Coating material and coating film forming method

A coating material with specific resin, scaly particles, and viscosity modifier addresses roughness and unevenness issues, achieving a smooth and aesthetically pleasing film.

JP7590921B2Active Publication Date: 2024-11-27BEKKU KK
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021086840
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-05-25
Filing Date
2021-05-24
Publication Date
2024-11-27
Estimated Expiration
2041-05-24

AI Technical Summary

Technical Problem

Existing coating materials containing colored mica result in films with rough edges, uneven patterns, and insufficient concealment due to scaly particles overlapping, leading to an unsatisfactory aesthetic appearance.

Method used

A coating material comprising an aqueous resin, scaly particles, and an associative viscosity modifier, with specific particle size distributions and viscosity characteristics, is used to form a film with reduced roughness and enhanced aesthetics.

Benefits of technology

The solution results in a smooth, flat film with excellent aesthetic appearance and balanced patterns, minimizing particle bounce and roughness during application.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007590921000001
    Figure 0007590921000001
  • Figure 0007590921000002
    Figure 0007590921000002
Patent Text Reader

Abstract

To form a coat having reduced roughness and a flat, beautiful appearance.SOLUTION: A coating material contains an aqueous resin (A) and scaly particles (B). Relative to 100 pts.wt. of the solid content of the aqueous resin (A), the scaly particles (B) are 5-200 pts.wt. The coating material contains an associative viscosity modifier (C) as a viscosity modifier and has a viscosity of 1-50 Pa s and a thixotropy-index (TI value) of 4 or more.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a novel coating material. [Background technology]

[0002] Conventionally, decorative finishing materials that impart the aesthetic appearance of natural stone to buildings and civil engineering structures have been known. In recent years, there have been an increasing number of cases where decorative finishing with design features such as the diverse colors peculiar to natural stone is desired. For example, Patent Document 1 describes a coating material containing colored mica and a binder resin as such a material. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2013-224363 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, when a coating material containing colored mica is applied as in Patent Document 1, the ends of the scaly particles may rise up, resulting in a rough coating. In addition, the scaly particles tend to overlap (crowd together) in parts, which may cause the pattern to become uneven, or may result in insufficient hiding of some areas, resulting in the formation of an uneven pattern.

[0005] The present invention has been made in consideration of the above points, and an object of the present invention is to provide a coating material and a coating formation method that are capable of forming a coating that has little roughness and is flat and has excellent aesthetic appearance by a simple method. [Means for solving the problem]

[0006] As a result of intensive research to solve the above problems, the present inventors came up with the idea that a coating material containing an aqueous resin, scaly particles, and a specific viscosity adjuster can be given a specific viscosity, thereby obtaining a coating film that is flat and has excellent aesthetic appearance with less roughness, and thus completed the present invention. That is, the present invention has the following characteristics.

[0007] That is, the present invention has the following features. 1. A coating material comprising an aqueous resin (A) and scaly particles (B), wherein the scaly particles (B) are 100 parts by weight of the aqueous resin (A) based on the solid content. 10 Contains up to 200 parts by weight The scale-like particles (B) include large particles (b1) having a short diameter of more than 2 mm, medium particles (b2) having a short diameter of more than 0.7 mm and not more than 2 mm, and small particles (b3) having a short diameter of 0.7 mm or less, The coating material contains an associative viscosity modifier (C) as a viscosity modifier, has a viscosity of 1 to 50 Pa·s, and a thixotropy index (TI value) of 4 or more. the law of nature, In the coating material, the mixing ratio of the powder particles (E) excluding the scale-like particles (B) is 5 parts by weight or less per 100 parts by weight of the solid content of the aqueous resin (A). A coating material characterized by: 2. The weight ratio of the medium particles (b2) and the small particles (b3) to the large particles (b1), [(b2)+(b3)] / (b1), is 1 or more and 50 or less. 3. A coating method for forming a coating film by applying a coating material to a wall surface, the coating material comprising an aqueous resin (A) and scaly particles (B), the scaly particles (B) being mixed in an amount of 100 parts by weight of the aqueous resin (A) based on a solid content of the aqueous resin (A). 10 Contains up to 200 parts by weight The scale-like particles (B) include large particles (b1) having a short diameter of more than 2 mm, medium particles (b2) having a short diameter of more than 0.7 mm and not more than 2 mm, and small particles (b3) having a short diameter of 0.7 mm or less, The coating material contains an associative viscosity modifier (C) as a viscosity modifier, has a viscosity of 1 to 50 Pa·s, and a thixotropy index (TI value) of 4 or more. the law of nature, In the coating material, the mixing ratio of the powder particles (E) excluding the scale-like particles (B) is 5 parts by weight or less per 100 parts by weight of the solid content of the aqueous resin (A). A method for forming a coating comprising the steps of: 4. The method for forming a coating film according to 3., wherein a weight ratio of the medium particles (b2) and small particles (b3) to the large particles (b1), [(b2)+(b3)] / (b1), is 1 or more and 50 or less. Effect of the Invention

[0008] According to the present invention, it is possible to obtain a coating film that is smooth and has excellent appearance with little roughness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] Hereinafter, an embodiment of the present invention will be described.

[0010] <Coating material> The coating material of the present invention is characterized by comprising an aqueous resin (A) and scaly particles (B), and further comprising an associative viscosity modifier (C) as a viscosity modifier.

