DURABLE CONDUCTIVE POLYURETHANE COMPOSITION AND METHOD FOR APPLYING SAME - Patent application

The polyurethane composition with an aliphatic polyester urethane matrix and fluorinated ionic additive addresses conductivity and durability issues in aircraft transparencies, providing effective static dissipation and erosion resistance.

JP7592132B2Active Publication Date: 2024-11-29GKN AEROSPACE TRANSPARENCY SYSTEMS INC
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
JP2023137301
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-11-22
Filing Date
2023-08-25
Publication Date
2024-11-29
Estimated Expiration
2038-11-16

AI Technical Summary

Technical Problem

Existing transparent polyurethane coatings for aircraft transparencies lack sufficient electrical conductivity, erosion resistance, and environmental durability, particularly at low temperatures and under exposure to elements, leading to static charge buildup and potential damage.

Method used

A polyurethane composition comprising an aliphatic polyester urethane matrix with sulfonate functionality and a hydrophobic fluorinated ionic antistatic additive, such as tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide, to enhance conductivity and stability, combined with a package of stabilizers for durability.

Benefits of technology

The composition maintains high p-static dissipative performance across varying temperatures and environmental conditions, ensuring electrical safety and structural integrity of aircraft transparencies.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007592132000001
    Figure 0007592132000001
  • Figure 0007592132000002
    Figure 0007592132000002
  • Figure 0007592132000003
    Figure 0007592132000003
Patent Text Reader

Abstract

SOLUTION: There is provided a polyurethane composition suitable for coating a surface of a substrate. The polyurethane composition can include an aliphatic polyester urethane matrix and a fluorinated ionic antistatic additive. The aliphatic polyester urethane matrix can comprise an aliphatic diisocyanate, a polyester polyol having a polyester diol and a polyester triol, and sulfonated polyester urethane polyol.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates generally to polyurethane compositions and coated aircraft transparencies incorporating such compositions, and more particularly to transparent polyurethane compositions having excellent static dissipation capabilities, excellent erosion resistance, and excellent environmental durability. [Background technology]

[0002] Transparencies used in modern military aircraft often require protective erosion-resistant coatings or films on their exterior surfaces. Such protective outer layers are necessary to prevent damage to fragile underlying metallic or ceramic conductive coatings such as gold, silver, or indium tin oxide (ITO), or to protect plastic surfaces with limited environmental durability such as polycarbonate. Clear polyurethane coatings and films are preferred in these applications because of their excellent transparency, excellent erosion resistance, and good environmental durability.

[0003] The exterior surfaces of aircraft transparencies, especially in high performance modern military aircraft, are subject to electrostatic charging. This charging is caused by contact with ice crystals and other particles during flight, resulting in the transfer of charge to the surface via triboelectric or friction effects. This phenomenon is known in industry as precipitation charging or p-static charging.

[0004] p-Static charging of the non-conductive (dielectric) outer surfaces of aircraft transparencies can cause several serious problems affecting aircraft performance, the service life of the transparencies, and personnel safety. Discharges during flight can cause damage to the outer coating layers by dielectric breakdown, or can cause electronic interference with equipment. Such charge build-up can also pose an electric shock hazard to flight and ground personnel.

[0005] To avoid these problems caused by p-static charging, the outer layers of aircraft transparencies need to be sufficiently conductive to allow charge to be dissipated across the surface to the fuselage or through the thickness of the layer to an underlying conductive ground layer. Like most organic polymers, polyurethanes are generally poor conductors of electricity. As a result, polyurethanes cannot be used satisfactorily without modification in applications requiring static dissipative properties.

[0006] Several methods have been used to modify polyurethanes to increase their electrical conductivity and thus better dissipate static charge buildup. In one such method, conductive fibers or particles are incorporated into the polyurethane matrix. However, this method is not suitable for use with transparent polyurethanes, since the conductive filler material is opaque and significantly reduces the light transmittance of the modified material.

[0007] Another method to modify polyurethanes to increase their electrical conductivity involves incorporating conductive polymers such as polyaniline or polythiophene salts into the polyurethane matrix. However, again, this method is not suitable for use with transparent polyurethanes because the conductive polymer additive forms a dispersed phase, reducing transparency. Furthermore, polyaniline, polythiophene, and other conductive polymers do not have good environmental stability, generally reducing the overall resistance to weathering and environmental degradation.

[0008] Yet another method of modifying polyurethanes to increase their electrical conductivity is to use hydrophilic additives, such as amines and quaternary ammonium salts, to increase the surface conductivity of polyurethanes. These additives work by migrating to the surface of the polyurethane where they attract water, thereby creating a conductive film. However, this method is not suitable for polyurethane coatings and laminates, because the additives also migrate to the surface of the polyurethane that contacts the underlying substrate, resulting in a loss of adhesion. Furthermore, such additives can lose their effectiveness over time, as they can leach out of the polyurethane under normal use conditions.

[0009] Yet another method of modifying polyurethanes to increase electrical conductivity, hitherto only available for polyurethane foams, involves the addition of an ionizable metal salt in combination with an enhancer. The preferred salt cations are alkali or alkaline earth metal ions, and the preferred anions are the conjugate bases of inorganic acids or C2-C4 carboxylic acids. The preferred enhancers are salts or esters of phosphate esters and fatty acids. None of these known additives for increasing the electrical conductivity of polyurethanes has been considered entirely satisfactory for use in transparent polyurethanes, particularly those used as coatings for modern military aircraft transparencies.

[0010] In general, non-ionic additives and polyol modifiers have been found to significantly improve electrical conductivity only when used at high levels, but may adversely affect other important properties such as transparency and mechanical strength. Ionic additives, including quaternary ammonium salts and ionizable metal salts, are generally more effective at increasing electrical conductivity. The most effective known additives of this type are ionizable metal salts of perfluoroalkylsulfonic acids. However, none of these ionic additives are considered completely satisfactory for use in transparent polyurethanes used as coatings because they are temporary and lose transparency, adhesion, and conductivity over time.

[0011] One recent modification of transparent polyurethanes to enhance their electrical conductivity is described in US Pat. No. 5,399,323 to Sandlin et al., in which improved polyurethane compositions are developed incorporating a specified additive in the range of 0.5 to 5.0 weight percent to enhance electrical conductivity without adversely affecting the transparency of the composition and its adhesion to the underlying substrate. The specified additive is an ionizable metal salt of a perfluoroalkylsulfonimide, the metal being an alkali metal, with the preferred perfluoroalkylsulfonimide being trifluoromethanesulfonimide. The most preferred salt is lithium trifluoromethanesulfonimide available under the trade name Fluorad™ HQ115 from 3M.

[0012] The use of Fluorad™ HQ115 in the preferred polyether urethane composition in the range of 1.0 to 3.0 weight percent can improve the electrical conductivity of the composition by approximately two orders of magnitude, thereby reducing the risk of electrostatic charge accumulating to the point where a shock hazard occurs or the polyurethane coating is damaged by a sudden discharge of electrical current. Transparent polyurethanes modified with Fluorad™ HQ115 are very durable in mechanical properties and exhibit excellent erosion resistance to the harmful effects of exposure to the elements. However, the electrical conductivity of transparent polyurethanes modified with Fluorad™ HQ115 is strongly temperature dependent. As temperatures decrease, the electrical conductivity and ability to dissipate accumulated surface charge decrease significantly. Electrical conductivity is also sensitive to the harmful effects of exposure to the elements and can lose conductivity under normal conditions of use. When modern military aircraft are operated in the field, surface temperatures of transparencies as low as -40°C or lower can occur regularly, so the electrostatic discharge capability must be maintained at low temperatures and be able to withstand the harmful effects of exposure to the elements. Thus, transparent polyurethane compositions modified with the defined lithium trifluoromethanesulfonimide additive, Fluorad™ HQ115, are not considered to be entirely satisfactory with respect to these requirements as surface coatings for transparencies used in modern military aircraft.

[0013] The most recent development to address the problem of static charge buildup on aircraft transparencies is described in U.S. Patent No. 5,399,333 to Moncur et al., in which a multi-layer coating system is developed that includes a first transparent inner polyurethane layer, an intermediate conductive layer disposed on the first transparent inner polyurethane layer, and a second transparent outer polyurethane layer disposed on the conductive layer. The intermediate conductive layer is between the inner and outer polyurethane layers and is formed by coating the first transparent inner polyurethane layer with a colloidal indium tin oxide nanoparticle dispersion that is cured with a silicate binder to form a mesh or porous network that allows the outer polyurethane layer to interact and bond with the inner polyurethane layer through the porous network. The first transparent inner polyurethane layer is relatively thick and is formed by applying an aliphatic polyester urethane precursor solution having about 70% solids to a transparent substrate, followed by evaporating the solvent and thermally curing the precursor. The second transparent outer polyurethane layer is relatively thin and is formed by applying an aliphatic polyester urethane precursor solution having about 45% solids to a conductive layer, followed by evaporating the solvent and thermally curing the precursor. The solids content of both polyurethane precursor solutions can be adjusted to give the desired layer thickness and will depend on the properties of the particular polyurethane used.

