Gas Sensors

A gas sensor combining platinum nanowires with a high-resistance semiconductor oxide layer addresses sensitivity and speed issues in existing oxygen sensors by creating dual conduction paths, enabling rapid and sensitive oxygen detection at low temperatures.

JP7593687B2Active Publication Date: 2024-12-03THE JAPAN SCI & TECH AGENCY
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023502307
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-02-25
Filing Date
2022-02-15
Publication Date
2024-12-03
Estimated Expiration
2042-02-15

AI Technical Summary

Technical Problem

Existing oxygen gas sensors, such as those using solid electrolytes and oxide semiconductors, suffer from insufficient sensitivity and slow response speeds, particularly at lower operating temperatures, and gas sensors with platinum nanowires do not detect oxygen gas effectively.

Method used

A gas sensor is developed that combines platinum nanowires with a high-resistance semiconductor oxide layer, forming two conduction paths to enhance sensitivity and response speed by injecting carriers through the nanowire into the oxide layer, achieving ohmic contact and reducing activation energy.

Benefits of technology

The sensor achieves fast response speed and high sensitivity to oxygen gas, operating effectively at low temperatures and across a wide range of oxygen concentrations, with potential for low power consumption and wide applicability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007593687000005
    Figure 0007593687000005
  • Figure 0007593687000006
    Figure 0007593687000006
  • Figure 0007593687000007
    Figure 0007593687000007
Patent Text Reader

Abstract

Provided is a gas sensor that has a fast response speed and high sensitivity to oxygen gas. This gas sensor 100 has: a substrate 10; a first pad electrode 12A and a second pad electrode 12B; a nanowire 14 comprising a specific metal; and an oxide layer 16 comprising a highly resistant semiconductor comprising an oxide from a different type of metal from the metal that constitutes the nanowire 14. The first pad electrode 12A and the second pad electrode 12B are formed upon the substrate 10. The nanowire 14 couples the first pad electrode 12A and the second pad electrode 12B and is formed upon the substrate 10. The oxide layer 16 is formed so as to abut the nanowire 14. A high-speed response and high sensitivity to oxygen gas is achieved as a result of this contact between the nanowire 14 and the oxide layer 16.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a gas sensor that combines nanowires made of a specific metal with an oxide made of a high-resistance semiconductor. [Background technology]

[0002] Currently, various gas sensors are used in electrical appliances, vehicles, ships, aircraft, and the like that support our daily lives. For example, in an automobile, it is necessary to control the mixture ratio of air and fuel supplied to the engine in order to improve the combustion efficiency of the engine and ensure that exhaust gas meets environmental standards, and an oxygen gas sensor using a solid electrolyte (e.g., zirconia) as described in Patent Document 1 is used in the control system. Another known oxygen gas sensor is a resistive oxygen gas sensor using an oxide semiconductor as described in Patent Document 2.

[0003] Non-Patent Document 1 also describes a gas sensor in which a first pad electrode, a second pad electrode, and a platinum nanowire connecting these pad electrodes are formed on a glass substrate. This gas sensor detects hydrogen gas based on a change in resistance detected between the first pad electrode and the second pad electrode when a constant voltage is applied between the first pad electrode and the second pad electrode. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2015-137998 A [Patent Document 2] JP 2003-149189 A [Non-patent literature]

[0005] [Non-Patent Document 1] F. Yang et al., The Surface Scattering-Based Detection of Hydrogen in Air Using a Platinum Nanowire, Nano Lett. 12 (2012) 2924-2930 Summary of the Invention [Problem to be solved by the invention]

[0006] An oxygen gas sensor using a solid electrolyte as described in Patent Document 1 requires a reference gas, and has problems of insufficient sensitivity to oxygen and slow response speed (response time of about several tens of seconds).In addition, a resistance-type oxygen gas sensor using an oxide semiconductor as described in Patent Document 2 can achieve a response speed of 10 seconds or less at very high operating temperatures such as 900°C or 600°C, but at relatively low operating temperatures of about 300°C, the response time is several hundred seconds or more, and the response speed is slow, so it cannot be said to meet industrial needs.

[0007] In addition, the gas sensor using platinum nanowires described in Non-Patent Document 1 detects hydrogen gas, but does not describe its detection of oxygen gas. In other words, the sensor characteristics such as response speed and sensitivity to oxygen gas have not been verified at all.

[0008] In view of the above problems, an object of the present invention is to provide a gas sensor having a high response speed and high sensitivity to oxygen gas. [Means for solving the problem]

[0009] In order to solve the above problems, the present inventors have conducted extensive research and have obtained the following findings. The present inventors have conceived of a gas sensor that combines a nanowire made of a specific metal such as platinum (Pt) with an oxide layer made of a specific high-resistance semiconductor. By arranging the nanowire in contact with the oxide layer made of a high-resistance semiconductor, in addition to the first conductive path through which carriers (oxygen vacancies, electrons, etc.) pass through the nanowire, a second conductive path is formed in which carriers (oxygen vacancies, electrons, etc.) are injected from the nanowire into the oxide layer, move through the oxide layer, and return to the nanowire. The present inventors have found that the presence of these two conductive paths makes it possible to obtain the remarkable effects of a fast response speed and high sensitivity to oxygen gas.

[0010] The present invention, which has been completed based on the above findings, has the following essential features. [1] A substrate having an insulating surface; a first pad electrode and a second pad electrode formed on or above the insulating surface of the substrate; a nanowire formed on or above the insulating surface of the substrate, connecting the first pad electrode and the second pad electrode, the nanowire being made of at least one selected from platinum (Pt), palladium (Pd), rhodium (Rh), ruthenium (Ru), osmium (Os), iridium (Ir), and alloys thereof; an oxide layer in contact with the nanowire, the oxide layer being made of a high-resistance semiconductor of an oxide of a metal different from the metal constituting the nanowire, the oxide layer satisfying at least one of the following: (I) being located between the insulating surface of the substrate and the nanowire and in contact with the bottom surface of the nanowire, or (II) being located on the nanowire and in contact with the top surface of the nanowire; having A gas sensor that causes a current to flow between the first pad electrode and the second pad electrode, and detects a gas based on a change in an electrical signal detected between the first pad electrode and the second pad electrode.

[0011] [2] The gas sensor according to the above [1], wherein the line width of the nanowire is 5 nm or more and 150 nm or less, preferably 50 nm or less, and more preferably 30 nm or less.

[0012] [3] The gas sensor according to the above [1] or [2], wherein the thickness of the nanowire is 1 nm or more and 20 nm or less, preferably 10 nm or less.

[0013] [4] The gas sensor according to any one of the above [1] to [3], wherein the length of the nanowire is 80 nm or more, preferably 400 nm or more, and 1 m or less.

[0014] [5] The gas sensor according to any one of the above [1] to [4], wherein the high-resistance semiconductor constituting the oxide layer is one or more selected from cerium oxide, tin oxide, zirconium oxide, zinc oxide, tungsten oxide, iron oxide, nickel oxide, cerium-zirconium oxide, titanium oxide, cobalt oxide, niobium oxide, tantalum oxide, rhodium oxide, and hafnium oxide.

