Paint stripping composition for buildings or structures
A low-benzyl alcohol paint stripping composition using a specific compound and ester solvent addresses health risks and temperature stability issues, ensuring safe and efficient paint removal.
Patent Information
- Application Number
- JP2021018869
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-09
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2041-02-09
AI Technical Summary
Existing paint stripping compositions containing benzyl alcohol pose health risks due to poisoning and require special equipment for safe use, and they lack sufficient stripping performance and stability in low-temperature environments.
A paint stripping composition with a low benzyl alcohol content, utilizing a compound of the form R 1 -(OCH(R 2 )-CH(R 3 )) n -OH, combined with an ester solvent, to enhance stripping performance and maintain stability in low temperatures.
The composition suppresses benzyl alcohol poisoning, allows safe spraying without special equipment, and maintains effective peeling performance even in low-temperature conditions.
Smart Images

Figure 0007591815000001 
Figure 0007591815000002 
Figure 0007591815000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating stripping composition for buildings or structures which contains a small amount of benzyl alcohol, has excellent stripping performance, and is stable in properties even in low temperature environments. [Background technology]
[0002] Usually, the surfaces of buildings and structures such as bridges are painted to provide various functions, such as surface protection, strength maintenance, and aesthetic improvement. When the coating film formed on the buildings and structures deteriorates over time due to the effects of ultraviolet rays, the above functions are reduced. Therefore, it is necessary to periodically peel off the deteriorated coating film and repaint it.
[0003] Known methods for removing coatings formed on buildings and structures include physical methods, such as using tools such as disc grinders, electric wire brushes, or wire brushes to remove the coating, or spraying and impacting abrasives to remove the coating. However, with physical methods, some of the coating is dispersed as fine dust-like coating fragments. If workers inhale these fine coating fragments, they may cause serious health problems. This health problem is particularly serious when removing coatings that contain harmful substances such as asbestos.
[0004] In order to solve the problem of scattering of the coating film, a method using a coating film stripping composition is known. By applying the coating film stripping composition to soften and swell the coating film, the coating film can be physically stripped using a stripping tool such as a scraper. This method can suppress the generation of fine dust-like coating film pieces. Generally, a coating film stripping composition contains a solvent for softening and swelling the coating film. For example, Patent Document 1 discloses a resin remover containing ethylene glycol monoalkyl ether and an inorganic acid or an organic acid. Patent Document 2 describes a coating film stripper containing γ-butyrolactone, N-methyl-2-pyrrolidone, and bentonite.
[0005] Currently, many coating film stripping compositions containing benzyl alcohol are commercially available. For example, Patent Document 3 discloses a coating film stripping agent containing an alcohol-based solvent, water, and a rheology control agent, and exemplifies the alcohol-based solvent with benzyl alcohol. Patent Document 4 discloses a coating film stripping composition containing a solvent and a fatty acid ester, and exemplifies the solvent with an aromatic hydroxy compound such as benzyl alcohol. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 9-59546 [Patent Document 2] JP 2013-18887 A [Patent Document 3] JP 2019-131651 A [Patent Document 4] JP 2014-177599 A Summary of the Invention [Problem to be solved by the invention]
[0007] In recent years, there have been many poisoning accidents caused by the use of coating film stripping compositions containing benzyl alcohol. A notice from the Ministry of Health, Labor and Welfare, Labor Standards Bureau, Safety and Health Department (partially revised on August 17, 2020, Kianka-hatsu No. 1019, October 19, 2020) introduces that workers who use gas masks have also experienced poisoning symptoms when spraying stripping compositions containing benzyl alcohol. Therefore, the notice advises that workers should use air-supplied masks for the time being. However, the use of air-supplied masks reduces the efficiency of spraying work. On the other hand, Patent Document 4 points out that stripping compositions containing dibasic acid esters and stripping compositions containing ethylene glycol monoalkyl ethers do not have sufficient stripping action. Therefore, there has been a demand for the development of a coating film stripping composition with a low content of benzyl alcohol and excellent stripping performance.
