Secondary battery, device including secondary battery, method for producing secondary battery, and adhesive composition

The use of a crosslinkable polymer-based adhesive composition strengthens adhesion in secondary batteries, addressing cycle life and structural stability issues by enhancing interaction forces between battery components.

JP7590414B2Active Publication Date: 2024-11-26CONTEMPORARY AMPEREX TECHNOLOGY (HONG KONG) LIMITED
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2022513130
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-12-03
Publication Date
2024-11-26
Estimated Expiration
2039-12-03

AI Technical Summary

Technical Problem

Existing secondary batteries face challenges in cycle life and structural stability due to inadequate adhesion between materials, leading to issues like negative electrode sheet expansion and film peeling during charge/discharge cycles.

Method used

A secondary battery design utilizing an adhesive composition formed by crosslinking a crosslinkable polymer substrate and a crosslinking agent, with specific monomer units and compounds, enhances adhesion between substances, forming a strong interaction force.

Benefits of technology

The improved adhesion significantly enhances the cycle life and safety performance of secondary batteries by reducing negative electrode sheet expansion and film peeling, thereby stabilizing the battery structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590414000021
    Figure 0007590414000021
  • Figure 0007590414000022
    Figure 0007590414000022
  • Figure 0007590414000023
    Figure 0007590414000023
Patent Text Reader

Abstract

The present invention relates to a secondary battery (5), a device including the secondary battery (5), a method for manufacturing the secondary battery (5), and an adhesive composition. The secondary battery (5) includes an adhesive used to bond a first material and a second material, the adhesive including a polymer obtained by crosslinking the adhesive composition, the adhesive composition including a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate including one or more monomer units represented by formula (I), the crosslinking agent including a compound represented by formula (II), and the crosslinking agent including a compound represented by formula (II), wherein R1, R2, and R3 are independently selected from H and linear or branched alkyl groups having 1 to 8 carbon atoms, R4 is an active hydrogen-containing polar group, R5 is a group exhibiting reactivity with R4, R6 is selected from H and substituted or unsubstituted hydrocarbon groups having 1 to 8 carbon atoms, and n is an even number equal to or greater than 4, with 2≦m≦n. The cycle life of the secondary battery (5) is effectively improved. JPEG2022545913000021.jpg2366
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present application relates to the technical field of secondary batteries, and in particular to a secondary battery, a device including a secondary battery, a method for manufacturing a secondary battery, and an adhesive composition. [Background technology]

[0002] Secondary batteries, such as lithium-ion secondary batteries, have high charge / discharge performance, no memory effect, and are environmentally friendly, and are therefore widely used in electric vehicles and consumer electronic products. With the rapid popularity of new energy vehicles, the demand for power-type secondary batteries has increased explosively. The market has higher requirements for the service life of secondary batteries. Therefore, it is necessary to provide new technologies that can further improve the cycle life of secondary batteries. Summary of the Invention

[0003] The present application provides a secondary battery having a long cycle life, a device including the secondary battery, a method for producing the secondary battery, and an adhesive composition capable of improving the cycle life of the secondary battery.

[0004] In order to achieve the above object, a first aspect of the present application provides a secondary battery, the secondary battery comprising an adhesive used to bond a first substance and a second substance, the adhesive comprising a polymer obtained by crosslinking an adhesive composition, the adhesive composition comprising a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate comprising one or more types of monomer units represented by formula (I), the crosslinking agent comprising a compound represented by formula (II), JPEG0007590414000001.jpg54142 Here, the above R 1 , R 2 and R 3 are each independently selected from H and a linear or branched alkyl group having 1 to 8 carbon atoms; Above R 4 is an active hydrogen-containing polar group, Above R 5 is the above R 4is a group that exhibits reactivity towards Above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, The above n is an even number of 4 or more, 2≦m≦n, and preferably m≧3.

[0005] A second aspect of the present application provides a device including the secondary battery according to the first aspect of the present application.

[0006] A third aspect of the present application provides an adhesive composition, the adhesive composition comprising a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate comprising one or more of the monomer units represented by formula (I) and the crosslinking agent comprising a compound represented by formula (II): JPEG0007590414000002.jpg52149 Here, the above R 1 , R 2 and R 3 are each independently selected from H and a linear or branched alkyl group having 1 to 8 carbon atoms; Above R 4 is an active hydrogen-containing polar group, Above R 5 is the above R 4 is a group that exhibits reactivity towards Above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, The above n is an even number of 4 or more, 2≦m≦n, and preferably m≧3.

[0007] A fourth aspect of the present application provides a method for producing a secondary battery, the method comprising the step of adhering a first substance and a second substance using an adhesive, the adhesive comprising a polymer obtained by crosslinking a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate comprising one or more types of monomer units represented by formula (I), and the crosslinking agent comprising a compound represented by formula (II), JPEG0007590414000003.jpg46142 Here, the above R 1 , R 2 and R3 are each independently selected from H and a linear or branched alkyl group having 1 to 8 carbon atoms; Above R 4 is an active hydrogen-containing polar group, Above R 5 is the above R 4 is a group that exhibits reactivity towards Above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, The above n is an even number of 4 or more, 2≦m≦n, and preferably m≧3.

[0008] The secondary battery according to the present application uses an adhesive to bond a first material and a second material. The adhesive is obtained by crosslinking an adhesive composition containing a crosslinkable polymer substrate and a crosslinking agent. The crosslinkable polymer substrate contains a monomer unit represented by formula (I), which has an active hydrogen-containing polar group, and thus has a high affinity between the adhesive and both the first material and the second material, and therefore has a strong interaction between the first material and the second material. In particular, the crosslinking agent contains a compound represented by formula (II), which has two or more groups that exhibit reaction activity with the active hydrogen-containing polar group of the monomer unit, and thus forms a good crosslinked structure after the adhesive composition is crosslinked, and can greatly improve the interaction force between the first material and the second material. Therefore, a strong adhesion is formed between the first material and the second material in the secondary battery, and both the structural stability and cycle life of the battery can be improved.

[0009] In particular, when both the first material and the second material are negative active materials, strong interaction can be formed between particles of the negative active material due to the adhesive action of the adhesive, thereby significantly improving the cohesive strength of the negative sheet, thereby effectively mitigating the problems of expansion during cold rolling of the negative sheet and during the charge / discharge cycle of the secondary battery, thereby improving both the cycle life and safety performance.

[0010] When the first material is a negative active material and the second material is a negative current collector, the adhesive has a strong adhesive force between the negative active material and the negative current collector, so that the negative active material is effectively attached to the negative current collector, and the negative sheet has a high adhesive strength and a low risk of film peeling and powder falling off. The negative sheet has a small volume change during the charge and discharge cycle process, and can reduce the cycle expansion of the battery. Therefore, the cycle life and safety performance of the battery can both be improved. [Brief description of the drawings]

[0011] In the following, in order to more clearly explain the technical solutions of the embodiments of the present application, drawings necessary for the embodiments of the present application are briefly introduced. Obviously, the drawings described below are only some embodiments of the present application, and those skilled in the art can further obtain other drawings based on the drawings without any creative efforts.

[0012] [Figure 1] 1 is a schematic diagram of a secondary battery according to an embodiment of the present application. [Diagram 2] FIG. 1 is a schematic diagram of a battery module according to an embodiment of the present application. [Diagram 3] 1 is a schematic diagram of a battery pack according to an embodiment of the present application. [Figure 4] FIG. 4 is an exploded view of FIG. [Diagram 5] 1 is a schematic diagram of an apparatus according to an embodiment of the present application;

[0013] Here, the explanation of the reference numerals is as follows. 1 Battery pack 2 Upper case 3 Lower housing 4 Battery Module 5 Secondary battery DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] In order to make the inventive objectives, technical solutions and beneficial technical effects of the present application clearer, the present application will be described in more detail in combination with examples below. It should be understood that the examples described herein are merely for interpreting the present application, and are not intended to limit the present application.