[0015] [6] The gas sensor according to any one of the above [1] to [5], wherein the oxide layer has a thickness of 5 nm or more, and preferably 100 nm or less.

[0016] [7] The gas sensor according to any one of the above [1] to [6], wherein the nanowire and the oxide layer are in ohmic contact with each other.

[0017] [8] The gas sensor according to any one of the above [1] to [7], wherein the substrate is any one of a glass substrate, an alumina substrate, a zirconia substrate, and a silicon substrate having a silicon oxide film formed on the surface thereof.

[0018] [9] The gas sensor according to any one of the above [1] to [8], wherein the first pad electrode and the second pad electrode are made of the same metal as the nanowire.

[0019]

[10] The gas sensor according to any one of the above [1] to [9], wherein the gas is oxygen gas. Effect of the Invention

[0020] The gas sensor of the present invention has a fast response speed and high sensitivity to oxygen gas. [Brief description of the drawings]

[0021] [Figure 1A] FIG. 1 is a schematic perspective view of a gas sensor 100 according to an embodiment of the present invention. [Figure 1B] FIG. 1 is a schematic top view of a gas sensor 100. [Figure 1C] FIG. 2 is a cross-sectional view of FIG. 1B. [Figure 1D] FIG. 2 is a cross-sectional view taken along line II-II of FIG. 1B. [Diagram 2] 1A to 1E are diagrams illustrating a manufacturing process of the gas sensor 100 according to an embodiment of the present invention. [Diagram 3] 1 shows SEM images of the top surface of a gas sensor with various values ​​of nanowire line width W and line length L. [Figure 4] 1 is a graph showing changes in current I over time in Experimental Example 1. [Diagram 5] 13 is a graph showing changes in current I over time in Experimental Example 2. [Figure 6] 13 is a graph showing changes in current I over time in Experimental Example 3. [Figure 7A] 13 is a graph showing changes in current I over time in Experimental Example 4. [Figure 7B] 13 is a graph showing changes in current I over time in Experimental Example 4. [Figure 8A] 13 is a graph showing changes in current I over time in Experimental Example 5. [Figure 8B] 13 is a graph showing changes in current I over time in Experimental Example 5. [Figure 9] 13 is a graph showing the change over time of current I in Experimental Example 6. [Figure 10] 13 is a graph showing the change over time of current I in Experimental Example 7. [Figure 11] 13 is a graph showing the change over time of current I in Experimental Example 8. [Figure 12] 13 is a graph showing the change over time of current I in Experimental Example 9. [Figure 13] 13(A) and 13(B) are graphs showing the change in current I over time in Experimental Example 10. [Figure 14] 13 is a graph showing the change over time of current I in Experimental Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0022] (Gas sensor) 1A, 1B, 1C, and 1D, a gas sensor 100 according to an embodiment of the present invention includes a substrate 10, a first pad electrode 12A, a second pad electrode 12B, a nanowire 14 made of a specific metal, and an oxide layer 16 made of a high resistance semiconductor. The first pad electrode 12A and the second pad electrode 12B are formed on or above the substrate 10. The nanowire 14 connects the first pad electrode 12A and the second pad electrode 12B and is formed on or above the substrate 10. The oxide layer 16 is formed so as to be in contact with the nanowire 14. Although detailed effects will be described later, in this embodiment, the contact between the nanowire 14 and the oxide layer 16 realizes high-speed response and high sensitivity to oxygen gas. In this specification, "A formed on or above B" means that A is formed directly on B or indirectly via another layer.

[0023] [Gas detection mechanism] In the gas sensor 100, a current is passed between the first pad electrode 12A and the second pad electrode 12B, and gas is detected based on a change in an electric signal detected between the first pad electrode 12A and the second pad electrode 12B. For example, as shown in FIG. 1B, a power supply 18 and an ammeter 20 are connected in series between the first pad electrode 12A and the second pad electrode 12B, and a voltmeter 22 is connected in parallel thereto. In this case, the power supply 18 applies a constant voltage between the first pad electrode 12A and the second pad electrode 12B, and the ammeter 20 detects a change in the current between the first pad electrode 12A and the second pad electrode 12B, and gas is detected based on the detected change in current. Alternatively, gas can be detected based on a change in the voltage detected between the first pad electrode 12A and the second pad electrode 12B, while a constant current is passed between the first pad electrode 12A and the second pad electrode 12B. Also, instead of the above-mentioned change in current or voltage, gas can be detected based on a change in resistance detected between the first pad electrode 12A and the second pad electrode 12B. That is, the above-mentioned "electrical signal" means a current, a voltage, or a resistance. In this embodiment, the gas sensor circuit can be configured with two terminals, so that the gas sensor can be constructed without increasing the wiring or the circuit. Although the type of gas detected in this embodiment is not particularly limited, this embodiment is suitable for detecting oxygen gas.

[0024] [substrate] The substrate 10 supports the first pad electrode 12A and the second pad electrode 12B, as well as the nanowires 14 and oxide layer 16 that serve as the gas detector. The substrate 10 is not particularly limited as long as it has an insulating surface, and may be, for example, an insulating substrate such as a glass substrate, an alumina substrate, or a zirconia substrate, or a silicon substrate having a silicon oxide film formed on its surface. The shape and dimensions of the substrate 10 are not particularly limited, but when a substrate whose main surface is rectangular is used, the dimensions may be, for example, in the range of length: 10 to 300 mm x width: 10 to 300 mm x thickness: 0.3 to 1.2 mm.

[0025] [First pad electrode and second pad electrode] The first pad electrode 12A and the second pad electrode 12B are a pair of electrodes necessary for supplying a current to the nanowire 14 and detecting a change in an electric signal corresponding to a change in gas concentration. The shape and dimensions of the first pad electrode 12A and the second pad electrode 12B are not particularly limited as long as they are formed on or above the insulating surface of the substrate 10, but when the shape of the main surface is rectangular, the dimensions can be, for example, in the range of length: 30 to 500 μm × width: 30 to 500 μm × thickness: 10 to 500 nm. The metal constituting the first pad electrode 12A and the second pad electrode 12B is not particularly limited and may be any metal, but from the viewpoint of process simplicity, it is preferable that the metal is the same type as the nanowire described below.

[0026] [Nanowires] The nanowire 14 is one of the elements constituting the gas detection unit, which connects the first pad electrode 12A and the second pad electrode 12B and is formed on or above the insulating surface of the substrate 10. It is essential that the nanowire 14 is made of one or more selected from platinum (Pt), palladium (Pd), rhodium (Rh), ruthenium (Ru), osmium (Os), iridium (Ir), and alloys thereof. Among them, it is preferable that the nanowire 14 is made of one or more selected from platinum (Pt), palladium (Pd), and alloys thereof, and it is most preferable that the nanowire 14 is made of one or more selected from platinum (Pt) and alloys thereof. These elements used in the nanowire 14 are platinum group elements and function as catalysts. The platinum group elements as catalysts have the effect of activating gas, promoting gas adsorption and chemical reaction between oxide and gas, increasing the amount of adsorbed oxygen, and increasing oxygen ions. These catalytic effects improve the sensitivity of the gas response.

