Grinding method

A two-step polishing method with adaptive pressure adjustments addresses non-uniform film thickness issues by reversing distribution profiles to enhance uniformity, particularly at the wafer's outer periphery.

JP7590913B2Active Publication Date: 2024-11-27EBARA CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021076023
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-04-28
Publication Date
2024-11-27
Estimated Expiration
2041-04-28

AI Technical Summary

Technical Problem

The challenge of achieving uniform film thickness across the wafer during chemical mechanical polishing is exacerbated by significant variations in film thickness in the radial direction, particularly at the outer periphery, despite adjustments in airbag pressure.

Method used

A polishing method involving two distinct polishing steps with different pressure conditions is employed, where the first step adjusts pressure based on real-time feedback to achieve uniformity within a tolerance range, and the second step reverses the film thickness distribution to address non-uniformity at the outer periphery by actively polishing thicker areas and suppressing thinner areas.

Benefits of technology

This approach significantly improves the uniformity of film thickness across the wafer, particularly at the outer periphery, by dynamically adjusting pressure conditions to counteract residual thickness variations.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590913000002
    Figure 0007590913000002
  • Figure 0007590913000003
    Figure 0007590913000003
  • Figure 0007590913000004
    Figure 0007590913000004
Patent Text Reader

Abstract

To provide a polishing method that can improve the uniformity of wafer thickness.SOLUTION: A polishing method includes a second polishing step for polishing a substrate under second polishing conditions. The second polishing conditions include a polishing condition determined to form a second polishing profile having an opposite distribution to the distribution of a first polishing profile.SELECTED DRAWING: Figure 7
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a polishing method. [Background technology]

[0002] Chemical mechanical polishing (CMP) is known as a technique in the manufacturing process of semiconductor devices. A polishing apparatus for performing CMP includes a polishing table that supports a polishing pad and a polishing head that holds a wafer.

[0003] When a wafer is polished using such a polishing apparatus, the wafer is held by the polishing head and pressed against the polishing surface of the polishing pad with a predetermined pressure. At this time, the polishing table and the polishing head are moved relative to each other to bring the wafer into sliding contact with the polishing surface, thereby polishing the surface of the wafer.

[0004] Furthermore, a signal corresponding to the wafer thickness is detected by a film thickness sensor to obtain the wafer thickness distribution. Based on the wafer thickness distribution, the pressure of multiple airbags arranged concentrically on the polishing head is controlled. The film thickness sensor rotates together with the polishing table, and the polishing head that holds the wafer also rotates. Usually, the moving path of the film thickness sensor across the wafer surface is different every time the polishing table rotates. As an index value for controlling the pressure of each airbag, usually, the film thicknesses measured at different measuring points on each concentric airbag are averaged to calculate a value that represents the film thickness in each airbag. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] International Publication No. 2015 / 163164 [Patent Document 2] JP 2005-11977 A Summary of the Invention [Problem to be solved by the invention]

[0006] In recent years, the required degree of uniformity in film thickness has been increasing. In an area of ​​the wafer corresponding to one of the concentrically arranged airbags, the film thickness varies greatly in the radial direction of the wafer, and there is a problem that even if the pressure of the airbag corresponding to that area is adjusted, it is not possible to improve the film thickness uniformity beyond a certain level.

[0007] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a polishing method capable of improving the uniformity of the film thickness on a wafer. [Means for solving the problem]

[0008] In one embodiment, a polishing method is provided in which a substrate is pressed against a polishing surface of a polishing pad by a polishing head having a plurality of pressure chambers including a specific pressure chamber, the polishing method comprising: a first polishing step of polishing the substrate under a first polishing condition; and a second polishing step of polishing the substrate under a second polishing condition determined based on a first polishing profile along a radial direction of a specific region of the substrate corresponding to the specific pressure chamber, the first polishing condition being obtained by previously polishing a substrate different from the substrate under the first polishing condition, the second polishing condition including a polishing condition determined in advance such that a second polishing profile having a distribution inverse to that of the first polishing profile is formed, and the second polishing step is performed after the first polishing step.

[0009] In one embodiment, the specific pressure chamber includes an edge pressure chamber that presses the outermost periphery of the substrate. In one embodiment, the second polishing conditions include polishing conditions that are determined by adjusting the pressure in a pressure chamber other than the specific pressure chamber. In one embodiment, the second polishing conditions include polishing conditions that are determined by adjusting a pressure in an adjacent pressure chamber that is adjacent to an edge pressure chamber that presses the outermost periphery of the substrate.

[0010] In one embodiment, the second polishing conditions include polishing conditions that are determined by adjusting a pressing force of a retainer ring disposed so as to surround an outermost periphery of the substrate against the polishing surface. In one embodiment, the first polishing conditions include polishing conditions for polishing the substrate while feedback-controlling the pressure of each of the plurality of pressure chambers based on a film thickness of the substrate corresponding to each of the plurality of pressure chambers measured using a film thickness sensor during polishing. In one embodiment, the substrate is polished under the first polishing condition, and after a predetermined switching condition is satisfied, the substrate is polished under the second polishing condition.

