow direction from the resin reservoir 64. The opening and closing of the valve 62 is controlled by a control device 70.
[0041] The drive mechanism 80 is a device that moves the second mold 22, which is a movable mold. In this embodiment, the drive mechanism 80 is a lifting device that lifts and lowers the second mold 22 to open and close the mold body 20. When clamping the mold body 20, the drive mechanism 80 lowers the second mold 22 in the -Y direction approaching the first mold 21 side in response to a command from the control device 70. On the other hand, when releasing the second mold 22 from the first mold 21, the drive mechanism 80 raises the second mold 22 in the +Y direction away from the first mold 21 in response to a command from the control device 70.
[0042] The control device 70 applies driving force to and controls each of the components 40, 50, 60, 62, and 80 of the manufacturing apparatus 1 described above. In Fig. 2, the electrical connection state of each of the components 40, 50, 60, 62, and 80 of the manufacturing apparatus 1 that are electrically connected to and controlled by the control device 70 is diagrammatically illustrated by dashed lines.
[0043] A-3. Tank manufacturing method: 3 is a flowchart showing a method for manufacturing the tank 100 using the manufacturing apparatus 1. In this embodiment, after step S1, the manufacturing apparatus 1 executes steps S2 to S8 shown in FIG.
[0044] First, a preparation step (step S1) is performed. The preparation step (step S1) is a step of preparing a preform 120 and a tank manufacturing mold 2.
[0045] After the preparation step (step S1), the arrangement step (step S2) is executed. The arrangement step (step S2) is a step of arranging the preform 120 in the arrangement chamber 200 of the tank manufacturing mold 2 and clamping the first mold 21 and the second mold 22. Specifically, first, in a state in which the second mold 22 is raised by the driving mechanism 80, an operator attaches the preform 120 to the support mechanism 208, thereby supporting the preform 120 on the support mechanism 208. As a result, the preform 120 is accommodated in the first mold recess 215 of the first mold 21. Next, the driving mechanism 80 lowers the second mold 22 toward the first mold 21 in accordance with a command from the control device 70, so that the first mold opposing wall 211 and the second mold opposing wall 221 come into contact with each other. As a result, as shown in FIG. 2, the first mold 21 and the second mold 22 are clamped, and the preform 120 is accommodated in the arrangement chamber 200. At least a part of the work in the placement step (step S2) may be performed mechanically.
[0046] 3, after the placement step (step S2), a degassing step (step S4) is executed. The degassing step (step S4) is a step of vacuum degassing the placement chamber 200. Specifically, the vacuum pump 50 starts vacuum degassing in accordance with a command from the control device 70. The vacuum pump 50 then continues vacuum degassing, for example, until the completion time when the injection of the resin is completed in the subsequent injection step (step S5).
[0047] After the degassing step (step S4), an injection step (step S5) is performed. The injection step (step S5) is a step of injecting the resin stored in the resin reservoir 64 into the placement chamber 200 in order to impregnate the fiber layer 121 of the preform 120 with the resin. Specifically, the valve 62 is opened and the pressurizing device 60 starts pressurizing the resin reservoir 64 in accordance with a command from the control device 70. This causes the resin to flow through the second mold pipe 228 provided in the second mold 22, and the resin is injected from the second gate 229 toward the preform 120. At this time, the temperature of the mold body 20 is adjusted by the temperature adjustment device 40 so that the temperature of the mold body 20 is lower than the curing temperature of the resin.
[0048] After the injection step (step S5), an impregnation step (step S6) is performed. The impregnation step (step S6) is a step of impregnating the fiber bundle 12 forming the fiber layer 121 of the preform 120 with a resin. The resin injected toward the preform 120 gradually impregnates the fiber layer 121 from the outermost layer 12b side toward the innermost layer 12a side. Therefore, at least a part of the impregnation step (step S6) is performed simultaneously in parallel with the injection step (step S5) at a point in time after the injection step (step S5) is started.
[0049] After the impregnation step (step S6), a curing step (step S7) is performed. The curing step (step S7) is a step of curing the resin impregnated into the fiber bundle 12 in the impregnation step (step S6). In this embodiment, a thermosetting resin is used as the resin forming the reinforcing layer 90. Therefore, the manufacturing apparatus 1 cures the resin by heating in the curing step (step S7). Specifically, the temperature adjustment device 40 adjusts the temperature of the mold body 20 to be equal to or higher than the curing temperature of the resin. As a result, the resin cures and the fiber reinforced resin layer 15 is formed.