[0008] In addition, the work of removing coatings from buildings and structures is usually carried out outdoors. Therefore, coating stripping compositions are sometimes used outdoors in winter. Therefore, coating stripping compositions are required to have stable properties even in low temperature environments, particularly below freezing. For example, the stripping composition is required to maintain fluidity without solidifying even in low temperature environments.
[0009] An object of the present invention is to provide a coating stripping composition for buildings or structures which contains a small amount of benzyl alcohol, has excellent stripping performance, and is stable in properties even in low temperature environments. [Means for solving the problem]
[0010] The coating stripping composition for buildings or structures of the present invention contains a compound of formula (1) (hereinafter referred to as "compound (1)") and an ester solvent, and has a benzyl alcohol content of less than 1% by weight: R1-(OCH(R2)-CH(R3)) n -OH (1)
[0011] In formula (1), R1 is C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 R2 and R3 are each independently hydrogen, C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 is an aryl group; and n is an integer of 1 or greater. Effect of the Invention
[0012] The composition of the present invention has a low content of benzyl alcohol, so that poisoning caused by benzyl alcohol can be suppressed, and the work can be performed without using special equipment such as an air supply mask when spraying. In addition, the composition of the present invention has excellent stripping performance compared to a composition containing benzyl alcohol. Furthermore, the composition of the present invention has stable properties even in a low temperature environment, so that it can be suitably used for coating film stripping work outdoors in winter. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] A coating stripping composition for buildings or structures according to one embodiment of the present invention (hereinafter simply referred to as "the composition") contains compound (1) and an ester solvent, and has a benzyl alcohol content of less than 1% by weight. R1-(OCH(R2)-CH(R3)) n -OH (1)
[0014] As mentioned above, Patent Document 4 points out that the stripping action of a stripping composition containing ethylene glycol monoalkyl ether is insufficient. Patent Document 1 also discloses that ethylene glycol monoalkyl ether, propylene glycol alkyl ether, and the like are not effective when used alone. Furthermore, as disclosed in Patent Document 4, propylene glycol alkyl ether is only known as a component of a dip-type coating film stripper, and its stripping performance against architectural coating films, particularly architectural coating films (finishing coating materials) made of acrylic resin, was not known. In contrast, it has been newly discovered that the present composition has a completely unexpected effect of being superior in stripping performance to the case of using benzyl alcohol by using compound (1).
[0015] The composition contains compound (1). Compound (1) may be used alone or in combination of two or more kinds.
[0016] In formula (1), R1 is C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 The C is an aryl group. 1-20 Alkyl group, C 2-20 Alkenyl and alkynyl groups, and C 5-20 The upper and lower limits of the number of carbon atoms in the aryl group can be any integer within the above range. 5-20 An aryl group, more preferably C 5-12An aryl group is preferable, and a phenyl group is more preferable. 5-20 The aryl group may have other substituents on the ring, or may be unsubstituted. For example, R1 may be a substituted phenyl group or an unsubstituted phenyl group.
[0017] In formula (1), R2 and R3 are each independently hydrogen, C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 It is an aryl group. 1-20 Alkyl group, C 2-20 Alkenyl and alkynyl groups, and C 5-20 The above explanation applies to the aryl group. R2 and R3 may be the same group or atom, or may be different groups or atoms. For example, one of R2 and R3 is a hydrogen atom and the other is a C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 Alternatively, R2 and R3 may both be hydrogen atoms, or both may be C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 It may be an aryl group.
[0018] Preferably, one of R2 and R3 is a hydrogen atom and the other is C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 More preferably, one of R2 and R3 is a hydrogen atom and the other is a C 1-20 Alkyl group, C 1-10 Alkyl group, C 1-5 Alkyl group or C 1-3 It is an alkyl group.
[0019] In formula (1), n is an integer of 1 or more. The upper and lower limits of n can be appropriately selected as integers of 1 or more as necessary. Preferably, n is an integer of 1 to 100, more preferably, n is an integer of 1 to 50, even more preferably, n is an integer of 1 to 10, and particularly preferably, n is an integer of 1 to 5.