[0014] This multi-layer coating system addresses the problem of static electricity build-up on aircraft transparencies via a "drain across" mechanism, which allows surface static electricity to drain through a second transparent polyurethane layer, onto the conductive material layer, and then onto the edge of the conductive material layer that is fitted to the airframe. This "drain across" multi-layer coating system has demonstrated efficiency in dissipating surface static electricity build-up on aircraft transparencies and maintains high p-static dissipation performance even under temperature changes and exposure to the elements. However, this multi-layer coating system has poor erosion resistance, resulting in loss of the outer polyurethane layer during intense rain erosion testing. Delamination occurs during rain erosion testing, as the interaction between the outer and inner polyurethane layers through the porous network of the intermediate conductive material layer cannot provide sufficient bonding between these two polyurethane layers to withstand the test conditions. Therefore, the multi-layer coating system cannot be considered as fully satisfactory as a surface coating for transparencies used in modern military aircraft with respect to erosion resistance requirements. [Prior art documents] [Patent documents]

[0015] [Patent Document 1] U.S. Patent No. 6,458,875 [Patent Document 2] U.S. Patent No. 9,580,564 Summary of the Invention [Problem to be solved by the invention]

[0016] It can be readily appreciated that there exists a need for a transparent polyurethane composition having improved electrical conductivity that can be applied to the exterior surfaces of modern military aircraft transparencies to provide the transparencies with a protective layer having excellent static dissipation capabilities at all operating temperatures, excellent erosion resistance, and excellent environmental durability. The present invention fulfills this need and provides further related advantages. [Means for solving the problem]

[0017] The present invention is embodied in a polyurethane composition suitable for coating the surface of a substrate. In one embodiment, the composition includes an aliphatic polyester urethane matrix and a fluorinated ionic antistatic additive. The aliphatic polyester urethane matrix includes an aliphatic diisocyanate, a polyester polyol having a polyester diol and a polyester triol, and a sulfonated polyester urethane polyol. Each feature or concept is independent, but can be combined with features of any other concept disclosed in this application.

[0018] In one embodiment, the aliphatic diisocyanate is selected from the group consisting of hexamethylene diisocyanate, methylene bis(4-cyclohexyl isocyanate), and isophorone diisocyanate. In another embodiment, the aliphatic diisocyanate comprises methylene bis(4-cyclohexyl isocyanate). Each feature or concept is independent but can be combined with features of any other concept disclosed in this application.

[0019] In any one of the foregoing embodiments, the polyester diol can include polycaprolactone diol. In one embodiment, the polycaprolactone diol is initiated with a compound selected from the group consisting of 1,4-butanediol, diethylene glycol, and neopentyl glycol. In another embodiment, the polyester diol has an average molecular weight of about 400 g / mole to about 4,000 g / mole. In a further embodiment, the polyester diol includes polycaprolactone diol having an average molecular weight of about 830 g / mole and initiated with diethylene glycol. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0020] In any one of the foregoing embodiments, the polyester triol can include polycaprolactone triol. In one embodiment, the polycaprolactone triol is initiated with trimethylolpropane. In another embodiment, the polyester triol has an average molecular weight of about 300 g / mol to about 3,000 g / mol. In a further embodiment, the polyester triol includes polycaprolactone triol having an average molecular weight of about 540 g / mol initiated with trimethylolpropane. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0021] In any one of the preceding embodiments, the polyester polyol may further comprise a chain extender. In one embodiment, the chain extender is selected from the group consisting of ethylene glycol, 1,4-butanediol, and 2-ethyl-1,3-hexanediol. Each feature or concept is independent, but may be combined with features of any other concept disclosed herein.

[0022] In any one of the foregoing embodiments, the sulfonated polyesterurethane polyol can include an anionic dispersion of an aliphatic polyesterurethane resin. In one embodiment, the sulfonated polyesterurethane polyol is about 3% to about 15% by weight of the composition. In another embodiment, the sulfonated polyesterurethane polyol is about 5% to about 10% by weight of the composition. Each feature or concept is independent, but can be combined with features of any other concept disclosed in this application.

[0023] In any one of the above embodiments, the aliphatic polyester urethane matrix may be about 85% to about 98% by weight of the composition. In one embodiment, the aliphatic polyester urethane matrix is ​​about 88% to about 95% by weight of the composition. Each feature or concept is independent, but can be combined with features of any other concept disclosed in this application.

[0024] In any one of the foregoing embodiments, the fluorinated ionic antistatic additive can include a quaternary ammonium salt of a fluorinated sulfonimide. In one embodiment, the quaternary ammonium salt of a fluorinated sulfonimide is selected from the group consisting of tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide and quaternary alkylammonium bis-(trifluoromethanesulfonyl)imide. In another embodiment, the quaternary ammonium salt of a fluorinated sulfonimide includes tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide. In a further embodiment, the fluorinated ionic antistatic additive is about 1% to about 10% by weight of the composition. In an additional embodiment, the fluorinated ionic antistatic additive is about 3% to about 8% by weight of the composition. Each feature or concept is independent but can be combined with features of any other concept disclosed in the present application.

[0025] In any one of the foregoing embodiments, the composition may further comprise a catalyst selected from the group consisting of dibutyltin dilaurate and dibutyltin diacetate. In one embodiment, the catalyst is about 0.001% to about 0.02% by weight of the composition. In another embodiment, the catalyst is about 0.003% to about 0.01% by weight of the composition. Each feature or concept is independent but may be combined with features of any other concept disclosed herein.

[0026] In any one of the foregoing embodiments, the composition may further comprise a stabilizer package. In one embodiment, the stabilizer package comprises one or more of a UV absorber, a light stabilizer, and a heat stabilizer. In another embodiment, the stabilizer package comprises a UV absorber, a light stabilizer, and a heat stabilizer. In a further embodiment, the UV absorber is selected from the group consisting of hydroxyphenyl-triazine, hydroxyphenyl-benzotriazole, and hydroxyphenyl-benzophenone. In an additional embodiment, the light stabilizer comprises a hindered amine light stabilizer. In yet another embodiment, the heat stabilizer comprises a sterically hindered phenolic antioxidant. In one embodiment, the heat stabilizer comprises pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate). In another embodiment, the stabilizer package is from about 0.5% to about 4% by weight of the composition. In a further embodiment, the stabilizer package is from about 1% to about 3% by weight of the composition. Each feature or concept stands alone but can be combined with features of any other concept disclosed in this application.

[0027] In any one of the above embodiments, the composition may further comprise a first surfactant. In one embodiment, the first surfactant comprises a polyalkylene oxide-modified heptamethyltrisiloxane. In another embodiment, the first surfactant is about 0.05% to about 1% by weight of the composition. In a further embodiment, the first surfactant is about 0.1% to about 0.5% by weight of the composition. Each feature or concept is independent, but may be combined with features of any other concept disclosed herein.

[0028] In any one of the above embodiments comprising a first surfactant, the composition can further comprise a second surfactant. In one embodiment, the second surfactant comprises a polyether-modified polydimethylsiloxane or a polyester-modified hydroxy-functional polydimethylsiloxane. In another embodiment, the second surfactant comprises a polyester-modified hydroxy-functional polydimethylsiloxane. In a further embodiment, the second surfactant is about 0.05% to about 1% by weight of the composition. In an additional embodiment, the second surfactant is about 0.1% to about 0.5% by weight of the composition. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0029] In any one of the above embodiments, the composition can further comprise an aprotic solvent. In one embodiment, the aprotic solvent is selected from the group consisting of n-pentyl propionate, ethyl 3-ethoxypropionate, 2-butoxyethyl acetate, di-isobutyl ketone and methyl isobutyl ketone. Each feature or concept is independent, but can be combined with the features of any other concept disclosed in this application.

[0030] The present invention is also embodied in a method for preparing a polyurethane composition suitable for coating a surface of a substrate. In one embodiment, the method includes mixing a polyester diol and a polyester triol with a sulfonated polyester urethane dispersion to form a homogeneous sulfonated polyol mixture, and mixing the homogeneous sulfonated polyol mixture with ingredients including an aliphatic diisocyanate, a fluorinated ionic antistatic additive, and a catalyst to form a polyurethane coating composition. Each feature or concept is independent, but can be combined with the features of any other concept disclosed in this application.

[0031] In one embodiment, the sulfonated polyester urethane dispersion is mixed with a polyester diol and a polyester triol at about 90° C. to about 105° C. for about 48 hours. In another embodiment, the polyester diol comprises a polycaprolactone diol having an average molecular weight of about 830 g / mol and initiated with diethylene glycol. In a further embodiment, the polyester triol comprises a polycaprolactone triol having an average molecular weight of about 540 g / mol and initiated with trimethylolpropane. In an additional embodiment, the sulfonated polyester urethane dispersion comprises an anionic dispersion of an aliphatic polyester urethane resin. In yet another embodiment, the sulfonated polyester urethane dispersion is about 5% to about 10% by weight of the composition. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0032] In one embodiment, the aliphatic diisocyanate comprises methylene bis(4-cyclohexyl isocyanate). In another embodiment, the fluorinated ionic antistatic additive comprises tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide. In a further embodiment, the fluorinated ionic antistatic additive is from about 3% to about 8% by weight of the composition.

