Optical molding device and method for manufacturing three-dimensional objects
The stereolithography apparatus addresses the issue of height variations in coating films by using a recoater with specific angles and heating, ensuring uniform thickness and improved accuracy in 3D object production.
Patent Information
- Application Number
- JP2024554194
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2023-07-27
- Filing Date
- 2024-05-29
- Publication Date
- 2024-11-28
- Estimated Expiration
- 2044-05-29
AI Technical Summary
The existing stereolithography methods face challenges in maintaining uniform thickness and accuracy of coating films due to variations in height differences between cured and uncured surfaces, leading to issues like sagging overhangs and deviations from the designed shape.
A stereolithography apparatus with a recoater design that includes a sweeping member with specific angles and distances between front and rear surfaces, along with controlled shear stress and optional heating, to minimize height differences and improve modeling accuracy.
The apparatus effectively reduces height differences between cured and uncured surfaces, enhancing the accuracy and uniformity of the coating films, thereby improving the precision of the final 3D objects.
Smart Images

Figure 0007591337000001 
Figure 0007591337000002 
Figure 0007591337000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a stereolithography apparatus, and more particularly to the application of materials therein. [Background technology]
[0002] 3D modeling is a processing method that has a great advantage in that it can directly mold and process complex 3D shapes. It offers a much higher degree of freedom than the conventional cutting method used to obtain 3D objects, and its advantages have attracted a great deal of attention in recent years.
[0003] A widely known example of a prior 3D photolithography method, which is one of the 3D modeling methods, is the free liquid surface method, which is realized by a scanning exposure system using a laser beam and a galvanometer mirror. Also known is a backside exposure method called the regulated liquid surface method, in which one layer is modeled through the glass from the bottom side of a container containing a photocurable material by one-step exposure using a DMD, and then the model is lifted up to the required thickness and material is filled under the model, repeating this exposure and lifting process to model (see, for example, Patent Document 1).
[0004] However, in recent years, a method of applying a photocurable resin to a flat surface and exposing the surface by laser scanning has been widely used as a three-dimensional optical modeling method. For example, a method is already known in which a paste-like modeling material called a slurry, which is a mixture of a photocurable monomer resin (liquid) and ceramic powder, is supplied to one end of a modeling surface, and the modeling material is thinly applied to the modeling surface by horizontally moving a blade-shaped application member (sweeping member) called a recoater, and a necessary area is exposed from above the coating film obtained by this method by laser scanning to harden the modeling material, thereby obtaining a three-dimensional object (see, for example, Patent Document 2).
[0005] Furthermore, when obtaining a shaped object by the controlled liquid level method, a mode in which a smooth layer of a building material is obtained by using a doctor blade is already known (see, for example, Patent Document 3).
[0006] Meanwhile, in order to maintain suitable physical properties such as the viscosity of a photocurable composition, i.e., a slurry, used in 3D photopolymerization, an embodiment is already known in which a temperature control member for adjusting the temperature of the photocurable composition is attached to a dispenser (discharge means) that discharges the slurry (see, for example, Patent Document 4). [Prior art documents] [Patent documents]
[0007] [Patent Document 1] JP 2017-124631 A [Patent Document 2] Patent No. 7014480 [Patent Document 3] Patent Publication No. 2022-24960 [Patent Document 4] Patent No. 6438919 Summary of the Invention
[0008] For example, in the case of a modeling method in which supply and application of a slurry and exposure of a predetermined area of the formed coating film are repeated as disclosed in Patent Document 2, each coating film is essentially required to be formed with a uniform thickness. In other words, the upper surface of the coating film is required to be horizontal at a target height.
[0009] However, except in exceptional cases such as the first application, the modeling surface, i.e., the surface to which the slurry is applied, will include a mixture of the top surface of the area (hardened area) that has been hardened by the most recent exposure (hereinafter referred to as the hardened surface) and the top surface of the unhardened area that has not been exposed to light and remains in a paste-like slurry state (hereinafter referred to as the unhardened surface).
[0010] Therefore, when the recoater is moved horizontally at a predetermined height to sweep-coat the slurry supplied to one end of the surface to be coated in order to form a new coating film on a certain modeling surface, a coating film is formed uniformly with a substantially targeted thickness on the hardened area, whereas on the unhardened area, shear stress is generated in the slurry that already constitutes the unhardened surface as the recoater moves, and an excessive amount of slurry moves (is carried away) in the direction of the recoater movement, resulting in the thickness of the coating film newly formed on the unhardened surface being smaller than the thickness of the coating film formed on the hardened surface. That is, the height of the upper surface of the coating film on the unhardened surface (hereinafter simply referred to as the height of the coating film) may be slightly lower than the height of the coating film on the hardened surface.
[0011] If exposure is performed in such a state where the height of the coating film varies depending on the location, for example, the area directly below which was uncured may be exposed, causing the overhanging portion that extends or protrudes horizontally above the uncured area to sag downward, resulting in the shape of the molded object differing from the designed shape and compromising the molding precision.
[0012] Such defects are thought to be influenced by a complex number of factors, including the viscosity of the slurry, the surface tension, the adhesive force to the recoater surface and the adhesive force to the cured surface, the distance from the bottom end of the recoater to the cured surface, the distance to the top surface of the cured area below the uncured area, or the distance to the top surface of the modeling table, the moving speed of the recoater, etc. Furthermore, they also depend on the shape of the model and the form of the unexposed parts. Although the effect may be small depending on the modeling shape, it is not easy to fundamentally avoid the occurrence of such defects regardless of the modeling shape.
[0013] The present invention has been made in consideration of the above-mentioned problems, and aims to provide an optical molding apparatus that can reduce the height difference that occurs in a coating film formed on a modeling surface when obtaining a three-dimensional object by repeatedly applying a slurry and exposing a predetermined area of the formed coating film to light.
[0014] In order to solve the above-mentioned problems, a first aspect of the present invention is an optical modeling apparatus for obtaining a three-dimensional model, comprising: a modeling table; a discharge means for discharging a slurry having thixotropy onto the modeling table; a sweeping member; a sweeping means for sweeping-coating the slurry discharged onto the modeling table by horizontally moving the sweeping member in a predetermined sweeping position to form a slurry film; and an exposure means for exposing a predetermined area of the slurry film according to an exposure pattern created in advance based on three-dimensional shape data, wherein the sweeping member in the sweeping position has a front surface facing in the direction of travel of the sweeping coating and a rear surface facing in the opposite direction to the direction of travel, The angle α that the front surface makes with respect to the horizontal plane satisfies 30°<α<90°, At least near the lowest end of the sweep member, the distance in the traveling direction between the front and rear surfaces is uniform or becomes smaller toward the lowest end of the sweep member, and at the lowest end of the front surface or the lowest end of the rear surface, the distance in the traveling direction between the front and rear surfaces is 0.9 mm or less.
[0015] A second aspect of the present invention is a photo-polymerization apparatus according to the first aspect, wherein the sweeping means sweeps the slurry at a shear rate at which a shear stress is applied to the slurry such that the viscosity of the slurry is 1 Pa·s or more and 50 Pa·s or less.
[0017] The present invention 3 The embodiment is 1st or 2nd In the optical shaping apparatus according to the aspect of the present invention, the angle β that the rear surface forms with respect to the horizontal plane satisfies 30°<β<(180°-α).
[0018] The present invention 4 The third aspect is the optical shaping apparatus according to the first or second aspect, further comprising an in-sweep heating unit that heats the slurry being swept by the movement of the sweep member.
[0019] The present invention 5 The embodiment is 4In the optical molding apparatus according to the aspect, the sweeping heating means is a heater that heats the sweeping member, and the sweeping member heated by the heater moves to sweep the slurry, while the sweeping member heats the slurry.
[0020] The present invention 6 The embodiment is 5 In the optical shaping apparatus according to the aspect, the sweeping means includes a sweeping member holding means for holding the sweeping member, and the heater is attached to the sweeping member holding means.
[0021] The present invention 7 The embodiment of the present invention is a method for manufacturing a three-dimensional object, comprising: a discharge step of discharging a slurry having thixotropy onto a modeling table; a sweeping step of sweeping and applying the slurry discharged onto the modeling table by horizontally moving a sweeping member in a predetermined sweeping position to form a slurry film; and an exposure step of exposing a predetermined area of the slurry film to light according to an exposure pattern that is created in advance based on three-dimensional shape data, wherein in the sweeping step, the sweeping member has a front surface facing in the direction of progression of the sweep application and a rear surface facing in the opposite direction to the progression direction, The angle α that the front surface makes with respect to the horizontal plane satisfies 30°<α<90°, The slurry is applied after determining the sweeping posture of the sweeping member so that, at least near the lowest end of the sweeping member, the distance between the front and rear surfaces in the traveling direction is uniform or becomes smaller toward the lowest end of the sweeping member, and so that, at the lowest end of the front face or the lowest end of the rear face, the distance between the front and rear surfaces in the traveling direction is 0.9 mm or less.