[0015] For simplicity, only some numerical ranges are explicitly disclosed herein. However, any lower limit may be combined with any upper limit to form a range not explicitly stated, and any lower limit may be combined with any other lower limit to form a range not explicitly stated, and similarly, any upper limit may be combined with any other upper limit to form a range not explicitly stated. Also, although not explicitly stated, each point or single value between the endpoints of a range is included within the range. Thus, each point or single value may be combined with any other point or single value as its own lower limit or upper limit, or combined with any other lower limit or upper limit to form a range not explicitly stated.

[0016] It should be noted that in the description of this specification, unless otherwise specified, "more than" and "less than" are inclusive of the target number, and "multiple types" in "one type or multiple types" means two types or more than two types.

[0017] The above summary of the invention of this application is not intended to describe each embodiment or every implementation disclosed herein. The following description more particularly illustrates and describes exemplary embodiments. Throughout this application, guidance is provided through a series of examples that can be used in various combinations. In each example, the enumeration is used only as a representative group and should not be interpreted as exhaustive.

[0018] Electric energy, as an economical, practical, clean and easy to control and convert form of energy, is being applied to more and more devices. Secondary batteries have the advantages of high energy density, portability, no memory effect, environmental friendliness, etc., and thus become the preferred option for power supply of devices. [Secondary battery]

[0019] Accordingly, a first aspect of the present application provides a secondary battery.

[0020] The secondary battery includes a positive electrode sheet, a negative electrode sheet, a separator, and an electrolyte. During the charge and discharge process of the battery, active ions shuttle between the positive electrode sheet and the negative electrode sheet to perform insertion and desorption. The separator is provided between the positive electrode sheet and the negative electrode sheet to perform the function of isolation. The electrolyte performs the function of ion transport between the positive electrode sheet and the negative electrode sheet.

[0021] In practical manufacture and application, it is generally necessary to use an adhesive to realize adhesion between a first material and a second material in a secondary battery. The adhesive performance between the first material and the second material has an important effect on the performance (e.g., cycle life, etc.) of the secondary battery, and further affects the working performance and working efficiency of the device. The present application provides a secondary battery including an adhesive, which is used to bond the first material and the second material and can ensure a high adhesive effect between the first material and the second material.

[0022] In the secondary battery according to the present application, the adhesive comprises a polymer obtained by crosslinking an adhesive composition, the adhesive composition comprises a crosslinkable polymer base and a crosslinking agent, the crosslinkable polymer base comprises a monomer unit represented by formula (I), and the crosslinking agent comprises a compound represented by formula (II), JPEG0007590414000004.jpg42150 Here, the above R 1 , R 2 and R 3 are each independently selected from H and a linear or branched alkyl group having 1 to 8 carbon atoms; R 4 is an active hydrogen-containing polar group, Above R 5 is the above R 4 is a group that exhibits reactivity towards Above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, The above n is an even number of 4 or more, 2≦m≦n, and preferably m≧3.

[0023] In the secondary battery of the present application, the monomer unit represented by formula (I) is a basic structural unit of the crosslinkable polymer substrate. 1 is selected from H, a linear or branched alkyl group having 1 to 8 carbon atoms, and preferably from H, a linear or branched alkyl group having 1 to 4 carbon atoms. For example, R 1 is selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, n-heptyl, n-octyl, and the like. R 1 is preferably selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl; R 1 is more preferably selected from H, a methyl group, and an ethyl group, and particularly preferably H.

[0024] R 1 is selected from linear or branched alkyl groups having 1 to 8 carbon atoms, the alkyl group may have one or more hydrogens replaced with other elements or groups. The other elements may be, but are not limited to, F, Cl, O, etc. The other groups may be, but are not limited to, hydroxyl groups, amine groups, phenyl groups, methoxy groups, etc.

[0025] In some embodiments, R 2 is selected from H, a linear or branched alkyl group having 1 to 8 carbon atoms, and preferably from H, a linear or branched alkyl group having 1 to 4 carbon atoms. For example, R 2 is selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, n-heptyl, n-octyl, and the like. R 2is preferably selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl; R 2 is more preferably selected from H, a methyl group, an ethyl group, an n-propyl group, and an isopropyl group.

[0026] R 2 is selected from linear or branched alkyl groups having 1 to 8 carbon atoms, the alkyl group may have one or more hydrogens replaced with other elements or groups. The other elements may be, but are not limited to, F, Cl, O, etc. The other groups may be, but are not limited to, hydroxyl groups, amine groups, phenyl groups, methoxy groups, etc.

[0027] In some embodiments, R 3 is selected from H, a linear or branched alkyl group having 1 to 8 carbon atoms, and preferably from H, a linear or branched alkyl group having 1 to 4 carbon atoms. For example, R 3 is selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, n-heptyl, n-octyl, and the like. R 3 is preferably selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl; R 3 is more preferably selected from H, a methyl group, and an ethyl group, and particularly preferably H or a methyl group.

[0028] R 3 is selected from linear or branched alkyl groups having 1 to 8 carbon atoms, the alkyl group may have one or more hydrogens replaced with other elements or groups. The other elements may be, but are not limited to, F, Cl, O, etc. The other groups may be, but are not limited to, hydroxyl groups, amine groups, phenyl groups, methoxy groups, etc.

[0029] In some embodiments, R 4 teeth, Selected from JPEG0007590414000005.jpg3578.

[0030] Above R 7 is selected from H, a substituted or unsubstituted alkyl group having 1 to 6 carbon atoms, and preferably from H, a substituted or unsubstituted alkyl group having 1 to 4 carbon atoms. For example, R 7 may be selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, and the like. R 7 is preferably selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl.

[0031] R 7 is selected from substituted alkyl groups having 1 to 6 carbon atoms, the alkyl groups may have one or more hydrogens substituted with other elements or groups. The other elements may be, but are not limited to, F, Cl, O, etc. The other groups may be, but are not limited to, hydroxyl groups, phenyl groups, and amine groups.

[0032] The above a is 0 or 1, and the above R 1 is selected from a phenylene group and a substituted or unsubstituted alkylene group having 1 to 6 carbon atoms, and X is -COOH, -SO 3 H, -SO 2 H, a hydroxyl group, a mercapto group, and an amino group. 1 is selected from a phenylene group and a substituted or unsubstituted alkylene group having 1 to 4 carbon atoms, and X is selected from -COOH and a hydroxy group.

[0033] In some embodiments, when a is 1, R 1is selected from the group consisting of phenylene, methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, tert-butylene, pentylene, isopentylene and hexylene. 1 is selected from the group consisting of phenylene, methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, and tert-butylene, and more preferably R 1 is selected from a phenylene group, a methylene group, and an ethylene group.

[0034] R 1 In the formula (I), one or more hydrogens may be replaced with other elements or groups. The elements may be, but are not limited to, F, Cl, O, etc. The groups may be, but are not limited to, hydroxyl groups, phenyl groups, amine groups, etc.

[0035] These groups have high reactivity and strong polarity, and can further strengthen the interaction between the first substance and the second substance, thereby improving the adhesive strength thereof.

[0036] In some preferred embodiments, R 4 teeth, Selected from JPEG0007590414000006.jpg2685.

[0037] In some preferred embodiments, the monomer unit represented by formula (I) can be selected from one or more of the following monomer units a to d: JPEG0007590414000007.jpg76121

[0038] In some embodiments, the crosslinkable polymer substrate may be a homopolymer or a copolymer, and the copolymer may be a random copolymer, a block copolymer, an alternating copolymer, or a graft copolymer.

[0039] In some preferred embodiments, the crosslinkable polymer substrate may be a copolymer of monomer units with different acid-base properties, which not only strengthens the interaction between the first and second materials but also improves the stability of the adhesive during battery cycling, allowing the strong interaction between the first and second materials to be maintained for a long period of time.

[0040] In some preferred embodiments, the crosslinkable polymeric substrate comprises one or more of a copolymer of monomeric units a and d, a copolymer of monomeric units c and d, a copolymer of monomeric units b, c and d, and more preferably, the crosslinkable polymeric substrate comprises a copolymer of monomeric units b, c and d.