[0033] In one embodiment, the catalyst comprises dibutyltin dilaurate. In another embodiment, the catalyst is about 0.003% to about 0.01% by weight of the composition. Each feature or concept is independent but may be combined with features of any other concept disclosed herein.

[0034] In one embodiment, the components further comprise an aprotic solvent, a stabilizer package, a first surfactant, and a second surfactant. In another embodiment, the aprotic solvent comprises n-pentyl propionate. In a further embodiment, the stabilizer package comprises a UV absorber, a light stabilizer, and a heat stabilizer. In an additional embodiment, the UV absorber is selected from the group consisting of hydroxyphenyl-triazine, hydroxyphenyl-benzotriazole, and hydroxyphenyl-benzophenone. In yet another embodiment, the light stabilizer comprises a hindered amine light stabilizer. In one embodiment, the heat stabilizer comprises a sterically hindered phenolic antioxidant. In another embodiment, the stabilizer package is about 1% to about 3% by weight of the composition. In a further embodiment, the polyurethane composition comprises about 70% solids. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0035] The invention is also embodied in a method of applying a coating to a surface of a substrate. In one embodiment, the method includes coating a surface with a polyurethane composition of any one of the preceding embodiments relating to polyurethane compositions. In one embodiment, the method further includes curing the coated surface at a first cure temperature of about 50° C. to about 60° C. for about 12 hours, and re-curing the coated surface at a second cure temperature of about 75° C. to about 85° C. for about 24 hours. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0036] The present invention is embodied in another method of applying a coating to a surface of a substrate. In one embodiment, the method includes coating a surface with a polyurethane composition prepared by any one of the methods described above for preparing a polyurethane composition. In one embodiment, the method further includes curing the coated surface at a first cure temperature of about 50° C. to about 60° C. for about 12 hours, and re-curing the coated surface at a second cure temperature of about 75° C. to about 85° C. for about 24 hours. Each feature or concept is independent but can be combined with features of any other concept disclosed herein.

[0037] In any one of the above embodiments relating to the method of applying a coating to a surface of a substrate, the substrate can be acrylic. In one embodiment, the substrate is transparent. In another embodiment, the first cure temperature is about 54° C. In a further embodiment, the second cure temperature is about 82° C. Each feature or concept is independent, but can be combined with features of any other concept disclosed herein.

[0038] In any one of the above-mentioned embodiments relating to the method of applying a coating to a surface of a substrate, the method can further include preparing the surface before coating with the transparent polyurethane composition. In one embodiment, the preparing step includes coating the surface with a polysiloxane coating to form a base-coated surface, coating the base-coated surface with a three-layer indium tin oxide (ITO) / gold / ITO film stack to form an ITO-coated surface, coating the ITO-coated surface with a 0.1% silicate coating solution to form a silicate-coated surface, heating the silicate-coated surface at about 82° C. for about 1 hour, coating the silicate-coated surface with a 0.1% aminosilane primer solution to form an aminosilane-coated surface, coating the aminosilane-coated surface with an 18% polyurethane thermoset adhesive solution to form a polyurethane thermoset coating surface, and curing the polyurethane thermoset coating surface at about 20° C. to about 25° C. for about 16 hours. Each feature or concept stands alone but can be combined with features of any other concept disclosed in this application.

[0039] In any of the above-described embodiments relating to the method of applying a coating to a surface of a substrate, the 18% polyurethane thermosetting adhesive solution can include a solvent selected from the group consisting of cyclohexanone and 3-ethoxypropionate. Each feature or concept is independent but can be combined with features of any other concept disclosed in this application.

[0040] The present invention is also embodied in a laminate comprising a substrate having a surface and a coating of a polyurethane composition disposed on the surface. In one embodiment, the polyurethane composition can be any one of the polyurethane compositions described above. In another embodiment, the coating can be applied to the surface by any one of the methods described above for applying a coating to a substrate surface. Each feature or concept stands alone but can be combined with features of any other concept disclosed herein.

[0041] In one embodiment, the coating has a thickness of about 75 μm to about 100 μm. 11 The coating has an electrical volume resistivity of ohms / cm or less. In a further embodiment, the coating has a luminous transmittance of about 65% to about 70%. In an additional embodiment, the coating has a haze of about 0.90% to about 1.40%. In yet another embodiment, the coating does not include an ionizable metal salt of a perfluoroalkylsulfonate. In one embodiment, the coating does not include a colloidal indium tin oxide nanoparticle dispersion. In another embodiment, the substrate is acrylic. In a further embodiment, the substrate is transparent. In a further embodiment, the coating is transparent. In an additional embodiment, the surface is an exterior surface of an aircraft transparency. Each feature or concept stands alone but may be combined with features of any other concepts disclosed herein.

[0042] Other features and advantages of the present invention should be apparent from the following description of the preferred embodiment, which illustrates, by way of example, the principles of the invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0043] The present invention relates to a transparent polyurethane composition having substantially improved electrical conductivity. In one embodiment, the transparent polyurethane composition comprises: (1) a thermosetting aliphatic polyester urethane matrix containing sulfonate functional groups in the range of about 85 to about 98 weight percent of the bulk of the transparent polyurethane composition. The urethane polymer is formed by reacting an aliphatic diisocyanate, a polyester diol, optionally a polyester triol, and a polyester urethane diol and triol mixture containing sulfonate functionality in the backbone with (2) a hydrophobic fluorinated ionic antistatic additive, tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide (available from 3M under the trade name FC-4400), in the range of about 1 to about 10 weight percent for improved electrical conductivity, (3) a catalyst in the range of about 10 to about 200 ppm for curing the thermosetting polyurethane composition, (4) a stabilizer package including a UV absorber, a light stabilizer, and a heat stabilizer in the range of about 0.5 to about 4 weight percent for improved environmental durability, (5) optional surface active agents or surfactants for flow / leveling control and improved coating surface cosmetic properties, and (6) an optional aprotic solvent as a carrier for the composition.

[0044] Thermosetting aliphatic polyester urethane matrix A thermosetting aliphatic polyesterurethane matrix formed from an aliphatic isocyanate, a polyester polyol (a triol / diol mixture) and a sulfonate-containing urethane polyester polyol is provided as the body of a transparent polyurethane composition. Aliphatic polyesterurethanes are preferred due to their excellent chemical, abrasion and weather resistance. Representative liquid monomeric aliphatic or cycloaliphatic diisocyanates suitable for the present invention include hexamethylene diisocyanate, methylene bis(4-cyclohexyl isocyanate) and isophorone diisocyanate. A preferred diisocyanate for the present invention is methylene bis(4-cyclohexyl isocyanate) available as Desmodur® W from Covestro. Representative polyester triols suitable for the present invention include polycaprolactone-based Capa® 3031, Capa® 3041, Capa® 3050, Capa® 3091, Capa® 3121, Capa® 3201, and Capa® 3301, available from Perstorp Specialty Chemicals, Inc., having average molecular weights (g / mol) ranging from about 300 to about 3000. A preferred polyester triol for the present invention is Capa® 3050, having an average molecular weight (g / mol) of about 540. Representative polyester diols suitable for the present invention include polycaprolactone-based Capa® 2043, Capa® 2054, Capa® 2085, Capa® 2100, Capa® 2125, Capa® 2205, Capa® 2304, and Capa® 2402 having average molecular weights (g / mol) ranging from about 400 to about 4000, available from Perstorp Specialty Chemicals, Inc. A preferred polyester diol for the present invention is Capa® 2085, having an average molecular weight (g / mol) of about 830.Chain extenders such as ethylene glycol, 1,4-butanediol (BDO), 2-ethyl-1,3-hexanediol (EHD), etc., can be added to the polyol as needed to adjust performance. The polyurethane matrix containing sulfonate functional groups is typically used in a weight percent range of about 85% to about 98%, more typically about 88% to about 95%, based on the total weight of solids in the composition. In one embodiment, the polyurethane matrix containing sulfonate functional groups is about 85%, about 86%, about 87%, about 88%, about 89%, about 90%, about 91%, about 92%, about 93%, about 94%, about 95%, about 96%, about 97%, or about 98% by weight of the composition. In another embodiment, the polyurethane matrix is ​​in a range defined by any two of the preceding values.

