Resin composition

A resin composition combining epoxy resin, active ester curing agent, and hydrocarbon polymer with a terpene skeleton addresses the need for insulating layers with low dielectric loss tangent and crack resistance, enhancing the performance of printed wiring boards and semiconductor devices.

JP7593372B2Active Publication Date: 2024-12-03AJINOMOTO CO INC
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2022079273
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-05-13
Publication Date
2024-12-03
Estimated Expiration
2042-05-13

AI Technical Summary

Technical Problem

There is a demand for insulating layers in printed wiring boards with low dielectric loss tangent and excellent crack resistance, which existing technologies have not adequately addressed.

Method used

A resin composition is formulated using epoxy resin, an active ester curing agent, and a hydrocarbon polymer containing a terpene skeleton, optionally combined with other components like inorganic fillers and radically polymerizable compounds, to achieve a cured product with low dielectric loss tangent and improved crack resistance.

Benefits of technology

The resin composition results in a cured product with a low dielectric loss tangent, excellent crack resistance, and high glass transition temperature, suitable for use in insulating layers of printed wiring boards and semiconductor devices.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593372000001
    Figure 0007593372000001
  • Figure 0007593372000002
    Figure 0007593372000002
  • Figure 0007593372000003
    Figure 0007593372000003
Patent Text Reader

Abstract

To provide a resin composition that can yield a cured product with low dielectric loss tangent and superior crack resistance, and the like.SOLUTION: A resin composition contains (A) an epoxy resin, (B) an active ester compound, and (C) a hydrocarbon polymer having a terpene skeleton.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, and further to a sheet-like laminate material, a resin sheet, a printed wiring board, and a semiconductor device obtained by using the resin composition. [Background technology]

[0002] A known manufacturing technique for printed wiring boards is a build-up method in which insulating layers and conductor layers are alternately stacked. In the build-up method, the insulating layers are generally formed by curing a resin composition.

[0003] Various maleimide compounds containing a non-aromatic ring skeleton have been known so far (Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2019-203122 A Summary of the Invention [Problem to be solved by the invention]

[0005] In recent years, there has been a demand for insulating layers having a low dielectric tangent and excellent crack resistance.

[0006] An object of the present invention is to provide a resin composition capable of giving a cured product having a low dielectric tangent and excellent crack resistance, and a sheet-like laminate material, a resin sheet, a printed wiring board, and a semiconductor device obtained using the resin composition. [Means for solving the problem]

[0007] Means for Solving the Problems of the Invention The present inventors conducted intensive research and found that by incorporating a combination of an epoxy resin, an active ester-based curing agent, and a hydrocarbon polymer containing a terpene skeleton as components of a resin composition into the resin composition, it is possible to obtain a cured product having a low dielectric tangent and excellent crack resistance, which led to the completion of the present invention.

[0008] That is, the present invention includes the following. [1] (A) epoxy resin, (B) an active ester compound, and (C) A resin composition containing a hydrocarbon polymer having a terpene skeleton. [2] The resin composition according to [1], wherein the component (C) contains either a polyterpene resin or an aromatic modified terpene resin. [3] The resin composition according to [1] or [2], wherein the component (C) does not have a polar group. [4] The resin composition according to any one of [1] to [3], wherein the softening point of component (C) is 50° C. or higher. [5] The resin composition according to any one of [1] to [4], wherein the content of the component (C) is 1 mass % or more, relative to 100 mass % of the resin component. [6] The resin composition according to any one of [1] to [5], further comprising (D) a radically polymerizable compound. [7] The resin composition according to any one of [1] to [6], further comprising (E) an inorganic filler. [8] The resin composition according to [7], wherein the content of the (E) component is 40 mass% or more, relative to 100 mass% of the non-volatile components in the resin composition. [9] The resin composition according to any one of [1] to [8], further comprising (F) a curing agent.

[10] A sheet-like laminate material comprising the resin composition according to any one of [1] to [9].

[11] A resin sheet comprising a support and a resin composition layer formed on the support from the resin composition according to any one of [1] to [9].

[12] A printed wiring board having an insulating layer made of a cured product of the resin composition according to any one of [1] to [9].

[13] A semiconductor device comprising the printed wiring board according to

[12] . Effect of the Invention

[0009] According to the resin composition of the present invention, it is possible to provide a resin composition capable of giving a cured product having a low dielectric tangent and excellent crack resistance, and a sheet-like laminate material, a resin sheet, a printed wiring board, and a semiconductor device obtained using the resin composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below based on its preferred embodiments. However, the present invention is not limited to the following embodiments and examples, and can be modified as desired without departing from the scope of the claims of the present invention and their equivalents. In the present invention, the content of each component in the resin composition is the value when the non-volatile components in the resin composition are 100 mass %, unless otherwise specified. In addition, in this specification, "dielectric constant" means "relative dielectric constant" unless otherwise specified.

[0011] [Resin composition] The resin composition of the present invention includes (A) an epoxy resin, (B) an active ester compound, and (C) a hydrocarbon polymer containing a terpene skeleton. By using such a resin composition, a cured product having a low dielectric tangent (Df) and excellent crack resistance can be obtained. In addition, the resin composition can also provide a cured product having a high glass transition temperature (Tg) and a low relative dielectric constant (Dk).

[0012] It has been known that (C) a hydrocarbon polymer containing a terpene skeleton is used for adhesive applications. However, the present inventors have found that by incorporating (C) a hydrocarbon polymer containing a terpene skeleton into a resin composition, it is possible to obtain a cured product having excellent dielectric tangent and crack resistance, and have found that the dielectric tangent is particularly excellent even at high temperatures. As far as the present inventors know, the technical idea of ​​obtaining a cured product having excellent dielectric tangent and crack resistance by incorporating (C) a hydrocarbon polymer containing a terpene skeleton into a resin composition used for insulation applications has not been proposed at all in the past.

[0013] The resin composition of the present invention may further contain optional components in combination with the components (A) to (C). Examples of the optional components include a radical polymerizable compound (D), an inorganic filler (E), a curing agent (F), a curing accelerator (G), other additives (H), and a solvent (I). Each component contained in the resin composition will be described in detail below.

[0014] <(A) Epoxy resin> The resin composition contains, as component (A), an epoxy resin (A), which is a curable resin having an epoxy group.

[0015] Examples of the (A) epoxy resin include bixylenol type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bisphenol AF type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol novolac type epoxy resin, phenol novolac type epoxy resin, tert-butyl-catechol type epoxy resin, naphthalene type epoxy resin, naphthol type epoxy resin, anthracene type epoxy resin, glycidylamine type epoxy resin, glycidyl ester type epoxy resin, and the like. Examples of the epoxy resins include cresol novolac type epoxy resins, phenol aralkyl type epoxy resins, biphenyl type epoxy resins, linear aliphatic epoxy resins, epoxy resins having a butadiene structure, alicyclic epoxy resins, heterocyclic epoxy resins, spiro ring-containing epoxy resins, cyclohexane type epoxy resins, cyclohexane dimethanol type epoxy resins, naphthylene ether type epoxy resins, trimethylol type epoxy resins, tetraphenylethane type epoxy resins, isocyanurate type epoxy resins, phenolphthalimidine type epoxy resins, phenolphthalein type epoxy resins, etc. (A) The epoxy resins may be used alone or in combination of two or more.

[0016] The resin composition preferably contains, as the (A) epoxy resin, an epoxy resin having two or more epoxy groups in one molecule. The proportion of the epoxy resin having two or more epoxy groups in one molecule relative to 100% by mass of the non-volatile components of the (A) epoxy resin is preferably 50% by mass or more, more preferably 60% by mass or more, and particularly preferably 70% by mass or more.

[0017] Epoxy resins include epoxy resins that are liquid at a temperature of 20° C. (hereinafter sometimes referred to as "liquid epoxy resins") and epoxy resins that are solid at a temperature of 20° C. (hereinafter sometimes referred to as "solid epoxy resins"). The resin composition may contain only liquid epoxy resins as the epoxy resins, may contain only solid epoxy resins, or may contain a combination of liquid epoxy resins and solid epoxy resins.

[0018] The liquid epoxy resin is preferably a liquid epoxy resin having two or more epoxy groups in one molecule.

[0019] As the liquid epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol AF type epoxy resin, naphthalene type epoxy resin, glycidyl ester type epoxy resin, glycidyl amine type epoxy resin, phenol novolac type epoxy resin, alicyclic epoxy resin having an ester skeleton, cyclohexane type epoxy resin, cyclohexane dimethanol type epoxy resin, and epoxy resin having a butadiene structure are preferred, and naphthalene type epoxy resin is more preferred.

[0020] Specific examples of liquid epoxy resins include "HP4032", "HP4032D", and "HP4032SS" (naphthalene type epoxy resins) manufactured by DIC Corporation; "828US", "828EL", "jER828EL", "825", and "Epicoat 828EL" (bisphenol A type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER807" and "1750" (bisphenol F type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "jER152" (phenol novolac type epoxy resin) manufactured by Mitsubishi Chemical Corporation; "630", "630LSD", and "604" (glycidylamine type epoxy resins) manufactured by Mitsubishi Chemical Corporation; "ED-523T" (glycirol type epoxy resin) manufactured by ADEKA Corporation; and "EP-3950L" and "EP-3980S" (glycidylamine type epoxy resins) manufactured by ADEKA Corporation. glycidylamine type epoxy resin); ADEKA's "EP-4088S" (dicyclopentadiene type epoxy resin); Nippon Steel Chemical & Material Chemical's "ZX1059" (mixture of bisphenol A type epoxy resin and bisphenol F type epoxy resin); Nagase Chemtex's "EX-721" (glycidyl ester type epoxy resin); Daicel's "Celloxide 2021P" (alicyclic epoxy resin having an ester skeleton); Daicel's "PB-3600", Nippon Soda's "JP-100" and "JP-200" (epoxy resin having a butadiene structure); Nippon Steel Chemical & Material Chemical's "ZX1658" and "ZX1658GS" (liquid 1,4-glycidylcyclohexane type epoxy resin), etc. These may be used alone or in combination of two or more types.

[0021] As the solid epoxy resin, a solid epoxy resin having three or more epoxy groups in one molecule is preferable, and an aromatic solid epoxy resin having three or more epoxy groups in one molecule is more preferable.

[0022] As the solid epoxy resin, bixylenol type epoxy resin, naphthalene type epoxy resin, naphthalene type tetrafunctional epoxy resin, naphthol novolac type epoxy resin, cresol novolac type epoxy resin, dicyclopentadiene type epoxy resin, trisphenol type epoxy resin, naphthol type epoxy resin, biphenyl type epoxy resin, naphthylene ether type epoxy resin, anthracene type epoxy resin, bisphenol A type epoxy resin, bisphenol AF type epoxy resin, phenol aralkyl type epoxy resin, tetraphenylethane type epoxy resin, phenolphthalimidine type epoxy resin, and phenolphthalein type epoxy resin are preferred, and naphthalene type epoxy resin and biphenyl type epoxy resin are more preferred.

[0023] Specific examples of solid epoxy resins include "HP4032H" (naphthalene type epoxy resin) manufactured by DIC Corporation; "HP-4700" and "HP-4710" (naphthalene type tetrafunctional epoxy resins) manufactured by DIC Corporation; "N-690" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "N-695" (cresol novolac type epoxy resin) manufactured by DIC Corporation; "HP-7200", "HP-7200HH", "HP-7200H", and "HP-7200L" (dicyclopentadiene type epoxy resins) manufactured by DIC Corporation; and "EXA-7311" manufactured by DIC Corporation. , "EXA-7311-G3", "EXA-7311-G4", "EXA-7311-G4S", "HP6000" (naphthylene ether type epoxy resin); "EPPN-502H" (trisphenol type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC7000L" (naphthol novolac type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.; "NC3000H", "NC3000", "NC3000L", "NC3000FH", "NC3100" (biphenyl type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN475V", "ESN4 100V" (naphthalene type epoxy resin); "ESN485" (naphthol type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "ESN375" (dihydroxynaphthalene type epoxy resin) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "YX4000H", "YX4000", "YX4000HK", "YL7890" (bixylenol type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YL6121" (biphenyl type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "YX8800" (anthracene type epoxy resin) manufactured by Mitsubishi Chemical Co., Ltd.; "Y Examples of epoxy resins include "X7700" (phenol aralkyl type epoxy resin); "PG-100" and "CG-500" manufactured by Osaka Gas Chemicals; "YL7760" (bisphenol AF type epoxy resin) manufactured by Mitsubishi Chemical; "YL7800" (fluorene type epoxy resin) manufactured by Mitsubishi Chemical; "jER1010" (bisphenol A type epoxy resin) manufactured by Mitsubishi Chemical; "jER1031S" (tetraphenylethane type epoxy resin) manufactured by Mitsubishi Chemical; and "WHR991S" (phenolphthalimidine type epoxy resin) manufactured by Nippon Kayaku Co., Ltd.These may be used alone or in combination of two or more.

[0024] When a solid epoxy resin and a liquid epoxy resin are used in combination as the (A) epoxy resin, the mass ratio thereof (solid epoxy resin:liquid epoxy resin) is preferably 1:0.01 to 1:50, more preferably 1:0.05 to 1:10, and particularly preferably 1:0.1 to 1:3. By setting the mass ratio of the liquid epoxy resin to the solid epoxy resin within this range, the following effects can be obtained: 1) when used in the form of a resin sheet, appropriate adhesion is provided, 2) when used in the form of a resin sheet, sufficient flexibility is obtained and handling is improved, and 3) a cured product having sufficient breaking strength can be obtained.

[0025] The epoxy equivalent of the (A) epoxy resin is preferably 50 g / eq. to 5,000 g / eq., more preferably 60 g / eq. to 2,000 g / eq., even more preferably 70 g / eq. to 1,000 g / eq., and even more preferably 80 g / eq. to 500 g / eq. The epoxy equivalent is the mass of the resin per equivalent of epoxy group. This epoxy equivalent can be measured according to JIS K7236.

[0026] The weight average molecular weight (Mw) of the epoxy resin (A) is preferably from 100 to 5,000, more preferably from 250 to 3,000, and further preferably from 400 to 1500. The weight average molecular weight of the resin can be measured by gel permeation chromatography (GPC) as a polystyrene-equivalent value.

[0027] The content of the epoxy resin (A) is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability. The upper limit of the content of the epoxy resin is preferably 25% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on 100% by mass of the non-volatile components in the resin composition, from the viewpoint of obtaining the desired effects of the present invention significantly.