[0011] In one embodiment, the switching condition includes switching from the first polishing conditions to the second polishing conditions when a difference between a maximum value and a minimum value of the film thickness in the specific region exceeds a predetermined threshold value. In one embodiment, the switching condition is based on the time required to eliminate the difference between the maximum and minimum film thicknesses of the specific region by polishing under the second polishing conditions, and the remaining polishing time until the final target film thickness is reached. In one embodiment, the specific pressure chamber includes an edge pressure chamber that presses the outermost periphery of the substrate, and the pressure of the edge pressure chamber is controlled based on the second polishing condition, while the pressure of the other pressure chambers except for the edge pressure chamber is controlled based on the first polishing condition. Effect of the Invention

[0012] The polishing method includes a second polishing step of polishing the substrate under second polishing conditions. By polishing the substrate in the second polishing step, it is possible to improve the uniformity of the film thickness in a specific region of the wafer. [Brief description of the drawings]

[0013] [Figure 1] FIG. 1 is a schematic diagram illustrating an embodiment of a polishing apparatus. [Diagram 2] FIG. 2 is a cross-sectional view of a polishing head. [Diagram 3]FIG. 13 is a diagram illustrating an example of a spectrum generated by an operation control unit. [Figure 4] FIG. 1 shows an example of a process for obtaining multiple reference spectra. [Diagram 5] 13 is a diagram showing a plurality of pressing regions of a wafer divided according to a plurality of pressure chambers; FIG. [Figure 6] FIG. 4 is a diagram showing a polishing profile of a wafer when the wafer is polished under a first polishing condition. [Figure 7] FIG. 4 is a diagram showing second polishing conditions. [Figure 8] FIG. 4 is a graph showing the polishing rates of wafers polished under first and second polishing conditions. [Figure 9] 1A to 1C are diagrams illustrating an example of a process for polishing a wafer to be polished. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] Hereinafter, an embodiment of the present invention will be described in detail with reference to the drawings. Fig. 1 is a schematic diagram showing one embodiment of a polishing apparatus. As shown in Fig. 1, the polishing apparatus includes a polishing table 3 that supports a polishing pad 2, a polishing head 1 that presses a wafer W (such as a substrate) having a film against the polishing pad 2, a table motor 6 that rotates the polishing table 3, a polishing liquid supply nozzle 5 for supplying a polishing liquid such as a slurry onto the polishing pad 2, a film thickness sensor 40 (in this embodiment, an optical film thickness sensor 40) that measures the film thickness of the wafer W, and an operation control unit 9 for controlling the operation of the polishing apparatus. The upper surface of the polishing pad 2 constitutes a polishing surface 2a that polishes the wafer W.

[0015] The polishing head 1 is connected to a head shaft 10, and the head shaft 10 is connected to a polishing head motor (not shown) via a connecting means such as a belt. The polishing head motor rotates the polishing head 1 together with the head shaft 10 in the direction indicated by the arrow. The polishing table 3 is connected to a table motor 6, and the table motor 6 is configured to rotate the polishing table 3 and the polishing pad 2 in the direction indicated by the arrow.

[0016] The wafer W is polished as follows. While the polishing table 3 and polishing head 1 are rotated in the direction indicated by the arrow in Fig. 1, a polishing liquid is supplied from a polishing liquid supply nozzle 5 to the polishing surface 2a of the polishing pad 2 on the polishing table 3. While the wafer W is rotated around the head shaft 10 by the polishing head 1, the wafer W is pressed against the polishing surface 2a of the polishing pad 2 by the polishing head 1 with the polishing liquid present on the polishing pad 2. The polishing table 3 rotates around its center CP. The surface of the wafer W is polished by the chemical action of the polishing liquid and the mechanical action of the abrasive grains contained in the polishing liquid or the polishing pad 2.

[0017] The operation control unit 9 is composed of at least one computer. The operation control unit 9 includes a storage device 9a in which a program is stored, and a calculation device 9b that executes calculations according to instructions included in the program. The calculation device 9b includes a CPU (Central Processing Unit) or a GPU (Graphics Processing Unit) that executes calculations according to instructions included in the program stored in the storage device 9a. The storage device 9a includes a main storage device (e.g., random access memory) that can be accessed by the calculation device 9b, and an auxiliary storage device (e.g., a hard disk drive or a solid state drive) that stores data and programs.

[0018] The operation control unit 9 is electrically connected to the film thickness sensor 40. In this embodiment, the film thickness sensor 40 guides light to the surface of the wafer W, detects the light reflected from the wafer W, and outputs a signal corresponding to the film thickness of the wafer W to the operation control unit 9. The operation control unit 9 measures the film thickness of the wafer W based on the signal sent from the film thickness sensor 40 (more specifically, the intensity measurement data of the light reflected from the wafer W).

[0019] In this embodiment, the film thickness sensor 40 is an optical film thickness sensor, but may be another film thickness sensor as long as the film thickness of the wafer W can be measured by the operation control unit 9. In other words, the film thickness sensor 40 is a sensor that detects a physical quantity related to the film thickness of the wafer W. As an example, the film thickness sensor 40 may be an eddy current sensor. The eddy current sensor detects an eddy current corresponding to the film thickness of the wafer W by passing a magnetic flux through the conductive film of the wafer W with its sensor coil to generate an eddy current, and outputs an eddy current signal. The operation control unit 9 measures the film thickness of the wafer W based on this eddy current signal.

[0020] In this embodiment, the film thickness sensor 40 includes a light source 44 that emits light, a spectroscope 47, and an optical sensor head 7 connected to the light source 44 and the spectroscope 47. The optical sensor head 7, the light source 44, and the spectroscope 47 are attached to the polishing table 3 and rotate integrally with the polishing table 3 and the polishing pad 2. The optical sensor head 7 is positioned at a position where it crosses the surface of the wafer W on the polishing pad 2 every time the polishing table 3 and the polishing pad 2 rotate once.