[0027] The shape of nanowire 14 is not particularly limited, but as shown in FIG. 1D, it is preferable that the cross-sectional shape perpendicular to the extension direction of nanowire 14 is rectangular.

[0028] The line width W of nanowire 14 is not particularly limited as long as it is on the order of nm (i.e., less than 1 μm), but from the viewpoint of more fully realizing high-speed response and high sensitivity to oxygen gas, it is preferably 150 nm or less, more preferably 50 nm or less, and even more preferably 30 nm or less. Moreover, from the viewpoint of high-speed response and high sensitivity, the narrower the line width W of nanowire 14, the more preferable it is, so there is no particular lower limit. However, due to process constraints, it is preferable that the line width W of nanowire 14 be 5 nm or more.

[0029] The thickness of the nanowire 14 is not particularly limited, but from the viewpoint of more fully realizing a high-speed response and high sensitivity to oxygen gas, it is preferably 20 nm or less, and more preferably 10 nm or less. Moreover, from the viewpoint of a high-speed response and high sensitivity, the thinner the thickness of the nanowire 14, the more preferable, and therefore the lower limit of the thickness is not particularly limited. However, from the viewpoint of process constraints and electrical conduction as a nanowire, the thickness of the nanowire 14 is preferably 1 nm or more.

[0030] The cross-sectional area of ​​the nanowire 14 perpendicular to the extending direction is not particularly limited, but from the viewpoint of more fully realizing high-speed response and high sensitivity to oxygen gas, it is preferably 3000 nm 2 It is preferable that the thickness is less than 1500 nm. 2 More preferably, it is 1000 nm or less. 2 More preferably, it is 600 nm or less. 2 More preferably, it is 500 nm or less. 2 More preferably, it is 300 nm or less. 2 It is more preferable that the cross-sectional area of ​​the nanowire 14 perpendicular to the extending direction is smaller from the viewpoint of high-speed response and high sensitivity, and therefore the lower limit is not particularly limited. However, due to process constraints, the cross-sectional area of ​​the nanowire 14 perpendicular to the extending direction is preferably 15 nm or less. 2 More preferably, it is equal to or greater than this.

[0031] The length L of the nanowire 14 is not particularly limited, but from the viewpoint of more fully realizing a high-speed response and high sensitivity to oxygen gas, it is preferably 80 nm or more, and more preferably 400 nm or more. The length L of the nanowire 14 is preferably as long as possible from the viewpoint of a high-speed response and high sensitivity, and therefore, the upper limit of the length L of the nanowire 14 is not particularly limited. However, due to process constraints, the length L of the nanowire 14 is preferably 1 m or less.

[0032] [Oxide layer] The oxide layer 16 is made of a high-resistance semiconductor and is in contact with the nanowire 14. In this embodiment, high-speed response and high sensitivity to oxygen gas are achieved by this contact between the nanowire 14 and the oxide layer 16. It is essential that the contact between the nanowire 14 and the oxide layer 16 satisfies at least one or both of the following: (I) the oxide layer 16 is located between the insulating surface of the substrate 10 and the nanowire 16 and is in contact with the lower surface of the nanowire 14, or (II) the oxide layer 16 is located on the nanowire 14 and is in contact with the upper surface of the nanowire 14.

[0033] As shown in Fig. 1A, this embodiment relates to the above-mentioned mode (I), in which an oxide layer 16 is located on the insulating surface of a substrate 10, and a first pad electrode 12A, a second pad electrode 12B, and a nanowire 14 are located on the oxide layer 16. However, the present invention is not limited to this, and may relate to the above-mentioned mode (II), for example, the first pad electrode 12A, a second pad electrode 12B, and a nanowire 14 may be located on the insulating surface of a substrate 10, and an oxide layer 16 may be formed on the nanowire 14. The above-mentioned modes (I) and (II) also include a case where the nanowire 14 is embedded in the oxide layer 16, or a case where the oxide layer 16 contacts the side surface of the nanowire 14 in addition to the upper and lower surfaces.

[0034] The high-resistance semiconductor constituting the oxide layer 16 may be any oxide semiconductor having a resistivity of 1 Ω·m or more and 100,000 Ω·m or less at 300° C., and is preferably at least one selected from, for example, cerium oxide (CeO2), tin oxide (SnO2), zirconium oxide (ZrO2), zinc oxide (ZnO), tungsten oxide (WO3), iron oxide (Fe2O3), nickel oxide (NiO), cerium-zirconium oxide (CeZrO4), titanium oxide (TiO2), cobalt oxide (Co3O4), niobium oxide (Nb2O5), tantalum oxide (Ta2O5), rhodium oxide (Rh2O3), and hafnium oxide (HfO2), and among these, it is particularly preferable to use at least one selected from cerium oxide, tin oxide, and zirconium oxide. The oxide semiconductor may be not only an oxide of stoichiometric composition, but also an oxide deviating from the stoichiometric composition, and may contain oxides with different oxidation numbers. Oxygen is adsorbed on the surface of the oxide semiconductor constituting the oxide layer 16. The adsorbed oxygen extracts electrons from the oxide semiconductor, and O - Or O 2- The oxygen ions are as follows: Oxygen ion O - Or O 2- Since it has a negative charge, in the case of an n-type semiconductor, it depletes the surface and reduces the electrical conductivity, while in the case of a p-type semiconductor, it increases the carrier concentration and increases the electrical conductivity. When oxygen ions adsorbed on the surface react chemically with gas, the oxygen ions are removed and the surface charge caused by the oxygen ions disappears. This changes the electrical conductivity of the oxide semiconductor. This change in electrical conductivity in the oxide semiconductor changes the electrical conductivity flowing parallel to the nanowire, leading to the detection of the gas response.

[0035] It is important that the high resistance semiconductor (oxide semiconductor) constituting the oxide layer 16 is an oxide of a metal different from the metal constituting the nanowire 14. The adsorption, generation, and annihilation of oxygen / oxygen ions, and further the generation and annihilation of oxygen vacancies, each require activation energy, and these activation energies depend on the oxide semiconductor. For example, when the oxide semiconductor is an oxide of the metal constituting the nanowire 14, such as the combination of Pt / PtO2, the activation energy is high, the response time and recovery time of the gas sensor are slow, and the sensitivity is low. On the other hand, when the oxide semiconductor is an oxide of a metal different from the metal constituting the nanowire 14, the activation energy is low, and the response time and recovery time of the gas sensor are fast, and the sensitivity is high.

[0036] The thickness of the oxide layer 16 is not particularly limited, but is preferably 5 nm or more from the viewpoint of more fully realizing high-speed response and high sensitivity to oxygen gas. Regarding the oxide layer 16 located in the position of the above aspect (I), the upper limit of the thickness is not particularly limited, but since the effect of the present invention is saturated even if the thickness is excessive, the thickness of the oxide layer 16 is preferably 100 nm or less from the viewpoint of cost and process time. Regarding the oxide layer 16 located in the above position (II), the upper limit of the thickness is not particularly limited, but since an excessive thickness leads to poor gas permeability and insufficient supply of gas to the nanowires 14, the thickness of the oxide layer 16 is preferably 100 nm or less.