[0022] The present invention 8 The embodiment is 7 In the method for producing a three-dimensional object according to the aspect of the present invention, in the sweeping step, the slurry being swept by the movement of the sweeping member is heated.
[0023] The first to third aspects of the present invention 8According to this aspect, in the intermediate product of a three-dimensional object obtained by repeatedly applying the slurry and exposing a specific area of the formed coating film to light, the height difference between the hardened and unhardened parts on the upper surface is suppressed, thereby improving the molding accuracy of the object.
[0024] In particular, 4 or 6 and 8 According to this aspect, by heating the slurry during sweep application, the smoothness of the slurry when applied can be improved, thereby further reducing the height difference between the cured and uncured portions. [Brief description of the drawings]
[0025] [Figure 1] FIG. 1 is a side view showing a schematic configuration of a photo-fabrication apparatus 1. [Diagram 2] FIG. 13 is a schematic side view for explaining slurry coating in the optical molding apparatus 1 in which the recoater 31 has a cutting edge 31L. [Diagram 3] FIG. 1 shows viscoelastic properties for a representative slurry material. [Figure 4] 3 is a diagram showing an ideal state after a slurry SL is applied to an upper surface 11s of the intermediate body 11 shown in FIG. 2 at a predetermined pitch p. [Diagram 5] FIG. 13 is a diagram showing a state in which application of the slurry SL is started after the slurry SL has been discharged onto an uncured surface located on the negative side of the modeling table 10 in the x-axis direction. [Figure 6] 6 is a diagram showing a state where recoater 31 has moved further from the state shown in FIG. 5 and has reached a position above hardened portion 12. FIG. [Figure 7] FIG. 7 is a diagram showing a state where the recoater 31 has moved further from the state shown in FIG. 6 and has reached above the second uncured portion 13b. [Figure 8] 8 is a diagram showing a schematic view of the intermediate product 11 shown in FIG. 2 after the application of slurry has been finally completed through the steps shown in FIGS. 5 to 7. FIG. [Figure 9]FIG. 13 is a diagram showing the state after the area RE1 is exposed. [Figure 10] FIG. 13 is a plan view showing an exposure pattern used in evaluating the effect of a recoater shape. [Figure 11] FIG. 13 is a diagram showing the shape of a recoater 31 used in the recoater shape effect evaluation, together with the posture when the recoater is attached to a recoat unit 30 and the slurry is applied by sweeping. [Figure 12] FIG. 13 is a diagram showing the shape of a recoater 31 used in the recoater shape effect evaluation, together with the posture when the recoater is attached to a recoat unit 30 and the slurry is applied by sweeping. [Figure 13] 13 is a captured image of the upper surface of an intermediate body 11 produced by using a type C recoater 31 to apply a slurry SL after the 50th exposure. [Figure 14] 13 is a histogram showing the results of height measurement after forming 50 layers when a type C recoater 31 is used. [Figure 15] 11 is a histogram showing the results of height measurement after forming 50 layers when a type G recoater 31 is used. [Figure 16] 13 is a graph showing the change in height difference between a cured surface 12s and an uncured surface 13s with respect to the number of layers when seven types of recoaters 31 are used. [Figure 17] 1A to 1C are diagrams showing examples of main shapes of the recoater 31 that are different from types F and G. [Figure 18] 13A and 13B are diagrams showing examples of further different shapes of the recoater 31. [Figure 19] 11A to 11C are diagrams illustrating the influence of differences in the shape of the recoater 31 on the molding of an object having an overhang. [Figure 20] 11A to 11C are diagrams illustrating the influence of differences in the shape of the recoater 31 on the molding of an object having an overhang. [Figure 21] 13 is a diagram showing a recoater 31 in a sweeping position in which the front inclination angle α is larger than when the cutting edge 31L is parallel to the horizontal plane. [Figure 22] FIG. 13 is a diagram illustrating a heating means during sweeping. [Diagram 23]13 is a graph showing the change in height difference between a cured surface 12s and an uncured surface 13s with respect to the number of layers when a type G recoater 31 is heated and when it is not heated. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0026] <First embodiment> <Outline of the photolithography device> FIG. 1 is a side view showing a schematic configuration of a photo-fabrication apparatus 1 according to a first embodiment of the present invention. The photo-fabrication apparatus 1 according to this embodiment is an apparatus that, roughly speaking, applies a paste-like thixotropic material called a slurry, which is a mixture of a photo-curable monomer resin (liquid) and ceramic powder (e.g., alumina), on a modeling table 10 in a thin layer, irradiates the obtained slurry film (layer) with light from a laser, LED, or the like, and exposes necessary areas to harden the resin, and repeats this process for the slurry films that are sequentially stacked to obtain a three-dimensional object (laminate). The photo-fabrication apparatus 1 includes a control circuit including a recording medium. The control circuit controls each part of the photo-fabrication apparatus 1 according to a program stored in the storage medium.
[0027] The optical modeling apparatus 1 mainly includes a modeling table 10, a discharge unit (an example of a discharge means) 20 that discharges slurry onto the modeling table 10, a recoating unit (an example of a sweeping means) 30 that sweeps the discharged slurry to form a slurry film (layer), and an exposure unit (an example of an exposure means) 40 that exposes the slurry film based on pattern data for exposure. Note that exposure based on pattern data for exposure performed by the exposure unit 40 in the optical modeling apparatus 1 may be referred to as drawing. The recoating unit 30 includes an electric motor and moves under the control of a control circuit.
[0028] In Figure 1, the direction in which the recoating unit 30 sweeps over the modeling table 10 is the positive x-axis direction, and the upward vertical direction is the positive z-axis direction, in a right-handed xyz coordinate system (a similar coordinate system will be used hereinafter).
[0029] The modeling table 10 is a rectangular table in a plan view, on whose upper surface 10s modeling is performed. The modeling table 10 is movable up and down in the z-axis direction. The lifting and lowering operation is realized by a lifting mechanism 10a.
[0030] Generally speaking, the modeling table 10 is lowered by a required amount each time the formation of the model progresses (each time the formation of a layer is completed).
[0031] The modeling table 10 is made of, for example, aluminum. In order to be able to model a large object, the modeling table 10 desirably has a modeling area of at least 600 mm×600 mm or more, and more desirably has a modeling area of 650 mm×650 mm or more.
[0032] 1, for simplicity of illustration, the intermediate body 11 obtained during modeling is directly laminated on the upper surface 10s of the modeling table 10, but it may be configured such that a film (not shown) is fixed on the modeling table 10 and the intermediate body 11 is laminated on the film. For example, the modeling table 10 may be provided with a suction groove (not shown) for suction-fixing the film, and the film may be vacuum-adsorbed by applying negative pressure to the suction groove in a state where the film is laid on the upper surface 10s of the modeling table 10.
[0033] The discharge unit 20 discharges the slurry for modeling stored in a storage section (not shown) onto the modeling table 10. The discharge unit 20 is, for example, configured of a pump equipped with a screw inside, and as the screw rotates, the slurry is discharged vertically downward (in the negative direction of the z-axis) from a nozzle 20n at the lower end as shown by an arrow AR1.
[0034] The slurry is discharged onto the upper surface 10s of the modeling table 10 at the start of modeling, and during modeling, the slurry is discharged onto the upper surface 11s of the modeling intermediate body 11, which is a laminate of slurry films that have been formed up to that point and have been partially exposed. The slurry is usually discharged near the end of the modeling table 10 in the negative x-axis direction that is close to the movement start position of the recoating unit 30, but depending on the modeling content, the slurry may be discharged at a position closer to the positive x-axis direction or may be discharged at multiple locations.
[0035] The recoat unit 30 applies the slurry discharged onto the modeling table 10 by sweeping it with a recoater (one example of a sweeping member) 31. The recoater 31 is a thin plate-like member, also called a blade, attached to the recoat unit 30 with its longitudinal direction extending in the y-axis direction. The recoater 31 is preferably made of metal (e.g., stainless steel) or glass, and its size in the y-axis direction is approximately the same as the size of the modeling table 10 in the y-axis direction.
[0036] The recoater 31 is moved in the x-axis direction by the movement of the recoat unit 30 while being kept at a predetermined distance from the modeling table 10. The recoater 31 spreads the slurry discharged onto the modeling table 10 (more specifically, the upper surface 10s of the modeling table 10 or the upper surface 11s of the modeling intermediate body 11) in the x-axis direction by this moving operation, thereby forming a slurry film.