[0045] Hydrophobic fluorinated ion antistatic additive Hydrophobic fluorinated ionic antistatic additives have been formulated into polyurethane compositions to enhance electrical conductivity. By appropriately selecting the antistatic additive, the composition can exhibit high electrical conductivity and meet the p-static dissipation requirements of the coated transparency. In the past, salts of quaternary ammonium cations or salts of fluorinated sulfonimide anions have been used as antistatic additives to enhance electrical conductivity of polyurethanes with limited success, such as the examples described in U.S. Pat. No. 5,399,343. The benefits of using a single compound of a quaternary ammonium cation in combination with a fluorinated sulfonimide anion as an antistatic additive in polyurethane compositions to enhance electrical conductivity have not been explored before. The hydrophobic fluorinated ionic antistatic additives FC-4400 and FC-5000 are salts containing both a quaternary ammonium cation and a fluorinated sulfonimide anion. By combining a quaternary ammonium cation and a fluorinated sulfonimide anion as a single compound, FC-4400 or FC-5000 becomes more efficient at improving electrical conductivity. Furthermore, the hydrophobic fluorinated ionic antistatic additive FC-4400 or FC-5000 is fully compatible with the other components of the polyurethane composition, so it can be loaded in a wide range of weight percents without compromising other performance of the composition. FC-4400 is an ionic liquid antistatic salt of a quaternary ammonium cation with a fluorinated sulfonimide anion of tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide with the formula (n-C4H9)3(CH3)N+-N(SO2CF3)2. FC-5000 is an ionic liquid antistatic salt of a quaternary ammonium cation containing a fluorinated sulfonimide anion with a single primary alcohol group in the quaternary ammonium with the formula R4N+-N(SO2CF3)2. The preferred hydrophobic fluorinated ionic antistatic additive for the present invention is FC-4400. The hydrophobic fluorinated ionic antistatic additive is typically used in the range of from about 1% to about 10%, more typically in the range of from about 3% to about 8%, based on the total weight of solids in the composition.In one embodiment, the hydrophobic fluorinated ionic antistatic additive is about 1%, about 2%, about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, or about 10% by weight of the composition. In another embodiment, the hydrophobic fluorinated ionic antistatic additive is in a range defined by any two of the preceding values.

[0046] Sulfonated polyester urethane polyol The polyester urethane polyol incorporating sulfonate ion functional groups in the backbone is used to interact with the hydrophobic fluorinated ionic antistatic additive FC-4400 or FC-5000 additive. The sulfonated polyester urethane polyol has multiple sulfonate ion functional groups in the backbone and hydroxyl functional groups at the chain ends. The sulfonated polyester urethane polyol can be cured into the polyurethane matrix through the hydroxyl functional groups at the chain ends, while the sulfonate ion functional groups in the backbone bond with the ionic groups of the hydrophobic fluorinated ionic antistatic additive through ionic interactions to form a stable crosslinked network in which the hydrophobic fluorinated ionic antistatic additive is uniformly dispersed in the polyurethane matrix. The synergistic interaction between the sulfonated polyester urethane polyol and the hydrophobic fluorinated ionic antistatic additive substantially enhances the electrical conductivity of the polyurethane composition. Meanwhile, the formation of a stable crosslinked network prevents the loss of the hydrophobic fluorinated ionic antistatic additive, so that the transparent polyurethane can withstand the deleterious effects of weathering and maintain high electrical conductivity. Sulfonated polyesterurethane polyols are prepared by reacting a non-sulfonated polyol with a sulfonated polyesterurethane. Representative sulfonated polyesterurethanes suitable for the present invention include Bayhydrol® 140AQ, Bayhydrol® UH240, Baybond® PU402A and Impranil® DL1554 available from Bayer Material Science (now Covestro). A preferred sulfonated polyesterurethane polyol for the present invention is Bayhydrol® 140AQ, which is a 40% solids aqueous dispersion of sulfonated aliphatic anionic polyesterurethane resin. These materials are available as aqueous dispersions and are reacted with a non-sulfonated polyol to remove water and produce a sulfonated polyol.The sulfonated polyester urethane is typically used in the range of about 3% to about 15% by weight, more typically in the range of 5% to 10% by weight, based on the total weight of solids in the composition. In one embodiment, the sulfonated polyester urethane is about 3%, about 4%, about 5%, about 6%, about 7%, about 8%, about 9%, about 10%, about 11%, about 12%, about 13%, about 14%, or about 15% by weight of the composition. In another embodiment, the sulfonated polyester urethane is in a range defined by any two of the foregoing values.

[0047] Catalyst for curing polyurethane compositions Catalysts are used to cure thermosetting polyurethane compositions. Catalysts accelerate polyurethane network formation. Representative catalysts suitable for the present invention include dibutyltin dilaurate and dibutyltin diacetate available from Sigma-Aldrich, and bismuth and zinc compounds available from Shepherd Chemical Company. Catalysts are typically used in the range of about 10 ppm to about 200 ppm, more typically about 30 ppm to about 100 ppm, based on the total weight of solids in the composition. In one embodiment, the catalyst is present at about 10 ppm, about 20 ppm, 30 ppm, 40 ppm, 50 ppm, 60 ppm, 70 ppm, 80 ppm, 90 ppm, 100 ppm, 110 ppm, 120 ppm, 130 ppm, 140 ppm, 150 ppm, 160 ppm, 170 ppm, 180 ppm, 190 ppm, or 200 ppm by weight of the composition. In another embodiment, the catalyst is present in a range defined by any two of the preceding values.

[0048] Stabilizer package A stabilizer package including UV absorbers, light stabilizers, and heat stabilizers is incorporated into the composition for improved environmental durability. The stabilizer package provides effective stabilization against the harmful effects of light and the elements.

[0049] The UV absorber is typically a compound of the hydroxyphenyl-triazine, hydroxyphenyl-benzotriazole or hydroxyphenyl-benzophenone class. The UV absorber competitively absorbs UV light that is harmful to the polyurethane composition. Representative UV absorbers suitable for the present invention include Tinuvin® 400, Tinuvin® 405, Tinuvin® 460, Tinuvin® 477 and Tinuvin® 479 of the hydroxyphenyl-triazine class, and Tinuvin® 928, Tinuvin® 1130, Tinuvin® 328, Tinuvin® 99-2 and Tinuvin® 384-2 of the hydroxyphenylbenzotriazole class, available from BASF. The preferred UV absorber for the present invention is Tinuvin® 479, which has a very high extinction coefficient in the UV-B and UV-A ranges. The high extinction coefficient allows the formulation of compositions with reduced UV absorber content.

[0050] The light stabilizer is usually a hindered amine light stabilizer (HALS), which can trap free radicals and act as a radical scavenger in the autoxidation cycle, inhibiting the photooxidative degradation of polymeric materials. Representative light stabilizers suitable for the present invention include Tinuvin® 123, Tinuvin® 144, Tinuvin® 152, Tinuvin® 292, or Tinuvin® 5100, available from BASF. The preferred light stabilizer for the present invention is Tinuvin® 152, which has a reactive primary hydroxyl, which allows Tinuvin® 152 to be cured into a polyurethane network to improve compatibility and resistance to migration.

[0051] The heat stabilizer is typically a sterically hindered phenolic antioxidant that protects the composition from thermo-oxidative degradation. Exemplary heat stabilizers suitable for the present invention include IRGANOX® 1010, IRGANOX® 1076, IRGANOX® 1135, or IRGANOX® 245, available from BASF. Standard selection criteria for heat stabilizers for application in this composition are low color, good compatibility, high resistance to extraction, and low volatility, with IRGANOX® 1010 being the preferred one.

[0052] The stabilizer package provides enhanced protection when used in combination. The Tinuvin® 479 / Tinuvin® 152 / IRGANOX® 1010 stabilizer package provides the most effective stability against the harmful effects of light and weather. The stabilizer package is typically used in the range of about 0.5% to about 4%, more typically in the range of about 1% to about 3% by weight, based on the total weight of solids in the composition. In one embodiment, the stabilizer package is about 0.5%, about 1%, about 1.5%, about 2%, about 2.5%, about 3%, about 3.5%, or about 4% by weight of the composition. In another embodiment, the stabilizer package is in the range defined by any two of the aforementioned values.

[0053] Surfactants Surface active agents or surfactants that control the wetting or spreading of the coating are advantageously used in the composition to provide satisfactory flow-and-leveling properties to the coating surface, eliminate coating defects such as spalling and craters, and increase surface slip. Exemplary surfactants suitable for the present invention include silicone-based flow / leveling agents Silwet® L-77, L-7200, L-7600, L-7604, L-7605, and L-7657 available from Momentive Performance Materials, Inc., and silicone-based surface additives BYK-300, BYK-306, BYK-313, BYK-333, BYK-370, and BYK-378 available from BYK Chemie. Silwet® silicone surfactants are modified trisiloxanes that have excellent wetting, spreading, and leveling properties. Preferred for the present invention is the powerful Silwet® L-77, which combines a very low molecular weight trisiloxane with a polyether group. BYK silicone surface additives are modified polydimethylsiloxanes to increase surface slip. Preferred for the present invention is the reactive BYK-370, a polyester-modified hydroxyl-functional polydimethylsiloxane. BYK-370 can be crosslinked through its primary OH group into a polyurethane network, permanently increasing surface slip. The synergistic use of Silwet® L-77 and BYK-370 provides an excellent combination of spreading / flow / leveling and permanent surface slip enhancement. Each surfactant is typically used in a weight percent range of about 0.05% to about 1%, more typically about 0.1% to about 0.5%, based on the total weight of solids in the composition.In one embodiment, each surfactant is about 0.05%, about 0.1%, about 0.15%, about 0.2%, about 0.25%, about 0.3%, about 0.35%, about 0.4%, about 0.45%, about 0.5%, about 0.55%, about 0.6%, about 0.65%, about 0.7%, about 0.75%, about 0.8%, about 0.85%, about 0.9%, about 0.95%, or about 1.0% by weight of the composition. In another embodiment, each surfactant is within a range defined by any two of the preceding values.