[0050] At this time, part of the resin injected toward the preform 120 impregnates the inside of the fiber layer 121, while the remaining resin flows between the preform 120 and the inner surface 20a of the mold body 20. Therefore, in the curing step (step S7), the resin that has not impregnated the fiber layer 121 is cured on the outer circumferential side of the fiber reinforced resin layer 15. As a result, a resin layer 17 made only of resin is formed on the radially outer side of the fiber reinforced resin layer 15, as shown in the right diagram of FIG.
[0051] After the curing step (step S7), a demolding step (step S8) is performed. The demolding step (step S8) is a step of separating the first mold 21 and the second mold 22 to separate the tank 100 from the mold body 20. Specifically, the driving mechanism 80, in accordance with a command from the control device 70, raises the second mold 22 in the +Y direction to separate it from the first mold 21. As a result, the first mold 21 and the second mold 22 are separated, and the tank 100 shown in the right diagram of FIG. 1 becomes in a state where it can be taken out from the mold body 20. The manufacturing method of the tank 100 is completed by performing each step (steps S1 to S8) up to the demolding step (step S8) shown in FIG. 3.
[0052] A-4. Detailed configuration of tank manufacturing mold: The shape of the preform 120 may vary depending on how the fiber bundle 12 is wound around the outer surface 10b of the liner 10. In other words, unevenness different from a predetermined shape (hereinafter, a reference shape) may occur in a part of the outermost layer 12b of the fiber layer 121 in the preform 120. At this time, if the tank manufacturing mold 2 and the preform 120 come into contact with each other due to the variation in the shape of the preform 120, the fibers at the contact part T may not be sufficiently impregnated with the resin. Therefore, in order to more reliably impregnate the fibers of the fiber layer 121 with the resin, it is preferable to form a flow path (gap) between the mold body 20 and the preform 120 for allowing the resin to flow. Furthermore, in the manufacturing process of the tank 100 by the RTM method, it is even more preferable to be able to correct the variation in the shape of the preform 120 so that the shape of the preform 120 approaches the reference shape. Therefore, in this embodiment, the tank 100 is manufactured using a tank manufacturing mold 2 having a plurality of ribs 23 and a flow path portion 27. In the present embodiment, the following description will be given taking as an example a case where the tank 100 is manufactured using a preform 120 in which the outermost layer 12b of the fiber layer 121 is formed by helical winding.
[0053] Fig. 4 is a perspective view of the inside of the tank manufacturing mold 2 in the first embodiment seen from the outside. Fig. 4 shows the tank manufacturing mold 2 in a state in which the preform 120 is placed in the placement chamber 200 and the mold body 20 is clamped. In Fig. 4, in order to easily visually confirm the configuration of the placement chamber 200 and the positional relationship between the tank manufacturing mold 2 and the preform 120, a portion of the tank manufacturing mold 2 and the preform 120 are extracted and the inside of the tank manufacturing mold 2 is seen through. In Fig. 4, the outline of the preform 120 is indicated by a dashed line.
[0054] Fig. 5 is a cross-sectional view taken along line 5-5 of Fig. 4. Fig. 5 is a schematic diagram showing a YZ cross section of the tank manufacturing mold 2 and the preform 120 in the impregnation step (step S6).
[0055] The ribs 23 correct any variation in shape that occurs in the preform 120 and form a flow path 27 for circulating the resin. As shown in Fig. 5, each of the ribs 23 protrudes radially inward from the inner surface 20a of the mold body 20 and faces the fiber bundles 12 of the outermost layer 12b of the fiber layer 121 when the preform 120 is arranged.
[0056] 4, the rib 23 has a bottom surface 230, an opposing surface 231, and a side surface 235. The bottom surface 230 is formed by the inner surface 20a of the mold body 20. The side surface 235 connects the bottom surface 230 and the opposing surface 231.
[0057] FIG. 6 is an enlarged view of the first region R1 in FIG. 5. The facing surface 231 faces the outermost layer 12b of the fiber layer 121 in the arrangement state of the preform 120. When a part of the fiber bundle 12 in the outermost layer 12b of the preform 120 protrudes radially outward and a part of the preform 120 has a shape different from the reference shape, the facing surface 231 comes into contact with the protruding part 12T in the process of clamping the first mold 21 and the second mold 22. Then, by placing the mold body 20 in a clamped state, the protruding part 12T is pushed radially inward by the facing surface 231 so as to approach the reference shape. In this way, by forming a plurality of ribs 23 on the inner surface 20a of the mold body 20, it is possible to correct the variation in shape that occurs in the preform 120 in the arrangement step (step S2) shown in FIG. 3. In FIG. 6, the part of the preform 120 whose shape is corrected by the ribs 23 is illustrated as a correction region A.