[0041] Furthermore, the crosslinkable polymer substrate may further selectively contain one or more of the monomer units represented by the following III-1 and III-2. JPEG0007590414000008.jpg45131

[0042] The present inventors have found that when the crosslinkable polymer substrate further comprises the monomer unit III-1, it can provide the particulate material with excellent dispersion performance, so that the slurry can be further stabilized and the processing performance of the membrane layer can be improved.When the crosslinkable polymer substrate further comprises the monomer unit III-2, it can further improve the affinity between the adhesive and the first and second substances, so that the interaction between the first and second substances can be further improved.

[0043] In the secondary battery of the present application, the compound represented by formula (II) is a crosslinking agent. In some embodiments, in the compound represented by formula (II), n is an even number between 4 and 18, preferably between 8 and 12. Also, preferably, m≧3, or m≧5, or m=n. This provides high crosslinking reaction efficiency between the crosslinkable polymer substrate and the crosslinking agent, and improves the crosslinked structure, thereby further improving the interaction between the first substance and the second substance.

[0044] In some embodiments, in the compound of formula (II), R 5 is -(R 2 ) b -Y, wherein b is 0 or 1, and R 2 is selected from linear or branched alkylene groups having 1 to 12 carbon atoms, and the above Y is selected from halogen, alkenyl group, azide group, amino group, carboxyl group, aldehyde group, hydroxyl group, sulfonic acid group, sulfinic acid group, phenolic hydroxy group, and epoxy group.

[0045] In some embodiments, when b is 1, R 2 is selected from methylene, ethylene, propylene, isopropylene, butylene, isobutylene, sec-butylene, tert-butylene, pentylene, isopentylene, hexylene, heptylene, and octylene. 2 is selected from a methylene group, an ethylene group, a propylene group, an isopropylene group, a butylene group, an isobutylene group, a sec-butylene group, and a tert-butylene group.

[0046] R 2 In the above, one or more hydrogen atoms may be replaced with other elements or groups. The other elements may be, but are not limited to, F, Cl, O, etc. The other groups may be, but are not limited to, hydroxyl groups, phenyl groups, amine groups, etc.

[0047] Preferably, R 2 is selected from linear or branched alkylene groups having 1 to 8 carbon atoms, and more preferably, R 2 is selected from linear or branched alkylene groups having 1 to 4 carbon atoms.

[0048] Preferably, Y is selected from an amino group, a carboxyl group, a hydroxyl group, and an epoxy group.

[0049] In some preferred embodiments, R 5is selected from halogen, alkenyl group, azide group, amino group, carboxyl group, aldehyde group, hydroxyl group, sulfonic acid group, sulfinic acid group, phenolic hydroxyl group, and epoxy group, and more preferably, R 5 is selected from an amino group, a carboxyl group, a hydroxyl group, and an epoxy group.

[0050] R 5 The group has high reactivity and strong polarity, and can further strengthen the interaction between the first substance and the second substance, thereby improving the adhesive strength thereof.

[0051] In some embodiments, in the compound represented by formula (II), R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, preferably R 6 is selected from H and substituted or unsubstituted hydrocarbon groups having 1 to 4 carbon atoms. For example, R 6 is selected from H, methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl, tert-butyl, n-pentyl, isopentyl, n-hexyl, n-heptyl, n-octyl, etc., preferably R 6 is selected from the group consisting of methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, and more preferably R 6 is selected from H, a methyl group, an ethyl group, an n-propyl group, and an isopropyl group.

[0052] R 6 In the formula (I), one or more hydrogens may be replaced with other elements or groups. The elements may be, but are not limited to, F, Cl, O, etc. The groups may be, but are not limited to, hydroxyl groups, amine groups, etc.

[0053] The secondary battery of the present application uses an adhesive to bond a first material and a second material. The adhesive includes a polymer obtained by crosslinking the adhesive composition. The adhesive composition includes a crosslinkable polymer base and a crosslinking agent. The crosslinkable polymer base includes a monomer unit represented by formula (I), which has an active hydrogen-containing polar group, and thus has good affinity between the adhesive and both the first material and the second material, and therefore has a strong interaction between the first material and the second material. In particular, the crosslinking agent includes a compound represented by formula (II), which has two or more groups that exhibit reaction activity with the active hydrogen-containing polar group of the monomer unit, and forms a good crosslinked structure by crosslinking the adhesive composition, thereby greatly improving the interaction force between the first material and the second material. Therefore, strong adhesion can be formed between the first material and the second material in the secondary battery, and both the structural stability and cycle life of the battery can be improved.

[0054] In some embodiments, the crosslinked polymer of the adhesive composition has a three-dimensional crosslinked network structure, which significantly enhances the adhesive bond between the first and second materials.

[0055] In some embodiments, the adhesive further comprises other adhesive materials. As an example, the adhesive may further comprise one or more of styrene butadiene rubber, sodium carboxymethylcellulose, polyvinylidene fluoride, polyvinylidene fluoride copolymers, polytetrafluoroethylene, polystyrene, polyacrylonitrile, polyimide, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan. As another example, the adhesive may further comprise one or more of styrene butadiene rubber, sodium carboxymethylcellulose, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan.

[0056] According to the secondary battery of the present application, one or more of the positive electrode sheet, the negative electrode sheet and the separator of the secondary battery comprise a polymer obtained by crosslinking the adhesive composition described herein.

[0057] In some embodiments, when one or more of the positive electrode sheet, the negative electrode sheet, and the separator include a polymer obtained by crosslinking the adhesive composition described herein, they may further include other adhesive materials. The other adhesive materials may be as described above.

[0058] In some preferred embodiments, the negative electrode sheet comprises a polymer obtained by crosslinking the adhesive composition described herein.

[0059] In some preferred embodiments, the negative electrode film of the negative electrode sheet includes a polymer obtained by crosslinking the adhesive composition described herein. When the negative electrode film includes the polymer, the force between the negative electrode active material particles can be significantly improved, and thus the rebound of the negative electrode sheet can be significantly reduced.

[0060] In some embodiments, the negative electrode film may further include other adhesive materials. The other adhesive materials may be as described above. For example, the negative electrode film may further include one or more of styrene butadiene rubber and sodium carboxymethyl cellulose.

[0061] Preferably, the mass occupancy of the crosslinked adhesive composition in the negative electrode film may be ≧0.5%, ≧0.6%, or ≧1.0%, and may further be ≦4.0%, ≦3.0%, or ≦2.0%. When the mass occupancy of the crosslinked adhesive composition in the negative electrode film is within an appropriate range, the above-mentioned effects of the adhesive can be effectively exhibited, and at the same time, the secondary battery can have a high energy density. More preferably, the mass occupancy of the crosslinked adhesive composition in the negative electrode film is 1.0% to 3.0%. [Negative electrode sheet]

[0062] The negative electrode sheet of the secondary battery of the present application includes a negative electrode current collector and a negative electrode film provided on at least one surface of the negative electrode current collector. For example, the negative electrode current collector has two surfaces opposing each other in its thickness direction, and the negative electrode film is laminated on one or both of the two opposing surfaces of the negative electrode current collector.

[0063] The negative electrode current collector can be made of a material having good electrical conductivity and mechanical strength, and in some embodiments, the negative electrode current collector can be made of copper foil.

[0064] The negative electrode film includes a negative electrode active material. The present application does not particularly limit the type of the negative electrode active material, and it can be selected according to actual needs. In some embodiments, the negative electrode active material may include one or more of silicon-based materials (e.g., elemental silicon, silicon oxygen compounds, silicon carbon composites, silicon nitrogen compounds, silicon alloys, etc.), graphite materials (e.g., artificial graphite, natural graphite), tin-based materials (e.g., elemental tin, tin oxygen compounds, tin alloys, etc.), mesocarbon microbeads (abbreviated as MCMB), hard carbon, soft carbon, lithium titanate, and other metals that can form an alloy with the active ion.