[0021] The storage device 9a stores therein a program for generating a spectrum and detecting the film thickness of the wafer W, which will be described later. The light emitted from the light source 44 is transmitted to the optical sensor head 7 and guided from the optical sensor head 7 to the surface of the wafer W. The light is reflected by the surface of the wafer W, and the reflected light from the surface of the wafer W is received by the optical sensor head 7 and sent to the spectroscope 47. The spectroscope 47 separates the reflected light according to wavelength. In this way, the film thickness sensor 40 detects the intensity of the reflected light at each wavelength and sends the reflected light intensity measurement data to the operation control unit 9.

[0022] 2 is a cross-sectional view of the polishing head 1. As shown in FIG. 2, the polishing head 1 includes an elastic membrane 65 for pressing the wafer W against the polishing surface 2a of the polishing pad 2, a head body 21 for holding the elastic membrane 65, an annular drive ring 62 disposed below the head body 21, and an annular retainer ring 60 fixed to the lower surface of the drive ring 62.

[0023] The elastic membrane 65 is attached to the lower part of the head body 21. The head body 21 is fixed to the end of the head shaft 10, and the head body 21, elastic membrane 65, drive ring 62, and retainer ring 60 are configured to rotate together with the rotation of the head shaft 10. The retainer ring 60 and drive ring 62 are configured to be movable up and down relative to the head body 21. The head body 21 is formed of resin such as engineering plastic (e.g., PEEK).

[0024] The lower surface of the elastic membrane 65 constitutes a substrate pressing surface 65a that presses the wafer W against the polishing surface 2a of the polishing pad 2. The retainer ring 60 is disposed so as to surround the substrate pressing surface 65a, and the wafer W is surrounded by the retainer ring 60. Four pressure chambers 70, 71, 72, and 73 are provided between the elastic membrane 65 and the head body 21.

[0025] Pressure chamber 70 is a circular central pressure chamber located in the center, pressure chamber 73 is an annular edge pressure chamber located on the outermost periphery, and pressure chambers 71 and 72 are intermediate pressure chambers located between pressure chamber 70 and pressure chamber 73.

[0026] The pressure chambers 70, 71, 72, and 73 are formed by the elastic membrane 65 and the head body 21. The central pressure chamber 70 is circular, and the other pressure chambers 71, 72, and 73 are annular. These pressure chambers 70, 71, 72, and 73 are arranged (divided) concentrically. In this embodiment, the elastic membrane 65 forms four pressure chambers 70 to 73, but the number of pressure chambers described above is an example and may be changed as appropriate.

[0027] The pressure chambers 70, 71, 72, and 73 are connected to gas transfer lines F1, F2, F3, and F4, respectively. One end of the gas transfer lines F1, F2, F3, and F4 is connected to a compressed gas supply source (not shown) as a utility provided in a factory where the polishing apparatus is installed. Compressed gas such as compressed air is supplied to the pressure chambers 70, 71, 72, and 73 through the gas transfer lines F1, F2, F3, and F4. When the compressed gas is supplied to the pressure chambers 70 to 73, the elastic film 65 expands, and the compressed gas in the pressure chambers 70 to 73 presses the wafer W against the polishing surface 2a of the polishing pad 2 through the elastic film 65. The pressure chambers 70 to 73 function as actuators for pressing the wafer W against the polishing surface 2a of the polishing pad 2.

[0028] The retainer ring 60 is disposed around the elastic film 65 and is an annular member that comes into contact with the polishing surface 2a of the polishing pad 2. The retainer ring 60 is disposed so as to surround the outermost periphery of the wafer W, and prevents the wafer W from jumping out of the polishing head 1 during polishing of the wafer W, and can adjust the film thickness distribution on the outermost periphery of the wafer W by adjusting the elastic behavior (rebound) of the polishing pad 2.

[0029] An upper portion of the drive ring 62 is connected to an annular retainer ring pressing device 80. The retainer ring pressing device 80 applies a downward load to the entire upper surface 60b of the retainer ring 60 via the drive ring 62, thereby pressing the lower surface 60a of the retainer ring 60 against the polishing surface 2a of the polishing pad 2.

[0030] The retaining ring pressing device 80 includes an annular piston 81 fixed to the upper part of the drive ring 62, and an annular rolling diaphragm 82 connected to the upper surface of the piston 81. A retaining ring pressure chamber 83 is formed inside the rolling diaphragm 82. This retaining ring pressure chamber 83 is connected to the compressed gas supply source via a gas transfer line F5. The compressed gas is supplied into the retaining ring pressure chamber 83 through the gas transfer line F5.

[0031] When compressed gas is supplied from the compressed gas supply source to the retaining ring pressure chamber 83, the rolling diaphragm 82 presses the piston 81 downward, the piston 81 presses the drive ring 62 downward, and the drive ring 62 further presses the entire retaining ring 60 downward. In this manner, the retaining ring pressing device 80 presses the lower surface 60a of the retaining ring 60 against the polishing surface 2a of the polishing pad 2. The drive ring 62 is detachably connected to the retaining ring pressing device 80. In one embodiment, the retaining ring pressing device 80 may have a structure that presses the lower surface 60a of the retaining ring 60 against the polishing surface 2a of the polishing pad 2 by applying the downward force of the polishing head 1 to the retaining ring 60.