[0020] Regarding the combination of R1 to R3 and n, any combination described above can be specifically selected. 5-20 An aryl group, one of R2 and R3 is a hydrogen atom, and the other is C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 An example of the compound is an aryl group, and n is an integer of 1 to 100. More preferably, R1 is C 5-12 An aryl group, one of R2 and R3 is a hydrogen atom, and the other is C 1-10 and n is an integer of 1 to 10. More preferably, R1 is a substituted or unsubstituted phenyl group, one of R2 and R3 is a hydrogen atom, and the other is a C 1-5 It is an alkyl group and n is an integer of 1 to 5.
[0021] Specific examples of compound (1) include diethylene glycol methyl ether, polyethylene glycol methyl ether, propylene glycol phenyl ether, propylene glycol methyl ether, ethylene glycol isopropyl ether, diethylene glycol methyl ether, ethylene glycol benzyl ether, and diethylene glycol hexyl ether.
[0022] The content of compound (1) in the present composition is not particularly limited and may be within an appropriate range as necessary. The content of compound (1) in the total amount (100% by weight) of the present composition may be generally 1 to 95% by weight, preferably 1 to 90% by weight, more preferably 3 to 85% by weight, and more preferably 5 to 80% by weight.
[0023] The present composition contains the ester-based solvent. Generally, the freezing point of compound (1) is high, for example, the freezing point of propylene glycol phenyl ether is 11°C. Therefore, a coating film stripping composition containing compound (1) such as propylene glycol phenyl ether may solidify in a low temperature environment, particularly below freezing point of 0°C or less, and may be difficult to apply. By containing the ester-based solvent, the present composition can suppress solidification in a low temperature environment without affecting the stripping performance. The ester-based solvent may be used alone or in combination of two or more.
[0024] The type of the ester-based solvent is not particularly limited. Examples of the ester-based solvent include dibasic acid esters and fatty acid esters. For example, either one of dibasic acid esters and fatty acid esters may be used as the ester-based solvent, or both may be used together. When dibasic acid esters and fatty acid esters are used as the ester-based solvent, the viscosity of the composition, particularly the viscosity of the composition containing a thickener, can be increased, which is preferable, compared with the case where only one of them is used.
[0025] Examples of the dibasic acid ester include succinic acid ester, glutaric acid ester, and adipic acid ester. Specific examples of the dibasic acid ester include dimethyl succinate, dimethyl glutaric acid, dimethyl adipate, diethyl succinate, diethyl glutaric acid, and diethyl adipate. The dibasic acid ester may be used alone or in combination with two or more kinds. In general, a mixture of two or more kinds is preferred because it is inexpensively available. Examples of the mixture of dibasic acid esters include "DBE" manufactured by Sigma-Aldrich.
[0026] The fatty acid ester may be a saturated fatty acid ester or an unsaturated fatty acid ester. Examples of the fatty acid ester include esters of fatty acids having 8 to 20 carbon atoms, or esters of fatty acids having 8 to 20 carbon atoms and alcohols having 1 to 6 carbon atoms. Specific examples of the fatty acid ester include methyl caprylate, methyl caprate, methyl laurate, methyl myristate, methyl palmitate, methyl palmitoleate, methyl stearate, methyl oleate, methyl linoleate, methyl linolenate, butyl palmitate, butyl stearate, octyl palmitate, isopropyl myristate, and isopropyl palmitate. The fatty acid ester may be used alone or in combination with two or more types. In general, a mixture of two or more types is preferred because it is inexpensively available. Examples of the mixture of fatty acid esters include "TOENOL#2180-70" manufactured by Toei Chemical Co., Ltd.
[0027] The content of the ester solvent is not particularly limited and may be within an appropriate range as required. The content of the ester solvent in the total amount of the composition (100% by weight) is usually 1 to 97% by weight, preferably 5 to 95% by weight, and more preferably 10 to 90% by weight. When two or more kinds of the ester solvents are used, the total amount of the ester solvents may be within the above range.