[0065] The negative electrode film further includes an adhesive. In some preferred embodiments, the adhesive may include a polymer obtained by crosslinking the above-mentioned adhesive composition. The adhesive action of the polymer can form a strong interaction between the solid particle materials (e.g., negative electrode active material, conductive agent, etc.) in the negative electrode film, thereby improving the cohesive strength of the negative electrode film. At the same time, there is a strong adhesive force between the negative electrode film and the negative electrode current collector. As a result, the negative electrode film is effectively bonded to the negative electrode current collector, making the negative electrode sheet have high strength and less likely to peel off or fall off. Therefore, the rebound problem during the cold rolling of the negative electrode sheet and the charge / discharge cycle of the secondary battery is effectively alleviated, and the expansion of the negative electrode sheet during the cycle of the battery is significantly reduced. The volume change of the battery is significantly reduced, so that the energy density, cycle life, and safety performance of the battery can all be improved.

[0066] In some embodiments, the adhesive may further include other adhesive materials for the negative electrode film. For example, the adhesive may further include one or more of styrene butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC-Na), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA) and polyvinyl butyral (PVB), such as one or more of styrene butadiene rubber, sodium carboxymethyl cellulose, polyacrylic acid, sodium polyacrylate, polyvinyl alcohol, sodium alginate, polymethacrylic acid, and carboxymethyl chitosan. Preferably, the adhesive may further include styrene butadiene rubber and sodium carboxymethyl cellulose.

[0067] By using the adhesive composition of the present application and other adhesive materials, it is possible to obtain a high adhesive effect while simultaneously providing the negative electrode film and negative electrode sheet with appropriate strength and flexibility, thereby enabling the negative electrode film and negative electrode sheet to have high processing performance.

[0068] In some embodiments, the negative electrode film may further include a conductive agent. For example, the conductive agent used in the negative electrode film may include one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0069] In some embodiments, a functional coating layer may be optionally provided between the negative electrode current collector and the negative electrode film, or on the surface of the negative electrode film that is away from the negative electrode current collector. The functional coating layer may include a polymer obtained by crosslinking the adhesive composition described herein. Optionally, the functional coating layer may further include other functional materials (e.g., conductive agents, ceramic particles, etc.). The present application does not limit the specific type of functional material, which may be selected according to actual functional demands. The adhesive composition described herein has a strong adhesive effect after crosslinking, so that it can have a strong adhesive force between each component in the functional coating layer or between the functional coating layer and the negative electrode current collector and / or the negative electrode film. This allows the functional coating layer to better exhibit its performance.

[0070] The preferred solutions of adhesive or adhesive composition herein are also applied to the negative electrode sheet herein to constitute each specific embodiment of the negative electrode sheet, and for the sake of simplicity of the specification, the description is omitted here. [Positive electrode sheet]

[0071] The positive electrode sheet of the secondary battery of the present application includes a positive electrode current collector and a positive electrode film provided on at least one surface of the positive electrode current collector and including a positive electrode active material. For example, the positive electrode current collector has two surfaces facing each other in its thickness direction, and the positive electrode film is laminated on either one or both of the two facing surfaces of the positive electrode current collector.

[0072] The positive electrode current collector can be made of a material having good electrical conductivity and mechanical strength, and in some embodiments, the positive electrode current collector can be made of aluminum foil.

[0073] The present application does not particularly limit the specific type of the positive electrode active material, and any material for the positive electrode of a secondary battery known in the art can be used, and those skilled in the art can select it according to actual needs.

[0074] In some embodiments, the secondary battery may be a lithium-ion secondary battery. The positive electrode active material is selected from lithium transition metal oxides and their modified materials, and the modified materials may be obtained by doping and / or coating the lithium transition metal oxides. For example, the lithium transition metal oxide is one or more of lithium cobalt oxide, lithium nickel oxide, lithium manganese oxide, lithium nickel manganese oxide, lithium nickel cobalt manganese oxide, lithium nickel cobalt aluminum oxide, and lithium-containing phosphates with an olivine structure.

[0075] For example, the positive electrode active material of a secondary battery is LiCoO 2 , LiNiO 2 , LiMnO 2 , LiMn 2 O 4 , LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O 2 (NCM111), LiNi 0.5 Co 0.2 Mn 0.3 O 2 (NCM523), LiNi 0.6Co 0.2 Mn 0.2 O 2 (NCM622), LiNi 0.8 Co 0.1 Mn 0.1 O 2 (NCM811), LiNi 0.85 Co 0.15 Al 0.05 O 2 , LiFePO 4 (LFP) and LiMnPO 4 The resin is selected from one or more of the following:

[0076] The positive electrode film further includes an adhesive. In some preferred embodiments, the adhesive may include a polymer obtained by crosslinking the above-mentioned adhesive composition. The adhesive action of the polymer can form a strong interaction between the solid particle materials (e.g., positive electrode active material, conductive agent, etc.) in the positive electrode film, thereby improving the cohesive strength of the positive electrode film. At the same time, a strong adhesive force can be obtained between the positive electrode film and the positive electrode current collector. This allows the positive electrode film to be effectively adhered to the positive electrode current collector, so that the positive electrode sheet has high strength and is less likely to peel off or fall off.

[0077] In some embodiments, the adhesive may further include other adhesive materials for the positive electrode film. For example, the adhesive may further include one or more of styrene butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC-Na), polyacrylic acid (PAA), sodium polyacrylate (PAAS), polyvinyl alcohol (PVA), sodium alginate (SA), polymethacrylic acid (PMAA), carboxymethyl chitosan (CMCS), polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), ethylene-vinyl acetate copolymer (EVA), polyvinyl alcohol (PVA), and polyvinyl butyral (PVB), such as one or more of polyvinylidene fluoride, polytetrafluoroethylene, ethylene-vinyl acetate copolymer, polyvinyl alcohol, and polyvinyl butyral.

[0078] In some embodiments, the positive electrode film may further include a conductive agent. The type of the conductive agent is not particularly limited, and a person skilled in the art may select it according to actual functional demands. For example, the conductive agent used in the positive electrode film may include one or more of graphite, superconducting carbon, acetylene black, carbon black, ketjen black, carbon dots, carbon nanotubes, graphene, and carbon nanofibers.

[0079] In some embodiments, a functional coating layer may be optionally provided between the positive current collector and the positive electrode film, or on the surface of the positive electrode film facing the positive current collector. The functional coating layer may include a polymer obtained by crosslinking the adhesive composition described herein. Optionally, the functional coating layer may further include other functional materials (e.g., conductive agents, ceramic particles, etc.). The present application does not limit the specific type of functional material, which may be selected according to actual functional demands. The adhesive composition described herein has a strong adhesive effect after crosslinking, so that it can have a high adhesive strength between each component in the functional coating layer or between the functional coating layer and the positive current collector and / or the positive electrode film. This allows the functional coating layer to better exhibit its performance.

[0080] The preferred solutions of adhesive or adhesive composition herein are also applied to the positive electrode sheet herein to constitute each specific embodiment of the positive electrode sheet, and for the sake of simplicity of the specification, the description is omitted here. [Electrolyte]

[0081] The secondary battery of the present disclosure further includes an electrolyte. The electrolyte serves to transport ions between the positive electrode sheet and the negative electrode sheet. The type of electrolyte of the present application is not particularly limited and can be selected according to actual needs. For example, the electrolyte may be at least one selected from a solid electrolyte and a liquid electrolyte (i.e., an electrolytic solution).

[0082] In some embodiments, the electrolyte uses an electrolyte solution. The electrolyte solution includes an electrolyte salt and a solvent. The electrolyte solution is infiltrated into the core to transport ions. For example, the core may be a laminated core formed by sequentially stacking a positive electrode sheet, a separator, and a negative electrode sheet, or a wound core formed by sequentially stacking a positive electrode sheet, a separator, and a negative electrode sheet, and winding the core.