[0037] The recoater 31 may be cleaned by a cleaning unit (not shown) after the coating operation.
[0038] In an exemplary embodiment, when the recoater 31 is attached to the recoat unit 30, a blade edge 31L (a portion connecting the lowermost end of the front surface 31F facing the traveling direction of the recoater 31 and the rear surface 31B facing in the opposite direction to the traveling direction of the recoater 31) of the recoater 31 forms an elongated flat surface. Therefore, in Fig. 1, it is assumed that the blade edge 31L is a flat surface extending in the y-axis direction, and the recoater 31 is shown as an isosceles trapezoid in cross section, but this is merely a schematic illustration.
[0039] The exposure unit (exposure means) 40 is a light source having one or more projectors equipped with light-emitting elements that irradiate light such as lasers and LEDs. The exposure unit 40 performs pattern exposure (projection) on the slurry coating film formed on the modeling table 10. Exposure by the exposure unit 40 is performed, for example, by a DMD projection method. That is, the exposure unit 40 is moved in a stepwise or continuous manner in the x-axis direction while a projection (exposure) pattern (data) is poured in and the pattern is projected. Then, after completing the movement in one direction, the exposure unit 40 is moved a predetermined distance in the y-axis direction, and exposure is performed while moving again in the opposite direction in the x-axis direction. In this case, exposure is performed in strips for each region of a predetermined width. These operations are repeated until exposure is completed for all modeling target areas in each layer. Instead of moving the exposure unit 40, the modeling table 10 may be moved to perform pattern exposure (projection), or both the exposure unit 40 and the modeling table 10 may be moved to perform pattern exposure (projection).
[0040] <Details of the slurry application process> Fig. 2 is a schematic side view for explaining slurry coating in the optical molding apparatus 1 in which the recoater 31 has a cutting edge 31L, as shown in Fig. 1. Fig. 2 shows a state in which a coating film of a slurry SL is further formed and laminated on the upper surface 11s of the already formed intermediate body 11 having a thickness d.
[0041] 2 has a hardened portion 12 that is hardened continuously from the upper surface 10s of the modeling table 10 by performing exposure with the same exposure pattern in the repeated application of slurry and the subsequent exposure, and an unhardened portion 13 that is unhardened continuously from the upper surface 10s of the modeling table 10. In other words, the unhardened portion 13 is a portion where the previously discharged slurry SL has accumulated without being hardened. The slurry that constitutes the unhardened portion 13 is referred to as the deposited slurry.
[0042] Furthermore, the uncured portion 13 has a first uncured portion 13a located in front of the cured portion 12 (negative side in the x-axis direction) in the x-axis direction, which is the moving direction of the recoater 31 when applying the slurry SL, and a second uncured portion 13b located behind the cured portion 12 (positive side in the x-axis direction). In this case, the upper surface 11s of the intermediate body 11 is composed of an upper surface 12s of the cured portion 12, an upper surface 13as of the first uncured portion 13a, and an upper surface 13bs of the second uncured portion 13b. The upper surface 12s of the cured portion 12 is also referred to as a cured surface 12s. The upper surface 13as of the first uncured portion 13a and the upper surface 13bs of the second uncured portion 13b are also referred to as an uncured surface 13as and an uncured surface 13bs, respectively, and both are collectively referred to as an uncured surface 13s.
[0043] In the case shown in FIG. 2, the slurry SL is discharged onto the uncured surface 13as of the intermediate body 11 that is on the negative side in the x-axis direction.
[0044] In FIG. 2, for ease of explanation, the upper surface 11s of the intermediate body 11 is shown to be uniformly flat. However, in reality, the upper surface 11s is not necessarily flat for reasons that will be described later.
[0045] When applying the slurry, the height of the modeling table 10 is adjusted so that the blade tip 31L of the recoater 31 is separated from the upper surface 11s of the intermediate body 11 by a pitch p corresponding to the thickness (target thickness) of the slurry film to be formed.
[0046] More specifically, assuming that the height of the cutting edge 31L relative to the upper surface 10s of the modeling table 10 is h, the height of the modeling table 10 is adjusted so that h=d+p is satisfied. During slurry application, the recoater 31 is moved so that the cutting edge 31L is aligned along a straight line (hereinafter, the cutting edge movement line) L parallel to the x-axis and whose height from the upper surface 10s is h as shown in FIG.
[0047] From the viewpoint of modeling accuracy and modeling time, the target thickness is desirably set to about 50 μm to 100 μm in practice, and in this case, the pitch p is also set to about 50 μm to 100 μm.
[0048] In this way, when the pitch p is set to about 50 μm to 100 μm, the viscosity of the slurry SL is sufficient to be 100 Pa·s or less, and is preferably 1 Pa·s or more and 50 Pa·s or less. In such a case, a slurry film of a target thickness can be suitably formed. Furthermore, it is more preferable that the viscosity is 30 Pa·s or less. Also, it is more preferable that the viscosity is about 5 Pa·s.
[0049] However, since the slurry SL is a thixotropic material, the viscosity during application changes depending on the application speed (i.e., the moving speed of the recoater 31). Fig. 3 is a diagram showing the viscoelastic properties of representative slurry materials. More specifically, Fig. 3 is a graph showing the dependency of the viscosity of a slurry material on the shear rate applied to the slurry material. The slurry material is a mixture of 45 vol% photocurable resin and 55 vol% alumina powder, and the alumina powder used has an average particle size of 0.6 μm and a particle size distribution in the range of 0.2 μm to 2 μm.
[0050] For example, if the target thickness is 100 μm (=0.1 mm) and the application speed of the slurry SL according to the graph is 2 mm / s, the shear rate is 2 / 0.1 = 20 / s. According to Fig. 3, the viscosity of the slurry SL at this shear rate is 10 Pa s.
[0051] During coating, the moving speed of the recoater 31 is set based on the viscoelastic properties shown in FIG. 3 so as to achieve a viscosity that falls within the above-mentioned viscosity range.
[0052] As the ceramic powder used in the slurry material, aluminum nitride, zirconia, silicon nitride, etc. can be used in addition to alumina.
[0053] Fig. 4 is a diagram showing an ideal state after the slurry SL is applied to the upper surface 11s of the intermediate body 11 shown in Fig. 2 at a predetermined pitch p. After the application is completed, as shown in Fig. 4, a slurry film 14 having a uniform thickness corresponding to the pitch p is formed over the entire upper surface 11s of the intermediate body 11, and then the slurry film 14 is exposed by the exposure unit 40, which is an ideal modeling mode. Fig. 2 also assumes that the intermediate body 11 is obtained through such an ideal mode.
[0054] However, in actual modeling, the application of the slurry and the subsequent exposure are not necessarily performed in such an ideal manner. In particular, when the slurry is applied to a modeling intermediate 11 in which the cured portion 12 and the uncured portion 13 are mixed and the latter is present to a considerable extent as shown in Fig. 2, it is difficult to form a slurry film in such an ideal manner. To explain this, Figs. 5 to 9 are diagrams showing in stages how the slurry SL is applied to the upper surface 11s of the modeling intermediate 11 shown in Fig. 2 at a predetermined pitch p, and how the slurry is exposed following the application.
[0055] FIG. 5 shows a state in which application of the slurry SL is started after the slurry SL is discharged onto the uncured surface 13as located on the negative side of the x-axis direction of the modeling table 10 as shown in FIG. 2. In this case, the recoater 31 moves above the first uncured portion 13a in the positive direction of the x-axis so that the blade tip 31L is along the blade tip movement line L. As a result, as shown in FIG. 5, the slurry SL comes into contact with the front surface 31F facing the moving direction of the moving recoater 31, and the slurry SL is swept and spread in a horizontal plane. During this movement, the blade tip 31L applies a shear stress SS to the slurry SL. The shear stress SS at this time is proportional to the viscosity of the slurry SL, which is determined based on the viscoelasticity characteristics as shown in FIG. 3 from the shear speed determined from the height h of the blade tip 31L and the movement speed of the recoater 31.
[0056] The shear stress SS also acts on the first unhardened portion 13a immediately below the applied slurry SL. The first unhardened portion 13a is made of the deposited slurry of the same material as the applied slurry SL. The shear stress SS generated in the slurry SL and the first unhardened portion 13a below the cutting edge 31L is countered by a resistance force resulting from the viscous resistance of the slurry itself and a frictional force that the first unhardened portion 13a receives from the modeling table 10, which is harder than the first unhardened portion 13a immediately below the first unhardened portion 13a. However, since these resistance and frictional forces are weaker than the shear stress, more slurry than necessary may be carried away by the recoater 31 and moved in the positive direction of the x-axis.