[0028] When a dibasic acid ester and a fatty acid ester are used as the ester solvent, their contents and ratios are not particularly limited and can be appropriately set as necessary. In the total amount of the present composition (100% by weight), the content of the dibasic acid ester can be 0.5 to 90% by weight, preferably 2.5 to 80% by weight, more preferably 5 to 70% by weight, and more preferably 5 to 60% by weight, and the content of the fatty acid ester can be 0.5 to 90% by weight, preferably 2.5 to 80% by weight, more preferably 5 to 70% by weight, and more preferably 10 to 60% by weight. The ratio of the dibasic acid ester and the fatty acid ester (dibasic acid ester: fatty acid ester) can be 1: (0.1 to 10), preferably 1: (0.15 to 8), more preferably 1: (0.2 to 6), and more preferably 1: (0.3 to 4) by weight.
[0029] In this composition, the content of benzyl alcohol is less than 1% by weight, preferably less than 0.75% by weight, and more preferably less than 0.5% by weight, based on the total amount of the composition (100% by weight). When the content of benzyl alcohol is within the above range, it is possible to suppress poisoning caused by benzyl alcohol, and it is also preferable that the peeling work can be performed without using special equipment such as an air supply mask when spraying. In addition, the description "the content of benzyl alcohol is less than 〇% by weight" in the claims and this document does not mean that benzyl alcohol is contained as an essential component in this composition. Therefore, the lower limit of the content of benzyl alcohol in this composition may be 0% by weight.
[0030] In general, coating films are provided not only on horizontal surfaces but also on vertical surfaces of structures. It is preferable to increase the viscosity of the present composition, since it is possible to easily apply the present composition to vertical surfaces of structures and peel off the coating film. The viscosity of the present composition (measured with a B-type viscometer under conditions of rotor No. 4, rotation speed: 30 rpm, and temperature of 20°C) can be, for example, in the range of 3 to 50 Pa·s. There is no particular limitation on the method for increasing the viscosity of the present composition. Examples of such methods include a method of adding a thickener, as well as a method of adding a resin or a surfactant.
[0031] The type of the thickener is not particularly limited. The thickener may be any thickener that is generally used in coating film strippers. Specific examples of the thickener include silica, sepiolite, bentonite, montmorillonite, polysaccharides such as cellulose, acrylic thickeners, and alkylamides. The thickener may be used alone or in combination of two or more.
[0032] The content of the thickener is not particularly limited and may be within an appropriate range as necessary. The content of the thickener may be generally 1 to 30% by weight, preferably 2 to 15% by weight, and more preferably 3 to 20% by weight, based on 100% by weight of the total amount of the composition.
[0033] The present composition may contain one or more of other known components used in coating film stripping compositions, so long as the effect of the composition is not significantly impaired. Specific examples of the other components include solvents (e.g., N-methyl-2-pyrrolidone and γ-butyrolactone), rust inhibitors, detergents, surfactants, acids (e.g., organic acids), and alkalis (e.g., organic amines) known in stripping compositions.
[0034] The composition is used to remove a coating film formed on a building or structure. The type of the building or structure is not particularly limited. Specific examples of the building include houses (individual homes, apartments, condominiums, buildings, etc.), schools, gates, fences, etc. Specific examples of the structure include steel structures such as bridges, pedestrian bridges, water gates, and steel towers.
[0035] There is no particular limitation on the site on which the coating film is formed in the building or structure. The coating film may be formed on the outdoor surface or indoor surface of the building or structure. As described above, the composition has stable properties even in a low-temperature environment. Therefore, it is preferable that the coating film is formed on the outdoor surface of the building or structure.
[0036] The material on which the coating film is formed is not particularly limited. Examples of the material include general materials that constitute structures. Specific examples of the material include metals (steel, etc.), concrete, glass, mortar, and ALC.