[0011] The aqueous resin (A) (hereinafter referred to as "component (A)") is not particularly limited, but is preferably one or more selected from water-soluble resins and water-dispersible resins (resin emulsions). Examples of the resin include vinyl acetate resins, polyester resins, alkyd resins, vinyl chloride resins, epoxy resins, acrylic resins, urethane resins, acrylic silicone resins, fluororesins, and the like, or composites thereof. These resins can be used alone or in combination of two or more. In the present invention, acrylic resins and acrylic silicone resins are preferred. These components (A) may also have crosslinking reactivity. When a component (A) having crosslinking reactivity is used, the water resistance, weather resistance, chemical resistance, and the like of the coating can be improved.

[0012] In the present invention, acrylic resin is particularly suitable as component (A). Acrylic resin is a resin in which (meth)acrylic acid alkyl ester is the main component of the resin skeleton, and other monomers are copolymerized as necessary. In the present invention, acrylic acid alkyl ester and methacrylic acid alkyl ester are collectively referred to as (meth)acrylic acid alkyl ester. Moreover, a monomer is a general term for a compound having a polymerizable unsaturated double bond.

[0013] Examples of (meth)acrylic acid alkyl esters include methyl (meth)acrylate, ethyl (meth)acrylate, isopropyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, octyl (meth)acrylate, cyclohexyl (meth)acrylate, and the like. One or more of these can be used.

[0014] Specific examples of other monomers include, for example, Aromatic monomers such as styrene, 2-methylstyrene, vinyltoluene, t-butylstyrene, chlorostyrene, vinylanisole, vinylnaphthalene, divinylbenzene, phenyl (meth)acrylate, and benzyl (meth)acrylate; Nitrile group-containing monomers such as (meth)acrylonitrile, vinylidene cyanide, and α-cyanoethyl (meth)acrylate; Amide group-containing monomers such as maleic acid amide, (meth)acrylamide, N-monoalkyl (meth)acrylamide, N,N-dialkyl (meth)acrylamide, 2-(dimethylamino)ethyl (methacrylate), N-[3-(dimethylamino)propyl] (meth)acrylamide, and vinylamide; Carbonyl group-containing monomers such as acrolein, diacetone (meth)acrylamide, vinyl methyl ketone, vinyl ethyl ketone, and vinyl butyl ketone;

[0015] Carboxyl group-containing monomers such as (meth)acrylic acid, crotonic acid, maleic acid, itaconic acid, fumaric acid, isocrotonic acid, and salicylic acid; Amino group-containing monomers such as aminomethyl acrylate, aminoethyl acrylate, aminopropyl (meth)acrylate, amino-n-butyl (meth)acrylate, butylvinylbenzylamine, vinylphenylamine, p-aminostyrene, N-methylaminoethyl (meth)acrylate, and Nt-butylaminoethyl (meth)acrylate; Epoxy group-containing monomers such as glycidyl (meth)acrylate, diglycidyl fumarate, 3,4-epoxycyclohexyl (meth)acrylate, 3,4-epoxyvinylcyclohexane, allyl glycidyl ether, ε-caprolactone-modified glycidyl (meth)acrylate, and β-methylglycidyl (meth)acrylate; Hydroxyl group-containing monomers such as hydroxypropyl (meth)acrylate, ethylene glycol mono(meth)acrylate, and glycerol mono(meth)acrylate; vinylidene halide monomers such as vinylidene fluoride; Alkoxysilyl group-containing monomers, such as vinyltrimethoxysilane, vinyltriethoxysilane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, and γ-(meth)acryloyloxypropylmethyldimethoxysilane; Examples of the vinyl ether include ethylene, propylene, isoprene, butadiene, vinyl ether, vinyl ketone, etc. These may be used alone or in combination of two or more.

[0016] When the above-mentioned alkoxysilyl group-containing monomer is used as the other monomer, an acrylic silicone resin can be obtained.

[0017] The component (A) can be produced by emulsion polymerization of a monomer group obtained by appropriately mixing the above-mentioned monomers. Any known method can be used as the polymerization method, and in addition to normal emulsion polymerization, soap-free emulsion polymerization, feed emulsion polymerization, seed emulsion polymerization, etc. can also be used. During polymerization, an emulsifier, initiator, dispersant, polymerization inhibitor, polymerization retarder, buffer, chain transfer agent, etc. can be used.

[0018] As the emulsifier, various surfactants that can be used in emulsion polymerization can be used, and these may be reactive types (reactive surfactants) having polymerizable unsaturated double bonds. As the emulsifier, anionic surfactants and nonionic surfactants may be used alone or in combination.

[0019] The glass transition temperature (hereinafter simply referred to as "Tg") of the component (A) is preferably set to -50°C to 50°C. If Tg is within this range, the effects of the present invention can be stably obtained. In the present invention, Tg is a value calculated by Fox's formula. In addition, the average particle size of the component (A) is preferably 300 nm or less (more preferably 20 to 200 nm). If the average particle size is within this range, the water resistance, weather resistance, chemical resistance, etc. of the coating can be improved. In addition, the average particle size referred to here is a value measured by dynamic light scattering.