[0054] Optional Solvent Optionally, an aprotic solvent can be used to mix the composition and to serve as a composition carrier. Exemplary aprotic solvents suitable for the present invention include n-pentyl propionate (nPP), ethyl 3-ethoxypropionate (EEP), 2-butoxyethyl acetate (BEA), di-isobutyl ketone (DIBK) and methyl isobutyl ketone (MIBK). The weight percentage of any aprotic solvent can vary depending on the coating thickness required when the composition is flow coated onto the exterior surface of an aircraft transparency.

[0055] Highlights of cutting edge polyurethane performance The polyurethane composition of the present invention can be conveniently flow coated onto the exterior surface of transparencies used in modern military aircraft, including exterior conductive coatings, to provide the transparencies with a protective layer having excellent static dissipation capability, excellent erosion resistance, and excellent environmental resistance at all operating temperatures. Table 1 summarizes the electrical conductivity and rain erosion resistance performance of the polyurethane composition of the present invention and state-of-the-art systems such as those described in U.S. Patent No. 5,399,433 and U.S. Patent No. 5,399,433. Electrical volume resistivity measured at about -6°C, about -28°C, and about -40°C is shown for samples without QUV exposure and after 5 weeks of QUV exposure. Rain erosion resistance results after about 10 minutes, about 30 minutes, and about 60 minutes at about 927 km / h are shown for samples without QUV exposure and after about 5 weeks of QUV exposure. The accelerated QUV device was operated using UVB-313EL fluorescent lamps with cycles of about 50°C / about 7 hours of UV exposure and about 50°C / about 5 hours of condensation (UV off, high humidity). Electrical volume resistivity >10 14 A "no" means that the sample had no measurable resistivity or the sample experienced dielectric breakdown during the p-static dissipation test. "Pass" means that the sample had less than 10% coating loss after the test. "Fail" means that the sample had more than 10% coating loss after the test. Both samples were coated with a conductive gold stack coating as described in the examples.

[0056] [Table 1]

[0057] As described in US Pat. No. 5,993,136, transparent polyurethanes modified with Fluorad™ HQ115, a lithium trifluoromethanesulfonimide additive, enhance electrical conductivity and therefore improve static discharge capability, but the improved static discharge capability is not maintained at low temperatures and cannot withstand the deleterious effects of exposure to the elements. On the other hand, the “Drain-Across” multi-layer coating system described in US Pat. No. 5,993,136 demonstrates efficiency in dissipating surface static charges that build up on aircraft transparencies and maintains high p-static dissipation performance regardless of temperature changes and exposure to the elements, but exhibits poor erosion resistance and loses the outer polyurethane layer during vigorous rain erosion testing. None of these prior art systems are considered fully satisfactory as surface coatings for transparencies used on modern military aircraft.

[0058] The polyurethane compositions of the embodiments, which combine sulfonate functionality in the backbone and incorporate the hydrophobic fluorinated ionic antistatic additive tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide FC-4400 as an additive, exhibit substantially improved electrical conductivity and therefore maintain high p-static dissipation capability as aircraft transparency surface coatings at all operating temperatures. It is believed that the synergistic interaction between the hydrophobic fluorinated ionic antistatic additive FC-4400 and the sulfonated polyester urethane matrix is ​​responsible for this substantial improvement in electrical conductivity. It is believed that the hydrophobic fluorinated ionic antistatic additive FC-4400 strongly interacts with the sulfonic acid functionality, resulting in the maintenance of high electrical conductivity and p-static dissipation capability after the deleterious effects of exposure to the elements.

[0059] Method for preparing a polyurethane composition The present invention is also embodied in a method of preparing a polyurethane composition suitable for coating a surface of a substrate, in one embodiment, the method includes mixing a polyester diol and a polyester triol with a sulfonated polyester urethane dispersion to form a homogeneous sulfonated polyol mixture, and mixing the homogeneous sulfonated polyol mixture with ingredients including an aliphatic diisocyanate, a fluorinated ionic antistatic additive, and a catalyst to form a polyurethane coating composition.

[0060] In one embodiment, the sulfonated polyester urethane dispersion is mixed with a polyester diol and a polyester triol at about 90° C. to about 105° C. for about 48 hours. In another embodiment, the polyester diol comprises a polycaprolactone diol having an average molecular weight of about 830 g / mol and initiated with diethylene glycol. In a further embodiment, the polyester triol comprises a polycaprolactone triol having an average molecular weight of about 540 g / mol and initiated with trimethylolpropane. In an additional embodiment, the sulfonated polyester urethane dispersion comprises an anionic dispersion of an aliphatic polyester urethane resin. In yet another embodiment, the sulfonated polyester urethane dispersion is about 5% to about 10% by weight of the composition.

[0061] In one embodiment, the aliphatic diisocyanate comprises methylene bis(4-cyclohexyl isocyanate). In another embodiment, the fluorinated ionic antistatic additive comprises tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide. In a further embodiment, the fluorinated ionic antistatic additive is from about 3% to about 8% by weight of the composition.

[0062] In one embodiment, the catalyst comprises dibutyltin dilaurate, hi another embodiment, the catalyst is from about 0.003% to about 0.01% by weight of the composition. In one embodiment, the components further comprise an aprotic solvent, a stabilizer package, a first surfactant, and a second surfactant. In another embodiment, the aprotic solvent comprises n-pentyl propionate. In a further embodiment, the stabilizer package comprises a UV absorber, a light stabilizer, and a heat stabilizer. In an additional embodiment, the UV absorber is selected from the group consisting of hydroxyphenyl-triazine, hydroxyphenyl-benzotriazole, and hydroxyphenyl-benzophenone. In yet another embodiment, the light stabilizer comprises a hindered amine light stabilizer. In one embodiment, the heat stabilizer comprises a sterically hindered phenolic antioxidant. In another embodiment, the stabilizer package is about 1% to about 3% by weight of the composition. In a further embodiment, the polyurethane composition comprises about 70% solids.

[0063] How to Apply the Coating The invention is also embodied in a method of applying a coating to a surface of a substrate. In one embodiment, the method includes coating the surface with any one of the novel polyurethane compositions described above. The method further includes curing the coated surface at a first cure temperature of about 50° C. to about 60° C. for about 12 hours, and re-curing the coated surface at a second cure temperature of about 75° C. to about 85° C. for about 24 hours.

[0064] The present invention is embodied in another method of applying a coating to a surface of a substrate. In one embodiment, the method includes coating a surface with a polyurethane composition prepared by any one of the methods described above for preparing a polyurethane composition. The method further includes curing the coated surface at a first cure temperature of about 50° C. to about 60° C. for about 12 hours, and re-curing the coated surface at a second cure temperature of about 75° C. to about 85° C. for about 24 hours.

[0065] For any of these methods of applying a coating to the surface of a substrate, the substrate can be acrylic. In one embodiment, the substrate is transparent. In another embodiment, the first cure temperature is about 54°C. In a further embodiment, the second cure temperature is about 82°C.

[0066] For any of these methods of applying a coating to a surface of a substrate, the method can further include preparing the surface prior to coating the surface with the transparent polyurethane composition. In one embodiment, the preparing step includes coating the surface with a polysiloxane coating to form a base coated surface, coating the base coated surface with a three layer indium tin oxide (ITO) / gold / ITO film stack to form an ITO coated surface, coating the ITO coated surface with a 0.1% silicate coating solution to form a silicate coated surface, heating the silicate coated surface at about 82° C. for about 1 hour, coating the silicate coated surface with a 0.1% aminosilane primer solution to form an aminosilane coated surface, coating the aminosilane coated surface with an 18% polyurethane thermoset adhesive solution to form a polyurethane thermoset coated surface, and curing the polyurethane thermoset coated surface at about 20° C. to about 25° C. for about 16 hours.

[0067] For any of these methods of applying the coating to the surface of a substrate, the 18% polyurethane thermosetting adhesive solution can include a solvent selected from the group consisting of cyclohexanone and 3-ethoxypropionate.

[0068] laminate The invention is also embodied in a laminate that includes a substrate having a surface and a coating of a polyurethane composition disposed on the surface. In one embodiment, the polyurethane composition can be any one of the novel polyurethane compositions described above. In another embodiment, the coating can be applied to the surface by any one of the methods described above for applying a coating to a surface of a substrate.