[0028] From the viewpoint of obtaining a cured product exhibiting good mechanical strength and insulation reliability, the content of the (A) epoxy resin, relative to 100 mass% of the resin component in the resin composition, is preferably 10 mass% or more, more preferably 20 mass% or more, and even more preferably 30 mass% or more, and the upper limit is preferably 60 mass% or less, more preferably 50 mass% or less, and even more preferably 40 mass% or less.

[0029] In the present invention, the "resin component" of the resin composition refers to the non-volatile components constituting the resin composition excluding the inorganic filler (E) described below.

[0030] <(B) Active ester compound> The resin composition contains an active ester compound (B) as the component (B). The active ester compound (B) has the function of curing the epoxy resin (A). The active ester compound (B) as the component (B) does not include those that fall under the above-mentioned component (A). The active ester compound (B) may be used alone or in combination of two or more kinds.

[0031] As the (B) active ester compound, a compound having an active ester group as an active group that reacts with the (A) epoxy resin can be used. Specifically, as the (B) component, it is preferable to include either a compound having a structure represented by formula (B-1) or a compound containing an aromatic ester skeleton and an unsaturated bond.

[0032] (Compound having a structure represented by formula (B-1)) One embodiment of the component (B) is preferably a compound having a structure represented by formula (B-1). [ka] In the formula, R 1 , R 2 and R 3 (1)R 1 is a hydrogen atom, a halogen atom, a methyl group, or R 11-A- and R 2 and R 3 each independently represents a hydrogen atom or a substituent, or (2) R 1 and R 2 are linked together to form an aromatic carbocyclic ring which may have a substituent, and R 3 represents a hydrogen atom or a substituent, or (3) R 2 and R 3 are linked together to form an aromatic carbocyclic ring which may have a substituent, and R 1 is a hydrogen atom, a halogen atom, a methyl group, or R 11 -A- stands for;R 4 and R 5 each independently represents a hydrogen atom or a substituent; R 11 represents an optionally substituted alkyl group, an optionally substituted alkenyl group, or an optionally substituted aryl group; A represents -CH2-, -CH(CH3)-, -CO-, or -O-; * represents a bonding site.

[0033] R 1 When R does not form an aromatic carbocyclic ring, R is a hydrogen atom, a halogen atom, a methyl group, or 11 Represents -A-. R 1 When R does not form an aromatic carbocyclic ring, in one embodiment, R is preferably a hydrogen atom, a methyl group, or 11 -A-; more preferably, a hydrogen atom or R 11 -A-.

[0034] A represents -CH2-, -CH(CH3)-, -CO-, or -O-. In one embodiment, A is preferably -CH2- or -CH(CH3)-; more preferably -CH(CH3)-.

[0035] R 11 represents an alkyl group which may have a substituent, an alkenyl group which may have a substituent, or an aryl group which may have a substituent.

[0036] R 11The alkyl group, alkenyl group, and aryl group represented by may have a substituent. Examples of the substituent include a halogen atom, an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group (an alkyl group substituted with an aryl group), an alkyl-aryl-alkyl group (an alkyl group substituted with an aryl group substituted with an alkyl group), an alkenyl-aryl-alkyl group (an alkyl group substituted with an aryl group substituted with an alkenyl group), an aryl-aryl-alkyl group (an alkyl group substituted with an aryl group substituted with an aryl group), an alkyl-aryl group, an alkenyl-aryl group, an aryl-aryl group, an alkyl-oxy group, an alkenyl-oxy group, an aryl-oxy group, an alkyl-carbonyl group, an alkenyl-carbonyl group, an aryl-carbonyl group, an alkyl-oxy-carbonyl group, an alkenyl-oxy-carbonyl group, an aryl-oxy-carbonyl group, an alkyl-carbonyl-oxy group, an alkenyl-carbonyl-oxy group, and an aryl-carbonyl-oxy group.

[0037] R 11 In one embodiment, is preferably an aryl group which may have a substituent; more preferably an aryl group; and particularly preferably a phenyl group.

[0038] R 2 and R 3 and each independently represent a hydrogen atom or a substituent, when they do not form an aromatic carbocyclic ring.

[0039] R 2 and R 3 The substituent represented by the formula: 11 The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0040] R 2 and R 3When not forming an aromatic carbocyclic ring, in one embodiment, each independently is preferably a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, or an alkyl-aryl group; more preferably a hydrogen atom, an alkyl group, an aryl group, or an aryl-alkyl group.

[0041] R 1 , R 2 and R 3 When it forms an aromatic carbocyclic ring, R 1 and R 2 Or R 2 and R 3 are linked together to form an aromatic carbocyclic ring which may be substituted.

[0042] R 1 , R 2 and R 3 The substituents in the aromatic carbocyclic ring formed by R 11 The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0043] R 1 , R 2 and R 3 When R forms an aromatic carbocyclic ring, in one embodiment, 1 and R 2 Or R 2 and R 3 are bonded together to preferably form a benzene ring which may have a substituent; more preferably form a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group; and even more preferably form an (unsubstituted) benzene ring.

[0044] R 4 and R 5 each independently represents a hydrogen atom or a substituent.

[0045] R 4 and R 5 The substituent represented by the formula: 11The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0046] R 4 and R 5 are each independently, in one embodiment, preferably a hydrogen atom, an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, or an alkyl-aryl group; more preferably a hydrogen atom, an alkyl group, an aryl group, or an aryl-alkyl group.

[0047] In the first embodiment, preferably, R 1 , R 2 , R 4 and R 5 is a hydrogen atom, and R 3 is an alkyl group or an aryl group; more preferably, R 1 , R 2 , R 4 and R 5 is a hydrogen atom, and R 3 is a methyl group or a phenyl group.

[0048] In the second embodiment, preferably, R 1 is a hydrogen atom or R 11 -A-, A is -CH2- or -CH(CH3)-, R 11 is an aryl group, and R 2 , R 3 , R 4 and R 5 is a hydrogen atom or an aryl-alkyl group (particularly preferably, R 1 R 11 -A- and / or R 2 , R 3 , R 4 and R 5 at least one of R is an aryl-alkyl group; more preferably, R 1 is a hydrogen atom or R 11 -A-, A is -CH(CH3)-, and R 11 is a phenyl group, and R 2 , R 3, R 4 and R 5 is a hydrogen atom or an α-methylbenzyl group (particularly preferably, R 1 R 11 -A- and / or R 2 , R 3 , R 4 and R 5 at least one of which is an α-methylbenzyl group).

[0049] In the third embodiment, preferably, R 1 and R 2 are bonded together to form a benzene ring, and R 3 , R 4 and R 5 is a hydrogen atom, or R 2 and R 3 are bonded together to form a benzene ring, and R 1 , R 4 and R 5 is a hydrogen atom.

[0050] In a preferred embodiment, the component (B) is a compound having a structure represented by formula (B-2). [ka] In the formula, ring 1 each independently represents an optionally substituted aromatic carbocycle or an optionally substituted non-aromatic carbocycle; ring Y 1 and ring Z 1 each independently represents an aromatic carbocyclic ring which may have a substituent; X b are each independently a single bond, -C(R b )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-; R b each independently represents a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, or two R bare bonded together to form a non-aromatic carbocyclic ring which may have a substituent; b' represents 0 or an integer of 1 or more; each c' independently represents 0, 1, 2, or 3; each d' independently represents 0 or 1; and other symbols are as described above. The b' and c' units may be the same or different for each structural unit.

[0051] Ring X 1 each independently represents an aromatic carbocyclic ring which may have a substituent, or a non-aromatic carbocyclic ring which may have a substituent.

[0052] Ring X 1 The substituents in the aromatic carbocycle represented by the formula: 11 The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0053] Ring X 1 are each independently, in one embodiment, preferably a benzene ring which may have a substituent, a naphthalene ring which may have a substituent, or a non-aromatic carbon ring having 5 to 12 carbon atoms which may have a substituent; and more preferably, (1) a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group, (2) a naphthalene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group, or (3) a non-aromatic carbon ring having 5 to 12 carbon atoms which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, an alkyl-aryl group, and an oxo group (particularly preferably a tetrahydrodicyclopentadiene ring).

[0054] Ring Y 1 each independently represents an aromatic carbocyclic ring which may have a substituent.

[0055] Ring Y 1 The substituents in the aromatic carbocycle represented by the formula: 11The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0056] Ring Y 1 are each independently, in one embodiment, preferably a benzene ring which may have a substituent, or a naphthalene ring which may have a substituent; and more preferably, (1) a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group, or (2) a naphthalene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group.

[0057] Ring Z 1 each independently represents an aromatic carbocyclic ring which may have a substituent.

[0058] Ring Z 1 The substituents in the aromatic carbocycle represented by the formula: 11 The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0059] Ring Z 1 are each independently, in one embodiment, preferably a benzene ring which may have a substituent, or a naphthalene ring which may have a substituent; and more preferably, (1) a benzene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group, or (2) a naphthalene ring which may be substituted with a group selected from an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, and an alkyl-aryl group.

[0060] X b are each independently a single bond, -C(R b )2-, -O-, -CO-, -S-, -SO-, -SO2-, -CONH-, or -NHCO-. X b are each independently, in one embodiment, preferably a single bond, -C(Rb ) 2-, or -O-; more preferably, a single bond or -O-.

[0061] R b each independently represents a hydrogen atom, an optionally substituted alkyl group, or an optionally substituted aryl group, or two R b R are linked together to form a non-aromatic carbocyclic ring which may be substituted. b The substituents in the alkyl group represented by the formula R 11 The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0062] R b are each independently, in one embodiment, preferably a hydrogen atom or an alkyl group which may have a substituent; more preferably a hydrogen atom or an alkyl group; and particularly preferably a hydrogen atom or a methyl group.

[0063] b' represents 0 or an integer of 1 or more. In one embodiment, b' is preferably 0 or an integer of 1 to 100; more preferably 0 or an integer of 1 to 10; and particularly preferably 0 or an integer of 1 to 5.

[0064] Each c' independently represents 0, 1, 2, or 3. Each c' independently in one embodiment is preferably 0, 1, or 2; more preferably 0 or 1.

[0065] Each d' independently represents 0 or 1.

[0066] Examples of the partial structure represented by formula (Y') in formula (B-2) include structures represented by formulas (Y-1) to (Y-12) and the like. [ka] In the formula, Y 1 represents an aromatic carbocyclic ring which may have a substituent. [ka] In the formula, R y each independently represents an alkyl group, an alkenyl group, an aryl group, an aryl-alkyl group, or an alkyl-aryl group; each y independently represents 0, 1, or 2; and other symbols are as defined above.

[0067] The component (B) may contain, in addition to the resin represented by formula (B-2), a reaction intermediate resin generated during synthesis (e.g., a resin having a hydroxy group and / or a carboxy group at one or both ends), a resin derived from raw material impurities, etc.

[0068] The compound having the structure represented by formula (B-1) may be a commercially available product, or may be synthesized by a known method or a method similar thereto. Commercially available products of the compound having the structure represented by formula (B-1) include active ester compounds containing a dicyclopentadiene-type diphenol structure, such as "EXB9451", "EXB9460", "EXB9460S", "HPC-8000-65T", "HPC-8000L-65TM", "HPC-8000H", and "HPC-8000H-65TM" (manufactured by DIC Corporation); active ester compounds containing a naphthalene structure, such as "HP-B-8151-62T", "EXB-8100L-65T", "EXB-9416-70BK", "EXB-8", Examples of active ester compounds that include "HPC-8150-62T" (manufactured by DIC Corporation); "EXB9401" (manufactured by DIC Corporation) as a phosphorus-containing active ester compound; "DC808" (manufactured by Mitsubishi Chemical Corporation) as an active ester compound which is an acetylated product of phenol novolac; "YLH1026", "YLH1030", and "YLH1048" (manufactured by Mitsubishi Chemical Corporation) as active ester compounds which are benzoylated products of phenol novolac; and "PC1300-02-65MA" (manufactured by Air Water Corporation) as an active ester compound containing a styryl group and a naphthalene structure.

[0069] (Compound containing an aromatic ester skeleton and an unsaturated bond) Another embodiment of the component (B) is a compound containing an aromatic ester skeleton and an unsaturated bond.

[0070] The compound containing an aromatic ester skeleton and an unsaturated bond has an aromatic ester skeleton. The aromatic ester skeleton refers to a skeleton having an ester bond and an aromatic ring bonded to one end or both ends of the ester bond. Among them, those having aromatic rings at both ends of the ester bond are preferred. Examples of groups having such a skeleton include an arylcarbonyloxy group, an aryloxycarbonyl group, an arylenecarbonyloxy group, an aryleneoxycarbonyl group, an arylcarbonyloxyarylene group, an aryloxycarbonylarylene group, an arylenecarbonyloxyarylene group, and an aryleneoxycarbonylarylene group. The number of carbon atoms of the group having such a skeleton is preferably 7 to 20, more preferably 7 to 15, and even more preferably 7 to 11. The aromatic hydrocarbon group such as an aryl group and an arylene group may have a substituent.

[0071] The aryl group is preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and even more preferably an aryl group having 6 to 10 carbon atoms. Examples of such aryl groups include those obtained by removing one hydrogen atom from a monocyclic aromatic compound such as a phenyl group, a furanyl group, a pyrrolyl group, a thiophene group, an imidazolyl group, a pyrazolyl group, an oxazolyl group, an isoxazolyl group, a thiazolyl group, an isothiazolyl group, a pyridinyl group, a pyrimidinyl group, a pyridazinyl group, a pyrazinyl group, or a triazinyl group; and those obtained by removing one hydrogen atom from a condensed ring aromatic compound such as a naphthyl group, anthracenyl group, a phenalenyl group, a phenanthrenyl group, a quinolinyl group, an isoquinolinyl group, a quinazolyl group, a phthalazinyl group, a pteridinyl group, a coumarinyl group, an indole group, a benzimidazolyl group, a benzofuranyl group, or an acridinyl group.

[0072] The arylene group is preferably an arylene group having 6 to 30 carbon atoms, more preferably an arylene group having 6 to 20 carbon atoms, and further preferably an arylene group having 6 to 10 carbon atoms. Examples of such arylene groups include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group (-C6H4-C6H4-).

[0073] The compound containing an aromatic ester skeleton and an unsaturated bond contains an unsaturated bond. This allows the dielectric constant of the cured product to be excellent. The unsaturated bond also contributes to the curing reaction of the resin composition. The contribution of the unsaturated bond to the curing reaction suppresses the use of a part of the ester site of the aromatic ester skeleton in the curing reaction, and as a result, the curing shrinkage rate is suppressed.