[0020] The scaly particles (B) (hereinafter referred to as "component (B)") impart an excellent design to the formed coating. In addition, component (B) is also advantageous in terms of thinning and weight reduction of the formed coating. The present invention is characterized in that the scaly particles (B) are contained in an amount of 5 to 200 parts by weight (preferably 10 to 100 parts by weight, more preferably 15 to 80 parts by weight) per 100 parts by weight of the solid content of the aqueous resin (A). When the above range is satisfied, a coating having a design such as a natural stone look can be obtained. In the present invention, "α to β" is synonymous with "α or more and β or less".

[0021] Examples of such (B) components include inorganic pieces such as mica, sericite, clay, talc, plate-like kaolin, barium sulfate flakes, glass flakes, alumina flakes, shell pieces, and metal pieces, as well as rubber pieces, plastic pieces, and wood pieces. Also included are those that are used as base particles and colored. The coloring treatment is not particularly limited, but examples include a method in which a colorant containing a pigment or dye is coated (or adsorbed) on the base particles, and a method in which the base particles are subjected to a baking treatment or the like. In the present invention, it is preferable to use mica that has been coated with a colorant (colored mica). One or more types of (B) components (one color or two or more colors) can be used in combination to express various colors. In the present invention, it is preferable to use colored scaly particles (scaly colored particles), particularly colored mica (colored mica).

[0022] The "scaly particles" in the present invention are not particularly limited as long as they are scaly (thin), but are preferably particles with an aspect ratio (ratio of "minor diameter / thickness") of 1.5 to 2000 (more preferably 2 to 500, and even more preferably 3 to 100). In addition, it is preferable that the ratio of the minor diameter to the major diameter (minor diameter / major diameter) is 0.3 to 1 (more preferably 0.4 to 1, and even more preferably 0.5 to 1). When the size of the scaly particles satisfies the above range, the shape is easily visible and is suitable for design. Furthermore, a design layer excellent in terms of thinning and weight reduction can be formed. The "minor diameter", "major diameter", and "thickness" mentioned here are calculated by placing the scaly particles stably on a horizontal surface and observing them from above using a microscope, with the length of the shortest part being the "minor diameter", the length of the longest part being the "major diameter", and the maximum height from the bottom being the "thickness".

[0023] In the present invention, it is preferable that the component (B) contains large particles (b1) having a minor axis of more than 2 mm (hereinafter referred to as "large particles (b1)"). By containing the large particles (b1), a large pattern design can be effectively imparted to the formed coating. In the present invention, even when such large particles (b1) are contained, it is possible to suppress the edge from jumping up, and it is possible to form a formed coating having little roughness and excellent flatness and aesthetics.

[0024] Furthermore, in addition to the large particles (b1), the component (B) preferably contains medium particles (b2) (hereinafter referred to as "medium particles (b2)") with a short diameter of more than 0.7 mm and 2 mm or less, and small particles (b3) (hereinafter referred to as "small particles (b3)") with a short diameter of 0.7 mm or less. By using components (B) of different sizes in this way, it is possible to form a coating with less roughness and excellent flatness and aesthetics, and it is possible to form a coating with a well-balanced pattern (arrangement) without the unevenness of the scale-like particles. This makes it possible to impart colors such as natural stone and designs such as large patterns.

[0025] In the present invention, it is preferable to use the large particles (b1), the medium particles (b2), and the small particles (b3) in combination at a specific weight ratio, and it is preferable that the weight ratio [(b2)+(b3)] / (b1) of the medium particles (b2) and the small particles (b3) to the large particles (b1) is 1 or more and 50 or less (more preferably 3 or more and 40 or less, and even more preferably 5 or more and 30 or less). When such a range is satisfied, the medium particles (b2) are mainly visually recognized as the base pattern (base color) of the formed coating, and the small particles (b3) act as a component that imparts a small design to the formed coating and imparts hiding properties, etc. to the formed coating. As a result, the large particles (b1) are less likely to be biased, and a formed coating having excellent aesthetics and a good balance (arrangement) of the large pattern of the large particles (b1) in the base pattern formed by the medium particles (b2) and the small particles (b3) can be formed. Furthermore, the medium particles (b2) and small particles (b3) can sufficiently suppress the end jumping of the large particles (b1), and a flat coating with even less roughness can be formed. Furthermore, the weight ratio (b2) / (b3) of the medium particles (b2) to the small particles (b3) is preferably 1 or more and 30 or less (more preferably 1.5 or more and 20 or less, and even more preferably 2 or more and 10 or less). When such a range is satisfied, the above effect can be further enhanced.

[0026] The mechanism of action by which such an effect is obtained is not limited, but for example, the medium particles (b2) and small particles (b3) smaller than the large particles (b1) act as spacers for the large particles (b1) and contribute to the dispersibility of the large particles (b1). In addition, the small particles (b3) smaller than the medium particles (b2) act as spacers for the medium particles (b2) and contribute to the dispersibility of the medium particles (b2). As a result, it is presumed that the (B) component dispersed in the coating material can maintain good dispersibility for the large particles (b1), medium particles (b2), and small particles (b3). In particular, it is presumed that in a coating material containing a relatively large amount of medium particles (b2), the large particles (b1) and small particles (b3) are dispersed in the medium particles (b2) in a well-balanced manner. It is presumed that by applying such a coating material, the particles are less likely to be biased, a coating with a well-balanced pattern is formed, and the jumping up of the particle ends can be sufficiently suppressed.