[0057] As a result, as shown in FIG. 6, a recess 16 (16a) may be formed in the upper part (positive side in the z-axis direction) of the first uncured portion 13a. For the sake of simplicity, the example of FIG. 5 assumes that the application of the slurry SL is started from the ideal state of FIG. 2. However, in reality, from the time when the second layer of slurry is applied, a difference occurs between the height of the slurry in the cured portion 12 (the distance from the upper surface 10s of the modeling table 10 to the upper surface of the coating film applied on the cured portion 12) and the height of the slurry in the first uncured portion 13a (the distance from the upper surface 10s of the modeling table 10 to the upper surface of the coating film applied on the first uncured portion 13a). This difference increases as the layers are piled up, but tends to be almost constant when a certain number of layers is exceeded. In FIG. 5, the thickness of the first uncured portion 13a is reduced by application, but in reality, the thickness of the first uncured portion 13a tends to increase with each application, although it becomes smaller than the target thickness. The amount of slurry carried away from first unhardened portion 13a tends to decrease toward hardened portion 12.
[0058] FIG. 6 shows a state where the recoater 31 has moved further from the state shown in FIG.
[0059] As shown in FIG. 6, in this situation, the blade tip 31L also applies a shear stress SS to the slurry SL as the recoater 31 moves. However, unlike the case shown in FIG. 5 where the recoater 31 is on the first uncured portion 13a, the hardened portion 12 that has been hardened by exposure is close to the blade tip 31L at a pitch p. In other words, a material that is harder than the applied slurry SL is close to the blade tip 31L. The shear stress in this state is proportional to the viscosity based on the shear rate determined by the distance p from the hardened surface 12s to the recoater 31 and the moving speed of the recoater 31. Since the distance p is much smaller than the height h at the time of recoating on the uncured portion 13a, the shear rate becomes much faster, and the viscosity based on the characteristics of FIG. 3 becomes much lower than that at the time of recoating on the uncured portion 13a. In this case, the hardened portion 12 applies a friction force FF as a corresponding resistance to the shear stress SS by the blade tip 31L. Therefore, the slurry SL applied to the hardened portion 12 is unlikely to be carried away by the recoater 31 due to its low viscosity. Therefore, a slurry film 17 having a thickness approximately equal to the pitch p is formed on the upper surface 12s of the hardened portion 12. In other words, a slurry film 17 having an upper surface 17s at a height approximately equal to the blade tip movement line L is formed.
[0060] FIG. 7 shows a state where the recoater 31 has moved further from the state shown in FIG. 6 and has reached above the second uncured portion 13b.
[0061] In this case, as in the case where the cutting edge 31L moves above the first unhardened portion 13a, the cutting edge 31L applies a shear stress SS to the slurry SL and the second unhardened portion 13b, which may cause more slurry than necessary to be carried away and moved in the positive direction of the x-axis.
[0062] As a result, as shown in FIG. 7, a recess 16 (16b) may be formed in the upper part (positive side in the z-axis direction) of the second unhardened portion 13b. As in the example of FIG. 5, the example of FIG. 7 also assumes that the application of the slurry SL is started from the ideal state of FIG. 2. Therefore, in reality, from the time when the second layer of slurry is applied, a difference occurs between the height of the slurry in the hardened portion 12 and the height of the slurry in the second unhardened portion 13b. This difference also widens as the layers are piled up, but tends to become almost constant after a certain number of layers. In FIG. 7, the thickness of the second unhardened portion 13b is reduced by application, but in reality, the thickness of the second unhardened portion 13b tends to increase with each application, although it becomes smaller than the target thickness. The amount of slurry carried away from the second unhardened portion 13b tends to be less near the hardened portion 12.
[0063] FIG. 8 is a schematic diagram showing the state of the intermediate product 11 shown in FIG. 2 after the application of the slurry has been finally completed through the steps shown in FIGS.
[0064] When performing the operation of applying slurry to the upper surface 11s of the intermediate body 11 in the manner shown in Figure 2, what is originally intended by such operation is to form a slurry film 14 of a thickness approximately equal to the pitch p in a layered manner over the entire intermediate body 11, as shown in Figure 4. However, in reality, as shown in Figure 8, although a slurry film 17 of that thickness is formed on the hardened portion 12, a recess 16 having a height lower than the upper surface 17s of the slurry film 17 is formed on the upper part of the unhardened portion 13.
[0065] Depending on the viscosity of the slurry (the newly applied slurry SL and the deposited slurry 15) and the arrangement of the hardened portion 12, leveling may occur in the unhardened portion 13 after the recoater 31 has passed, reducing the height difference (height difference) between the hardened surface 12s and the unhardened surface 13s; however, for simplicity of explanation, this point will not be taken into consideration hereinafter.
[0066] Depending on the shape of the printing, the uncured portion 13 may not be continuous from the upper surface 10s of the printing table 10 to the upper surface 11s of the printing intermediate body 11 as in Fig. 8, but may exist on a hardened portion that is formed within a certain range from the upper surface 10s of the printing table 10. In such a case, the frictional force that the uncured portion 13 receives from the hardened portion directly below is relatively large compared to the frictional force that the uncured portion receives from the printing table 10 when there is no hardened portion, and therefore there is a tendency for the formation of recesses 16 to be reduced compared to when there is no hardened portion.
[0067] Furthermore, when multiple hardened portions 12 are present discretely in the x-axis direction, the smaller the distance between their hardened surfaces 12s in the x-axis direction, the more likely it is that recesses will be formed in the unhardened portions 13 between the hardened portions 12.
[0068] However, it is exceptional that no recesses are formed in the intermediate body 11 after all the repeated slurry applications in forming the intermediate body 11. That is, the upper surface 11s of the intermediate body 11 after the sweep application of the slurry SL usually has some degree of height difference, and the exposure unit 40 targets the upper surface 11s having such height difference. In this case, a particular problem occurs when the exposure range (hardening target range) set in the exposure pattern for such exposure is above the previously existing hardened portion 12 and is a range for forming a so-called overhang shape that forms a new hardened portion protruding from the hardened portion 12 in the horizontal plane.
[0069] In Fig. 8, a region RE1 wider than the cured portion 12 in the X-axis direction is the exposure range in the exposure pattern intended to form such an overhang shape. Furthermore, Fig. 9 shows the state after the region RE1 is exposed.
[0070] By performing exposure to light in the area RE1 as the exposure range, a new cured portion 18 is formed on the cured portion 12 as shown in Figure 9. The cured portion 18 is composed of a first portion 18a formed on the cured portion 12, and a second portion 18b and a third portion 18c that are continuous with the first portion 18a and extend above the first uncured portion 13a and the second uncured portion 13b.
[0071] The first portion 18a is a portion where the slurry film 17 has hardened, is supported downward by the hardened portion 12, and has a thickness substantially the same as the pitch p when the slurry is applied.
[0072] On the other hand, the second portion 18b and the third portion 18c are portions in which a part of the first uncured portion 13a and a part of the second uncured portion 13b are cured, respectively. In reality, both of them should extend horizontally from the first portion 18a, and the cured portion 18 should be formed into a flat plate having a uniform thickness as a whole. However, in reality, both the second portion 18b and the third portion 18c are continuous with the first portion 18a, but are merely supported downward by the uncured portion 13, which is softer than the cured portion 12 and has a recess 16 at its upper portion. Therefore, as shown in FIG. 9, the shapes of the second portion 18b and the third portion 18c are sagging shapes corresponding to the recess 16 at the upper portion of the uncured portion 13. This means that the cured portion 18 is not shaped in the shape assumed at the time of design.
[0073] Moreover, the formation of recesses in the uncured portions 13 when the slurry is applied, and the sagging of the overhanging portions when an overhanging shape is to be formed by subsequent exposure, as described above, can also occur when the slurry SL is applied to a shaping intermediate 11 in which a recess has already been formed in the upper part of the uncured portion 13, rather than the ideal shaping intermediate 11 shown in Fig. 2. This means that depending on the shape of the object to be created, the height difference between the hardened portion 12 and the uncured portion 13 increases each time the slurry SL is applied, and therefore the shape of the hardened portion 18 formed by exposure after each slurry application gradually deviates from the design, and the shaping accuracy of the finally obtained object may be significantly reduced.
[0074] Furthermore, the formation of recesses in the unhardened portion 13 during application of the slurry is due to the shear stress SS applied to the slurry SL by the blade 31L of the recoater 31 as described above, and such shear stress SS is essential for application of the slurry SL. Therefore, it is considered that the height difference between the hardened portion 12 and the unhardened portion 13 due to the formation of recesses is, in principle, unavoidable.