[0037] [Contact between nanowire and oxide layer] As described above, in this embodiment, it is essential that the nanowire 14 and the oxide layer 16 are in contact with each other, specifically that they form an ohmic contact. This forms, in addition to a first conductive path through which carriers (oxygen vacancies, electrons, etc.) pass through the nanowire 14, a second conductive path is formed through which carriers (oxygen vacancies, electrons, etc.) are injected from the nanowire 14 into the oxide layer 16, move through the oxide layer 16, and return to the nanowire 14. The presence of these two conductive paths provides the remarkable effects of a fast response speed and high sensitivity to oxygen gas.

[0038] Although not intended to limit the present invention, the present inventors believe that the mechanism by which such effects are obtained is as follows.

[0039] In oxides, oxygen defects (oxygen vacancies) occur depending on the oxygen concentration, and the lower the oxygen concentration, the higher the oxygen defect density. These oxygen defect sites trap electrons and act as donor sites that release the electrons. Electrons released from these oxygen defects are supplied to the conductor and become carriers, which conduct through bands, or they conduct through hopping between oxygen defect sites.

[0040] The metals (Pt, Pd, etc.) that make up the nanowires contribute to reducing the activation energy that creates oxygen defects through catalytic action, making it easier for oxygen defects to occur. In addition, they lower the activation energy for the transfer of electrons (charge injection) at the interface between the metal and oxide, reducing the height of the Schottky barrier between the metal and oxide. Oxygen defects also contribute to thinning the width of the Schottky barrier to a few tens of nanometers or less in order to increase the carrier density near the interface. Both the reduction in barrier height through catalytic action and the increase in carrier density through oxygen defects reduce the resistance based on the Schottky barrier between the metal and oxide, making ohmic contact possible. At an interface that has become ohmic contact, the resistance is almost constant regardless of the electric field at the interface, making it difficult to inhibit the transfer of electrons at the metal / oxide interface.

[0041] Atoms of metals (Pt, Pd, etc.) in contact with an oxide diffuse relatively easily into the oxide during metal deposition on the oxide or annealing at several hundreds of degrees Celsius, and are atomically doped into the oxide. When an oxide is doped with metal atoms in this way, its catalytic action becomes extremely high compared to bulk metals. In an oxide doped with metal atoms, oxygen defects are more likely to occur due to the high catalytic action, the barrier height is lower, and the barrier width is more likely to become thin due to the increased carrier concentration, compared to an undoped oxide. Due to these effects, doping of an oxide with metal atoms contributes to improving the gas sensor response due to the ease of oxygen defects, forming ohmic contacts, reducing ohmic resistance, and improving the electronic conductivity in the oxide.

[0042] Electrons injected from the metal to the oxide through the ohmic contact at the metal / oxide interface can flow through the oxide by band conduction or hopping conduction and return to the nanowire with which it is in ohmic contact. When a voltage is applied to both ends of a nanowire where a metal nanowire and an oxide are in contact, electronic conduction occurs in the metal within the metallic nanowire. This electronic conduction within the wire is supplemented by electronic conduction through a conduction path (bypass circuit) where charges injected from the metal to the oxide are conducted through the oxide and return to the metal. The current flowing through this bypass circuit via the oxide is strongly dependent on the oxygen vacancy concentration, resulting in high sensitivity of the gas sensor response.

[0043] In an ohmic contact, the contact resistance does not depend on the electric field, so the frequency of electron injection between the metal and oxide does not depend on the voltage applied to the wire end. This leads to the results of the present invention, where the gas sensor response is obtained even at an applied voltage of several tens of mV, similar to that at a high applied voltage.

[0044] It has been reported that the oxidation of metal on the metal surface increases the surface scattering in metallic conduction, and the change in conductivity due to the amount of this surface scattering results in a gas sensor response. A reduction action occurs at the interface where the metal and oxide contact, which causes oxygen vacancies in the oxide. This reduction action leads to the reduction of the metal whose surface is oxidized. At the metal interface in contact with the oxide, the reduction action makes the metal less likely to oxidize, which reduces the surface scattering in metallic conduction within the metal wire. Furthermore, as is clear from the process of forming ohmic contacts, the surface scattering at the metal / oxide contact interface depends on the oxygen vacancy concentration, which changes the barrier height and barrier width of the Schottky interface. The gas sensor using the change in the surface scattering frequency of the electrical conduction of the metal nanowire and the present invention have different surface scattering mechanisms in electrical conduction, since the surface scattering is due to the oxygen vacancies of the oxide, unlike the surface scattering due to the oxidation of the surface of the metal alone as described above.

[0045] [effect] As described above, the gas sensor 100 of this embodiment has the advantages of a fast response speed to oxygen gas (i.e., a short response time and a short recovery time) and high sensitivity. The gas sensor 100 of this embodiment also has the advantage of being able to detect oxygen gas even at a low operating temperature (for example, about 60 to 300°C). The gas sensor 100 of this embodiment also has the advantage of being able to detect oxygen gas even at a low oxygen gas concentration, thereby having a wide range of detectable oxygen gas concentrations.

[0046] [Gas sensor manufacturing method] A suitable method for manufacturing the gas sensor 100 of this embodiment will be described with reference to FIGS.

[0047] 2(A), first, an oxide layer 16 is formed on a substrate 10. Specifically, a precursor solution of the oxide constituting the oxide layer 16 is prepared, and the precursor solution is applied onto the substrate 10, after which the substrate 10 is subjected to a heat treatment. For example, when forming a cerium oxide (CeO2) layer, a cerium oxide (CeO2) precursor solution of a predetermined concentration can be prepared by dissolving cerium acetate hydrate Ce(CH3CO2)3·xH2O in propionic acid.