[0058] In addition, when a pin-shaped protrusion that contacts the fiber bundle 12 of the outermost layer 12b at approximately points is provided on the inner surface 20a of the mold body 20, the contact area with the fiber bundle 12 of the outermost layer 12b is smaller than when the rib 23 is provided. Therefore, when a pin-shaped protrusion is provided on the inner surface 20a of the mold body 20, a flow path through which the resin J flows can be secured, but the pin-shaped protrusion may pierce the fiber bundle 12 of the preform 120. If the pin-shaped protrusion pierces the fiber bundle 12 of the preform 120, the variation in the shape of the preform 120 cannot be corrected. In contrast, in this embodiment, the opposing surface 231 of the rib 23 and the fiber bundle 12 of the outermost layer 12b contact each other on their faces. This makes it possible to more reliably correct the variation in the shape of the preform 120.
[0059] FIG. 7 is a diagram showing a schematic external shape of the rib 23 in the first embodiment. In this embodiment, the shape of the rib 23 is a quadrangular pyramid shape with the inner surface 20a of the mold body 20 as the bottom surface 230. Therefore, the facing surface 231 and the inner surface 20a of the mold body 20 as the bottom surface 230 are generally parallel to each other. The area of the facing surface 231 is smaller than the area of the bottom surface 230. The bottom surface 230 and the facing surface 231 are connected by four side surfaces 235. In this embodiment, the shape of the facing surface 231 is generally square. Note that the shape of the rib 23 is not limited to this. The shape of the rib 23 may be, for example, a truncated cone shape or a truncated polygonal pyramid shape in which the bottom surface 230 and the facing surface 231 are pentagonal or more.
[0060] FIG. 8 is a diagram showing a detailed configuration of the flow path section 27 and the relationship between the fiber directions FD1, FD2 and the flow path directions GD1, GD2. FIG. 8 is an enlarged view of a part of FIG. 4, and shows a representative part of the fiber bundles 12 in the outermost layer 12b of the fiber layer 121. Specifically, FIG. 8 shows two fiber bundles 12 wound by helical winding so that the winding angle α is 55 degrees, respectively, and the two fiber bundles 12 cross each other by being folded back at a predetermined folding back position. In reality, in the outermost layer 12b of the fiber layer 121, a large number of fiber bundles 12 are wound in a spiral shape in the circumferential direction LD of the preform 120 at a predetermined winding angle α (55 degrees in this embodiment) in a state where they are close to or in contact with each other.
[0061] The flow path portion 27 is formed to impregnate the fiber bundles 12 of the fiber layer 121 with the resin J injected toward the preform 120 in the impregnation step (step S6). Specifically, the flow path portion 27 is formed between a first rib 23m and a second rib 23n as adjacent ribs 23, as shown in Fig. 8. That is, the flow path portion 27 is formed by the side surfaces 235m, 235n of the adjacent ribs 23m, 23n and the inner surface 20a of the mold body portion 20, as shown in Fig. 8.
[0062] In this embodiment, the ribs 23 are formed as a first rib group 238 in which the ribs 23 are arranged along the axial direction OD, as shown in FIG. 4. In FIG. 4, a part of the first rib group 238 is shown surrounded by a two-dot chain line. The first rib group 238 is arranged so as to be repeatedly arranged along the circumferential direction LD centered on the central axis O. That is, the ribs 23 are arranged in a lattice shape on the inner surface 20a of the mold body 20, spaced apart from each other by a predetermined distance. As a result, in this embodiment, as shown in FIG. 8, the flow path portion 27 is composed of a first flow path portion 271 extending along the axial direction OD and a second flow path portion 272 extending along the circumferential direction LD. The first flow path direction GD1, which is the direction in which the first flow path portion 271 extends, is the direction along the axial direction OD. The second flow path direction GD2, which is the direction in which the second flow path portion 272 extends, is the direction along the circumferential direction LD centered on the central axis O.
[0063] In the arrangement state of the preform 120, the flow path directions GD1, GD2 in which the flow path portions 271, 272 extend are different from the fiber directions FD1, FD2 in which the fiber bundles 12 in the outermost layer 12b of the fiber layer 121 extend. In the example shown in FIG. 8, the flow path directions GD1, GD2 are along the axial direction OD and the circumferential direction LD, while the fiber directions FD1, FD2 are inclined by the winding angle α with respect to the central axis O. In this way, since the fiber directions FD1, FD2 are different from the flow path directions GD1, GD2, it is possible to prevent the fiber bundles 12 forming the outermost layer 12b from being buried in the flow path portion 27. As a result, even if the inner surface 20a of the mold body portion 20 and the preform 120 come into contact with each other, the flow path portion 27 exists in the vicinity of the contact portion T, so that the resin J can be caused to flow in the flow path portion 27, thereby allowing the resin J to be sufficiently impregnated. In other words, it is possible to ensure a void portion B for allowing the resin J to flow in the vicinity of the contact portion T. This makes it possible to more reliably form a flow path for the resin J using the flow path section 27, thereby reducing the possibility that the flow of the resin J in the flow path section 27 will be impeded in the impregnation step (step S6) shown in FIG.