[0032] The gas transfer lines F1, F2, F3, F4, and F5 extend via a rotary joint 25 attached to the head shaft 10. The polishing apparatus further includes pressure regulators R1, R2, R3, R4, and R5, which are provided on the gas transfer lines F1, F2, F3, F4, and F5, respectively. Compressed gas from a compressed gas supply source is independently supplied to the pressure chambers 70 to 73 and the retaining ring pressure chamber 83 through the pressure regulators R1 to R5. The pressure regulators R1 to R5 are configured to adjust the pressure of the compressed gas in the pressure chambers 70 to 73 and the retaining ring pressure chamber 83. The pressure regulators R1 to R5 are connected to the operation control unit 9.

[0033] The pressure regulators R1 to R5 can change the internal pressures of the pressure chambers 70 to 73 and the retainer ring pressure chamber 83 independently of each other, and thus the pressing force of the wafer W against the polishing surface 2a in the four corresponding regions of the wafer W, i.e., the central portion, the inner middle portion, the outer middle portion, and the edge portion, and the pressing force of the retainer ring 60 against the polishing pad 2 can be adjusted independently. The gas transfer lines F1, F2, F3, F4, and F5 are also connected to air release valves (not shown), respectively, and the pressure chambers 70 to 73 and the retainer ring pressure chamber 83 can be opened to the atmosphere. In this embodiment, the elastic membrane 65 forms four pressure chambers 70 to 73, but in one embodiment, the elastic membrane 65 may form fewer or more than four pressure chambers.

[0034] Fig. 3 is a diagram showing an example of a spectrum generated by the operation control unit. In Fig. 3, the horizontal axis represents the wavelength of light reflected from the wafer, and the vertical axis represents the relative reflectance derived from the intensity of the reflected light. The relative reflectance is an index value indicating the intensity of reflected light, and is the ratio of the light intensity to a predetermined reference intensity. By dividing the light intensity (actual intensity) at each wavelength by the predetermined reference intensity, it is possible to remove unnecessary noise, such as variations in intensity inherent to the optical system of the device or the light source, from the actual intensity.

[0035] The reference intensity is the intensity of light measured in advance for each wavelength, and the relative reflectance is calculated for each wavelength. Specifically, the relative reflectance is calculated by dividing the light intensity (actual intensity) at each wavelength by the corresponding reference intensity.

[0036] The operation control unit 9 is configured to generate a spectrum of the reflected light from the reflected light intensity measurement data. The spectrum of the reflected light is expressed as a line graph (i.e., a spectral waveform) showing the relationship between the wavelength and intensity of the reflected light. The intensity of the reflected light can also be expressed as a relative value such as reflectance or relative reflectance.

[0037] In actual polishing, the corrected actual intensity is obtained by subtracting the dark level (background intensity obtained under conditions where light is blocked) from the actual intensity, and the corrected standard intensity is obtained by subtracting the dark level from the standard intensity, and the relative reflectance is obtained by dividing the corrected actual intensity by the corrected standard intensity. Specifically, the relative reflectance R(λ) can be obtained using the following formula (1).

number

[0038] The operation control unit 9 generates a spectrum as shown in FIG. 3 from the intensity measurement data of the reflected light. Furthermore, the operation control unit 9 determines the film thickness of the wafer W from the spectrum of the reflected light. The spectrum of the reflected light changes according to the film thickness of the wafer W. Therefore, the operation control unit 9 can determine the film thickness of the wafer W from the spectrum of the reflected light. Hereinafter, in this specification, the spectrum generated from the reflected light from the wafer W being polished is referred to as a measured spectrum.

[0039] The operation control unit 9 is configured to determine the film thickness from a comparison between the measured spectrum (i.e., the measured data) and a plurality of reference spectra (i.e., the reference data). The operation control unit 9 compares the measured spectrum generated during polishing with a plurality of reference spectra to determine the reference spectrum having the closest shape to the measured spectrum, and obtains the film thickness associated with the determined reference spectrum. The reference spectrum having the closest shape to the measured spectrum is the spectrum having the smallest difference in relative reflectance between the reference spectrum and the measured spectrum.

[0040] The multiple reference spectra are obtained in advance by polishing a reference wafer having the same or similar initial film thickness as the wafer to be polished (hereinafter, in this specification, wafer W corresponds to the wafer to be polished), and each reference spectrum can be associated with the film thickness at the time the reference spectrum was obtained. That is, each reference spectrum was obtained at a different film thickness, and the multiple reference spectra correspond to multiple different film thicknesses. Therefore, the current film thickness can be estimated by determining the reference spectrum whose shape is closest to the measured spectrum.

[0041] 4 is a diagram showing an example of a process for acquiring a plurality of reference spectra. First, a reference wafer having the same or equivalent film thickness as the wafer W is prepared. The reference wafer is transferred to film thickness measuring instrument 170 (see FIG. 1), and the initial film thickness of the reference wafer is measured by film thickness measuring instrument 170 (see step S101). Film thickness measuring instrument 170 is electrically connected to operation controller 9.

[0042] Next, the reference wafer is polished while a slurry as a polishing liquid is supplied to the polishing pad 1 (see step S102). During the polishing of the reference wafer, light is irradiated onto the surface of the reference wafer, and the spectrum of the reflected light from the reference wafer (i.e., the reference spectrum) is obtained (see step S103).

[0043] The reference spectrum is acquired every time the polishing table 3 rotates once. Thus, a plurality of reference spectra are acquired during polishing of the reference wafer. After polishing of the reference wafer is completed, the reference wafer is transferred again to the film thickness measuring instrument 170, and the film thickness (i.e., the final film thickness) of the polished reference wafer is measured (see step S104).