[0074] The unsaturated bond is preferably a carbon-carbon unsaturated bond such as an ethylenically unsaturated bond. The unsaturated bond is preferably contained in a substituent having at least one unsaturated bond. Examples of the unsaturated bond include unsaturated bonds contained in unsaturated hydrocarbon groups such as an alkenyl group having 2 to 30 carbon atoms and an alkynyl group having 2 to 30 carbon atoms. The unsaturated bond is preferably contained in a substituent of the aromatic hydrocarbon group at the terminal, and more preferably contained in the substituents of the aromatic hydrocarbon groups at both terminals.

[0075] Examples of the alkenyl group having 2 to 30 carbon atoms include a vinyl group, an allyl group, a propenyl group, an isopropenyl group, a 1-propenyl group, a 1-butenyl group, a 2-butenyl group, a 3-butenyl group, a 1-hexenyl group, a 2-hexenyl group, a 3-hexenyl group, a 4-hexenyl group, a 5-hexenyl group, a 1-octenyl group, a 2-octenyl group, a 1-undecenyl group, a 1-pentadecenyl group, a 3-pentadecenyl group, and a 4-pentadecenyl group. Examples of such an alkyl group include a 7-pentadecenyl group, a 1-octadecenyl group, a 2-octadecenyl group, a cyclopentenyl group, a cyclohexenyl group, a cyclooctenyl group, a 1,3-butadienyl group, a 1,4-butadienyl group, a hexa-1,3-dienyl group, a hexa-2,5-dienyl group, a pentadeca-4,7-dienyl group, a hexa-1,3,5-trienyl group, and a pentadeca-1,4,7-trienyl group.

[0076] Examples of the alkynyl group having 2 to 30 carbon atoms include an ethynyl group, a propargyl group, a 1-butynyl group, a 2-butynyl group, a 3-butynyl group, a 3-pentynyl group, a 4-pentynyl group, and a 1,3-butadiynyl group.

[0077] Of these, an alkenyl group having 2 to 30 carbon atoms is preferable, an alkenyl group having 2 to 10 carbon atoms is more preferable, an alkenyl group having 2 to 5 carbon atoms is even more preferable, an allyl group, an isopropenyl group, or a 1-propenyl group is even more preferable, and an allyl group is particularly preferable.

[0078] The compound containing an aromatic ester skeleton and an unsaturated bond may have, in addition to the aromatic ester skeleton, any of an aromatic hydrocarbon group, an aliphatic hydrocarbon group, an oxygen atom, a sulfur atom, and a group consisting of a combination thereof. The term "aromatic hydrocarbon group" means a hydrocarbon group containing an aromatic ring, and the aromatic ring may be any of a monocyclic, polycyclic, and heterocyclic ring.

[0079] The aromatic hydrocarbon group is preferably a divalent aromatic hydrocarbon group, more preferably an arylene group or an aralkylene group, and even more preferably an arylene group. The arylene group is preferably an arylene group having 6 to 30 carbon atoms, more preferably an arylene group having 6 to 20 carbon atoms, and even more preferably an arylene group having 6 to 10 carbon atoms. Examples of such an arylene group include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group. The aralkylene group is preferably an aralkylene group having 7 to 30 carbon atoms, more preferably an aralkylene group having 7 to 20 carbon atoms, and even more preferably an aralkylene group having 7 to 15 carbon atoms. Among these, a phenylene group is preferable.

[0080] The aliphatic hydrocarbon group is preferably a divalent aliphatic hydrocarbon group, more preferably a divalent saturated aliphatic hydrocarbon group, and further preferably an alkylene group or a cycloalkylene group. The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and further preferably an alkylene group having 1 to 3 carbon atoms. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a 1-methylmethylene group, a 1,1-dimethylmethylene group, a 1-methylethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a pentylene group, and a hexylene group.

[0081] The cycloalkylene group is preferably a cycloalkylene group having 3 to 20 carbon atoms, more preferably a cycloalkylene group having 3 to 15 carbon atoms, and even more preferably a cycloalkylene group having 5 to 10 carbon atoms. Examples of the cycloalkylene group include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cyclopentylene group, a cycloheptylene group, and cycloalkylene groups represented by the following formulas (a) to (d). In the formulas (a) to (d), "*" represents a bond. [ka]

[0082] The aromatic ester skeleton, the aromatic hydrocarbon group, the aliphatic hydrocarbon group, and the unsaturated hydrocarbon group may have a substituent. The substituent is R 11 The substituents are the same as the substituents that may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I).

[0083] The compound containing an aromatic ester skeleton and an unsaturated bond is preferably either a compound represented by the following general formula (B-3) or a compound represented by the following general formula (B-4). [ka] (In general formula (B-3), Ar 11 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent; Ar 12 each independently represents a divalent aromatic hydrocarbon group which may have a substituent; Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof. n represents an integer of 0 to 10. [ka] (In general formula (B-4), Ar 21 represents an aromatic hydrocarbon group having a valence of m which may have a substituent, Ar 22 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent; and m represents an integer of 2 or 3.

[0084] In general formula (B-3), Ar 11Each independently represents a monovalent aromatic hydrocarbon group which may have a substituent. Examples of the monovalent aromatic hydrocarbon group include monocyclic aromatic compounds such as phenyl, furanyl, pyrrolyl, thiophene, imidazolyl, pyrazolyl, oxazolyl, isoxazolyl, thiazolyl, isothiazolyl, pyridinyl, pyrimidinyl, pyridazinyl, pyrazinyl, and triazinyl, from which one hydrogen atom has been removed; and condensed aromatic compounds such as naphthyl, anthracenyl, phenalenyl, phenanthrenyl, quinolinyl, isoquinolinyl, quinazolyl, phthalazinyl, pteridinyl, coumarinyl, indole, benzimidazolyl, benzofuranyl, and acridinyl, from which one hydrogen atom has been removed; and among these, from the viewpoint of obtaining the effects of the present invention remarkably, the phenyl group is preferred. Ar 11 The monovalent aromatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have. Among them, Ar 11 The substituent preferably contains an unsaturated bond. Ar 12 each independently represents a divalent aromatic hydrocarbon group which may have a substituent. Examples of the divalent aromatic hydrocarbon group include an arylene group and an aralkylene group, and an arylene group is preferred. As the arylene group, an arylene group having 6 to 30 carbon atoms is preferred, an arylene group having 6 to 20 carbon atoms is more preferred, and an arylene group having 6 to 10 carbon atoms is even more preferred. Examples of such an arylene group include a phenylene group, a naphthylene group, an anthracenylene group, and a biphenylene group. As the aralkylene group, an aralkylene group having 7 to 30 carbon atoms is preferred, an aralkylene group having 7 to 20 carbon atoms is more preferred, and an aralkylene group having 7 to 15 carbon atoms is even more preferred. Among these, a phenylene group is preferred.

[0085] Ar 12 The divalent aromatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0086] In general formula (B-3), Ar 13 each independently represents a divalent aromatic hydrocarbon group which may have a substituent, a divalent aliphatic hydrocarbon group which may have a substituent, an oxygen atom, a sulfur atom, or a divalent group consisting of a combination thereof, and a divalent group consisting of a combination thereof is preferable. 12 The divalent aromatic hydrocarbon group represented by the formula (I) is the same as the divalent aromatic hydrocarbon group represented by the formula (I).

[0087] As the divalent aliphatic hydrocarbon group, a divalent saturated aliphatic hydrocarbon group is more preferable, an alkylene group or a cycloalkylene group is preferable, and a cycloalkylene group is more preferable.

[0088] The alkylene group is preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 1 to 6 carbon atoms, and further preferably an alkylene group having 1 to 3 carbon atoms. Examples of the alkylene group include a methylene group, an ethylene group, a propylene group, a 1-methylmethylene group, a 1,1-dimethylmethylene group, a 1-methylethylene group, a 1,1-dimethylethylene group, a 1,2-dimethylethylene group, a butylene group, a 1-methylpropylene group, a 2-methylpropylene group, a pentylene group, and a hexylene group.

[0089] The cycloalkylene group is preferably a cycloalkylene group having 3 to 20 carbon atoms, more preferably a cycloalkylene group having 3 to 15 carbon atoms, and even more preferably a cycloalkylene group having 5 to 10 carbon atoms. Examples of the cycloalkylene group include a cyclopropylene group, a cyclobutylene group, a cyclopentylene group, a cyclohexylene group, a cyclopentylene group, a cycloheptylene group, and cycloalkylene groups represented by the above formulas (a) to (d), and the cycloalkylene group represented by formula (c) is preferred.

[0090] The divalent group formed by these combinations is preferably a divalent group formed by combining a divalent aromatic hydrocarbon group which may have a substituent and a divalent aliphatic hydrocarbon group which may have a substituent, and more preferably a divalent group formed by alternately combining a plurality of divalent aromatic hydrocarbon groups which may have a substituent and a plurality of divalent aliphatic hydrocarbon groups which may have a substituent. Specific examples of the divalent group include the following divalent groups (B1) to (B8). In the formula, b1 to b7 represent integers of 0 to 10, preferably integers of 0 to 5. "*" represents a bond, and the wavy line represents a structure obtained by reaction of an aromatic compound, an acid halide of an aromatic compound, or an ester of an aromatic compound used in synthesizing the component (B). [ka] [ka]

[0091] Ar 13 The divalent aromatic hydrocarbon group and the divalent aliphatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0092] In the general formula (B-3), n represents an integer of 0 to 10, preferably an integer of 0 to 5, and more preferably an integer of 0 to 3. When the compound represented by the general formula (B-3) is an oligomer or polymer, n represents the average value thereof.

[0093] In general formula (B-4), Ar 21 represents an m-valent aromatic hydrocarbon group which may have a substituent. As the m-valent aromatic hydrocarbon group, an m-valent aromatic hydrocarbon group having 6 to 30 carbon atoms is preferable, an m-valent aromatic hydrocarbon group having 6 to 20 carbon atoms is more preferable, and an m-valent aromatic hydrocarbon group having 6 to 10 carbon atoms is even more preferable. Ar 21The aromatic hydrocarbon group having a valence of m represented by the formula (I) may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0094] In general formula (B-4), Ar 22 each independently represents a monovalent aromatic hydrocarbon group which may have a substituent. 22 represents Ar in general formula (B-3). 11 The aromatic hydrocarbon group represented by Ar 22 The monovalent aromatic hydrocarbon group represented by may have a substituent. The substituent is the same as the substituent that the aromatic ester skeleton may have.

[0095] In formula (B-4), m represents an integer of 2 or 3, with 2 being preferred.

[0096] Specific examples of the compound containing an aromatic ester skeleton and an unsaturated bond include the following compounds. Specific examples of the compound containing an aromatic ester skeleton and an unsaturated bond include the compounds described in paragraphs 0068 to 0071 of International Publication No. 2018 / 235424 and paragraphs 0113 to 0115 of International Publication No. 2018 / 235425. However, the compound containing an aromatic ester skeleton and an unsaturated bond is not limited to these specific examples. In the formula, s represents an integer of 0 or 1 or more, and r represents an integer of 1 to 10. [ka]

[0097] The compound containing an aromatic ester skeleton and an unsaturated bond may be synthesized by a known method. The compound containing an aromatic ester skeleton and an unsaturated bond may be synthesized by, for example, the method described in WO 2018 / 235424 or WO 2018 / 235425.

[0098] From the viewpoint of obtaining the remarkable effects of the present invention, the weight average molecular weight of the compound containing an aromatic ester skeleton and an unsaturated bond is preferably 150 or more, more preferably 200 or more, and even more preferably 250 or more, and is preferably 3000 or less, more preferably 2000 or less, and even more preferably 1500 or less. The weight average molecular weight of the compound containing an aromatic ester skeleton and an unsaturated bond is a polystyrene-equivalent weight average molecular weight measured by gel permeation chromatography (GPC).

[0099] From the viewpoint of obtaining the effects of the present invention significantly, the unsaturated bond equivalent of the compound containing an aromatic ester skeleton and an unsaturated bond is preferably 50 g / eq or more, more preferably 100 g / eq or more, even more preferably 150 g / eq, and is preferably 2000 g / eq or less, more preferably 1000 g / eq or less, even more preferably 500 g / eq or less. The unsaturated bond equivalent is the mass of the (B) component containing one equivalent of an unsaturated bond.

[0100] The ratio of the epoxy group equivalent of the (A) epoxy resin to the active ester group equivalent of the (B) active ester compound (active ester group equivalent of the active ester compound / epoxy group equivalent of the epoxy resin) is preferably 0.4 or more, more preferably 0.5 or more, even more preferably 0.6 or more, and is preferably 1.8 or less, more preferably 1.5 or less, even more preferably 1.3 or less. Here, the "epoxy group equivalent of the epoxy resin" is the total value obtained by dividing the mass of the non-volatile component of the epoxy resin present in the resin composition by the epoxy equivalent. In addition, the "active ester group equivalent of the active ester compound" is the total value obtained by dividing the mass of the non-volatile component of the active ester compound present in the resin composition by the active ester group equivalent. By setting the ratio of the epoxy resin to the (B) component within such a range, the effects of the present invention can be obtained significantly.

[0101] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (B) component is, when the non-volatile components in the resin composition are taken as 100 mass%, preferably 1 mass% or more, more preferably 3 mass% or more, even more preferably 5 mass% or more, and is preferably 30 mass% or less, more preferably 25 mass% or less, even more preferably 20 mass% or less, or 15 mass% or less.

[0102] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (B) component, when the resin component in the resin composition is taken as 100 mass%, is preferably 30 mass% or more, more preferably 35 mass% or more, and even more preferably 45 mass% or more, and the upper limit is preferably 70 mass% or less, more preferably 60 mass% or less, and even more preferably 55 mass% or less.

[0103] <(C) Hydrocarbon polymer containing a terpene skeleton> The resin composition contains a hydrocarbon polymer containing a terpene skeleton as component (C). The hydrocarbon polymer containing a terpene skeleton as component (C) does not include those corresponding to the above-mentioned components (A) and (B). By including component (C) in the resin composition, it is possible to obtain a cured product having excellent dielectric tangent and crack resistance. The component (C) may be used alone or in combination of two or more types.