[0075] <Evaluation of the effect of recoater shape on modeling accuracy> As described above, it is considered that the difference in height between the hardened portion 12 and the unhardened portion 13 in the unhardened portion 13 when the slurry is applied is unavoidable in principle. However, if such a difference in height does not substantially affect the molding accuracy, it is considered that it is permissible in practice.
[0076] In addition, it is considered that the shear stress SS that the blade tip 31L of the recoater 31 applies to the slurry SL depends on the shape (particularly the vicinity of the blade tip) of the recoater 31. It is also considered that by devising such a shape, it is possible to suppress the height difference between the hardened portion 12 and the unhardened portion 13 during application of the slurry to a level that does not substantially affect the molding accuracy.
[0077] Figures 10 to 16 are figures for explaining an evaluation (recoater shape impact evaluation) of the effect of the shape of the recoater 31 on the formation of the height difference between the hardened portions 12 and the unhardened portions 13 in the intermediate product, which was conducted by the inventor in consideration of the above points.
[0078] 10 is a plan view showing an exposure pattern used in the recoater shape influence evaluation. A region RE1 seen in white indicates the exposure range in the exposure pattern. On the other hand, a region RE2 indicates the measurement range for height measurement, which will be described later.
[0079] The region RE1 is composed of two concentric rings with a width of 1.5 mm and a rectangular portion of 40 mm x 25 mm on the outer side. The central portion of the inner ring is a circle with a diameter of 3 mm. The two concentric rings and the rectangular portion on the outer side are spaced apart by 1.5 mm in the radial direction of the concentric rings. Each time the slurry is applied, exposure is performed using the exposure pattern shown in FIG. 10 to form a shaped intermediate body 11 including three columnar cured portions 12 with the two concentric rings and the rectangle as cross sections. The exposure pattern is such that a recess 16 is formed in the uncured portion 13, resulting in a height difference on the upper surface 11s of the shaped intermediate body 11.
[0080] 11 and 12 show the shapes of all 7 types (type A to type G) of recoaters 31 used in the recoater shape influence evaluation, together with the posture (sweep posture) when the recoaters 31 are attached to the recoat unit 30 and sweep-apply the slurry. Each recoater 31 is moved in the positive direction of the x-axis (rightward as viewed in the drawing) by the recoat unit 30 in the sweep posture shown in the drawing when applying the slurry. Although not shown in FIGS. 11 and 12, the recoater 31 is attached to the recoat unit 30 and used while being held by a holder (an example of a sweep member holding means) 32 (see FIG. 22) of the recoat unit 30.
[0081] In each recoater 31, the maximum thickness (blade thickness) is 5 mm, the cutting edge 31L in the sweeping position is a flat surface parallel to the horizontal plane (xy plane), and the front surface 31F facing the direction of sweep coating is an inclined surface continuing from the cutting edge 31L and forming an angle of 60° with the horizontal plane. Note that the recoater 31 has another surface continuing from the cutting edge 31L, the rear surface 31B facing in the opposite direction to the direction of sweep coating.
[0082] The angle that the front surface 31F forms with respect to the horizontal plane when the recoater 31 is in the sweeping position (hereinafter, the front surface inclination angle α) is preferably less than 90° and may be 70° or less. When the front surface inclination angle α is less than 90°, it is considered that not only the weight of the slurry SL but also the force of the front surface 31F is added as the coating pressure acting vertically downward on the slurry SL during coating. Therefore, it is considered that the slurry SL that comes into contact with the front surface 31F during coating is more likely to fall from the front surface 31F, and as a result, it is possible to reduce the occurrence of non-coating due to the recoater 31 slipping upward.
[0083] Moreover, the front surface inclination angle α may be more than 30°, and may be 50° or more. When the front surface inclination angle α is more than 30°, it is considered that the action of shear stress via the slurry SL attached to the front surface 31F can be reduced, and the removal of the slurry SL can be reduced. In addition, it is considered that the application pressure acting vertically downward can be prevented from becoming too large, and therefore the risk of deformation of the intermediate body 11 due to the application pressure can be reduced.
[0084] Therefore, since it is desirable for the front surface inclination angle α to be 30°<α<90°, in all of the seven types of recoaters 31 shown in Figures 11 and 12, the front surface inclination angle α is set to 60°, which is the intermediate value of this angle range.
[0085] In addition, the angle that the rear surface 31B forms with respect to the horizontal plane when the recoater 31 is in the sweeping position (hereinafter, rear surface inclination angle β) may be more than 30° and may be 50° or more. By making the rear surface inclination angle β more than 30°, it is considered that the possibility of the slurry SL being carried away by the rear surface 31B can be reduced. In addition, it is considered that the increase in the coating pressure acting vertically downward by the rear surface 31B can be reduced, and the possibility of the intermediate body 11 being deformed due to the coating pressure can be reduced. In addition, the rear surface inclination angle β may be (180°-α) or less than (180°-α). When the rear surface inclination angle β is less than (180°-α), the thickness of the recoater 31 can be increased as it moves away from the cutting edge 31L, and the strength of the recoater 31 can be improved.
[0086] These seven types of recoaters 31 have in common that the cutting edge 31L in the sweeping state is flat, but there are various differences in the combination of the thickness of the cutting edge 31L in the x-axis direction (hereinafter referred to as cutting edge thickness) and the angle that the rear surface 31B makes with the horizontal plane (hereinafter referred to as rear surface inclination angle).
[0087] The type A recoater 31 has a blade tip thickness of 5.77 mm and a rear inclination angle of 120°.
[0088] The type B recoater 31 has a blade tip thickness of 2 mm and a rear inclination angle of 90°.
[0089] The type C recoater 31 has a blade tip thickness of 2 mm and a rear inclination angle of 60°.
[0090] The type D recoater 31 has a blade tip thickness of 2 mm and a rear inclination angle of 120°.
[0091] The type E recoater 31 has a blade tip thickness of 0.9 mm and a rear inclination angle of 60°.
[0092] The type F recoater 31 has a blade tip thickness of 0.5 mm and a rear inclination angle of 60°.
[0093] The type G recoater 31 has a blade tip thickness of 0.2 mm and a rear inclination angle of 90°.
[0094] The slurry SL used for modeling had viscoelastic properties, as shown in Figure 3, with a viscosity of 50 Pa·s or less when the shear rate was 1 / s or more. The coating speed was 2 mm / s, and the coating pitch p, which corresponds to the target thickness of the slurry film, was 100 μm. In other words, the shear rate during coating was 20 / s. Modeling was performed at room temperature. The lamination of the slurry film by coating the slurry under these conditions and the subsequent exposure were repeated up to 50 times, with some exceptions.
[0095] Fig. 13 is a captured image of the top surface of the intermediate body 11 produced by using the type C recoater 31 to apply the slurry SL after the 50th exposure. It can be seen that the height difference corresponding to the exposure pattern shown in Fig. 10 has been formed.
[0096] In order to understand the change in such height difference during the modeling process, the height of the upper surface of the modeling intermediate body 11 after exposure (also called the coated surface height) was measured at multiple measurement points within the region RE2 shown in Fig. 10 for every 5th or 10th layer while the stacking of the slurry film and exposure were repeated under the above-mentioned conditions. A laser displacement meter was used for the measurements.
[0097] Specifically, the measurement points were 26 points each at 2 mm pitch in both the x-axis and y-axis directions, for a total of 26 x 26 = 576 points. Also, the number of measurement points on the hardened surface 12s corresponding to the region RE1 in Fig. 10 was the same as the number of measurement points on the unhardened surface 13s corresponding to the region RE2 excluding the region RE1.
[0098] A histogram of the measurement points in 10 μm intervals was then created from the height measurements obtained at all 576 points.
[0099] Fig. 14 is a histogram showing the results of height measurement after forming 50 layers when a type C recoater 31 is used, while Fig. 15 is a histogram showing the results of height measurement after forming 50 layers when a type G recoater 31 is used.
[0100] Two peaks appear in these histograms. Although not shown in the drawings, the two peaks also appear in all histograms created in a similar manner. Considering the formation mode of the recesses 16 described with reference to Figures 4 to 9, the difference value of the measurement values corresponding to the two peaks appearing in each histogram can be considered to correspond to a representative height difference between the cured surface 12s and the uncured surface 13s on the upper surface 11s of the intermediate body 11.
[0101] For example, the histogram shown in FIG. 14 shows that when a type C recoater 31 is used, a height difference of about 240 μm occurs between the cured surface 12s and the uncured surface 13s, which is larger than the target thickness of 100 μm.