[0044] When the polishing rate of the reference wafer is constant, the film thickness decreases linearly with polishing time. The polishing rate can be calculated by dividing the difference between the initial film thickness and the final film thickness by the polishing time at which the final film thickness is reached. As described above, the reference spectrum is periodically acquired every time the polishing table 3 rotates, so that the polishing time at which each reference spectrum is acquired can be calculated from the rotation speed of the polishing table 3. In this way, the operation control unit 9 determines the film thickness corresponding to each reference spectrum (see step S105).

[0045] Each reference spectrum can be associated (linked) to a corresponding film thickness. Therefore, the operation control unit 9 can determine the reference spectrum having the closest shape to the measured spectrum during polishing of the wafer W, and thereby determine the current film thickness of the wafer W from the film thickness associated with the reference spectrum.

[0046] Hereinafter, a process of polishing the wafer W to be polished will be described. First, it is necessary to determine a first polishing condition (in other words, a final target film thickness flat condition) under which the film thickness uniformity of the wafer W to be polished falls within a predetermined allowable range.

[0047] The first polishing condition may be a polishing condition (control of the pressure in each of the pressure chambers 70, 71, 72, 73, and 83) that is determined in advance so as to make the final target film thickness flat. The operation control unit 9 is configured to polish the wafer W while controlling the pressure in each of the pressure chambers 70, 71, 72, 73, and 83 based on the first polishing condition.

[0048] Fig. 5 is a diagram showing a plurality of pressing regions of the wafer divided according to a plurality of pressure chambers. As shown in Fig. 5, the operation control unit 9 divides the wafer W into a plurality of pressing regions A1 to A4 according to a plurality of pressure chambers 70, 71, 72, and 73. These pressing regions A1 to A4 are arranged concentrically with the center CPW of the wafer W. A notch Nt is formed on the outer edge of the wafer W.

[0049] In one embodiment, the first polishing condition may be a polishing condition (CLC: closed loop control) in which the pressure of each of the pressure chambers 70-73 is feedback-controlled in real time based on the film thickness measured by the film thickness sensor 40 during polishing of the wafer W so that the film thickness (average film thickness) of each of the regions A1-A4 of the wafer W becomes the average film thickness of the entire wafer W. More specifically, the operation control unit 9 calculates the average film thickness value in each of the pressing regions A1-A4 based on the film thickness of the wafer W measured based on the signal output from the film thickness sensor 40. Thereafter, the operation control unit 9 controls the pressure in the pressure chambers 70-73 corresponding to the pressing regions A1-A4 by controlling each of the pressure regulators R1-R4 so that the difference between the average film thickness value of each of the pressing regions A1-A4 and the average film thickness value of the entire wafer W is reduced.

[0050] The operation control unit 9 may control the pressure within the retaining ring pressure chamber 83 by controlling the pressure regulator R5 based on a method similar to that described above.

[0051] Fig. 6 is a diagram showing a polishing profile of a wafer when the wafer is polished under the first polishing condition. In Fig. 6, the horizontal axis represents the radial distance of the wafer W, and the vertical axis represents the film thickness distribution of the wafer W. The thick line in Fig. 6 indicates the boundary between the pressing area A4 located on the outermost periphery of the wafer W and corresponding to the pressure chamber 73, and the pressing area inside the pressing area A4. In the embodiment shown in Fig. 6, the polishing profile of the wafer W will be described as the film thickness distribution in the radial direction of the wafer W after polishing the wafer W when the wafer W is polished for a predetermined time, but the polishing profile of the wafer W may include a polishing rate distribution in the radial direction of the wafer W.

[0052] When the wafer W is polished under the first polishing condition, the uniformity of the film thickness of the wafer W falls within a predetermined tolerance in other regions including the center of the wafer W (i.e., regions excluding the outermost periphery), while the radial variation of the remaining film (film thickness after polishing) of the wafer W may be large in a specific region including the outermost periphery of the wafer W. That is, the difference in film thickness between a portion with a large film thickness and a portion with a small film thickness is large in the specific region including the outermost periphery of the wafer W. The polishing profile of the outermost periphery of the wafer W is likely to be steep and asymmetric due to the influence of the rebound of the polishing pad 2, etc., and it is difficult to obtain a flat film thickness distribution by simply adjusting the pressure of the pressure chamber in the specific region including the outermost periphery of the wafer W. The variation in film thickness after polishing (so-called remaining film range) in the specific region including the outermost periphery of the wafer W tends to increase as the polishing time under the first polishing condition increases.

[0053] Therefore, in this embodiment, the operation control unit 9 is configured to polish the wafer W based on a second polishing condition that reduces the variation in the film thickness in the radial direction of the wafer W at the outermost periphery of the wafer W. In the embodiment shown below, an embodiment in which the variation in the film thickness of the wafer W at the outermost periphery of the wafer W is reduced will be described as an example of the specific region of the wafer W, but the specific region of the wafer W is not limited to the outermost periphery of the wafer W. The film thickness variation of the wafer W may also occur in other regions of the wafer W except for the outermost periphery.

[0054] Fig. 7 is a diagram showing the second polishing conditions. In Fig. 7, the horizontal axis represents the radial distance of the wafer W, and the vertical axis represents the film thickness distribution of the wafer W. In the embodiment shown in Fig. 7, the polishing profile of the wafer W will be described as the film thickness distribution in the radial direction of the wafer W after polishing the wafer W for a predetermined time, but the polishing profile of the wafer W may also include a polishing rate distribution in the radial direction of the wafer W.