[0064] Further, in this embodiment, as shown in FIG. 8, the flow path widths L1, L2, which are the width of the flow path portion 27, are smaller than the fiber width L12, which is the width of the fiber bundle 12. That is, the preparation step (step S1) shown in FIG. 3 includes a step of winding the fiber bundle 12 having the fiber width L12 larger than the flow path widths L1, L2 around the preform 120 in order to form the outermost layer 12b of the fiber layer 121. Note that the "flow path widths L1, L2" referred to here refer to the interval between the first rib 23m and the second rib 23n adjacent to each other, as shown in FIG. 8. In other words, the flow path widths L1, L2 are the shortest distance between the first rib 23m and the second rib 23n adjacent to each other, and are the linear separation distance. In this way, the possibility that the fiber bundle 12 forming the outermost layer 12b is buried in the flow path portion 27 can be further reduced.
[0065] In this embodiment, in order to facilitate release of the tank 100 from the tank manufacturing mold 2, the gradient of the side surface 235 of the rib 23 is changed depending on the formation position in the circumferential direction LD about the central axis O, as shown in Fig. 5. Hereinafter, the gradient of the side surface 235 in Fig. 6 is referred to as the reference gradient, and the rib 23 in Fig. 6 is also referred to as the reference rib 23s.
[0066] Fig. 9 is an enlarged view of the second region R2 in Fig. 5. In Fig. 9, a gradient rib 23t in which the gradient of the side surface 235 of the rib 23 is changed by a predetermined angle with respect to the reference gradient is shown by a solid line. In Fig. 9, the reference rib 23s is also shown by a dotted line to facilitate comparison between the case where the rib 23 in the second region R2 is the reference rib 23s and the case where the gradient rib 23t is used.
[0067] For example, when the upper side (the +Y direction side in this embodiment) of the tank 100 is released by moving the first mold 21 in the separation direction RD (FIG. 5), the outer surface 17b of the resin layer 17 and the inner surface 20a of the tank manufacturing mold 2 are unlikely to interfere with each other in the first region R1 shown in FIG. 6. On the other hand, when the shape of the rib 23 is the same in the first region R1 and the second region R2, that is, when the reference rib 23s is provided in the second region R2, the outer surface 17b of the resin layer 17 and the inner surface 20a of the tank manufacturing mold 2 are likely to interfere with each other, particularly at the corners 291, during release. The "corner 291" referred to here refers to the connection portion where the side surface 235 of the rib 23 and the inner surface 20a of the mold body 20 are connected, and the surrounding area of the connection portion. Therefore, in an area such as the second region R2 where the resin layer 17 and the mold body 20 are likely to interfere with each other during demolding, a gradient rib 23t is formed with a draft gradient (draft angle) greater than the standard gradient on the inner surface 20a of the mold body 20. In this way, the tank 100 can be easily demolded from the tank manufacturing mold 2.
[0068] In this embodiment, as shown in FIG. 1, in the preform 120, the outer diameter of the cylindrical portion 950 is larger than the outer diameter of the spherical portions 951 and 952. As shown in FIG. 4, in the arrangement state of the preform 120, the space B1 formed between the cylindrical portion 950 and the body portion 205 is smaller than the space B2 formed between the second spherical portion 952 and the second dome portion 202. Therefore, the fiber bundle 12 wound around the cylindrical portion 950 is less likely to be impregnated with the resin J than the fiber bundle 12 wound around the spherical portions 951 and 952. Therefore, in this embodiment, as shown in FIG. 4, the multiple ribs 23 are formed on the inner surface 200a of the body portion 205 of the mold main body portion 20, but are not formed on the inner surface 202a of the second dome portion 202. Although not shown in FIG. 4, the multiple ribs 23 are not formed on the inner surface of the first dome portion 201 as in the second dome portion 202. In this way, the fiber bundle 12 can be easily impregnated with the resin J in the cylindrical portion 950, which is more difficult to impregnate with the resin than the spherical portions 951 and 952.
[0069] A-5. Detailed configuration of the through hole 170: Fig. 10 is a diagram for explaining a detailed configuration of the through-hole 170. Fig. 10 shows an enlarged view of the third region R3 in Fig. 1.