[0048] The precursor materials for obtaining each oxide are listed below. One or more of these precursor materials can be used. Cerium oxide (CeO2): cerium acetate hydrate Ce(CH3CO2)3·xH2O; cerium nitrate hexahydrate Ce[NO3]3·6H2O; cerium acetylacetonate hydrate Ce[C5H7O2]3·xH2O Tin oxide (SnO2): Anhydrous tin(II) chloride SnCl2: Tin(II) acetylacetonate C 10 H 14 O4Sn; Tin(IV) tert-butoxide Sn[OC(CH3)3]4 Zirconium oxide (ZrO2): Zirconium(IV) butoxide Zr(OC4H9)4; Zirconium(IV) isopropoxide isopropanol complex Zr(OCH(CH3)2)4·(CH3)2CHOH; Zirconium(IV) oxynitrate hydrate ZrO(NO3)2·xH2O Zinc oxide (ZnO); Zinc nitrate hexahydrate Zn[NO3]2·6H2O; Zinc(II) acetylacetonate C 10 H 14 O4Zn;Zinc acetate dihydrate Zn[CH3COO]2·2H2O Tungsten oxide (WO3): Tungsten(VI) chloride WCl6; Tungsten(VI) ethoxide C 12 H 30 O6W Iron oxide (Fe2O3): Iron nitrate nonahydrate Fe[NO3]3·9H2O; Iron(II) acetate Fe[CO2CH3]2; Iron(III) acetylacetonate Fe[C5H7O2]3 Nickel oxide (NiO): Nickel(II) acetylacetonate Ni(C5H7O2)2; Nickel(II) acetate tetrahydrate Ni[OCOCH3]2·4H2O; Nickel(II) nitrate hexahydrate Ni[NO3]2·6H2O Cerium-zirconium oxide (CeZrO4): cerium acetate hydrate Ce(CH3CO2)3·xH2O; zirconium(IV) butoxide Zr(OC4H9)4 Titanium oxide (TiO2): Titanium(IV) isopropoxide Ti[OCH(CH3)2]4; Titanium(IV) butoxide Ti(OCH2CH2CH2CH3)4 Cobalt oxide (Co3O4): Cobalt nitrate hexahydrate Co[NO3]2·6H2O; Cobalt(II) acetylacetonate Co(C5H7O2)2; Cobalt(II) acetate [CH3CO2]2Co; Cobalt(II) chloride CoCl2 Niobium oxide (Nb2O5): Niobium(V) chloride NbCl5; Niobium(V) ethoxide Nb(OCH2CH3)5; Niobium n-butoxide C 20 H 45 NbO5 Tantalum oxide (Ta2O5): Tantalum(V) ethoxide Ta(OC2H5)5; Tantalum(V) tetraethoxide 2,4-pentanedionate C 13 H 27 O6Ta; Tantalum(V) chloride TaCl5 Rhodium oxide (Rh2O3): Rhodium(II) acetate dimer Rh2(OOCCH3)4; Rhodium(III) nitrate hydrate N3O9Rh·xH2O; Rhodium(III) acetylacetonate [CH3COCHCOCH3]3Rh Hafnium oxide (HfO2): Hafnium(IV) chloride HfCl4; Hafnium(IV) 2,4-pentanedionate C 20 H 28 O8Hf; Hafnium(IV) nitrate Hf(NO3)4

[0049] As the solvent, one or more selected from propionic acid, 2-methoxyethanol (CH3OCH2CH2OH), and 1-butanol (C4H9OH) can be used. The concentration of the precursor solution is not particularly limited, but is preferably about 0.05 to 0.5 mol / kg depending on the desired film thickness. The coating method is not particularly limited, but a spin coating method can be suitably used. The rotation speed in this case may be appropriately determined depending on the desired thickness, but may be in the range of 1000 to 4000 rpm, for example. The oxide layer 16 is required to have two functions, namely, electrical conductivity and gas permeability. In order to obtain high electrical conductivity, it is necessary to form a conductive path, and if there is a grain boundary or the like, it is difficult to obtain a response due to carrier traps at the boundary. On the other hand, in order to realize the increase and decrease of oxygen vacancies in the oxide in response to the gas atmosphere in the oxide near the nanowire, a porous structure with good gas permeability is desired. From the viewpoint of obtaining these two functions, the heat treatment conditions are preferably a heat treatment in which the atmosphere temperature is kept in the range of 250 to 800°C in an air atmosphere for 0.5 to 2 hours. The thickness of the oxide layer 16 may be adjusted by performing the combination of coating and heat treatment multiple times.

[0050] Next, as shown in FIG. 2(B), a resist film 30 is formed on the oxide layer 16. The resist film 30 can be formed by applying a photoresist composition for electron beam exposure onto the oxide layer 16 and drying it. There are no particular limitations on the application method, but a spin coating method can be suitably used. The thickness of the resist film 30 may be appropriately set so as to be thicker than the nanowires 14 to be formed (so as to be thicker than both of the nanowires 14 and the pad electrodes 12A, 12B when they are formed at the same time).

[0051] Next, as shown in FIG. 2(C), the resist film 30 is developed to form a mask pattern 32 having a predetermined shape. The mask pattern 32 is produced by exposing the resist film 30 by electron beam lithography and developing it. The shape of the mask pattern 32 may be appropriately set according to the line width W and length L of the nanowire 14 to be formed. As shown in FIGS. 2(C) to 2(E), when the nanowire 14 and the pad electrodes 12A and 12B are formed at the same time, the shape of the mask pattern 32 may be determined according to the dimensions of the nanowire 14 and the pad electrodes 12A and 12B to be formed. In the portion of the mask pattern 32 where the resist film has been removed, the oxide layer 16 is exposed.

[0052] Next, as shown in FIG. 2(D), a metal film 34 is formed by, for example, electron beam evaporation or sputtering. At this time, a first portion 34A of the metal film is formed on the mask pattern 32, and a second portion 34B of the metal film is formed on the oxide layer 16 in a portion of the mask pattern 32 where the resist film has been removed. The metal film 34 preferably includes a Ti layer having a thickness of about 1 to 5 nm and a layer made of a metal (e.g., Pt) constituting the nanowire 14 and the pad electrodes 12A and 12B formed thereon. The Ti layer functions as an adhesive layer for adhering the layer made of a metal constituting the nanowire 14 and the pad electrodes 12A and 12B onto the oxide layer 16. As the adhesive layer, a Cr layer may be used instead of the Ti layer.

[0053] Next, as shown in FIG. 2(E), the mask pattern 32 is peeled off, and the first portion 34A of the metal film formed thereon is removed by a lift-off process to form the nanowire 14 and the pad electrodes 12A and 12B on the oxide layer 16. In this example, as shown in FIGS. 2(C) to 2(E), the nanowire 14 and the pad electrodes 12A and 12B are formed at the same time. However, it is also possible to form only the nanowire 14 in the above process, and then form the pad electrodes 12A and 12B separately, for example, by using a general photolithography method. The Ti layer or Cr layer is formed as an adhesive layer for adhering the nanowire 14 on the oxide layer 16, but Ti or Cr diffuses into the metal layer during the deposition of the metal constituting the nanowire 14, and most of the Ti layer or Cr layer disappears. Although Ti or Cr remains in islands in some places between the oxide layer 16 and the nanowire 14, the oxide layer 16 and the nanowire 14 are in direct contact with each other in most places, forming an ohmic contact.

[0054] The gas sensor 100 can be fabricated through the above steps. The gas sensor 100 fabricated according to Figs. 2(A)-(E) has the above-mentioned contact state (I) between the nanowire 14 and the oxide layer 16. By reversing the order of forming the nanowire 14 and the oxide layer 16 (i.e., reversing the order of the steps of Figs. 2(A) and 2(B)-(E)), a gas sensor can be fabricated having the above-mentioned contact state (II) between the nanowire 14 and the oxide layer 16. However, in this case, the oxide layer 16 is also formed on the pad electrodes 12A and 12B. Therefore, it is necessary to remove the oxide layer 16 on the pad electrodes 12A and 12B by, for example, argon sputtering, reactive ion etching, physical scratching, or other methods to enable electrical contact with the pad electrodes 12A and 12B. EXAMPLES

[0055] [Experimental Example 1] <Fabrication of gas sensor> The gas sensor was fabricated in the following procedure: First, a Si substrate (length: 15 mm × width: 15 mm × thickness: 0.5 mm) with a surface layer of about 1 μm made of SiO2 was prepared.