[0104] The terpene skeleton generally refers to a molecular skeleton having a structure formed by polymerizing terpenes. Since terpenes generally have isoprene (C5H8) as a structural unit, the (C) hydrocarbon polymer containing a terpene skeleton can be a hydrocarbon polymer containing isoprene as a structural unit, and preferably does not have a polar group. The terpene is preferably a cyclic terpene, and therefore the (C) component preferably contains a cyclic terpene skeleton having a structure formed by polymerizing a cyclic terpene. The polar group refers to a polar atomic group, and examples thereof include a hydroxyl group, an amino group, and a carboxyl group. Specific examples of the (C) hydrocarbon polymer containing a terpene skeleton include polyterpene resins which are homopolymers or copolymers of cyclic terpenes such as α-pinene, β-pinene, and dipentene (limonene); and aromatic modified terpene resins which are copolymers of the above-mentioned cyclic terpenes and aromatic monomers. The (C) component preferably contains either a polyterpene resin or an aromatic modified terpene resin, and more preferably contains a polyterpene resin. The polyterpene resin is preferably a homopolymer of any one of cyclic terpenes, α-pinene, β-pinene, and dipentene, and more preferably a homopolymer of dipentene.

[0105] As the aromatic monomer, an aromatic monomer that can be copolymerized with a cyclic terpene can be used. Examples of such aromatic monomers include styrene. The aromatic monomer may have a substituent. Examples of the substituent include R 11 The substituents are the same as the substituents which may be possessed by the alkyl group, alkenyl group, and aryl group represented by the formula (I). From the viewpoint of obtaining the effects of the present invention remarkably, it is preferable that the aromatic monomer does not have a polar group.

[0106] From the viewpoint of significantly obtaining the effects of the present invention, the softening point of the component (C) is preferably 50° C. or higher, more preferably 75° C. or higher, even more preferably 100° C. or higher or 120° C. or higher, and is preferably 200° C. or lower, more preferably 180° C. or lower, even more preferably 150° C. or lower or 130° C. or lower. The softening point is a value measured in accordance with JIS K7234.

[0107] The (C) component may be a commercially available product, or may be synthesized by a known method or a method similar thereto. Commercially available polyterpene resins include, for example, "PX1250" manufactured by Yasuhara Chemical Co., Ltd. Commercially available aromatic modified terpene resins include, for example, "TO125" manufactured by Yasuhara Chemical Co., Ltd.

[0108] From the viewpoint of obtaining the effects of the present invention remarkably, the weight average molecular weight of the (C) component is preferably 500 or more, more preferably 600 or more, and even more preferably 700 or more, and is preferably 10,000 or less, more preferably 6,000 or less, and even more preferably 4,000 or less.

[0109] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (C) component is preferably 0.1% by mass or more, more preferably 0.5% by mass or more, and even more preferably 1% by mass or more, and is preferably 5% by mass or less, more preferably 3% by mass or less, and even more preferably 2% by mass or less, based on 100% by mass of non-volatile components in the resin composition.

[0110] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (C) component, when the resin component in the resin composition is taken as 100 mass%, is preferably 1 mass% or more, more preferably 2 mass% or more, and even more preferably 3 mass% or more, and the upper limit is preferably 15 mass% or less, more preferably 10 mass% or less, and even more preferably 8 mass% or less.

[0111] The mass ratio of the epoxy resin (A) to the component (C) in the resin composition (component (A) / component (C)) is, from the viewpoint of significantly obtaining the effects of the present invention, preferably 1 or more, more preferably 3 or more, even more preferably 5 or more, and is preferably 20 or less, more preferably 15 or less, and particularly preferably 10 or less.

[0112] The mass ratio of the (C) component to the (B) active ester compound in the resin composition ((B) component / (C) component) is, from the viewpoint of significantly obtaining the effects of the present invention, preferably 1 or more, more preferably 3 or more, and particularly preferably 5 or more, and is preferably 20 or less, more preferably 15 or less, and particularly preferably 10 or less.

[0113] <(D) Radical polymerizable compound> The resin composition may contain a radical polymerizable compound (D) as an optional component. The radical polymerizable compound (D) as the component (D) does not include those corresponding to the above-mentioned components (A) to (C). The component (D) may be used alone or in combination of two or more kinds.

[0114] (D) radical polymerizable compound may be, for example, a compound having a radical polymerizable unsaturated group. The radical polymerizable unsaturated group is not particularly limited as long as it is radical polymerizable, but is preferably an ethylenically unsaturated group having a carbon-carbon double bond at the end or inside, specifically, it may be an unsaturated aliphatic group such as an allyl group, a 3-cyclohexenyl group, etc.; an unsaturated aliphatic group-containing aromatic group such as a p-vinylphenyl group, a m-vinylphenyl group, a styryl group, etc.; an α,β-unsaturated carbonyl group such as an acryloyl group, a methacryloyl group, a maleoyl group (maleimide group when imidized), a fumaroyl group, etc. The (D) radical polymerizable compound preferably has one or more radical polymerizable unsaturated groups, more preferably has two or more radical polymerizable unsaturated groups.

[0115] As the (D) other radically polymerizable compound, a wide variety of known radically polymerizable compounds can be used, and there is no particular limitation thereon. Examples of the radically polymerizable compound include a maleimide-based radically polymerizable compound having two or more maleimide groups, a vinylphenyl-based radically polymerizable compound having two or more vinylphenyl groups, and a (meth)acrylic-based radically polymerizable compound having two or more acryloyl groups and / or methacryloyl groups.

[0116] The maleimide radical polymerizable compound is not particularly limited, and may be an aliphatic maleimide compound containing an aliphatic amine skeleton, or an aromatic maleimide compound containing an aromatic amine skeleton. Commercially available products include, for example, "BMI-1500", "BMI-1700", "BMI-3000J", "BMI-689", and "BMI-2500" (dimer diamine structure-containing maleimide compounds) manufactured by Designer Molecules, Inc., "BMI-6100" (aromatic maleimide compound) manufactured by Designer Molecules, "MIR-5000-60T" and "MIR-3000-70MT" (biphenylaralkyl-type maleimide compounds) manufactured by Nippon Kayaku Co., Ltd., "BMI-70" and "BMI-80" manufactured by K.I. Chemical Industry Co., Ltd., "BMI-2300" and "BMI-TMH" manufactured by Daiwa Kasei Kogyo Co., Ltd., and "SLK-2600" manufactured by Shin-Etsu Chemical Co., Ltd. In addition, as the maleimide-based radically polymerizable compound, a maleimide resin (maleimide compound containing an indane ring skeleton) disclosed in the Japan Institute of Invention and Innovation's Technical Journal Publication No. 2020-500211 may be used.

[0117] The vinylphenyl radical polymerizable compound is not particularly limited, but in one embodiment, it is preferably a thermoplastic resin having a vinylphenyl group, more preferably a resin selected from modified polyphenylene ether resins having a vinylphenyl group and modified polystyrene resins having a vinylphenyl group. Commercially available products include, for example, "OPE-2St 1200" and "OPE-2St 2200" (vinylbenzyl modified polyphenylene ether resins) manufactured by Mitsubishi Gas Chemical Company, Inc.; "ODV-XET-X03", "ODV-XET-X04", and "ODV-XET-X05" (divinylbenzene / styrene copolymers) manufactured by Nippon Steel Chemical & Material Co., Ltd.; "A-DOG" manufactured by Shin-Nakamura Chemical Co., Ltd.; and "DCP-A" manufactured by Kyoeisha Chemical Co., Ltd.

[0118] The (meth)acrylic radical polymerizable compound is not particularly limited, but in one embodiment, it is preferably a thermoplastic resin having an acryloyl group and / or a methacryloyl group, and more preferably a resin selected from a modified polyphenylene ether resin having an acryloyl group and / or a methacryloyl group, and a modified polystyrene resin having an acryloyl group and / or a methacryloyl group. Examples of commercially available products include "SA9000" and "SA9000-111" (methacrylic modified polyphenylene ether resins) manufactured by SABIC Innovative Plastics.

[0119] The functional group equivalent of the component (D) is preferably 100 g / eq. to 20,000 g / eq., more preferably 200 g / eq. to 15,000 g / eq., and even more preferably 300 g / eq. to 10,000 g / eq. The functional group equivalent of the component (D) is the mass of the (D) other radically polymerizable compound per equivalent of the radically polymerizable unsaturated group (i.e., maleimide group, vinylphenyl group, acryloyl group, methacryloyl group, etc.).

[0120] The weight average molecular weight (Mw) of the component (D) is preferably 500 to 50,000, more preferably 700 to 20,000. The number average molecular weight (Mn) of the other radically polymerizable compounds (D) is preferably 500 to 50,000, more preferably 700 to 20,000. The weight average molecular weight is a polystyrene-equivalent weight average molecular weight measured using gel permeation chromatography (GPC).

[0121] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (D) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.1 mass% or more, more preferably 0.2 mass% or more, even more preferably 0.3 mass% or more, and is preferably 3 mass% or less, more preferably 2 mass% or less, even more preferably 1.5 mass% or less.

[0122] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (D) component, relative to 100 mass% of the resin component in the resin composition, is preferably 0.1 mass% or more, more preferably 0.5 mass% or more, even more preferably 1 mass% or more, and is preferably 10 mass% or less, more preferably 8 mass% or less, even more preferably 5 mass% or less.

[0123] The mass ratio of the (C) component to the (D) component in the resin composition ((D) component / (C) component) is, from the viewpoint of significantly obtaining the effects of the present invention, preferably 0.1 or more, more preferably 0.2 or more, even more preferably 0.3 or more, and is preferably 3 or less, more preferably 1 or less, and particularly preferably 0.8 or less.

[0124] <(E) Inorganic filler> The resin composition of the present invention may contain an inorganic filler (E) as an optional component. The inorganic filler (E) is contained in the resin composition in the form of particles.

[0125] (E) An inorganic compound is used as the material of the inorganic filler. (E) Examples of the material of the inorganic filler include silica, alumina, glass, cordierite, silicon oxide, barium sulfate, barium carbonate, talc, clay, mica powder, zinc oxide, hydrotalcite, boehmite, aluminum hydroxide, magnesium hydroxide, calcium carbonate, magnesium carbonate, magnesium oxide, boron nitride, aluminum nitride, manganese nitride, aluminum borate, strontium carbonate, strontium titanate, calcium titanate, magnesium titanate, bismuth titanate, titanium oxide, zirconium oxide, barium titanate, barium zirconate titanate, barium zirconate, calcium zirconate, zirconium phosphate, and zirconium tungstate phosphate. Among these, silica is particularly suitable. Examples of silica include amorphous silica, fused silica, crystalline silica, synthetic silica, and hollow silica. In addition, spherical silica is preferable as the silica. The (E) inorganic filler may be used alone or in combination of two or more kinds in any ratio.

[0126] The average particle size of the (E) inorganic filler is not particularly limited, but is preferably 10 μm or less, more preferably 5 μm or less, even more preferably 2 μm or less, even more preferably 1 μm or less, and particularly preferably 0.7 μm or less. The lower limit of the average particle size of the (E) inorganic filler is not particularly limited, but is preferably 0.01 μm or more, more preferably 0.05 μm or more, even more preferably 0.1 μm or more, and particularly preferably 0.2 μm or more. The average particle size of the (E) inorganic filler can be measured by a laser diffraction / scattering method based on the Mie scattering theory. Specifically, the particle size distribution of the inorganic filler is prepared on a volume basis using a laser diffraction / scattering type particle size distribution measuring device, and the median diameter is taken as the average particle size. The measurement sample can be prepared by weighing 100 mg of the inorganic filler and 10 g of methyl ethyl ketone into a vial and dispersing it by ultrasonic waves for 10 minutes. The measurement sample was measured using a laser diffraction type particle size distribution measuring device with blue and red light source wavelengths, and the particle size distribution of the inorganic filler on a volume basis was measured using a flow cell method, and the average particle size was calculated as the median diameter from the particle size distribution obtained. An example of a laser diffraction type particle size distribution measuring device is the "LA-960" manufactured by Horiba, Ltd.

[0127] The specific surface area of ​​the (E) inorganic filler is not particularly limited, but is preferably 0.1 m 2 / g or more, more preferably 0.5m 2 / g or more, more preferably 1m 2 / g or more, particularly preferably 3m 2 The upper limit of the specific surface area of ​​the (E) inorganic filler is not particularly limited, but is preferably 100 m 2 / g or less, more preferably 70m 2 / g or less, more preferably 50m 2 / g or less, particularly preferably 40m 2 The specific surface area of ​​the inorganic filler is obtained by adsorbing nitrogen gas onto the surface of a sample using a specific surface area measuring device (Macsorb HM-1210 manufactured by Mountech Co., Ltd.) according to the BET method, and calculating the specific surface area using the BET multipoint method.

[0128] The (E) inorganic filler may be a non-hollow inorganic filler with a porosity of 0 volume % (preferably non-hollow silica), or a hollow inorganic filler with a porosity of more than 0 volume % (preferably hollow silica), or may contain both. The porosity of the hollow inorganic filler is preferably 70 volume % or less, more preferably 50 volume % or less, and particularly preferably 30 volume % or less. The lower limit of the porosity of the (E) inorganic filler may be, for example, more than 0 volume %, 1 volume % or more, 5 volume % or more, 10 volume % or more, etc. The porosity P (volume %) of the inorganic filler is defined as the volume-based ratio of the total volume of one or more voids present inside the particle to the total volume of the particle based on the outer surface of the particle (total volume of voids / volume of particle), and is, for example, a measured value D of the actual density of the inorganic filler. M (g / cm 3 ), and the theoretical value of the material density of the material forming the inorganic filler D T (g / cm 3 ) is used to calculate the following formula (1):

[0129]

number

[0130] (E) The actual density of the inorganic filler can be measured, for example, by using a true density measuring device. Examples of the true density measuring device include ULTRAPYCNOMETER 1000 manufactured by QUANTACHROME. For example, nitrogen is used as the measurement gas.

[0131] (E) Inorganic filler may be a commercially available product. (E) Inorganic filler commercially available products include, for example, "UFP-30" manufactured by Denka Chemical Industry Co., Ltd.; "SP60-05" and "SP507-05" manufactured by Nippon Steel & Sumikin Materials Co., Ltd.; "YC100C", "YA050C", "YA050C-MJE", and "YA010C" manufactured by Admatechs Co., Ltd.; "UFP-30" manufactured by Denka Co., Ltd.; "Silfil NSS-3N", "Silfil NSS-4N", and "Silfil NSS-5N" manufactured by Tokuyama Corporation; "SC2500SQ", "SO-C4", "SO-C2", and "SO-C1" manufactured by Admatechs Co., Ltd.; "DAW-03" and "FB-105FD" manufactured by Denka Co., Ltd.; and "BA-S" manufactured by JGC Catalysts and Chemicals Co., Ltd.

[0132] (E) The inorganic filler is preferably treated with a surface treatment agent from the viewpoint of improving moisture resistance and dispersibility. Examples of the surface treatment agent include fluorine-containing silane coupling agents, aminosilane coupling agents, epoxysilane coupling agents, mercaptosilane coupling agents, silane coupling agents, alkoxysilanes, organosilazane compounds, titanate coupling agents, etc. Furthermore, the surface treatment agent may be used alone or in any combination of two or more types.