[0055] The operation control unit 9 polishes a wafer having the same or equivalent initial film thickness as the wafer W to be polished, based on the first polishing conditions. Thereafter, the operation control unit 9 determines second polishing conditions based on a first polishing profile (film thickness distribution or polishing rate distribution of the wafer W after polishing) obtained by polishing under the first polishing conditions. The second polishing conditions are polishing conditions that are determined (adjusted) in advance so as to form a second polishing profile having a distribution that is inverse to the distribution of the first polishing profile (more specifically, the distribution of the pressing area on the wafer W corresponding to a specific pressure chamber).

[0056] In other words, the second polishing conditions are polishing conditions under which the thicker film thickness portion at the outermost periphery of the polished wafer W polished under the first polishing conditions is polished more actively, and polishing of the thinner film thickness portion at the outermost periphery of the polished wafer W is suppressed. The second polishing profile has a distribution in which the positive and negative signs of the numerical values ​​indicating the film thickness or polishing rate of the wafer W are inverted compared to the distribution of the first polishing profile. The curve indicating the distribution of the second polishing profile and the curve indicating the distribution of the first polishing profile are ideally line-symmetrical to each other.

[0057] 7, in the film thickness distribution on the coordinate system specified by the radial distance of the wafer W and the film thickness of the wafer W corresponding to the distance, the curve showing the film thickness distribution on the outermost periphery of the wafer W (the curve showing the distribution of the second polishing profile) is line-symmetrical with respect to the reference line with respect to the curve showing the film thickness distribution on the outermost periphery of the wafer W polished under the first polishing conditions (see the dashed line in FIG. 7). Note that in the embodiment shown in FIG. 7, the curve showing the distribution of the second polishing profile is drawn as an ideal curve.

[0058] The second polishing conditions are determined by polishing a wafer having the same or equivalent initial film thickness as the wafer W to be polished. First, the wafer W is polished under the first polishing conditions in advance to confirm the first polishing profile. Then, another wafer is polished, and the second polishing conditions are experimentally determined so that the polishing profile after the polishing has a distribution opposite to that of the first polishing profile. Alternatively, in one embodiment, the wafer W is first polished under the first polishing conditions, and then the polishing conditions are switched from the first polishing conditions to polish the wafer W. The second polishing conditions, which are the switching conditions from the first polishing conditions, are experimentally determined so that the polishing profile after the polishing has a flat distribution. In one embodiment, the second polishing conditions may be selected from a database of polishing conditions and polishing profiles stored in the storage device 9a in advance, and / or may be determined by polishing simulation.

[0059] The operation control unit 9 stores second polishing conditions in its storage device 9a, and is configured to polish the wafer W based on the second polishing conditions. More specifically, the operation control unit 9 polishes the wafer W based on the second polishing conditions while controlling the pressure of a specific pressure chamber among the multiple pressure chambers 70, 71, 72, 73, and 83 at a predetermined fixed value. The second polishing conditions include polishing conditions for polishing the wafer W based on the second polishing profile while controlling the pressure of a specific pressure chamber at a predetermined fixed value.

[0060] In this embodiment, the specific pressure chamber includes the edge pressure chamber 73 that presses the outermost periphery of the wafer W, and an adjacent pressure chamber adjacent to the edge pressure chamber 73. The adjacent pressure chamber includes at least one of the intermediate pressure chamber 72 and the retainer ring pressure chamber 83. In this embodiment, the adjacent pressure chamber is both the intermediate pressure chamber 72 and the retainer ring pressure chamber 83. In one embodiment, the specific pressure chamber may be only the edge pressure chamber 73.

[0061] The second polishing conditions include polishing conditions determined by adjusting the pressure of a specific pressure chamber. In one embodiment, the second polishing conditions may include polishing conditions determined by adjusting the pressure of a pressure chamber other than the specific pressure chamber. For example, when the specific pressure chamber is the edge pressure chamber 73, the second polishing conditions include polishing conditions determined by adjusting the pressure of an adjacent pressure chamber adjacent to the edge pressure chamber 73.

[0062] In one embodiment, the second polishing conditions may include polishing conditions determined by adjusting the pressing force of the retainer ring 60 disposed to surround the outermost periphery of the wafer W against the polishing surface 2a. In this case, the operation control unit 9 controls the retainer ring pressing device 80 that applies the downward force of the polishing head 1 to the retainer ring 60, based on the second polishing conditions.

[0063] In this embodiment, the operation control unit 9 controls the pressure of each of the edge pressure chambers 73 and the adjacent pressure chambers 72, 83 based on the second polishing conditions, while feedback-controlling the pressure of each of the other pressure chambers 70, 71 other than the edge pressure chamber 73 and the adjacent pressure chambers 72, 83 based on the first polishing conditions.

[0064] The first polishing condition is a polishing condition in which the pressure of each of the pressure chambers 70, 71 is feedback-controlled during polishing so that the difference between the average film thickness value of the areas corresponding to each of the other pressure chambers 70, 71 and the overall average film thickness value of the wafer W is reduced based on the signal output from the film thickness sensor 40.