[0056] Next, cerium acetate hydrate Ce(CH3CO2)3·xH2O (Sigma-Aldrich, 99.9%) was dissolved in propionic acid (Wako Chemical Co., Ltd.) to prepare a 0.4 mol / kg cerium oxide (CeO2) precursor solution. After mixing, the precursor solution was stirred at 1000 rpm on a hot plate (110°C) for 30 minutes to obtain a clear and homogenous solution. The solution was then passed through a 0.2 μm PTFE syringe filter and stored at 4°C.

[0057] The precursor solution was applied onto the substrate by spin coating at 4000 rpm, and then heat-treated at 250°C for 1 hour using a rapid thermal analyzer (RTA) to form a cerium oxide (CeO2) layer (thickness: 28 nm) on the substrate. The resistivity of cerium oxide (CeO2) at 300°C is 200 Ω·m.

[0058] Next, Pt nanowires were formed on the CeO2 layer using an electron beam drawing device EBL (ELS-7500EX manufactured by Elionix). Specifically, electron beam resist ZEP-520A was applied on the CeO2 layer by spin coating, and then a mask pattern of a predetermined shape was drawn using the EBL device. Then, a Ti layer (thickness: 3 nm) and a Pt layer (thickness: 10 nm) were formed on the Ti layer by electron beam deposition. After that, a lift-off process was performed to peel off the mask pattern, and Pt nanowires (line width W: 8 nm, line thickness: 10 nm, line length L: 416 nm, cross-sectional shape perpendicular to the line: rectangular) were formed on the CeO2 layer. The Ti layer was formed as an adhesive layer for adhering the Pt nanowires on the CeO2 layer, but Ti diffused into the Pt layer during the deposition of the Pt layer, and most of the Ti layer disappeared. Although islands of Ti remain between the CeO2 layer and the Pt nanowire in some places, in most places the CeO2 layer is in direct contact with the Pt nanowire, forming an ohmic contact, that is, the CeO2 layer is located between the substrate and the Pt nanowire, and in contact with the bottom surface of the Pt nanowire.

[0059] Next, a first pad electrode and a second pad electrode (150 μm × 150 μm) each consisting of a Ti layer (thickness: 5 nm) and a Pt layer (thickness: 40 nm) on top of it were fabricated using a general photolithography method. In this way, a gas sensor combining a CeO2 layer and a Pt nanowire was fabricated.

[0060] <Oxygen gas detection test> The gas sensor was placed in a measurement chamber with variable oxygen pressure, and a semiconductor parameter analyzer system (Keysight Technologies B1500A) was used to apply a constant voltage (V = 1.0 V) between the first and second pad electrodes. Based on the change in the current I detected between the first and second pad electrodes, a test was conducted to detect oxygen gas, and various sensor characteristics were evaluated. The operating temperature T was set to 300°C (573K). When oxygen gas was ON, the oxygen gas pressure was set to 10 -3 When the oxygen gas is turned off, the oxygen gas pressure is changed from 5 Pa to 10 -3Pa (vacuum). That is, the oxygen pressure P O2 The pressure was set to 5 Pa. No carrier gas was introduced into the measurement chamber, only oxygen gas. The oxygen gas was turned on at 0 seconds and turned off at 300 seconds. Figure 4 is a graph showing the change in current I over time.

[0061] Here, the parameters relating to the sensor characteristics are defined as follows: I :Current value at a certain time I0: Initial current value I 01 : Initial current value (current value when oxygen gas is ON) I 02 : Initial current value (current value when oxygen gas is off) I s : Saturation current value I s1 : Saturation current value (after oxygen gas is turned on) I s2 : Saturation current value (after oxygen gas is turned off) ΔI1=I 01 -I s1 ΔI2=I 02 -I s2 Sensitivity S(%)=(ΔI1 / I 01 ) x 100 Response time t res : Current value I is the initial current value I 01 The time required for a change of 90% of ΔI1 from Recovery time t rec : Current value I is the initial current value I 02 The time required for a change of 90% of ΔI2 from If the current value does not saturate even after 300 seconds have passed since the oxygen gas was turned on or off, the current value at the time 300 seconds have passed since the oxygen gas was turned on or off is regarded as the saturated current value.

[0062] In this experiment, the response time t res is 21 seconds, recovery time t recThe time to response was 20 seconds, realizing a high-speed response to oxygen gas. In addition, the sensitivity S was 2.4%, realizing high sensitivity to oxygen gas.

[0063] [Experimental Example 2] A gas sensor was fabricated under the same conditions as in Experimental Example 1, except that the line width W of the Pt nanowire was changed to five levels, namely, 23 nm, 50 nm, 74 nm, and 124 nm (see the left side of Figure 3), in addition to 8 nm. The gas sensor was fabricated under the same conditions as in Experimental Example 1 (applied voltage V = 1.0 V, operating temperature T = 300 °C (573 K), oxygen pressure P O2 An oxygen gas detection test was conducted at a pressure of 100 psi (0.025 Pa). The oxygen gas was turned on at 0 seconds and off at 300 seconds. Figure 5 is a graph showing the change in current I over time at each level. Table 1 shows the sensor performance at each level.

[0064] [Table 1]

[0065] As is clear from Table 1, the narrower the line width W, the faster the response to oxygen gas. On the other hand, the sensitivity S had little dependency on the line width W.

[0066] [Experimental Example 3] Gas sensors were fabricated under the same conditions as in Experimental Example 1, except that the Pt nanowire length L was changed to five levels, namely 980 nm, 288 nm, 191 nm, and 93 nm, in addition to 416 nm (see the right side of Figure 3). Gas sensors were fabricated under the same conditions as in Experimental Example 1 (applied voltage V = 1.0 V, operating temperature T = 300 °C (573 K), oxygen pressure P O2 An oxygen gas detection test was conducted at a pressure of 100 psi (0.025 Pa). The oxygen gas was turned on at 0 seconds and off at 300 seconds. Figure 6 is a graph showing the change in current I over time at each level. Table 2 shows the sensor performance at each level.

[0067] [Table 2]

[0068] As is clear from Table 2, the longer the line length L, the faster the response and the higher the sensitivity to oxygen gas.

[0069] [Experimental Example 4] The gas sensor was fabricated under the same conditions as in Experimental Example 1. The conditions were the same as in Experimental Example 1 (operating temperature T = 300°C (573K), oxygen pressure P O2 An oxygen gas detection test was conducted at a pressure of 100 psi (=5 Pa). The oxygen gas was turned on for 100 seconds and off for 500 seconds. Figures 7A and 7B are graphs showing the change in current I over time at each level. The sensitivity S at each level is also shown in the graphs.

[0070] It can be seen from Figures 7A and 7B that the response time and recovery time are independent of the applied voltage V. Furthermore, the sensitivity S is also independent of the applied voltage V, and is approximately the same value between 1.42 and 1.56%. Furthermore, a response is observed even when the applied voltage V is 10 mV. Therefore, the gas sensor of this experimental example can operate sufficiently even at an applied voltage as low as 10 mV, if measures are taken to reduce noise. This contributes to the realization of a gas sensor with low power consumption.