[0037] Specific examples of the architectural coating film include thin coating material E, waterproof thin coating material E, thick coating material E, multi-layer coating material E, waterproof multi-layer coating material E, and multi-layer coating material RE described in JIS A 6909. Specific examples of the coating film for steel structures include coating system A (long-type etching primer, lead-based rust-preventive paint type 1, long oil phthalic acid resin paint), coating system B (long-type etching primer, lead-based rust-preventive paint type 1, phenolic resin MIO paint, chlorinated rubber paint), coating system C (epoxy resin paint or modified epoxy resin paint, polyurethane resin paint), and the like described in the Steel Road Bridge Painting and Corrosion Prevention Handbook (revised edition) published by the Japan Road Association.
[0038] The type of the coating film is not particularly limited. Specific examples of the coating film include coating films mainly composed of acrylic resin, polyester resin, polyurethane resin, epoxy resin, and alkyd melamine resin. Coating films mainly composed of acrylic resin are generally used as architectural coating films, but it is not known that compound (1) such as propylene glycol phenyl ether is effective for removing coating films mainly composed of acrylic resin. In contrast, the present composition can be suitably used for removing coating films mainly composed of acrylic resin (note that the "main component" means a resin component whose content is 50% by weight or more in 100% by weight of the coating film, or the resin component with the largest content when there are two or more resin components).
[0039] The composition is usually applied to a coating film on the surface of a building or structure. After leaving the composition for a certain period of time (usually about 24 hours) as necessary after application, the coating film is peeled off using a peeling tool such as a scraper. There are no particular limitations on the specific form of the "application" as long as the composition can be attached to the surface of a building or structure by a method other than immersion. Specific examples of the "application" include a form in which the composition is applied directly with a brush or the like and a form in which the composition is sprayed with a spray or the like.
[0040] There is no particular limitation on the method of preparing the composition. As described above, the composition has a low content of benzyl alcohol, so it can suppress poisoning caused by benzyl alcohol, and has superior stripping performance compared to compositions containing benzyl alcohol. Therefore, the composition can be prepared and used by, for example, replacing the benzyl alcohol of a commercially available coating stripper containing benzyl alcohol with compound (1) such as propylene glycol phenyl ether. EXAMPLES
[0041] The present invention will be specifically described below with reference to examples. Note that the present invention is not limited to the embodiments shown in the examples. The embodiments of the present invention can be modified in various ways within the scope of the present invention depending on the purpose, application, etc.
[0042] (1) Preparation of Paint Stripping Composition The components and ratios of the coating film stripping compositions of the Examples and Comparative Examples are shown in Tables 1 and 2. The content of each component in Tables 1 and 2 is in weight percent. The coating film stripping compositions of the Examples and Comparative Examples were prepared by stirring and mixing each component with a propeller blade. The details of the components in Tables 1 and 2 are as follows: Propylene glycol phenyl ether (Dowanol PPH, manufactured by The Dow Chemical Company) Dibasic acid ester: "DBE" manufactured by Sigma-Aldrich Viscosifier; Organically modified bentonite
[0043] (2) Peeling test 1 (for buildings) Each of the coating film stripping compositions of the Examples and Comparative Examples was applied to the multi-layer coating material E (sprayed tile) at a rate of 0.5 kg / m. 2 The coating was applied to the sample and left in a thermostatic chamber at 20°C for 24 hours. The coating was then peeled off with a scraper. The peeling state was evaluated based on the following criteria. The results are shown in Table 1. ◎: Easily removable 〇: Peelable △: Difficult to peel off ×: Quite difficult to peel off
[0044] (3) Peel test 2 (for structures) Each of the coating film stripping compositions of the Examples and Comparative Examples was applied at 1.0 kg / m to the A coating system (phthalic acid system). 2 The coating was applied and left in a thermostatic chamber at 20°C for 24 hours. The coating was then peeled off with a scraper. The peeling state was evaluated based on the same criteria as in Peeling Test 1. The results are shown in Table 2.