[0083] In some embodiments, the electrolyte salt is LiPF 6 (Lithium hexafluorophosphate), LiBF 4 (Lithium tetrafluoroborate), LiClO 4 (lithium perchlorate), LiAsF 6 (lithium hexafluoroarsenate), LiFSI (lithium difluorosulfonylimide), LiTFSI (lithium bis(trifluoromethanesulfonyl)imide), LiTFS (lithium trifluoromethanesulfonate), LiDFOB (lithium difluorooxalate borate), LiBOB (lithium disoxalate borate), LiPO 2 F 2 (lithium difluorophosphate), LiDFOP (lithium difluorodisalophosphate), and LiTFOP (lithium tetrafluorooxalophosphate).

[0084] In some embodiments, the solvent may be one or more of ethylene carbonate (EC), propylene carbonate (PC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), dimethyl carbonate (DMC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), butylene carbonate (BC), fluoroethylene carbonate (FEC), methyl formate (MF), methyl acetate (MA), ethyl acetate (EA), propyl acetate (PA), methyl propionate (MP), ethyl propionate (EP), propyl propionate (PP), methyl butyrate (MB), ethyl butyrate (EB), 1,4-butyrolactone (GBL), sulfolane (SF), dimethyl sulfone (MSM), methyl ethyl sulfone (EMS), and diethyl sulfone (ESE).

[0085] In some embodiments, the electrolyte may further include additives. For example, the additives may include additives for forming a negative electrode film, additives for forming a positive electrode film, or additives that can improve a specific performance of the battery, such as additives for improving the overcharge performance of the battery, additives for improving the high temperature performance of the battery, and additives for improving the low temperature performance of the battery.

[0086] In some embodiments, the electrolyte may be a solid electrolyte, such as a polymer electrolyte. [Separator]

[0087] In some secondary batteries using an electrolyte and solid electrolyte, a separator is further included. The separator serves to isolate the positive electrode sheet and the negative electrode sheet. The separator includes a substrate and optionally includes a functional coating layer provided on at least one surface of the substrate. The functional coating layer can be used to improve the heat resistance, mechanical strength, etc. of the separator. Optionally, the functional coating layer may further include other functional materials (e.g., ceramic particles, other polymers, etc.). The present application does not particularly limit the type of substrate of the separator, and may be any well-known substrate of a porous structure separator having good chemical stability and mechanical stability. In some embodiments, the material of the substrate of the separator may be one or more types selected from glass fiber, nonwoven fabric, polyethylene, and polypropylene. The separator may be a single layer film or a multi-layer composite film. When the separator is a multi-layer composite film, the materials of each layer may be the same or different.

[0088] In some preferred embodiments, the functional coating layer of the separator may include a polymer obtained by crosslinking the adhesive composition described above. The polymer has a strong adhesive effect, so that the functional coating layer has a strong adhesive force between each component in the functional coating layer or between the functional coating layer and the substrate, so that the functional coating layer can better exert the effect of improving the performance of the separator.

[0089] The preferred solutions relating to adhesives or adhesive compositions herein also apply to the separators herein and constitute specific embodiments of the separators, and for the sake of brevity, the description is omitted here.

[0090] In some embodiments, the secondary battery may include an exterior and a core sealed within the exterior. The number of cores included in the secondary battery may be one or more and can be adjusted according to demand.

[0091] In some embodiments, the exterior of the secondary battery may be a soft pack (e.g., a bag-shaped soft pack, the material of which may be plastic, for example, one or more of polypropylene (PP), polybutylene terephthalate (PBT), polybutylene succinate (PBS), etc.) or a hard case (e.g., an aluminum case, etc.).

[0092] The present application does not particularly limit the shape of the secondary battery, which may be cylindrical, rectangular, or any other shape. Figure 1 shows a secondary battery 5 having a rectangular structure as an example.

[0093] In some embodiments, the secondary batteries can be assembled to form a battery module, and the number of secondary batteries included in the battery module can be multiple, and the specific number can be adjusted according to the application and capacity of the battery module.

[0094] Fig. 2 shows an example of a battery module 4. Referring to Fig. 2, in the battery module 4, a plurality of secondary batteries 5 may be arranged sequentially along the length direction of the battery module 4. Of course, the batteries may be arranged in any other manner. Furthermore, the plurality of secondary batteries 5 may be fixed by a fastener.

[0095] Optionally, the battery module 4 may further include a case having an accommodating space, in which the multiple secondary batteries 5 are accommodated.

[0096] In some embodiments, the battery modules can be further assembled to form a battery pack, and the number of battery modules included in the battery pack can be adjusted according to the application and capacity of the battery pack.

[0097] 3 and 4 show an example of a battery pack 1. Referring to Fig. 3 and Fig. 4, the battery pack 1 may include a battery box and a plurality of battery modules 4 arranged in the battery box. The battery box includes an upper housing 2 and a lower housing 3, and the upper housing 2 is arranged to cover the lower housing 3, and may form an enclosed space for accommodating the battery modules 4. The plurality of battery modules 4 may be arranged in the battery box in any manner. [Manufacturing method]

[0098] The present application further provides a method for producing a secondary battery, the method comprising: applying an adhesive composition to one or more of a positive electrode sheet, a negative electrode sheet, and a separator; and causing a crosslinking reaction of the adhesive composition by heat treatment, the adhesive composition comprising a crosslinkable polymer base and a crosslinking agent, the crosslinkable polymer base comprising a monomer unit represented by formula (I), the crosslinking agent comprising a compound represented by formula (II), JPEG0007590414000009.jpg47151 Here, the above R 1 , R 2 and R 3 are each independently selected from H and a linear or branched alkyl group having 1 to 8 carbon atoms; Above R 4 is an active hydrogen-containing polar group, Above R 5 is the above R 4 is a group that exhibits reactivity towards Above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, The above n is an even number of 4 or more, 2≦m≦n, and preferably m≧3.

[0099] In some embodiments, the temperature at which the adhesive composition is heat-treated to crosslink it may be 60° C. to 160° C., preferably 60° C. to 140° C., and more preferably 80° C. to 120° C. For example, the crosslinkable polymer substrate and the crosslinking agent are crosslinked at a heating temperature of 60° C. to 160° C., 60° C. to 140° C., or 80° C. to 120° C. to form a polymer having a three-dimensional crosslinked network structure.

[0100] In some embodiments, the manufacture of the secondary battery further includes assembling the negative electrode sheet, the positive electrode sheet, the separator, and the electrolyte to form the secondary battery.

[0101] In some embodiments, a core is obtained by sequentially winding or stacking a positive electrode sheet, a separator, and a negative electrode sheet, with the separator acting as an insulator between the positive electrode sheet and the negative electrode sheet, and the core is placed in an outer casing, and an electrolyte is injected and sealed, thereby obtaining a secondary battery.

[0102] In some preferred embodiments, the method for producing the secondary battery includes applying the adhesive composition of the present application to a negative electrode sheet.

[0103] In some further preferred embodiments, the process for producing a negative electrode sheet using the adhesive composition of the present application is as follows.

[0104] In S10, a negative electrode slurry is provided, the negative electrode slurry including a negative electrode active material, an adhesive composition described herein, and an optional conductive agent. In some embodiments, in step S10, the negative electrode active material, the adhesive composition described herein, and the optional conductive agent can be dispersed in a solvent to form a uniform negative electrode slurry, and the solvent can be deionized water. The order of addition is not particularly limited. For example, a solution of the adhesive composition can be obtained first, and then the negative electrode active material and other additive materials can be added to the solution. Furthermore, each component of the adhesive, the negative electrode active material, and other additives can be added to the solvent respectively to obtain the negative electrode slurry.

[0105] In S20, the negative electrode slurry is applied to at least one surface of a negative electrode current collector to obtain a negative electrode film.