[0102] On the other hand, the histogram shown in FIG. 15 shows that when a type G recoater 31 is used, the height difference between the cured surface 12s and the uncured surface 13s remains at about 50 μm, which is smaller than the target thickness of 100 μm.
[0103] Since the interval is set to 10 μm, the value of the height difference obtained based on the peak position of each histogram may include an error of up to 20 μm, but this does not pose any particular problem in terms of grasping the trend of the height difference. Of course, it is also possible to create a histogram by setting an even smaller interval.
[0104] 16 is a graph showing the change in height difference between the cured surface 12s and the uncured surface 13s versus the number of layers when using each of the seven types of recoaters 31. Note that the type C recoater 31 and the type F recoater 31 were measured twice.
[0105] FIG. 16 shows that the smaller the cutting edge thickness, the smaller the difference in height between the hardened surface 12s and the unhardened surface 13s tends to be, and furthermore, when the cutting edge thickness is the same, the difference in the rear surface inclination angle does not affect the magnitude of the difference in height.
[0106] Furthermore, when a type E recoater 31 with a cutting edge thickness of 0.9 mm or less is used, it is confirmed that the height difference is suppressed to 150 μm or less, which is relatively close to the target thickness. In particular, when a type F or type G recoater 31 with a cutting edge thickness of 0.5 mm or less is used, it is confirmed that the height difference is suppressed to approximately the same as or less than the target thickness of 100 μm. In particular, when a type G recoater 31 with a cutting edge thickness of 0.2 mm is used, the height difference is suppressed to about 50 μm when 30 or more layers are laminated.
[0107] <Recoater shape> Next, a desirable shape of the recoater 31 will be described based on the results of the recoater shape effect evaluation shown in FIG.
[0108] As described above, the smaller the blade thickness, the smaller the height difference between the hardened surface 12s and the unhardened surface 13s tends to be. When the blade thickness is 0.9 mm or less, the height difference can be suppressed to near the target thickness of the slurry film, while there is no dependency on the rear surface inclination angle. This means that the height difference between the hardened surface 12s and the unhardened surface 13s can be suppressed by making the blade thickness of the recoater 31 as small as possible. That is, the blade thickness may be 0.9 mm or less. The blade thickness may also be 0.5 mm or less, and is preferably 0.2 mm or less. In this case, the height difference between the hardened surface 12s and the unhardened surface 13s is suppressed to the same level as the target thickness or less.
[0109] The thickness of the cutting edge may be 0.1 mm or more. By making the thickness of the cutting edge 0.1 mm or more, chipping of the cutting edge can be reduced.
[0110] In addition, in all of the recoaters 31 of types A to G illustrated in Fig. 11 and Fig. 12, the cutting edge 31L is parallel to the horizontal plane, but depending on the mounting accuracy, the recoater 31 may be mounted on the recoat unit 30 with the cutting edge 31L not parallel to the horizontal plane. Fig. 21 is a diagram showing the recoater 31 in a sweeping position with a larger front inclination angle α than when the cutting edge 31L is parallel to the horizontal plane.
[0111] 21, when the bottom end of the front surface 31A is higher than the bottom end of the rear surface 31B, the distance in the x-axis direction between the front surface 31A and the rear surface 31B at the bottom end of the front surface 31A is the cutting edge thickness. On the other hand, when the bottom end of the rear surface 31B is higher than the bottom end of the front surface 31A by being attached to the recoating unit 30 in a sweeping position in which the front surface inclination angle α is small, the distance in the x-axis direction between the front surface 31A and the rear surface 31B at the bottom end of the rear surface 31B is the cutting edge thickness.
[0112] That is, the distance 31T in the x-axis direction between the lowermost end of the front surface 31A or the lowermost end of the rear surface 31B, whichever is higher, is the cutting edge thickness.
[0113] However, there is a limit to the precision of machining in intentionally making the cutting edge 31L thin. For example, in the case of a stainless steel recoater 31, it is not necessarily easy to accurately achieve a cutting edge thickness of less than 0.2 mm.
[0114] On the other hand, even if the cutting edge 31L of the recoater 31 in the sweeping position is actually flat and the cutting edge thickness is 0.9 mm or less, from a macroscopic perspective, it may be perceived as simply having a horizontal thickness that decreases toward the lowest cutting edge, and the lowest end of the front surface 31F and the lowest end of the rear surface 31B being in contact with each other.
[0115] Even if it is viewed in this way, if the horizontal thickness of the recoater 31 within a range below a certain height is 0.9 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less, the horizontal thickness at the bottom end of the recoater 31 should be 0.9 mm or less, 0.5 mm or less, or 0.2 mm or less, regardless of whether or not a flat surface exists, and even if there is no need to specifically specify the thickness of the flat surface.
[0116] In other words, when the recoater 31 in the sweeping position becomes thinner at least near the bottom end toward the bottom end, the thickness of the recoater 31 in the x-axis direction at the bottom end of the recoater 31 or within a predetermined range in the vertical direction from the bottom end should be 0.9 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less. The types E, F and G of recoaters 31 shown in Fig. 12 also satisfy this requirement.
[0117] When using such a recoater 31, it is possible to obtain a shaped intermediate body 11 in which the height difference between the hardened surface 12s and the unhardened surface 13s on the upper surface is suppressed to a level that is permissible in light of the shaping accuracy of the shaped object, simply by setting the pitch p, which is the distance between the shaping table 10 or the shaped intermediate body 11 and the lowest end, according to the target thickness. As a result, the shaping accuracy of the shaped object is improved.
[0118] This also applies to the case where the recoater 31 in the sweeping position has a uniform horizontal thickness at least in a predetermined range in the vertical direction from the bottom end, because in this case, if the range is uniform within a thickness of 0.9 mm or less, 0.5 mm or less, or 0.2 mm or less in the horizontal direction, the horizontal thickness of the bottom end will naturally be the same.
[0119] In view of the above, in this embodiment, when the recoater 31 is in the sweeping position, at least the vicinity of its lowest end is set so that the thickness in the x-axis direction decreases or remains constant toward the lowest end, and the thickness in the x-axis direction at the lowest end or within a predetermined range in the vertical direction from the lowest end is set to 0.9 mm or less, more preferably 0.5 mm or less, and even more preferably 0.2 mm or less. In this embodiment, such requirements are referred to as recoater shape requirements.
[0120] When modeling is performed using a photo-lithography apparatus 1 in which the recoater 31 satisfies the recoater shape requirements, the height difference between the cured surface 12s and the uncured surface 13s on the upper surface 11s of the intermediate body 11 can be reduced to an acceptable range in light of the modeling accuracy.
[0121] The above-mentioned type F and type G recoaters 31 satisfy the recoater shape requirements. However, recoaters 31 that satisfy the recoater shape requirements are not limited to these.
[0122] Figure 17 shows examples of main shapes of the recoater 31 that are different from type F and type G. Figure 17(a) is a schematic cross-sectional view of the recoater 31 when it is in the sweeping position.
[0123] 17(a), a front surface 31F that spreads the slurry in the positive direction of the x-axis when applying the slurry forms an angle α of 30°<α<90° with the horizontal plane. A rear surface 31B on the opposite side in the x-axis direction to the front surface 31F forms an angle β of 30°<β<180°-α with the horizontal plane. Here, the requirement of β<180°-α indicates that the thickness of at least the portion near the bottom end of the recoater 31 becomes smaller toward the bottom end.
[0124] However, in Fig. 17(a), the front surface 31F and the rear surface 31B are shown to form an angle at the bottom end 31E of the recoater 31, but this is merely a schematic (macro) illustration, and the actual shape of the vicinity of the bottom end 31E can take various forms while satisfying the above-mentioned recoater shape conditions. Figs. 17(b) to (e) show more detailed shape examples of the vicinity area A of the bottom end 31E of such a recoater 31.
[0125] 17(b) shows an embodiment in which the bottom end 31E of the recoater 31 has a flat cutting edge, and the cutting edge thickness, which is the length of the bottom end 31E in the x-axis direction, is 0.5 mm. The shape of the recoater 31 near the bottom end is similar to that of the type G recoater 31.
[0126] On the other hand, Fig. 17(c) shows an embodiment in which the portion with a length of 0.5 mm in the x-axis direction is located above the lowest end 31E of the recoater 31, and the lowest end 31E has a flat cutting edge. In this case, the cutting edge thickness at the lowest end 31E is smaller than 0.5 mm. This corresponds to the embodiment in Fig. 17(b) in which the cutting edge thickness of the recoater 31 is smaller than 0.5 mm.
[0127] Also, FIG. 17(d) shows an embodiment in which the length in the x-axis direction is 0.5 mm, the cutting edge is not flat but has a corner pointing vertically downward, and the bottom end 31E of the recoater 31 is located lower than the bottom ends of the front surface 31F and rear surface 31B.