[0065] FIG. 8 is a diagram showing the polishing rate of a wafer polished under the first polishing condition and the second polishing condition. In FIG. 8, the horizontal axis represents the radial distance of the wafer W, and the vertical axis represents the polishing rate of the wafer W. FIG. 8 shows an enlarged view of the polishing rate of the outer portion of the wafer W. As shown in FIG. 8, the polishing rate in the pressing area A4 on the wafer W under the first polishing condition and the polishing rate in the pressing area A4 on the wafer W under the second polishing condition are inverted to each other. Therefore, the operation control unit 9 can improve the uniformity of the film thickness on the outermost periphery of the wafer W by polishing the wafer W under a combination of the first polishing condition and the second polishing condition.

[0066] 9 is a diagram showing an example of a process for polishing a wafer to be polished. As shown in step S201 of FIG. 9, the operation control unit 9 polishes the wafer W under the first polishing condition (first polishing process). Thereafter, the operation control unit 9 judges whether a predetermined switching condition is satisfied (see step S202), and if the switching condition is not satisfied (see "No" in step S202), the operation control unit 9 continues step S201. If the switching condition is satisfied (see "Yes" in step S202), the operation control unit 9 switches the polishing condition from the first polishing condition to the second polishing condition (see step S203), and polishes the wafer W under the second polishing condition (second polishing process).

[0067] When the variation in the remaining film thickness (more specifically, the difference between the maximum and minimum film thickness) on the outermost periphery (i.e., specific region) of the wafer W is too large, even if the polishing conditions are switched from the first polishing conditions to the second polishing conditions, the variation in the film thickness on the outermost periphery of the wafer W may not be eliminated. Therefore, the operation control unit 9 may switch the polishing conditions from the first polishing conditions to the second polishing conditions (first switching conditions) when the difference between the maximum and minimum film thicknesses on the outermost periphery of the wafer W during polishing of the wafer W under the first polishing conditions (so-called remaining film range) exceeds a predetermined threshold value.

[0068] When the film thickness varies greatly in a specific region of the wafer W corresponding to a specific pressure chamber, the film thickness variation may not be eliminated even if the pressure of the specific pressure chamber is adjusted. Therefore, in the above-described embodiment, the operation control unit 9 switches the polishing conditions from the first polishing conditions to the second polishing conditions when the range of the remaining film on the wafer W under the first polishing conditions exceeds a predetermined threshold value.

[0069] Even if the polishing conditions are switched from the first polishing conditions to the second polishing conditions when the remaining polishing time is too short, there is a risk that the variation in film thickness in a specific region of the wafer W will not be eliminated. Therefore, the operation control unit 9 may switch the polishing conditions from the first polishing conditions to the second polishing conditions (second switching conditions) based on the time required to eliminate the difference between the maximum and minimum film thicknesses of the outermost periphery of the wafer W by polishing under the second polishing conditions and the remaining polishing time until the final target film thickness is reached, as the switching condition.

[0070] The polishing rate when the wafer W is polished under the second polishing conditions is known in advance through the process of determining the second polishing conditions. Therefore, when the wafer W is polished under the second polishing conditions, the operation control unit 9 can calculate the time required to reduce (eliminate) the remaining film range of the wafer W during polishing of the wafer W under the first polishing conditions. Therefore, in one embodiment, the operation control unit 9 may switch the polishing conditions from the first polishing conditions to the second polishing conditions when the required polishing time under the second polishing conditions reaches or approaches a predetermined remaining time. The predetermined remaining time is, for example, the same as the time required for the film thickness of the wafer W to reach the final target film thickness when the wafer W is polished under the second polishing conditions after the switching timing.

[0071] More specifically, while the wafer W is being polished under the first polishing conditions, the operation control unit 9 calculates the time required to reduce the remaining film thickness range of the wafer W under the second polishing conditions (i.e., the required polishing time) and the remaining polishing time (i.e., the remaining time). The remaining polishing time is calculated based on the following formula: remaining polishing time=(current film thickness of the wafer W-target film thickness of the wafer W) / estimated polishing rate under the second polishing conditions

[0072] If the required polishing time is smaller than the remaining time (required polishing time << remaining time), the polishing time under the second polishing conditions will be longer, and the remaining film profile of the wafer W will deteriorate. If the required polishing time is the same as the remaining time (required polishing time = remaining time), the remaining film range of the wafer W will be resolved, and the film thickness of the wafer W will reach the target film thickness (ideal state). If the required polishing time is greater than the remaining time (required polishing time > remaining time), the film thickness of the wafer W will reach the target film thickness before the remaining film range is resolved, and the remaining film range will not be resolved completely. Continuing polishing in this state will result in over-polishing. Therefore, it is desirable for the operation control unit 9 to switch the polishing conditions from the first polishing conditions to the second polishing conditions when the required polishing time and the remaining time are the same.

[0073] According to the second switching condition, when there is a difference in the total polishing amount, it is possible to change the allowable remaining film range in polishing under the first polishing condition, and therefore it is possible to perform optimization according to a difference in the initial film thickness of the wafer W. Note that, in the case of polishing to remove a film on the wafer W, the "time required to reach the final target film thickness" means the time required for the final target film thickness to be zero, that is, the time required to clear the excess film.

[0074] In one embodiment, the operation control unit 9 may switch the polishing condition from the first polishing condition to the second polishing condition based on the first switching condition and the second switching condition. In one embodiment, the operation control unit 9 may switch the polishing condition from the first polishing condition to the second polishing condition when the overall average film thickness of the wafer W reaches a predetermined film thickness. In one embodiment, the operation control unit 9 may switch the polishing condition from the first polishing condition to the second polishing condition when the polishing time of the wafer W reaches a predetermined polishing time.