[0071] [Experimental Example 5] The gas sensors were fabricated under the same conditions as in Experimental Example 1. The operating temperature T was varied (303K, 333K, 363K, 393K, 423K, 453K, 543K, 573K), but the conditions were the same as in Experimental Example 1 (applied voltage V = 1.0V, oxygen pressure P O2 = 5 Pa). The oxygen gas was turned on at 0 seconds and off at 300 seconds. The operating temperature T was adjusted by adjusting the temperature setting of a microheater installed on the back side of the substrate. Figures 8A and 8B are graphs showing the change in current I over time at each level. Table 3 shows the sensor performance at each level.

[0072] [Table 3]

[0073] As is clear from Table 3, the higher the operating temperature T, the faster the response and the higher the sensitivity to oxygen gas. In addition, the fact that a response was obtained even at an operating temperature T of 303 K, which is almost room temperature, suggests that there is no need to raise the sensor temperature during gas sensor operation. This shows that the gas sensor of the present invention can be driven with low power consumption without heating by a heater.

[0074] [Experimental Example 6] The gas sensor was fabricated under the same conditions as in Experimental Example 1. O2 An oxygen gas detection test was conducted under the same conditions as in Experimental Example 1 (applied voltage V=1.0 V, operating temperature T=300°C (573K)), except that the pressure was set to various levels (10 Pa, 5 Pa, 3 Pa, 0.1 Pa). The oxygen gas was turned on at 0 seconds and turned off at 300 seconds. Figure 9 is a graph showing the change in current I over time at each level. Table 4 shows the sensor performance at each level.

[0075] [Table 4]

[0076] As is clear from Table 4, the sensitivity S depends on the oxygen pressure, and the higher the oxygen pressure, the higher the sensitivity. On the other hand, the response time and recovery time do not depend very much on the oxygen pressure. In addition, a response is obtained even at an oxygen pressure of 0.1 Pa, which shows that the range of detectable oxygen gas concentrations is wide.

[0077] [Experimental Example 7] A gas sensor was fabricated under the same conditions as in Experimental Example 1, except that the line thickness of the Pt nanowire was set to three levels: 3 nm, 6 nm, and 10 nm. The gas sensor was fabricated under the same conditions as in Experimental Example 1 (applied voltage V = 1.0 V, operating temperature T = 300 °C (573 K), oxygen pressure P O2= 5 Pa). The oxygen gas was turned on at 0 seconds, and was switched off / on every 100 seconds thereafter. Figure 10 is a graph showing the change in current I over time at each level. The sensitivity S calculated from Figure 10 was 3.8% at a thickness of 3 nm, 2.5% at a thickness of 6 nm, and 3.6% at a thickness of 10 nm. This shows that the sensitivity S does not depend very much on the Pt thickness. If the line thickness of the Pt nanowire is less than 1 nm, electrical conduction as a Pt nanowire cannot be obtained, so the line thickness is preferably 1 nm or more.

[0078] [Experimental Example 8] A gas sensor was fabricated under the same conditions as in Experimental Example 1, except that the thickness of the CeO2 layer was set to two levels, 28 nm and 56 nm. The gas sensor was fabricated under the same conditions as in Experimental Example 1 (applied voltage V = 1.0 V, operating temperature T = 300 °C (573 K), oxygen pressure P O2 =5 Pa), an oxygen gas detection test was also conducted at the same time. The oxygen gas was turned on at 0 seconds, and was switched off / on every 100 seconds thereafter. Figure 11 is a graph showing the change in current I over time at each level. It can be seen from Figure 11 that the response time and recovery time do not depend on the thickness of the CeO2 layer. Furthermore, the sensitivity S calculated from Figure 11 was 2.5% for both levels. This shows that the sensitivity S does not depend on the thickness of the CeO2 layer.

[0079] [Experimental Example 9] A gas sensor was fabricated under the same conditions as in Experimental Example 1, except that the order of forming the CeO2 layer and the Pt nanowires was reversed. That is, first, a Si substrate with a surface layer made of SiO2 was prepared as in Experimental Example 1. Next, Pt nanowires were formed on the SiO2 layer using an electron beam drawing device EBL (ELS-7500EX manufactured by Elionix). Specifically, electron beam resist ZEP-520A was applied on the SiO2 layer by spin coating, and then a mask pattern of a predetermined shape was drawn using the EBL device. Then, a Ti layer (thickness: 3 nm) and a Pt layer (thickness: 10 nm) were formed on the Ti layer by electron beam deposition. Then, a lift-off process was performed to peel off the mask pattern, and Pt nanowires (line width W: 8 nm, line thickness: 10 nm, line length L: 416 nm, cross-sectional shape perpendicular to the line: rectangular) were formed on the SiO2 layer. The Ti layer was formed as an adhesive layer for adhering the Pt nanowires to the SiO2 layer.

[0080] Next, using a conventional photolithography method, a first pad electrode and a second pad electrode (150 μm × 150 μm) each consisting of a Ti layer (thickness: 5 nm) and a Pt layer (thickness: 40 nm) on top of it were fabricated on the SiO2 layer.

[0081] Next, the precursor solution was applied by spin coating at 4000 rpm so as to cover the SiO2 layer of the substrate, the Pt nanowires, and the first and second pad electrodes, and then heat-treated at 400°C for 1 hour using a rapid thermal processing (RTA) to form a cerium oxide (CeO2) layer (thickness: 28 nm) so as to cover the SiO2 layer of the substrate, the Pt nanowires, and the first and second pad electrodes. In this case, the Pt nanowires are embedded in the CeO2 layer. That is, the CeO2 layer is located on the Pt nanowires and is in contact with the top surface of the Pt nanowires. The CeO2 layer is also in contact with the side surface of the Pt nanowires. The CeO2 layer and the Pt nanowires form an ohmic contact.

[0082] Finally, the CeO2 layer on the first and second pad electrodes was physically scratched to remove it, allowing electrical contact to be made from the first and second pad electrodes. In this way, a gas sensor combining a CeO2 layer and a Pt nanowire was fabricated.

[0083] The same conditions as in Experiment 1 (applied voltage V = 1.0 V, operating temperature T = 300 °C (573 K), oxygen pressure P O2 An oxygen gas detection test was conducted at a pressure of 0.05 Pa (=5 Pa). The oxygen gas was turned on at 0 seconds, and was switched off and on every 100 seconds thereafter. FIG. 12 is a graph showing the change in current I over time. In this experimental example, the response time t res is 25 seconds, recovery time t rec The time to response was 68 seconds or more, realizing a high-speed response to oxygen gas. In addition, the sensitivity S was 1.5%, realizing high sensitivity to oxygen gas.

[0084] [Experimental Example 10] A gas sensor was fabricated under the same conditions as in Experimental Example 1, except that the oxide layer was a SnO2 layer or a ZrO2 layer instead of a CeO2 layer. Then, the gas sensor was fabricated under the same conditions as in Experimental Example 1 (applied voltage V = 1.0 V, operating temperature T = 300 °C (573 K), oxygen pressure P O2 = 5 Pa), an oxygen gas detection test was performed.

[0085] In the case of the SnO2 layer, the oxygen gas was turned on at 100 seconds, and then switched off and on approximately every 100 seconds. Figure 13(A) is a graph showing the change in current I over time. Response time t res is 12 seconds, recovery time t rec The time to response was 8 seconds, realizing a high-speed response to oxygen gas. In addition, the sensitivity S was 2.3%, realizing high sensitivity to oxygen gas.