[0128] Also, as shown in Figure 17(e), the length in the x-axis direction is 0.5 mm, but the cutting edge is not flat but has a curved surface that is convex vertically downward, and the bottom end 31E of the recoater 31 is located at a lower position than the bottom ends of the front surface 31F and rear surface 31B.
[0129] For example, even if the recoater 31 is machined to have a flat cutting edge with a cutting edge thickness of less than 0.5 mm as shown in Fig. 17(c), due to the limit of machining accuracy, the shape may actually be as shown in Fig. 17(d) or 17(e). Even in such a case, if the position of the lowest end 31E with respect to the intermediate body 11 during slurry application satisfies a predetermined pitch p, it is possible to perform slurry application with a small height difference between the hardened surface 12s and the unhardened surface 13s, as in the case of using the recoater 31 with the shape shown in Fig. 17(b) or 17(c). Also, the cutting edge may have a depression that is recessed vertically upward, contrary to Fig. 17(d) or 17(e).
[0130] The recoater 31 shown in FIG. 17(a) has a through hole 31h at its upper portion that can be used for attachment to the recoat unit 30, and also has a step 31s at the upper portion of the front surface 31F, but these provisions are not essential.
[0131] FIG. 18 is a diagram showing a further example of a different shape of the recoater 31 that is not based on the macroscopic configuration shown in FIG. 17(a).
[0132] Fig. 18(a) shows an example in which the bottom end 31E of the recoater 31 has a flat cutting edge, the cutting edge thickness, which is the length of the bottom end 31E in the x-axis direction, is 0.5 mm, and β=α>30°. The cutting edge thickness may be greater than 0.5 mm and equal to or less than 0.9 mm, or may be less than 0.5 mm. In addition, this recoater 31 may have a shape in the vicinity of the bottom end 31E shown in Fig. 17(d) or Fig. 17(e) combined.
[0133] Fig. 18(b) shows an example in which the bottom end 31E of the recoater 31 has a flat cutting edge, the cutting edge thickness, which is the length of the bottom end 31E in the x-axis direction, is 0.5 mm, and α<β<90°. The cutting edge thickness may be greater than 0.5 mm and less than 0.9 mm, or may be less than 0.5 mm. In addition, this recoater 31 may have a shape in the vicinity of the bottom end 31E shown in Fig. 17(d) or 17(e).
[0134] Fig. 18(c) shows an example in which the bottom end 31E of the recoater 31 has a flat cutting edge, the cutting edge thickness, which is the length of the bottom end 31E in the x-axis direction, is 0.5 mm, and β=180°-α, so that the recoater 31 as a whole has a uniform thickness while being inclined at least near the bottom end 31E. In this recoater 31, the cutting edge thickness may be greater than 0.5 mm and equal to or less than 0.9 mm, or may be less than 0.5 mm. In addition, this recoater 31 may have a shape in which the shape in the vicinity of the bottom end 31E shown in Fig. 17(d) or Fig. 17(e) is combined.
[0135] Fig. 18(d) shows an example in which the bottom end 31E of the recoater 31 has a flat cutting edge, the cutting edge thickness, which is the length of the bottom end 31E in the x-axis direction, is 0.5 mm, and 90°<β<180°-α. The cutting edge thickness may be smaller than 0.5 mm. In addition, this recoater 31 may have a shape in the vicinity of the bottom end 31E shown in Fig. 17(d) or Fig. 17(e).
[0136] Even when using a recoater 31 having the shape illustrated in FIGS. 18(a) to (d), it is possible to apply slurry with a small difference in height between the hardened surface 12s and the unhardened surface 13s.
[0137] <Modeling example> 19 and 20 are diagrams showing the influence of differences in the shape of the recoater 31 on the formation of an object having an overhang.
[0138] The objects shown in Figures 19(a) and 20(a) were both produced using a recoater 31 with a flat cutting edge 31L at the lowest end 31E and a cutting edge thickness of 2 mm. Such a recoater 31 does not satisfy the above-mentioned recoater shape conditions. In the objects shown in Figures 19(a) and 20(a), overhang sagging is observed at the locations indicated by arrows AR3 and AR4.
[0139] More specifically, in the object shown in Fig. 19(a), sagging occurs in the overhang that protrudes in the left-right direction as viewed in the drawing, whereas in the object shown in Fig. 20(a), sagging occurs in the overhang that protrudes in the direction perpendicular to the drawing.
[0140] In contrast, the object shown in Figures 19(b) and 20(b) was obtained by applying the same printing conditions as those used to print the object shown in Figures 19(a) and 20(a), except that a recoater 31 was used that had a blade tip 31L with a flat surface at its bottom end 31E and a blade tip thickness of 0.2 mm, which satisfied the recoater shape conditions.
[0141] In the objects shown in Figs. 19(b) and 20(b), the sagging of the overhangs as seen in Figs. 19(a) and 20(a) is suppressed.
[0142] The results show that sagging of the overhang is suppressed by performing modeling so as to satisfy the recoater shape conditions. This is because modeling using the recoater 31 that satisfies the recoater shape conditions reduces the height difference between the hardened surface 12s and the unhardened surface 13s caused by the formation of a recess on the upper surface (unhardened surface) 13s of the unhardened portion 13 of the modeling intermediate body 11 to an allowable range in light of modeling accuracy.
[0143] <Second embodiment> In the first embodiment described above, modeling is performed at room temperature. However, when the temperature of the slurry used in stereolithography is increased, the viscosity decreases, and the ease and uniformity of application improves.
[0144] For example, the optical molding apparatus disclosed in Patent Document 4 adjusts the temperature of the slurry by a temperature adjusting member attached to a dispenser (discharging means) corresponding to the discharging unit 20.
[0145] If the slurry is heated in this manner and discharged from the dispenser, when the discharged slurry adheres to the modeling table or the coating film already formed thereon, heat is diffused from the slurry to the modeling table and the coating film, and the temperature of the slurry drops below that before it was discharged. During the subsequent sweep coating by the recoater, the recoater in contact with the slurry also absorbs heat, so the temperature of the slurry drops even more rapidly. As the temperature drops, the viscosity of the slurry increases, so that during the sweep coating by the recoater, a slurry with a higher viscosity than that before it was discharged is ultimately applied.
[0146] In this embodiment, taking the above points into consideration, a configuration (a heating means during sweeping) capable of heating (or warming) the swept slurry only during the sweeping coating by the recoater, which directly affects the uniformity of the coating film, is added to the optical molding apparatus 1 according to the first embodiment, thereby further reducing the height difference occurring in the coating film formed on the modeling surface. Furthermore, with this configuration, the viscosity of the slurry during sweeping coating can be reduced without heating the slurry held in the discharge means 20, so that damage to the slurry that may occur when heated for a long time can also be reduced.
[0147] Fig. 22 is a diagram illustrating such a heating means during sweeping. Fig. 22(b) shows a recoater 31 heated by a heater 33 as one aspect of the heating means during sweeping, and Fig. 22(a) shows a recoater 31 according to the first embodiment that is not heated by the heating means during sweeping, for comparison. The heater 33 is provided, for example, so as to be in contact with the recoater 31. As the recoater 31, the type G recoater 31 shown in Fig. 12 is used as an example.
[0148] Although specific examples were omitted in the first embodiment, regardless of which of the various shapes of recoater 31 is used as shown in Figures 17 and 18, the recoater 31 is attached to the recoat unit 30 while being held by the holder 32 of the recoat unit 30 and then used.
[0149] 22(a) illustrates an example in which the recoater 31 is attached to the recoat unit 30 while being held by a pair of holders 32a, 32b and used. In this case, the pair of holders 32a, 32b are preferably provided along the extension direction of the recoater 31 (the direction perpendicular to the drawing in FIG. 22) with a length equal to that of the recoater 31. However, the actual shapes and attachment manners of the holders 32a, 32b vary depending on the actual shape of the recoater 31, and what is shown in FIG. 22 is merely a schematic example.
[0150] 17(a), in the case where the recoater 31 has a through hole 31h that can be used for attachment to the recoat unit 30, the through hole 31h may be used for holding by the holder 32. Alternatively, the recoater 31 may be held by being sandwiched between the main body of the recoat unit 30 and a long plate member that serves as the other side of the holder 32.
[0151] 22(b) illustrates an example in which heaters 33 (33a, 33b) as one mode of heating means during sweeping are fitted (embedded) in recesses provided on the contact surfaces of the pair of holders 32a, 32b that hold the recoater 31 in the mode shown in Fig. 22(a) with the recoater 31. In this case, the heaters 33 are provided over substantially the entire range in the extension direction of the recoater 31. In addition, when the heater 33 is provided, the holder 32 is made of a highly insulating material that is less thermally deformed at least in the range of the heating temperature of the heater 33.