[0070] The through holes 170 are formed in the process of forming the resin layer 17 by the RTM method. Specifically, in the impregnation step (step S6), as shown in FIG. 8, a plurality of ribs 23 provided on the inner surface 20a of the mold body 20 locally block the flow of the resin J flowing between the preform 120 and the inner surface 20a of the mold body 20. On the other hand, the resin J flows through the portion where the ribs 23 are not formed, i.e., the flow path portion 27. As a result, a plurality of through holes 170 are formed in the resin layer 17, as shown in FIG. 10. That is, the through holes 170 are hollow portions having a shape that follows the shape of the ribs 23.
[0071] Here, the fluid G1 such as hydrogen gas stored in the internal space 10p of the tank 100 may penetrate the liner 10 and the fiber reinforced resin layer 15 and enter between the fiber reinforced resin layer 15 and the resin layer 17, although the amount is small. At this time, the resin layer 17 is formed of a material having a high gas barrier property and low strength compared to the fiber reinforced resin layer 15 in order to ensure the tank strength. The "strength" referred to here refers to, for example, the magnitude of the fracture strain, and "low strength" refers to, for example, a large fracture strain. Therefore, the fluid G2 that penetrates between the fiber reinforced resin layer 15 and the resin layer 17 accumulates between the fiber reinforced resin layer 15 and the resin layer 17 without penetrating the resin layer 17. Then, the resin layer 17 gradually expands according to the amount of accumulated fluid G2, and when the fluid G2 accumulated between the fiber reinforced resin layer 15 and the resin layer 17 exceeds a predetermined amount, the resin layer 17 breaks. If the resin layer 17 breaks, the resin layer 17 may become cloudy or may generate abnormal noise. For example, if the resin layer 17 becomes cloudy, the appearance of the tank 100 may be impaired.
[0072] Therefore, in this embodiment, a plurality of through holes 170 are formed in the resin layer 17 to communicate the fiber reinforced resin layer 15 with the outside. This allows the fluid G2 that has entered between the fiber reinforced resin layer 15 and the resin layer 17 to be discharged into the atmosphere through the through holes 170 formed in the resin layer 17. In other words, the fluid G2 that has entered between the fiber reinforced resin layer 15 and the resin layer 17 can be prevented from accumulating between the fiber reinforced resin layer 15 and the resin layer 17. This reduces the possibility that the resin layer 17 will break. In addition, the resin layer 17 can be prevented from becoming cloudy or generating abnormal noise, thereby reducing the possibility that the quality of the tank 100 will deteriorate.
[0073] It is preferable that the dimension LJ (FIG. 6) of the rib 23 in the protruding direction of the rib 23 is approximately equal to the thickness L17 (FIG. 10) of the resin layer 17. The "protruding direction of the rib 23" referred to here is the direction from the inner surface 20a of the mold body 20 toward the radially inward direction. In this way, the fiber reinforced resin layer 15 can be more reliably connected to the outside in the portion where the through hole 170 is formed.
[0074] According to the first embodiment, as shown in Fig. 2 and Fig. 4, the tank 100 is manufactured by the RTM method using a tank manufacturing mold 2 having a plurality of ribs 23 and a flow path portion 27. At this time, as shown in Fig. 8, in the arrangement state of the preform 120, the fiber directions FD1, FD2 are different from the flow path directions GD1, GD2, so that it is possible to prevent the fiber bundle 12 from being embedded in the flow path portion 27. As a result, even if the inner surface 20a of the mold body portion 20 and the preform 120 come into contact with each other, the fiber bundle 12 at the contact portion T can be sufficiently impregnated with the resin J by circulating the resin J through the flow path portion 27.
[0075] B. Second embodiment: Fig. 11 is a perspective view of the inside of the tank manufacturing mold 24 in the second embodiment seen from the outside. Fig. 11, like Fig. 4, shows the tank manufacturing mold 24 in a state in which the preform 120 is placed in the placement chamber 200 and the mold body 240 is clamped. In Fig. 11, in order to easily visually confirm the configuration of the placement chamber 200 and the positional relationship between the tank manufacturing mold 24 and the preform 120, a portion of the tank manufacturing mold 24 and the preform 120 are extracted and the inside of the tank manufacturing mold 24 is seen through. In Fig. 11, the outline of the preform 120 is indicated by a dashed line.
[0076] In this embodiment, the ribs 234 also protrude radially inward from the inner surface 240a of the mold body 240, and face the fiber bundles 12 of the outermost layer 12b of the fiber layer 121 in the arrangement state of the preform 120. The function of the ribs 234 is the same as in the first embodiment. In contrast, in this embodiment, the shape of the ribs 234 and the arrangement of the ribs 234 on the inner surface 240a of the mold body 240 are different from those in the first embodiment (FIG. 4). The other configurations and the manufacturing method of the tank 100 are the same as in the first embodiment. The same reference numerals are given to the same configurations as in the first embodiment, and the description is omitted. Note that, in this embodiment, the tank 100 is manufactured using a preform 120 in which the outermost layer 12b of the fiber layer 121 is formed by helical winding with a winding angle α of 55 degrees.