[0075] After executing step S203 in FIG. 9, the operation control unit 9 ends polishing of the wafer W (see step S205) by receiving an end point detection signal from the film thickness sensor 40 indicating that the overall average film thickness of the wafer W has reached the target film thickness or that the material formed on the wafer W has reached the interface with a different material (see "Yes" in step S204). If the end point detection signal has not been received (see "No" in step S204), the operation control unit 9 continues polishing of the wafer W under the second polishing condition. If the remaining film range in the specific region is not equal to or less than a predetermined value when the end point detection signal is received, the operation control unit 9 may continue polishing of the wafer W under the second polishing condition. In addition, the operation control unit 9 may issue an alarm if the remaining film range in the specific region is not equal to or less than a predetermined value when the end point detection signal is received.

[0076] In the above-described embodiment, the polishing head 1 has a plurality of pressure chambers (air bags), but the pressing elements for pressing the wafer W are not limited to this. The technical idea of ​​the present invention is applicable when a plurality of pressing elements that apply the same pressure to the wafer W are arranged in the radial direction of the wafer W. An example of the pressing element is a piezoelectric element.

[0077] The above-described embodiments have been described for the purpose of enabling a person having ordinary skill in the art to practice the present invention. Various modifications of the above-described embodiments are naturally possible for a person skilled in the art, and the technical idea of ​​the present invention can be applied to other embodiments. Therefore, the present invention is not limited to the described embodiments, but is to be interpreted in the broadest scope according to the technical idea defined by the claims. [Explanation of symbols]

[0078] 1 Polishing head 2 Polishing Pads 2a Polished surface 3 Polishing table 5 Polishing fluid supply nozzle 6 Table Motor 7 Optical Sensor Head 9. Operation control section 9a Storage device 9b Arithmetic unit 10 Head shaft 21 Head body 25 Rotary joint 40 Film Thickness Sensor 44 Light source 47 Spectrometer 60 Retainer ring 60a Bottom 60b top surface 62 Drive Ring 65 Elastic Membrane 65a Board pressing surface 70 Central Pressure Chamber 71 Intermediate Pressure Chamber 72 Intermediate Pressure Chamber 73 Edge Pressure Chamber 80 Retainer ring pressing device 81 Piston 82 Rolling Diaphragm 83 Retainer ring pressure chamber 170 Film Thickness Measuring Instrument

Claims

1. A polishing method in which a substrate is pressed against a polishing surface of a polishing pad by a polishing head having a plurality of pressure chambers including a specific pressure chamber, comprising: The polishing method includes: a first polishing step of polishing the substrate under first polishing conditions; a second polishing step of polishing the substrate under second polishing conditions determined based on a first polishing profile along a radial direction of a specific region of the substrate corresponding to the specific pressure chamber, the first polishing profile being obtained by polishing a substrate different from the substrate under the first polishing conditions in advance; the second polishing conditions include polishing conditions that are predetermined to form a second polishing profile having a distribution that is inverse to a distribution of the first polishing profile; The second polishing step is carried out after the first polishing step; The substrate different from the substrate is a substrate having an initial thickness that is the same as or similar to the substrate to be polished; A polishing method, wherein the first polishing profile and the second polishing profile include a film thickness distribution or a polishing rate distribution of the substrate.

2. The polishing method according to claim 1 , wherein the specific pressure chamber includes an edge pressure chamber that presses an outermost periphery of the substrate.

3. 3. The polishing method according to claim 1, wherein the second polishing conditions include polishing conditions that are determined by adjusting a pressure in a pressure chamber other than the specific pressure chamber.

4. 4. The polishing method according to claim 1, wherein the second polishing conditions include polishing conditions determined by adjusting a pressure in an adjacent pressure chamber adjacent to an edge pressure chamber that presses the outermost periphery of the substrate.

5. The polishing method according to any one of claims 1 to 4, wherein the second polishing conditions include polishing conditions determined by adjusting a pressing force of a retainer ring arranged to surround the outermost periphery of the substrate against the polishing surface.

6. The polishing method according to any one of claims 1 to 5, wherein the first polishing conditions include polishing conditions for polishing the substrate while feedback-controlling the pressure of each of the plurality of pressure chambers based on film thicknesses of the substrate corresponding to each of the plurality of pressure chambers measured using a film thickness sensor during polishing.

7. 7. The polishing method according to claim 1, further comprising the steps of: polishing the substrate under the first polishing condition; and, after a predetermined switching condition is satisfied, polishing the substrate under the second polishing condition.

8. 8. The polishing method according to claim 7, wherein the switching condition is to switch from the first polishing condition to the second polishing condition when a difference between a maximum value and a minimum value of the film thickness in the specific region becomes larger than a predetermined threshold value.

9. 8. The polishing method according to claim 7, wherein the switching condition is based on a time required to eliminate a difference between a maximum value and a minimum value of a film thickness in the specific region by polishing under the second polishing condition, and a remaining polishing time until a final target film thickness is reached.

10. the specific pressure chamber includes an edge pressure chamber that presses the outermost periphery of the substrate, 10. The polishing method according to claim 1, further comprising controlling a pressure in the edge pressure chamber based on the second polishing condition, while controlling a pressure in the other pressure chambers except the edge pressure chamber based on the first polishing condition.

Citation Information

Patent Citations

  • Device and method for substrate polishing

    JP2005011977A

  • Polishing device, polishing method and polishing control program

    JP2019217595A

  • Substrate treatment apparatus and method for specifying region to be partially polished in substrate treatment apparatus

    JP2020110871A

  • Polishing method and polishing apparatus

    WO2015163164A1