[0106] In S30, the negative electrode coating layer is dried under heating conditions to remove the solvent and to cause a crosslinking reaction between the crosslinkable polymer base and the crosslinking agent. In some embodiments, in step S30, the drying temperature may be 60° C. to 140° C., 60° C. to 140° C., or 80° C. to 120° C., or 95° C. to 120° C. Under heating conditions, the R of the crosslinkable polymer substrate may be 4 R of group and crosslinker 5 The group undergoes a crosslinking reaction to form a crosslinked structure.

[0107] In S40, the dried negative electrode coating layer is subjected to a process such as cold rolling, and then a negative electrode sheet is obtained.

[0108] The preferred solutions relating to the adhesive or adhesive composition herein also apply to the manufacturing method herein and constitute specific embodiments of the manufacturing method, and for the sake of simplicity of the specification, the description is omitted here. [Device]

[0109] A second aspect of the present application provides a device including the secondary battery of the first aspect of the present application, the secondary battery providing power to the device, which may include, but is not limited to, mobile devices (e.g., mobile phones, laptops, etc.), electric vehicles (e.g., pure electric vehicles, hybrid electric vehicles, plug-in hybrid electric vehicles, electric bicycles, electric scooters, electric golf carts, electric trucks, etc.), electric trains, ships and satellites, energy storage systems, etc.

[0110] The device can select a secondary battery, a battery module or a battery pack according to the needs of its use.

[0111] 5 shows an example of an apparatus, such as a pure electric vehicle, a hybrid electric vehicle, or a plug-in hybrid electric vehicle, etc. A battery pack or battery module may be used to meet the device's requirements for high power and high energy density of secondary batteries.

[0112] Other example devices may be mobile phones, tablets, notebook computers, etc. Such devices generally require light weight and thinness and may use secondary batteries as a power source. [Adhesive composition]

[0113] The present invention provides an adhesive composition comprising a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate comprising one or more of the monomer units represented by formula (I) and the crosslinking agent comprising a compound represented by formula (II): JPEG0007590414000010.jpg46147 Here, the above R 1 , R 2 and R 3 are each independently selected from H and a linear or branched alkyl group having 1 to 8 carbon atoms; Above R 4 is an active hydrogen-containing polar group, Above R 5 is the above R 4 is a group that exhibits reactivity towards Above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms, The above n is an even number of 4 or more, 2≦m≦n, and preferably m≧3.

[0114] The specific and preferred solutions of the adhesive composition described hereinabove also apply here, and for the sake of brevity, the description is omitted here.

[0115] In some embodiments, the weight percentage of the crosslinkable polymer substrate in the adhesive composition is ≧70%, ≧75%, ≧80%, ≧85%, or ≧90%, or even ≦99%, ≦98%, ≦97%, ≦96%, or ≦95%, based on the total weight of the crosslinkable polymer substrate and the crosslinking agent. Preferably, the weight percentage of the crosslinkable polymer substrate is 75% to 95%, more preferably 85% to 95%, based on the total weight of the crosslinkable polymer substrate and the crosslinking agent. This allows the adhesive to form a good crosslinked three-dimensional network, and therefore the adhesive effect can be effectively exerted.

[0116] In some embodiments, the weight average molecular weight of the crosslinkable polymer substrate may be 200,000 to 800,000, preferably 400,000 to 600,000. The polymer adhesive material has an appropriate molecular weight and has good solubility in polar solvents (e.g., water), while allowing the resulting solution to have an appropriate viscosity, which is advantageous for uniformly dispersing solid phase materials (e.g., negative electrode active materials, conductive agents, etc.) in the solution.

[0117] The molecular weight of the crosslinkable polymer substrate can be measured using methods common in the art, for example, using laser light scattering techniques, which are well known to those skilled in the art.

[0118] In some embodiments, the viscosity of a 10 wt % aqueous solution containing the adhesive composition is 150 mPa·s to 20000 mPa·s, preferably 600 mPa·s to 5000 mPa·s, and more preferably 600 mPa·s to 4000 mPa·s, so that when the adhesive composition is used to prepare a slurry for a film or coating layer (e.g., a negative electrode slurry), the solid phase material (e.g., a negative electrode active material, a conductive agent, etc.) can be more uniformly dispersed in the slurry.

[0119] The viscosity of the 10 wt% aqueous solution containing the adhesive composition can be measured using a method commonly used in the art. For example, it can be measured using a viscometer (e.g., Brookfield DV2T viscometer, USA), and the technique is well known to those skilled in the art. For example, 1 g of the adhesive composition is dissolved in 9 g of deionized water, and the viscosity of the resulting solution is measured and recorded as the viscosity of the 10 wt% aqueous solution containing the adhesive composition.

[0120] In some embodiments, the pH of a 10 wt % aqueous solution containing the adhesive composition is pH>7, preferably 7.5 to 10.5, and more preferably 8.0 to 10.0. The inventors have found that when the crosslinkable polymer substrate has an appropriate content of active hydrogen, the crosslinked structure is improved and the adhesive has high stability.

[0121] In some embodiments, the pH of the crosslinkable polymer substrate can be adjusted by incorporating monomer units with different acidic and basic properties.

[0122] The pH of the crosslinkable polymer substrate can be measured using a method commonly used in the art. For example, 1 g of the adhesive composition is dissolved in 9 g of deionized water, and the pH of the resulting solution is measured and recorded as the pH of a 10 wt% aqueous solution containing the adhesive composition.

[0123] In some embodiments, both the crosslinkable polymeric substrate and the crosslinking agent can be prepared by methods known in the art or purchased commercially.

[0124] In some embodiments, one or more of the monomers corresponding to the monomer unit represented by formula (I) can be polymerized in the presence of an initiator to obtain a crosslinkable polymer substrate. The type of initiator is not particularly limited and may be selected from the general selection in the art. For example, the initiator may be at least one selected from azo-based initiators (e.g., azobisisobutyronitrile, azobisisobutylamidine hydrochloride, azobisisobutylimidazoline hydrochloride, azobiscyanovaleric acid, azobisisopropylimidazoline, etc.). The polymerization conditions and the amount of initiator used are not particularly limited and may be selected according to the specific types of monomer and initiator. Working Example

[0125] The following examples are provided to more specifically illustrate the disclosed contents of the present application, and these examples are provided for illustrative purposes only, and it is obvious to those skilled in the art that various modifications and changes can be made within the scope of the disclosed contents of the present application.Unless otherwise specified, all parts, percentages, and ratios reported in the following examples are calculated by weight, and all reagents used in the examples can be purchased or synthesized according to conventional methods, and can be used directly without further processing, and all equipment used in the examples can be purchased. 1. Crosslinkable polymer substrate and crosslinking agent:

[0126] 1. The crosslinkable polymer substrate A used in each of the following examples is 1 ~A 6 is selected from.

[0127] (1)A 1 is a homopolymer of monomer unit c and has a molecular weight of 450,000. It can be purchased from TCI.

[0128] (2)A 2 is a copolymer of monomer units b, c and d. Preparation method: CH 2 =C(CH 3)COOH, CH 2 =CHCONH 2 , C.H. 2 =CHOH was added in a molar ratio of 20:65:15 and polymerized in the presence of an initiator azodiisobutylamidine hydrochloride, and the amount of the initiator used was 0.5 parts by weight for 100 parts by weight of the above three types of monomers. The polymerization temperature was 25°C to 35°C, the polymerization pressure was 101 kPa, and the polymerization time was 2 to 4 hours. 2 A 2 The weight average molecular weight is 450,000.

[0129] (3)A 3 is a copolymer of monomer unit c and monomer unit d. Preparation method: CH 2 =CHCONH 2 and C.H. 2 =CHOH was added in a molar ratio of 85:15 and polymerized in the presence of an initiator azodiisobutylamidine hydrochloride, and the amount of the initiator used was 0.5 parts by weight per 100 parts by weight of the above two types of monomers. The polymerization temperature was 25°C to 35°C, the polymerization pressure was 101 kPa, and the polymerization time was 2 to 4 hours. 3 A 3 The weight average molecular weight is 550,000.