[0027] In the present invention, the minor axis of component (B) refers to the length of the shortest part when the scale-like particles are stably placed on a horizontal surface, as described above, and the large particles (b1), medium particles (b2), and small particles (b3) can be classified by sieving using a metal mesh sieve (standard sieve) specified in JIS Z8801-1:2000. In this case, if the opening of the standard sieve is "a", the length of the diagonal line "L = √2a" can be considered to correspond to the minor axis. Specifically, 100 g of component (B) is weighed out and sieved for 10 minutes using a test method (manual sieving) in accordance with JIS K 0069, Large particles (b1) are those that do not pass through a 12 mesh (a=1.4 mm, L=2.0 mm) sieve. Those that pass through a 12 mesh (a=1.4mm, L=2.0mm) sieve but do not pass through a 30 mesh (a=0.5mm, L=0.7mm) sieve are called medium particles (b2), Those that pass through a 30 mesh (a=0.5mm, L=0.7mm) sieve are small particles (b3), Let us assume that. The upper limit of the large particles (b1) is preferably those that pass through a 6.5 mesh (a=2.8 mm, L=4.0 mm) sieve (particles with a minor axis of 4 mm or less), whereas the lower limit of the small particles (b3) is preferably those that do not pass through a 70 mesh (a=0.21 mm, L=0.3 mm) sieve (particles with a minor axis of more than 0.3 mm).

[0028] In the present invention, the component (B) may be monochromatic (one color only) or multi-colored depending on the desired design. When the component (B) is monochromatic (one color only), a coating having a pattern derived from the shape of each particle can be obtained.

[0029] When the (B) component is of a plurality of colors, it is preferable that the component contains particles of at least two or more colors (more preferably, two to six colors). This allows a coating film to have a pattern derived from the shape of each particle and a design such as a variety of colors. The embodiment in which the (B) component contains two or more colors can be set according to the desired pattern (design). In the present invention, it is preferable that the large particles (b1) and the medium particles (b2) contain particles of different colors. This allows the large accent design to be effectively recognized, and a coating film with excellent aesthetics can be easily formed. In addition, it is preferable that the small particles (b3) contain particles of the same color system as the large particles (b1) or the medium particles (b2) (more preferably, the medium particles (b2)). This gives the formed coating a sense of depth, and further improves aesthetics.

[0030] Moreover, the large particles (b1), the medium particles (b2), and the small particles (b3) may each contain particles of two or more colors. In particular, when the large particles (b1) contain two or more colors, the sense of variegation is improved, and the aesthetic appearance can be further enhanced. When the medium particles (b2) contain two or more colors, it is preferable that the medium particles (b2') that become the base pattern (base color) of the formed coating are contained in the medium particles (b2) at 50% by weight or more (more preferably 55% by weight or more). The medium particles (b2') may contain two or more types of particles of a single color (only one color) or similar colors (similar colors). This makes the accent design of the large particles (b1) easier to see, and the aesthetic appearance can be improved. Furthermore, when the small particles (b3) are of two or more colors, it is preferable that the small particles (b3') which become the base pattern (base color) of the formed coating and have the same color system as the hollow particles (b2') account for 60% by weight or more (more preferably 65% ​​by weight or more) of the small particles (b3).

[0031] In the above component (B), a different color refers to a color difference (ΔE) of preferably 10 or more (more preferably 15 or more). Also, the same color system (similar or similar colors) refers to a color difference (ΔE) of preferably less than 10 (preferably 8 or less). The color difference (ΔE) referred to here is a value measured using a color difference meter, and can be calculated from the respective L*, a*, and b* values ​​according to the following formula. <Formula>△E={(L *1 -L *2 ) 2 +(a *1 -a *2 ) 2 +(b *1 -b *2 ) 2} 0.5 During the ceremony, L *1 , a *1 , b *1 are the first color of the (B) component, L * , a * , b * . L *2 , a *2 , b *2are the second color of the (B) component, L * , a * , b * . Furthermore, the L*, a*, and b* of component (B) can be calculated by placing component (B) on a glass plate until the glass surface is covered, and then covering the component with a PE film (colorless and transparent) and measuring the surface.

[0032] As described above, when the coating material of the present invention contains a combination of large particles (b1), medium particles (b2), and small particles (b3) as component (B), the dispersibility of component (B) can be sufficiently ensured. This allows good dispersibility to be obtained even when a small amount of dispersant is added (preferably 0.1% by weight or less in the coating material, and more preferably no dispersant is added) compared to conventional coating materials. This allows the coating film to exhibit excellent water resistance and other properties.

[0033] The present invention is characterized in that it contains an associative viscosity modifier (C) (hereinafter also referred to as "component (C)") as a viscosity modifier. The associative viscosity modifier is a viscosity modifier that forms a network structure by associating molecules in an aqueous medium through hydrophobic interactions to impart viscosity, and is a polymer consisting of hydrophobic and hydrophilic sites. By containing such component (C), the viscosity can be improved and a flat coating can be easily formed due to hydrophobic interactions occurring between at least one of the hydrophobic groups of component (A), component (B), and other components (medium, additives, etc.) and hydrophobic interactions between components (C). In particular, when a coating is formed by spray coating, the edge jumping of component (B) can be sufficiently suppressed, and a flatter coating with less roughness can be easily formed. Furthermore, component (C) is also advantageous in terms of coating properties such as water resistance.