[0077] In this embodiment, the multiple ribs 234 are formed as a second rib group 248 in which multiple ribs 234 are arranged along the axial direction OD. In FIG. 11, a part of the second rib group 248 is shown by surrounding it with a two-dot chain line. The second rib group 248 is arranged on the inner surface 240a of the mold body 240 so as to be repeatedly arranged in the circumferential direction LD centered on the central axis O. At this time, the formation positions of the adjacent second rib groups 248m, 248n are shifted by a predetermined distance in the axial direction OD. That is, in this embodiment, the multiple ribs 234 are arranged alternately on the inner surface 240a of the mold body 240, spaced apart by a predetermined distance.
[0078] Fig. 12 is a diagram showing the configuration of the flow path section 27 and the relationship between the fiber directions FD1, FD2 and the flow path directions GD1, GD3 in the second embodiment. Fig. 12 is an enlarged view of a part of Fig. 11, and shows a representative part of the fiber bundles 12 in the outermost layer 12b of the fiber layer 121. Fig. 12 also shows two fiber bundles 12 that cross each other as a result of being folded back at a predetermined folding back position.
[0079] In this embodiment, the flow path section 27 is composed of a first flow path section 271 extending along the axial direction OD and a plurality of third flow path sections 273 extending along the circumferential direction LD. Therefore, the first flow path direction GD1, which is the direction in which the first flow path section 271 extends, is a direction along the axial direction OD. Also, the third flow path direction GD3, which is the direction in which the third flow path section 273 extends, is a direction along the circumferential direction LD. In contrast, the fiber directions FD1 and FD2 are inclined by the winding angle α (55 degrees in this embodiment) with respect to the central axis O. That is, even in this embodiment, the fiber directions FD1 and FD2 are different from the flow path directions GD1 and GD3. This can reduce the possibility that the fiber bundle 12 forming the outermost layer 12b will be buried in the flow path section 27.
[0080] Furthermore, in this embodiment, the shape of the rib 234 is a quadrangular pyramid shape formed by a bottom surface 242 formed by the inner surface 240a of the mold body 240, a rectangular opposing surface 241, and four side surfaces 245 connecting the bottom surface 242 and the opposing surface 241. Specifically, for the opposing surface 241, the dimension LR1 of the rib 234 in the circumferential direction LD of the preform 120 is the same as that of the first embodiment (FIG. 4), and the dimension LR2 of the rib 234 in the axial direction OD of the preform 120 is larger than that of the first embodiment. In this way, when a part of the fiber bundle 12 in the outermost layer 12b of the preform 120 protrudes radially outward, the possibility of the fiber bundle 12 coming into contact with the opposing surface 231 can be increased. This makes it possible to more reliably correct the shape variation occurring in the preform 120.
[0081] 12, the fiber directions FD1, FD2 and the flow path directions GD1, GD2 can be made different from each other in the manufacturing process of the tank 100. This makes it possible to prevent the fiber bundles 12 forming the outermost layer 12b from being embedded in the flow path portion 27, and therefore allows the fiber bundles 12 to be sufficiently impregnated with the resin J.
[0082] C. Third embodiment: Fig. 13 is a perspective view of the inside of the tank manufacturing mold 26 in the third embodiment seen from the outside. Fig. 13, like Fig. 4, shows the tank manufacturing mold 26 in a state in which the preform 126 is placed in the placement chamber 200 and the mold body 260 is clamped. In Fig. 13, in order to easily visually confirm the configuration of the placement chamber 200 and the positional relationship between the tank manufacturing mold 26 and the preform 126, a part of the tank manufacturing mold 26 and the preform 126 are extracted and the inside of the tank manufacturing mold 26 is seen through. In Fig. 13, the outline of the preform 120 is indicated by a dashed line.
[0083] In this embodiment, the multiple ribs 23 also protrude radially inward from the inner surface 260a of the mold body 260, and face the fiber bundles 12 in the outermost layer 12b of the fiber layer 121 in the arrangement state of the preform 120. The shape and function of the ribs 23 are similar to those of the first embodiment. In contrast, in this embodiment, the winding angle β of the fiber bundles 12 in the outermost layer 12b and the arrangement of the multiple ribs 23 on the inner surface 260a of the mold body 260 are different from those of the first embodiment (FIG. 4). The other configurations and the manufacturing method of the tank 100 are the same as those of the first embodiment. The same reference numerals are used for the same configurations as those of the first embodiment, and the description will be omitted.