[0130] (4)A 4 is a copolymer of monomer unit a and monomer unit d. Preparation method: CH 2 =CHCOOH and CH 2 =CHOH was added in a molar ratio of 85:15 and polymerized in the presence of an initiator azodiisobutylamidine hydrochloride, and the amount of the initiator used was 0.5 parts by weight per 100 parts by weight of the above two types of monomers. The polymerization temperature was 25°C to 35°C, the polymerization pressure was normal pressure, and the polymerization time was 2 to 4 hours. 4 A 4 The weight average molecular weight is 600,000.

[0131] (5)A 5 is a copolymer of monomer unit b, monomer unit d and monomer unit III-1. Preparation method: CH 2 =C(CH 3 )COOH, CH 2 =CHOH, CH 2 =CHCOONa was added in a molar ratio of 70:15:15, and polymerization reaction was carried out in the presence of an initiator, azodiisobutylamidine hydrochloride. The amount of the initiator used was 0.5 parts by weight per 100 parts by weight of the above three types of monomers. The polymerization temperature was 25°C to 35°C, the polymerization pressure was normal pressure, and the polymerization time was 2 to 4 hours. 5 A 5 The weight average molecular weight is 500,000.

[0132] (6)A 6 is a copolymer of monomer unit b, monomer unit d and monomer unit III-2. Preparation method: CH 2 =C(CH 3 )COOH, CH 2 =CHOH, CH 2 =CHCN was added in a molar ratio of 70:15:15 and polymerized in the presence of an initiator, azodiisobutylamidine hydrochloride. The amount of the initiator used was 0.5 parts by weight per 100 parts by weight of the above three types of monomers. The polymerization temperature was 25°C to 35°C, the polymerization pressure was normal pressure, and the polymerization time was 2 to 4 hours. A crosslinkable polymer substrate A was prepared. 6 A 6 The weight average molecular weight is 350,000.

[0133] 2. The crosslinking agent B used in each of the following examples is 1 ~B 3 (B 1 ~B 3 (available from Gelest, Inc.). JPEG0007590414000011.jpg6287 2. Battery manufacturing Example 1 Preparation of Adhesive Composition

[0134] The above crosslinkable polymer substrate A 1 and crosslinker B 1 and physically mixing them in a mass ratio of 95:5 to obtain the adhesive composition of the present application. Manufacture of negative electrode sheets

[0135] Negative electrode active material: artificial graphite, conductive agent: Super-P, the adhesive composition prepared above, styrene butadiene rubber SBR, and sodium carboxymethyl cellulose CMC-N are mixed in a mass ratio of 96:1:1:1.5:0.5 in an appropriate amount of deionized water by thorough stirring to form a uniform negative electrode slurry, which is then applied to a negative electrode current collector copper foil, dried, and cold-rolled to obtain a negative electrode sheet. The drying temperature for the negative electrode coating layer is 80℃ to 150℃. Manufacture of positive electrode sheets

[0136] Positive electrode active material LiNi 0.5 Co 0.2 Mn 0.3 O 2 (NCM523), conductive agent Super P, adhesive PVDF are mixed with an appropriate amount of NMP in a weight ratio of 96:2:2 and stirred thoroughly to form a homogeneous positive electrode slurry. The positive electrode slurry is applied to the surface of the positive electrode current collector aluminum foil, and after drying and cold rolling, a positive electrode sheet is obtained. Preparation of electrolyte

[0137] Ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) were mixed uniformly in a volume ratio of 1:1:1, and then LiPF 6 is uniformly dissolved in the above solution to obtain an electrolyte, in which LiPF 6 The concentration is 1 mol / L. Separator

[0138] Use polyethylene (PE) film. Secondary battery manufacturing

[0139] A positive electrode sheet, a separator, and a negative electrode sheet are sequentially stacked and wound to obtain a core. The core is then placed inside an outer casing, dried to remove moisture, and the above-mentioned electrolyte solution is injected and sealed. After going through processes such as chemical formation and aging, a secondary battery is obtained. Examples 2 to 19 and Comparative Examples 1 to 3

[0140] The difference from Example 1 is that a different secondary battery is obtained by changing the adhesive in the negative electrode sheet. Details are as shown in Table 1. Testing Part 1. Negative electrode sheet cohesion test:

[0141] The negative electrode sheet after one-sided coating and cold rolling is taken and cut to prepare a test sample with a length of 100 mm and a width of 10 mm. A stainless steel plate with a width of 25 mm is taken, double-sided tape (width) is attached, and the test sample is attached to the double-sided tape on the stainless steel plate, where the negative electrode current collector and the double-sided tape are bonded. A 2000g press roller is used to roll back and forth on the surface of the sample three times (300mm / min). After that, a tape with a width of 10 mm and a thickness of 50 μm is attached to the surface of the negative electrode film, and a 2000g press roller is used to roll back and forth on the surface three times (300mm / min). The tape was folded 180 degrees, and the tape and the negative electrode film were manually peeled off by 25 mm. The sample was fixed to an Instron 336 tensile tester, and the peeling surface was aligned with the force line of the tester (i.e., 180° peeling was performed). The sample was continuously peeled off at 300 mm / min to obtain a cohesive strength curve of the negative electrode sheet. The average value of the stable part was taken as the peeling force F. 0 Then, the measured cohesive force of the negative electrode sheet is F = F 0 / width of the test sample, and the unit of measure for F is N / m. 2. Battery cycle performance test

[0142] The first charge and discharge are performed in an environment of 25°C, and constant current and constant voltage charging is performed with a charge current of 0.5C (i.e., the current value at which the theoretical capacity is completely discharged within 2 hours) until the upper limit voltage reaches 4.25V. Thereafter, constant current discharging is performed with a discharge current of 0.5C until the final voltage reaches 2.8V, and the initial discharge capacity value is recorded. Next, 1000 charge and discharge cycles are performed, the discharge capacity value during the cycle process is recorded, and the cycle capacity retention rate is calculated. Capacity retention at 1000th cycle = (discharge capacity at 1000th cycle / discharge capacity at first cycle) x 100%. 3. Battery cycle expansion force test

[0143] The battery is attached to a steel plate jig, and the bottom and four side surfaces of the battery are pressed tightly against the steel plate jig. The preload of the steel plate is adjusted to 2000 N. A pressure sensor is placed between the steel plate jig and the battery and connected to a computer, which measures the expansion force value of the battery after 1000 cycles.

[0144] [Table 1]

[0145] In Table 1, The weight ratio A:B indicates the weight ratio of the crosslinkable polymer substrate and the crosslinker in the adhesive composition; A+B weight occupancy indicates the weight occupancy of the crosslinkable polymer substrate and the crosslinking agent in the negative electrode coating layer, The SBR weight percentage indicates the weight percentage of SBR in the negative electrode coating layer, The CMC-Na weight occupancy indicates the weight occupancy of CMC-Na in the negative electrode coating layer.

[0146] As can be seen from the comparison of Examples 1 to 19 and Comparative Examples 1 to 3, the adhesive composition of the present application contains the crosslinkable polymer base and the crosslinking agent, and has a strong interaction force between the negative active material particles of the negative electrode sheet using the adhesive composition, so that the cohesive force of the negative electrode sheet is significantly improved. At the same time, the negative electrode sheet has a higher adhesive force. The secondary battery using the negative electrode sheet has a significantly improved cycle life and a significantly reduced cycle expansion force.

[0147] Comparative Example 1 uses conventional SBR and CMC-Na as adhesives, Comparative Example 2 uses crosslinkable polymer substrate, SBR and CMC-Na as adhesives, Comparative Example 3 uses crosslinking agent, SBR and CMC-Na as adhesives, and the interaction force between the negative electrode active material particles is low, so the cohesive force of the negative electrode sheet is low. The battery using the negative electrode sheet has poor cycle life and high cycle expansion force.

[0148] As can be seen from the results of Examples 1 to 6, by selecting an appropriate crosslinkable polymer substrate, the cohesive strength of the negative electrode sheet can be further improved, and the cycle life and low cycle expansion performance of the battery can be further improved.