[0133] Examples of commercially available surface treatment agents include Shin-Etsu Chemical Co., Ltd.'s "KBM403" (3-glycidoxypropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM803" (3-mercaptopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBE903" (3-aminopropyltriethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM573" (N-phenyl-3-aminopropyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "SZ-31" (hexamethyldisilazane), Shin-Etsu Chemical Co., Ltd.'s "KBM103" (phenyltrimethoxysilane), Shin-Etsu Chemical Co., Ltd.'s "KBM-4803" (long-chain epoxy-type silane coupling agent), and Shin-Etsu Chemical Co., Ltd.'s "KBM-7103" (3,3,3-trifluoropropyltrimethoxysilane).

[0134] From the viewpoint of improving the dispersibility of the inorganic filler, the degree of surface treatment with the surface treatment agent is preferably within a predetermined range. Specifically, 100% by mass of the inorganic filler is preferably surface-treated with 0.2% to 5% by mass of the surface treatment agent, more preferably 0.2% to 3% by mass, and even more preferably 0.3% to 2% by mass.

[0135] The degree of surface treatment with the surface treatment agent can be evaluated by the amount of carbon per unit surface area of ​​the inorganic filler. From the viewpoint of improving the dispersibility of the inorganic filler, the amount of carbon per unit surface area of ​​the inorganic filler is set to 0.02 mg / m 2 More than 0.1 mg / m is preferable. 2 More preferably, 0.2 mg / m or more 2 On the other hand, from the viewpoint of preventing an increase in the melt viscosity of the resin composition or the melt viscosity in the form of a sheet, it is more preferable that the melt viscosity is 1.0 mg / m 2 Less than 0.8 mg / m is preferred. 2 Less than 0.5 mg / m is more preferable. 2 The following is even more preferred:

[0136] (E) The amount of carbon per unit surface area of ​​the inorganic filler can be measured after the surface-treated inorganic filler is washed with a solvent (e.g., methyl ethyl ketone (MEK)). Specifically, a sufficient amount of MEK as a solvent is added to the inorganic filler that has been surface-treated with a surface treatment agent, and ultrasonic cleaning is performed at 25°C for 5 minutes. After removing the supernatant and drying the solid content, the amount of carbon per unit surface area of ​​the inorganic filler can be measured using a carbon analyzer. As the carbon analyzer, the "EMIA-320V" manufactured by Horiba, Ltd., or the like can be used.

[0137] From the viewpoint of significantly obtaining the effects of the present invention, the content of the (E) inorganic filler, when the non-volatile components in the resin composition are taken as 100 mass%, is preferably 40 mass% or more, more preferably 50 mass% or more, even more preferably 60 mass% or more, or 70 mass% or more, and is preferably 90 mass% or less, more preferably 85 mass% or less, and even more preferably 80 mass% or less.

[0138] The mass ratio of the (C) component to the (E) inorganic filler in the resin composition ((E) component / (C) component) is preferably 10 or more, more preferably 20 or more, even more preferably 30 or more, 40 or more, or 50 or more, and is preferably 80 or less, more preferably 70 or less, and even more preferably 60 or less.

[0139] <(F) Hardener> The resin composition may contain a (F) curing agent (excluding those corresponding to the (B) component) as an optional component. The (F) curing agent as the (F) component does not include those corresponding to the above-mentioned (A) to (E). The (F) component may be used alone or in combination of two or more types.

[0140] Examples of the (F) component include phenol-based curing agents, naphthol-based curing agents, benzoxazine-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents. Among them, from the viewpoint of obtaining the effects of the present invention remarkably, the (F) component is preferably one or more of phenol-based curing agents, naphthol-based curing agents, cyanate ester-based curing agents, and carbodiimide-based curing agents, more preferably one of phenol-based curing agents and naphthol-based curing agents, and further preferably contains a phenol-based curing agent.

[0141] As the phenol-based curing agent and naphthol-based curing agent, from the viewpoint of heat resistance and water resistance, a phenol-based curing agent having a novolac structure or a naphthol-based curing agent having a novolac structure is preferable. Also, from the viewpoint of adhesion to the conductor layer, a nitrogen-containing phenol-based curing agent is preferable, and a triazine skeleton-containing phenol-based curing agent is more preferable.

[0142] Specific examples of phenol-based curing agents and naphthol-based curing agents include, for example, "MEH-7700", "MEH-7810", and "MEH-7851" manufactured by Meiwa Kasei Co., Ltd., "NHN", "CBN", and "GPH" manufactured by Nippon Kayaku Co., Ltd., "SN170", "SN180", "SN190", "SN475", "SN485", "SN495", "SN-495V", "SN375", and "SN395" manufactured by Nippon Steel & Sumikin Chemical Co., Ltd., and "TD-2090", "LA-7052", "LA-7054", "LA-1356", "LA3018-50P", and "EXB-9500" manufactured by DIC Corporation.

[0143] Specific examples of benzoxazine-based curing agents include "HFB2006M" manufactured by Showa Polymer Co., Ltd., and "Pd" and "Fa" manufactured by Shikoku Chemical Industry Co., Ltd.

[0144] Examples of the cyanate ester curing agent include bifunctional cyanate resins such as bisphenol A dicyanate, polyphenol cyanate, oligo(3-methylene-1,5-phenylene cyanate), 4,4'-methylenebis(2,6-dimethylphenyl cyanate), 4,4'-ethylidene diphenyl dicyanate, hexafluorobisphenol A dicyanate, 2,2-bis(4-cyanate)phenylpropane, 1,1-bis(4-cyanate phenylmethane), bis(4-cyanate-3,5-dimethylphenyl)methane, 1,3-bis(4-cyanate phenyl-1-(methylethylidene))benzene, bis(4-cyanate phenyl)thioether, and bis(4-cyanate phenyl)ether; polyfunctional cyanate resins derived from phenol novolac and cresol novolac; and prepolymers in which these cyanate resins are partially converted to triazine. Specific examples of cyanate ester-based curing agents include "PT30" and "PT60" (phenol novolac type multifunctional cyanate ester resins), "ULL-950S" (multifunctional cyanate ester resin), "BA230", and "BA230S75" (prepolymers in which part or all of bisphenol A dicyanate has been converted to triazine to form a trimer), all of which are manufactured by Lonza Japan.

[0145] Specific examples of carbodiimide-based curing agents include "V-03" and "V-07" manufactured by Nisshinbo Chemical Inc.

[0146] When the curing agent is contained as the (F) component, the ratio of the amount of the (A) component to the (B) component and the (F) component is the ratio of [total number of epoxy groups in the (A) component]:[total number of active groups in the (B) component and the (F) component], which is preferably in the range of 1:0.01 to 1:5, more preferably 1:0.05 to 1:3, and even more preferably 1:0.1 to 1:2. Here, the "number of epoxy groups in the (A) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (A) component present in the resin composition by the epoxy equivalent. In addition, the "number of active groups in the (B) component and the (F) component" refers to the total value obtained by dividing the mass of the non-volatile component of the (B) component and the (F) component present in the resin composition by the active group equivalent. By setting the ratio of the amount of the (B) component and the (F) component to the (A) component within such range, the effect of the present invention can be obtained remarkably.

[0147] When the curing agent is contained as the (F) component, the ratio of the amount of the (A) component to all the (F) components is preferably in the range of 1:0.01 to 1:1, more preferably 1:0.03 to 1:0.5, and even more preferably 1:0.05 to 1:0.3, in terms of the ratio of [total number of epoxy groups in the (A) component]:[total number of active groups in the (F) component]. Here, the "number of active groups in the (F) component" refers to the total value of all values ​​obtained by dividing the mass of the non-volatile components of the (F) component present in the resin composition by the active group equivalent. By setting the ratio of the (A) component to the (F) component within this range, the effects of the present invention can be obtained significantly.

[0148] From the viewpoint of significantly obtaining the desired effects of the present invention, the content of the (F) component, relative to 100 mass% of the non-volatile components in the resin composition, is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, and more preferably 0.5 mass% or more, and is preferably 5 mass% or less, more preferably 3 mass% or less, and even more preferably 1.5 mass% or less.

[0149] From the viewpoint of significantly obtaining the effects of the present invention, the content of the (F) component, relative to 100 mass% of the resin component in the resin composition, is preferably 2 mass% or more, more preferably 3 mass% or more, even more preferably 3.5 mass% or more, and is preferably 8 mass% or less, more preferably 6 mass% or less, even more preferably 5 mass% or less.

[0150] <(G) Curing accelerator> The resin composition may contain a (G) curing accelerator as an optional component. The (G) curing accelerator as this (G) component does not include those corresponding to the above-mentioned (A) to (F) components. The (G) curing accelerator functions as a curing catalyst that accelerates the curing of the (A) epoxy resin. The (G) curing accelerator may be used alone or in any combination of two or more types.

[0151] Examples of the (G) curing accelerator include phosphorus-based curing accelerators, urea-based curing accelerators, guanidine-based curing accelerators, imidazole-based curing accelerators, metal-based curing accelerators, amine-based curing accelerators, etc. Among these, curing accelerators selected from amine-based curing accelerators and metal-based curing accelerators are preferred, and amine-based curing accelerators are particularly preferred.

[0152] Examples of the phosphorus-based curing accelerator include aliphatic phosphonium salts such as tetrabutyl phosphonium bromide, tetrabutyl phosphonium chloride, tetrabutyl phosphonium acetate, tetrabutyl phosphonium decanoate, tetrabutyl phosphonium laurate, bis(tetrabutyl phosphonium)pyromellitate, tetrabutyl phosphonium hydrogenhexahydrophthalate, tetrabutyl phosphonium 2,6-bis[(2-hydroxy-5-methylphenyl)methyl]-4-methylphenolate, and di-tert-butyldimethylphosphonium tetraphenylborate; methyl triphenyl phosphonium bromide, ethyl triphenyl phosphonium bromide, propyl triphenyl phosphonium bromide, butyl triphenyl phosphonium bromide, benzyl triphenyl phosphonium chloride, tetraphenyl phosphonium bromide, p-tolyl triphenyl phosphonium tetra-p-tolylborate, tetraphenyl phosphonium bromide, and the like. aromatic phosphonium salts such as tetraphenylborate, tetraphenylphosphonium tetra-p-tolylborate, triphenylethylphosphonium tetraphenylborate, tris(3-methylphenyl)ethylphosphonium tetraphenylborate, tris(2-methoxyphenyl)ethylphosphonium tetraphenylborate, (4-methylphenyl)triphenylphosphonium thiocyanate, tetraphenylphosphonium thiocyanate, and butyltriphenylphosphonium thiocyanate; aromatic phosphine-borane complexes such as triphenylphosphine-triphenylborane; aromatic phosphine-quinone adducts such as triphenylphosphine-p-benzoquinone adduct; aliphatic phosphines such as tributylphosphine, tri-tert-butylphosphine, trioctylphosphine, di-tert-butyl(2-butenyl)phosphine, di-tert-butyl(3-methyl-2-butenyl)phosphine, and tricyclohexylphosphine;Dibutylphenylphosphine, di-tert-butylphenylphosphine, methyldiphenylphosphine, ethyldiphenylphosphine, butyldiphenylphosphine, diphenylcyclohexylphosphine, triphenylphosphine, tri-o-tolylphosphine, tri-m-tolylphosphine, tri-p-tolylphosphine, tris(4-ethylphenyl)phosphine, tris(4-propylphenyl)phosphine, tris(4-isopropylphenyl)phosphine, tris(4-butylphenyl)phosphine, tris(4-tert-butylphenyl)phosphine, tris(2,4-dimethylphenyl)phosphine, tris(2,5-dimethylphenyl)phosphine, tris(2,6-dimethylphenyl)phosphine Examples of aromatic phosphines include tris(3,5-dimethylphenyl)phosphine, tris(2,4,6-trimethylphenyl)phosphine, tris(2,6-dimethyl-4-ethoxyphenyl)phosphine, tris(2-methoxyphenyl)phosphine, tris(4-methoxyphenyl)phosphine, tris(4-ethoxyphenyl)phosphine, tris(4-tert-butoxyphenyl)phosphine, diphenyl-2-pyridylphosphine, 1,2-bis(diphenylphosphino)ethane, 1,3-bis(diphenylphosphino)propane, 1,4-bis(diphenylphosphino)butane, 1,2-bis(diphenylphosphino)acetylene, and 2,2'-bis(diphenylphosphino)diphenyl ether.

[0153] Examples of the urea-based curing accelerator include 1,1-dimethylurea; aliphatic dimethylureas such as 1,1,3-trimethylurea, 3-ethyl-1,1-dimethylurea, 3-cyclohexyl-1,1-dimethylurea, and 3-cyclooctyl-1,1-dimethylurea; 3-phenyl-1,1-dimethylurea, 3-(4-chlorophenyl)-1,1-dimethylurea, 3-(3,4-dichlorophenyl)-1,1-dimethylurea, 3-(3-chloro-4-methylphenyl)-1,1-dimethylurea, 3-(2-methylphenyl)-1,1-dimethylurea, 3-(4-methylphenyl)-1,1-dimethylurea, and 3-(3,4-dimethylphenyl)-1,1-dimethylurea. aromatic dimethylureas such as butylurea, 3-(4-isopropylphenyl)-1,1-dimethylurea, 3-(4-methoxyphenyl)-1,1-dimethylurea, 3-(4-nitrophenyl)-1,1-dimethylurea, 3-[4-(4-methoxyphenoxy)phenyl]-1,1-dimethylurea, 3-[4-(4-chlorophenoxy)phenyl]-1,1-dimethylurea, 3-[3-(trifluoromethyl)phenyl]-1,1-dimethylurea, N,N-(1,4-phenylene)bis(N',N'-dimethylurea), and N,N-(4-methyl-1,3-phenylene)bis(N',N'-dimethylurea) [toluene bisdimethylurea].

[0154] Examples of the guanidine curing accelerator include dicyandiamide, 1-methylguanidine, 1-ethylguanidine, 1-cyclohexylguanidine, 1-phenylguanidine, 1-(o-tolyl)guanidine, dimethylguanidine, diphenylguanidine, trimethylguanidine, tetramethylguanidine, pentamethylguanidine, 1,5,7-triazabicyclo[4.4.0]dec-5-ene, 7-methyl-1,5,7-triazabicyclo[4.4.0]dec-5-ene, 1-methylbiguanide, 1-ethylbiguanide, 1-n-butylbiguanide, 1-n-octadecylbiguanide, 1,1-dimethylbiguanide, 1,1-diethylbiguanide, 1-cyclohexylbiguanide, 1-allylbiguanide, 1-phenylbiguanide, and 1-(o-tolyl)biguanide.