[0069] In one embodiment, the coating has a thickness of about 75 μm to about 100 μm. 11 It has an electrical volume resistivity of ohms / cm or less. In a further embodiment, the coating has a luminous transmittance of about 65% to about 70%. In an additional embodiment, the coating has a haze of about 0.90% to about 1.40%. In yet another embodiment, the coating does not include an ionizable metal salt of a perfluoroalkylsulfonate. In one embodiment, the coating does not include a colloidal indium tin oxide nanoparticle dispersion. In another embodiment, the substrate is acrylic. In a further embodiment, the substrate is transparent. In a further embodiment, the coating is transparent. In an additional embodiment, the surface is an exterior surface of an aircraft transparency.

[0070] From the above description, it should be understood that the present invention provides a polyurethane composition suitable as a surface coating for aircraft transparencies. The polyurethane composition coating can maintain high p-static dissipation performance regardless of temperature changes and exposure to the elements, thus avoiding the risk of static electricity accumulating to the point where a shock hazard occurs or the polyurethane coating is damaged by rapid discharge of current. The transparent polyurethane of the present invention is also very durable, exhibiting excellent erosion resistance and retention of mechanical properties after exposure to the elements.

[0071] Specific methods, devices, and materials have been described, although any methods and materials similar or equivalent to those described can be used in the practice or testing of the present invention. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which this invention belongs.

[0072] As used in this application, singular words such as "a" and "an" mean "one or more" unless there is a clear intent to limit the element to "one." The term "about" refers to the value it modifies ±2%.

[0073] As used in this application, the term "hydrophobic" means lacking an affinity for water, and a surface is considered hydrophobic if it has a water contact angle of at least about 80 degrees. As used herein, the term "transparent" means having a light transmittance of at least about 85% when measured on a polyurethane film having a thickness of about 255 μm to about 510 μm using the ASTM D1003 standard.

[0074] Without further elaboration, it is believed that one skilled in the art can use the above description to make and use the present invention to its fullest extent. Other objects, features, and advantages of the present embodiment will become apparent from the following specific examples. The specific examples, although showing specific embodiments, are provided by way of illustration only. Thus, the present invention also includes those various changes and modifications within the spirit and scope of the present invention that may become apparent to those skilled in the art from this detailed description. The following examples are illustrative only and are not intended to limit the present disclosure in any manner. EXAMPLES

[0075] Aircraft grade (MIL-PRF-25690 compliant) stretched acrylic sheets with dimensions of 38.1 cm x 81.28 cm were prepared using the procedure described in US Patent No. 5,999,333 and used as substrates for evaluating transparent polyurethane compositions in the following examples. The preparation procedure can be summarized as follows: The acrylic sheets were first coated with a conventional polysiloxane hard coat agent as a base coating. The base coated acrylic sheets were then coated with a three-layer indium tin oxide (ITO) / gold / ITO thin film stack using a sputtering process to a sheet resistance of about 15 ohms / square. A 0.1% silicate coating solution is then flow coated onto the ITO surface coating and allowed to air dry for about 1 hour before being heated in an air oven at about 82°C for about 1 hour. A 0.1% aminosilane primer solution is then flow coated onto the silicate coating and allowed to air dry for about 1 hour. An 18% polyurethane thermoset adhesive solution in cyclohexanone, 3-ethoxypropionate (EEP), or other suitable solvent prepared from a moisture-curable aromatic polyether urethane based on methylene diphenyl diisocyanate (MDI) and polytetramethylene oxide polyol is flow coated onto the primed ITO coating and allowed to cure overnight at room temperature.

[0076] Table 2 summarizes the electrical volume resistivity results for the polyurethane compositions described in Examples 1-7 below. 14 An electrical volume resistivity greater than 0.05 means that the resistivity of the sample is not measurable or the sample will undergo dielectric breakdown during the p-static dissipation test.

[0077] [Table 2]

[0078] Example 1 Aliphatic polyester urethane compositions containing the lithium trifluoromethanesulfonimide additive Fluorad® HQ115 for electrical conductivity enhancement as described in Patent Document 1 are modified with Bayhydrol® 140AQ as shown in the formula in Table 3. Bayhydrol® 140AQ is a 40% solids aqueous dispersion of sulfonated polyester urethane polyol with sulfonate ion functionality incorporated into the backbone and hydroxyl functionality at the chain end. Bayhydrol® 140AQ is reacted with other polyols by first mixing at about 93°C to about 104°C for about 48 hours, and water is removed to form a homogeneous sulfonated polyol mixture. The sulfonated polyol mixture is then compounded with isocyanates and other ingredients in n-pentyl propionate solvent with about 50 ppm dibutyltin dilaurate catalyst to form a clear polyurethane precursor mixture with 70% solids. The resulting polyurethane precursor mixture was flow coated onto the prepared acrylic substrate and subsequently cured at about 54°C for about 12 hours and then at about 82°C for about 24 hours to form a clear polyurethane topcoat about 75-100 μm thick. Samples of the coated acrylic were exposed to accelerated QUV for 5 weeks. The accelerated QUV equipment was operated using UVB-313EL fluorescent lamps with cycles of about 7 hours of UV exposure at about 50°C and about 5 hours of condensation (UV off, high humidity) at about 50°C. The electrical volume resistivity of samples without QUV exposure and after 5 weeks of QUV exposure was measured at about -6°C, about -28°C and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2, above. The results show that the incorporation of sulfonated polyester urethane polyol from Bayhydrol® 140AQ into the composition can improve electrical conductivity compared to a composition without Bayhydrol® 140AQ, as described in US Patent No. 5,991,333. This improvement in conductivity is an additive effect of Fluorad™ HQ115 and Bayhydrol® 140AQ, with no strong synergistic interaction between these two components.This increase in conductivity does not provide the polyurethane with sufficient p-static dissipation capability at low temperatures, nor does it tolerate the deleterious effects of exposure to the elements. In separate experiments, it is also observed that increasing the concentration of the hydrophilic additive Fluorad™ HQ115 in the composition has limited effect on electrical conductivity and induces haze in the composition.

[0079] [Table 3]

[0080] Example 2 An aliphatic polyester urethane composition equivalent to that described in US Pat. No. 6,399,633, except for the replacement of the hydrophilic lithium trifluoromethanesulfonimide additive Fluorad™ HQ115 with the hydrophobic fluorinated ionic antistatic additive tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide FC-4400, was formulated using about 50 ppm of dibutyltin dilaurate catalyst in n-pentylpropionate solvent as shown in Table 4 to form a clear polyurethane precursor with a solids content of 70%. The resulting polyurethane precursor mixture was flow coated onto the prepared acrylic substrate and subsequently cured at about 54° C. for about 12 hours and then at about 82° C. for about 24 hours to form a clear polyurethane topcoat with a thickness of about 75-100 μm. Samples of the coated acrylic were exposed to accelerated QUV for 5 weeks. The QUV exposure procedure is described in Example 1. The electrical volume resistivity of the samples without QUV exposure and after 5 weeks of QUV exposure was measured at about -6°C, about -28°C, and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2, as described above. The results show that the hydrophobic fluorinated ionic antistatic additive FC-4400 is more effective at improving the electrical conductivity of the composition than the hydrophilic additive Fluorad™ HQ115, but this improvement in electrical conductivity cannot provide the polyurethane with sufficient p-static dissipation capability at low temperatures and tolerate the deleterious effects of exposure to the elements.

[0081] [Table 4]

[0082] Example 3 An aliphatic polyester urethane composition containing hydrophobic fluorinated ionic antistatic additive tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide FC-4400 and sulfonated polyester urethane polyol Bayhydrol® 140AQ is prepared as shown in the formula in Table 5. The sulfonated polyester urethane dispersion Bayhydrol® 140AQ is reacted with other polyols by first mixing at about 93°C to about 104°C for about 48 hours to remove water and form a homogeneous sulfonated polyol mixture. The sulfonated polyol mixture is then compounded with isocyanates and other ingredients in n-pentyl propionate solvent with about 50 ppm of dibutyltin dilaurate catalyst to form a transparent polyurethane precursor with a solid content of 70%. The resulting polyurethane precursor is flow coated onto the prepared acrylic substrate, followed by curing at about 54°C for about 12 hours and then at about 82°C for about 24 hours to form a transparent conductive topcoat with a thickness of about 75 to 100 μm. The coated acrylic samples are exposed to accelerated QUV for about 5 weeks. The QUV exposure procedure is described in Example 1. The electrical volume resistivity of the samples without QUV exposure and after 5 weeks of QUV exposure is measured at about -6°C, about -28°C, and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2 as described above. The results show that the incorporation of the hydrophobic fluorinated ionic antistatic additive FC-4400 in the composition together with the sulfonated polyester urethane polyol Bayhydrol® 140AQ can substantially improve the electrical conductivity significantly higher than the FC-4400 technical data sheet provided by the supplier 3M. It is believed that the synergistic interaction between the hydrophobic fluorinated ionic antistatic additive FC-4400 and the sulfonated polyester urethane matrix is ​​responsible for this substantial improvement in electrical conductivity. The improved electrical conductivity enables the material to withstand the deleterious effects of temperature changes and weathering exposure, and maintains the high p-static dissipative performance of the polyurethane regardless of temperature changes or weathering exposure.