[0084] In this embodiment, the multiple ribs 23 are formed as a third rib group 268 in which the multiple ribs 23 are arranged along an inclination direction ID inclined at a predetermined angle with respect to the axial direction OD. In FIG. 13, a part of the third rib group 268 is illustrated by being surrounded by a two-dot chain line. In the example illustrated in FIG. 13, the inclination direction ID is a direction inclined at 45 degrees with respect to the axial direction OD. That is, the third rib group 268 in this embodiment is arranged at a position rotated 45 degrees around the central axis O from the first rib group 238 (FIG. 4) in the first embodiment. Note that the inclination angle of the inclination direction ID with respect to the axial direction OD is not limited to this, and may be another angle.
[0085] Fig. 14 is a diagram showing the configuration of a flow path section 27 and the relationship between the fiber direction FD3 and the flow path directions GD4 and GD5 in the third embodiment. Fig. 14 is an enlarged view of a part of Fig. 13, and shows a representative part of the fiber bundles 12 in the outermost layer 12b of the fiber layer 121.
[0086] In this embodiment, the flow path section 27 is composed of a fourth flow path section 274 extending along the inclination direction ID and a fifth flow path section 275 extending in a direction perpendicular to the inclination direction ID. Therefore, the fourth flow path direction GD4, which is the direction in which the fourth flow path section 274 extends, is a direction along the inclination direction ID. Moreover, the fifth flow path direction GD5, which is the direction in which the fifth flow path section 275 extends, is a direction perpendicular to the inclination direction ID. In contrast, in this embodiment, the outermost layer 12b in the fiber layer 121 is formed by hoop winding with a winding angle β of 90 degrees. That is, the fiber direction FD3 is a direction inclined by the winding angle β (90 degrees) with respect to the central axis O. Therefore, even in this embodiment, the fiber direction FD3 is different from the flow path directions GD4 and GD5.
[0087] According to the third embodiment, as shown in Fig. 14, in the manufacturing process of the tank 100 using the preform 126 in which the outermost layer 12b is formed by hoop winding, the fiber direction FD3 and the flow path directions GD4, GD5 can be made different. This makes it possible to prevent the fiber bundle 12 forming the outermost layer 12b from being buried in the flow path portion 27. Therefore, even if the inner surface 20a of the mold body portion 20 and the preform 120 come into contact with each other, the fiber bundle 12 can be sufficiently impregnated with the resin J by circulating the resin J through the flow path portion 27.
[0088] D. Other embodiments: D-1. Other embodiment 1: In the above embodiment, the rib 23 is formed only on the inner surface 200a of the trunk portion 205 of the mold body portion 20. However, the present disclosure is not limited to this. The rib 23 may be formed on both the inner surface 200a of the trunk portion 205 and the inner surfaces 202a of the two dome portions 201, 202 of the mold body portion 20. In this embodiment, the rib 23 can correct the variation in shape of the spherical portions 951, 952 of the preform 120.
[0089] D-2. Other embodiment 2: In the above embodiment, the flow path widths L1, L2 are formed to be smaller than the fiber width L12. However, the present disclosure is not limited to this. The flow path widths L1, L2 and the fiber width L12 may be the same, or the flow path widths L1, L2 may be formed to be larger than the fiber width L12. Even in such a form, the fiber directions FD1 to FD3 and the flow path directions GD1 to GD5 are different in the arrangement state of the preform 120, so that the fiber bundles 12 forming the outermost layer 12b can be prevented from being buried in the flow path portion 27.