[0155] Examples of the imidazole-based curing accelerator include 2-methylimidazole, 2-undecylimidazole, 2-heptadecylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 1,2-dimethylimidazole, 2-ethyl-4-methylimidazole, 2-phenylimidazole, 2-phenyl-4-methylimidazole, 1-benzyl-2-methylimidazole, and 1-benzyl-2-methylimidazole. Phenylimidazole, 1-cyanoethyl-2-methylimidazole, 1-cyanoethyl-2-undecylimidazole, 1-cyanoethyl-2-ethyl-4-methylimidazole, 1-cyanoethyl-2-phenylimidazole, 1-cyanoethyl-2-undecylimidazolium trimellitate, 1-cyanoethyl-2-phenylimidazolium trimellitate, 2,4-diamino-6-[2'-methylimidazolyl -(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-undecylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-ethyl-4'-methylimidazolyl-(1')]-ethyl-s-triazine, 2,4-diamino-6-[2'-methylimidazolyl-(1')]-ethyl-s-triazine isocyanuric acid adduct, 2-phenylimidazole isocyanuric acid adduct imidazole compounds such as 2-phenyl-4,5-dihydroxymethylimidazole, 2-phenyl-4-methyl-5-hydroxymethylimidazole, 2,3-dihydro-1H-pyrrolo[1,2-a]benzimidazole, 1-dodecyl-2-methyl-3-benzylimidazolium chloride, 2-methylimidazoline, and 2-phenylimidazoline, as well as adducts of imidazole compounds and epoxy resins.

[0156] As the imidazole-based curing accelerator, commercially available products may be used, for example, "1B2PZ", "2MZA-PW", "2PHZ-PW", and "C11Z-A" manufactured by Shikoku Chemical Industry Co., Ltd., and "P200-H50" manufactured by Mitsubishi Chemical Corporation.

[0157] Examples of metal-based curing accelerators include organometallic complexes or organometallic salts of metals such as cobalt, copper, zinc, iron, nickel, manganese, and tin. Specific examples of organometallic complexes include organocobalt complexes such as cobalt(II) acetylacetonate and cobalt(III) acetylacetonate, organocopper complexes such as copper(II) acetylacetonate, organozinc complexes such as zinc(II) acetylacetonate, organoiron complexes such as iron(III) acetylacetonate, organonickel complexes such as nickel(II) acetylacetonate, and organomanganese complexes such as manganese(II) acetylacetonate. Examples of organometallic salts include zinc octylate, tin octylate, zinc naphthenate, cobalt naphthenate, tin stearate, and zinc stearate.

[0158] Examples of the amine curing accelerator include trialkylamines such as triethylamine and tributylamine, 4-dimethylaminopyridine, benzyldimethylamine, 2,4,6-tris(dimethylaminomethyl)phenol, and 1,8-diazabicyclo(5,4,0)-undecene.

[0159] As the amine-based curing accelerator, a commercially available product may be used, for example, "MY-25" manufactured by Ajinomoto Fine-Techno Co., Ltd.

[0160] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (G) component, when the non-volatile components in the resin composition are taken as 100 mass%, is preferably 0.01 mass% or more, more preferably 0.05 mass% or more, even more preferably 0.1 mass% or more, and is preferably 1.5 mass% or less, more preferably 1 mass% or less, even more preferably 0.5 mass% or less.

[0161] From the viewpoint of obtaining the effects of the present invention prominently, the content of the (G) component, when the resin component in the resin composition is taken as 100 mass%, is preferably 0.1 mass% or more, more preferably 0.3 mass% or more, even more preferably 0.5 mass% or more, and is preferably 5 mass% or less, more preferably 3 mass% or less, even more preferably 1.5 mass% or less.

[0162] <(H) Other Additives> The resin composition of the present invention may further contain any additive as a non-volatile component. Examples of such additives include thermoplastic resins; radical polymerization initiators such as peroxide radical polymerization initiators and azo radical polymerization initiators; thermoplastic resins such as phenoxy resins, polyvinyl acetal resins, polyolefin resins, polysulfone resins, polyethersulfone resins, polyphenylene ether resins, polycarbonate resins, polyether ether ketone resins, and polyester resins; organic fillers such as rubber particles; organic metal compounds such as organic copper compounds, organic zinc compounds, and organic cobalt compounds; colorants such as phthalocyanine blue, phthalocyanine green, iodine green, diazo yellow, crystal violet, titanium oxide, and carbon black; polymerization inhibitors such as hydroquinone, catechol, pyrogallol, and phenothiazine; leveling agents such as silicone leveling agents and acrylic polymer leveling agents; thickeners such as bentone and montmorillonite; silicone defoamers, acrylic defoamers, fluorine defoamers, and vinyl resin defoamers. Antifoaming agents such as foaming agents; ultraviolet absorbers such as benzotriazole-based ultraviolet absorbers; adhesion improvers such as urea silanes; adhesion promoters such as triazole-based adhesion promoters, tetrazole-based adhesion promoters, and triazine-based adhesion promoters; antioxidants such as hindered phenol-based antioxidants; fluorescent brighteners such as stilbene derivatives; surfactants such as fluorine-based surfactants and silicone-based surfactants; phosphorus-based flame retardants (e.g., phosphate ester compounds, phosphazene compounds, phosphinic acid compounds, red phosphorus). Flame retardants such as nitrogen-based flame retardants (e.g., melamine sulfate), halogen-based flame retardants, and inorganic flame retardants (e.g., antimony trioxide); dispersants such as phosphate-based dispersants, polyoxyalkylene-based dispersants, acetylene-based dispersants, silicone-based dispersants, anionic dispersants, and cationic dispersants; stabilizers such as borate-based stabilizers, titanate-based stabilizers, aluminate-based stabilizers, zirconate-based stabilizers, isocyanate-based stabilizers, carboxylic acid-based stabilizers, and carboxylic anhydride-based stabilizers. (H) Other additives may be used alone or in combination of two or more at any ratio. The content of (H) other additives can be appropriately determined by those skilled in the art.

[0163] <(I) Solvent> The resin composition may further contain an arbitrary solvent as a volatile component in addition to the non-volatile components described above. (I) As the solvent, a known solvent can be appropriately used, and the type is not particularly limited, and an organic solvent is preferable. (I) As the solvent, for example, ketone-based solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc.; ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, isobutyl acetate, isoamyl acetate, methyl propionate, ethyl propionate, γ-butyrolactone, etc.; ether-based solvents such as tetrahydropyran, tetrahydrofuran, 1,4-dioxane, diethyl ether, diisopropyl ether, dibutyl ether, diphenyl ether, anisole, etc.; alcohol-based solvents such as methanol, ethanol, propanol, butanol, ethylene glycol, etc.; 2-ethoxyethyl acetate, propylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, ethyl diglycol acetate, γ-butyrolactone, methyl methoxypropionate, etc. Examples of the solvent include ether ester solvents such as ethyl acetate, ester alcohol solvents such as methyl lactate, ethyl lactate, and methyl 2-hydroxyisobutyrate, ether alcohol solvents such as 2-methoxypropanol, 2-methoxyethanol, 2-ethoxyethanol, propylene glycol monomethyl ether, and diethylene glycol monobutyl ether (butylcarbitol), amide solvents such as N,N-dimethylformamide, N,N-dimethylacetamide, and N-methyl-2-pyrrolidone, sulfoxide solvents such as dimethyl sulfoxide, nitrile solvents such as acetonitrile and propionitrile, aliphatic hydrocarbon solvents such as hexane, cyclopentane, cyclohexane, and methylcyclohexane, and aromatic hydrocarbon solvents such as benzene, toluene, xylene, ethylbenzene, and trimethylbenzene. (I) The solvent may be used alone or in combination of two or more in any ratio.

[0164] In one embodiment, the content of the (I) solvent is not particularly limited, but when all components in the resin composition are taken as 100 mass%, it can be, for example, 60 mass% or less, 40 mass% or less, 30 mass% or less, 20 mass% or less, 15 mass% or less, 10 mass% or less, etc.

[0165] <Method of producing resin composition> The resin composition of the present invention can be produced, for example, by adding components (A) to (C), and if necessary components (D) to (I) to any preparation vessel in any order and / or all or a part of them at the same time and mixing them. In the process of adding and mixing each component, the temperature can be appropriately set, and heating and / or cooling may be performed temporarily or throughout. In the process of adding and mixing or thereafter, the resin composition may be stirred or shaken using a stirring or shaking device such as a mixer to disperse it uniformly. In addition, degassing may be performed under low pressure conditions such as under vacuum at the same time as stirring or shaking.

[0166] <Characteristics of resin composition> By using a resin composition containing a combination of components (A) to (C), a cured product having a low dielectric tangent (Df) and excellent crack resistance can be obtained. In addition, the resin composition can also provide a cured product having a high glass transition temperature (Tg) and a low relative dielectric constant (Dk).

[0167] The resin composition cured at 190°C for 90 minutes exhibits the characteristic of having a low dielectric loss tangent (Df) at room temperature. Thus, an insulating layer with excellent dielectric loss tangent is obtained. The dielectric loss tangent (Df) of the cured resin composition measured at 5.8 GHz and 23°C is preferably 0.005 or less, 0.004 or less, and more preferably 0.003 or less. There is no particular lower limit, but it may be 0.00001 or more. The dielectric loss tangent at 23°C can be measured by the method described in the examples below.

[0168] A cured product obtained by curing a resin composition at 190°C for 90 minutes usually exhibits the characteristic of a low dielectric loss tangent (Df) at high temperatures. Thus, an insulating layer with excellent dielectric loss tangent is obtained. The dielectric loss tangent (Df) of the cured product measured at 5.8 GHz and 90°C is preferably 0.0032 or less, 0.003 or less, more preferably 0.0029 or less. There is no particular limit to the lower limit, but it may be 0.00001 or more. The dielectric loss tangent at 90°C can be measured by the method described in the examples below.

[0169] The cured product obtained by curing the resin composition at 130°C for 30 minutes and then at 170°C for 30 minutes exhibits excellent crack resistance. Thus, an insulating layer with excellent crack resistance is obtained. Specifically, a layer made of a cured product of the resin composition is formed on a core material having 100 copper pad parts. The layer made of the cured product is roughened, and 100 copper pad parts after the roughening treatment are observed to check for the presence or absence of cracks. In this case, the number of cracks is preferably 10 or less. The crack resistance can be evaluated by the method described in the examples below.

[0170] A cured product obtained by curing a resin composition at 190°C for 90 minutes usually exhibits the characteristic of having a low dielectric constant (Dk) at room temperature. Thus, an insulating layer with excellent dielectric constant is obtained. The dielectric constant (Dk) of the cured product of the resin composition measured at 5.8 GHz and 23°C is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.5 or less. There is no particular restriction on the lower limit, but it may be 0.1 or more. The dielectric constant at 23°C can be measured by the method described in the examples below.

[0171] A cured product obtained by curing a resin composition at 190°C for 90 minutes usually exhibits the characteristic of having a low dielectric constant (Dk) at high temperatures. Thus, an insulating layer with excellent dielectric constant is obtained. The dielectric constant (Dk) of the cured product of the resin composition measured at 5.8 GHz and 90°C is preferably 5.0 or less, more preferably 4.0 or less, and even more preferably 3.5 or less. There is no particular restriction on the lower limit, but it may be 0.1 or more. The dielectric constant at 90°C can be measured by the method described in the examples below.

[0172] A cured product obtained by curing a resin composition at 190°C for 90 minutes usually exhibits the characteristic of having a high glass transition temperature (Tg). The glass transition temperature (Tg) of the cured product is preferably 100°C or higher, more preferably 110°C or higher, and even more preferably 120°C or higher. There is no particular upper limit, but it may be 500°C or lower. The glass transition temperature can be measured by DSC (differential scanning calorimetry) at a heating rate of 10°C / min.

[0173] <Applications of resin composition> The resin composition of the present invention can be suitably used as a resin composition for insulating purposes, particularly as a resin composition for forming an insulating layer. Specifically, it can be suitably used as a resin composition for forming an insulating layer (resin composition for forming an insulating layer for forming a conductor layer) for forming a conductor layer (including a rewiring layer) formed on an insulating layer. In addition, in a printed wiring board described later, it can be suitably used as a resin composition for forming an insulating layer of a printed wiring board (resin composition for forming an insulating layer of a printed wiring board). The resin composition of the present invention can also be used in a wide range of applications requiring a resin composition, such as a resin sheet, a sheet-like laminate material such as a prepreg, a solder resist, an underfill material, a die bonding material, a semiconductor encapsulant, a hole filling resin, and a component embedding resin.

[0174] In addition, for example, when a semiconductor chip package is manufactured through the following steps (1) to (6), the resin composition of the present invention can be suitably used as a resin composition for a rewiring formation layer (resin composition for forming a rewiring formation layer) as an insulating layer for forming a rewiring layer, and as a resin composition for sealing a semiconductor chip (resin composition for sealing a semiconductor chip). When a semiconductor chip package is manufactured, a rewiring layer may be further formed on the sealing layer. (1) A step of laminating a temporary fixing film onto a substrate; (2) a step of temporarily fixing a semiconductor chip on a temporary fixing film; (3) forming an encapsulation layer on the semiconductor chip; (4) peeling the substrate and the temporary fixing film from the semiconductor chip; (5) forming a rewiring formation layer as an insulating layer on the surface of the semiconductor chip from which the base material and the temporary fixing film have been peeled off; and (6) A process of forming a rewiring layer as a conductor layer on the rewiring formation layer.

[0175] Furthermore, the resin composition of the present invention provides an insulating layer with good component embedding properties, and therefore can be suitably used when the printed wiring board is a circuit board with built-in components.

[0176] [Sheet-type laminated material] The resin composition of the present invention can be used by coating in the form of a varnish, but from an industrial perspective, it is generally preferred to use the resin composition in the form of a sheet-like laminate material containing the resin composition.

[0177] As the sheet-like laminate material, the following resin sheets and prepregs are preferred.

[0178] In one embodiment, the resin sheet includes a support and a resin composition layer provided on the support, and the resin composition layer is formed from the resin composition of the present invention.

[0179] The thickness of the resin composition layer is preferably 50 μm or less, more preferably 40 μm or less, from the viewpoint of making the printed wiring board thinner and being able to provide a cured product with excellent insulation even if the cured product of the resin composition is a thin film. The lower limit of the thickness of the resin composition layer is not particularly limited, but can usually be 5 μm or more, 10 μm or more, etc.