[0083] [Table 5]

[0084] Example 4 Transparent aliphatic polyester urethane compositions with increasing content of hydrophobic fluorinated ionic antistatic additive FC-4400 were prepared as shown in Table 6 to further explore the synergistic interaction between the hydrophobic fluorinated ionic antistatic additive FC-4400 and the sulfonated polyester urethane polyol from Bayhydrol® 140AQ. The sulfonated polyester urethane dispersion Bayhydrol® 140AQ is first reacted with other polyols by mixing at about 93°C to about 104°C for about 48 hours to remove water and form a homogeneous sulfonated polyol mixture. The sulfonated polyol mixture is then compounded with isocyanates and other ingredients in n-pentyl propionate solvent with about 50 ppm of dibutyltin dilaurate catalyst to form a transparent polyurethane precursor with 70% solids. The resulting polyurethane precursor is flow coated onto the prepared acrylic substrate and subsequently cured at about 54°C for about 12 hours and then at about 82°C for about 24 hours to form a transparent conductive topcoat with a thickness of about 75-100 μm. The coated acrylic sample is exposed to accelerated QUV for about 5 weeks. The QUV exposure procedure is described in Example 1. The electrical volume resistivity of the sample without QUV exposure and the sample after 5 weeks of QUV exposure was measured at about -6°C, about -28°C and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2 above. The results show that increasing the content of hydrophobic fluorinated ionic antistatic additive FC-4400 further improves the overall electrical conductivity of the composition. The improved electrical conductivity allows it to withstand the harmful effects of temperature changes and exposure to the elements, maintaining the high p-static dissipative performance of the polyurethane regardless of temperature changes and exposure to the elements.

[0085] [Table 6]

[0086] Example 5 An aliphatic polyester urethane composition comparable to that described in Example 3 was prepared as per the formula shown in Table 7, except that the chain extender 1,4-butanediol (BDO) was removed from the composition. The sulfonated polyester urethane dispersion Bayhydrol® 140AQ is reacted with other polyols by first mixing at about 93°C to about 104°C for about 48 hours to remove water and form a homogenous sulfonated polyol mixture. The sulfonated polyol mixture is then compounded with isocyanates and other ingredients in n-pentyl propionate solvent with about 50 ppm of dibutyltin dilaurate catalyst to form a transparent polyurethane precursor with a 70% solids content. The resulting polyurethane precursor is flow coated onto a prepared acrylic substrate and subsequently cured at about 54°C for about 12 hours and then at about 82°C for about 24 hours to form a transparent conductive topcoat with a thickness of about 75 to 100 μm. The coated acrylic samples are exposed to accelerated QUV for about 5 weeks. The QUV exposure procedure is described in Example 1. The electrical volume resistivity of the samples without QUV exposure and after 5 weeks of QUV exposure was measured at about -6°C, about -28°C and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2 above. The results show that removing the chain extender 1,4-butanediol from the composition has a positive impact on electrical conductivity. The improved electrical conductivity allows the composition to withstand the deleterious effects of temperature changes and exposure to the elements, and maintains the high p-static dissipative performance of the polyurethane regardless of temperature changes and exposure to the elements.

[0087] [Table 7]

[0088] Accelerated QUV exposure Clear polyurethane coated acrylic samples were tested for light transmission, haze, adhesion, and overall appearance using accelerated QUV exposure for up to 5 weeks. The accelerated QUV equipment was operated using UVB-313EL fluorescent lamps at cycles of 50°C / 7 hours UV exposure and 50°C / 5 hours condensation (UV off, high humidity). Test samples were removed from the QUV equipment weekly and checked for light transmission (%), haze (%), adhesion (%), and overall appearance. Light transmission (%) and haze (%) were measured according to ASTM A2124-2000. D-1003. Percent adhesion was measured according to ASTM D-3359. Test results for the samples of Example 5 are shown in Table 8. The results show that the polyurethane exhibits virtually no degradation in light transmission, percent haze, percent adhesion and overall appearance upon QUV exposure, indicating excellent environmental durability against the deleterious effects of light and the elements.

[0089] [Table 8]

[0090] Rain Erosion Samples of clear polyurethane coated acrylic without QUV exposure and after 5 weeks of QUV exposure were tested for rain erosion resistance. Four samples were prepared from the coated acrylic with and without UV exposure. The coated acrylic was first cut to dimensions of about 2.54 cm by about 2.54 cm by about 0.635 cm, step machined across the top edge, and filled with a gray elastomeric material about 0.238 cm thick and about 0.476 cm wide, flush with the remaining sample surface, for mounting in the test holder. Rain erosion test parameters were an impact angle of about 30 degrees, rainfall of about 2.54 cm / hr, and test speed of about 927 km / hr. Sample pairs were tested at the end of a zero lift centripetal arm. The average size of the raindrops was about 2.0 mm. The test samples were inspected for delamination or damage to the topcoat before testing, about 10 minutes after exposure, about 30 minutes after exposure, and about 60 minutes after exposure. Test results for the samples of Example 5 are shown in Table 9. The results show that the polyurethane topcoat exhibits excellent erosion resistance with and without QUV exposure.

[0091] [Table 9]

[0092] Example 6 Transparent aliphatic polyester urethane compositions without the chain extender 1,4-butanediol (BDO) were prepared by increasing the content of hydrophobic fluorinated ionic antistatic additive FC-4400 in the composition as shown in the formula in Table 10. The sulfonated polyester urethane dispersion Bayhydrol 140 AQ is reacted with other polyols by first mixing at about 93°C to about 104°C for about 48 hours to remove water and form a homogeneous sulfonated polyol mixture. The sulfonated polyol mixture is then compounded with isocyanates and other ingredients in n-pentyl propionate solvent with about 50 ppm of dibutyltin dilaurate catalyst to form a transparent polyurethane precursor mixture with a solids content of 70%. The resulting polyurethane precursor mixture is flow coated onto the prepared acrylic substrate and subsequently cured at about 54°C for about 12 hours and then at about 82°C for about 24 hours to form a transparent polyurethane topcoat with a thickness of about 75 to 100 μm. The coated acrylic samples were exposed to accelerated QUV for 5 weeks. The QUV exposure procedure is described in Example 1. The electrical volume resistivity of the samples without QUV exposure and after 5 weeks of QUV exposure was measured at about -6°C, about -28°C, and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2 as described above. The results show that increasing the content of hydrophobic fluorinated ionic antistatic additive FC-4400 in the composition has a positive effect on electrical conductivity. The increased electrical conductivity allows the polyurethane to withstand the harmful effects of temperature changes and exposure to the elements, and maintains its high p-static dissipative performance regardless of temperature changes and exposure to the elements.

[0093] [Table 10]

[0094] Example 7 A transparent aliphatic polyester urethane composition with high content of FC-4400 and Bayhydrol 140 AQ was prepared as shown in the formula in Table 11 to further investigate the synergy between sulfonated polyester urethane polyols from hydrophobic fluorinated ionic antistatic additive FC-4400 and Bayhydrol® 140AQ. The sulfonated polyester urethane dispersion Bayhydrol® 140AQ is first reacted with other polyols by mixing at about 93°C to about 104°C for about 48 hours to remove water and form a homogeneous sulfonated polyol mixture. The sulfonated polyol mixture is then compounded with isocyanate and other ingredients in n-pentyl propionate solvent with about 50 ppm of dibutyltin dilaurate catalyst to form a transparent polyurethane precursor with 70% solids. The resulting polyurethane precursor is flow coated onto the prepared acrylic substrate, followed by curing at about 54°C for about 12 hours and then at about 82°C for about 24 hours to form a transparent conductive topcoat with a thickness of about 75-100 μm. The coated acrylic sample is exposed to accelerated QUV for about 5 weeks. The QUV exposure procedure is described in Example 1. The electrical volume resistivity of the sample without QUV exposure and the sample after 5 weeks of QUV exposure was measured at about -6°C, about -28°C and about -40°C using the method described in ASTM D-257. The electrical volume resistivity results are shown in Table 2 above. The results show that maximizing the content of hydrophobic fluorinated ionic antistatic additive FC-4400 and sulfonated polyester urethane dispersion Bayhydrol 140 AQ in the composition has a positive effect on electrical conductivity. The increased electrical conductivity allows the composition to withstand the harmful effects of temperature changes and exposure to the elements, and maintains the high p-static dissipative performance of the polyurethane regardless of temperature changes and exposure to the elements.