[0090] The present disclosure is not limited to the above-mentioned embodiment, and can be realized in various configurations without departing from the spirit of the present disclosure. For example, the technical features of the embodiments corresponding to the technical features in each aspect described in the Summary of the Invention can be appropriately replaced or combined to solve some or all of the above-mentioned problems or to achieve some or all of the above-mentioned effects. Furthermore, if a technical feature is not described as essential in this specification, it can be appropriately deleted. [Explanation of symbols]
[0091] 1... manufacturing device, 2, 24, 26... tank manufacturing mold, 10... liner, 10b... outer surface of liner, 10d... opening, 10p... internal space, 10r... tip, 12... fiber bundle, 12T... protruding portion, 12a... innermost layer, 12b... outermost layer, 15... fiber reinforced resin layer, 15b... outer surface of fiber reinforced resin layer, 17... resin layer, 17b... outer surface of resin layer, 20, 240, 260... mold body, 20a, 240a, 260a... inner surface, 21... first mold, 22... second mold, 23, 234, 236... rib, 23m... first rib, 23n... second rib, 23s... reference rib, 23 t...gradient rib, 27...flow path, 40...temperature control device, 50...vacuum pump, 60...pressurizing device, 62...valve, 64...resin reservoir, 70...control device, 80...driving mechanism, 90...reinforcing layer, 95...container body, 100...tank, 120, 126...preform, 120r...one end side, 120s...other end side, 121...fiber layer, 170...through hole, 181...valve side nozzle, 182...end side nozzle, 200...placement chamber, 201...first dome portion, 202...second dome portion, 202a...inner surface of second dome portion, 205...body portion, 205a...inner surface of body portion, 208...supporting mechanism Structure, 211...first type opposing wall, 212...first type bottom wall, 215...first type recess, 216...first type bottom surface, 217, 217m, 217n...first type connection surface, 218...first type pipe section, 219...first gate, 221...second type opposing wall, 222...second type top wall, 225...second type recess, 226...second type top surface, 227, 227m, 227n...second type connection surface, 228...second type pipe section, 229...second gate, 230, 242...bottom surface, 231, 241...opposing surface, 235, 235m, 235n, 245...side surface, 238...first rib group, 248, 248m, 248n...second rib group, 268...third rib group, 271...first flow path portion, 272...second flow path portion, 273...third flow path portion, 274...fourth flow path portion, 275...fifth flow path portion, 291...corner portion, 950...cylindrical portion, 950r...one end portion, 950s...other end portion, 951...first spherical portion, 952...second spherical portion, A...correction area, B...void portion, B1,B2...space portion, CD...radial direction, FD1~FD3...fiber direction, G1,G2...fluid, GD1...first flow path direction, GD2...second flow path direction, GD3...third flow path direction, GD4...fourth flow path direction, GD5...fifth flow path direction, ID...inclination direction, J...resin, L1,L2...flow path width, L12...fiber width, L17...resin layer thickness, LD...circumferential direction, LJ...rib dimension in protruding direction, LR1...rib dimension in circumferential direction, LR2...rib dimension in axial direction, O...center axis, OD...axial direction, R1...first region, R2...second region, R3...third region, RD...separation direction, T...contact area, α,β...winding angle,
Claims
1. A method for manufacturing a tank, comprising the steps of: A preparation step of preparing a preform in which a plurality of layers of fiber bundles are wound around an outer surface of a liner that forms an internal space of a tank, and a mold; and an impregnation step of injecting a resin into the mold in a state in which the preform is placed in the mold to impregnate the fiber bundle with the resin, The mold is A mold body portion, a plurality of ribs protruding from an inner surface of the mold body and facing the fiber bundles of the outermost layer in the arranged state; a flow path portion formed between a first rib and a second rib as the ribs adjacent to each other, the flow path portion through which the resin flows, A method for manufacturing a tank, wherein, in the arranged state, a fiber direction in which the fiber bundles in the outermost layer extend is different from a flow path direction in which the flow path portion extends.
2. A method for manufacturing the tank according to claim 1, comprising the steps of: When the distance between the first rib and the second rib is defined as the flow path width of the flow path portion and the width of the fiber bundle is defined as the fiber width, The method for manufacturing a tank, wherein the preparation step includes a step of winding the fiber bundle, the fiber bundle having the fiber width larger than the flow path width, around the preform to form the outermost layer.
3. A method for manufacturing the tank according to claim 1 or 2, comprising the steps of: The mold body portion is A cylindrical body portion, Two dome portions are provided at both ends of the body portion, and the diameter of the dome portions decreases with increasing distance from the body portion, A method for manufacturing a tank, wherein the rib is formed on the inner surface of the body portion.
4. A mold for manufacturing a tank, comprising: A mold body portion, a preform, in which a plurality of layers of fiber bundles are wound around an outer surface of a liner that protrudes from an inner surface of the mold body and forms an internal space of a tank, is placed in the mold; and a plurality of ribs that face the fiber bundles of the outermost layer in a state where the preform is placed in the mold; a flow path portion formed between a first rib and a second rib as the ribs adjacent to each other, the flow path portion through which a resin to be impregnated into the fiber bundle in the arranged state flows, A tank manufacturing mold, wherein in the arranged state, a fiber direction in which the fiber bundles in the outermost layer extend is different from a flow path direction in which the flow path portion extends.
Citation Information
Patent Citations
Method for manufacturing high-pressure tank
JP2019142118A
Hydrogen tank
JP2020118288A
Manufacturing method of high pressure tank
JP2021167653A
A unidirectional reinforcement and a method of producing a unidirectional reinforcement
WO2014013137A1