[0034] Component (C) is a hydrophobic group-modified polymer in which the hydrophobic site is bonded to a polymer such as a soluble polymer, a water-dispersible polymer, or a swellable polymer, and examples thereof include hydrophobically modified ethoxylated urethane (HEUR), hydrophobically modified alkali-swellable / soluble emulsion (HASE), hydrophobically modified hydroxyethyl cellulose (HMHEC), hydrophobized polyacrylamide, etc. These can be used alone or in combination of two or more.

[0035] In the present invention, it is preferable to include hydrophobically modified ethoxylated urethane (HEUR) (c1) (hereinafter also referred to as "(c1) component") as the (C) component. The (c1) component is, for example, a bifunctional hydrophilic polyether polyol and a hydrophobic compound bonded via a urethane bond, and has hydrophobic alkyl groups at both ends. The alkyl group can also have a branched chain. Specific examples of such (c1) components include hydrophobically modified polyoxyethylene urethane resins and nonionic hydrophobically modified polyoxyethylene urethane block copolymers. By including such a (c1) component, the effect of suppressing the edge jumping of the (B) component is enhanced, and a coating film with less roughness and a flatter coating can be easily formed.

[0036] Furthermore, in the present invention, it is preferable to use, as component (C), the above-mentioned component (c1) in combination with one or more associative viscosity modifiers (c2) (hereinafter also referred to as "component (c2)") selected from hydrophobically modified alkali-swellable / soluble emulsions (HASE), hydrophobically modified hydroxyethyl cellulose (HMHEC), and hydrophobized polyacrylamides. Examples of hydrophobically modified alkali-swellable / soluble emulsions (HASE) include hydrophobically modified alkali-soluble emulsions and hydrophobically modified poly(meth)acrylic acids.

[0037] The mixing ratio of (c1) / (c2) is preferably 100 / 0 to 10 / 90 (preferably 98 / 2 to 30 / 70) in terms of solid weight ratio. In such a case, the effect of suppressing the settling of the (B) component can be enhanced. In addition, since the (B) component is stably dispersed in the coating material during coating, coating workability is excellent, and the (B) component is unlikely to be biased, forming a coating film with a well-balanced pattern.

[0038] The mixing ratio of the (C) component is preferably 0.05 to 10 parts by weight (more preferably 0.1 to 8 parts by weight) in terms of solid content relative to 100 parts by weight of the solid content of the (A) component. When this range is satisfied, the above-mentioned effects can be fully exhibited.

[0039] In the present invention, the viscosity modifier may contain a viscosity modifier (C') other than the above-mentioned component (C) (hereinafter also referred to as "component (C')"). The component (C') is not particularly limited, and examples thereof include an alkali swelling type viscosity modifier (ASE), a cellulose-based viscosity modifier (HEC), polyvinyl alcohol, an inorganic viscosity modifier, and the like. These may be used alone or in combination of two or more.

[0040] The coating material of the present invention contains the above-mentioned (A) component and the above-mentioned (B) component in a specific weight ratio, and further contains the above-mentioned (C) component, and is characterized in that the viscosity is 1 to 50 Pa·s (preferably 5 to 45 Pa·s, more preferably 10 to 40 Pa·s, and even more preferably 13 to 35 Pa·s) and the thixotropy index (TI value) (hereinafter also referred to as "TI value") is 4 or more (preferably 4.5 to 10, more preferably 5 to 9.5, particularly preferably 5.5 to 9, and most preferably 6 to 8.5). In such a case, a flat coating film with little roughness can be formed. In the present invention, the viscosity and TI value of the coating material satisfy the above ranges, and thus the coating workability is good and the orientation of the above-mentioned (B) component is enhanced, which is preferable in terms of improving the coating workability and the finish. The above viscosity and TI value are values ​​obtained by measuring the coating material to be applied (at the time of application), and if dilution is required at the time of application, they are measured after dilution.

[0041] Generally, the TI value of a coating material is set to 2 or more for the purpose of imparting an uneven pattern (for example, JP 2009-056429 A, etc.). In contrast, the present invention has discovered that when scaly particles are included, a flat coating with little roughness can be formed by setting the TI value to 4 or more. In particular, the coating material of the present invention is less likely to cause the edges of component (B) to jump up during spray coating, and a flat coating can be formed.

[0042] In the present invention, the viscosity is a value determined by measuring the viscosity at 20 rpm (the indicator value at the fourth revolution) using a BH type viscometer. The thixotropy index (TI) is a value determined by the following formula using a BH type viscometer. The measurement temperature in both cases is 25°C. <Formula>TI=η1 / η2 (In the formula, η1 is the viscosity at 2 rpm (Pa s: indicator value at the second rotation). η2 is the viscosity at 20 rpm (Pa s: indicator value at the fourth rotation).)

[0043] The coating material of the present invention preferably contains an organic solvent (D) (hereinafter also referred to as "component (E)") having a solubility in water (at 20°C) of less than 10 g / 100 g (preferably 0.5 to 9 g / 100 g, more preferably 1 to 8 g / 100 g). By containing such an organic solvent (D), the effects of the present invention can be further enhanced. In the present invention, the solubility in water refers to the maximum mass (g) that can be dissolved in 100 g of water. The measurement temperature is 20°C.