[0149] As can be seen from the results of Examples 2, 7 and 8, by selecting an appropriate crosslinking agent, the cohesive strength of the negative electrode sheet can be further improved, and the cycle life and low cycle expansion performance of the battery can be further improved.

[0150] As can be seen from the results of Examples 2 and 9 to 14, when the weight ratio of the crosslinkable polymer base to the crosslinking agent in the adhesive composition is appropriate, the cohesive strength of the negative electrode sheet can be further improved, and the cycle life and low cycle expansion performance of the battery can be further improved.

[0151] As can be seen from the results of Examples 2 and 15 to 19, by rationally combining the crosslinkable polymer matrix and the crosslinking agent with SBR and CMC-Na, the negative electrode sheet can have high cohesive strength, and at the same time, the battery can have a long cycle life and low cycle expansion force.

[0152] Although the specific embodiments of the present application have been described above, the scope of protection of the present application is not limited thereto, and those skilled in the art can easily think of various equivalent modifications or replacements within the technical scope disclosed in the present application, and these modifications or replacements should be included in the scope of the present application. Therefore, the scope of protection of the present application shall be equivalent to the scope of protection of the claims.

Claims

1. A secondary battery, The secondary battery includes a positive electrode sheet, a negative electrode sheet, and a separator, One or more selected from the positive electrode sheet and the negative electrode sheet includes an adhesive used to bond a first material and a second material; The adhesive comprises a polymer obtained by crosslinking an adhesive composition, the adhesive composition comprising a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate comprising one or more of the monomer units represented by formula (I), the crosslinking agent comprising a compound represented by formula (II), Here, the above R 1 , R 2 and R 3 are each independently selected from H, a linear or branched alkyl group having 1 to 8 carbon atoms; The above R 4 teeth, is selected from The above R 5 is -(R 2 ) b -Y, b is 0 or 1, and R 2 is selected from a linear or branched alkylene group having 1 to 4 carbon atoms, and Y is selected from an amino group, a carboxyl group, a hydroxyl group, and an epoxy group; The above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms; The n is an even number equal to or greater than 4, and 2≦m≦n. The weight average molecular weight of the crosslinkable polymer substrate is 200,000 to 800,000. Secondary battery.

2. m≧3; The secondary battery according to claim 1 .

3. The polymer has a cross-linked three-dimensional network structure. The secondary battery according to claim 1 or 2.

4. The monomer unit represented by the formula (I) includes one or more of the following a to d: The secondary battery according to claim 1 .

5. The crosslinkable polymer substrate comprises one or more of a copolymer of monomer units a and d, a copolymer of monomer units c and d, and a copolymer of monomer units b, c and d; The secondary battery according to claim 4 .

6. The crosslinkable polymer substrate comprises a copolymer of monomer units b, c and d; The secondary battery according to claim 5 .

7. The crosslinkable polymer substrate further contains one or more of the monomer units represented by the following III-1 and III-2: The secondary battery according to claim 1 .

8. the adhesive further comprises one or more of styrene butadiene rubber, sodium carboxymethylcellulose, polyvinylidene fluoride, polyvinylidene fluoride copolymers, polytetrafluoroethylene, polystyrene, polyacrylonitrile, polyimide, sodium alginate, and carboxymethyl chitosan; The secondary battery according to claim 1 .

9. The negative electrode sheet contains the adhesive. The secondary battery according to claim 1 .

10. The negative electrode sheet includes a negative electrode current collector and a negative electrode film provided on at least one surface of the negative electrode current collector, the negative electrode film includes the polymer, and a mass occupancy rate of the crosslinked adhesive composition in the negative electrode film is ≧0.5%. The secondary battery according to claim 9.

11. The mass occupancy rate of the crosslinked adhesive composition in the negative electrode film is 1.0% to 3.0%. The secondary battery according to claim 10.

12. A device comprising the secondary battery according to any one of claims 1 to 11.

13. 1. An adhesive composition comprising: a crosslinkable polymer substrate and a crosslinking agent, the crosslinkable polymer substrate comprising one or more of the monomer units represented by formula (I) and the crosslinking agent comprising a compound represented by formula (II), Here, the above R 1 , R 2 and R 3 are each independently selected from H, a linear or branched alkyl group having 1 to 8 carbon atoms; The above R 4 teeth, is selected from The above R 5 is -(R 2 ) b -Y, b is 0 or 1, and R 2 is selected from a linear or branched alkylene group having 1 to 4 carbon atoms, and Y is selected from an amino group, a carboxyl group, a hydroxyl group, and an epoxy group; The above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms; The n is an even number equal to or greater than 4, and 2≦m≦n. The weight average molecular weight of the crosslinkable polymer substrate is 200,000 to 800,000. Adhesive composition.

14. m≧3; The adhesive composition of claim 13.

15. The weight average molecular weight of the crosslinkable polymer substrate is 400,000 to 600,000. The adhesive composition according to claim 13 or 14.

16. Based on the total weight of the crosslinkable polymer substrate and the crosslinking agent, the weight percentage of the crosslinkable polymer substrate is ≧70%; The adhesive composition according to any one of claims 13 to 15.

17. Based on the total weight of the crosslinkable polymer substrate and the crosslinking agent, the weight percentage of the crosslinkable polymer substrate is 75% to 95%. The adhesive composition of claim 16.

18. Based on the total weight of the crosslinkable polymer substrate and the crosslinking agent, the weight percentage of the crosslinkable polymer substrate is 85% to 95%. The adhesive composition of claim 17.

19. The adhesive composition further comprises: (1) The viscosity of a 10% by weight aqueous solution of the adhesive composition is 150 mPa·s to 20,000 mPa·s; (2) The pH value of a 10% by weight aqueous solution of the adhesive composition is pH>7. Satisfy one or more of the following: The adhesive composition according to any one of claims 13 to 18.

20. The adhesive composition further comprises: (1) The viscosity of a 10% by weight aqueous solution of the adhesive composition is 600 mPa·s to 4000 mPa·s; (2) The pH value of a 10% by weight aqueous solution of the adhesive composition is 7.5 to 10.

5. Satisfy one or more of the following:

20. The adhesive composition of claim 19.

21. A method for manufacturing a secondary battery, comprising: Adhering a first material and a second material with an adhesive; The adhesive comprises a crosslinkable polymer substrate and a polymer obtained by crosslinking a crosslinking agent; The secondary battery includes a positive electrode sheet, a negative electrode sheet, and a separator, and one or more selected from the positive electrode sheet and the negative electrode sheet include an adhesive; The crosslinkable polymer substrate comprises one or more of the monomer units represented by formula (I), and the crosslinker comprises a compound represented by formula (II), Here, the above R 1 , R 2 and R 3 are each independently selected from H, a linear or branched alkyl group having 1 to 8 carbon atoms; The above R 4 teeth, is selected from The above R 5 is -(R 2 ) b -Y, b is 0 or 1, and R 2 is selected from a linear or branched alkylene group having 1 to 4 carbon atoms, and Y is selected from an amino group, a carboxyl group, a hydroxyl group, and an epoxy group; The above R 6 is selected from H, a substituted or unsubstituted hydrocarbon group having 1 to 8 carbon atoms; The n is an even number equal to or greater than 4, and 2≦m≦n. The weight average molecular weight of the crosslinkable polymer substrate is 200,000 to 800,000. Manufacturing method.

22. m≧3; The method of claim 21.

23. The crosslinkable polymer substrate and the crosslinking agent are crosslinked under heating conditions. The method of claim 21 or 22.

24. The heating temperature is 60°C to 160°C. The method of claim 23.

Citation Information

Patent Citations

  • Rare earth alloy doped zinc-manganese battery and preparation method thereof

    CN110492092A

  • Binder aqueous solution for lithium ion battery, slurry for lithium ion battery, manufacturing methods thereof, electrode for lithium ion battery, separator for lithium ion battery, separator / electrode laminate for lithium ion battery, and lithium ion battery

    JP2019057487A