[0086] In the case of the ZrO2 layer, the oxygen gas was turned on at 0 seconds and turned off at 600 seconds. Figure 13(B) is a graph showing the change in current I over time. Response time t res The recovery time t recThe time required for the detection was longer than 2 hours. The sensitivity S was 97%, which means that high sensitivity to oxygen gas was achieved.

[0087] The SnO2 layer was formed by the following procedure: Tin(II) acetylacetonate C was added to propionic acid (manufactured by Wako Chemical Co., Ltd.). 10 H 14 0.4 mol / kg tin oxide (SnO2) precursor solution was prepared by dissolving O4Sn (Sigma-Aldrich, 99.9%). After mixing, the precursor solution was stirred at 1000 rpm on a hot plate (110°C) for 30 minutes to obtain a clear and homogenous solution. The solution was then passed through a 0.2 μm PTFE syringe filter and stored at 4°C.

[0088] The precursor solution was applied onto the substrate by spin coating at 3000 rpm, and then heat-treated at 300°C for 1 hour using a rapid thermal analyzer (RTA) to form a tin oxide (SnO2) layer (thickness: 30 nm) on the substrate. The resistivity of tin oxide (SnO2) at 300°C is 10 Ω·m.

[0089] The ZrO2 layer was formed as follows. A sputtering target made of ZrO2 was used to perform sputtering in an Ar atmosphere to form a zirconium oxide (ZrO2) layer (thickness: 30 nm) on the substrate. The resistivity of zirconium oxide (ZrO2) at 300°C is 80,000 Ω·m.

[0090] [Experimental Example 11] The gas sensor was fabricated under the same conditions as in Experimental Example 1. Then, the applied voltage V d An oxygen gas detection test was carried out under the same conditions as in Experimental Example 1 (operating temperature T = 300°C (573K)), except that the input voltage was set to 0.1 V and nitrogen gas (flow rate: 1000sccm) was flowed into the measurement chamber as the carrier gas. The oxygen gas was turned ON at 0 seconds and OFF at 600 seconds. The oxygen gas flow rate was 50sccm and the oxygen concentration was 5%. Figure 14 is a graph showing the change in current I over time. This experimental example shows that oxygen gas can be detected even in an environment where a carrier gas is present. [Industrial Applicability]

[0091] The gas sensor of the present invention has a fast response speed to oxygen gas and high sensitivity, and therefore may be applicable to oxygen sensors in internal combustion engines, breath sensors, and the like. [Explanation of symbols]

[0092] 100 Gas Sensor 10 Substrate 12A 1st pad electrode 12B Second pad electrode 14 Nanowires 16 Oxide layer 18 Power supply 20 ammeter 22 Voltmeter 30 Resist film 32 Mask Pattern 34 Metal Film 34A First part of metal film 34B Second part of metal film

Claims

1. a substrate having an insulating surface; a first pad electrode and a second pad electrode formed on the insulating surface of the substrate; a nanowire formed on the insulating surface of the substrate, the nanowire connecting the first pad electrode and the second pad electrode, the nanowire being made of one or more metals selected from platinum (Pt), palladium (Pd), rhodium (Rh), ruthenium (Ru), osmium (Os), iridium (Ir), and alloys thereof; an oxide layer in contact with the nanowire, the oxide layer being made of a high-resistance semiconductor of an oxide of a metal different from the metal constituting the nanowire, the oxide layer satisfying at least one of the following: (I) being located between the insulating surface of the substrate and the nanowire and in contact with the bottom surface of the nanowire, or (II) being located on the nanowire and in contact with the top surface of the nanowire; having The line width of the nanowire is 5 nm or more and 150 nm or less; A gas sensor that causes a current to flow between the first pad electrode and the second pad electrode, and detects a gas based on a change in an electrical signal detected between the first pad electrode and the second pad electrode.

2. A substrate having an insulating surface; a first pad electrode and a second pad electrode formed on the insulating surface of the substrate; a nanowire formed on the insulating surface of the substrate, the nanowire connecting the first pad electrode and the second pad electrode, the nanowire being made of one or more metals selected from platinum (Pt), palladium (Pd), rhodium (Rh), ruthenium (Ru), osmium (Os), iridium (Ir), and alloys thereof; an oxide layer in contact with the nanowire, the oxide layer being made of a high-resistance semiconductor of an oxide of a metal different from the metal constituting the nanowire, the oxide layer satisfying at least one of the following: (I) being located between the insulating surface of the substrate and the nanowire and in contact with the bottom surface of the nanowire, or (II) being located on the nanowire and in contact with the top surface of the nanowire; having The thickness of the nanowire is 1 nm or more and 20 nm or less; A gas sensor that causes a current to flow between the first pad electrode and the second pad electrode, and detects a gas based on a change in an electrical signal detected between the first pad electrode and the second pad electrode.

3. A substrate having an insulating surface; a first pad electrode and a second pad electrode formed on the insulating surface of the substrate; a nanowire formed on the insulating surface of the substrate, the nanowire connecting the first pad electrode and the second pad electrode, the nanowire being made of one or more metals selected from platinum (Pt), palladium (Pd), rhodium (Rh), ruthenium (Ru), osmium (Os), iridium (Ir), and alloys thereof; an oxide layer in contact with the nanowire, the oxide layer being made of a high-resistance semiconductor of an oxide of a metal different from the metal constituting the nanowire, the oxide layer satisfying at least one of the following: (I) being located between the insulating surface of the substrate and the nanowire and in contact with the bottom surface of the nanowire, or (II) being located on the nanowire and in contact with the top surface of the nanowire; having A gas sensor that detects oxygen gas based on a change in an electrical signal detected between the first pad electrode and the second pad electrode by passing an electric current between the first pad electrode and the second pad electrode.

4. The gas sensor according to any one of claims 1 to 3, wherein the length of the nanowire is 80 nm or more.

5. 5. The gas sensor according to claim 1, wherein the high resistance semiconductor constituting the oxide layer is at least one selected from the group consisting of cerium oxide, tin oxide, zirconium oxide, zinc oxide, tungsten oxide, iron oxide, nickel oxide, cerium-zirconium oxide, titanium oxide, cobalt oxide, niobium oxide, tantalum oxide, rhodium oxide, and hafnium oxide.

6. 6. The gas sensor according to claim 1, wherein the oxide layer has a thickness of 5 nm or more.

7. The gas sensor according to any one of claims 1 to 6, wherein the nanowire and the oxide layer are in ohmic contact with each other.

8. 8. The gas sensor according to claim 1, wherein the substrate is any one of a glass substrate, an alumina substrate, a zirconia substrate, and a silicon substrate having a silicon oxide film formed on a surface thereof.

9. 9. The gas sensor according to claim 1, wherein the first pad electrode and the second pad electrode are made of the same metal as the nanowire.

Citation Information

Patent Citations

  • Resistance type oxygen sensor

    JP2003149189A

  • nano sensor

    JP2004515782A

  • Fluid sensor and method

    JP2005283578A

  • Method and apparatus for detecting hydrogen gas

    JP2006526155A

  • Gas sensor element and gas sensor

    JP2015137998A