[0044] Examples of such (D) components include ethylene glycol monohexyl ether, ethylene glycol-2-ethylhexyl ether, ethylene glycol monobutyl ether acetate, ethylene glycol dibutyl ether, diethylene glycol monohexyl ether, diethylene glycol monobutyl ether acetate, diethylene glycol dibutyl ether, propylene glycol monobutyl ether, propylene glycol phenyl ether, propylene glycol diacetate, dipropylene glycol monobutyl ether, dipropylene glycol tertiary butyl ether, tripropylene glycol monobutyl ether, octylene glycol, 2-ethylhexylene glycol, 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate, 2,2,4-trimethyl-1,3-pentanediol diisobutyrate, benzyl alcohol, etc. These can be used alone or in combination of two or more.

[0045] The content of the (D) component is 1 to 50 parts by weight (preferably 3 to 30 parts by weight) per 100 parts by weight of the solid content of the (A) component. In such a case, a smoother coating film with less roughness can be easily formed.

[0046] The coating material of the present invention may contain powder (E) such as granular aggregate (hereinafter also referred to as "component (E)") in addition to the above components, within a range that does not impair the effects of the present invention. The component (E) has a different shape from the component (B). Examples of such component (E) include crushed natural stone, ceramic powder, ceramic powder, rubber granules, metal granules, resin beads, silica sand, feldspar, silica stone, kansui stone, glass beads, and colored versions of these. The mixing ratio of component (E) is preferably 80 parts by weight or less (more preferably 25 parts by weight or less, even more preferably 10 parts by weight or less, and particularly preferably 5 parts by weight or less) relative to 100 parts by weight of the solid content of component (A). An embodiment that does not contain component (E) is also suitable.

[0047] The coating material of the present invention can be produced by uniformly mixing the above-mentioned components by a known method, but if necessary, other components that can usually be used in coating materials can also be mixed in. Examples of such components include color pigments, extender pigments, fibers, film-forming assistants, leveling agents, coupling agents, plasticizers, antifreeze agents, pH adjusters, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, antifoaming agents, ultraviolet absorbers, light stabilizers, antioxidants, water, etc.

[0048] The coating material of the present invention is an aqueous coating material containing an aqueous medium as a medium. The pH of the coating material is preferably 7 to 12 (more preferably 7.5 to 11). In such a range, the effect of the present invention can be sufficiently enhanced. Furthermore, the non-volatile content of the coating material is preferably 10 to 80% by weight (more preferably 15 to 70% by weight). In such a range, a formed coating film having design characteristics such as various colors unique to natural stone and excellent flatness and aesthetic appearance with less roughness can be obtained. The non-volatile content can be set by adjusting the blending ratio of each component. The aqueous medium is a medium mainly containing water, and may be mixed with water-soluble solvents such as lower alcohols, polyhydric alcohols, ether compounds, ester compounds, and alkylene oxide-containing compounds as necessary.

[0049] <Film formation method> The coating material of the present invention is applied to a substrate to form a coating. The substrate constitutes the surface of a building, civil engineering structure, etc. Examples of such substrates include concrete, mortar, siding board, extrusion molding board, gypsum board, perlite board, slate board, plywood, brick, plastic board, metal plate, glass, porcelain tile, etc. These substrates may have a coating already formed on their surface, or may have wallpaper attached thereto, etc.

[0050] The coating material of the present invention can be applied, for example, with a brush, trowel, roller, spray, etc. to form a coating. In the present invention, spray application or roller application is preferred, and it is particularly preferred to form a coating by spray coating using a spray. This makes it possible to easily form a coating that is less likely to be biased in the scale-like particles (B), has a good balance (arrangement) of the pattern, and is flat and aesthetically excellent with little roughness.

[0051] The amount of the coating material of the present invention to be applied is not particularly limited, but is preferably 0.05 to 1 kg / m per application. 2 (More preferably 0.1 to 0.8 kg / m 2 The number of times of application can be set depending on the desired design, but is preferably 1 to 2 times (more preferably 2 times). In such a case, the effect of the present invention can be fully exhibited.

[0052] The coating material may be dried preferably at room temperature (0 to 40° C.). When the coating material is applied multiple times, it is desirable to apply the subsequent coating material after the previous coating film has dried.

[0053] The coating formed by the above method is advantageous in terms of thinning and weight reduction, etc. The thickness (dry film thickness) of the coating of the present invention is preferably 50 to 1000 μm (more preferably 80 to 800 μm, and even more preferably 100 to 500 μm), and the dry coating weight is preferably 0.1 to 0.8 kg / m 2 (More preferably 0.2 to 0.5 kg / m 2 Even though it is a thin film, it has little roughness and is flat, making it possible to obtain a design with excellent aesthetics.

[0054] In the present invention, it is preferable to apply a primer to the surface of the substrate to form a colored coating, and then apply a coating material. As the primer for forming the colored coating, a material containing a resin and a pigment can be used. In the present invention, the color, gloss, etc. can be set by adjusting the type and mixing ratio of the pigment. The mixing ratio of the resin and the pigment is preferably 5 to 500 parts by weight (more preferably 20 to 400 parts by weight, and even more preferably 30 to 300 parts by weight) of the pigment per 100 parts by weight of the resin solid content.