[0095] [Table 11]

[0096] The present invention has been described in detail with reference only to the presently preferred embodiments. Those skilled in the art will appreciate that various modifications can be made without departing from the invention. Accordingly, the present invention is defined solely by the scope of the following claims. The technical ideas that can be understood from the above-described embodiment will be described below as supplementary notes. [Appendix 1] 1. A polyurethane composition suitable for coating a surface of a substrate, said composition comprising: An aliphatic polyester urethane matrix and a fluorinated ionic antistatic additive, the aliphatic polyester urethane matrix comprising: an aliphatic diisocyanate; a polyester polyol having a polyester diol and a polyester triol; a sulfonated polyester urethane polyol; A composition comprising: [Appendix 2] 2. The composition of claim 1, wherein the aliphatic diisocyanate is selected from the group consisting of hexamethylene diisocyanate, methylene bis(4-cyclohexyl isocyanate) and isophorone diisocyanate. [Appendix 3] 3. The composition of claim 2, wherein the polyester diol has an average molecular weight of about 830 g / mole and comprises a polycaprolactone diol initiated with diethylene glycol. [Appendix 4] 4. The composition of claim 3, wherein the polyester triol has an average molecular weight of about 540 g / mole and comprises a polycaprolactone triol initiated with trimethylolpropane. [Appendix 5] 5. The composition of claim 4, wherein the polyester polyol further comprises a chain extender selected from the group consisting of ethylene glycol, 1,4-butanediol, and 2-ethyl-1,3-hexanediol. [Appendix 6] 5. The composition of claim 4, wherein the sulfonated polyesterurethane polyol comprises an anionic dispersion of an aliphatic polyesterurethane resin. [Appendix 7] 7. The composition according to claim 6, wherein the sulfonated polyester urethane polyol is about 5% to about 10% by weight of the composition. [Appendix 8] 8. The composition according to claim 7, wherein the aliphatic polyester urethane matrix is ​​about 85% to about 98% by weight of the composition. [Appendix 9] 9. The composition of claim 8, wherein the fluorinated ionic antistatic additive comprises a quaternary ammonium salt of a fluorinated sulfonimide selected from the group consisting of tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide and quaternary alkylammonium bis-(trifluoromethanesulfonyl)imide. [Appendix 10] 10. The composition of claim 9, wherein the fluorinated ionic antistatic additive is about 3% to about 8% by weight of the composition. [Appendix 11] 1. A method for preparing a polyurethane composition suitable for coating a surface of a substrate, the method comprising: mixing a polyester diol and a polyester triol with the sulfonated polyester urethane dispersion to form a homogeneous sulfonated polyol mixture; mixing the homogeneous sulfonated polyol mixture with ingredients including an aliphatic diisocyanate, a fluorinated ionic antistatic additive, and a catalyst to form a polyurethane coating composition; The method includes: [Appendix 12] 12. The method of claim 11, wherein the sulfonated polyester urethane dispersion is mixed with a polyester diol and a polyester triol at about 90° C. to about 105° C. for about 48 hours. [Appendix 13] 13. The method of claim 12, wherein the polyester diol has an average molecular weight of about 830 g / mol and comprises a polycaprolactone diol initiated with diethylene glycol. [Appendix 14] 14. The method of claim 13, wherein the polyester triol has an average molecular weight of about 540 g / mol and comprises a polycaprolactone triol initiated with trimethylolpropane. [Appendix 15] 15. The method of claim 14, wherein the sulfonated polyester urethane dispersion comprises an anionic dispersion of an aliphatic polyester urethane resin and is about 5% to about 10% by weight of the composition. [Appendix 16] 16. The method of claim 15, wherein the aliphatic diisocyanate comprises methylene bis(4-cyclohexyl isocyanate). [Appendix 17] 17. The method of claim 16, wherein the fluorinated ionic antistatic additive comprises tri-n-butylmethylammonium bis-(trifluoromethanesulfonyl)imide and is about 3% to about 8% by weight of the composition. [Appendix 18] The method according to claim 17 further comprises: coating a surface with the polyurethane composition; curing the coated surface at a first curing temperature of about 50° C. to about 60° C. for about 12 hours; re-curing the coated surface at a second curing temperature of about 75°C to about 85°C for about 24 hours; The method includes: [Appendix 19] 19. The method of claim 18, wherein the coating is transparent and the substrate is a clear acrylic. [Appendix 20] 20. The method of claim 19, wherein the surface is an exterior surface of an aircraft transparency. [Appendix 21] 21. The method of claim 20, wherein the first cure temperature is about 54° C. and the second cure temperature is about 82° C. [Appendix 22] The method of claim 21, further comprising preparing a surface prior to coating the surface with the transparent polyurethane composition, the preparing step comprising: coating the surface with a polysiloxane coating to form a base coated surface; coating the base-coated surface with a three-layer indium tin oxide (ITO) / gold / ITO film stack to form an ITO-coated surface; coating the ITO-coated surface with a 0.1% silicate coating solution to form a silicate-coated surface; heating the silicate-coated surface at about 82° C. for about 1 hour; coating the silicate-coated surface with a 0.1% aminosilane primer solution to form an aminosilane-coated surface; coating the aminosilane coated surface with an 18% polyurethane thermoset adhesive solution to form a polyurethane thermoset coated surface; Curing the polyurethane thermosetting coating surface at about 20°C to about 25°C for about 16 hours; A method comprising: [Appendix 23] A laminate, the laminate comprising: a coating disposed on a surface of a substrate, the coating comprising: The polyurethane composition includes an aliphatic polyester urethane matrix and a fluorinated ionic antistatic additive, the aliphatic polyester urethane matrix comprising: an aliphatic diisocyanate; a polyester polyol having a polyester diol and a polyester triol; a sulfonated polyester urethane polyol; Including, laminate. [Appendix 24] 24. The laminate of claim 23, wherein the coating has a thickness of about 75 μm to about 100 μm. [Appendix 25] The coating is heated to about -40°C for about 10 11 25. The laminate of claim 24, having an electrical volume resistivity of less than or equal to ohms / cm. [Appendix 26] 26. The laminate of claim 25, wherein the coating has a luminous transmittance of about 65% to about 70%. [Appendix 27] 27. The laminate of claim 26, wherein the coating has a haze of about 0.90% to about 1.40%. [Appendix 28] 28. The laminate of claim 27, wherein the coating does not include an ionizable metal salt of a perfluoroalkylsulfonate or a colloidal indium tin oxide nanoparticle dispersion. [Appendix 29] 28. The laminate of claim 27, wherein the coating is transparent and the substrate is a clear acrylic. [Appendix 30] 30. The laminate of claim 29, wherein the surface is an exterior surface of an aircraft transparency.

Claims

1. 1. A polyurethane composition suitable for coating a surface of a substrate, said composition comprising: comprising an aliphatic polyester urethane matrix and a fluorinated ionic antistatic additive; The composition, when coated on the surface of the substrate, has an electrical volume resistivity of about 10 11 ohms / cm or less at about -40°C, the aliphatic polyester urethane matrix comprises a sulfonated polyester urethane polyol, and the fluorinated ionic antistatic additive comprises a quaternary ammonium salt of a fluorinated sulfonimide.

2. The composition described in claim 1, wherein the aliphatic polyester urethane matrix further comprises an aliphatic diisocyanate and a polyester polyol including a polyester diol and a polyester triol.

3. A method for coating a surface of a substrate with a polyurethane composition, the method comprising: A method comprising flow coating the surface with the polyurethane composition of claim 1 to form a coated surface.

4. The method of claim 3, wherein the surface is an outer surface of a transparent body of an aircraft.

5. A laminate, the laminate comprising: a coating disposed on a surface of a substrate; The coating comprises an aliphatic polyester urethane matrix and a fluorinated ionic antistatic additive; The coating has an electrical volume resistivity of about 10 11 ohms / cm or less at about -40°C, the aliphatic polyesterurethane matrix comprises a sulfonated polyesterurethane polyol, and the fluorinated ionic antistatic additive comprises a quaternary ammonium salt of a fluorinated sulfonimide.

6. The laminate of claim 5, wherein the coating is transparent.

7. The laminate of claim 5, wherein the coating has a thickness of about 75 μm to about 100 μm.

8. The laminate of claim 6 , wherein the coating has a luminous transmittance of greater than about 65%.

9. 9. The laminate of claim 8, wherein the coating has a haze value of less than about 1.50%.

10. 6. The laminate of claim 5, wherein the coating does not include an ionizable metal salt of a perfluoroalkylsulfonate or a colloidal indium tin oxide nanoparticle dispersion.

11. 11. The laminate of claim 10, wherein the coating is clear and the substrate is a clear acrylic.

12. 12. The laminate of claim 11, wherein the surface is an exterior surface of an aircraft transparency.

Citation Information

Patent Citations

  • Antistatic, optically transparent, pressure-sensitive adhesive

    JP2010523806A

  • Transparent polyurethane protective coating, film and laminate composition with enhanced electrostatic dissipation capability, and methods for making the same

    JP2012040870A

  • Electrostatic dissipative TPU and its composition

    JP2013508474A

  • Electrophotographic member, process cartridge, and electrophotographic apparatus

    JP2015232704A

  • Surface protective film

    JP2016186010A