[0045] [Table 1]
[0046] [Table 2]
[0047] (4) Coagulation tests Mixtures were prepared in the proportions (wt%) shown in Table 3 using the propylene glycol phenyl ether, dibasic acid ester, and methyl oleate used in the preparation of the coating stripping compositions of the Examples. These mixtures were placed in a freezer at -5°C, and after 24 hours, the presence or absence of solidification was visually confirmed. The results are shown in Table 3. In addition, the presence or absence of solidification was visually confirmed for the solvent compositions of Examples 1 to 4 and Comparative Example (propylene glycol phenyl ether, dibasic acid ester, and methyl oleate) using the same method as above. The results are shown in Table 4. In Tables 3 and 4, "◯" means that solidification did not occur, and "×" means that solidification occurred.
[0048] [Table 3]
[0049] [Table 4]
[0050] From Tables 1 and 2, the coating film stripping compositions of the examples show excellent stripping performance in both the multi-layer coating material E and the coating system A. This result shows that the coating film stripping compositions of the examples can be suitably used for stripping coating films from both buildings and structures.
[0051] From Table 1, the coating film stripping compositions of the Examples containing propylene glycol phenyl ether have superior coating film stripping performance compared to Comparative Examples 2 to 9 in which a solvent other than benzyl alcohol was used. In addition, when Comparative Example 1 in which benzyl alcohol was used as the solvent was compared to Comparative Examples 2 to 9 in which a solvent other than propylene glycol phenyl ether was used instead of benzyl alcohol, Comparative Examples 2 to 9 have inferior stripping performance compared to Comparative Example 1. In contrast, Example 2 in which propylene glycol phenyl ether was used instead of benzyl alcohol has superior coating film stripping performance compared to Comparative Example 1. This result shows that the use of propylene glycol phenyl ether instead of benzyl alcohol improves stripping performance compared to the use of other solvents.
[0052] From Table 3, it was confirmed that propylene glycol phenyl ether alone solidified at -5°C. On the other hand, from Tables 3 and 4, a mixture containing propylene glycol phenyl ether and an ester-based solvent (dibasic acid ester and / or oleic acid methyl ester) did not solidify even at -5°C. From this result, the coating film stripping composition of this example has stable properties even under conditions below freezing point and can be applied. Furthermore, from Table 4, since solidification is suppressed even when propylene glycol phenyl ether is used instead of benzyl alcohol, the coating film stripping composition of this example does not lose its stability in low temperature environments even when propylene glycol phenyl ether is used instead of benzyl alcohol.
Claims
1. A coating stripping composition for buildings or structures, comprising a compound of formula (1) and an ester solvent, the content of the ester solvent being 40 to 90% by weight, and the content of benzyl alcohol being less than 1% by weight: R 1 -(OCH(R 2 )-EH(R 3 )) n -OH (1) During the ceremony, R 1 is C 2-20 Alkenyl or alkynyl group, or C 5-20 is an aryl group; R 2 and R 3 are each independently a hydrogen atom, C 1-20 Alkyl group, C 2-20 Alkenyl or alkynyl group, or C 5-20 is an aryl group; n is an integer of 1 or more.
2. R 1 C 5-20 is an aryl group, R 2 and R 3 One of the groups is a hydrogen atom and the other is C 1-20 2. The coating stripping composition of claim 1, wherein n is an alkyl group and n is an integer from 1 to 10.
3. The coating stripping composition according to claim 1 or 2, wherein the ester-based solvent comprises either or both of a dibasic acid ester and a fatty acid ester.
4. A method for removing a coating film from a building or structure, comprising applying a coating film on the surface of the building or structure to the coating film of the building or structure a coating film stripping composition according to any one of claims 1 to 3, and then peeling the coating film off using a stripping tool.
Citation Information
Patent Citations
Remover for resin
JP1997059546A
Fatty acid ester-based solvent, printing ink composition, and ink cleanser for printer
JP2005154317A
COMPOSITION FOR REMOVING FLOOR PAINT THAT WILL INCREASE AFTER DILUTION AND REMOVAL METHOD
JP2008537037A
Coating film peeling agent, and method for peeling coating film