[0055] The color tone of the colored coating may be appropriately set according to the desired design, but in the present invention, it is preferable to set the hue (common color) close to that of the medium particles (b2) of the component (B). This can enhance the effect of preventing unevenness in the formed coating. In addition, it can give the formed coating a greater sense of depth, etc., and form a multi-layer coating with excellent aesthetics.

[0056] It is desirable to set the color tone of the colored coating so that the color difference (ΔE) between the color tone of the medium particles (b2') that form the base pattern (base color) in the medium particles (b2) is 20 or less (preferably 0.5 to 15, more preferably 1 to 12, and even more preferably 1.5 to 10). In such a case, a laminated coating with excellent aesthetic appearance can be obtained. The color difference (ΔE) referred to here is a value measured using a color difference meter, and can be calculated from the respective L*, a*, and b* values ​​according to the following formula. <Formula>△E={(L *1 -L *2 ) 2 +(a *1 -a *2 ) 2 +(b *1 -b *2 ) 2} 0.5 During the ceremony, L *1 , a *1 , b *1 is the L of the colored coating * , a * , b * . L *2 , a *2 , b*2 is the L of the medium particle (b2') * , a * , b * . The L*, a*, and b* of the medium particle (b2') can be calculated by placing the (b2) component on a glass plate until the glass surface is covered, and then measuring the surface that is covered with a PE film (colorless and transparent).

[0057] As the resin for the undercoat material, the same resin as that for the coating material can be used.

[0058] As the pigment of the undercoat material, known color pigments, extender pigments, etc. can be used. Among them, examples of color pigments include titanium oxide, zinc oxide, carbon black, lamp black, bone black, graphite, black iron oxide, copper chromium black, cobalt black, copper manganese iron black, red iron oxide, molybdate orange, permanent red, permanent carmine, anthraquinone red, perylene red, quinacridone red, yellow iron oxide, titanium yellow, fast yellow, benzimidazolone yellow, chrome green, cobalt green, phthalocyanine green, ultramarine blue, Prussian blue, cobalt blue, phthalocyanine blue, quinacridone violet, dioxazine violet, aluminum flake pigment, pearl pigment, and luster pigment. By using one or more of these color pigments, it is possible to color the material to any hue.

[0059] Examples of the extender pigment include heavy calcium carbonate, kansui stone, light calcium carbonate, white carbon, kaolin, clay, china clay, diatomaceous earth, barite powder, barium sulfate, precipitated barium sulfate, silica sand, silica stone powder, quartz powder, resin beads, glass beads, hollow balloons, etc., and one or more of these can be used. By appropriately setting the type of extender pigment, the mixing ratio, etc., the coating material can be adjusted to a desired glossiness.

[0060] In addition to the above components, the undercoat material of the present invention may contain known additives, such as aggregates, dyes, thickeners, wetting agents, antifreeze agents, film-forming assistants, preservatives, antifungal agents, anti-algae agents, antibacterial agents, dispersants, antifoaming agents, ultraviolet absorbers, light stabilizers, antioxidants, catalysts, diluting solvents, etc., within the range that does not significantly impair the effects of the present invention. The undercoat material can be manufactured by uniformly mixing the above-mentioned components by a standard method.

[0061] The undercoat material can be applied, for example, with a brush, trowel, roller, spray, etc. to form a colored coating. The amount of the undercoat material applied is not particularly limited, but is preferably 0.05 to 1 kg / m per application. 2 (More preferably 0.1 to 0.8 kg / m 2 The number of times of application can be set depending on the desired design, but is preferably 1 to 2 times (more preferably 2 times). In such a case, the effect of the present invention can be fully exhibited.

[0062] The drying of the undercoat material is preferably carried out at room temperature (0 to 40°C), and after the undercoat material is dried, the coating material of the present invention can be applied by the above-mentioned method. When applying the undercoat material multiple times, it is preferable to apply the subsequent undercoat material after the coating film of the previous undercoat material has dried, and then apply the coating material of the present invention after drying. EXAMPLES

[0063] The following examples will clarify the features of the present invention.

[0064] (Coating material 1~23) Based on the formulations shown in Tables 1 and 2, the raw materials were mixed in a conventional manner and the pH was adjusted to 8.5 to produce coating materials 1 to 16.

[0065] The following components were used: (A) Water-based resin Acrylic resin emulsion [solid content 50% by weight, medium: water] (B) Scaly particles (b1) Large particles (b1-1) Black mica piece [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average value): 0.95, minor diameter / thickness (average value): 11.4] (b1-2) White mica piece [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average value): 0.88, minor diameter / thickness (average value): 10.7] (b1-3) Light cream-colored mica pieces [minor diameter: over 2 mm and less than 4 mm, minor diameter / major diameter (average): 0.92, minor diameter / thickness (average): 11.5] (b2) Medium particles (b2-1) Gray mica pieces [minor diameter: over 0.7 mm and 2 mm or less, minor diameter / major diameter (average value): 0.87, minor diameter / thickness (average value): 10.5] (b3) Small particles (b3-1) Gray mica pieces [minor diameter: over 0.3 mm and less than 0.7 mm, minor diameter / major diameter (average): 0.92, minor diameter / thickness (average): 11.4] (b3-2) White mica piece [minor diameter: over 0.3 mm and less than 0.7 mm, minor diameter / major diameter (average value): 0.94, minor diameter / thickness (average value): 11.0] (C) Viscosity adjuster (c1) Hydrophobically modified polyoxyethylene urethane resin (HEUR) [solid content 30% by weight] (c2) Hydrophobically modified alkali-swellable acrylic resin emulsion (HASE) [solid content 30% by weight] (C') Other viscosity modifiers (C'-1) Alkali swelling acrylic resin emulsion (ASE) [solid content 30% by weight] (C'-2) Hydroxyethyl cellulose (HEC; powder) (D) Organic solvent (d1) Dipropylene glycol monobutyl ether (solubility in water 5g / 100g) (d2) 2,2,4-trimethyl-1,3-pentanediol monoisobutyrate (solubility in water 0.09g / 100g) (others) Additives (defoamers, UV absorbers)