[0180] Examples of the support include films made of plastic materials, metal foils, and release papers, with films made of plastic materials and metal foils being preferred.

[0181] When a film made of a plastic material is used as the support, examples of the plastic material include polyesters such as polyethylene terephthalate (hereinafter sometimes abbreviated as "PET") and polyethylene naphthalate (hereinafter sometimes abbreviated as "PEN"), polycarbonate (hereinafter sometimes abbreviated as "PC"), acrylics such as polymethyl methacrylate (PMMA), cyclic polyolefins, triacetyl cellulose (TAC), polyether sulfide (PES), polyether ketone, polyimide, etc. Among these, polyethylene terephthalate and polyethylene naphthalate are preferred, and inexpensive polyethylene terephthalate is particularly preferred.

[0182] When a metal foil is used as the support, examples of the metal foil include copper foil, aluminum foil, etc., and copper foil is preferred. As the copper foil, a foil made of a single metal, copper, or an alloy of copper and another metal (e.g., tin, chromium, silver, magnesium, nickel, zirconium, silicon, titanium, etc.) may be used.

[0183] The surface of the support to be bonded to the resin composition layer may be subjected to a matte treatment, a corona treatment, or an antistatic treatment.

[0184] In addition, as the support, a support with a release layer having a release layer on the surface to be bonded to the resin composition layer may be used. The release agent used in the release layer of the support with a release layer may be, for example, one or more release agents selected from the group consisting of alkyd resins, polyolefin resins, urethane resins, and silicone resins. The support with a release layer may be a commercially available product, for example, "SK-1", "AL-5", and "AL-7" manufactured by Lintec Corporation, "Lumirror T60" manufactured by Toray Industries, Inc., "Purex" manufactured by Teijin Limited, and "Unipeel" manufactured by Unitika Limited, which are PET films having a release layer mainly composed of an alkyd resin-based release agent.

[0185] The thickness of the support is not particularly limited, but is preferably in the range of 5 μm to 75 μm, and more preferably in the range of 10 μm to 60 μm. When a support with a release layer is used, it is preferable that the total thickness of the support with a release layer is in the above range.

[0186] In one embodiment, the resin sheet may further include an optional layer as necessary. For example, such an optional layer may be a protective film equivalent to the support provided on the surface of the resin composition layer that is not bonded to the support (i.e., the surface opposite to the support). The thickness of the protective film is not particularly limited, but is, for example, 1 μm to 40 μm. By laminating the protective film, adhesion of dirt and the like to the surface of the resin composition layer and scratches can be suppressed.

[0187] The resin sheet can be produced, for example, by preparing a liquid resin composition as is or a resin varnish by dissolving the resin composition in an organic solvent, applying this onto a support using a die coater or the like, and then drying to form a resin composition layer.

[0188] The organic solvent may be the same as the organic solvent described as a component of the resin composition. The organic solvent may be used alone or in combination of two or more kinds.

[0189] Drying may be performed by a known method such as heating or hot air blowing. Drying conditions are not particularly limited, but drying is performed so that the content of the organic solvent in the resin composition layer becomes 10% by mass or less, preferably 5% by mass or less. Although it varies depending on the boiling point of the organic solvent in the resin composition or resin varnish, for example, when a resin composition or resin varnish containing 30% by mass to 60% by mass of the organic solvent is used, the resin composition layer can be formed by drying at 50°C to 150°C for 3 minutes to 10 minutes.

[0190] The resin sheet can be stored in a rolled state. When the resin sheet has a protective film, it can be used by peeling off the protective film.

[0191] In one embodiment, the prepreg is formed by impregnating a sheet-like fiber substrate with the resin composition of the present invention.

[0192] The sheet-like fiber substrate used for the prepreg is not particularly limited, and can be a substrate commonly used for prepreg, such as glass cloth, aramid nonwoven fabric, liquid crystal polymer nonwoven fabric, etc. From the viewpoint of thinning the printed wiring board, the thickness of the sheet-like fiber substrate is preferably 50 μm or less, more preferably 40 μm or less, even more preferably 30 μm or less, and particularly preferably 20 μm or less. The lower limit of the thickness of the sheet-like fiber substrate is not particularly limited. It is usually 10 μm or more.

[0193] The prepreg can be produced by a known method such as a hot melt method or a solvent method.

[0194] The thickness of the prepreg may be in the same range as that of the resin composition layer in the above-mentioned resin sheet.

[0195] The sheet-like laminate material of the present invention can be suitably used for forming an insulating layer of a printed wiring board (for an insulating layer of a printed wiring board), and can be more suitably used for forming an interlayer insulating layer of a printed wiring board (for an interlayer insulating layer of a printed wiring board).

[0196] [Printed wiring board] The printed wiring board of the present invention includes an insulating layer made of a cured product obtained by curing the resin composition of the present invention.

[0197] The printed wiring board can be produced, for example, by using the above-mentioned resin sheet by a method including the following steps (I) and (II). (I) A step of laminating a resin sheet on an inner layer substrate such that a resin composition layer of the resin sheet is bonded to the inner layer substrate. (II) A step of curing (e.g., heat curing) the resin composition layer to form an insulating layer.

[0198] The "inner layer substrate" used in step (I) is a member that becomes the substrate of the printed wiring board, and examples thereof include a glass epoxy substrate, a metal substrate, a polyester substrate, a polyimide substrate, a BT resin substrate, and a thermosetting polyphenylene ether substrate. The substrate may have a conductor layer on one or both sides, and the conductor layer may be patterned. An inner layer substrate having a conductor layer (circuit) formed on one or both sides of the substrate may be called an "inner layer circuit substrate". In addition, an intermediate product on which an insulating layer and / or a conductor layer is to be formed during the manufacture of a printed wiring board is also included in the "inner layer substrate" of the present invention. When the printed wiring board is a circuit board with built-in components, an inner layer substrate with built-in components may be used.

[0199] The lamination of the inner layer substrate and the resin sheet can be carried out, for example, by thermocompression bonding the resin sheet to the inner layer substrate from the support side. Examples of the member for thermocompression bonding the resin sheet to the inner layer substrate (hereinafter also referred to as the "thermocompression bonding member") include a heated metal plate (such as a SUS plate) or a metal roll (SUS roll). It is preferable to press the thermocompression member not directly onto the resin sheet, but via an elastic material such as heat-resistant rubber so that the resin sheet can sufficiently follow the surface irregularities of the inner layer substrate.

[0200] The lamination of the inner layer substrate and the resin sheet may be performed by a vacuum lamination method. In the vacuum lamination method, the thermocompression temperature is preferably in the range of 60°C to 160°C, more preferably in the range of 80°C to 140°C, the thermocompression pressure is preferably in the range of 0.098MPa to 1.77MPa, more preferably in the range of 0.29MPa to 1.47MPa, and the thermocompression time is preferably in the range of 20 seconds to 400 seconds, more preferably in the range of 30 seconds to 300 seconds. The lamination may be performed under reduced pressure conditions, preferably at a pressure of 26.7hPa or less.

[0201] The lamination can be performed by a commercially available vacuum laminator, such as a vacuum pressure laminator manufactured by Meiki Seisakusho Co., Ltd., a vacuum applicator manufactured by Nikko Materials Co., Ltd., or a batch type vacuum pressure laminator.

[0202] After lamination, the laminated resin sheet may be smoothed under normal pressure (atmospheric pressure), for example, by pressing a thermocompression member from the support side. The pressing conditions for the smoothing treatment may be the same as the thermocompression conditions for the lamination. The smoothing treatment may be performed using a commercially available laminator. The lamination and smoothing treatment may be performed consecutively using the commercially available vacuum laminator.

[0203] The support may be removed between step (I) and step (II) or after step (II).

[0204] In step (II), the resin composition layer is cured (for example, thermally cured) to form an insulating layer made of a cured product of the resin composition. The curing conditions for the resin composition layer are not particularly limited, and conditions that are usually adopted when forming an insulating layer for a printed wiring board may be used.

[0205] The thermal curing conditions for the resin composition layer vary depending on the type of resin composition, etc., but in one embodiment, the curing temperature is preferably 120° C. to 240° C., more preferably 150° C. to 220° C., and even more preferably 170° C. to 210° C. The curing time is preferably 5 minutes to 120 minutes, more preferably 10 minutes to 100 minutes, and even more preferably 15 minutes to 100 minutes.

[0206] Before the resin composition layer is thermally cured, the resin composition layer may be preheated at a temperature lower than the curing temperature. For example, prior to thermally curing the resin composition layer, the resin composition layer may be preheated at a temperature of 50° C. to 120° C., preferably 60° C. to 115° C., more preferably 70° C. to 110° C. for 5 minutes or more, preferably 5 minutes to 150 minutes, more preferably 15 minutes to 120 minutes, and even more preferably 15 minutes to 100 minutes.

[0207] In manufacturing a printed wiring board, the steps of (III) drilling holes in the insulating layer, (IV) roughening the insulating layer, and (V) forming a conductor layer may be further carried out. These steps (III) to (V) may be carried out according to various methods known to those skilled in the art for use in manufacturing printed wiring boards. When the support is removed after step (II), the support may be removed between step (II) and step (III), between step (III) and step (IV), or between step (IV) and step (V). In addition, the formation of the insulating layer and the conductor layer in steps (II) to (V) may be repeated to form a multilayer wiring board, as necessary.

[0208] In another embodiment, the printed wiring board of the present invention can be manufactured using the above-mentioned prepreg. The manufacturing method is basically the same as when a resin sheet is used.

[0209] Step (III) is a step of drilling holes in the insulating layer, which allows holes such as via holes and through holes to be formed in the insulating layer. Step (III) may be performed using, for example, a drill, a laser, plasma, etc., depending on the composition of the resin composition used to form the insulating layer. The dimensions and shape of the holes may be appropriately determined depending on the design of the printed wiring board.

[0210] Step (IV) is a step of roughening the insulating layer. Usually, smears are also removed in this step (IV). The procedure and conditions of the roughening treatment are not particularly limited, and known procedures and conditions that are usually used when forming an insulating layer of a printed wiring board can be adopted. For example, the insulating layer can be roughened by carrying out a swelling treatment with a swelling liquid, a roughening treatment with an oxidizing agent, and a neutralization treatment with a neutralizing liquid in this order.

[0211] The swelling liquid used in the roughening treatment is not particularly limited, but includes an alkaline solution, a surfactant solution, etc., and is preferably an alkaline solution, and more preferably a sodium hydroxide solution or a potassium hydroxide solution. Examples of commercially available swelling liquids include "Swelling Dip Securigans P" and "Swelling Dip Securigans SBU" manufactured by Atotech Japan. The swelling treatment using the swelling liquid is not particularly limited, but can be performed by immersing the insulating layer in a swelling liquid at 30°C to 90°C for 1 to 20 minutes, for example. From the viewpoint of suppressing the swelling of the resin of the insulating layer to an appropriate level, it is preferable to immerse the insulating layer in a swelling liquid at 40°C to 80°C for 5 to 15 minutes.

[0212] The oxidizing agent used in the roughening treatment is not particularly limited, but examples thereof include an alkaline permanganate solution in which potassium permanganate or sodium permanganate is dissolved in an aqueous solution of sodium hydroxide. The roughening treatment using an oxidizing agent such as an alkaline permanganate solution is preferably performed by immersing the insulating layer in an oxidizing agent solution heated to 60°C to 100°C for 10 minutes to 30 minutes. The concentration of permanganate in the alkaline permanganate solution is preferably 5% by mass to 10% by mass. Examples of commercially available oxidizing agents include alkaline permanganate solutions such as "Concentrate Compact CP" and "Dosing Solution Securigans P" manufactured by Atotech Japan.

[0213] The neutralizing solution used in the roughening treatment is preferably an acidic aqueous solution, and a commercially available product such as "Reduction Solution Securigant P" manufactured by Atotech Japan can be mentioned.

[0214] The treatment with the neutralizing solution can be carried out by immersing the surface that has been roughened with an oxidizing agent in a neutralizing solution at 30° C. to 80° C. for 5 to 30 minutes. From the viewpoint of workability, etc., a method in which the object that has been roughened with an oxidizing agent is immersed in a neutralizing solution at 40° C. to 70° C. for 5 to 20 minutes is preferred.

[0215] In one embodiment, the root mean square roughness (Rq) of the insulating layer surface after the roughening treatment is preferably 500 nm or less, more preferably 400 nm or less, and even more preferably 300 nm or less. The lower limit is not particularly limited, and may be, for example, 1 nm or more, 2 nm or more, etc. The root mean square roughness (Rq) of the insulating layer surface can be measured using a non-contact surface roughness meter.

[0216] Step (V) is a step of forming a conductor layer, and the conductor layer is formed on the insulating layer. The conductor material used for the conductor layer is not particularly limited. In a preferred embodiment, the conductor layer contains one or more metals selected from the group consisting of gold, platinum, palladium, silver, copper, aluminum, cobalt, chromium, zinc, nickel, titanium, tungsten, iron, tin and indium. The conductor layer may be a single metal layer or an alloy layer, and examples of the alloy layer include layers formed from alloys of two or more metals selected from the above group (e.g., nickel-chromium alloy, copper-nickel alloy and copper-titanium alloy). Among these, from the viewpoints of versatility in forming the conductor layer, cost, ease of patterning, and the like, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy, a copper-nickel alloy, or a copper-titanium alloy is preferred, a single metal layer of chromium, nickel, titanium, aluminum, zinc, gold, palladium, silver, or copper, or an alloy layer of a nickel-chromium alloy is more preferred, and a single metal layer of copper is even more preferred.

[0217] The conductor layer may be a single-layer structure or a multi-layer structure in which two or more single metal layers or alloy layers made of different kinds of metals or alloys are laminated. When the conductor layer has a multi-layer structure, the layer in contact with the insulating layer is preferably a single metal layer of chromium, zinc or titanium, or an alloy layer of a nickel-chromium alloy.

[0218] The thickness of the conductor layer depends on the desired design of the printed wiring board, but is generally 3 μm to 35 μm, and preferably 5 μm to 30 μm.

[0219] In one embodiment, the conductor layer may be formed by plating. For example, a conductor layer having a desired wiring pattern can be formed by plating the surface of the insulating layer by a conventionally known technique such as a semi-additive method or a full-additive method, and from the viewpoint of ease of production, it is preferable to form the conductor layer by the semi-additive method. An example of forming the conductor layer by the semi-additive method will be described below.