[0152] Examples of the heater 33 include an electric heating wire heater such as a silicon belt heater, and an electric heater such as a strip-shaped lamp heater. The heater 33 generates heat when electricity is applied from a heater power source (not shown), so that the recoater 31 in contact with the heater 33 is heated uniformly without temperature variation depending on the location (especially in the extension direction).
[0153] In this embodiment, under the control of the control circuit, the recoater 31 is heated by a sweep heating means such as the heater 33, while sweep coating of slurry for modeling is performed in the same manner as in the first embodiment.
[0154] 1 and 2, the sweep coating is similar to that of the first embodiment in that a coating film is formed by sweeping the slurry SL discharged from the discharge unit 20 by the recoater 31. However, this embodiment differs from the first embodiment in that the recoater 31 is heated, and therefore the slurry SL is swept while being heated mainly by heat transfer from the recoater 31.
[0155] Fig. 23 is a graph showing the change in height difference between the cured surface 12s and the uncured surface 13s versus the number of layers when a type G recoater 31 is used, and a slurry film is laminated and then exposed to light under the same conditions as in the recoater shape evaluation in the first embodiment, both when the recoater is heated to 44°C by the heater 33 and when the recoater is not heated. The height difference between the two is determined using histograms such as those shown in Figs. 13 and 14, as in the first embodiment. The results when the recoater is not heated are the same as those shown in Fig. 16.
[0156] However, when modeling is performed while the recoater 31 is heated, the height difference when the number of layers is 50 cannot be identified in the histogram, unlike the cases shown in Figures 14 and 15, and is therefore set to 0. In reality, although there may be some height difference between the two, since two clear peaks corresponding to the two do not appear, the value is considered to be at least smaller than the height difference in the non-heated case where two peaks are identified as shown in Figure 15.
[0157] 23, including this point, it can be seen that the height difference between the hardened surface 12s and the unhardened surface 13s tends to be smaller when the recoater 31 is heated than when it is not heated. This is thought to be due to the effect that the viscosity of the slurry SL decreases with the increase in temperature due to heat transfer from the recoater 31, improving the smoothness during application.
[0158] More specifically, the slurry SL is heated only for a short period of time when it comes into contact with and comes close to the moving recoater 31, but the amount of the slurry SL discharged from the discharge unit 20 for one sweep coating is small compared to the amount of slurry held in the discharge unit 20, and the amount of the slurry SL that momentarily comes into contact with and comes close to the moving recoater 31 is estimated to be at most 5 cc to 10 cc. Naturally, since its heat capacity is sufficiently small, it is considered that the viscosity of the slurry SL will be sufficiently reduced to a level suitable for sweep coating even during the momentary contact and closeness while being swept by the recoater 31.
[0159] Moreover, since the recoater 31 moves away from the coating film each time a single sweep coating is completed, there is no risk of the coating film losing its shape due to low viscosity, and furthermore, the formed coating film is not damaged due to exposure to heat for a long period of time.
[0160] In other words, the embodiment in which sweep coating is performed while heating the recoater 31 is an embodiment in which the viscosity of the slurry SL can be temporarily reduced as desired only during sweep coating, when a low viscosity is preferable.
[0161] The heating temperature of the recoater 31 is preferably about 40°C to 50°C. In this case, the viscosity of the slurry can be suitably reduced so that the sweep coating can be suitably performed without causing separation of the slurry, and the portions other than the recoater 31 are not excessively heated. By setting the heating temperature of the recoater 31 to 50°C or less, the sweep coating can be suitably performed without causing problems such as separation of the slurry or an excessive decrease in viscosity, and the portions other than the recoater 31 can be prevented from being excessively heated. On the other hand, by setting the heating temperature of the recoater 31 to 40°C or more, the effect of reducing the viscosity of the slurry SL by heating can be suitably obtained.
[0162] 22(b), the heater 33 (33a, 33b) is fitted into the recesses of the pair of holders 32a, 32b, but this is not essential, and the heater 33 (33a, 33b) may be sandwiched and fixed between the pair of holders 32a, 32b and the recoater 31 facing them. In this case, the respective sandwiching surfaces of the pair of holders 32a, 32b and the recoater 31 may be flat, or at least one of the sandwiching surfaces may be a recess or a curved surface.
[0163] In addition, in FIG. 22(b), the heaters 33 (33a, 33b) are provided on both of the pair of holders 32a, 32b, respectively, but an embodiment in which the heater 33 is provided on only one of the pair of holders 32a, 32b may also be used.
[0164] Alternatively, a configuration may be adopted in which the heater 33 is embedded inside the holder 32 and does not come into direct contact with the recoater 31, or a configuration in which the heater 33 having adhesive (sticky) properties is affixed to the holder 32 that holds the recoater 31, or directly to the recoater 31.
[0165] Furthermore, the heating means during sweeping is not limited to the heater 33, and any means that can directly or indirectly heat the slurry SL that comes into contact with the recoater 31 moving for sweep coating uniformly throughout the entire extension direction of the recoater 31 can be used as the heating means during sweeping.
Claims
1. A photolithography apparatus for obtaining a three-dimensional object, comprising: A modeling table and a discharge means for discharging a slurry having thixotropy onto the modeling table; A sweep member; a sweeping means for sweeping and applying the slurry discharged onto the modeling table by horizontally moving the sweeping member in a predetermined sweeping position to form a slurry film; an exposure means for exposing a predetermined area of the slurry film according to an exposure pattern that is created in advance based on three-dimensional shape data; Equipped with The sweep member in the sweeping position has a front surface facing in a direction of travel of the sweep coating and a rear surface facing in a direction opposite to the direction of travel, The angle α that the front surface forms with respect to the horizontal plane satisfies 30°<α<90°, At least near the bottom end of the sweep member, the distance between the front surface and the rear surface in the direction of travel is uniform or decreases toward the bottom end of the sweep member; and At the lowest end of the front surface or the lowest end of the rear surface, the distance between the front surface and the rear surface in the traveling direction is 0.9 mm or less. Stereolithographic device.
2. The optical shaping apparatus according to claim 1 , The sweeping means sweeps the slurry at a shear rate at which a shear stress is applied to the slurry such that the viscosity of the slurry is 1 Pa·s or more and 50 Pa·s or less. Stereolithographic device.
3. The optical shaping apparatus according to claim 1 or 2, The angle β that the rear surface forms with respect to the horizontal plane satisfies 30°<β<(180°-α); Stereolithographic device.
4. The optical shaping apparatus according to claim 1 or 2, a during-sweep heating means for heating the slurry being swept by the movement of the sweep member; The optical shaping apparatus further comprises:
5. The optical shaping apparatus according to claim 4, the heating means during sweeping is a heater for heating the sweeping member, and while the sweeping member heated by the heater moves to sweep the slurry, the sweeping member heats the slurry; Stereolithographic device.
6. The optical shaping apparatus according to claim 5 , The sweep means includes a sweep member holding means for holding the sweep member, the heater is attached to the sweep member holding means; Stereolithographic device.
7. A method for manufacturing a three-dimensional object, comprising the steps of: A step of discharging a thixotropic slurry onto a modeling table; a sweeping step of sweeping the slurry discharged onto the modeling table by horizontally moving a sweeping member in a predetermined sweeping position to form a slurry film; an exposure step of exposing a predetermined area of the slurry film according to an exposure pattern that is created in advance based on three-dimensional shape data; Equipped with In the sweeping step, the sweep member has a front surface facing the direction of travel of the sweep coating and a rear surface facing the opposite direction to the direction of travel, the angle α that the front surface forms with respect to a horizontal plane satisfies 30°<α<90°, and at least near the lowest end of the sweep member, the distance between the front surface and the rear surface in the direction of travel is uniform or becomes smaller toward the lowest end of the sweep member, and At the lowest end of the front surface or the lowest end of the rear surface, a distance between the front surface and the rear surface in the traveling direction is 0.9 mm or less. After the sweeping position of the sweeping member is determined, the slurry is applied. A method for manufacturing a three-dimensional object.
8. The method for producing a three-dimensional object according to claim 7, In the sweeping step, the slurry being swept by the movement of the sweep member is heated. A method for manufacturing a three-dimensional object.
Citation Information
Patent Citations
Scraper comprising zirconia sintered material
JP2006035162A
Method and apparatus for layer thickness control in additive manufacturing
US20200262150A1
A recoating device and method for applying a layer of build material capable of solidification on a working surface
US20210362413A1
Stereolithography device
WO2023058309A1
Manufacture of molecular chain wire