[0066] Example 1 A primer (light gray) was spray painted onto the substrate (slate board). Next, coating material 1, which had been adjusted (diluted with water) to the viscosity and TI value shown in Table 1, was applied with a spray gun (diameter: 5.5 mm) in an amount of 0.8 kg / m 2 The coating was then dried and hardened at 23°C for 24 hours to form a patterned coating, which was used as test specimen (I).

[0067] <Evaluation> The following evaluations were carried out, and the results are shown in Table 1. Texture (touch) The coating that was formed was rated on a four-point scale of A>B>C>D, with "A" being the least rough coating and "D" being the rough coating. ·Design 1 (Aesthetics) Those with little bias in the scaly colored particles and a good balance of the pattern were given an "AA" rating, while those with a poorer pattern were given a "D", and the evaluation was on a five-level scale from AA>A>B>C>D. ·Design 2 (Design stability) The coating material 1 was left to stand for 24 hours, and then painted to form a patterned coating, which was used as specimen (II). Specimens (I) and (II) were compared, and those that produced similar patterns were given an "A" rating, while those that produced inferior patterns were given a "D" rating, and were rated on a four-level scale of A>B>C>D.

[0068] (Examples 2 to 20, Comparative Examples 1 to 3) Patterned coatings were formed and evaluated in the same manner as in Example 1, except that Coating Materials 2 to 23 were used instead of Coating Material 1. The results are shown in Table 1.

[0069] In Examples 1 to 20, it was possible to form coatings that had a good feel and pattern balance and were excellent in appearance. In particular, in Examples 3 to 7 and 10 to 14, the coating material had excellent stability during painting work, and a coating film having an excellent design with excellent aesthetics could be stably formed. Furthermore, in Example 14, there was little bias in the large, medium, and small scale-like particles, and the pattern was well-balanced and had a design with excellent color diversity. On the other hand, the films formed in Comparative Examples 1 to 3 had a rough feel and were inferior in texture.

[0070]

Table 1

[0071]

Table 2

Claims

1. A coating material comprising an aqueous resin (A) and scaly particles (B), the coating material containing 10 to 200 parts by weight of the scaly particles (B) per 100 parts by weight of the solid content of the aqueous resin (A); the scale-like particles (B) include large particles (b1) having a short diameter of more than 2 mm, medium particles (b2) having a short diameter of more than 0.7 mm and not more than 2 mm, and small particles (b3) having a short diameter of 0.7 mm or less; the coating material includes an associative viscosity modifier (C) as a viscosity modifier, and has a viscosity of 1 to 50 Pa s and a thixotropy index (TI value) of 4 or more; The coating material is characterized in that the mixing ratio of the powdery or granular material (E) excluding the scaly particles (B) is 5 parts by weight or less per 100 parts by weight of the solid content of the aqueous resin (A).

2. The coating material as described in claim 1, characterized in that the weight ratio of the medium particles (b2) and small particles (b3) to the large particles (b1), [(b2) + (b3)] / (b1), is 1 or more and 50 or less.

3. A method for forming a coating film by applying a coating material to a wall surface, the coating material comprising an aqueous resin (A) and scaly particles (B), the coating material comprising 10 to 200 parts by weight of the scaly particles (B) per 100 parts by weight of a solid content of the aqueous resin (A), the scale-like particles (B) include large particles (b1) having a short diameter of more than 2 mm, medium particles (b2) having a short diameter of more than 0.7 mm and not more than 2 mm, and small particles (b3) having a short diameter of 0.7 mm or less; the coating material includes an associative viscosity modifier (C) as a viscosity modifier, and has a viscosity of 1 to 50 Pa s and a thixotropy index (TI value) of 4 or more; The coating material is characterized in that the mixing ratio of the powder (E) excluding the scaly particles (B) is 5 parts by weight or less per 100 parts by weight of the solid content of the aqueous resin (A).

4. The coating forming method as described in claim 3, characterized in that the weight ratio of the medium particles (b2) and small particles (b3) to the large particles (b1), [(b2) + (b3)] / (b1), is 1 or more and 50 or less.

Citation Information

Patent Citations

  • Coating composition having neptunian stone-like multicolored pattern, and coating finish by using the same

    JP2000086942A

  • Water paint composition and method for forming paint film with the same

    JP2005225927A

  • Decorative coating material and decorative building material

    JP2006152231A

  • Coating method

    JP2011212675A

  • Clear coating composition for ceramic building material

    JP2013224363A