[0220] First, a plating seed layer is formed on the surface of an insulating layer by electroless plating. Next, a mask pattern is formed on the formed plating seed layer to expose a part of the plating seed layer corresponding to a desired wiring pattern. After a metal layer is formed on the exposed plating seed layer by electrolytic plating, the mask pattern is removed. Thereafter, unnecessary plating seed layer is removed by etching or the like to form a conductor layer having a desired wiring pattern.

[0221] In another embodiment, the conductor layer may be formed using a metal foil. When the conductor layer is formed using a metal foil, it is preferable to carry out step (V) between steps (I) and (II). For example, after step (I), the support is removed, and a metal foil is laminated on the exposed surface of the resin composition layer. The lamination of the resin composition layer and the metal foil may be carried out by a vacuum lamination method. The lamination conditions may be the same as those described for step (I). Next, step (II) is carried out to form an insulating layer. Thereafter, a conductor layer having a desired wiring pattern can be formed by a conventionally known technique such as a subtractive method or a modified semi-additive method, using the metal foil on the insulating layer.

[0222] The metal foil can be produced by a known method such as an electrolytic method, a rolling method, etc. Commercially available metal foils include, for example, HLP foil and JXUT-III foil manufactured by JX Nippon Mining & Metals Corporation, and 3EC-III foil and TP-III foil manufactured by Mitsui Mining & Smelting Co., Ltd.

[0223] [Semiconductor Devices] The semiconductor device of the present invention includes the printed wiring board of the present invention. The semiconductor device of the present invention can be manufactured by using the printed wiring board of the present invention.

[0224] Examples of the semiconductor device include various semiconductor devices used in electric appliances (for example, computers, mobile phones, digital cameras, and televisions) and vehicles (for example, motorcycles, automobiles, trains, ships, and aircraft). EXAMPLES

[0225] The present invention will be specifically described below with reference to examples. The present invention is not limited to these examples. In the following, "parts" and "%" representing amounts mean "parts by mass" and "% by mass", respectively, unless otherwise specified. Unless otherwise specified, the temperature and pressure conditions are room temperature (23°C) and atmospheric pressure (1 atm).

[0226] <Synthesis Example 1: Synthesis of active ester compound (B-1)> In a flask equipped with a thermometer, dropping funnel, condenser, distillation tube, and stirrer, 320g (2.0 mol) of 2,7-dihydroxynaphthalene, 184g (1.7 mol) of benzyl alcohol, and 5.0g of paratoluenesulfonic acid monohydrate were charged and stirred at room temperature while blowing in nitrogen. The temperature was then raised to 150°C, and the mixture was stirred for 4 hours while distilling off the water produced. After the reaction was completed, 900g of methyl isobutyl ketone and 5.4g of 20% aqueous sodium hydroxide solution were added to neutralize the mixture, and the aqueous layer was removed by separation. The mixture was washed three times with 280g of water, and methyl isobutyl ketone was removed under reduced pressure to obtain 460g of benzyl-modified naphthalene compound (A-1). The obtained benzyl-modified naphthalene compound (A-1) was a black solid, and had a hydroxyl equivalent of 180g / equivalent.

[0227] In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 203.0 g of isophthalic acid chloride (molar number of acid chloride groups: 2.0 mol) and 1400 g of toluene were charged, and the system was purged with reduced pressure and nitrogen to dissolve. Next, 113.9 g (0.67 mol) of orthophenylphenol and 240 g of benzyl-modified naphthalene compound (A-1) (molar number of phenolic hydroxyl groups: 1.33 mol) were charged, and the system was purged with reduced pressure and nitrogen to dissolve. Then, 0.70 g of tetrabutylammonium bromide was dissolved, and while applying nitrogen gas purge, the system was controlled to 60°C or less, and 400 g of 20% aqueous sodium hydroxide solution was dropped over 3 hours. Then, stirring was continued under these conditions for 1.0 hour. After the reaction was completed, the mixture was left to stand for liquid separation, and the aqueous layer was removed. Further, water was added to the toluene layer in which the reactant was dissolved, and the mixture was stirred and mixed for 15 minutes, and the mixture was allowed to stand and separated to remove the aqueous layer. This operation was repeated until the pH of the aqueous layer reached 7. Thereafter, water was removed by decanting to obtain an active ester compound (B-1) in a toluene solution state with a non-volatile content of 61.5 mass%. The active ester equivalent of the obtained active ester compound (B-1) was 238 g / eq.

[0228] <Synthesis Example 2: Synthesis of active ester compound (B-2)> In a flask equipped with a thermometer, a dropping funnel, a cooling tube, a fractionating tube, and a stirrer, 165g of a polyaddition reaction resin of dicyclopentadiene and phenol (hydroxyl equivalent: 165g / eq., softening point 85°C), 134g (1.0mol) of orthoallylphenol, and 1200g of toluene were charged, and the system was purged with nitrogen under reduced pressure. Next, 203g (1.0mol) of isophthalic acid chloride was charged, and the system was purged with nitrogen under reduced pressure. 0.6g of tetrabutylammonium bromide was added, and while performing a nitrogen gas purging treatment, the system was controlled to 60°C or less, and 412g of a 20% aqueous sodium hydroxide solution was dropped over 3 hours. After the dropwise addition was completed, the mixture was stirred for 1.0 hour. After the reaction was completed, the aqueous layer was removed by standing and separating. Water was further added to the obtained toluene layer, and the mixture was stirred for 15 minutes, and the aqueous layer was removed by standing and separating. This operation was repeated until the pH of the aqueous layer reached 7. The non-volatile content was adjusted to 70% by mass by drying with heat, to obtain an active ester compound (B-2) represented by the following formula. In the formula, each s is independently an integer of 0 or 1 or more, and the average value of r calculated from the charge ratio is 1. The dashed line in the formula represents a structure obtained by reaction of isophthalic acid chloride and a polyaddition reaction resin of phenol and / or ortho-allylphenol. The ester group equivalent of the obtained active ester resin was calculated from the charge ratio to be 214 g / eq. [ka]

[0229] <Production of resin varnish> Each component was weighed out in the amount of parts by mass shown in the table below, and then mixed with 10 parts of MEK and 10 parts of cyclohexanone, and uniformly dispersed using a high-speed rotating mixer to obtain a resin varnish. The details of each component shown in the table are as follows. (A) Component: ·HP-4032-SS: Functional group equivalent 144g / eq., manufactured by DIC ESN-475V: Functional group equivalent weight 330g / eq., manufactured by Nippon Steel Chemical & Material Co., Ltd. ·NC-3100: Functional group equivalent 258g / eq., manufactured by Nippon Kayaku Co., Ltd. (B) Ingredients: HPC-8150-62T: functional group equivalent weight 223g / eq., non-volatile content 62% by mass in toluene solution, manufactured by DIC Corporation HPC-8000-65T: Functional group equivalent weight 229g / eq., non-volatile content 65% by mass in toluene solution, manufactured by DIC Corporation Active ester compound (B-1): Synthesized in Synthesis Example 1 Active ester compound (B-2): Synthesized in Synthesis Example 2 PC1300-02: Methyl amyl ketone solution with functional group equivalent of 199 g / eq. and non-volatile content of 65% by mass, manufactured by Air Water Performance Chemicals (C) Ingredients: PX1250: Terpene resin with a softening point of 125°C, manufactured by Yasuhara Chemical Co., Ltd. TO125: Aromatic modified terpene resin with a softening point of 125°C, manufactured by Yasuhara Chemical Co., Ltd. (D) Ingredients: Maleimide A: a compound represented by the following formula (1) (Mw / Mn = 1.81, t'' = 1.47 (mainly 1, 2 or 3)) synthesized by the method described in Synthesis Example 1 of the Japan Institute of Invention and Innovation's Technical Journal Publication No. 2020-500211, MEK solution with 62% non-volatile components [ka] MIR-5000-60T: toluene solution with 60% non-volatile content, manufactured by Nippon Kayaku Co., Ltd. MIR-3000-70T: BMI-689: Designer Molecules A-DOG: Manufactured by Nippon Kayaku Co., Ltd. OPE-2St-1200: toluene solution with 65% non-volatile content, manufactured by Mitsubishi Gas Chemical Co., Ltd. SLK-2600: Anisole solution with 50% non-volatile content, manufactured by Shin-Etsu Chemical Co., Ltd. (E) Ingredients: SO-C2: Spherical silica surface-treated with an amine-based alkoxysilane compound (Shin-Etsu Chemical Co., Ltd.'s "KBM573"), with an average particle size of 0.5 μm and a specific surface area of ​​5.8 m 2 / g, manufactured by Admatechs Co., Ltd. BA-S: Spherical silica with hollow parts, surface-treated with an amine-based alkoxysilane compound ("KBM573" manufactured by Shin-Etsu Chemical Co., Ltd.), average particle size 2-3 μm, manufactured by JGC Catalysts and Chemicals Co., Ltd. (F) Ingredients: LA-3018-50P: 1-methoxy-2-propanol solution with functional group equivalent of 151 g / eq. and non-volatile content of 50% by mass, manufactured by DIC Corporation (G) Ingredients: 1B2PZ: Shikoku Chemical Industry Co., Ltd.

[0230] [Table 1] *In the table, the content of component (C) represents the content (mass %) when the resin component is taken as 100 mass %, and the content of component (E) represents the content (mass %) when the non-volatile components in the resin composition are taken as 100 mass %.

[0231] <Measurement of dielectric constant and dielectric tangent> (1) Preparation of resin sheet A having a resin composition layer thickness of 40 μm A polyethylene terephthalate film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. On the release layer of this support, the resin varnish obtained in the examples and comparative examples was uniformly applied so that the thickness of the resin composition layer after drying was 40 μm. Thereafter, the resin composition was dried at 80°C to 100°C (average 90°C) for 4 minutes to obtain a resin sheet A including a support and a resin composition layer.

[0232] (2) Preparation of hardened product The resin sheet A obtained in each of the examples and comparative examples was cured for 90 minutes in an oven at 190° C. The support was peeled off from the resin sheet A taken out of the oven to obtain a cured product of the resin composition layer.

[0233] (3) Measurement of dielectric constant and dielectric loss tangent Each evaluation cured product was cut into a length of 80 mm and a width of 2 mm, and the dielectric constant and dielectric tangent (Dk and Df values) were measured by the cavity resonance perturbation method using an Agilent Technologies HP8362B at a measurement frequency of 5.8 GHz and measurement temperatures of 23°C and 90°C. Measurements were performed on two test pieces, and the average was calculated.

[0234] (4) Measurement of glass transition temperature (Tg) Each cured product for evaluation was cut into an evaluation sample with a length of 20 mm and a width of 6 mm. The glass transition temperature (Tg) of this evaluation sample was measured at a heating rate of 5°C / min from 25°C to 250°C using a TMA device manufactured by Rigaku Corporation. The same test piece was measured twice, and the second value was recorded.

[0235] <Preparation of Resin Sheet B Having a Resin Composition Layer Thickness of 25 μm> A polyethylene terephthalate film with a release layer ("AL5" manufactured by Lintec Corporation, thickness 38 μm) was prepared as a support. On the release layer of this support, the resin varnish obtained in the examples and comparative examples was uniformly applied so that the thickness of the resin composition layer after drying was 25 μm, and dried at 70°C to 80°C (average 75°C) for 2.5 minutes to obtain a resin sheet B including a support and a resin composition layer.

[0236] <Evaluation of crack resistance after desmear treatment> The 25 μm thick resin sheet B prepared above was laminated on both sides of a core material (Hitachi Chemical Co., Ltd. "E705GR", thickness 400 μm) in which circular copper pads (copper thickness 35 μm) with a diameter of 350 μm were formed in a grid pattern at intervals of 400 μm so that the residual copper ratio was 60%. Using a batch-type vacuum pressure laminator (Nikko Materials Co., Ltd. 2-stage build-up laminator "CVP700"), the resin composition layer was bonded to the inner layer substrate. This lamination was performed by decompressing for 30 seconds to an atmospheric pressure of 13 hPa or less, and then pressing for 30 seconds at a temperature of 100 ° C and a pressure of 0.74 MPa. This was placed in a 130 ° C oven and heated for 30 minutes, and then transferred to a 170 ° C oven and heated for 30 minutes. The support layer was then peeled off, and the resulting circuit board was immersed in a swelling solution, Swelling Dip Securigant P, manufactured by Atotech Japan, at 60°C for 10 minutes. Next, the circuit board was immersed in a roughening solution, Concentrate Compact P (aqueous solution of KMnO4: 60g / L, NaOH: 40g / L), manufactured by Atotech Japan, at 80°C for 30 minutes. Finally, the circuit board was immersed in a neutralizing solution, Reduction Solution Securigant P, manufactured by Atotech Japan, at 40°C for 5 minutes. 100 copper pads of the circuit board after the roughening treatment were observed to check for the presence or absence of cracks in the resin composition layer, and were evaluated according to the following criteria. ○: 10 or less cracks ×: More than 10 cracks

[0237] [Table 2]

Claims

1. (A) an epoxy resin, (B) an active ester compound, and (C) a hydrocarbon polymer having a terpene skeleton, The component (C) is a resin composition having no polar group.

2. The resin composition according to claim 1 , wherein the component (C) comprises either a polyterpene resin or an aromatic modified terpene resin.

3. The resin composition according to claim 1, wherein the softening point of the component (C) is 50°C or higher.

4. The resin composition according to claim 1 , wherein the content of the component (C) is 1% by mass or more, based on 100% by mass of the resin component.

5. The resin composition according to claim 1 , further comprising (D) a radically polymerizable compound.

6. The resin composition according to claim 1 , further comprising (E) an inorganic filler.

7. The resin composition according to claim 6, wherein the content of the component (E) is 40% by mass or more, based on 100% by mass of non-volatile components in the resin composition.

8. The resin composition according to claim 1 , further comprising (F) a curing agent.

9. A sheet-like laminate material comprising the resin composition according to any one of claims 1 to 8.

10. A resin sheet comprising a support and a resin composition layer formed from the resin composition according to any one of claims 1 to 8 provided on the support.

11. A printed wiring board comprising an insulating layer made of a cured product of the resin composition according to any one of claims 1 to 8.

12. A semiconductor device comprising the printed wiring board according to claim 11.

Citation Information

Patent Citations

  • Epoxy resin composition for sealing semiconductor and method for sealing semiconductor

    JP1996208806A

  • Thermosetting composition, and sealing article and sealing structure made by using it

    JP2002121351A

  • Resin composition

    JP2003201402A

  • Insulation sheet and laminated structural body

    JP2009224109A

  • Thermosetting resin composition, resin film for interlayer insulation, composite film, printed wiring board and method for producing the same

    JP2019157027A